Thermoplastic resin film and production method of the same

A thermoplastic resin film with a sea-island structure and optimized stretching achieves balanced gas barrier, impact resistance, and heat sealability by flattening and dispersing gas-barrier resin layers, addressing the limitations of previous methods.

JP2024146409APending Publication Date: 2024-10-15TOPPAN HOLDINGS INC

Patent Information

Application Number
JP2023059276
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing thermoplastic resin films struggle to achieve a balance between good gas barrier properties, impact resistance, and heat sealability, as methods like lamination and simple kneading often result in poor adhesion, peeling, and compromised performance.

Method used

A thermoplastic resin film with a sea-island structure is developed, where a heat-sealable thermoplastic resin contains a gas-barrier thermoplastic resin, stretched to flatten the latter in the film's plane direction, with at least 0.3 layers per 1 μm thickness, and a 2°C or more higher heat of fusion peak temperature in the 1st Run compared to the 2nd Run, using differential scanning calorimetry.

Benefits of technology

The film achieves improved gas barrier properties and impact resistance while maintaining heat sealability, with optimized stretching and composition enhancing the dispersion and flattening of the gas-barrier resin layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146409000001_ABST
    Figure 2024146409000001_ABST
Patent Text Reader

Abstract

To provide a thermoplastic resin film having preferable gas barrier, impact resistance and heat seal ability, and a production method thereof.SOLUTION: There is provided a thermoplastic resin film which is extended and includes: a heat seal thermoplastic resin; and a gas barrier thermoplastic resin, in the heat seal thermoplastic resin, the gas barrier thermoplastic resin exists as an island, namely a sea-island structure is formed. The gas barrier thermoplastic resin has a shape which expands in a flat-state to a plane direction of the film, and from any point on the surface of the film to a thickness direction of the film, 0.3 layers or more layers are overlapped per 1 μm of a film thickness. In measurement by a differential scanning calorimeter of the film, a fusion heat peak temperature in 1st Run is higher by 2°C or more than a fusion heat peak temperature in 2nd Run.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic resin film having good gas barrier properties, impact resistance and heat sealability, and a method for producing the same. [Background technology]

[0002] In general, plastic films have properties such as being lightweight, being chemically stable, being easy to process, being flexible and strong, and being capable of being mass-produced. For these reasons, plastic films are used in a variety of applications. Applications of plastic films are diverse, including, for example, packaging materials for packaging food and medicines, intravenous drip packs, shopping bags, posters, tapes, optical films for use in liquid crystal televisions, protective films, window films to be attached to windows, vinyl greenhouses, building materials, and the like. For such applications, appropriate plastic materials are selected according to the application.

[0003] For example, plastic films made of polyolefins are widely used as packaging materials because they have moderate flexibility, transparency, and excellent heat sealability. In addition, they have excellent water vapor barrier properties, but on the other hand, they are poor gas barrier films against oxygen gas and the like. Therefore, depending on the application, a barrier film in which a gas barrier layer is provided by deposition or coating on a plastic film made of a resin with excellent gas barrier properties, or a polyester or polyamide, is laminated with a polyolefin film to obtain a packaging material with excellent gas barrier properties. However, laminating multiple plastic films makes the manufacturing process complicated and increases costs. In addition, the adhesion between the films is not necessarily good, and peeling occurs at the film interface, which can result in poor impact resistance, i.e., poor protection performance for the contents.

[0004] Therefore, Patent Documents 1 and 2 propose packaging materials with excellent gas barrier properties, which are made by kneading multiple plastics rather than laminating them. Since ordinary kneading alone would result in multiple plastics becoming finely dispersed, resulting in poor gas barrier properties, they attempt to flatten the gas barrier resin by stretching the film to elongate the dispersed structure. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2003-155419 [Patent Document 2] Patent Publication 2016-150949 Summary of the Invention [Problem to be solved by the invention]

[0006] However, it is difficult to say that the methods of either document achieve all of the gas barrier properties, impact resistance, and heat sealability at the same time. In order to improve the gas barrier properties, it is necessary to sufficiently flatten the gas barrier resin, in order to improve the impact resistance, it is necessary to finely disperse multiple resins, and in order to improve the heat sealability, it is necessary to arrange a heat sealable resin on the surface, but neither Patent Document 1 nor 2 has achieved the improvement of all of these.

[0007] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a thermoplastic resin film having good gas barrier properties, impact resistance and heat sealability, and a method for producing the same. [Means for solving the problem]

[0008] In order to solve the above problems, a representative film of the present invention is a thermoplastic resin film that contains a heat-sealable thermoplastic resin and a gas-barrier thermoplastic resin, and has a sea-island structure in which the gas-barrier thermoplastic resin exists as islands in the heat-sealable thermoplastic resin, and is stretched, the gas-barrier thermoplastic resin has a shape that spreads flat in the plane direction of the film, and overlaps with 0.3 layers per 1 μm of film thickness from any point on the surface of the film toward the thickness direction of the film, and when the film is measured with a differential scanning calorimeter, the peak temperature of the heat of fusion in a first run is 2° C. or more higher than the peak temperature of the heat of fusion in a second run. Effect of the Invention

[0009] According to the present invention, it is possible to provide a thermoplastic resin film having good gas barrier properties, impact resistance and heat sealability, and a method for producing the same. Problems, configurations and effects other than those described above will become apparent from the following description of the embodiments. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of a thermoplastic resin film according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view illustrating a schematic diagram of another example of the thermoplastic resin film of the present embodiment. [Diagram 3] FIG. 2 is a diagram showing the time profile of heating and cooling temperatures in measuring the peak temperature of heat of fusion of the thermoplastic resin film of the present embodiment using a differential scanning calorimeter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In addition, each figure is a schematic diagram, and the size and shape of each part are appropriately exaggerated for ease of understanding. In addition, in order to simplify the explanation, the same reference numerals are used to denote corresponding parts in each figure.

[0012] As shown in FIG. 1, the thermoplastic resin film 1 of the present embodiment contains a heat-sealable thermoplastic resin 2 and a gas-barrier thermoplastic resin 3, and a sea-island structure in which the gas-barrier thermoplastic resin exists as islands in the heat-sealable thermoplastic resin is formed and stretched. The thickness of the thermoplastic resin film 1 after stretching is appropriately selected depending on the application, but for general applications, it is usually preferable to be in the range of 10 μm to 200 μm. The gas-barrier thermoplastic resin 3 is layered at 0.3 layers or more per 1 μm of film thickness from any point on the film surface toward the thickness direction of the film. In other words, when a needle is pierced in a direction intersecting the surface of the thermoplastic resin film, for example, in a film with a thickness of 10 μm, it means that the gas-barrier thermoplastic resin can be pierced through three layers or more no matter where it is pierced. Furthermore, when this thermoplastic resin film 1 is measured by a differential scanning calorimeter (DSC), the peak temperature of the heat of fusion in the 1st run is 2° C. or higher than the peak temperature of the heat of fusion in the 2nd run.

[0013] Here, the heat of fusion peak temperature in the 1st run and the 2nd run is a value measured by a method conforming to JIS K7121 (2012). Specifically, as shown in Figure 3, first, the initial temperature is held at either a temperature 100°C lower than the heat of fusion peak temperature or room temperature, whichever is lower, until the device stabilizes (a), then the sample is heated at a heating rate of 10°C per minute to a temperature that is lower than the thermal degradation temperature and is 30°C higher than the end of the heat of fusion peak (b), and held at this temperature for 10 minutes (c). The apex temperature of the heat of fusion peak obtained from the DSC curve obtained when the heating temperature was in the range of (a) to (b) in Figure 3 (1st run) was determined as the heat of fusion peak temperature in the 1st run. Next, the sample was cooled at a rate of 10°C per minute until it reached the initial temperature (d), and then held at the initial temperature until the device stabilized (e). The sample was then heated at a rate of 10°C per minute to a temperature that was lower than the thermal degradation temperature and 30°C higher than the end of the melting peak (f), and held at this temperature for 10 minutes (g). The apex temperature of the heat of fusion peak obtained from the DSC curve obtained when the heating temperature was in the range of (e) to (f) in Figure 3 (2nd Run) was determined as the heat of fusion peak temperature in the 2nd Run.

[0014] The heat-sealable thermoplastic resin 2 forms the sea of ​​the sea-island structure, which allows the thermoplastic resin film 1 to have heat-sealability. This allows the heat-sealable layer 4 and the thermoplastic resin film 1 to be strongly adhered to each other even when another heat-sealable layer 4 is further laminated on at least one surface of the thermoplastic resin film 1 as shown in FIG. Furthermore, since the gas barrier thermoplastic resin 3 has a shape that spreads flat in the plane direction of the film, the gas barrier property can be improved due to the labyrinth effect.

[0015] Furthermore, the gas barrier thermoplastic resin 3 can be further improved in gas barrier properties and impact resistance by being overlapped at 0.3 layers or more per 1 μm of film thickness from any point on the surface of the film toward the thickness direction of the film. In order to improve the impact resistance of a film having an island-in-sea structure, it is necessary to disperse the impact stress, that is, to make the dispersion structure fine, but in the case of a flattened and spread shape, it is difficult to define "fine". According to the present invention, it has been found that good impact resistance can be obtained by overlapping at 0.3 layers or more of the gas barrier thermoplastic resin 3 per 1 μm of film thickness in the thickness direction of the film. Therefore, for example, in a thickness range suitable for general use, the gas barrier thermoplastic resin is overlapped at 3 layers or more in a film with the thinnest thickness of 10 μm, and at the thickest thickness of 200 μm, and good gas barrier properties and impact resistance can be obtained. The number of overlapping layers of the gas barrier thermoplastic resin 3 is preferably 0.5 or more layers per 1 μm of film thickness, more preferably 0.8 or more layers per 1 μm of film thickness, and even more preferably 1.0 or more layers per 1 μm of film thickness.

[0016] A known method can be used to confirm the number of overlaps of the gas barrier thermoplastic resin 3. For example, after embedding the film in a resin or the like as necessary, a cross section of the film can be cut out using a microtome or the like, and the cross section can be observed and confirmed using an optical microscope, a scanning electron microscope, a transmission electron microscope, or the like. If necessary, the contrast of the image can be improved by dyeing. It can also be confirmed using a scanning probe microscope or a laser Raman microscope. Any other observation method that has sufficient resolution for the dispersion state can be used.

[0017] In order to spread the gas barrier thermoplastic resin 3 flat in the plane direction of the film and to overlap 0.3 layers or more per 1 μm of film thickness, the thermoplastic resin film 1 must be stretched, and when the thermoplastic resin film 1 is measured with a differential scanning calorimeter (DSC), the peak temperature of the heat of fusion in the first run must be 2°C or more higher than the peak temperature of the heat of fusion in the second run.

[0018] That is, when the film is stretched, the gas barrier thermoplastic resin 3 dispersed in the film can be flattened while increasing the number of overlaps. In addition, by optimizing process conditions such as the stretch ratio, stretching temperature, stretching speed, and preheating time, if the peak temperature of heat of fusion in the 1st run is 2°C or higher than the peak temperature of heat of fusion in the 2nd run, the dispersed gas barrier thermoplastic resin 3 will be in a sufficiently flat state. On the other hand, if this temperature difference is less than 2°C, the flattening is insufficient and good gas barrier properties and impact resistance cannot be obtained. This temperature difference is more preferably 3°C or more, and even more preferably 5°C or more.

[0019] Here, the stretching may be, for example, simultaneous biaxial stretching or sequential biaxial stretching, or may be multi-stage stretching in which further stretching is performed after simultaneous or sequential biaxial stretching, or may be uniaxial stretching only in the machine direction (MD) or width direction (TD). In the case of uniaxial stretching, since an unstretched film is likely to stretch in the machine direction, uniaxial stretching in the width direction is preferred in order to more effectively spread the gas barrier thermoplastic resin 3 in a flat shape. For the same reason, the stretching ratio is preferably greater in the width direction than in the machine direction.

[0020] The molten resin may be stretched by a stretching method other than those described above during the period from immediately after discharge from the die until it is cooled and solidified. However, the peak temperature of the heat of fusion in the first run must be at least 2°C higher than the peak temperature of the heat of fusion in the second run, and the stretching method described above is preferable to achieve this.

[0021] Although not particularly specified, it is preferable that the size of the dispersed gas barrier thermoplastic resin 3 is random, and it is also preferable that the overlap in the film thickness direction is random. Regular overlapping may lead to a decrease in gas barrier properties and impact resistance, but by making it difficult to create a state in which the sizes and overlaps are uniform, it is possible to reduce the occurrence of parts that can cause performance degradation. In addition, the aspect ratio, which represents the ratio of the length of the major axis to the length of the minor axis of the flat gas barrier thermoplastic resin 3 in the thickness cross section of the film, is preferably large. For example, when the total area of ​​the gas barrier thermoplastic resin 3 in the thickness cross section of the film is taken as 100%, it is preferable that 50% or more of the area has an aspect ratio of 10 or more, and it is even more preferable that 50% or more of the area has an aspect ratio of 15 or more.

[0022] It is preferable to select the difference between the peak temperatures of the heat of fusion of the heat-sealable thermoplastic resin 2 and the gas-barrier thermoplastic resin 3 so that the absolute value is 0°C or more and 10°C or less.

[0023] The heat of fusion peak temperature here refers to the heat of fusion peak temperature in the second run measured by a differential scanning calorimeter according to the method described above.

[0024] When the absolute value of the difference between the heat of fusion peak temperatures is 0° C. or more and 10° C. or less, the gas-barrier thermoplastic resin 3 can be more easily flattened when stretched. The absolute value of this difference between the heat of fusion peak temperatures is more preferably 0° C. or more and 8° C. or less, and even more preferably 0° C. or more and 5° C. or less.

[0025] The heat-sealable thermoplastic resin 2 is not particularly limited, but may be a single or multiple selected from low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) obtained by copolymerizing α-olefin and ethylene, polypropylene including homopolymer, random copolymer, block copolymer, etc., cycloolefin polymer, cycloolefin copolymer obtained by copolymerizing cycloolefin and olefin, ethylene-vinyl acetate copolymer obtained by copolymerizing the above-mentioned olefin and vinyl acetate, and ethylene-methyl acrylate copolymer (EMA), ethylene-ethyl acrylate copolymer (EEA), ethylene-butyl acrylate copolymer (EBA), ethylene-methacrylic acid copolymer (EMAA), etc. obtained by modifying the side chain of olefin, and may be used as appropriate.

[0026] The gas barrier thermoplastic resin 3 is not particularly limited, but may be selected from aromatic polyamide resin, polyvinyl alcohol resin, polyester containing furandicarboxylic acid group or naphthalenedicarboxylic acid group, polyvinylidene chloride resin, polymetaxylene adipamide (polyamide MXD6), ethylene-vinyl alcohol copolymer (EVOH), etc., either alone or in combination. In the case of polyamide MXD6, it has the advantage of being usable as a packaging material for boiling and retorting, since it is hot water resistant in addition to gas barrier properties.

[0027] The mixing ratio of the gas barrier thermoplastic resin 3 is not particularly limited, but in order to achieve both gas barrier properties and impact resistance, it is preferably 5wt% to 50wt%, more preferably 10wt% to 40wt%, and even more preferably 20wt% to 40wt%.

[0028] Among them, it is preferable that the heat sealable thermoplastic resin 2 is polypropylene, ethylene-polypropylene copolymer or block polypropylene, and the gas barrier thermoplastic resin 3 is ethylene-vinyl alcohol copolymer (EVOH). In this case, the heat sealability is good and the gas barrier property is also high, and further, the dispersion structure of the gas barrier thermoplastic resin 3 can be easily made flat. In addition, since the ethylene ratio of the ethylene-vinyl alcohol copolymer (EVOH) can control the peak temperature of heat of fusion, it is also easy to control the difference in the peak temperature of heat of fusion between the heat sealable thermoplastic resin 2 and the gas barrier thermoplastic resin 3.

[0029] Furthermore, the thermoplastic resin film 1 may contain a compatibilizer in order to improve the dispersibility of the gas barrier thermoplastic resin 3 in the heat sealable thermoplastic resin 2 and the adhesive strength of the phase interface. Examples of the compatibilizer are not particularly limited, but polymers containing polar groups such as hydroxyl groups, carboxyl groups, carbonyl groups, amide groups, and maleic anhydride groups are preferred. In particular, maleic anhydride modified resin polyolefins are preferably used. The mixing ratio is preferably 1 wt% to 20 wt%, more preferably 3 wt% to 15 wt%, and even more preferably 5 wt% to 12 wt%. This allows both gas barrier properties and impact resistance to be achieved.

[0030] In addition, various additives may be mixed into the thermoplastic resin film 1. For example, additives such as nucleating agents, reinforcing fillers, antioxidants, heat stabilizers, weathering agents, light stabilizers, plasticizers, ultraviolet absorbers, antistatic agents, flame retardants, flame retardant assistants, slip agents, antiblocking agents, antifogging agents, lubricants, pigments, dyes, dispersants, copper damage inhibitors, neutralizing agents, bubble inhibitors, weld strength improvers, natural oils, synthetic oils, and waxes may be used, and rubber components such as elastomers may be used to further improve impact resistance. These may be used alone or in combination of two or more.

[0031] As shown in FIG. 2, a heat seal layer 4 may be laminated on at least one surface of the thermoplastic resin film 1. In this case, it is preferable that the heat seal layer 4 does not contain a gas barrier thermoplastic resin 3. The material of the heat seal layer 4 may be the same as or different from the heat sealable thermoplastic resin 2. The material of the heat seal layer 4 can be selected according to the heat sealing temperature, but by using a material that has excellent adhesion to the heat sealable thermoplastic resin 2, delamination between layers can be prevented.

[0032] Furthermore, a functional layer may be disposed on the surface of the thermoplastic resin film 1 opposite to the surface on which the heat seal layer 4 is disposed. The functional layer is, for example, a printed layer, a vapor deposition layer, or another coating layer.

[0033] The method for producing the thermoplastic resin film 1 in this embodiment includes the steps of: (1) selecting a heat-sealable thermoplastic resin 2 and a gas-barrier thermoplastic resin 3 such that the difference between the absolute value of the peak heat of fusion temperatures of the heat-sealable thermoplastic resin 2 and the gas-barrier thermoplastic resin 3 in a second run measured with a differential scanning calorimeter is 0°C or more and 10°C or less; (2) kneading a thermoplastic resin containing the heat-sealable thermoplastic resin 2, the gas-barrier thermoplastic resin 3, and a compatibilizer using a twin-screw extruder; (3) extrusion molding the kneaded thermoplastic resin; and (4) biaxially stretching the extruded thermoplastic resin such that the peak heat of fusion temperature in the first run is 2°C or more higher than the peak heat of fusion temperature in the second run measured with a differential scanning calorimeter, forming a sea-island structure in which the gas-barrier thermoplastic resin 3 exists as islands in the heat-sealable thermoplastic resin 2. Since the difference in the peak temperature of heat of fusion between the heat-sealable thermoplastic resin 2 and the gas-barrier thermoplastic resin 3 is 0°C or more and 10°C or less, the gas-barrier thermoplastic resin 3 is easily flattened in the film, the degree of dispersion is improved by adding a compatible solvent and kneading before extrusion molding, and the dispersion structure in the film is further stretched by biaxial stretching. As a result, the gas-barrier thermoplastic resin 3 exists as islands in a sea-island structure, and 0.3 layers or more overlap per 1 μm of film thickness in the thickness direction of the film, thereby improving impact resistance, gas barrier properties, and heat sealability.

[0034] The thermoplastic resin film 1 may be formed, for example, by a method in which an unstretched film is produced by injection molding, extrusion molding, inflation molding, blow molding, compression molding, or the like, and then stretched. Alternatively, a method in which the film is stretched after melting and before cooling, such as inflation molding or blow molding, may be used.

[0035] As a method for mixing the heat-sealable thermoplastic resin 2 and the gas-barrier thermoplastic resin 3, a method of kneading them with, for example, a single screw extruder, a twin screw extruder, or a kneader before molding may be used. By kneading a plurality of resins, the dispersion size can be reduced and strength such as impact resistance can be improved. As a kneading method, a method in which a strong shear stress is applied, such as a twin screw extruder or a kneader, is preferable, and a method that allows continuous production, such as a twin screw extruder, is more preferable.

[0036] When a plurality of layers are laminated, they may be produced by any method, such as a film-forming method using a die via a feed block or a multi-manifold.

[0037] The stretching method of the thermoplastic resin film 1 may be any method such as simultaneous biaxial stretching, sequential biaxial stretching, multi-stage stretching in which further stretching is performed after simultaneous or sequential biaxial stretching, or uniaxial stretching. In particular, biaxial stretching is preferable to give excellent mechanical properties in both the machine direction (MD) and the width direction (TD). Since an unstretched film is likely to stretch in the machine direction, the stretching ratio is preferably larger in the width direction than in the machine direction. In the case of uniaxial stretching, uniaxial stretching in the width direction is preferable to spread the gas barrier thermoplastic resin 3 more effectively in a flat shape. The stretching ratio can be suitably selected, and is preferably, for example, 2 to 10 times.

[0038] The thermoplastic resin film 1 according to the present embodiment can be laminated with other substrates to form a packaging material. In the case of a packaging material using the thermoplastic resin film 1 as a single film or a laminate, it can be used for a three-sided bag, a two-handled bag, a gusseted bag, a pouch with a spout, a pouch with a beak, and the like, in addition to a standing pouch. The manufacturing style of the packaging material (packaging bag) is not particularly limited.

[0039] As described above, in either case where the thermoplastic resin film 1 is used as a single film or laminated with another substrate, it is possible to carry out a surface modification treatment to improve suitability for post-processing as appropriate. For example, it is possible to carry out a surface modification treatment on the surface that comes into contact with another substrate in order to improve printability when used as a single film and lamination suitability when used as a laminated structure. As the surface modification treatment, a method of expressing functional groups by oxidizing the film surface such as corona discharge treatment, plasma treatment, and frame treatment, and modification by a wet process such as coating an easy-adhesion layer can be suitably used.

[0040] The production method is not limited to the above-mentioned method, and the resin molded body formed into a film by a molding machine may be subjected to an in-line, off-line, or batch-type stretching treatment. In addition, there is no restriction on adding other necessary steps or additives as appropriate. EXAMPLES

[0041] Examples prepared by the present inventors will be described in detail below in comparison with comparative examples, but the present invention is not limited to only the following examples.

[0042] Example 1 The heat-sealable thermoplastic resin 2 was a homopolypropylene (PP) resin "PC412A" manufactured by Sunallomer Co., Ltd., the gas-barrier thermoplastic resin 3 was an ethylene-vinyl alcohol copolymer (EVOH) resin "Eval E105B" manufactured by Kuraray Co., Ltd., and the compatibilizer was a maleic anhydride-modified polypropylene (PP-MAH) resin "Rikeaid MG-441P" manufactured by Riken Vitamin Co., Ltd. The above three resins were dry-blended in the order of 55 wt%, 35 wt%, and 10 wt%, and an unstretched film (sheet) with a thickness of 1 mm was produced by extrusion molding manufactured by Plastics Engineering Research Institute Co., Ltd. Then, a stretched film with a thickness of 50 μm was produced by a batch-type biaxial stretching machine manufactured by Eversokki Co., Ltd. The stretching ratio was 4 times in both the machine direction and the width direction of the unstretched film.

[0043] Comparative Example 1 Comparative Example 1 was the same as Example 1, except that an unstretched film having a thickness of 50 μm was produced by extrusion molding, and the subsequent stretching step was not carried out.

[0044] Comparative Example 2 Comparative Example 2 was the same as Comparative Example 1, except that an unstretched film with a thickness of 1 mm was extruded from a T-die, and then the film was pulled by hand in a molten state at a position approximately 100 mm away from the T-die (referred to as melt stretching 1 here) to produce a film with a thickness of approximately 50 μm.

[0045] Example 2 Example 2 was the same as Example 1, except that, in comparison with Comparative Example 2, the extruded resin was manually pulled (herein referred to as melt-stretching 2) at a position where it was cooler (a position about 300 mm away from the T-die and where the temperature was maintained before solidification) to produce a film with a thickness of about 50 μm, and the subsequent stretching process was not performed.

[0046] Example 3 Example 3 was the same as Example 1, except that a master batch was prepared in advance by kneading three resins, namely, a heat-sealable thermoplastic resin 2, a gas-barrier thermoplastic resin 3, and a compatibilizer, in a twin-screw extruder manufactured by The Japan Steel Works, Ltd., and extrusion molding was then carried out.

[0047] Comparative Example 3 Comparative Example 3 was the same as Comparative Example 1, except that a master batch was prepared in advance by kneading three resins, namely, a heat-sealable thermoplastic resin 2, a gas-barrier thermoplastic resin 3, and a compatibilizer, in a twin-screw extruder manufactured by The Japan Steel Works, Ltd., and extrusion molding was then carried out.

[0048] Example 4 Example 4 was the same as Example 3, except that no compatibilizer was used, and only heat-sealable thermoplastic resin 2 and gas-barrier thermoplastic resin 3 were used in a mixing ratio of 65 wt% and 35 wt%, respectively.

[0049] Comparative Example 4 Comparative Example 4 was the same as Comparative Example 3, except that no compatibilizer was used, and only heat-sealable thermoplastic resin 2 and gas-barrier thermoplastic resin 3 were used in their mixing ratios of 65 wt% and 35 wt%, respectively.

[0050] Comparative Example 5 Comparative Example 5 was the same as Comparative Example 1, except that no compatibilizer was used, and only the heat-sealable thermoplastic resin 2 and the gas-barrier thermoplastic resin 3 were used in a mixing ratio of 65 wt% and 35 wt%, respectively, and an unstretched film (sheet) having a thickness of 1 mm was produced by extrusion molding, and then a stretched film having a thickness of 50 μm was produced by a batch-type biaxial stretching machine.

[0051] Comparative Example 6 Comparative Example 6 was the same as Comparative Example 1, except that no compatibilizer was used, and only heat-sealable thermoplastic resin 2 and gas-barrier thermoplastic resin 3 were used, with their mixing ratios being 65 wt% and 35 wt%, respectively.

[0052] Comparative Example 7 Comparative Example 7 was the same as Comparative Example 1, except that an ethylene-vinyl acetate copolymer (EVA) resin "EV450" manufactured by Dow Mitsui Polychemicals Co., Ltd. was used as the compatibilizer.

[0053] (Calculation of the number of overlaps of the gas barrier thermoplastic resin 3) The thickness cross-section observation of the obtained film was carried out by cutting out a sample to 2 mm x 5 mm (observation part is 2 mm), embedding it in visible light curable embedding resin "D-800" manufactured by JEOL Ltd., and cutting out the cross-section using an ultramicrotome "EM UC7i" manufactured by Leica Microsystems in the order of a glass knife and a diamond knife. Then, in order to create a contrast difference in the observation images of the heat sealable thermoplastic resin 2 and the gas barrier thermoplastic resin 3, they were stained with ruthenium tetroxide, and the cross-section was cut out again using an ultramicrotome with a diamond knife to obtain an observation cross-section. The observation test pieces were cut out at 10 randomly selected points for each sample. For the observation, a scanning electron microscope "SU8020" manufactured by Hitachi High-Technologies Corporation was used to observe the above cross-section in the image while changing the observation magnification from 1000 times to 20000 times as needed, and the overlap number was calculated.

[0054] (Calculation of the fusion heat peak temperature difference between the 1st run and the 2nd run) The peak temperature of the heat of fusion in the first run and the peak temperature of the heat of fusion in the second run of the obtained film were measured using a differential scanning calorimeter "DSC7020" manufactured by Hitachi High-Tech Science Corporation according to the method of JIS K7121 (2012). Specifically, about 5 mg of the obtained film was cut out and sealed in an AL pan, and then, as shown in Figure 3, it was held at room temperature until the device stabilized (a), and then heated from room temperature to 230 ° C at a rate of 10 ° C / min (b). The peak temperature of the heat of fusion in the first run was obtained from the DSC curve obtained in the range of heating temperature (a) to (b) in Figure 3 (1st run). After that, it was held at 230 ° C for 10 minutes (c), cooled to room temperature at a rate of 10 ° C / min (d), and held at room temperature for 10 minutes (e). After that, the temperature was raised again from room temperature to 230°C at a rate of 10°C / min (f), and the peak temperature of the heat of fusion in the 2nd run was obtained from the DSC curve obtained in the heating temperature range of (e) to (f) in Figure 3 (2nd run). The difference in the peak temperature of the heat of fusion between the 1st run and the 2nd run was calculated by subtracting the peak temperature of the heat of fusion in the 2nd run from the peak temperature of the heat of fusion in the 1st run.

[0055] (Gas barrier property evaluation) For the gas barrier property evaluation, oxygen permeability was measured in a dry environment at 30℃ using a highly sensitive water vapor permeability measuring device "GTR-3000" manufactured by GTR Tech Co., Ltd. For each film obtained, those with an oxygen permeability of 40cc / m2 / day / atm or less when converted to a film thickness of 100μm were marked as "Good", and those exceeding 40cc / m2 / day / atm were marked as "Poor".

[0056] (Impact resistance evaluation) Impact resistance was evaluated using a film impact tester manufactured by Toyo Seiki Co., Ltd., with measurements taken at a temperature of -5°C, a weighing capacity of 1.5 J, and a bullet size of 1.5 inches. Measurements of 50 mJ or more were marked as "good," and measurements of less than 50 mJ were marked as "bad."

[0057] (comprehensive evaluation) Regarding the overall evaluation, a sample that received a score of "good" in both the gas barrier property evaluation and the impact resistance evaluation was given an overall evaluation of "good", and a sample that received a score of "bad" in either evaluation was given an overall evaluation of "bad".

[0058] Table 1 shows a list of the conditions and evaluation results in Examples 1, 2, 3, and 4 and Comparative Examples 1, 2, 3, 4, 5, 6, and 7.

[0059] [Table 1]

[0060] (Examples 5, 6, 7, 8, 9, 10, 11, 12, 13, 14) Examples 5, 6, 7, 8, 9, 10, 11, 12, 13, and 14 were similar to Example 1, except that either or both of the materials for the heat-sealable thermoplastic resin 2 and the gas-barrier thermoplastic resin 3 were changed. In Examples 5, 6 and 7, the material of the gas barrier thermoplastic resin 3 was an ethylene-vinyl alcohol copolymer (EVOH) resin "EVAL G156B", "EVAL H171B" and "EVAL F171B" manufactured by Kuraray Co., Ltd., respectively. In Examples 8, 9, 10, and 11, the heat-sealable thermoplastic resin 2 was a homopolypropylene (PP) resin "PC600A" manufactured by Sunallomer Co., Ltd., and the material of the gas-barrier thermoplastic resin 3 was an ethylene-vinyl alcohol copolymer (EVOH) resin "EVAL G156B," "EVAL E105B," "EVAL H171B," or "EVAL F171B" manufactured by Kuraray Co., Ltd. In Examples 12, 13, and 14, the heat-sealable thermoplastic resin 2 was a random polypropylene (PP) resin "F227" manufactured by Prime Polymer Co., Ltd., and the material for the gas-barrier thermoplastic resin 3 was an ethylene-vinyl alcohol copolymer (EVOH) resin "EVAL G156B," "EVAL E105B," and "EVAL H171B," manufactured by Kuraray Co., Ltd., respectively.

[0061] The obtained film was evaluated in the same manner as above for the number of overlaps of the gas barrier thermoplastic resin 3, the difference in the peak temperature of heat of fusion between the 1st run and the 2nd run, and the impact resistance. The gas barrier property was evaluated in the same manner as above, except that the evaluation classification was divided into three categories: oxygen permeability of 20cc / m2 / day / atm or less was evaluated as "◎", oxygen permeability of 40cc / m2 / day / atm or less was evaluated as "〇", and oxygen permeability of more than 40cc / m2 / day / atm was evaluated as "×". In addition, the overall evaluation was also as follows: a gas barrier property evaluation of "◎" and an impact resistance evaluation of "〇" were evaluated as "◎", a both evaluation of "〇" were evaluated as "〇", and a both evaluation of "×" were evaluated as "×".

[0062] (Measurement of the peak temperature of heat of fusion of each resin) The heat of fusion peak temperatures of the heat sealable thermoplastic resin 2 and the gas barrier thermoplastic resin 3 were measured in the same manner as the measurement of the heat of fusion peak temperature of the thermoplastic resin film 1, using a differential scanning calorimeter "DSC7020" manufactured by Hitachi High-Tech Science Corporation, in accordance with JIS K7121 (2012). Specifically, about 5 mg of each resin pellet was cut out and sealed in an AL pan, and after keeping it at room temperature until the device stabilized, as shown in FIG. 3, (a), the temperature was raised from room temperature to 230°C at a rate of 10°C / min (b), and after keeping it at 230°C for 10 minutes (c), the temperature was lowered to room temperature at a rate of 10°C / min (d), and kept at room temperature for 10 minutes (e). Then, the temperature was raised again from room temperature to 230°C at a rate of 10°C / min (f). The peak temperature of the heat of fusion in the 2nd run was determined from the DSC curves obtained in the heating temperature range (e) to (f) in FIG. 3, and this temperature was taken as the peak temperature of the heat of fusion for each resin.

[0063] Table 2 shows a list of the conditions and evaluation results in Example 1 and Examples 5, 6, 7, 8, 9, 10, 11, 12, 13, and 14.

[0064] [Table 2]

[0065] (Evaluation Results) As shown in Table 1, in Example 1, the successive biaxial stretching step was performed, which promoted flattening of the gas barrier thermoplastic resin 3, and at the same time increased the number of overlaps of the gas barrier thermoplastic resin 3 and the difference in the heat of fusion peak temperature between the 1st run and the 2nd run, and accordingly, the gas barrier property and impact resistance were improved, and both were evaluated as "Good." On the other hand, in Comparative Example 1, the successive biaxial stretching step was not performed, and therefore the flattening and dispersion of the gas barrier thermoplastic resin 3 was insufficient, resulting in no difference in the heat of fusion peak temperature, and both the gas barrier property and impact resistance were evaluated as "Poor."

[0066] In Comparative Example 2, the film was stretched in a molten state by pulling it by hand, as compared to Comparative Example 1, which was not subjected to sequential biaxial stretching. However, no effect was observed, and both the gas barrier property and the impact resistance were rated as "x". On the other hand, as in Example 2, it was found that, depending on the stretching conditions, both the gas barrier property and the impact resistance were improved and rated as "o". In Example 2, when the film was stretched by hand in a molten state at a temperature lower than that of Comparative Example 2, the number of overlaps of the gas barrier thermoplastic resin 3 and the difference in the heat of fusion peak temperature between the 1st run and the 2nd run increased.

[0067] In Comparative Example 3, a compatibilizer was added and a kneading process using a twin-screw extruder was carried out in advance, which allowed the gas barrier thermoplastic resin 3 to be finely dispersed, and the impact resistance was rated "good." However, since no stretching was performed, the shape was not flattened, and the gas barrier property was rated "poor." On the other hand, in Example 3, in which sequential biaxial stretching was performed in comparison with Comparative Example 3, the gas barrier thermoplastic resin 3 became flat and the number of overlaps increased, improving the gas barrier property and rated "good" as in Example 1.

[0068] In Comparative Example 4, a kneading step using a twin-screw extruder was carried out in advance, but a compatibilizer was not added, and neither stretching was performed, so the gas barrier thermoplastic resin 3 was not sufficiently flattened and dispersed, and there was no difference in the heat of fusion peak temperature, resulting in both results being "x". On the other hand, in Example 4, in which a successive biaxial stretching step was carried out in comparison with Comparative Example 4, the gas barrier thermoplastic resin 3 was flattened and the number of overlaps increased, resulting in both gas barrier property and impact resistance being "good".

[0069] In Comparative Example 6, since the stretching process was not performed, the gas barrier thermoplastic resin 3 was stretched in the flow direction and was flat, but was not stretched in the width direction and was round. In addition, the dispersion size was also large, and the number of overlaps was small. As a result, both the gas barrier property and the impact resistance were "x". On the other hand, in Comparative Example 5, unlike Comparative Example 6, a sequential biaxial stretching process was performed, and although the fusion heat peak temperature difference between the 1st run and the 2nd run was improved, the original dispersion size of the gas barrier thermoplastic resin 3 was large, and the number of overlaps of the gas barrier thermoplastic resin 3 did not increase much even after stretching. Therefore, unlike Examples 1, 3, and 4, both the gas barrier property and the impact resistance were "x".

[0070] In Comparative Example 7, no stretching was performed, but the shape of the gas-barrier thermoplastic resin 3 was flattened and the overlap number exceeded 0.3, so the gas barrier property was rated as "good". However, due to the large dispersion size, the impact resistance was rated as "poor".

[0071] As shown in Table 2, in Examples 1, 5, 8, 9, 10, 12, and 13, in which the difference between the peak temperatures of the heat of fusion of the heat-sealable thermoplastic resin 2 and the gas-barrier thermoplastic resin 3 was 0°C or more and 10°C or less in absolute value, the shape of the gas-barrier thermoplastic resin 3 was particularly flattened, and the gas barrier property was rated as "◎". On the other hand, in Examples 6, 7, 11, and 14, in which the difference between the peak temperatures of the heat of fusion of the heat-sealable thermoplastic resin and the gas-barrier thermoplastic resin was greater than 10°C in absolute value, the gas barrier property was rated as "◯". In all of the Examples, the impact resistance was rated as "◯".

[0072] From the results of Examples 1 to 4 and Comparative Examples 1 to 7, films that were stretched, had a gas barrier thermoplastic resin overlap number of 0.3 or more layers per 1 μm of film thickness, and had a first run whose heat of fusion peak temperature was 2°C or more higher than the second run's heat of fusion peak temperature, had good gas barrier properties and impact resistance, and were overall evaluated as "good." Furthermore, from the results of Examples 1 and 5 to 14, it was confirmed that a film in which the difference between the peak temperatures of the heat of fusion of the heat-sealable thermoplastic resin and the gas-barrier thermoplastic resin is an absolute value of 0°C or more and 10°C or less has better gas barrier properties.

[0073] Furthermore, for example, the present invention can have the following configuration. (1) A thermoplastic resin film comprising a heat-sealable thermoplastic resin and a gas-barrier thermoplastic resin, in which a sea-island structure is formed in which the gas-barrier thermoplastic resin exists as islands in the heat-sealable thermoplastic resin, It is stretched, the gas barrier thermoplastic resin has a flattened shape extending in the plane direction of the film, and overlaps with 0.3 layers or more per 1 μm of film thickness from any point on the surface of the film toward the thickness direction of the film, In the measurement of the film by a differential scanning calorimeter, the peak temperature of heat of fusion in the first run is 2°C or more higher than the peak temperature of heat of fusion in the second run. A thermoplastic resin film characterized by: (2) The thermoplastic resin film according to (1) above, having a thickness of 10 μm or more and 200 μm or less. (3) The thermoplastic resin film described in (1) above, characterized in that the difference between the heat of fusion peak temperatures of the heat-sealable thermoplastic resin and the gas-barrier thermoplastic resin in a second run measured with a differential scanning calorimeter is, in absolute value, 0°C or more and 10°C or less. (4) The thermoplastic resin film according to the above (1), further comprising a compatibilizer. (5) The thermoplastic resin film according to any one of (1) to (4) above, characterized in that the heat-sealable thermoplastic resin is polypropylene, an ethylene-polypropylene copolymer or a block polypropylene, and the gas-barrier thermoplastic resin is an ethylene-vinyl alcohol copolymer. (6) A heat seal layer is further laminated on at least one surface of the thermoplastic resin film according to any one of (1) to (5) above, the heat seal layer does not contain the gas barrier thermoplastic resin; A thermoplastic resin film characterized by: (7) selecting a heat sealable thermoplastic resin and a gas barrier thermoplastic resin, the difference between the heat of fusion peak temperatures in a second run of the heat sealable thermoplastic resin and the gas barrier thermoplastic resin being 0°C or more and 10°C or less in absolute value, a step of kneading the heat sealable thermoplastic resin, the gas barrier thermoplastic resin, and a thermoplastic resin containing a compatibilizer by a twin-screw extruder; extrusion molding the kneaded thermoplastic resin; biaxially stretching the extruded thermoplastic resin such that the peak temperature of heat of fusion in a first run is 2° C. or more higher than the peak temperature of heat of fusion in a second run, as measured by a differential scanning calorimeter; Including, The method for producing a thermoplastic resin film comprises forming a sea-island structure in which the gas barrier thermoplastic resin exists as islands in the heat sealable thermoplastic resin. [Explanation of symbols]

[0074] 1 Thermoplastic resin film 2. Heat-sealable thermoplastic resin 3. Gas barrier thermoplastic resin 4 Heat seal layer

Claims

1. A thermoplastic resin film comprising a heat-sealable thermoplastic resin and a gas-barrier thermoplastic resin, in which a sea-island structure is formed in which the gas-barrier thermoplastic resin exists as islands in the heat-sealable thermoplastic resin, It is stretched, the gas barrier thermoplastic resin has a flattened shape extending in a plane direction of the film, and overlaps with 0.3 layers or more per 1 μm of film thickness from any point on the surface of the film toward the thickness direction of the film, In the measurement of the film by a differential scanning calorimeter, the peak temperature of heat of fusion in the first run is higher by 2° C. or more than the peak temperature of heat of fusion in the second run. A thermoplastic resin film characterized by:

2. The thermoplastic resin film according to claim 1 , which has a thickness of 10 μm or more and 200 μm or less.

3. 2. The thermoplastic resin film according to claim 1, wherein the difference between the peak temperatures of heat of fusion of the heat sealable thermoplastic resin and the gas barrier thermoplastic resin in the second run measured by a differential scanning calorimeter is 0° C. or more and 10° C. or less in absolute value.

4. The thermoplastic resin film of claim 1 , further comprising a compatibilizer.

5. The thermoplastic resin film according to any one of claims 1 to 4, characterized in that the heat-sealable thermoplastic resin is polypropylene, an ethylene-polypropylene copolymer or a block polypropylene, and the gas-barrier thermoplastic resin is an ethylene-vinyl alcohol copolymer.

6. A heat seal layer is further laminated on at least one surface of the thermoplastic resin film according to any one of claims 1 to 4, the heat seal layer does not contain the gas barrier thermoplastic resin; A thermoplastic resin film characterized by:

7. selecting a heat-sealable thermoplastic resin and a gas-barrier thermoplastic resin, the difference between the peak temperatures of heat of fusion in the second run of the heat-sealable thermoplastic resin and the gas-barrier thermoplastic resin being 0° C. or more and 10° C. or less in absolute value, as measured by a differential scanning calorimeter; a step of kneading the heat sealable thermoplastic resin, the gas barrier thermoplastic resin, and a thermoplastic resin containing a compatibilizer by a twin-screw extruder; extrusion molding the kneaded thermoplastic resin; A step of biaxially stretching the extruded thermoplastic resin such that, in measurement by a differential scanning calorimeter, the peak temperature of heat of fusion in a first run is 2° C. or more higher than the peak temperature of heat of fusion in a second run; Including, The method for producing a thermoplastic resin film comprises forming a sea-island structure in which the gas barrier thermoplastic resin exists as islands in the heat sealable thermoplastic resin.

Citation Information

Patent Citations

  • Resin composition and its molded product

    JP2003155419A

  • Molding and method for producing the same

    JP2016150949A

Cited By

  • Adhesive film, and monolayer or multilayer film

    WO2025205936A1