Positive electrode material and preparation method for the same, positive electrode sheet, lithium ion battery, and lithium ion battery pack
The optimized carbon-coated lithium manganese iron phosphate cathode material addresses conductivity and polarization issues, enhancing electrical performance and cycle life through controlled carbon distribution and exposure, achieving improved battery performance.
Patent Information
- Application Number
- JP2023215326
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2023-12-20
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-12-20
AI Technical Summary
Lithium manganese iron phosphate cathode materials suffer from poor conductivity and high charge/discharge polarization, with carbon coatings presenting challenges such as high carbon content reducing material compaction and limited coating efficiency, leading to poor high-temperature cycle life.
A positive electrode material comprising lithium manganese iron phosphate with a surface coating of carbon, where the carbon content is controlled between 1.4% to 4.7% of the total mass, and a specific distribution of carbon layers with a thickness ratio of 10-15:5-10, and metal exposure rate of 68% to 88%, enhancing electrical performance.
The optimized carbon coating improves electrical performance and cycle life of the cathode materials, achieving gram capacity exceeding 140mAh/g, DCR below 120, and cycle life exceeding 800 cycles.
Smart Images

Figure 2024146736000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of lithium ion batteries, in particular to a positive electrode material, its preparation method, and a positive electrode sheet. [Background technology]
[0002] Since its development, lithium-ion batteries have been favored in various technical fields due to the advantages of high energy density, stable discharge voltage, and long service life. In addition, lithium-ion batteries are commonly adopted in portable energy storage tools, especially in the new energy automobile industry, which is currently popular worldwide. As an important part of lithium-ion batteries, the selection of the positive electrode material directly affects the performance of lithium-ion batteries. The positive electrode materials mainly include lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, etc. Lithium iron phosphate has the advantages of good structural stability, good thermal stability, good safety performance, good cycle life, and abundant raw material sources, and is therefore more commonly adopted in the fields of energy storage batteries and electric vehicle batteries. However, the voltage plateau of lithium iron phosphate is only 3.4V vs. Li / Li+, which limits the energy density of lithium iron phosphate. Lithium manganese iron phosphate has the same olivine structure as lithium iron phosphate and has a higher voltage plateau than lithium iron phosphate.
[0003] However, lithium manganese iron phosphate has poor electrical conductivity and high charge / discharge polarization. At present, the electrical conductivity of lithium manganese iron phosphate is mainly modified by coating it with carbon materials, which improves the rate characteristics of lithium manganese iron phosphate and improves its polarization. However, there are some serious technical challenges in carbon coating. First, the carbon content of the coating is high, which reduces the compression of the material due to the high specific surface area of carbon. Second, the coating efficiency is limited, the material is not well protected, and the main performance shows that the high temperature cycle life is limited. Therefore, the preparation of lithium manganese iron phosphate material with low carbon content, good coating effect, and good stability is very important for the research and development of electrochemical devices. Summary of the Invention [Problem to be solved by the invention]
[0004] In view of the above-mentioned shortcomings of the related art, the object of the present invention is as follows. [Means for solving the problem]
[0005] In a first aspect, a positive electrode material is provided, which includes lithium manganese iron phosphate and carbon coating the surface of particles of the lithium manganese iron phosphate, the chemical formula of which is Li a Mn x Fe 1-x-y M y PO4, where 0.9≦a≦1.10, 0≦x≦1.0, 0≦y≦0.02, 0.5≦x / (1-xy)≦0.9, M is a doping element selected from one or more of Ti, Mg, Ni, Co, Al, V, Cr, Zr, and Nb, and carbon accounts for 1.4% to 4.7% of the total mass of the positive electrode material.
[0006] In combination with the first aspect, in one implementation, carbon coats the surface of the lithium manganese iron phosphate particles, forming, from the inside out, a core body made of lithium manganese iron phosphate, a fused layer of lithium manganese iron phosphate fused with carbon, and a coating layer made of carbon.
[0007] Referring to the first embodiment, in one implementation, the thickness ratio of the fusion layer to the coating layer is (10-15):(5-10).
[0008] In combination with the first aspect, in one implementation, the carbon percentage at a first depth from the surface of the coating layer is 1.2%≦W1≦2.3%, and the first depth is within the fusion layer.
[0009] In combination with the first aspect, in one implementation, the carbon percentage at a second depth from the surface of the coating layer is 0.8%≦W2≦1.8%, the second depth is within the fusion layer, and the second depth is deeper than the first depth.
[0010] In combination with the first aspect, in one implementation, the ratio of the carbon fraction at a first depth from the surface of the coating layer to the carbon fraction at a second depth is 1.05≦W1 / W2≦1.8.
[0011] In combination with the first aspect, in one implementation, the first depth is in the range of 5 nm to 20 nm from the surface of the coating layer.
[0012] In combination with the first aspect, in one implementation, the second depth is in the range of 90 nm to 100 nm from the surface of the coating layer.
[0013] In combination with the first aspect, in one implementation, the metal exposure rate P after the lithium iron manganese phosphate particles are coated with carbon is me is 68%≦P me ≦88%, metal exposure rate P me =n me / n tol where n me is the total molar amount of all metal elements on the surface of the lithium manganese iron phosphate particle, and n tol is the total molar amount of all elements on the surface of the lithium iron manganese phosphate particle.
[0014] In a second aspect, a method for preparing a positive electrode material is provided, in which a carbon source, a manganese source, a lithium source, an iron source, a doping element and a phosphorus source are mixed and dried, and then pre-baking and pre-fusion are carried out at a first-stage temperature, and then the temperature is increased to a second-stage temperature to continue baking to obtain a positive electrode material, and / or the first-stage temperature is 300°C-500°C, the pre-baking time is 10-20 hours, and / or the second-stage temperature is 500°C-650°C, and the baking time is 10-20 hours.
[0015] In combination with the second aspect, in one implementation, the carbon source is selected from one or more of glucose, fructose, polyethylene glycol, sucrose, and / or the manganese source is one or more of manganese sulfate, manganese nitrate, manganese chloride, and / or the iron source is one or more of ferric nitrate and ferric chloride, and / or the phosphorus source is one or more of ammonium dihydrogen phosphate and diammonium hydrogen phosphate, and / or the doping element is selected from a sulfate, nitrate, or chloride salt of the corresponding doping element, and / or the lithium source is lithium carbonate.
[0016] In a third aspect, a positive electrode sheet is provided, the essential element being that the ingredients for preparation include the positive electrode material described in either the first or second aspect above. Effect of the Invention
[0017] As described above, the positive electrode material and electrochemical device of the present invention have at least the following beneficial effects: The carbon content of the positive electrode material is 1.4%-4.7%, which is lower than the carbon content of common positive electrode materials, but the covering effect is good, and the application of such positive electrode material in electrode sheets and batteries can exhibit improved electrical performance. [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a schematic diagram showing a layer structure formed by coating with carbon on the surface of a particle of lithium iron manganese phosphate according to the present invention. [Diagram 2] FIG. 2 is a comparative diagram showing a comparison of cycle life curves at 45° C. between Example 1 of the present invention and Comparative Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The implementation of the present invention is shown below by a specific embodiment. Those skilled in the art can easily understand the advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied by other different specific implementation methods, and various modifications or changes can be made to the details in this specification based on different perspectives and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiment is merely for illustrating the present invention, and is not for limiting the protection scope of the present invention.
[0020] The term "coating" refers to the use of another material to form a uniform, thin layer structure that can cover the active material on the surface of the active material, and the term "carbon coating" refers to coating the surface of the active material with a thin carbon film layer, forming a high strength, high conductivity, and high corrosion resistance carbide layer on the surface of the active material.
[0021] Some embodiments of the present invention provide a cathode material comprising lithium manganese iron phosphate and carbon, the chemical formula of the lithium manganese iron phosphate being Li a Mn x Fe 1-x-y M y PO4, where 0.9≦a≦1.10, 0≦x≦1.0, 0≦y≦0.02, 0.5≦x / (1-xy)≦0.9, and M is a doping element selected from one or more of Ti, Mg, Ni, Co, Al, V, Cr, Zr, and Nb. Carbon coats the surface of the lithium manganese iron phosphate particles, and the carbon accounts for 1.4% to 4.7% of the total mass of the positive electrode material.
[0022] Referring to Fig. 1, carbon coats the surface of the lithium manganese iron phosphate particles, and from the inside to the outside, a core body d1 made of lithium manganese iron phosphate, a fused layer d2 of lithium manganese iron phosphate fused with carbon, and a coating layer d3 made of carbon are formed. The thickness ratio of the fused layer d2 to the coating layer d3 is (10-15):(5-10). Within the fused layer, the proportion of carbon in the fused layer gradually increases from the core body to the distance away from the core body along the thickness direction.
[0023] In some embodiments, the carbon percentage increases gradually, specifically, the carbon percentage at a first depth from the surface of the coating layer is 1.2%≦W1≦2.3%, and the first depth is located within the range of the fusion layer. The carbon percentage at a second depth from the surface of the coating layer is 0.8%≦W2≦1.8%, and the second depth is located within the range of the fusion layer, and the second depth is deeper than the first depth. The carbon percentage here refers to the local carbon content in a specific depth range measured by the etching XPS test method. The dispersion percentage of carbon in the fusion layer is reflected by the penetration depth of carbon in the particles of lithium manganese iron phosphate. The better the fusion effect of carbon and lithium manganese iron phosphate, the higher the electrical performance. Therefore, the electrical performance of the positive electrode material can be controlled by controlling the distribution of carbon content in the fusion layer.
[0024] In order to improve the coating effect and increase the cycle life, in some embodiments, the ratio of the carbon fraction at the first depth and the carbon fraction at the second depth is further limited, specifically, the ratio of the carbon fraction at the first depth from the surface of the coating layer to the carbon fraction at the second depth is 1.05≦W1 / W2≦1.8.
[0025] In one specific implementation, based on the thickness ratio of the fusion layer d2 to the coating layer d3 being (10-15):(5-10), the first depth is in the range of 5 nm to 20 nm from the surface of the coating layer, and the second depth is preferably in the range of 90 nm to 100 nm from the surface of the coating layer.
[0026] In addition, in some embodiments, the effect of carbon coating is further required to improve the performance of the positive electrode material. Specifically, the metal exposure rate P after the lithium manganese iron phosphate particles are coated with carbon is me is 68%≦P me ≦88%, metal exposure rate P me =n me / n tol where n me is the total molar amount of all metal elements on the surface of the lithium manganese iron phosphate particle, the metal elements include transition metal elements, n tolis the total molar amount of all elements on the surface of the lithium manganese iron phosphate particles. Note that the contents of C, Fe, and Mn on the surface of the lithium manganese iron phosphate particles are measured by EDS method, and the molar amount of surface (Fe+Mn) is divided by the total molar amount of surface C, Fe, and Mn to obtain the metal exposure rate.
[0027] One embodiment of the present invention provides a method for preparing a positive electrode material. A carbon source, a manganese source, a lithium source, an iron source, a doping element, and a phosphorus source are mixed and dried, and then pre-fired at a temperature of 300°C to 500°C for 10 to 20 hours for pre-fusion. Then, the temperature is increased to 500 to 650°C, and the firing is continued for 10 to 20 hours to obtain a positive electrode material.
[0028] It should be noted that the pre-firing temperature is very important for the pre-fusion of the carbon source, and pre-firing improves the quality of the carbon material coating and increases the penetration depth. If the pre-firing temperature is too low, the fusion effect between carbon and other raw materials will not be favorable, and if the pre-firing temperature is too high, the carbon source will be pre-carbonized and the effect of pre-fusion will not be achieved. In both cases, the electrical performance will be deteriorated. The firing temperature is very important for the carbon coating effect. If the firing temperature is too low, the cracks in the carbon source will not be sufficient to completely form an amorphous carbon coating. If the firing temperature is too high, the carbon source will volatilize, and the fusion effect between the carbon source and the main material will be deteriorated. In both cases, the electrical performance will be deteriorated. Therefore, it is necessary to select a suitable firing temperature.
[0029] In some embodiments, the carbon source is selected from one or more of glucose, fructose, polyethylene glycol, and sucrose.It should be noted that the carbon source is not limited to one or more of glucose, fructose, polyethylene glycol, and sucrose, and other organic carbon sources may be adopted.Compared with inorganic carbon sources, the pre-fusion effect of organic carbon sources is better.
[0030] In some embodiments, the manganese source is one or more of manganese sulfate, manganese nitrate, and manganese chloride.
[0031] In some embodiments, the iron source is one or more of iron nitrate and iron chloride.
[0032] In some embodiments, the phosphorus source is one or more of ammonium dihydrogen phosphate and diammonium hydrogen phosphate.
[0033] In some embodiments, the doping elements are selected from sulfate, nitrate, or chloride salts of the corresponding doping elements.
[0034] In some embodiments, the lithium source is lithium carbonate.
[0035] As part of one embodiment of the present invention, a positive electrode sheet is provided, the preparation of the raw material of which includes the above positive electrode material.
[0036] In some embodiments, the method for preparing the positive electrode sheet includes mixing the positive electrode material of any of the embodiments with the conductive agent Super P and the binder polyvinylidene fluoride (PVDF) based on a weight ratio of 97:1.5:1.5, adding the solvent N-methylpyrrolidone (NMP) and stirring the mixture to thoroughly mix to obtain a positive electrode slurry, and coating the positive electrode slurry on an aluminum foil of a positive electrode current collector, followed by drying, cold pressing, slitting, and other processes to finally obtain a positive electrode sheet.
[0037] Examples 1 to 8 and Comparative Examples 1 to 10
[0038] I. Based on the various embodiments in Table 1, the positive electrode sheets prepared using different parameters of the positive electrode material were laminated with the same separator film and negative electrode sheet, respectively, with the separator film between the positive electrode sheet and the negative electrode sheet to play the role of separation. Then, the outside was covered with an aluminum-plastic film, and after drying, the same electrolyte was injected into each one. After packaging, standing, and chemical treatment, the soft-pack batteries with a capacity of 1 Ah were finally completed.
[0039] Table 1: Parameters of the positive electrode materials used in Examples 1 to 8
[0040] [Table 1]
[0041] II. Based on the comparative examples in Table 2, the positive electrode sheets prepared using different parameters of the positive electrode material were laminated with the same separator film and negative electrode sheet, respectively, with the separator film between the positive electrode sheet and the negative electrode sheet to fulfill the function of separation. Then, the outside was covered with an aluminum-plastic film, and after drying, the same electrolyte was injected into each one. After packaging, leaving, and chemical treatment, finally, soft-pack batteries with a capacity of 1 Ah were completed.
[0042] Table 2: Parameters of the positive electrode materials used in Comparative Examples 1 to 10
[0043] [Table 2]
[0044] III. Test Methods: A gram capacity test, a DCR test, and a cycle test were carried out on the batteries obtained in the above examples and comparative examples.
[0045] 1. Gram capacity test method: Charge and discharge were performed three cycles at 0.33C at 25°C within the range of 2.5 to 4.2V, and the gram capacity of the positive electrode was obtained by dividing the discharge capacity of the third cycle by the total mass of the positive electrode material.
[0046] 2.DCR test method: Charge and discharge three cycles at 0.33C at 25℃, the discharge capacity of the third cycle is 100% of the cell capacity. Then adjust the cell capacity to 70% at 0.33C, i.e. 70% SOC. Discharge at a current density of 4C for 30s, and divide the voltage difference before and after discharge by the discharge current. The result is the 70% SOC DCR.
[0047] 3. Cycle test method: Charge and discharge were performed at 1C at 45°C within the range of 2.5 to 4.2 V until the remaining capacity was 80% of the initial capacity. The number of cycles is the cycle life of the material.
[0048] IV. Test Results
[0049] Test results for various examples are shown in Table 3.
[0050] Table 3: Test results for Examples 1 to 8
[0051] [Table 3]
[0052] Result explanation:
[0053] 1. In Examples 1-8, the gram capacity was over 140 mAh / g. Most of the DCR results were below 120, with a few exceeding 120. The cycle life reached an average of over 800 cycles, most exceeding 900 cycles, and some exceeding 1000 cycles.
[0054] 2. Comparison of Comparative Examples 1 to 3 with Examples 1 to 8:
[0055] 2 is a comparison diagram showing a comparison of cycle life curves at 45° C. between Example 1 and Comparative Examples 1 and 2. The capacity of Example 1 decreased steadily, while the capacity of Comparative Examples 1 and 2 decreased at an accelerating rate.
[0056] In Comparative Examples 1 and 3, the metal exposure rate Pme , the carbon fraction at the first depth (hereinafter, W1), the carbon fraction at the second depth (hereinafter, W2), and the ratio of the carbon fraction at the first depth to the carbon fraction at the second depth (hereinafter, W1 / W2) are outside the preferred ranges of the present invention. The gram capacity does not exceed 130, the DCR is higher than 140, and the cycle life is lower than 500 times. Compared with Examples 1 to 8, there is a large difference between the test results of various parameters, and the performance is significantly optimized when the parameters are in the preferred ranges.
[0057] 3. Comparison of Comparative Examples 4-5 with Examples 1-3:
[0058] When W1 or W2 in Comparative Example 4 or 5 does not meet the preferred range, the metal exposure rate is relatively high, indicating that the infiltration of carbon into the lithium manganese iron phosphate is not uniform. Also, the gram capacity is lower than 140 mAh / g, the DCR is higher than 130, and the cycle life is only about 600 times. Compared with Examples 1 to 3, the test results of Comparative Examples 4 to 5 are relatively poor.
[0059] 4. Comparison of Comparative Example 6 with Examples 3 to 5:
[0060] In Comparative Example 6, the metal exposure rate, W1 and W2 are within the preferred range, but when the W1 / W2 ratio is outside the value range set by the present invention, the carbon penetration is not uniform, the gram capacity is lower than 140, the DCR is higher than 130, and the cycle life is lower than 700 times. The overall performance is relatively poor. In Examples 3 to 5, by optimizing the W1 / W2 ratio, the gram capacity increases to more than 140, the DCR is about 120, and the cycle life is maintained at more than 800 times, showing a significant improvement. With other parameters unchanged, the W1 / W2 ratio adopting the value range set by the present invention can further improve the performance of the battery.
[0061] 5. Comparison of Comparative Example 6 with other Comparative Examples:
[0062] The gram capacity, DCR and cycle life of Comparative Example 6 are all better than those of other Comparative Examples, which indirectly indicates that the metal exposure rate, W1 and W2 can further improve the performance of the battery by adopting the value range set by the present invention.
[0063] 6. Comparison of Comparative Examples 7 to 9 with Examples 6 to 8:
[0064] When only one of W1, W2, and the ratio of W1 / W2 is within the preferred range, the metal exposure rate exceeds the preferred range, the carbon coating effect is relatively poor, and the performance of gram capacity, DCR, and cycle life are all poor.
[0065] 7. Comparison of Comparative Examples 4 to 9 with Comparative Examples 1 to 3 and 10:
[0066] Among the metal exposure rate, W1, W2, and the ratio of W1 / W2 in Comparative Examples 4 to 9, at least one of the parameter conditions for the four parameters adopts the value range set by the present invention. In Comparative Examples 1 to 3, the value ranges for the four parameters are outside the value range set by the present invention. The gram capacity, DCR, and cycle life of Comparative Examples 4 to 9 are all better than those of Comparative Examples 1 to 3 and 10. This shows that it is possible to improve the performance of a battery when at least one of the four parameters, among the metal exposure rate, W1, W2, and the ratio of W1 / W2, adopts the value range set by the present invention.
[0067] Comparison of Examples 9-11 with Comparative Examples 11-12:
[0068] Some of the examples and comparative examples of the present invention provide a method for preparing a positive electrode material. According to the parameter conditions shown in Table 4, first, polyethylene glycol, manganese sulfate, iron nitrate, lithium carbonate, doping element, and ammonium dihydrogen phosphate were mixed and dried, and then pre-baked at a first temperature for 10-20 hours for pre-fusion. Then, the temperature was increased to a second temperature and baking was continued for 10-20 hours to obtain a positive electrode material. The prepared positive electrode material was used to fabricate a soft-pack battery with a capacity of 1 Ah based on the battery fabrication methods of Examples 1-8. The batteries obtained in the above-mentioned examples and comparative examples were respectively subjected to a gram capacity test, a DCR test, and a cycle test. The results are shown in Table 4.
[0069] Table 4: Carbon content in the positive electrode material, carbon coating effect, and effect of pre-baking on battery performance
[0070] [Table 4]
[0071] The results show that: In Comparative Examples 11 and 12, when the pre-baking temperature is lower than 300°C or pre-baking is not performed, even if the baking temperature meets the requirements, the carbon coating effect of the positive electrode material is poor, the carbon content and carbon ratio do not meet the requirements of the present invention, the gram capacity of the battery is relatively low, the cycle life is lower than 500 times, and the overall performance of the battery is relatively poor. In Examples 9 to 11, when the pre-baking temperature is increased while adopting the value range set by the present invention for the pre-baking temperature while keeping other conditions unchanged, the obtained positive electrode material has an improved carbon coating effect, the carbon content and carbon ratio all meet the values set by the present invention, the gram capacity of the battery is improved, the cycle life is increased to more than 800 times, even more than 1000 times, and the overall performance of the battery is improved.
[0072] Examples 12 to 14 and Comparative Example 13:
[0073] Some of the examples and comparative examples of the present invention provide a method for preparing a positive electrode material. According to the parameter conditions shown in Table 5, first, a carbon source, manganese sulfate, iron chloride, lithium carbonate, a doping element, and ammonium dihydrogen phosphate were mixed and dried, and then pre-baked at a first temperature for 10-20 hours for pre-fusion. Then, the temperature was increased to a second temperature and the baking was continued for 10-20 hours to obtain a positive electrode material. The prepared positive electrode material was used to prepare a soft-pack battery with a capacity of 1 Ah based on the battery preparation methods of Examples 1-8. The batteries obtained in the above-mentioned examples and comparative examples were respectively subjected to a gram capacity test, a DCR test, and a cycle test. The results are shown in Table 5.
[0074] Table 5: Carbon content of the positive electrode material, carbon coating effect, and effect of organic and inorganic carbon sources on battery performance.
[0075] [Table 5]
[0076] The results show that, in comparison with Examples 12-14 and Comparative Example 13, the parameters related to carbon coating and carbon content in the positive electrode materials obtained by using inorganic carbon sources cannot be within the range of values set by the present invention, and the overall performance of the batteries is inferior to that of the batteries prepared by using organic carbon sources.
[0077] Examples 15 to 17 and Comparative Example 14:
[0078] Some of the examples and comparative examples of the present invention provide a method for preparing a positive electrode material. According to the parameter conditions shown in Table 6, first, fructose, manganese chloride, iron nitrate, lithium carbonate, doping element, and ammonium dihydrogen phosphate were mixed and dried, and then pre-baked at a first temperature for 10-20 hours for pre-fusion. Then, the temperature was increased to a second temperature and the baking was continued for 10-20 hours to obtain a positive electrode material. The prepared positive electrode material was used to fabricate a soft-pack battery with a capacity of 1 Ah based on the battery fabrication methods of Examples 1-8. The batteries obtained in the above-mentioned examples and comparative examples were respectively subjected to a gram capacity test, a DCR test, and a cycle test. The results are shown in Table 6.
[0079] Table 6: Carbon content of the positive electrode material, carbon coating effect, and effect of calcination temperature on battery performance
[0080] [Table 6]
[0081] The results show that: Comparing Examples 15 to 17 with Comparative Example 14, when the sintering temperature is within the range of the present invention, the higher the temperature, the better the battery performance; when the sintering temperature is not within the range of the present invention, the battery performance is relatively poor. [Industrial Applicability]
[0082] Furthermore, the positive electrode material of the present invention, its preparation method, positive electrode sheet containing the same, lithium ion battery containing the same, and lithium ion battery pack containing the same can be used in the electronics field, and thus have high industrial applicability.
[0083] It should be noted that the test results of the above examples are only to illustrate the obvious advantages of the cathode material of the present invention under the same conditions, and the battery test results do not represent the optimal test results of the battery made with the cathode material of the present invention.
[0084] The above-described embodiments are illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Those skilled in the art may modify or change the above-described embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by those skilled in the art without departing from the spirit and technical ideas disclosed in the present invention are also intended to be encompassed in the scope of the claims of the present invention. [Explanation of symbols]
[0085] 1: Core body 2: Fusion layer 3: Covering layer d2: Thickness of the fusion layer d3: thickness of coating layer
Claims
1. Lithium iron manganese phosphate; Carbon coating the surface of the lithium manganese iron phosphate particles; Including, The chemical formula of the lithium manganese iron phosphate is Li a Mn x Fe 1-x-y M y P.O. 4 0.9≦a≦1.10, 0≦x≦1.0, 0≦y≦0.02, 0.5≦x / (1−x−y)≦0.9; M is a doping element selected from one or more of Ti, Mg, Ni, Co, Al, V, Cr, Zr, and Nb; The carbon comprises 1.4% to 4.7% of the total mass of the positive electrode material; Positive electrode material.
2. The carbon coats the surface of the particles of the lithium manganese iron phosphate, and from the inside to the outside, a core body made of the lithium manganese iron phosphate, a fused layer of the lithium manganese iron phosphate fused with the carbon, and a coating layer made of the carbon are formed. The positive electrode material according to claim 1 .
3. The thickness ratio of the fusion layer to the coating layer is (10-15):(5-10); The positive electrode material according to claim 2 .
4. The carbon percentage at a first depth from the surface of the coating layer is 1.2%≦W1≦2.3%, and the first depth is within the range of the fused layer. The positive electrode material according to claim 2 .
5. The carbon percentage at a first depth from the surface of the coating layer is 1.2%≦W1≦2.3%, and the first depth is within the range of the fused layer. The positive electrode material according to claim 3 .
6. The carbon percentage at a second depth from the surface of the coating layer is 0.8%≦W2≦1.8%, the second depth is within the range of the fused layer, and the second depth is deeper than the first depth. The positive electrode material according to claim 4.
7. The carbon percentage at a second depth from the surface of the coating layer is 0.8%≦W2≦1.8%, the second depth is within the range of the fused layer, and the second depth is deeper than the first depth. The positive electrode material according to claim 5 .
8. a ratio of the proportion of carbon at the first depth from the surface of the coating layer to the proportion of carbon at the second depth is 1.05≦W1 / W2≦1.8; The positive electrode material according to claim 6.
9. a ratio of the proportion of carbon at the first depth from the surface of the coating layer to the proportion of carbon at the second depth is 1.05≦W1 / W2≦1.8; The positive electrode material according to claim 7.
10. The first depth is between 5 nm and 20 nm from the surface of the coating layer. The positive electrode material according to claim 8.
11. The first depth is between 5 nm and 20 nm from the surface of the coating layer. The positive electrode material according to claim 9.
12. The second depth is between 90 nm and 100 nm from the surface of the coating layer. The positive electrode material according to claim 8.
13. The second depth is between 90 nm and 100 nm from the surface of the coating layer. The positive electrode material according to claim 9.
14. The metal exposure rate P after the particles of the lithium manganese iron phosphate are coated with the carbon me is 68% or less P me ≦88%, and the metal exposure rate P me = n me / n tol where n me is the total molar amount of all metal elements on the surface of the particle of the lithium manganese iron phosphate, and n tol is the total molar amount of all elements at the surface of the particle of the lithium iron manganese phosphate; The positive electrode material according to claim 1 .
15. After mixing and drying a carbon source, a manganese source, a lithium source, an iron source, a doping element, and a phosphorus source, pre-firing and pre-fusion are carried out at a first stage temperature, and then the first stage temperature is increased to a second stage temperature to continue the firing to obtain the positive electrode material; (1) the first stage temperature is 300°C to 500°C, and the pre-firing time is 10 to 20 hours; and (2) the second stage temperature is 500°C to 650°C, and the firing time is 10 to 20 hours; At least one of the following conditions is satisfied: A method for preparing a positive electrode material.
16. (a) the carbon source is selected from one or more of glucose, fructose, polyethylene glycol, and sucrose; (b) the manganese source is one or more of manganese sulfate, manganese nitrate, and manganese chloride; (c) the iron source is one or more of iron nitrate and iron chloride; (d) the phosphorus source is one or more of ammonium dihydrogen phosphate and diammonium hydrogen phosphate; (e) the doping elements are selected from the sulfate, nitrate or chloride salts of the corresponding doping elements; and (f) the lithium source is lithium carbonate; At least one of the following conditions is further satisfied: A method for preparing the cathode material of claim 15.
17. A raw material comprising the positive electrode material according to claim 1. Positive electrode sheet.
18. A raw material comprising the positive electrode material obtained by using the preparation method according to claim 15. Positive electrode sheet.
19. The positive electrode sheet according to claim 17, Lithium-ion battery.
20. 20. The lithium ion battery of claim 19, Lithium-ion battery pack.
Citation Information
Patent Citations
Secondary battery and method of manufacturing positive electrode material therefor
JP2004303496A
Polyanion-based positive electrode active material and method of manufacturing the same
JP2018006156A
Cathode active material for lithium-ion secondary battery
JP2023041288A
Cited By
Positive electrode active material, electrode, and battery
JP2026115254A
Positive electrode active material, electrode, and battery
JP2026115339A
Positive electrode active material, electrode, and battery
JP2026116130A
Positive electrode active material, electrode, and battery
JP7779370B1
Positive electrode active material, electrode, and battery
JP7779436B1