Electrode composition for lithium ion battery
The electrode composition for lithium-ion batteries, using an alkylene oxide adduct of a phenol compound as a dispersant, addresses the decomposition issues of polyvinylpyrrolidone, enhancing electrical performance and capacity retention.
Patent Information
- Application Number
- JP2024045910
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-03-22
AI Technical Summary
Existing lithium-ion battery electrode compositions face challenges in achieving high capacity and performance due to the use of dispersants like polyvinylpyrrolidone, which can cause decomposition reactions, leading to decreased battery performance.
An electrode composition for lithium-ion batteries comprising an electrode active material, binder resin, and conductive aid, with a dispersant that is an alkylene oxide adduct of a phenol compound, having specific weight ratios and characteristics to enhance dispersibility and stability, including a dispersant with a carbon and hydrogen ratio of 55% by weight or less and a weight ratio of electrode active material between 78 to 97% based on the solid weight of the composition.
The proposed composition results in electrodes with improved electrical resistance, coulombic efficiency, and capacity retention, balancing strength, conductivity, and capacity.
Smart Images

Figure 2024144262000001 
Figure 2024144262000002 
Figure 2024144262000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode composition for a lithium ion battery. [Background technology]
[0002] Lithium-ion batteries, which have the characteristics of high voltage and high energy density, are widely used in the field of portable information devices, and have established their position as the standard battery for portable terminals such as mobile phones and notebook computers. While their uses are expanding, their application to hybrid vehicles and electric vehicles, in addition to the conventional applications, is being considered, and some have already been put into practical use. In order to further popularize these, secondary batteries with higher capacity and higher output are required, and the application of various technologies is being attempted.
[0003] To increase the capacity of lithium-ion batteries, it is necessary to increase the proportion of active material in the electrodes, and it is preferable to use less of the other components such as binder resin, conductive additives, etc. However, simply reducing the amount of these components used will not ensure the strength and electronic conductivity of the resulting electrode, resulting in a deterioration of battery performance, and therefore additives (mainly dispersants) that can reduce the amount of binder resin, conductive additives, etc. used while maintaining battery performance have been investigated.
[0004] For example, Patent Document 1 uses methyl cellulose, polyvinylpyrrolidone, polyvinyl alcohol, etc. as polymer-based dispersants. However, these dispersants, particularly polyvinylpyrrolidone, themselves undergo a decomposition reaction in the positive electrode potential range (3 to 5 V), raising concerns that this may degrade battery performance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2014-181140 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in view of the above-mentioned circumstances, and has an object to provide an electrode composition for a lithium ion battery, which can provide an electrode for a lithium ion battery having excellent cell performance (electrical resistance value, coulombic efficiency, capacity retention rate). [Means for solving the problem]
[0007] As a result of extensive investigations, the present inventors arrived at the present invention. The present invention is an electrode composition for lithium ion batteries, comprising an electrode active material, a binder resin, a conductive assistant, and a dispersant, the dispersant being an alkylene oxide adduct of a phenol compound, the total weight ratio of carbon atoms constituting an aromatic ring skeleton in the dispersant and hydrogen atoms bonded to the carbon atoms being 55% by weight or less based on the weight of the dispersant, the weight ratio of the electrode active material being 78 to 97% by weight based on the solid content weight of the electrode composition for lithium ion batteries, the weight ratio of the binder resin being 1 to 20% by weight based on the solid content weight of the electrode composition for lithium ion batteries, the weight ratio of the conductive assistant being 1 to 5% by weight based on the solid content weight of the electrode composition for lithium ion batteries, and the weight ratio of the dispersant being 2 to 20% by weight based on the weight of the conductive assistant. Effect of the Invention
[0008] According to the present invention, it is possible to provide an electrode composition for a lithium ion battery that can provide an electrode for a lithium ion battery having excellent cell performance (electrical resistance value, coulombic efficiency, capacity retention rate). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The lithium ion battery electrode composition of the present invention is an electrode composition for lithium ion batteries that contains an electrode active material, a binder resin, a conductive assistant, and a dispersant. The lithium ion battery electrode composition of the present invention contains an electrode active material. The electrode active material may be a positive electrode active material or a negative electrode active material. When the electrode active material is a positive electrode active material, the electrode composition for lithium ion batteries of the present invention can be used as a positive electrode composition for lithium ion batteries, and when the electrode active material is a negative electrode active material, the electrode composition for lithium ion batteries of the present invention can be used as a negative electrode composition for lithium ion batteries.
[0010] There are no particular limitations on the positive electrode active material as long as it can be used as a positive electrode active material for a lithium ion battery. For example, composite oxides of lithium and transition metals {composite oxides containing one type of transition metal (e.g., LiCoO2, LiNiO2, LiAlMnO4, LiMnO2, and LiMn2O4), composite oxides containing two types of transition metal elements (e.g., LiFeMnO4, LiNi 1-x Co x O2, LiMn 1-y Co y O2, LiNi 1 / 3 Co 1 / 3 Al 1 / 3 O2 and LiNi 0.8 Co 0.15 Al 0.05 O2) and composite oxides containing three or more metal elements [e.g. LiM a M' b M'' c O2(M, M' and M'' are different transition metal elements and satisfy a+b+c=1. For example, LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 Examples of the conductive polymer include lithium-containing transition metal phosphates (e.g., LiFePO4, LiCoPO4, LiMnPO4, and LiNiPO4), transition metal oxides (e.g., MnO2 and V2O5), transition metal sulfides (e.g., MoS2 and TiS2), and conductive polymers (e.g., polyaniline, polypyrrole, polythiophene, polyacetylene, poly-p-phenylene, and polyvinylcarbazole), and two or more of these may be used in combination. The lithium-containing transition metal phosphate may have some of the transition metal sites substituted with other transition metals.
[0011] From the viewpoint of the electrical characteristics of the battery, the volume average particle diameter of the positive electrode active material is preferably 0.01 to 100 μm, more preferably 0.1 to 35 μm, and even more preferably 2 to 30 μm.
[0012] In this specification, the volume average particle size refers to the particle size (Dv50) at an integrated value of 50% in the particle size distribution determined by the Microtrack method (laser diffraction / scattering method). The Microtrack method is a method for determining the particle size distribution by utilizing scattered light obtained by irradiating particles with laser light. The volume average particle size can be measured using a Microtrack manufactured by Nikkiso Co., Ltd.
[0013] The negative electrode active material is not particularly limited as long as it can be used as a negative electrode active material for a lithium ion battery. Examples of materials constituting the negative electrode active material include carbon-based materials and silicon-based materials. Among them, it is preferable that the negative electrode active material is made of a carbon-based material.
[0014] Examples of carbon-based materials include graphite, non-graphitizable carbon, amorphous carbon, resin sinters (e.g., phenolic resins and furan resins sintered and carbonized), and cokes (e.g., pitch coke, needle coke, and petroleum coke). The material may be a mixture of a carbon-based material and a conductive polymer (e.g., polyacetylene and polypyrrole), a metal oxide (titanium oxide and lithium-titanium oxide), and a metal alloy (lithium-tin alloy, lithium-aluminum alloy, aluminum-manganese alloy, etc.). Materials that do not contain lithium or lithium ions inside may be subjected to a pre-doping process to include lithium or lithium ions in a part or all of the inside.
[0015] Examples of silicon-based materials include silicon oxide (SiO x ), a Si-C composite, a Si-Al alloy, a Si-Li alloy, a Si-Ni alloy, a Si-Fe alloy, a Si-Ti alloy, a Si-Mn alloy, a Si-Cu alloy, and a Si-Sn alloy. Examples of Si-C composites include silicon carbide and carbon particles whose surfaces are coated with silicon and / or silicon carbide, as well as silicon particles and silicon oxide particles whose surfaces are coated with carbon and / or silicon carbide. The particles made of silicon-based materials may be single particles (also called primary particles), or may form composite particles obtained by agglomeration of primary particles (i.e., secondary particles obtained by agglomeration of primary particles made of silicon-based materials). Composite particles may be formed when primary particles of particles made of silicon-based materials are aggregated by their adsorptive power, or when primary particles are aggregated by adsorption via other materials. As a method for forming composite particles by binding primary particles via other materials, for example, a method of mixing primary particles of particles made of silicon-based materials with a polymer compound constituting a coating film may be mentioned.
[0016] From the viewpoint of the electrical characteristics of the battery, the volume average particle diameter of the negative electrode active material is preferably 0.1 to 100 μm, more preferably 1 to 50 μm, and even more preferably 2 to 20 μm.
[0017] The lithium ion battery electrode composition of the present invention contains a binder resin. The binder resin is not particularly limited as long as it is a resin having a binder function (adhesive strength). Examples of the binder resin include starch, polyvinylidene fluoride (PVdF), polyvinyl alcohol, polyvinylpyrrolidone, polytetrafluoroethylene, tetrafluoroethylene, polyacrylic acid, sodium polyacrylate, polyacrylic acid ester, polymethacrylic acid ester, styrene-butadiene rubber (SBR), polyethylene, and polypropylene. The binder resin broadly includes a thickener, and an example of the thickener is carboxymethyl cellulose (CMC).
[0018] The lithium ion battery electrode composition of the present invention contains a conductive assistant. The conductive assistant is not particularly limited as long as it is a material having electrical conductivity. Examples of conductive assistants include metals [aluminum, stainless steel (SUS), silver, gold, copper, titanium, etc.], carbon [graphite (flaky graphite (UP)), carbon black (acetylene black, ketjen black, furnace black, channel black, thermal lamp black, etc.), carbon nanofibers (CNF), carbon nanotubes (CNT), etc.], and mixtures thereof. These conductive assistants may be used alone or in combination of two or more. In addition, alloys or metal oxides of these may be used. From the viewpoint of electrical stability, acetylene black is preferred.
[0019] In addition, carbon-based materials are used both as negative electrode active materials and conductive assistants, but in this application, those with a volume average particle diameter of 15 μm or more are considered to be negative electrode active materials, and those with a volume average particle diameter of less than 15 μm are considered to be conductive assistants.
[0020] The lithium ion battery electrode composition of the present invention contains a dispersant. The dispersant is an alkylene oxide adduct of a phenol compound. Examples of the phenol compound include monocyclic phenol compounds (such as phenol and cresol), bisphenol compounds (such as bisphenol A, bisphenol F, and bisphenol S), and polycyclic phenol compounds (such as tribenzylphenol, dibenzylphenol, benzylphenol, 2,4-bis(α,α-dimethylbenzyl)phenol, and phenolphthalein). Among these, from the viewpoint of dispersibility of the conductive assistant, etc., preferred are bisphenol compounds and polycyclic phenol compounds, and more preferred are polycyclic phenol compounds.
[0021] The alkylene oxide (hereinafter abbreviated as AO) to be added to the phenol compound includes AO having 2 to 4 carbon atoms, such as ethylene oxide (hereinafter abbreviated as EO), 1,2-propylene oxide (hereinafter abbreviated as PO), 1,3-propylene oxide, 1,2-, 1,3- or 2,3-butylene oxide, and tetrahydrofuran (hereinafter abbreviated as THF). Among these, EO or PO is preferred from the viewpoint of dispersibility of the conductive assistant.
[0022] The total weight ratio of carbon atoms constituting the aromatic ring skeleton and hydrogen atoms bonded to carbon atoms in the dispersant is 55% by weight or less based on the weight of the dispersant. From the viewpoint of dispersibility of the conductive assistant, the total weight ratio of the carbon atoms constituting the aromatic ring skeleton in the dispersant and the hydrogen atoms bonded to the carbon atoms is preferably 52% by weight or less, and more preferably 35% by weight or less, based on the weight of the dispersant.
[0023] In the present invention, the ratio of the total weight of the carbon atoms constituting the aromatic ring skeleton and the hydrogen atoms bonded to the carbon atoms in the dispersant can be calculated from the weight of the phenol compound used in the reaction for synthesizing the alkylene oxide adduct of the phenol compound, which is the dispersant, and the number of moles of the alkylene oxide added. 1 It is also possible to calculate it by measuring H-NMR. 1 When measured by H-NMR, specifically, it can be determined by the following measurement conditions and analysis method.
[0024] <Sample preparation method> 100 mg of the measurement object and 10 mg of an internal standard substance (e.g., tetramethylsilane) are weighed out into an NMR tube, 0.45 ml of a deuterated solvent (e.g., deuterated chloroform) is added to dissolve them, and measurement is performed under the following measurement conditions. < 1 H-NMR measurement conditions> Equipment: Bruker Biospin "AVANCE III HD400" Number of times: 4 <Analysis method> The weight percentage (wt%) of hydrogen atoms bonded to carbon atoms constituting the aromatic ring skeleton is calculated from the integral ratio of the peaks derived from the carbon atoms constituting the aromatic ring skeleton and the hydrogen atoms bonded to the carbon atoms, and the peak of the protons derived from the methyl group of the internal standard substance. That is, the total weight percentage (wt%) of the carbon atoms constituting the aromatic ring skeleton and the hydrogen atoms bonded to the carbon atoms is calculated from the integral ratio of the protons derived from the hydrogen atoms bonded to the carbon atoms constituting the aromatic ring skeleton near the chemical shift of 6.5 to 7.5 ppm, the integral ratio of the protons derived from the methyl group of the internal standard substance at the chemical shift of 0 ppm, and the charged weights of the sample and the internal standard substance. The total weight ratio of the carbon atoms constituting the aromatic ring skeleton and the hydrogen atoms bonded to the carbon atoms (% by weight) = Aa / (Ai / Pi) × Ma / Mi × Wi / Ws × 100 where Aa is the integral ratio of the peak of the proton derived from the hydrogen atom bonded to the carbon atom constituting the aromatic ring skeleton, Ai is the integral ratio of the peak of the proton derived from the methyl group of the internal standard substance, Pi is the number of protons of the internal standard substance, Ma is the molecular weight of the dispersant, Mi is the molecular weight of the internal standard substance, Wi is the charge weight (mg) of the internal standard substance, and Ws is the charge weight (mg) of the sample. The total weight ratio of the carbon atoms constituting the aromatic ring skeleton and the hydrogen atoms bonded to the carbon atoms in the dispersant can be adjusted by the molecular weight and the number of moles of the alkylene oxide to be added.
[0025] The hydroxyl group concentration of the dispersant is preferably 0.5 to 10% by weight, more preferably 1 to 7% by weight, based on the weight of the dispersant. In the present invention, the hydroxyl group concentration of the dispersant can be determined from the weight of the phenol compound used in the reaction when synthesizing the alkylene oxide adduct of the phenol compound, which is the dispersant, and the number of moles of the alkylene oxide added. 1 It is also possible to calculate it by measuring H-NMR. 1 When measured by H-NMR, specifically, it can be determined by the following measurement conditions and analysis method.
[0026] <Sample preparation method> 100 mg of the measurement object and 10 mg of an internal standard substance (e.g., tetramethylsilane) are weighed out into an NMR tube, 0.45 ml of a deuterated solvent (e.g., deuterated chloroform) is added to dissolve them, and measurement is performed under the following measurement conditions. < 1 H-NMR measurement conditions> Equipment: Bruker Biospin "AVANCE III HD400" Number of times: 4 <Analysis method> The concentration of hydroxyl groups (wt%) is calculated from the integral ratio of the peak derived from hydroxyl groups to the peak derived from the proton of the methyl group of the internal standard. That is, the concentration of hydroxyl groups (wt%) is calculated from the integral ratio of the proton derived from hydroxyl groups at a chemical shift of about 3.5 to 4.5 ppm, the integral ratio of the proton derived from the methyl group of the internal standard at a chemical shift of 0 ppm, and the charged weights of the sample and the internal standard. Hydroxyl group concentration (wt%)=Ab / (Ai / Pi)×Ma / Mi×Wi / Ws×100 where Ab is the integral ratio of the peak of the proton derived from the hydroxyl group, Ai is the integral ratio of the peak of the proton derived from the methyl group of the internal standard substance, Pi is the number of protons of the internal standard substance, Ma is the molecular weight of the dispersant, Mi is the molecular weight of the internal standard substance, Wi is the charge weight (mg) of the internal standard substance, and Ws is the charge weight (mg) of the sample. The content of hydroxyl groups can be adjusted by appropriately adjusting the composition and charge equivalent of the raw materials constituting the dispersant.
[0027] The weight average molecular weight of the dispersant is preferably 1,000 to 10,000, and more preferably 1,000 to 3,000, from the viewpoint of dispersibility of the conductive assistant. The weight average molecular weight of the dispersant can be determined by GPC (gel permeation chromatography) measurement under the following conditions: A sample dispersant is dissolved in a solvent such as orthodichlorobenzene, N'-dimethylformamide (DMF), or tetrahydrofuran (THF) to prepare a 0.25 wt% solution, and the insoluble portion is filtered through a PTFE filter having a diameter of 1 μm to prepare a sample solution. Apparatus: Alliance GPC V2000 (Waters) Solvent: orthodichlorobenzene, DMF, THF Standard material: polystyrene sample Concentration: 3mg / ml Column stationary phase: PLgel 10um, MIXED-B, 2 columns in series (Polymer Laboratories) Column temperature: 135℃
[0028] The dispersant can be produced by carrying out an addition reaction of an alkylene oxide to the phenol compound by a known method.
[0029] The lithium ion battery electrode composition of the present invention is an electrode composition for lithium ion batteries comprising an electrode active material, a binder resin, a conductive assistant and a dispersant, and the weight ratio of the electrode active material is 78 to 97% by weight based on the solid content weight of the electrode composition for lithium ion batteries. If the weight ratio of the electrode active material is less than 78% by weight based on the solid content weight of the electrode composition for lithium ion batteries, the capacity of the resulting battery is reduced, and if it exceeds 97% by weight, the conductivity of the resulting electrode is deteriorated. From the viewpoint of the balance between battery capacity and conductivity, the weight ratio of the electrode active material is preferably 89 to 92% by weight based on the solid content weight of the electrode composition for lithium ion batteries. The "solids weight of the electrode composition for lithium ion batteries" means the weight of the materials excluding volatile components such as an organic solvent described later (the total weight of the electrode active material, binder resin, conductive assistant, dispersant, etc.) Specifically, the weight of the residue when the electrode composition for lithium ion batteries is heated at 100°C for 8 hours is defined as the solids weight.
[0030] In the lithium ion battery electrode composition of the present invention, the weight ratio of the binder resin is 1 to 20% by weight based on the solid content weight of the lithium ion battery electrode composition. If the weight ratio of the binder resin is less than 1% by weight based on the solid content weight of the lithium ion battery electrode composition, the strength of the obtained electrode is insufficient, and if it exceeds 20% by weight, the capacity of the obtained battery is reduced. From the viewpoint of the balance between electrode strength and battery capacity, the weight ratio of the binder resin is preferably 3 to 10% by weight based on the solid content weight of the lithium ion battery electrode composition.
[0031] In the lithium ion battery electrode composition of the present invention, the weight ratio of the conductive assistant is 1 to 5 wt% based on the solid content weight of the lithium ion battery electrode composition. If the weight ratio of the conductive assistant is less than 1 wt% based on the solid content weight of the lithium ion battery electrode composition, the conductivity of the obtained electrode will deteriorate, and if it exceeds 5 wt%, the capacity of the obtained battery will be reduced. From the viewpoint of the balance between battery capacity and conductivity, the weight ratio of the conductive assistant is preferably 2 to 5 wt% based on the solid content weight of the lithium ion battery electrode composition.
[0032] In the electrode composition for lithium ion batteries of the present invention, the weight ratio of the dispersant is 2 to 20% by weight based on the weight of the conductive assistant. If the weight ratio of the dispersant is less than 2% by weight based on the weight of the conductive assistant, the conductivity of the obtained electrode will deteriorate, and if it exceeds 20% by weight, a side reaction may occur, which may adversely affect the battery performance. From the viewpoint of battery performance, the weight ratio of the dispersant is preferably 5 to 20% by weight based on the weight of the conductive assistant for lithium ion batteries.
[0033] The lithium ion battery electrode composition of the present invention may contain an organic solvent as necessary. An example of the organic solvent is N-methyl-2-pyrrolidone (NMP).
[0034] The present specification discloses the following:
[0035] The present disclosure (1) is an electrode composition for lithium ion batteries, comprising an electrode active material, a binder resin, a conductive assistant, and a dispersant, the dispersant being an alkylene oxide adduct of a phenol compound, the total weight ratio of carbon atoms constituting an aromatic ring skeleton in the dispersant and hydrogen atoms bonded to the carbon atoms being 55% by weight or less based on the weight of the dispersant, the weight ratio of the electrode active material being 78 to 97% by weight based on the solid content weight of the electrode composition for lithium ion batteries, the weight ratio of the binder resin being 1 to 20% by weight based on the solid content weight of the electrode composition for lithium ion batteries, the weight ratio of the conductive assistant being 1 to 5% by weight based on the solid content weight of the electrode composition for lithium ion batteries, and the weight ratio of the dispersant being 2 to 20% by weight based on the weight of the conductive assistant.
[0036] The present disclosure (2) is the electrode composition for a lithium ion battery according to the present disclosure (1), wherein the hydroxyl group concentration of the dispersant is 0.5 to 10% by weight based on the weight of the dispersant.
[0037] The present disclosure (3) is the electrode composition for a lithium ion battery according to the present disclosure (1) or (2), in which the weight average molecular weight of the dispersant is 1,000 to 10,000. EXAMPLES
[0038] The present invention will now be described in detail with reference to examples. However, the present invention is not limited to these examples as long as it does not depart from the gist of the present invention.
[0039] (Production Example 1: Production of Dispersant 1) Ethylene oxide (EO) was added to tribenzylphenol to produce alkylene oxide adducts of phenol compounds. The average number of moles of EO added was 14. 500 parts of the alkylene oxide adduct and 98 parts of solid potassium hydroxide that had been crushed in advance under a nitrogen stream were placed in a sealed container, and the mixture was heated to 80° C. with stirring. Then, 74 parts of methylene chloride were added over about 30 minutes, and the mixture was reacted at 80° C. for about 3 hours. This reaction product was diluted with 500 parts of toluene, the potassium hydroxide and potassium chloride were filtered off, and the volatile matter was removed under reduced pressure to obtain Dispersant 1. The weight average molecular weight was 1,000. From the weight of the phenol compound (tribenzylphenol) used in the reaction and the weight of ethylene oxide added to the phenol compound (tribenzylphenol), the ratio of the total weight of the carbon atoms constituting the aromatic ring skeleton and the hydrogen atoms bonded to the carbon atoms to the total weight of the alkylene oxide adduct, and the hydroxyl group concentration in the alkylene oxide adduct were calculated and are shown in Table 1.
[0040] (Production Example 2: Production of Dispersant 2) An alkylene oxide adduct of a phenolic compound was produced by adding ethylene oxide (EO) to bisphenol A. The average number of moles of EO added was 18. 500 parts of the alkylene oxide adduct and 98 parts of solid potassium hydroxide that had been crushed in advance under a nitrogen stream were placed in a sealed container, and the mixture was heated to 80° C. with stirring. Then, 74 parts of methylene chloride were added over about 30 minutes, and the mixture was reacted at 80° C. for about 3 hours. This reaction product was diluted with 500 parts of toluene, the potassium hydroxide and potassium chloride were filtered off, and the volatile matter was removed under reduced pressure to obtain Dispersant 2. The weight average molecular weight was 1,020. From the weight of bisphenol A used in the reaction and the weight of ethylene oxide added to bisphenol A, the ratio of the total weight of the carbon atoms constituting the aromatic ring skeleton and the hydrogen atoms bonded to the carbon atoms to the total weight of the alkylene oxide adduct, and the hydroxyl group concentration in the alkylene oxide adduct were calculated and are shown in Table 1.
[0041] (Production Example 3: Production of Dispersant 3) Propylene oxide (PO) was added to bisphenol A to produce an alkylene oxide adduct of a phenol compound. The average number of moles of PO added was 5. 500 parts of the alkylene oxide adduct and 98 parts of solid potassium hydroxide that had been crushed in advance under a nitrogen stream were placed in a sealed container, and the mixture was heated to 80° C. with stirring. Then, 74 parts of methylene chloride were added over about 30 minutes, and the mixture was reacted at 80° C. for about 3 hours. This reaction product was diluted with 500 parts of toluene, the potassium hydroxide and potassium chloride were filtered off, and the volatile matter was removed under reduced pressure to obtain Dispersant 3. The weight average molecular weight was 560. From the weight of bisphenol A used in the reaction and the weight of propylene oxide added to bisphenol A, the ratio of the total weight of the carbon atoms constituting the aromatic ring skeleton and the hydrogen atoms bonded to the carbon atoms to the total weight of the alkylene oxide adduct, and the hydroxyl group concentration in the alkylene oxide adduct were calculated and are shown in Table 1.
[0042] (Production Examples 4 to 10: Production of Dispersants 4 to 10) Dispersants 4, 5, 6, 7, 8, 9, and 10 were produced in the same manner as in Production Example 1, except that the type of starting material (phenol compound) and the number of moles of EO added were changed as shown in Table 1.
[0043] [Table 1]
[0044] (Examples 1 to 9 and Comparative Examples 1 to 3: Preparation of Positive Electrode Compositions for Lithium Ion Batteries) The dispersant and binder resin were weighed out according to the weight parts in Table 2, and N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration of the resulting solution was 60% by weight. The mixture was stirred at 2000 rpm for 4 minutes using a planetary stirring type mixer and kneader {Awatori Rentaro [manufactured by Thinky Corporation]} to completely dissolve the binder resin and dispersant. The positive electrode active material and conductive assistant were then added in the weight parts shown in Table 2, and the mixture was stirred at 2000 rpm for 4 minutes using Awatori Rentaro to prepare a positive electrode composition for lithium ion batteries. The positive electrode active material is LiNi 0.8 Co 0.15 Al 0.05 The O2 powder "HED NCA 7050" (referred to as "NCA" in Table 2, manufactured by BTBM) was used. As the conductive assistant, acetylene black "Denka Black Li100" (referred to as "AB(Li100)" in Tables 2 and 3, manufactured by Denka Co., Ltd.) was used. Polyvinylidene fluoride (referred to as "PVDF" in Table 2, manufactured by Kishida Chemical) was used as the binder resin. The amount of each material listed in Table 2 is shown by weight (wt %) based on the solid content of the lithium ion battery positive electrode composition.
[0045] <Measurement of Viscosity of Electrode Composition (Electrode Slurry)> The viscosity of the positive electrode composition and the negative electrode composition was measured using a rheometer [MCR302, [Anton Paar]] with a cone plate CP25 and a shear rate of 0.1 to 100 s -1 , 25℃, shear rate 10 s -1 The viscosity at this point was recorded and is shown in Tables 2 and 3.
[0046] [Table 2]
[0047] (Preparation of batteries for charge / discharge tests: for positive electrode) The positive electrode composition for lithium ion batteries was applied to one side of a current collector (aluminum foil, manufactured by Hosen Co., Ltd.) using a wire bar in the atmosphere, pre-dried overnight, and then punched out to a diameter of 15 mm, further dried at 120°C under reduced pressure (1.3 kPa) for 4 hours, and pressed to the target electrode density (electrode thickness) using a press to prepare a positive electrode for evaluation. Starting from the positive electrode side, the positive electrode, a separator [product name "#3501", manufactured by Celgard], and lithium foil were stacked in this order, and an electrolyte (manufactured by Kishida Chemical, EC:DEC (1:1 v / v%), LiPF6 concentration: 1 mol / L) was injected, followed by vacuum lamination to prevent oxygen from entering, to prepare a battery for charge / discharge tests.
[0048] (Examples 10 to 18 and Comparative Examples 4 to 6: Preparation of negative electrode compositions for lithium ion batteries) The dispersant was weighed out according to the blending amounts shown in Table 3, water was added so that the resulting aqueous solution had a solid content concentration of 45% by weight, and stirring was performed for 2 minutes at 2000 rpm using a planetary stirring type mixer / kneader "Awatori Rentaro" (manufactured by Thinky Corporation). Furthermore, sodium carboxymethylcellulose (CMCNa: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was weighed out and added according to the blending amounts shown in Table 3, and stirring was performed for 5 minutes at 2000 rpm using a planetary stirring type mixer / kneader "Awatori Rentaro" (manufactured by Thinky Corporation) to dissolve the CMCNa. Next, the negative electrode active material and conductive assistant were added in the blending amounts shown in Table 3, and then stirring was performed for 4 minutes at 2000 rpm using the Awatori Rentaro. Finally, styrene butadiene rubber (referred to as SBR in Table 3, manufactured by Zeon Corporation) was weighed out according to the compounding amounts shown in Table 3, and the mixture was stirred at 2000 rpm for 10 seconds using a planetary stirring type mixer / kneader "Awatori Rentaro" (manufactured by Thinky Corporation) to prepare a negative electrode composition for a lithium ion battery. Graphite particles "SNG-WXA1" (referred to as "graphite" in Table 3) were used as the negative electrode active material. As the conductive assistant, acetylene black "Denka Black Li100" (referred to as "AB" in Tables 2 and 3, manufactured by Denka Co., Ltd.) and / or carbon nanotubes "NC7000" (referred to as "CNT" in Tables 2 and 3, manufactured by Nanocyl Corporation) were used. The amount of each material listed in Table 3 is shown by weight (wt %) based on the solid content of the negative electrode composition for a lithium ion battery.
[0049] [Table 3]
[0050] (Preparation of batteries for charge / discharge tests: for negative electrodes) The negative electrode composition for lithium ion batteries was applied to one side of a current collector (copper foil) using a wire bar in the atmosphere, pre-dried overnight, and then punched out to a diameter of 16 mm, further dried at 100°C under reduced pressure (1.3 kPa) for 4 hours, and pressed to the target electrode density (electrode thickness) using a press machine to prepare a negative electrode for evaluation. Starting from the negative electrode side, the negative electrode, a separator [product name "#3501", manufactured by Celgard], and lithium foil were stacked in this order, and an electrolyte (manufactured by Kishida Chemical, EC:DEC (1:1 v / v%), LiPF6 concentration: 1 mol / L) was injected, followed by vacuum lamination to prevent oxygen from entering, to prepare a battery for charge / discharge tests.
[0051] <Positive electrode half-cell charge / discharge test> At 25° C., the initial performance of the charge / discharge test battery (for positive electrode) prepared by the following method was evaluated using a charge / discharge measuring device "HJ-SD8" (manufactured by Hokuto Denko Corporation). Using the constant current constant voltage charging method (also known as CCCV mode), the battery was charged up to 4.2 V at a current of 0.05 C, and then charged while maintaining 4.2 V until the current value reached 0.0025 C. After a 10-minute break, the battery was discharged down to 2.5 V at a current of 0.05 C. The charged capacity was defined as [initial charge capacity (mAh)], and the discharged capacity was defined as [initial discharge capacity (mAh)].
[0052] <Negative electrode half-cell charge / discharge test> The initial performance of the charge / discharge test battery (for negative electrode) was evaluated at 25° C. using a charge / discharge measuring device “HJ-SD8” [manufactured by Hokuto Denko Corporation] according to the following method. The battery was charged to 0V at a current of 0.05C using the constant current charging method (also known as CC mode), and after a 10-minute rest, it was discharged to 1.5V at a current of 0.05C. The charged capacity was defined as [initial charge capacity (mAh)], and the discharged capacity was defined as [initial discharge capacity (mAh)].
[0053] The initial coulombic efficiency was calculated using the following formula, and the results are shown in Tables 2 and 3. Initial coulombic efficiency (%) = [initial discharge capacity] / [initial charge capacity] x 100 In addition, the electrical resistance (10sDCR) was calculated from the voltage at the start of discharge and after 10 seconds had elapsed using the following formula. 10sDCR(Ω cm 2 ) = ([Voltage before discharge starts (V)] - [Voltage 10 seconds after discharge starts (V)]) / [Current during discharge (A)] × 1.77 (1.77 cm 2 )
[0054] The above charge and discharge cycle was repeated 10 times. The battery capacity at the first charge (initial discharge capacity) and the battery capacity at the 10th charge cycle (discharge capacity after 10 cycles) were used to calculate the discharge capacity retention rate according to the following formula. The results are shown in Tables 2 and 3. Note that the larger the value, the less the battery deteriorated. Discharge capacity retention rate (%) = [Discharge capacity at 10th cycle] / [Discharge capacity at 1st cycle] × 100 [Industrial Applicability]
[0055] Lithium ion batteries equipped with an electrode obtained from the lithium ion battery electrode composition of the present invention are particularly useful as lithium ion batteries for use in mobile phones, personal computers, hybrid automobiles, and electric automobiles.
Claims
1. An electrode composition for a lithium ion battery comprising an electrode active material, a binder resin, a conductive assistant, and a dispersant, The dispersant is an alkylene oxide adduct of a phenol compound, the total weight ratio of carbon atoms constituting an aromatic ring skeleton and hydrogen atoms bonded to carbon atoms in the dispersant is 55% by weight or less based on the weight of the dispersant, the weight ratio of the electrode active material is 78 to 97% by weight based on the solid content weight of the lithium ion battery electrode composition, the weight ratio of the binder resin is 1 to 20% by weight based on the solid content weight of the lithium ion battery electrode composition, and the weight ratio of the conductive assistant is 1 to 5% by weight based on the solid content weight of the lithium ion battery electrode composition; The weight ratio of the dispersant is 2 to 20% by weight based on the weight of the conductive assistant.
2. 2. The electrode composition for lithium ion batteries according to claim 1, wherein the hydroxyl group concentration of the dispersant is 0.5 to 10% by weight based on the weight of the dispersant.
3. The electrode composition for lithium ion batteries according to claim 1, wherein the weight average molecular weight of the dispersant is 1,000 to 10,000.
Citation Information
Patent Citations
Nonaqueous electrolytic solution battery
JP2004186035A
Fine carbon fiber dispersion liquid and method for producing the same
JP2014181140A