Solid secondary battery and manufacturing method thereof
By adjusting the areas and distances of the battery layers and incorporating an insulating frame, the solid-state secondary battery effectively prevents short-circuiting and enhances cycle characteristics through uniform metal deposition and reduced resistance.
Patent Information
- Application Number
- JP2023059656
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Solid-state secondary batteries face issues with cycle characteristics due to potential short-circuiting and increased resistance caused by metal ion precipitation at the edges of the solid electrolyte and intermediate layers, leading to local side reactions and deterioration.
The areas and distances of the positive electrode active material layer, solid electrolyte layer, intermediate layer, and negative electrode layer are carefully adjusted to satisfy specific relationships, with the outer periphery of the positive electrode active material layer surrounded by an insulating frame, and an intermediate layer with controlled thickness and composition to prevent metal accumulation and ensure uniform deposition.
This configuration significantly reduces the likelihood of short-circuiting between the positive and negative electrode layers, improving cycle characteristics and storage performance by minimizing metal accumulation and maintaining uniform reactions.
Smart Images

Figure 2024146632000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a solid secondary battery and a method for producing the same. [Background technology]
[0002] In recent years, research and development into secondary batteries that contribute to energy efficiency has been conducted to ensure that more people have access to affordable, reliable, sustainable, and advanced energy. Among secondary batteries, solid-state secondary batteries using solid electrolytes have attracted particular attention because of their superiority in terms of improved safety due to the non-flammability of the solid electrolyte and higher energy density.
[0003] In a solid-state secondary battery, repeated charging and discharging may cause the precipitation of metal ions such as lithium ions used as a charge transfer medium between the solid electrolyte layer and the negative electrode layer. The precipitation of the metal may cause a decrease in the adhesion of the interface, which may result in a decrease in the performance of the solid-state secondary battery. In response to this problem, a technology is known in which a layer on which lithium metal can be precipitated is provided to cover the negative electrode current collector, and the lithium metal is precipitated approximately uniformly on the surface of the coating layer, thereby making it difficult for dead lithium to be generated (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-129159 A Summary of the Invention [Problem to be solved by the invention]
[0005] By the way, in a solid-state secondary battery, improving cycle characteristics is an issue. However, when a layer (intermediate layer) on which a metal can be deposited is provided between the solid electrolyte layer and the negative electrode current collector, if the dimensions, structural design, and process conditions are inappropriate, metal ions, which are charge transfer media, tend to precipitate at the ends of the solid electrolyte layer and the intermediate layer when charge and discharge are repeated. When metal ions precipitate at the ends of the solid electrolyte layer and the intermediate layer, the deposited metal may accumulate, causing the positive electrode layer and the negative electrode layer to short-circuit, or local side reactions may occur and the resistance may increase, possibly degrading the cycle characteristics.
[0006] The present invention has been made in view of the above circumstances, and an object thereof is to provide a solid-state secondary battery in which the positive electrode layer and the negative electrode layer are less likely to short-circuit even when charge and discharge are repeated, and a method for manufacturing the same. And, by extension, it contributes to improving energy efficiency.
Means for Solving the Problems
[0007] The inventors of the present invention have found that the above problems can be solved by adjusting the areas of the positive electrode active material layer, the solid electrolyte layer, the intermediate layer, and the negative electrode layer in a top view so as to satisfy a predetermined relationship, and have completed the present invention. Therefore, the present invention provides the following.
[0008] (1) A solid-state secondary battery comprising an electrode laminate and an exterior body that houses the electrode laminate, wherein the electrode laminate has a positive electrode layer, a negative electrode layer, a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, and an intermediate layer provided between the negative electrode layer and the solid electrolyte layer, the positive electrode layer includes a positive electrode current collector and a positive electrode active material layer, and when the area of the positive electrode active material layer in a top view is Sp, the area of the solid electrolyte layer in a top view is Ss, the area of the intermediate layer in a top view is Sm, and the area of the negative electrode layer in a top view is Sn, the relationship Sp < Sn ≦ Sm ≦ Ss is satisfied.
[0009] According to the solid secondary battery of (1), since the areas of the positive electrode active material layer, the solid electrolyte layer, the intermediate layer, and the negative electrode layer in plan view satisfy the above relationship, it is difficult for metal to accumulate at the ends of the solid electrolyte and the intermediate layer even when charge and discharge are repeated. For this reason, it becomes difficult for the positive electrode layer and the negative electrode layer to short-circuit, and the cycle characteristics are improved.
[0010] (2) When one direction parallel to the upper surface when the electrode laminate is viewed from above is defined as the first direction, the distance from the central portion to the end portion of the positive electrode active material layer in the first direction is Xp, the distance from the central portion to the end portion of the solid electrolyte layer in the first direction is Xs, the distance from the central portion to the end portion of the intermediate layer in the first direction is Xm, and the distance from the central portion to the end portion of the negative electrode layer in the first direction is Xn, the relationship Xp < Xn ≦ Xm ≦ Xs is satisfied. When a direction parallel to the upper surface and orthogonal to the first direction when the electrode laminate is viewed from above is defined as the second direction, the distance from the central portion to the end portion of the positive electrode active material layer in the second direction is Yp, the distance from the central portion to the end portion of the solid electrolyte layer in the second direction is Ys, the distance from the central portion to the end portion of the intermediate layer in the second direction is Ym, and the distance from the central portion to the end portion of the negative electrode layer in the second direction is Yn, the solid secondary battery according to (1), which satisfies the relationship Yp < Yn ≦ Ym ≦ Ys.
[0011] (2) According to the solid secondary battery of (2), since the distances from the central portion to the end portions of the positive electrode active material layer, the solid electrolyte layer, the intermediate layer, and the negative electrode layer in the first direction and the second direction satisfy the above relationship, it becomes even more difficult for metal to accumulate at the ends of the solid electrolyte layer and the intermediate layer even when charge and discharge are repeated. For this reason, it becomes even more difficult for the positive electrode layer and the negative electrode layer to short-circuit, and the cycle characteristics are further improved.
[0012] (3) The solid secondary battery according to (1) or (2), wherein the outer periphery of the positive electrode active material layer is surrounded by an insulating frame.
[0013] According to the solid secondary battery of (3), since the outer periphery of the positive electrode active material layer is surrounded by an insulating frame, even if metal accumulates at the ends of the solid electrolyte layer and the intermediate layer, it is difficult for the metal to penetrate into the positive electrode active material layer. Therefore, the positive electrode layer and the negative electrode layer are less likely to short-circuit, and the cycle characteristics are further improved.
[0014] (4) When one direction parallel to the upper surface when the electrode laminate is viewed from above is defined as the first direction, the distance from the central portion to the end portion of the insulating frame in the first direction is Xi, the distance from the central portion to the end portion of the positive electrode active material layer in the first direction is Xp, the distance from the central portion to the end portion of the solid electrolyte layer in the first direction is Xs, the distance from the central portion to the end portion of the intermediate layer in the first direction is Xm, and the distance from the central portion to the end portion of the negative electrode layer in the first direction is Xn, the relationship Xp < Xn ≦ Xm ≦ Xs < Xi is satisfied. When a direction parallel to the upper surface and orthogonal to the first direction when the electrode laminate is viewed from above is defined as the second direction, the distance from the central portion to the end portion of the insulating frame in the second direction is Yi, the distance from the central portion to the end portion of the positive electrode active material layer in the second direction is Yp, the distance from the central portion to the end portion of the solid electrolyte layer in the second direction is Ys, the distance from the central portion to the end portion of the intermediate layer in the second direction is Ym, and the distance from the central portion to the end portion of the negative electrode layer in the second direction is Yn, the solid secondary battery according to (3), which satisfies the relationship Yp < Yn ≦ Ym ≦ Ys < Yi.
[0015] (4) According to the solid secondary battery of (4), since the distances from the central portion to the end portions of the insulating frame, the positive electrode active material layer, the solid electrolyte layer, the intermediate layer, and the negative electrode layer in the first direction and the second direction satisfy the above relationships, the positive electrode layer and the negative electrode layer are even less likely to short-circuit, and the cycle characteristics are further improved.
[0016] (5) The solid secondary battery according to any one of (1) to (4), wherein the thickness of the intermediate layer in the stacking direction of the electrode laminate is 5 μm or less.
[0017] According to the solid-state secondary battery of (5), since the thickness of the intermediate layer is 5 μm or less, the deposition position of the metal, which is the charge transfer medium during charging, can be between the intermediate layer and the negative electrode layer. This can greatly reduce the frequency of direct contact between the electrolyte layer and the deposited metal, suppressing local deterioration of the electrolyte layer and current concentration, and improving cycle characteristics and storage characteristics. In addition, a relatively elastic intermediate layer can be arranged between the hard electrolyte layer and the deposited metal, making it easier to follow the expansion and contraction caused by the deposition and dissolution of the metal, allowing for a uniform reaction in the in-plane and thickness directions, resulting in reduced resistance and improved cycle characteristics.
[0018] (6) The solid secondary battery according to any one of (1) to (5), wherein the intermediate layer contains metal nanoparticles and amorphous carbon.
[0019] According to the solid secondary battery of (6), the electronic conductivity of the intermediate layer can be ensured, and the particles constituting the intermediate layer and the charge transfer medium can be prevented from reacting with each other to form an alloy.
[0020] (7) The solid secondary battery according to any one of (1) to (6), wherein a ratio of a thickness of the positive electrode layer to a thickness of the negative electrode layer in a discharged state is 1.9 or more.
[0021] According to the solid-state secondary battery of (7), since the ratio of the thickness of the positive electrode layer to the thickness of the negative electrode layer is the above value, it is possible to ensure a clearance between the electrode laminate and the exterior body. By ensuring the clearance, it is possible to prevent the electrode laminate from excessively contacting the exterior body or the tab lead-out portion that leads the positive electrode tab and the negative electrode tab to the outside. In addition, when the electrode laminate expands and contracts due to charging and discharging, the positive electrode tab and the negative electrode tab can easily follow the expansion and contraction of the electrode laminate.
[0022] (8) The solid secondary battery according to any one of (1) to (7), further comprising a restraining member that applies a restraining force to the electrode laminate in a stacking direction of the electrode laminate, and where an area of the restraining member in a top view is Sr, the relationship Sn≦Sr is satisfied.
[0023] In the solid-state secondary battery of (8), the electrode laminate is restrained by a restraining member that satisfies the above-mentioned relationship, so that metal can be uniformly deposited on the surface of the negative electrode layer, and metal is less likely to accumulate at the ends of the solid electrolyte layer and the intermediate layer, making it more difficult for the positive electrode layer and the negative electrode layer to short-circuit, and improving cycle characteristics.
[0024] (9) A method for manufacturing a solid secondary battery, comprising: preparing a cathode layer including a cathode current collector and a cathode active material layer; forming a solid electrolyte layer on a surface of the cathode active material layer of the cathode layer; forming an intermediate layer on a surface of the solid electrolyte layer opposite to the cathode active material layer side; and forming a negative electrode layer on a surface of the intermediate layer opposite to the solid electrolyte layer side.
[0025] According to the method for producing a solid secondary battery of (9), after the intermediate layer is formed on the surface of the solid electrolyte layer, the negative electrode layer is formed on the surface of the intermediate layer, so that a solid secondary battery in which the areas of the solid electrolyte layer, the intermediate layer, and the negative electrode layer in a top view satisfy the relationship Sn≦Sm≦Ss can be produced in an industrially advantageous manner. Effect of the Invention
[0026] According to the present invention, it is possible to provide a solid-state secondary battery in which the positive electrode layer and the negative electrode layer are unlikely to short-circuit even after repeated charging and discharging, and a method for producing the same. [Brief description of the drawings]
[0027] [Figure 1] FIG. 2 is a top view of an electrode stack of a solid secondary battery according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II of FIG. [Diagram 3] 3 is a cross-sectional view showing a charged state of the electrode stack shown in FIG. 2. [Figure 4] FIG. 1 is a cross-sectional view of a solid secondary battery according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Hereinafter, embodiments of the present invention will be described with reference to the drawings. However, the embodiments described below are merely examples of the present invention, and the present invention is not limited to the following.
[0029] FIG. 1 is a top view of an electrode laminate of a solid secondary battery according to an embodiment of the present invention. FIG. 2 is a cross-sectional view taken along line II-II in FIG. 1, and FIG. 3 is a cross-sectional view showing the charged state of the electrode laminate shown in FIG. 2. FIG. 4 is a cross-sectional view of a solid secondary battery having the electrode laminate shown in FIGS. 1 to 3. In FIGS. 1 to 4, the X direction indicated by the arrow X is a direction (first direction) parallel to the upper surface of the electrode laminate when viewed from above. The Y direction indicated by the arrow Y is a direction (second direction) parallel to the upper surface of the electrode laminate when viewed from above and perpendicular to the X direction. The Z direction indicated by the arrow Z is the stacking direction of the electrode laminate.
[0030] The solid secondary battery 100 of this embodiment includes an electrode laminate 1, as shown in FIG. As shown in Figs. 1 to 3, the electrode laminate 1 is a laminate in which a positive electrode layer 10, a solid electrolyte layer 20, an intermediate layer 30, and a negative electrode layer 40 are laminated in this order. The positive electrode layer 10 includes a positive electrode current collector 11 and a positive electrode active material layer 12. The outer periphery of the positive electrode active material layer 12 is surrounded by an insulating frame 15. The negative electrode layer 40 includes a negative electrode current collector 41. The electrode laminate 1 shown in Figs. 1 and 2 is in a discharged state, and the electrode laminate 1 shown in Fig. 3 is in a charged state. The negative electrode layer 40 in a charged state has a metal precipitate layer 42 formed by precipitation of metal ions, which are a charged negative electrode active material, on the surface of the negative electrode current collector 41 on the intermediate layer 30 side. The metal precipitate layer 42 acts as a negative electrode active material layer and releases metal ions during discharge. The thickness of the negative electrode layer 40 of the electrode laminate 1 changes with charging and discharging.
[0031] 1, the electrode laminate 1 has a rectangular shape in which the X direction is longer than the Y direction when viewed from above. The electrode laminate 1 may have a square or circular shape when viewed from above.
[0032] When the area of the upper surface view of the positive electrode active material layer 12 is Sp, the area of the upper surface view of the solid electrolyte layer 20 is Ss, the area of the upper surface view of the intermediate layer 30 is Sm, and the area of the upper surface view of the negative electrode layer 40 is Sn, the electrode laminate 1 satisfies the relationship of Sp < Sn ≤ Sm ≤ Ss. In this embodiment, the relationship between the areas of the respective layers is set to be Sp < Sn = Sm < Ss. The relationship between the areas of the respective layers may be Sp < Sn < Sm = Ss, or may be Sp < Sn = Sm = Ss, or Sp < Sn < Sm < Ss. By the areas of the respective layers satisfying the above relationship, in the electrode laminate 1 in the upper surface view, the end portion of the positive electrode active material layer 12 is located most inward, and the end portions of the other layers (solid electrolyte layer 20, intermediate layer 30, negative electrode layer 40) are located outside the end portion of the positive electrode active material layer 12. In the electrode laminate 1 having such a configuration, since the end portion of the positive electrode active material layer 12 and the end portions of the other layers are at positions separated from each other, metal ions (charge transfer media) released from the positive electrode active material layer 12 during charging are less likely to precipitate on the end portions of the other layers. Therefore, even when charge and discharge are repeated, it becomes difficult for metal to accumulate on the end portions of the solid electrolyte layer 20 and the intermediate layer 30. The ratio Sn / Sp of the area Sn of the negative electrode layer 40 to the area Sp of the positive electrode active material layer 12 may be, for example, in the range of 1.05 to 1.45. The ratio Sm / Sp of the area Sm of the intermediate layer 30 to the area Sp of the positive electrode active material layer 12 may be, for example, in the range of 1.10 to 1.45. The ratio Ss / Sp of the area Ss of the solid electrolyte layer 20 to the area Sp of the positive electrode active material layer 12 may be, for example, in the range of 1.25 to 2.00.
[0033] In the electrode laminate 1, it is preferable that the distances from the central portion C to the end portions in the X direction (first direction) of the insulating frame 15 and each layer satisfy the relationship of Xp < Xn ≤ Xm ≤ Xs < Xi. Xp is the distance from the central portion C to the end portion in the X direction of the positive electrode active material layer 12, Xn is the distance from the central portion C to the end portion in the X direction of the negative electrode layer 40, Xm is the distance from the central portion C to the end portion in the X direction of the intermediate layer 30, Xs is the distance from the central portion C to the end portion in the X direction of the solid electrolyte layer 20, and Xi is the distance from the central portion C to the end portion in the X direction of the insulating frame 15. In this embodiment, the relationship of the distances is Xp < Xn = Xm < Xs < Xi. The relationship of the distances may be Xp < Xn < Xm = Xs < Xi, Xp < Xn = Xm = Xs < Xi, or Xp < Xn < Xm < Xs < Xi.
[0034] Further, it is preferable that the distances from the central portion C to the end portions in the Y direction (second direction) of the insulating frame 15 and each layer satisfy the relationship of Yp < Yn ≤ Ym ≤ Ys < Yi. Yp is the distance from the central portion C to the end portion in the Y direction of the positive electrode active material layer 12, Yn is the distance from the central portion to the end portion in the Y direction of the negative electrode layer 40, Ym is the distance from the central portion C to the end portion in the Y direction of the intermediate layer 30, Ys is the distance from the central portion C to the end portion in the Y direction of the solid electrolyte layer 20, and Yi is the distance from the central portion C to the end portion in the Y direction of the insulating frame 15. In this embodiment, the relationship of the distances is Yp < Yn = Ym < Ys < Yi. The relationship of the distances may be Yp < Yn < Ym = Ys < Yi, Yp < Yn = Ym = Ys < Yi, or Yp < Yn < Ym < Ys < Yi.
[0035] By satisfying Xp < Xn < Xi for the distance in the X direction and Yp < Yn < Yi for the distance in the Y direction, the solid electrolyte layer 20 can be densified, and the intrusion of metal from the end of the solid electrolyte layer 20 can be suppressed. Further, by satisfying Xp < Xn ≦ Xm ≦ Xs for the distance in the X direction and Yp < Yn ≦ Ym ≦ Ys for the distance in the Y direction, the solid electrolyte layer 20 and the metal deposition layer 42 do not directly contact even at the end of the solid electrolyte layer 20. Therefore, the infiltration of metal into the solid electrolyte layer 20 and metal deposition can be suppressed, and the reduction decomposition of the solid electrolyte layer 20 can be suppressed. Furthermore, by satisfying the relationship of Xp < Xn ≦ Xm ≦ Xs < Xi for the distance in the X direction and Yp < Yn ≦ Ym ≦ Ys < Yi for the distance in the Y direction, even if metal accumulates at the end of the solid electrolyte layer 20 or the intermediate layer 30, the metal is less likely to penetrate into the positive electrode active material layer. Moreover, by satisfying the above relationship, when the electrode laminate 1 is pressed in the stacking direction to densify the electrode laminate 1, the influence of the thickness step between the positive electrode active material layer 12 and the insulating frame 15 can be reduced, and the entire solid electrolyte layer 20 facing the negative electrode layer 40 can be densified.
[0036] The positive electrode current collector 11 is not particularly limited in terms of material and shape as long as it has a function of collecting current of the positive electrode layer 10. The area of the positive electrode current collector 11 in a top view is preferably the same as or larger than that of the positive electrode active material layer 12. Examples of the material of the positive electrode current collector 11 include aluminum, aluminum alloy, stainless steel, nickel, iron, and titanium, among which aluminum, aluminum alloy, and stainless steel are preferable. Examples of the shape of the positive electrode current collector 11 include a foil shape and a plate shape.
[0037] The positive electrode active material layer 12 contains at least one kind of positive electrode active material. The positive electrode active material is not particularly limited, and those used in the positive electrode layer of a general solid secondary battery can be used. As the positive electrode active material, for example, a layered active material containing lithium, a spinel-type active material, an olivine-type active material, etc. can be used. Specific examples of the positive electrode active material include lithium cobaltate (LiCoO2), lithium nickelate (LiNiO2), LiNi pMn q Co r O2(p+q+r=1), LiNi p Al q Co r O2(p+q+r=1), lithium manganese oxide (LiMn2O4), Li 1+x Mn 2-x-y Examples of such materials include Li-Mn spinel substituted with different elements represented by MO4 (x+y=2, M=at least one selected from Al, Mg, Co, Fe, Ni, and Zn), lithium titanate (oxide containing Li and Ti), and lithium metal phosphate (LiMPO4, M=at least one selected from Fe, Mn, Co, and Ni).
[0038] The positive electrode active material layer 12 may optionally contain a solid electrolyte in order to improve the charge transfer medium conductivity. It may also optionally contain a conductive assistant in order to improve the conductivity. Furthermore, it may also optionally contain a binder in order to achieve flexibility. There are no particular limitations on the solid electrolyte, conductive assistant, and binder, and those used in the positive electrode layer of a general solid secondary battery may be used.
[0039] The insulating frame 15 has a volume resistivity of 1×10 at 20°C. 12 The insulating frame 15 may have a resistivity of Ω·cm or more. The insulating frame 15 may be an organic material or an inorganic material. Examples of the material of the insulating frame 15 include rubber, glass, resin (polyimide, polybenzimidazole, polyamideimide, polyetherimide, polyacetal, polyphenylene sulfide, polyetheretherketone, tetrafluoroethylene, 6-polyamide (6-nylon), ultra-high molecular weight polyethylene, polyethylene, polypropylene, polyvinyl chloride resin, polystyrene, polyethylene terephthalate, ABS resin, etc.), and ceramics (alumina, zirconia, silicon nitride, aluminum nitride, mullite, steatite, magnesia, sialon, macerite, etc.). The insulation frame 15 preferably has a dielectric breakdown voltage per unit thickness of 10 kV / mm or more, and more preferably has a dielectric breakdown voltage of 100 kV / mm or more. The material of the insulating frame 15 may be a single material or a composite material, and may contain a small amount of binder or additive.
[0040] The solid electrolyte layer 20 is a layer laminated between the positive electrode layer 10 and the negative electrode layer 40. The solid electrolyte layer 20 contains at least one type of solid electrolyte material. The solid electrolyte layer 20 can conduct a charge transfer medium between the positive electrode layer 10 and the negative electrode layer 40 via the solid electrolyte material contained in the solid electrolyte layer 20.
[0041] The solid electrolyte material is not particularly limited as long as it has charge transfer medium conductivity. For example, a sulfide solid electrolyte material, an oxide solid electrolyte material, a nitride solid electrolyte material, a halide solid electrolyte material, etc. can be used.
[0042] Examples of sulfide solid electrolyte materials include Li2S-P2S5, Li2S-P2S5-LiI, etc. The above description of "Li2S-P2S5" means a sulfide solid electrolyte material made using a raw material composition containing Li2S and P2S5, and the same applies to other similar descriptions. The sulfide solid electrolyte material may have an argyrodite-type crystal structure.
[0043] Examples of oxide solid electrolyte materials include NASICON-type oxides, garnet-type oxides, perovskite-type oxides, etc. Examples of NASICON-type oxides include oxides containing Li, Al, Ti, P, and O (e.g., Li 1.5 Al 0.5 Ti 1.5 (PO4)3). Examples of garnet-type oxides include oxides containing Li, La, Zr, and O (e.g., Li7La3Zr2O 12 Examples of perovskite oxides include oxides containing Li, La, Ti, and O (for example, LiLaTiO3).
[0044] The solid electrolyte layer 20 may contain a binder. There are no particular limitations on the binder, and any binder that is used in solid electrolyte layers of general solid secondary batteries can be used.
[0045] The porosity of the solid electrolyte layer 20 is lower than that of the intermediate layer 30 described later, for example, less than 10%. The particle size of the solid electrolyte material constituting the solid electrolyte layer 20 is, for example, 0.5 to 10 μm in median size (D50), and is preferably larger than that of the particles constituting the intermediate layer 30 described later.
[0046] The porosity of the solid electrolyte layer 20 can be calculated, for example, by the following formula (1): In formula (1), the "packing ratio" refers to the percentage of the density of the solid electrolyte layer after molding relative to the true density. Porosity (%)=100-Filling rate (%) (1)
[0047] The intermediate layer 30 is a layer laminated between the solid electrolyte layer 20 and the negative electrode layer 40. The intermediate layer 30 has the function of suppressing non-uniform deposition of metal ions at the interface of the negative electrode layer 40 and improving the interface adhesion.
[0048] The intermediate layer 30 preferably has electron conductivity and voids through which metal ions (e.g., lithium ions) serving as a charge transfer medium can pass. When the intermediate layer 30 has voids, when the solid secondary battery 100 is charged, the metal ions moving from the solid electrolyte layer 20 toward the negative electrode layer 40 pass through the intermediate layer 30 and are precipitated on the surface of the negative electrode current collector 41 of the negative electrode layer 40 on the intermediate layer 30 side, forming a metal precipitate layer 42 (a layer of metallic lithium). By passing through the intermediate layer 30, the metal precipitate layer 42 can be uniformly formed on the surface of the negative electrode current collector 41. In addition, by having voids, the intermediate layer 30 has flexibility capable of following the change in thickness of the negative electrode layer 40 accompanying charging and discharging. Therefore, even when the solid secondary battery 100 is repeatedly charged and discharged, the interfacial adhesion can be maintained, and the durability of the solid secondary battery 100 can be improved.
[0049] The porosity of the intermediate layer 30 is preferably higher than that of the solid electrolyte layer 20. This allows many voids through which metal ions can pass to be formed inside the intermediate layer 30, so that the metal deposit layer 42 can be more uniformly formed on the surface of the negative electrode current collector 41. In addition, the intermediate layer 30 becomes more flexible, so that the ability to follow changes in the thickness of the negative electrode layer 40 is improved. The porosity of the intermediate layer 30 can be, for example, 40 to 70%. The porosity of the intermediate layer 30 can be calculated in the same manner as the porosity of the solid electrolyte layer 20.
[0050] The thickness of the intermediate layer 30 may be 5 μm or less. By making the thickness of the intermediate layer 30 5 μm or less, the deposition position of the metal, which is the charge transfer medium during charging, can be between the intermediate layer 30 and the negative electrode layer 40. This can greatly reduce the frequency of direct contact between the solid electrolyte layer 20 and the deposited metal, suppressing local deterioration and current concentration of the solid electrolyte layer 20, and improving cycle characteristics and storage characteristics. In addition, the relatively elastic intermediate layer 30 can be disposed between the hard solid electrolyte layer 20 and the deposited metal, making it easier to follow the expansion and contraction caused by the deposition and dissolution of the metal, allowing a uniform reaction in the in-plane and thickness directions, thereby obtaining the effects of reducing resistance and improving cycle characteristics. In order to obtain the effects of further reducing resistance and improving cycle characteristics, the thickness of the intermediate layer may be 3 μm or less, or may be within the range of 1 to 3 μm.
[0051] The intermediate layer 30 preferably contains amorphous carbon and metal nanoparticles. The intermediate layer 30 may further contain a binder as a binding material to maintain the structure.
[0052] Unlike graphite, amorphous carbon is less likely to react with metals such as lithium and form an alloy, and therefore can suppress the formation of dendrites and improve the cycle characteristics of solid secondary batteries. The amorphous carbon may be either easily graphitized carbon (soft carbon) or difficultly graphitized carbon (hard carbon). In addition, the amorphous carbon may be any carbon allotrope that does not show a clear crystalline state, and may be an aggregate of fine graphite crystals. Specific examples of amorphous carbon include carbon blacks such as acetylene black, furnace black, and ketjen black, coke, activated carbon, CNT (carbon nanotube), fullerene, and graphene.
[0053] Examples of metal nanoparticles include metal nanoparticles of tin (Sn), silicon (Si), zinc (Zn), magnesium (Mg), gold (Au), platinum (Pt), palladium (Pd), silver (Ag), aluminum (Al), bismuth (Bi), and antimony (Sb). The content of the metal nanoparticles in the intermediate layer 30 is preferably more than 0 mass% and 30 mass% or less. When the intermediate layer 30 contains metal nanoparticles, the electronic conductivity of the intermediate layer 30 can be increased, and the metal precipitate layer 42 can be generated more uniformly. In addition, since the metal nanoparticles have a high Young's modulus compared to amorphous carbon, the structure of the intermediate layer 30 can be maintained even when high-pressure pressing is performed when manufacturing the solid secondary battery 100.
[0054] The particle diameter of the amorphous carbon and metal nanoparticles is preferably smaller than that of the solid electrolyte material. This allows the intermediate layer 30 to enter the gap between the solid electrolyte materials constituting the interface of the solid electrolyte layer 20, thereby increasing the contact area between the solid electrolyte layer 20 and the intermediate layer 30 and improving the adhesion. The particle diameter of the amorphous carbon may be, for example, in the range of 0.02 to 0.10 μm in terms of median diameter (D50). The particle diameter of the metal nanoparticles may be, for example, in the range of 0.02 to 0.20 μm in terms of median diameter (D50).
[0055] The binder is preferably one that can improve the adhesion between the particles constituting the intermediate layer 30 and between the intermediate layer 30 and the solid electrolyte layer 20. There are no particular limitations on the binder, and it is possible to use binders that are generally used in solid secondary batteries. Examples of binders include acrylic acid-based polymers, cellulose-based polymers, styrene-based polymers, vinyl acetate-based polymers, urethane-based polymers, fluoroethylene-based polymers, and PVDF-based polymers.
[0056] The negative electrode current collector 41 is a laminate having a current collecting substrate 41a and a metal layer 41b laminated on the surface of the current collecting substrate 41a. There are no particular limitations on the material or shape of the current collecting substrate 41a as long as it has the function of collecting current from the negative electrode layer 40. Examples of materials for the current collecting substrate 41a include nickel, copper, and stainless steel. Examples of the shape of the current collecting substrate 41a include a foil shape, a plate shape, and the like.
[0057] The metal layer 41b is not particularly limited in material or shape as long as it has a function of densely precipitating a charge transfer medium such as lithium ions. When the charge transfer medium is lithium ions, the material of the metal layer 41b can be metallic lithium or a metal that forms an alloy with lithium. Examples of metals that form an alloy with lithium include Mg, Si, Au, Ag, In, Ge, Sn, Pb, Al, and Zn. The metal that forms the metal layer 41b may be in the form of a powder or a thin film. By using the negative electrode current collector 41 having this metal layer 41b, a uniform metal deposition layer 42 can be formed on the surface of the negative electrode current collector 41. The metal layer 41b may be omitted and lithium ions may be directly deposited on the current collector substrate 41a.
[0058] 4, the electrode laminate 1 is housed in an exterior body 50. A pair of restraining members 60 for applying a restraining force to the electrode laminate 1 are disposed on the outer surface of the exterior body 50. The solid secondary battery 100 has a positive electrode tab (not shown) having one end connected to the positive electrode current collector 11 and the other end protruding outward, and a negative electrode tab (not shown) having one end connected to the negative electrode current collector 41 and the other end protruding outward.
[0059] The exterior body 50 is expandable and contractable in accordance with the change in thickness of the negative electrode due to charging and discharging. A laminate film can be used as the material of the exterior body 50. As the laminate film, a laminate film having a three-layer structure in which an inner resin layer, a metal layer, and an outer resin layer are laminated in this order from the inside can be used. The outer resin layer may be, for example, a polyamide (nylon) layer or a polyethylene terephthalate (PET) layer, the metal layer may be, for example, an aluminum layer, and the inner resin layer may be, for example, a polyethylene layer or a polypropylene layer. In addition, an adhesive layer may be included between each layer, and the layers may be integrated by heat, pressure, or the like.
[0060] In order to ensure clearance inside the exterior body 50, the ratio of the thickness of the positive electrode layer 10 to the thickness of the negative electrode layer 40 (the thickness of the negative electrode current collector 41) in a discharged state (thickness of the positive electrode layer 10 / thickness of the negative electrode layer 40) may be 1.9 or more.
[0061] The restraining member 60 is intended to apply a restraining force in the stacking direction of the electrode laminate 1. When the area of the restraining member 60 in a top view is Sr and the area of the negative electrode layer 40 in a top view is Sn, it is preferable that the relationship Sn≦Sr is satisfied. When the area Sr of the restraining member 60 satisfies this relationship, the restraining force acts uniformly on the surface of the negative electrode layer 40. Therefore, during charging, metal ions can be uniformly precipitated on the surface of the negative electrode layer 40, so that metal is less likely to accumulate at the ends of the solid electrolyte layer 20 and the intermediate layer 30. There is no particular restriction on the material of the restraining member 60, and a material generally used for solid-state batteries can be used. The restraining force of the restraining member 60 on the electrode laminate 1 may be within a range of, for example, 0.1 to 10 MPa.
[0062] Next, a method for manufacturing the solid secondary battery 100 of this embodiment will be described. The electrode laminate 1 can be produced, for example, by a method including a positive electrode layer preparation step, a solid electrolyte layer formation step, an intermediate layer formation step, and a negative electrode layer formation step.
[0063] The positive electrode layer preparation step is a step of preparing a positive electrode layer 10. The positive electrode layer 10 can be prepared, for example, by forming a positive electrode active material layer 12 on the surface of a positive electrode current collector 11. The positive electrode active material layer 12 can be formed by applying a positive electrode active material layer slurry and drying it. The positive electrode active material layer slurry can be a dispersion of a positive electrode active material containing a solvent, a positive electrode active material, and optionally a conductive assistant and a binder. In the positive electrode layer preparation step, it is preferable to arrange an insulating frame 15 so as to surround the outer periphery of the positive electrode active material layer 12.
[0064] The solid electrolyte layer forming step is a step of forming a solid electrolyte layer 20 on the surface of the positive electrode active material layer 12 of the positive electrode layer 10. As a method for forming the solid electrolyte layer 20, a method of directly applying the solid electrolyte layer slurry to the surface of the positive electrode active material layer 12 and drying it, or a method of applying the solid electrolyte layer slurry to the surface of a separately prepared support sheet and drying it to form a solid electrolyte layer 20, and transferring the solid electrolyte layer 20 to the surface of the positive electrode active material layer 12 at a predetermined pressure can be used. As the solid electrolyte layer slurry, for example, a dispersion liquid of a solid electrolyte containing a solvent, a solid electrolyte, and an optional binder can be used. As a method for forming the solid electrolyte layer 20, a method of integrating the solid electrolyte layer with a substrate, making it independent, and then arranging it on the positive electrode layer can be used. As the substrate, for example, a nonwoven fabric or a woven fabric can be used. As the material of the substrate, a polyester resin such as PET can be used.
[0065] The intermediate layer forming step is a step of forming an intermediate layer 30 on the surface of the solid electrolyte layer 20 opposite to the positive electrode active material layer 12 side. The intermediate layer 30 can be formed by directly applying an intermediate layer slurry to the surface of the solid electrolyte layer 20 and drying it, or by applying the intermediate layer slurry to the surface of a separately prepared support sheet, drying it, and transferring the intermediate layer 30 to the surface of the solid electrolyte layer 20 at a predetermined pressure. As the intermediate layer slurry, for example, a dispersion of an intermediate layer forming material containing a solvent, metal nanoparticles, amorphous carbon, and an optional binder can be used.
[0066] The negative electrode layer forming step is a step of forming the negative electrode layer 40 on the surface of the intermediate layer 30 opposite to the solid electrolyte layer 20. As a method for forming the negative electrode layer 40, a method in which a previously prepared negative electrode current collector 41 is disposed on the surface of the intermediate layer 30 can be used.
[0067] In this manner, an electrode laminate 1 is obtained in which the positive electrode layer 10, the solid electrolyte layer 20, the intermediate layer 30, and the negative electrode layer 40 are laminated in this order. The obtained electrode laminate 1 may be optionally pressed in the lamination direction to increase the density of the electrode laminate 1.
[0068] The solid secondary battery 100 can be fabricated as follows. One end of the positive electrode tab is connected to the positive electrode current collector 11 of the obtained electrode laminate 1, and one end of the negative electrode tab is connected to the negative electrode current collector 41. Next, the electrode laminate 1 is housed in an exterior body 50 so that the other ends of the positive electrode tab and the negative electrode tab protrude, and the exterior body 50 is sealed. Then, a restraining member 60 is disposed on the outer surface of the exterior body 50, and the electrode laminate 1 is restrained with a predetermined restraining force.
[0069] The intermediate layer forming step and the negative electrode layer forming step may be performed simultaneously. For example, the intermediate layer 30 of an intermediate layer-negative electrode layer laminate in which the intermediate layer 30 and the negative electrode layer 40 are integrated and made independent in advance may be disposed on the surface of the solid electrolyte layer 20. The intermediate layer-negative electrode layer laminate can be obtained, for example, by applying an intermediate layer slurry to the surface of the negative electrode current collector 41 and drying it to form the intermediate layer 30.
[0070] In the solid secondary battery 100 of this embodiment configured as described above, the areas of the positive electrode active material layer 12, the solid electrolyte layer 20, the intermediate layer 30, and the negative electrode layer 40 in a top view satisfy the above relationship, so that metal is less likely to accumulate at the ends of the solid electrolyte layer 20 and the intermediate layer 30 even after repeated charging and discharging. As a result, the positive electrode layer 10 and the negative electrode layer 40 are less likely to short-circuit, improving cycle characteristics.
[0071] Furthermore, according to the solid secondary battery 100 of this embodiment, the distances from the center to the ends in the X and Y directions of the positive electrode active material layer 12, the solid electrolyte layer 20, the intermediate layer 30, and the negative electrode layer 40 satisfy the above-mentioned relationships, so that even if charging and discharging are repeated, metal is less likely to accumulate at the ends of the solid electrolyte layer 20 and the intermediate layer 30. As a result, the positive electrode layer 10 and the negative electrode layer 40 are less likely to short-circuit, and the cycle characteristics are further improved.
[0072] Furthermore, according to the solid secondary battery 100 of this embodiment, the outer periphery of the positive electrode active material layer 12 is surrounded by the insulating frame 15, and further, the distances from the center to the ends in the X direction and Y direction of the insulating frame 15, the positive electrode active material layer 12, the solid electrolyte layer 20, the intermediate layer 30, and the negative electrode layer 40 satisfy the above-mentioned relationships, so that even if metal accumulates at the ends of the solid electrolyte layer 20 and the intermediate layer 30, the metal is unlikely to find its way into the positive electrode active material layer 12. As a result, the positive electrode layer 10 and the negative electrode layer 40 are less likely to short-circuit, and cycle characteristics are further improved.
[0073] Furthermore, according to the manufacturing method of the solid secondary battery 100 of the present embodiment, the solid electrolyte layer 20, the intermediate layer 30, and the negative electrode layer 40 are formed in this order on the positive electrode active material layer 12, so that a solid secondary battery in which the areas of the solid electrolyte layer 20, the intermediate layer 30, and the negative electrode layer 40 in a top view satisfy the relationship Sn≦Sm≦Ss can be manufactured in an industrially advantageous manner.
[0074] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment. For example, in the solid secondary battery 100 of this embodiment, the outer periphery of the positive electrode active material layer 12 is surrounded by an insulating frame 15, but the insulating frame 15 may be omitted. In this case, it is preferable that the end of the surface of the solid electrolyte layer 20 on the positive electrode active material layer 12 side, which is not in contact with the positive electrode active material layer 12, is covered with an insulating material to prevent metal from being deposited between the end of the solid electrolyte layer 20 and the positive electrode active material layer 12. It is also preferable that the thickness of the insulating material of the positive electrode active material layer 12 and the end are made equal to each other so that no steps are generated when the electrode laminate 1 is pressed to densify it.
[0075] In addition, in the solid secondary battery 100 of this embodiment, the metal precipitate layer 42 is used as the negative electrode active material layer, but the negative electrode active material layer is not limited thereto. The negative electrode active material layer may be a layer containing a negative electrode active material capable of absorbing and releasing a charge transfer medium such as lithium ions. In this case, the negative electrode active material layer may be disposed on the surface of the current collecting substrate 41a. As the negative electrode active material, a material used in the negative electrode of a general solid secondary battery can be used. When the charge transfer medium is lithium ions, examples of the negative electrode active material include lithium transition metal oxides such as lithium titanate, transition metal oxides such as TiO2, Nb2O3 and WO3, Si, SiO, metal sulfides, metal nitrides, and carbon materials such as artificial graphite, natural graphite, graphite, soft carbon and hard carbon. The negative electrode active material layer may optionally contain a solid electrolyte from the viewpoint of improving the conductivity of the charge transfer medium. In addition, it may optionally contain a conductive assistant to improve the conductivity. Furthermore, it may optionally contain a binder from the viewpoint of expressing flexibility. As for the solid electrolyte, the conductive assistant, and the binder, those generally used in solid secondary batteries can be used. EXAMPLES
[0076] The present invention will be described in detail below using examples, but the present invention is not limited to these examples.
[0077] <Example 1> [Preparation of positive electrode layer] As a positive electrode current collector, a rectangular aluminum foil having a length of 30.0 mm in the X direction, a length of 30.0 mm in the Y direction, and a thickness of 15 μm was prepared. A mixture of 80 parts by mass of lithium nickel cobalt manganese composite oxide (NCM622) as the positive electrode active material, 17 parts by mass of an argyrodite-type sulfide solid electrolyte as the solid electrolyte, 2 parts by mass of carbon black as the conductive assistant, and 1 part by mass of an SBR (styrene butadiene rubber) binder as the binder was used. The mixture was dispersed in 43 parts by mass of butyl butyrate to prepare a positive electrode active material layer slurry. The obtained positive electrode active material layer slurry was applied to the center of the positive electrode current collector in a size of 20.0 mm in the X direction, 20.0 mm in the Y direction, and 27 mg / cm2 in weight per unit area after drying. 2 The positive electrode layer was thus produced by applying the positive electrode active material thereto using a bar coater method so as to obtain a positive electrode active material layer.
[0078] [Installation of insulating frame] An insulating sheet having a length of 30.0 mm in the X direction, a length of 30.0 mm in the Y direction, and a thickness of 80 μm was prepared. An opening having a length of 20.0 mm in the X direction and a length of 20.0 mm in the Y direction was formed in the center of the insulating sheet to prepare an insulating frame. The obtained insulating frame was placed around the positive electrode active material layer.
[0079] [Preparation of solid electrolyte layer] A dispersion of an argyrodite-type sulfide solid electrolyte (median diameter: 3 μm) was applied to a support sheet and dried to obtain a sheet having a length of 27.0 mm in the X direction, a length of 27.0 mm in the Y direction, and a drying weight of 20 mg / cm. 2 The argyrodite-type sulfide solid electrolyte layer was formed so that the argyrodite-type sulfide layer formed on the support sheet was transferred to the center of the positive electrode active material layer to prepare a solid electrolyte layer.
[0080] [Creation of intermediate layer] A total of 95 parts by mass of Sn particles (median diameter: 0.07 μm) as metal nanoparticles, acetylene black (particle diameter 0.05 μm) as amorphous carbon, and 5 parts by mass of a PVDF-based binder as a binder were mixed. The resulting mixture was dispersed in 1000 parts by mass of NMP (N-methyl-2-pyrrolidone) to prepare an intermediate layer slurry. The obtained intermediate layer slurry was applied to a substrate foil by a gravure coater method in a size of 22.0 mm in the X direction, 22.0 mm in the Y direction, and 0.4 mg / cm 2 The resulting intermediate layer was transferred to the center of the solid electrolyte layer to prepare an intermediate layer.
[0081] [Preparation of negative electrode current collector] A laminated metal foil was prepared by laminating a copper foil having a thickness of 10 μm and a lithium foil having a thickness of 40 μm. This laminated metal foil was cut to a size of 21.0 mm in the Y direction × 21.0 mm in the Y direction to prepare a negative electrode current collector. The obtained negative electrode current collector was placed in the center of the intermediate layer so that the lithium foil was in contact with the intermediate layer. In this way, an electrode laminate was obtained in which the positive electrode layer, the solid electrolyte layer, the intermediate layer, and the negative electrode current collector were laminated in this order.
[0082] [Preparation of solid-state secondary batteries] The electrode laminate obtained above was pressed to increase density, and then tabs were attached to each of the positive and negative current collectors, after which the electrode laminate was housed in a bag-shaped laminate pack. The laminate pack was then sealed in an argon atmosphere. The thicknesses of each layer after pressing are shown in Tables 1 to 3.
[0083] A restraining member having a length of 21.0 mm in the X direction and a length of 21.0 mm in the Y direction was prepared. This restraining member was placed so as to face the negative electrode current collector of the electrode laminate from the surface of the laminate pack, and a restraining force of 3 MPa was applied to the electrode laminate to produce a solid secondary battery.
[0084] <Examples 2 to 5> A solid secondary battery was produced in the same manner as in Example 1, except that the dimensions of the positive electrode current collector, the positive electrode active material layer, and the insulating frame were changed to the dimensions shown in Table 1, the dimensions of the solid electrolyte layer and the intermediate layer were changed to the dimensions shown in Table 2, and the dimensions of the negative electrode current collector and the restraining member were changed to the dimensions shown in Table 3.
[0085] <Battery characteristics> The solid secondary batteries prepared in Examples 1 to 5 were subjected to a cycle test in which charging and discharging were repeated at a charging upper limit voltage of 4.3 V, a discharging lower limit voltage of 2.65 V, and a C rate of 1 / 3 C. The ratio of the discharging capacity to the charging capacity in the second cycle (discharging capacity / charging capacity×100) was calculated. The results are shown in Table 3 as the second charging and discharging efficiency.
[0086] [Table 1]
[0087] [Table 2]
[0088] [Table 3]
[0089] From the battery characteristic results shown in Table 3, it can be seen that the solid secondary batteries of Examples 1 to 5, in which the dimensions of the positive electrode active material layer, solid electrolyte layer, intermediate layer, and negative electrode current collector are all within the range of the present invention, all exhibit high second charge-discharge efficiency. [Explanation of symbols]
[0090] 1 Electrode laminate 10 Positive electrode layer 11 Positive electrode current collector 12 Cathode active material layer 15 Insulation frame 20 Solid electrolyte layer 30 Middle Class 40 Negative electrode layer 41 Negative electrode current collector 41a Current collector substrate 41b Metal layer 42 Metal deposit layer 50 Exterior body 60 Restraint member 100 Solid state secondary battery
Claims
1. The electrode stack includes an electrode laminate and an exterior body that houses the electrode laminate. the electrode stack includes a positive electrode layer, a negative electrode layer, a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, and an intermediate layer provided between the negative electrode layer and the solid electrolyte layer; the positive electrode layer includes a positive electrode current collector and a positive electrode active material layer, a top view area of the positive electrode active material layer is Sp, a top view area of the solid electrolyte layer is Ss, a top view area of the intermediate layer is Sm, and a top view area of the negative electrode layer is Sn, satisfying a relationship of Sp<Sn≦Sm≦Ss.
2. a first direction is a direction parallel to an upper surface of the electrode laminate when viewed from above, Xp is a distance from a center to an end of the positive electrode active material layer in the first direction, Xs is a distance from a center to an end of the solid electrolyte layer in the first direction, Xm is a distance from a center to an end of the intermediate layer in the first direction, and Xn is a distance from a center to an end of the negative electrode layer in the first direction, the relationship Xp<Xn≦Xm≦Xs is satisfied, 2. The solid secondary battery according to claim 1, wherein a second direction is a direction parallel to an upper surface of the electrode stack when viewed from above and perpendicular to the first direction, a distance from a center to an end of the positive electrode active material layer in the second direction is Yp, a distance from a center to an end of the solid electrolyte layer in the second direction is Ys, a distance from a center to an end of the intermediate layer in the second direction is Ym, and a distance from a center to an end of the negative electrode layer in the second direction is Yn, satisfying a relationship of Yp<Yn≦Ym≦Ys.
3. The solid secondary battery according to claim 1 , wherein an outer periphery of the positive electrode active material layer is surrounded by an insulating frame.
4. a first direction is a direction parallel to an upper surface of the electrode stack when viewed from above, a distance from a center to an end of the insulating frame in the first direction is Xi, a distance from a center to an end of the positive electrode active material layer in the first direction is Xp, a distance from a center to an end of the solid electrolyte layer in the first direction is Xs, a distance from a center to an end of the intermediate layer in the first direction is Xm, and a distance from a center to an end of the negative electrode layer in the first direction is Xn, the relationship Xp<Xn≦Xm≦Xs<Xi is satisfied, 4. The solid state secondary battery according to claim 3, wherein a second direction is a direction parallel to an upper surface of the electrode stack when viewed from above and perpendicular to the first direction, a distance from a center to an end of the insulating frame in the second direction is Yi, a distance from a center to an end of the positive electrode active material layer in the second direction is Yp, a distance from a center to an end of the solid electrolyte layer in the second direction is Ys, a distance from a center to an end of the intermediate layer in the second direction is Ym, and a distance from a center to an end of the negative electrode layer in the second direction is Yn, satisfying a relationship of Yp<Yn≦Ym≦Ys<Yi.
5. The solid secondary battery according to claim 1 , wherein the intermediate layer has a thickness of 5 μm or less in a stacking direction of the electrode stack.
6. The solid state secondary battery according to claim 1 , wherein the intermediate layer comprises metal nanoparticles and amorphous carbon.
7. 2. The solid secondary battery according to claim 1, wherein a ratio of a thickness of the positive electrode layer to a thickness of the negative electrode layer in a discharged state is 1.9 or more.
8. a restraining member that applies a restraining force to the electrode stack in a stacking direction of the electrode stack, The solid secondary battery according to claim 1 , wherein when an area of the restraining member in a top view is Sr, a relationship of Sn≦Sr is satisfied.
9. preparing a positive electrode layer including a positive electrode current collector and a positive electrode active material layer; forming a solid electrolyte layer on a surface of the positive electrode active material layer of the positive electrode layer; forming an intermediate layer on a surface of the solid electrolyte layer opposite to a positive electrode active material layer; and forming a negative electrode layer on a surface of the intermediate layer opposite to the solid electrolyte layer side.
Citation Information
Patent Citations
Nonaqueous electrolyte battery
JP2011086554A
Lithium ion secondary battery and method for manufacturing lithium ion secondary battery
JP2018181636A
Series laminate type all-solid battery
JP2019096476A
All-solid battery
JP2020098696A
Method of manufacturing solid-state battery and solid-state battery
JP2023000783A
Cited By
Battery device
WO2026224798A1