Zeolite membrane composite body, separation device, dehydration device, and method of manufacturing zeolite membrane composite body

The zeolite membrane composite with a metal support and through-holes addresses fluid permeability issues, enhancing separation and dehydration efficiency through a gas deposition method, ensuring high performance and durability.

JP2024143240APending Publication Date: 2024-10-11OSAKA GAS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023055809
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing zeolite membrane composites face challenges in adjusting fluid permeability and performance due to the influence of the metal support's porosity and pore shape, limiting their versatility and efficiency in separation and dehydration processes.

Method used

A zeolite membrane composite with a metal support featuring through-holes of 10 μm or less and a zeolite membrane with specific pore sizes is developed, allowing for adjustable fluid permeability and enhanced separation performance, using a gas deposition method to form the membrane without requiring acid treatment or high-temperature heat treatment.

Benefits of technology

The composite achieves high permeability and selectivity for various applications, enabling efficient separation and dehydration processes while maintaining the durability of the metal support, and can be produced in a shorter time compared to traditional hydrothermal synthesis methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143240000001_ABST
    Figure 2024143240000001_ABST
Patent Text Reader

Abstract

To provide a zeolite membrane composite body which has a metal support body in which a through hole is formed, and a zeolite membrane, and can be used in various applications.SOLUTION: A zeolite membrane composite body C has a metal support body K in which a through hole K1 having a hole diameter of 10 μm or less is formed, and a zeolite membrane M formed on a surface Ka of the metal support body K.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a zeolite membrane composite, a separation device, a dehydration device, and a method for producing a zeolite membrane composite. [Background technology]

[0002] In recent years, various research and development efforts have been conducted on zeolite membrane composites formed by forming a zeolite membrane on a porous body, for applications such as the separation of specific molecules by utilizing the molecular sieving action of zeolite.

[0003] As such a zeolite membrane composite, for example, one in which a zeolite membrane is formed on the surface of a metal support is known (Patent Documents 1 and 2). The use of a metal support has advantages such as easy airtightness when modularized and high breakage resistance of the support.

[0004] Patent Document 1 discloses a composite in which the surface of a porous metal oxide support is coated with metal oxide particles or metal nitride particles, and a zeolite membrane is formed on the coated surface.

[0005] Patent Document 2 discloses a composite obtained by treating a tubular porous metal support with a base or acid, and then forming a zeolite membrane on the treated portion. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2001-146416 A [Patent Document 2] JP 2010-142809 A Summary of the Invention [Problem to be solved by the invention]

[0007] When the molecular sieving action of zeolite is utilized in a zeolite membrane composite, the performance of the zeolite membrane composite (type of fluid that can be treated and permeation rate) is also affected by the fluid permeability of the metal support. Therefore, in order to realize the performance required of the zeolite membrane composite depending on the application, it is advantageous if the metal support used as the support has a fluid permeability that can be easily adjusted. The fluid permeability of the metal support is affected by the porosity, pore shape, etc. of the metal support.

[0008] Here, if the metal support has through holes that penetrate from the front to the back by hole processing, the fluid permeability can be easily adjusted by adjusting the number and diameter of the through holes. Therefore, if a metal support having through holes is used as a support, the performance such as the type of fluid that can be separated and the permeation speed can be easily changed, and it is considered that it will be easy to use it for various purposes.

[0009] The above Patent Documents 1 and 2 present knowledge about a method for forming a zeolite membrane on the surface of a porous metal support by using a porous metal support as a support for a zeolite membrane composite. However, in order to broaden the range of applications of zeolite membrane composites, it is desirable to accumulate knowledge about zeolite membrane composites using a metal support as a support.

[0010] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a zeolite membrane composite which has a metal support having through holes formed therein and a zeolite membrane and can be easily used for various applications, a method for producing the zeolite membrane composite, and a separation device and a dehydration device which use the zeolite membrane composite. [Means for solving the problem]

[0011] The zeolite membrane composite according to the present invention for achieving the above object has the following characteristic configuration: The device has a metal support having through-holes with a pore size of 10 μm or less, and a zeolite membrane formed on the surface of the metal support.

[0012] According to the above-mentioned characteristic configuration, by having a metal support having through-holes and a zeolite membrane, the fluid permeability of the metal support can be easily adjusted, and the performance such as the type of fluid that can be separated and the permeation rate can be easily changed. Therefore, the zeolite membrane composite having the above-mentioned characteristic configuration can be easily used for various applications.

[0013] Further characteristic features of the zeolite membrane composite according to the present invention are as follows: A portion of the zeolite membrane that overlaps with the through-hole when viewed in at least a direction perpendicular to the surface of the metal support is: The maximum pore size is greater than the pore size of the aluminosilicate constituting the zeolite membrane and is 6 nm or less; The average pore size is 4.5 nm or less.

[0014] If the zeolite membrane has defects that are extremely larger than the pore size of the aluminosilicate, or if the zeolite membrane has many defects larger than the pore size of the aluminosilicate, the selectivity for the separation target decreases, and the functions of the zeolite membrane, such as separation of the separation target from the fluid and removal of water, decrease. According to the above characteristic configuration, the zeolite membrane does not have any large defects in the portions overlapping with the through-holes, i.e., the portions to which the fluid is supplied through the through-holes. As a result, the zeolite membrane composite can fully exhibit the functions of the zeolite membrane.

[0015] Further characteristic features of the zeolite membrane composite according to the present invention are as follows: The maximum height (Sz) of the surface of the metal support is 1.5 μm or less.

[0016] If the maximum height (Sz) of the surface of the metal support is low, the formation of a zeolite membrane on the surface of the metal support by a gas deposition method or the like is favorable. Therefore, according to the above-mentioned characteristic configuration, for example, when the zeolite membrane is formed by a gas deposition method, the adhesion between the metal support and the zeolite membrane can be increased.

[0017] Further characteristic features of the zeolite membrane composite according to the present invention are as follows: The zeolite membrane has a thickness of 0.1 μm or more and 100 μm or less at a portion overlapping with the through-hole when viewed in a direction perpendicular to the surface of the metal support.

[0018] If the permeability of a zeolite membrane is low, it becomes difficult for a fluid to pass through the zeolite membrane, and the efficiency of separating the target to be separated from the fluid, removing water, etc. decreases. According to the above-mentioned characteristic configuration, the portion of the zeolite membrane to which the fluid is supplied through the through-holes has appropriate permeability, so that the function of the zeolite membrane is fully exerted.

[0019] The characteristic configuration of the separation device according to the present invention for achieving the above object is as follows: The present invention is characterized in that the above-mentioned zeolite membrane composite is included, and gas separation is performed by the zeolite membrane composite.

[0020] According to the above characteristic configuration, it is possible to separate and recover an arbitrary component from a mixed gas containing a plurality of components.

[0021] The characteristic configuration of the dehydrator according to the present invention for achieving the above object is as follows: The present invention has the above-mentioned zeolite membrane composite, and dehydrates a mixed fluid containing water by using the zeolite membrane composite.

[0022] According to the above characteristic configuration, water can be separated from a mixed fluid containing water, and therefore water and other components in the mixed fluid can be separated and recovered.

[0023] The method for producing a zeolite membrane composite according to the present invention for achieving the above object is characterized by the following features: A method for producing a zeolite membrane composite having a metal support having through holes with a pore size of 10 μm or less formed therein and a zeolite membrane formed on a surface of the metal support, comprising the steps of: The method includes a zeolite membrane formation step of forming a zeolite membrane on the surface of the metal support by a gas deposition method.

[0024] Generally, zeolite membranes are formed on a porous support by a liquid-phase synthesis method called hydrothermal synthesis. A raw material solution containing aluminum and silicon, which are the main raw materials of the zeolite membrane, is mixed with a solution containing various cationic species, and a hydrothermal synthesis method is performed under high-temperature and high-pressure hydrothermal conditions to form seed crystals. A porous body is then immersed in the dispersion in which the seed crystals are dispersed, and the seed crystals are attached to the porous body. This process is repeated several times. In addition, when forming a zeolite membrane by hydrothermal synthesis, a structure-directing agent is required to determine the size of the pores that can separate the target molecules by molecular sieving, and a heat treatment step is usually performed to remove the structure-directing agent after the formation of the zeolite membrane. This heat treatment step requires heating at 400 to 1000°C for 10 to 200 hours depending on the type of structure-directing agent. Thus, when forming a zeolite membrane by hydrothermal synthesis, multiple steps are required to obtain a desired zeolite membrane, and it takes a considerable amount of time to form the membrane. In addition, there are problems such as the durability of the metal support being reduced by exposure to acids or bases during hydrothermal synthesis, or the metal support being deteriorated by the need for heat treatment to remove the structure-directing agent. However, according to the above-mentioned characteristic configuration, the zeolite membrane can be formed by using the gas deposition method, which can perform the membrane formation process in a shorter time than the hydrothermal synthesis method and does not require treatment with an acid or base or heat treatment at high temperature. Therefore, the above-mentioned method for producing a zeolite membrane composite can suitably produce a zeolite membrane composite that can be easily used for various applications in a shorter time and with less deterioration or decrease in the durability of the metal support, compared to the case where the hydrothermal synthesis method is used. In addition, the separation performance of the zeolite membrane composite includes permeability and selectivity, and the permeability depends on the pore size of the support as well as the properties of the zeolite membrane. The larger the pore size of the support, the higher the permeability. However, if the pore size of the support is large, the dispersion liquid leaks out of the pores during seed crystal formation when the zeolite membrane is formed by hydrothermal synthesis. Therefore, when the zeolite membrane is formed by hydrothermal synthesis, the pore size of the support cannot be made large. However, the above-mentioned method for producing a zeolite membrane composite does not require complicated steps, and it is possible to form a zeolite membrane on a metal support having through-holes with a relatively large pore size by a gas deposition method that does not require an acid treatment, etc. Therefore, the above-mentioned method for producing a zeolite membrane composite can easily produce a high-performance (high permeability) zeolite membrane composite.

[0025] The method for producing a zeolite membrane composite according to the present invention further comprises the steps of: In the zeolite membrane forming step, an aerosol in which aluminosilicate particles are dispersed in a carrier gas is sprayed toward a surface of the metal support to form the zeolite membrane on the surface; The particles have an average particle size smaller than the pore size of the through-holes.

[0026] According to the above-mentioned characteristic configuration, a zeolite membrane can be formed by the so-called aerosol deposition method using particles having a particle diameter smaller than the pore diameter of the through-holes. The aerosol deposition method enables the membrane formation process in a shorter time than the hydrothermal synthesis method, and does not require treatment with an acid or base or heat treatment at high temperature. Therefore, according to the above-mentioned method for producing a zeolite membrane composite, a zeolite membrane composite can be suitably produced in a shorter time and while suppressing deterioration or degradation of the durability of the metal support, as compared with the case of using the hydrothermal synthesis method. Effect of the Invention

[0027] As described above, the zeolite membrane composite, the method for producing the zeolite membrane composite, and the separation device and dehydration device using the zeolite membrane composite according to the present invention have a metal support having through holes and a zeolite membrane, and can be easily used for various applications. [Brief description of the drawings]

[0028] [Figure 1] FIG. 1 is a diagram showing a schematic configuration of a zeolite membrane composite according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing a schematic configuration of a membrane forming apparatus used in a method for producing a zeolite membrane composite according to an embodiment of the present invention. [Diagram 3] 4A to 4C are diagrams for explaining a procedure for separating a mixed gas using the separation device according to the present embodiment. [Figure 4] 1 is a graph showing the measurement results by the nanoperm porometry method in Example 1. [Diagram 5] 1 is a graph showing the measurement results by the nanoperm porometry method in Example 2. [Figure 6] 1 is a graph showing the measurement results by nanoperm porometry in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] Hereinafter, a zeolite membrane composite according to an embodiment, a method for producing the zeolite membrane composite, and a separation device using the zeolite membrane composite will be described with reference to the drawings. In the following description, the terms "upper" and "lower" refer to the upper and lower sides in the drawings.

[0030] [Zeolite membrane composite C] First, the zeolite membrane composite C of this embodiment will be described.

[0031] Fig. 1 is a schematic diagram showing a zeolite membrane composite C according to this embodiment. As shown in Fig. 1, the zeolite membrane composite C has a metal support K having through holes K1 with a pore size of 10 µm or less formed therein, and a zeolite membrane M formed on a surface Ka of the metal support K.

[0032] [Metal support K] The metal support K plays a role of supporting the zeolite membrane M and maintains the strength of the zeolite membrane composite C, and is generally plate-shaped in this embodiment. The material of the metal support K is not particularly limited, and may be appropriately selected from, for example, ferritic stainless steel, austenitic stainless steel, nickel-based alloy, etc., taking into consideration the strength of the zeolite membrane composite C and the cost. The metal support K in this embodiment is made of ferritic stainless steel.

[0033] The metal support K has a plurality of through holes K1 with a diameter of 10 μm or less, penetrating from the surface (front surface) on which the zeolite membrane M is formed to the back surface. Specifically, in this embodiment, the metal support K is a metal plate in which a plurality of through holes K1 with approximately circular opening edges are formed by mechanical, chemical, or optical perforation (hole processing) such as punching, etching, or laser processing so as to linearly penetrate from the front surface to the back surface of the metal plate.

[0034] The fluid permeability of the metal support K can be adjusted by changing the number and pore size of the through holes K1. Therefore, the zeolite membrane composite C of this embodiment can change the type of fluid that can be separated and the permeation rate simply by changing the number and pore size of the through holes K1 of the metal support K, and can be easily used for various applications.

[0035] If the diameter of the through hole K1 is too small, the fluid does not easily flow through the through hole K1, the amount of fluid supplied to the zeolite membrane M decreases, and as a result, separation and dehydration of the fluid may become impossible. Therefore, the diameter of the through hole K1 is preferably 0.1 μm or more. On the other hand, the diameter of the through hole K1 affects the membrane formability when the zeolite membrane M is formed on the surface Ka of the metal support K by the gas deposition method. Specifically, the smaller the diameter of the through hole K1, the better the membrane formability, and the fewer the number of defects in the zeolite membrane M and the smaller the size of the defects tend to be. Therefore, the diameter of the through hole K1 is preferably 7.5 μm or less, and more preferably 5.0 μm or less. The shape of the opening edge of the through hole K1 is not limited to a circle, and may be an ellipse or a rectangle. In this case, the hole diameter refers to the diameter of a circle circumscribing the opening edge.

[0036] The thickness H1 of the metal support K may be appropriately set based on the fluid permeability and the strength required for the zeolite membrane composite C. Specifically, if the thickness H1 of the metal support K is too thick, the permeability decreases and too little fluid flows through the zeolite membrane M, whereas if the thickness H1 is too thin, sufficient strength of the zeolite membrane composite C cannot be ensured. Therefore, the thickness H1 of the metal support K is preferably 0.1 mm or more and 2 mm or less, more preferably 0.15 mm or more and 1.5 mm or less, and even more preferably 0.2 mm or more and 1 mm or less.

[0037] From the viewpoint of the formability of the zeolite membrane M on the surface Ka of the metal support K by a gas deposition method (specifically, an aerosol deposition method), the maximum height (Sz) is preferably 1.5 μm or less, and more preferably 1.4 μm or less.

[0038] [Zeolite Membrane M] The zeolite membrane M plays a role in separating specific molecules by utilizing the molecular sieve action of zeolite (aluminosilicate). The zeolite constituting the zeolite membrane M can be appropriately selected from known zeolite species having various skeletal structures according to the molecular size of the object to be separated. For example, faujasite (FAU) with a crystal pore diameter of 0.74 nm, or A-type zeolite (LTA) with a pore diameter of 0.41 nm can be used.

[0039] In this embodiment, the zeolite membrane M has an overlapping portion M1 that overlaps with the through-hole K1 and a non-overlapping portion M2 that does not overlap with the through-hole K1 when viewed in a direction perpendicular to the surface Ka of the metal support K. In this embodiment, the overlapping portion M1 and the non-overlapping portion M2 of the zeolite membrane M (i.e., the entire zeolite membrane M) have a maximum pore size that exceeds the pore size of the aluminosilicate constituting the zeolite membrane M and is 6 nm or less, and an average pore size that is 4.5 nm or less. For example, when the zeolite membrane M is made of FAU-type zeolite (aluminosilicate), the overlapping portion M1 and the non-overlapping portion M2 of the zeolite membrane M have a maximum pore size that exceeds 0.41 nm and is 6 nm or less, and an average pore size that is 4.5 nm or less.

[0040] In a defect-free zeolite membrane M, there are no voids larger than the pore size of the aluminosilicate that constitutes the zeolite membrane M. Therefore, when voids larger than the pore size of the aluminosilicate are present in the zeolite membrane M, the voids are considered to be defects. When defects are present in the zeolite membrane M, the fluid supplied to the zeolite membrane M flows preferentially through the defective parts rather than through the original pores of the zeolite, thereby reducing the selectivity for the separation target.

[0041] Here, when the overlapping portion M1 of the zeolite membrane M satisfies the above conditions for the maximum pore size and the average pore size, the overlapping portion M1 does not have any defects extremely larger than the pore size of the aluminosilicate, and the number of defects larger than the pore size of the aluminosilicate is small. In this case, although the overlapping portion M1 has defects larger than the pore size of the aluminosilicate, when a fluid is supplied to the overlapping portion M1, a decrease in selectivity for the separation target is suppressed. Therefore, according to the zeolite membrane composite C of this embodiment, separation of the separation target from the mixed fluid and removal of water (dehydration) can be efficiently performed.

[0042] Here, the maximum pore size and average pore diameter of the zeolite membrane M can be measured by a nanoperm porometry method.

[0043] Nanoperm porometry is a method for measuring pore size distribution using the capillary condensation phenomenon, and its principle is that water, a condensable component, undergoes capillary condensation within the pores in the membrane, filling the pores and inhibiting the permeation of nitrogen, a non-condensable component. The relationship between the vapor pressure of the condensed water component in the pores and the size of the pores filled by condensation is expressed by the following formula 1. In formula 1, d is the Kelvin diameter [m], ν is the molar volume [m 3 / mol], R is the gas constant [J / mol / K], T is the temperature [K], σ is the surface tension [N / m], θ is the contact angle [deg], P is the vapor pressure [Pa], and Ps is the saturated vapor pressure at the measurement temperature [Pa]. By changing the concentration of nitrogen and water vapor, the vapor pressure of the mixed gas changes, and the pore size (Kelvin diameter) at which water condenses changes accordingly. If the permeability of dry nitrogen that does not contain water vapor is measured, and then water vapor is added and the permeability is measured again, all pores smaller than the pore size at which condensation occurs are blocked, preventing nitrogen permeation and reducing the nitrogen permeability. In the nanoperm porometry method, mixed gases of nitrogen and water vapor at various concentrations are supplied to the membrane, and the pore size distribution is estimated from the rate of decrease in nitrogen permeability (Tsuru Minoru, FY2006 Grant Research Report I (issued March 2008)).

[0044]

number

[0045] In the measurement by the nanoperm porometry method of the present application, the nitrogen permeability was measured by changing the water vapor concentration in the range of 1 to 50 nm in pore size where condensation occurs, and the water vapor concentration at which the nitrogen permeability is about 50% of the permeability of dry nitrogen was obtained, and the value obtained by converting the water vapor concentration into the pore size was defined as the average pore size of the membrane, and the point at which the permeability reached about 0% (lower limit of detection) was defined as the maximum pore size of the membrane. The permeability was measured by measuring the flow rate of nitrogen permeating the membrane using a high-precision membrane flowmeter (HORIBA, SF-1U, volumetric tube unit VP-1U used), measuring the transmembrane pressure difference using a pressure gauge (Krone, KDM30), and dividing the permeated nitrogen flow rate by the transmembrane pressure difference and membrane area to calculate the nitrogen permeability per unit membrane area and pressure difference. In addition, the permeability of dry nitrogen was set to 1, and the nitrogen permeability when a nitrogen-water vapor mixed gas was supplied was normalized.

[0046] The thickness H2 of the zeolite membrane M may be appropriately set in consideration of the permeability of the fluid. Specifically, if the thickness H2 of the zeolite membrane M is too thick, the permeability is reduced, making it difficult for the fluid to pass through the zeolite membrane M, and the efficiency of separation of the separation target from the mixed fluid and removal of water (dehydration) is reduced. Conversely, if the thickness H2 is too thin, the permeability is too high, and the efficiency of separation of the separation target from the mixed fluid and removal of water (dehydration) is reduced. Therefore, the thickness H2 of the zeolite membrane M, more specifically, the thickness H2 of the overlapping portion M1 of the zeolite membrane M is preferably 0.1 μm or more and 100 μm or less, more preferably 0.2 μm or more and 80 μm or less, and even more preferably 0.5 μm or more and 50 μm or less.

[0047] Next, a method for producing the zeolite membrane composite C according to this embodiment will be described. First, a membrane forming apparatus 1 used in this production method will be described.

[0048] [Film deposition equipment 1] Fig. 2 is a diagram showing a schematic configuration of the film forming apparatus 1. As shown in Fig. 2, the film forming apparatus 1 is an apparatus that ejects an aerosol, in which raw material powder made of aluminosilicate particles is dispersed in a carrier gas, toward a surface Ka of a metal support K to form a zeolite film M on the surface Ka of the metal support K. In other words, the film forming apparatus 1 is an apparatus that forms a zeolite film M on the surface Ka of the metal support K by an aerosol deposition method.

[0049] In this embodiment, the film forming apparatus 1 includes a processing chamber 2 in which a metal support K is arranged, a holding section 4 which holds the metal support K which is the target of the film forming processing, a moving mechanism 3 configured to move the holding section 4, an aerosol transport pipe 5 which ejects an aerosol from an ejection tip 5a, an aerosol generating section 15 which generates an aerosol in which raw material powder is dispersed in a gas, a raw material powder supply mechanism 16 which delivers the raw material powder to the aerosol generating section 15, and a carrier gas delivery mechanism 18 which delivers a carrier gas to the aerosol generating section 15.

[0050] The processing chamber 2 is made of an airtight casing, and has an opening 2a formed on the upper end surface. A holder 4 and an aerosol transport pipe 5 are disposed inside the processing chamber 2. A mechanical booster pump P1 and a vacuum pump P2 serving as exhaust equipment are connected to the opening 2a of the processing chamber 2 via an exhaust pipe S1. The pressure inside the processing chamber 2 is reduced to a predetermined pressure (for example, about 0.25 kPa) or less by exhausting gas by the mechanical booster pump P1 and the vacuum pump P2.

[0051] The holding unit 4 is configured to be able to hold the metal support K with the surface Ka facing downward so that the surface Ka is parallel to a horizontal plane. Known methods such as a method using vacuum suction or a method using Coulomb force can be used to hold the metal support K.

[0052] The moving mechanism 3 is composed of a horizontal drive mechanism (not shown) that moves the holder 4 in the horizontal direction, an elevation drive mechanism (not shown) that moves the holder 4 in the vertical direction, etc. Although the moving mechanism 3 is shown to be disposed outside the processing chamber 2 in FIG. 2, the moving mechanism 3 may be disposed inside the processing chamber 2.

[0053] The aerosol transport pipe 5 is a cylindrical straight pipe member, and the cross-sectional shape of the ejection end 5a is slit-shaped. The aerosol transport pipe 5 is disposed in the processing chamber 2 so that the ejection end 5a faces the holding part 4. The end of the aerosol transport pipe 5 opposite the ejection end 5a is connected to the aerosol generating part 15. With this aerosol transport pipe 5, the aerosol is ejected from the ejection end 5a toward the surface Ka of the metal support K.

[0054] As described above, the aerosol generating unit 15 is configured to generate an aerosol in which raw material powder is dispersed in a gas. The aerosol generating unit 15 is connected to the aerosol transport pipe 5, as well as the raw material supply pipe S2 and the carrier gas delivery pipe S3 described below. The aerosol generating unit 15 generates an aerosol in which raw material powder supplied at a constant speed by the raw material powder supply mechanism 16 and a carrier gas delivered by the carrier gas delivery mechanism 18 are mixed. The generated aerosol is delivered to the aerosol transport pipe 5.

[0055] The raw material powder supply mechanism 16 is composed of a raw material powder supply unit 17, a raw material supply pipe S2, etc. Raw material powder is stored in the raw material powder supply unit 17. The raw material powder is supplied to the aerosol generating unit 15 through the raw material supply pipe S2. The raw material powder will be described in detail later.

[0056] The carrier gas delivery mechanism 18 is composed of a gas supply unit 19, a carrier gas pressure control unit 20, a carrier gas flow rate control unit 21, a carrier gas delivery pipe S3, and the like.

[0057] A carrier gas supply pipe S3 is connected to the gas supply unit 19. The gas supply unit 19 is configured to supply a carrier gas such as air, N2, He, or Ar to the carrier gas supply pipe S3 by a compressor or a gas cylinder.

[0058] The carrier gas delivery pipe S3 is for delivering the carrier gas supplied from the gas supply unit 19 to the aerosol generation unit 15. In this embodiment, the carrier gas delivered from the gas supply unit 19 is delivered to the aerosol generation unit 15 via the carrier gas pressure control unit 20 and the carrier gas flow rate control unit 21 in this order. That is, the carrier gas delivery pipe S3 is composed of a plurality of pipes connecting the gas supply unit 19, the carrier gas pressure control unit 20, the carrier gas flow rate control unit 21, and the aerosol generation unit 15. A pressure sensor Q for detecting the pressure in the carrier gas delivery pipe S3 is provided between the carrier gas flow rate control unit 21 and the aerosol generation unit 15 in the carrier gas delivery pipe S3.

[0059] The carrier gas pressure control unit 20 stabilizes the carrier gas flowing through the carrier gas delivery pipe S3 at an appropriate pressure. The carrier gas flow rate control unit 21 controls the flow rate of the carrier gas flowing through the carrier gas delivery pipe S3. The operations of the carrier gas pressure control unit 20 and the carrier gas flow rate control unit 21 are appropriately controlled by a control device based on the pressure detected by the pressure sensor Q.

[0060] [Raw material powder] The raw material powder is composed of aluminosilicate particles, and in this embodiment, the aluminosilicate particles have an average particle size smaller than the hole size of the through holes K1 of the metal support K. Specifically, in this embodiment, the aluminosilicate particles have an average particle size of 0.5 μm or more and 10 μm or less. As the aluminosilicate constituting the raw material powder, those having various skeletal structures such as FAU and LTA can be used.

[0061] [Method for producing zeolite membrane composite C] Next, a method for producing the zeolite membrane composite C according to this embodiment will be described. This production method includes a zeolite membrane formation step of forming a zeolite membrane M by a gas deposition method on a surface Ka of a metal support K in which through-holes K1 with a pore size of 10 μm or less are formed. In this embodiment, in the zeolite membrane formation step, an aerosol in which aluminosilicate particles are dispersed in a carrier gas is sprayed toward the surface Ka of the metal support K to form the zeolite membrane M on the surface Ka. The aluminosilicate particles used have an average particle size smaller than the pore size of the through-holes K1.

[0062] Specifically, in this embodiment, first, the carrier gas is fed from the gas supply unit 19 to the aerosol generation unit 15 while adjusting the flow rate and pressure of the carrier gas flowing through the carrier gas feed pipe S3 by the carrier gas pressure control unit 20 and the carrier gas flow rate control unit 21. In the aerosol generation unit 15, an aerosol is generated in which the fed carrier gas and the raw material powder fed from the raw material powder supply unit 17 are mixed. The generated aerosol is fed to the aerosol transport pipe 5.

[0063] The aerosol fed to the aerosol transport pipe 5 is ejected from the ejection end 5a toward the surface Ka of the metal support K, and the ejected aerosol collides with the surface Ka of the metal support K, forming a zeolite membrane M on the surface Ka (zeolite membrane formation process).

[0064] As described above, in the method for producing the zeolite membrane composite C according to this embodiment, the zeolite membrane M is formed by a gas deposition method (specifically, an aerosol deposition method). Therefore, compared with the case where the zeolite membrane M is formed by a hydrothermal synthesis method, the zeolite membrane composite C can be produced in a short time while suppressing a decrease in durability or deterioration of the metal support K. Moreover, the method for producing the zeolite membrane composite C according to this embodiment does not require complicated steps, and it is possible to form a zeolite membrane on a metal support having through-holes with a relatively large pore size by a gas deposition method that does not require an acid treatment, etc. Therefore, the method for producing the zeolite membrane composite C makes it possible to easily produce a zeolite membrane composite C with high performance (high permeability).

[0065] [Separation device] By configuring the zeolite membrane composite C as described above, the zeolite membrane composite C can be used as a separation device. That is, a separation device that separates gases can be realized by the zeolite membrane composite C, and any component can be separated and recovered from a mixed gas containing a plurality of components. The zeolite membrane composite C can be used, for example, to separate a mixed gas of carbon dioxide and methane or a mixed gas of carbon dioxide and nitrogen.

[0066] Fig. 3 is a diagram for explaining a procedure for separating a mixed gas when the zeolite membrane composite C is used as a separation device. As shown in Fig. 3, when the zeolite membrane composite C is used as a separation device, a mixed gas containing a separation target is supplied from the back surface Kb side of the metal support K. The supplied mixed gas is supplied to the overlapping portion M1 of the zeolite membrane M through the through-hole K1, and when the mixed gas permeates the overlapping portion M1, the separation target is separated by the molecular sieving action of the zeolite.

[0067] [Examples and Comparative Examples] Hereinafter, Examples 1 and 2 and Comparative Examples 1 and 2 will be described. In Examples 1 and 2 and Comparative Example 1, the conditions other than the diameter of the through holes were set to the same, and the metal support was moved back and forth along the horizontal direction while spraying the aerosol onto the surface to perform a membrane forming process for a predetermined time to prepare a zeolite membrane composite. The aerosol transport tube used had a slit-shaped flow path cross section at the ejection end and a flow path cross-sectional area of ​​20 mm x 0.5 mm. The distance between the ejection end and the surface of the metal support was set to 50 mm. Furthermore, as the raw material powder, particles of FAU-type aluminosilicate with an average particle size of 1.6 μm were used. The flow rate of the transport gas was set to 30 L / min, and the pressure in the processing chamber was set to 0.25 kPa. In each example, a zeolite membrane with a thickness of approximately 10 to 50 μm was formed.

[0068] The diameter of the through holes in the metal support used was about 5 μm in Example 1, about 7.5 μm in Example 2, and about 15 μm in Comparative Example 1. The surface height (Sz) of the metal support used was 1.5 μm or less.

[0069] On the other hand, Comparative Example 2 is a zeolite membrane composite reported in "Hasegawa Y, Tanaka T, Watanabe K, et al., Korean J. Chem. Eng. 2002;19(2):309-313" (hereinafter referred to as "References"), in which an FAU-type zeolite membrane is formed on the surface of a cylindrical alumina by hydrothermal synthesis.

[0070] The zeolite membrane composites of Examples 1 and 2 and Comparative Example 1 were measured by the nanoperm porometry method described above, and these zeolite membrane composites were used to separate a mixed gas with a carbon dioxide molar fraction of 0.2 and a nitrogen molar fraction of 0.8.

[0071] Figures 4 to 6 are graphs showing the results of measuring the zeolite membrane composites of Examples 1 and 2 and Comparative Example 1 by the above-mentioned nanoperm porometry method, with Figure 4 being the graph for Example 1, Figure 5 being the graph for Example 2, and Figure 6 being the graph for Comparative Example 1. Table 1 is a table summarizing the maximum pore size and average pore diameter obtained by the measurement by the nanoperm porometry method. Table 2 is a table summarizing the selectivity (carbon dioxide / nitrogen selectivity) of each Example and each Comparative Example. The selectivity of Comparative Example 2 in Table 2 is a value described in a reference document.

[0072] [Table 1]

[0073] [Table 2]

[0074] As shown in Figs. 4 to 6 and Table 1, the maximum pore size of the zeolite membrane composite is 1.5 nm in Example 1, 6 nm in Example 2, and 50 nm in Comparative Example 1, and all of the zeolite membrane composites have pores that exceed the pore size (0.74 nm) of FAU-type aluminosilicate. However, in Examples 1 and 2, the maximum pore size is 6 µm or less, and the average pore size is 4.5 µm or less, so that a certain level of selectivity is shown as shown in Table 2, and it is found that carbon dioxide can be selectively permeated compared to nitrogen. In contrast, in Comparative Example 1, the maximum pore size is far larger than the pore size of FAU-type aluminosilicate, and the average pore size is also 25 nm, so that no selectivity is shown as shown in Table 2.

[0075] From the above, it is found that by setting the pore size of the through-holes formed in the metal support to 10 μm or less, a zeolite membrane having a maximum pore size of more than 0.74 nm and not more than 6 nm and an average pore size of not more than 4.5 nm can be formed on the surface of the metal support. In addition, even if the maximum pore size of the zeolite membrane exceeds the pore size of the aluminosilicate constituting the zeolite membrane, the decrease in selectivity can be suppressed depending on the maximum pore size and the average pore size. In particular, if the maximum pore size is not more than 6 nm and the average pore size is not more than 4.5 nm, a certain level of selectivity is shown, and if the maximum pore size and the average pore size are smaller, high selectivity is shown.

[0076] Moreover, when Examples 1 and 2 in which the zeolite membrane was formed by the aerosol deposition method were compared with Comparative Example 2 in which the zeolite membrane was formed by the hydrothermal synthesis method, both showed high selectivity. This shows that there is no significant difference in selectivity depending on the method of forming the zeolite membrane. Therefore, the zeolite membrane composite in which the zeolite membrane is formed by the gas deposition method (aerosol deposition method) has an advantage over the zeolite membrane formed by the hydrothermal synthesis method in that it can be manufactured in a short time and with reduced deterioration and degradation of the durability of the metal support while providing equivalent performance compared to the zeolite membrane formed by the hydrothermal synthesis method.

[0077] [Another embodiment] [1] In the above embodiment, the metal support K is generally plate-shaped, but the present invention is not limited to this. For example, the metal support K may be bent or otherwise processed into a box-like or cylindrical shape, and the zeolite membrane may be formed on the outer surface of the plate-shaped metal support K.

[0078] [2] In the above embodiment, the overlapping portion M1 and the non-overlapping portion M2 of the zeolite membrane M are both described as having a maximum pore size that exceeds the pore size of the aluminosilicate constituting the zeolite membrane M and is 6 nm or less, and an average pore size that is 4.5 nm or less. However, the present invention is not limited to such an embodiment. Only one of the overlapping portion M1 and the non-overlapping portion M2 may satisfy the above conditions for the maximum pore size and the average pore size, or neither of the overlapping portion M1 and the non-overlapping portion M2 may satisfy the above conditions for the maximum pore size and the average pore size. From the viewpoint of fully exerting the function of the zeolite membrane M, it is preferable that the overlapping portion M1 to which the fluid is supplied through the through-hole K1 of the metal support K satisfies the above conditions for the maximum pore size and the average pore size.

[0079] [3] In the above embodiment, the zeolite membrane M is formed by the aerosol deposition method, but the present invention is not limited to this. The zeolite membrane M may be formed by other gas deposition methods.

[0080] [4] In the above embodiment, the zeolite membrane composite C is used as a separation device, but the present invention is not limited to this embodiment. For example, the zeolite membrane composite C may be used as a dehydration device. In this case, water can be separated from a mixed fluid containing water, and therefore water and other components in the mixed fluid can be separated and recovered. The zeolite membrane composite C can be used in various applications in which the molecular sieve action of zeolite can be utilized.

[0081] [5] In the above embodiment, a cylindrical straight tube member is used as the aerosol transport tube 5, and the cross-sectional shape of the ejection end 5a is slit-shaped, but the present invention is not limited to this. The cross-sectional shape of the ejection end of the aerosol transport tube is not limited to a rectangular shape such as a slit, but may be a circle, an ellipse, or a polygon such as a triangle.

[0082] [6] In the above embodiment, the holder 4 holds the metal support K so that the surface Ka faces downward, but the present invention is not limited to this. The positions of the holder and the ejection end of the aerosol transport pipe may be switched up and down, and the holder may hold the substrate so that the surface to be treated faces upward.

[0083] In addition, the configurations disclosed in the above embodiments (including other embodiments, the same applies below) can be applied in combination with configurations disclosed in other embodiments, provided no contradiction arises. Furthermore, the embodiments disclosed in this specification are illustrative, and the embodiments of the present invention are not limited thereto, and can be appropriately modified within the scope that does not deviate from the purpose of the present invention. [Explanation of symbols]

[0084] 1: Film deposition equipment 2: Processing room 3: Movement mechanism 5: Aerosol transport pipe 15: Aerosol generating section 16: Raw material powder supply mechanism 18: Carrier gas supply mechanism C: Zeolite membrane composite K: Metal support Ka: Surface K1: Through hole M: Zeolite membrane M1: Overlapped part (part that overlaps with the through hole)

Claims

1. A zeolite membrane composite comprising: a metal support having through-holes with a pore size of 10 μm or less formed therein; and a zeolite membrane formed on the surface of the metal support.

2. A portion of the zeolite membrane that overlaps with the through-hole when viewed in at least a direction perpendicular to the surface of the metal support is: The maximum pore size is greater than the pore size of the aluminosilicate constituting the zeolite membrane and is 6 nm or less; 2. The zeolite composite membrane according to claim 1, having an average pore size of 4.5 nm or less.

3. 2. The zeolite membrane composite according to claim 1, wherein the maximum height (Sz) of the surface of the metal support is 1.5 μm or less.

4. 2. The zeolite membrane composite according to claim 1, wherein the thickness of the zeolite membrane at a portion overlapping with the through-hole when viewed in a direction perpendicular to the surface of the metal support is 0.1 μm or more and 100 μm or less.

5. A separation device comprising the zeolite membrane composite according to any one of claims 1 to 4, which separates a gas by means of the zeolite membrane composite.

6. A dehydration apparatus comprising the zeolite membrane composite according to any one of claims 1 to 4, which dehydrates a mixed fluid containing water by using the zeolite membrane composite.

7. A method for producing a zeolite membrane composite having a metal support having through holes with a pore size of 10 μm or less formed therein and a zeolite membrane formed on a surface of the metal support, comprising the steps of: A method for producing a zeolite membrane composite, comprising the step of forming a zeolite membrane on the surface of the metal support by a gas deposition method.

8. In the zeolite membrane forming step, an aerosol in which aluminosilicate particles are dispersed in a carrier gas is sprayed toward a surface of the metal support to form the zeolite membrane on the surface; The method for producing a zeolite membrane composite according to claim 7 , wherein the particles have an average particle size smaller than the pore size of the through-holes.

Citation Information

Patent Citations

  • Zeolite, method of producing the same, and method of separating gases by utilizing the zeolite

    JP2001146416A

  • Method for manufacturing zeolite membrane

    JP2010142809A