Secondary battery and manufacturing method for the same
The separator design with a conductive and non-conductive region configuration on the lithium metal secondary battery separator addresses misalignment and short circuit issues, maintaining stability and capacity through electrode alignment and reduced contact risks.
Patent Information
- Application Number
- JP2024046686
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Lithium metal secondary batteries face issues with misalignment and short circuits due to changes in negative electrode layer thickness during charging and discharging, and the formation of lithium dendrites, which can penetrate separators and cause shorts.
A separator with an extending portion beyond the positive electrode layer, featuring a conductive region on the negative electrode side and a non-conductive region at the end, prevents contact between the conductive layer and the positive electrode or lead wire, using a long insulating porous film with alternating folds to maintain electrode alignment.
This design reduces the likelihood of short circuits and maintains electrode layer density, ensuring stable operation and high capacity even with significant negative electrode layer thickness changes.
Smart Images

Figure 2024144275000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a secondary battery and a method for manufacturing the same. [Background technology]
[0002] In recent years, research and development has been conducted on secondary batteries that contribute to energy efficiency in order to ensure that more people have access to affordable, reliable, sustainable, and advanced energy. In order to improve the energy density of secondary batteries, secondary batteries with a stacked structure in which multiple positive electrode layers and negative electrode layers are stacked alternately have been considered. In this stacked structure secondary battery, it has been considered to fold a long separator in a zigzag shape and arrange the positive electrode layers and negative electrode layers alternately at the folded parts in order to suppress misalignment of the positive electrode layers and negative electrode layers (Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2020 / 003846 [Patent Document 2] International Publication No. 2020 / 003847 Summary of the Invention [Problem to be solved by the invention]
[0004] In the technology related to secondary batteries, increasing the capacity is an issue. In order to increase the capacity of secondary batteries, it is desired to put lithium metal secondary batteries using metallic lithium as the negative electrode active material into practical use. However, in lithium metal secondary batteries, the thickness of the negative electrode layer changes significantly due to charging and discharging. For this reason, in a lithium metal secondary battery having a laminated structure in which multiple positive electrode layers and negative electrode layers are alternately stacked, there is a risk that the positional deviation between the positive electrode layer and the negative electrode layer may easily occur due to the change in the thickness of the negative electrode layer caused by charging and discharging.
[0005] In addition, in lithium metal secondary batteries, repeated charging and discharging causes an SEI layer (solid electrolyte intermediate phase) to accumulate at the interface between the current collector of the negative electrode layer and lithium, making it easier for lithium dendrites to form during charging. When lithium dendrites form, they may penetrate the separator and cause a short circuit between the positive electrode layer and the negative electrode layer. In addition, when lithium dendrites form, the density of the layer of metallic lithium (negative electrode active material layer) deposited on the negative electrode current collector decreases, and the lithium secondary battery may expand excessively during charging.
[0006] According to the study by the present inventors, by using a laminate in which a conductive layer is laminated on the surface of a porous film as a separator and arranging the conductive layer on the negative electrode layer side, it is possible to suppress short circuit caused by dendrites and a decrease in density of the active material layer of the negative electrode layer in a charged state. However, in a secondary battery using a separator having a conductive layer on the surface on the negative electrode layer side, there is a risk that the conductive layer will come into contact with the positive electrode layer or the positive electrode lead wire connecting the positive electrode layer and the positive electrode terminal, causing a short circuit between the positive electrode layer and the negative electrode layer.
[0007] The present invention has been made in view of the above, and aims to provide a secondary battery and a manufacturing method thereof in which, even if the thickness of the negative electrode layer changes significantly due to charging and discharging and the separator has a conductive layer on the negative electrode layer side, the conductive layer is unlikely to come into contact with the positive electrode layer or the positive electrode lead wire, and the positive electrode layer and the negative electrode layer are unlikely to short-circuit, thereby contributing to energy efficiency. [Means for solving the problem]
[0008] The present inventors have found that in order to solve the above problems, it is effective to provide an extension portion of the separator that extends outward beyond the end of the positive electrode layer on the side that connects to the positive electrode terminal, so that at least a portion of the portion that contacts the negative electrode layer is a conductive region provided with a conductive layer, and at least a portion of the end of the extension portion on the positive electrode terminal side is a non-conductive region not provided with a conductive layer, and have completed the present invention. Therefore, the present invention provides the following.
[0009] (1) A secondary battery comprising: an electrode laminate having a positive electrode layer, a negative electrode layer, and a separator disposed between the positive electrode layer and the negative electrode layer; an electrolyte; an exterior housing that accommodates the electrode laminate and the electrolyte; a positive electrode terminal and a negative electrode terminal provided on the exterior housing; a positive electrode lead wire that electrically connects the positive electrode layer and the positive electrode terminal; and a negative electrode lead wire that electrically connects the negative electrode layer and the negative electrode terminal, wherein the separator has an extension that extends outward beyond an end of the positive electrode layer on a side that connects to the positive electrode terminal, and at least a part of a portion of a surface of the separator on the negative electrode layer side that contacts the negative electrode layer is a conductive region provided with a conductive layer, and at least a part of an end of the extension on the positive electrode terminal side is a non-conductive region not provided with the conductive layer.
[0010] In the secondary battery of (1), at least a part of the extension portion of the separator that extends outward beyond the end of the positive electrode layer on the side connected to the positive electrode terminal is a non-conductive region, so that even if the thickness of the negative electrode layer changes significantly due to charging and discharging, the conductive layer provided on the portion of the separator that contacts the negative electrode layer is unlikely to come into contact with the positive electrode layer or the positive electrode lead wire, thereby making it difficult for a short circuit to occur between the positive electrode layer and the negative electrode layer.
[0011] (2) The separator includes a long insulating porous membrane, and the conductive region and the non-conductive region provided on one surface of the long insulating porous membrane, the conductive region extending along the length direction of the long insulating porous membrane, the non-conductive region being disposed at least at one end in the width direction of the long insulating porous membrane, and a first fold folded along the length direction so that the surface on the long insulating porous membrane side faces inward, and a second fold folded along the length direction so that the surface on the side where the conductive region and the non-conductive region are disposed faces inward. the positive electrode layer is sandwiched between the first folds and the non-conductive region is located in a position that becomes the extension portion; the negative electrode layer is sandwiched between the second folds and is located in contact with the conductive region; the positive electrode terminal is electrically connected to an end of the positive electrode layer on the side where the non-conductive region is located, and the negative electrode terminal is electrically connected to an end of the negative electrode layer on the side opposite to the side where the non-conductive region is located.
[0012] In the secondary battery of (2), the separator is a long separator, and the positive electrode layer is located at the first fold and the negative electrode layer is located at the second fold, so that the positive electrode layer and the negative electrode layer are less likely to be misaligned. In addition, a strip-shaped conductive layer is formed along the length of the long separator, and the length of the conductive layer in the length direction is longer than the length of the negative electrode layer, so that the effect of the conductive layer can be reliably obtained. Furthermore, the non-conductive region of the long separator becomes an extension, so that the conductive layer is less likely to come into contact with the positive electrode layer or the positive electrode lead wire.
[0013] (3) The secondary battery according to (1) or (2), wherein an end of the conductive region on the positive electrode terminal side is located at the same position as or inside an end of the negative electrode layer on the positive electrode terminal side.
[0014] In the secondary battery of (3), the end of the extension portion is a non-conductive region, so that the conductive layer is less likely to come into contact with the positive electrode layer or the positive electrode lead wire.
[0015] (4) The secondary battery according to any one of (1) to (3), wherein the non-conductive region is disposed only at the end of the separator on the positive electrode terminal side.
[0016] According to the secondary battery of (4), the area other than the end of the extension portion becomes a conductive region, and the contact area between the conductive layer and the negative electrode layer is increased, so that it is possible to suppress short circuits caused by dendrites and a decrease in the density of the active material layer of the negative electrode layer in a charged state.
[0017] (5) The secondary battery according to any one of (1) to (4), wherein the negative electrode active material is metallic lithium.
[0018] According to the secondary battery of (5), since the negative electrode active material is metallic lithium, it is possible to increase the capacity.
[0019] (6) A long insulating porous film, a conductive region provided with a conductive layer arranged on one surface of the long insulating porous film, and a non-conductive region not provided with a conductive layer, the conductive region extending along the length direction of the long insulating porous film, the non-conductive region arranged on at least one end in the width direction of the long insulating porous film, a first fold formed by folding a long laminate sheet zigzag and folding the long laminate sheet along the length direction so that the surface on the long insulating porous film side is on the inside, and a first fold formed by folding the long laminate sheet zigzag ... and a second fold formed by folding the separator along the length direction so that the surface of the side on which the non-conductive region is disposed is on the inside, the first fold being alternately overlapped with a positive electrode layer and a negative electrode layer being alternately arranged on the second fold so that they face each other. A method for manufacturing a secondary battery comprising the steps of: connecting a positive electrode terminal via a positive electrode lead wire to an end of the positive electrode layer on the side on which the non-conductive region is disposed, and connecting a negative electrode terminal via a negative electrode lead wire to an end of the negative electrode layer opposite to the side to which the positive electrode terminal is connected.
[0020] According to the method for manufacturing a secondary battery in (6), a positive electrode terminal is connected to the end of the positive electrode layer on the side where the non-conductive region is arranged via a positive electrode lead wire, so that a secondary battery having an extension part extended from the end of the positive electrode layer on the side where it is connected to the positive electrode terminal can be manufactured industrially advantageously. In addition, since the positive electrode layer is arranged on the first fold of the long separator and the negative electrode layer is arranged on the second fold, the obtained secondary battery is less likely to have a positional deviation between the positive electrode layer and the negative electrode layer. Furthermore, a strip-shaped conductive layer is formed along the length direction of the long separator, and the length of the conductive layer in the length direction is longer than the length of the negative electrode layer, so that the obtained secondary battery can reliably obtain the effect of the conductive layer. Effect of the Invention
[0021] According to the present invention, it is possible to provide a secondary battery and a manufacturing method thereof in which the thickness of the negative electrode layer changes significantly due to charging and discharging, and even if a separator having a conductive layer on the negative electrode layer side is used, the conductive layer is unlikely to come into contact with the positive electrode layer or a positive electrode lead wire, and the positive electrode layer and the negative electrode layer are unlikely to short-circuit. [Brief description of the drawings]
[0022] [Figure 1] 1 is a perspective view of a secondary battery according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 2 is a cross-sectional view taken along line III-III in FIG. [Figure 4] FIG. 2 is a plan view of a separator that can be used in the secondary battery according to one embodiment of the present invention. [Diagram 5] 5 is a cross-sectional view taken along line VV in FIG. 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, embodiments of the present invention will be described with reference to the drawings. However, the embodiments described below are merely examples of the present invention, and the present invention is not limited to the following.
[0024] Fig. 1 is a perspective view of a secondary battery according to one embodiment of the present invention. Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1, and Fig. 3 is a cross-sectional view taken along line III-III in Fig. 1. Fig. 4 is a plan view of a separator that can be used in the secondary battery according to one embodiment of the present invention. Fig. 5 is a cross-sectional view taken along line VV in Fig. 4.
[0025] The secondary battery 100 according to this embodiment includes an electrode laminate 10 having a positive electrode layer 20, a negative electrode layer 30, and a long separator 40 disposed between the positive electrode layer 20 and the negative electrode layer 30, an electrolyte (not shown), and an exterior body 50 that contains the electrode laminate 10 and the electrolyte. The positive electrode layer 20 includes a positive electrode current collector 21 and a positive electrode active material layer 22 laminated on both sides of the positive electrode current collector 21. The negative electrode layer 30 includes a negative electrode current collector 31 and a lithium foil 32 laminated on both sides of the negative electrode current collector 31. The secondary battery 100 is a lithium metal secondary battery. A lithium metal secondary battery is a secondary battery that uses metallic lithium as the negative electrode active material. During charging, lithium is released from the positive electrode active material layer 22, and the lithium is precipitated on the surface of the lithium foil 32 to form a metallic lithium layer. For this reason, the thickness of the negative electrode layer 30 increases during charging. On the other hand, during discharge, lithium is released from the metallic lithium layer and is absorbed in the positive electrode active material layer 22. Therefore, the thickness of the negative electrode layer 30 decreases during discharge. Therefore, the thickness of the negative electrode layer 30 changes greatly due to charging and discharging. The secondary battery 100 shown in Figs. 1 to 3 is in a discharged state. As shown in Fig. 2, the widths of the positive electrode layer 20, the negative electrode layer 30, and the long separator 40 are such that the long separator 40 is the widest, the negative electrode layer 30 is the next widest, and the positive electrode layer 20 is the narrowest.
[0026] The secondary battery 100 further includes a positive electrode terminal 24 and a negative electrode terminal 34 provided on the exterior body 50, a positive electrode lead wire 23 electrically connecting the positive electrode layer 20 (positive electrode current collector 21) and the positive electrode terminal 24, and a negative electrode lead wire 33 electrically connecting the negative electrode layer 30 (negative electrode current collector 31) and the negative electrode terminal 34. A portion of the positive electrode terminal 24 and the negative electrode terminal 34 are exposed to the outside. The positive electrode terminal 24 is disposed along the width direction of the long separator 40 (a direction perpendicular to the length direction of the long separator 40), and the negative electrode terminal 34 is disposed at a position facing each other with the electrode stack 10 in between.
[0027] The long separator 40 has an extension portion 40a that extends outward beyond the end of the positive electrode layer 20 on the side connected to the positive electrode terminal 24. The extension length of the extension portion 40a varies depending on the thickness of the positive electrode layer 20, the size of the positive electrode lead wire 23, the thickness of the conductive layer 42, etc., but is, for example, equal to or greater than the thickness of the positive electrode active material layer 22. When the width of the positive electrode layer 20 is wider than the width of the negative electrode layer 30, the extension portion 40a may extend beyond the end of the negative electrode layer 30.
[0028] In the long separator 40, at least a part of the surface on the negative electrode layer 30 side that contacts the negative electrode layer 30 is a conductive region 401 provided with a conductive layer 42, and at least a part of the end of the extension portion 40a on the positive electrode terminal side is a non-conductive region 402 on which the conductive layer 42 is not provided. The width of the conductive layer 42 (the length in the direction perpendicular to the longitudinal direction of the long separator 40) may be larger than the width of the positive electrode layer 20, or may be equal to or smaller than the width of the negative electrode layer 30. The width of the conductive layer 42 at the end of the conductive layer 42 (conductive region 401) on the negative electrode terminal 34 side may exceed the negative electrode layer 30, or may be disposed up to the end of the long separator 40. The end of the conductive layer 42 on the positive electrode terminal 24 side may be the same as or more inward than the end of the negative electrode layer 30 on the positive electrode terminal 24 side. In this embodiment, the end of the conductive layer 42 on the positive electrode terminal 24 side is located inside the end of the negative electrode layer 30 on the positive electrode terminal 24 side. The non-conductive region 402 may be disposed only at the end of the long separator 40 on the positive electrode terminal 24 side. The width of the non-conductive region is preferably wider than at least the thickness of the positive electrode active material layer 22.
[0029] The long separator 40 includes a long insulating porous membrane 41, a conductive region 401 arranged on the surface of the long insulating porous membrane 41 on the negative electrode layer 30 side, and a non-conductive region 402 (see FIG. 4). The conductive region 401 has a strip-shaped conductive layer 42 arranged along the length of the long insulating porous membrane 41. The non-conductive region 402 does not have a conductive layer 42. At least one end in the width direction of the long insulating porous membrane 41 is the non-conductive region 402. In this embodiment, the non-conductive region 402 is arranged at one end in the width direction of the long insulating porous membrane 41. The long separator 40 is formed such that a first fold 43 and a second fold 44 are alternately folded over each other. The first fold 43 is a portion folded along the length direction so that the surface on the long insulating porous membrane 41 side faces inward. The first fold 43 has a tip 43a and an opening 43b located on the opposite side to the tip 43a. The second fold 44 is a portion folded along the length direction so that the surface on which the conductive region 401 and the non-conductive region 402 are arranged faces inward. The second fold 44 has a tip 44a and an opening 44b located on the opposite side to the tip 44a.
[0030] The positive electrode layer 20 is disposed on the first fold 43, and the negative electrode layer 30 is disposed on the second fold 44 so as to face each other. The positive electrode layer 20 contacts the long insulating porous membrane 41 of the long separator 40, and the negative electrode layer 30 contacts the conductive layer 42 of the long separator 40. The positive electrode terminal 24 is connected to the end of the positive electrode layer 20 (positive electrode current collector 21) on the side where the non-conductive region 402 is disposed. As a result, the non-conductive region 402 of the long separator 40 acts as the extension portion 40a. The negative electrode terminal 34 is connected to the end of the negative electrode layer 30 (negative electrode current collector 31) on the opposite side to the side where the positive electrode terminal 24 is connected. The end of the positive electrode layer 20 on the opposite side to the side where it is connected to the positive electrode terminal 24 (the side where the negative electrode layer 30 is connected to the negative electrode terminal 34) may be located inside the end of the negative electrode layer 30.
[0031] The material of the positive electrode collector 21 is not particularly limited, and aluminum, for example, can be used. The material of the positive electrode lead wire 23 may be the same as the material of the positive electrode collector 21, or may be different from the material of the positive electrode collector 21. The positive electrode lead wire 23 may be integrally connected to the positive electrode collector 21. In this embodiment, the positive electrode lead wire 23 is formed by extending the positive electrode collector 21, and is integrally connected to the positive electrode collector 21. The material of the positive electrode terminal 24 may be the same as the material of the positive electrode lead wire 23, or may be different from the material of the positive electrode lead wire 23. The positive electrode terminal 24 may be integrally connected to the positive electrode lead wire 23. In this embodiment, the positive electrode terminal 24 and the positive electrode lead wire 23 are separate members and are electrically connected.
[0032] The positive electrode active material layer 22 includes a positive electrode active material. Examples of the positive electrode active material include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), LiNi p Mn q Co r O2(p+q+r=1), LiNi p Al q Co r O2(p+q+r=1), lithium manganese oxide (LiMn2O4), Li 1+x Mn 2-x-y M y Examples of the positive electrode active material layer 22 include a different element-substituted Li-Mn spinel represented by O4 (x+y=2, M=at least one selected from Al, Mg, Co, Fe, Ni, and Zn), lithium titanate (an oxide containing Li and Ti), and lithium metal phosphate (LiMPO4, M=at least one selected from Fe, Mn, Co, and Ni). The positive electrode active material layer 22 may contain various additives used as materials for positive electrode active material layers, such as a binder and a conductive assistant.
[0033] The material of the negative electrode current collector 31 is not particularly limited, and for example, copper can be used. The material of the negative electrode lead wire 33 may be the same as the material of the negative electrode current collector 31, or may be different from the material of the negative electrode current collector 31. The negative electrode lead wire 33 may be integrally connected to the negative electrode current collector 31. In this embodiment, the negative electrode lead wire 33 is formed by extending the negative electrode current collector 31, and is integrally connected to the negative electrode current collector 31. The material of the negative electrode terminal 34 may be the same as the material of the negative electrode lead wire 33, or may be different from the material of the negative electrode lead wire 33. The negative electrode terminal 34 may be integrally connected to the negative electrode lead wire 33. In this embodiment, the negative electrode terminal 34 and the negative electrode lead wire 33 are separate members and are electrically connected.
[0034] As the long insulating porous film 41 of the long separator 40, for example, a known one used as a separator for a secondary battery, such as a porous sheet or a nonwoven fabric sheet, can be used. Examples of the material of the porous sheet include polyolefins such as polyethylene and polypropylene, aramid, polyimide, and fluororesin. Examples of the material of the nonwoven fabric sheet include glass fiber and cellulose fiber. The thickness of the long insulating porous film 41 is not particularly limited, but is preferably 10 μm or more from the viewpoint of blocking dendrites of lithium metal, and is preferably 15 μm or less from the viewpoint of reducing resistance in the battery. The thickness of the long insulating porous film 41 is more preferably within the range of 10 to 12 μm. In addition, the air permeability of the long insulating porous film 41 is not particularly limited, but is preferably 200 sec / 100 mL or less from the viewpoint of reducing resistance in the battery, and is more preferably 150 sec / 100 mL or less. The porosity of the long insulating porous membrane 41 is not particularly limited, but from the viewpoint of uniform diffusion of lithium in the long separator 40 and the strength of the long separator 40, it is preferably in the range of 40 to 60%.
[0035] The conductive layer 42 of the long separator 40 does not have to be laminated over the entire conductive region 401. As shown in FIG. 5, the conductive layer 42 may be laminated so as to cover a part of the hole 41a of the long insulating porous membrane 41 in the conductive region 401. The electrical conductivity of the conductive layer 42 is not particularly limited, but is preferably 1.0×10 1 ~1.0×10 5 The electrical conductivity of the conductive layer 42 is in the range of 1.0×10 1 When the electrical conductivity is 1.0×10 S / cm or more, lithium can be deposited on the surface of the conductive layer 42, and the lithium dendrite can be prevented from growing on the positive electrode layer 20 side and causing a short circuit. 5 By ensuring that the conductivity is equal to or less than S / cm, lithium can be deposited uniformly on the surface of the conductive layer 42.
[0036] In both the discharged and charged states, the conductive layer 42 is in electrical contact with either the negative electrode layer 30 or metallic lithium deposited on the negative electrode layer 30. This makes the potential of the conductive layer 42 and the potential of the negative electrode current collector 31 the same, allowing lithium to be more uniformly deposited between the conductive layer 42 of the long separator 40 and the lithium foil 32.
[0037] The electrical conductivity of the conductive layer 42 may be lower than that of the negative electrode current collector 31, i.e., the electrical conductivity of the negative electrode current collector 31 may be higher than that of the conductive layer 42. By making the electrical conductivity of the negative electrode current collector 31 higher than that of the conductive layer 42, concentrated deposition of lithium on the long insulating porous film 41 side of the conductive layer 42 can be prevented, and damage to the conductive layer 42 due to the concentrated deposition of lithium can be suppressed. The electrical conductivity of the conductive layer 42 may be within a range of 1 / 10 to 1 / 100000 of the electrical conductivity of the negative electrode current collector 31, for example.
[0038] The peel strength of the conductive layer 42 from the long insulating porous membrane 41 is not particularly limited, but is preferably 10 N / m or more, and more preferably 30 N / m or more. When the peel strength of the conductive layer 42 is as high as the above value, the conductive layer 42 functions stably for a long period of time, and thus the charge / discharge cycle life is extended.
[0039] The surface resistivity of the conductive layer 42 is 200 Ω / cm 2 It may be the following.
[0040] The thickness of the conductive layer 42 may be within a range of 0.01 to 5 μm. When the thickness of the conductive layer 42 is 0.01 μm or more, the above-mentioned effects of the conductive layer 42 can be obtained. When the thickness of the conductive layer 42 is 5 μm or less, the decrease in energy density due to the conductive layer 42 can be reduced.
[0041] The conductive layer 42 may be made of a conductive material such as a metal or carbon nanotube (CNT). Examples of metals include Cu, Zn, Ti, and Sn. These conductive materials may be used alone or in combination of two or more.
[0042] The coating method for forming the conductive layer 42 on the long insulating porous film 41 is not particularly limited, and for example, a sputtering method or a coating method can be used. As the sputtering method, a DC sputtering method or an RF sputtering method can be used. The coating method is a method in which a coating liquid in which the material of the conductive layer 42 is dispersed is applied to the surface of the long insulating porous film 41 and dried.
[0043] The electrolytic solution includes an organic solvent and an electrolyte. Examples of the organic solvent include cyclic carbonates, chain carbonates, cyclic ethers, chain ethers, hydrofluoroethers, aromatic ethers, sulfones, cyclic esters, chain carboxylates, and nitriles. Examples of the cyclic carbonates include ethylene carbonate, propylene carbonate, vinylene carbonate, and fluoroethylene carbonate. Examples of the chain carbonates include dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. Examples of the cyclic ethers include tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, and 4-methyl1,3-dioxolane. Examples of the chain ethers include 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, and diethyl ether. Examples of hydrofluoroethers include 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis(2,2,2-trifluoroethyl)ether, 1,2-bis(1,1,2,2-tetrafluoroethoxy)ethane, and the like. Examples of aromatic ethers include anisole. Examples of sulfones include sulfolane and methylsulfolane. Examples of cyclic esters include γ-butyrolactone, and the like. Examples of chain carboxylates include acetates, butyrates, and propionates. Examples of nitriles include acetonitrile and propionitrile. The organic solvents may be used alone or in combination of two or more.
[0044] The electrolyte is a source of lithium ions, which are charge transfer media, and contains a lithium salt. Examples of the lithium salt include LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC(CF3SO2)3, LiN(CF3SO2)2(LiTFSI), LiN(FSO2)2(LiFSI), and LiBC4O8. The lithium salt may be used alone or in combination of two or more. The concentration of the electrolyte is, for example, within the range of 1.5 to 4.0 mol / L.
[0045] The exterior body 50 is expandable and contractable in accordance with changes in the thickness of the electrode laminate 10 (particularly changes in the thickness of the negative electrode layer 30) due to charging and discharging. A laminate film can be used as the material of the exterior body 50. A laminate film having a three-layer structure in which an inner resin layer, a metal layer, and an outer resin layer are laminated in this order from the inside can be used as the laminate film. The inner resin layer and the outer resin layer can be made of, for example, polyethylene terephthalate (PET), polyamide (nylon), or polypropylene (PP). The metal layer can be made of, for example, aluminum.
[0046] The secondary battery 100 of this embodiment can be manufactured by a method including, for example, a long separator fabrication step, an electrode layer arrangement step, a terminal connection step, an exterior body accommodation step, and a sealing step.
[0047] The long separator production process is a process for producing a long separator 40 in which the above-mentioned first fold 43 and second fold 44 are alternately overlapped. The long separator 40 can be produced by zigzag folding a long laminated sheet including a long insulating porous membrane 41, a conductive region 401 having a conductive layer 42 arranged on one surface of the long insulating porous membrane 41, and a non-conductive region 402 not having the conductive layer 42, the conductive region 401 extending along the length of the long insulating porous membrane 41, and the non-conductive region 402 arranged at least on one end in the width direction of the long insulating porous membrane 41.
[0048] The electrode layer arrangement step is a step of arranging the positive electrode layer 20 on the first fold 43 and the negative electrode layer 30 on the second fold 44 so as to face each other. This step results in an electrode laminate 10. The positive electrode layer 20 can be arranged by inserting the positive electrode layer 20 through the opening 43b of the first fold 43. The negative electrode layer 30 can be arranged by inserting the negative electrode layer 30 through the opening 44b of the second fold 44. The long separator production step and the electrode layer arrangement step may be carried out in parallel. For example, after arranging the positive electrode layer 20 on the surface of the long insulating porous membrane 41 side of the long laminate sheet, the long laminate sheet may be folded along the length direction so that the surface on the long insulating porous membrane 41 side is on the inside, and then the negative electrode layer 30 may be arranged on the surface on the conductive layer 42 side, and then the long laminate sheet may be folded along the length direction so that the surface on the conductive layer 42 side is on the inside.
[0049] The terminal connection step is a step of connecting a positive electrode terminal 24 to an end of the positive electrode layer 20 (positive electrode current collector 21) of the electrode laminate 10 via a positive electrode lead wire 23, and connecting a negative electrode terminal 34 to an end of the negative electrode layer 30 (negative electrode current collector 31) via a negative electrode lead wire 33. The positive electrode terminal 24 is connected to the end of the positive electrode layer 20 on the side where the non-conductive region 402 of the long separator 40 is arranged. The negative electrode terminal 34 is connected to the end of the negative electrode layer 30 on the side opposite to the side to which the positive electrode terminal 24 is connected.
[0050] The exterior body accommodation process is a process of accommodating the electrode stack 10, having the positive electrode terminal 24 and the negative electrode terminal 34 connected thereto, and an electrolyte (not shown) in the exterior body 50, so that portions of the positive electrode terminal 24 and the negative electrode terminal 34 are exposed to the outside. The sealing step is a step of sealing the electrode stack 10 to which the positive electrode terminal 24 and the negative electrode terminal 34 are connected, and the exterior body 50 that contains the electrolyte.
[0051] According to the secondary battery 100 of this embodiment configured as described above, the long separator 40 has the extension portion 40a that extends outward beyond the end of the positive electrode layer 20 on the side connected to the positive electrode terminal 24, so that even if the thickness of the negative electrode layer 30 changes significantly due to charging and discharging, the conductive layer 42 provided on the portion of the long separator 40 that contacts the negative electrode layer 30 is unlikely to come into contact with the positive electrode layer 20 or the positive electrode lead wire 23. Therefore, a short circuit between the positive electrode layer 20 and the negative electrode layer 30 is unlikely to occur.
[0052] According to the secondary battery 100 of this embodiment, the long separator 40 is formed such that the first fold 43 and the second fold 44 are alternately overlapped, and the positive electrode layer 20 is located at the first fold 43, and the negative electrode layer 30 is located at the second fold 44, so that the positive electrode layer 20 and the negative electrode layer 30 are less likely to be misaligned. In addition, the end of the conductive region 401 on the positive electrode terminal 24 side is located inside the end of the negative electrode layer 30 on the positive electrode terminal 24 side, and the end of the extension portion 40a is the non-conductive region 402, so that the conductive layer 42 is less likely to come into contact with the positive electrode layer 20 or the positive electrode lead wire 23. Furthermore, the non-conductive region 402 is disposed only at the end of the long separator 40 on the positive electrode terminal 24 side, and the area other than the end of the extension portion 40a is the conductive region 401, and the contact area between the conductive layer 42 and the negative electrode layer 30 is large, so that it is possible to suppress a short circuit caused by dendrites and a decrease in the density of the active material layer of the negative electrode layer in a charged state.
[0053] According to the secondary battery 100 of this embodiment, the end of the positive electrode layer 20 on the side opposite to the side connected to the positive electrode terminal 24 (the side where the negative electrode layer 30 connects to the negative electrode terminal 34) is located more inward than the end of the long separator 40, making it even less likely that the end of the positive electrode layer 20 on the side opposite to the side connected to the positive electrode terminal 24 will come into contact with the conductive layer 42 of the long separator 40.
[0054] Moreover, according to the method for producing the secondary battery 100 of this embodiment, the above-mentioned secondary battery 100 can be produced industrially advantageously.
[0055] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments and can be modified as appropriate. In the secondary battery 100 of this embodiment, the long separator 40 is used, but the separator is not limited thereto. Separator sheets may be interposed between the multiple positive electrode layers 20 and the negative electrode layers 30. In this case, an extension portion is provided for each separator sheet, which extends outward beyond the end of the positive electrode layer on the side connected to the positive electrode terminal, and at least a part of the surface of the separator sheet on the negative electrode layer side that contacts the negative electrode layer is made into a conductive region where a conductive layer is provided, and at least a part of the end of the extension portion on the positive electrode terminal side is made into a non-conductive region where no conductive layer is provided.
[0056] In the secondary battery 100 of this embodiment, the negative electrode layer 30 uses a metallic lithium layer deposited during charging as the negative electrode active material layer, but the negative electrode active material layer is not limited thereto. As the negative electrode active material layer, a layer containing a negative electrode active material that absorbs lithium during charging and releases lithium during discharging may be used. As the negative electrode active material, lithium transition metal oxides such as lithium titanate, transition metal oxides such as TiO2, Nb2O3 and WO3, SiO, metal sulfides, metal nitrides, and carbon materials such as artificial graphite, natural graphite, graphite, soft carbon and hard carbon can be used. In addition, as the negative electrode active material, a metal that forms an alloy with lithium can be used. Examples of metals that form an alloy with lithium include Mg, Si, Au, Ag, In, Ge, Sn, Pb, Al and Zn.
[0057] The long separator 40 may have an extension extending in the length direction, and the extension may be wound around the outer surface of the electrode stack 10 so that the surface on the long insulating porous membrane 41 side is on the outer side. By winding the extension around the outer surface of the electrode stack 10, a restraining force is imparted to the electrode stack 10 by the extension, making it more difficult for the positive electrode layer 20 and the negative electrode layer to become misaligned.
[0058] [Experimental Example] The effect of a secondary battery in which a laminate in which a conductive layer is laminated on the surface of an insulating porous film is used as a separator and the conductive layer is arranged on the negative electrode layer side will be described with reference to an experimental example.
[0059] [Experimental Example 1] (Preparation of separator) An insulating porous membrane (film thickness: 20 μm, porosity: 58%, air permeability: 92 sec / 100 mL) was prepared. A copper conductive layer having a thickness of 0.08 μm was formed on one surface of the insulating porous membrane by RF sputtering. The insulating porous membrane with the copper conductive layer formed thereon was punched out to a size of 40 mm × 50 mm to prepare a separator.
[0060] (Preparation of positive electrode layer) Acetylene black (AB) as an electron conductive material, polyvinylidene fluoride (PVDF) as a binder, and polyvinylpyrrolidone (PVP) as a dispersant were premixed with N-methyl-2-pyrrolidone (NMP) as a dispersion solvent, and wet-mixed in a planetary centrifugal mixer to obtain a premixed slurry. 0.8 Co 0.1 Mn 0.1 O2 (NCM811) and the pre-dope material were mixed with the obtained premixed slurry, and a dispersion process was performed using a planetary mixer to obtain a positive electrode active material paste. NCM811 has a median diameter of 12 μm. Next, the obtained positive electrode active material paste was applied to an aluminum positive electrode collector not having a primer layer, dried, pressed with a roll press, and then dried in a vacuum at 120 ° C. to form a positive electrode plate having a positive electrode active material layer. The obtained positive electrode plate was punched out to a size of 30 mm × 40 mm to form a positive electrode layer.
[0061] (Preparation of negative electrode layer) Copper foil with a thickness of 10 μm (electrical conductivity: 6.5 × 10 6 A clad material was prepared by bonding a 20 μm-thick lithium foil and a 100 μm-thick ...
[0062] (electrolyte) An electrolyte was prepared by dissolving LiFSI in 1,2-dimethoxyethane (DME) at a concentration of 4 mol / L.
[0063] (Preparation of lithium metal secondary batteries) A copper conductive layer of a separator was laminated on the lithium foil side of the negative electrode current collector, and a positive electrode active material layer of a positive electrode layer was laminated on the surface opposite to the copper conductive layer of the separator to produce an electrode laminate in which the negative electrode layer, separator, and positive electrode layer were laminated in this order. Next, a positive electrode terminal was attached to the positive electrode current collector of the obtained electrode laminate via a positive electrode lead wire, and a negative electrode terminal was attached to the copper foil of the negative electrode current collector via a negative electrode lead wire. The laminate with the positive electrode terminal and negative electrode terminal attached was placed in a laminate film bag, and then an electrolyte was added, and the laminate film bag was sealed to produce a lithium metal secondary battery.
[0064] [Experimental Example 2] A lithium metal secondary battery was produced in the same manner as in Experimental Example 1, except that in the production of the separator, a zinc conductive layer having a thickness of 0.06 μm was formed by RF sputtering instead of the copper conductive layer.
[0065] [Experimental Example 3] A lithium metal secondary battery was produced in the same manner as in Experimental Example 1, except that a carbon nanotube (CNT) conductive layer having a thickness of 2.1 μm was formed by coating instead of a copper conductive layer in the production of a separator. The carbon nanotube conductive layer was formed as follows. First, carbon nanotubes were added in an amount such that the solid content concentration was 4 mass% using N-methyl-N-pyrrolidinone (NMP) as a solvent, and PVDF (#9300, manufactured by Kureha Corporation) was added as a binder in an amount of 5 mass parts per 95 mass parts of carbon nanotubes. Next, a dispersion treatment was performed for 10 minutes using a rotation / revolution mixer at 1000 rpm to prepare a coating liquid. The obtained coating liquid was applied to the surface of an insulating porous film using a doctor blade and dried.
[0066] [Experimental Example 4] A lithium metal secondary battery was produced in the same manner as in Experimental Example 1, except that in the production of the separator, a tin conductive layer having a thickness of 0.06 μm was formed by RF sputtering instead of the copper conductive layer.
[0067] [Comparative Experiment Example 1] A lithium metal secondary battery was produced in the same manner as in Experimental Example 1, except that in the production of the separator, no copper conductive layer was formed.
[0068] [evaluation] The electrical conductivity, surface resistivity, and peel strength of the conductive layer of the separator prepared in each experiment were measured by the following methods. The results are shown in Table 1 together with the material, coating method, and thickness of the conductive layer of the separator. The lithium metal secondary batteries fabricated in each of the experimental examples and comparative experimental examples were measured for the presence or absence of short circuits and the rate of lithium thickness increase by the following methods. The results are shown in Table 1.
[0069] (Electrical conductivity and surface resistivity of conductive layer) The electrical conductivity and surface resistivity were measured using a high-precision, high-performance resistivity meter (Nitto Seiko Analytech Co., Ltd., Loresta GP TCP-600).
[0070] (peel strength) A conductive layer 5.0 cm long and 2.5 cm wide was attached to a 2.5 cm wide adhesive tape that was attached to a fixed plate. One end of the conductive layer was then folded back 180 degrees and pulled up at a speed of 300 mm / min using an electric measuring stand (manufactured by Imada Co., Ltd.) to peel the conductive layer from the insulating porous film. The load required from the start of peeling the conductive layer to the end of peeling was measured using a digital force gauge (manufactured by Imada Co., Ltd.). The average value of the load obtained was divided by the width of the adhesive tape to obtain the peel strength.
[0071] (Whether or not there is a short circuit in the lithium metal secondary battery) The lithium metal secondary battery immediately after fabrication was left to stand at a measurement temperature of 25° C. for 24 hours. After leaving the lithium metal secondary battery stationary, the first charge / discharge cycle described below was performed for three cycles, and then the second charge / discharge cycle described below was performed for 50 cycles to check whether or not the lithium metal secondary battery had a short circuit. If the charge capacity of the lithium metal secondary battery was 105% or more of the discharge capacity before charging, it was deemed that a short circuit had occurred, and it was deemed that a short circuit had occurred.
[0072] (First charge / discharge cycle) The charging was performed under the conditions of constant current charging at a current value of 2.2 mA up to 4,300 V, followed by constant voltage charging for 60 minutes at a voltage value of 4,300 V. The discharging was performed under the conditions of constant current discharging at a current value of 4 mA down to 2.65 V. The battery was left to stand for 30 minutes between discharging and charging.
[0073] (2nd charge / discharge cycle) The charging conditions were constant current charging at 74 mA to 3.823 V, 52 mA to 4.051 V, 46 mA to 4.173 V, and 22 mA to 4.300 V, followed by constant voltage charging for 90 minutes at 4.300 V. The discharging conditions were constant current discharging at 18 mA to 2.65 V. The battery was left to stand for 30 minutes between discharging and charging.
[0074] (Lithium thickness increase rate in lithium metal secondary batteries) The thickness T1 (μm) of the negative electrode layer at the initial charge and the thickness T2 (μm) of the negative electrode layer at the charge after 50 cycles (total thickness of the negative electrode current collector and metallic lithium layer) were measured, and the lithium thickness increase rate T (μm / cycle) was calculated using the following formula. T(μm / cycle)=(T2-T1) / 50
[0075] The thickness T1 (μm) of the negative electrode layer during the initial charge was measured as follows. The lithium metal secondary battery immediately after fabrication was left to stand at a measurement temperature of 25° C. for 24 hours. The lithium metal secondary battery after standing was subjected to the first charge / discharge cycle for three cycles. Next, constant current charging was performed at a current value of 14.7 mA up to 4,300 V, followed by constant voltage charging at a voltage value of 4,300 V for 60 minutes to charge the lithium metal secondary battery. The charged lithium metal secondary battery was left standing for 30 minutes, disassembled, and the negative electrode layer was taken out and its thickness was measured as the thickness T1 of the negative electrode layer.
[0076] The thickness T2 of the negative electrode layer during charging after 50 cycles was measured as follows. The lithium metal secondary battery immediately after fabrication was left to stand at a measurement temperature of 25° C. for 24 hours. The lithium metal secondary battery after standing was subjected to the first charge / discharge cycle three cycles, and then the second charge / discharge cycle 50 cycles. The lithium metal secondary battery was then charged by performing a constant current charge to 4.300 V at a current value of 14.7 mA, followed by a constant voltage charge at a voltage value of 4.300 V for 60 minutes. The charged lithium metal secondary battery was then left to stand for 30 minutes, disassembled, and the negative electrode layer was removed and its thickness was measured as the thickness T2 of the negative electrode layer.
[0077] [Table 1]
[0078] As shown in Table 1, the lithium metal secondary batteries of Experimental Examples 1 to 4, which are equipped with separators having conductive layers, are less likely to short-circuit even when repeatedly charged and discharged, have a low rate of lithium thickness increase, and produce a metallic lithium layer (negative electrode active material layer) that is dense and has high density when charged. In contrast, the lithium metal secondary battery of Comparative Experimental Example 1, which is equipped with a separator without a conductive layer, is more likely to short-circuit when repeatedly charged and discharged, and has a high rate of lithium thickness increase, which shows that a coarse and low-density negative electrode active material layer is produced when charged. [Explanation of symbols]
[0079] 10 Electrode laminate 20 Positive electrode layer 21 Positive electrode current collector 22 Cathode active material layer 23 Positive lead wire 24 Positive terminal 30 Negative electrode layer 31 Negative electrode current collector 33 Negative lead wire 34 Negative terminal 40 Long separator 40a Extension 401 Conductive area 402 Non-conductive area 41 Long insulating porous film 41a Hole 42 Conductive layer 43 1st Turnaround 43a Tip 43b opening 44 2nd Turnaround 44a Tip 44b opening 50 Exterior body 100 Secondary battery
Claims
1. an electrode stack including a positive electrode layer, a negative electrode layer, and a separator disposed between the positive electrode layer and the negative electrode layer; An electrolyte; an exterior body that accommodates the electrode stack and the electrolyte; A positive electrode terminal and a negative electrode terminal provided on the exterior body; a positive electrode lead wire electrically connecting the positive electrode layer and the positive electrode terminal; a negative electrode lead wire electrically connecting the negative electrode layer and the negative electrode terminal, the separator has an extension portion that extends outward beyond an end of the positive electrode layer on a side connected to the positive electrode terminal, at least a part of a portion of a surface of the separator on the negative electrode layer side that is in contact with the negative electrode layer is a conductive region having a conductive layer provided thereon, and at least a part of an end of the extension portion on the positive electrode terminal side is a non-conductive region on which the conductive layer is not provided.
2. The separator includes a long insulating porous membrane, and the conductive region and the non-conductive region provided on one surface of the long insulating porous membrane, the conductive region extending along the length direction of the long insulating porous membrane, the non-conductive region being disposed at least at one end in the width direction of the long insulating porous membrane, and the separator is formed so that a first fold folded along the length direction so that the surface facing the long insulating porous membrane is on the inside and a second fold folded along the length direction so that the surface on the side where the conductive region and the non-conductive region are disposed is on the inside are alternately overlapped, the positive electrode layer is sandwiched between the first fold and the non-conductive region is located at a position that becomes the extension portion, and the negative electrode layer is sandwiched between the second fold and is located in contact with the conductive region, the positive electrode terminal is electrically connected to an end of the positive electrode layer on the side where the non-conductive region is disposed; The secondary battery according to claim 1 , wherein the negative electrode terminal is electrically connected to an end of the negative electrode layer opposite to the end on which the non-conductive region is disposed.
3. The secondary battery according to claim 1 , wherein an end of the conductive region on the positive electrode terminal side is located at the same position as or inside an end of the negative electrode layer on the positive electrode terminal side.
4. The secondary battery according to claim 1 , wherein the non-conductive region is disposed only at an end of the separator on the positive electrode terminal side.
5. 2. The secondary battery according to claim 1, wherein the negative electrode active material is metallic lithium.
6. a step of producing a long separator including a long insulating porous membrane, a conductive region provided with a conductive layer disposed on one surface of the long insulating porous membrane, and a non-conductive region not provided with a conductive layer, the conductive region extending along the length of the long insulating porous membrane, and the non-conductive region disposed at at least one end in the width direction of the long insulating porous membrane, by zigzag folding a long laminated sheet to form a first fold folded along the length direction so that the surface on the long insulating porous membrane side faces inward, and a second fold folded along the length direction so that the surfaces on the side where the conductive region and the non-conductive region are disposed face inward, the first fold being alternately overlapped; disposing a positive electrode layer on the first fold and a negative electrode layer on the second fold so that they face each other; connecting a positive electrode terminal via a positive electrode lead wire to an end of the positive electrode layer on a side where the non-conductive region is located, and connecting a negative electrode terminal via a negative electrode lead wire to an end of the negative electrode layer opposite to the side to which the positive electrode terminal is connected.
Citation Information
Patent Citations
Active material for batteries, electrode, nonaqueous electrolyte battery and battery pack
JP2015084320A
Lithium secondary battery
JP2016225261A
Porous separator and lithium secondary battery including same
JP2021534562A
Separator laminate for lithium secondary battery, electrode assembly including the same, and lithium secondary battery
JP2022519361A
Secondary battery and method of manufacturing the same
JP2022552536A
Cited By
Non-aqueous electrolyte secondary battery
WO2026205532A1