Battery module, manufacturing method for battery module, and inspection method for laser welding

By using laser etching marks with predefined patterns to inspect welding quality in battery modules, the challenges of detecting defects in laser welding are addressed, allowing for real-time monitoring and maintaining production efficiency.

JP2024143487APending Publication Date: 2024-10-11AESC JAPAN LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023056202
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Laser welding in battery modules is prone to defects due to equipment abnormalities and workpiece deformations, making it difficult to detect and respond to changes in welding quality, which can lead to production delays and reduced productivity.

Method used

Incorporating laser etching marks with specific patterns on both sides of the welding joints, allowing for real-time inspection of welding quality by comparing actual marks with pre-designed patterns to detect abnormalities in the laser welding process.

Benefits of technology

Facilitates easy and efficient inspection of factors affecting welding quality, enabling in-line monitoring and reducing the need for destructive testing, thus maintaining production efficiency and quality control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143487000001_ABST
    Figure 2024143487000001_ABST
Patent Text Reader

Abstract

To easily inspect the factor that has an influence on quality of laser welding.SOLUTION: A battery module includes a laser welding part 200 formed in a positive electrode tab 120, and a left laser etching mark 210 and a right laser etching mark 220 formed on both sides of the laser welding part 200 in the positive electrode tab 120. An inspection method for the laser welding includes a step of inspecting whether the laser etching mark formed on a process object where the laser welding part is formed and a pre-designed laser etching mark are the same or different.SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a battery module, a manufacturing method for a battery module, and a method for inspecting laser welding. [Background technology]

[0002] In recent years, various battery modules including a plurality of battery cells have been developed. For example, as described in Patent Document 1 or 2, a battery module may be provided with an identifier formed by a laser. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2019 / 193869 [Patent Document 2] JP 2006-40875 A Summary of the Invention [Problem to be solved by the invention]

[0004] In battery modules, laser welding may be used to join various objects to be processed, such as joining the tabs of battery cells, joining the tabs and bus bars, and assembling the housing. Laser welding is required to have various qualities, such as impact resistance, vibration resistance, and environmental resistance tests. However, the laser welding device used for laser welding may have abnormalities due to changes over time, and the objects to be processed may have various abnormalities, such as deformation of the tabs and abnormalities in the assembly accuracy of the housing. When such abnormalities occur, it may be difficult to suppress laser welding defects such as poor joints in laser welding and abnormal resistance values ​​of laser welded parts. On the other hand, such laser welding defects may be detected by methods such as laser welding monitoring (LWM) and resistance value measurement. However, even if such methods are used, it may be relatively difficult to immediately determine the cause of the laser welding defects and to respond to changes over time in the laser welding defects. In addition, the frequency of occurrence of such laser welding defects may be random, and it may be relatively difficult to grasp the signs of laser welding defects. Therefore, when a laser welding defect occurs, it may be necessary to stop the laser welding line and inspect the laser welds before and after the laser welding defect occurs, for example, by destructive testing. Therefore, it can be relatively difficult to easily inspect factors that affect the quality of laser welding.

[0005] One object of the present invention is to easily inspect factors that affect the quality of laser welding. Other objects of the present invention will become apparent from the description of this specification. [Means for solving the problem]

[0006] One aspect of the present invention is as follows. [1] A laser weld formed on the workpiece; a laser etching mark formed on at least one of both sides of the laser weld in the workpiece; A battery module comprising: [2] The battery module according to [1], wherein the laser etching mark has a corner. [3] The battery module according to [1] or [2], wherein the laser etched marks have a plurality of patterns that at least partially overlap each other. [4] The battery module according to any one of [1] to [3], wherein the laser etching marks have a plurality of patterns whose centers overlap each other. [5] The battery module according to any one of [1] to [4], wherein the laser-etched mark is inspected for similarity or difference from a predesigned laser-etched mark. [6] forming a laser weld on a workpiece; forming a laser etching mark on at least one of both sides of the laser weld in the workpiece; A method for manufacturing a battery module comprising: [7] A method for inspecting laser welding, comprising a step of inspecting whether a laser etching mark formed on a workpiece on which a laser weld is to be formed is different from a predesigned laser etching mark. Effect of the Invention

[0007] According to the above-described aspects of the present invention, factors that affect the quality of laser welding can be easily inspected. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a perspective view of a portion of a battery module according to the embodiment. [Diagram 2] FIG. 4 is a diagram showing a cross section of a laser welded portion according to an embodiment. [Diagram 3] FIG. 1 is a diagram showing an example of a laser welding device for laser welding a workpiece. [Figure 4] 4A to 4C are views for explaining a first example of a method for forming a laser welded portion. [Diagram 5] 6A to 6C are diagrams for explaining a second example of a method for forming a laser welded portion. [Figure 6]5A to 5C are diagrams illustrating a method of forming a left-side first laser etching pattern, a laser welded portion, and a right-side first laser etching pattern according to an embodiment. [Figure 7] 1A to 1C are diagrams for explaining a method of forming a left laser etching mark and a right laser etching mark according to an embodiment. [Figure 8] 5A to 5C are diagrams illustrating a method of forming a first laser etching pattern according to an embodiment. [Figure 9] 1 is a graph showing an example of the relationship between laser power and laser spot size in a first laser etching pattern. [Figure 10] FIG. 4 is a diagram for explaining a method for measuring a laser spot size in a first laser etching pattern. [Figure 11] FIG. 2 is a cross-sectional view of an object to be processed in an etching mode. [Figure 12] FIG. 2 is a cross-sectional view of a workpiece in a melting mode. [Figure 13] 1A to 1C are diagrams showing a first example of an abnormality in the shape of a first laser etching pattern. [Figure 14] FIG. 11 is a diagram showing a second example of an abnormality in the shape of the first laser etching pattern. [Figure 15] FIG. 11 is a diagram showing a third example of an abnormality in the shape of the first laser etching pattern. [Figure 16] 13A to 13C are diagrams showing a fourth example of an abnormality in the shape of the first laser etching pattern. [Figure 17] FIG. 13 is a diagram showing a fifth example of an abnormality in the shape of the first laser etching pattern. [Figure 18] FIG. 11 is a diagram showing a first example of an abnormality in the shape of a laser-etched mark. [Figure 19] FIG. 13 is a diagram showing a second example of an abnormal shape of a laser etched mark. [Figure 20] 13A and 13B are diagrams showing laser etching marks according to a modified example. [Figure 21] 11A to 11C are diagrams for explaining another example of the laser welding inspection method according to the embodiment. [Figure 22]11A to 11C are diagrams for explaining another example of the laser welding inspection method according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, embodiments and modifications of the present invention will be described with reference to the drawings. In all the drawings, similar components are given similar reference numerals and descriptions thereof will be omitted as appropriate.

[0010] Fig. 1 is a perspective view of a portion of a battery module 10 according to an embodiment. Fig. 2 is a diagram showing a cross section of a laser welded portion 200 according to an embodiment.

[0011] In each figure, an X-axis, a Y-axis, and a Z-axis that are perpendicular to each other are shown for the purpose of explanation. Hereinafter, the directions parallel to the X-axis, Y-axis, and Z-axis are referred to as the X-direction, the Y-direction, and the Z-direction, respectively, as necessary. Hereinafter, the side indicated by the arrow indicating the X-axis is referred to as the +X side, and the opposite side of the side indicated by the arrow indicating the X-axis is referred to as the -X side, as necessary. Hereinafter, the side indicated by the arrow indicating the Y-axis is referred to as the +Y side, and the opposite side of the side indicated by the arrow indicating the Y-axis is referred to as the -Y side, as necessary. Hereinafter, the side indicated by the arrow indicating the Z-axis is referred to as the +Z side, and the opposite side of the side indicated by the arrow indicating the Z-axis is referred to as the -Z side, as necessary. Hereinafter, the direction perpendicular to the Z-axis is referred to as the XY plane direction, the direction perpendicular to the Y-axis is referred to as the ZX plane direction, and the direction perpendicular to the X-axis is referred to as the YZ plane direction, as necessary. Hereinafter, the direction of rotation around a direction parallel to the Z direction is referred to as the θ direction, as necessary.

[0012] In some figures, a white circle with an X indicating the X-axis, Y-axis, or Z-axis indicates that the arrow of the axis indicated by the white circle is pointing from the front to the back of the page. A white circle with a black dot indicating the X-axis, Y-axis, or Z-axis indicates that the arrow of the axis indicated by the white circle is pointing from the back to the front of the page.

[0013] The battery module 10 according to the embodiment includes a plurality of battery cells 100. Each battery cell 100 extends substantially parallel to the XY plane direction. Each battery cell 100 has a thickness substantially parallel to the Z direction. The plurality of battery cells 100 are stacked substantially parallel to the Z direction. Each battery cell 100 has a battery element (not shown), an exterior material 110, a positive electrode tab 120, and a negative electrode tab 130. In one example, the battery element includes a plurality of positive electrodes and a plurality of negative electrodes stacked alternately in the Z direction. The positive electrodes and the negative electrodes adjacent to each other in the Z direction are separated from each other by a separator (not shown). However, the structure of the battery element is not limited to this example.

[0014] The exterior material 110 contains a battery element (not shown) and an electrolyte (not shown). The exterior material 110 is made of, for example, an aluminum laminate.

[0015] The positive electrode tab 120 is electrically connected to the positive electrode of the battery element. The positive electrode tab 120 is made of, for example, at least one of aluminum and an aluminum alloy. The surface of the positive electrode tab 120 may be subjected to secondary processing such as a corrosion-resistant protective coating or a plating film. However, the material constituting the positive electrode tab 120 is not limited to this example as long as it is a material with a relatively high electrical conductivity, that is, a material with a relatively low electrical resistivity.

[0016] The negative electrode tab 130 is electrically connected to the negative electrode of the battery element. The negative electrode tab 130 is made of, for example, at least one of copper and a copper alloy. The surface of the negative electrode tab 130 may be subjected to secondary processing such as a corrosion-resistant protective coating or a plating film. However, the material constituting the negative electrode tab 130 is not limited to this example as long as it is a material with relatively high electrical conductivity, that is, a material with relatively low electrical resistivity. The material constituting the positive electrode tab 120 and the material constituting the negative electrode tab 130 may be the same or different.

[0017] In each battery cell 100, the positive electrode tab 120 and the negative electrode tab 130 are pulled out on opposite sides of the exterior material 110 in the Y direction. However, the method of pulling out the positive electrode tab 120 and the negative electrode tab 130 is not limited to this example. For example, the positive electrode tab 120 and the negative electrode tab 130 may be pulled out from the same side on the +Y side or -Y side of the exterior material 110. In this example, the positive electrode tab 120 and the negative electrode tab 130 are aligned approximately parallel to the X direction.

[0018] In the embodiment, a plurality of cell groups including a plurality of battery cells 100 electrically connected in parallel are electrically connected in series. In the example shown in FIG. 1, eight cell groups each including two battery cells 100 are illustrated in schematic form. However, the number of cell groups included in the actual battery module 10 is not limited to the example shown in FIG. 1. In the example shown in FIG. 1, two positive electrode tabs 120 are drawn out toward the -Y side from two battery cells 100 included in the third cell group from the +Z side, and two negative electrode tabs 130 are drawn out toward the -Y side from two battery cells 100 included in the fourth cell group from the +Z side. As shown in FIG. 2, these positive electrode tabs 120 and negative electrode tabs 130 are joined to each other by a laser welded portion 200. Therefore, in the example shown in FIG. 1, the two battery cells 100 included in the third cell group from the +Z side and the two battery cells 100 included in the fourth cell group from the +Z side are electrically connected in series. Such joints between the positive electrode tabs 120 and the negative electrode tabs 130 are provided alternately on the +Y side and the -Y side of the battery module 10. Thus, in the example shown in Fig. 1, eight cell groups are electrically connected in series.

[0019] The manner of electrical connection of the multiple battery cells 100 is not limited to the above-mentioned example. For example, multiple cell groups including three or more battery cells 100 electrically connected in parallel may be electrically connected in series. Alternatively, multiple single battery cells 100 may simply be connected in series.

[0020] The method for joining the positive electrode tab 120 and the negative electrode tab 130 to each other may be laser welding alone, or may be a combination of laser welding and another joining method. For example, joining methods such as a crimping technique, FSW (friction stir welding), ultrasonic welding, TIG (tungsten inert gas) welding, and MIG (metal inert gas) welding may be combined.

[0021] The laser welded portion 200 is formed by irradiating the joint between the positive electrode tab 120 and the negative electrode tab 130 with a laser from the side where the positive electrode tab 120 is located. In the example shown in FIG. 2, the laser welded portion 200 is formed by irradiating the joint between the positive electrode tab 120 and the negative electrode tab 130 with a laser from the +Z side. As shown in FIG. 2, the laser welded portion 200 at least partially reaches the negative electrode tab 130. Therefore, the positive electrode tab 120 and the negative electrode tab 130 are joined to each other.

[0022] Fig. 3 is a diagram showing an example of a laser welding apparatus 50 for laser welding a workpiece W. In the example shown in Fig. 3, the workpiece W is mounted on a stage 550 that is substantially perpendicular to the Z direction. The workpiece W is laser welded by the laser welding apparatus 50 as follows. However, the structure of the laser welding apparatus for laser welding the workpiece W is not limited to the structure of the laser welding apparatus 50 shown in Fig. 3.

[0023] 3, a laser beam B is emitted from a laser oscillator 502 via an optical fiber 504. The laser beam B passes through a beam expander 506 and a focus lens 508 in this order, and is incident on a galvanometer mirror optical system 510. The beam diameter of the laser beam B is expanded by the beam expander 506. By moving the focus lens 508 in a direction approximately parallel to the optical axis of the laser beam B, the position of the focus of the laser beam B on the workpiece W in the Z direction can be adjusted.

[0024] After entering the galvanometer mirror optical system 510, the laser beam B passes through a condenser lens 512 and enters a movable mirror 514. After being reflected by the movable mirror 514, the laser beam B passes through a cover glass 516 and is irradiated onto an object to be processed W. The movable mirror 514 makes it possible to adjust the irradiation position of the laser beam B on the object to be processed W in the X and Y directions.

[0025] The tip of the optical fiber 504, the beam expander 506, the focus lens 508, and the galvanometer mirror optical system 510 can be moved in the XY plane direction by a moving unit 520. The moving unit 520 makes it possible to adjust the irradiation position of the laser beam B on the workpiece W in the X, Y, and Z directions.

[0026] The stage 550 is movable in the X, Y, Z, and θ directions. The stage 550 makes it possible to adjust the irradiation position of the laser beam B on the workpiece W in the X, Y, Z, and θ directions.

[0027] In the example shown in Fig. 2, two positive electrode tabs 120 and two negative electrode tabs 130 to be joined to each other correspond to the workpiece W shown in Fig. 3. In this example, a laser beam B is irradiated to the joint between the positive electrode tabs 120 and the negative electrode tabs 130 from the +Z side.

[0028] The welding conditions of the workpiece W may differ depending on whether the materials to be welded are homogeneous or heterogeneous. For example, when dissimilar materials are welded, if the welding conditions are not optimal, an intermetallic compound film (IMC) may be formed at a high melting point in the welded portion of dissimilar materials such as aluminum-copper. When an IMC is formed, defects such as high hardness of the IMC or brittleness of the IMC may occur. Alternatively, if the welding conditions are not optimal in the welded portion of homogeneous materials such as aluminum-aluminum, defects such as melting cracks at the welded portion may occur. Therefore, in order to avoid these defects, the welding conditions of the workpiece W must be set to the optimal conditions. The welding conditions of the workpiece W may deviate from the optimal conditions due to various abnormalities such as an abnormality of the laser oscillator 502 of the laser welding device 50 or an abnormality of various optical systems such as the galvanometer mirror optical system 510. Therefore, the various abnormalities of the laser welding device 50 may affect the joining strength of the laser welded portion 200. In other words, this embodiment can be used to determine whether the joining strength of the laser welded portion 200 is good or bad in the inspection described below.

[0029] FIG. 4 is a diagram for explaining a first example of a method for forming the laser welded portion 200. As shown in FIG.

[0030] In Fig. 4, the circles on the laser welded portion 200 indicate spots generated by a laser irradiated from the +Z side. In the example shown in Fig. 4, a plurality of spots are continuously generated substantially parallel to the X direction from the left side to the right side of the positive electrode tab 120 to form the laser welded portion 200. The laser oscillator 502 can be either a continuous oscillation CW (continuous wave) type or a pulse oscillation type depending on predetermined conditions such as the welding purpose and the characteristics of the workpiece W. In the example shown in Fig. 4, the laser oscillator 502 is a continuous oscillation CW type.

[0031] Fig. 5 is a diagram for explaining a second example of a method for forming the laser welded portion 200. The second example shown in Fig. 5 is similar to the first example shown in Fig. 4 except for the following points.

[0032] In the example shown in Fig. 5, wobbling welding is performed, as indicated by the dashed arrow virtually attached to the right side of the laser welded portion 200 in Fig. 5. In the example shown in Fig. 5, a plurality of spots are continuously generated in a clockwise direction from the left side to the right side of the positive electrode tab 120, thereby forming the laser welded portion 200.

[0033] In the laser welding illustrated in FIG. 4 and FIG. 5, the long-term operation of the laser welding apparatus 50 may cause phenomena such as wear of each movable element of the laser welding apparatus 50 and thermal lens effect of various optical lenses. For example, phenomena such as burning of the movable mirror 514 and displacement of the movable mirror 514 due to an abnormal operation of the movable mirror 514, blocking of the laser beam B by various optical lenses such as the beam expander 506, the focus lens 508, the condenser lens 512, and the cover glass 516, and a decrease in the transmittance of various optical lenses may occur. It may be relatively difficult to discover such phenomena in daily pre-maintenance. It may also be relatively difficult to grasp the signs of the above-mentioned phenomena. Furthermore, simply stopping production equipment and increasing the frequency of maintenance will result in a decrease in productivity.

[0034] FIG. 6 is a diagram for explaining a method for forming a left first laser etching pattern 212 (hereinafter simply referred to as the left first pattern 212), a laser welded portion 200, and a right first laser etching pattern 222 (hereinafter simply referred to as the right first pattern 222) according to an embodiment. FIG. 7 is a diagram for explaining a method for forming a left laser etching mark 210 (hereinafter simply referred to as the left mark 210) and a right laser etching mark 220 (hereinafter simply referred to as the right mark 220) according to an embodiment. Hereinafter, for the sake of explanation, the -X side is referred to as the left side, and the +X side is referred to as the right side, as necessary. However, the left side and the right side do not necessarily mean the directions when the battery module 10 is used.

[0035] 6, a laser is irradiated from the +Z side to form the left side first pattern 212 on the left side portion of the positive electrode tab 120. The left side first pattern 212 has a substantially ∞ shape.

[0036] 6, a laser weld 200 is formed from the left side to the right side of the positive electrode tab 120 by laser irradiation from the +Z side. The laser weld 200 extends approximately parallel to the X direction. The left first pattern 212 is located on the left side of the left end of the laser weld 200.

[0037] 6, a right-side first pattern 222 is formed on the right portion of the positive electrode tab 120 by laser irradiation from the +Z side. The left-side first pattern 212 and the right-side first pattern 222 have substantially the same shape. The right-side first pattern 222 is located on the right side of the right end of the laser welded portion 200. The left-side first pattern 212 and the right-side first pattern 222 are located on both the left and right sides of the laser welded portion 200 in the X direction.

[0038] Next, as shown in FIG. 7, a left second laser etching pattern 214 (hereinafter simply referred to as the left second pattern 214) is formed on the left portion of the positive electrode tab 120 by laser irradiation from the +Z side. The left first pattern 212 and the left second pattern 214 are substantially symmetrical patterns. The left first pattern 212 and the left second pattern 214 at least partially overlap each other. Thus, a left mark 210 having the left first pattern 212 and the left second pattern 214 is formed. The left mark 210 is substantially in the shape of a + surrounded by a substantially square.

[0039] Next, as shown in FIG. 7, a right second laser etching pattern 224 (hereinafter simply referred to as the right second pattern 224) is formed on the right part of the positive electrode tab 120 by laser irradiation from the +Z side. The right first pattern 222 and the right second pattern 224 are substantially symmetrical patterns. The right first pattern 222 and the right second pattern 224 at least partially overlap each other. Thus, a right mark 220 having the right first pattern 222 and the right second pattern 224 is formed. The right mark 220 is substantially in the shape of a + surrounded by a substantially square. The left mark 210 and the right mark 220 are located on both the left and right sides of the laser welded portion 200 in the X direction.

[0040] The optimum conditions for laser irradiation to form the laser welded portion 200 are generally determined in advance according to the type of the workpiece W. For example, when the workpiece W is an aluminum alloy and a copper alloy and the aluminum alloy and the copper alloy are laser welded to each other, the optimum conditions for laser irradiation are, for example, a laser wavelength of 1064 nm, a focused laser spot diameter of 72 μm, and a laser output of 1000 W. These optimum conditions are constant if the ambient environment of the workpiece W and the external environment of the workpiece W, such as the gas atmosphere, are constant.

[0041] The laser output for forming the left mark 210 and the right mark 220 is lower than the laser output under the optimum conditions of laser irradiation for forming the laser welded portion 200. The left mark 210 and the right mark 220 are formed in an etching mode described below with reference to Figs. 9 to 12. For example, when the optimum conditions of laser irradiation for forming the laser welded portion 200 are the above-mentioned example, the laser output for forming the left mark 210 and the right mark 220 is about 1 / 3 of the laser output under the optimum conditions, that is, about 200 W to 400 W. In this example, a recess having a depth of about 10 µm to 30 µm is formed on the surface of the object to be processed by laser etching.

[0042] 6 and 7, a left mark 210 and a right mark 220 are formed on both sides in the X direction of the laser welded portion 200 in the positive electrode tab 120. However, one of the left mark 210 and the right mark 220 does not have to be formed.

[0043] Hereinafter, when there is no need to particularly distinguish between the left mark 210 and the right mark 220 in the description, the left mark 210 and the right mark 220 may be simply referred to as the mark 210. Hereinafter, when there is no need to particularly distinguish between the left first pattern 212 and the right first pattern 222 in the description, the left first pattern 212 and the right first pattern 222 may be simply referred to as the first pattern 212. Hereinafter, when there is no need to particularly distinguish between the left second pattern 214 and the right second pattern 224 in the description, the left second pattern 214 and the right second pattern 224 may be simply referred to as the second pattern 214.

[0044] Fig. 8 is a diagram showing a method for forming a first pattern 212 according to an embodiment. For the purpose of explanation, six arrows, a first arrow A1 to a sixth arrow A6, are virtually shown in Fig. 8. Circles shown along the first pattern 212 in Fig. 8 indicate laser spots generated by laser irradiation.

[0045] The first pattern 212 is formed as follows: The second pattern 214 is formed symmetrically with respect to the Y axis with respect to the method for forming the first pattern 212, which will be described below.

[0046] First, as shown by the first arrow A1, a plurality of laser spots are sequentially generated substantially parallel to the X direction from the -X side to the +X side. Thus, a first line pattern L1 substantially parallel to the X direction is generated. The first line pattern L1 includes a plurality of laser spots arranged substantially parallel to the X direction.

[0047] Next, as shown by the second arrow A2, multiple laser spots are generated in sequence from the -Y side toward the +Y side, approximately parallel to the Y direction. Thus, a second line pattern L2 approximately parallel to the Y direction is generated. The second line pattern L2 includes multiple laser spots arranged approximately parallel to the Y direction. The +X side end of the first line pattern L1 and the -Y side end of the second line pattern L2 are approximately perpendicular to each other. Thus, the first pattern 212 has a substantially right-angled corner portion formed by the intersection of the +X side end of the first line pattern L1 and the -Y side end of the second line pattern L2.

[0048] Next, as shown by the third arrow A3, multiple laser spots are generated in sequence from the +X side to the -X side, approximately parallel to the X direction. Thus, a third line pattern L3 approximately parallel to the X direction is generated. The third line pattern L3 includes multiple laser spots arranged approximately parallel to the X direction. The +Y side end of the second line pattern L2 and the +X side end of the third line pattern L3 are approximately perpendicular to each other. Thus, the first pattern 212 has a substantially right-angled corner portion formed by the intersection of the +Y side end of the second line pattern L2 and the +X side end of the third line pattern L3.

[0049] Next, as shown by the fourth arrow A4, multiple laser spots are generated in sequence from the +Y side to the -Y side, approximately parallel to the Y direction. Thus, a fourth line pattern L4 that is approximately parallel to the Y direction is generated. The fourth line pattern L4 includes multiple laser spots arranged approximately parallel to the Y direction. The -X side end of the third line pattern L3 and the +Y side end of the fourth line pattern L4 are approximately perpendicular to each other. Thus, the first pattern 212 has a substantially right-angled corner portion formed by the intersection of the -X side end of the third line pattern L3 and the +Y side end of the fourth line pattern L4.

[0050] Next, as shown by the fifth arrow A5, a plurality of laser spots are sequentially generated substantially parallel to the X direction from the +X side to the -X side. Thus, a fifth line pattern L5 substantially parallel to the X direction is generated. The fifth line pattern L5 includes a plurality of laser spots arranged substantially parallel to the X direction. The -Y side end of the fourth line pattern L4 and the +X side end of the fifth line pattern L5 are substantially perpendicular to each other. Thus, the first pattern 212 has a substantially right-angled corner portion formed by the intersection of the -Y side end of the fourth line pattern L4 and the +X side end of the fifth line pattern L5.

[0051] Next, as shown by the sixth arrow A6, a plurality of laser spots are sequentially generated substantially parallel to the Y direction from the -Y side toward the +Y side. Thus, a sixth line pattern L6 substantially parallel to the Y direction is generated. The sixth line pattern L6 includes a plurality of laser spots arranged substantially parallel to the Y direction. The -X side end of the fifth line pattern L5 and the -Y side end of the sixth line pattern L6 are substantially perpendicular to each other. Thus, the first pattern 212 has a substantially right-angled corner portion formed by the intersection of the -X side end of the fifth line pattern L5 and the -Y side end of the sixth line pattern L6.

[0052] In the first pattern 212, the third line pattern L3 and the fifth line pattern L5 are positioned at approximately equal distances from the first line pattern L1 in the Y direction. In the first pattern 212, the second line pattern L2 and the sixth line pattern L6 are positioned at approximately equal distances from the fourth line pattern L4 in the X direction.

[0053] 8, the -X side end of the first line pattern L1 protrudes toward the -X side from the +Y side end of the sixth line pattern L6. This makes it easier to identify the starting position for forming the first pattern 212. However, the -X side end of the first line pattern L1 does not have to protrude toward the -X side from the +Y side end of the sixth line pattern L6.

[0054] Fig. 9 is a graph showing an example of the relationship between the laser output and the laser spot size in the first pattern 212. Fig. 10 is a diagram for explaining a method for measuring the laser spot size in the first pattern 212. Fig. 11 is a cross-sectional view of the workpiece W in the etching mode. Fig. 12 is a cross-sectional view of the workpiece W in the melting mode. In the examples shown in Figs. 9 to 12, the workpiece W is an aluminum alloy. However, the workpiece W is not limited to an aluminum alloy and may be, for example, copper.

[0055] 9 indicates the laser output (unit: W) for forming the first pattern 212. The vertical axis of the graph shown in Fig. 9 indicates the laser spot size (unit: μm) in the first pattern 212.

[0056] The plot of M(X) in the graph shown in Fig. 9 indicates that M(X) = (X1 + X2 + X3 + X4) / 4. As shown in Fig. 10, X1 indicates the width in the X direction at approximately the center in the Y direction of the second line pattern L2. X2 indicates the width in the X direction of the fourth line pattern L4 at a portion located at approximately equal distances from the first line pattern L1 and the third line pattern L3. X3 indicates the width in the X direction of the fourth line pattern L4 at a portion located at approximately equal distances from the first line pattern L1 and the fifth line pattern L5. X4 indicates the width in the X direction of the sixth line pattern L6 at approximately the center in the Y direction.

[0057] The plot of M(Y) in the graph shown in Fig. 9 indicates that M(Y) = (Y1 + Y2 + Y3 + Y4) / 4. As shown in Fig. 10, Y1 indicates the width in the Y direction of a portion of the first line pattern L1 located at approximately equal distances from the fourth line pattern L4 and the sixth line pattern L6. Y2 indicates the width in the Y direction of a portion of the first line pattern L1 located at approximately equal distances from the fourth line pattern L4 and the second line pattern L2. Y3 indicates the width in the Y direction of the third line pattern L3 at approximately the center in the X direction. Y4 indicates the width in the Y direction of the fifth line pattern L5 at approximately the center in the X direction.

[0058] As shown in FIG. 9, M(X) and M(Y) are both about 100 μm when the laser output is around 240 W to 350 W. When the laser output is around 240 W to 350 W, the laser irradiation by the laser welding device 50 is in the etching mode. In the etching mode, as shown in FIG. 11, a recess W1 is formed on the surface of the workpiece W on the +Z side by laser etching. When M(X) and M(Y) in the etching mode are the theoretical values ​​of the laser spot diameter when focused or are close to them, it can be said that the focus of the focus lens 508 is on the workpiece W. In other words, in the embodiment, the laser spot diameter can be measured from M(X) and M(Y) without using a special device. Therefore, the laser spot diameter can be measured in a short time compared to the case where a special device is used. Even if the laser spot system is not theoretical, the same geodesic measurement can be performed by always maintaining the above-mentioned about 100 μm as a default value.

[0059] As shown in Fig. 9, when the laser output is 400 W or more, both M(X) and M(Y) are approximately 200 µm or more. When the laser output is 400 W or more, the laser irradiation by the laser welding device 50 is in the melting mode. In the melting mode, as shown in Fig. 12, an expanded portion W2 is formed on the +Z side surface of the workpiece W by laser melting. The expanded portion W2 is formed by a volume expansion of the molten workpiece W.

[0060] The relationship between the pattern width and the laser output shown in Fig. 9 varies depending on the type of the workpiece. This is because the threshold value of the laser output for laser etching the workpiece may vary depending on the material properties (e.g., laser absorptivity, thermal conductivity, expansion coefficient, etc.) of the workpiece. Therefore, a plurality of relationships between the laser output and the laser spot size shown in Fig. 9 may be prepared in advance depending on the type of the workpiece.

[0061] Next, a first example of a method for inspecting laser welding by the laser welding device 50 will be described with reference to Figs. 13 to 17. In Figs. 13 to 17, the laser welding is inspected by inspecting whether or not the shape of the actual first pattern 212 is different from the shape of the first pattern designed in advance. In other words, the presence or absence of various abnormalities such as equipment abnormalities and signs of various abnormalities can be judged in real time each time welding is performed, and the stability of the quality of the laser welding can be monitored. Note that even when the left second pattern 214, the right first pattern 222, and the right second pattern 224 are used, the laser welding can be inspected in the same way as when the first pattern 212 is used.

[0062] FIG. 13 is a diagram showing a first example of an abnormality in the shape of the first pattern 212. As shown in FIG.

[0063] 13, the width in the Y direction of the first line pattern L1 between the end of the first line pattern L1 on the -X side and the intersection of the first line pattern L1 and the fourth line pattern L4 is narrower than the width designed in advance. From this abnormality in the shape of the first pattern 212, for example, an abnormality in the laser welding device 50 such as a decrease in the matching and tracking function of the laser oscillator 502 and the galvanometer mirror optical system 510, a decrease in the initial output of the laser oscillator 502, or an abnormality in the focus lens 508, or an abnormality on the side of the workpiece W such as a missetting of the workpiece W or a positional deviation of the workpiece W due to an abnormality in the jig, or a deviation in the assembly accuracy of the workpiece W, can be inferred.

[0064] FIG. 14 is a diagram showing a second example of the abnormality in the shape of the first pattern 212. In FIG.

[0065] 14, the width of all the line patterns of the first pattern 212 is narrower than the predesigned width. From this shape abnormality of the first pattern 212, for example, an abnormality of the laser welding device 50 such as an abnormality of the focus lens 508, a drop in the output of the laser oscillator 502, or an abnormality of the galvanometer mirror optical system 510, or an abnormality on the side of the workpiece W to be processed such as a missetting of the workpiece W or a positional deviation of the workpiece W due to an abnormality in the jig, or an error in the assembly accuracy of the workpiece W, can be inferred.

[0066] FIG. 15 is a diagram showing a third example of the abnormality in the shape of the first pattern 212. In FIG.

[0067] 15, the width of all the line patterns of the first pattern 212 is wider than the predesigned width. From this shape abnormality of the first pattern 212, it is presumed that there is an abnormality in the laser welding device 50 such as a decrease in the tracking function of the galvanometer mirror optical system 510, a malfunction of the galvanometer mirror optical system 510, a synchronization failure between the laser oscillator 502 and the galvanometer mirror optical system 510, or an excessive or decreased output of the laser oscillator 502, in particular, an abnormality in the laser focus due to an abnormal operation of the focus lens 508.

[0068] FIG. 16 is a diagram showing a fourth example of the abnormality in the shape of the first pattern 212. In FIG.

[0069] In the example shown in Fig. 16, the shape from the +X side end of the first line pattern L1 to the +Y side end of the fourth line pattern L4 via the second line pattern L2 and the third line pattern L3 is deformed from the pre-designed shape. Specifically, the shape from the +X side end of the first line pattern L1 to the +Y side end of the fourth line pattern L4 via the second line pattern L2 and the third line pattern L3 is an approximately circular pattern. Also, the shape from the -Y side end of the fourth line pattern L4 to the sixth line pattern L6 via the fifth line pattern L5 is deformed from the pre-designed shape. Specifically, the shape from the -Y side end of the fourth line pattern L4 to the sixth line pattern L6 via the fifth line pattern L5 is an approximately elliptical pattern. This abnormality in the shape of the first pattern 212 suggests an abnormality in the laser welding apparatus 50, such as a decrease in the tracking function of the galvanometer mirror optical system 510, a malfunction of the galvanometer mirror optical system 510, a poor synchronization between the laser oscillator 502 and the galvanometer mirror optical system 510, a decrease in the output of the laser oscillator 502, or an abnormality in the stage 550.

[0070] FIG. 17 is a diagram showing a fifth example of an abnormality in the shape of the first pattern 212. In FIG.

[0071] In the example shown in FIG. 17, the shape from the +X side end of the first line pattern L1 to the +Y side end of the fourth line pattern L4 via the second line pattern L2 and the third line pattern L3 is deformed from the pre-designed shape. Specifically, the shape from the +X side end of the first line pattern L1 to the +Y side end of the fourth line pattern L4 via the second line pattern L2 and the third line pattern L3 is a substantially elliptical pattern. In addition, the corner between the -Y side end of the fourth line pattern L4 and the +X side end of the fifth line pattern L5, and the corner between the -X side end of the fifth line pattern L5 and the -Y side end of the sixth line pattern L6 are deformed from the pre-designed shape. Specifically, these corners are rounded. This abnormality in the shape of the first left pattern 212 suggests an abnormality in the laser welding device 50, such as an abnormality in the reduction ratio of the galvanometer mirror optical system 510, a decrease in the tracking function of the galvanometer mirror optical system 510, poor synchronization between the laser oscillator 502 and the galvanometer mirror optical system 510, or an abnormality in various optical systems.

[0072] In the inspection described with reference to Figs. 13 to 17, various abnormalities such as an abnormality in the laser welding device 50 can be detected from abnormalities in the shape of the first pattern 212, and the signs of the various abnormalities can be grasped. Abnormalities in the shape of the first pattern 212 can be detected by a relatively simple method such as microscope observation or automatic image inspection. When observing abnormalities in the shape of the first pattern 212 by such a method, it is also possible to inspect the quality of the laser welding in-line without stopping the production line. Therefore, factors that affect the quality of the laser welding can be inspected relatively easily.

[0073] Next, a second example of a method for inspecting laser welding by laser welding apparatus 50 will be described with reference to Fig. 18 to Fig. 19. In Fig. 18 to Fig. 19, the laser welding is inspected by inspecting whether or not there is a difference between the shape of the actual mark 210 and the shape of a mark designed in advance.

[0074] FIG. 18 is a diagram showing a first example of an abnormality in the shape of the mark 210. In FIG.

[0075] 18, at least one of the first pattern 212 and the second pattern 214 is shifted in the Y direction from a predesigned position. From this shape abnormality of the mark 210, an abnormality of the stage 550 in the Y direction, an abnormality of the mechanical system of the galvanometer mirror optical system 510, an abnormality of the laser welding device 50 such as an abnormality in the irradiation position of the laser beam B, or an abnormality on the side of the workpiece W such as an abnormality in the fixing jig of the workpiece W or an abnormality in the assembly of a structure including the workpiece W can be inferred.

[0076] FIG. 19 is a diagram showing a second example of an abnormality in the mark 210. In FIG.

[0077] 19, at least one of the first pattern 212 and the second pattern 214 is shifted in the X and Y directions from a predesigned position. From this shape abnormality of the mark 210, an abnormality of the stage 550 in the X and Y directions, an abnormality of the mechanical system of the galvanometer mirror optical system 510, an abnormality of the laser welding device 50 such as an abnormality in the irradiation position of the laser beam B, or an abnormality on the side of the workpiece W such as an abnormality in the fixing jig for the workpiece W or an abnormality in the assembly of a structure including the workpiece W can be inferred.

[0078] 18 to 19, similarly to the inspection described with reference to Figures 13 to 17, various abnormalities such as an abnormality in the laser welding device 50 can be detected from an abnormality in the shape of the mark 210, and signs of the various abnormalities can be grasped. Therefore, factors that affect the quality of laser welding can be inspected relatively easily.

[0079] Next, a third example of the method for inspecting laser welding performed by laser welding apparatus 50 will be described with reference to FIG.

[0080] In this example, the laser welding is inspected by inspecting whether the actual positions of the left mark 210 and the right mark 220 are different from the positions of the left mark and the right mark designed in advance. Specifically, the heat generated when the laser welded portion 200 is formed may cause deformation of the workpiece, such as elongation or displacement of the positive electrode tab 120. The deformation of the workpiece may cause at least one of the distance in the X direction between the position of the left mark 210 in the X direction and the position of the right mark 220 in the X direction, and the distance in the Y direction between the position of the left mark 210 in the Y direction and the position of the right mark 220 in the Y direction. For example, the deformation of the positive electrode tab 120 due to the influence of heat generated when the laser welded portion 200 is formed can be grasped by the deviation of the position of the right first pattern 222 relative to the left first pattern 212 from the design position. Furthermore, after the influence of heat generated during the formation of the laser welded portion 200 disappears, by irradiating the laser for forming the first right pattern 222 and the second left pattern 214, even if the deformation of the positive electrode tab 120 returns to normal or the position of the first left pattern 212 shifts, various deformations of the positive electrode tab 120, such as the return of the deformation of the positive electrode tab 120 and the shift in the position of the first left pattern 212, can be grasped. Therefore, the deformation of the workpiece due to laser welding can be estimated from the positions of the left mark 210 and the right mark 220. Therefore, factors that affect the quality of laser welding can be inspected relatively easily.

[0081] In addition, the laser welding may be inspected by inspecting whether the shape of the actual mark 210 is different from the shape of a pre-designed mark. For example, if an abnormality occurs in the laser output and the laser output becomes high, the mark 210 becomes distorted and the mark 210 cannot be read. Therefore, from this abnormality in the mark 210, an abnormality in the laser output can be inferred. Therefore, factors that affect the quality of the laser welding can be inspected relatively easily.

[0082] FIG. 20 is a diagram showing a laser-etched mark 210A according to a modified example.

[0083] The laser etching mark 210A has an outer laser etching pattern 212A (hereinafter, simply referred to as the outer pattern 212A) and an inner laser etching pattern 214A (hereinafter, simply referred to as the inner pattern 214A). The outer pattern 212A is a substantially square frame pattern. The inner pattern 214A is a substantially square pattern. The inner pattern 214A is surrounded by the outer pattern 212A. In one example, the outer pattern 212A is formed, and then the inner pattern 214A is formed. In this example, the inner pattern 214A can be formed in a state in which there is an area surrounded by the outer pattern 212A. Therefore, compared to the case in which the outer pattern 212A is formed after the inner pattern 214A is formed, it is possible to simplify the inspection by visual inspection or a camera or the like for forming the inner pattern 214A at the center of the outer pattern 212A in the XY plane direction. However, the outer pattern 212A may be formed after the inner pattern 214A is formed. Alternatively, the inner pattern 214A and the outer pattern 212A may be formed simultaneously.

[0084] In the design of the laser etching mark 210A, the center of the outer pattern 212A in the XY plane direction and the center of the inner pattern 214A in the XY plane direction overlap each other in the Z direction. Therefore, if an abnormality occurs in the laser welding device 50, the center of the outer pattern 212A in the XY plane direction and the center of the inner pattern 214A in the XY plane direction may be misaligned. Therefore, from this abnormality in the laser etching mark 210A, an abnormality in the laser welding device 50 can be inferred. Therefore, factors that affect the quality of laser welding can be relatively easily inspected.

[0085] The shape of the laser etched mark is not limited to the shapes described in the above embodiment and modified examples.

[0086] For example, the laser etching mark may have a corner. In this example, an abnormality in the laser welding device 50 can be inferred from the roundness of the corner.

[0087] Alternatively, the laser etching mark may include a plurality of laser etching patterns that at least partially overlap each other. In this example, a malfunction of the laser welding apparatus 50 can be inferred from a misalignment of the plurality of laser etching patterns.

[0088] Alternatively, the laser etching mark may have a plurality of laser etching patterns whose centers overlap each other. In this example, an abnormality in the laser welding apparatus 50 can be inferred from the misalignment of the centers of the plurality of laser etching patterns.

[0089] FIG. 21 is a diagram for explaining another example of the laser welding inspection method according to the embodiment.

[0090] In the example shown in FIG. 21 , each of the positive electrode tab 120 and the negative electrode tab 130 and the bus bar 140 are joined to each other by a laser welded portion 200. In the example shown in FIG. 21 , the laser welded portion 200 that joins the positive electrode tab 120 and the bus bar 140 to each other is divided into two in the X direction. A left mark 210 and a right mark 220 are formed on both sides of the two divided laser welded portions 200 in the X direction. Similarly, the laser welded portion 200 that joins the negative electrode tab 130 and the bus bar 140 to each other is divided into two in the X direction. A left mark 210 and a right mark 220 are formed on both sides of the two divided laser welded portions 200 in the X direction.

[0091] 21 , in the same manner as in the above-described example, factors that affect the quality of laser welding can be easily inspected using the left mark 210 and the right mark 220. Furthermore, from the inspection results of the left mark 210 and the right mark 220 provided on the positive electrode tab 120 or the negative electrode tab 130, the assembly position accuracy of various parts during the manufacturing process of the battery module 10 or a product including the battery module 10 can be visualized, and can also be used for quality assurance of the battery module 10 or a product including the battery module 10.

[0092] FIG. 22 is a diagram for explaining another example of the laser welding inspection method according to the embodiment.

[0093] The housing 150 shown in FIG. 22 houses, for example, a plurality of battery cells 100 shown in FIG. 1. The housing 150 has a top plate 151, a bottom plate 152, a front plate 153, a rear plate 154, a first side plate 155, and a second side plate 156. A portion of the top plate 151 overlapping with the first side plate 155 and an upper end portion of the first side plate 155 are joined to each other by a laser welded portion 200. A first left pattern 212 and a first right pattern 222 are formed on both sides of the laser welded portion 200. A portion of the top plate 151 overlapping with the second side plate 156 and an upper end portion of the second side plate 156 are joined to each other by the laser welded portion 200. A first left pattern 212 and a first right pattern 222 are formed on both sides of the laser welded portion 200.

[0094] In the example shown in FIG. 22, similarly to the above-mentioned example, factors that affect the quality of laser welding can be easily inspected using the left first pattern 212 and the right first pattern 222.

[0095] Although the embodiment and modified examples of the present invention have been described above with reference to the drawings, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. [Explanation of symbols]

[0096] 10 battery module, 50 laser welding device, 100 battery cell, 110 exterior material, 120 positive electrode tab, 130 negative electrode tab, 140 bus bar, 150 housing, 151 top plate, 152 bottom plate, 153 front plate, 154 rear plate, 155 first side plate, 156 second side plate, 200 laser welded portion, 210 left side laser etching mark, left side mark, mark, 210A laser etching mark, 212 left side first laser etching pattern, left side first pattern, first pattern, 212A outer laser etching pattern, outer pattern, 214 left side second laser etching pattern, left side second pattern, second pattern, 214A inner laser etching pattern, inner pattern, 220 right side laser etching mark, right side mark, 222 right side first laser etching pattern, right side first pattern, 224 right side second laser etching pattern, right side second pattern, 502 Laser oscillator, 504, optical fiber, 506, beam expander, 508, focus lens, 510, galvanometer mirror optical system, 512, condenser lens, 514, movable mirror, 516, cover glass, 520, moving unit, 550, stage, A1, first arrow, A2, second arrow, A3, third arrow, A4, fourth arrow, A5, fifth arrow, A6, sixth arrow, B, laser beam, L1, first line pattern, L2, second line pattern, L3, third line pattern, L4, fourth line pattern, L5, fifth line pattern, L6, sixth line pattern, W, processing object

Claims

1. A laser weld formed on the workpiece; a laser etching mark formed on at least one of both sides of the laser weld in the workpiece; A battery module comprising:

2. The battery module of claim 1 , wherein the laser etched mark has a corner.

3. The battery module of claim 1 , wherein the laser etched marks have a plurality of patterns that at least partially overlap one another.

4. The battery module of claim 1 , wherein the laser etched marks have a plurality of patterns with overlapping centers.

5. The battery module according to any one of claims 1 to 4, wherein the laser etching mark is inspected for similarity or difference with a predesigned laser etching mark.

6. forming a laser weld on a workpiece; forming a laser etching mark on at least one of both sides of the laser weld in the workpiece; A method for manufacturing a battery module comprising:

7. A method for inspecting laser welding, comprising a step of inspecting whether a laser etching mark formed on a workpiece on which a laser weld is to be formed is different from a predesigned laser etching mark.

Citation Information

Patent Citations

  • Method and device for inspecting laser welding quality

    JP2005111538A

  • Laser weldment and laser welding quality determination method for battery

    JP2016207412A

  • Manufacturing method of battery case cover

    JP2020145173A

  • Battery pack and automobile including same

    JP2020514984A

  • Bus bar

    WO2021153436A1