Negative electrode active material for sodium ion battery and method for producing the same, negative electrode material, and sodium ion battery
A metal sulfide, like FeS2 and Fe7S8, with a leaf-like structure, addresses the capacity retention issue in sodium ion batteries by enhancing cycle stability through a controlled synthesis process, ensuring high capacity retention.
Patent Information
- Application Number
- JP2023060417
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
AI Technical Summary
Existing negative electrode active materials for sodium ion batteries, such as FeS2, suffer from insufficient capacity retention after repeated use, particularly in terms of cycle capacity characteristics.
The use of a specific metal sulfide, such as FeS2 and Fe7S8, with a leaf-like structure, as the negative electrode active material, produced through a method involving the heating of an iron source and sulfur source, enhances the battery's capacity and cycle stability.
The proposed metal sulfide active material enables sodium ion batteries to maintain a large capacity even after repeated use, significantly improving cycle capacity characteristics.
Smart Images

Figure 2024147413000002 
Figure 2024147413000003 
Figure 2024147413000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative electrode active material for a sodium ion battery, a method for producing the same, a negative electrode material, and a sodium ion battery. [Background technology]
[0002] Currently, lithium-ion batteries (LIBs) are the mainstream of storage batteries, but in recent years, sodium-ion batteries (SIBs) have been expected to be one of the most promising storage batteries of the future. SIBs are the most potential alternative to LIBs, due to their abundant sodium resources, wide distribution, similar energy storage mechanism to LIBs, and low cost.
[0003] In sodium-ion batteries, compounds containing various metals have attracted attention, and transition metal sulfides are known as representative examples. Such sulfides have unique physical properties and are expected to provide effective ion diffusion paths by repeatedly inserting and extracting Na ions.
[0004] For example, it has been proposed to use FeS2 as an active material for sodium ion batteries (e.g., Non-Patent Document 1), and research into improving it is being conducted through morphology control, nanocrystallization, element substitution, hybridization, introduction of defects, and so on. [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] F. Wang et al., Chemical Engineering Journal 380 (2020). Summary of the Invention [Problem to be solved by the invention]
[0006] However, even when FeS2 is used as an anode active material for sodium ion batteries, the capacity of the battery after repeated use is insufficient, and there are still problems in terms of cycle capacity characteristics. Therefore, there is a strong demand for the development of an anode active material that can improve the battery characteristics, especially the cycle capacity characteristics, of sodium ion batteries.
[0007] The present invention has been made in view of the above, and has an object to provide a negative electrode active material capable of constructing a sodium ion battery that can have a large capacity even after repeated use. [Means for solving the problem]
[0008] Means of the Invention The present inventors have conducted extensive research to achieve the above object, and as a result have found that the above object can be achieved by using a sulfide of a specific metal, thereby completing the present invention.
[0009] That is, the present invention includes, for example, the subject matter described in the following sections. Item 1 A negative electrode active material for a sodium ion battery containing a metal sulfide, The metal sulfide contains FeS2 and Fe7S8, and is a negative electrode active material for a sodium ion battery. Section 2 A negative electrode active material for a sodium ion battery containing a metal sulfide, The metal sulfide is a sulfide containing at least one metal selected from the group consisting of Cr and Ni. Section 3 Item 2. The negative electrode active material for a sodium ion battery according to item 1, wherein the metal sulfide is a powder having a leaf-like structure. Section 4 Item 4. A negative electrode material comprising the negative electrode active material for a sodium ion battery according to any one of items 1 to 3. Section 5 Item 5. A sodium ion battery comprising the negative electrode material according to item 4. Section 6 A method for producing a negative electrode active material for a sodium ion battery according to any one of items 1 to 3, A step 1 of heating a raw material liquid containing an iron source to obtain a precursor; step 2 of heat treating the precursor in the presence of a sulfur source to produce a metal sulfide; A method for producing a negative electrode active material comprising the steps of: Effect of the Invention
[0010] According to the negative electrode active material for a sodium ion battery of the present invention, a sodium ion battery capable of maintaining a large capacity even after repeated use can be constructed. [Brief description of the drawings]
[0011] [Figure 1] 1A and 1B are SEM images of the negative electrode active material obtained in Example 1, and 1C and 1D are SEM images of the negative electrode active material obtained in Comparative Example 1. [Diagram 2] 2 shows the results of X-ray diffraction measurement (XRD) of the negative electrode active material obtained in Example 1. [Diagram 3] 6(a), (b), and (c) are TEM images of the negative electrode active material obtained in Example 1. (d) is an HRTEM image of the negative electrode active material obtained in Example 1. (e) is an SAED pattern of the negative electrode active material obtained in Example 1. (f) is an EDS analysis result of the metal sulfide powder containing FeS2 and Fe7S8 in the negative electrode active material obtained in Example 1. [Figure 4] 1 shows the results of a constant current charge / discharge test of the batteries assembled in Preparation Example 1 (negative electrode active material of Example 1) and Preparation Example 2 (negative electrode active material of Comparative Example 1). [Diagram 5] (a) shows the results of evaluating the cycle capacity characteristics of the batteries assembled in Preparation Example 1 and Preparation Example 2 at various current densities, and (b) shows the results of the cycle characteristics of the battery assembled in Preparation Example 1 at a current density of 2Ag-1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expressions "containing" and "comprise" include the concepts of "containing", "comprises", "consists essentially of" and "consists only of".
[0013] 1. Negative electrode active material for sodium ion batteries The negative electrode active material for sodium ion batteries of the present invention (hereinafter simply referred to as "negative electrode active material") contains a metal sulfide. In one embodiment of the negative electrode active material of the present invention, the metal sulfide contains FeS2 and Fe7S8. Hereinafter, in the present invention, the negative electrode active material for sodium ion batteries containing the metal sulfide containing FeS2 and Fe7S8 will be referred to as "negative electrode active material A". Moreover, the metal sulfide contained in the negative electrode active material A will be referred to as "metal sulfide a".
[0014] The negative electrode active material A can be used to construct a sodium ion battery that can have a large capacity even after repeated use. That is, the negative electrode active material A can be used to improve cycle capacity characteristics of a sodium ion battery. Therefore, the negative electrode active material of the present invention can be suitably used as an active material for forming a negative electrode material for constituting a sodium ion battery.
[0015] The metal sulfide a contained in the negative electrode active material A contains at least two types of iron sulfide, FeS2 and Fe7S8.
[0016] In the metal sulfide a, the content ratio of FeS2 and Fe7S8 is not particularly limited. For example, the mass ratio of FeS2 and Fe7S8, FeS2:Fe7S8, can be 10:1 to 0.1:1, preferably 8:1 to 1:1, and more preferably 4:1 to 2:1.
[0017] Whether or not FeS2 and Fe7S8 are present in the metal sulfide a can be confirmed from the XRD spectrum of the negative electrode active material A, specifically, it can be determined from the presence or absence of a signal of FeS2 and a signal of Fe7S8.
[0018] Metal sulfide a may contain components other than FeS2 and Fe7S8, or may consist only of FeS2 and Fe7S8. The metal sulfide preferably contains 50 mass% or more of FeS2 and Fe7S8, more preferably 80 mass% or more, even more preferably 90 mass% or more, and particularly preferably 95 mass% or more.
[0019] The metal sulfide a is a solid and can take various forms, such as powder, lump, granule, fiber, etc. In particular, the metal sulfide a is preferably a powder having a leaf-like structure. This enhances the function of the metal sulfide a as an active material, and when applied to a sodium ion battery, the cycle capacity characteristics can be particularly improved.
[0020] The leaf-like structure is a structure having many leaves on a branch. The shape of the leaf is not particularly limited, and may be, for example, a fern-like shape, a lavender-like shape, or a rosemary-like shape.
[0021] In the negative electrode active material A, the content ratio of Fe and sulfur (S) is not particularly limited. For example, the content ratio of Fe can be 5 to 60 mass% relative to the total mass of Fe and sulfur, preferably 10 to 50 mass%, more preferably 15 to 40 mass%, further preferably 20 to 35 mass%, and particularly preferably 25 to 27 mass%. The negative electrode active material A can contain elements other than Fe and sulfur as long as the effects of the present invention are not impaired.
[0022] The negative electrode active material A may contain other components in addition to the metal sulfide a, as long as the effects of the present invention are not impaired. The negative electrode active material A preferably contains 80 mass% or more of the metal sulfide a, more preferably 90 mass% or more, even more preferably 95 mass% or more, and particularly preferably 99 mass% or more. The negative electrode active material A may be composed only of the metal sulfide a.
[0023] The form of the negative electrode active material A is not particularly limited, and may be in various forms such as powder, lump, granule, fiber, etc. When the negative electrode active material A is in powder form, the metal sulfide a contained in the powder has the above-mentioned leaf-like structure.
[0024] In another embodiment of the negative electrode active material of the present invention, the metal sulfide is a sulfide containing at least one metal selected from the group consisting of at least Cr and Ni. Hereinafter, in the present invention, a negative electrode active material for a sodium ion battery containing a sulfide containing at least one metal selected from the group consisting of at least Cr and Ni will be referred to as "negative electrode active material B". In addition, the sulfide contained in negative electrode active material B will be referred to as "metal sulfide b".
[0025] The metal sulfide b may be, for example, a sulfide containing Cr, and specific examples include Cr3S4, NiCr2S4, TiCr2S4, and FeCr2S4. In addition, the metal sulfide b may be one or more selected from the group consisting of NiS, NiS2, Ni3S2, Ni7S6, and Ni9S8. The shape of the metal sulfide b may be, for example, the same as that of the metal sulfide a. Therefore, the metal sulfide b is also preferably a powder having a leaf-like structure.
[0026] 2. Method for producing negative electrode active material The method for producing the negative electrode active material of the present invention is not particularly limited, and for example, a wide variety of known production methods can be adopted. The negative electrode active material of the present invention includes the negative electrode active material A and the negative electrode active material B. For example, the method for producing the negative electrode active material A includes a production method including the following steps 1 and 2. Step 1: A step of heating a raw material liquid containing an iron source to obtain a precursor. Step 2: Heat treating the precursor in the presence of a sulfur source to produce a metal sulfide.
[0027] (Process 1) Step 1 is a step of heating a raw material liquid containing an iron source, and by this step, a precursor of the negative electrode active material is obtained.
[0028] The iron source may be an Fe body, an Fe compound, or a mixture thereof, and is preferably an Fe compound. The type of Fe compound is not particularly limited, and examples thereof include inorganic compounds, chlorides, and organic compounds of Fe. Examples of inorganic compounds of Fe include nitrates, sulfates, chlorides, oxides, chlorates, perchlorates, chloride complexes, carbonates, hydrogencarbonates, phosphates, and hydrogenphosphates of Co, cyanides, cyanide salts, and compounds containing oxoanions (ferrates). Examples of organic compounds of Fe include acetates, oxalates, formates, and succinates.
[0029] Among them, the iron source is preferably an inorganic compound of Fe, and more preferably a cyanide salt of Fe (for example, potassium hexacyanoferrate (III); K3[Fe(CN)6]).
[0030] The raw material liquid used in step 1 contains a solvent in addition to the iron source. As the solvent, water can be used, and various organic solvents can also be used. Examples of the organic solvent include N-methyl-2-pyrrolidone (NMP), dimethylformamide (DMF), oleic acid, ethylene glycol, octadecene, and ethylenediamine. The solvent used in step 1 can also be a mixture of water and an organic solvent. The solvent used in step 1 is preferably water.
[0031] There are no particular limitations on the content ratio of the iron source and the solvent in the raw material solution used in step 1. For example, the concentration of the iron source in the raw material solution used in step 1 can be 0.1 to 100 mM, preferably 0.2 to 50 mM, more preferably 0.5 to 30 mM, and further preferably 1 to 20 mM.
[0032] In step 1, the raw material liquid is heat-treated. For example, the heat treatment method includes a method in which the raw material is placed in a container, the container is sealed, and the inside of the container is heated. When the solvent in the raw material is water, this is a so-called hydrothermal synthesis method.
[0033] The temperature in the container during the heat treatment in step 1 is not particularly limited, and can be, for example, 100 to 400° C., and preferably 150 to 250° C. The heating time is also not particularly limited, and can be appropriately determined depending on the heating temperature, and can be, for example, 6 to 40 hours. The pressure in the container during the heat treatment can also be appropriately set.
[0034] After the heat treatment in step 1 is completed, the product can be taken out by an appropriate method. For example, if the product is obtained as a solid, the solid is separated by a method such as centrifugation, After washing and drying, the product can be obtained as a solid.
[0035] In step 1, the precursor obtained by the heat treatment is preferably freeze-dried. The freeze-drying method is not particularly limited, and for example, known freeze-drying conditions can be widely applied.
[0036] (Process 2) Step 2 is a step for generating a sulfide by heat-treating the precursor obtained in step 1 in the presence of a sulfur source.
[0037] The sulfur source used in step 2 is preferably a compound containing sulfur. In this case, metal sulfide a containing FeS2 and Fe7S8 is likely to be produced.
[0038] Examples of the sulfur-containing compound include a wide variety of known sulfur compounds, such as thioacetamide (CHCSNH), thiourea (SC(NH)), cysteine (CHNOS), sodium thiosulfate (NaS0), ammonium sulfide ((NH)S), sodium sulfide (NaS), etc. In addition, in the sulfur-containing compound, a part of the sulfur element may be replaced with Se and / or Te element.
[0039] The sulfur source used in step 2 is particularly preferably thioacetamide (CH3CSNH2). In this case, metal sulfides a containing FeS2 and Fe7S8 are particularly likely to be produced.
[0040] In step 2, the sulfur source can be used alone or in combination of two or more kinds.
[0041] In step 2, the method of heat-treating the precursor in the presence of a sulfur source is not particularly limited, and for example, a known sulfurization method can be widely adopted. Among them, it is preferable to adopt a solid sulfurization method as the sulfurization method. Specifically, a method of heat-treating the space in which the solid sulfur source and the solid precursor exist is preferable. In this method, for example, a container containing a solid sulfur source and a container containing the solid precursor obtained in step 1 are placed in a sealed container, and the sealed container is heat-treated to generate a sulfide.
[0042] The temperature of the heat treatment in step 2 can be, for example, 150 to 700°C, preferably 200 to 600°C, more preferably 300 to 550°C, and further preferably 400 to 530°C. The time of the heat treatment can be appropriately set depending on the temperature and the like, and is, for example, 1 to 5 hours. The heat treatment in step 2 can be performed in a vacuum atmosphere. In addition, the heat treatment in step 2 is preferably performed in a vacuum atmosphere. In this case, metal sulfide a containing FeS2 and Fe7S8 is likely to be generated. After the heating in a vacuum atmosphere, it is preferable not to perform another heat treatment in an inert gas atmosphere.
[0043] The ratio of the precursor and the sulfur source used in step 2 is not particularly limited, and the sulfur source may be used in an excess amount relative to the precursor.
[0044] In the above step 2, the precursor obtained in step 1 is sulfurized to obtain the target metal sulfide, i.e., metal sulfide a containing FeS2 and Fe7S8. The obtained metal sulfide a can be used as the negative electrode active material A, and the metal sulfide a can be combined with other components as necessary to be used as the negative electrode active material A.
[0045] In addition, when producing the negative electrode active material B, the same production method as that of the negative electrode active material A can be adopted, except that the iron source is replaced with a corresponding metal source in the step 1. For example, the negative electrode active material B can be produced by using K3[Cr(CN)6] and K2[Ni(CN)4] as the metal source.
[0046] 3. Negative electrode materials The negative electrode material of the present invention may contain other components, for example, known components used in the negative electrode material of a sodium ion battery, as long as it contains the negative electrode active material A or the negative electrode active material B. For example, the negative electrode material of the present invention may contain a conductive assistant and a binder in addition to the above-mentioned negative electrode active material.
[0047] The conductive assistant may be, for example, a wide variety of known conductive assistants used to form electrode materials for various batteries. Examples of the conductive assistant include various carbon materials, such as hard carbon, soft carbon, graphene, reduced graphene oxide, natural graphite, artificial graphite, conductive carbon black, and carbon fibers. Examples of carbon fibers include carbon nanofibers and carbon nanotubes. Other conductive assistants include metal powders such as copper and nickel, metal fibers, and conductive ceramic materials.
[0048] Examples of the binder include a wide variety of known binders used to form electrode materials for various batteries. Examples of the binder include various resin materials, specifically, polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR), polyethylene terephthalate, polyacrylonitrile (PAN), polyvinyl alcohol (PVA), polyethylene oxide (PEO), polyethylene, polypropylene, etc.
[0049] The content of the negative electrode active material in the negative electrode material is not particularly limited. For example, the content of the negative electrode active material is preferably 50 to 95 mass %, more preferably 60 to 90 mass %, based on the total mass of the negative electrode active material, conductive assistant, and binder contained in the negative electrode material.
[0050] The content of the conductive assistant in the negative electrode material is not particularly limited. For example, the conductive assistant is preferably contained in an amount of 3 to 30 mass %, more preferably 5 to 20 mass %, based on the total mass of the negative electrode active material, the conductive assistant, and the binder contained in the negative electrode material.
[0051] The content of the binder in the negative electrode material is not particularly limited. For example, the binder is preferably contained in an amount of 3 to 30 mass %, more preferably 5 to 20 mass %, based on the total mass of the negative electrode active material, conductive assistant, and binder contained in the negative electrode material.
[0052] The negative electrode material may be composed of only a negative electrode active material, a conductive assistant, and a binder, or may contain other components.
[0053] The method for preparing the negative electrode material is not particularly limited, and for example, a known method for preparing a negative electrode material can be widely adopted. For example, the negative electrode material can be prepared by mixing the negative electrode active material, the conductive assistant, and the binder in a predetermined ratio by an appropriate method. When preparing the negative electrode material, a solvent can be used to disperse the negative electrode active material, the conductive assistant, and the binder. Examples of the solvent include water and various organic solvents, such as lower alcohol compounds having 1 to 3 carbon atoms, NMP (N-methyl-2-pyrrolidone), etc. When the negative electrode material contains a solvent, it is, for example, in the form of a slurry or a paste.
[0054] 4. Sodium-ion battery The sodium ion battery of the present invention is not particularly limited in other configurations as long as it includes the negative electrode material, and may have, for example, the same configuration as a known sodium ion battery. The sodium battery of the present invention is more preferably a sodium ion secondary battery. The sodium battery may be an all-solid-state sodium battery.
[0055] The sodium ion battery may include, for example, a positive electrode, a negative electrode, an electrolyte, and a separator. The size and shape of the battery may be appropriately determined depending on the application.
[0056] The positive electrode can have a structure composed of, for example, a metal foil and a positive electrode material. Examples of metals for forming the metal foil include aluminum, titanium, platinum, molybdenum, stainless steel, and copper. Known positive electrode materials can be widely used as the positive electrode material. For example, examples of materials constituting the positive electrode material include sodium metal, NaFePO4, Na3V2(PO4)3, Na x Examples of the positive electrode include MO4 (M=Co, Mn, V, Fe), etc. The positive electrode can be produced by a known method, for example, a method of coating a positive electrode material on a metal foil.
[0057] The negative electrode may have a structure in which the negative electrode active material of the present invention is supported on a metal foil. Examples of the metal foil include aluminum, titanium, platinum, molybdenum, stainless steel, copper, etc. The negative electrode may be produced by a known method.
[0058] In the sodium ion battery, the type of electrolyte is not particularly limited, and for example, a known electrolyte can be used. The electrolyte may be either a solid electrolyte or a liquid electrolyte.
[0059] The liquid electrolyte may be a solution in which the electrolyte is dissolved in a solvent. The electrolyte may be various sodium salts, such as NaPF6, NaClO4, NaCF3SO3, NaFSI, NaTFSI, etc. The solvent may be water, diglyme, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, propyl acetate, fluoroethylene carbonate, propylene carbonate, ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, etc.
[0060] Examples of solid electrolytes include inorganic materials such as sulfides and oxides, and polymeric materials such as PEO (polyethylene oxide).
[0061] As the separator, a known separator applied to a secondary battery can be used, and examples thereof include materials formed of polyolefin resins such as polyethylene and polypropylene; polyimide; polyvinyl alcohol; fluororesins such as aminated polyethylene oxide polytetrafluoroethylene; acrylic resins; nylon; aromatic aramid; inorganic glass; ceramics, etc. The separator can be in the form of a porous membrane, nonwoven fabric, woven fabric, etc. Other examples of the separator include various polymer membranes and inorganic electrolytes. Examples of inorganic electrolytes include LiLaTiO3, Li7La3Zr2O 12 (LLZO), Na3Zr2Si2PO 12 , Na 11 Sn2PS 12, Na3PSe4, etc. EXAMPLES
[0062] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples.
[0063] Example 1 A raw material solution was obtained by dissolving 1 mmol of K3[Fe(CN)6] in 60 mL of deionized water. This raw material solution was transferred to a 100 mL autoclave lined with Teflon (registered trademark), and the autoclave was sealed and heated at 200 ° C for 20 hours to perform hydrothermal synthesis to obtain a precursor (step 1). This precursor was collected by centrifugation, and then freeze-dried for 24 hours to obtain a precursor powder. Next, 100 mg of the precursor and 0.8 g of thioacetamide (TAA) powder were placed in a porcelain boat so as not to contact each other, and heated at 500 ° C for 3 hours in a tubular furnace under a vacuum atmosphere. As a result, the target metal sulfide was obtained as a negative electrode active material (step 2).
[0064] Comparative Example 1 A raw material solution was obtained by dissolving 1 mmol of K3[Fe(CN)6] in 60 mL of deionized water. This raw material solution was transferred to a 100 mL capacity autoclave lined with Teflon (registered trademark), the autoclave was sealed, and the precursor was obtained by hydrothermal synthesis at 200 ° C for 20 hours. This precursor was collected by centrifugation, and then freeze-dried for 24 hours to obtain a precursor powder. Next, 100 mg of the precursor and 0.8 g of thioacetamide (TAA) powder were placed in a porcelain boat so as not to contact each other, and heated at 500 ° C for 3 hours in a tubular furnace under a vacuum atmosphere to obtain a metal sulfide. 100 mg of this metal sulfide and 0.8 g of sulfur powder were placed on the downstream side and upstream side of argon described below, respectively, and this porcelain boat was heated at 400 ° C for 3 hours in a tubular furnace while argon was flowing. As a result, a metal sulfide for comparison was obtained as a negative electrode active material.
[0065] (Example 1) A battery was produced using the negative electrode active material obtained in Example 1. Specifically, a negative electrode material slurry was prepared, which consisted of the negative electrode active material, superP (conductive carbon black) as a conductive additive, and polyvinylidene fluoride (PVDF) dissolved in methylpyrrolidinone as a binder. In this slurry, the ratio of the negative electrode active material:superP:PVDF was 7.5:1.5:1 (mass ratio). The slurry was coated on copper foil and dried in a vacuum at 80°C for 12 hours to produce a negative electrode with a diameter of 12 mm. A battery was assembled by a known method using this negative electrode, a positive electrode (sodium metal with aluminum foil), and a separator ("Whatman GF / C glass fiber filter paper" provided by Cytiva) impregnated with a liquid electrolyte. The electrolyte was a 1M sodium trifluoromethanesulfonate solution, and the solvent for this solution was diglyme.
[0066] (Example 2) Batteries were assembled in the same manner as in Preparation Example 1, except that the negative electrode active materials obtained in Example 1 were replaced with the negative electrode active materials obtained in Comparative Example 1.
[0067] (Evaluation Results) 1(a) and (b) show SEM images of the negative electrode active material obtained in Example 1, and Fig. 1(c) and (d) show SEM images of the negative electrode active material obtained in Comparative Example 1. From Fig. 1(a) and (b), it was found that the negative electrode active material obtained in Example 1 has a leaf-like structure.
[0068] FIG. 2 shows the results of X-ray diffraction measurement (XRD) of the negative electrode active material obtained in Example 1. For the X-ray diffraction measurement, Rigaku's "SmartLab" was used, and the measurement was performed using a Cu-Kα (λ=1.540Å) radiation source in the range of 2θ=10 to 100°. Note that FIG. 2 also shows the XRD patterns of Fe2S (JCPDS: 71-2219) and Fe7S8 (JCPDS: 71-0591) for reference.
[0069] From the XRD pattern in FIG. 2, it was confirmed that the metal sulfides in the negative electrode active material obtained in Example 1 contained FeS2 and Fe7S8.
[0070] 3(a), (b), and (c) are TEM images of the negative electrode active material obtained in Example 1, (d) is an HRTEM image of the negative electrode active material obtained in Example 1, (e) is an SAED pattern of the negative electrode active material obtained in Example 1, and (f) is an EDS analysis result of the metal sulfide powder containing FeS2 and Fe7S8 in the negative electrode active material obtained in Example 1.
[0071] From Fig. 3(a), (b) and (c), it was found that the negative electrode active material obtained in Example 1 had a leaf-like structure. Moreover, from Fig. 4(d) and (e), since the SAED pattern showed multiple concentric circles, it was confirmed that the metal sulfide containing FeS2 and Fe7S8 was a hybrid heterojunction. Moreover, from the EDS analysis result of Fig. 3(f), it was also confirmed that Fe and S elements were uniformly distributed in the negative electrode active material (metal sulfide) obtained in Example 1.
[0072] FIG. 4 shows the results of a constant current charge / discharge test of the batteries assembled in Preparation Example 1 (negative electrode active material of Example 1) and Preparation Example 2 (negative electrode active material of Comparative Example 1). The measurements were performed using a LAND battery test system "CT2001A" (Wuhan LAND electronics Co., Ltd. China). The measurement temperature was 30° C., and the applied voltage was 0.3 to 3 V (1 Ag -1 In FIG. 4, the first Y axis represents the capacity (mAhg -1 ), and the second Y-axis indicates coulombic efficiency (%).
[0073] Table 1 shows the initial capacity (mAhg -1 ), initial coulombic efficiency (%), and capacity retention (%) at the 200th cycle.
[0074] As can be seen from Table 1 and FIG. 4, the battery (Preparation Example 1) using the negative electrode active material obtained in Example 1 exhibited high capacity retention even after the second cycle, and had a capacity of 685.2 mAhg at the 200th cycle. -1This corresponds to a capacity retention rate of 93.1% based on the charge capacity at the second cycle, and it was confirmed that the negative electrode active material of Comparative Example 1 has extremely superior cycle characteristics.
[0075] [Table 1]
[0076] FIG. 5(a) shows the results of evaluating the cycle capacity characteristics of the batteries assembled in Preparation Example 1 and Preparation Example 2 with changes in current density. FIG. 5(b) shows the results of evaluating the cycle capacity characteristics of the batteries assembled in Preparation Example 1 with changes in current density. -1 The results show the cycle characteristics at 1000 s.
[0077] As shown in FIG. 5(a), the current density of the battery of Preparation Example 1 was 0.1 to 0.2, 1.0, 2.0, 5.0, 10 and 20Ag -1 When the concentration was increased to 721.4, 730.7, 673.2, 649.8, 563.7, 486.3, and 307.2 mAhg, respectively. -1 The reversible capacity was achieved by setting the current density at 0.1Ag -1 When reverted back to 747.7mAhg -1 Therefore, it was revealed that the battery using the negative electrode active material obtained in Example 1 had excellent cycle capacity characteristics.
[0078] As shown in FIG. 5(b), the battery of Example 1 has a 2Ag -1 So, after 1100 cycles, it was 631.9mAhg. -1 It was also found that a high charging capacity could be achieved.
Claims
1. A negative electrode active material for a sodium ion battery containing a metal sulfide, The metal sulfide is FeS 2 and Fe 7 S 8 A negative electrode active material for a sodium ion battery comprising:
2. A negative electrode active material for a sodium ion battery containing a metal sulfide, The metal sulfide is a sulfide containing at least one metal selected from the group consisting of Cr and Ni.
3. 2. The negative electrode active material for a sodium ion battery according to claim 1, wherein the metal sulfide is a powder having a leaf-like structure.
4. A negative electrode material comprising the negative electrode active material for a sodium ion battery according to any one of claims 1 to 3.
5. A sodium ion battery comprising the negative electrode material of claim 4.
6. A method for producing a negative electrode active material for a sodium ion battery according to any one of claims 1 to 3, A step 1 of heating a raw material liquid containing an iron source to obtain a precursor; step 2 of heat-treating the precursor in the presence of a sulfur source to produce a metal sulfide; A method for producing a negative electrode active material comprising the steps of:
Citation Information
Patent Citations
Negative electrode active material, negative electrode material, alkaline ion battery including negative electrode material, and manufacturing method of negative electrode active material
JP2022123563A
Porous materials for battery electrodes
WO2021216769A1