Powder for thermal spraying

A thermal spray powder with composite particles improves uniformity and conductivity in fuel electrodes by optimizing pore size distribution and bonding, enhancing the performance of solid oxide fuel cells and electrolysis cells.

JP2024145869AActive Publication Date: 2024-10-15FUJIMI INCORPORATED
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023058417
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Existing fuel electrodes in solid oxide fuel cells and electrolysis cells require improved uniformity of ceramic and metal particle dispersion to enhance electrical conductivity and reduce interfacial resistance.

Method used

A thermal spray powder composed of composite particles with specific pore size distribution and bonding characteristics, including ceramic and transition metal compound particles, is used to form electrodes, ensuring uniform dispersion and improved electrical conductivity.

Benefits of technology

The solution enhances the uniformity and conductivity of the thermal spray coating, leading to increased efficiency and performance of solid oxide fuel cells and electrolysis cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145869000001_ABST
    Figure 2024145869000001_ABST
Patent Text Reader

Abstract

To provide a technique to improve the uniformity of components in thermal spray coatings.SOLUTION: Powder for thermal spraying is used to form electrodes for solid oxide fuel cells or solid oxide electrolysis cells. The powder for thermal spraying has a peak in a range of 0.15 μm or more and 1 μm or less in a log differential pore volume distribution with a pore diameter of 1 μm or less obtained by a mercury intrusion method.SELECTED DRAWING: Figure 12
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to thermal spray powders. [Background technology]

[0002] A solid oxide fuel cell (SOFC) and a solid oxide electrolysis cell (SOEC) include an air electrode, a fuel electrode, and a solid electrolyte layer. In this regard, Patent Document 1 discloses a fuel electrode for a solid oxide fuel cell, which is a particle mixture of electrolyte material particles having an average particle size D50 of 0.1 to 0.6 μm and nickel oxide particles having an average particle size D50 of 0.5 to 1.5 μm, and is characterized in that the particle mixture is obtained by firing the particle mixture in which the mass ratio of the electrolyte material particles to the nickel oxide particles is 35:65 to 50:50. The document states that the above configuration can reduce the interface resistance between the fuel electrode and the electrolyte.

[0003] Patent Document 2 discloses a nickel-ion conductive ceramic mixed powder used for the fuel electrode. This mixed powder contains metallic nickel particles (A) with a median diameter of 10 nm to 200 nm and ion conductive ceramic particles (B) with a median diameter of 10 nm to 200 nm. This mixed powder is characterized in that the content of nickel element contained in the mixed powder and the content of ion conductive ceramic particles are in a volume ratio of [nickel element] / [ion conductive ceramic particles]=20 / 80 to 80 / 20. The document describes that it is possible to achieve both high catalytic activity and high conductivity, reduce the internal resistance value, and improve the operating efficiency as a functional material. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-266713 A [Patent Document 2] Patent Publication No. 2021-28417 Summary of the Invention [Problem to be solved by the invention]

[0005] Incidentally, the fuel electrode is a porous film that contains ion-conductive ceramic particles and metal particles, with voids formed between the particles (see Patent Documents 1 and 2). In such a fuel electrode, it is required that the ceramic particles, metal particles, and voids are uniformly dispersed.

[0006] In view of these circumstances, an object of the present invention is to provide a technique for improving the uniformity of components in a thermal spray coating. [Means for solving the problem]

[0007] The thermal spray powder disclosed herein is a thermal spray powder for forming electrodes for solid oxide fuel cells or solid oxide electrolysis cells. The thermal spray powder has a peak in the range of 0.15 μm or more and 1 μm or less in the log differential pore volume distribution of pores with diameters of 1 μm or less obtained by mercury intrusion porosimetry. By using a thermal spray powder of this configuration, the uniformity of the components in the thermal spray coating can be improved.

[0008] In a preferred embodiment of the thermal spray powder disclosed herein, the thermal spray powder contains composite particles including ion-conductive ceramic particles and transition metal compound particles. By using a thermal spray powder having such a composition, it is possible to increase the uniformity of the components in the thermal spray coating and to impart electrical conductivity to the thermal spray coating.

[0009] In a preferred embodiment of the thermal spray powder disclosed herein, the composite particles have a region where the primary particles are in contact with each other and where there is no particle interface at the contact portion. This configuration makes it easier to achieve a desired pore size distribution in the thermal spray powder. This makes it possible to further improve the uniformity of the components in the thermal spray coating.

[0010] In another preferred embodiment of the thermal spray powder disclosed herein, the ratio of ceramic particles to transition metal compound particles (ceramic particles:transition metal compound particles) is 60:40 to 20:80. This configuration can improve the ion conductivity of the formed thermal spray coating while suppressing a decrease in the electrical conductivity of the electrodes. This can increase the operating efficiency of the SOFC or SOEC.

[0011] In another preferred embodiment of the thermal spray powder disclosed herein, the median diameter (D 50 ) is 10 μm or more and 100 μm or less. This configuration can improve the fluidity of the thermal spray powder.

[0012] In another preferred embodiment of the thermal spray powder disclosed herein, the ceramic particles are zirconia particles containing a rare earth metal oxide. Such ceramic particles are suitable for achieving the effects of the technology disclosed herein. The transition metal compound particles are preferably nickel oxide particles. Such transition metal compound particles are suitable for achieving the effects of the technology disclosed herein.

[0013] In another preferred embodiment of the thermal spray powder disclosed herein, when the thermal spray powder is subjected to a reduction treatment in a hydrogen gas atmosphere at a treatment temperature of 800° C. for two hours and then heated in an air atmosphere from room temperature to 1200° C. at a temperature increase rate of 10 K / min for thermogravimetric analysis, the temperature at which the weight increases by 3% is 470° C. or higher and 570° C. or lower. With this configuration, when a thermal spray coating formed from this thermal spray powder is used to form an electrode, the conductivity of the electrode can be increased.

[0014] In another preferred embodiment of the thermal spray powder disclosed herein, the peak is in the range of 0.15 μm or more and 0.23 μm or less. This configuration can further improve the uniformity of the components in the thermal spray coating. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a cross-sectional view of a SOFC 10. [Diagram 2] FIG. 2 is a plan view of the thermal spray powder of Example 3. [Diagram 3] FIG. 3 is an enlarged image of FIG. [Figure 4] FIG. 4 is a cross-sectional view of the thermal spray powder of Example 3. [Diagram 5] FIG. 5 is a plan view of the thermal spray powder of Example 4. [Figure 6] FIG. 6 is an enlarged image of FIG. [Figure 7] FIG. 7 is a cross-sectional view of the thermal spray powder of Example 4. [Figure 8] FIG. 8 is a plan view image of the thermal spray powder of the comparative example. [Figure 9] FIG. 9 is an enlarged view of FIG. [Figure 10] FIG. 10 is a cross-sectional view of the thermal spray powder of the comparative example. [Figure 11] FIG. 11 is a graph showing the log differential pore volume distribution of each example. [Figure 12] FIG. 12 is a graph showing the log differential pore volume distribution of each example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] A preferred embodiment of the technology disclosed herein will be described below. Matters other than those specifically mentioned in this specification and necessary for implementing the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The technology disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in the relevant field. In the specification, the expression "X to Y" indicating a numerical range means "X or more and Y or less" unless otherwise specified, and also means a range "greater than X and less than Y", a range "greater than X and less than Y", and a range "greater than X and less than Y".

[0017] <Definition> In this specification, the term "thermal spray powder" refers to a powdered material used for thermal spraying. In addition, in this specification, the term "composite particle" refers to a particulate matter (in the form of a particle) that is composed of a plurality of different materials, and the plurality of materials are bonded together to behave as a single particle. Examples of the composite particle include granulated particles and granulated sintered particles composed of at least two or more types of materials. In addition, in this specification, the term "primary particle" refers to the smallest unit that can be identified as a granular matter from the appearance among the morphological components that make up the thermal spray powder. Therefore, when the composite particle that makes up the thermal spray powder disclosed here includes a secondary particle, for example, the particle that makes up the secondary particle is called a primary particle. Here, the term "secondary particle" refers to a particulate matter in which the primary particles are bonded three-dimensionally to behave as a single particle. Examples of the "secondary particle" referred to here include granulated particles and particles sintered after granulation (granulated sintered particles).

[0018] The term "bonding" as used herein refers to the direct or indirect bonding of two or more primary particles. Examples of "bonding" include bonding between primary particles by chemical reaction, bonding between primary particles attracting each other by simple adsorption, bonding using the anchor effect of allowing an adhesive or the like to penetrate into the unevenness of the primary particle surface, bonding between primary particles using the effect of attraction due to static electricity, and bonding in which the surfaces of primary particles are melted and integrated. In addition, with respect to secondary particles composed of two or more materials, "bonding" includes bonding in which one material constitutes the primary particles and the other material is melted and integrated with the primary particles. In addition, in this specification, the term "raw material particles" refers to particles that constitute the powder in the raw material stage used to prepare the thermal spray powder disclosed herein.

[0019] <Method of measuring median diameter> In this specification, the "median diameter" of a thermal spray powder and primary particles constituting secondary particles (thermal spray powder) refers to the median diameter (D) at an integrated value of 50% in a volume-based particle size distribution measured by a particle size distribution measuring device based on a laser scattering / diffraction method. 50The median diameter is measured, for example, using a commercially available measuring device.

[0020] In the above-mentioned Patent Documents 1 and 2, screen printing, doctor blade, and the like are given as means for applying a paste (slurry) for forming an electrode, which contains a powder material, to a substrate. On the other hand, the present inventors wanted to form an electrode by thermal spraying of a powder material. Thermal spraying is a process in which a powder material is made molten or semi-molten and sprayed onto a substrate surface to form a film, and is completely different from processes such as screen printing and doctor blade. For this reason, the present inventors investigated the composition of a powder material (powder for thermal spraying) that is suitable for forming an electrode by thermal spraying and can increase the uniformity of the components in the thermal spray coating.

[0021] <Composition of thermal spray powder> The thermal spray powder disclosed herein may include, for example, composite particles containing ceramic particles and transition metal compound particles. The thermal spray powder is preferably composed of composite particles containing ceramic particles and transition metal compound particles, but may include unavoidable impurities resulting from the manufacturing process of the ceramic particles, the transition metal compound particles, or the composite particles. The content of the unavoidable impurities in the entire thermal spray powder is generally 5 mass% or less, preferably 3 mass% or less, more preferably 1 mass% or less, even more preferably 0.5 mass% or less, particularly preferably 0.1 mass% or less, and the closer to 0 mass%, the better.

[0022] The ceramic particles have, for example, ion conductivity. Here, the ceramic particles may have oxide ion conductivity. As the ceramic constituting the ceramic particles, a ceramic used for this type of application is appropriately selected. As such a ceramic, for example, a metal oxide can be mentioned. As the metal oxide, for example, zirconium oxide (zirconia) and cerium oxide (ceria) are preferably used.

[0023] The zirconium oxide may be stabilized zirconia in which one or more stabilizers are dissolved. The stabilizer-dissolved zirconia means zirconia containing a stabilizer. Examples of the stabilizer include rare earth metal oxides such as scandium oxide (Sc2O3), yttrium oxide (yttria; Y2O3), cerium oxide (ceria; CeO2), gadolinium oxide (gadolinia; Gd2O3), and ytterbium oxide (Yb2O3); and alkaline earth metal oxides such as calcium oxide (calcia; CaO) and magnesium oxide (magnesia; MgO). Preferably, the ceramic particles are zirconia particles containing a rare earth metal oxide. The effect of the technology disclosed herein is better realized when an electrode (here, a fuel electrode) containing zirconia particles containing a rare earth metal oxide is produced as the ceramic particles. Of these, scandia-stabilized zirconia particles and yttria-stabilized zirconia particles are preferably used.

[0024] The cerium oxide here can be doped ceria, which is ceria doped with a rare earth metal oxide such as yttrium oxide (yttria; Y2O3), samarium oxide (samaria; Sm2O3), or gadolinium oxide (gadolinia; Gd2O3).

[0025] The median diameter of the ceramic particles is not limited as long as the effect of the technology disclosed herein is realized. The median diameter is, for example, 0.01 μm to 5 μm, preferably 0.05 μm to 2.5 μm, more preferably 0.1 μm to 1 μm, and further preferably 0.1 μm to 0.5 μm. By setting the median diameter of the ceramic particles within the above range, the dispersibility of the ceramic particles in the composite particles can be improved, and in turn, the uniformity of the components in the thermal spray coating can be improved. This can improve the operating efficiency of the SOFC or SOEC.

[0026] The transition metal compound includes substances exhibiting metallic properties, such as alloys, solid solutions, and intermetallic compounds made of the transition metal element and at least one of other metal elements and metalloid elements, and compounds (e.g., oxides, etc.) of the transition metal element and nonmetallic elements. Examples of the transition metal compound include oxides (transition metal oxides) of 3d transition elements such as titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), and copper (Cu); metals such as precious metal elements such as ruthenium (Ru), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), platinum (Pt), gold (Au), and silver (Ag); and alloys such as platinum-palladium alloys and platinum-rhodium alloys. Other examples include oxides (transition metal oxides) such as cobalt oxide (CoO, Co2O3, Co3O4), copper oxide (CuO, Cu2O), silver oxide (AgO, Ag2O), and tungsten oxide (WO, W2O3, WO3, WO6). Among these, nickel oxide is preferred. Transition metal compound particles (transition metal compound particles) become transition metal particles, for example, by reduction. Therefore, during operation of the SOFC or SOEC, the transition metal compound particles become transition metal particles and exhibit catalytic activity and electronic conductivity. Therefore, it is preferable that the transition metal compound particles are larger than the ceramic particles. For example, the median diameter of the transition metal compound particles is preferably larger than the median diameter of the ceramic particles. The median diameter of the transition metal compound particles is not limited as long as the effect of the technology disclosed herein is realized. The median diameter is, for example, about 0.01 μm to 10 μm, preferably 0.05 μm to 5 μm, more preferably 0.1 μm to 2 μm, and further preferably 0.1 μm to 1 μm. By setting the median diameter of the transition metal compound particles within the above range, the dispersibility of the transition metal compound particles in the composite particles can be increased, and in turn, the uniformity of the components in the thermal spray coating can be improved. This can improve the conductivity of the electrodes of the SOFC or SOEC.

[0027] The mixing ratio (here, mass ratio) of ceramic particles and transition metal compound particles in the thermal spray powder can be a factor affecting the performance of SOFC or SOEC, the uniformity of components in the thermal spray coating, and the like. From this viewpoint, the mass ratio of ceramic particles to transition metal compound particles (ceramic particles:transition metal compound particles) is preferably, for example, 80:20 to 20:80, or 70:30 to 30:70. In a preferred embodiment, the mass ratio (ceramic particles:transition metal compound particles) is 60:40 to 20:80. When the mass ratio of ceramic particles to transition metal compound particles (ceramic particles:transition metal compound particles) is 80:20 to 20:80, or 70:30 to 30:70, it is possible to improve the electrical conductivity of the electrode in the formed thermal spray coating while suppressing a decrease in ion conductivity.

[0028] The composite particles may be particles produced by, for example, mixing ceramic particles and transition metal compound particles. The composite particles are particles containing different materials, i.e., ceramic particles and transition metal compound particles, but the ceramic particles and transition metal compound particles are integrated with each other and behave as a single particle. For this reason, for example, if the ceramic particles and transition metal compound particles are well dispersed in the composite particles, the uniformity of the components in the thermal spray coating may be improved.

[0029] The form of the composite particles is not limited as long as the ceramic particles and the transition metal compound particles are integrated and the effect of the technology disclosed herein can be realized. The composite particles may be, for example, granulated particles. In this case, the granulated particles (secondary particles) can be produced, for example, by mixing ceramic particles (primary particles), transition metal compound particles (primary particles), and other optional components (for example, binder, solvent, etc.) together and granulating them.

[0030] The composite particles are preferably particles in which the primary particles are in contact with each other and have a region where there is no particle interface at the contact portion. The composite particles are preferably sintered particles. The sintered particles can be produced by producing granulated particles from ceramic particles and transition metal compound particles as described above, and then sintering the granulated particles (such particles are sometimes referred to as granulated sintered particles). In the sintered particles, the ceramic particles and the transition metal compound particles are bonded in a state where a neck is formed at the contact portion between the primary particles by sintering, and the neck grows as solid-phase diffusion progresses at the neck, changing the state from point contact to surface contact. Such bonding is realized, for example, by the diffusion of at least a part of the ceramic particles or the transition metal compound particles. Preferably, the ceramic particles, which are primary particles, and the transition metal compound particles are bonded in a state where there is a region where there is no particle interface at the contact portion. This, for example, increases the conductivity of the electrode. The granulated sintered particles have a higher strength than the granulated particles before sintering. Therefore, by using the granulated sintered particles as the composite particles, a desired pore size distribution is realized and easily maintained in the thermal spray powder. For this reason, by using such granulated and sintered particles, it is possible to produce a thermal spray coating with improved uniformity of components.

[0031] The median diameter (D) at 50% cumulative volumetric particle size distribution based on the laser diffraction scattering method of the thermal spray powder disclosed herein 50 ) is not particularly limited and can be a size suitable for the specifications of the device used. The median diameter is, for example, 1 μm or more. The larger the median diameter, the more the handleability, flowability, etc. of the thermal spray material can be improved. From this viewpoint, the median diameter is appropriately 3 μm or more, preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more. On the other hand, if the median diameter is too large, there is a concern that the thermal spray powder may not be sufficiently melted during thermal spraying. From this viewpoint, the median diameter is, for example, 300 μm or less, preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less.

[0032] When a thermal spray powder is measured by mercury intrusion porosimetry, for example, in a log differential pore volume distribution in a pore size range of 1 μm or less, the pore size originating from the gaps between primary particles (i.e., the gaps within composite particles) can be measured. On the other hand, in a log differential pore volume distribution in a pore size range of more than 1 μm, the pore size originating from the gaps between secondary particles can be measured. Therefore, by analyzing the log differential pore volume distribution in a pore size range of 1 μm or less, the bonding state (necking state) between the ceramic particles and the transition metal compound particles in the thermal spray powder and the degree of formation of gaps within the composite particles can be grasped.

[0033] The thermal spray powder disclosed herein preferably has a peak in the range of 0.15 μm to 1 μm in the log differential pore volume distribution with pore diameters of 1 μm or less obtained by mercury intrusion porosimetry. This indicates that the bonding state (necking state) between the ceramic particles and the transition metal compound particles in the composite particles is in a favorable state, and appropriate voids are formed within the composite particles. For this reason, by thermally spraying the above-mentioned thermal spray powder, a thermal spray coating with improved component uniformity can be formed. From this perspective, the thermal spray powder preferably has a peak in the range of 0.15 μm to 0.5 μm, more preferably in the range of 0.15 μm to 0.3 μm, and even more preferably in the range of 0.15 μm to 0.23 μm in the log differential pore volume distribution with pore diameters of 1 μm or less obtained by mercury intrusion porosimetry. The term "peak" as used herein refers to a portion that stands out and has a high height (a portion that occurs frequently) in the log differential pore volume distribution (curve) (see FIG. 11). In other words, the "peak" can also be expressed as a point at which the sign of the slope of the tangent to the log differential pore volume distribution (curve) changes from "+" to "-".

[0034] The mercury intrusion method is a method for determining the pore size distribution of a powder from the relationship between the pressure applied to infiltrate mercury into the pores of the powder and the amount of mercury intruded into the pores of the powder. The pore size distribution measurement based on the mercury intrusion method is carried out, for example, based on JIS R1655:2003 (Pore size distribution test method for molded bodies using mercury intrusion method for fine ceramics). In addition, the "log differential pore volume distribution" in this specification is also called log differential pore size frequency distribution, dV / d(logD) (where D indicates the diameter of the pores and V indicates the pore volume), etc., and is a form of expression of pore distribution that is generally used to express the pore distribution in a relatively wide pore size range.

[0035] The log differential pore volume distribution can be created from the relationship between the amount of mercury intrusion (i.e., pore volume) and the change in unit pore size (which may be a change in unit pressure) obtained by measuring the pore size distribution based on mercury intrusion porosimetry. Specifically, the log differential pore volume distribution can be created by dividing the differential pore volume (dV), which is the increase in pore volume, by the logarithmic difference value d (logD) of the pore size, and plotting this against the average pore size in each pore size range (see FIG. 11). In this specification, the apex of the peak and the like are grasped based on the pore size distribution characteristics obtained by measuring the pore size distribution by mercury intrusion porosimetry in a measurement range of 0.0036 nm to 1 μm. For example, two peaks can be obtained in the log differential pore volume distribution of the thermal spray powder (here, composite particles) disclosed herein (see FIG. 11). The larger-diameter peak of the two peaks can be a peak derived from the pores between the composite particles contained in the thermal spray powder. On the other hand, the smaller peak of the two peaks may be a peak derived from pores in the composite particles. In this specification, the "peak" is not a peak derived from gaps between composite particles, but a peak derived from pores in the composite particles, and may be the highest peak in the log differential pore volume distribution (curve) for pore diameters of 1 μm or less.

[0036] After the thermal spray powder is sprayed to form a thermal spray coating, the thermal spray coating can be used as an electrode for an SOFC or SOEC after being subjected to a reduction treatment. In the thermal spray coating, the transition metal compound components derived from the transition metal compound particles are reduced to transition metal components by this reduction treatment. The transition metal components are the main component for the electrode to exhibit electrical conductivity, so it is preferable that they are not easily oxidized. From this viewpoint, the thermal spray powder disclosed herein is preferably one that has a temperature of 470°C or more and 570°C or less at a 3% weight increase when the thermal spray powder is subjected to a reduction treatment at a treatment temperature of 800°C for 2 hours in a hydrogen gas atmosphere, heated from room temperature (30°C) to 1200°C at a heating rate of 10K / min in an air atmosphere and subjected to a thermogravimetric analysis. Alternatively, from the viewpoint of realizing the effect of the technology disclosed herein, it is more preferable that the temperature at which the weight increases by 3% is 470°C or more and 520°C or less. The "temperature at which the weight increases by 3%" is defined as the "point of change in weight of 3%" in the test example described later.

[0037] Here, when the thermal spray powder is subjected to a predetermined reduction treatment, the transition metal compound particles in the thermal spray powder are reduced to form transition metal particles. In the above-mentioned thermogravimetric analysis, the thermal spray powder after reduction treatment is heated in an air atmosphere, thereby oxidizing the transition metal particles. This increases the weight of the thermal spray powder. For the reduced thermal spray powder, the fact that the temperature at which the weight increases by 3% in the thermogravimetric analysis satisfies the above range indicates that when the thermal spray coating obtained by spraying the thermal spray powder is reduced to form an electrode, the transition metal component in the thermal spray coating is not easily oxidized. By using a thermal spray powder having this characteristic, the conductivity of the electrode can be further improved.

[0038] <Method of manufacturing thermal spray powder> The thermal spray powder disclosed herein can be prepared, for example, by mixing ceramic particles and transition metal compound particles as raw material particles together with other optional components and compositing them. In particular, the thermal spray powder is preferably composed of granulated and sintered particles in which ceramic particles and transition metal compound particles are mixed. The thermal spray powder may be, for example, a thermal spray powder composed of granulated and sintered particles as secondary particles in which the primary particles are three-dimensionally bonded with gaps between them, the primary particles being formed by mixing the respective raw material particles (primary particles), granulating them, and further sintering them.

[0039] The granulation sintering method is a method in which raw material particles are granulated into the form of secondary particles, and then sintered to bond (sinter) the raw material particles together. In the granulation sintering method, granulation can be performed by a granulation method such as dry granulation or wet granulation. Examples of the granulation method include rolling granulation, fluidized bed granulation, stirring frame granulation, crushing granulation, melt granulation, spray granulation, and microemulsion granulation. Among them, spray granulation is a preferred granulation method.

[0040] According to the spray granulation method, for example, a powder material can be manufactured by the following procedure. That is, first, raw material particles including ceramic particles and transition metal compound particles are prepared, and the surface of the raw material particles is stabilized by a protective agent or the like as necessary. Then, for example, the raw material particles stabilized as necessary, together with organic materials such as binders and spacer particles as optional components, are dispersed in an appropriate solvent to prepare a spray liquid. Here, the raw material particles are dispersed in the solvent by using a mixer such as a homogenizer or a blade stirrer, a disperser, or the like. Then, droplets are formed from the spray liquid by an ultrasonic sprayer or the like. The droplets are carried by an air flow and passed through a spray drying device (spray dryer), thereby forming granulated particles. The granulated particles thus obtained are introduced into a predetermined firing furnace and fired. As a result, a thermal spray material consisting of granulated sintered particles in the form of secondary particles in which primary particles are bonded (sintered) with gaps can be manufactured. Here, the primary particles may have almost the same size and shape as the raw material particles, or the raw material particles may be bonded in a state in which they have grown by firing.

[0041] In the above manufacturing process, when the droplets are dried, the raw material particles and the binder are in a uniform mixed state. The raw material particles are bound by the binder to form the mixed particles. When spacer particles are used, the raw material particles and the spacer particles are bound by the binder in a uniform mixed state to form the mixed particles. Then, by firing the mixed particles, the binder (and the spacer particles) disappear (burn out) and the raw material particles are sintered. As a result, secondary particles are formed in a form in which the primary particles are bound (sintered) with gaps between them. During sintering, depending on the composition, size, etc., some of the raw material particles may become liquid phase and contribute to binding with other particles. Therefore, the median diameter of the primary particles may be larger than that of the raw material particles of the starting material. The median diameter of the secondary particles, the median diameter of the primary particles, and the size and ratio of the gaps formed between the primary particles can be designed according to the desired form of the secondary particles.

[0042] The concentration of the raw material particles in the spray liquid is preferably, for example, 10% by mass to 80% by mass. Examples of the binder to be added include polyvinyl alcohol (PVA) and carboxymethyl cellulose (CMC). For example, water can be used as the solvent. The amount of the binder to be added is preferably adjusted to a ratio of 0.05% by mass to 10% by mass (for example, 1% by mass to 5% by mass) relative to the mass of the raw material particles.

[0043] In sintering the granulated particles, the granulated particles are heat-treated (fired) for 1 hour to 10 hours at a predetermined temperature (approximately 600° C. to 1600° C. (preferably 700° C. to 1500° C., more preferably 800° C. to 1400° C., and even more preferably 1000° C. to 1300° C.)) in an air atmosphere; an inert atmosphere such as a nitrogen atmosphere or a rare gas atmosphere; or in a vacuum. The above-mentioned predetermined temperature may be, for example, the set temperature of a firing furnace. The temperature and time when the granulated particles are heat-treated can be appropriately set so as to produce a thermal spray powder having a desired pore size distribution. The firing temperature and time can be appropriately set so as to achieve a desired median diameter for the thermal spray powder, a temperature at which the weight increases by 3% in thermogravimetric analysis in an air atmosphere, and the like. After the heat treatment, the obtained granulated and sintered particles may be crushed and classified as necessary.

[0044] <Applications of thermal spray powder> By spraying the thermal spray powder disclosed herein by various thermal spraying methods, thermal spray coatings can be produced on various substrates. The thermal spray powder can be particularly preferably used to produce thermal spray coatings by plasma spraying methods such as atmospheric plasma spraying (APS), low pressure plasma spraying (LPS), and high pressure plasma spraying. The thermal spray powder can also be suitably used for high velocity flame spraying such as high velocity oxygen flame (HVOF) thermal spraying, warm spray thermal spraying, and high velocity air flame (HVAF) thermal spraying. The thermal spray powder may be supplied to a thermal spraying device in a powder state, or may be supplied to a thermal spraying device in a slurry state in which the powder is dispersed in a suitable dispersion medium.

[0045] The thermal spray powder disclosed herein is used, for example, to form an electrode of a solid oxide fuel cell (SOFC) or a solid oxide electrolysis cell (SOEC). The thermal spray powder is preferably used as a material for forming a fuel electrode of an SOFC or SOEC. An SOFC can extract power (electrical energy) from chemical energy generated, for example, from a combustion reaction between hydrogen and oxygen. An SOEC can cause a chemical reaction that produces hydrogen and oxygen from water (e.g., water vapor) by applying electrical energy to the water.

[0046] FIG. 1 is a cross-sectional view of SOFC 10. FIG. 1 shows a laminated structure of electrodes and solid electrolyte layers in SOFC 10. As shown in FIG. 1, SOFC 10 includes a fuel electrode 1, an air electrode 2, and a solid electrolyte layer 3. In SOFC 10, the fuel electrode 1 is the anode, and the air electrode 2 is the cathode. In this specification, the term "anode" refers to an electrode from which electrons flow into an external circuit. Also, the term "cathode" refers to an electrode into which electrons flow from an external circuit.

[0047] The fuel electrode 1 here is an electrode where hydrogen reacts with oxide ions. In this embodiment, the reaction between hydrogen and oxide ions produces water and releases electrons. These electrons generate electricity. As shown in FIG. 1, the fuel electrode 1 is provided on one surface of the solid electrolyte layer 3. In this embodiment, the fuel electrode 1 is formed by using the thermal spray powder disclosed herein.

[0048] The air electrode 2 here is an electrode at which oxygen in the air receives electrons. In this embodiment, at the air electrode, oxygen in the supplied air receives electrons released from the fuel electrode 1, and oxide ions are generated. As shown in FIG. 1, the air electrode 2 is provided on the other surface of the solid electrolyte layer 3 (in FIG. 1, the surface opposite to the surface on which the fuel electrode 1 is formed). As the air electrode 2, various air electrodes proposed so far may be used without any particular restrictions. For this reason, a description of the configuration of the air electrode 2 will be omitted here.

[0049] Here, the solid electrolyte layer 3 is a layer having a function of conducting oxide ions. In this embodiment, oxide ions generated at the air electrode 2 pass through the solid electrolyte layer 3 and are supplied to the fuel electrode 1. As shown in FIG. 1, the solid electrolyte layer 3 is sandwiched between the fuel electrode 1 and the air electrode 2. As the solid electrolyte layer 3, various solid electrolyte layers proposed so far may be used without any particular restrictions. For this reason, a description of the configuration of the solid electrolyte layer 3 will be omitted here.

[0050] The method for manufacturing the SOFC 10 may include, for example, a preparation step, a lamination step, a spraying step, and a firing step. The preparation step is, for example, a step of preparing a green sheet for the solid electrolyte layer 3. In this step, for example, a slurry for forming the solid electrolyte layer 3 may be applied onto a carrier sheet, formed into a predetermined shape and dimensions, and dried to prepare the green sheet for the solid electrolyte layer 3. The method for applying the slurry for forming the solid electrolyte layer 3 onto the carrier sheet is not particularly limited, and for example, a conventional application method such as a screen printing method or a doctor blade method may be adopted.

[0051] The lamination step is, for example, a step of laminating a green sheet of the air electrode 2 on one surface of a green sheet of the solid electrolyte layer 3. In this step, for example, a slurry for forming the air electrode 2 is applied to one surface (here, the surface opposite to the carrier sheet) of the green sheet of the solid electrolyte layer 3, and the green sheet of the air electrode 2 is laminated on the green sheet of the solid electrolyte layer 3 by forming the slurry into a predetermined shape and size and drying it. Then, the carrier sheet may be removed from the green sheet of the solid electrolyte layer 3. The method of applying the slurry for forming the air electrode 2 to the green sheet of the solid electrolyte layer 3 is not particularly limited, and for example, a conventional application method such as a screen printing method or a doctor blade method may be adopted.

[0052] The thermal spraying step is, for example, a step of spraying the thermal spray powder disclosed herein onto the other surface of the green sheet of the solid electrolyte layer 3. In this step, for example, the thermal spray powder is sprayed onto the surface of the green sheet of the solid electrolyte layer 3 opposite to the surface on which the green sheet of the air electrode 2 is laminated. This forms a thermal spray coating of the thermal spray powder disclosed herein, which serves as a precursor of the fuel electrode 1.

[0053] The firing step is, for example, a step of firing a laminate of a green sheet of the solid electrolyte layer 3 provided with a thermal spray coating and a green sheet of the air electrode 2. As a result, the anode 1, the air electrode 2, and the solid electrolyte layer 3 are mutually sintered, and a laminated structure of the anode 1, the air electrode 2, and the solid electrolyte layer 3 in the SOFC 10 is formed.

[0054] As described above, the thermal spray powder disclosed herein is a thermal spray powder for forming electrodes of SOFCs or SOECs. The thermal spray powder preferably contains composite particles of ion-conductive ceramic particles and transition metal compound particles. The thermal spray powder preferably has a peak in the range of 0.15 μm or more and 1 μm or less in the log differential pore volume distribution of pores with a diameter of 1 μm or less obtained by mercury intrusion porosimetry.

[0055] In the thermal spray powder, ceramic particles and transition metal compound particles are contained in a composite particle state. Therefore, when the thermal spray powder is thermally sprayed, uneven distribution of the ceramic components derived from the ceramic particles and the transition metal compound components derived from the transition metal compound particles in the thermal spray coating can be suppressed. In addition, in the thermal spray powder, a peak is obtained in the range of 0.15 μm to 1 μm in the log differential pore volume distribution of pores with a diameter of 1 μm or less obtained by mercury intrusion porosimetry, so that a preferable bonding state (necking state) is realized between the ceramic particles and the transition metal compound particles. Therefore, by using the thermal spray powder disclosed herein, the uniformity of the components of the thermal spray coating can be improved. In addition, it is considered that the bonding between the transition metal compound particles is generated by realizing a preferable bonding state within the granules, and a good contact state between the transition metals after the reduction treatment is generated. Therefore, an electron path (electron passage) between the transition metals is efficiently formed, and the conductivity of the electrode can be improved.

[0056] Furthermore, by using the thermal spray powder disclosed herein, it is expected that the uniformity of the components in the thermal spray coating can be improved, and the three-phase interfaces between the voids, the ceramic component (ceramic particles), and the transition metal compound component (transition metal compound particles) can be more uniformly dispersed. By forming an electrode (e.g., anode) of an SOFC or SOEC from such a thermal spray coating, it is expected that both the power generation efficiency in the SOFC and the hydrogen production efficiency in the SOEC can be improved.

[0057] Test examples relating to the present invention will be described below, but it is not intended that the present invention be limited to those shown in the following test examples. In the following description, the notation "%" is based on mass unless otherwise specified.

[0058] <Production Example> Example 1 A starting material was prepared containing yttria-stabilized zirconia (YSZ) particles as ceramic particles, nickel oxide (NiO) particles as transition metal compound particles, polyvinyl alcohol (PVA) as a binder, and water (ion-exchanged water) as a solvent. The median diameter of the YSZ particles was 0.2 μm. The median diameter of the NiO particles was 0.7 μm. The median diameters of the YSZ particles and the NiO particles were calculated based on the volume-based particle size distribution measured using a laser diffraction particle size distribution measuring device (Malvern Panalytical, Mastersizer 3000). 50 The median diameter of the YSZ particles and NiO particles was measured under wet dispersion using water, taking into consideration the dispersion state of each powder during particle size distribution measurement. When the total of the YSZ particles and NiO particles was taken as 100%, the proportion of the YSZ particles was 40% and the proportion of the NiO particles was 60%. When the total of the starting materials was taken as 100%, the proportion of PVA was 2% and the proportion of water was 50%.

[0059] Next, the starting materials were mixed and dispersed to prepare a slurry. This slurry was sprayed into an air stream using a spray granulator and dried to produce granulated particles. Next, the granulated particles were placed in an alumina sagger and fired in an air atmosphere to produce granulated and sintered particles. In this firing, the sagger containing the granulated particles was held at a temperature of 950°C for 4 hours. Next, the granulated and sintered particles were crushed and classified to obtain a thermal spray powder having a predetermined particle size distribution. This thermal spray powder was used as the thermal spray powder of this example.

[0060] Example 2 The sintering temperature for sintering the granulated particles was 1040° C. Other than this, the thermal spray powder according to this example was produced using the same materials and procedures as in Example 1.

[0061] Example 3 The sintering temperature for sintering the granulated particles was 1200° C. Other than this, the same materials and procedures as in Example 1 were used to produce the thermal spray powder of this example.

[0062] Example 4 The sintering temperature for sintering the granulated particles was set to 1300° C. Other than this, the thermal spray powder according to this example was produced using the same materials and procedures as in Example 1.

[0063] (Comparative Example) The sintering temperature for sintering the granulated particles was 200° C. Other than this, the thermal spray powder according to this example was produced using the same materials and procedures as in Example 1.

[0064] [SEM observation] Cross-sectional images and planar images were obtained for the thermal spray powders of Examples 1 to 4 and the thermal spray powder of the Comparative Example using a benchtop SEM (Phenom ProX, manufactured by Phenom-World). For reference, FIGS. 2 to 10 show the cross-sectional images and planar images of the thermal spray powders as follows. FIG. 2 is a planar image of the thermal spray powder of Example 3. FIG. 3 is an enlarged image of FIG. 2. FIG. 4 is a cross-sectional image of the thermal spray powder of Example 3. FIG. 5 is a planar image of the thermal spray powder of Example 4. FIG. 6 is an enlarged image of FIG. 5. FIG. 7 is a cross-sectional image of the thermal spray powder of Example 4. FIG. 8 is a planar image of the thermal spray powder of the Comparative Example. FIG. 9 is an enlarged view of FIG. 8. FIG. 10 is a cross-sectional image of the thermal spray powder of the Comparative Example.

[0065] [Median diameter measurement] For the thermal spray powders of Examples 1 to 4 and the thermal spray powder of the Comparative Example, the volumetric particle size distribution was measured using a laser diffraction particle size distribution measuring device (Mastersizer 3000, manufactured by Malvern Panalytical) to obtain the median diameter. The results are shown in the "Median diameter (μm)" column in Table 1. The median diameter of the thermal spray powder was measured under dry dispersion using compressed air, taking into consideration the dispersion state of each powder during the particle size distribution measurement.

[0066] [Pore volume] The pore volumes of the thermal spray powders of Examples 1 to 4 and the thermal spray powder of the Comparative Example were measured using a mercury intrusion porosimeter (POREMASTER-60, manufactured by Quantachrome Corp.) Specifically, the pore volumes were measured at a mercury contact angle of 140° and a surface tension of 480 erg / cm 2 The measurement was carried out under the condition of (0.480 N / m). Here, the cumulative pore volume (cc / g) of pores with a diameter of 1 μm or less (specifically, pores with a diameter in the range of 0.0036 μm to 0.98 μm) was measured. The measurement results are shown in the "Pore volume (cc / g)" column of Table 1.

[0067] The cumulative pore volume of pores with diameters of 1 μm or less measured as described above was defined as the "pore volume" of each thermal spray powder. The most frequent diameter (peak top position) of the log differential pore volume distribution was measured within the range of the "pore volume" defined as above. The measurement results are shown in the "Peak Top Position (μm)" column of Table 1. Figures 11 and 12 are graphs showing the log differential pore volume distribution of each example. Figure 12 shows an enlarged view of the range of pore diameters of 1 μm or less in the graph of Figure 11. In Figures 11 and 12, the X-axis shows "pore diameter (μm)" and the Y-axis shows "log differential pore volume (cc / g)." The reason why the cumulative pore volume for pore diameters of 1 μm or less was defined as the “pore volume” of each thermal spray powder is that the pore volume measured in the range of pore diameters greater than 1 μm contains many voids between the particles of the thermal spray powder (here, voids between secondary particles).

[0068] [Thermogravimetric analysis] The thermal spray powders of Examples 1 to 4 and the thermal spray powder of Comparative Example were subjected to reduction treatment. A thermogravimetric analysis was performed on each thermal spray powder after reduction treatment using a thermogravimetric differential thermal analyzer (STA2500 Regulus, manufactured by Netzsch). Specifically, 37.5 mg ± 2.5 mg of each thermal spray powder that had been subjected to reduction treatment was placed in an alumina pan, and the weight change of each thermal spray powder was measured when the temperature was raised from room temperature (30°C) to 1200°C at a heating rate of 10 K / min in an air atmosphere. The temperature at which the weight increased by 3% was defined as the "3% weight change point". The results are shown in "3% weight change point (°C)" in Table 1. In the reduction treatment, each thermal spray powder was held at a temperature of 800°C for 2 hours in a reducing atmosphere (hydrogen gas atmosphere).

[0069] <Preparation of thermal spray coating> Thermal spray coatings were produced by atmospheric plasma spraying using the thermal spray powders of Examples 1 to 4 and the thermal spray powder of the Comparative Example. An aluminum substrate was used as the substrate. The thermal spraying conditions were as follows: Thermal spray machine: SG-100 (Praxair) Powder feeder: Model 1264 (Praxair) Plasma working gas: Argon (Ar) gas (50 psi (0.34 MPa)); and Helium (He) gas (50 psi (0.34 MPa)) Plasma power: 34kW Plasma generation voltage: 37V Plasma generation current: 900A Spray powder supply rate: 17.5±5g / min Spray distance (distance from spray gun to substrate): 120mm Spray gun traverse speed: 400mm / s

[0070] [Evaluation of uniformity of components in thermal spray coating] The composition of the thermal spray coating of each example produced as described above was analyzed using SEM and energy dispersive X-ray spectroscopy (EDS) (Phenom ProX, manufactured by Phenom-World Corp.) Specifically, the following operations (1) to (7) were performed. (1) A composite of an aluminum substrate and a thermal spray coating was cut to obtain a thermal spray coating of a specified dimension, to obtain a test piece. (2) The test piece was immersed in an aqueous solution of sodium hydroxide to dissolve the aluminum substrate and isolate the thermal spray coating. (3) The isolated thermal spray coating was subjected to a reduction treatment under the same conditions as those described in the above [Thermogravimetric analysis] section. (4) The thermal sprayed coating after reduction treatment was embedded in epoxy resin and subjected to mechanical polishing and cross-section polishing. (5) For the surface polished in (4), the cross-sectional structure of the thermal spray coating was observed and analyzed by SEM and EDS in a field of view (approximately 27 μm × 27 μm) at a magnification of 10,000 times. In addition, one field of view was divided into 16, and the composition of the thermal spray coating in each divided field of view was quantified using a Phenom ProX manufactured by Phenom-World. Note that, here, the field of view was selected at an arbitrary position in the cross-sectional structure of the thermal spray coating, but the field of view was not selected from the surface side of the thermal spray coating or the region 20 μm from the substrate side. (6) The procedure of (5) was repeated five times, and the composition of the thermal spray coating was quantified in an 80-division field of view. (7) The coefficient of variation (standard deviation / average value) was calculated for the quantitative values ​​of Ni atoms in the 80-division field of view. The results are shown in the "coefficient of variation" column in Table 1. The coefficient of variation is an index for evaluating the uniformity of the components in a thermal spray coating. Here, the smaller the coefficient of variation, the better the uniformity of the components.

[0071] [Measurement of electrical conductivity of thermal spray coating] The electrical conductivity of the thermal spray coatings of Examples 1 to 4 and the thermal spray coating of the Comparative Example was measured using a low resistivity meter (Loresta GP MCP-T610, manufactured by Mitsubishi Analytech Co., Ltd.) Specifically, the following operations (1) to (3) were performed. (1) Each thermal spray powder was sprayed onto an alumina substrate (30 mm x 30 mm x 5 mm) to produce a thermal spray coating. The thermal spray conditions were the same as those described in the above section <Production of Thermal Spray Coating>. (2) The thermal spray coating was subjected to a reduction treatment to obtain a measurement sample. The conditions of the reduction treatment here were the same as those described in the above [Thermogravimetric analysis] section. (3) In an environment of temperature: 21°C and relative humidity: 37%, the measurement probe was brought into contact with the sample to measure the conductivity of the sample. The conductivity was measured at three points for each sample, and the average value was calculated. The results are shown in Table 1 as "Conductivity (×10 2 The values ​​are shown in the "S / cm" column. [App characteristics] The application characteristics were evaluated for the thermal spray coatings of Examples 1 to 4 and the thermal spray coating of the Comparative Example. 2 S / cm or more is marked with "◎", and the coefficient of variation is 0.09 or more and the conductivity is 3×10 2 S / cm or more is marked as "○", and the coefficient of variation is 0.09 or more and 3×10 2 Apps that scored below S were given an "X" rating and their overall characteristics were evaluated.

[0072] [Table 1]

[0073] As shown in Table 1, the thermal spray powders of Examples 1 to 4 have a peak in the range of 0.15 μm or more and 1 μm or less in the log differential pore volume distribution of pores with diameters of 1 μm or less obtained by mercury intrusion porosimetry. It was found that, when the thermal spray powders of Examples 1 to 4 are used, a thermal spray coating having a smaller coefficient of variation (i.e., a thermal spray coating with improved uniformity of composition) can be produced, as shown in Table 1, than the thermal spray coating of the comparative example. In addition, the thermal spray coatings produced using the thermal spray powders of Examples 1 to 4 had higher electrical conductivity and better application characteristics than the thermal spray coating of the comparative example. From these facts, it was found that the thermal spray powders of Examples 1 to 4 are preferable as thermal spray powders used to form electrodes (here, fuel electrodes) of SOFCs or SOECs.

[0074] Although specific examples of the technology disclosed herein have been described above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above.

[0075] The technology disclosed herein includes the inventions relating to the following items 1 to 9. [Item 1] A thermal spray powder for forming an electrode of a solid oxide fuel cell or a solid oxide electrolysis cell, comprising: A thermal spray powder having a peak in the range of 0.15 μm or more and 1 μm or less in the log differential pore volume distribution for pores with diameters of 1 μm or less obtained by mercury intrusion porosimetry. [Item 2] ionically conductive ceramic particles; Transition metal compound particles; 2. The thermal spray powder according to claim 1, comprising composite particles comprising: [Item 3] 3. The thermal spray powder according to item 2, wherein the composite particles have a region where the primary particles are in contact with each other and where there is no particle interface at the contact portion. [Item 4] 4. The thermal spray powder according to item 2 or 3, wherein a mass ratio of the ceramic particles to the transition metal compound particles (ceramic particles:transition metal compound particles) is 60:40 to 20:80. [Item 5] Median diameter (D 50 5. The thermal spray powder according to any one of items 1 to 4, wherein the average particle size is 10 μm or more and 100 μm or less. [Item 6] 5. The thermal spray powder according to any one of items 2 to 4, wherein the ceramic particles are zirconia particles containing a rare earth metal oxide. [Item 7] 5. The thermal spray powder according to any one of items 2 to 4, wherein the transition metal compound particles are nickel oxide particles. [Item 8] 8. The thermal spray powder according to any one of items 1 to 7, wherein the thermal spray powder has been subjected to a reduction treatment in a hydrogen gas atmosphere at a treatment temperature of 800° C. for two hours, and when the thermal spray powder is heated from room temperature to 1200° C. at a temperature increase rate of 10 K / min in an air atmosphere and subjected to thermogravimetric analysis, the temperature at which the weight increases by 3% is 470° C. or higher and 570° C. or lower. [Item 9] 9. The thermal spray powder according to any one of items 1 to 8, wherein the peak is in the range of 0.15 μm or more and 0.23 μm or less. [Explanation of symbols]

[0076] 1 Fuel electrode 2 Air electrode 3 Solid electrolyte layer 10 SOFC

Claims

1. A thermal spray powder for forming an electrode of a solid oxide fuel cell or a solid oxide electrolysis cell, comprising: A thermal spray powder having a peak in the range of 0.15 μm or more and 1 μm or less in a log differential pore volume distribution of pores having a diameter of 1 μm or less obtained by mercury intrusion porosimetry.

2. ionically conductive ceramic particles; Transition metal compound particles; The thermal spray powder of claim 1 , comprising composite particles comprising:

3. The thermal spray powder according to claim 2 , wherein the composite particles have a region where the primary particles are in contact with each other and where there is no particle interface at the contact portion.

4. 3. The thermal spray powder according to claim 2, wherein a mass ratio of the ceramic particles to the transition metal compound particles (ceramic particles:transition metal compound particles) is 60:40 to 20:

80.

5. Median diameter (D) based on laser diffraction scattering method 50 3. The thermal spray powder according to claim 1, wherein the average particle diameter is 10 μm or more and 100 μm or less.

6. The thermal spray powder according to claim 2 , wherein the ceramic particles are zirconia particles containing a rare earth metal oxide.

7. The thermal spray powder according to claim 2 , wherein the transition metal compound particles are nickel oxide particles.

8. 3. The thermal spray powder according to claim 1 or 2, wherein when the thermal spray powder is subjected to a reduction treatment in a hydrogen gas atmosphere at a treatment temperature of 800° C. for two hours and then heated from room temperature to 1,200° C. at a temperature increase rate of 10 K / min in an air atmosphere and subjected to thermogravimetric analysis, the temperature at which the weight increases by 3% is 470° C. or higher and 570° C. or lower.

9. The thermal spray powder according to claim 1 , wherein the peak is in the range of 0.15 μm or more and 0.23 μm or less.

Citation Information

Patent Citations

  • Powder for flame spray and flame spray material

    JP2016138309A

  • Powder for spray coating

    JP2016156046A

  • Metal supported solid oxide fuel cell and method for manufacturing the same

    US20140051006A1

  • Filtration membrane and methods of use and manufacture thereof

    US20200353424A1

  • Fuel electrode for solid-oxide fuel cell

    JP2009266713A