Multilayer structure, laminate, and method for manufacturing multilayer structure
The multilayer structure addresses viewing angle dependence by employing a first layer angled less than 5.0° and a second layer tilted at 5.0° or more, using block copolymers to ensure consistent color perception and narrow half-width.
Patent Information
- Application Number
- JP2023056161
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing multilayer structures that exhibit structural colors due to multilayer film interference suffer from significant viewing angle dependence, leading to varying colors when viewed from different angles.
A multilayer structure is designed with a first layer having a multilayer film structure arranged at an angle of less than 5.0° and a second layer tilted at an angle of 5.0° or more with respect to a reference plane, utilizing block copolymers to form lamellar structures that reduce viewing angle dependence while maintaining a low half-width.
The structure achieves reduced viewing angle dependence and maintains a narrow half-width, allowing consistent color perception regardless of the viewing angle, while selectively reflecting visible light.
Smart Images

Figure 2024143461000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer structure, a laminate, and a method for producing a multilayer structure. [Background technology]
[0002] There are multilayer structures that exhibit structural colors due to optical phenomena in the microstructure of an object. Structural colors are reflected light that occurs due to diffraction, interference, scattering, or the like of light in a microstructure on the order of the wavelength of light, and therefore have the advantage that they do not fade due to light, unlike coloring using colorants such as pigments and dyes.
[0003] Structural colors due to multilayer interference, which occurs when thin films with fine uneven structures are stacked in multiple layers, are produced by the interference of light reflected at the interfaces of adjacent thin films in the multilayer film layer, and are often observed as the colors of natural creatures such as morpho butterflies.
[0004] As a multilayer structure that exhibits structural color due to multilayer film interference, for example, a color-producing structure having a structure in which two types of polymeric substances with different optical refractive indices are continuously and alternately laminated, and which has a reflective and interference effect and exhibits colors with wavelengths in the visible light region by the reflection and interference effect of natural light, has been disclosed (see, for example, Patent Document 1). Summary of the Invention [Problem to be solved by the invention]
[0005] However, the color-developing structure having reflection and interference effects of Patent Document 1 has a problem in that different colors are visible when viewed from different angles, that is, it has high viewing angle dependency.
[0006] An object of one embodiment of the present invention is to provide a multilayer structure capable of reducing viewing angle dependency while maintaining a low half-value width. [Means for solving the problem]
[0007] One aspect of the present invention is A multilayer structure having a first layer and a second layer and exhibiting selective reflection, the first layer has a multilayer structure arranged at an angle of less than 5.0° with respect to a reference plane of the multilayer structure when viewed from a cross section of the multilayer structure, The second layer is a multilayer structure having a multilayer film structure arranged at an angle of 5.0° or more with respect to the reference plane in at least one direction when viewed from the cross section of the multilayer structure. Effect of the Invention
[0008] One embodiment of the present invention can provide a multilayer structure capable of reducing viewing angle dependency while maintaining a low half-value width. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a cross-sectional view illustrating a schematic configuration of a multilayer structure according to one embodiment. [Diagram 2] FIG. 2 is an explanatory diagram illustrating a microphase-separated structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiments of the present invention will be described in detail. In order to facilitate understanding of the description, the same components in each drawing are given the same reference numerals, and duplicated descriptions will be omitted. In addition, the scale of each member in the drawings may differ from the actual scale. In the specification, "~" indicating a range of numerical values means that the numerical values before and after it are included as the lower and upper limits, unless otherwise specified.
[0011] <Multilayer structure> A multilayer structure according to one embodiment of the present invention will be described. The multilayer structure according to one embodiment has a first layer and a second layer, and exhibits selective reflection. The multilayer structure according to one embodiment may further have other layers as necessary in addition to the first layer and the second layer, or may be composed of the first layer and the second layer.
[0012] Selective reflection refers to reflecting a part of incident light and selectively reflecting light having a predetermined wavelength (incident light). The light reflected by selective reflection can be measured by measuring the reflection spectrum of the multilayer structure using a spectrophotometer (for example, an ultraviolet-visible-infrared spectrophotometer (automatic absolute reflectance measurement system) manufactured by JASCO Corporation). The multilayer structure according to one embodiment may selectively reflect light to emit visible light, which is light having a wavelength in the visible light range (380 nm to 780 nm).
[0013] Fig. 1 is a cross-sectional view showing a schematic configuration of a multilayer structure according to one embodiment. As shown in Fig. 1, the multilayer structure 1 according to one embodiment has a first layer 11 and a second layer 12, and may further have other layers as necessary. The multilayer structure 1 may include the first layer 11 and the second layer 12 laminated in this order.
[0014] [First layer] 1, the first layer 11 is preferably located below the multilayer structure 1. The first layer 11 is a layer containing a block copolymer as a main component, and may further contain optional components such as additives and dyes depending on the purpose.
[0015] (Block Copolymer) The block copolymer forming the first layer 11 may contain a plurality of types of polymer blocks and may be composed of a plurality of types of polymer blocks. Any block copolymer may be used, and is not particularly limited as long as it forms a desired structure, and may be appropriately selected. A diblock copolymer that forms a lamellar structure (plate structure) is preferable.
[0016] Examples of diblock copolymers include polystyrene-b-polyisoprene, polystyrene-b-polytert-butyl methacrylate, polystyrene-b-poly(2-vinylpyridine), polystyrene-b-polymethylacrylate, polybutadiene-b-polyisoprene, polybutadiene-b-poly(2-vinylpyridine), polybutadiene-b-poly(tert-butyl methacrylate), polyisoprene-b-poly(tert-butyl methacrylate), and the like.
[0017] In order for the block copolymer to form a lamellar structure, the volume fraction of the two polymer blocks forming the block copolymer is preferably 0.35 to 0.65. If the volume fraction of the two polymer blocks is 0.35 to 0.65, the microphase separation structure formed by the block copolymer forms a lamellar structure, and the formation of different shapes such as a sphere structure and a cylinder structure is suppressed, so that the first layer 11 can have a regular fine structure. By including the block copolymer, the first layer 11 can have a regular laminated structure having a predetermined angle with respect to a reference plane such as a substrate described later. Since the domain width of the lamellar structure can be changed depending on the molecular weight of the block copolymer, the wavelength of the reflected light generated in the first layer 11 can be controlled.
[0018] The thickness (domain width) of the lamellar structure is preferably 50 nm to 400 nm, more preferably 70 nm to 380 nm, and even more preferably 100 nm to 350 nm, from the viewpoint of reflecting incident light having a wavelength in the ultraviolet or infrared region. If the thickness of the lamellar structure is too thin, the wavelength region of the reflected light is in the UV region. On the other hand, if the thickness of the lamellar structure is too thick, the wavelength region of the reflected light is in the infrared region, making it difficult to use or to obtain suitable selective reflection.
[0019] In this specification, the thickness of the lamellar structure refers to the length in the direction perpendicular to the main surface of the first layer 11. The thickness of the lamellar structure may be, for example, the thickness measured at an arbitrary location on the cross section of the first layer 11, or may be the average value of the measured values measured at several arbitrary locations. Hereinafter, the definition of thickness is the same for other members.
[0020] The first layer 11 has a multilayer film structure 110 arranged at an angle of less than 5.0° with respect to a reference plane, which is the main surface of a substrate or the like on which the multilayer structure 1 is placed, when viewed from a cross section of the multilayer structure 1. The multilayer film structure 110 preferably includes a microphase separation structure. The microphase separation structure is a multilayer film structure in which units having different refractive indices are stacked. The microphase separation structure is preferably a lamellar structure (flat plate structure). The multilayer film structure 110 may be composed of a microphase separation structure.
[0021] The fact that the multilayer structure 110 is arranged at an angle of less than 5.0° with respect to the reference plane may be obtained, for example, by calculating the inclination angle of the layers constituting the multilayer structure 110 from an image obtained by observing the cross section of the multilayer structure 1 with a scanning electron microscope (SEM). The method of calculating the inclination angle is not particularly limited as long as the inclination of the layers constituting the multilayer structure 110 can be calculated, but for example, the inclination angle may be calculated as follows. That is, images are obtained by SEM at several points (e.g., three points) in the cross section of the first layer 11. The pattern obtained from the obtained image is divided into sectors at predetermined angles (e.g., 5°) in all directions, and polar coordinate conversion is performed. The results of the polar coordinate conversion are tallied for each azimuth component to obtain the distribution of the inclination angle of the orientation. The ratio of the inclination angle in the cross section of the first layer 11 is calculated from the average distribution of several measurement points.
[0022] The calculation of the tilt angle described above can be performed using a general image processing method, for example, Python, C++, or the like, or image processing software such as ImageJ.
[0023] When the polymer blocks constituting a block copolymer have different refractive indices, the microphase-separated structure formed by self-organization of the block copolymer forms a multilayer film in which units having different refractive indices are stacked.
[0024] For example, as shown in Fig. 2, a block copolymer has two types of units A and B with different refractive indices, and the refractive indices of the two types of units A and B are n1 and n2, respectively, and the thicknesses (domain widths) are d1 and d2, respectively. In this case, the first layer 11 is a multilayer film having a microphase separation structure formed by laminating a block copolymer having two types of units A and B. In this case, the wavelength λ of the first layer 11 is calculated by the following formula (I). λ[nm]=2(n1×d1+n2×d2) (I)
[0025] The multilayer film structure 110 may be arranged at an angle of less than 5.0° with respect to the reference plane, and is preferably arranged approximately parallel to the reference plane.
[0026] The "reference surface" refers to the main surface of a substrate or the like on which the multilayer structure 1 is placed. The reference surface is, for example, the surface (substrate surface) of a substrate such as paper or a plastic film, the surface of a building, the surface of a road, etc., and also includes a coated surface of a layer-forming liquid composition used to form the first layer 11 or the second layer 12.
[0027] The thickness of the first layer 11 is preferably 1 μm to 50 μm, more preferably 3 μm to 40 μm, and further preferably 5 μm to 30 μm. If the thickness of the first layer 11 is 1 μm or more, a laminate structure that reflects incident light is sufficiently obtained, so that a decrease in reflectance can be suppressed. If the thickness of the first layer 11 is 50 μm or less, a laminate structure that reflects incident light is sufficiently obtained, so that a decrease in reflectance can be suppressed. In addition, an increase in the time required for drying can be suppressed, so that a decrease in productivity can be suppressed, and the formation of different laminate structures due to different drying times for the surface layer and the inside of the coating film can be suppressed, so that a regular laminate structure can be formed.
[0028] The width of the first layer 11 is not particularly limited, and may be set so that the multilayer structure 1 can select visible light having a desired wavelength and develop a structural color.
[0029] [Second Layer] 1, the second layer 12 is preferably laminated on the upper surface of the first layer 11 and located above the multilayer structure 1. When the second layer is located above, the viewing angle dependency of the multilayer structure 1 can be further reduced.
[0030] The second layer 12 contains a block copolymer as a main component, and may further contain optional components such as additives and dyes for film formation, as appropriate depending on the purpose. The block copolymer contained in the second layer 12 can be the block copolymer contained in the first layer 11. The block copolymer is the same as the block copolymer contained in the first layer 11, and therefore details will be omitted.
[0031] The second layer 12 has a multilayer film structure 120 that is arranged tilted in at least one direction at an angle of 5.0° or more with respect to a reference plane of the multilayer structure 1 when viewed from the cross section of the multilayer structure 1.
[0032] The multilayer structure 120 may have either or both of a multilayer structure arranged at an angle of 5.0° or more and less than 90° with respect to a reference plane of the multilayer structure 1 when viewed from the cross-section of the multilayer structure 1, and a multilayer structure arranged at an angle of more than 90° and not more than 175° with respect to a reference plane of the multilayer structure 1 when viewed from the cross-section of the multilayer structure 1.
[0033] That is, the multilayer structure 120 may have, for example, a multilayer structure 120A arranged at an angle of 5.0° or more to the right relative to the reference plane of the multilayer structure 1 when viewed from the cross-section of the multilayer structure 1, and a multilayer structure 120B arranged at an angle of 5.0° or more to the left relative to the reference plane of the multilayer structure 1 when viewed from the cross-section of the multilayer structure 1.
[0034] The multilayer structure 120 preferably includes a microphase-separated structure, similar to the first layer 11. The microphase-separated structure is preferably a lamellar structure, similar to the microphase-separated structure contained in the first layer 11. The multilayer structure 120 may be composed of a microphase-separated structure, similar to the multilayer structure 110.
[0035] The multilayer film structure 120 may be arranged at an angle of 5.0° or more with respect to the reference plane in at least one direction, and is preferably a multilayer film structure arranged in a direction substantially inclined with respect to the reference plane.
[0036] The fact that the multilayer structure 120 is arranged at an angle of 5.0° or more with respect to the reference plane in at least one direction may be obtained by calculating the inclination angle of the layers constituting the multilayer structure 120, similar to the multilayer structure 110 described above. The inclination angle may be calculated using the same method as that for calculating the inclination of the layers constituting the multilayer structure 110. That is, images are obtained by SEM at several points (e.g., three points) in the cross section of the second layer 12. The pattern obtained from the obtained image is divided into sectors at predetermined angles (e.g., 5°) in all directions, and polar coordinate conversion is performed. The results of the polar coordinate conversion obtained are collected for each azimuth component to obtain the distribution of the inclination angle of the orientation. The average value of the distribution of several measurement points is calculated to calculate the inclination angle of the layers constituting the multilayer structure 120 in the cross section of the second layer 12.
[0037] The second layer 12 preferably has the multilayer film structure 120 in 80% or more, more preferably 90% or more, even more preferably 95% or more, and most preferably 100% of the cross section of the second layer 12. If the multilayer film structure 120 exists in 80% or more of the cross section of the second layer 12, the second layer 12 can suppress a decrease in the reflectance of incident light and can suppress viewing angle dependency.
[0038] In addition, the presence of the multilayer structure 120 in 80% or more of the cross section of the second layer 12 means that when calculating the inclination angle of the layers constituting the multilayer structure 120, 80% or more of the layers contain components inclined by 5° or more with respect to all azimuth components obtained by performing polar coordinate conversion.
[0039] The thickness of the second layer 12 is preferably 1 μm to 30 μm, more preferably 3 μm to 25 μm, and even more preferably 5 μm to 20 μm. If the thickness of the second layer 12 is 1 μm or more, a laminated structure that reflects incident light is sufficiently obtained, so that a decrease in reflectance is suppressed. If the thickness of the second layer 12 is 30 μm or less, it is possible to suppress the formation of many layers in which the resin is randomly arranged with respect to the reference plane, so that viewing angle dependency can be suppressed even if a multi-layer structure is formed.
[0040] The width of the second layer 12, like the first layer 11, is not particularly limited as long as it is set so that the multilayer structure 1 can select visible light having a desired wavelength and exhibit a structural color.
[0041] When the thickness of the first layer 11 is X and the thickness of the second layer 12 is Y, it is preferable to satisfy the following relational formula (1) in order to narrow the half-width of the reflected light from the multilayer structure 1 and reduce the viewing angle dependency. Y / X<1.0 (1)
[0042] The multilayer structure 1 selectively reflects light by enhancing the intensity of the reflected light due to optical effects such as optical interference. As described above, selective reflection refers to reflecting a part of the light incident on the multilayer structure 1 and selectively reflecting light having a predetermined wavelength, and a method for measuring the reflected light due to selective reflection will not be described here.
[0043] The multilayer structure 1 can emit visible light (wavelength 380 nm to 780 nm) by selectively reflecting light having a predetermined wavelength. Visible light having a desired wavelength can be selected and emitted as a structural color by setting the widths, refractive indices, etc. of the first layer 11 and the second layer 12 constituting the multilayer structure 1. When the multilayer structure 1 emits visible light, for example, the first layer 11 may have a width of 150 nm and a refractive index of 1.5, and the second layer 12 may have a width of 150 nm and a refractive index of 1.4.
[0044] The refractive index of the multilayer structure 1 is determined depending on the units of the block copolymer constituting the first layer 11 and the second layer 12 contained in the multilayer structure 1. For example, when the block copolymer is poly(styrene-b-isoprene) (PS-b-PI), the refractive index of polystyrene is 1.59 and the refractive index of polyisoprene is 1.52. The refractive index of each unit of the block copolymer constituting the first layer 11 and the second layer 12 is 1.35 to 1.90.
[0045] The light selectively reflected by the multilayer structure 1 (reflected light) varies depending on the thickness (domain width) of the multilayer film structures 110 and 120 of the first layer 11 included in the multilayer structure 1. As described above, the multilayer film structures 110 and 120 are formed of block copolymers, and therefore the thicknesses of the multilayer film structures 110 and 120 vary depending on the molecular chain length of the block copolymer. In order to obtain the light selectively reflected by the multilayer structure 1 (reflected light), for example, the molecular chain length of the block copolymer is preferably 40 nm to 500 nm, more preferably 45 nm to 450 nm, and more preferably 50 nm to 400 nm. If the molecular chain length is 40 nm to 500 nm, the multilayer structure 1 can reflect light having a wavelength in the visible light range and can develop a structural color. If the molecular chain length of the block copolymer is too long, it is necessary to strictly control the movement of the polymer due to self-organization, and it becomes difficult to form a lamellar structure.
[0046] The half-width of the selectively reflected light (reflected light) of the multilayer structure 1 is preferably 200 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less.
[0047] Furthermore, the multilayer structure 1 may have a protective layer or the like on its surface side (upper side in FIG. 1). The protective layer is not particularly limited and can be appropriately selected depending on the purpose. For example, it can be formed by coating a resin such as a thermosetting resin or an ultraviolet-curing resin, or by attaching a transparent resin film. By providing a protective layer on the surface of the multilayer structure 1, it is possible to provide excellent robustness such as weather resistance, abrasion resistance, and impact resistance.
[0048] <Manufacturing method> A method for producing a multilayer structure according to one embodiment will be described.
[0049] In one embodiment of a method for producing a multilayer structure, a layer-forming liquid composition containing a block copolymer dissolved in a solvent having a boiling point of 60° C. to 250° C. is prepared (layer-forming liquid composition preparation step).
[0050] The layer-forming liquid composition contains a block copolymer and an organic solvent, and may contain additives, surfactants, colorants, and the like, as necessary.
[0051] The concentration of the block copolymer in the layer-forming liquid composition is preferably 5 wt% to 40 wt%, and more preferably 5 wt% to 20 wt%. If the concentration in the ink is 5 wt% to 40 wt%, a sufficiently regular laminated structure can be formed. In addition, since the viscosity of the solution is prevented from becoming too high, it is possible to prevent the molecular motion in the liquid film from decreasing during drying, and also to prevent the number of options for soluble block copolymers from becoming limited.
[0052] The solvent is not particularly limited and can be appropriately selected according to the purpose. The boiling point of the solvent is preferably 60°C to 250°C. If the boiling point is 60°C or higher, the following solvents can be used to prevent drying from starting immediately after coating, so that the resin material can be dried in a state where self-organization is sufficient, and a sufficient multilayer film structure can be formed. If the boiling point is 250°C or lower, the time required for drying after coating can be prevented from being too long, so that a decrease in productivity can be suppressed, and the type of drying method can be prevented from being limited, so that drying can be reliably controlled. In addition, the layer structure to be formed can be controlled by selecting the drying speed by controlling the drying speed of the solvent.
[0053] Specific examples of the solvent include toluene, xylene, anisole, cyclohexanone, diethylene glycol dimethyl ether, dimethylformamide (DMF), dimethylsulfoxide (DMSO), and cumene.
[0054] Next, the layer-forming liquid composition is applied onto the substrate to form a first coating film, and the first coating film is dried to form a first layer 11 on the substrate, the first layer 11 having a multilayer film structure 110 arranged at an angle of less than 5.0° relative to the substrate when viewed from a cross-section of the substrate (first layer formation process).
[0055] The substrate used to form the first layer 11 is not particularly limited and can be appropriately selected depending on the purpose. Examples of the substrate include paper, thread, fiber, cloth, leather, metal, plastic, glass, wood, ceramics, and composite materials thereof.
[0056] The method for forming the first layer is not particularly limited and can be appropriately selected depending on the purpose. For example, a bar coater method, a spin coat method, a casting method, an inkjet method, etc. can be mentioned. Among these, the inkjet method is particularly preferable from the viewpoint of high productivity, etc.
[0057] The term "drying" means that the solvent contained in the layer-forming liquid composition is completely evaporated.
[0058] The drying method is not particularly limited and can be appropriately selected depending on the purpose. As described later, the first coating film is dried more gently than the second coating film used to form the second layer 12. Examples of methods for slowly progressing the drying include a method of drying by leaving it to stand in the air and a solvent annealing method of drying in a solvent atmosphere.
[0059] Next, a layer-forming composition is applied onto the first layer 11 to form a second coating film, and the second coating film is dried to form a second layer 12 on the first layer 11, the second layer 12 having a multilayer film structure 120 arranged at an angle of 5.0° or more relative to the substrate in at least one direction when viewed from the cross-section of the substrate (second layer formation process).
[0060] The drying of the second coating film may be adjusted based on the drying time required for drying the second coating film or the volatilization rate of the solvent contained in the second coating film.
[0061] The drying time and the evaporation rate of the solvent refer to the time required for the solvent contained in the layer-forming liquid composition to completely evaporate. The evaporation rate of the solvent can be calculated from the change in mass of the layer-forming liquid composition and the drying time.
[0062] The drying method is not particularly limited and can be appropriately selected depending on the purpose. As described later, the second coating film is dried faster than the first coating film. Examples of methods for speeding up the drying include heating, blowing air, and drying under vacuum.
[0063] The drying time for drying the second coating film is not particularly limited as long as the second layer 12 can be formed to have a multilayer film structure 120, and may be set appropriately. The drying time may be shorter than the drying time for drying the first coating film, and may be, for example, 1 / 4 to 2 / 3 of the drying time for drying the first coating film.
[0064] The evaporation rate of the solvent contained in the second coating film is not particularly limited as long as the second layer 12 can be formed to have a multilayer film structure 120, and may be set as appropriate. The evaporation rate may be slower than the evaporation rate of the solvent contained in the first coating film, and may be, for example, 1 / 4 to 2 / 3 of the evaporation rate of the solvent contained in the first coating film.
[0065] The second layer may be formed by the same method as the first layer, and from the viewpoint of high productivity, the inkjet method is particularly preferred.
[0066] The drying speed in the steps of forming the first layer and the second layer is important in producing the multilayer structure 1. In the self-organization of the block copolymers contained in the first coating film and the second coating film to form a microphase-separated structure during the formation of the first layer 11 and the second layer 12, the drying method and drying speed greatly affect the regularity and orientation of the layered structures such as the multilayer film structures 110 and 120.
[0067] That is, when preparing the first coating film, the second coating film, and other films, by using a drying method that allows the drying of the solvent to proceed slowly, the lamellar structures formed are aligned at an angle of less than 5° to the reference plane of the substrate, etc., and the layer can be formed to have a more regular laminated structure, resulting in a layer with a narrow half-value width. On the other hand, when the drying of the solvent proceeds rapidly, the lamellar structures formed are aligned in a direction inclined at 5° or more to the reference plane of the substrate, etc., and the lamellar structures are aligned randomly in multiple directions, resulting in a layer with low viewing angle dependency that can reflect light of the same wavelength regardless of the angle of incidence of light.
[0068] As described above, by forming the second layer 12 on the first layer 11, the multilayer structure 1 shown in FIG. 1 can be produced.
[0069] Thus, the multilayer structure 1 according to one embodiment has a first layer 11 and a second layer 12, and the first layer 11 has a multilayer film structure 110, and the second layer 12 has a multilayer film structure 120. The multilayer film structure 110 has a structure in which the multilayer film structure 1 is arranged at an angle of less than 5.0° with respect to the reference plane of the multilayer structure 1 when viewed from the cross section of the multilayer structure 1, and the multilayer film structure 120 has a structure in which the multilayer film structure 1 is arranged at an angle of 5.0° or more with respect to the reference plane when viewed from the cross section of the multilayer structure 1, and is arranged at an angle of 5.0° or more with respect to the reference plane at least in one direction. Since the multilayer structure can form different stacked structures in the first layer 11 and the second layer 12, it is possible to form a stacked structure in which the functions are separated in each layer. Since the multilayer film structure 110 has a regularly arranged stacked structure, the reflected light is reinforced by the action of interference, and therefore the multilayer film structure 110 has a high reflectance and a narrow half-width. However, the optical path length when reflected changes depending on the angle of the incident light, and the wavelength of the reflected light is different, so the viewing angle dependency is high. On the other hand, since the multilayer structure 120 has a random arrangement of regular laminated structures, it can reflect light incident from any direction with the same thickness (domain width), and the change in color depending on the angle is suppressed. Therefore, the multilayer structure 120 can reflect light with a constant optical path length regardless of the angle of incidence, so that the viewing angle dependency can be reduced.
[0070] Therefore, since the multilayer structure 1 can achieve both viewing angle dependence and half-width by separating the functions of the first layer 11 and the second layer 12, it is possible to reduce the viewing angle dependence while maintaining a low half-width. Therefore, the multilayer structure 1 can emit only a specific color and suppress changes in the color emission due to the observation angle.
[0071] The multilayer structure 1 can emit visible light as a structural color. As a result, the multilayer structure according to one embodiment can reflect only light having a certain wavelength among incident light and transmit light having the remaining wavelengths without absorbing it, so that the reflected light having a certain wavelength can be visually confirmed as a structural color.
[0072] The multilayer structure 1 can include a lamellar structure in the first layer 11 and the second layer 12. The lamellar structure is a microphase separation structure formed by a block copolymer, and the first layer 11 can have a multilayer film structure 110 having a regular laminated structure, and the second layer 12 can have a multilayer film structure 110 having an irregular laminated structure in which layers are randomly arranged in multiple directions. Since the first layer 11 and the second layer 12 of the multilayer structure 1 include a lamellar structure, a multilayer structure film having a different refractive index can be formed in the thickness direction, and therefore selective reflection can be performed in the surface direction, and structural color can be more reliably expressed.
[0073] In the multilayer structure 1, the thickness of the lamellar structure contained in the first layer 11 and the second layer 12 can be set to 50 nm to 400 nm, which enables the multilayer structure 1 to reflect incident light having a wavelength in the UV region to the infrared region.
[0074] When the thickness of the first layer 11 is X and the thickness of the second layer 12 is Y, the multilayer structure 1 can satisfy the following formula (1). By making the second layer 12 thinner than the first layer 11, the second layer 12 can fully receive the reflected light of the first layer 11, and the half-width of the multilayer structure 1 can be narrowed. Although the first layer 11 has viewing angle dependency, it has a regular laminated structure and is a highly ordered film, so that the reflectance is high and the half-width is narrow. Therefore, by satisfying the following formula (1), the multilayer structure 1 can more reliably narrow the half-width of the reflected light and more reliably suppress the viewing angle dependency. Y / X<1.0 (1)
[0075] The multilayer structure 1 can contain at least one type of block copolymer in each of the first layer 11 and the second layer 12. The multilayer structure 1 can exhibit any structural color by selecting the type of block copolymer.
[0076] In the multilayer structure 1, the multilayer film structure 110 can be arranged approximately parallel to a reference plane. This allows the multilayer structure 1 to better exhibit the function of the first layer 11, thereby improving the reflectance of the first layer 11 and reliably exhibiting a high reflectance, while further narrowing the half-width of the reflected light and further suppressing the viewing angle dependency. The multilayer structure 1 according to the embodiment of the present invention may have the first layer 11 and the second layer 12 alternately and repeatedly.
[0077] <Laminate> The laminate according to an embodiment includes a substrate and a multilayer structure according to an embodiment, and may include other members as necessary. The laminate according to an embodiment includes a substrate and a multilayer structure according to an embodiment stacked on the substrate.
[0078] The substrate is not particularly limited, and any material can be used as long as it can laminate the multilayer structure according to one embodiment. Examples of the substrate that can be used include a plastic substrate, a silicon (Si) substrate, a metal plate, and a glass substrate.
[0079] Examples of materials that can be used to form the plastic substrate include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate (PC), polypropylene (PP), polymethyl methacrylate (PMMA), and polyimide (PI).
[0080] The plastic substrate may be transparent, translucent or opaque. The term "transparent" refers to a substrate having a visible light (light having a wavelength of 380 to 780 nm) transmittance to such an extent that the inside of the substrate can be visually recognized from the outside, and the visible light transmittance is 40% or more, preferably 80% or more, and more preferably 90% or more. The light transmittance is measured using "Plastics - Determination of total light transmittance and total light reflectance" as specified in JIS K 7375:2008.
[0081] Examples of materials that can be used to form the metal plate include aluminum, copper, stainless steel, and tantalum.
[0082] The thickness of the substrate is not particularly limited, and may be any appropriate thickness depending on the application of the laminate according to one embodiment, the material of the substrate, and the like.
[0083] The other members are not particularly limited and can be appropriately selected depending on the purpose. For example, an adhesive layer and the like can be mentioned.
[0084] The laminate according to an embodiment includes a multilayer structure according to an embodiment, and thus the half-width and viewing angle dependency can be reduced, and only a specific color can be produced while suppressing changes in color production due to the observation angle. Therefore, the laminate according to an embodiment can produce structural colors due to multilayer interference, which are often observed as colors of organisms in nature, such as morpho butterflies, with the same color production when viewed from any angle, and can produce vivid colors with low viewing angle dependency.
[0085] The laminate according to one embodiment can be suitably used in, for example, electronic devices such as wearable devices and smartphones, home appliances, audio products, computers, displays, in-vehicle products, watches, accessories, optical components, doors, window glass, building materials, and the like.
[0086] Although the embodiment has been described above, the above embodiment is presented as an example, and the present invention is not limited to the above embodiment. The above embodiment can be implemented in various other forms, and various combinations, omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. EXAMPLES
[0087] The embodiments will be described in more detail below with reference to examples and comparative examples, but the embodiments are not limited to these examples and comparative examples.
[0088] <Fabrication of structure> [Example 1] A 10 wt% solution of poly(styrene-b-isoprene) in cumene was applied to a black PET substrate by bar coating and then thoroughly dried in air to produce a coating film with a thickness of 20 μm. Next, a 10 wt% solution of poly(styrene-b-isoprene) in diethylene glycol dimethyl ether was similarly applied by bar coating and thoroughly dried while heating on a hot plate to produce a multilayer structure with a total thickness of 30 μm.
[0089] [Example 2] A 10 wt% solution of poly(styrene-b-tert-butyl methacrylate) in cumene was applied to a black PET substrate by bar coating and then thoroughly dried in air to produce a coating film with a thickness of 20 μm. Next, a 10 wt% solution of poly(styrene-b-tert-butyl methacrylate) in cyclohexanone was similarly applied by bar coating and then thoroughly dried while heating on a hot plate to produce a multilayer structure with a total thickness of 30 μm.
[0090] [Example 3] A 10 wt% solution of poly(styrene-b-isoprene) in cumene was applied to a black PET substrate by bar coating and then thoroughly dried in air to produce a coating film with a thickness of 20 μm. Next, a 10 wt% solution of poly(styrene-b-isoprene) in diethylene glycol dimethyl ether was similarly applied by bar coating and thoroughly dried while heating on a hot plate to produce a multilayer structure with a total thickness of 50 μm.
[0091] [Comparative Example 1] A 10 wt% cumene solution of poly(styrene-b-isoprene)-(Mn=411 kDa) was applied onto a black PET substrate by the bar coating method, and then thoroughly dried in air to prepare a 20 μm-thick coating film (single-layer structure).
[0092] [Comparative Example 2] A 10 wt% solution of poly(styrene-b-isoprene) (Mn=411 kDa) in diethylene glycol dimethyl ether was applied by the bar coating method, and then thoroughly dried while being heated on a hot plate to produce a 10 μm-thick coating film (single-layer structure).
[0093] [Comparative Example 3] A 10 wt% cumene solution of poly(styrene-b-isoprene) was coated on a black PET substrate by bar coating and then thoroughly dried in air to produce a coating film with a thickness of 10 μm. A 10 wt% diethylene glycol dimethyl ether solution of poly(styrene-b-isoprene) was then coated on the substrate by bar coating and then thoroughly dried in air to produce a multilayer structure with a total thickness of 20 μm.
[0094] [Comparative Example 4] A 10 wt% cumene solution of poly(styrene-b-isoprene)-(Mn=411 kDa) was applied by bar coating, and then thoroughly dried while heated on a hot plate to produce a multilayer structure with a thickness of 19 μm. Next, a 10 wt% polyethylene glycol dimethyl ether solution of poly(styrene-b-isoprene)-(Mn=411 kDa) was similarly applied by bar coating, and then thoroughly dried while heated on a hot plate to produce a multilayer structure with a total thickness of 42 μm.
[0095] <Evaluation> The cross section of each of the structures (multilayer structure or single layer structure) of the examples and comparative examples was observed by SEM to obtain an image. From the obtained image, the inclination angle of the constituent layers was calculated as follows. In addition, the viewing angle dependency and half width of each of the structures of the examples and comparative examples were measured and evaluated as follows.
[0096] (Calculating the inclination angle) The cross-section of the structure (multilayer structure or single-layer structure) was taken by the resin embedding method, and three points in each cross-section were observed by SEM to obtain the observed image. The inclination angle of the layers constituting the structure, as seen in the obtained cross-sectional SEM image, was calculated using image processing software (Python). Specifically, the contrast of the obtained cross-sectional SEM image was adjusted, and the pattern obtained from the image by 2D FFT processing was divided into sectors of 5 degrees in all directions, and polar coordinate conversion was performed. The results were collected for each azimuth component to obtain the distribution of the inclination angle of the orientation. The inclination angle in the cross-section was calculated by calculating the average value of the distribution of the three measurement points. Note that the inclination of the arrangement of the second layer is 80% or more in the layer means that 80% or more of the components in the layer are inclined by 5° or more with respect to all azimuth components.
[0097] [Viewing angle dependence] The obtained multilayer structure was measured at incident angles of 5°, 15°, 30°, and 45° and receiving angles of -75° to 75° in 15° increments using a revolutionary spectrophotometric colorimeter GCMS-11 manufactured by Murakami Color Research Laboratory Co., Ltd., and the Lch (lightness (L), chroma (c), and hue (h)) color space was calculated. The viewing angle dependency was evaluated based on the following evaluation criteria using the standard deviation ΔH of the hue (h) at each angle. (Evaluation Criteria) A: ΔH≦10 B:10<ΔH
[0098] [Half width] The reflectance of the obtained multilayer structure was measured using a JASCO ultraviolet-visible-infrared spectrophotometer (automatic absolute reflectance measurement system) under the conditions of an incident angle of 90°, a detection angle of 0°, a polarizer of 45°, a measurement range of 300 nm to 780 nm, and a scanning speed of 1000 nm / min. From the obtained reflectance spectrum, the peak wavelength λ_max and the half-width FWHM relative to the peak top were calculated, and the ratio X obtained by dividing the half-width FWHM by the wavelength λ was used to evaluate the reflectance according to the following evaluation criteria. (Evaluation Criteria) A:X≦10 B:10 <X≦20 C:X>20
[0099] Table 1 shows the type of block copolymer in the structures of the prepared Examples and Comparative Examples, the thickness X and angle of the first layer 11, the thickness Y and angle of the second layer 12, the thickness Y / thickness X, whether or not a multilayer structure was formed, and the evaluation results of the viewing angle dependency and half width as evaluation results of the structures.
[0100] [Table 1]
[0101] From Table 1, it was confirmed that the viewing angle dependency and the half width were both low in each of the Examples, whereas it was confirmed that the viewing angle dependency or the half width was high in each of the Comparative Examples.
[0102] Therefore, the structural laminate of each Example can have a low half-width and viewing angle dependency if the first layer is formed of a multilayer film structure arranged at an angle of less than 5.0° with respect to the reference plane of the multilayer structure when viewed from the cross section of the multilayer structure, and the second layer is formed of a multilayer film structure arranged at an angle of 5.0° or more with respect to the reference plane when viewed from the cross section of the multilayer structure. Therefore, it can be said that the multilayer structure of each Example can be provided as a color-developing structure or the like in which only a specific color can be seen even when viewed from different angles.
[0103] The aspects of the embodiment of the present invention are as follows, for example. <1> A multilayer structure having a first layer and a second layer and exhibiting selective reflection, the first layer has a multilayer structure arranged at an angle of less than 5.0° with respect to a reference plane of the multilayer structure when viewed from a cross section of the multilayer structure, The second layer has a multilayer structure in which, when viewed from a cross section of the multilayer structure, the second layer is arranged at an angle of 5.0° or more in at least one direction with respect to the reference plane. <2> The multilayer structure emits visible light. <1> The multilayer structure according to claim 1. <3> The first layer and the second layer have a lamellar structure. <1> or <2> The multilayer structure according to claim 1. <4> The thickness of the lamellar structure is 50 nm to 400 nm. <3> The multilayer structure according to claim 1. <5> When the thickness of the first layer is X and the thickness of the second layer is Y, the following formula (1) is satisfied: <1> ~ <4> 13. The multilayer structure according to claim 12 . Y / X<1.0 (1) <6> The first layer and the second layer each comprise at least one block copolymer. <1> ~ <5> 13. The multilayer structure according to claim 12 . <7> When viewed from the cross section of the multilayer structure, the multilayer film structure arranged at an angle of less than 5.0° with respect to the reference plane is arranged parallel to the reference plane. <1> ~ <6> 13. The multilayer structure according to claim 12 . <8> A substrate; On the substrate <1> ~ <7> A multilayer structure according to any one of the above items, A laminate having the following structure: <9> A method for producing a multilayer structure having a first layer and a second layer and exhibiting selective reflection, comprising the steps of: forming a first layer on a substrate, the first layer having a multilayer structure arranged at an angle of less than 5.0° with respect to the substrate when viewed from a cross section of the substrate; forming a second layer on the first layer, the second layer having a multilayer structure inclined in at least one direction at an angle of 5.0° or more with respect to the substrate when viewed from a cross section of the substrate; A method for producing a multilayer structure comprising the steps of: [Explanation of symbols]
[0104] 1 Multilayer structure 11 First Layer 12 Second Layer 110 A multilayer film structure in which the multilayer structure is arranged at an angle of less than 5.0° to the reference plane of the multilayer structure when viewed from the cross section of the multilayer structure. 120 A multilayer film structure in which, when viewed from the cross section of the multilayer structure, the multilayer structure is tilted in at least one direction at an angle of 5.0° or more with respect to the reference plane of the multilayer structure. 120A A multilayer film structure in which the layers are arranged at an angle of 5.0° or more to the right of the reference plane of the multilayer structure when viewed from the cross section of the multilayer structure. 120B A multilayer film structure in which the layers are arranged at an angle of 5.0° or more to the left of the reference plane of the multilayer structure when viewed from the cross section of the multilayer structure. [Prior art documents] [Patent documents]
[0105] [Patent Document 1] Japanese Patent Application Publication No. 07-034324
Claims
1. A multilayer structure having a first layer and a second layer and exhibiting selective reflection, the first layer has a multilayer structure arranged at an angle of less than 5.0° with respect to a reference plane of the multilayer structure when viewed from a cross section of the multilayer structure, The second layer has a multilayer structure in which, when viewed from a cross section of the multilayer structure, the second layer is arranged at an angle of 5.0° or more in at least one direction with respect to the reference plane.
2. 10. The multilayer structure according to claim 1, wherein the multilayer structure emits visible light.
3. 10. The multi-layer structure of claim 1, wherein the first layer and the second layer have a lamellar structure.
4. 4. The multilayer structure according to claim 3, wherein the lamellar structure has a thickness of 50 nm to 400 nm.
5. 2. The multilayer structure according to claim 1, wherein the thickness of the first layer is X and the thickness of the second layer is Y, and the following formula (1) is satisfied: Y / X<1.0...(1)
6. 10. The multi-layer structure of claim 1, wherein said first layer and said second layer each comprise at least one block copolymer.
7. The multilayer structure according to claim 1 , wherein the multilayer film structures arranged at an angle of less than 5.0° to the reference plane when viewed from a cross section of the multilayer structure are arranged parallel to the reference plane.
8. A substrate; The multilayer structure of claim 1 provided on the substrate; A laminate having the following structure:
9. A method for producing a multilayer structure having a first layer and a second layer and exhibiting selective reflection, comprising the steps of: forming a first layer on a substrate, the first layer having a multilayer structure arranged at an angle of less than 5.0° with respect to the substrate when viewed from a cross section of the substrate; forming a second layer on the first layer, the second layer having a multilayer structure inclined in at least one direction at an angle of 5.0° or more with respect to the substrate when viewed from a cross section of the substrate; A method for producing a multilayer structure comprising the steps of:
Citation Information
Patent Citations
Color-developing structure material having reflection and interference action
JP1995034324A