Secondary cell and secondary cell system

Using silicon particles with a clathrate structure and controlling the basis weight ratio in silicon-based batteries addresses durability issues, enhancing their structural integrity and capacity retention.

JP2024144468AActive Publication Date: 2024-10-11TOYOTA JIDOSHA KK
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024116902
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-11
Estimated Expiration
2041-12-28

AI Technical Summary

Technical Problem

Batteries using silicon-based negative electrode active materials face durability issues due to significant expansion and contraction during charging and discharging, leading to particle cracking and reduced energy density.

Method used

Employing silicon particles with a clathrate structure as the negative electrode active material and maintaining a specific ratio of basis weight between the Li-containing compound in the positive electrode and silicon particles in the negative electrode, along with controlling the charging voltage to 4.2V or less, to minimize expansion and maintain structural integrity.

Benefits of technology

The solution enhances the durability and capacity retention of secondary batteries by reducing the utilization rate of silicon particles, suppressing expansion, and preventing structural collapse, thereby improving long-term performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144468000001_ABST
    Figure 2024144468000001_ABST
Patent Text Reader

Abstract

To improve durability of a secondary cell using silicon negative electrode active materials.SOLUTION: A secondary cell includes a negative electrode 10, an electrolyte layer 20, and a positive electrode 30, the negative electrode 10 including Si particles as negative electrode active materials, the positive electrode 30 including Li-containing compounds as positive electrode active materials, the Si particles having a clathrate structure, where a ratio C1 / C2 of a basis weight C1 of the Li-containing compounds in the positive electrode 30 to a basis weight C2 of the Si particles in the negative electrode 10 is equal to or larger than 3.40 and equal to or smaller than 8.33.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application discloses a secondary battery and a secondary battery system using a silicon-based negative electrode active material. [Background technology]

[0002] Batteries using silicon-based negative electrode active materials are known. For example, Patent Document 1 discloses a lithium ion secondary battery using silicon oxide as the negative electrode active material. Patent Document 2 discloses a lithium ion secondary battery using silicon clathrate II as the negative electrode active material. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-113547 A [Patent Document 2] Patent Publication No. 2021-034279 Summary of the Invention [Problem to be solved by the invention]

[0004] There is room for improvement in the durability of batteries using silicon-based negative electrode active materials. [Means for solving the problem]

[0005] As one of the means for solving the above problems, the present application provides: A secondary battery having a negative electrode, an electrolyte layer, and a positive electrode, The negative electrode has Si particles as a negative electrode active material, The positive electrode has a Li-containing compound as a positive electrode active material, The Si particles have a clathrate structure, a ratio C1 / C2 of a basis weight C1 of the Li-containing compound in the positive electrode to a basis weight C2 of the Si particles in the negative electrode is 8.33 or less; secondary battery Disclose.

[0006] In the secondary battery of the present disclosure, the ratio C1 / C2 may be 2.87 or more.

[0007] In the secondary battery of the present disclosure, The Li-containing compound may contain at least Li, at least one of Ni, Co, and Mn, and O as constituent elements.

[0008] As one of the means for solving the above problems, the present application provides: A secondary battery according to the present disclosure; A control unit that controls charging and discharging of the secondary battery; Equipped with The control unit controls the charging voltage of the secondary battery to 4.2 V or less. Secondary Battery System Disclose. Effect of the Invention

[0009] The secondary battery of the present disclosure has excellent durability. [Brief description of the drawings]

[0010] [Figure 1] 1 shows a schematic configuration of a secondary battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] 1. Secondary battery The secondary battery of the present disclosure has a negative electrode, an electrolyte layer, and a positive electrode. Here, the negative electrode has Si particles as a negative electrode active material, and the positive electrode has a Li-containing compound as a positive electrode active material. The Si particles have a clathrate structure. The ratio C1 / C2 of the basis weight C1 of the Li-containing compound in the positive electrode to the basis weight C2 of the Si particles in the negative electrode is 8.33 or less. FIG. 1 shows a schematic configuration of a secondary battery 100 according to an embodiment. As shown in FIG. 1, the secondary battery 100 has a negative electrode 10, an electrolyte layer 20, and a positive electrode 30.

[0012] 1.1 Negative electrode The negative electrode 10 contains Si particles as a negative electrode active material. As shown in Fig. 1, the negative electrode 10 may include a negative electrode active material layer 11 and a negative electrode current collector 12. In this case, the negative electrode active material layer 11 may contain Si particles as a negative electrode active material.

[0013] 1.1.1 Negative electrode active material layer The negative electrode active material layer 11 contains Si particles as the negative electrode active material, and may further contain an electrolyte, a conductive assistant, a binder, and the like. The negative electrode active material layer 11 may also contain various additives. The content of each component in the negative electrode active material layer 11 is not particularly limited, and may be appropriately determined according to the performance of the intended battery. For example, the content of the negative electrode active material may be 40 mass% or more, 50 mass% or more, or 60 mass% or more, and may be 100 mass% or less, or 90 mass% or less, assuming that the entire negative electrode active material layer 11 (total solid content) is 100 mass%. The thickness of the negative electrode active material layer 11 is also not particularly limited, and may be, for example, 1 μm or more, 10 μm or more, or 30 μm or more, and may be 1 mm or less, 500 μm or less, or 100 μm or less.

[0014] The Si particles as the negative electrode active material have a clathrate structure. When the Si particles have a clathrate structure, the expansion and contraction of the Si particles accompanying the charging and discharging of the battery becomes relatively small, and the durability of the battery is easily improved. Whether or not the Si particles have a clathrate structure can be easily determined from Raman spectroscopy, XRD, and the like. In the present application, the 325±10 cm -1 Maximum peak intensity at I 325 and 205±10cm -1 Maximum peak intensity at I 205 Comparison with I 325 / I 205 is in the range of 1.03 to 1.21, the Si particles are considered to have a clathrate structure. The Si particles as the negative electrode active material may have an oxide film or may contain impurities such as carbon.

[0015] The size of the Si particles as the negative electrode active material is not particularly limited. The average particle size of the Si particles may be, for example, 0.1 μm or more, 0.3 μm or more, 0.5 μm or more, or 0.7 μm or more, and may be 50 μm or less, 30 μm or less, 10 μm or less, or 5 μm or less. The average particle size of the Si particles is the particle size (median size) at an integrated value of 50% in the volume-based particle size distribution obtained by a laser diffraction / scattering method.

[0016] The negative electrode active material layer 11 may contain other negative electrode active materials in addition to the above-mentioned Si particles as the negative electrode active material. For example, the negative electrode active material layer 11 may contain at least one selected from silicon-based active materials such as Si, Si alloys, and silicon oxide other than clathrate silicon; carbon-based active materials such as graphite and hard carbon; various oxide-based active materials such as lithium titanate; metallic lithium, lithium alloys, and the like as the other negative electrode active materials. The proportion of Si particles having a clathrate structure in the negative electrode active material contained in the negative electrode active material layer 11 may be, for example, more than 50 mass%, 70 mass% or more, 90 mass% or more, or 95 mass% or more. Alternatively, the negative electrode active material layer 11 may contain only Si particles having a clathrate structure as the negative electrode active material.

[0017] The electrolyte may be a solid electrolyte or a liquid electrolyte (electrolytic solution). When the secondary battery 100 is an all-solid-state battery, the negative electrode active material layer 11 may contain a solid electrolyte as the electrolyte. When the secondary battery 100 is an electrolyte battery, the negative electrode active material layer 11 may contain an electrolyte as the electrolyte.

[0018] The solid electrolyte may be any known solid electrolyte for secondary batteries. The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, inorganic solid electrolytes are preferred because of their excellent ionic conductivity and heat resistance. Examples of inorganic solid electrolytes include lithium lanthanum zirconate, LiPON, and Li 1+X Al X Ge 2-XExamples of the solid electrolyte include oxide solid electrolytes such as (PO4)3, Li-SiO-based glass, and Li-Al-SO-based glass; and sulfide solid electrolytes such as Li2S-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Si2S-P2S5, Li2S-P2S5-LiI-LiBr, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, and Li2S-P2S5-GeS2. In particular, the performance of the sulfide solid electrolyte, particularly the sulfide solid electrolyte containing Li2S-P2S5, is high. The solid electrolyte may be amorphous or crystalline. The solid electrolyte may be, for example, particulate. Only one type of solid electrolyte may be used alone, or two or more types may be used in combination.

[0019] The electrolyte may contain, for example, lithium ions as carrier ions. The electrolyte may be an aqueous electrolyte or a non-aqueous electrolyte. The composition of the electrolyte may be the same as that of the electrolyte of a lithium ion battery. For example, the electrolyte may be a carbonate-based solvent in which a lithium salt is dissolved at a predetermined concentration. Examples of the carbonate-based solvent include fluoroethylene carbonate (FEC), ethylene carbonate (EC), and dimethyl carbonate (DMC). Examples of the lithium salt include LiPF6.

[0020] Examples of the conductive assistant include carbon materials such as vapor grown carbon fiber (VGCF), acetylene black (AB), ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF); and metal materials such as nickel, aluminum, and stainless steel. The conductive assistant may be, for example, particulate or fibrous, and the size is not particularly limited. Only one type of conductive assistant may be used alone, or two or more types may be used in combination.

[0021] Examples of the binder include polyimide (PI)-based binders, butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, and polytetrafluoroethylene (PTFE)-based binders. In particular, when the negative electrode active material layer 11 contains polyimide as a binder, the expansion and contraction of the Si particles is more easily suppressed. The polyimide may be obtained by heating a polyamic acid to cause an imidization reaction (dehydration and cyclization). The polyamic acid may be aromatic or aliphatic, but is preferably one having an aromatic ring from the viewpoint of being a high-strength binder when it becomes a polyimide. Only one type of binder may be used alone, or two or more types may be used in combination.

[0022] 1.1.2 Negative electrode current collector The negative electrode current collector 12 may be any of those generally used as negative electrode current collectors for secondary batteries. The negative electrode current collector 12 may be in the form of a foil, a plate, a mesh, a punched metal, or a foam. The negative electrode current collector 12 may be a metal foil or a metal mesh, or may be a carbon sheet. In particular, metal foil is excellent in terms of ease of handling. The negative electrode current collector 12 may be made of a plurality of foils or sheets. Examples of metals constituting the negative electrode current collector 12 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, and the like. In particular, from the viewpoint of ensuring reduction resistance and being difficult to alloy with lithium, the negative electrode current collector 12 may contain at least one metal selected from Cu, Ni, and stainless steel. The negative electrode current collector 12 may have some kind of coating layer on its surface for the purpose of adjusting resistance, etc. The negative electrode current collector 12 may be a metal foil or a substrate plated or vapor-deposited with the above metal. When the negative electrode current collector 12 is made of a plurality of metal foils, some layer may be present between the plurality of metal foils. The thickness of the negative electrode current collector 12 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0023] 1.2 Electrolyte layer The electrolyte layer 20 contains at least an electrolyte. When the secondary battery 100 is a solid battery (a battery containing a solid electrolyte that may or may not contain liquid), the electrolyte layer 20 contains a solid electrolyte and may further contain a binder or the like. In this case, the content of the solid electrolyte and the binder or the like in the electrolyte layer 20 is not particularly limited. On the other hand, when the secondary battery 100 is an electrolyte battery, the electrolyte layer 20 contains an electrolyte solution and may further have a separator or the like for holding the electrolyte solution and preventing contact between the negative electrode 10 and the positive electrode 30. The thickness of the electrolyte layer 20 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.

[0024] The solid electrolyte, the electrolytic solution, the binder, and the like are as described above. The separator may be any separator that is normally used in secondary batteries, and may be made of resin such as polyethylene (PE), polypropylene (PP), polyester, and polyamide. The separator may have a single layer structure or a multi-layer structure. Examples of the multi-layer structure separator include a separator with a two-layer structure of PE / PP, or a separator with a three-layer structure of PP / PE / PP or PE / PP / PE. The separator may be made of a nonwoven fabric such as a cellulose nonwoven fabric, a resin nonwoven fabric, or a glass fiber nonwoven fabric.

[0025] 1.3 Positive electrode 1, the positive electrode 30 may include a positive electrode active material layer 31 and a positive electrode current collector 32. In this case, the positive electrode active material layer 31 may include a positive electrode active material.

[0026] 1.3.1 Cathode active material layer The positive electrode active material layer 31 includes a positive electrode active material, and may further include an electrolyte, a conductive assistant, a binder, and the like. The positive electrode active material layer 31 may also include various additives. The content of each component in the positive electrode active material layer 31 is not particularly limited, and may be appropriately determined according to the performance of the intended battery. For example, the content of the positive electrode active material may be 50 mass% or more, 60 mass% or more, or 70 mass% or more, and may be 100 mass% or less, or 90 mass% or less, with the entire positive electrode active material layer 31 being taken as 100 mass%. The thickness of the positive electrode active material layer 31 is also not particularly limited, and may be, for example, 1 μm or more, 10 μm or more, or 30 μm or more, and may be 1 mm or less, 500 μm or less, or 100 μm or less.

[0027] The positive electrode active material may be any known positive electrode active material for secondary batteries. Among known active materials, a material that exhibits a potential (charge / discharge potential) at which lithium ions, which are carrier ions, are absorbed and released that is higher than the charge / discharge potential of the Si particles having the clathrate structure can be used as the positive electrode active material. Examples of such positive electrode active materials include various Li-containing compounds. More specifically, lithium cobalt oxide, lithium nickel oxide, Li 1±α Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O 2±δ , lithium manganate, lithium spinel compounds (Li 1+x Mn 2-x-y M y Various lithium-containing oxides such as Li-Mn spinel substituted with different elements having a composition represented by LiMPO4 (where M is one or more selected from Al, Mg, Co, Fe, Ni, and Zn), lithium titanate, and lithium metal phosphate (LiMPO4, where M is one or more selected from Fe, Mn, Co, and Ni) may be used. In particular, when the Li-containing compound as the positive electrode active material contains at least Li, at least one of Ni, Co, and Mn, and O as constituent elements, a higher effect can be expected. Only one type of positive electrode active material may be used alone, or two or more types may be used in combination. The positive electrode active material may be, for example, particulate, and the size is not particularly limited. The particles of the positive electrode active material may be solid particles or hollow particles. The particles of the positive electrode active material may be primary particles, or may be secondary particles in which a plurality of primary particles are aggregated. The average particle size of the particles of the positive electrode active material may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less.

[0028] A protective layer containing a Li-ion conductive compound may be formed on the surface of the positive electrode active material. That is, the positive electrode active material layer 31 may include a composite having a positive electrode active material and a protective layer provided on the surface of the positive electrode active material. This makes it easier to suppress reactions between the positive electrode active material and sulfides (such as sulfide solid electrolytes). Examples of Li-ion conductive compounds include Li3BO3, LiBO2, Li2CO3, LiAlO2, Li4SiO4, Li2SiO3, Li3PO4, Li2SO4, Li2TiO3, and Li4Ti5O. 12 , Li2Ti2O5, Li2ZrO3, LiNbO3, Li2MoO4, and Li2WO4. The coverage (area ratio) of the protective layer on the surface of the positive electrode active material may be, for example, 70% or more, 80% or more, or 90% or more. The thickness of the protective layer may be, for example, 0.1 nm or more or 1 nm or more, and may be 100 nm or less, or 20 nm or less.

[0029] The electrolyte, conductive assistant, and binder may be selected from those exemplified as those that can be contained in the negative electrode active material layer 11. The electrolyte, conductive assistant, and binder may each be used alone or in combination of two or more kinds.

[0030] 1.3.2 Positive electrode current collector The positive electrode collector 32 may be any of those generally used as a positive electrode collector for a secondary battery. The positive electrode collector 32 may be in the form of a foil, a plate, a mesh, a punched metal, or a foam. The positive electrode collector 32 may be made of a metal foil or a metal mesh. In particular, a metal foil is excellent in terms of ease of handling. The positive electrode collector 32 may be made of a plurality of foils. Examples of metals constituting the positive electrode collector 32 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, and stainless steel. In particular, the positive electrode collector 32 may contain Al from the viewpoint of ensuring oxidation resistance. The positive electrode collector 32 may have some kind of coating layer on its surface for the purpose of adjusting resistance. The positive electrode collector 32 may be a metal foil or a base material on which the above metal is plated or vapor-deposited. In addition, when the positive electrode current collector 32 is made of multiple metal foils, some layer may be present between the multiple metal foils. The thickness of the positive electrode current collector 32 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0031] 1.4 Weight of active material Conventionally, negative electrodes using Si particles as the negative electrode active material have attracted attention as they have a high energy density. However, when Si particles are used as the negative electrode active material, the Si particles expand and contract significantly during charging and discharging, and the particles are prone to cracking. Until now, the adverse effects of the expansion and contraction of Si particles have been suppressed by silicidation of Si or mixing with graphite, but in this case, the ratio of other elements increases, and in some cases, elements other than Si account for 50 mass% or more, which may cause a decrease in energy density.

[0032] On the other hand, Si particles having a clathrate structure have small expansion and contraction during charging and discharging, and are easier to improve the durability of the secondary battery compared to normal Si particles. In addition, according to the new findings of the present inventor, when Si particles having a clathrate structure are used as the negative electrode active material, there is a correlation between the utilization capacity of the negative electrode during charging (utilization rate of Si particles, i.e., Li absorption rate of Si particles) and the durability of the secondary battery. That is, the lower the utilization rate of Si particles having a clathrate structure, the higher the ratio of non-expansion regions, and the more significantly the amount of expansion and contraction can be reduced. In addition, it is possible to suppress the collapse of the clathrate structure due to excessive expansion and contraction, and the clathrate structure is easily maintained even when charging and discharging are repeated. As a result, the durability of the secondary battery is further improved. Here, as far as the present inventor has confirmed, the utilization rate of Si particles during charging is approximately 1:1 correlated with the basis weight of the positive and negative electrode active materials. That is, the greater the basis weight of the positive electrode active material and the smaller the basis weight of the negative electrode active material, the higher the utilization rate of the negative electrode active material.

[0033] In the secondary battery 100, it is important that the ratio C1 / C2 between the weight C1 of the Li-containing compound in the positive electrode 30 and the weight C2 of the Si particles in the negative electrode 10 is 8.33 or less. By making the ratio C1 / C2 8.33 or less, the utilization rate of the Si particles is sufficiently reduced as described above, and the expansion of the Si particles during charging is suppressed. As a result, the durability of the secondary battery 100 can be improved, and the capacity of the secondary battery 100 is unlikely to decrease even if it is repeatedly charged and discharged. In addition, the lower limit value of the ratio C1 / C2 may be set within a range that ensures the capacity required for the secondary battery 100. For example, the ratio C1 / C2 is preferably 0.50 or more, 1.00 or more, 1.50 or more, 2.00 or more, 2.50 or more, 2.87 or more, 3.00 or more, or 3.40 or more.

[0034] The weight of the Si particles in the negative electrode 10 and the weight of the Li-containing compound in the positive electrode 30 can be appropriately adjusted according to the intended battery performance within a range in which the above ratio C1 / C2 is satisfied. The weight of the Si particles in the negative electrode 10 is, for example, 0.1 mg / cm 2 More than 0.5mg / cm 2 More than 1.0mg / cm2 More than 1.5mg / cm 2 or more than 2.0 mg / cm 2 or more, 10.0 mg / cm 2 Below, 8.5mg / cm 2 Less than or equal to 7.0 mg / cm 2 The weight per unit area of ​​the Li-containing compound in the positive electrode 30 may be, for example, 0.5 mg / cm 2 More than 1.0mg / cm 2 More than 12.5mg / cm 2 or more, or 15.0 mg / cm2 or more, and 40.0 mg / cm 2 Below 30mg / cm 2 Less than or equal to 25.0 mg / cm 2 may be also possible.

[0035] The basis weight of the active material in the electrode can be determined by various methods. For example, the basis weight of the active material can be determined by observing the cross section of the electrode with a SEM or the like and determining the ratio of the active material contained in the active material layer by elemental analysis or the like. Alternatively, the active material layer can be peeled off from the secondary battery, the mass of the active material contained in the active material layer can be measured, and the basis weight of the active material can be determined from this and the area of ​​the electrode.

[0036] 1.5 Other configurations The secondary battery 100 may have the above-mentioned components housed inside an exterior body. Any known exterior body for a battery can be used as the exterior body. A plurality of secondary batteries 100 may be electrically connected and stacked in any manner to form an assembled battery. In this case, the assembled battery may be housed inside a known battery case. The secondary battery 100 may also have other obvious components such as necessary terminals. The shape of the secondary battery 100 may be, for example, a coin type, a laminate type, a cylindrical type, a square type, or the like.

[0037] 1.6 Manufacturing method of secondary batteries The secondary battery 100 can be manufactured by applying a known method. For example, it can be manufactured as follows. However, the manufacturing method of the secondary battery 100 is not limited to the following method, and each layer may be formed by, for example, dry molding. (1) The negative electrode active material constituting the negative electrode active material layer is dispersed in a solvent to obtain a negative electrode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. The negative electrode layer slurry is then applied to the surface of a negative electrode current collector using a doctor blade or the like, and then dried to form a negative electrode active material layer on the surface of the negative electrode current collector, thereby forming a negative electrode. (2) The positive electrode active material constituting the positive electrode active material layer is dispersed in a solvent to obtain a positive electrode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. The positive electrode layer slurry is applied to the surface of a positive electrode current collector using a doctor blade or the like, and then dried to form a positive electrode active material layer on the surface of the positive electrode current collector, forming a positive electrode. (3) An electrolyte layer (solid electrolyte layer or separator) is sandwiched between the negative electrode and the positive electrode to obtain a laminate having a negative electrode current collector, a negative electrode active material layer, an electrolyte layer, a positive electrode active material layer, and a positive electrode current collector in this order. Other members such as terminals are attached to the laminate as necessary. (4) The laminate is housed in a battery case, and in the case of an electrolyte battery, the battery case is filled with electrolyte, and the laminate is immersed in the electrolyte and sealed in the battery case to form a secondary battery. In the case of an electrolyte battery, the electrolyte may be impregnated in the negative electrode active material layer, the separator, and the positive electrode active material layer at the above step (3).

[0038] 2. Secondary Battery System The technology of the present disclosure also has an aspect as a system for controlling the charging and discharging of a secondary battery. That is, the secondary battery system of the present disclosure includes the above-mentioned secondary battery 100 and a control unit (not shown) that controls the charging and discharging of the secondary battery 100, and is characterized in that the control unit controls the charging voltage of the secondary battery 100 to 4.2 V or less. By controlling the charging voltage of the secondary battery 100 to 4.2 V or less, the utilization rate of Si particles as the negative electrode active material can be kept low, and the durability of the secondary battery 100 can be improved based on the above-mentioned mechanism.

[0039] The control unit may be any one capable of controlling the charging and discharging of the secondary battery 100 as described above. For example, when charging the secondary battery by supplying electricity from a power source to the secondary battery, the voltage of the secondary battery may be measured successively, and the supply of electricity from the power source may be continued or stopped so that the measured voltage does not exceed 4.2V, thereby continuing or stopping the charging. When the control unit controls the charging and discharging of the secondary battery 100, the lower limit of the charging voltage and the upper and lower limits of the discharging voltage of the secondary battery 100 are not particularly limited, and the lower limit of the charging voltage may be determined according to the desired battery performance. If the charging voltage is too low, sufficient performance as the secondary battery 100 may not be obtained.

[0040] 3. Supplementary Information As described above, according to the technology of the present disclosure, by using Si particles having a clathrate structure as the negative electrode active material and controlling the utilization rate of the Si particles, the ratio of the non-expansion region of the Si particles increases during charging, suppressing the expansion and contraction of the Si particles during charging and discharging, and also suppressing the collapse of the clathrate structure due to excessive expansion and contraction, so that the clathrate structure is easily maintained even when charging and discharging are repeated. As a result, the durability of the secondary battery is improved. It is believed that such an effect is achieved regardless of the type of secondary battery (electrolyte battery, solid battery). EXAMPLES

[0041] The technology of the present disclosure will be described in more detail below with reference to examples, but the technology of the present disclosure is not limited to the following examples.

[0042] 1. Preparation of silicon negative electrode active material As the silicon negative electrode active material, crystalline silicon and clathrate silicon were each prepared.

[0043] 1.1 Preparation of crystalline silicon Silicon particles (Kojundo Kagaku, 5 μm) were milled using a planetary ball mill (Fritsch Classic Line) to obtain crystalline silicon powder. The crystalline silicon did not have a clathrate structure.

[0044] 1.2 Preparation of silicon clathrate Si particles and Na particles were mixed in a molar ratio of 1:1 and heated at 700°C to synthesize NaSi. The mixture was then heated at 340°C to remove Na. The mixture was then heated at 430°C to further remove Na, after which it was pulverized using a planetary ball mill at 150 rpm for 3 hours to obtain a powder. The resulting powder had a clathrate structure (clathrate silicon).

[0045] 2. Preparation of Positive Electrode In a PP container, NMP as a solvent, a 5 wt% butyl butyrate solution of a PVDF-based binder, and LiNi as a positive electrode active material were placed. 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (average particle size 6 μm) and VGCF as a conductive additive were added and stirred for 10 minutes with a mixer (ARE-310, manufactured by Thinky Corporation) to obtain a positive electrode slurry. The positive electrode slurry was applied to an Al foil (manufactured by Showa Denko K.K.) by the blade method using an applicator. The applied electrode was dried on a hot plate at 80°C for 60 minutes. The concentration of the positive electrode slurry and the amount of application were adjusted to change the basis weight of the positive electrode active material.

[0046] 3. Preparation of the Negative Electrode NMP as a solvent, polyamic acid (U Varnish A, Ube Industries) as a binder to become polyimide, silicon active material as a negative electrode active material, and VGCF and KB as conductive assistants were added to a PP container, and stirred for 10 minutes with a mixer (ARE-310, Thinky Corporation) to obtain a negative electrode slurry. The mixture was applied to Cu foil (Furukawa Electric Co., Ltd.) by the blade method using an applicator. The coated electrode was dried on a hot plate at 80°C for 60 minutes. The concentration and coating amount of the negative electrode slurry were adjusted to change the basis weight of the negative electrode active material.

[0047] 4. Battery Preparation The prepared positive electrode was punched out to φ14 mm, while the negative electrode was punched out to φ16 mm, and then set in a roll press machine and pressed at 20 kN / cm. The negative electrode was then baked at 350 ° C for 2 h in an Ar atmosphere to cause an imidization reaction of the polyamic acid. Each electrode was moved to a glove box, and 1 ml of electrolyte (1.2 M LiPF6 solution. Solvent was FEC:EC:EMC:DMC = 1:2:4:3 vol%) was dropped onto the active material layer of the negative electrode, a separator (made of PP) was laminated, 1 ml of electrolyte was dropped again, and then the positive electrode was laminated, and a coin cell was produced using an automatic coin cell caulking machine (manufactured by Hosensha).

[0048] 4.1 Comparative Example 1 The positive electrode active material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2) basis weight of 28.480mg / cm 2 The mass of the negative electrode active material (crystalline silicon) in the negative electrode is 4.838 mg / cm 2 That is, the ratio C1 / C2 of the weight C1 of the positive electrode active material in the positive electrode to the weight C2 of the negative electrode active material in the negative electrode was set to 5.89.

[0049] 4.2 Comparative Example 2 The positive electrode active material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2) basis weight of 17.978mg / cm 2The mass of the negative electrode active material (crystalline silicon) in the negative electrode is 6.660 mg / cm 2 That is, the ratio C1 / C2 of the weight C1 of the positive electrode active material in the positive electrode to the weight C2 of the negative electrode active material in the negative electrode was set to 2.70.

[0050] 4.3 Comparative Example 3 The positive electrode active material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2) basis weight of 20.114mg / cm 2 The mass of the negative electrode active material (crystalline silicon) in the negative electrode was set to 2.050 mg / cm 2 That is, the ratio C1 / C2 of the weight C1 of the positive electrode active material in the positive electrode to the weight C2 of the negative electrode active material in the negative electrode was set to 9.81.

[0051] 4.4 Example 1 The positive electrode active material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2) basis weight of 23.674mg / cm 2 The weight of the negative electrode active material (clathrate silicon) in the negative electrode is 4.756 mg / cm 2 That is, the ratio C1 / C2 of the weight C1 of the positive electrode active material in the positive electrode to the weight C2 of the negative electrode active material in the negative electrode was set to 4.98.

[0052] 4.5 Example 2 The positive electrode active material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2) basis weight of 19.224mg / cm 2 The weight of the negative electrode active material (clathrate silicon) in the negative electrode was 5.658 mg / cm 2 That is, the ratio C1 / C2 of the weight C1 of the positive electrode active material in the positive electrode to the weight C2 of the negative electrode active material in the negative electrode was set to 3.40.

[0053] 4.6 Example 3 The positive electrode active material (LiNi 1 / 3 Co1 / 3 Mn 1 / 3 O2) basis weight of 21.182mg / cm 2 The weight of the negative electrode active material (clathrate silicon) in the negative electrode was set to 2.542 mg / cm 2 That is, the ratio C1 / C2 of the weight C1 of the positive electrode active material in the positive electrode to the weight C2 of the negative electrode active material in the negative electrode was set to 8.33.

[0054] 4.7 Comparative Example 4 The positive electrode active material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2) basis weight of 22.517mg / cm 2 The weight of the negative electrode active material (clathrate silicon) in the negative electrode was 1.804 mg / cm 2 That is, the ratio C1 / C2 of the weight C1 of the positive electrode active material in the positive electrode to the weight C2 of the negative electrode active material in the negative electrode was set to 12.48.

[0055] 5. Charge / discharge cycle test The produced coin cell was charged at a constant current of 0.2 mA to 4.2 V, and then discharged at 0.2 mA to 2.5 V, with the battery capacity at this time taken as the initial capacity. The charge-discharge test was repeated 50 times, in which the battery was charged at a constant current of 2 mA to 4.2 V, and then discharged at a constant current of 2 mA. The battery capacity was then measured at a constant current of 0.2 mA to 4.2 V, and then discharged at 0.2 mA to 2.5 V, and the ratio to the initial capacity was calculated to confirm the durability performance after 50 cycles. The durability performance of Comparative Example 1 was taken as the standard (100%), and the durability performance of Comparative Examples 2 to 4 and Examples 1 to 3 was evaluated relative to each other.

[0056] In addition, the negative electrode was taken out after the first charge and discharge and measured by Raman spectroscopy (wavelength 532 nm). The obtained Raman spectrum was analyzed and found to have a peak intensity of 325±10 cm -1 Maximum peak intensity at I 325 and 205±10cm -1 Maximum peak intensity at I 205 Comparison with I 325 / I 205 The ratio I was calculated.325 / I 205 When the ratio is within the range of 1.03 to 1.21, it can be said that the Si particles have a clathrate structure.

[0057] 6. Evaluation Results The evaluation results are shown in Table 1 below.

[0058] [Table 1]

[0059] The results shown in Table 1 reveal the following. First, a comparison between Comparative Examples 1 to 3 and Examples 1 to 3 reveals that the durability of secondary batteries is higher when clathrate silicon is used as the negative electrode active material than when crystalline silicon is used. This is believed to be due to the fact that clathrate silicon expands and contracts less during charging and discharging the battery than crystalline silicon.

[0060] Moreover, from a comparison between Comparative Example 4 and Examples 1 to 3, it is found that even if clathrate silicon is used as the negative electrode active material, when the active material area ratio C1 / C2 is too large (i.e., when there is too much positive electrode active material relative to the negative electrode active material and the utilization rate of the negative electrode active material is too high), the durability of the secondary battery is reduced. This is presumed to be due to the following mechanism. That is, in a secondary battery, it is considered that the higher the utilization rate of Si particles during charging, the greater the amount of expansion of the Si particles, and the greater the amount of expansion, the more likely the Si particles are to crack or the more likely the clathrate structure is to collapse. It is considered that in Comparative Example 4, cracking of the Si particles and collapse of the clathrate structure occurred during charging, and the capacity of the negative electrode was greatly reduced.

[0061] 7. Consideration of solid-state batteries The case where the technology of the present disclosure is applied to a solid-state battery (a battery containing a solid electrolyte as the electrolyte) was also examined.

[0062] 7.1 Preparation of the negative electrode The above negative electrode active material (crystalline silicon or clathrate silicon), sulfide solid electrolyte (Li2S-P2S5-based glass ceramic), conductive assistant (VGCF), butyl butyrate solution containing 5% by weight of PVdF-based binder, and butyl butyrate were added to a polypropylene container, and stirred for 30 seconds with an ultrasonic dispersion device (UH-50, manufactured by SMT). Next, the container was shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.). The mixture was applied to a negative electrode current collector (Cu foil, manufactured by UACJ) by the blade method using an applicator, and dried for 30 minutes on a hot plate at 100 ° C. This resulted in a negative electrode having a negative electrode current collector and a negative electrode active material layer.

[0063] 7.2 Preparation of the positive electrode The positive electrode active material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, average particle size 6μm), sulfide solid electrolyte (Li2S-P2S5-based glass ceramic), conductive assistant (VGCF), butyl butyrate solution containing 5% by weight of PVdF-based binder, and butyl butyrate were added and stirred for 30 seconds with an ultrasonic dispersion device (UH-50, manufactured by SMT). Next, the container was shaken for 3 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.). The mixture was applied to a positive electrode collector (Al foil, manufactured by Showa Denko) by the blade method using an applicator, and dried for 30 minutes on a hot plate at 100°C. This resulted in a positive electrode having a positive electrode collector and a positive electrode active material layer. The area of ​​the positive electrode was made smaller than that of the negative electrode.

[0064] 7.3 Preparation of solid electrolyte layer A sulfide solid electrolyte (Li2S-P2S5-based glass ceramic), a heptane solution containing 5% by weight of a butylene rubber-based binder, and heptane were added to a polypropylene container, and the mixture was stirred for 30 seconds with an ultrasonic dispersing device (UH-50, manufactured by SMT). Next, the container was shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.). The mixture was applied onto a release sheet (Al foil) by the blade method using an applicator, and dried on a hot plate at 100°C for 30 minutes. This resulted in a transfer member having a release sheet and a solid electrolyte layer.

[0065] 7.4 Battery Construction A solid electrolyte layer for bonding was placed on the positive electrode active material layer of the positive electrode, and the layer was set in a roll press machine and pressed at 100 kN / cm and 165°C. This resulted in a first laminate. Next, the negative electrode was set in a roll press machine and pressed at 60 kN / cm and 25°C. This resulted in a pressed negative electrode. Then, a solid electrolyte layer for bonding and a transfer member were placed in order from the negative electrode active material layer side. At this time, the solid electrolyte layer for bonding and the solid electrolyte layer in the transfer member were placed so as to face each other. The obtained laminate was set in a flat uniaxial press machine and temporarily pressed at 100 MPa and 25°C for 10 seconds. Then, the release sheet was peeled off from the solid electrolyte layer. This resulted in a second laminate. Next, the solid electrolyte layer for bonding in the first laminate and the solid electrolyte layer in the second laminate were placed so as to face each other, and the first laminate was set in a flat uniaxial press machine and pressed at 400 MPa and 135°C for 1 minute. This resulted in a solid battery for evaluation.

[0066] 7.4.1 Comparative Example 5 Crystalline silicon was used as the negative electrode active material, and the ratio C1 / C2 of the weight per unit area C1 of the positive electrode active material in the positive electrode to the weight per unit area C2 of the negative electrode active material in the negative electrode was set to 5.50.

[0067] 7.4.2 Example 4 Clathrate silicon was used as the negative electrode active material, and the ratio C1 / C2 of the basis weight C1 of the positive electrode active material in the positive electrode to the basis weight C2 of the negative electrode active material in the negative electrode was set to 2.87.

[0068] 7.4.3 Example 5 Clathrate silicon was used as the negative electrode active material, and the ratio C1 / C2 of the basis weight C1 of the positive electrode active material in the positive electrode to the basis weight C2 of the negative electrode active material in the negative electrode was set to 3.71.

[0069] 7.5 Charge / discharge cycle test The durability performance after 50 cycles was confirmed for each of the sulfide solid state batteries fabricated as described above, in the same manner as in Examples 1 to 3 and Comparative Examples 1 to 4. The durability performance of Comparative Example 5 was taken as the standard (100%), and the durability performance of Examples 4 and 5 was evaluated relative to it. In addition, the negative electrode after the first charge and discharge was taken out and measured by Raman spectroscopy (wavelength 532 nm). The obtained Raman spectrum was analyzed to obtain a Raman spectrum of 325±10 cm -1 Maximum peak intensity at I 325 and 205±10cm -1 Maximum peak intensity at I 205 Comparison with I 325 / I 205 The ratio I was calculated. 325 / I 205 When the ratio is within the range of 1.03 to 1.21, it can be said that the Si particles have a clathrate structure.

[0070] 7.6 Evaluation Results The evaluation results are shown in Table 2. As shown in Table 2, it can be seen that the technology of the present disclosure provides the same effects in solid-state batteries as in electrolyte batteries.

[0071] [Table 2]

[0072] 8. Summary From the above results, it can be said that the secondary battery having the following configurations (1) to (4) has excellent durability. (1) The negative electrode contains Si particles as a negative electrode active material. (2) The positive electrode contains a Li-containing compound as a positive electrode active material. (3) The Si particles have a clathrate structure. (4) The ratio C1 / C2 of the weight C1 of the Li-containing compound in the positive electrode to the weight C2 of the Si particles in the negative electrode is 8.33 or less.

[0073] In the above examples, examples using specific positive electrodes and electrolytes are shown, but the technology of the present disclosure does not particularly limit the types of positive electrodes and electrolytes. In the above examples, a specific current collector, binder, and conductive assistant are shown in the negative electrode, but the technology of the present disclosure does not particularly limit the configuration of the negative electrode other than the negative electrode active material. Based on the above estimated mechanism, it is considered that the durability of the secondary battery is improved by using a specific negative electrode active material and adjusting the active material weight ratio C1 / C2 within a predetermined range, regardless of the type of battery (electrolyte battery, solid battery) or material. [Explanation of symbols]

[0074] 10 negative electrode 11 Negative electrode active material layer 12 Negative electrode current collector 20 Electrolyte layer 30 positive electrode 31 Cathode active material layer 32 Positive electrode current collector 100 Secondary battery

Claims

1. A secondary battery having a negative electrode, an electrolyte layer, and a positive electrode, The negative electrode has Si particles as a negative electrode active material, The positive electrode has a Li-containing compound as a positive electrode active material, The Si particles have a clathrate structure, The amount C of the Li-containing compound in the positive electrode 1 and the weight C of the Si particles in the negative electrode. 2 Comparison with C 1 / C 2 is less than or equal to 8.33; Secondary battery.

2. The ratio C1 / C2 is 2.87 or more. The secondary battery according to claim 1 .

3. The Li-containing compound contains, as constituent elements, at least Li, at least one of Ni, Co, and Mn, and O. The secondary battery according to claim 1 or 2.

4. The secondary battery according to any one of claims 1 to 3, A control unit that controls charging and discharging of the secondary battery; Equipped with The control unit controls the charging voltage of the secondary battery to 4.2 V or less. Secondary battery system.

Citation Information

Patent Citations

  • All-solid battery and its manufacturing method

    JP2019192563A

  • Type ii clathrates for rechargeable battery anodes

    US20150380724A1

  • Copolymer for electrode binder and lithium ion secondary battery

    WO2021044968A1

  • Negative electrode material for lithium ion secondary battery, negative electrode for lithium ion secondary battery and lithium ion secondary battery

    JP2020113547A

  • Negative electrode active material including silicon clathrate ii

    JP2021034279A