Cathode active material for lithium ion secondary battery with coating layer, solution for coating layer formation, manufacturing method of cathode active material for lithium ion secondary battery with coating layer, and all-solid lithium ion secondary battery

A coating layer of lithium metal composite oxide with specific elemental composition and coverage on the positive electrode active material addresses the capacity loss issue in all-solid lithium ion secondary batteries, ensuring stable performance through suppressed interfacial reactions and resistance formation.

JP2024146674APending Publication Date: 2024-10-15SUMITOMO METAL MINING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023093516
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-06-06
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional lithium ion secondary batteries face a decrease in battery capacity due to the formation of a high-resistance layer at the interface between the solid electrolyte and the positive electrode active material during charging and discharging, which is not effectively addressed by existing coating layers like lithium niobate or compounds containing phosphoric acid.

Method used

A coating layer composed of lithium metal composite oxide with a layered rock salt structure, containing lithium, nickel, and a pentavalent transition metal element, such as niobium, is applied to the surface of the positive electrode active material, achieving a coverage of 60% or more, which suppresses interfacial reactions and maintains battery capacity.

Benefits of technology

The proposed coating layer significantly enhances the capacity retention of all-solid lithium ion secondary batteries by preventing the formation of resistance layers and improving stability during high voltage charging, maintaining high initial discharge capacity and output characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146674000001_ABST
    Figure 2024146674000001_ABST
Patent Text Reader

Abstract

To provide cathode active material for a lithium ion secondary battery with a coating layer, which is applied to an all-solid lithium ion secondary battery using a solid electrolyte and enables suppression of reduction of battery capacity when the lithium ion secondary battery is charged / discharged repeatedly.SOLUTION: Cathode active material for a lithium ion secondary battery with a coating layer is provided, comprising a lithium metal composite oxide and a coating layer which covers at least a part of a surface of the lithium metal composite oxide at a coverage rate of 60% or more. The lithium metal composite oxide has layered rock salt structure and contains lithium (Li), nickel (N) and M elements (M) at a ratio of substance quantities Li:Ni:M=a:1-x:x in which (a) and (x) satisfy relations of 0.98≤a≤1.20 and 0≤x≤1.0 and the M elements are one or more kinds of elements excluding lithium, nickel and oxygen. The coating layer contains lithium, phosphor and Z elements and the Z elements are at least one or more kinds of pentavalent transition metal elements.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for a lithium ion secondary battery with a coating layer, a solution for forming a coating layer, a method for producing a positive electrode active material for a lithium ion secondary battery with a coating layer, and an all-solid-state lithium ion secondary battery. [Background technology]

[0002] In recent years, with the widespread use of electric vehicles, there has been a strong demand for the development of small, lightweight secondary batteries having high energy density, such as lithium-ion secondary batteries.

[0003] Currently, in typical lithium-ion secondary batteries, oxides such as LiCoO2, LiNiO2, and LiMn2O4 are used as the positive electrode active material for lithium-ion secondary batteries (hereinafter also referred to as the "positive electrode active material"). Lithium metal, lithium alloys, metal oxides, carbon, etc. are used as the negative electrode active material for lithium-ion secondary batteries. In addition, as the electrolyte, an electrolyte in which a Li salt such as LiClO4 or LiPF6 is dissolved as a supporting salt in an organic solvent such as ethylene carbonate, dimethyl carbonate, or ethyl methyl carbonate is used.

[0004] Among the components of lithium-ion secondary batteries, the electrolyte in particular is a factor that limits battery performance such as fast charging and lifespan due to its chemical properties such as heat resistance and potential window. Therefore, research and development is currently being actively conducted on all-solid-state lithium-ion secondary batteries that improve battery performance by using a solid electrolyte instead of an electrolyte.

[0005] As research and development of all-solid-state lithium-ion secondary batteries progresses, it has been proposed, for example in Patent Document 1, that sulfide-based solid electrolytes have high lithium ion conductivity and are preferable for use in all-solid-state lithium-ion secondary batteries.

[0006] However, as disclosed in Non-Patent Document 1, when a sulfide-based solid electrolyte comes into contact with an oxide positive electrode active material, a reaction occurs at the interface between the solid electrolyte and the positive electrode active material during charging and discharging, and a high resistance layer is generated, which inhibits the operation of the battery. As a result, the battery capacity decreases when the battery is repeatedly charged and discharged.

[0007] In order to suppress the formation of this high resistance layer, it has been proposed in, for example, Non-Patent Document 1 to provide a coating layer made of lithium niobate on the surface of the positive electrode active material. However, lithium niobate has a resistance of 4.6 V (vs. Li / Li + ) or higher, it decomposes, releasing oxygen and interdiffusing with the sulfur in the solid electrolyte layer to produce by-products that act as resistance, and the formation of a resistance layer may not be sufficiently prevented. In addition, mixing is likely to occur at the interface between the positive electrode active material and the coating layer, which is not sufficient to suppress the increase in resistance. For this reason, even when a coating layer made of lithium niobate is provided, the battery capacity decreases with repeated charging and discharging.

[0008] As a compound that has the effect of suppressing the mixing that occurs between the above-mentioned positive electrode active material and the coating layer, a compound containing phosphoric acid is effective, and it has been proposed in Non-Patent Document 2 and elsewhere that it is extremely stable compared to lithium niobate and the like.

[0009] However, compounds containing phosphoric acid have difficulty existing in a basic state, and when used in an acidic solution, they corrode the surface of the positive electrode active material. In addition, when used in an organic solution, P (phosphorus) is easily lost when heated, making it difficult to control the composition. For this reason, it has been difficult to form a coating layer on the surface of the positive electrode active material using compounds containing phosphoric acid. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2014-56661 A [Non-patent literature]

[0011] [Non-Patent Document 1] Narumi Ohta et al., "LiNbO3-coated LiCoO2 as cathode material for all solid-state lithium secondary batteries", Electrochemistry Communications 9 (2007) 1486-1490 [Non-Patent Document 2] William D. et al., "Interface Stability in Solid-State Batteries", Chem.Mater.2016,28,266-273 Summary of the Invention [Problem to be solved by the invention]

[0012] In view of the problems associated with the above-described conventional techniques, one aspect of the present invention aims to provide a positive electrode active material for a lithium ion secondary battery with a coating layer, which is applicable to an all-solid-state lithium ion secondary battery using a solid electrolyte and can suppress a decrease in battery capacity during repeated charging and discharging. [Means for solving the problem]

[0013] In order to solve the above problem, according to one aspect of the present invention, A lithium metal composite oxide; A coating layer that covers at least a part of the surface of the lithium metal composite oxide and has a coverage rate of 60% or more, The lithium metal composite oxide has a layered rock salt structure and contains lithium (Li), nickel (Ni), and an M element (M) in a ratio of Li:Ni:M=a:1-x:x in terms of the amount of substance, where a and x satisfy the relationships 0.98≦a≦1.20 and 0≦x≦1.0, and the M element is one or more elements excluding lithium, nickel, and oxygen, The coating layer contains lithium, phosphorus, and a Z element, and the Z element is at least one kind of pentavalent transition metal element, thereby providing a positive electrode active material for a lithium ion secondary battery with a coating layer. Effect of the Invention

[0014] According to one aspect of the present invention, it is possible to provide a positive electrode active material for a lithium ion secondary battery with a coating layer, which is applicable to an all-solid-state lithium ion secondary battery using a solid electrolyte and can suppress a decrease in battery capacity when repeatedly charged and discharged. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a cross-sectional schematic diagram of a coating layer-attached positive electrode active material for a lithium ion secondary battery according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a lithium-ion secondary battery. [Diagram 3] FIG. 3 is an explanatory diagram of a cross-sectional configuration of a test battery used for evaluating battery characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, the form for carrying out the present invention will be described with reference to the drawings. However, the present invention is not limited to the following embodiment, and various modifications and substitutions can be made to the following embodiment without departing from the scope of the present invention.

[0017] The positive electrode active material for a lithium ion secondary battery with a coating layer, the solution for forming a coating layer, the method for producing the positive electrode active material for a lithium ion secondary battery with a coating layer, and the all-solid-state lithium ion secondary battery according to one embodiment of the present invention will be described in the following order.

[0018] 1. Positive electrode active material for lithium-ion secondary batteries with coating layer 1-1. Lithium metal composite oxide 1-2.Coating layer 1-3. Other characteristics of the positive electrode active material for lithium-ion secondary batteries with a coating layer 2. Solution for forming coating layer, and method for producing positive electrode active material for lithium ion secondary battery with coating layer 3. All-solid-state lithium-ion secondary battery 3-1. Positive electrode 3-2. Negative electrode 3-3.Solid electrolyte layer 3-4. Shape and structure of secondary batteries 3-5. Battery evaluation of secondary batteries <1. Positive electrode active material with coating layer for lithium-ion secondary batteries> The inventors of the present invention have studied a positive electrode active material for a lithium ion secondary battery with a coating layer, which can be applied to an all-solid-state lithium ion secondary battery (hereinafter also referred to as a "secondary battery") using a solid electrolyte and can suppress the decrease in battery capacity when repeatedly charged and discharged. Specifically, they have conducted intensive research on a positive electrode active material for a lithium ion secondary battery with a coating layer (hereinafter also referred to as a "positive electrode active material with a coating layer") having a coating layer that can suppress an interfacial reaction with a solid electrolyte and a positive electrode active material. As a result, they have found that by coating a coating layer containing lithium, phosphorus, and Z elements on the surface of a lithium metal composite oxide, which is a positive electrode active material, in a certain amount or more so as to achieve a predetermined coverage rate, the coating layer can be applied to a secondary battery and the decrease in battery capacity when repeatedly charged and discharged can be suppressed, and have completed the present invention.

[0019] As shown in the schematic cross-sectional view of FIG. 1, the coating layer-attached positive electrode active material 10 for lithium ion secondary batteries of this embodiment can have a lithium metal composite oxide 11, which is a positive electrode active material, and a coating layer 12 that coats at least a part of the surface of the lithium metal composite oxide 11. Note that FIG. 1 is a schematic cross-sectional view in which the lithium metal composite oxide 11 is shown as a circle, but the cross-sectional shape does not have to be a circle and can have any shape. As will be described later, the coating layer 12 only needs to coat at least a part of the surface of the lithium metal composite oxide 11, and does not need to coat the entire surface of the lithium metal composite oxide 11, and does not need to have a constant thickness.

[0020] Hereinafter, each of the components contained in the coating layer-formed positive electrode active material for a lithium ion secondary battery according to this embodiment will be described. <1-1. Lithium metal composite oxide> The lithium metal composite oxide, which is the positive electrode active material of the coating layer-attached positive electrode active material of this embodiment, has a layered rock salt structure and can contain lithium (Li), nickel (Ni), and an M element (M) in a substance amount ratio of Li:Ni:M=a:1-x:x. In the above formula, Ni is nickel, and the M element is one or more elements excluding lithium, nickel, and oxygen.

[0021] The value of a in the above formula, which indicates the lithium content, can be 0.98 or more and 1.20 or less. That is, 0.98≦a≦1.20 can be satisfied. The value of a is more preferably 1.00 or more and 1.10 or less.

[0022] By setting the value of a to 0.98 or more, the internal resistance of a secondary battery using a coating layer-attached positive electrode active material containing a lithium metal composite oxide can be suppressed, and the output characteristics can be improved. Also, by setting the value of a to 1.20 or less, the initial discharge capacity of a secondary battery using a coating layer-attached positive electrode active material containing the lithium metal composite oxide can be maintained high. That is, by setting the value of a in the above-mentioned range, the output characteristics and capacity characteristics of a secondary battery using a coating layer-attached positive electrode active material containing the lithium metal composite oxide can be improved.

[0023] Nickel (Ni) in the lithium metal composite oxide is an element that contributes to increasing the capacity of a secondary battery using a positive electrode active material containing the lithium metal composite oxide. In the lithium metal composite oxide, a part or all of the nickel can be replaced by the M element. Therefore, the value of x representing the amount of nickel replacement can be set to 0≦x≦1.0. However, as described above, nickel (Ni) is an element that contributes to increasing the capacity of a secondary battery using a positive electrode active material containing the lithium metal composite oxide, so it is preferable that the lithium metal composite oxide contains nickel, and x is preferably 0≦x≦0.7. It is more preferable that x is particularly 0≦x≦0.65.

[0024] The M element is one or more elements other than lithium, nickel, and oxygen, and can replace part or all of the nickel. The M element can include at least one element selected from the group consisting of Al (aluminum), Ti (titanium), V (vanadium), Mn (manganese), Fe (iron), Co (cobalt), Cu (copper), Zr (zirconium), Nb (niobium), Mo (molybdenum), Ta (tantalum), and W (tungsten).

[0025] It is particularly preferable that the M element contains at least cobalt. When the lithium metal composite oxide contains cobalt, the structure of the lithium metal composite oxide is easily stabilized during charging and discharging, and therefore deterioration of the lithium metal composite oxide during high-voltage use of the secondary battery can be suppressed.

[0026] The structure of the lithium metal composite oxide can be identified by analytical techniques such as X-ray diffraction, electron beam diffraction, etc. The mass ratio of elements contained in the lithium metal composite oxide and the positive electrode active material with a coating layer can be understood by analytical techniques such as X-ray fluorescence analysis, ICP emission spectrometry, etc.

[0027] The volume average particle diameter of the lithium metal composite oxide particles, as measured by a laser diffraction scattering type particle size distribution analyzer, is preferably 1 μm or more and 10 μm or less, more preferably 2 μm or more and 7 μm or less, and even more preferably 3 μm or more and 5 μm or less. This is because, when the volume average particle diameter of the lithium metal composite oxide particles is 1 μm or more and 10 μm or less, the battery capacity per volume can be sufficiently increased in a secondary battery using a positive electrode active material with a coating layer containing the lithium metal composite oxide particles as a positive electrode. <1-2. Covering layer> The coating layer can contain lithium, phosphorus, and Z elements.

[0028] For example, the coating layer may contain a compound or mixture containing one or more selected from lithium, phosphorus, Z element, and oxygen. The mixture may be a mixture of compounds containing one or more selected from lithium, phosphorus, Z element, and oxygen, and the coating layer may contain, for example, two or more of a Li-PO compound, a Li-PZO compound, and a Li-ZO compound.

[0029] The Z element is at least one kind of pentavalent transition metal element, and is preferably Nb (niobium).

[0030] By disposing a coating layer on the surface of the lithium metal composite oxide particles, an increase in the interfacial resistance between the lithium metal composite oxide and the solid electrolyte can be suppressed in a secondary battery having a positive electrode including the positive electrode active material with a coating layer of this embodiment. (Coverage rate) The coating layer is preferably disposed so that the surface coverage of the lithium metal composite oxide particles is at least a predetermined value.

[0031] The coverage rate of the coating layer, specifically the coverage area of ​​the lithium metal composite oxide particles, can be calculated using the results of semi-quantitative analysis by X-ray photoelectron spectroscopy (XPS). Specifically, it can be known from the ratio of the amount of substance of the sum of phosphorus, Z element, nickel, and M element to the amount of substance of phosphorus and Z element present on the surface, which is known from the results of semi-quantitative analysis by XPS on the positive electrode active material with a coating layer. The coverage rate of the coating layer can be calculated, for example, by the following formula (1). In the following formula (1), P, Z, Ni, and M correspond to the amounts of substance of phosphorus, Z element, nickel, and M element, respectively, measured by XPS.

[0032] (Coverage rate of coating layer (%)) = (P + Z) / (P + Z + Ni + M) × 100 (1) Due to its characteristics, XPS can selectively obtain information from the surface of the object to be measured, from 1 nm to 5 nm, so the composition ratio of the surface layer of the material can be known from the results of XPS measurement. The coverage of the coating layer is preferably 60% or more, more preferably 65% ​​or more, and even more preferably 70% or more. By making the coverage 60% or more, it is possible to prevent both the interfacial reaction between the lithium metal composite oxide and the solid electrolyte and the interfacial mixing between the lithium metal composite oxide and the coating layer, and to suppress deterioration during cycles. In addition, the coating layer contains lithium, phosphorus, and Z elements, which enhances stability even during high-voltage charging.

[0033] The upper limit of the coverage is not particularly limited, but can be, for example, 100% or less, and is preferably 90% or less. (Ratio of the amount of Z element to phosphorus) It is preferable that Z / P, which is the ratio of the amount of substance of the Z element (Z) to the phosphorus (P) contained in the coating layer, satisfies 0.5≦Z / P≦3.0. By setting Z / P within the above range, it is possible to particularly enhance the effect of preventing both the interfacial reaction between the lithium metal composite oxide and the solid electrolyte, and the interfacial mixing between the lithium metal composite oxide and the coating layer. The amount of substance of phosphorus and the amount of substance of the Z element in the above formula can also be measured and calculated by XPS. (Coating layer thickness) There is no need for a clear boundary between the coating layer and the lithium metal composite oxide particles. Therefore, the coating layer refers to a portion or region in the surface side region of the positive electrode active material with a coating layer of this embodiment where the concentration of phosphorus and Z element is higher than that of the lithium metal composite oxide particles, i.e., the central region. The coating layer may be partially dissolved in the lithium metal composite oxide.

[0034] The content of the coating layer is not particularly limited, but it is preferable to adjust the content, specifically the calculated thickness of the coating layer, according to the specific surface area of ​​the lithium metal composite oxide particles to be coated. Specifically, the thickness of the coating layer when formed, calculated from the specific surface area of ​​the lithium metal composite oxide particles forming the coating layer and the amount of the coating layer forming solution to be applied, is preferably 5 nm or more and 15 nm or less. By making the thickness of the coating layer 5 nm or more, the coverage rate can be easily made 60% or more, and the coating layer can be formed stably. In addition, by making the thickness of the coating layer 5 nm or more, the reaction between the lithium metal composite oxide and the solid electrolyte can be particularly suppressed.

[0035] Furthermore, by setting the thickness of the coating layer to 15 nm or less, the influence on the movement of lithium ions between the lithium metal composite oxide and the solid electrolyte can be particularly suppressed. <1-3. Other characteristics of the positive electrode active material for lithium-ion secondary batteries with a coating layer> So far, the lithium metal composite oxide and the coating layer have been described. It is preferable that the positive electrode active material with a coating layer of this embodiment has the following properties.

[0036] The positive electrode active material with a coating layer of this embodiment is preferably composed only of the above-mentioned lithium metal composite oxide particles and the coating layer, but impurities may be mixed in during production. In particular, moisture is an impurity that may be mixed in when forming the coating layer. Since moisture may cause hydrolysis and deterioration of the solid electrolyte and affect the initial discharge capacity, it is preferable that the moisture content is controlled within a predetermined range.

[0037] The coating layer-attached positive electrode active material of the present embodiment preferably has a water content (moisture content) of 0.08% by mass or less. By setting the water content to 0.08% by mass or less, the hydrolysis reaction of the solid electrolyte can be more reliably suppressed in a secondary battery using the coating layer-attached positive electrode active material.

[0038] As described above, it is preferable to set the moisture content of the coating layer-attached positive electrode active material of this embodiment to 0.08 mass % or less, since this more reliably suppresses the hydrolysis reaction of the solid electrolyte. The moisture content of the coating layer-attached positive electrode active material of this embodiment can be evaluated by, for example, the Karl Fischer method at a heating temperature of 300° C.

[0039] The lower limit of the moisture content of the coating layer-attached positive electrode active material of this embodiment can be set to 0 mass % or more. <2. Method for producing coating layer-forming solution and coating layer-formed positive electrode active material for lithium-ion secondary battery> (Method of manufacturing positive electrode active material with coating layer) A configuration example of the coating layer forming solution and the method for producing the coating layer-attached positive electrode active material according to the present embodiment will be described. According to the method for producing the coating layer-attached positive electrode active material according to the present embodiment, the above-mentioned coating layer-attached positive electrode active material can be produced, so some of the items already described will not be described. Note that the method for producing the coating layer-attached positive electrode active material according to the present embodiment is one example of a production method, and the above-mentioned method for producing the coating layer-attached positive electrode active material is not limited to the production method described below.

[0040] The method for producing a coating layer-attached positive electrode active material of the present embodiment can include a precursor formation step and a heat treatment step, which will be described below.

[0041] Each step will be described below. (Precursor formation process) In the precursor formation step, a solution for forming a coating layer is applied to the surfaces of particles of lithium metal composite oxide, followed by drying, to form a precursor.

[0042] The lithium metal composite oxide supplied to the precursor forming step is the same as the lithium metal composite oxide already described in the coating layer-attached positive electrode active material. That is, the lithium metal composite oxide has a layered rock salt structure, and can contain lithium (Li), nickel (Ni), and M element (M) in a ratio of Li:Ni:M=a:1-x:x in terms of the substance amount ratio. a and x satisfy the relationships 0.98≦a≦1.20 and 0≦x≦1.0, and the M element can be one or more elements other than lithium, nickel, and oxygen. A more preferable form of the lithium metal composite oxide has already been described, and therefore the description will be omitted.

[0043] The coating layer forming solution is a solution in which lithium, phosphorus, and Z element are all dissolved, and the Z element is at least one pentavalent transition metal element. The preferred form of the Z element has already been described, so the description will be omitted. The coating layer forming solution is a solution used to form the coating layer of the above-described coating layer-attached positive electrode active material.

[0044] The coating layer forming solution can be prepared, for example, by mixing a solution containing Li-ZO and a solution containing Li-PO while adjusting the pH. The coating layer forming solution may be prepared by adding and mixing components such as lithium, phosphorus, and a compound that serves as a supply source of Z element to a solvent such as water. The solvent used in the coating layer forming solution is not limited to water, and one or more types selected from water and alcohols such as ethanol can be used. The coating layer forming solution can be formed while adjusting the content ratio of each element so that the coating layer to be formed has a desired composition. The obtained solution is preferably a transparent and dissolved solution rather than a sol solution in which nanoparticles are dispersed. In other words, the obtained coating layer forming solution is preferably a solution in which lithium, phosphorus, and Z elements are all dissolved.

[0045] A completely dissolved solution means that the added components are dissolved and no precipitate is visually observed, and can be, for example, a transparent solution as described above.

[0046] Z / P, which is the ratio of the amount of substance of element Z (Z) to phosphorus (P) contained in the coating layer-forming solution, preferably satisfies, for example, 0 < Z / P ≦ 3.0, and more preferably satisfies 0.5 ≦ Z / P ≦ 3.0. For the coating layer-forming solution, by setting Z / P within the above range, for the coating layer of the positive electrode active material with a coating layer produced using the coating layer-forming solution, the ratio of the amount of substance of element Z (Z) to the contained phosphorus (P) can be easily set within a predetermined range.

[0047] In the precursor formation step, the coating layer-forming solution can be applied to and dried on the particles of the lithium metal composite oxide. As the coating and drying apparatus to be used at this time, any method can be used as long as it can thinly and uniformly coat the lithium metal composite oxide particles, and a method of spraying the coating layer-forming solution while stirring and flowing the powder of the lithium metal composite oxide is preferred. When stirring and flowing, an apparatus that is less likely to be damaged by particle crushing or impact can be preferably used. For example, a rolling fluidization apparatus can be used. In addition, the rolling fluidization apparatus is preferred because it can also be dried simultaneously by heating from the outside or adjusting the temperature of the gas (such as air) introduced into the apparatus. The drying temperature may be equal to or higher than the temperature at which the solvent contained in the coating layer-forming solution evaporates. (Heat treatment step) In the heat treatment step, the precursor can be heat-treated.

[0048] The heat treatment step can be carried out for the precursor in which the dried product of the coating layer-forming solution is disposed on the surface of the particles of the lithium metal composite oxide formed in the precursor formation step, for the purpose of completely evaporating the solvent.

[0049] The atmosphere for the heat treatment step may be an air atmosphere, but more preferably, air from which carbon dioxide has been removed or an oxygen atmosphere can be used. The heat treatment temperature is preferably 300°C or higher at which the solvent is reliably evaporated. In addition, when it is necessary to increase the crystallinity of the coating layer, it is preferable to perform the heat treatment at a temperature of 600°C or lower. By performing the heat treatment at 600°C or lower, it is possible to reliably suppress the occurrence of mixing between the lithium metal composite oxide and the coating layer. The heat treatment time depends on the thickness of the coating layer, but is preferably 1 hour or more and 10 hours or less. By performing the heat treatment for 1 hour or more, the solvent in the coating layer can be sufficiently reduced and removed. In addition, by setting the heat treatment time to 10 hours or less, productivity can be increased.

[0050] Therefore, in the heat treatment step, for example, the precursor is preferably heat treated in dry air or an oxygen atmosphere at a heat treatment temperature of 300°C to 600°C for 1 hour to 10 hours, and the atmosphere is more preferably an oxygen atmosphere.

[0051] The coated positive electrode active material obtained after the heat treatment step can have a lithium metal composite oxide and a coating layer that coats at least a part of the surface of the lithium metal composite oxide. The coating layer preferably has a coverage of 60% or more as described for the coated positive electrode active material. The method of determining the coverage and the preferred range of the coverage have already been described, so the description will be omitted. <3. All-solid-state lithium-ion secondary battery> Next, a configuration example of the all-solid-state lithium-ion secondary battery of this embodiment will be described. For example, as shown in Fig. 2, the all-solid-state lithium-ion secondary battery 20 of this embodiment can have a positive electrode 21 including the above-mentioned positive electrode active material with a coating layer, a negative electrode 23, and a solid electrolyte layer 22. These members can be sealed in a container 24. The positive electrode 21 and the negative electrode 23 can be provided with a positive electrode terminal 211 and a negative electrode terminal 231, respectively, so that they can be connected to members outside the container 24.

[0052] Each component of the secondary battery of this embodiment will be described below. Note that the embodiment described below is merely an example, and the all-solid-state lithium-ion secondary battery of the present invention can be embodied in a form in which various modifications and improvements are made based on the embodiment described in this specification and on the knowledge of those skilled in the art. In addition, the all-solid-state lithium-ion secondary battery of this embodiment is not particularly limited in its use. <3-1. Positive electrode> The positive electrode can be formed by molding the positive electrode mixture. The positive electrode can be appropriately processed according to the battery to be used. For example, the positive electrode can be subjected to a compression treatment using a press or the like to increase the electrode density.

[0053] The above-mentioned positive electrode mixture can be formed, for example, by mixing the above-mentioned powdered positive electrode active material with a coating layer and a solid electrolyte.

[0054] The solid electrolyte is added to the electrode to provide it with suitable ionic conductivity.

[0055] The material of the solid electrolyte is not particularly limited, but may be, for example, Li3PS4, Li7P3S 11 , Li 10 GeP2S 12 Sulfide-based solid electrolytes such as Li7La3Zr2O 12 , Li 0.34 La 0.51 TiO 2.94 For example, an oxide-based solid electrolyte such as SiO2 or a polymer-based electrolyte such as PEO can be used.

[0056] A binder and a conductive agent (conductive assistant) may also be added to the positive electrode mixture.

[0057] The conductive agent is added to the electrode to give it suitable conductivity. The material of the conductive agent is not particularly limited, but examples of the conductive agent that can be used include graphite such as natural graphite, artificial graphite, and expanded graphite, as well as acetylene black, Ketjen Black (registered trademark), carbon nanotubes, and fibrous graphite.

[0058] The binder plays a role of binding the positive electrode active material with the coating layer, but it does not need to be added if not necessary. The binder used in the positive electrode mixture is not particularly limited, but one or more types selected from, for example, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene propylene diene rubber, styrene-based thermoplastic elastomer, hydrogenated styrene-based thermoplastic elastomer, cellulose-based resin, polyacrylic acid, etc. can be used.

[0059] The mixing ratio of each material in the positive electrode mixture is not particularly limited. For example, the content of the positive electrode active material with the coating layer in the positive electrode mixture can be 50 parts by mass or more and 90 parts by mass or less, and the content of the solid electrolyte can be 10 parts by mass or more and 50 parts by mass or less.

[0060] However, the method for producing the positive electrode is not limited to the above-mentioned example, and other methods may be used. <3-2. Negative electrode> The negative electrode can be formed by molding a metal (lithium metal, indium metal, lithium-indium alloy, lithium-aluminum alloy, Si or an alloy containing Si, etc.) or a negative electrode mixture.

[0061] Although the components constituting the negative electrode mixture and the composition thereof are different, the negative electrode mixture can be formed in substantially the same manner as the positive electrode described above, and various treatments are carried out as necessary in the same manner as the positive electrode.

[0062] The negative electrode mixture can be prepared by mixing a negative electrode active material and a solid electrolyte. As the negative electrode active material, for example, an occlusion material capable of occluding and desorbing lithium ions can be used.

[0063] The storage material is not particularly limited, and may be one or more selected from, for example, natural graphite, artificial graphite, organic compound sintered bodies such as phenolic resin, and powders of carbon materials such as coke. When such a storage material is used as the negative electrode active material, a sulfide electrolyte such as Li3PS4 may be used as the solid electrolyte, as in the positive electrode. <3-3.Solid electrolyte layer> The solid electrolyte contained in the solid electrolyte layer may be, for example, an inorganic solid electrolyte. Examples of the inorganic solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes.

[0064] The oxide-based solid electrolyte is not particularly limited, and any oxide-based solid electrolyte that contains oxygen (O) and has lithium ion conductivity and electronic insulation properties can be used. Examples of oxide-based solid electrolytes include lithium phosphate (Li3PO4), Li3PO4N X , LiBON X , LiNbO3, LiTaO3, Li2SiO3, Li4SiO4-Li3PO4, Li4SiO4-Li3VO4, Li2O-B2O3-P2O5, Li2O-SiO2, Li2O-B2O3-ZnO, Li 1+X Al X Ti 2-X (PO4)3(0≦X≦1), Li 1+X Al X Ge 2-X (PO4)3(0≦X≦1), LiTi2(PO4)3, Li 3X La 2 / 3-X TiO3(0≦X≦2 / 3), Li5La3Ta2O 12 , Li7La3Zr2O 12 , Li6BaLa2Ta2O 12 , Li 3.6 S 0.6 P 0.4 Examples include O4.

[0065] The sulfide-based solid electrolyte is not particularly limited, and any electrolyte that contains sulfur (S) and has lithium ion conductivity and electronic insulation can be used. Examples of sulfide-based solid electrolytes include Li2S-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li6PS5Cl, Li6PS5Br, Li 10 GeP2S 12, Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 etc.

[0066] As the inorganic solid electrolyte, materials other than those mentioned above may be used, for example, Li3N, LiI, Li3N-LiI-LiOH, etc. may be used. <3-4. Shape and composition of secondary batteries> Next, an example of the arrangement and configuration of the components of the secondary battery of this embodiment will be described.

[0067] The secondary battery of this embodiment having the positive electrode, negative electrode, and solid electrolyte layer described above can be made into various shapes such as a coin type or a laminate type, which can be applied with a certain pressure. Regardless of the shape, the positive electrode and the negative electrode can be laminated via a solid electrolyte, as described with reference to FIG. 2. Then, the positive electrode current collector and the positive electrode terminal leading to the outside, and the negative electrode current collector and the negative electrode terminal leading to the outside can be connected using a current collecting lead or the like, and the battery can be sealed in a battery case to form a secondary battery.

[0068] The secondary battery of this embodiment using the above-described positive electrode active material with a coating layer can be an all-solid-state lithium ion secondary battery having a charge / discharge capacity equivalent to that of a lithium ion battery using an electrolyte solution. <3-5. Battery evaluation of secondary batteries> The secondary battery according to this embodiment using the above-described positive electrode active material with a coating layer can be evaluated under the following conditions, for example.

[0069] Specifically, a test battery 30 shown in FIG. 3 was constructed using the coating layer-attached cathode active material of this embodiment as a cathode, and the current density was set to 0.5 mA / cm 2 As a result, the cutoff voltage is 4.8V (vs. Li / Li + ) and then charge it to the cut-off voltage of 3.0V (vs. Li / Li) after one hour of rest. +) for 50 cycles, and the capacity retention rate is compared with that of a battery without a coating layer or a battery with a different coating layer to evaluate its effectiveness.

[0070] The use of the secondary battery of this embodiment is not particularly limited, and it can be suitably used for various applications requiring a power source. In addition, since the secondary battery of this embodiment has a charge / discharge capacity equivalent to that of a lithium-ion secondary battery using an electrolyte and can be miniaturized, it is also suitable as a power source for electric vehicles that are limited in mounting space. EXAMPLES

[0071] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way. [Example 1] (1) Physical properties of lithium metal composite oxide particles (1-1)Chemical composition The chemical composition of the lithium metal composite oxide was quantitatively analyzed using an ICP optical emission spectrometer (VARIAN, 725ES) and it was confirmed that the mass ratio of Li, Ni, Co, and Al was Li:Ni:Co:Al=1.02:0.80:0.15:0.05. (1-2) Crystal structure The crystal structure of the lithium metal composite oxide was measured using XRD (X'Pert, PROMRD, manufactured by PANALYTICAL Corporation), and was found to have a layered rock-salt structure belonging to the R-3m structure. (1-3) Specific surface area The BET specific surface area of ​​the lithium metal composite oxide was measured using a fully automatic BET specific surface area measuring device (Maxsorb, manufactured by Mountec Co., Ltd.) and found to be 0.58 m 2 / g. (1-4) Volume average particle size The volume average particle size of the lithium metal composite oxide was measured using a laser diffraction scattering type particle size distribution measuring device (Microtrack HRA, manufactured by Nikkiso Co., Ltd.) and found to be 5.8 μm.

[0072] (2) Manufacturing of the positive electrode active material with a coating layer (2-1) Preparation of solution for forming coating layer The coating layer forming solution was prepared by adding hydrogen peroxide, niobium hydroxide, ammonia water, lithium hydroxide, and LiH2PO4 to ion-exchanged water in a predetermined order, mixing them together, and dissolving them all. The resulting coating layer forming solution was mixed so that the mass ratio (Nb / P) of niobium (Nb) to phosphorus (P) contained therein was 1.0. The Nb / P value in the above coating layer forming solution is shown in the "Nb / P in coating layer forming solution" column in Table 1.

[0073] (2-2) Formation of the coating layer Li 1.02 Ni 0.80 Co 0.15 Al 0.05 The lithium metal composite oxide powder of O2 was subjected to the following precursor formation step and heat treatment step to produce a positive electrode active material with a coating layer.

[0074] (Precursor formation process) The total surface area (m2) of the total weight (g) of the lithium metal composite oxide particles that form the coating layer 2 ) is the specific surface area (m 2 / g. The density of the LiPO3 crystal (2.46 g / cm3) was calculated based on the total surface area. 3 ), the density of LiNbO3 crystal (4.65g / cm 3 ) was used, and the amount of the coating layer forming solution was adjusted by calculating so that the target coating layer thickness would be 7 nm. The target coating layer thickness is shown in the "Coating layer thickness (target value)" column in Table 1. Next, 500 g of lithium metal composite oxide powder was weighed out and fluidized in a rolling fluidized granulation coating device (Powrex Corporation, MP-01), and the coating layer forming solution was sprayed into the fluidized bed. At this time, the temperature of the air supplied into the fluidized bed was controlled to 120°C, and the precursor was formed by slowly coating the precursor for 4 hours.

[0075] (Heat treatment process) The precursor, which is a powder obtained in the precursor formation step, was collected, and the precursor was subjected to a heat treatment at 300°C for 2 hours in an oxygen atmosphere to produce a coating layer containing Li, P, and Nb from which the water solvent had been completely removed. A composition analysis was performed on the cross section of the obtained coating layer-containing cathode active material using EDX, and it was confirmed that the coating layer was disposed on the surface of the lithium metal composite oxide. It was also confirmed that the following other examples have the same structure. (3) Evaluation of the coated cathode active material The thus obtained positive electrode active material with a coating layer was evaluated as follows.

[0076] (3-1) Surface analysis The positive electrode active material with the coating layer was measured using an XPS (Versa Probe II, manufactured by ULVAC-PHI). 3 / 2 Spectrum, Co=2p 3 / 2 spectrum, Al=2p spectrum, P=2p spectrum, Nb=3d 5 / 2 The amount of each element (at%) on the surface of the coated positive electrode active material was obtained from the semi-quantitative values ​​calculated from the area of ​​each peak in the spectrum. The coverage rate, which is the ratio of the sum of the amounts of P and Nb present on the surface to the sum of the amounts of P, Nb, Ni, Co, and Al, was (P+Nb) / (P+Nb+Ni+Co+Al)×100=86%. The evaluation results are shown in the "Coverage rate" column in Table 1.

[0077] In addition, the ratio of the amount of Nb to P was calculated to be 0.96 (Nb / P). The evaluation results are shown in the "Nb / P" column of Table 1.

[0078] (3-2) Moisture content The moisture content of the positive electrode active material with a coating layer was measured using a Karl Fischer moisture meter (manufactured by Kyoto Electronics Manufacturing Co., Ltd., model: MKC210) at a heating temperature of 300° C., and was found to be 0.045% by mass.

[0079] (4) Preparation of secondary batteries For battery evaluation of the positive electrode active material with a coating layer, a battery (hereinafter referred to as a "test battery") having a structure shown in Fig. 3, which is an all-solid-state lithium ion secondary battery, was used. The test battery 30 is composed of a case and a compacted powder cell 31 housed in the case.

[0080] The case has a negative electrode can 32 which is hollow and has one open end, and a positive electrode can 33 which is placed in the opening of the negative electrode can 32. When the positive electrode can 33 is placed in the opening of the negative electrode can 32, a space for accommodating the compacted powder cell 31 is formed between the positive electrode can 33 and the negative electrode can 32. The positive electrode can 33 is fixed to the negative electrode can 32 with a thumbscrew 34 and a nut 35.

[0081] The negative electrode can 32 is provided with a negative terminal, and the positive electrode can 33 is provided with a positive terminal. The case is provided with an insulating sleeve 36, which fixes the negative electrode can 32 and the positive electrode can 33 so that they are kept out of contact with each other.

[0082] A pressure screw 37 is provided at the closed end of the negative electrode can 32, and after the positive electrode can 33 is fixed to the negative electrode can 32, the pressure screw 37 is tightened toward the compact cell storage space, thereby holding the compact cell 31 in a pressurized state through a hemispherical washer 38. A screw-in plug 39 is provided at the end of the negative electrode can 32 where the pressure screw 37 is located. O-rings 40 are provided between the negative electrode can 32 and the positive electrode can 33 and between the negative electrode can 32 and the plug 39, which seal the gap between the negative electrode can 32 and the positive electrode can 33 and maintain the airtightness inside the case.

[0083] The compact cell 31 is a pellet made of a positive electrode layer, a solid electrolyte layer, and a negative electrode layer, which are stacked in this order. It is housed in a case so that the positive electrode layer contacts the inner surface of the positive electrode can 33 through the lower current collector 41, and the negative electrode layer contacts the inner surface of the negative electrode can 32 through the upper current collector 42, a washer 38, and a pressure screw 37. The lower current collector 41, the compact cell 31, and the upper current collector 42 are protected by a sleeve 43 to prevent electrical contact between the positive electrode layer and the negative electrode layer.

[0084] Such a test battery 30 was fabricated as follows.

[0085] First, 60 mg of the coated cathode active material and 40 mg of Li3PS4 solid electrolyte were mixed in a mortar to prepare a cathode mixture. Next, a mold capable of producing pellets with a diameter of 10 mm was prepared, and 60 mg of the solid electrolyte was placed in the mold and pressed at 10 MPa. Next, 15 mg of the cathode mixture was added, and the mixture was pressed at 360 MPa to obtain a two-layer pellet consisting of a tightly bonded cathode layer and solid electrolyte layer.

[0086] From the bottom up, the lower electrode, a pellet with the positive electrode layer facing downwards, indium foil to become the negative electrode layer, and the upper electrode were layered in this order, and the electrodes were sealed in a case, after which the pressure screws 37 were tightened with a torque of 6 N·m to 7 N·m to provide a restraining force. The test battery 30 was fabricated in a glove box with an Ar atmosphere and a dew point controlled at -80°C. (5) Evaluation of secondary batteries The cycle characteristics of the test battery were measured under the following conditions.

[0087] A rest period of 1 hour was allowed until the open circuit voltage (OCV) became approximately stable. Then, a constant current density of 0.5 mA / cm was applied. 2 The cutoff voltage is 4.8V (vs. Li / Li + ) after 1 hour of rest, the cut-off voltage was 3.0V (vs. Li / Li + ) Reverse current up to a current density of 0.5mA / cm 2 This operation from charging to discharging was counted as "1 cycle," and 50 cycles were performed in total. The capacity retention rate (%) was calculated by dividing the discharge capacity (mAh / g) at the 50th cycle by the discharge capacity (mAh / g) at the 2nd cycle.

[0088] Since the capacity of a battery varies depending on the battery materials, configuration, and measurement conditions, the capacity retention rate is shown in Table 1 as a relative ratio when the capacity retention rate of the LiNbO3-coated lithium metal composite oxide shown in Comparative Example 1 is set to 1. When the relative ratio exceeds 1, it means that the capacity retention rate is high, that is, deterioration is suppressed, and when applied to an all-solid-state lithium ion secondary battery using a solid electrolyte, the decrease in battery capacity when repeatedly charged and discharged can be suppressed. In Example 1, the capacity retention rate, which is a relative ratio, was 1.44. The evaluation results are shown in the "Capacity retention rate (relative ratio)" column in Table 1.

[0089] [Example 2] In Example 2, the lithium metal composite oxide was Li 1.1 Ni 0.38 Co 0.32 Mn 0.30 O2 (layered rock salt structure, specific surface area = 0.68 m 2 / g, volume average particle size=4.7 μm) was used. A positive electrode active material with a coating layer was produced under the same conditions as in Example 1 except for the above points, and was evaluated.

[0090] In addition, when calculating the coverage rate after the heat treatment, (P + Nb) / (P + Nb + Ni + Co + Mn) × 100 is calculated. Mn in the above formula is Mn = 2p obtained by measuring the positive electrode active material with a coating layer by XPS. 3 / 2 The amount of Mn (at%) was calculated from the semi-quantitative value calculated from the peak area of ​​the spectrum.

[0091] After the heat treatment, the coverage was 88%, and the Nb / P ratio was 0.96. The capacity retention rate, which is a relative ratio in the battery evaluation, was 1.39.

[0092] [Example 3] When preparing the coating layer forming solution, the Nb / P ratio in the coating layer forming solution was set to 0.5. A positive electrode active material with a coating layer was prepared and evaluated under the same conditions as in Example 1 except for the above. The coverage after the heat treatment was 85%, and Nb / P was 0.52. The capacity retention rate, which is a relative ratio in the battery evaluation, was 1.30.

[0093] [Example 4] When preparing the solution for forming the coating layer, the Nb / P ratio in the solution for forming the coating layer was set to 3.0. A positive electrode active material with a coating layer was prepared and evaluated under the same conditions as in Example 1 except for the above. The coverage after the heat treatment was 82%, and Nb / P was 2.9. The capacity retention rate, which is a relative ratio in the battery evaluation, was 1.28.

[0094] [Example 5] In the precursor forming step, the amount of the solution for forming the coating layer was adjusted based on the calculation so that the target coating layer thickness would be 5 nm. A positive electrode active material with a coating layer was produced and evaluated under the same conditions as in Example 1 except for the above. The coverage after the heat treatment was 68%, and Nb / P was 1.1. The capacity retention rate, which is a relative ratio in the battery evaluation, was 1.32. [Example 6] For the coating layer forming solution, lithium hydroxide and an aqueous solution of LiH2PO4 dissolved in ion-exchanged water were added in the prescribed order to the niobium oxide inorganic coating solution "Bailar Nb-G6000" manufactured by Taki Chemical Co., Ltd., and mixed to prepare an aqueous solution in which all was dissolved. The resulting coating layer forming solution was mixed so that the mass ratio (Nb / P) of niobium (Nb) to phosphorus (P) contained therein was 1.0.

[0095] A positive electrode active material with a coating layer was produced and evaluated under the same conditions as in Example 1 except for the above points. The coverage after the heat treatment was 88%, and Nb / P was 1.0. The capacity retention rate, which is a relative ratio in the battery evaluation, was 1.36. [Example 7] The coating layer forming solutions were prepared by mixing the two solutions: a Li-Nb solution in which lithium ethoxide and niobium ethoxide were dissolved in ethanol, and a Li-P solution in which lithium ethoxide and triethyl phosphate were dissolved in ethanol.

[0096] In addition, the coating layer forming solution was mixed so that the substance ratios of Li:Nb and Li:P were 1:1 and 1:30, respectively, and triethyl phosphate was added in excess. In other words, the resulting coating layer forming solution was mixed so that the substance ratio (Nb / P) of niobium (Nb) to phosphorus (P) contained therein was 1 / 30.

[0097] A positive electrode active material with a coating layer was produced and evaluated under the same conditions as in Example 1 except for the above points. The coverage after the heat treatment was 86%, and Nb / P was 0.95. The capacity retention rate, which is a relative ratio in the battery evaluation, was 1.33.

[0098] [Comparative Example 1] As the coating layer forming solution, lithium ethoxide and niobium ethoxide were weighed out so that Li:Nb=1:1 (substance amount ratio) and dissolved in ethanol to use. A positive electrode active material with a coating layer was produced and evaluated under the same conditions as in Example 1 except for the above points. The coverage rate after heat treatment was 81%. The capacity retention rate, which is a relative ratio in the battery evaluation, was set to 1.00 as a reference.

[0099] [Comparative Example 2] As the solution for forming the coating layer, a solution was used in which a Li-Nb solution, which is a solution in which lithium ethoxide and niobium ethoxide are dissolved in ethanol, and a Li-P solution in which lithium ethoxide and triethyl phosphate are dissolved in ethanol were mixed. When the Li-Nb solution and the Li-P solution were mixed, the ratio of Li:Nb and Li:P was adjusted to 1:1 in terms of substance amount and mixed. A positive electrode active material with a coating layer was produced and evaluated under the same conditions as in Example 1 except for the above points. The coverage after the heat treatment was 32%, and Nb / P was 28. The capacity retention rate, which is a relative ratio in the battery evaluation, was 1.02.

[0100] [Comparative Example 3] When preparing the solution for forming the coating layer, the Nb / P in the solution for forming the coating layer was set to 0.3. A positive electrode active material with a coating layer was prepared and evaluated under the same conditions as in Example 1 except for the above. The coverage after the heat treatment was 83%, and Nb / P was 0.26. The capacity retention rate, which is a relative ratio in the battery evaluation, was 0.94.

[0101] [Comparative Example 4] When preparing the solution for forming the coating layer, the Nb / P in the solution for forming the coating layer was set to 3.6. A positive electrode active material with a coating layer was prepared and evaluated under the same conditions as in Example 1 except for the above. The coverage after the heat treatment was 80%, and the Nb / P was 3.7. The capacity retention rate, which is a relative ratio in the battery evaluation, was 1.05.

[0102] [Comparative Example 5] In the precursor forming step, the amount of the solution for forming the coating layer was adjusted based on the calculation so that the target coating layer thickness would be 2.4 nm. A positive electrode active material with a coating layer was produced and evaluated under the same conditions as in Example 1 except for the above. The coverage after the heat treatment was 53%, and Nb / P was 1.0. The capacity retention rate, which is a relative ratio in the battery evaluation, was 1.10.

[0103] [Table 1] [Explanation of symbols]

[0104] 10. Positive electrode active material for lithium-ion secondary batteries with coating layer 11 Lithium metal oxide 12 Covering layer 20 All-solid-state lithium-ion secondary battery 21 Positive electrode 211 Positive terminal 22 Solid electrolyte layer 23 Negative electrode 231 Negative terminal 24 Container 30 Test Battery 31 Powder Compaction Cell 32 Anode can 33 Positive electrode can 34 Thumb screw 35 Nut 36 Insulating sleeve 37 Pressure screw 38 Washer 39 Plug 40 O-ring 41 Lower current collector 42 Upper current collector 43 Sleeve

Claims

1. A lithium metal composite oxide; a coating layer that covers at least a part of the surface of the lithium metal composite oxide and has a coverage rate of 60% or more; The lithium metal composite oxide has a layered rock salt structure and contains lithium (Li), nickel (Ni), and an M element (M) in a ratio of Li:Ni:M=a:1-x:x in terms of the amount of substance, where a and x satisfy the relationships 0.98≦a≦1.20 and 0≦x≦1.0, and the M element is one or more elements excluding lithium, nickel, and oxygen, The coating layer contains lithium, phosphorus, and a Z element, and the Z element is at least one kind of pentavalent transition metal element.

2. 2. The positive electrode active material for a lithium ion secondary battery with a coating layer according to claim 1, wherein the M element is at least one selected from the group consisting of Al, Ti, V, Mn, Fe, Co, Cu, Zr, Nb, Mo, Ta, and W.

3. 3. The positive electrode active material for a lithium ion secondary battery with a coating layer according to claim 1, wherein Z / P, which is a ratio of the amount of substance of the Z element (Z) to phosphorus (P) contained in the coating layer, satisfies 0.5≦Z / P≦3.

0.

4. The positive electrode active material for a lithium ion secondary battery with a coating layer according to claim 1 or 2, wherein the Z element is niobium.

5. A coating layer forming solution used for forming the coating layer of the coating layer-formed positive electrode active material for lithium ion secondary batteries according to claim 1 or 2, A coating layer forming solution in which lithium, phosphorus, and the Z element are all dissolved.

6. a precursor forming step of applying a coating layer forming solution to the surface of a lithium metal composite oxide particle and drying the solution to form a precursor; A heat treatment step of heat treating the precursor, The lithium metal composite oxide has a layered rock salt structure and contains lithium (Li), nickel (Ni), and an M element (M) in a ratio of Li:Ni:M=a:1-x:x in terms of the amount of substance, where a and x satisfy the relationships 0.98≦a≦1.20 and 0≦x≦1.0, and the M element is one or more elements excluding lithium, nickel, and oxygen, The method for producing a positive electrode active material for a lithium ion secondary battery with a coating layer, wherein the coating layer forming solution is a solution in which lithium, phosphorus, and a Z element are all dissolved, and the Z element is at least one kind of pentavalent transition metal element.

7. 7. The method for producing a positive electrode active material for a lithium ion secondary battery with a coating layer according to claim 6, wherein in the heat treatment step, the precursor is heat treated in an oxygen atmosphere at a heat treatment temperature of 300° C. or more and 600° C. or less for 1 hour or more and 10 hours or less.

8. A positive electrode, a negative electrode, and a solid electrolyte layer; The positive electrode of an all-solid-state lithium ion secondary battery comprises the positive electrode active material for a lithium ion secondary battery with a coating layer according to claim 1 or 2.

Citation Information

Patent Citations

  • Positive electrode composite material and sulfide all-solid battery arranged by use thereof

    JP2016039062A

  • Positive electrode active material for all-solid lithium ion secondary battery, manufacturing method thereof, and all-solid lithium ion secondary battery

    JP2021103671A

  • Active material particles, electrode, power storage element, all-solid-state secondary cell, method for manufacturing active material particles, and power storage device

    WO2022163585A1

  • Sulfide solid electrolyte

    JP2014056661A