Zeolite membrane composite body, separation device, dehydration device, and method of manufacturing zeolite membrane composite body
The use of a porous glass support with specific dimensions and aerosol deposition for forming a zeolite membrane composite addresses performance limitations, enabling efficient gas separation and dehydration with improved efficiency and reduced production time.
Patent Information
- Application Number
- JP2023055806
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing zeolite membrane composites face challenges in achieving optimal performance due to variations in fluid separation efficiency and dehydration capabilities, which are influenced by the type of aluminosilicate, porosity of the support, and material of the support, limiting their range of applications.
A zeolite membrane composite using a porous glass support with an average pore diameter of 50 nm to 100 μm and a zeolite membrane thickness of 0.1 μm to 100 μm, formed via a gas deposition method, particularly aerosol deposition, allowing for efficient separation and dehydration without the need for high-temperature heat treatment.
The method enables the production of a zeolite membrane composite with high permeability and selectivity, suitable for various applications, including gas separation and dehydration, in a shorter time compared to traditional hydrothermal synthesis methods.
Smart Images

Figure 2024143237000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a zeolite membrane composite, a separation device, a dehydration device, and a method for producing a zeolite membrane composite. [Background technology]
[0002] In recent years, various research and development efforts have been conducted on zeolite membrane composites formed by forming a zeolite membrane on a porous body, for applications such as the separation of specific molecules by utilizing the molecular sieving action of zeolite.
[0003] As such a zeolite membrane composite, there have been proposed one using a porous ceramic support or a metal support (Patent Documents 1 to 3).
[0004] Patent Document 1 discloses a composite in which a zeolite membrane is formed on the surface of a ceramic sintered body (such as an alumina sintered body, a mullite sintered body, or a titania sintered body) by a hydrothermal synthesis method.
[0005] On the other hand, Patent Document 2 discloses a composite in which the surface of a porous metal oxide support is coated with metal oxide particles or metal nitride particles, and a zeolite membrane is formed on the coated surface by a hydrothermal synthesis method.
[0006] Furthermore, Patent Document 3 discloses a composite obtained by treating a tubular porous metal support with a base or acid, and then forming a zeolite membrane on the treated portion by a hydrothermal synthesis method. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2020 / 255867 [Patent Document 2] JP 2001-146416 A [Patent Document 3] JP 2010-142809 A Summary of the Invention [Problem to be solved by the invention]
[0008] Zeolite membrane composites are used for various applications, and the required performance (type of fluid that can be separated, permeation rate, etc.) varies depending on the application. The performance of a zeolite membrane composite is affected by the type of aluminosilicate that constitutes the zeolite membrane, the porosity of the support, and also the material of the support. Therefore, in order to expand the range of applications of zeolite membrane composites, it is desirable to accumulate knowledge about supports that can be used for zeolite membrane composites.
[0009] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a zeolite membrane composite which has a porous glass support as a support for a zeolite membrane and can be used for various applications, a method for producing the zeolite membrane composite, and a separation apparatus and a dehydration apparatus which use the zeolite membrane composite. [Means for solving the problem]
[0010] The zeolite membrane composite according to the present invention for achieving the above object has the following characteristic configuration: The present invention is characterized by having a porous glass support and a zeolite membrane formed on the surface of the porous glass support.
[0011] According to the above-mentioned characteristic configuration, the zeolite membrane formed on the porous glass support enables separation of a target substance from a fluid and removal of water. In other words, the zeolite membrane composite having the above-mentioned characteristic configuration can be used in various applications that utilize the functions of the zeolite membrane.
[0012] Further characteristic features of the zeolite membrane composite according to the present invention are as follows: The porous glass support has an average pore size of 50 nm or more and 100 μm or less.
[0013] If the average pore size of the porous glass support is small, the fluid permeability is low and the amount of fluid flowing to the zeolite membrane is reduced, resulting in a decrease in the efficiency of separation of the target to be separated from the fluid and removal of water. On the other hand, if the average pore size is large, the formation of the zeolite membrane on the surface of the porous glass support by a gas deposition method or the like becomes poor. According to the above characteristic configuration, the zeolite membrane has good membrane quality and the porous glass support has appropriate permeability, so that the function of the zeolite membrane is fully exerted.
[0014] Further characteristic features of the zeolite membrane composite according to the present invention are as follows: The zeolite membrane has a thickness of 0.1 μm or more and 100 μm or less.
[0015] If the permeability of the zeolite membrane is low, it becomes difficult for the fluid to pass through the zeolite membrane, and the efficiency of separating the target to be separated from the fluid, removing water, etc. decreases. According to the above-mentioned characteristic configuration, the zeolite membrane has an appropriate permeability, so that the function of the zeolite membrane is sufficiently exhibited.
[0016] The characteristic configuration of the separation device according to the present invention for achieving the above object is as follows: The present invention is characterized in that the above-mentioned zeolite membrane composite is included, and gas separation is performed by the zeolite membrane composite.
[0017] According to the above characteristic configuration, it is possible to separate and recover an arbitrary component from a mixed gas containing a plurality of components.
[0018] The characteristic configuration of the dehydrator according to the present invention for achieving the above object is as follows: The present invention has the above-mentioned zeolite membrane composite, and dehydrates a mixed fluid containing water by using the zeolite membrane composite.
[0019] According to the above characteristic configuration, water can be separated from a mixed fluid containing water, and therefore water and other components in the mixed fluid can be separated and recovered.
[0020] The method for producing a zeolite membrane composite according to the present invention for achieving the above object is characterized by the following features: A method for producing a zeolite membrane composite having a porous glass support and a zeolite membrane formed on a surface of the porous glass support, comprising the steps of: The method includes a zeolite membrane forming step of forming a zeolite membrane on the surface of the porous glass support by a gas deposition method.
[0021] Generally, zeolite membranes are formed on a porous support by a liquid-phase synthesis method called hydrothermal synthesis. A raw material solution containing aluminum and silicon, which are the main raw materials of the zeolite membrane, is mixed with a solution containing various cationic species, and a hydrothermal synthesis method is performed under high-temperature and high-pressure hydrothermal conditions to form seed crystals. A porous body is then immersed in the dispersion in which the seed crystals are dispersed, and the seed crystals are attached to the porous body. This process is repeated several times. In addition, when forming a zeolite membrane by a hydrothermal synthesis method, a structure-directing agent is required to determine the size of the pore diameter that allows the separation of the target molecules by molecular sieving, and a heat treatment step is usually performed to remove the structure-directing agent after the formation of the zeolite membrane. This heat treatment step requires heating at 400 to 1000°C for 10 to 200 hours depending on the type of structure-directing agent. Thus, when forming a zeolite membrane by hydrothermal synthesis, multiple steps are required to obtain a desired zeolite membrane, and it takes a considerable amount of time to form the membrane. In addition, heat treatment is required to remove the structure-directing agent, and it is difficult to use a porous glass support as a support from the viewpoint of heat resistance. However, according to the above-mentioned characteristic configuration, the gas deposition method is used, which allows the membrane formation process to be performed in a shorter time than the hydrothermal synthesis method and does not require heat treatment at high temperatures. Therefore, a porous glass support is used as a support, and a zeolite membrane can be formed on the surface of the porous glass support in a shorter time than the hydrothermal synthesis method. Therefore, the above-mentioned method for producing a zeolite membrane composite can suitably produce a zeolite membrane composite having a porous glass support as a support in a shorter time than the case of using the hydrothermal synthesis method. In addition, the separation performance of the zeolite membrane composite includes permeability and selectivity, and the permeability depends on the pore size of the support as well as the properties of the zeolite membrane. The larger the pore size of the support, the higher the permeability. However, if the pore size of the support is large, the dispersion liquid leaks out of the pores during seed crystal formation when the zeolite membrane is formed by hydrothermal synthesis. Therefore, when the zeolite membrane is formed by hydrothermal synthesis, the pore size of the support cannot be made large. However, in the above-mentioned method for producing a zeolite membrane composite, a porous glass support is used as the support. Generally, a porous glass support has random pore shapes. Therefore, in the above-mentioned method for producing a zeolite membrane composite, it is possible to form a zeolite membrane by the gas deposition method even if the pore size is large. Therefore, the above-mentioned method for producing a zeolite membrane composite can produce a high-performance (high permeability) zeolite membrane composite.
[0022] The method for producing a zeolite membrane composite according to the present invention further comprises the steps of: The zeolite membrane forming step is characterized in that an aerosol in which aluminosilicate particles are dispersed in a carrier gas is sprayed toward the surface of the porous glass support to form a zeolite membrane on the surface.
[0023] According to the above-mentioned characteristic configuration, a zeolite membrane can be formed by the so-called aerosol deposition method. The aerosol deposition method enables the membrane formation process in a shorter time than the hydrothermal synthesis method, and does not require heat treatment at high temperatures. Therefore, according to the above-mentioned method for producing a zeolite membrane composite, a zeolite membrane composite having a porous glass support as a support can be preferably produced in a shorter time than when the hydrothermal synthesis method is used. Effect of the Invention
[0024] As described above, the zeolite membrane composite, the method for producing the zeolite membrane composite, and the separation device and dehydration device using the zeolite membrane composite according to the present invention are provided with a porous glass support as a support for the zeolite membrane, and can be used for various applications. [Brief description of the drawings]
[0025] [Figure 1] FIG. 1 is a diagram showing a schematic configuration of a zeolite membrane composite according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing a schematic configuration of a membrane forming apparatus used in a method for producing a zeolite membrane composite according to an embodiment of the present invention. [Diagram 3] 4A to 4C are diagrams for explaining a procedure for separating a mixed gas using the separation device according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, a zeolite membrane composite according to an embodiment, a method for producing the zeolite membrane composite, and a separation device using the zeolite membrane composite will be described with reference to the drawings. In the following description, the terms "upper" and "lower" refer to the upper and lower sides in the drawings.
[0027] [Zeolite membrane composite C] First, the zeolite membrane composite C of this embodiment will be described.
[0028] Fig. 1 is a schematic diagram showing a zeolite membrane composite C according to this embodiment. As shown in Fig. 1, the zeolite membrane composite C has a porous glass substrate K and a zeolite membrane M formed on a surface Ka of the porous glass substrate K. In this embodiment, the porous glass substrate K corresponds to the "porous glass support".
[0029] [Porous glass substrate K] The porous glass substrate K, which is generally plate-shaped in this embodiment, serves as a support for the zeolite membrane M and maintains the strength of the zeolite membrane composite C. As the porous glass substrate K, one produced by a known method or a commercially available one can be used.
[0030] The average pore diameter of the porous glass substrate K is not particularly limited, but if the average pore diameter is too small, the fluid permeability is reduced, and the amount of fluid flowing to the zeolite membrane M is reduced, and as a result, separation and dehydration of the fluid may become impossible. Conversely, if the average pore diameter is too large, the film-forming properties of the zeolite membrane M by the gas deposition method (specifically, the aerosol deposition method) may be reduced. Therefore, the average pore diameter is preferably 50 nm or more and 100 μm or less. For example, the porous glass substrate K may have pores with a pore diameter of 50 to 100 nm, or may have pores with a pore diameter of 50 to 100 μm.
[0031] The thickness H1 of the porous glass substrate K may be appropriately set based on the fluid permeability and the strength required for the zeolite membrane composite C. Specifically, if the thickness H1 of the porous glass substrate K is too thick, the permeability decreases and too little fluid flows to the zeolite membrane M, whereas if the thickness H1 is too thin, sufficient strength of the zeolite membrane composite C cannot be ensured. Therefore, the thickness H1 of the porous glass substrate K is preferably 0.1 mm or more and 3 mm or less, more preferably 0.3 mm or more and 2 mm or less, and even more preferably 0.5 mm or more and 1.2 mm or less.
[0032] The shape and surface roughness of the surface Ka of the porous glass substrate K are not particularly limited. The surface Ka of the porous glass substrate K may have any shape and surface roughness that allows a zeolite membrane M to be formed on the surface Ka. Specifically, the shape and surface roughness may be such that a zeolite membrane M can be formed on the surface Ka by a gas deposition method (specifically, an aerosol deposition method), and the shape and surface roughness may be similar to those of a commercially available product.
[0033] [Zeolite Membrane M] The zeolite membrane M plays a role in separating specific molecules by utilizing the molecular sieve action of zeolite (aluminosilicate). The zeolite membrane M is made of zeolite (aluminosilicate). The zeolite constituting the zeolite membrane M can be appropriately selected from known zeolite species having various skeletal structures according to the molecular size of the separation target. For example, chabazite (CHA) with a crystal pore diameter of 0.38 nm, faujasite (FAU) with a pore diameter of 0.74 nm, A-type zeolite (LTA) with a pore diameter of 0.41 nm, etc. can be used.
[0034] The thickness H2 of the zeolite membrane M may be appropriately set in consideration of the permeability of the fluid. Specifically, if the thickness H2 of the zeolite membrane M is too thick, the permeability is reduced, making it difficult for the fluid to pass through the zeolite membrane M, and the efficiency of separation of the separation target from the mixed fluid and removal of water (dehydration) is reduced. Conversely, if the thickness H2 is too thin, the permeability is too high, and the efficiency of separation of the separation target from the mixed fluid and removal of water (dehydration) is reduced. Therefore, the thickness H2 of the zeolite membrane M is preferably 0.1 μm or more and 100 μm or less, more preferably 0.2 μm or more and 80 μm or less, and even more preferably 0.5 μm or more and 50 μm or less.
[0035] In the zeolite membrane composite C of this embodiment, the zeolite membrane M formed on the surface Ka of the porous glass substrate K enables separation of a target substance from a mixed fluid and removal of water (dehydration).
[0036] Next, a method for producing the zeolite membrane composite C according to this embodiment will be described. First, a membrane forming apparatus 1 used in this production method will be described.
[0037] [Film deposition equipment 1] Fig. 2 is a diagram showing a schematic configuration of the film forming apparatus 1. As shown in Fig. 2, the film forming apparatus 1 is an apparatus that ejects an aerosol, in which raw material powder made of aluminosilicate particles is dispersed in a carrier gas, toward the surface Ka of the porous glass substrate K to form a zeolite film M on the surface Ka of the porous glass substrate K. In other words, the film forming apparatus 1 is an apparatus that forms a zeolite film M on the surface Ka of the porous glass substrate K by an aerosol deposition method.
[0038] In this embodiment, the film forming apparatus 1 includes a processing chamber 2 in which a porous glass substrate K is disposed, a holding unit 4 which holds the porous glass substrate K which is the target of the film forming processing, a moving mechanism 3 configured to move the holding unit 4, an aerosol transport pipe 5 which ejects an aerosol from an ejection tip 5a, an aerosol generation unit 15 which generates an aerosol in which raw material powder is dispersed in a gas, a raw material powder supply mechanism 16 which delivers the raw material powder to the aerosol generation unit 15, and a carrier gas delivery mechanism 18 which delivers a carrier gas to the aerosol generation unit 15.
[0039] The processing chamber 2 is made of an airtight casing, and has an opening 2a formed on the upper end surface. A holder 4 and an aerosol transport pipe 5 are disposed inside the processing chamber 2. A mechanical booster pump P1 and a vacuum pump P2 serving as exhaust equipment are connected to the opening 2a of the processing chamber 2 via an exhaust pipe S1. The pressure inside the processing chamber 2 is reduced to a predetermined pressure (for example, about 0.75 kPa) or less by exhausting gas by the mechanical booster pump P1 and the vacuum pump P2.
[0040] The holder 4 is configured to be able to hold the porous glass substrate K with the surface Ka facing downward so that the surface Ka is parallel to a horizontal plane. Known techniques such as a technique using vacuum suction or a technique using Coulomb force can be used to hold the porous glass substrate K.
[0041] The moving mechanism 3 is composed of a horizontal drive mechanism (not shown) that moves the holder 4 in the horizontal direction, an elevation drive mechanism (not shown) that moves the holder 4 in the vertical direction, etc. Although the moving mechanism 3 is shown to be disposed outside the processing chamber 2 in FIG. 2, the moving mechanism 3 may be disposed inside the processing chamber 2.
[0042] The aerosol transport pipe 5 is a cylindrical straight pipe member, and the cross-sectional shape of the ejection end 5a is circular. The aerosol transport pipe 5 is disposed in the processing chamber 2 so that the ejection end 5a faces the holding part 4. The end of the aerosol transport pipe 5 opposite the ejection end 5a is connected to the aerosol generating part 15. With this aerosol transport pipe 5, the aerosol is ejected from the ejection end 5a toward the surface Ka of the porous glass substrate K.
[0043] As described above, the aerosol generating unit 15 is configured to generate an aerosol in which raw material powder is dispersed in a gas. The aerosol generating unit 15 is connected to the aerosol transport pipe 5, as well as the raw material supply pipe S2 and the carrier gas delivery pipe S3 described below. The aerosol generating unit 15 generates an aerosol in which raw material powder supplied at a constant speed by the raw material powder supply mechanism 16 and a carrier gas delivered by the carrier gas delivery mechanism 18 are mixed. The generated aerosol is delivered to the aerosol transport pipe 5.
[0044] The raw material powder supply mechanism 16 is composed of a raw material powder supply unit 17, a raw material supply pipe S2, etc. Raw material powder is stored in the raw material powder supply unit 17. The raw material powder is supplied to the aerosol generating unit 15 through the raw material supply pipe S2. The raw material powder will be described in detail later.
[0045] The carrier gas delivery mechanism 18 is composed of a gas supply unit 19, a carrier gas pressure control unit 20, a carrier gas flow rate control unit 21, a carrier gas delivery pipe S3, and the like.
[0046] A carrier gas supply pipe S3 is connected to the gas supply unit 19. The gas supply unit 19 is configured to supply a carrier gas such as air, N2, He, or Ar to the carrier gas supply pipe S3 by a compressor or a gas cylinder.
[0047] The carrier gas delivery pipe S3 is for delivering the carrier gas supplied from the gas supply unit 19 to the aerosol generation unit 15. In this embodiment, the carrier gas delivered from the gas supply unit 19 is delivered to the aerosol generation unit 15 via the carrier gas pressure control unit 20 and the carrier gas flow rate control unit 21 in this order. That is, the carrier gas delivery pipe S3 is composed of a plurality of pipes connecting the gas supply unit 19, the carrier gas pressure control unit 20, the carrier gas flow rate control unit 21, and the aerosol generation unit 15. A pressure sensor Q for detecting the pressure in the carrier gas delivery pipe S3 is provided between the carrier gas flow rate control unit 21 and the aerosol generation unit 15 in the carrier gas delivery pipe S3.
[0048] The carrier gas pressure control unit 20 stabilizes the carrier gas flowing through the carrier gas delivery pipe S3 at an appropriate pressure. The carrier gas flow rate control unit 21 controls the flow rate of the carrier gas flowing through the carrier gas delivery pipe S3. The operations of the carrier gas pressure control unit 20 and the carrier gas flow rate control unit 21 are appropriately controlled by a control device based on the pressure detected by the pressure sensor Q.
[0049] [Raw material powder] The raw material powder is composed of aluminosilicate particles, and in this embodiment, the aluminosilicate particles have an average particle size of 0.5 μm to 10 μm. As the aluminosilicate constituting the raw material powder, those having various skeletal structures such as FAU and LTA can be used.
[0050] [Method for producing zeolite membrane composite C] Next, a method for producing the zeolite membrane composite C according to this embodiment will be described. This production method includes a zeolite membrane formation step of forming a zeolite membrane M on the surface Ka of a porous glass substrate K by a gas deposition method. In this embodiment, in the zeolite membrane formation step, an aerosol in which aluminosilicate particles are dispersed in a carrier gas is ejected toward the surface Ka of the porous glass substrate K to form the zeolite membrane M on the surface Ka.
[0051] Specifically, in this embodiment, first, the carrier gas is fed from the gas supply unit 19 to the aerosol generation unit 15 while adjusting the flow rate and pressure of the carrier gas flowing through the carrier gas feed pipe S3 by the carrier gas pressure control unit 20 and the carrier gas flow rate control unit 21. In the aerosol generation unit 15, an aerosol is generated in which the fed carrier gas and the raw material powder fed from the raw material powder supply unit 17 are mixed. The generated aerosol is fed to the aerosol transport pipe 5.
[0052] The aerosol fed to the aerosol transport pipe 5 is ejected from the ejection tip 5a toward the surface Ka of the porous glass substrate K, and the ejected aerosol collides with the surface Ka of the porous glass substrate K, forming a zeolite membrane M on the surface Ka (zeolite membrane formation process).
[0053] As described above, in the method for producing the zeolite membrane composite C according to this embodiment, the zeolite membrane M is formed by a gas deposition method (specifically, an aerosol deposition method). Therefore, by using a porous glass substrate K as a support, the zeolite membrane M can be formed on the surface Ka of the porous glass substrate K in a shorter time than by the hydrothermal synthesis method. In other words, according to the method for producing the zeolite membrane composite C according to this embodiment, the zeolite membrane composite C including the porous glass substrate K as a support can be produced in a shorter time than by the hydrothermal synthesis method.
[0054] In the method for producing the zeolite membrane composite C according to this embodiment, a porous glass substrate K is used as a support. Generally, porous glass has random pore shapes. Therefore, in the method for producing the zeolite membrane composite C according to this embodiment, even if the pore size of the porous glass support is large, a zeolite membrane can be formed by the gas deposition method, and a high-performance (high permeability) zeolite membrane composite C can be produced.
[0055] [Separation device] By configuring the zeolite membrane composite C as described above, the zeolite membrane composite C can be used as a separation device. That is, a separation device that separates gases can be realized by the zeolite membrane composite C, and any component can be separated and recovered from a mixed gas containing a plurality of components. The zeolite membrane composite C can be used, for example, to separate a mixed gas of carbon dioxide and methane or a mixed gas of carbon dioxide and nitrogen.
[0056] Fig. 3 is a diagram for explaining a procedure for separating a mixed gas when the zeolite membrane composite C is used as a separation device. As shown in Fig. 3, when the zeolite membrane composite C is used as a separation device, a mixed gas containing a separation target is supplied from the back surface Kb side of the porous glass substrate K. The supplied mixed gas is supplied to the zeolite membrane M through the pores of the porous glass substrate K, and when the mixed gas permeates the zeolite membrane M, the separation target is separated by the molecular sieving action of the zeolite.
[0057] [Examples and Comparative Examples] Examples 1 to 3 and Comparative Examples 1 to 4 are described below. In Examples 1 to 3, the conditions other than the average pore size of the porous glass substrate used and the skeletal structure of the aluminosilicate used were set to be the same, and the porous glass substrate was moved in the horizontal direction while spraying an aerosol onto the surface to perform a film formation process for a predetermined time, thereby producing a zeolite membrane composite using a so-called aerosol deposition method. The aerosol transport pipe used had a circular cross-sectional shape at the ejection end. Furthermore, the flow rate of the transport gas was 30 L / min, and the pressure in the processing chamber was 0.25 kPa. In each example, a zeolite membrane with a thickness of approximately 20 μm was formed.
[0058] A porous glass substrate having pores with a pore size of 50 to 100 nm was used in Example 1, and a porous glass substrate having pores with a pore size of 50 to 100 μm was used in Examples 2 and 3. Furthermore, as the raw material powder, LTA-type aluminosilicate particles with an average particle size of 1 μm were used in Examples 1 and 2, and CHA-type aluminosilicate particles with an average particle size of 1 μm were used in Example 3.
[0059] On the other hand, in Comparative Examples 1 to 3, a zeolite membrane composite was prepared by forming a zeolite membrane containing an LTA-type aluminosilicate on the surface of a porous alumina tube by hydrothermal synthesis, following the method reported in "Masahiro Seshimo, Bo Liu, Hey Ryeon Lee, Katsunori Yogo, Yuichiro Yamaguchi, Nobuyuki Shigaki, Yasuhiro Mogi, Hidetoshi Kita and Shin-ichi Nakao, Membrane Reactor for Methanol Synthesis Using Si-Rich LTA Zeolite Membrane, Membranes 2021, 11(7), 505".
[0060] Comparative Example 4 is a zeolite membrane composite reported in "N. Kosinov et al., Journal of Materials Chemistry A, 2 (2014) 13083" (hereinafter referred to as "References"), in which a membrane made of CHA-type zeolite is formed on the surface of a hollow fiber membrane made of α-alumina by hydrothermal synthesis.
[0061] The permeabilities of a plurality of single-component gases were measured using the zeolite membrane composites of Examples 1 to 3 and Comparative Examples 1 to 3, and the selectivity was calculated from the ratio of the permeabilities. As the permeabilities of single-component gases, the permeabilities of carbon dioxide, nitrogen, and carbon tetrafluoride were measured in Examples 1 and 2 and Comparative Examples 1 to 3, and the permeabilities of carbon dioxide and nitrogen were measured in Example 3.
[0062] Table 1 shows the zeolite types and selectivities (carbon dioxide / nitrogen selectivity, carbon dioxide / carbon tetrafluoride selectivity) of the examples and comparative examples. The selectivity of Comparative Example 4 in Table 1 is the value described in the reference literature.
[0063] [Table 1]
[0064] As shown in Table 1, the zeolite membrane composites of Examples 1 to 3 and Comparative Examples 1 to 4 differ in the type of zeolite, the type of support, and the method for forming the zeolite membrane, but all of them show a certain degree of selectivity and can selectively permeate carbon dioxide compared to nitrogen and carbon tetrafluoride.
[0065] Comparing Example 1 and Example 2, both show similar selectivity. From this, it is presumed that the function of the zeolite membrane is fully exhibited as long as the average pore size of the porous glass substrate is at least in the range of 50 nm to 100 μm.
[0066] In addition, when Examples 1 and 2 in which the zeolite membrane is composed of an LTA-type aluminosilicate are compared with Comparative Examples 1 to 3, the types of supports are different, but all of the zeolite membrane composites show the same level of selectivity. In addition, when Example 3 in which the zeolite membrane is composed of a CHA-type aluminosilicate is compared with Comparative Example 4, the types of supports are different, but all of the zeolite membrane composites show the same level of selectivity. From this, it is found that a porous glass substrate can be used as the support of the zeolite membrane composite, and that the zeolite membrane composite using the porous glass substrate as the support fully exhibits the function of the zeolite membrane.
[0067] Similarly, when Examples 1 and 2 are compared with Comparative Examples 1 to 3, and Example 3 with Comparative Example 4, the selectivity is equivalent if the framework structure of the aluminosilicate constituting the zeolite membrane is the same, although there is a difference in the method of forming the zeolite membrane. From this, it is presumed that the method of forming the zeolite membrane does not cause a large difference in selectivity. Therefore, a zeolite membrane composite in which the zeolite membrane is formed by a gas deposition method (aerosol deposition method) is advantageous in that it can be produced in a short time while having the same performance as a zeolite membrane formed by a hydrothermal synthesis method.
[0068] [Another embodiment] [1] In the above embodiment, the porous glass support is a plate-shaped porous glass substrate K. However, the present invention is not limited to this embodiment. For example, a porous glass support made of plate-shaped porous glass and having a box-like or cylindrical shape may be used, and a zeolite membrane may be formed on the outer surface of the porous glass support.
[0069] [2] In the above embodiment, the zeolite membrane M is formed by the aerosol deposition method, but the present invention is not limited to this. The zeolite membrane M may be formed by other gas deposition methods.
[0070] [3] In the above embodiment, the zeolite membrane composite C is used as a separation device, but the present invention is not limited to this embodiment. For example, the zeolite membrane composite C may be used as a dehydration device. In this case, water can be separated from a mixed fluid containing water, and therefore water and other components in the mixed fluid can be separated and recovered. The zeolite membrane composite C can be used in various applications in which the molecular sieve action of zeolite can be utilized.
[0071] [4] In the above embodiment, a cylindrical straight tube member is used as the aerosol transport tube 5, and the cross-sectional shape of the ejection end 5a is circular, but this is not limited to the above. The cross-sectional shape of the ejection end of the aerosol transport tube may be elliptical, or may be polygonal, such as triangular or rectangular (including slits).
[0072] [5] In the above embodiment, the holder 4 holds the porous glass substrate K so that the surface Ka faces downward, but the present invention is not limited to this. The positions of the holder and the ejection end of the aerosol transport pipe may be switched up and down, and the holder may hold the substrate so that the surface to be treated faces upward.
[0073] In addition, the configurations disclosed in the above embodiments (including other embodiments, the same applies below) can be applied in combination with configurations disclosed in other embodiments, provided no contradiction arises. Furthermore, the embodiments disclosed in this specification are illustrative, and the embodiments of the present invention are not limited thereto, and can be appropriately modified within the scope that does not deviate from the purpose of the present invention. [Explanation of symbols]
[0074] 1: Film deposition equipment 2: Processing room 3: Movement mechanism 5: Aerosol transport pipe 15: Aerosol generating section 16: Raw material powder supply mechanism 18: Carrier gas supply mechanism C: Zeolite membrane composite K: Porous glass substrate (porous glass support) Ka: Surface M: Zeolite membrane
Claims
1. A zeolite membrane composite comprising a porous glass support and a zeolite membrane formed on the surface of the porous glass support.
2. 2. The zeolite membrane composite according to claim 1, wherein the porous glass support has an average pore size of 50 nm or more and 100 μm or less.
3. 2. The zeolite membrane composite according to claim 1, wherein the zeolite membrane has a thickness of 0.1 μm or more and 100 μm or less.
4. A separation device comprising the zeolite membrane composite according to any one of claims 1 to 3, and performing gas separation by means of the zeolite membrane composite.
5. A dehydration device comprising the zeolite membrane composite according to any one of claims 1 to 3, and dehydrating a mixed fluid containing water by the zeolite membrane composite.
6. A method for producing a zeolite membrane composite having a porous glass support and a zeolite membrane formed on a surface of the porous glass support, comprising the steps of: A method for producing a zeolite composite membrane, comprising the step of forming a zeolite membrane on the surface of the porous glass support by a gas deposition method.
7. 7. The method for producing a zeolite membrane composite according to claim 6, wherein in the zeolite membrane formation step, an aerosol in which aluminosilicate particles are dispersed in a carrier gas is ejected toward a surface of the porous glass support to form a zeolite membrane on the surface.
Citation Information
Patent Citations
Zeolite, method of producing the same, and method of separating gases by utilizing the zeolite
JP2001146416A
Method for manufacturing zeolite membrane
JP2010142809A
Zeolite membrane composite body, method for producing zeolite membrane composite body, separation device, membrane reaction device, and separation method
WO2020255867A1