Styrenic resin composition, injection molding and on-vehicle component

The styrenic resin composition addresses mechanical weaknesses and welding issues of styrene-unsaturated carboxylic acid resins by incorporating core-shell rubber particles and additives, enhancing toughness and weldability while enabling chemical recycling.

JP2024148172APending Publication Date: 2024-10-17PS JAPAN CORP

Patent Information

Application Number
JP2024061114
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-04
Filing Date
2024-04-04
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Styrene-unsaturated carboxylic acid resins lack sufficient mechanical strength, particularly impact resistance, and face issues with compatibility during thermal welding of resin components, leading to potential separation, and are difficult to recycle due to the generation of cyanide gas.

Method used

A styrenic resin composition comprising styrene-unsaturated carboxylic acid resin, core-shell rubber particles, and optional additives like impact-resistant styrenic resin, acrylic elastomer, and lubricating oil, with specific mass ratios to enhance toughness, rigidity, and weldability, particularly with acrylic resin materials.

Benefits of technology

The composition achieves improved heat resistance, toughness, and weldability, reducing the risk of separation during thermal welding and facilitating chemical recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148172000001
    Figure 2024148172000001
  • Figure 2024148172000002
    Figure 2024148172000002
  • Figure 2024148172000003
    Figure 2024148172000003
Patent Text Reader

Abstract

To provide a styrenic resin composition which is excellent in heat resistance, toughness, rigidity, and weldability to an acrylic resin material. A styrenic resin composition contains a styrene-unsaturated carboxylic acid-based resin (A) containing a styrenic monomer unit (a1) and an unsaturated carboxylic acid-based monomer unit (a2), and rubbery particles (B) having a core-shell structure containing a (meth)acrylate monomer unit (b1), wherein, with respect to the total amount (100 mass%) of the styrenic resin composition, the content of the styrene-unsaturated carboxylic acid-based resin (A) is 40 mass% to 95 mass%, and the content of the rubbery particles (B) is 5 mass% to 60 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a styrene-based resin composition, an injection-molded article formed using the styrene-based resin composition, and an in-vehicle part made of the injection-molded article. [Background technology]

[0002] Styrene-unsaturated carboxylic acid resins, such as styrene-methacrylic acid copolymer resins, are excellent in heat resistance, transparency, rigidity, and appearance, are inexpensive, and can be easily reused by thermal decomposition into styrene monomers, and have excellent chemical recycling properties, and therefore are widely used as packaging materials for food containers such as lunch boxes and side dishes, foam boards for residential insulation, diffusion plates for liquid crystal televisions containing a diffusion agent, etc. Therefore, future development is expected for applications requiring heat resistance, such as vehicle lighting fixtures such as headlamps, rear lamps, fog lamps, and turn lamps, or vehicle interior and exterior materials, home appliances, or office automation equipment. However, compared with general-purpose styrene-based resins, styrene-unsaturated carboxylic acid-based resins have a problem in that they are inferior in mechanical strength, and therefore there is a demand for a technology that can impart mechanical strength to the styrene-unsaturated carboxylic acid-based resins. For example, Patent Document 1 describes a technique for improving toughness while maintaining practical heat resistance by blending a styrene-methacrylic acid copolymer with impact-resistant polystyrene and a methyl methacrylate-butadiene-styrene copolymer (hereinafter also referred to as MBS resin). On the other hand, Patent Documents 2 and 3 are cited as technologies related to materials used in vehicle lamps. Patent Document 2 discloses a technology that solves the problem that a lamp in which a methyl methacrylate resin having a molecular weight of about 100,000, which is the material of a lamp lens, and an ABS resin, which is the material of a lamp body, are thermally welded together, and that the joint of the lenses is prone to cracking due to welding distortion. More specifically, a technology is disclosed relating to a resin composition in which a multilayer structure polymer including a soft rubber layer is blended with a methacrylic resin. Patent Document 3 discloses a technology related to a resin composition in which a maleimide copolymer composed of an aromatic vinyl monomer unit, a vinyl cyanide monomer unit, and a maleimide monomer unit is kneaded and mixed with one or more resins selected from ABS resin, ASA resin, AES resin, and SAN resin. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-44086 A [Patent Document 2] Japanese Patent Application Publication No. 07-282602 [Patent Document 3] International Publication No. 2021 / 006265 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the technology of Patent Document 1 above did not improve mechanical strength sufficiently. In particular, the improvement in impact resistance when a notch is provided was insufficient, and it was confirmed that increasing the amount of MBS resin to improve impact resistance did not provide sufficient heat resistance and rigidity. As described in Patent Document 2 above, heat welding such as hot plate welding has been used as a means for joining a resin lamp lens and a resin lamp body. However, when joining resin molded products together, a new problem occurs in that the lamp lens and the lamp body may peel off due to the compatibility between different resins. Furthermore, although the technology of Patent Document 3 above considers chemical resistance, heat resistance, impact resistance, and fluidity, it does not consider toughness, rigidity, or thermal weldability between different resins. In addition, in response to the recent trend toward the creation of a recycling-oriented society, there is a demand for chemical recycling of resin materials, etc. However, since ABS resin is difficult to recycle due to the generation of cyanide gas, alternatives to ABS resin are required. Therefore, an object of the present disclosure is to provide a styrene-based resin composition that is excellent in heat resistance, toughness, rigidity, and weldability with acrylic resin materials. [Means for solving the problem]

[0005] The present inventors have conducted intensive research in view of the above problems, and as a result, have succeeded in realizing a styrene-based resin composition excellent in heat resistance, toughness, rigidity, and adhesion to acrylic resin materials by containing a predetermined amount of a styrene-unsaturated carboxylic acid-based resin (A) and a core-shell rubber-like particle (B), an injection molded article using the same, and an on-vehicle part made of the injection molded article, thereby completing the present disclosure. That is, the present disclosure is as follows.

[0006] [1] A styrene-based resin composition comprising: a styrene-unsaturated carboxylic acid-based resin (A) containing a styrene-based monomer unit (a1) and an unsaturated carboxylic acid-based monomer unit (a2); and a core-shell rubber-like particle (B) containing a (meth)acrylic acid ester monomer unit (b1), A styrene-based resin composition, wherein the content of the styrene-unsaturated carboxylic acid-based resin (A) is 40% by mass to 95% by mass, and the content of the rubber-like particles (B) is 5% by mass to 60% by mass, relative to the total amount (100% by mass) of the styrene-based resin composition.

[0007] [2] The styrene-based resin composition according to [1] above, wherein the core-shell rubber particles (B) further contain styrene-based monomer units (b4), and the content of the styrene-based monomer units (b4) is 5 mass% or less relative to the total amount (100 mass%) of the core-shell rubber particles (B).

[0008] [3] The styrene-based resin composition according to [1] or [2], wherein the content of the (meth)acrylic acid ester monomer unit (b1) contained in the rubber-like particles (B) having a core-shell structure is 3 to 40 mass% based on the total amount (100 mass%) of the rubber-like particles (B) having a core-shell structure.

[0009] [4] The styrene-based resin composition according to any one of [1] to [3] above, wherein the rubber-like particles (B) having a core-shell structure further contain conjugated diene monomer units (b2), and the content of the conjugated diene monomer units (b2) is 50 to 90 mass% relative to the total amount (100 mass%) of the rubber-like particles (B) having a core-shell structure.

[0010] [5] The styrene-based resin composition according to any one of [1] to [4], further comprising 0.5 to 30 mass% of an impact-resistant styrene-based resin (C) relative to the total amount (100 mass%) of the styrene-based resin composition.

[0011] [6] The styrene-based resin composition according to any one of [1] to [5] above, further comprising 0.05 to 3.00 mass % of a lubricating oil (G).

[0012] [7] The styrene-based resin composition further contains a lubricating oil (G), and the core-shell rubber particles (B) further contain a styrene-based monomer unit (b4); The styrene-based resin composition according to any one of [1] to [6], wherein, when the content of the styrene-based monomer unit (b4) is Y and the content of the lubricating oil (G) is X, Y / X≦10.

[0013] [8] The styrene-based resin composition according to any one of the items [1] to [7], wherein the lubricating oil (G) is a silicone oil.

[0014] [9] The styrene-based resin composition according to any one of [1] to [8], wherein the core-shell rubber particles (B) further contain one or more selected from the group consisting of conjugated diene monomer units (b2) and siloxane monomer units (b3), and the total content of the conjugated diene monomer units (b2) and the siloxane monomer units (b3) is 50 mass% or more based on the total amount (100 mass%) of the core-shell rubber particles (B).

[0015]

[10] Notched Charpy impact strength (ISO179 compliant, test condition 1eA) is 4.0kJ / m 2 The styrene-based resin composition according to any one of the above items [1] to [9].

[0016]

[11] The styrene-based resin composition according to any one of [1] to

[10] , wherein the total content of all styrene-based monomer units is 72 mass% or less, based on the total amount (100 mass%) of the styrene-based resin composition.

[0017]

[12] The styrene-based resin composition according to any one of [1] to

[11] above, further comprising 0.5 mass% or more of one or more selected from the group consisting of an impact resistant styrene-based resin (C), a styrene-based elastomer (D) and an acrylic elastomer (E) relative to the total amount (100 mass%) of the styrene-based resin composition.

[0018]

[13] The styrene-based resin composition according to any one of [1] to

[12] , further comprising 1.0 mass% or more of an acrylic resin (F) relative to the total amount (100 mass%) of the styrene-based resin composition.

[0019]

[14] The styrene-based resin composition according to any one of [1] to

[12] above, which has a lightness (L*) of 50 or less.

[0020]

[15] An injection-molded article obtained by injection molding the styrene-based resin composition according to any one of [1] to

[14] above.

[0021]

[16] The injection molded article according to

[15] above, which is welded to an acrylic resin material.

[0022]

[17] The injection molded article according to

[15] or

[16] , which is used for mounting on a vehicle. Effect of the Invention

[0023] According to the present disclosure, there is provided a styrene-based resin composition for use in a molded article having excellent heat resistance, toughness, rigidity, and weldability with an acrylic resin material. According to the present disclosure, it is possible to provide an injection molded article having excellent heat resistance, toughness, rigidity, and weldability with acrylic resin materials, and an in-vehicle part made of the injection molded article. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment, and can be modified in various ways within the scope of the gist of the present invention.

[0025] [Styrene-based resin composition] The styrene-based resin composition in this embodiment (hereinafter, sometimes simply referred to as a resin composition) contains a styrene-unsaturated carboxylic acid-based resin (A) having a styrene-based monomer unit (a1) and an unsaturated carboxylic acid-based monomer unit (a2), and rubber-like particles (B) having a core-shell structure containing (meth)acrylic acid ester monomer units (b1), and the content of the styrene-unsaturated carboxylic acid-based resin (A) is 40% by mass to 95% by mass and the content of the rubber-like particles (B) is 5% by mass to 60% by mass relative to the total amount (100% by mass) of the styrene-based resin composition. In addition, the styrene-based resin composition in the present embodiment may further contain, as necessary, one or more selected from the group consisting of an impact resistant styrene-based resin (C), a styrene-based elastomer (D), an acrylic elastomer (E), an acrylic resin (F) and a lubricating oil (G). This makes it possible to provide a styrene-based resin composition that is excellent in heat resistance, toughness, rigidity, and weldability with acrylic resin materials, particularly in thermal weldability. As a method for welding or joining (particularly, heat welding or heat joining) general resin molded products together, for example, joining with adhesive such as hot melt, heat joining by thermal melting such as hot plate welding, vibration welding using frictional heat generated by vibrating the joint between resin molded products, laser welding using heat absorbed by the joint by irradiating a laser beam to the joint between resin molded products, etc. are used. However, in any welding or joining method, when welding or joining different resin molded products together, the welding or joining force is greatly influenced by the compatibility between the two resins. The styrene-based resin composition of this embodiment contains a styrene-unsaturated carboxylic acid-based resin (A) of a specific composition and a core-shell structured rubber-like particle (B) containing a (meth)acrylic acid ester monomer unit (b1) in a specific blending amount, and therefore it is considered that a styrene-based resin composition can be provided that exhibits good welding properties (e.g., heat welding properties) particularly with respect to acrylic resin materials, and that the presence of the core-shell structured rubber-like particle (B) provides excellent toughness and rigidity. Hereinafter, each component contained in the styrene-based resin composition in the present embodiment will be described.

[0026] "Styrene-unsaturated carboxylic acid resin (A)" The styrene-unsaturated carboxylic acid resin (A) in this embodiment is a copolymer resin (hereinafter also simply referred to as resin (A)) consisting of a styrene-based monomer unit (a1) and an unsaturated carboxylic acid-based monomer unit (a2) as essential components, and contributes to improving the heat resistance of the styrene-based resin composition. In addition, the styrene-unsaturated carboxylic acid resin (A) may further contain a (meth)acrylic acid ester monomer (a2-2) and / or other monomer unit (a3) ​​as necessary, in addition to the essential components of the styrene-based monomer unit (a1) and the (meth)acrylic acid monomer unit (a2-1). The content of the styrene-unsaturated carboxylic acid resin (A) is 40 to 95 mass%, preferably 45 to 94 mass%, more preferably 50 to 93 mass%, and even more preferably 55 to 92 mass% based on the total amount (100 mass%) of the styrene-based resin composition. By making the content of styrene-unsaturated carboxylic acid resin (A) 40 mass% or more, the effect of imparting heat resistance can be sufficiently obtained, and by making it 95 mass% or less, the effect of improving impact resistance due to the rubber-like particles (B) described below can be obtained. The styrene-unsaturated carboxylic acid resin (A) of the present embodiment is preferably a random copolymer or an alternating copolymer.

[0027] <Styrene-based monomer (a1)> In the styrene-unsaturated carboxylic acid resin (A) of this embodiment, the content of the styrene-based monomer unit (a1) is 60 to 98 mass%, preferably 70 to 97 mass%, more preferably 75 to 95 mass%, even more preferably 80 to 95 mass%, and most preferably 82 to 90 mass%, based on the total amount of the styrene-unsaturated carboxylic acid resin (A). If the content of the styrene-based monomer unit (a1) is less than 60 mass%, it will lead to a decrease in fluidity and moldability, and if it is more than 98 mass%, it will be difficult to contain a desired amount of (meth)acrylic acid monomer unit (a2-1) described below, and in particular, the effect of improving heat resistance by the (meth)acrylic acid monomer unit (a2-1) will not be sufficiently obtained.

[0028] In this embodiment, the styrene-based monomer (a1) is not particularly limited, but examples thereof include styrene, α-methylstyrene, β-methylstyrene, paramethylstyrene, orthomethylstyrene, metamethylstyrene, chlorostyrene, bromostyrene, etc. From an industrial viewpoint, styrene and α-methylstyrene are particularly preferred, and styrene is more preferred. As the styrene-based monomer (a1), these may be used alone or in combination of two or more.

[0029] The abundance ratio of the styrene monomer in the styrene monomer (a1) (=styrene content) is preferably 90.0 mass% or more, more preferably 95.0 mass% or more, even more preferably 99.0 mass% or more, still more preferably 99.5 mass% or more, and most preferably 99.9 mass% or more. By making the content of the styrene monomer in the styrene monomer (a1) 90.0 mass% or more, the polymerization reaction can be easily controlled in an industrial process during the production of the styrene-unsaturated carboxylic acid resin (A), and the polymerization conversion rate can be maintained high.

[0030] In this specification, the term "styrene monomer unit (a1)" refers to a repeating unit constituting a polymer obtained by polymerizing a styrene monomer (a1), and is a repeating unit (or structural unit) in which the carbon-carbon double bond in the styrene monomer (a1) becomes a single bond (-CC-) through a polymerization reaction or crosslinking reaction of the styrene monomer (a1). Other monomer units in this specification have the same meaning.

[0031] <Unsaturated carboxylic acid monomer (a2)> In the styrene-unsaturated carboxylic acid resin (A) of the present embodiment, the unsaturated carboxylic acid monomer unit (a2) improves heat resistance, heat resistance, oil resistance, mechanical strength, scratch resistance, and compatibility with the rubber-like particles (B) and acrylic resin (F) described below, and also improves the weldability of the styrene resin composition with an acrylic resin material, in particular the thermal weldability. The unsaturated carboxylic acid monomer (a2) includes a (meth)acrylic acid monomer (a2-1) and a (meth)acrylic acid ester monomer (a2-2).

[0032] <(Meth)acrylic acid monomer (a2-1)> In the styrene-unsaturated carboxylic acid resin (A) of the present embodiment, the (meth)acrylic acid monomer unit (a2-1) improves heat resistance, oil resistance, and compatibility with the rubber-like particles (B) and acrylic resin (F) described below, or improves the weldability, particularly the thermal weldability, of the entire styrene resin composition to an acrylic resin material. When the styrene-unsaturated carboxylic acid resin (A) of this embodiment contains the (meth)acrylic acid monomer unit (a2-1), the content of the (meth)acrylic acid monomer unit (a2-1) is preferably 2 to 40 mass%, more preferably 3 to 35 mass%, more preferably 5 to 30 mass%, even more preferably 8 to 25 mass%, and most preferably 10.5 to 20 mass% based on the total amount of the styrene-unsaturated carboxylic acid resin (A). In another embodiment, the content of the (meth)acrylic acid monomer unit (a2-1) is preferably 3 to 20 mass%, more preferably 4 to 17 mass%, and even more preferably 8 to 14 mass%. If the content of the (meth)acrylic acid monomer unit (a2-1) is less than 2 mass%, the effect of significantly improving heat resistance is insufficient. In addition, if the content of the (meth)acrylic acid monomer unit (a2-1) exceeds 40% by mass, the resin viscosity increases, which leads to a decrease in processability, and the water absorption rate increases, which leads to bubbles during molding, and the viscosity becomes too high during production, which is not preferable. By making the content of the (meth)acrylic acid monomer unit (a2-1) 2% by mass or more, the heat resistance can be improved, and by making the content 40% by mass or less, the viscosity can be prevented from increasing too much. In particular, by making the content of the (meth)acrylic acid monomer unit (a2-1) 8 to 25% by mass, good compatibility with the acrylic resin (F) can be obtained. In addition, when the acrylic resin (F) is further kneaded into the styrene resin composition, the styrene resin composition as a whole can efficiently obtain better weldability to the acrylic resin material, particularly the effect of improving heat weldability and strength.

[0033] In this embodiment, the (meth)acrylic acid monomer (a2-1) may be acrylic acid or methacrylic acid. From an industrial viewpoint, the (meth)acrylic acid monomer unit (a2-1) may be used alone or in combination of two or more. As the (meth)acrylic acid monomer (a2-1), methacrylic acid is particularly preferred because it has a large effect of improving heat resistance.

[0034] <(Meth)acrylic acid ester monomer (a2-2)> In this embodiment, the styrene-unsaturated carboxylic acid resin (A) may further contain a (meth)acrylic acid ester monomer unit (a2-2). The (meth)acrylic acid ester monomer unit (a2-2) plays a role in improving the weldability to the acrylic resin, particularly the effect of improving heat weldability, compatibility with the rubber particles (B) and / or the acrylic resin (F), oil resistance, mechanical strength, and scratch resistance, which are insufficient with the (meth)acrylic acid monomer unit (a2-1) alone. The (meth)acrylic acid ester monomer unit (a2-2) may be a monomer unit represented by the following general formula (1): [ka] (In the above general formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 2 represents an ester substituent, specifically, represents an alkyl group having 1 to 12 carbon atoms. In this embodiment, the ester substituent of the (meth)acrylic acid ester monomer unit (a2-2) (R 2 The number of carbon atoms in the ester substituent is preferably 10 or less, more preferably 8 or less, and even more preferably 4 or less. If the number of carbon atoms in the ester substituent exceeds 10, the effect of lowering heat resistance is significant, which is not preferred.

[0035] In the present embodiment, the (meth)acrylic acid ester monomer (a2-2) may, for example, be methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, or decyl (meth)acrylate. These may be used alone or in combination. As the (meth)acrylic acid ester monomer (a2-2), methyl (meth)acrylate or butyl (meth)acrylate is preferred from the viewpoint of industrial availability, and methyl methacrylate is particularly preferred from the viewpoint of suppressing a decrease in heat resistance. When the styrene-unsaturated carboxylic acid resin (A) of the present embodiment contains the (meth)acrylic acid ester monomer unit (a2-2), the content of the (meth)acrylic acid ester monomer unit (a2-2) in the styrene-unsaturated carboxylic acid resin (A) is, for example, preferably in a range of 1 to 40 mass%, more preferably 2 to 32 mass%, more preferably 3 to 20 mass%, even more preferably 3 to 17 mass%, still more preferably 3 to 15 mass%, and most preferably 4 to 10 mass%, relative to the total amount of the styrene-unsaturated carboxylic acid resin (A).

[0036] <Preferable form of styrene-unsaturated carboxylic acid resin (A)> The styrene-unsaturated carboxylic acid resin (A) of this embodiment may be a multipolymer containing (meth)acrylic acid monomer units (a2-1) and (meth)acrylic acid ester monomer units (a2-2). That is, the styrene-unsaturated carboxylic acid resin (A) of this embodiment may be a binary copolymer of the styrene monomer units (a1) and (meth)acrylic acid monomer units (a2-1), a ternary copolymer in which the styrene monomer (a1), the (meth)acrylic acid monomer (a2-1), and the (meth)acrylic acid ester monomer (a2-2) are copolymerized, or a ternary copolymer containing the styrene monomer units (a1) and two kinds of (meth)acrylic acid monomer units (a2-1). This further improves the effects of heat welding to the acrylic resin material, compatibility with the rubber particles (B) and the acrylic resin (F), surface hardness, and mechanical strength. In addition, the effect of improving the thermal weldability between the styrene-based resin composition and the acrylic resin material can be obtained. In addition, when an unsaturated carboxylic acid ester monomer unit such as the (meth)acrylic acid ester monomer unit (a2-2) is arranged adjacent to an unsaturated carboxylic acid monomer unit such as the (meth)acrylic acid unit (a2-1) in the polymer chain, an effect such as suppressing a crosslinking reaction between unsaturated carboxylic acids can be obtained.

[0037] In particular, when attaching importance to the thermal weldability with the acrylic resin material and the compatibility with the rubber particles (B), and attaching importance to the impact resistance improvement effect of the rubber particles (B), and the improvement of the weldability between the styrene resin composition and the acrylic resin material, especially the effect of improving the thermal weldability, the styrene-unsaturated carboxylic acid resin (A) is preferably a terpolymer in which the styrene monomer unit (a1), the (meth)acrylic acid monomer unit (a2-1), and the (meth)acrylic acid ester monomer unit (a2-2) are copolymerized. Moreover, the terpolymer is more preferably a random copolymer.

[0038] In the present embodiment, when the styrene-unsaturated carboxylic acid resin (A) has a styrene-based monomer unit (a1), a (meth)acrylic acid monomer unit (a2-1), and a (meth)acrylic acid ester monomer unit (a2-2), the content of the (meth)acrylic acid monomer unit (a2-1) is preferably 2 to 30 mass%, and the content of the (meth)acrylic acid ester monomer unit (a2-2) is preferably more than 0 to 20 mass%, based on the total amount of the styrene-unsaturated carboxylic acid resin (A). More preferably, the content of the (meth)acrylic acid monomer unit (a2-1) is more than 0 to 20 mass%, based on the total amount of the styrene-unsaturated carboxylic acid resin (A). The content of the (meth)acrylic acid monomer unit (a2-1) is 3 to 25 mass%, and the content of the (meth)acrylic acid ester monomer unit (a2-2) is 2 to 17 mass%, more preferably, the content of the (meth)acrylic acid monomer unit (a2-1) is 5 to 20 mass%, and the content of the (meth)acrylic acid ester monomer unit (a2-2) is 3 to 15 mass%, and even more preferably, the content of the (meth)acrylic acid monomer unit (a2-1) is 9 to 17 mass%, and the content of the (meth)acrylic acid ester monomer unit (a2-2) is 4 to 10 mass%. By suppressing the content of the (meth)acrylic acid ester monomer unit (a2-2) to 20 mass% or less, a composition having excellent fluidity during molding can be obtained.

[0039] <Other monomers (a3)> The styrene-unsaturated carboxylic acid resin (A) in this embodiment includes the above-mentioned styrene monomer unit (a1) and the (meth)acrylic acid monomer unit (a2-1) and / or the (meth)acrylic acid ester monomer unit (a2-2). It may further have other monomer units (a3) ​​other than the above. That is, in this embodiment, the other monomer unit (a3) ​​may be copolymerized with a monomer other than the two monomers shown above without any particular limitation as long as it is copolymerizable with the styrene-based monomer unit (a1), the (meth)acrylic acid monomer unit (a2-1) and / or the (meth)acrylic acid ester monomer unit (a2-2) within a range that does not impair the effects of the invention. For example, examples of the other monomer (a3) ​​other than the three monomers shown above include maleic anhydride, maleic acid, fumaric acid, itaconic acid, (meth)acrylonitrile, dimethyl maleate, dimethyl fumarate, diethyl fumarate, ethyl fumarate, maleimide, and nucleus-substituted maleimide. In this embodiment, when the styrene-unsaturated carboxylic acid resin (A) contains another monomer (a3), the content of the other monomer (a3) ​​relative to the total amount of the styrene-unsaturated carboxylic acid resin (A) is preferably 12 mass% or less, more preferably 5 mass% or less, and even more preferably 2 mass% or less.

[0040] <Characteristics of styrene-unsaturated carboxylic acid resin (A)> In the styrene-unsaturated carboxylic acid resin (A) in this embodiment, the contents of the styrene-based monomer unit (a1), the (meth)acrylic acid monomer unit (a2-1), the (meth)acrylic acid ester monomer unit (a2-2) and the other monomer unit (a3) ​​can be quantified using a calibration curve prepared using a resin in which each monomer unit is known, using pyrolysis GC / MS. The melt flow rate of the styrene-unsaturated carboxylic acid resin (A) in this embodiment at 200°C may be preferably 0.2 to 4.0, more preferably 0.3 to 3.5, and even more preferably 0.4 to 3.0. When the melt flow rate is 0.2 or more, it is preferable from the viewpoint of fluidity, and when it is 4.0 or less, it is preferable from the viewpoint of mechanical strength of the resin. In the present disclosure, the melt flow rate is a value measured at 200°C under a load of 5 kg in accordance with ISO 1133.

[0041] The weight average molecular weight (Mw) of the styrene-unsaturated carboxylic acid resin (A) in this embodiment is preferably 100,000 to 400,000 in terms of standard polystyrene, more preferably 120,000 to 300,000, even more preferably 140,000 to 280,000, and still more preferably 170,000 to 230,000. When the weight average molecular weight is 100,000 to 400,000, the styrene-unsaturated carboxylic acid resin (A) obtained has an excellent practical balance between impact strength and fluidity. On the other hand, the number average molecular weight (Mn) of the styrene-unsaturated carboxylic acid resin (A) is preferably in the range of 40,000 to 150,000, more preferably 50,000 to 120,000, and further preferably 60,000 to 110,000. The Z-average molecular weight (Mz) of the styrene-unsaturated carboxylic acid resin (A) is preferably in the range of 200,000 to 700,000, more preferably 250,000 to 500,000, and even more preferably 300,000 to 450,000. The average molecular weights can be measured by gel permeation chromatography using polystyrene as a standard.

[0042] The Vicat softening temperature of the styrene-unsaturated carboxylic acid resin (A) in this embodiment is preferably 105 to 135°C, more preferably 107 to 130°C, even more preferably 108 to 128°C, even more preferably 115°C to 127°C, and most preferably 120 to 126°C. By making the Vicat softening temperature of the styrene-unsaturated carboxylic acid resin (A) 105°C or higher, the heat resistance of the composition can be improved, and by making it 135°C or lower, it becomes easy to knead with the acrylic resin (F). The Vicat softening temperature in this specification is measured according to ISO 306 under a load of 5 kg and a heating rate of 50°C / min or a load of 1 kg and a heating rate of 120°C / min.

[0043] <Method for producing styrene-unsaturated carboxylic acid resin (A)> The method for producing the styrene-unsaturated carboxylic acid resin (A) of this embodiment will be described below. The method for producing the styrene-unsaturated carboxylic acid resin (A) of the present embodiment preferably includes a step of mixing a styrene monomer (a1), an unsaturated carboxylic acid monomer (e.g., a (meth)acrylic acid monomer (a2-1) and / or a (meth)acrylic acid ester monomer (a2-2)), and, if necessary, other monomer units (a3), and a solvent to prepare a mixed solution, a polymerization step of polymerizing the mixed solution to produce a reaction product, and a step of recovering the reaction product. The polymerization method for the styrene-unsaturated carboxylic acid resin (A) is not particularly limited, but for example, a radical polymerization method, among which a bulk polymerization method or a solution polymerization method can be preferably used. Specifically, the polymerization method mainly comprises a polymerization step of polymerizing polymerization raw materials (monomer components) and a devolatilization step of removing volatile matters such as unreacted monomers and polymerization solvent from the polymerization product.

[0044] In this embodiment, when the polymerization raw material is polymerized to obtain the styrene-unsaturated carboxylic acid resin (A), the polymerization raw material composition typically contains a polymerization initiator. Examples of the polymerization initiator include organic peroxides, such as peroxyketals such as 2,2-bis(t-butylperoxy)butane, 1,1-bis(t-butylperoxy)cyclohexane, and n-butyl-4,4-bis(t-butylperoxy)valerate, dialkyl peroxides such as di-t-butyl peroxide, t-butylcumyl peroxide, and dicumyl peroxide, diacyl peroxides such as acetyl peroxide and isobutyryl peroxide, peroxydicarbonates such as diisopropyl peroxydicarbonate, peroxyesters such as t-butylperoxyacetate, ketone peroxides such as acetylacetone peroxide, and hydroperoxides such as t-butyl hydroperoxide. Of these, 1,1-bis(t-butylperoxy)cyclohexane is preferred from the viewpoints of decomposition rate and polymerization rate.

[0045] In this embodiment, a chain transfer agent may be used as necessary during polymerization of the styrene-unsaturated carboxylic acid resin (A). Examples of the chain transfer agent include α-methylstyrene linear dimer, n-dodecyl mercaptan, t-dodecyl mercaptan, and n-octyl mercaptan.

[0046] The polymerization method of the styrene-unsaturated carboxylic acid resin (A) can be solution polymerization using a polymerization solvent. As the polymerization solvent, aromatic solvents such as toluene, ethylbenzene, propylbenzene, butylbenzene, etc. are preferable, and a solvent system in which the solubility of the styrene-unsaturated carboxylic acid resin (A) is adjusted by combining polar solvents such as alcohols or ketones as necessary may be used. In this embodiment, the polymerization solvent is preferably used in the range of 3 to 35 parts by mass, more preferably 5 to 30 parts by mass, relative to 100 parts by mass of the total monomers constituting the styrene-unsaturated carboxylic acid resin (A). If the polymerization solvent exceeds 35 parts by mass relative to 100 parts by mass of the total monomers, the polymerization rate decreases and the molecular weight of the resulting resin also decreases, so that the mechanical strength of the resin tends to decrease. In addition, if the polymerization solvent is less than 3 parts by mass, it may be difficult to control the heat removal during polymerization. It is preferable to add the polymerization solvent in a ratio of 3 to 35 parts by mass relative to 100 parts by mass of the total monomers, because this makes it easier to uniformize the quality and also in terms of controlling the polymerization temperature. Furthermore, when the monohydric alcohol having 10 or more carbon atoms, which is an optional additive component of the styrene-based resin composition of the present embodiment, is added from the polymerization system, it is preferable to add the monohydric alcohol having 10 or more carbon atoms in a proportion of 1 to 10 mass % relative to 100 mass % of the total polymerization solvent.

[0047] The apparatus used in the polymerization step for obtaining the styrene-unsaturated carboxylic acid resin (A) in this embodiment is not particularly limited, and may be appropriately selected according to a general polymerization method for styrene-based resins. For example, in the case of bulk polymerization, a polymerization apparatus having one or more completely mixed reactors connected thereto can be used. The devolatilization step is also not particularly limited, and in the case of bulk polymerization, polymerization is continued until the final amount of unreacted monomer is preferably 40% by mass or less, more preferably 30% by mass or less, and further preferably 20% by mass or less, and devolatilization treatment is performed by a known method in order to remove volatile matters such as unreacted monomer. For example, a normal devolatilization apparatus such as a flash drum, a twin-screw devolatilizer, a thin film evaporator, or an extruder can be used, but a devolatilization apparatus with a small retention portion is preferred. The temperature of the devolatilization treatment is usually about 190 to 280°C, and from the viewpoint of suppressing decomposition, 190 to 260°C is more preferred. The pressure in the devolatilization treatment is usually about 0.13 to 4.0 kPa, preferably 0.13 to 3.0 kPa, and more preferably 0.13 to 2.0 kPa. Desirable devolatilization methods include, for example, a method of removing volatile matters by reducing pressure under heating, and a method of removing volatile matters through an extruder or the like designed for the purpose of removing volatile matters.

[0048] "Rubber-like particles with a core-shell structure (B)" In this embodiment, the rubber-like particles (B) having a core-shell structure containing the (meth)acrylic acid ester monomer unit (b1) (also simply referred to as rubber-like particles (B)) have the role of improving the impact resistance of the styrene-based resin composition, particularly the impact resistance when the styrene-based resin composition has a cutout portion such as a notch, i.e., toughness. The core-shell rubber particle (B) of this embodiment has a structure in which a low glass transition temperature (Tg) crosslinked polymer as a core portion and a shell portion containing a polymer mainly composed of (meth)acrylic acid ester monomer units (b1) and at least a part of the core portion is covered with the shell portion. The rubber particle (B) may have one or more core portions. The low glass transition temperature (Tg) crosslinked polymer constituting the core part is preferably a low glass transition temperature (Tg) crosslinked polymer having as its main component one or more selected from the group consisting of (meth)acrylic acid ester monomer units (b1), conjugated diene monomer units (b2) and siloxane monomer units (b3). The polymer constituting the shell part is preferably a polymer mainly composed of (meth)acrylic acid ester monomer units (b1), and may further contain a styrene-based monomer unit (b4) described below, if necessary. Therefore, the polymer constituting the shell part may be a polymer containing one or more monomer units selected from the (meth)acrylic acid ester monomer units (b1), or a copolymer having one or more monomer units selected from the styrene-based monomer units (b4) and one or more monomer units selected from the (meth)acrylic acid ester monomer units (b1). In this specification, the term "main component" refers to a component that accounts for 50% by mass or more of the total amount of the crosslinked body or polymer, and more preferably 60% by mass or more, 70% by mass or more, 80% by mass or more, 95% by mass or more, and 98% by mass or more in that order.

[0049] The content of the rubber-like particles (B) having a core-shell structure in this embodiment is 5 to 60% by mass, more preferably 11 to 40% by mass, even more preferably 16 to 35% by mass, even more preferably 17 to 30% by mass, and most preferably 18 to 26% by mass, based on the total amount (100% by mass) of the styrene-based resin composition. By making the content 5% by mass or more based on the total amount (100% by mass) of the styrene-based resin composition, impact resistance can be improved. On the other hand, by making the content 60% by mass or less based on the total amount (100% by mass) of the styrene-based resin composition, deterioration of heat resistance and rigidity can be prevented. In particular, by making the content 16% by mass or more, impact resistance against notches such as notches is improved. Also, by making the content 30% by mass or less, a styrene-based resin composition having an excellent balance between impact resistance and rigidity can be obtained. In addition, the core-shell rubber particles (B) in this specification can be distinguished by an electron microscope in the same manner as the calculation method of the average particle size of the rubber polymer particles (C-2) described later. When the styrene resin composition of this embodiment contains the impact-resistant styrene resin (C) and the core-shell rubber particles (B) described later, the rubber particles (B) and the rubber polymer particles (C-2) are distinguished by an electron microscope. If necessary, the rubber particles (B) and the rubber polymer particles (C-2) may be treated with osmium tetroxide and / or ruthenium complex.

[0050] <(Meth)acrylic acid ester monomer unit (b1)> The core-shell rubber particles (B) of this embodiment contain (meth)acrylic acid ester monomer units (b1). The (meth)acrylic acid ester monomer units (b1) improve the affinity at the styrene-unsaturated carboxylic acid resin (A) interface and play an important role in improving the impact resistance of the entire styrene resin composition by the rubber particles (B), as well as improving the weldability with acrylic resin materials, particularly the effect of improving heat weldability, and improving the stability and oil resistance of the rubber particles (B). The (meth)acrylic acid ester monomer unit (b1) may be contained in either the core part and / or the shell part of the rubber-like particle (B) having a core-shell structure. When the (meth)acrylic acid ester monomer unit (b1) is contained in the core part, it may form a composite rubber with a low glass transition temperature (Tg) polymer crosslinker mainly composed of a conjugated diene monomer unit (b2) or a siloxane monomer unit (b3) described later, and not only improves impact resistance by generating internal crazes, but also improves thermal stability and oil resistance. On the other hand, when the (meth)acrylic acid ester monomer unit (b1) is contained in the shell part, it improves the affinity of the styrene-unsaturated carboxylic acid resin (A) interface, thereby improving impact resistance. In addition, it also improves the weldability of the styrene resin composition with the acrylic resin material, particularly the heat weldability. In another embodiment of the core-shell rubber particles (B) in this embodiment, the core and / or shell may be composed mainly of (meth)acrylic acid ester monomer units (b1). This not only improves impact resistance by internal craze generation, but also improves thermal stability or weather resistance. Since the core has a relatively low glass transition temperature (Tg) and preferably has high affinity with the styrene-unsaturated carboxylic acid resin (A), the number of carbon atoms of the ester substituent of the (meth)acrylic acid ester monomer units (b1) is preferably 1 to 10, more preferably 2 to 7, and even more preferably 3 to 5. The core portion of the rubber-like particle (B) having a core-shell structure may be composed only of (meth)acrylic acid ester monomer units (b1), or the shell portion of the rubber-like particle (B) may be composed only of (meth)acrylic acid ester monomer units (b1).

[0051] The chemical structure of the (meth)acrylic acid ester monomer unit (b1) is preferably a monomer unit represented by the following general formula (1), similar to the (meth)acrylic acid ester monomer unit (a2-2). [ka] (In the above general formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 2 represents an ester substituent, specifically, represents an alkyl group having 1 to 12 carbon atoms. In this embodiment, the ester substituent of the (meth)acrylic acid ester monomer unit (b1) (R 2 The number of carbon atoms of ) is preferably 10 or less, more preferably 7 or less, and even more preferably 4 or less. In particular, by making it 7 or less, affinity at the interface with the styrene-unsaturated carboxylic acid resin (A) can be maintained.

[0052] Examples of the (meth)acrylic acid ester monomer (b1) in this embodiment include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and decyl (meth)acrylate. These can be used alone or in combination. As the (meth)acrylic acid ester monomer (b1), methyl (meth)acrylate or butyl (meth)acrylate is preferred from the viewpoints of industrial availability, thermal stability, heat resistance, and interface affinity with the styrene-unsaturated carboxylic acid resin (A). In particular, methyl methacrylate is preferred from the viewpoints of heat resistance and interface affinity with the styrene-unsaturated carboxylic acid resin (A), and butyl acrylate and methyl acrylate are preferred from the viewpoints of thermal stability. In addition, when the (meth)acrylic acid ester monomer unit (b1) is contained in the core of the rubber-like particle (B) having a core-shell structure and forms a complex with a phase consisting of the conjugated diene monomer unit (b2) and / or the siloxane monomer unit (b3), the (meth)acrylic acid ester monomer unit (b1) is preferably composed mainly of butyl acrylate (more than 50 mass%) from the viewpoint of improving impact resistance. On the other hand, when the (meth)acrylic acid ester monomer unit (b1) is contained in the shell phase, the (meth)acrylic acid ester monomer unit (b1) is preferably composed mainly of methyl methacrylate (more than 50 mass%) and partially containing butyl acrylate and / or methyl acrylate from the viewpoint of affinity at the interface with the styrene-unsaturated carboxylic acid resin (A). In other words, when the (meth)acrylic acid ester monomer units (b1) are contained in the core of the rubber-like particle (B) and form a complex with a phase consisting of the conjugated diene monomer units (b2) and / or the siloxane monomer units (b3), it is preferable that the (meth)acrylic acid ester monomer units (b1) in the core are mainly composed of butyl acrylate. On the other hand, when the (meth)acrylic acid ester monomer unit (b1) is contained in the shell part of the rubber-like particle (B), the (meth)acrylic acid ester monomer unit (b1) in the shell part is preferably mainly composed of methyl methacrylate, and the shell part may partially contain butyl acrylate and / or methyl acrylate.

[0053] In this embodiment, the range of the content of the (meth)acrylic acid ester monomer unit (b1) in the entire core-shell rubber particles (B) is preferably 3 to 40 mass%, next preferably 5 to 35 mass%, more preferably 7 to 30 mass%, even more preferably 10 to 27 mass%, further more preferably 15 to 25 mass%, and most preferably 10 to 22 mass% based on the total amount of the core-shell rubber particles (B). By making it in the range of 3 to 40 mass%, the styrene resin composition has an excellent balance of rigidity and impact resistance, and by making it particularly 7 to 30 mass%, the toughness due to the improvement of the affinity at the interface with the styrene-unsaturated carboxylic acid resin (A) and the weldability of the styrene resin composition to the acrylic resin material, especially the heat weldability, are excellent.

[0054] <Conjugated diene monomer unit (b2)> In this embodiment, the core-shell rubber particles (B) may contain a conjugated diene monomer unit (b2). The conjugated diene monomer (b2) is a diolefin having a pair of conjugated double bonds, such as 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene. From the viewpoint of industrial availability, 1,3-butadiene and 2-methyl-1,3-butadiene (isoprene) are preferred, and 1,3-butadiene is more preferred from the viewpoint of improving impact strength.

[0055] When the core-shell rubber particles (B) contain conjugated diene monomer units (b2), the conjugated diene monomer units (b2) preferably form the core portion. The conjugated diene monomer units (b2) are crosslinked by a radical crosslinking reaction during polymerization or by a crosslinking agent to form a low glass transition temperature (Tg) polymer crosslinked body in the core portion, which promotes craze generation upon impact and improves impact resistance.

[0056] In addition, the conjugated diene monomer (b2) in the rubber-like particle (B) may have multiple structures depending on the position of the double bond to be polymerized and the transfer of the double bond during polymerization. For example, in the case of 1,3-butadiene, a monomer unit is formed that is a mixture of a monomer unit with a 1,4-cis structure, a monomer unit with a 1,4-trans structure, and a monomer unit with a 1,2-vinyl structure. Since all of these are monomer units derived from the conjugated diene monomer (b2), all of these structures are collectively referred to as the conjugated diene monomer unit (b2) in this specification.

[0057] The content of the conjugated diene monomer unit (b2) in the core-shell rubber particles (B) is preferably 50-90% by mass, more preferably 60-87% by mass, even more preferably 65-85% by mass, and even more preferably 68-83% by mass, based on the total mass of the rubber particles (B). By making the content of the conjugated diene monomer unit (b2) 50% by mass or more, impact resistance is greatly improved, which is preferable. In addition, by making it 90% by mass or less, compatibility of the shell with the styrene-unsaturated carboxylic acid resin (A) can be ensured.

[0058] <Siloxane monomer unit (b3)> In this embodiment, the core-shell rubber particles (B) preferably contain a siloxane monomer unit (b3), which is a so-called organosiloxane monomer structure represented by the following general formula (2).

[0059] [ka] (In the above general formula (2), R 3 and R 4 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a phenyl group, and one or more -CH2- in the alkyl group may be replaced with -O- so that they are not adjacent to each other.

[0060] R in the general formula (2) 3 and R 4 is preferably an alkyl group having 1 to 10 carbon atoms or a phenyl group, more preferably an alkyl group having 1 to 7 carbon atoms, even more preferably an alkyl group having 1 to 5 carbon atoms, still more preferably an alkyl group having 1 to 3 carbon atoms, and most preferably a methyl group.

[0061] When the core-shell rubber particles (B) contain siloxane monomer units (b3), the siloxane monomer units (b3) preferably form the core. The siloxane monomer units (b3) are crosslinked with a crosslinking agent to form a low glass transition temperature (Tg) polymer crosslinked body in the core, which promotes craze generation upon impact and improves impact resistance. In addition, the crosslinked material of the siloxane-based monomer unit (b3) may form a composite rubber having an island-in-sea structure morphology together with a crosslinked material of the (meth)acrylic acid ester monomer unit (b1), thereby forming internal crazes in the core portion, thereby improving impact resistance.

[0062] The content of the siloxane monomer unit (b3) in the rubber-like particles (B) having a core-shell structure is preferably in the range of 15 to 90 mass %, more preferably 20 to 80 mass %, and even more preferably 25 to 70 mass %, based on the entire rubber-like particles (B) having a core-shell structure.

[0063] <Styrene-based monomer unit (b4)> The core-shell rubber particles (B) of this embodiment may contain a styrene monomer unit (b4). When the styrene monomer unit (b4) is contained, the styrene monomer unit (b4) preferably forms a shell portion. The styrene monomer (b4) is not particularly limited, but examples thereof include styrene, α-methylstyrene, β-methylstyrene, paramethylstyrene, orthomethylstyrene, metamethylstyrene, chlorostyrene, and bromostyrene. In particular, from an industrial viewpoint, styrene and α-methylstyrene are preferred, and styrene is more preferred. As the styrene monomer (b4), these can be used alone or in a mixture of two or more kinds. In this case, the abundance ratio of the styrene monomer in the styrene monomer (b4) (=styrene content) is preferably 90.0 mass% or more, more preferably 95.0 mass% or more, even more preferably 99.0 mass% or more, even more preferably 99.5 mass% or more, and most preferably 99.9 mass% or more. By setting the content of the styrene monomer in the styrene-based monomer (b4) to 90.0% by mass or more, it becomes easy to control the polymerization reaction in an industrial process, and it becomes easy to control the polymerization conversion rate.

[0064] The content of the styrene monomer unit (b4) contained in the core-shell rubber particles (B) is preferably 30% by mass or less, 25% by mass or less, 22% by mass or less, 18% by mass or less, 14% by mass or less, 12% by mass or less, 10% by mass or less, 8.0% by mass or less, 5.0% by mass or less, 4.0% by mass or less, 3.0% by mass or less, 2.0% by mass or less, 1.0% by mass or less, 0.5% by mass or less, 0.1% by mass or less, more preferably 0% by mass. In particular, by making it 5.0% by mass or less, the affinity of the interface with the styrene-unsaturated carboxylic acid resin (A) is excellent, and the impact resistance improvement effect is easily obtained. In addition, when the core-shell rubber particles (B) contain the styrene monomer unit (b4), the lower limit of the content of the styrene monomer unit (b4) may be more than 0 mass% based on the entire rubber particles (B). The preferred range of the content of the styrene monomer unit (b4) is more than 0 mass% and 5.0 mass% or less based on the entire rubber particles (B).

[0065] <Other monomers (b5)> The core-shell rubber particles (B) in this embodiment may further have (meth)acrylic acid monomer units (b1) and, if necessary, other monomer units (b5) other than the conjugated diene monomer units (b2), the siloxane monomer units (b3) and the styrene monomer units (b4). That is, in this embodiment, the other monomer unit (b5) may be copolymerized with a monomer other than the above-mentioned monomers without any particular limitation, so long as it is copolymerizable with the (meth)acrylic acid monomer unit (b1), and the conjugated diene monomer unit (b2), the siloxane monomer unit (b3), and the styrene monomer unit (b4), which are contained as necessary, within a range that does not impair the effects of the invention. For example, examples of the other monomer (b5) other than the three monomers shown above include maleic anhydride, maleic acid, fumaric acid, itaconic acid, (meth)acrylonitrile, dimethyl maleate, dimethyl fumarate, diethyl fumarate, ethyl fumarate, maleimide, and nucleus-substituted maleimide. In this embodiment, when the core-shell rubber particles (B) have the other monomer (b5), the content of the other monomer (b5) is preferably 12% by mass or less, more preferably 5% by mass or less, and even more preferably 2% by mass or less, based on the entire core-shell rubber particles (B). The content of the other monomer (b5) is preferably in the range of more than 0% by mass and 5.0% by mass or less, based on the entire rubber particles (B).

[0066] <Particle size of core-shell rubber particles (B)> The average particle size of the core-shell rubber particles (B) is preferably 0.10 to 2.0 μm, next preferably 0.12 to 1.7 μm, more preferably 0.14 to 1.2 μm, even more preferably 0.15 to 1.0 μm, still more preferably 0.16 to 0.50 μm, or 0.19 to 0.30 μm. In particular, by making the particle size in the range of 0.10 to 2.0 μm, the effect of improving the impact resistance of the styrene-based resin composition is excellent. In the present disclosure, the average particle size is measured from a cross-sectional observation image taken with a transmission electron microscope, as described later in the Examples section.

[0067] <Preferable morphology of rubber particles (B) having a core-shell structure> The preferred form of the rubber particles (B) having a core-shell structure in this embodiment is that the core is a crosslinked low glass transition temperature (Tg) polymer mainly composed of one or more selected from the group consisting of (meth)acrylic acid ester monomer units (b1), conjugated diene monomer units (b2) and siloxane monomer units (b3), and the shell is a polymer mainly composed of (meth)acrylic acid ester monomer units (b1). Another preferred form of the rubber particles (B) having a core-shell structure in this embodiment is that the core contains a crosslinked low glass transition temperature (Tg) polymer mainly composed of one or more selected from the group consisting of conjugated diene monomer units (b2) and siloxane monomer units (b3), and the shell is a polymer mainly composed of (meth)acrylic acid ester monomer units (b1). In this embodiment, the core-shell rubber particles (B) contain one or more types selected from the group consisting of conjugated diene monomer units and siloxane monomer units, and the total content of the conjugated diene monomer units (b2) or the siloxane monomer units (b3) is preferably 50 mass% or more based on the total amount (100 mass%) of the core-shell rubber particles (B). When emphasis is placed on improving toughness, the preferred form of the low glass transition temperature (Tg) polymer crosslinked material constituting the core part is one that contains conjugated diene monomer units (b2) as the main component, and particularly preferably a polybutadiene rubber that contains butadiene monomer units as the main component. When emphasis is placed on weather resistance as well as on toughness improvement, the core part is preferably composed primarily of one or more selected from the group consisting of (meth)acrylic acid ester monomer units (b1) and siloxane-based monomer units (b3), and is particularly preferably a composite rubber having an islands-in-sea structure composed of a silicone rubber composed primarily of polydimethylsiloxane and an acrylic rubber composed primarily of (n-butyl) acrylate monomer units. A preferred form of the polymer constituting the shell portion is a polymer mainly composed of (meth)acrylic acid ester monomer units (b1), and more preferably the content of methyl methacrylate monomer units is 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, still more preferably 95% by mass or more, still more preferably 97% by mass or more, still more preferably 98% by mass or more, and most preferably 99% by mass or more, based on the total amount of the shell portion. By making the content of methyl methacrylate monomer units 90% by mass or more based on the total amount of the shell portion, it is possible to improve the compatibility at the interface with the styrene-unsaturated carboxylic acid resin (A) and obtain a high toughness improving effect.

[0068] <Method for producing rubber particles (B) with core-shell structure> The method for producing the core-shell rubber particles (B) is preferably an emulsion polymerization method in which rubber latex (e.g., polybutadiene-based rubber latex, polyorganosiloxane-based rubber latex, polyorganosiloxane-acrylic rubber composite latex, etc.) particles (core part) are produced, and then the shell phase is graft-copolymerized. This allows the particle size to be controlled to a desired size.

[0069] <<Impact-resistant styrene resin (C)>> In a preferred embodiment of the present invention, the styrene resin composition preferably contains an impact-resistant styrene resin (C) (also simply referred to as resin (C)). By containing an appropriate amount of the rubber-modified styrene resin (C), the styrene resin composition exhibits a combined effect with the rubber particles (B), and a styrene resin composition or an injection molded article having excellent impact strength can be obtained. The rubber-modified styrene-based resin (C) of this embodiment has a structure in which rubber-like polymer particles (C-2) are dispersed in a styrene-based polymer matrix (C-1) of a resin containing styrene-based monomer units (c1) and, if necessary, other monomer units (c3). The rubber-like polymer particles (C-2) are dispersed in the styrene-based polymer matrix (C-1) of a resin containing styrene-based monomer units (c1) and, if necessary, other monomer units (c3). The rubber-like polymer particles (C-2) are dispersed in a styrene-based polymer matrix (C-1) of a resin containing styrene-based monomer units (c1) and, if necessary, other monomer units (c3). The rubber-like polymer particles (C-2) are grafted to and / or encapsulated in a rubber-like polymer (CR) having conjugated diene-based monomer units (c2) such as polybutadiene monomer units. That is, the impact-resistant styrene resin (C) may be a so-called high impact polystyrene resin (HIPS resin) obtained by polymerizing a styrene monomer (c1) and, if necessary, other monomers (c3) in the presence of a rubber-like polymer (CR). In other words, the impact-resistant styrene resin (C) of this embodiment contains a styrene polymer matrix (C-1) and rubber-like polymer particles (C-2). The rubber-like polymer particles (C-2) are particles composed of a rubber-like polymer (CR), and a styrene polymer composed of a styrene monomer (c1) and, if necessary, other monomers (c3) is grafted to the surface of the particles and / or is encapsulated within the rubber-like polymer particles (C-2). The styrene polymer matrix (C-1) is a continuous phase of a resin composed of a styrene monomer (c1) and, if necessary, other monomers (c3). Furthermore, the rubber-modified styrene-based resin (C) preferably has an islands-in-sea structure in which the rubber-like polymer particles (C-2) (island phase) are present in a styrene-based polymer matrix (C-1) (sea phase). Therefore, the polymer matrix (C-1) contains a styrene-based polymer obtained by copolymerizing a styrene-based monomer (c1) and, if necessary, other monomers (c3). The rubber-like polymer particles (C-2) are crosslinked rubber particles mainly composed of a rubber-like polymer (CR) having a conjugated diene-based monomer unit (c2), and the surface of the particles is grafted with a styrene-based polymer containing the styrene-based monomer unit (c1) and, if necessary, other monomers (c3), and the styrene-based polymer may be further encapsulated in the crosslinked rubber particles.

[0070] When the styrene-based composition of the present embodiment contains an impact-resistant styrene-based resin (C), the content of the impact-resistant styrene-based resin (C) in the styrene-based composition is preferably 0.5 to 30 mass%, more preferably 2 to 25 mass%, even more preferably 3 to 20 mass%, and even more preferably 4 to 17 mass% relative to the total amount of the styrene-based resin composition. In particular, by making the content of the impact-resistant styrene-based resin (C) in the range of 0.5 to 30 mass%, an impact resistance improving effect is exhibited by interaction with the rubber-like particles (B), and by making it in the range of 3 to 20 mass%, a styrene-based resin composition having an excellent impact resistance improving effect and heat welding property to an acrylic resin material can be obtained.

[0071] <Styrene monomer (c1)> In this embodiment, the styrene-based monomer (c1) is not particularly limited, but examples thereof include styrene, α-methylstyrene, β-methylstyrene, paramethylstyrene, orthomethylstyrene, metamethylstyrene, chlorostyrene, bromostyrene, etc. From an industrial viewpoint, styrene and α-methylstyrene are particularly preferred, and styrene is more preferred. As the styrene-based monomer (c1), these can be used alone or in combination of two or more kinds.

[0072] The abundance ratio of the styrene monomer in the styrene monomer (c1) (=styrene content) is preferably 90.0 mass% or more, more preferably 95.0 mass% or more, even more preferably 99.0 mass% or more, even more preferably 99.5 mass% or more, and most preferably 99.9 mass% or more. By making the content of the styrene monomer in the styrene monomer (c1) 90.0 mass% or more, it is easy to control the polymerization reaction in an industrial process during the production of the impact resistant styrene resin (C), and the polymerization conversion rate can be maintained high.

[0073] <Conjugated diene monomer (c2)> The rubber-like polymer (CR) or rubber-like polymer particles (C-2) in this embodiment contain conjugated diene monomer units (c2) as a constituent component. In the present specification, the conjugated diene monomer (c2) is a diolefin monomer having a pair of conjugated double bonds, and examples thereof include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, etc. From the viewpoint of industrial availability, 1,3-butadiene and 2-methyl-1,3-butadiene (isoprene) are preferred. The position of the double bond of the conjugated diene monomer (c2) rearranges during polymerization, and the structure of the conjugated diene monomer unit in the rubber polymer (CR) is, in the case of 1,3-butadiene, a mixture of monomer units having a 1,4-cis structure, a monomer unit having a 1,4-trans structure, and a monomer unit having a 1,2-vinyl structure. All of these are collectively referred to as conjugated diene monomer units (c2). In this embodiment, the content of the conjugated diene monomer unit (c2) in the impact resistant styrene resin (C) is preferably 0.5 to 20.0 mass%, more preferably 1.0 to 15.0 mass%, and even more preferably 2.0 to 13.0 mass%, based on the total amount of the impact resistant styrene resin (C). The content of the conjugated diene monomer unit (c2) in the impact resistant styrene resin (C) and the styrene resin composition can be measured by the procedure described in the Examples section below or a method equivalent thereto.

[0074] <Other monomers (c3)> Examples of the other monomer (unit) (c3), which is an optional component of the impact-resistant styrene-based resin (C) of this embodiment, include (meth)acrylic acid ester-based monomers such as methyl acrylate, ethyl acrylate, propyl acrylate, (n-butyl) acrylate, isopropyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, (n-butyl) methacrylate, and isopropyl methacrylate, as well as maleic anhydride, N-phenylmaleimide, and N-cyclohexylmaleimide. Among these, (n-butyl) acrylate and methyl methacrylate are preferred from the viewpoints of industrial availability and ease of copolymerization with the styrene-based monomer unit (c3), and methyl methacrylate is most preferred from the viewpoints of the heat weldability and heat resistance of the entire styrene-based resin composition to acrylic resin materials. In this embodiment, the content of the other monomer (unit) (c3) in the impact resistant styrene-based resin (C) is preferably 70 mass % or less, and more preferably 60 mass % or less, based on the total amount of the impact resistant styrene-based resin (C).

[0075] In particular, when the impact-resistant styrene resin (C) contains a (meth)acrylic acid ester monomer as the other monomer (c3), the (meth)acrylic acid ester monomer is preferably contained in an amount of 30 to 60 mass%, more preferably 33 to 58 mass%, even more preferably 36 to 56 mass%, and even more preferably 39 to 54 mass% relative to the total amount of the polymer matrix (C-1). By setting the amount in the range of 30 to 60 mass%, compatibility with the styrene-unsaturated carboxylic acid resin (A) is excellent, and by setting the amount in the range of 36 to 56 mass%, a balance between compatibility with the styrene-unsaturated carboxylic acid resin (A) and heat-weldability to acrylic resin materials is excellent.

[0076] <Rubber-like polymer particles (C-2)> In this embodiment, the rubber-like polymer (CR) constituting the rubber-like polymer particles (C-2) in the impact-resistant styrene-based resin (C) is preferably formed from a conjugated diene-based monomer (c2), and more preferably is a polymer having a conjugated diene-based monomer unit (c2). Specific examples of the rubber-like polymer (CR) that can be used include polybutadiene, polyisoprene, natural rubber, polychloroprene, styrene-butadiene copolymer, acrylonitrile-butadiene copolymer, etc., but from an industrial point of view, polybutadiene and styrene-butadiene copolymer are preferred. As the polybutadiene, high-cis polybutadiene having a high cis content, low-cis polybutadiene having a low cis content, or both of these can be used. The structure of the styrene-butadiene copolymer may be a random structure, a block structure, or a combination of these. These rubber-like polymers (CR) may be used alone or in combination of two or more. Saturated rubber obtained by hydrogenating butadiene rubber can also be used.

[0077] In this embodiment, it is preferable that the rubber-like polymer particles (C-2), which are dispersed particles of the rubber-like polymer (CR), contain (occlude) a polymer containing a styrene-based monomer unit (c1) and, if necessary, other monomers (c3). The form of the occlusion is preferably a so-called salami-structured dispersed particle in which the rubber-like polymer (C-2) contains a plurality of island-like domain phases consisting of a polymer having a styrene-based monomer unit (c1). In addition, a polymer containing a styrene-based monomer unit (c1) and, if necessary, other monomers (c3) may be grafted to the surface of the rubber-like polymer particles (C-2).

[0078] In this embodiment, the average particle size of the rubber-like polymer particles (C-2) in the impact-resistant styrene-based resin (C) is preferably 0.4 to 5.0 μm, more preferably 0.5 to 4.0 μm, and even more preferably 0.7 to 3.0 μm. By making it 0.4 μm or more, it is possible to introduce rubber-like polymer particles (C-2) having a large particle size relative to the particle size of the rubber-like particles (B) constituting the styrene-based resin composition, so that it is possible to bear the initial stress concentration when an impact is applied to the styrene-based resin composition. This improves the impact resistance. By making it 5.0 μm or less, the number of particles introduced can be increased. The impact-resistant styrene-based resin (C) is obtained by polymerizing a styrene-based monomer (c1) in a reactor equipped with a stirrer in the presence of a rubber-like polymer (CR), and the average particle size of the rubber-like polymer particles (C-2) can be adjusted by the number of revolutions of the stirrer, the molecular weight of the rubber-like polymer (C-2) used, etc. In the present disclosure, the average particle size of the rubber-like polymer particles (C-2) is a value measured from a cross-sectional observation image by a transmission electron microscope, as shown in the Examples section described later. Note that the rubber-like polymer particles (C-2) are stretched in the orientation field during injection molding or stretched sheet molding, and the particle size increases by about 105 to 400%.

[0079] In this embodiment, the melt flow rate of the impact resistant styrene resin (C) at 200°C is preferably 0.5 to 10.0 g / 10 min, more preferably 0.7 to 8.0 g / 10 min, and even more preferably 1.0 to 7.0 g / 10 min. If the melt flow rate is in the range of 0.5 to 10.0 g / 10 min, the mixture with the styrene-unsaturated carboxylic acid resin (A) is good, and the mechanical strength is also good. In the present disclosure, the melt flow rate is a value measured at 200°C under a load of 5 kg in accordance with ISO 1133.

[0080] When the styrene-based resin composition of the present embodiment contains an impact-resistant styrene-based resin (C), the chloroform-insoluble matter of the styrene-based resin composition is preferably 10% to 40%, more preferably 15% to 35%, and even more preferably 20% to 30%. The "chloroform insoluble matter" of the styrene resin composition refers to the components that are not dissolved in chloroform after adding 1 g of the styrene resin composition to 20 ml of chloroform and shaking at 23°C for 2 hours, and the chloroform insoluble matter can be the total amount of the rubber-like polymer particles (C-2) and the core-shell rubber-like particles (B) in the impact-resistant styrene resin (C) relative to the total amount of the styrene resin composition. The content of the rubber-like polymer particles (C-2) includes the resin encapsulated in the particles and the polymer to be grafted. The content of the rubber-like particles (B) includes the core and shell parts and the polymer to be grafted. Specifically, the "chloroform insoluble matter" is calculated by the following method. 1 g (W1) of the measurement object was weighed out in a precipitation tube, 20 mL of chloroform was added, and the mixture was shaken at 23°C for 2 hours, and then centrifuged for 60 minutes in a centrifuge (Sakuma Seisakusho Co., Ltd., SS-2050A rotor: 6B-N6L) at 4°C, 20,000 rpm, and 45,100×G. The precipitation tube was slowly tilted at about 45 degrees, and the supernatant liquid was decanted and removed. The mass of the insoluble matter containing chloroform was weighed out, and this mass was designated as W5. The mixture was then vacuum dried at 160°C and 3 kPa or less for 1 hour, and cooled to room temperature in a desiccator. The mass of the chloroform insoluble matter was then weighed out, and this mass was designated as W6. The chloroform insoluble matter was then recovered from the precipitation tube. The chloroform insoluble matter and the swelling index of the chloroform insoluble matter were calculated by the following formula. Swelling index of chloroform insoluble matter = (W5 / W6) Chloroform insolubles (%) = (W6 / W1) x 100

[0081] <Production method of impact-resistant styrene resin (C)> The method for producing the impact-resistant styrene-based resin (C) is not particularly limited, but it can be produced by bulk polymerization (or solution polymerization) in which a styrene-based monomer (c1) and, if necessary, other monomers (c3) and a solvent are polymerized in the presence of a rubber-like polymer (CR), bulk-suspension polymerization that transitions to suspension polymerization during the reaction, or emulsion graft polymerization in which a styrene-based monomer (c1) is polymerized in the presence of latex particles that are a rubber-like polymer (C-2). In bulk polymerization, the rubber-like polymer (CR), the styrene-based monomer (c1), and, if necessary, other monomers (c3), an organic solvent, an organic peroxide, and / or a chain transfer agent are continuously supplied to a polymerization apparatus that is composed of a complete mixing reactor or a tank reactor and a plurality of tank reactors connected in series, to produce the resin.

[0082] <<Styrene-based elastomer (D)>> In a preferred embodiment of this embodiment, the styrene-based resin composition further contains a styrene-based elastomer (D) (also simply referred to as elastomer (D)). The styrene-based elastomer (D) used in the styrene-based resin composition of the present disclosure is a block copolymer having a hard block made of a styrene-based monomer (unit) (d1) and a soft block made of a conjugated diene-based monomer (unit) (d2). As the styrene-based elastomer (D), a block copolymer having a hard block made of a styrene-based monomer unit (d1) and a soft block made of a butadiene monomer unit is more preferred. The styrene monomer (d1) may be the same as the styrene monomer (a1) described above, and the conjugated diene monomer (d2) may be the same as the conjugated diene monomer (c2) described above.

[0083] Preferred chain structures of the block copolymerization of the styrene-based elastomer (D) include a styrene-based monomer unit (d1)-butadiene monomer unit diblock type, a styrene-based monomer unit (d1)-butadiene monomer unit-styrene-based monomer unit (d1) triblock type, a butadiene monomer unit-styrene-based monomer unit (d1)-butadiene monomer unit triblock type, etc. From the viewpoint of improving mechanical strength, the styrene-based elastomer (D) is preferably a triblock type block copolymer of a styrene-based monomer unit (d1)-butadiene monomer unit-styrene-based monomer unit (d1).

[0084] The content of the styrene monomer unit (d1) and the conjugated diene monomer unit (d2) constituting the styrene elastomer (D) is preferably 20-70% by mass, more preferably 25-50% by mass, and the content of the conjugated diene monomer unit (d2) is the remainder of 100% by mass, based on the total amount of the styrene elastomer (D). If the content of the styrene monomer unit (d1) is 20-70% by mass, the dispersibility in the styrene-unsaturated carboxylic acid resin (A) is appropriately improved, and a product excellent in mechanical strength and appearance can be obtained. Methods for producing the styrene-based elastomer (D) such as styrene-butadiene elastomer include radical polymerization, anionic polymerization, and polymer reaction methods, with the anionic polymerization method being preferred from the industrial viewpoint.

[0085] When the styrene-based composition of the present embodiment contains a styrene-based elastomer (D), the content of the styrene-based elastomer (D) may be preferably 0.5 to 10.0 mass%, more preferably 1.0 to 7.0 mass%, and even more preferably 1.5 to 4.5 mass%, based on the total amount of the styrene-based resin composition. The styrene-based elastomer (D) in this embodiment is a polymer different from the rubber-like polymer (CR) or the rubber-like polymer particles (C-2).

[0086] <<Acrylic elastomer (E)>> In a preferred embodiment of this embodiment, the styrene-based resin composition preferably contains an acrylic elastomer (E) (also simply referred to as elastomer (E)). The acrylic elastomer (E) used in the styrene-based resin composition of the present disclosure is a block copolymer having a hard block of methyl methacrylate monomer units (e1) and a soft block of acrylic ester monomer units (e2). As the acrylic elastomer (E), a block copolymer having a hard block of methyl methacrylate monomer (unit) and a soft block of acrylic ester monomer units (e2) is more preferred. Thus, the acrylic elastomer (E) is a block copolymer, whereas the acrylic resin (F) described below is a random polymer or an alternating polymer, and thus the two are different. Examples of the acrylic acid ester monomer (e2) include the same monomers as the acrylic acid ester monomer units of the following (meth)acrylic acid ester monomer units (f1).

[0087] Preferred chain structures of the block copolymerization of the acrylic elastomer (E) include a methyl methacrylate-acrylic acid ester (e2) block type, a methyl methacrylate-acrylic acid ester (e2)-methyl methacrylate triblock type, an acrylic acid ester (e2)-methyl methacrylate-acrylic acid ester (e2) triblock type, and the like. From the viewpoint of improving mechanical strength, the methyl methacrylate-acrylic acid ester (e2)-methyl methacrylate triblock type is preferred.

[0088] Regarding the content of the methyl methacrylate monomer (e1) and the acrylic ester monomer (e2) constituting the acrylic elastomer (E), the content of the methyl methacrylate monomer (e1) is preferably 20-65 mass%, more preferably 30-55 mass%, based on the total amount of the acrylic elastomer (E). On the other hand, the content of the acrylic ester monomer (e2) is the remainder of 100 mass%. If the content of the methyl methacrylate monomer (e1) is 20-65%, the dispersibility in the styrene-unsaturated carboxylic acid resin (A) is appropriately improved, and a product excellent in mechanical strength and appearance can be obtained.

[0089] When the styrene-based composition of the present embodiment contains an acrylic elastomer (E), the content of the acrylic elastomer (E) is preferably 0.5 to 20 mass%, more preferably 1 to 10 mass%, and even more preferably 2 to 6 mass%, relative to the total amount of the styrene-based resin composition. By setting the content in the range of 0.5 to 20 mass%, it is possible to suppress a decrease in heat resistance and improve mechanical strength when added to a styrene-based resin composition.

[0090] <<Acrylic resin (F)>> As one aspect of this embodiment, the styrene-based resin composition may contain an acrylic resin (F) (also simply referred to as resin (F)). The acrylic resin (F) contains a (meth)acrylic acid ester monomer unit (f1). The acrylic resin (F) may be a random polymer or an alternating polymer. By containing a predetermined amount of the acrylic resin (F), the styrene-based resin composition as a whole is more effectively able to improve the weldability of the acrylic resin material, in particular, to improve the thermal weldability, impact resistance, oil resistance, and scratch resistance. In this specification, the acrylic resin (F) is a general term for synthetic resins containing more than 40 mass % of (meth)acrylic acid ester monomer units (f1). In the present disclosure, the number average molecular weight (Mn), weight average molecular weight (Mw) and Z average molecular weight (Mz) of the acrylic resin (F) are values ​​measured using gel permeation chromatography (GPC) as described in the Examples section below. The acrylic resin (F) may contain a branched structure, but preferably has a polymer structure that is soluble in various solvents (acetone, tetrahydrofuran, chloroform, etc.).

[0091] When the styrene-based resin composition of the present embodiment contains an acrylic resin (F), the content of the acrylic resin (F) relative to the total amount (100 mass%) of the styrene-based resin composition is preferably 1 to 50 mass%, more preferably 2 to 36 mass%, even more preferably 3 to 31 mass%, even more preferably 6 to 28 mass%, still more preferably 8 to 25 mass%, and most preferably 11 to 22 mass%. By setting the content of the acrylic resin (F) to 1 to 50% by mass, the above-mentioned effects can be obtained while suppressing the decrease in the heat resistance improved by the styrene-unsaturated carboxylic acid resin (A). In this embodiment, when emphasis is placed on the moldability or low moisture absorption of the styrene-based resin composition, the content of the acrylic resin (F) is preferably less than 1 mass % and more preferably less than 0.5 mass % based on the entire styrene-based resin composition. The monomer unit constituting the acrylic resin (F) of this embodiment is a (meth)acrylic acid ester monomer unit (f1), and is preferably a repeating unit containing a (meth)acrylic acid monomer unit (f2) and a (meth)acrylic acid ester monomer unit (f1), or a repeating unit containing two or more kinds of (meth)acrylic acid ester monomer units (f1). In particular, it is more preferable that the acrylic resin (F) contains two or more kinds of (meth)acrylic acid ester monomer units (f1).

[0092] In this embodiment, the content of the (meth)acrylic acid ester monomer unit (f1) is preferably more than 40 mass%, more preferably more than 50 mass%, even more preferably more than 60 mass%, even more preferably more than 70 mass%, even more preferably more than 80 mass%, and most preferably more than 90 mass%, based on the total amount of the acrylic resin (F). By making the content of the (meth)acrylic acid ester monomer unit (f1) more than 40 mass%, it is possible to improve compatibility with the styrene-unsaturated carboxylic acid resin (A), and in particular, by making it more than 90 mass%, it is possible to obtain higher compatibility with the styrene-unsaturated carboxylic acid resin (A). The (meth)acrylic acid ester monomer unit (f1) and the (meth)acrylic acid monomer unit (f2) of this embodiment will be described below.

[0093] <(Meth)acrylic acid ester monomer (f1)> The (meth)acrylic acid ester monomer unit (f1) constituting the acrylic resin (F) of this embodiment includes a methacrylic acid ester monomer unit (f1-1) and an acrylic acid ester monomer unit (f1-2). Examples of the (meth)acrylic acid ester monomer (f1) that is a precursor of the methacrylic acid ester monomer unit (f1) include methyl acrylate, ethyl acrylate, (n-butyl) acrylate, (2-ethylhexyl) acrylate, (n-octyl) acrylate, benzyl acrylate, methyl methacrylate, butyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, cyclohexyl methacrylate, phenyl methacrylate, (2-ethylhexyl) methacrylate, (n-octyl) methacrylate, and benzyl methacrylate. Among them, the (meth)acrylic acid ester monomer (f1) is preferably methyl acrylate, n-butyl acrylate, or methyl methacrylate, because they are industrially readily available and inexpensive. The (meth)acrylic acid ester monomer (f1) may be used alone or in combination, and it is preferable to use two kinds of (meth)acrylic acid ester monomers in combination.

[0094] As a preferred embodiment of the monomer units constituting the acrylic resin (F) of the present embodiment, from the viewpoint of achieving both heat resistance and thermal decomposition property, among the monomer units listed above, it is preferred to contain two kinds of (meth)acrylic acid ester monomers (f1), more preferred is a combination of a copolymerized methacrylic acid ester species and an acrylic acid ester species, further preferred is a methyl methacrylate-methyl acrylate copolymer, a methyl methacrylate-(n-butyl) acrylate copolymer, and most preferred is a methyl methacrylate-methyl acrylate copolymer.

[0095] <(Meth)acrylic acid monomer (f2)> In this embodiment, the (meth)acrylic acid monomer (f2) may be acrylic acid or methacrylic acid. In the present embodiment, when the acrylic resin (F) contains a (meth)acrylic acid monomer (f2), the upper limit of the content of the (meth)acrylic acid monomer unit (f2) relative to the total amount of the acrylic resin (F) is preferably 30 mass% or less, 25 mass% or less, 20 mass% or less, 15 mass% or less, 12 mass% or less, and 10 mass% or less, in that order.

[0096] <Preferable form of acrylic resin (F)> A preferred acrylic resin (F) of this embodiment is preferably a binary or ternary copolymer, and is a methacrylic acid ester-acrylic acid ester copolymer obtained by copolymerizing a methacrylic acid ester species (methacrylic acid ester monomer unit (f1-1)) with an acrylic acid ester species (acrylic acid ester monomer unit (f1-2)), and is preferably a copolymer containing 0.3 to 20 mass% of acrylic acid ester monomer unit (f1-2) based on the total amount of the methacrylic acid ester-acrylic acid ester copolymer, more preferably a copolymer containing 0.5 to 15 mass% of acrylic acid ester monomer unit (f1-2), still more preferably a copolymer containing 1.0 to 12 mass% of acrylic acid ester monomer unit (f1-2), and even more preferably a copolymer containing 1.5 to 10 mass% of acrylic acid ester monomer unit (f1-2).

[0097] The acrylic resin (F) of the present embodiment is preferably a methyl methacrylate-methyl acrylate copolymer, and more preferably a copolymer containing 0.5 to 12 mass% of methyl acrylate based on the total amount of the copolymer, which allows the effect of adding the acrylic resin (F) to be obtained while minimizing the decrease in heat resistance improved by the styrene-unsaturated carboxylic acid resin (A).

[0098] <Other monomers (f3)> The acrylic resin (F) of this embodiment may further have other monomer units (f3) other than the above-mentioned (meth)acrylic acid ester monomer units (f1) and (meth)acrylic acid monomer units (f2). That is, the other monomer (f3) may be copolymerized with a monomer other than the above-mentioned monomers without any particular limitation as long as it is copolymerizable with the (meth)acrylic acid monomer (f2) and / or the (meth)acrylic acid ester monomer (f1) and does not impair the effects of the invention. For example, other monomers (f3) other than the above-mentioned monomers include styrene, maleic anhydride, maleic acid, fumaric acid, itaconic acid, dimethyl maleate, dimethyl fumarate, diethyl fumarate, ethyl fumarate, maleimide, and nucleus-substituted maleimides such as N-phenylmaleimide and N-cyclohexylmaleimide. In this embodiment, the content of the other monomer units (f3) is preferably 0 to 20 mass%, more preferably 0 to 15 mass%, and even more preferably 0 to 10 mass%, based on the total amount of the acrylic resin (F).

[0099] The weight average molecular weight (Mw) of the acrylic resin (F) is preferably 50,000 to 1,000,000, more preferably 60,000 to 900,000, even more preferably 70,000 to 300,000, and even more preferably 80,000 to 250,000. By making the weight average molecular weight (Mw) of the acrylic resin (F) 50,000 or more, strength can be imparted when kneaded with the styrene-unsaturated carboxylic acid resin (A), and by making the weight average molecular weight (Mw) 1,000,000 or less, the viscosity difference with the styrene-unsaturated carboxylic acid resin (A) can be suppressed, the (meth)acrylic resin can be well dispersed in the styrene resin composition, and the generation of unmelted matter derived from the acrylic resin (F) can be suppressed, and a resin composition and an injection molded article with good appearance can be obtained.

[0100] <Method of producing acrylic resin (F)> The method for producing the acrylic resin (F) of the present embodiment is not particularly limited, but it can be produced by processes such as bulk polymerization, solution polymerization with the addition of a solvent, or suspension polymerization in which an organic layer is dispersed in water using a suspending agent and polymerized. In particular, since the acrylic resin (F) has a high viscosity, a polymerization process using suspension polymerization is preferred.

[0101] <<Lubricating Oil (G)>> In a preferred embodiment of the present invention, the styrene resin composition further contains a lubricating oil (G) (also simply referred to as oil (G)). The styrene resin composition containing the lubricating oil (G) exhibits an effect of improving flowability and an effect of improving impact resistance (toughness) due to the interaction with the core-shell structured rubber particles (B) and the impact-resistant styrene resin (C) in the resin composition. The lubricating oil (G) used in this embodiment is a general term for oily or waxy substances at room temperature that have a pour point of 110° C. or lower. The content of the lubricating oil (G) in the styrene-based resin composition of this embodiment is preferably 0.05 to 3.00 mass%, next preferably 0.07 to 2.50 mass%, more preferably 0.10 to 2.30 mass%, further preferably 0.20 to 1.50 mass%, even more preferably 0.30 to 1.50 mass%, further more preferably 0.30 to 1.50 mass%, further more preferably 0.30 to 1.00 mass%, and most preferably 0.40 to 0.70 mass%. If it is 0.05 mass% or less, the effect of improving the fluidity cannot be obtained, and if it is 3.00 mass% or more, the heat resistance is reduced. In particular, by setting it in the range of 0.30 to 1.00 mass%, a styrene-based resin composition having an excellent balance of fluidity, impact resistance, rigidity, and heat resistance can be obtained.

[0102] Specific examples of the lubricating oil (G) used in this embodiment include mineral oils (minerals) produced from crude oil, chemically synthesized oils, natural vegetable oils, etc. Mineral oils include paraffin and naphthene, chemically synthesized oils include poly-α-olefin oligomers, polybutene oligomers, ethylene propylene copolymer oligomers, fatty acid esters, natural gas modified oils (GTL), alkylbenzene, silicone oils, and polyalkylene glycol oligomers, and natural oils include nut oil, tung oil, shea oil, alfalfa oil, poppy seed oil, pumpkin oil, winter squash oil, millet oil, barley oil, quinoa oil, rye oil, kukui oil, passionflower oil, shea butter, aloe vera oil, sweet almond oil, peach kernel oil, soybean oil, and cashew oil. , peanut oil, avocado oil, baobab oil, borage oil, broccoli oil, calendula oil, camellia oil, canola oil, carrot oil, safflower oil, flax oil, rapeseed oil, cottonseed oil, coconut oil, pumpkin seed oil, wheat germ oil, jojoba oil, lily oil, macadamia oil, corn oil, medfoam oil, monoi oil, hazelnut oil, apricot kernel oil, walnut oil, olive oil, evening primrose oil, palm oil, blackcurrant seed oil, kiwi seed oil, grapeseed oil, pistachio oil, musk rose oil, sesame oil, soybean oil, sunflower oil, castor oil, watermelon oil, etc. The lubricating oil (G) may be chemically modified from the above. For example, the amount of double bonds may be adjusted by hydrogenation (hydrogen addition), or the lubricating oil (G) may be epoxidized, aminated, or mercaptoized, as necessary. Liquid paraffin and silicone oil are preferred because they are industrially available. Silicone oil is particularly preferred from the viewpoint of improving impact resistance. The preferred content of silicone oil is the same as the content range of the lubricating oil (G) described above.

[0103] In this embodiment, the kinetic viscosity of the lubricating oil (G) is 1000 mm at 25° C. 2 / s or less, and 20 to 1000 mm 2 / s is more preferable, and 50 to 500 mm 2 / s, and more preferably 70 to 300 mm 2 It is even more preferred that / s.

[0104] The pour point of the lubricating oil (G) in this embodiment is 110 ° C or less, preferably 100 ° C or less, more preferably 90 ° C or less, even more preferably 80 ° C or less, even more preferably 50 ° C or less, even more preferably 30 ° C or less, even more preferably 10 ° C or less, even more preferably 0 ° C or less, even more preferably -20 ° C or less, even more preferably -30 ° C or less, and particularly preferably -40 ° C or less. If the pour point of the lubricating oil (G) is more than 100 ° C, the lubricating oil (G) is difficult to disperse in the styrene resin composition, and the addition or mixing operation becomes difficult. In particular, by using a lubricating oil (G) with a pour point of -30 ° C or less, a high impact resistance improvement effect can be obtained.

[0105] The lubricating oil (G) preferably has a low content of low boiling point components in order to avoid problems with volatile matters during extrusion molding. The 5% distillation temperature, calculated at normal pressure from the reduced pressure distillation method or gas chromatography method according to JIS K2254, is preferably 400°C or higher.

[0106] In this embodiment, when the content of the styrene monomer unit (b4) contained in the core-shell rubber particles (B) is X and the content of the lubricating oil (G) is Y, it is preferable that X / Y≦10. If X / Y≦10, a more excellent effect of improving impact resistance can be obtained.

[0107] The method of adding the lubricating oil (G) to the styrene-based resin composition is not particularly limited, and examples thereof include a method of adding the lubricating oil (G) in the polymerization step, and a method of kneading the lubricating oil (G) using a known kneader such as a single-screw extruder, a twin-screw extruder, or a Banbury mixer. The identity of the lubricating oil (G) in this embodiment can be easily confirmed by a person skilled in the art using a general method. For example, pyrolysis GC-MS, liquid chromatography (LC), 1 H-NMR or 13 Identification, quantification, and molecular weight measurement can be performed using various analytical devices such as C-NMR.

[0108] When the lubricating oil (G) is a silicone oil, the amount added can also be specified in terms of the amount of Si (silicon). In terms of the amount of silicon, the amount is preferably 150 ppm to 10,000 ppm, more preferably 300 ppm to 8,000 ppm, even more preferably 500 ppm to 7,000 ppm, and even more preferably 1,000 ppm to 5,000 ppm, based on the total amount of the styrene-based resin composition (100% by mass). When quantifying the amount of silicon, it can be measured by a method such as plasma emission spectroscopy (ICP method).

[0109] The kinetic viscosity of the silicone oil at 25°C is preferably 10mm 2 / s~5000mm 2 / s, more preferably 15mm 2 / s~3000mm 2 / s, more preferably 20 mm 2 / s~1000mm 2 / s, more preferably 30 mm 2 / s~500mm 2 / s, more preferably 50 mm 2 / s~200mm2 / s.

[0110] Examples of silicone oils include dimethylpolysiloxane, methylphenylpolysiloxane, methylethylpolysiloxane, etc. Among these, dimethylpolysiloxane is preferred because it is commercially available and inexpensive.

[0111] <<Optional Added Ingredients>> In addition to the above components (A) to (G), the styrene-based resin composition of this embodiment may contain various optional additive components that are generally used in known styrene-based resins in order to achieve known functions and effects. Examples of the optional additive components of this embodiment include monohydric alcohols having 10 or more carbon atoms, higher fatty acid surfactants, antioxidants, heat stabilizers, ultraviolet absorbers, light stabilizers, lubricants, release agents, plasticizers, antiblocking agents, antistatic agents, antifogging agents, colorants, etc. There are no particular restrictions on the method of blending, but examples include a method of adding the additives during polymerization and polymerizing them, a method of mixing the additives in advance with a blender before melt-kneading after polymerization and melt-kneading them with an extruder or Banbury mixer, and a method of preparing a high-concentration master batch and kneading them. The styrene-based resin composition of the present embodiment may contain one or more additive components selected from the group consisting of monohydric alcohols having 10 or more carbon atoms, higher fatty acid surfactants, antioxidants, heat stabilizers, UV absorbers, light stabilizers, lubricants, release agents, plasticizers, antiblocking agents, antistatic agents, antifogging agents, and colorants.

[0112] <Monohydric alcohols with 10 or more carbon atoms> In the present embodiment, the monohydric alcohol having 10 or more carbon atoms (hereinafter, simply referred to as alcohol) is an optional additive component, which suppresses gelation of the styrene-unsaturated carboxylic acid resin (A) during molding, and contributes to improving the appearance of the styrene-based resin composition and the molded article made of the styrene-based resin composition having a good appearance. The content of the monohydric alcohol having 10 or more carbon atoms is 0.01 to 1.0 mass%, preferably 0.03 to 0.8 mass%, more preferably 0.05 to 0.6 mass%, and even more preferably 0.07 to 0.5 mass%, based on the total amount (100 mass%) of the styrene-based resin composition. By making the content of the monohydric alcohol having 10 or more carbon atoms 0.01 mass% or more, it is possible to suppress gelation of the styrene-unsaturated carboxylic acid resin (A) during molding processing. On the other hand, by making it 1.0 mass% or less, it is possible to suppress the decrease in heat resistance and the generation of odor. By making the content of the monohydric alcohol having 10 or more carbon atoms 0.07 to 0.5 mass%, a sufficient gel suppression effect can be obtained without particularly decreasing heat resistance.

[0113] The monohydric alcohol having 10 or more carbon atoms is an alcohol having 10 or more carbon atoms and containing one hydroxyl group, and may contain heteroatoms such as oxygen or nitrogen in the carbon chain constituting the alcohol, and may contain bonds other than single bonds such as double bonds, triple bonds, ester bonds, amide bonds, etc. in the carbon chain. The number of carbon atoms is preferably 16 or more, more preferably 17 or more, and even more preferably 18 to 50. The monohydric alcohol having 10 or more carbon atoms may be contained in a styrene-based resin composition or a molded product made of a styrene-based resin composition. Therefore, by making a monohydric alcohol having 10 or more carbon atoms present (or adding it) in a polymerization solution used for polymerizing the styrene-unsaturated carboxylic acid-based resin (A), the monohydric alcohol may remain in the resin composition, which is the final product, or may be added when kneading the styrene-unsaturated carboxylic acid-based resin (A) and the rubber-like particles (B) and mixed in an extruder to contain it.

[0114] In this embodiment, the boiling point of the monohydric alcohol having 10 or more carbon atoms is preferably 260° C. or higher, more preferably 270° C. or higher, and even more preferably 290° C. or higher. If the boiling point of the alcohol is lower than 260° C., it becomes highly volatile and tends to generate an unpleasant odor during molding, etc.

[0115] The monohydric alcohol having 10 or more carbon atoms is not particularly limited, but examples thereof include 1-hexadecanol, isohexadecanol, 1-octadecanol (stearyl alcohol), 5,7,7-trimethyl-2-(1,3,3-trimethylbutyl)-1-octanol, isooctadecanol, 1-isoisoeicosanol, 8-methyl-2-(4-methylhexyl)-1-decanol, 2-heptyl-1-undecanol, 2-heptyl-4-methyl-1-decanol, 2-(1,5-dimethylhexyl)-(5,9-dimethyl)-1-decanol, and polyoxyethylene alkyl ethers.

[0116] The polyoxyethylene alkyl ether is preferably a compound represented by the following general formula (3). [ka] (In the above general formula (3), R is an alkyl group having 12 to 20 carbon atoms, and X represents the average number of ethylene oxides added and is an integer of 1 to 15.) Specific product names of preferred alcohols include "Fine Oxocol 180" manufactured by Nissan Chemical Industries, Ltd., and "Emulgen 109P" and "Kalcol 8098" manufactured by Kao Corporation.

[0117] <Antioxidants> The antioxidant in this embodiment is an optional additive component, and is added to the styrene-based resin composition as necessary for the purpose of long-term stability, molding stability, etc. Examples of the antioxidant include hindered phenol-based antioxidants such as octadecyl-3-(3,5-tertiary butyl-4-hydroxyphenyl)propionate and 4,6-bis(octylthiomethyl)-o-cresol (product Irganox 1076), and phosphorus-based antioxidants such as tris(2,4-di-tertiary butylphenyl)phosphite (product Irgafos 176). These may be used alone or in combination of two or more types as appropriate. In particular, a phenol-based antioxidant, which is a primary antioxidant, and a phosphorus-based antioxidant, which is a secondary antioxidant, are combined to exhibit an excellent synergistic effect. The amount of the antioxidant added is preferably 0.001 to 3.0 mass% relative to the entire styrene-based resin composition (100 mass%), more preferably 0.010 to 2.0 mass%, even more preferably 0.050 to 1.0 mass%, still more preferably 0.080 to 0.8 mass%, and even more preferably 0.1 to 0.6 mass%.

[0118] <Release agent> The release agent in this embodiment is an optional additive component, and it is preferable that the styrene-based resin composition contains a release agent, especially when the composition is subjected to injection molding. The release agent may be contained in the form of an internal lubricant that is kneaded when preparing the styrene-based resin composition, or in the form of an external lubricant that is dry-blended with the styrene-based resin composition immediately after granulation, or in a combination of the two forms.

[0119] The content of the release agent in this embodiment is preferably 0.001 to 2.0% by mass relative to the total amount (100% by mass) of the styrene-based resin composition, and the upper limit is 1.8% by mass or less, 1.7% by mass or less, 1.6% by mass or less, 1.5% by mass or less, 1.4% by mass or less, 1.3% by mass or less, 1.2% by mass or less, 1.1% by mass or less, 1.0% by mass or less, 0.9% by mass or less, 0.8% by mass or less, 0.7% by mass or less, and % or less, and 0.6% or less are more preferable, and the lower limit is preferably 0.003% by mass or more, 0.005% by mass or more, 0.007% by mass or more, 0.009% by mass or more, 0.012% by mass or more, 0.031% by mass or more, 0.066% by mass or more, 0.090% by mass or more, 0.11% by mass or more, 0.16% by mass or more, 0.21% by mass or more, 0.26% by mass or more, and 0.31% by mass or more. By setting the content in the range of 0.001 to 2.0% by mass, a styrene-based resin composition having excellent release properties can be obtained, and by setting the content in the range of 0.01 to 0.8% by mass, a styrene-based resin composition having an excellent balance between release properties and heat resistance can be obtained.

[0120] When the styrene resin composition of the present embodiment contains a release agent as an internal lubricant, the content of the internal lubricant is preferably 0.05 to 2.0 mass%, more preferably 0.10 to 1.5 mass%, more preferably 0.13 to 1.0 mass%, and even more preferably 0.17 to 0.8 mass%, relative to the total amount (100 mass%) of the styrene resin composition. In particular, by setting the content in the range of 0.13 to 1.0 mass%, excessive bleeding out can be suppressed, and a styrene resin composition with excellent release properties can be obtained.

[0121] When the styrene-based resin composition of the present embodiment contains a mold release agent as an external lubricant, the content of the mold release agent as the external lubricant is preferably in the range of 0.005 to 0.5 mass%, more preferably 0.007 to 0.2 mass%, and even more preferably 0.008 to 0.1 mass%, relative to the total amount (100 mass%) of the styrene-based resin composition. In particular, by setting the content in the range of 0.008 to 0.1 mass%, it is possible to suppress mold contamination and obtain a styrene-based resin composition with excellent mold releasability.

[0122] Examples of the release agent of the present embodiment include stearyl alcohol, stearic acid, zinc stearate, calcium stearate, glycerin, glycerol mosstearate, ethylene bisstearic acid amide, stearic acid amide, oleic acid amide, erucic acid amide, glycerin, glycerin monostearate, glycerin distearate, glycerin tristearate and other glycerin-based esters, pentaerythritol stearate, etc. From the viewpoint of compatibility with styrene-based resins, ethylene bisstearic acid amide, stearyl alcohol, stearic acid, zinc stearate, and calcium stearate are preferred.

[0123] <Light stabilizer> The light stabilizer in this embodiment is an optional additive component, and is preferably added as necessary when the styrene-based resin composition is used in applications where light degradation, such as outdoors, is a concern. The light stabilizer does not have ultraviolet absorbing ability itself, but it has a function of preventing the deterioration and coloring of the styrene-based resin composition caused by radicals by capturing and detoxifying photoradicals generated by the styrene-based resin composition absorbing ultraviolet light. Due to this mechanism, it is expected to function as a thermal radical scavenger, so it can also function as a heat stabilizer. As the light stabilizer, a hindered amine-based compound is preferable, and examples of the hindered amine-based compound include secondary amine type, tertiary amine type, and NOR type. The light stabilizer can be used alone or in combination of two or more types, and by using the ultraviolet absorber described later in combination, a higher light resistance effect can be obtained. In other words, it is possible to suppress coloring and strength reduction after exposure due to long-term outdoor use of the styrene-based resin composition or its molded product. Light stabilizers function mainly on the resin surface where photoradical generation is common, so if you want to make them more effective, low molecular weight types are preferable. However, if you want to prevent mold contamination due to excessive bleed-out or if you need a longer-term stabilizing effect, you will need to adjust the molecular weight appropriately or consider using both low molecular weight and high molecular weight types in combination.

[0124] The content of the light stabilizer is preferably 0.001 to 2.0% by mass relative to the total amount of the styrene-based resin composition, with the upper limit being 1.8% by mass or less, 1.6% by mass or less, 1.4% by mass or less, 1.2% by mass or less, 1.0% by mass or less, 0.8% by mass or less, and 0.7% by mass or less being preferred in this order, and the lower limit being 0.005% by mass or more, 0.010% by mass or more, 0.021% by mass or more, 0.051% by mass or more, 0.061% by mass or more, 0.071% by mass or more, 0.079% by mass or more, 0.089% by mass or more, 0.12% by mass or more, and 0.17% by mass or more being preferred in this order. The content of the light stabilizer can be selected from any combination of the upper and lower limits described above.

[0125] The light stabilizer is preferably a hindered amine compound.Specific examples of the hindered amine compound include bis(1,2,2,6-pentamethyl-4-piperidyl)sebacate, bis(1-undecaneoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, N'-bis(2,2,6,6-tetramethylpiperidin-4-yl)hexane-1,6-diamine, butyl(3,5-di-t-butyl- Specific product names include ADK STAB LA-52, ADK STAB LA-57, ADK STAB LA-63P, ADK STAB LA-68, ADK STAB LA-72, ADK STAB LA-77Y, ADK STAB LA-77G, ADK STAB LA-81, manufactured by ADEKA CORPORATION, JF-90G and JF-95, manufactured by Johoku Chemical Co., Ltd., Chimassorb 2020FDL, Chimassorb 944FDL, and Tinuvn 622SF, manufactured by BASF Japan Ltd.

[0126] <Ultraviolet absorbing agent> The ultraviolet absorber in this embodiment is an optional additive component, and is preferably added as necessary when the styrene-based resin composition is used in applications where photodegradation is a concern, such as outdoors. The ultraviolet absorber absorbs ultraviolet light absorbed by the styrene-based resin composition instead of the styrene-based resin composition, converts it into heat or chemical energy, and suppresses the generation of photoradicals due to ultraviolet light absorption by the styrene-based resin composition, thereby suppressing deterioration and coloration of the resin. The ultraviolet absorber is preferably a compound having two or more aromatic rings bonded via a linking group containing an atom having an unpaired electron (oxygen atom, nitrogen atom, sulfur atom, phosphorus atom, etc.), and one or more aromatic rings having a phenolic hydroxyl group. The compound may have a chemical structure that absorbs light, becomes excited, and then converts it into chemical energy. Examples of ultraviolet absorbers include benzotriazole-based compounds, triazine-based compounds, benzophenone-based compounds, benzoate-based compounds, cyanoacrylate-based compounds, oxalic acid anilide-based compounds, malonic acid ester-based compounds, formamidine-based compounds, and salicylate-based compounds. These ultraviolet absorbents can be used alone or in combination of two or more kinds, and by using the light stabilizer and the ultraviolet absorbent in combination, it is possible to achieve a higher light resistance effect, in other words, to suppress coloring and strength reduction after exposure of the styrene-based resin composition. In addition, ultraviolet absorbents that can absorb ultraviolet wavelengths (250 to 350 nm) that are easily absorbed by the resin added to the styrene-based resin composition are preferred. As the ultraviolet absorbing agent, a benzotriazole-based compound, a triazine-based compound, a benzophenone-based compound, or a cyanoacrylate-based compound is more preferable.

[0127] The content of the ultraviolet absorber in this embodiment is preferably 0.001 to 2.0% by mass relative to the total amount of the styrene-based resin composition, with the upper limit being 1.8% by mass or less, 1.6% by mass or less, 1.4% by mass or less, 1.2% by mass or less, 1.0% by mass or less, 0.8% by mass or less, and 0.7% by mass or less being preferred in this order, and the lower limit being 0.005% by mass or more, 0.010% by mass or more, 0.021% by mass or more, 0.051% by mass or more, 0.061% by mass or more, 0.071% by mass or more, 0.079% by mass or more, 0.089% by mass or more, 0.12% by mass or more, and 0.17% by mass or more being preferred in this order. The content of the ultraviolet absorber can be selected from any combination of the upper limit and lower limit values ​​described above.

[0128] Examples of the benzotriazole-based compound include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-tert-octylphenol, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 6-(2-benzotriazolyl)-4-tert-octyl-6'-tert-butyl-4'-methyl-2,2'-methylenebisphenol]2-(2'-hydroxy-3'-tert Specific product names include ADK STAB LA-32, ADK STAB LA-36, and ADK STAB LA-36RG manufactured by ADEKA CORPORATION, JF-77, JF-79, JF-80, JF-83, JF-832, and JAST-500 manufactured by Johoku Chemical Co., Ltd., and Tinuvin P, Tinuvin 234, Tinuvin 234FF, Tinuvin 326, Tinuvin 329, and Tinuvin 360 manufactured by BAST Japan.

[0129] Examples of the triazine-based compound include 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol, 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine, N,N',N''-tri(m-tolyl)-1,3,5-triazine-2,4,6-triamine, 2,4,6-tris(4-butoxy-2-hydroxyphenyl)-1,3,5-triazine, 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1,3,5-triazine, and ethylhexanoyloxyphenyl. Examples of the compound include xyltriazine, 2-(2,4-dihydroxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4,6-tris(2,4-dihydroxyphenyl)-1,3,5-triazine, bemotodinol, 2-(2-hydroxy-4-methoxyphenyl)-4,6-diphenyl-1,3,5-triazine, and 2-(2,4-dihydroxyphenyl)-4,6-diphenyl-1,3,5-triazine. Specific product names include Adeka STAB LA-46 and Adeka STAB LA-F70 manufactured by ADEKA CORPORATION, and Tinuvin 1577ED and Tinuvin 1600 manufactured by BAST Japan.

[0130] Examples of the benzophenone compounds include 2-hydroxy-4-(octyloxy)benzophenone, 2-hydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,4-dihydroxybenzophenone, and 2,2',4,4'-tetrahydroxybenzophenone. Specific product names include Adeka STAB 1413 manufactured by ADEKA Corporation, and Chimassorb 81 and Chimassorb 81 FL manufactured by BAST Japan.

[0131] Two or more kinds of ultraviolet absorbents may be used in combination, and a preferred embodiment is a combination of an ultraviolet absorbent capable of efficiently absorbing the region (wavelength 250-300 nm) where the ultraviolet absorption peak derived from the aromatic of the styrene resin is sensitized with photodegradation, and an ultraviolet absorbent capable of efficiently absorbing the region of ultraviolet rays that most frequently hits the earth's surface (wavelength 300-400 nm). Specifically, as an ultraviolet absorbent capable of efficiently absorbing wavelengths of 250-300 nm, a combination ultraviolet absorbent in which a triazine ultraviolet absorbent is combined with a benzotriazole ultraviolet absorbent or a benzophenone ultraviolet absorbent is preferred.

[0132] <Coloring agent> The colorant in this embodiment is an optional additive component, and is used when it is necessary to color the styrene-based resin composition. In particular, when the styrene-based resin composition is applied as an in-vehicle related member, it is often colored black. By coloring it black, it is possible to impart a preferable appearance for in-vehicle application and resistance to some heat and light. The colorant is not particularly limited, but carbon black, titanium oxide, and organic dyes can be used. Examples of carbon black include those produced by the furnace method (furnace black), channel method (channel black), acetylene method (acetylene black), and thermal method (thermal black).

[0133] When the styrene resin composition is colored black with carbon black, the content of carbon black in the styrene resin composition is preferably 0.05 to 5.0% by mass relative to the total amount (100% by mass) of the styrene resin composition. If the content of carbon black is less than 0.05% by mass, the desired blackness is not expressed and the color becomes grayish, and if the content of carbon black exceeds 5.0% by mass, the blackness does not change. Therefore, from the viewpoint of cost and mechanical strength, it is preferably 5.0% by mass or less. The method of adding the colorant is not particularly limited. It may be added after polymerization, directly mixed during kneading, or added during kneading using a high-concentration master batch.

[0134] <Colorant masterbatch> Hereinafter, a method of adding a colorant, which is an optional additive component in this embodiment, using a master batch will be described. As the base resin of the masterbatch, it is preferable to use the styrene-unsaturated carboxylic acid resin (A) which is an essential component of this embodiment, or the acrylic resin (F) which is a preferred additive component. The content of the base resin in the masterbatch is preferably 30 to 70 mass% relative to the total amount of the masterbatch, more preferably in the range of 40 to 60 mass%. By making it 30 mass% or more, it is possible to impart viscoelasticity as a resin, and it becomes easy to handle. By making it 70 mass% or less, it becomes easy to make the desired amount of colorant exist in the styrene resin composition, and it is also excellent in terms of cost. The content of the colorant in the masterbatch is preferably 30 to 70 mass% relative to the total amount of the masterbatch, more preferably in the range of 40 to 60 mass%, for the same reasons as above.

[0135] When the colorant is a powder pigment such as carbon black, it is preferable to contain a dispersant in addition to the base resin and the colorant when preparing the masterbatch. The dispersant may be any commonly used dispersant, such as higher fatty acid metal salts such as stearic acid, zinc stearate, magnesium stearate, and calcium stearate, higher fatty acid amides such as ethylene bisstearic acid amide, polyethylene wax, and modified polyethylene wax. From the viewpoint of reactivity with the styrene-unsaturated carboxylic acid resin (A), polyethylene wax is preferred. The content of the dispersant is preferably 2 to 20% by mass, more preferably 3 to 17% by mass, based on the total amount of the masterbatch. Although it depends on the amount of the colorant, by making it 2% by mass or more, the colorant can be dispersed, and by making it 20% by mass or less, the decrease in heat resistance of the styrene-based resin composition can be suppressed.

[0136] The masterbatch can be produced by blending the base resin (preferably resin (A) or resin (F)) with a colorant and, if necessary, a dispersant, and then adjusting the blend using a kneading extruder or kneader. The kneading temperature is preferably in the range of 200 to 280°C, and more preferably in the range of 220 to 260°C.

[0137] <<Component configuration of preferred embodiment of styrene-based resin composition>> The styrene-based resin composition of the present embodiment has a resin (A) and rubber-like particles (B) having a core-shell structure, and the total content of the resin (A) and the rubber-like particles (B) having a core-shell structure may preferably be 65 to 100 mass%, more preferably 75 to 95 mass%, based on the entire styrene-based resin composition. The styrene-based resin composition of the present embodiment comprises a resin (A), rubber-like particles (B) having a core-shell structure, and any additive components, and the total content of the resin (A), the rubber-like particles (B) having a core-shell structure, and any additive components preferably accounts for 70 to 100 mass%, and more preferably 80 to 95 mass%, of the entire styrene-based resin composition.

[0138] The styrene-based resin composition of the present embodiment comprises resin (A), rubber-like particles (B) having a core-shell structure, and resin (C), and the total content of the resin (A), the rubber-like particles (B) having a core-shell structure, and the resin (C) is preferably 70 to 100% by mass, and more preferably 80 to 90% by mass, based on the entire styrene-based resin composition. The styrene-based resin composition of the present embodiment comprises resin (A), rubber-like particles (B) having a core-shell structure, resin (C), and any additive components, and the total content of the resin (A), the rubber-like particles (B) having a core-shell structure, resin (C), and any additive components preferably accounts for 85 to 100 mass%, and more preferably 90 to 95 mass%, of the entire styrene-based resin composition. The styrene-based resin composition of the present embodiment comprises resin (A), rubber-like particles with a core-shell structure (B), resin (C), lubricating oil (G), and any additive components, and the total content of the resin (A), the rubber-like particles with a core-shell structure (B), the resin (C), and the any additive components preferably accounts for 85 to 100 mass%, and more preferably 90 to 95 mass%, of the entire styrene-based resin composition.

[0139] The styrene-based resin composition of the present embodiment comprises a resin (A), rubber-like particles (B) having a core-shell structure, and an elastomer (D), and the total content of the resin (A), the rubber-like particles (B) having a core-shell structure, and the elastomer (D) is preferably 70 to 100 mass%, more preferably 75 to 95 mass%, and even more preferably 80 to 90 mass%, based on the entire styrene-based resin composition. The styrene-based resin composition of the present embodiment comprises a resin (A), a rubber-like particle (B) having a core-shell structure, an elastomer (D), and any additive components, and the total content of the resin (A), the rubber-like particle (B) having a core-shell structure, the elastomer (D), and the any additive components preferably accounts for 80 to 100 mass%, more preferably 85 to 97 mass%, and even more preferably 90 to 95 mass%, of the entire styrene-based resin composition. The styrene-based resin composition of the present embodiment comprises a resin (A), a rubber-like particle (B) having a core-shell structure, an elastomer (D), a lubricating oil (G), and any additive components, and the total content of the resin (A), the rubber-like particle (B) having a core-shell structure, the elastomer (D), the lubricating oil (G), and the any additive components is preferably 80 to 100% by mass, more preferably 85 to 97% by mass, and even more preferably 90 to 95% by mass, based on the entire styrene-based resin composition.

[0140] The styrene-based resin composition of the present embodiment comprises a resin (A), rubber-like particles (B) having a core-shell structure, and an elastomer (E), and the total content of the resin (A), the rubber-like particles (B) having a core-shell structure, and the elastomer (E) may preferably be 70 to 100% by mass, and more preferably 80 to 90% by mass, based on the entire styrene-based resin composition. The styrene-based resin composition of the present embodiment comprises a resin (A), a rubber-like particle (B) having a core-shell structure, an elastomer (E), and any additive components, and the total content of the resin (A), the rubber-like particle (B) having a core-shell structure, the elastomer (E), and the any additive components preferably accounts for 85 to 100 mass%, and more preferably 90 to 95 mass%, of the entire styrene-based resin composition. The styrene-based resin composition of the present embodiment comprises a resin (A), a rubber-like particle (B) having a core-shell structure, an elastomer (E), a lubricating oil (G), and any additive components, and the total content of the resin (A), the rubber-like particle (B) having a core-shell structure, the elastomer (E), the lubricating oil (G), and the any additive components preferably accounts for 85 to 100 mass%, and more preferably 90 to 95 mass%, of the entire styrene-based resin composition.

[0141] The styrene-based resin composition of the present embodiment comprises a resin (A), a rubber-like particle (B) having a core-shell structure, and a resin (F), and the total content of the resin (A), the rubber-like particle (B) having a core-shell structure, and the elastomer (F) preferably accounts for 70 to 100 mass%, and more preferably 80 to 90 mass%, of the entire styrene-based resin composition. The styrene-based resin composition of the present embodiment comprises resin (A), rubber-like particles (B) having a core-shell structure, resin (F), and any additive components, and the total content of the resin (A), the rubber-like particles (B) having a core-shell structure, resin (F), and any additive components preferably accounts for 85 to 100 mass%, and more preferably 90 to 95 mass%, of the entire styrene-based resin composition. The styrene-based resin composition of the present embodiment comprises resin (A), rubber-like particles (B) having a core-shell structure, resin (F), lubricating oil (G), and any additive components, and the total content of the resin (A), the rubber-like particles (B) having a core-shell structure, resin (F), the lubricating oil (G), and any additive components preferably accounts for 85 to 100 mass%, and more preferably 90 to 95 mass%, of the entire styrene-based resin composition.

[0142] The styrene-based resin composition of the present embodiment comprises a resin (A), rubber-like particles (B) having a core-shell structure, and a lubricating oil (G), and the total content of the resin (A), the rubber-like particles (B) having a core-shell structure, and the lubricating oil (G) is preferably 70 to 100 mass%, and more preferably 80 to 90 mass%, of the entire styrene-based resin composition. The styrene-based resin composition of the present embodiment comprises a resin (A), a rubber-like particle (B) having a core-shell structure, a lubricating oil (G), and any additive components, and the total content of the resin (A), the rubber-like particle (B) having a core-shell structure, the lubricating oil (G), and any additive components preferably accounts for 85 to 100 mass%, and more preferably 90 to 95 mass%, of the entire styrene-based resin composition.

[0143] <<Preferred embodiment of styrene-based resin composition>> In the styrene-based resin composition of the present embodiment, the styrene-unsaturated carboxylic acid-based resin (A) and the core-shell rubber-like particles (B) preferably have a sea-island structure in which the styrene-unsaturated carboxylic acid-based resin (A) is the sea and the core-shell rubber-like particles (B) are the islands. When a rubber-modified styrene-based resin (C) is used, it is preferable that the matrix portion of the styrene-unsaturated carboxylic acid-based resin (A) and the rubber-modified styrene-based resin (C) is the sea phase, and the rubber particles contained in the rubber-modified styrene-based resin (C) are the island phase. In addition, the rubber particles that become the island phase of the sea-island structure may be a mixture of the core-shell rubber-like particles (B) and the rubber-like polymer particles (C-2) contained in the rubber-modified styrene-based resin (C).

[0144] <<Best mode for styrene resin compositions>> A particularly preferred embodiment of the present invention is a styrene-unsaturated carboxylic acid resin composition containing a styrene-unsaturated carboxylic acid resin (A) containing a styrene-based monomer unit (a1) and an unsaturated carboxylic acid-based monomer unit (a2), a core-shell structured rubber-like particle (B) containing a (meth)acrylic acid ester monomer unit (b1), and a silicone oil, the content of the styrene-unsaturated carboxylic acid resin (A) is 40% by mass to 95% by mass, and the content of the rubber particles (B) is 5% by mass to 60% by mass, relative to the total amount (100% by mass) of the styrene resin composition; the rubber-like particles (B) contain the (meth)acrylic acid ester monomer units (b1), the conjugated diene monomer units (b2) and the styrene monomer units (b4), and, relative to the total amount (100 mass%) of the rubber-like particles (B), the content of the (meth)acrylic acid ester monomer units (b1) is 3 to 40 mass%, the content of the conjugated diene monomer units (b2) is 50 to 90 mass%, and the content of the silicone oil is 0.30 to 1.50 mass%, When the content of the styrene-based monomer unit (b4) is Y and the content of the silicone oil is X, the styrene-based resin composition satisfies Y / X≦10. This provides excellent properties such as heat resistance, toughness, rigidity, and weldability with acrylic resin materials. In particular, the composition as a whole has excellent toughness.

[0145] When a rubber-modified styrene-based resin (C) is used in the styrene-based resin composition of this embodiment, the rubber particles contained in the rubber-modified styrene-based resin (C) may have a core-shell structure or a salami-like structure, and a salami-like structure is particularly preferred from the viewpoint of impact resistance.

[0146] [Physical properties and characteristics of styrene-based resin compositions] The physical properties and characteristics of the styrene-based resin composition in this embodiment will be described below. <Vicat softening temperature (°C) of styrene-based resin composition> In this embodiment, the Vicat softening temperature of the styrene-based resin composition is preferably 110 ° C. or higher, more preferably 112 ° C. or higher, even more preferably 115 ° C. or higher, even more preferably 118 ° C. or higher, and most preferably 120 ° C. or higher. By setting the Vicat softening temperature to 110 ° C. or higher, a molded body with excellent heat resistance can be obtained, and by setting it to 120 ° C. or higher, a molded body usable for in-vehicle parts can be obtained. The Vicat softening temperature can be measured under conditions of a load of 1 kg and a heating rate of 120 ° C. / hour in accordance with ISO306. In addition, it may be measured under conditions of a load of 5 kg and a heating rate of 50 ° C. / hour as necessary, in which case the range of 105 ° C. or higher is preferable, and more preferably the range of 110 ° C. or higher.

[0147] <Melt mass flow rate (g / 10 min) of styrene-based resin composition> In this embodiment, the melt mass flow rate of the styrene-based resin composition is preferably in the range of 1.0 to 20.0 g / 10 min, more preferably 1.0 to 10.0 g / 10 min, more preferably 2.0 to 9.0 g / 10 min, and even more preferably 2.5 to 8.0 g / 10 min. By setting the melt flow rate to 1.0 g / 10 min or more, good moldability can be obtained, and by setting it to 10.0 g / 10 min or less, a resin with excellent strength can be obtained. The melt mass flow rate is a value measured under conditions of 220°C and a load of 10 kg in accordance with ISO1133. In addition, it may be measured under conditions of 200°C and a load of 5 kg as necessary, and in that case, it is preferably in the range of 0.1 to 3.0 g / 10 min, more preferably in the range of 0.2 to 1.5 g / 10 min.

[0148] <Charpy impact strength of styrene resin composition (kJ / m 2 )> In this embodiment, the Charpy impact strength (notched) of the styrene-based resin composition is 4.0 kJ / m 2 More preferably, it is 4.5 kJ / m or more. 2 More preferably, 5.0 kJ / m 2 More preferably, 6.0 kJ / m2 More preferably, 8.0 kJ / m 2 More than 10.0 kJ / m 2 That's it. 4.0kJ / m 2 By setting the compression ratio at 10.0 kJ / m or more, an injection molded article having excellent toughness can be obtained. 2 By doing so, it is possible to obtain an injection molded article having toughness suitable for in-vehicle use.

[0149] <Flexural modulus of styrene-based resin composition (MPa)> In this embodiment, the flexural modulus of the styrene-based resin composition is preferably 2000 MPa or more, more preferably 2100 MPa or more, and further preferably 2200 MPa or more. By setting the flexural modulus to 2000 MPa or more, a molded product having excellent rigidity can be obtained.

[0150] <Tensile yield stress of styrene resin composition (MPa)> In this embodiment, the tensile yield stress of the styrene-based resin composition is preferably 35 MPa or more, more preferably 40 MPa or more, and further preferably 42 MPa or more. By setting the tensile yield stress to 35 MPa or more, a molded product having an excellent balance between rigidity and strength can be obtained.

[0151] <Lightness (L*)(-) of styrene-based resin composition> In this embodiment, the lightness (L*) of the styrene-based resin composition is preferably 50 or less, and more preferably 45 or less, 40 or less, 38 or less, 36 or less, 34 or less, and 32 or less in that order. By setting the lightness (L*) to 50 or less, a styrene-based resin composition and a molded article thereof having excellent light resistance can be obtained, and further, by setting the lightness (L*) to 38 or less, excellent color tone can be obtained.

[0152] <Density of styrene resin composition (g / cm 3 )> In this embodiment, the density of the styrene-based resin composition is 1.20 g / cm 3 Preferably less than 1.15 g / cm 3 More preferably, 1.10 g / cm or less.3 More preferably, 1.09 g / cm 3 More preferably, 1.08 g / cm 3 or less, and even more preferably 1.07 g / cm 3 More preferably, 1.06 g / cm 3 The density is 1.20 g / cm 3 By setting the above as follows, it is possible to contribute to reducing the weight of the molded body.

[0153] <Content of total styrene monomer in styrene resin composition> In this embodiment, the content of all styrene monomer residues contained in the styrene resin composition is preferably 3000 μg / g or less, more preferably 2000 μg / g or less, even more preferably 1500 μg / g or less, even more preferably 1000 μg / g or less, even more preferably 900 μg / g or less, even more preferably 800 μg / g or less, and even more preferably 700 μg / g or less. By making the content of all styrene monomer residues 3000 μg / g or less, it is possible to suppress the generation of bubbles from the heated surface during heat welding. On the other hand, it is preferable to contain 100 μg / g or more because it improves fluidity. The styrene monomer contained in the styrene resin composition is basically a polymerization residue.

[0154] <Content of styrene dimer and trimer in styrene-based resin composition> In this embodiment, the content of styrene dimer and trimer contained in the styrene resin composition is preferably 1.00% by mass or less, more preferably 0.90% by mass or less, even more preferably 0.80% by mass or less, even more preferably 0.70% by mass or less, even more preferably 0.60% by mass or less, even more preferably 0.50% by mass or less, and even more preferably 0.40% by mass or less. By making the content of styrene dimer and trimer 1.00% by mass or less, it is possible to suppress the generation of bubbles from the heated surface during heat welding. On the other hand, it is preferable to contain 0.10% by mass or more because it improves the flowability. The content of styrene dimer and trimer contained in the styrene resin composition is basically a by-product generated during polymerization.

[0155] <Content of all styrene-based monomer units in styrene-based resin composition> In addition, the styrene resin composition in this embodiment has an upper limit of the content of all styrene monomer units (the total amount of styrene monomer units in each resin constituting the styrene resin composition) relative to the total amount (100% by mass) of the styrene resin composition, preferably 72% by mass or less, more preferably 71% by mass or less, 70% by mass or less, 69% by mass or less, 68% by mass or less, 69% by mass or less, and 68% by mass or less in that order. By making the sum of all styrene monomer units in the styrene resin composition 72% by mass or less, a styrene resin composition having excellent thermal adhesion with an acrylic resin material can be obtained. The lower limit of the content of all styrene monomer units is preferably 45% by mass or more, more preferably 46% by mass or more, 47% by mass or more, more preferably 48% by mass or more, 49% by mass or more, 50% by mass or more, and 51% by mass or more in that order. By making the sum of all styrene monomer units in the styrene resin composition 45% by mass or more, a styrene resin composition having easy moldability, low water absorption, and low specific gravity can be obtained. The range of the total content of styrene-based monomer units in the styrene-based resin composition can be any combination of the above upper and lower limits. The total styrene-based monomer units refers to the sum of the styrene-based monomer units (a1) contained in the styrene-unsaturated carboxylic acid resin (A), the styrene-based monomer units (b4) contained in the rubber particles (B) having a core-shell structure described below, the styrene-based monomer units (c1) contained in the impact resistant styrene-based resin (C), the styrene-based monomer units (d1) contained in the styrene-based elastomer (D), the styrene-based monomer units as other monomer units (f3) contained in the acrylic resin (F), and the styrene-based monomer units contained in the constituent components of the styrene-based resin composition including other optional components.

[0156] <Content of total conjugated diene monomer units in styrene-based resin composition> In this embodiment, the content of all conjugated diene monomer units contained in the styrene-based resin composition is preferably 0 to 25 mass%, more preferably 5 to 20 mass%, even more preferably 8 to 19 mass%, and most preferably in the range of 10 to 18 mass%, based on the entire styrene-based resin composition. In particular, by setting the content of all conjugated diene monomer units in the range of 8 to 19 mass%, it is possible to obtain a resin composition having an excellent balance between impact strength and rigidity, and an injection-molded article obtained by molding the composition. The total conjugated diene monomer units is the sum of the conjugated diene monomer units (b2) contained in the rubber particles (B) having a core-shell structure, the conjugated diene monomer (c2) contained in the impact resistant styrene resin (C), the conjugated diene monomer (d2) contained in the styrene elastomer (D), and the conjugated diene monomer units contained in the components of the styrene resin composition including other optional components.

[0157] <Content of all (meth)acrylic acid monomer units in styrene-based resin composition> In this embodiment, the content of all (meth)acrylic acid monomer units contained in the styrene-based resin composition is preferably 2 to 20 mass% relative to the total amount (100 mass%) of the styrene-based resin composition, preferably 3 to 15 mass%, more preferably 4 to 11 mass%, and even more preferably 5 to 9 mass%. When the content of all (meth)acrylic acid monomers in the entire styrene-based resin composition is within the above range, the effect of improving heat resistance and thermal weldability with acrylic resin materials can be sufficiently obtained. The total (meth)acrylic acid monomer units refers to the sum of the (meth)acrylic acid monomer units (a2-1) contained in the styrene-unsaturated carboxylic acid resin (A), the (f2) contained in the acrylic resin (F), and the (meth)acrylic acid monomers contained in the components of the styrene resin composition including other optional components.

[0158] <Content of total methyl acrylate monomer units in styrene-based resin composition> In this embodiment, the content of all methyl acrylate monomer units contained in the styrene-based resin composition is preferably 0 to 10 mass%, and more preferably in the range of 0.3 to 3.0 mass%, relative to the total amount (100 mass%) of the styrene-based resin composition.

[0159] <Total rubber particles in styrene-based resin composition> The average particle size of all the rubber particles contained in the styrene-based resin composition of this embodiment is preferably 0.08 to 5.0 μm, more preferably 0.10 to 4.5 μm, even more preferably 0.12 to 4.0 μm, even more preferably 0.14 to 3.5 μm, even more preferably 0.16 to 3.0 μm, even more preferably 0.16 to 3.0 μm, even more preferably 0.18 to 3.0 μm, even more preferably 0.20 to 2.0 μm, and even more preferably 0.22 to 1.5 μm. When the average particle size of all the rubber particles, so-called apparent rubber particles, is within the above range, the effect of imparting strength to the styrene-based resin composition is maximized. The total amount of all rubber particles (including encapsulated resin) in the entire styrene-based resin composition of this embodiment is preferably 5.0 to 30 mass%, more preferably 8.0 to 28 mass%, even more preferably 10 to 26 mass%, and even more preferably 14 to 26 mass%, relative to the total amount (100 mass%) of the styrene-based resin composition. In particular, when the amount is in the range of 10 to 26 mass%, a styrene-based resin composition with excellent toughness can be obtained. The total rubber particles is the sum of the rubber particles having a core-shell structure (B) and the rubber polymer particles (C-2) (including grafts / occluded particles) contained in the impact resistant styrene resin (C). The average particle size of all the rubber particles is measured using a laser diffraction particle size measuring device under the following conditions. In a disposable polypropylene cup, 1 gmg of the measurement object (styrene resin composition) and 20 mL of N,N-dimethylformamide were placed, and ultrasonic vibration was applied for 3 minutes to dissolve and disperse the mixture. While vibrating, a part of the cloudy sample liquid was taken and placed in a measurement cell. While stirring with a rotor, the particle size (d50%) and integral distribution curve of the dispersed matter of the N,N-dimethylformamide solution containing the styrene resin composition were obtained using a laser diffraction particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.). At this time, the refractive index of the sample was 1.6-0.00i, and the refractive index of the solvent was 1.43.

[0160] [Method of producing styrene-based resin composition] In the present embodiment, the method for producing the styrene-based resin composition is not particularly limited, and the method for blending, melting, kneading, and granulating the styrene-unsaturated carboxylic acid-based resin (A) containing the styrene-based monomer unit (a1) and the unsaturated carboxylic acid-based monomer unit (a2), the core-shell structured rubber-like particles (B) containing the (meth)acrylic acid ester monomer unit (b1), and optional components (at least one selected from the group consisting of the impact-resistant styrene-based resin (C), the styrene-based elastomer (D), the acrylic elastomer (E), the acrylic resin (F), and optional additive components) is not particularly limited, and a method commonly used in the production of general styrene resins can be used. For example, the above-mentioned components blended (mixed) using a drum tumbler, Henschel mixer, etc. are melted and kneaded using a Banbury mixer, a single-screw extruder, a twin-screw extruder, a kneader, etc., and granulated using a rotary cutter, a fan cutter, etc., to obtain the styrene-based resin composition. The resin temperature during melting and kneading is preferably 180 to 240°C. In order to achieve a target resin temperature, it is preferable to set the cylinder temperature of the extruder or the like to a temperature 10 to 20°C lower than the resin temperature. If the resin temperature is less than 180°C, mixing will be insufficient, which is not preferable. On the other hand, if the resin temperature exceeds 240°C, thermal decomposition of the resin will occur, which is not preferable.

[0161] [Molded products] The styrene-based resin composition according to the present disclosure is preferably used for injection blow molding, sheet (including film), injection molding, or extrusion molding. Therefore, this embodiment may be an injection molded article made of a styrene-based resin obtained by injection molding a styrene-based resin composition. Another aspect of this embodiment may be an injection molded article made of a styrene-based resin and an injection molded article having an acrylic resin material welded (for example, heat welded) to the injection molded article. The styrene-based resin composition of the present embodiment can be suitably used in molded articles, preferably injection molded articles (including injection compression), office automation equipment such as copiers, faxes, televisions, radios, tape recorders, video decks, personal computers, printers, telephones, information terminals, refrigerators, and microwave ovens, home appliances, housings and various parts of electric and electronic devices, vehicle lighting fixtures such as headlamps, rear lamps, fog lamps, and turn lamps, or vehicle interior and exterior materials, foamed heat insulating materials, insulating films, and the like. EXAMPLES

[0162] The present invention will now be described in detail with reference to examples and comparative examples, but the present invention is not limited to these examples. The resins, resin compositions, and molded articles in the examples and comparative examples were analyzed and evaluated as follows. [Evaluation of properties of each resin and resin composition] (1) Measurement of the content of each monomer unit The content of each monomer unit contained in each resin and resin composition prepared in the Examples and Comparative Examples was measured by pyrolysis GC / MS under the following conditions. Quantitative values ​​were obtained by a calibration curve method using standard samples with known contents of each monomer unit. <<Sample preparation>> 20 μg of the resin or composition prepared in each of the Examples and Comparative Examples was weighed out into a sample cup using a precision balance. <<Measurement conditions>> <Pyrolysis unit> Equipment: Frontier Labs PY-3030D Furnace temperature: 600℃ <GC / MSユニット> Equipment: Shimadzu GCMS-GP2020NX Column: Ultra Alloy-5 (Length 30m, film thickness 0.25μm, diameter 0.250mmφ) Column temperature: held at 50°C for 5 minutes, heated at 10°C / min, heated from 100°C at 7°C / min, and held at 300°C for 10 minutes. Inlet temperature: 300℃ Detector temperature: 300℃ Split ratio: 1 / 300 Carrier gas: Helium Detection device: Mass spectrometer (MSD) Detection conditions: Scan mode or SIM mode (when unnecessary peaks overlap with peaks to be detected) In addition, when detecting each monomer peak, in order to avoid saturation of peak intensity or overlapping of peaks to be detected, the amount of sample to be used, the column to be used, the rate of temperature rise, and other detection conditions may be appropriately adjusted.

[0163] (2) Measurement of average molecular weight The average molecular weights (Mn, Mw, Mz) of each of the resins and resin compositions produced in the Examples and Comparative Examples were measured as standard polystyrene-equivalent molecular weights by gel permeation chromatography (GPC) under the following conditions using a calibration curve method using standard polystyrene. Measuring equipment: Tosoh HLC-8220 Separation column: Two Tosoh TSK gel Super HZM-H (inner diameter 4.6 mm) connected in series Guard column: Tosoh TSK guard column Super HZ-H Measurement solvent: tetrahydrofuran (THF) Sample concentration: 5 mg of the measurement sample was dissolved in 10 mL of solvent and filtered through a 0.45 μm filter. Injection volume: 10μL Measurement temperature: 40℃ Flow rate: 0.35mL / min Detector: Differential refractometer To create the calibration curve, 11 types of TSK standard polystyrene (F-850, F-450, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000) manufactured by Tosoh were used. The calibration curve was created using a linear approximation equation. If there was any THF insoluble matter in the composition, the THF insoluble matter was removed using a membrane filter of about 0.2 to 0.5 μm before measurement.

[0164] (3) Melt mass flow rate (g / 10 min) Measurement was performed in accordance with ISO 1133. For Resin (A) and Resin (C), the measurement was performed under test conditions of 200°C and a load of 5 kg. For the styrene-based resin compositions prepared in the Examples and Comparative Examples, the measurement was performed under test conditions of 220°C and a load of 10 kg.

[0165] (4) Measurement of Vicat softening temperature (℃) The Vicat softening temperature of each resin and resin composition produced in the Examples and Comparative Examples was measured in accordance with ISO 306. For Resin (A) and Resin (F), the test conditions were a load of 5 kg and a heating rate of 50°C / hour. For the styrene-based resin compositions produced in the Examples and Comparative Examples, the test conditions were a load of 1 kg and a heating rate of 120°C / hour.

[0166] (5) Measurement of density (g / cm 3 ) The density of each of the resins and resin compositions produced in the examples and comparative examples was measured in accordance with ISO1183 (Method A).

[0167] (6) Measurement of the average particle size of rubber particles (μm) Regarding the average particle size (μm) of the rubber-like particles (B) having a core-shell structure and the rubber-like polymer particles (C-2) in the impact-resistant styrene-based resin (C), heat-pressed products of each resin and resin composition were prepared, and 200 rubber-like polymer particles were observed by cross-sectional observation using a transmission electron microscope. The average particle size (μm) of the rubber-like polymer particles was calculated based on the following formula (2): Average particle diameter=Σ(ni×Di 4 ) / Σ(ni×Di 3 ) {In the above formula (2), ni is the number of rubber-like polymer particles having a particle diameter Di, and Di is the average value of the major axis and minor axis of the rubber-like polymer particles.} The particle diameters were calculated by averaging the particle diameters (5 × 200 particles) obtained from images of five fields of view.

[0168] (7) Analysis of low molecular weight components The contents of monohydric alcohols having 10 or more carbon atoms, styrene monomer, and styrene dimers and trimers in the styrene-based resin compositions were measured by gas chromatography under the following conditions. <<Sample preparation>> After dissolving 1.0 g of resin in 5 mL of methyl ethyl ketone, 5 mL of hexane containing p-diethylbenzene adjusted to 200 μg / g as a standard substance was added to reprecipitate the polymer component, and the supernatant was collected as the measurement solution. <<Measurement conditions>> Measurement equipment: Agilent 6850 series GC system Detector: FID Column: DB-WAX (Length 60m, film thickness 0.50μm, diameter 0.320mmφ) Injection volume: 1μL Split ratio: 50:1 Column temperature: 100°C for 5 minutes → 10°C / min to 130°C → 10°C / min Heat to 180℃ → Hold at 180℃ for 10 minutes → 20℃ / min Heat to 220℃ → Hold at 220℃ for 10 minutes Inlet temperature: 230℃ Detector temperature: 300℃ Carrier gas: Helium In addition, when detecting each peak, in order to avoid overlap with other peaks or saturation of peak intensity, pretreatment such as dilution rate of the sample, the column used, the temperature rise rate, and other detection conditions may be appropriately adjusted.

[0169] (8) Tensile test, bending test and impact test (8-1) Dumbbell molding of styrene resin composition Each of the pellet-shaped resin compositions produced in the Examples and Comparative Examples was molded into a 4 mm dumbbell of Type A using an EC60N manufactured by Toshiba Machine Co., Ltd. under the following conditions. Pellet drying: 80℃ for 2 hours or more Measurement: 63mm Injection time: 20 seconds Pressure holding switch: Short shot point of 10mm or less Holding pressure: For short shots, the maximum injection pressure when holding pressure is 0 MPa x 1.0 MPa Pressure retention time: 10 seconds Cylinder temperature: 230-250-230-210℃ from nozzle side to hopper side Screw rotation speed: 100 rpm Cushion: 4.5~5.5mm Mold temperature: 60℃ Cooling time: 25 seconds

[0170] (8-2) Flexural modulus (MPa) A test piece of 80 x 10 x 4 mm was cut from the 4 mm thick dumbbell piece obtained in the previous section (8-1) using a cutting machine. A bending test was carried out at a bending speed of 2 mm / min in accordance with ISO178, and the bending modulus was measured. The n5 average value was taken as the measured value.

[0171] (8-3) Tensile yield stress (MPa) The 4 mm thick dumbbells obtained in the previous section (8-1) were subjected to a dumbbell tensile test in accordance with ISO527-1 (tensile speed 50 mm / min) to measure the tensile yield stress. The n5 average value was used as the measured value.

[0172] (8-4) Charpy impact test (with notch) (kJ / m 2 ) A notched test piece of 80 x 10 x 4 mm was prepared from the 4 mm thick dumbbell piece obtained in the previous section (8-1) using a cutting machine. The Charpy impact strength (with notch) was measured in accordance with ISO179 (1eA). The n5 average value was used as the measured value.

[0173] (9) Measurement of lightness (L*) (-) Each pellet-shaped resin composition produced in the Examples and Comparative Examples was injection molded into a 2 mm plate, and the lightness (L*) of the test piece was measured in accordance with JIS Z8722. The test piece used was a 2 mm thick plate produced by injection molding. A spectrophotometer (CM-2002 manufactured by Konica Minolta) was used to measure the lightness (L*). The measurement conditions were SCI mode (specular reflection included), The average value of n3 was used as the measured value.

[0174] (10) Acrylic heat-welding evaluation (10-1) Measurement of peel strength (N) For the styrene resin composition prepared in the examples and comparative examples and the acrylic resin Delpet 80N manufactured by Asahi Kasei Corporation, dumbbell pieces were prepared in the same manner as in the previous section (8-1). The dumbbell was cut at a point 5 cm from the gate side of each dumbbell piece to prepare a test piece (10A). Next, the opposite side of the ejection pin of the test piece of the styrene resin composition prepared in the examples and comparative examples and the opposite side of the ejection pin of the test piece of the acrylic resin Delpet 80N were overlapped at a point 3 cm from the cut surface, and fixed with heat-resistant Teflon (registered trademark) tape to prepare a test piece (10B). The test piece (10B) was placed in an oven set at a temperature of 150°C, and a 0.5 kg dumbbell preheated in the oven was placed on the adhesive surface of the styrene resin composition and the acrylic resin material of the test piece (10B) and left to stand in the oven for 10 minutes. At this time, in order to prevent thermal deformation of the dumbbell piece, it was fixed with a metal plate preheated in the oven. The test piece (10B) was removed from the oven and allowed to cool in air for 5 minutes to obtain a test piece (10C) in which the styrene resin composition and the acrylic resin material were thermally welded. The test piece (10C) was subjected to a tensile test at a tensile speed of 5 mm / min using Shima Autograph AGS-5kNX, and the test force (N) at the time of peeling the heat-welded interface was measured. The average n5 value was taken as the peel surface strength.

[0175] (10-2) Heating time in hot plate welding (seconds) The styrene resin compositions prepared in the examples and comparative examples were injection molded into a 1 cm thick housing-like part (10D) with an opening and a 2 cm adhesive surface on one side of a cube with three sides of 26 cm in length. Next, Asahi Kasei Corporation's acrylic resin Delpet 80N was injection molded into a plate-shaped cover part (10E) with a 2 cm smooth adhesive surface on the outer periphery of 30 cm x 30 cm. Next, the housing-like part (10D) and the plate-like cover part (10E) were placed via a hot plate heated to 300°C, and were brought within 1 cm of each other with their adhesive surfaces facing the hot plate. After a heating time (10T), the hot plate was removed, and the adhesive surfaces of the housing-like part (10D) and the plate-like cover part (10E) were pressed together. After air cooling for 3 minutes, a heat-welded body (10DE) was obtained. Ten heat-welded bodies (10DE) were created using the above method, and the number of heat-welded bodies (10DE) that peeled off when a palm was placed on the surface of the housing-like part (10D) and a shear stress was applied parallel to the surface of the housing-like part (10D) was counted. The minimum heating temperature (10T) at which 8 or more out of 10 peeled off was used as the heating time (seconds) for hot plate welding to evaluate the heat-weldability to acrylic. The heating time was increased in 5-second increments from 35 seconds.

[0176] (11) Weather resistance evaluation 2 mm plates of the styrene-based resin compositions prepared in the Examples and Comparative Examples were prepared by injection molding, and subjected to a weather resistance test under the test conditions of a black panel temperature of 63°C, rain, and 2000 hours using a Sunshine Weather Meter S80BBR manufactured by Suga Test Instruments Co., Ltd. The color difference (ΔE) after the weather resistance test was measured and evaluated according to the following criteria. ◎: ΔE is 1.0 or less 〇: ΔE is greater than 1.0 and less than 5.0 △: ΔE is greater than 5.0 and less than 8.0 ×: ΔE is greater than 8.0

[0177] [Preparation of each resin and production examples of styrene-based resin composition] The preparation of each resin and a specific method for producing the styrene-based resin composition will be described below. <Production Example of Styrene-Unsaturated Carboxylic Acid Resin (A)> -Preparation of resin (A1)- A polymerization raw material composition liquid consisting of 65.5 parts by mass of styrene, 3.3 parts by mass of methyl methacrylate, 5.8 parts by mass of methacrylic acid, 22.9 parts by mass of ethylbenzene, 2.5 parts by mass of 2-ethyl-1-hexanol, and 0.027 parts by mass of 1,1-bis(t-butylperoxy)cyclohexane was supplied to a complete mixing type reactor having a capacity of 3.6 liters at a rate of 0.8 liters / hour, and then continuously supplied to a volatilization device connected to a single screw extruder that removes volatile components such as unreacted monomers and polymerization solvents. The polymerization temperature of the complete mixing reactor was set to 130°C. The temperature of the single screw extruder was set to 210 to 230°C, and the pressure was set to 10 torr, and volatile components such as unreacted monomers and polymerization solvents were volatilized. The volatilized volatile components were condensed in a condenser through which a refrigerant of -5°C was passed, and were recovered as unreacted liquid, and the styrene-based resin was recovered as resin pellets. The physical properties of the resin (A1) obtained by the above-mentioned analytical methods are shown in Table 1 below.

[0178] -Preparation of Resin (A2) and Resin (A3)- Resin (A2) and resin (A3) were prepared in the same manner as for resin (A1). The compositions and physical properties of the obtained resins (A2) and (A3) are shown in Table 1.

[0179] -Preparation of resin (A4)- Using only styrene as a monomer, a styrene homopolymer resin (A4) having the composition and physical properties shown in Table 1 was obtained in the same manner as above.

[0180] [Table 1]

[0181] <Production Example of Core-Shell Structured Rubber Particles (B)> -Preparation of rubber particles (B1)- In a pressure vessel equipped with a stirrer, 200 parts by mass of pure water, 0.002 parts by mass of disodium salt of ethylenediaminetetraacetic acid, 0.0012 parts by mass of ferrous sulfate, 0.008 parts by mass of disodium salt of ethylenediaminetetraacetic acid, and 0.03 parts by mass of sodium polyoxyethylene alkyl ether phosphate were charged, and after deacidification, 100 parts by mass of butadiene, 0.05 parts by mass of sodium formaldehyde sulfoxylate, and 0.2 parts by mass of paramenthane hydroperoxide were added, and then 1.4 parts by mass of sodium polyoxyethylene alkyl ether phosphate was added dropwise over 6 hours. The reaction solution was kept at pH 6.5 to 7.5 at 50°C for 124 hours, and a diene rubber latex with a conversion rate of 98% by weight and an average particle size of 0.18 μm was obtained. Next, while maintaining the above-obtained rubber latex (solid content about 71 parts) at 60 ° C, 55 parts by mass of methyl methacrylate and 5 parts by mass of n-butyl acrylate as monomers were added over 1 hour. Simultaneously with the addition of the above-mentioned monomers, 0.09 parts by mass of t-butyl hydroperoxide and 0.1 parts by mass of sodium formaldehyde sulfoxylate were started to be added, and then the entire amount was added over 2 hours while maintaining the pH of the reaction solution at 6.5 to 7.5 and the temperature at about 60 ° C. The reaction solution was further maintained at about 60 ° C. for 1 hour to prepare a graft copolymer latex with an average particle size of 200 nm, and after adding 1 part by mass of Irganox 1076 as an antioxidant, the mixture was coagulated with an aqueous calcium chloride solution, washed with water, dehydrated and dried to obtain rubber-like polymer particles (B1) as powder. The composition and physical properties of the rubber-like polymer particles (D1) are shown in Table 4. -Preparation of rubber particles (B2), (B3), (B8) to (B11)- The feed amount of each monomer and the polymerization conditions were adjusted, and rubber-like particles (B2), (B3), (B8) to (B11) were prepared in the same manner as rubber-like particles (B1). The composition and physical properties of each of the obtained rubber-like particles (B) are shown in Table 2.

[0182] [Table 2]

[0183] In addition to the compositions shown in Table 2, the following products were used in the examples as rubber particles (B) having a core-shell structure containing (meth)acrylic acid ester monomer units (b1). The content of styrene monomer units in the rubber particles (B) having a core-shell structure is the value quantified by pyrolysis GC / MS described in the previous section (1). The compositions of the rubber particles (B4) to (B7) and (B12) having a core-shell structure are shown below. Rubber particles (B4): Methyl methacrylate-styrene-butadiene (MBS) rubber particles Shell: Methyl methacrylate-styrene copolymer Core: Polybutadiene Styrene monomer unit content in the entire rubber particles (B4): More than 5% by mass Mitsubishi Chemical's Metabrene C-223A (product name) Rubber particles (B5): Methyl methacrylate-butadiene (MB) rubber particles Shell: Polymethylmethacrylate Core: Polybutadiene Styrene monomer unit content in the entire rubber particles (B5): 5% by mass or less Mitsubishi Chemical Corporation: Metablen E-875A (product name) Rubber particles (B6): Acrylic-silicone rubber particles Shell: Polymethylmethacrylate Core: Polydimethylsiloxane-poly(n-butyl acrylate) composite Styrene monomer unit content in the entire rubber particles (B6): 5% by mass or less Mitsubishi Chemical Corporation: Metablen S-2130 (product name) Rubber particles (B7): Methyl methacrylate-styrene-butadiene (MBS) rubber particles Shell: Methyl methacrylate-styrene copolymer Core: Polybutadiene Styrene monomer unit content in the entire rubber particles (B7): More than 5% by mass Kaneka Kane Ace M511 (product name) Rubber particles (B12): Methyl methacrylate-butyl acrylate rubber particles Styrene monomer unit content in the entire rubber particles (B12): 5% by mass or less Mitsubishi Chemical Corporation: Metablen W-450A (product name)

[0184] <Production example of impact resistant styrene resin (C)> -Preparation of impact-resistant styrene resin (C1)- A polymerization apparatus in which three laminar flow reactors (1.5 liters) equipped with stirrers were connected in series and followed by a two-stage vented extruder was used to produce impact-resistant styrene resin (C1) (hereinafter referred to as resin (C1)). 82.4 parts by mass of styrene, 9.0 parts by mass of ethylbenzene, 8.6 parts by mass of high cis butadiene rubber 13HB manufactured by Ube Industries as a rubber-like polymer (CR), and 0.02 parts by mass of 1,1-bis(t-butylperoxy)cyclohexane were charged into a raw material tank equipped with a stirrer, and after dissolving the rubber components with a stirrer, this raw material solution was supplied to the reactor at a volume of 0.75 liters / hr, and polymerization was performed at a temperature of 110 to 120°C in the first reactor, 120 to 130°C in the second reactor, and 140 to 150°C in the third reactor. The extruder temperature was 210-240°C, the degree of vacuum was 3 kPa, and the total solid content in the polymerization liquid discharged from the final reactor was 70.5% by mass. The average particle size of the rubber-like polymer particles (C-2) was controlled by adjusting the rotation speed of the stirrer of the first-stage laminar flow reactor to 110 rpm. The composition and properties of the obtained resin (C1) are shown in Table 3.

[0185] -Preparation of resin (C2)- Resin (C2) having the composition and physical properties shown in Table 3 was obtained in the same manner as above, except that high cis butadiene rubber 15HB manufactured by Ube Industries was used as the rubber polymer (CR).

[0186] -Preparation of resins (C3) and (C4)- Using styrene, methyl methacrylate added as necessary, butyl acrylate added as necessary as monomers, and styrene-butadiene copolymer 625A manufactured by Asahi Kasei as rubber-like polymer (CR), resins (C3) and (C4) were obtained with the compositions and physical properties shown in Table 3 in the same manner as above.

[0187] [Table 3]

[0188] <Styrene-based elastomer (D) used in the examples> In the examples of this specification, the following two types of styrene-based elastomer (D) were used. (D1) Asahi Kasei Corporation's Tufprene 125 (product name) (D2) Asahi Kasei Tuftec M1913 (product name)

[0189] <Acrylic elastomer (E) used in the examples> In the examples of this specification, the following was used as the acrylic elastomer (E). (E1) Kuraray Clarity LA2270 (product name)

[0190] <Production example of acrylic resin (F)> -Preparation of resin (F1)- A 5L container equipped with an agitator was charged with 2 kg of water, 65 g of tribasic calcium phosphate, 39 g of calcium carbonate, and 0.39 g of sodium lauryl sulfate, and the suspension was prepared by mixing and stirring them. Next, 26 kg of water was charged into a 60L reactor and heated to 80°C to prepare for suspension polymerization. After confirming that the temperature had reached 80°C and was in a constant temperature state, 1.52 kg of methyl methacrylate, 0.22 kg of methyl acrylate, 0.99 g of lauroyl peroxide, 4.93 g of n-octyl mercaptan, and the above suspension were charged as polymerization raw materials. Thereafter, suspension polymerization was carried out while maintaining the temperature at about 80°C, and after observing the exothermic peak, the temperature was raised to 92°C at a rate of 1°C / min and the temperature was maintained at 92°C for 60 minutes. Subsequently, the mixture was cooled to 50°C, and 20% by mass of sulfuric acid was charged to dissolve the suspension. The polymerization reaction solution was then removed from the 60 L reactor and passed through a sieve with a mesh size of 1.7 mm to remove large aggregates, and the aqueous layer and solid matter were separated in a Buchner funnel to obtain a bead-like polymer. The bead-like polymer was washed and dehydrated five times with about 20 L of distilled water on the Buchner funnel, then dried and pelletized using a single-screw extruder to obtain resin (F1) as a pellet-like resin.

[0191] -Preparation of Resin (F2) to Resin (F5)- Resins (F2) to (F5) were prepared in the same manner as for the above resin (F1). The compositions and physical properties of the obtained resins (F2) to (F5) are shown in Table 4.

[0192] [Table 4]

[0193] <Lubricating Oil (G)> In the examples of this specification, when liquid paraffin was used as the lubricating oil (G), PS-350S (product name) manufactured by Sanko Chemical Industry Co., Ltd. was used. In the examples of this specification, when silicone oil is used as the lubricating oil (G), PP-17 (product name), polydimethylsiloxane oil manufactured by GE Toshiba Silicone, is used. The content of silicone oil in Table 5 is calculated from the amount of charge. On the other hand, when calculating the content of silicone oil from a styrene-based resin composition, it can be roughly calculated by quantifying the amount of silicon using plasma emission spectroscopy (ICP method). It was confirmed that the amount of silicon in the styrene-based resin composition containing silicone oil prepared in the examples was in the range of 150 ppm to 10,000 ppm in terms of the amount of silicon relative to the entire styrene-based resin composition (100% by mass).

[0194] <<Optional additives used in the examples>> <Monohydric alcohols with 10 or more carbon atoms> In the examples of this specification, the following alcohol species were used as monohydric alcohols having 10 or more carbon atoms. Nissan Chemical Co., Ltd.: Fine Oxocol 180 (product name) "Compound name: 5,7,7-trimethyl-2-(1,3,3-trimethylbutyl)-1-octanol" Kao Corporation: Emulgen 109P (product name) "Compound name: Polyoxyethylene (9) lauryl ether monoalcohol"

[0195] <Coloring agent> A carbon black masterbatch for coloring a styrene-based resin composition black was prepared according to the following procedure. -Preparation of black masterbatch- 2.8 kg of the resin (A1), 2.8 kg of carbon black, and 0.5 kg of polyethylene wax were dry blended, kneaded, extruded, and pelletized to obtain black pellets, a black master batch containing the resin (A1) as a base resin.

[0196] <Antioxidants> In the examples of the present specification, the following three types of antioxidants were used as antioxidants. Phenol-based antioxidant (1): Irganox 1076 (product name) manufactured by BASF Japan Ltd. "Compound name: Octadecyl-3-(3,5-tertiary-butyl-4-hydroxyphenyl)propionate" Phenol-based antioxidant (2): Sumitomo Chemical Co., Ltd. Sumilizer GS (product name) "Compound name: 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate" Phosphorus-based antioxidant: Irgafos168 (product name) manufactured by BASF Japan Ltd. "Compound name: Tris(2,4-di-tertiarybutylphenyl)phosphite"

[0197] <Light stabilizer> The following were used as light stabilizers in the examples herein: Hindered amine light stabilizer: Bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate

[0198] <Ultraviolet absorbing agent> In the examples of this specification, the following were used as ultraviolet absorbents: UV absorber: ADEKA Corporation LA-32 (product name) "Compound name: 2-(2H-benzotriazol-2-yl)-p-cresol"

[0199] <Release agent (internal lubricant)> In the examples of this specification, the following were used as release agents (external lubricants). Moisturizer: Kao Corporation's Kalcol 8098 (compound name: stearyl alcohol)

[0200] <Release agent (external lubricant)> In the examples of this specification, the following were used as release agents (external lubricants). External lubricant: Kao Wax EB-FF (chemical name: ethylene bis stearic acid amide) manufactured by Kao Corporation

[0201] <<Production Examples of Styrene-Based Resin Compositions and Foam Extrusion Sheets>> The method for producing the styrene-based resin composition and the injection-molded article will be described below. [Example 1] -Production of styrene-based resin composition- 93.0 parts by mass of the resin (A1) shown in Table 1 as the styrene-unsaturated carboxylic acid resin (A), 15.0 parts by mass of Mitsubishi Chemical's Metablen S2130 (B6) as the core-shell structured rubber particles (B), 0.5 parts by mass of silicone oil as the lubricating oil (G), and optional additives were added and dry blended in the formulation shown in Table 6. The styrene-based resin composition [1] was obtained as a pelletized resin through kneading extrusion and pelletization using a twin-screw extruder TEM26SS made by Shibaura Machine Co., Ltd. The screw rotation speed was 150 rpm, the cylinder temperature was 180 to 230 ° C, and the feed rate was 10 kg / h. The resin temperature was 250 to 260 ° C. The properties and physical properties of the styrene-based resin composition [1] and the evaluation results of the injection molded body are shown in Table 5.

[0202] [Examples 2 to 62] Styrenic resin compositions [2] to

[62] were obtained in the same manner as in Example 1, except that the formulation was changed as shown in the following Table 6. The evaluation results of the obtained styrenic resin compositions are shown in Table 5.

[0203] [Table 5-1]

[0204] [Table 5-2]

[0205] [Table 5-3]

[0206] [Table 5-4]

[0207] [Table 5-5]

[0208] [Comparative Examples 1 to 2 and Comparative Example 4] Styrene-based resin compositions of Comparative Examples 1 to 4 were obtained in the same manner as in Example 1, except that the formulation was changed as shown in the following Table 7. The evaluation results of the obtained styrene-based resin compositions are shown in Table 6.

[0209] [Comparative Example 3] In Comparative Example 3, instead of the styrene-based resin composition, heat-resistant ABS manufactured by Chimei Industrial, PA-777E (a resin composition consisting of a styrene-acrylonitrile-butadiene copolymer and a styrene-acrylonitrile-N-phenylmaleimide copolymer) was used and the same evaluation as in the Examples was carried out. The evaluation results are shown in Table 6. In the system using ABS, which is a styrene-acrylonitrile-based resin, the thermal weldability with the acrylic resin material was inferior to that of the styrene-based resin composition of the present application.

[0210] [Table 6] [Industrial Applicability]

[0211] The styrene-based resin composition of the present embodiment is excellent in heat resistance, toughness, rigidity, and thermal adhesion to acrylic resin materials. Therefore, the styrene-based resin composition of the present invention can be widely used for non-foamed or foamed sheets by extrusion molding, food packaging containers using them, or molded products by injection molding (electrical product parts, toys, daily necessities, various industrial parts), etc., and is particularly useful for in-vehicle parts that require heat resistance, toughness, rigidity, and thermal adhesion to acrylic resin materials, and plays a major role in the industrial world.

Claims

1. A styrene-unsaturated carboxylic acid resin composition comprising: a styrene-unsaturated carboxylic acid resin (A) containing a styrene monomer unit (a1) and an unsaturated carboxylic acid monomer unit (a2); and a core-shell rubber particle (B) containing a (meth)acrylic acid ester monomer unit (b1), A styrene-based resin composition, wherein the content of the styrene-unsaturated carboxylic acid-based resin (A) is 40% by mass to 95% by mass, and the content of the rubber-like particles (B) is 5% by mass to 60% by mass, relative to the total amount (100% by mass) of the styrene-based resin composition.

2. The styrene-based resin composition according to claim 1, wherein the rubber-like particles (B) having a core-shell structure further contain a styrene-based monomer unit (b4), and the content of the styrene-based monomer unit (b4) is 5 mass% or less based on the total amount (100 mass%) of the rubber-like particles (B) having a core-shell structure.

3. The styrene-based resin composition according to claim 1 or 2, wherein the content of the (meth)acrylic acid ester monomer unit (b1) contained in the rubber-like particles (B) having a core-shell structure is 3 to 40 mass% relative to the total amount (100 mass%) of the rubber-like particles (B) having a core-shell structure.

4. The styrene-based resin composition according to claim 1 or 2, wherein the rubber-like particles (B) having a core-shell structure further contain a conjugated diene monomer unit (b2), and the content of the conjugated diene monomer unit (b2) is 50 to 90 mass% relative to the total amount (100 mass%) of the rubber-like particles (B) having a core-shell structure.

5. The styrene-based resin composition according to claim 1 or 2, further comprising 0.5 to 30 mass % of an impact resistant styrene-based resin (C).

6. The styrene-based resin composition according to claim 1 or 2, further comprising 0.05 to 3.00 mass% of a lubricating oil (G).

7. The core-shell rubber particles (B) further contain a styrene-based monomer unit (b4), 7. The styrene-based resin composition according to claim 6, wherein Y / X≦10, where Y is the content of the styrene-based monomer unit (b4) and X is the content of the lubricating oil (G).

8. 3. The styrene-based resin composition according to claim 1, wherein the lubricating oil (G) is a silicone oil.

9. The styrene-based resin composition according to claim 1 or 2, wherein the core-shell rubber particles (B) further contain one or more selected from the group consisting of conjugated diene monomer units (b2) and siloxane monomer units (b3), and the total content of the conjugated diene monomer units (b2) and the siloxane monomer units (b3) is 50 mass% or more based on the total amount (100 mass%) of the core-shell rubber particles (B).

10. Notched Charpy impact strength (ISO179 compliant, test condition 1eA) is 4.0kJ / m 2 The styrene-based resin composition according to claim 1 or 2.

11. 3. The styrene-based resin composition according to claim 1, wherein the content of all styrene-based monomer units is 72 mass% or less relative to the total amount (100 mass%) of the styrene-based resin composition.

12. 3. The styrene-based resin composition according to claim 1 or 2, further comprising 0.5 mass% or more of one or more selected from the group consisting of an impact resistant styrene-based resin (C), a styrene-based elastomer (D), and an acrylic elastomer (E) relative to a total amount (100 mass%) of the styrene-based resin composition.

13. The styrene-based resin composition according to claim 1 or 2, further comprising 1.0 mass% or more of an acrylic resin (F) relative to the total amount (100 mass%) of the styrene-based resin composition.

14. The styrene-based resin composition according to claim 1 or 2, having a lightness (L*) of 50 or less.

15. 3. An injection molded article obtained by injection molding the styrene-based resin composition according to claim 1 or 2.

16. The injection molded article according to claim 15, which is welded to an acrylic resin material.

17. The injection molded article according to claim 14, which is mounted on a vehicle.

Citation Information

Patent Citations

  • Lighting fixture for vehicle

    JP1995282602A

  • Polystyrenic resin foamed sheet, polystyrenic resin laminated foamed sheet, and polystyrenic resin laminated foamed molded body

    JP2018044086A

  • Maleimide copolymer, method for producing same, resin composition and injection molded body

    WO2021006265A1

Cited By

  • Styrene-based resin composition and molded body

    WO2026205490A1