Secondary battery and manufacturing method for the same

The secondary battery design with a conductive layer on the negative electrode side and insulating layer on the positive electrode side, using an elongated separator, addresses misalignment and short circuits in lithium metal secondary batteries, maintaining active material density and preventing short circuits.

JP2024144240AActive Publication Date: 2024-10-11HONDA MOTOR CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024043657
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-19
Publication Date
2024-10-11
Estimated Expiration
2044-03-19

AI Technical Summary

Technical Problem

Lithium metal secondary batteries face issues with misalignment and short circuits due to changes in negative electrode thickness during charging and discharging, which are exacerbated by the formation of SEI layers and lithium dendrites, leading to potential short circuits and decreased active material density.

Method used

A secondary battery design with an elongated separator having insulating and conductive layers, where the conductive layer is positioned on the negative electrode side and the insulating layer on the positive electrode side, with extension parts wound around the electrode layer housing portion to prevent misalignment and short circuits.

Benefits of technology

The design effectively prevents misalignment and short circuits, maintaining active material density and enhancing energy efficiency by ensuring the conductive layer does not contact the positive electrode, even with significant thickness changes in the negative electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144240000001_ABST
    Figure 2024144240000001_ABST
Patent Text Reader

Abstract

To provide a secondary battery and a manufacturing method for the same, in which even if the thickness of a negative electrode layer largely changes due to charging and discharging, the displacement of a positive electrode layer and a negative electrode layer does not occur easily.SOLUTION: A secondary battery includes an electrode laminate, an electrolyte solution, and an exterior body that accommodates the electrode laminate and the electrolyte solution. The electrode laminate includes a positive electrode layer, a negative electrode layer, and a rectangular separator. The rectangular separator includes an electrode layer accommodation part including two or more folds that are folded in a zig-zag manner along a length direction, and an extension part that is connected to an end part of the electrode layer accommodation part in the length direction. The positive electrode layer and the negative electrode layer are disposed to face each of the folds and the extension part is wound around an external side surface of the electrode layer accommodation part.SELECTED DRAWING: Figure 8
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a secondary battery and a method for manufacturing the same. [Background technology]

[0002] In recent years, research and development has been conducted on secondary batteries that contribute to energy efficiency in order to ensure that more people have access to affordable, reliable, sustainable, and advanced energy. In order to improve the energy density of secondary batteries, secondary batteries with a stacked structure in which multiple positive electrode layers and negative electrode layers are stacked alternately have been considered. In this stacked structure secondary battery, it has been considered to fold a long separator in a zigzag shape and arrange the positive electrode layers and negative electrode layers alternately at the folded parts in order to suppress misalignment of the positive electrode layers and negative electrode layers (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2020 / 003846 [Patent Document 2] International Publication No. 2020 / 003847 Summary of the Invention [Problem to be solved by the invention]

[0004] In the technology related to secondary batteries, increasing the capacity is an issue. In order to increase the capacity of secondary batteries, it is desired to put lithium metal secondary batteries using metallic lithium as the negative electrode active material into practical use. However, in lithium metal secondary batteries, the thickness of the negative electrode layer changes significantly due to charging and discharging. For this reason, in a lithium metal secondary battery having a laminated structure in which multiple positive electrode layers and negative electrode layers are alternately stacked, there is a risk that the positional deviation between the positive electrode layer and the negative electrode layer may easily occur due to the change in the thickness of the negative electrode layer caused by charging and discharging.

[0005] In addition, in lithium metal secondary batteries, repeated charging and discharging causes an SEI layer (solid electrolyte intermediate phase) to accumulate at the interface between the current collector of the negative electrode layer and lithium, making it easier for lithium dendrites to form during charging. When lithium dendrites form, they may penetrate the separator and cause a short circuit between the positive electrode layer and the negative electrode layer. In addition, when lithium dendrites form, the density of the layer of metallic lithium (negative electrode active material layer) deposited on the negative electrode current collector decreases, and the lithium secondary battery may expand excessively during charging.

[0006] According to the study by the present inventors, by using a laminate in which a conductive layer is laminated on the surface of a porous membrane as a separator and arranging the conductive layer on the negative electrode layer side, it may be possible to suppress short circuits caused by dendrites and a decrease in the density of the active material layer of the negative electrode layer in a charged state. However, if a long separator having a conductive layer on one surface is folded in a zigzag shape and the positive electrode layer and the negative electrode layer are arranged to overlap each other alternately at the folded portion, the positive electrode layer and the conductive layer of the long separator may come into contact with each other, causing a short circuit between the positive electrode layer and the negative electrode layer.

[0007] The present invention has been made in view of the above, and aims to provide a secondary battery and a method for manufacturing the same in which the positive electrode layer and the negative electrode layer are unlikely to be misaligned even if the thickness of the negative electrode layer changes significantly due to charging and discharging. In particular, the present invention aims to provide a secondary battery and a method for manufacturing the same in which the positive electrode layer and the negative electrode layer are unlikely to be misaligned and the positive electrode layer and the negative electrode layer are unlikely to be short-circuited even if a separator having a conductive layer on one surface is used. This will ultimately contribute to energy efficiency. [Means for solving the problem]

[0008] The present inventors have found that in order to solve the above problems, it is effective to provide an extension of the long separator at the end of the electrode layer housing section in which the positive electrode layer and the negative electrode layer are arranged by folding the long separator zigzag, and to wrap the extension around the outer surface of the electrode layer housing section, and have completed the present invention.

[0009] (1) A secondary battery comprising: an electrode laminate, an electrolyte, and an exterior body that accommodates the electrode laminate and the electrolyte, the electrode laminate having a positive electrode layer, a negative electrode layer, and a long separator that includes an insulating porous membrane and a conductive layer provided on one surface of the insulating porous membrane, the long separator having an electrode layer accommodating section formed by alternately overlapping an insulating fold that is folded along the length direction so that a surface on the insulating porous membrane side is on the inside and a conductive fold that is folded along the length direction so that a surface on the conductive layer side is on the inside, and a first extension portion extending from one end of the electrode layer accommodating section in the length direction, the positive electrode layer being disposed in the insulating fold and the negative electrode layer being disposed in the conductive fold so that they face each other, and the first extension portion being wound around an outer surface of the electrode layer accommodating section so that the surface on the insulating porous membrane side is on the outside.

[0010] According to the secondary battery of (1), since the first extension portion is wound around the outer surface of the electrode layer housing portion, even if the thickness of the negative electrode layer changes significantly due to charging and discharging, the positive electrode layer and the negative electrode layer are unlikely to be misaligned. In addition, since the conductive layer of the long separator is disposed on the negative electrode layer side, short circuits caused by dendrites and a decrease in density of the negative electrode active material layer of the negative electrode layer in the charged state are suppressed. Furthermore, since the insulating porous membrane of the long separator is disposed on the positive electrode layer side, and the first extension portion is wound around the electrode layer housing portion with the surface on the insulating porous membrane side facing outward, the conductive layer of the long separator and the positive electrode layer are unlikely to come into contact with each other. Therefore, a short circuit between the positive electrode layer and the negative electrode layer is unlikely to occur.

[0011] (2) A second extension portion extending from the other end of the electrode layer accommodating portion in the longitudinal direction, The secondary battery according to (1), wherein the second extension portion extends so that a tip of the conductive fold is in contact with a surface of the insulating porous film.

[0012] In the secondary battery (2), since the second extension portion is in contact with the tip of the conductive fold, i.e., the opening of the insulating fold, the surface of the insulating porous membrane is in contact with the conductive layer of the long separator and the positive electrode layer, and therefore, a short circuit between the positive electrode layer and the negative electrode layer is less likely to occur.

[0013] (3) The secondary battery according to (1) or (2), wherein the conductive fold has an extension at the end of the fold, and the extension is bent toward the positive electrode layer.

[0014] In the secondary battery (3), the extension of the conductive fold is folded toward the positive electrode layer, so that the end of the positive electrode layer arranged on the opening side of the insulating fold is surrounded by the insulating porous membrane, making it even less likely that the conductive layer of the long separator and the positive electrode layer will come into contact with each other, and making it even less likely that a short circuit will occur between the positive electrode layer and the negative electrode layer.

[0015] (4) The secondary battery according to any one of (1) to (3), further comprising: a positive electrode terminal electrically connected to the positive electrode layer and at least a portion of which is exposed to the outside; and a negative electrode terminal electrically connected to the negative electrode layer and at least a portion of which is exposed to the outside, the positive electrode terminal and the negative electrode terminal being disposed in a direction perpendicular to the longitudinal direction of the long separator.

[0016] In the secondary battery of (4), the positive electrode terminal and the conductive layer of the long separator are unlikely to come into contact with each other, so that a short circuit between the positive electrode layer and the negative electrode layer is unlikely to occur.

[0017] (5) The secondary battery according to any one of (1) to (4), wherein the negative electrode active material is metallic lithium.

[0018] According to the secondary battery of (5), since the negative electrode active material is metallic lithium, it is possible to increase the capacity.

[0019] (6) A method for manufacturing a secondary battery, comprising: folding a part of a long laminate sheet including an insulating porous membrane and a conductive layer provided on one surface of the insulating porous membrane in a zigzag manner to produce a long separator having an electrode layer accommodating section formed by alternately overlapping an insulating fold folded along the length direction so that the surface on the insulating porous membrane side is on the inside and a conductive fold folded along the length direction so that the surface on the conductive layer side is on the inside, and a first extension portion extending from one end of the electrode layer accommodating section in the length direction; arranging a positive electrode layer on the insulating fold and a negative electrode layer on the conductive fold so that they face each other; and wrapping the first extension portion around an outer surface of the electrode layer accommodating section so that the surface on the insulating porous membrane side is on the outside.

[0020] According to the method for producing a secondary battery of (6), since the method includes a step of winding the first extension part of the long separator around the outer surface of the electrode layer housing part, even if the thickness of the negative electrode layer changes greatly due to charging and discharging, a secondary battery in which the positional deviation between the positive electrode layer and the negative electrode layer is unlikely to occur can be produced industrially advantageously. In addition, since the conductive layer of the long separator is arranged on the negative electrode layer side in the obtained secondary battery, a short circuit caused by dendrites and a decrease in the density of the negative electrode active material layer of the negative electrode layer in the charged state are suppressed. Furthermore, since the insulating porous membrane of the long separator is arranged on the positive electrode layer side in the obtained secondary battery, and the first extension part is wound around the surface of the electrode layer housing part on the insulating porous membrane side on the outside, the conductive layer of the long separator and the positive electrode layer are unlikely to come into contact with each other. Therefore, the obtained secondary battery is unlikely to cause a short circuit between the positive electrode layer and the negative electrode layer.

[0021] (7) A secondary battery comprising: an electrode laminate, an electrolyte, and an exterior body accommodating the electrode laminate and the electrolyte, wherein the electrode laminate has a positive electrode layer, a negative electrode layer, and a long separator, the long separator has an electrode layer accommodating section having two or more folds folded in a zigzag shape along its length, and an extension portion connected to an end portion in the length direction of the electrode layer accommodating section, the positive electrode layer and the negative electrode layer are arranged at each of the folds so as to face each other, and the extension portion is wound around an outer surface of the electrode layer accommodating section.

[0022] According to the secondary battery (7), since the first extension portion is wound around the outer surface of the electrode layer accommodating portion, the positive electrode layer and the negative electrode layer are less likely to become misaligned even if the thickness of the negative electrode layer changes significantly due to charging and discharging. Effect of the Invention

[0023] According to the present invention, it is possible to provide a secondary battery in which the positive electrode layer and the negative electrode layer are unlikely to be misaligned even if the thickness of the negative electrode layer changes significantly due to charging and discharging, and a method for manufacturing the same. In particular, according to the present invention, it is possible to provide a secondary battery in which the positive electrode layer and the negative electrode layer are unlikely to be misaligned and the positive electrode layer and the negative electrode layer are unlikely to be short-circuited, even if a separator having a conductive layer on one surface is used, and a method for manufacturing the same. [Brief description of the drawings]

[0024] [Figure 1] 1 is a perspective view of a secondary battery according to a first embodiment of the present invention; [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 2 is a cross-sectional view taken along line III-III in FIG. [Figure 4] 1 is a cross-sectional view of a separator used in a secondary battery according to a first embodiment of the present invention. [Diagram 5] 2 is a cross-sectional view showing a state in which a positive electrode layer and a negative electrode layer are disposed in an electrode layer receiving portion of a long separator in the production of a secondary battery according to the first embodiment of the present invention. FIG. [Figure 6] FIG. 4 is a cross-sectional view showing a modified example of the secondary battery according to the first embodiment of the present invention. [Figure 7] 13 is a cross-sectional view showing a state in which a positive electrode layer and a negative electrode layer are disposed in an electrode layer receiving portion of a long separator in the production of a secondary battery according to a modified example. FIG. [Figure 8] FIG. 4 is a cross-sectional view of a secondary battery according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Hereinafter, embodiments of the present invention will be described with reference to the drawings. However, the embodiments described below are merely examples of the present invention, and the present invention is not limited to the following.

[0026] [First embodiment] Fig. 1 is a perspective view of a secondary battery according to a first embodiment of the present invention. Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1, and Fig. 3 is a cross-sectional view taken along line III-III in Fig. 1. Fig. 4 is a cross-sectional view of a separator used in the secondary battery according to the first embodiment of the present invention.

[0027] The secondary battery 100 according to this embodiment includes an electrode laminate 10 having a positive electrode layer 20, a negative electrode layer 30, and a long separator 40 disposed between the positive electrode layer 20 and the negative electrode layer 30, an electrolyte (not shown), and an exterior body 50 that contains the electrode laminate 10 and the electrolyte. The positive electrode layer 20 includes a positive electrode current collector 21 and a positive electrode active material layer 22 laminated on both sides of the positive electrode current collector 21. The negative electrode layer 30 includes a negative electrode current collector 31 and a lithium foil 32 laminated on both sides of the negative electrode current collector 31. The secondary battery 100 is a lithium metal secondary battery. A lithium metal secondary battery is a secondary battery that uses metallic lithium as the negative electrode active material. During charging, lithium is released from the positive electrode active material layer 22, and the lithium is precipitated on the surface of the lithium foil 32 to form a metallic lithium layer. For this reason, the thickness of the negative electrode layer 30 increases during charging. On the other hand, during discharge, lithium is released from the metallic lithium layer and is absorbed in the positive electrode active material layer 22. Therefore, the thickness of the negative electrode layer 30 decreases during discharge. Thus, the thickness of the negative electrode layer 30 changes greatly due to charging and discharging. The secondary battery 100 shown in Figures 1 to 3 is in a discharged state.

[0028] The secondary battery 100 further includes a positive electrode terminal 24 and a negative electrode terminal 34 provided on the exterior body 50, a positive electrode lead wire 23 electrically connecting the positive electrode layer 20 (positive electrode current collector 21) and the positive electrode terminal 24, and a negative electrode lead wire 33 electrically connecting the negative electrode layer 30 (negative electrode current collector 31) and the negative electrode terminal 34. A portion of the positive electrode terminal 24 and the negative electrode terminal 34 are exposed to the outside. The positive electrode terminal 24 is disposed along the width direction of the long separator 40 (a direction perpendicular to the length direction of the long separator 40), and the negative electrode terminal 34 is disposed at a position facing each other with the electrode stack 10 in between.

[0029] The long separator 40 has an electrode layer accommodating section 45 formed by alternately folding over insulating folds 43 and conductive folds 44. The insulating folds 43 are folded along the length direction so that the surface on the insulating porous membrane 41 side is on the inside. The insulating folds 43 have a fold tip 43a and an opening 43b located on the opposite side to the tip 43a. The conductive folds 44 are folded along the length direction so that the surface on the conductive layer 42 side is on the inside.

[0030] The long separator 40 has a first extension 46 extending from an upper end of the electrode layer accommodating section 45 in the longitudinal direction, and a second extension 47 extending from a lower end of the electrode layer accommodating section 45 in the longitudinal direction. The first extension 46 is wound around the outer surface of the electrode layer accommodating section 45 with the surface on the insulating porous membrane 41 side facing outward. The number of turns of the first extension 46 is within a range of 1 to 3, for example. The second extension 47 extends so that the surface of the insulating porous membrane 41 comes into contact with the tip 44a of the fold of the conductive fold 44, i.e., the opening 43b of the insulating fold 43.

[0031] The positive electrode layer 20 is disposed on the insulating fold 43, and the negative electrode layer 30 is disposed on the conductive fold 44 so as to face each other. The negative electrode layer 30 contacts the conductive layer 42 of the long separator 40, and the positive electrode layer 20 contacts the insulating porous membrane 41 of the long separator 40.

[0032] The material of the positive electrode collector 21 is not particularly limited, and aluminum, for example, can be used. The material of the positive electrode lead wire 23 may be the same as the material of the positive electrode collector 21, or may be different from the material of the positive electrode collector 21. The positive electrode lead wire 23 may be integrally connected to the positive electrode collector 21. In this embodiment, the positive electrode lead wire 23 is formed by extending the positive electrode collector 21, and is integrally connected to the positive electrode collector 21. The material of the positive electrode terminal 24 may be the same as the material of the positive electrode lead wire 23, or may be different from the material of the positive electrode lead wire 23. The positive electrode terminal 24 may be integrally connected to the positive electrode lead wire 23. In this embodiment, the positive electrode terminal 24 and the positive electrode lead wire 23 are separate members and are electrically connected.

[0033] The positive electrode active material layer 22 includes a positive electrode active material. Examples of the positive electrode active material include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), LiNi p Mn q Co r O2(p+q+r=1), LiNi p Al q Co r O2(p+q+r=1), lithium manganese oxide (LiMn2O4), Li 1+x Mn 2-x-y M y Examples of the positive electrode active material layer 22 include a different element-substituted Li-Mn spinel represented by O4 (x+y=2, M=at least one selected from Al, Mg, Co, Fe, Ni, and Zn), lithium titanate (an oxide containing Li and Ti), and lithium metal phosphate (LiMPO4, M=at least one selected from Fe, Mn, Co, and Ni). The positive electrode active material layer 22 may contain various additives used as materials for positive electrode active material layers, such as a binder and a conductive assistant.

[0034] The material of the negative electrode current collector 31 is not particularly limited, and for example, copper can be used. The material of the negative electrode lead wire 33 may be the same as the material of the negative electrode current collector 31, or may be different from the material of the negative electrode current collector 31. The negative electrode lead wire 33 may be integrally connected to the negative electrode current collector 31. In this embodiment, the negative electrode lead wire 33 is formed by extending the negative electrode current collector 31, and is integrally connected to the negative electrode current collector 31. The material of the negative electrode terminal 34 may be the same as the material of the negative electrode lead wire 33, or may be different from the material of the negative electrode lead wire 33. The negative electrode terminal 34 may be integrally connected to the negative electrode lead wire 33. In this embodiment, the negative electrode terminal 34 and the negative electrode lead wire 33 are separate members and are electrically connected.

[0035] The long separator 40 has an insulating porous membrane 41 and a conductive layer 42 laminated on the surface of the insulating porous membrane 41 on the negative electrode layer 30 side. The conductive layer 42 does not have to be laminated on the entire insulating porous membrane 41. The conductive layer 42 may be laminated so as to cover part of the holes 41a of the insulating porous membrane 41, as shown in FIG.

[0036] As the insulating porous membrane 41, for example, a known one used as a separator for a secondary battery, such as a porous sheet or a nonwoven fabric sheet, can be used. Examples of the material of the porous sheet include polyolefins such as polyethylene and polypropylene, aramid, polyimide, and fluororesin. Examples of the material of the nonwoven fabric sheet include glass fiber and cellulose fiber. The thickness of the insulating porous membrane 41 is not particularly limited, but is preferably 10 μm or more from the viewpoint of blocking dendrites of lithium metal, and is preferably 15 μm or less from the viewpoint of reducing resistance in the battery. The thickness of the insulating porous membrane 41 is more preferably within the range of 10 to 12 μm. In addition, the air permeability of the insulating porous membrane 41 is not particularly limited, but is preferably 200 sec / 100 mL or less from the viewpoint of reducing resistance in the battery, and is more preferably 150 sec / 100 mL or less. The porosity of the insulating porous film 41 is not particularly limited, but from the viewpoints of uniform diffusion of lithium in the long separator 40 and the strength of the long separator 40, it is preferably within the range of 40 to 60%.

[0037] The electrical conductivity of the conductive layer 42 is not particularly limited, but is preferably 1.0×10 1 ~1.0×10 5 The electrical conductivity of the conductive layer 42 is in the range of 1.0×10 1 When the electrical conductivity is 1.0×10 S / cm or more, lithium can be deposited on the surface of the conductive layer 42, and the lithium dendrite can be prevented from growing on the positive electrode layer 20 side and causing a short circuit. 5 By ensuring that the conductivity is equal to or less than S / cm, lithium can be deposited uniformly on the surface of the conductive layer 42.

[0038] In both the discharged and charged states, the conductive layer 42 is in electrical contact with either the negative electrode layer 30 or metallic lithium deposited on the negative electrode layer 30. This makes the potential of the conductive layer 42 and the potential of the negative electrode current collector 31 the same, allowing lithium to be more uniformly deposited between the conductive layer 42 of the long separator 40 and the lithium foil 32.

[0039] The electrical conductivity of the conductive layer 42 may be lower than that of the negative electrode current collector 31, i.e., the electrical conductivity of the negative electrode current collector 31 may be higher than that of the conductive layer 42. By making the electrical conductivity of the negative electrode current collector 31 higher than that of the conductive layer 42, concentrated deposition of lithium on the insulating porous film 41 side of the conductive layer 42 can be prevented, and damage to the conductive layer 42 due to the concentrated deposition of lithium can be suppressed. The electrical conductivity of the conductive layer 42 may be within a range of 1 / 10 to 1 / 100000 of the electrical conductivity of the negative electrode current collector 31, for example.

[0040] The peel strength of the conductive layer 42 to the insulating porous membrane 41 is not particularly limited, but is preferably 10 N / m or more, and more preferably 30 N / m or more. When the peel strength of the conductive layer 42 is as high as the above value, the conductive layer 42 functions stably for a long period of time, and thus the charge / discharge cycle life is extended.

[0041] The surface resistivity of the conductive layer 42 is 200 Ω / cm 2 It may be the following.

[0042] The thickness of the conductive layer 42 may be within a range of 0.01 to 5 μm. When the thickness of the conductive layer 42 is 0.01 μm or more, the above-mentioned effects of the conductive layer 42 can be obtained. When the thickness of the conductive layer 42 is 5 μm or less, the decrease in energy density due to the conductive layer 42 can be reduced.

[0043] The conductive layer 42 may be made of a conductive material such as a metal or carbon nanotube (CNT). Examples of metals include Cu, Zn, Ti, and Sn. These conductive materials may be used alone or in combination of two or more.

[0044] The coating method for forming the conductive layer 42 on the insulating porous film 41 is not particularly limited, and for example, a sputtering method or a coating method can be used. As the sputtering method, a DC sputtering method or an RF sputtering method can be used. The coating method is a method in which a coating liquid in which the material of the conductive layer 42 is dispersed is applied to the surface of the insulating porous film 41 and dried.

[0045] The electrolytic solution includes an organic solvent and an electrolyte. Examples of the organic solvent include cyclic carbonates, chain carbonates, cyclic ethers, chain ethers, hydrofluoroethers, aromatic ethers, sulfones, cyclic esters, chain carboxylates, and nitriles. Examples of the cyclic carbonates include ethylene carbonate, propylene carbonate, vinylene carbonate, and fluoroethylene carbonate. Examples of the chain carbonates include dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. Examples of the cyclic ethers include tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, and 4-methyl1,3-dioxolane. Examples of the chain ethers include 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, and diethyl ether. Examples of hydrofluoroethers include 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis(2,2,2-trifluoroethyl)ether, 1,2-bis(1,1,2,2-tetrafluoroethoxy)ethane, and the like. Examples of aromatic ethers include anisole. Examples of sulfones include sulfolane and methylsulfolane. Examples of cyclic esters include γ-butyrolactone, and the like. Examples of chain carboxylates include acetates, butyrates, and propionates. Examples of nitriles include acetonitrile and propionitrile. The organic solvents may be used alone or in combination of two or more.

[0046] The electrolyte is a source of lithium ions, which are charge transfer media, and contains a lithium salt. Examples of the lithium salt include LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC(CF3SO2)3, LiN(CF3SO2)2(LiTFSI), LiN(FSO2)2(LiFSI), and LiBC4O8. The lithium salt may be used alone or in combination of two or more. The concentration of the electrolyte is, for example, within the range of 1.5 to 4.0 mol / L.

[0047] The exterior body 50 is expandable and contractable in accordance with changes in the thickness of the electrode laminate 10 (particularly changes in the thickness of the negative electrode layer 30) due to charging and discharging. A laminate film can be used as the material of the exterior body 50. A laminate film having a three-layer structure in which an inner resin layer, a metal layer, and an outer resin layer are laminated in this order from the inside can be used as the laminate film. Thermoplastic resins such as polyethylene terephthalate (PET), polyamide (nylon), and polypropylene (PP) can be used as the material of the inner resin layer and the outer resin layer. Aluminum can be used as the material of the metal layer, for example.

[0048] Next, a method for manufacturing the secondary battery 100 of this embodiment will be described. The electrode stack 10 can be produced, for example, by a method including a long separator producing step, an electrode layer arranging step, and a long separator winding step.

[0049] The long separator preparation step is a step of preparing a long separator 40 having an electrode layer accommodating portion 45, a first extending portion 46, and a second extending portion 47. The long separator 40 can be prepared by zigzag folding of a central portion of a long laminated sheet including an insulating porous membrane 41 and a conductive layer 42 provided on one surface of the insulating porous membrane 41 to form an insulating fold 43 folded along the length direction so that the surface on the insulating porous membrane 41 side faces inward, and a conductive fold 44 folded along the length direction so that the surface on the conductive layer 42 side faces inward, which are alternately folded over each other.

[0050] The electrode layer arrangement step is a step of arranging the positive electrode layer 20 on the insulating fold 43 and the negative electrode layer 30 on the conductive fold 44 so that they face each other. The positive electrode layer 20 can be arranged by inserting the positive electrode layer 20 through the opening 43b of the insulating fold 43. The negative electrode layer 30 can be arranged by inserting the negative electrode layer 30 through the opening 44b of the conductive fold 44. The long separator production step and the electrode layer arrangement step may be carried out in parallel. For example, after arranging the positive electrode layer 20 on the surface of the insulating porous membrane 41 side of the long laminated sheet, the long laminated sheet may be folded along the length direction so that the surface on the insulating porous membrane 41 side is on the inside, and then the negative electrode layer 30 may be arranged on the surface on the conductive layer 42 side, and then the long laminated sheet may be folded along the length direction so that the surface on the conductive layer 42 side is on the inside.

[0051] 5 is a cross-sectional view showing a state in which a positive electrode layer and a negative electrode layer are arranged in an electrode layer accommodating portion of a long separator of this embodiment. The portion of the long separator 40 that will become the second extension portion 47 is fixed by a chuck 60. The positive electrode layer 20 and the negative electrode layer 30 are arranged alternately in the electrode layer accommodating portion 45 formed by zigzag folding. The positive electrode layer 20 is arranged in the insulating fold 43 of the electrode layer accommodating portion 45, and the negative electrode layer 30 is arranged in the conductive fold 44. The end of the electrode layer accommodating portion 45 is a portion that will become the first extension portion 46.

[0052] The long separator winding process is a process of winding the first extension portion 46 around the outer surface of the electrode layer accommodating portion 45 of the long separator 40 so that the surface on the insulating porous membrane 41 side is on the outer side. In the case of the long separator shown in FIG. 5, the first extension portion 46 is wound around the outer surface of the electrode layer accommodating portion 45 so that the conductive layer 42 is on the inner side (clockwise in FIG. 5). When winding the first extension portion 46, the chuck 60 is removed, and the first extension portion 46 and the second extension portion 47 are overlapped so that the conductive layer 42 of the first extension portion 46 and the conductive layer 42 of the second extension portion 47 are in contact with each other. By doing so, the surface of the insulating porous membrane 41 of the second extension portion 47 is in contact with the opening 43b of the insulating fold 43 where the positive electrode layer 20 is arranged. Prior to the long separator winding step, the second extending portion of the long separator 40 may be arranged so that the surface on the insulating porous membrane 41 side comes into contact with the tip of the conductive fold 44 .

[0053] The secondary battery 100 can be produced as follows: A positive electrode terminal 24 is connected to the positive electrode current collector 21 of the positive electrode layer 20 of the obtained electrode laminate 10 via a positive electrode lead wire 23, and a negative electrode terminal 34 is connected to the negative electrode current collector 31 of the negative electrode layer 30 via a negative electrode lead wire 33. Next, the electrode laminate 10 is housed in an exterior body 50 so that parts of the positive electrode terminal 24 and the negative electrode terminal 34 protrude, and after an electrolyte is poured in, the exterior body 50 is sealed.

[0054] According to the secondary battery 100 of the present embodiment configured as described above, since the first extension portion 46 of the long separator 40 is wound around the outer surface of the electrode layer housing portion 45, even if the thickness of the negative electrode layer 30 changes significantly due to charging and discharging, the positive electrode layer 20 and the negative electrode layer 30 are unlikely to be misaligned. In addition, since the conductive layer 42 of the long separator 40 is disposed on the negative electrode layer 30 side, short circuits caused by dendrites and a decrease in the density of the negative electrode active material layer of the negative electrode layer 30 in the charged state are suppressed. Since the insulating porous membrane 41 of the long separator 40 is disposed on the positive electrode layer 20 side, and the first extension portion 46 is wound around the electrode layer housing portion 45 with the surface on the insulating porous membrane 41 side facing outward, the conductive layer 42 of the long separator 40 and the positive electrode layer 20 are unlikely to come into contact with each other. Therefore, a short circuit between the positive electrode layer 20 and the negative electrode layer 30 is unlikely to occur.

[0055] Furthermore, according to the secondary battery 100 of this embodiment, the second extension portion 47 contacts the tip 44a of the conductive fold 44, i.e., the opening 43b of the insulating fold 43, with the surface of the insulating porous membrane 41, making it more difficult for the conductive layer 42 and the positive electrode layer 20 to come into contact with each other, and making it more difficult for a short circuit to occur between the positive electrode layer 20 and the negative electrode layer 30. Note that, as long as the opening 43b of the insulating fold 43 is not in contact with the conductive layer, it is not necessary to extend the second extension portion 47 so that the tip 44a of the conductive fold 44 contacts the surface of the insulating porous membrane 41.

[0056] Furthermore, according to the secondary battery 100 of this embodiment, the positive electrode terminal 24 is disposed in a direction perpendicular to the longitudinal direction of the long separator 40, so that the positive electrode terminal 24 is unlikely to come into contact with the conductive layer 42. As a result, a short circuit between the positive electrode layer 20 and the negative electrode layer 30 is unlikely to occur. In the secondary battery 100 of this embodiment, the negative electrode active material is metallic lithium, and even if the thickness of the negative electrode layer changes significantly due to charging and discharging, the positive electrode layer and the negative electrode layer are unlikely to be misaligned, making it possible to achieve a high capacity.

[0057] Moreover, according to the method for producing the secondary battery 100 of this embodiment, the above-mentioned secondary battery 100 can be produced industrially advantageously.

[0058] In the secondary battery 100 of this embodiment, the folds of the electrode layer accommodating portion 45 of the long separator 40 are equally spaced, and the distance from the tip 43a of the insulating fold 43 to the opening 43b is the same as the distance from the tip 44a of the conductive fold 44 to the opening 44b. The folds of the electrode layer accommodating portion 45 are not limited to being equally spaced. For example, the distance from the tip 44a of the conductive fold 44 to the opening 44b may be extended to be longer than the distance from the tip 43a of the insulating fold 43 to the opening 43b. An example of a secondary battery in which the tip 44a of the conductive fold 44 is extended will be described.

[0059] FIG. 6 is a cross-sectional view showing a modified example of the secondary battery according to the first embodiment of the present invention, and corresponds to the cross-sectional view shown in FIG. 6 is the same as the secondary battery 100 described above, except that it has an extension 44c that is an extension of the folded tip 44a of the conductive fold 44. For this reason, the same components as those in the secondary battery 100 are denoted by the same reference numerals and detailed description thereof will be omitted.

[0060] The extension 44c of the conductive fold 44 is folded toward the opening 43b of the insulating fold 43 (the positive electrode layer 20 side) along the tip side of the longitudinal direction of the first extension. The outer side of the extension 44c of the conductive fold 44 is the insulating porous membrane 41. Therefore, by folding the extension 44c of the conductive fold 44 toward the positive electrode layer 20 side, the end of the positive electrode layer 20 arranged on the insulating fold 43 is surrounded by the insulating porous membrane 41, so that the conductive layer 42 of the long separator 40 and the positive electrode layer 20 are even less likely to come into contact with each other. Therefore, a short circuit between the positive electrode layer 20 and the negative electrode layer 30 is less likely to occur.

[0061] The secondary battery 101 can be manufactured by zigzag folding in the long separator manufacturing process so that the conductive fold 44 is longer than the insulating fold 43. FIG. 7 is a cross-sectional view showing a state in which a positive electrode layer and a negative electrode layer are arranged in an electrode layer accommodating portion of a long separator of a modified example. The portion of the long separator 40 that becomes the second extension portion 47 is fixed by a chuck 60. The positive electrode layer 20 is arranged in the insulating fold 43 of the electrode layer accommodating portion 45 formed by zigzag folding, and the negative electrode layer 30 is arranged in the conductive fold 44. The tip 44a of the conductive fold 44 is the extension portion 44c. The negative electrode layer 30 is not arranged in the extension portion 44c, and it can be folded. The tip of the electrode layer accommodating portion 45 is the portion that becomes the first extension portion 46. In the long separator winding process, the first extending portion 46 is wound (clockwise in FIG. 7 ) so that the conductive layer 42 is on the inside with respect to the outer surface of the electrode layer accommodating portion 45. When the first extending portion 46 is wound, the extension portion 44c of the conductive fold 44 is folded toward the opening 43b of the insulating fold 43.

[0062] In the modified secondary battery 101, the end of the positive electrode layer 20 is surrounded by the insulating porous membrane 41 by the extension portion 44c of the conductive fold 44, so compared to the secondary battery 100 of the above-mentioned embodiment in which the end of the positive electrode layer 20 is surrounded by the insulating porous membrane 41 by the second extension portion 47, the second extension portion 47 may be shortened or the second extension portion 47 may be omitted.

[0063] [Second embodiment] FIG. 8 is a cross-sectional view of a secondary battery according to a second embodiment of the present invention, which corresponds to the cross-sectional view of the secondary battery according to the first embodiment shown in FIG. The secondary battery 200 of this embodiment is the same as the secondary battery 100 of the first embodiment, except that the long separator 40 does not have a conductive layer. Therefore, the same components as those of the secondary battery 100 are denoted by the same reference numerals and detailed description thereof will be omitted.

[0064] In the secondary battery 200 of this embodiment, the electrode layer accommodating portion 45 of the long separator 40 has a fold that is zigzag folded along the length direction, and the positive electrode layer 20 and the negative electrode layer 30 are arranged to face each other at each fold. The first extension portion 46 is wound around the outer surface of the electrode layer accommodating portion 45. The second extension portion 47 extends so as to contact the opening of the fold in which the positive electrode layer 20 is arranged.

[0065] In the secondary battery 200 of this embodiment, the first extension portion 46 of the long separator 40 is wound around the outer surface of the electrode layer accommodating portion 45, so that, similar to the secondary battery 100 of the first embodiment, even if there is a large change in the thickness of the negative electrode layer 30 due to charging and discharging, the positive electrode layer 20 and the negative electrode layer 30 are less likely to become misaligned.

[0066] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments and can be modified as appropriate. For example, in the secondary battery of this embodiment, the negative electrode layer 30 uses a metallic lithium layer deposited during charging as the negative electrode active material layer, but the negative electrode active material layer is not limited thereto. As the negative electrode active material layer, a layer containing a negative electrode active material that absorbs lithium during charging and releases lithium during discharging may be used. As the negative electrode active material, lithium transition metal oxides such as lithium titanate, transition metal oxides such as TiO2, Nb2O3 and WO3, SiO, metal sulfides, metal nitrides, and carbon materials such as artificial graphite, natural graphite, graphite, soft carbon and hard carbon can be used. In addition, as the negative electrode active material, a metal that forms an alloy with lithium can be used. A metal that forms an alloy with lithium can be used. Examples of metals that form an alloy with lithium include Mg, Si, Au, Ag, In, Ge, Sn, Pb, Al and Zn.

[0067] [Experimental Example] The effect of a secondary battery in which a laminate in which a conductive layer is laminated on the surface of a porous membrane is used as a separator and the conductive layer is arranged on the negative electrode layer side will be described with reference to an experimental example.

[0068] [Experimental Example 1] (Preparation of separator) A porous membrane (film thickness: 20 μm, porosity: 58%, air permeability: 92 sec / 100 mL) was prepared. A copper conductive layer with a thickness of 0.08 μm was formed on one surface of the porous membrane by RF sputtering. The porous membrane with the copper conductive layer formed thereon was punched out to a size of 40 mm × 50 mm to prepare a separator.

[0069] (Preparation of positive electrode layer) Acetylene black (AB) as an electron conductive material, polyvinylidene fluoride (PVDF) as a binder, and polyvinylpyrrolidone (PVP) as a dispersant were premixed with N-methyl-2-pyrrolidone (NMP) as a dispersion solvent, and wet-mixed in a planetary centrifugal mixer to obtain a premixed slurry. 0.8 Co 0.1 Mn 0.1O2 (NCM811) and the pre-dope material were mixed with the obtained premixed slurry, and a dispersion process was performed using a planetary mixer to obtain a positive electrode active material paste. NCM811 has a median diameter of 12 μm. Next, the obtained positive electrode active material paste was applied to an aluminum positive electrode collector not having a primer layer, dried, pressed with a roll press, and then dried in a vacuum at 120 ° C. to form a positive electrode plate having a positive electrode active material layer. The obtained positive electrode plate was punched out to a size of 30 mm × 40 mm to form a positive electrode layer.

[0070] (Preparation of negative electrode layer) Copper foil with a thickness of 10 μm (electrical conductivity: 6.5 × 10 6 A clad material was prepared by bonding a 20 μm-thick lithium foil and a 100 μm-thick ... lithium foil. This clad material was punched out to a size of 34 mm × 44 mm to prepare a negative electrode current collector.

[0071] (electrolyte) An electrolyte was prepared by dissolving LiFSI in 1,2-dimethoxyethane (DME) at a concentration of 4 mol / L.

[0072] (Preparation of lithium metal secondary batteries) A copper conductive layer of a separator was laminated on the lithium foil side of the negative electrode current collector, and a positive electrode active material layer of a positive electrode layer was laminated on the surface opposite to the copper conductive layer of the separator to produce an electrode laminate in which the negative electrode layer, separator, and positive electrode layer were laminated in this order. Next, a positive electrode terminal was attached to the positive electrode current collector of the obtained electrode laminate via a positive electrode lead wire, and a negative electrode terminal was attached to the copper foil of the negative electrode current collector via a negative electrode lead wire. The laminate with the positive electrode terminal and negative electrode terminal attached was placed in a laminate film bag, and then an electrolyte was added, and the laminate film bag was sealed to produce a lithium metal secondary battery.

[0073] [Experimental Example 2] A lithium metal secondary battery was produced in the same manner as in Experimental Example 1, except that in the production of the separator, a zinc conductive layer having a thickness of 0.06 μm was formed by RF sputtering instead of the copper conductive layer.

[0074] [Experimental Example 3] A lithium metal secondary battery was produced in the same manner as in Experimental Example 1, except that a carbon nanotube (CNT) conductive layer having a thickness of 2.1 μm was formed by a coating method in place of the copper conductive layer in the production of the separator. The carbon nanotube conductive layer was formed as follows. First, carbon nanotubes were added in an amount such that the solid content concentration was 4 mass% using N-methyl-N-pyrrolidinone (NMP) as a solvent, and PVDF (#9300, manufactured by Kureha Corporation) was added as a binder in an amount of 5 mass parts per 95 mass parts of carbon nanotubes. Next, a dispersion treatment was performed for 10 minutes using a rotation / revolution mixer at 1000 rpm to prepare a coating liquid. The obtained coating liquid was applied to the surface of the porous membrane using a doctor blade and dried.

[0075] [Experimental Example 4] A lithium metal secondary battery was produced in the same manner as in Experimental Example 1, except that in the production of the separator, a tin conductive layer having a thickness of 0.06 μm was formed by RF sputtering instead of the copper conductive layer.

[0076] [Comparative Experiment Example 1] A lithium metal secondary battery was produced in the same manner as in Experimental Example 1, except that in the production of the separator, no copper conductive layer was formed.

[0077] [evaluation] The electrical conductivity, surface resistivity, and peel strength of the conductive layer of the separator prepared in each experiment were measured by the following methods. The results are shown in Table 1 together with the material, coating method, and thickness of the conductive layer of the separator. The lithium metal secondary batteries fabricated in each of the experimental examples and comparative experimental examples were measured for the presence or absence of short circuits and the rate of lithium thickness increase by the following methods. The results are shown in Table 1.

[0078] (Electrical conductivity and surface resistivity of conductive layer) The electrical conductivity and surface resistivity were measured using a high-precision, high-performance resistivity meter (Nitto Seiko Analytech Co., Ltd., Loresta GP TCP-600).

[0079] (peel strength) A conductive layer 5.0 cm long and 2.5 cm wide was attached to a 2.5 cm wide adhesive tape that was attached to a fixed plate. One end of the conductive layer was then folded back 180 degrees and pulled up at a speed of 300 mm / min using an electric measuring stand (manufactured by Imada Co., Ltd.) to peel the conductive layer from the porous film. The load required from the start of peeling the conductive layer to the end of peeling was measured using a digital force gauge (manufactured by Imada Co., Ltd.). The average value of the load obtained was divided by the width of the adhesive tape to obtain the peel strength.

[0080] (Whether or not there is a short circuit in the lithium metal secondary battery) The lithium metal secondary battery immediately after fabrication was left to stand at a measurement temperature of 25° C. for 24 hours. After leaving the lithium metal secondary battery stationary, the first charge / discharge cycle described below was performed for three cycles, and then the second charge / discharge cycle described below was performed for 50 cycles to check whether or not the lithium metal secondary battery had a short circuit. If the charge capacity of the lithium metal secondary battery was 105% or more of the discharge capacity before charging, it was deemed that a short circuit had occurred, and it was deemed that a short circuit had occurred.

[0081] (First charge / discharge cycle) The charging was performed under the conditions of constant current charging at a current value of 2.2 mA up to 4,300 V, followed by constant voltage charging for 60 minutes at a voltage value of 4,300 V. The discharging was performed under the conditions of constant current discharging at a current value of 4 mA down to 2.65 V. The battery was left to stand for 30 minutes between discharging and charging.

[0082] (2nd charge / discharge cycle) The charging conditions were constant current charging at 74 mA to 3.823 V, 52 mA to 4.051 V, 46 mA to 4.173 V, and 22 mA to 4.300 V, followed by constant voltage charging for 90 minutes at 4.300 V. The discharging conditions were constant current discharging at 18 mA to 2.65 V. The battery was left to stand for 30 minutes between discharging and charging.

[0083] (Lithium thickness increase rate in lithium metal secondary batteries) The thickness T1 (μm) of the negative electrode layer at the initial charge and the thickness T2 (μm) of the negative electrode layer (total thickness of the negative electrode current collector and metallic lithium layer) at the charge after 50 cycles were measured, and the lithium thickness increase rate T (μm / cycle) was calculated using the following formula. T(μm / cycle)=(T2-T1) / 50

[0084] The thickness T1 (μm) of the negative electrode layer during the initial charge was measured as follows. The lithium metal secondary battery immediately after fabrication was left to stand at a measurement temperature of 25° C. for 24 hours. The lithium metal secondary battery after standing was subjected to the first charge / discharge cycle for three cycles. Next, constant current charging was performed at a current value of 14.7 mA up to 4,300 V, followed by constant voltage charging at a voltage value of 4,300 V for 60 minutes to charge the lithium metal secondary battery. The charged lithium metal secondary battery was left standing for 30 minutes, disassembled, and the negative electrode layer was taken out and its thickness was measured as the thickness T1 of the negative electrode layer.

[0085] The thickness T2 of the negative electrode layer during charging after 50 cycles was measured as follows. The lithium metal secondary battery immediately after fabrication was left to stand at a measurement temperature of 25° C. for 24 hours. The lithium metal secondary battery after standing was subjected to the first charge / discharge cycle three cycles, and then the second charge / discharge cycle 50 cycles. The lithium metal secondary battery was then charged by performing a constant current charge to 4.300 V at a current value of 14.7 mA, followed by a constant voltage charge at a voltage value of 4.300 V for 60 minutes. The charged lithium metal secondary battery was then left to stand for 30 minutes, disassembled, and the negative electrode layer was removed and its thickness was measured as the thickness T2 of the negative electrode layer.

[0086] [Table 1]

[0087] As shown in Table 1, the lithium metal secondary batteries of Experimental Examples 1 to 4, which are equipped with separators having conductive layers, are less likely to short-circuit even when repeatedly charged and discharged, have a low rate of lithium thickness increase, and produce a metallic lithium layer (negative electrode active material layer) that is dense and has high density when charged. In contrast, the lithium metal secondary battery of Comparative Experimental Example 1, which is equipped with a separator without a conductive layer, is more likely to short-circuit when repeatedly charged and discharged, and has a high rate of lithium thickness increase, which shows that a coarse and low-density negative electrode active material layer is produced when charged. [Explanation of symbols]

[0088] 10 Electrode laminate 20 Positive electrode layer 21 Positive electrode current collector 22 Cathode active material layer 23 Positive lead wire 24 Positive terminal 30 Negative electrode layer 31 Negative electrode current collector 32 Lithium foil 33 Negative lead wire 34 Negative terminal 40 Long separator 41 Insulating porous membrane 41a Hole 42 Conductive layer 43 Insulating wrap 43a Tip 43b opening 44 Conductive wrap 44a Tip 44b opening 44c extension 45 Electrode layer housing 46 1st extension part 47 Second extension part 50 Exterior body 60 Chuck 100, 101, 200 secondary battery

Claims

1. The battery includes an electrode stack, an electrolyte solution, and an exterior body that accommodates the electrode stack and the electrolyte solution, the electrode stack includes a positive electrode layer, a negative electrode layer, and a long separator; The long separator includes an insulating porous membrane and a conductive layer provided on one surface of the insulating porous membrane, The long separator has an electrode layer accommodating section formed by alternately overlapping insulating folds folded along the length direction so that the surface on the insulating porous membrane side faces inward and conductive folds folded along the length direction so that the surface on the conductive layer side faces inward, and a first extension section extending from one end of the electrode layer accommodating section in the length direction, the positive electrode layer is disposed on the insulating fold and the negative electrode layer is disposed on the conductive fold so as to face each other; The secondary battery, wherein the first extending portion is wound around the outer surface of the electrode layer accommodating portion so that the surface on the insulating porous membrane side faces outward.

2. a second extension portion extending from the other end of the electrode layer accommodating portion in the longitudinal direction; The secondary battery according to claim 1 , wherein the second extension portion extends so that a tip of the conductive folded portion contacts a surface of the insulating porous film.

3. The conductive fold has an extension portion at the tip of the fold, The secondary battery according to claim 1 , wherein the extension is bent toward the positive electrode layer.

4. a positive electrode terminal electrically connected to the positive electrode layer and at least a portion of which is exposed to the outside; a negative electrode terminal electrically connected to the negative electrode layer and at least a portion of which is exposed to the outside, The secondary battery according to claim 1 , wherein the positive electrode terminal and the negative electrode terminal are arranged along a direction perpendicular to the longitudinal direction of the long separator.

5. The secondary battery according to claim 1 , wherein the negative electrode active material is metallic lithium.

6. a process of zigzag folding a portion of a long laminate sheet including an insulating porous membrane and a conductive layer provided on one surface of the insulating porous membrane, to produce a long separator having an electrode layer accommodating section formed by alternately overlapping insulating folds folded along the length direction so that the surface on the insulating porous membrane side faces inward and conductive folds folded along the length direction so that the surface on the conductive layer side faces inward, and a first extension section extending from one end of the electrode layer accommodating section in the length direction; disposing a positive electrode layer on the insulating fold and a negative electrode layer on the conductive fold so that they face each other; and winding the first extension portion around an outer surface of the electrode layer accommodating portion so that the surface on the insulating porous membrane side faces outward.

7. The battery includes an electrode stack, an electrolyte solution, and an exterior body that accommodates the electrode stack and the electrolyte solution, the electrode stack includes a positive electrode layer, a negative electrode layer, and a long separator; the long separator has an electrode layer accommodating portion having two or more zigzag folds along the length direction, and an extension portion connected to an end portion in the length direction of the electrode layer accommodating portion, the positive electrode layer and the negative electrode layer are disposed at each of the folds so as to face each other, The extension portion is wound around the outer surface of the electrode layer accommodating portion.

Citation Information

Patent Citations

  • Diaphragm and preparation method thereof and lithium ion battery

    CN108630867A

  • Electric storage device and method of manufacturing the same

    JP2010199281A

  • Power storage device and vehicle

    JP2013182819A

  • Nonaqueous electrolyte secondary battery

    JP2015153690A

  • Zigzag lamination body structure for secondary battery

    JP2016103425A