【0006】 本開示のナトリウムイオン二次電池は、可逆容量が大きい。
Smart Images

Figure 2024145933000001_ABST
Abstract
Description
[Technical field]
[0001] This application discloses a sodium ion secondary battery. [Background technology]
[0002] Patent Document 1 describes a compound having a P2 type structure and Na x Fe y Mn 1-y A Na-containing oxide having a chemical composition represented by O2 (x is less than 1, and y is 1 / 3 or more and less than 2 / 3) is disclosed. The Na-containing oxide is used as a positive electrode active material for a sodium ion secondary battery. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-201588 A Summary of the Invention [Problem to be solved by the invention]
[0004] Conventional sodium ion secondary batteries have room for improvement in terms of reversible capacity. [Means for solving the problem]
[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A sodium ion secondary battery having a positive electrode active material layer, the positive electrode active material layer contains Na-containing oxide particles as a positive electrode active material, The Na-containing oxide particles have a P2 type structure, The Na-containing oxide particles contain, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O, The Na-containing oxide particles are spherical, The surface of the Na-containing oxide particles has a plurality of crystallites and the average crystallite diameter of the crystallites is 600 nm or less, sodium ion secondary battery. <Aspect 2> A sodium ion secondary battery according to Aspect 1, wherein the average crystallite diameter of the crystallites is 450 nm or less, sodium ion secondary battery. <Aspect 3> A sodium ion secondary battery according to Aspect 1 or 2, wherein the Na-containing oxide particles contain at least Na, Mn, Ni, Co, and O as constituent elements, sodium ion secondary battery. <Aspect 4> A sodium ion secondary battery according to any one of Aspects 1 to 3, wherein the Na-containing oxide particles are Na a Mn x-p Ni y-q Co z-r M p+q+r O2 (where 0 < a ≤ 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). having a chemical composition represented by sodium ion secondary battery.
Advantages of the Invention
[0006] The sodium ion secondary battery of the present disclosure has a large reversible capacity.
Brief Description of the Drawings
[0007] [Figure 1] An example of the configuration of a sodium ion secondary battery is schematically shown. [Diagram 2] An example of the flow of a method for producing a Na-containing oxide having a P2-type structure is shown. [Diagram 3]1 shows X-ray diffraction patterns of the Na-containing oxides of Examples 1 and 2 and Comparative Examples 1 and 2. [Figure 4] 1 shows SEM photographs of the appearance of Na-containing oxide particles of Examples 1 and 2 and Comparative Examples 1 and 2. [Diagram 5] The relationship between crystallite size and discharge capacity (0.1C) is shown. [Figure 6] The relationship between crystallite size and capacity retention rate is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] FIG. 1 shows a schematic configuration of a sodium ion secondary battery according to one embodiment. As shown in FIG. 1, the sodium ion secondary battery 100 has a positive electrode active material layer 10. Here, the positive electrode active material layer 10 contains Na-containing oxide particles as a positive electrode active material. The Na-containing oxide particles have a P2 type structure. The Na-containing oxide particles contain at least one element selected from Mn, Ni, and Co, Na, and O as constituent elements. The Na-containing oxide particles are spherical. The surface of the Na-containing oxide particles has a plurality of crystallites. The average crystallite diameter of the crystallites is 600 nm or less. The sodium ion secondary battery 100 includes an obvious configuration as a secondary battery in addition to the positive electrode active material layer 10. For example, as shown in FIG. 1, the sodium ion secondary battery 100 may have an electrolyte layer 20, a negative electrode active material layer 30, a positive electrode current collector 40, and a negative electrode current collector 50.
[0009] 1.Cathode active material layer The positive electrode active material layer 10 contains at least the above-mentioned Na-containing oxide particles as a positive electrode active material, and may further contain an electrolyte, a conductive assistant, a binder, various additives, and the like. The contents of the positive electrode active material, electrolyte, conductive assistant, binder, and the like in the positive electrode active material layer 10 may be appropriately determined according to the intended battery performance. For example, the content of the positive electrode active material may be 40 mass% or more, 50 mass% or more, or 60 mass% or more, and may be 100 mass% or less, or 90 mass% or less, with the entire positive electrode active material layer 10 (total solid content) being 100 mass%. The shape of the positive electrode active material layer 10 is not particularly limited, and may be, for example, a sheet-like positive electrode active material layer having a substantially flat surface. The thickness of the positive electrode active material layer 10 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.
[0010] 1.1 Cathode active material The positive electrode active material layer 10 may contain only the above-mentioned Na-containing oxide particles as a positive electrode active material. Alternatively, the positive electrode active material layer 10 may contain, in addition to the above-mentioned Na-containing oxide particles, a different type of positive electrode active material (another positive electrode active material). The type of the other positive electrode active material is not particularly limited. From the viewpoint of further enhancing the effect of the technology of the present disclosure, the content of the other positive electrode active material in the positive electrode active material layer 10 may be small. For example, the content of the above-mentioned Na-containing oxide particles may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less.
[0011] 1.1.1 Crystal structure of Na-containing oxide particles The Na-containing oxide particles according to the embodiment have at least a P2 type structure (belonging to space group P63mc) as a crystal structure. The Na-containing oxide particles may have a crystal structure other than the P2 type structure in addition to the P2 type structure. Examples of the crystal structure other than the P2 type structure include various crystal structures (P3 type structure, etc.) formed when Na is desorbed from the P2 type structure. The Na-containing oxide particles may have a P2 type structure as a main phase. The crystal structure of the Na-containing oxide particles as a main phase may change depending on the charge / discharge state.
[0012] The surface of the Na-containing oxide particle according to the embodiment has a plurality of crystallites. When the surface of the Na-containing oxide particle is composed of a plurality of crystallites, a grain boundary is present on the surface of the particle. Here, the grain boundary may be an inlet and an outlet of intercalation. That is, when the Na-containing oxide particle has a plurality of crystallites on its surface, the effect of increasing the number of inlets and outlets of intercalation and decreasing the reaction resistance, the effect of shortening the distance of movement of sodium ions and decreasing the diffusion resistance, the absolute amount of expansion and contraction during charging and discharging is reduced, and the effect of cracking being less likely to occur can be expected. As a result, a large reversible capacity can be secured.
[0013] Here, it is considered that the smaller the crystallites on the surface of the Na-containing oxide particles, the higher the above-mentioned effect.In this embodiment, the average crystallite diameter of the crystallites on the surface of the Na-containing oxide particles is small, 600nm or less.The average crystallite diameter may be 550nm or less, 500nm or less, 450nm or less, 400nm or less, 380nm or less, 360nm or less, 340nm or less, or 320nm or less, or may be 50nm or more, 100nm or more, 150nm or more, 200nm or more, 250nm or more, or 300nm or more.
[0014] The "crystallites" and "average crystallite diameter" on the surface of the Na-containing oxide particles can be determined by observing the surface of the Na-containing oxide particles with a scanning electron microscope (SEM) or a transmission electron microscope (TEM). Specifically, when the surface of the Na-containing oxide particles is observed and one closed region surrounded by a grain boundary is observed, the region is regarded as a "crystallite". The maximum Feret diameter of the crystallite is determined and this is regarded as the "maximum diameter" of the crystallite. The minimum Feret diameter of the crystallite is determined and this is regarded as the "minimum diameter" of the crystallite. The average value ([maximum diameter + minimum diameter] / 2) of the "maximum diameter" and "minimum diameter" of the crystallite is regarded as the "crystallite diameter" of the crystallite. The "crystallite diameter" of each crystallite present on the surface of the Na-containing oxide particles is determined as described above, and the number average value is regarded as the "average crystallite diameter" of the crystallites on the surface of the Na-containing oxide particles. Here, when specifying the "average crystallite size", it is not necessary to determine all the "crystallite sizes" of the crystallites present on the surface of the Na-containing oxide particle. For example, from the crystallites on the surface of one Na-containing oxide particle, four or more crystallites are extracted in order of the largest crystallite size, and the number average value of each of the four or more extracted crystallites is calculated, which can be regarded as the "average crystallite size" of the crystallites on the surface of the Na-containing oxide particle.
[0015] The crystallites constituting the Na-containing oxide particles may have a first surface exposed on the particle surface, and the first surface may be planar. That is, the surface of the Na-containing oxide particles may have a structure in which a plurality of planes are connected. As described later, when producing the Na-containing oxide particles, crystallites having a planar first surface are easily obtained by growing the crystallites on the surface of the particles until one crystallite and another crystallite are connected to each other.
[0016] 1.1.2 Chemical composition of Na-containing oxide particles The Na-containing oxide particles according to the embodiment contain, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O. In particular, when the constituent elements contain at least Na, Mn, at least one element selected from Ni and Co, and O, and especially when the constituent elements contain at least Na, Mn, Ni, Co, and O, excellent performance as a positive electrode active material is easily obtained. Alternatively, when the constituent elements contain at least Na, Mn, Fe, and O, excellent performance as a positive electrode active material particle is easily obtained. However, the Na-containing oxide particles may release Na upon charging, and the amount of Na present may become close to 0. In one embodiment, the Na-containing oxide particles contain Na a Mn x-p Ni y-q Co z-r M p+q+rIt may have a chemical composition represented by O2 (where 0 < a ≤ 1.00, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). When the Na-containing oxide has such a chemical composition, the P2-type structure is likely to be maintained. In the above chemical composition, a is greater than 0, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, or 0.70 or less. Also, x is 0 or more, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. Also, y is 0 or more, and may be 0.10 or more or 0.20 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. Also, z is 0 or more, and may be 0.10 or more, 0.20 or more, or 0.30 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. The element M has little contribution to charge and discharge. In this regard, in the above chemical composition, since p + q + r is less than 0.17, a high charge and discharge capacity is likely to be ensured. p + q + r may be 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, or 0.10 or less. On the other hand, when the element M is included, the P2-type structure is likely to be stabilized. In the above chemical composition, p + q + r is 0 or more, and may be 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, or 0.10 or more. The composition of O is approximately 2, but is not necessarily exactly 2.0 and is indefinite.
[0017] 1.1.3 Shape of Na-containing oxide particles The P2 type structure is a hexagonal crystal system, has a large diffusion coefficient of Na ions, and is likely to grow crystals in a specific direction. In particular, when at least one of Mn, Ni, and Co is included as a transition metal element constituting the P2 type structure, the crystals tend to grow in a plate-like shape in a specific direction. Therefore, the Na-containing oxide having the P2 type structure usually becomes a plate-like particle with a large aspect ratio in which the crystal growth direction is biased in a specific direction. In contrast, the Na-containing oxide particles according to this embodiment are spherical, as described above. When the Na-containing oxide particles are spherical, the reaction resistance decreases due to the reduction in crystallite size, and the diffusion resistance inside the particles tends to decrease. Furthermore, in the positive electrode active material layer 10, it is considered that the degree of bending is reduced by spheroidization, and the sodium ion conduction resistance decreases. As a result, for example, the rate characteristics are improved and the reversible capacity is likely to increase. In addition, in this application, the "spherical particles" means particles having a circularity of 0.80 or more. The circularity of the particles may be 0.81 or more, 0.82 or more, 0.83 or more, 0.84 or more, 0.85 or more, 0.86 or more, 0.87 or more, 0.88 or more, 0.89 or more, or 0.90 or more. The circularity of the particles is 4πS / L 2 Here, S is the orthogonal projected area of the particle, and L is the perimeter of the orthogonal projected image of the particle. The circularity of a particle can be determined by observing the appearance of the particle with a scanning electron microscope (SEM), a transmission electron microscope (TEM), or an optical microscope. When a particle is made up of 100 or more particles, the circularity is measured, for example, as an average value as follows.
[0018] (1) First, the particle size distribution of the particles is measured. Specifically, the particle size at 10% cumulative value (D10) and the particle size at 90% cumulative value (D90) in the volume-based particle size distribution are determined by a laser diffraction / scattering method. (2) Regarding the appearance of the particles whose particle size distribution has been measured, images are observed using a SEM, TEM, or optical microscope, and from the particles contained in the images, 100 particles having a circle equivalent diameter (the diameter of a circle having the same area as the orthogonal projected area of the particle) equal to or greater than D10 and equal to or less than D90 as determined in (1) are randomly selected. (3) The circularity of each of the 100 extracted particles is determined by image processing, and the average value is regarded as the "circularity of the particle."
[0019] The Na-containing oxide particles according to the embodiment may be solid particles, hollow particles, or particles having voids. The size of the Na-containing oxide particles is not particularly limited, but it is considered that a smaller size is more advantageous. For example, the average particle diameter (D50) of the Na-containing oxide particles may be 0.1 μm or more and 10 μm or less, 1.0 μm or more and 8.0 μm or less, or 2.0 μm or more and 6.0 μm or less. The average particle diameter (D50) is the particle diameter (D50, median diameter) at an integrated value of 50% in the volume-based particle size distribution by a laser diffraction / scattering method.
[0020] 1.1.4 Manufacturing method of Na-containing oxide particles The Na-containing oxide particles according to the embodiment can be produced, for example, by the following method. That is, as shown in Fig. 2, the method for producing a Na-containing oxide according to one embodiment includes: S1: obtaining a precursor containing at least one element of Mn, Ni, and Co; S2: coating the surface of the precursor with a Na source to obtain a composite; and S3: calcining the composite to obtain Na-containing oxide particles having a P2 type structure.
[0021] In S1, a precursor containing at least one element of Mn, Ni, and Co is obtained. The precursor may contain at least Mn, one or both of Ni and Co, or may contain at least Mn, Ni, and Co. The precursor may be a salt containing at least one element of Mn, Ni, and Co. For example, the precursor may be at least one of carbonate, sulfate, nitrate, and acetate. Alternatively, the precursor may be a compound other than a salt. For example, the precursor may be a hydroxide. The precursor may be a hydrate. The precursor may be a combination of multiple types of compounds. The precursor may be particulate or may be spherical particles. The particle size of the particles made of the precursor is not particularly limited.
[0022] In S1, a precipitate as the precursor may be obtained by a coprecipitation method using an ion source capable of forming a precipitate in an aqueous solution with transition metal ions and a transition metal compound containing at least one element selected from Mn, Ni, and Co. This makes it easier to obtain spherical particles as the precursor. The "ion source capable of forming a precipitate in an aqueous solution with transition metal ions" may be at least one selected from, for example, sodium salts such as sodium carbonate and sodium nitrate, sodium hydroxide, and sodium oxide. The transition metal compound may be the above salt or hydroxide containing at least one element selected from Mn, Ni, and Co. Specifically, in S1, the ion source and the transition metal compound may be prepared as solutions, and the solutions may be dropped and mixed to obtain a precipitate as the precursor. In this case, for example, water is used as the solvent. In this case, various sodium compounds may be used as the base, and an aqueous ammonia solution or the like may be added to adjust the basicity. In the case of the coprecipitation method, for example, an aqueous solution of a transition metal compound and an aqueous solution of sodium carbonate are prepared, and the aqueous solutions are dropped and mixed to obtain a precipitate as the precursor. Alternatively, the precursor can be obtained by a sol-gel method, and in particular, by a coprecipitation method, spherical particles can be easily obtained as the precursor.
[0023] In S1, the precursor may contain element M. Element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. These elements M have, for example, a function of stabilizing the P2 type structure. The method of obtaining a precursor containing element M is not particularly limited. When the precursor is obtained by coprecipitation in S1, for example, an aqueous solution of a transition metal compound containing at least one of Mn, Ni, and Co, an aqueous solution of sodium carbonate, and an aqueous solution of a compound of element M are prepared, and each aqueous solution is dropped and mixed to obtain a precursor containing element M together with at least one element of Mn, Ni, and Co. Alternatively, in the manufacturing method of the present disclosure, element M may not be added in S1, and element M may be doped when Na-doping baking is performed in S2 and S3 described later.
[0024] In S2, the surface of the precursor obtained in S1 is coated with a Na source to obtain a composite. The Na source may be a salt containing Na, such as a carbonate or a nitrate, or may be a compound other than a salt, such as sodium oxide or sodium hydroxide. In S2, the amount of the Na source coated on the surface of the precursor may be determined taking into account the amount of Na lost during the subsequent calcination.
[0025] In S2, the coverage of the Na source on the surface of the precursor is not particularly limited. For example, in S2, the above-mentioned composite may be obtained by covering 40 area% or more, 50 area% or more, 60 area% or more, or 70 area% or more of the surface of the above-mentioned precursor with the Na source. Here, when the precursor obtained by S1 is a spherical particle, and the composite obtained by S2 is obtained by covering 40 area% or more of the surface of the precursor with the Na source, spherical Na-containing oxide particles having a P2 type structure are likely to be obtained in S3 described later. If the coverage of the Na source is small, when the composite is fired, P2 type crystals are likely to grow abnormally on the surface of the composite, and the Na-containing oxide is likely to become plate-like. If the coverage of the Na source is large, when the composite is fired, the crystallites of the P2 type crystals are likely to become small, and the Na-containing oxide is likely to become spherical particles corresponding to the shape of the precursor.
[0026] In S2, the method for coating the surface of the precursor with the Na source is not particularly limited. As described above, when 40% or more of the area of the surface of the precursor is coated with the Na source, various methods can be used. For example, a tumbling fluidized coating method or a spray drying method can be used. That is, a coating solution in which a Na source is dissolved is prepared, and the coating solution is brought into contact with the surface of the precursor, and dried at the same time or after the contact. By adjusting the coating conditions (temperature, time, number of times, etc.), 40% or more of the area of the surface of the precursor can be coated with the Na source.
[0027] In S2, the precursor may be coated with an M source together with a Na source. For example, in S2, the precursor obtained in S1, a Na source, and an M source containing at least one element M selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W may be mixed to obtain a composite. The M source may be, for example, a salt containing the element M, such as a carbonate or sulfate, or a compound other than a salt, such as an oxide or hydroxide. The amount of the M source relative to the precursor may be determined depending on the chemical composition of the Na-containing oxide after firing.
[0028] In S3, the composite obtained in S2 is fired to obtain Na-containing oxide particles having a P2 type structure. In S3, the composite may be optionally shaped and optionally pre-fired, and then fired. The pre-fire of the composite may be performed at a temperature equal to or lower than the temperature of the main firing. For example, the pre-fire may be performed at a temperature lower than 700°C. The pre-fire time is not particularly limited. The pre-fire atmosphere is also not particularly limited.
[0029] In S3, the composite may be sintered at a temperature of, for example, 700°C or more and 1100°C or less. It is preferably 800°C or more and 1000°C or less, more preferably 850°C or more and 900°C or less. If the sintering temperature is too low, Na doping is not performed, and if the sintering temperature is too high, O3 phase or the like is likely to be generated instead of P2 phase. In addition, if the sintering temperature is too high, the crystallites grow excessively and tend to become plate-like particles rather than spherical. As far as the inventors have confirmed, when the sintering temperature is 830°C or more and 920°C or less, Na-containing oxide particles having small crystallite size and spherical shape are likely to be obtained. The temperature rise condition from the preliminary sintering temperature to the sintering temperature is not particularly limited.
[0030] The firing time is not particularly limited, and may be, for example, 30 minutes or more and 48 hours or less. However, the shape of the Na-containing oxide particles can be controlled by the firing time. As described above, when the coverage rate of the Na source in the composite is 40 area % or more in S2, when the composite is fired in S3, P2 type crystals with small crystallites are likely to be formed on the surface. In S3, the P2 type crystals are grown along the surface of the particles so that one P2 type crystallite and another P2 type crystallite are connected to each other, so that the shape of the Na-containing oxide particles corresponds to the shape of the precursor. For example, when the precursor is a spherical particle, the Na-containing oxide particles can also be spherical particles. If the firing time is too short, Na doping is not performed and the desired P2 type structure is not obtained. On the other hand, if the firing time is too long, the crystallites grow excessively, and the particles tend to be plate-like rather than spherical. As far as the present inventors have confirmed, if the firing time is 30 minutes or more and 3 hours or less, spherical particles of Na-containing oxide are likely to be obtained.
[0031] 1.2 Electrolytes The electrolyte that can be contained in the positive electrode active material layer 10 may be a solid electrolyte, a liquid electrolyte (electrolytic solution), or a combination of these. The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. Examples of inorganic solid electrolytes include Na3Zr2PSi2O 12 and oxides such as Na2O-11Al2O3; NaBH4, NaB 10 H 10 , NaCB9H 10 , NaCB 11 H 12 , NaB 12 Cl 12 Hydrides and borides such as Na3PS4, Na3SbS4, Na 2.88 Sb 0.88 W 0.12Examples of the solid electrolyte include at least one selected from sulfides such as S4 and fluorides such as NaPF6 and NaBF4. The solid electrolyte may be, for example, particulate. Only one type of solid electrolyte may be used alone, or two or more types may be used in combination. The electrolytic solution may contain, for example, sodium ions as carrier ions. The electrolytic solution may be an aqueous electrolytic solution or a non-aqueous electrolytic solution. The composition of the electrolytic solution may be the same as that of the electrolytic solution of a sodium ion secondary battery known in the art. For example, the electrolytic solution may be a carbonate-based solvent in which a sodium salt is dissolved at a predetermined concentration. Examples of the carbonate-based solvent include fluoroethylene carbonate (FEC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), and the like. Examples of the sodium salt include NaPF6 and the like.
[0032] 1.3 Conductive additives The conductive assistant that can be contained in the positive electrode active material layer 10 may be at least one selected from carbon materials such as vapor grown carbon fiber (VGCF), acetylene black (AB), ketjen black (KB), carbon nanotubes (CNT), carbon nanofibers (CNF), etc.; and metal materials such as nickel, aluminum, stainless steel, etc. The conductive assistant may be, for example, particulate or fibrous, and its size is not particularly limited.
[0033] 1.4 Binder The binder that can be contained in the positive electrode active material layer 10 may be at least one selected from, for example, a butadiene rubber (BR)-based binder, a butylene rubber (IIR)-based binder, an acrylate butadiene rubber (ABR)-based binder, a styrene butadiene rubber (SBR)-based binder, a polyvinylidene fluoride (PVdF)-based binder, a polytetrafluoroethylene (PTFE)-based binder, a polyimide (PI)-based binder, and the like.
[0034] 2.Other configurations 2.1 Electrolyte layer The electrolyte layer 20 includes at least an electrolyte, and optionally includes a binder, etc. The electrolyte may be a solid electrolyte, a liquid electrolyte (electrolytic solution), or a combination of these. The electrolyte included in the electrolyte layer 20 may be appropriately selected from those exemplified as electrolytes that may be included in the above-mentioned positive electrode active material layer. The binder that may be included in the electrolyte layer 20 may also be appropriately selected from those exemplified as binders that may be included in the above-mentioned positive electrode active material layer. Only one type of electrolyte or binder may be used alone, or two or more types may be used in combination. The component composition, shape, etc. of the electrolyte layer 20 may be the same as those of the conventional ones.
[0035] 2.2 Negative electrode active material layer The negative electrode active material layer 30 includes at least a negative electrode active material, and may further include an electrolyte, a conductive assistant, a binder, various additives, and the like. The negative electrode active material may be any of various materials having a potential (charge / discharge potential) for absorbing and releasing sodium ions that is lower than that of the positive electrode active material. For example, an inorganic negative electrode active material such as metallic sodium may be used, or an organic compound may be used. The negative electrode active material may be used alone or in combination of two or more. Examples of the electrolyte that may be included in the negative electrode active material layer 30 include the above-mentioned solid electrolyte, electrolytic solution, or a combination thereof. Examples of the conductive assistant that may be included in the negative electrode active material layer 30 include the above-mentioned carbon material and metal material. The binder that may be included in the negative electrode active material layer 30 may be appropriately selected from those exemplified as the binder that may be included in the positive electrode active material layer 10. The electrolyte, conductive assistant, and binder may each be used alone or in combination of two or more. The component composition, shape, and the like of the negative electrode active material layer 30 may be the same as those of the conventional ones.
[0036] 2.3 Current collector The positive electrode current collector 40 and the negative electrode current collector 50 can be any of those generally used as current collectors for batteries. The current collectors 40 and 50 may be in the form of a foil, a plate, a mesh, a punched metal, or a foam. The current collectors 40 and 50 may be made of a metal foil or a metal mesh. Examples of metals constituting the current collectors 40 and 50 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, and stainless steel. In particular, the positive electrode current collector 40 may contain Al from the viewpoint of ensuring oxidation resistance. The negative electrode current collector 50 may contain at least one metal selected from Cu, Ni, and stainless steel from the viewpoint of ensuring reduction resistance. The current collectors 40 and 50 may have some kind of coating layer on their surfaces for the purpose of adjusting resistance. The current collectors 40 and 50 may be metal foil or a substrate on which the above metals are plated or vapor-deposited. The shapes of the current collectors 40, 50 may be the same as those of conventional current collectors. EXAMPLES
[0037] The sodium ion secondary battery according to the above embodiment can be modified in various ways without departing from the spirit of the present invention. The sodium ion secondary battery according to the present disclosure will be described in more detail below with reference to examples, but the technology of the present disclosure is not limited to the following examples.
[0038] 1. Preparation of Na-containing oxides with P2 structure 1.1 Preparation of precursor (1) MnSO4·5H2O, NiSO4·6H2O, and CoSO4·7H2O were weighed out to obtain the desired composition ratio, and dissolved in distilled water to obtain a concentration of 1.2 mol / L to obtain a first solution. In a separate container, Na2CO3 was dissolved in distilled water to obtain a concentration of 1.2 mol / L to obtain a second solution. (2) 1000 mL of pure water was placed in a reaction vessel (with a baffle plate), and 500 mL of the first solution and 500 mL of the second solution were each added dropwise at a rate of about 4 mL / min. (3) After the dropwise addition was completed, the mixture was stirred at room temperature at a stirring speed of 150 rpm for 1 hour to obtain a product. (4) The product was washed with pure water, subjected to solid-liquid separation using a centrifuge, and the precipitate was collected. (5) The obtained precipitate was dried overnight at 120°C, crushed in a mortar, and then fine particles were removed by air classification to obtain precursor particles. The precursor particles were a composite salt containing Mn, Ni, and Co, and were spherical particles with a circularity of 0.80 or more.
[0039] 1.2 Preparation of the complex (1) Na2CO3 as a Na source and the above precursor particles are mixed to obtain a composition after calcination as described below. 0.7 Mn 0.5 Ni 0.2 Co 0.3 It was weighed to be O2. (2) The weighed Na source and precursor particles were mixed by spray drying. Specifically, the weighed Na source and precursor particles were added to a solvent, and the dispersion solution in which the Na source was dissolved and the precursor particles were dispersed was spray dried. The spray drying temperature was 200°C, and the spray pressure was 0.3 MPa. A composite in which 75 area % of the surface of the precursor particles was covered with the Na source was obtained by spray drying.
[0040] 1.3 Firing of the composite The composite was placed in an alumina crucible and sintered under the following sintering conditions (1) to (7). (1) The alumina crucible containing the above composite is placed in a heating furnace. (2) The temperature inside the heating furnace is raised from room temperature to 600°C in two hours. (3) The inside of the heating furnace is kept at 600°C for six hours to perform pre-firing. (4) After the preliminary firing, the temperature inside the heating furnace is raised from 600° C. to the firing temperature. The firing temperatures are 870° C. for Example 1, 900° C. for Example 2, 950° C. for Comparative Example 1, and 980° C. for Comparative Example 2. (5) The temperature inside the heating furnace is maintained at the final firing temperature for one hour to perform the final firing. (6) After the main firing, the temperature inside the heating furnace is lowered from the main firing temperature to 250°C. (7) Remove the alumina crucible from the heating furnace at 250°C and allow it to cool in the air.
[0041] The fired product after cooling in the air was pulverized in a mortar in a dry atmosphere to obtain Na-containing oxide particles having a P2 type structure. 0.7 Mn 0.5 Ni 0.2 Co 0.3 It had a chemical composition indicated as O2.
[0042] 2.Evaluation of Na-containing oxide particles 2.1 Identification of crystal structure by X-ray diffraction measurement For each of the Na-containing oxide particles of Examples 1 and 2 and Comparative Examples 1 and 2, an X-ray diffraction measurement was performed using CuKα as a radiation source to obtain an X-ray diffraction pattern. Figure 3 shows the X-ray diffraction patterns of each of the Na-containing oxide particles of Examples 1 and 2 and Comparative Examples 1 and 2. As shown in Figure 3, it can be seen that all of the Na-containing oxide particles have a P2 type structure belonging to the space group P63mc.
[0043] 2.2 Appearance observation by SEM Fig. 4 shows SEM photographs of the appearance of each of the Na-containing oxides of Examples 1 and 2 and Comparative Examples 1 and 2. As is clear from Fig. 4, the Na-containing oxide particles of Examples 1 and 2 and Comparative Example 1 are spherical particles having a circularity of 0.80 or more. The surfaces of the spherical particles are composed of a plurality of crystallites. On the other hand, the Na-containing oxide particles of Comparative Example 2 are composed of plate-like single crystals. The following Table 1 shows the average crystallite diameter of the crystallites on the surface of each particle (the diameter of the plate-like particle itself for Comparative Example 2).
[0044] 3. Electrochemical Measurements P2-type Na-containing oxide particles, acetylene black, and PVdF were weighed out to a mass ratio of 80:15:5, and dispersed and mixed in N-methyl-2-pyrrolidone to form a slurry. The slurry was applied onto an Al foil, pressed, and then vacuum-dried at 120°C overnight to obtain a positive electrode. Metal Na foil was used for the negative electrode. A polycarbonate solution containing 1M NaPF6 was used as the electrolyte. A coin cell (CR2032) was produced using these positive electrode, negative electrode, and electrolyte. The produced coin cell was charged and discharged in a thermostatic chamber at 25°C at a voltage range of 1.5V-4.5V and a 0.1C rate (1C=200mA / g), and the discharge capacity (1) was measured. Subsequently, the discharge capacity (2) was measured when the cell was charged at a voltage range of 1.5V-4.5V and a 0.1C rate, and then discharged at 0.5C. The ratio of discharge capacity (2) to discharge capacity (1) ([discharge capacity (2) / discharge capacity (1)]×100) was calculated and evaluated as the capacity retention rate (output retention rate). The results are shown in Table 1 below and in FIGS. 5 and 6.
[0045] [Table 1]
[0046] 4. Evaluation Results 5 and 6, in Comparative Examples 1 and 2, the average crystallite diameter of the Na-containing oxide particles was significantly greater than 600 nm, the capacity of the coin cell was small, and the capacity retention rate was also poor at less than 60%. In contrast, in Examples 1 and 2, the average crystallite diameter of the Na-containing oxide particles was 600 nm or less, the capacity of the coin cell was large, and the capacity retention rate was also excellent at more than 60%.
[0047] 6. Summary As described above, in a sodium ion secondary battery, if the positive electrode active material layer contains Na-containing oxide particles as a positive electrode active material, the Na-containing oxide particles have a P2 type structure, the Na-containing oxide particles contain at least one element selected from Mn, Ni, and Co, Na, and O as constituent elements, the Na-containing oxide particles are spherical, the surfaces of the Na-containing oxide particles have a plurality of crystallites, and the average crystallite diameter of the crystallites is 600 nm or less, then the sodium ion secondary battery can be said to have a large reversible capacity. [Explanation of symbols]
[0048] 100 Sodium-ion secondary battery 10 Cathode active material layer 20 Electrolyte layer 30 Negative electrode active material layer 40 Positive electrode current collector 50 Negative electrode current collector
Claims
1. A sodium ion secondary battery having a positive electrode active material layer, the positive electrode active material layer contains Na-containing oxide particles as a positive electrode active material, The Na-containing oxide particles have a P2 type structure, The Na-containing oxide particles contain, as constituent elements, at least one element selected from Mn, Ni, and Co, Na, and O, The Na-containing oxide particles are spherical, The surface of the Na-containing oxide particle has a plurality of crystallites, and The average crystallite diameter of the crystallites is 600 nm or less. Sodium ion secondary battery.
2. The sodium ion secondary battery according to claim 1, The average crystallite diameter of the crystallites is 450 nm or less. Sodium ion secondary battery.
3. The sodium ion secondary battery according to claim 1, The Na-containing oxide particles contain at least Na, Mn, Ni, Co and O as constituent elements. Sodium ion secondary battery.
4. The sodium ion secondary battery according to any one of claims 1 to 3, The Na-containing oxide particles are a Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0<a≦1.00, x+y+z=1, and 0≦p+q+r<0.17; and element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), Sodium ion secondary battery.
Citation Information
Patent Citations
Positive electrode active material for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery
JP2015092454A
Control method of sodium ion secondary battery, controller for sodium ion secondary battery, and sodium ion secondary battery for use in control method or controller for sodium ion secondary battery
JP2017045600A
Nonaqueous electrolytic solution and power storage device
WO2018151234A1
Nickel-containing hydroxide and production method therefor
WO2019117027A1
Complex metal oxide, positive electrode active material for sodium secondary battery, positive electrode for sodium secondary battery, and the sodium secondary battery
JP2012201588A
Cited By
Positive electrode material for sodium-ion battery, preparation method therefor, positive electrode composition, sodium-ion secondary battery, and use thereof