Manufacturing method for battery
By measuring and adjusting the drying temperature based on the positional difference between the electrode sheet and separator ends, the method addresses separator damage in battery manufacturing, enhancing durability and efficiency.
Patent Information
- Application Number
- JP2023059437
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing battery manufacturing methods fail to effectively suppress damage to the separator in contact with the innermost electrode sheet of the wound body, leading to potential breakage and internal short circuits during overcharging.
A method for manufacturing a battery that involves measuring the positional difference between the ends of the electrode sheet and the separator, and adjusting the drying temperature based on this difference to control the thermal contraction of the separator, thereby minimizing damage.
The method effectively adjusts the drying temperature to match the positional difference, reducing separator damage and preventing tears, while also shortening the drying time for batteries with smaller differences and ensuring thorough drying for those with larger differences.
Smart Images

Figure 2024146495000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a battery. [Background technology]
[0002] It is known that a battery includes a wound body in which a positive electrode sheet, a negative electrode sheet, and a separator are wound in a stacked state (see, for example, Patent Document 1).
[0003] Patent Document 1 discloses a technology for a non-aqueous secondary battery, in which a cylindrical part is provided in the electrode plate group winding core space and fixed to the bottom of the exterior can or the sealing plate, and a heat-shrinkable resin film is wound around the cylindrical part and provided in contact with the innermost separator of the electrode group so as to link with the electrode group, and has a structure that causes the heat-shrinkage in the winding direction during overcharge. This suppresses buckling of the electrode plate group due to expansion of the electrode plates and internal short circuit due to breakage of the separator during overcharge.
[0004] In a battery, it is preferable to suppress damage to the separator provided in contact with the innermost electrode sheet of the wound body. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2005-174793 A Summary of the Invention [Problem to be solved by the invention]
[0006] In consideration of the above, an object of the present invention is to suppress damage to a separator provided in contact with an innermost electrode sheet of a wound body. [Means for solving the problem]
[0007] A first aspect of the present invention relates to a method for manufacturing a battery having a wound body in which a positive electrode sheet as an electrode sheet, a negative electrode sheet as the electrode sheet, and a separator are stacked and wound, and the method includes a position difference measurement step of measuring a position difference between one width direction end of the electrode sheet that is arranged on the innermost side of the wound body and one width direction end of the separator that protrudes in the width direction from the electrode sheet, and a drying step of drying the wound body at a drying temperature determined based on the position difference.
[0008] In a battery manufacturing method according to a second aspect of the present invention, in the battery manufacturing method according to the first aspect of the present invention, the position difference measuring step measures the position difference at a position corresponding to the R portion of the wound body.
[0009] In a battery manufacturing method according to a third aspect of the present invention, in the battery manufacturing method according to the first or second aspect of the present invention, the drying temperature is set higher as the position difference is smaller.
[0010] A fourth aspect of the present invention relates to a battery manufacturing method according to any one of the first to third aspects of the present invention, and further relates to a battery manufacturing method in which the drying temperature is set lower as the position difference is larger. Effect of the Invention
[0011] In the battery manufacturing method according to the first aspect of the present invention, the wound body is dried at a drying temperature determined based on the position difference, so that the wound body is dried at a drying temperature according to the position difference. Therefore, the amount of shrinkage of the separator is adjusted. As a result, it is possible to suppress damage to the separator provided in contact with the innermost electrode sheet of the wound body.
[0012] In the battery manufacturing method according to the second aspect of the present invention, the position difference is measured at a position corresponding to the R portion of the wound body, so that the position difference is measured at a sharp portion of the wound electrode sheet where the separator is likely to be damaged. Therefore, the amount of contraction of the separator is adjusted at the portion where the separator is likely to be damaged. As a result, damage to the portion of the separator that is likely to be damaged can be suppressed.
[0013] In the battery manufacturing method according to the third aspect of the present invention, the smaller the position difference is, the higher the drying temperature is set, so that the wound body with a small position difference is dried at a high drying temperature, thereby making it possible to reduce the drying time while suppressing damage to the separator.
[0014] In the battery manufacturing method according to the fourth aspect of the present invention, the larger the position difference is, the lower the drying temperature is set, so that the wound body with a large position difference is dried at a low temperature. Therefore, even if the wound body has a large position difference, it is possible to dry the wound body while suppressing damage to the separator. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a perspective view showing a lithium ion secondary battery according to an embodiment. [Diagram 2] 2 is a schematic diagram showing a partial cross section of the wound body according to the embodiment, showing the cross section taken along the line AA in FIG. [Diagram 3] 3 is a cross-sectional view showing a schematic view of a wound body according to the embodiment, showing the cross section taken along line BB in FIG. 2. [Figure 4] FIG. 2 is a perspective view showing the innermost circumference of a wound body according to the embodiment; [Diagram 5] FIG. 5 is an explanatory diagram illustrating the function of a battery. FIG. 5(A) is a diagram illustrating the stress acting on a separator when the cell is dried, and FIG. 5(B) is a diagram illustrating a state in which the separator is torn. [Figure 6]6A is a graph showing the relationship between the amount of shrinkage of the separator and the position difference or temperature, and FIG. 6B is a graph showing the relationship between the amount of shrinkage of the separator and the position difference portion, and FIG. 6B is a graph showing the relationship between the amount of shrinkage of the separator and the temperature. [Figure 7] FIG. 2 is a flow diagram showing a method for manufacturing a battery according to an embodiment. [Figure 8] 8A and 8B are diagrams for explaining the effects of the lithium ion secondary battery according to the embodiment, in which FIG. 8(A) is a graph showing the relationship between the cell drying temperature and the position difference for each example, and FIG. 8(B) is a table showing the separator breakage and drying time for each example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, the battery according to the embodiment will be described with reference to the drawings. The battery according to the embodiment will be described as an example of a lithium ion secondary battery constituting a battery module used as an on-board power source for electric vehicles, hybrid vehicles, etc. In each drawing, an arrow D indicates the longitudinal direction D of the lithium ion secondary battery 10, an arrow E indicates the depth direction E of the lithium ion secondary battery 10, an arrow F indicates the up-down direction F of the lithium ion secondary battery 10, and an arrow T indicates the thickness direction T of the wound body 30. The longitudinal direction D of the lithium ion secondary battery 10 coincides with the width direction G of the wound body 30, and one side of the width direction G of the wound body 30 is a positive electrode, and the other side of the width direction G of the wound body is a negative electrode.
[0017] [Configuration of lithium-ion secondary battery 10] As shown in FIG. 1, the lithium ion secondary battery 10 includes a lid assembly 20, a wound body 30, and a battery case 70.
[0018] (battery case 70) The battery case 70 is made of, for example, aluminum, and is formed in the shape of a rectangular box that is long in the longitudinal direction D and has an open top.
[0019] (Lid Assembly 20) The lid assembly 20 includes a lid member 21, a negative electrode current collector terminal 22 as a current collector terminal, a positive electrode current collector terminal 23 as a current collector terminal, a negative electrode external terminal 24 as an external terminal, and a positive electrode external terminal 25 as an external terminal.
[0020] <Cover member 21> The lid member 21 is made of, for example, aluminum, and is formed in a rectangular plate shape extending in the longitudinal direction D. The lid member 21 is provided with a safety valve 21A and a cap 26 that closes the injection port 21B.
[0021] The safety valve 21A opens when the internal pressure of the battery case 70 reaches a predetermined pressure, and discharges gas generated inside the battery case 70.
[0022] Inlet 21B is formed as a through hole penetrating in the plate thickness direction of lid member 21. Inlet 21B is used when injecting an electrolyte into battery case 70. Cap 26 is attached to inlet 21B, for example, by laser welding, and is hermetically sealed.
[0023] With the wound body 30, the negative electrode collector terminal 22, and the positive electrode collector terminal 23 housed inside the battery case 70, the lid member 21 is attached, for example, by laser welding, so as to cover the opening of the battery case 70.
[0024] <Negative electrode current collector terminal 22 and negative electrode external terminal 24> The negative electrode current collector terminal 22 and the negative electrode external terminal 24 are made of copper, and are disposed on the other end side in the longitudinal direction D of the battery case 70. The negative electrode current collector terminal 22 is formed in a rectangular plate shape with the plate thickness direction being the depth direction E. The negative electrode current collector terminal 22 is joined to the negative electrode current collector part 32 of the wound body 30 by, for example, ultrasonic welding. The negative electrode external terminal 24 is electrically connected to the negative electrode current collector terminal 22, and is exposed to the outside of the lid member 21.
[0025] <Positive electrode current collector terminal 23 and positive electrode external terminal 25> The positive electrode current collector terminal 23 is made of aluminum, for example, and is disposed at one end side in the longitudinal direction D of the battery case 70. The positive electrode current collector terminal 23 is formed in a rectangular plate shape with the depth direction E as the plate thickness direction. The positive electrode current collector terminal 23 is joined to the positive electrode current collector part 33 of the wound body 30 by, for example, resistance welding. The positive electrode external terminal 25 is electrically connected to the positive electrode current collector terminal 23 and exposed to the outside of the lid member 21.
[0026] (Wound body 30) As shown in FIG. 1, the wound body 30 has a power generating body 31 , a negative electrode current collecting portion 32 , and a positive electrode current collecting portion 33 .
[0027] As shown in FIG. 2, the wound body 30 is formed by winding a negative electrode sheet 40 as an electrode sheet, a positive electrode sheet 50 as an electrode sheet, and two separators 60 in a stacked state, so that the wound body 30 has a flat cross section.
[0028] The power generating body 31 is formed by stacking a region of the positive electrode sheet 50 coated with a positive electrode active material, a region of the negative electrode sheet 40 coated with a negative electrode active material, and a separator 60. The power generating body 31 has a function of storing electric energy of the lithium ion secondary battery 10.
[0029] The negative electrode current collecting part 32 is not coated with an active material, and is formed by winding a negative electrode sheet 40. The positive electrode current collecting part 33 is not coated with an active material, and is formed by winding a positive electrode sheet 50.
[0030] <Negative electrode sheet 40> 3, the negative electrode sheet 40 has a negative electrode active material 42 applied to both sides of a long strip-shaped negative electrode body 41. The negative electrode active material 42 has an outer periphery-side negative electrode active material 42A arranged on the outer periphery side, and an inner periphery-side negative electrode active material 42B arranged on the inner periphery side.
[0031] The negative electrode sheet 40 has the other end in the width direction G where the negative electrode active material 42 is not applied, and the negative electrode body 41 is exposed.
[0032] <Positive electrode sheet 50> The positive electrode sheet 50 is formed by applying a positive electrode active material 52 to both sides of a long strip-shaped positive electrode body 51. The positive electrode active material 52 has an outer periphery-side positive electrode active material 52A arranged on the outer periphery side, and an inner periphery-side positive electrode active material 52B arranged on the inner periphery side.
[0033] The positive electrode sheet 50 has one end in the width direction G where the positive electrode active material 52 is not applied, and the positive electrode body 51 is exposed.
[0034] <Separator 60> The separator 60 is formed of an insulating material such as polypropylene, polyethylene, etc. The separator 60 is disposed between the positive electrode sheet 50 and the negative electrode sheet 40, and insulates the positive electrode sheet 50 from the negative electrode sheet 40.
[0035] The separator 60 is provided so as to protrude from one side in the width direction G relative to the negative electrode sheet 40. The separator 60 is provided so as to protrude from the other side in the width direction G relative to the positive electrode sheet 50.
[0036] 3 and 4, the difference between the position of one widthwise end 40A of the negative electrode sheet 40 arranged on the innermost periphery of the wound body 30 among the electrode sheets and the position of one widthwise end 60A of the separator 60 protruding from the negative electrode sheet 40 to one side in the width direction G is defined as a position difference S. The portion of the separator 60 protruding from the negative electrode sheet 40 to one side in the width direction G is defined as a separator protruding portion 60B.
[0037] [Operation of lithium-ion secondary battery 10] In the lithium ion secondary battery 10 configured as described above, the output of the wound body 30 is taken from the negative electrode external terminal 24 and the positive electrode external terminal 25, and is used as a power source for electric vehicles, hybrid vehicles, and the like.
[0038] [Separator damage] In order to establish a spring constant in the lithium ion secondary battery 10 having the wound body 30, it is desirable to avoid applying pressure to the lithium ion secondary battery 10 as much as possible in a process in which heat is applied, such as cell drying. When the pressure applied to the lithium ion secondary battery 10 is suppressed, the separator 60 will undergo thermal contraction.
[0039] 5(A), when the separator 60 is thermally contracted, a uniformly distributed load of the cantilever acts on the separator protruding portion 60B. The separator protruding portion 60B is then deformed so as to bend toward the inner periphery in the thickness direction T. The amount of displacement of the widthwise end portion 60A of the separator 60 in this case in the thickness direction T is defined as the amount of contraction H.
[0040] The bending moment M acting on the separator protrusion 60B is expressed by the following formula. M=wL 2 / 2 M: Bending moment w: Equally distributed load L: Beam span (length of separator protrusion 60B)
[0041] As shown in FIG. 5(B), a bending moment M acting on the base end of separator protruding portion 60B causes a tear G, which is an example of damage, to occur at the base end of separator protruding portion 60B.
[0042] [Factors of shrinkage] In response to this, a factor investigation was conducted on the shrinkage amount H of the separator 60, and it was found that the position difference S and the drying temperature (cell drying temperature) in the drying process described below are related to the shrinkage amount H of the separator 60. As can be seen from FIG. 6(A), the larger the position difference S, the larger the shrinkage amount H tends to be. As can be seen from FIG. 6(B), the higher the cell drying temperature in the drying process, the larger the shrinkage amount H tends to be. From the viewpoint of shortening the drying time, the cell drying temperature is preferably 80° C. or higher. Furthermore, from the viewpoint of setting the cell drying temperature to 80° C. or higher and suppressing tearing G of the separator 60, it is preferable that the position difference S is 4 mm or less.
[0043] For this reason, in the lithium ion secondary battery 10 of this embodiment, the wound body 30 is dried at a cell drying temperature determined based on the position difference S.
[0044] [Method of manufacturing lithium ion secondary battery 10] The lithium ion secondary battery 10 is manufactured through a source process, a winding process, a case insertion / sealing process, a drying process, a liquid injection process, an activation process, and an inspection process.
[0045] (source process) As shown in FIG. 7, in the source process, the negative electrode sheet 40, the positive electrode sheet 50, and the separator 60 that constitute the battery element of the lithium ion secondary battery 10 are formed (step S1).
[0046] (Winding process / Position difference measurement process) In the winding process, the negative electrode sheet 40, the positive electrode sheet 50, and two separators 60 are wound in a stacked state into a substantially cylindrical shape to form the wound body 30 (step S2). The substantially cylindrical wound body 30 may be formed into a flat shape by pressing. In the winding process, a position difference measurement process is performed. In the position difference measurement process, a position difference S between one widthwise end 40A of the negative electrode sheet 40 arranged on the innermost side of the wound body 30 among the electrode sheets and one widthwise end 60A of the separator 60 protruding from the negative electrode sheet 40 to one side in the width direction G is measured by, for example, a sensor.
[0047] Preferably, the position difference S is measured at a position corresponding to the R portion 30A (see FIG. 2) at the upper part of the wound body 30. The R portion 30A is a portion having an arc-shaped vertical cross section formed in the wound body 30, and is a curved portion having the largest curvature.
[0048] The position difference S may be measured while the wound body 30 is being wound, after the wound body 30 is being wound, or before the wound body 30 is being wound.
[0049] (Case insertion / can sealing process) In the case insertion / sealing process, the negative electrode current collecting terminal 22 is joined to the negative electrode current collecting part 32 of the wound body 30 by, for example, ultrasonic welding, and the positive electrode current collecting terminal 23 is joined to the positive electrode current collecting part 33 of the wound body 30 by, for example, resistance welding. Then, the lid assembly 20 is inserted into the battery case 70, and the lid member 21 is attached to close the opening of the battery case 70 by, for example, laser welding.
[0050] (drying process) In the drying process, the lithium ion secondary battery 10 is vacuum-dried to remove moisture contained in the wound body 30 (step S4). In the drying process, the wound body 30 is dried at a cell drying temperature determined based on the position difference S. Specifically, lithium ion secondary batteries 10 with similar position differences S are dried in a drying chamber at a temperature determined based on the position difference S. In the drying process, the smaller the position difference, the higher the cell drying temperature is set. In the drying process, the larger the position difference, the lower the cell drying temperature is set.
[0051] (liquid injection process) In the liquid injection step, the electrolyte is injected from injection port 21B formed in lid member 21, and cap 26 is attached to injection port 21B by, for example, laser welding to seal it (step S5).
[0052] (activation process) In the activation process, the lithium ion secondary battery 10 is initially charged and then stored at high temperature for a certain period of time to perform high-temperature aging treatment to dissolve metallic foreign matter and stabilize the SEI (Solid Electrolyte Interphase) coating (step S6).
[0053] (Inspection process) In the inspection process, cell voltage, battery resistance, etc. are inspected (step S7) to select lithium-ion secondary batteries 10 that exhibit predetermined performance. In vehicle-mounted lithium-ion secondary batteries, multiple lithium-ion secondary batteries 10 are stacked to form a battery module.
[0054] [Effectiveness verification experiment] An experiment was carried out to confirm the effect of suppressing damage to the separator 60 of the lithium ion secondary battery 10 according to the embodiment.
[0055] In the experiment, Examples 1 to 3 in which the temperature of the drying process was determined based on the position difference S, and Comparative Examples 1 and 2 in which the temperature of the drying process was not determined based on the position difference S were prepared, and the occurrence of tear G in the separator 60 was confirmed.
[0056] In Example 1, the position difference S was 1 [mm], the cell drying temperature was 110 [°C], and the drying time was 30 [min]. In Example 2, the position difference S was 2 [mm], the cell drying temperature was 100 [°C], and the drying time was 45 [min]. In Example 3, the position difference S was 3 [mm], the cell drying temperature was 85 [°C], and the drying time was 60 [min]. In Comparative Example 1, the position difference S was 1 [mm], the cell drying temperature was 85 [°C], and the drying time was 70 [min]. In Comparative Example 2, the position difference S was 3 [mm], the cell drying temperature was 105 [°C], and the drying time was 40 [min].
[0057] No separator tear G occurred in Examples 1 to 3. No separator tear G occurred in Comparative Example 1. On the other hand, in Comparative Example 1, separator tear G occurred.
[0058] [Effect] The manufacturing method of the lithium ion secondary battery 10 of the embodiment is a manufacturing method of the lithium ion secondary battery 10 having a wound body 30 in which a positive electrode sheet 50 as an electrode sheet, a negative electrode sheet 40 as an electrode sheet, and a separator 60 are wound in a stacked state, and includes a position difference measurement step of measuring a position difference S between one widthwise end 40A of the negative electrode sheet 40 arranged on the innermost side of the wound body 30 among the electrode sheets and one widthwise end 60A of the separator 60 protruding in the width direction from the negative electrode sheet 40, and a drying step of drying the wound body 30 at a drying temperature determined based on the position difference S (see FIG. 4).
[0059] Incidentally, in the drying process for drying the wound body 30, the separator 60 may shrink, and the separator 60 provided in contact with the negative electrode sheet 40 on the innermost periphery side may be damaged.
[0060] Here, it has been found that the shrinkage amount H of the separator 60 is related to the position difference S and the drying temperature. By drying the wound body 30 at a drying temperature determined based on the position difference S, the wound body 30 is dried at a drying temperature according to the position difference S. Therefore, the shrinkage amount H of the separator 60 is adjusted. As a result, damage to the separator 60 provided in contact with the negative electrode sheet 40 on the innermost periphery of the wound body 30 can be suppressed.
[0061] In the manufacturing method of the lithium ion secondary battery 10 of the embodiment, in the position difference measuring step, the position difference S is measured at a position corresponding to the R portion 30A of the wound body 30 (see FIG. 4).
[0062] By measuring the position difference S at a position corresponding to the R portion 30A of the wound body 30, the position difference S is measured at a sharp portion of the wound negative electrode sheet 40 where the separator 60 is easily damaged. Therefore, the shrinkage amount H of the separator 60 is adjusted in the portion where the separator 60 is easily damaged. As a result, damage to the separator 60 can be suppressed in the portion where the separator 60 is easily damaged.
[0063] In the manufacturing method of the lithium ion secondary battery 10 of the embodiment, the smaller the position difference S is, the higher the drying temperature is set (see FIG. 8(A)).
[0064] By setting a higher drying temperature as the position difference S is smaller, the wound body 30 having a small position difference S is dried at a high drying temperature. Therefore, damage to the separator 60 can be suppressed and the drying time can be shortened.
[0065] In the manufacturing method of the lithium ion secondary battery 10 of the embodiment, the drying temperature is set lower as the position difference S is larger (see FIG. 8(A)).
[0066] By setting a lower drying temperature as the position difference S increases, the wound body 30 having a large position difference S is dried at a lower temperature. Therefore, even if the wound body 30 has a large position difference S, it is possible to dry the separator 60 while suppressing damage to the separator 60.
[0067] The lithium ion secondary battery of the present invention has been described above based on the above embodiment. However, the specific configuration is not limited to this embodiment, and design changes and the like are permitted as long as they do not deviate from the gist of the invention according to each claim of the claims.
[0068] In the above embodiment, an example has been shown in which the electrode sheet arranged on the innermost periphery of the wound body 30 is the negative electrode sheet 40. However, the electrode sheet arranged on the innermost periphery of the wound body may be the positive electrode sheet. In this case, it is sufficient to measure the position difference between one widthwise end of the positive electrode sheet arranged on the innermost periphery of the wound body and one widthwise end of the separator protruding in the width direction from the positive electrode sheet.
[0069] In the above embodiment, the wound body 30 has a flat cross section. However, the wound body is not limited to this, and may have a circular cross section.
[0070] In the above embodiment, the battery is a lithium ion secondary battery, but the battery is not limited to this and may be a battery including a wound body having a separator. [Explanation of symbols]
[0071] 10 Lithium-ion secondary battery (example of battery) 30 Wound body 30A R section 40 Negative electrode sheet (an example of an electrode sheet) 40A Width direction one end 50 Positive electrode sheet (an example of an electrode sheet) 60 Separator 60A Width direction one end S position difference
Claims
1. A method for manufacturing a battery having a wound body in which a positive electrode sheet as an electrode sheet, a negative electrode sheet as the electrode sheet, and a separator are wound in a stacked state, the method comprising the steps of: a position difference measuring step of measuring a position difference between one end in a width direction of the electrode sheet arranged on the innermost periphery side of the wound body and one end in a width direction of the separator protruding in the width direction from the electrode sheet; a drying step of drying the wound body at a drying temperature determined based on the position difference; A method for manufacturing a battery comprising the steps of:
2. In the position difference measuring step, the position difference is measured at a position corresponding to the R portion of the winding body. A method for producing the battery according to claim 1 .
3. The smaller the position difference is, the higher the drying temperature is set. A method for producing the battery according to claim 1 .
4. The larger the position difference, the lower the drying temperature is set. A method for producing the battery according to claim 1 .
Citation Information
Patent Citations
Nonaqueous secondary battery
JP2005174793A