Binder resin and battery
A copolymer-based binder resin with a carbonate skeleton and phosphoric acid group-containing (meth)acrylate compound addresses the adhesion and binding issues in secondary batteries, enhancing ionic conductivity and battery performance by controlling swelling properties.
Patent Information
- Application Number
- JP2023058831
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing binder resins for secondary batteries, such as those used in lithium ion batteries, face challenges in achieving optimal adhesion to metal foils and binding of inorganic materials while maintaining suitable swelling properties with electrolytic solutions, leading to poor adhesion and binding properties when exposed to electrolytes.
A binder resin with a specific copolymer structure, comprising a carbonate skeleton and a phosphoric acid group-containing (meth)acrylate compound, exhibits a swelling degree of 200% to 1000% in a mixed solvent of ethylene carbonate and dimethyl carbonate, ensuring excellent adhesion to metal foils and binding of inorganic materials without excessive swelling, thereby improving ionic conductivity and battery performance.
The binder resin enhances adhesion to metal foils and binding of inorganic materials, improving ionic conductivity and reducing the formation of the Solid Electrolyte Interphase (SEI) layer, thus extending the lifespan and performance of secondary batteries.
Smart Images

Figure 2024146111000027 
Figure 2024146111000028 
Figure 2024146111000029
Abstract
Description
[Technical field]
[0001] The present invention relates to a binder resin and a battery. [Background technology]
[0002] The binder resin is capable of binding the organic material, the inorganic material, and other materials together by being mixed with the organic material, the inorganic material, and other materials.
[0003] Patent Document 1 describes a polyalkylene carbonate resin containing a repeating unit represented by a specific chemical formula.
[0004] Patent Document 2 describes a binder composition for producing an electrode used in an electricity storage device. The binder composition described in Patent Document 2 contains a polymer (A) and a liquid medium (B), the polymer (A) is in the form of polymer particles, and the ratio (DA / DB) of the average particle diameter (DA) of the polymer particles measured by dynamic light scattering to the average particle diameter (DB) of the polymer particles measured by TEM observation is 2 to 10. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6023893 [Patent Document 2] International Publication No. 2016 / 039067 Summary of the Invention [Problem to be solved by the invention]
[0006] Binder resins are used in various applications, for example, as materials in the field of batteries. Binder resins are used, for example, in composite layers constituting electrodes of secondary batteries. Electrodes of secondary batteries generally include a current collector and a composite layer, and the composite layer contains, for example, an active material and a binder resin. By including a binder resin in the composite layer, properties such as adhesion between the composite layer and the current collector and binding properties of the active material included in the composite layer can be obtained.
[0007] The polyalkylene carbonate resin disclosed in Patent Document 1 is said to be able to exhibit improved thermal stability since it can suppress decomposition due to backbiting of polymer chains when exposed to heat during thermal curing or use. However, there is no description that the polyalkylene carbonate resin disclosed in Patent Document 1 functions as a binder resin, nor is there any description that the polyalkylene carbonate resin has adhesion to metal foil or is used as a binder resin for binding materials such as inorganic materials. Furthermore, there is no description that the polyalkylene carbonate resin disclosed in Patent Document 1 is a material suitable for use in electrodes of secondary batteries.
[0008] The binder composition described in Patent Document 2 is said to have an electrolyte swelling degree in the range of 100% to 130%, so that the polymer particles contained in the binder composition have an appropriate swelling property in the electrolyte, effectively reducing the electrode resistance, realizing better charge / discharge characteristics, and having excellent binding properties. On the other hand, Patent Document 2 discloses that the binder composition described in Patent Document 2 has poor binding properties for the active material contained in the composite layer and also poor adhesion between the composite layer and the current collector when the electrolyte swelling degree is higher than 130%.
[0009] As one of high-performance secondary batteries, secondary batteries using lithium ions or the like have been attracting attention. The secondary battery using lithium ions or the like includes, for example, a positive electrode, a negative electrode, an electrolyte, and a separator disposed between the positive electrode and the negative electrode. Further high performance is required for the secondary battery using lithium ions or the like, and various studies have been conducted on the materials used for the secondary battery. Various studies have also been conducted on the materials used for the electrodes of the secondary battery.
[0010] For example, when a binder resin is used in a composite layer of a secondary battery, it is required to have a better swelling property with respect to an electrolyte. On the other hand, the binder resin is also required to have adhesion to a metal foil as a current collector and binding property of an inorganic material as an active material contained in the composite layer. For this reason, further improvement of the binder resin is required.
[0011] An object of the present invention is to provide a binder resin that has excellent adhesion to metal foil and excellent binding ability to inorganic materials, and a battery containing the binder resin. [Means for solving the problem]
[0012] [1] A binder resin, The degree of swelling in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 is 200% or more and less than 1000%. Binder resin.
[0013] [2] In the binder resin according to [1], a binder resin-containing composition containing the binder resin is prepared, a laminate is produced in which a coating layer made of the binder resin-containing composition is provided on a metal foil, and then the laminate is immersed in the mixed solvent at a temperature of 23° C. for 24 hours without stirring; and the coating layer does not break or peel off from the metal foil. Binder resin.
[0014] [3] In the binder resin according to [2], The metal foil is a copper foil or an aluminum foil, When immersed in the mixed solvent, the coating layer does not peel off from the metal foil. Binder resin.
[0015] [4] In the binder resin according to any one of [1] to [3], The copolymer includes a structural unit represented by the following general formula (1) and a structural unit represented by the following general formula (2) in an amount of more than 1.0 mol % and not more than 20.0 mol %: Binder resin.
[0016] [ka]
[0017] (In the general formula (1) and the general formula (2), R 1 is a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or an alkoxyalkyl group having 1 to 8 carbon atoms; L 1 and L 2 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms; L 3 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms; X 1 is any one of the reactive groups represented by the following structural formula (2-1), (2-2), and (2-3).
[0018] [ka]
[0019] [5] In the binder resin according to [4], -L in the general formula (2) 3 -X 1 is any one of reactive groups represented by the following structural formula (2-4), the following structural formula (2-5), and the following structural formula (2-6): Binder resin.
[0020] [ka]
[0021] [6] The binder resin according to [4] or [5], The copolymer further contains at least one structural unit selected from the group consisting of a structural unit represented by the following general formula (3) and a structural unit represented by the following general formula (4), in an amount of 0.1 mol % to 30.0 mol %: Binder resin.
[0022] [ka]
[0023] (In the general formula (3) and the general formula (4), R 2 is a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or an alkoxyalkyl group having 1 to 8 carbon atoms; L 4 and L 5 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms; L 6 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms; X 2 is any one of the reactive groups represented by the following structural formula (4-1), (4-2), and (4-3).
[0024] [ka]
[0025] [7] In the binder resin according to any one of [4] to [6], The copolymer is further copolymerized with at least one phosphoric acid group-containing (meth)acrylate compound selected from the group consisting of the following general formula (5-1) and the following general formula (5-2): Binder resin.
[0026] [ka]
[0027] [ka]
[0028] (In the general formula (5-1), R 3 and R 4 are each independently a hydrogen atom or a methyl group; L 7 and L 8 are each independently an alkylene group having 2 to 4 carbon atoms, and in the general formula (5-2), R 5 is a hydrogen atom or a methyl group, and L 9 is an alkylene group having 2 to 4 carbon atoms.
[0029] [8] In the binder resin according to [7], The copolymer is obtained by copolymerizing 0.2 to 15.0 parts by mole of the phosphoric acid group-containing (meth)acrylate compound with respect to 100 parts by mole of the copolymer. Binder resin.
[0030] [9] A binder resin according to any one of [1] to [8], battery. Effect of the Invention
[0031] According to the present invention, it is possible to provide a binder resin that has excellent adhesion to metal foil and excellent binding properties for inorganic materials, and a battery that includes the binder resin. [Brief description of the drawings]
[0032] [Figure 1] 1 is a cross-sectional view illustrating an example of a main part of a battery according to an embodiment of the present invention. [Diagram 2] 1 is a chart showing the results of 1H-NMR measurement of the copolymer produced in Example 1. [Diagram 3] 1 is a chart showing the results of 1H-NMR measurement of the copolymer produced in Example 2. [Figure 4] 1 is a chart showing the results of 1H-NMR measurement of the copolymer produced in Example 3. [Diagram 5] 1 is a chart showing the results of 1H-NMR measurement of the copolymer produced in Example 4. [Figure 6] 1 is a chart showing the results of 1H-NMR measurement of the copolymer produced in Example 5. [Figure 7] 1 is a chart showing the results of 1H-NMR measurement of the copolymer produced in Example 6. [Figure 8] 1 is a chart showing the results of 1H-NMR measurement of the copolymer produced in Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] The present invention will be described below by taking an embodiment as an example, but the present invention is not limited to the content of the embodiment.
[0034] [Binder resin] A preferred example of the binder resin according to this embodiment will be described.
[0035] The binder resin according to the present embodiment has a swelling degree of 200% or more and less than 1000% in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1. The binder according to the present embodiment has the above-mentioned configuration, and therefore has excellent adhesion to metal foil and binding properties for inorganic materials. Specifically, when the binder resin according to the present embodiment is used as a material for a composite layer in an electrode of a secondary battery, the binder resin according to the present embodiment has excellent swelling properties in an electrolyte, and has excellent adhesion to metal foil and binding properties for inorganic materials. The reason for this is unclear, but is thought to be as follows.
[0036] Conventional binder resins, when used in the composite layer of secondary batteries such as lithium ion batteries, have been designed to have low swelling properties in response to an electrolyte, so that even if the binder resin swells with the electrolyte, it is possible to obtain adhesion between the composite layer and the current collector and binding between the active materials in the composite layer. It is considered that the composite layer in contact with the electrolyte has a contact area between the binder resin and the active material, and a contact area between the active material and the electrolyte, due to the electrolyte permeating into the composite layer. Conventional binder resins have low swelling with the electrolyte, so that ionic conductivity is difficult to be expressed. Therefore, in the contact area between the binder resin and the active material, the ionic conductivity of lithium ions and the like contained in the electrolyte is low. On the other hand, in the contact area between the active material and the electrolyte, the ionic conductivity of lithium ions and the like contained in the electrolyte is improved. In addition, since conventional binder resins have low swelling with the electrolyte, the area of the contact area between the binder resin and the active material does not expand much, and the area of the contact area is small. On the other hand, the area of the contact area between the active material and the electrolyte is large. It is believed that the electrolyte is less likely to decompose in the contact area between the binder resin and the active material, and therefore a decomposition layer of the electrolyte, called a solid electrolyte interphase (SEI) layer, is likely to form in the contact area between the active material and the electrolyte. When a conventional binder resin is used in the composite layer, as described above, the area of contact between the active material and the electrolyte is large, and therefore the area on which the SEI layer is formed is also large, which tends to shorten the life of the electrolyte.
[0037] In contrast, when the binder resin according to the present embodiment is used in a composite layer of a secondary battery such as a lithium ion battery, the binder resin according to the present embodiment has high swelling property with respect to the electrolyte solution because it contains a copolymer having a carbonate skeleton as the main polymer skeleton, and thus has improved compatibility with the electrolyte solution. The binder resin according to the present embodiment swells greatly upon contact with the electrolyte solution, thereby exhibiting ion conductivity. In addition, since the binder resin according to the present embodiment has high swelling property with respect to the electrolyte solution, the area of the contact region between the binder resin and the active material is increased, while the area of the contact region between the active material and the electrolyte solution is reduced. For this reason, when the binder resin according to the present embodiment is used, it is considered that the contact region between the binder resin and the active material exhibits ion conductivity and the electrolyte solution is difficult to decompose, and the area in which the SEI layer is formed is suppressed in the contact region between the active material and the electrolyte solution. As a result, when the binder resin according to this embodiment is used in a composite layer of a lithium ion secondary battery, the binder resin according to this embodiment is considered to contribute to improving the life of the electrolyte, and as a result, it is considered to lead to an improvement in the battery performance in the secondary battery using the binder resin according to this embodiment. However, if the swelling property with respect to the electrolyte is too high, the adhesion with the metal foil and the binding property of the inorganic material are likely to decrease. For this reason, the binder resin according to this embodiment does not swell too much with the electrolyte by suppressing the swelling degree with respect to a mixed solvent of ethylene carbonate and dimethyl carbonate at a volume ratio of 1:1 to 1000% or less, and therefore excellent adhesion with the metal foil is obtained, and excellent binding property between inorganic materials is obtained. As a result, when the binder resin according to this embodiment is used in a composite layer of a lithium ion secondary battery, it exhibits excellent swelling property with respect to the electrolyte, while also exhibiting excellent adhesion with the current collector and excellent binding property between active materials in the composite layer.
[0038] The binder resin according to the present embodiment is not particularly limited as long as it satisfies that the swelling degree in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 is 200% or more and less than 1000%, and the resin contained in the binder resin may be a homopolymer or a copolymer. Examples of the binder resin according to the present embodiment include acrylic resin, polyamide resin, polyamideimide resin, polyurethane resin, polyester resin, polyolefin resin, polycarbonate resin, polyvinyl alcohol resin, polyvinyl acetal resin, fluororesin, polyvinyl chloride resin, styrene-based thermoplastic elastomer, acrylic rubber, fluororubber, and polysaccharide polymer, and one or more of these are used. Among these, from the viewpoint of obtaining excellent adhesion to the metal foil and easily obtaining excellent binding properties between inorganic materials, the binder resin according to the present embodiment preferably contains a polycarbonate resin, more preferably contains a copolymer having a carbonate skeleton, and further preferably contains a copolymer having a carbonate skeleton including a structural unit represented by general formula (1) and a structural unit represented by general formula (2) described later.
[0039] (copolymer) Hereinafter, an example of a copolymer having a carbonate skeleton, which is a resin preferably used as the binder resin according to the present embodiment, will be described. As one aspect, the binder resin according to the present embodiment includes a copolymer containing a structural unit represented by the following general formula (1) and a structural unit represented by the following general formula (2) in an amount of more than 1.0 mol % and not more than 20.0 mol %. The copolymer preferably contains the structural unit represented by the following general formula (1) and the structural unit represented by the following general formula (2) in a total amount of 50.0 mol % or more based on the total amount of the structural units constituting the copolymer. In this specification, the structural unit represented by the following general formula (1) and the structural unit represented by the following general formula (2) may be referred to as a carbonate structural unit.
[0040] [ka]
[0041] In the general formula (1) and the general formula (2), R 1 is a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or an alkoxyalkyl group having 1 to 8 carbon atoms; L 1 and L 2 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms; L 3 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms; X 1 is any reactive group among the groups represented by the following structural formula (2-1), the following structural formula (2-2), and the following structural formula (2-3). In the following structural formula (2-1), the following structural formula (2-2), and the following structural formula (2-3), the wavy line represents L 3 represents the bonding position with
[0042] [ka]
[0043] In the general formula (1), R 1 is preferably a hydrogen atom, an alkyl group having 1 to 7 carbon atoms, or an alkoxyalkyl group having 1 to 7 carbon atoms, more preferably a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxyalkyl group having 1 to 6 carbon atoms, even more preferably an alkyl group having 1 to 6 carbon atoms or an alkoxyalkyl group having 1 to 6 carbon atoms, and particularly preferably an alkyl group having 1 to 5 carbon atoms or an alkoxyalkyl group having 1 to 5 carbon atoms.
[0044] In the general formula (1), R 1 When is an alkyl group having 1 to 8 carbon atoms, the alkyl group may be linear, branched, or alicyclic.
[0045] In the general formula (1), R 1 is an alkoxyalkyl group having from 1 to 8 carbon atoms, the alkoxyalkyl group is11 -OR 11 -L is a group represented by the formula: 11 -OR 11 In the group represented by the formula 11 is a single bond or an alkylene group having 1 to 7 carbon atoms; R 11 is an alkyl group having 1 to 8 carbon atoms. 11 And, R 11 The total number of carbon atoms is 1 to 8. -L 11 -OR 11 In the group represented by 11 -L is preferably a single bond or an alkylene group having 1 to 6 carbon atoms, more preferably a single bond or an alkylene group having 1 to 5 carbon atoms, and even more preferably a single bond or a methylene group. 11 -OR 11 In the group represented by 11 may be linear, branched, or alicyclic. -L 11 -OR 11 R in the group represented by 11 -L is preferably an alkyl group having 1 to 7 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and even more preferably an alkyl group having 1 to 5 carbon atoms. 11 -OR 11 R in the group represented by 11 may be linear, branched, or alicyclic.
[0046] In the general formula (1) and the general formula (2), L 1 and L 2 are each independently preferably a methylene group or an ethylene group, and more preferably a methylene group.
[0047] In the general formula (2), L 3is preferably a single bond, an alkylene group having 1 to 4 carbon atoms, or an oxyalkylene group having 1 to 4 carbon atoms, also preferably a single bond, an alkylene group having 2 to 4 carbon atoms, or an oxyalkylene group having 2 to 4 carbon atoms, and also preferably a single bond, an alkylene group having 1 to 3 carbon atoms, or an oxyalkylene group having 1 to 3 carbon atoms.
[0048] From the viewpoint of ease of synthesis, -L in the general formula (2) 3 -X 1 is preferably any one of the reactive groups represented by the following structural formula (2-4), (2-5), and (2-6): In the following structural formula (2-4), (2-5), and (2-6), the wavy line represents the bonding position with the methylene group to which any one of the following structural formula (2-4), (2-5), and (2-6) is bonded.
[0049] [ka]
[0050] The copolymer may be a random copolymer or a block copolymer. From the viewpoint of ease of synthesis, the copolymer is preferably a random copolymer.
[0051] For example, when the copolymer is a copolymer consisting of a constitutional unit represented by the general formula (1) and a constitutional unit represented by the general formula (2), the sum of the constitutional unit represented by the general formula (1) and the constitutional unit represented by the general formula (2) is 100 mol %. In this case, the ratio of the constitutional unit represented by the general formula (1) to the constitutional unit represented by the general formula (2) in the copolymer is as follows.
[0052] The ratio of the structural unit represented by the general formula (2) is more than 1.0 mol% and not more than 20.0 mol% relative to all structural units. When the content ratio of the structural unit represented by the general formula (2) exceeds 1.0 mol%, the ratio of the structural unit represented by the general formula (1) in the copolymer is not too high, so that the copolymer does not swell too much in the electrolyte, resulting in excellent adhesion to the metal foil and excellent binding properties to inorganic materials. When the content ratio of the structural unit represented by the general formula (2) is 20.0 mol% or less, the crosslink density of the copolymer is not too high, so that the copolymer improves its swelling property in the electrolyte. From the same viewpoint, the ratio of the structural unit represented by the general formula (2) is preferably 1.1 mol% or more, more preferably 1.5 mol% or more, even more preferably 1.8 mol% or more, and even more preferably 2.0 mol% or more. The ratio of the structural unit represented by the general formula (2) is preferably 19.0 mol% or less, more preferably 18.0 mol% or less, even more preferably 15.0 mol% or less, even more preferably 12.0 mol% or less, even more preferably 10.0 mol% or less, even more preferably 6.0 mol% or less, and even more preferably 5.0 mol% or less.
[0053] The ratio of the structural unit represented by the general formula (1) is 80.0 mol% or more and less than 99.0 mol% with respect to all structural units. The ratio of the structural unit represented by the general formula (1) is preferably 81.0 mol% or more, more preferably 82.0 mol% or more, even more preferably 85.0 mol% or more, even more preferably 88.0 mol% or more, even more preferably 90.0 mol% or more, even more preferably 94.0 mol% or more, and even more preferably 95.0 mol% or more. The ratio of the structural unit represented by the general formula (1) is preferably 98.9 mol% or less, more preferably 98.5 mol% or less, even more preferably 98.2 mol% or less, and even more preferably 98.0 mol% or less.
[0054] It is also preferable that the copolymer further contains at least one structural unit selected from the group consisting of structural units represented by the following general formula (3) and structural units represented by the following general formula (4) in an amount of 0.1 mol % or more and 30.0 mol % or less. That is, it is also preferable that at least one structural unit selected from the group consisting of structural units represented by the following general formula (3) and structural units represented by the following general formula (4) is 0.1 mol % or more and 30.0 mol % or less. That is, it is also preferable that the total of the structural units represented by the following general formula (3) and the structural units represented by the following general formula (4) is 0.1 mol % or more and 30.0 mol % or less with respect to the total structural units constituting the copolymer. In this specification, the structural units represented by the following general formula (3) and the structural units represented by the following general formula (4) may be referred to as ether structural units.
[0055] For example, when the copolymer is a copolymer composed of a constitutional unit represented by the general formula (1), a constitutional unit represented by the general formula (2), and at least one constitutional unit selected from the group consisting of a constitutional unit represented by the following general formula (3) and a constitutional unit represented by the following general formula (4), the copolymer has a total of 100 mol % of the constitutional unit represented by the general formula (1), the constitutional unit represented by the general formula (2), and at least one constitutional unit selected from the group consisting of a constitutional unit represented by the following general formula (3) and a constitutional unit represented by the following general formula (4).
[0056] [ka]
[0057] In the general formula (3) and the general formula (4), R 2 is a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or an alkoxyalkyl group having 1 to 8 carbon atoms; L 4 and L 5 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms; L 6 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms; X 2is any reactive group among the groups represented by the following structural formula (4-1), the following structural formula (4-2), and the following structural formula (4-3). In the groups represented by the following structural formula (4-1), the following structural formula (4-2), and the following structural formula (4-3), the wavy line represents L 6 represents the bonding position with
[0058] [ka]
[0059] In the general formula (3), R 2 is preferably a hydrogen atom, an alkyl group having 1 to 7 carbon atoms, or an alkoxyalkyl group having 1 to 7 carbon atoms, more preferably a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxyalkyl group having 1 to 6 carbon atoms, and even more preferably an alkyl group having 1 to 6 carbon atoms, or an alkoxyalkyl group having 1 to 6 carbon atoms.
[0060] In the general formula (3), R 2 When is an alkyl group having 1 to 8 carbon atoms, the alkyl group may be linear, branched, or alicyclic.
[0061] In the general formula (3), R 2 is an alkoxyalkyl group having from 1 to 8 carbon atoms, the alkoxyalkyl group is 21 -OR 21 -L is a group represented by the formula: 21 -OR 21 In the group represented by the formula 21 is a single bond or an alkylene group having 1 to 7 carbon atoms; R 21 is an alkyl group having 1 to 8 carbon atoms. 21 And, R 21 The total number of carbon atoms is 1 to 8. -L 21 -OR 21 In the group represented by 21-L is preferably a single bond or an alkylene group having 1 to 6 carbon atoms, more preferably a single bond or an alkylene group having 1 to 5 carbon atoms, and even more preferably a single bond or a methylene group. 21 -OR 21 In the group represented by 21 may be linear, branched, or alicyclic. -L 21 -OR 21 R in the group represented by 21 -L is preferably an alkyl group having 1 to 7 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and even more preferably an alkyl group having 1 to 5 carbon atoms. 21 -OR 21 R in the group represented by 21 may be linear, branched, or alicyclic.
[0062] In the general formula (3) and the general formula (4), L 4 and L 5 Each of and independently is preferably a methylene group or an ethylene group, and more preferably a methylene group.
[0063] In the general formula (4), L 6 is preferably a single bond, an alkylene group having 1 to 4 carbon atoms, or an oxyalkylene group having 1 to 4 carbon atoms, is preferably a single bond, an alkylene group having 2 to 4 carbon atoms, or an oxyalkylene group having 2 to 4 carbon atoms, and is also preferably a single bond, an alkylene group having 1 to 3 carbon atoms, or an oxyalkylene group having 1 to 3 carbon atoms.
[0064] From the viewpoint of ease of synthesis, -L in the general formula (4) 6 -X 2is preferably any one of reactive groups represented by the following structural formula (4-4), (4-5), and (4-6): In the following structural formula (4-4), (4-5), and (4-6), the wavy line represents the bonding position with the methylene group to which any one of the following structural formula (4-4), (4-5), and (4-6) is bonded.
[0065] [ka]
[0066] When the copolymer in the binder resin according to the present embodiment further contains an ether skeleton such as a structural unit represented by general formula (3) or the following general formula (4) in addition to the structural unit represented by general formula (1) and the structural unit represented by general formula (2), the glass transition temperature of the copolymer is lowered and the copolymer is made flexible, so that high ionic conductivity can be expected.
[0067] For example, in the case of a copolymer consisting of a constitutional unit represented by the general formula (1), a constitutional unit represented by the general formula (2), a constitutional unit represented by the general formula (3), and a constitutional unit represented by the general formula (4), the constitutional ratio is as follows.
[0068] The total ratio of the structural unit represented by the general formula (3) and the structural unit represented by the general formula (4) is preferably 0.1 mol% or more and 30.0 mol% or less with respect to all structural units constituting the copolymer, from the viewpoint of easily exerting the action and effect of the ether skeleton. If the total of the structural unit represented by the general formula (3) and the structural unit represented by the general formula (4) is 30.0 mol% or less with respect to all structural units constituting the copolymer, the ether skeleton tends to be less compatible with the electrolyte than the carbonate skeleton, so that the decrease in the swelling degree of the copolymer is suppressed and the decrease in ion conductivity is easily suppressed. From the same viewpoint, the total ratio of the constitutional units represented by the general formula (3) and the constitutional units represented by the general formula (4) is preferably 1.0 mol% or more, more preferably 2.0 mol% or more, and preferably 3.0 mol% or more, based on all constitutional units constituting the copolymer. The total ratio of the constitutional units represented by the general formula (3) and the constitutional units represented by the general formula (4) is more preferably 29.0 mol% or less, even more preferably 25.0 mol% or less, and particularly preferably 15.0 mol% or less, based on all constitutional units constituting the copolymer.
[0069] The ratio of the constitutional units represented by the general formula (2) is as described above. The ratio of the structural unit represented by general formula (1) is preferably 50.0 mol% or more, more preferably 55.0 mol% or more, even more preferably 60.0 mol% or more, and even more preferably 65.0 mol% or more, based on all structural units. The ratio of the structural unit represented by general formula (1) is preferably less than 98.9 mol%, more preferably 98.9 mol% or less, even more preferably 98.5 mol% or less, even more preferably 98.0 mol% or less, even more preferably 97.5 mol% or less, even more preferably 97.0 mol% or less, even more preferably 96.0 mol% or less, even more preferably 95.0 mol% or less, even more preferably 94.0 mol% or less, and even more preferably 92.0 mol% or less.
[0070] The molecular weight of the copolymer according to this embodiment, measured by the method shown in the measurement example, is preferably 5,000 or more and 5,000,000 or less, and more preferably 10,000 or more and 1,000,000 or less, when expressed as a weight average molecular weight (Mw). Furthermore, the molecular weight of the copolymer according to this embodiment, measured by the method shown in the measurement example, is preferably 3,000 or more and 3,000,000 or less, and more preferably 5,000 or more and 500,000 or less, when expressed as a number average molecular weight (Mn). Furthermore, the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is preferably from 1 to 10, and more preferably from 1.1 to 5. When the copolymer is used as a binder, the molecular weight and molecular weight distribution of the copolymer within the above ranges can provide an appropriate viscosity for the slurry during preparation of an electrode slurry, suppressing settling of the active material and conductive assistant, and providing sufficient dispersibility of the active material and conductive assistant.
[0071] The copolymer is preferably further copolymerized with a phosphoric acid group-containing (meth)acrylate compound such as 2-hydroxyalkyl(meth)acrylate acid phosphate and bis(2-methacryloyloxyalkyl) acid phosphate, since this makes it easier to obtain a binder resin with excellent adhesion to the metal foil and binding properties to inorganic materials. Specifically, the copolymer is preferably further copolymerized with at least one phosphoric acid group-containing (meth)acrylate compound selected from the group consisting of the following general formula (5-1) and the following general formula (5-2). When the phosphoric acid group-containing (meth)acrylate compound is copolymerized with the copolymer, a structure derived from the phosphoric acid group-containing (meth)acrylate compound is introduced into the side chain of the copolymer.
[0072] [ka]
[0073] [ka]
[0074] In the general formula (5-1), R 3 and R 4 are each independently a hydrogen atom or a methyl group; L 7 and L 8 are each independently an alkylene group having 2 to 4 carbon atoms. 5 is a hydrogen atom or a methyl group, and L 9is an alkylene group having 2 to 4 carbon atoms.
[0075] In the general formula (5-1), R 3 and R 4 is preferably a methyl group. 7 and L 8 are each independently preferably an ethylene group or a propylene group, and more preferably an ethylene group. In the general formula (5-2), R 5 is preferably a methyl group. 9 is preferably an ethylene group or a propylene group, and more preferably an ethylene group.
[0076] The phosphate group-containing (meth)acrylate compounds represented by the general formula (5-1) and the general formula (5-2) may be synthesized, or a commercially available product may be used.
[0077] In this specification, "(meth)acrylic" is a notation used to represent both "acrylic" and "methacrylic", "(meth)acryloyl" is a notation used to represent both "acryloyl" and "methacryloyl", and the same applies to other similar terms.
[0078] The binder resin according to the present embodiment is preferably a copolymer obtained by copolymerizing 0.2 to 15.0 mol parts of the phosphate group-containing (meth)acrylate compound with respect to 100 mol parts of the copolymer, from the viewpoint of easily obtaining a binder resin having a high degree of swelling and excellent adhesion to metal foil and binding ability to inorganic materials. The binder resin according to the present embodiment is preferably copolymerized with 0.3 mol parts or more of the phosphate group-containing (meth)acrylate compound with respect to 100 mol parts of the copolymer, and more preferably copolymerized with 0.5 mol parts or more. The binder resin according to the present embodiment is preferably copolymerized with 10.0 mol parts or less of the phosphate group-containing (meth)acrylate compound with respect to 100 mol parts of the copolymer, more preferably copolymerized with 8.0 mol parts or less, even more preferably copolymerized with 5.0 mol parts or less, and particularly preferably copolymerized with 3.0 mol parts or less.
[0079] The binder resin according to the present embodiment may contain other polymers in addition to the copolymer containing the constitutional unit represented by the general formula (1) and the constitutional unit represented by the general formula (2) in an amount of more than 1.0 mol% and not more than 20.0 mol%, or the copolymer obtained by further copolymerizing the copolymer with at least one phosphoric acid group-containing (meth)acrylate compound selected from the group consisting of the general formula (5-1) and the general formula (5-2), as long as the adhesion to the metal foil and the binding of the inorganic material are not hindered. From the viewpoint of obtaining a binder resin having excellent adhesion to the metal foil and binding of the inorganic material, the binder resin according to the present embodiment is preferably a copolymer containing the constitutional unit represented by the general formula (1) and the constitutional unit represented by the general formula (2) in an amount of more than 1.0 mol% and not more than 20.0 mol%, or the copolymer obtained by further copolymerizing the copolymer with at least one phosphoric acid group-containing (meth)acrylate compound selected from the group consisting of the general formula (5-1) and the general formula (5-2).
[0080] (Method of Producing Copolymer) The method for producing the copolymer is not particularly limited, and the copolymer can be obtained by a known method. Preferred methods for producing the copolymer include, for example, the following methods.
[0081] The copolymer can be produced by copolymerizing an epoxide monomer and carbon dioxide in the presence of a polymerization catalyst, as described in the Examples below. Specifically, the epoxide monomer undergoes ring-opening to become a structural unit represented by general formula (3) and a structural unit represented by general formula (4), while a portion of propylene oxide undergoes ring-opening and polymerization with carbon dioxide to become a structural unit represented by general formula (1) and a structural unit represented by general formula (2).
[0082] The polymerization catalyst used in producing the copolymer is not particularly limited, and examples thereof include metal salen complex catalysts such as cobalt salen complex catalysts, and composite metal cyanide complex catalysts such as organozinc catalysts.
[0083] The amount of the polymerization catalyst used in the copolymerization reaction of the epoxide monomer with carbon dioxide, for example, when a metal-salen complex catalyst is used, is preferably 0.05 mol or less, more preferably 0.01 mol or less, and particularly preferably 0.001 mol or less, per 1 mol of the epoxide monomer. Furthermore, when using a metal salen complex catalyst, a co-catalyst can be used. As the co-catalyst, for example, an onium salt compound is preferable. Specific examples of the onium salt compound are not particularly limited, but from the viewpoint of having high reaction activity, bis(triphenylphosphoranylidene)ammonium chloride, piperidine, bis(triphenylphosphoranylidene)ammonium fluoride, ammonium pentafluorobenzoate, and tetra-n-butylammonium chloride are preferable.
[0084] The amount of the polymerization catalyst used in the copolymerization reaction of an epoxide monomer with carbon dioxide is, for example, when a double metal cyanide complex catalyst (hereinafter referred to as a DMC catalyst (DMC catalyst)) is used, preferably 0.01 part by mass or less, more preferably 0.005 mol or less, and particularly preferably 0.003 part by mass or less, per part by mass of the epoxide monomer.
[0085] The optimum polymerization conditions vary depending on the type of catalyst. For example, the pressure of carbon dioxide in the reaction vessel is 0.1 MPa or more and 10 MPa or less, preferably 0.5 MPa or more and 5 MPa or less. In addition, for example, in the case of a cobalt salen complex catalyst, the polymerization temperature is preferably about room temperature (e.g., 25° C. or higher and 35° C. or lower) from the viewpoint of good catalytic action and accelerated reaction rate. In the case of a DMC catalyst, for example, the polymerization temperature is preferably about 40° C. or higher and 100° C. or lower, and more preferably about 50° C. or higher and 80° C. or lower.
[0086] In the method of copolymerizing an epoxide monomer with carbon dioxide, examples of the epoxide monomer used as a starting material include ethylene oxide, propylene oxide, 1,2-butylene oxide, 1,2-pentylene oxide, 1,2-hexylene oxide, 1,2-heptylene oxide, 1,2-octylene oxide, 1,2-decylene oxide, methyl glycidyl ether, ethyl glycidyl ether, butyl glycidyl ether, cyclopentene oxide, cyclohexene oxide, allyl glycidyl ether, glycidyl acrylate, glycidyl methacrylate, and 4-hydroxybutyl acrylate glycidyl ether. Note that, due to differences in reactivity, the molar ratio of the structural unit represented by general formula (1) and the structural unit represented by general formula (2) in the copolymer may not match the molar mixing ratio of the epoxide monomer serving as the starting material for the structural unit represented by general formula (1) and the epoxide monomer serving as the starting material for the structural unit represented by general formula (2).
[0087] When the copolymer used in the binder resin according to the present embodiment is a copolymer obtained by further copolymerizing at least one phosphoric acid group-containing (meth)acrylate compound selected from the group consisting of the general formula (5-1) and the general formula (5-2), the phosphoric acid group-containing (meth)acrylate compound is copolymerized with the copolymer obtained by copolymerizing an epoxide monomer and carbon dioxide. Specifically, for example, the phosphoric acid group-containing (meth)acrylate compound is copolymerized at a ratio of 0.2 to 15.0 mol parts per 100 mol parts of the copolymer obtained by copolymerizing an epoxide monomer and carbon dioxide. The polymerization method of the copolymer and the phosphoric acid group-containing (meth)acrylate compound may be a known polymerization method such as radical polymerization, anionic polymerization, or cationic polymerization, and radical polymerization is preferred from the viewpoint of polymerization suitability.
[0088] For radical polymerization, it is preferable to add a thermal radical initiator. Examples of the thermal radical initiator include azo compounds such as azobisisobutyronitrile, and organic peroxides such as benzoyl peroxide.
[0089] (Characteristics of binder resin) As described above, the swelling degree of the copolymer in the binder resin according to the present embodiment in a mixed solvent having a volume ratio of ethylene carbonate and dimethyl carbonate of 1:1 is 200 or more and less than 1000%. The swelling degree of the copolymer in the mixed solvent is preferably 240% or more, more preferably 280% or more, and even more preferably 300% or more. The swelling degree of the copolymer in the mixed solvent is preferably 999% or less, more preferably 990% or less, even more preferably 900% or less, even more preferably 700% or less, and even more preferably 500% or less. The swelling degree of the copolymer in the mixed solvent is the swelling degree after immersion in an electrolyte adjusted to 23°C at 23°C for 24 hours. The swelling degree of the copolymer in the mixed solvent is the swelling degree of the crosslinked product of the copolymer.
[0090] When the binder resin according to the present embodiment is used as an electrode material for a battery, when an electrolyte solution containing the above-mentioned mixed solvent and lithium ions or the like is applied to the binder resin according to the present embodiment, the thin film containing the copolymer swells. The binder resin according to the present embodiment exhibits ion conductivity by swelling with the electrolyte. In order to improve the performance of a battery using the binder resin according to the present embodiment, it is preferable that the ion conductivity of the binder resin is high, so that the swelling degree of the copolymer with respect to the mixed solvent is high. On the other hand, if the swelling degree of the copolymer with respect to the mixed solvent is too high, the adhesion to the metal foil and the binding of the inorganic material are reduced. Therefore, if the swelling degree of the copolymer with respect to the mixed solvent is less than 1000%, the adhesion to the metal foil and the binding of the inorganic material are excellent.
[0091] The binder resin according to the present embodiment is more excellent in adhesion to metal foil and binding of inorganic materials. After preparing a binder resin-containing composition containing the binder resin, and preparing a laminate in which a coating layer made of the binder resin-containing composition is provided on a metal foil, the laminate is immersed in the mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 at a temperature of 23°C for 24 hours without stirring. When the binder resin according to the present embodiment has such characteristics, the coating layer containing the binder resin according to the present embodiment does not break or peel from the metal foil, even though the binder resin according to the present embodiment has high swelling property with respect to the electrolyte. Therefore, when the binder resin according to the present embodiment is applied to an electrode material of a battery, the performance of the battery is improved.
[0092] In addition, in the laminate prepared above in which a coating layer made of the binder resin-containing composition is provided on a metal foil, the metal foil is preferably a copper foil or an aluminum foil. After preparing a laminate in which a coating layer made of the binder resin-containing composition is provided on a copper foil or an aluminum foil, the laminate is immersed in the mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 at a temperature of 23° C. for 24 hours without stirring, and it is preferable that the coating layer does not peel off from the metal foil. When the binder resin according to this embodiment has such characteristics, the binder resin according to this embodiment has high swelling property with respect to the electrolyte, but the coating layer containing the binder resin according to this embodiment does not peel off from the positive electrode current collector or the negative electrode current collector. Therefore, when the binder resin according to this embodiment is applied to the electrode material of a battery, the performance of the battery is improved.
[0093] [How to use binder resin] The binder resin according to the present embodiment has excellent adhesion to metal foil and binding ability to inorganic materials, and can be applied to applications requiring such properties. The binder resin according to the present embodiment is preferably applied to battery applications, for example. In this case, the binder resin according to the present embodiment is preferably a binder resin for battery electrodes, and is also preferably a binder resin for electrodes of secondary batteries such as lithium ion batteries. The binder resin according to the present embodiment may be applied as a binder resin used in a composite layer in a positive electrode, or may be applied as a binder resin used in a composite layer in a negative electrode.
[0094] [battery] Next, a preferred example of the battery according to this embodiment will be described.
[0095] The battery according to the present embodiment is a battery to which the binder resin according to the present embodiment is applied. The battery according to the present embodiment contains the binder resin according to the present embodiment as a material constituting the electrodes of the battery. The battery is composed of a positive electrode, a negative electrode, and an electrolyte layer disposed between the positive electrode and the negative electrode. By adopting such a configuration, a battery excellent in each characteristic can be obtained. In addition, the battery is preferably a secondary battery, and more preferably a secondary battery such as a lithium ion battery. The structure of the battery according to the present embodiment is not particularly limited, and may be a stacked structure or a wound structure.
[0096] Here, an example of a battery using the binder resin according to the present embodiment will be described with reference to the drawings. In the drawings, some parts are illustrated enlarged or reduced in size for ease of explanation.
[0097] FIG. 1 shows an example of a battery using the binder resin according to the present embodiment. The battery 100 shown in FIG. 1 is a lithium ion secondary battery. As shown in FIG. 1, the battery 100 includes a positive electrode 10, a negative electrode 20, and an electrolyte layer 30 between the positive electrode 10 and the negative electrode 20. The positive electrode 10 is composed of a positive electrode current collector 13 and a positive electrode mixture layer 11 laminated on the positive electrode current collector 13, and the negative electrode 20 is composed of a negative electrode current collector 23 and a negative electrode mixture layer 21 laminated on the negative electrode current collector 23. The electrolyte layer 30 is composed of an electrolyte 33 and a separator 31 impregnated with the electrolyte 33, and the separator 31 separates the positive electrode 10 side from the negative electrode 20 side. The battery 100 has a laminated structure in which a positive electrode current collector 13, a positive electrode mixture layer 11, an electrolyte layer 30, a negative electrode mixture layer 21, and a negative electrode current collector 23 are laminated in this order from the positive electrode current collector 13 toward the negative electrode current collector 23, and the laminated structure is housed inside a container (not shown). In the battery 100, the positive electrode mixture layer 11 and the negative electrode mixture layer 21 contain a binder resin (not shown) according to this embodiment. The positive electrode mixture layer 11 and the negative electrode mixture layer 21 contain the electrolyte solution 33 by being permeated with the electrolyte solution 33 of the electrolyte layer 30, and the binder resin according to this embodiment (not shown) is swelled by the electrolyte solution 33.
[0098] Although an example of the battery according to the present embodiment has been described above with reference to Fig. 1, the example of the battery according to the present embodiment is not limited thereto. The battery according to the present embodiment may adopt various forms as long as the binder resin according to the present embodiment is used.
[0099] When the battery according to this embodiment is a lithium ion secondary battery, as long as a binder resin is used in the composite layer of the electrode in the battery according to this embodiment, the various components of the lithium ion secondary battery are not particularly limited, and for example, materials that are generally used in lithium ion secondary batteries can be used.
[0100] Examples of materials used for the positive electrode current collector and the negative electrode current collector include metal foils or metal plates such as copper, aluminum, nickel, titanium, and stainless steel, as well as carbon sheets and carbon nanotube sheets. Among these, the materials used for the positive electrode current collector and the negative electrode current collector are preferably, for example, copper and aluminum. Copper and aluminum are more preferably copper foil and aluminum foil.
[0101] The positive electrode mixture layer is preferably composed of, for example, a positive electrode active material such as a lithium-containing composite oxide, a conductive assistant such as a carbon-based material, and the binder resin according to the present embodiment.
[0102] The negative electrode mixture layer is preferably composed of a negative electrode active material such as acetylene black, carbon nanotubes, carbon nanofibers, and graphene, and the binder resin according to the present embodiment.
[0103] The electrolyte layer is composed of, for example, an electrolytic solution and a separator. When a separator is used, the material of the separator is not particularly limited, and examples thereof include a porous resin sheet containing a resin such as polyolefin, polyester, or polyamide.
[0104] In the battery according to this embodiment, the electrolyte preferably contains a lithium salt and a carbonate-based solvent.
[0105] Specific examples of lithium salts include lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium 2-trifluoromethyl-4,5-dicyanoimidazolate, lithium 4,5-dicyano-1,2,3-triazolate, lithium bis(pentafluoroethylsulfonyl)imide, lithium borofluoride, lithium bis(oxalato)borate, lithium nitrate, lithium chloride, lithium bromide, and lithium fluoride. The lithium salt may be one or more of these exemplified lithium salts.
[0106] Examples of the carbonate-based solvent include dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethylene carbonate, propylene carbonate, and butylene carbonate. The carbonate-based solvent can be one or more of these lithium salts. Here, the carbonate-based solvent in this embodiment refers to a compound having a carbonate skeleton in its molecular structure.
[0107] The present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES
[0108] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these examples in any way.
[0109] Measurements and evaluations in the following Examples and Comparative Examples were carried out by the methods described below.
[0110] [Measurement of weight average molecular weight (Mw) and number average molecular weight (Mn)] Measurements were carried out under the following conditions using a gel permeation chromatograph (manufactured by Tosoh Corporation, product name "HLC-8320GPC"), and the values measured were converted into standard polystyrene equivalent values. (Measurement conditions) Column: "TSKgel guardcolumn SuperH-H", "TSKgel SuperHM-H", "TSKgel SuperHM-H", and "TSKgel SuperH2000" (all manufactured by Tosoh Corporation) connected in sequence Column temperature: 40℃ Developing solvent: Tetrahydrofuran (copolymer concentration 1% by mass) Standard material: polystyrene ·Injection volume: 20μL ·Flow rate: 0.60mL / min Detector: Differential refractometer
[0111] [Swelling degree measurement] Copolymer X was prepared by copolymerizing 100 mol parts of the copolymer obtained in each of the examples and comparative examples described below with 1 mol part of 2-methacryloyloxyethyl acid phosphate (manufactured by Kyoeisha Chemical Co., Ltd., product name "Light Ester P-2M"). 1-Hydroxycyclohexyl phenyl ketone was added as a photopolymerization initiator to the prepared copolymer X so that the copolymer: initiator = 97: 3 mass %, and the mixture was further diluted with ethyl acetate and stirred to prepare a solution for thin film formation with a solid content concentration of 30 mass %. A first release film (manufactured by Lintec Corporation, product name "SP-PET381031") was prepared, and the prepared solution for thin film formation was applied to the release-treated surface of this release film, and dried at 120 ° C. for 1 minute to form a thin film layer with a thickness of 10 μm. Furthermore, a second release film (manufactured by Lintec Corporation, product name "SP-PET382150") was prepared, and the release-treated surface of this release film was attached to the surface of the thin film layer. Thereafter, the laminate of the thin films sandwiched between the first release film and the second release film was placed on a stainless steel plate and irradiated with ultraviolet light [illuminance: 200 mW / cm ] at a temperature of 50°C. 2 , Accumulated light intensity: 1000mJ / cm 2The measurement was performed using an illuminance light meter manufactured by Eye Graphics Inc. (control unit: EYE UV METER UVPF-A2, light receiving unit: EYE UV METER PD-365A2) to obtain a thin film with a thickness of 10 μm.
[0112] The thin film obtained above was cut into pieces of about 3 cm (vertical) x about 3 cm (horizontal), and the obtained pieces of thin film were weighed to be about 1 g. The mass at this time was defined as W0. The pieces of thin film were wrapped in a polyester mesh (mesh size 200), and the mass of the pieces of thin film wrapped in the polyester mesh was weighed, and the mass of the pieces of thin film was calculated by subtracting the mass of the pieces of thin film. The pieces were immersed in a carbonate-based solvent [composition: mixed solvent of ethylene carbonate / dimethyl carbonate = 1 / 1 (volume ratio)] adjusted to a temperature of 23 ° C. for 24 hours at a temperature of 23 ° C. to swell. Thereafter, the pieces of thin film wrapped in the polyester mesh were pulled out, the solvent on the surface was wiped with a paper wiper, and the mass was measured, and the mass of the pieces of thin film after swelling was calculated by subtracting the mass of the polyester mesh alone. The mass at this time was defined as W1. The swelling degree was calculated using the following formula (F2). Swelling degree (%) = {(W1-W0) / W0} × 100 (F2) In formula (F2), W0 represents the mass of the thin film piece weighed before being wrapped in the polyester mesh, and W1 represents the mass of only the thin film piece after swelling.
[0113] [Metal foil adhesion and binding properties] As samples for evaluating metal foil adhesion and binding property, the following laminate A and laminate B were prepared. The metal foil adhesion and binding property of each of laminate A and laminate B were evaluated.
[0114] (Preparation of Laminate A) The copolymers obtained in each of the examples and comparative examples described below were dissolved in N-methyl-2-pyrrolidone (hereinafter, NMP). Next, acetylene black as a conductive assistant, azobisisobutyronitrile as a thermal radical generator, and 2-methacryloyloxyethyl acid phosphate (manufactured by Kyoeisha Chemical Co., Ltd., product name "Light Ester P-2M", in Table 3, indicated as phosphate group-containing (meth)acrylate compound) were added to the copolymer dissolved in NMP, and the mixture was dispersed for 30 minutes at 2000 rpm using a disperser. Next, lithium iron phosphate (LFP) was added as an active material, and the mixture was dispersed for 10 minutes at 2000 rpm using a rotation-revolution type mixer (manufactured by Thinky Corporation, product name "Awatori Rentaro") to prepare a binder resin-containing composition A, which was used as coating liquid A with a solid content concentration of 50 mass%. This coating solution A was applied to an aluminum foil having a thickness of 20 μm with an applicator and dried at 120° C. for 10 minutes to form a coating layer having a thickness of 120 μm, thereby producing a laminate A having a thickness of 140 μm. When this laminate A is used as an electrode in a secondary battery such as a lithium ion battery, the laminate A becomes a positive electrode, the coating layer is a composite layer, and the aluminum foil is a current collector.
[0115] (Preparation of Laminate B) The copolymers obtained in each of the examples and comparative examples described below were dissolved in NMP. Next, acetylene black as a conductive assistant, azobisisobutyronitrile as a thermal radical generator, and 2-methacryloyloxyethyl acid phosphate (manufactured by Kyoeisha Chemical Co., Ltd., product name "Light Ester P-2M", in Table 3, indicated as phosphate group-containing (meth)acrylate compound) were added to the copolymer dissolved in NMP, and the mixture was dispersed for 30 minutes at 2000 rpm using a disperser. Next, graphene was added as an active material, and the mixture was dispersed for 10 minutes at 2000 rpm using a rotation-revolution type mixer (manufactured by Thinky Corporation, product name "Awatori Rentaro") to prepare a binder resin-containing composition B, which was used as coating liquid B with a solid content concentration of 50 mass%. This coating solution B was applied to a copper foil having a thickness of 10 μm with an applicator and dried at 120° C. for 10 minutes to form a coating layer having a thickness of 150 μm, thereby producing a laminate B having a thickness of 160 μm. When this laminate B is used as an electrode in a secondary battery such as a lithium ion battery, the laminate B becomes a negative electrode, the coating layer is a composite layer, and the copper foil is a current collector.
[0116] (Evaluation of metal foil adhesion and binding (electrolyte immersion)) Each of the laminates A and B was punched out to have a diameter of 10 mm. As the lithium salt, lithium bis(trifluoromethanesulfonyl)imide was prepared, and as the carbonate-based solvent, a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 was prepared. The lithium salt was added to the mixed solvent so that the concentration was 1 mol / L, and the mixture was stirred well to prepare an electrolyte solution at a temperature of 23 ° C. The laminate A or laminate B was put into the prepared electrolyte solution, and immersed at a temperature of 23 ° C. for 24 hours without stirring. After immersion, the laminate A or laminate B was taken out from the electrolyte solution. The laminate A was visually inspected for peeling of the aluminum foil from the coating layer and the collapse of the coating layer, and the laminate B was visually inspected for peeling of the copper foil from the coating layer and the collapse of the coating layer, and evaluated according to the following evaluation criteria.
[0117] (Evaluation Criteria) A: The coating layer does not peel off from the aluminum foil or copper foil, and no collapse of the coating layer occurs. F: The coating layer peels off from the aluminum foil or copper foil, and / or the coating layer collapses.
[0118] [Example 1] (Synthesis of polymerization catalyst: Cobalt salen catalyst) (R,R)-N,N'-bis(3,5-di-tert-butylsalicylidene)-1.2-diaminocyclohexanecobalt(II) and pentafluorobenzoic acid were weighed out to a molar ratio of 1:1.1, placed in a flask, and dehydrated toluene was added. The flask was shielded from light with aluminum foil and reacted at room temperature for 20 hours (the chemical reaction formula is as follows). After the reaction was completed, the solvent was removed under reduced pressure and the mixture was washed several times with an excess amount of hexane. It was then vacuum dried at room temperature to obtain a cobalt salen complex.
[0119] [ka]
[0120] (Preparation of copolymer) As epoxide monomers, propylene oxide (epoxide monomer (1) in Table 1) and glycidyl methacrylate (epoxide monomer (2) in Table 1) were prepared. Propylene oxide and glycidyl methacrylate were mixed to a molar ratio of 97:3. Furthermore, the cobalt salen complex (polymerization catalyst) synthesized above and bis(triphenylphosphoranylidene)ammonium chloride were prepared as a cocatalyst. Next, they were weighed out so that the molar ratio of total epoxide monomer: catalyst: cocatalyst was 2000:1:1, and placed in a pressure vessel. Furthermore, 200 ppm of phenothiazine was added, and then ethyl acetate was added so that the total epoxide monomer: ethyl acetate was 50:50 (mass ratio). All of these operations were performed with the pressure vessel replaced with argon. Next, the pressure vessel was purged with carbon dioxide, and then carbon dioxide was introduced into the pressure vessel by a liquid pump, the pressure in the pressure vessel was set to 2.0 MPa, and the polymerization reaction was performed at 30°C for 18 hours. After the reaction was completed, chloroform was added to the contents of the pressure vessel to prepare a chloroform solution, and 1M hydrochloric acid was added and stirred. Next, the chloroform solution was dropped into stirred methanol to precipitate the product. The product was then vacuum dried at 50°C to obtain a copolymer. The structure of the obtained copolymer was confirmed by nuclear magnetic resonance spectroscopy ( 1When the copolymer was analyzed by H-NMR (Biospin Avance 500, Bruker) using CDCl3 (containing 0.03% by volume of tetramethylsilane) as a solvent, the molar ratio of the structural unit represented by general formula (1) (hereinafter also referred to as structural unit (1)), the structural unit represented by general formula (2) (hereinafter also referred to as structural unit (2)), the structural unit represented by general formula (3) (hereinafter also referred to as structural unit (3)), and the structural unit represented by general formula (4) (hereinafter also referred to as structural unit (4)) in the copolymer was structural unit (1):structural unit (2):structural unit (3):structural unit (4)=95.7:4.2:0.1:0 (see FIG. 2). The weight average molecular weight (Mw), number average molecular weight (Mn), and ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) of the copolymer are shown in Table 2.
[0121] [Example 2] As epoxide monomers, propylene oxide (epoxide monomer (1) in Table 1) and 4-hydroxybutyl acrylate glycidyl ether (epoxide monomer (2) in Table 1) were prepared. A copolymer was obtained in the same manner as in Example 1, except that propylene oxide and 4-hydroxybutyl acrylate glycidyl ether were mixed in a molar ratio of 97:3. The structure of the obtained copolymer was also determined in the same manner as in Example 1. 1 When confirmed by H-NMR, the molar ratio of structural unit (1): structural unit (2): structural unit (3): structural unit (4) in the obtained copolymer was as shown in Table 2 (see FIG. 3). In addition, the weight average molecular weight (Mw), number average molecular weight (Mn), and ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) of the obtained copolymer are shown in Table 2.
[0122] [Example 3] (Synthesis of polymerization catalyst: DMC catalyst) 1.33 g of potassium hexacyanocobaltate(III) (K3[Co(CN)6]; Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 20 mL of deionized water and added dropwise to a vigorously stirred 50°C zinc chloride solution (11.42 g of ZnCl2 dissolved in a mixed solution of 60 mL of deionized water and 30 mL of t-butyl alcohol) over 45 minutes. The mixture was then vigorously stirred for 60 minutes. The resulting white suspension was centrifuged at 5000 rpm to isolate a white solid. The isolated white solid was resuspended in a solution of t-butyl alcohol and deionized water (volume ratio of t-butyl alcohol:deionized water = 5:5) with vigorous stirring for 30 minutes. Then, the isolation and resuspension by centrifugation were repeated several times while gradually increasing the amount of t-butyl alcohol relative to water (volume ratio of t-butyl alcohol:deionized water was changed from 6:4 to 7:3, 8:2, and 9:1). Finally, the white solid was resuspended in t-butyl alcohol and isolated by centrifugation, and then dried under vacuum at 50 °C to a given mass to obtain the DMC catalyst Zn3(Cо[CN]6)2.
[0123] (Synthesis of copolymer) As epoxide monomers, propylene oxide (epoxide monomer (1) in Table 1) and glycidyl methacrylate (epoxide monomer (2) in Table 1) were prepared. Propylene oxide and glycidyl methacrylate were mixed to a molar ratio of 97:3. Furthermore, the DMC catalyst (polymerization catalyst) synthesized above was prepared. Next, the mass ratio of total epoxide monomers:DMC catalyst = 1000:1 was weighed and placed in a pressure-resistant container. Furthermore, 200 ppm of phenothiazine was added, and then ethyl acetate was added so that total epoxide monomers:ethyl acetate = 50:50 (mass ratio). All of these operations were performed with the pressure vessel replaced under an argon atmosphere. Next, the pressure vessel was purged with carbon dioxide, and then carbon dioxide was introduced into the pressure vessel by a liquid pump, the pressure in the pressure vessel was set to 4.0 MPa, and the polymerization reaction was performed at 60 ° C for 18 hours. After the reaction was completed, chloroform was added to the contents of the pressure vessel to prepare a chloroform solution, which was then dropped into stirred methanol to precipitate the product, which was then vacuum dried at 50°C to obtain a copolymer. As in Example 1, the structure of the obtained copolymer was 1 When confirmed by H-NMR, the molar ratio of structural unit (1): structural unit (2): structural unit (3): structural unit (4) in the obtained copolymer was as shown in Table 2 (see FIG. 4). In addition, the weight average molecular weight (Mw), number average molecular weight (Mn), and ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) of the obtained copolymer are shown in Table 2.
[0124] [Examples 4 to 7] A copolymer was obtained in the same manner as in Example 3, except that toluene was used as the polymerization solvent and the type and amount of the epoxide monomer were changed according to Table 1. The structure of the obtained copolymer was also determined in the same manner as in Example 1. 1 When confirmed by 1 H-NMR, the molar ratio of structural unit (1): structural unit (2): structural unit (3): structural unit (4) in the obtained copolymer was as shown in Table 2 (see FIGS. 5 to 8). In addition, the weight average molecular weight (Mw), number average molecular weight (Mn), and ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) of the copolymers obtained in Examples 4 to 7 are shown in Table 2.
[0125] In Table 1, the types of epoxide monomers are explained as follows: PO: Propylene oxide Ehex: 1,2-epoxyhexane Edec: 1,2-epoxydecane BGE: Butyl glycidyl ether Echex: 1,2-Epoxycyclohexane GMA: glycidyl methacrylate 4HBAGE: 4-Hydroxybutyl acrylate glycidyl ether
[0126] [Comparative Example 1] A copolymer was obtained in the same manner as in Example 1, except that the epoxide monomer was changed to a mixture of propylene oxide and glycidyl methacrylate in a molar ratio of 99:1. As in Example 1, the structure of the obtained copolymer was 1 When confirmed by 1 H-NMR, the molar ratio of structural unit (1): structural unit (2): structural unit (3): structural unit (4) in the obtained copolymer was as shown in Table 2. In addition, the weight average molecular weight (Mw), number average molecular weight (Mn), and ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) of the obtained copolymer are shown in Table 2.
[0127] [Table 1]
[0128] [Table 2]
[0129] [Table 3]
[0130] From the above results, it is found that the binder resins obtained in Examples 1 to 7 exhibit a high degree of swelling and are excellent in adhesion to metal foil and binding properties for inorganic materials. From this, it is found that the binder resin according to the present embodiment, when used in a composite layer in an electrode of a secondary battery, exhibits a high degree of swelling, but is also excellent in adhesion to a current collector and binding properties for an active material. [Explanation of symbols]
[0131] Reference Signs List 10: positive electrode, 11: positive electrode composite layer, 13: positive electrode current collector, 20: negative electrode, 21: negative electrode composite layer, 23: negative electrode current collector, 30: electrolyte layer, 31: separator, 33: electrolyte, 100: battery.
Claims
1. A binder resin, The degree of swelling in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 is 200% or more and less than 1000%. Binder resin.
2. The binder resin according to claim 1 , a binder resin-containing composition containing the binder resin is prepared, a laminate is produced in which a coating layer made of the binder resin-containing composition is provided on a metal foil, and then the laminate is immersed in the mixed solvent at a temperature of 23° C. for 24 hours without stirring; and the coating layer does not break or peel off from the metal foil. Binder resin.
3. The binder resin according to claim 2, The metal foil is a copper foil or an aluminum foil, When immersed in the mixed solvent, the coating layer does not peel off from the metal foil. Binder resin.
4. The binder resin according to any one of claims 1 to 3, The copolymer includes a structural unit represented by the following general formula (1) and a structural unit represented by the following general formula (2) in an amount of more than 1.0 mol % and not more than 20.0 mol %: Binder resin. 【Chemistry 1】 (In the general formula (1) and the general formula (2), R 1 is a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or an alkoxyalkyl group having 1 to 8 carbon atoms; L 1 and L 2 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms; L 3 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms; X 1 is any one of the reactive groups represented by the following structural formula (2-1), the following structural formula (2-2), and the following structural formula (2-3). 【Chemistry 2】
5. The binder resin according to claim 4, -L in the general formula (2) 3 -X 1 is any one of reactive groups represented by the following structural formula (2-4), the following structural formula (2-5), and the following structural formula (2-6): Binder resin. 【Chemistry 3】
6. The binder resin according to claim 4, The copolymer further contains at least one structural unit selected from the group consisting of a structural unit represented by the following general formula (3) and a structural unit represented by the following general formula (4), in an amount of 0.1 mol % to 30.0 mol %: Binder resin. 【Chemistry 4】 (In the general formula (3) and the general formula (4), R 2 is a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or an alkoxyalkyl group having 1 to 8 carbon atoms; L 4 and L 5 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms; L 6 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms; X 2 is any one of the reactive groups represented by the following structural formula (4-1), the following structural formula (4-2), and the following structural formula (4-3). 【Chemistry 5】
7. The binder resin according to claim 4, The copolymer is further copolymerized with at least one phosphoric acid group-containing (meth)acrylate compound selected from the group consisting of the following general formula (5-1) and the following general formula (5-2): Binder resin. 【Chemistry 6】 【Chemistry 7】 (In the general formula (5-1), R 3 and R 4 are each independently a hydrogen atom or a methyl group; L 7 and L 8 are each independently an alkylene group having 2 to 4 carbon atoms, and in the general formula (5-2), R 5 is a hydrogen atom or a methyl group, L 9 is an alkylene group having 2 to 4 carbon atoms.
8. The binder resin according to claim 7, The copolymer is obtained by copolymerizing 0.2 to 15.0 parts by mole of the phosphoric acid group-containing (meth)acrylate compound with respect to 100 parts by mole of the copolymer. Binder resin.
9. The binder resin according to any one of claims 1 to 3 is contained. battery.
Citation Information
Patent Citations
Aliphatic polycarbonate
WO2020153329A1
Winding for musical instrument
JP1985023893A
Binder composition for storage device electrode, slurry for storage device electrode, storage device electrode, and storage device
WO2016039067A1