Lithium secondary battery and manufacturing method thereof
The lithium secondary battery design with multiple lithium metal layers addresses dendrite formation by controlling lithium deposition, resulting in enhanced cycle characteristics and safety.
Patent Information
- Application Number
- JP2023061578
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-05
- Publication Date
- 2024-10-18
AI Technical Summary
Lithium metal nuclei are non-uniformly generated and grown on the surface of the negative electrode during charging, leading to dendrite formation, which causes electrolyte depletion, safety issues, and deterioration of cycle characteristics in lithium secondary batteries.
A lithium secondary battery design featuring a current collector layer, a first lithium metal layer, a second lithium metal layer with granular lithium metal, and a third porous lithium metal layer, where the average particle diameter of the granular lithium metal is larger than the average pore diameter of the third layer, with specific porosity and area ratios to suppress dendrite formation.
The battery exhibits improved charge/discharge cycle characteristics by suppressing negative electrode expansion and enhancing safety through controlled lithium deposition and dissolution.
Smart Images

Figure 2024148448000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a lithium secondary battery and a method for manufacturing the same. [Background technology]
[0002] Lithium batteries can achieve higher capacity than conventional nickel-metal hydride batteries and lead-acid batteries, and therefore they are attracting attention and being increasingly introduced as power sources for mobile phones and laptops, as well as for large-scale power storage and automobile power sources. However, due to the increasing functionality of various electronic devices and the growing demand for power sources, there are expectations for even higher capacity lithium batteries. Unlike lithium-ion secondary batteries, which charge and discharge by inserting and removing lithium ions into and from the material that constitutes the electrodes, lithium secondary batteries charge and discharge by depositing and dissolving lithium metal. As a light metal, lithium batteries have a capacity several to ten times that of graphite, and because they have an extremely base potential, there are high expectations for them. (Patent Documents 1 to 3) [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 11-214008 [Patent Document 2] JP 2000-133314 A [Patent Document 3] Patent No. 5317435 Summary of the Invention [Problem to be solved by the invention]
[0004] A problem that arises when using lithium metal as the negative electrode active material is that lithium metal nuclei are generated and grow unevenly on the surface of the negative electrode during charging. When lithium metal is unevenly deposited, the tips of the deposited lithium metal are more likely to come into contact with the electrolyte. This makes lithium deposition easier than other areas, and the tips of the deposited lithium metal continue to extend, depositing tree-like lithium metal (dendrites). The more dendrite formation progresses, the larger the specific surface area becomes, and the more reduction decomposition products are produced.
[0005] Furthermore, when the lithium metal dissolves during the discharge process, some of the lithium metal precipitated on the dendrites peels off, creating areas that cannot contribute to discharge (dead lithium), and the lithium metal becomes more pulverized.
[0006] The accumulation of reduction decomposition products and the pulverization of lithium metal progress with repeated cycles, causing the anode to expand significantly. This expansion of the anode is a major issue because it accelerates the depletion of the electrolyte, reduces safety, and leads to a deterioration of cycle characteristics.
[0007] The present disclosure has been made in view of the above problems, and provides a lithium secondary battery having excellent charge / discharge cycle characteristics and a method for producing the same. [Means for solving the problem]
[0008] [1] A lithium secondary battery comprising a negative electrode and a positive electrode, The negative electrode is A current collector layer; a first lithium metal layer made of lithium metal foil; a second lithium metal layer including granular lithium metal; a third lithium metal layer comprising lithium metal and being porous; in that order, a lithium secondary battery, wherein the average particle size of the granular lithium metal is larger than the average pore size of the third lithium metal layer; [2] The lithium secondary battery according to [1], wherein the third lithium metal layer has a porosity of 10 to 40%. [3] The lithium secondary battery according to [1] or [2], wherein the third lithium metal layer has an average pore size of 0.1 to 3 μm. [4] The lithium secondary battery according to any one of [1] to [3], wherein the granular lithium metal has an average particle size of 1 to 22 μm. [5] The lithium secondary battery according to any one of [1] to [4], wherein an area ratio S calculated by the following formula (1) is 60 area % or more. Area ratio S = {S3 / (S2+S3)} × 100... Equation (1) [In formula (1), S2 is the area of the second lithium metal layer on the main surface of the negative electrode facing the third lithium metal layer, and S3 is the area of the third lithium metal layer on the main surface of the negative electrode facing the third lithium metal layer.] [6] (a) preparing a lithium secondary battery precursor including a negative electrode having a current collector layer and a lithium metal foil, and a positive electrode; (b) charging the lithium secondary battery precursor at 0.01 to 0.5 C until the charge rate reaches 10 to 100%, and then discharging the lithium secondary battery precursor at 0.2 C to 2.5 C; Equipped with A method for producing a lithium secondary battery, comprising carrying out step (b) two or more times. Effect of the Invention
[0009] According to the present disclosure, a lithium secondary battery having excellent charge / discharge cycle characteristics and a method for producing the same are provided. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view of a lithium secondary battery according to one embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of a negative electrode 30C according to one embodiment. [Diagram 3]Fig. 3(a) is an SEM photograph of a part of a cross section of the negative electrode of the lithium secondary battery obtained in the example. Fig. 3(b) is an SEM photograph of the main surface of the negative electrode of the lithium secondary battery obtained in the example facing the third lithium metal layer. Fig. 3(c) is an SEM photograph of the main surface of the negative electrode of the lithium secondary battery obtained in the example facing the third lithium metal layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Preferred embodiments of the present disclosure will be described with reference to the drawings.
[0012] [Lithium secondary battery] 1, the lithium secondary battery 100 according to this embodiment includes a power generating element 90 and a case 80. The power generating element 90 is a laminate having a large number of negative electrodes 30C, positive electrodes 10, and separators 20. In the power generating element 90, the negative electrodes 30C and the positive electrodes 10 are alternately arranged, and the separators 20 are arranged between the negative electrodes 30C and the positive electrodes 10. Each layer of the power generating element 90 is impregnated with a nonaqueous electrolyte.
[0013] (Negative electrode 30C) 2 is a cross-sectional view of an anode 30C according to an embodiment. The anode 30C includes, in this order, a current collector layer 32, a first lithium metal layer 34 made of lithium metal foil, a second lithium metal layer 36 containing granular lithium metal 36a, and a third lithium metal layer 38 containing lithium metal and being porous. The anode 30C may include the first to third lithium metal layers on each of a pair of main surfaces of the current collector layer 32, or may include the first to third lithium metal layers only on one main surface of the current collector layer 32. The anode 30C may include the first to third lithium metal layers on one main surface of the current collector layer 32, and may include only the first lithium metal layer on the other main surface of the current collector layer 32.
[0014] The current collector layer 32 may be any conductive plate material, and may be, for example, a thin metal plate (metal foil) of copper, nickel, stainless steel, or an alloy thereof. Copper foil is preferable from the viewpoint of electrical conductivity. The copper foil may be a rolled copper foil or other copper foil. There is no limitation on the thickness of the current collector layer 32, but it may be, for example, 2 to 20 μm.
[0015] The thickness of the first lithium metal layer 34 is not particularly limited, but can be 2 μm or more and 50 μm or less.
[0016] The porosity of the first lithium metal layer 34 may be 1% or less, and it may be free of voids.
[0017] The second lithium metal layer 36 includes granular lithium metal 36a. The second lithium metal layer 36 may be an aggregate of granular lithium metal 36a. Adjacent granular lithium metal 36a may be partially joined together. The granular lithium metal 36a may be a single crystal.
[0018] The average particle size of the granular lithium metal 36a is larger than the average pore size of the third lithium metal layer 38 described later. The average particle size of the granular lithium metal 36a may be 1 to 22 μm. The average particle size is measured by the method described in the Examples described later.
[0019] The porosity of the second lithium metal layer 36 may be 3 to 40%. The porosity is measured by observing a cross-sectionally processed portion using a scanning electron microscope (SEM) and measuring the area of the voids.
[0020] The second lithium metal layer 36 may have a thickness of 1 to 25 μm.
[0021] The third lithium metal layer 38 contains lithium metal and is porous. The third lithium metal layer 38 does not contain the granular lithium metal contained in the second lithium metal layer 36.
[0022] The porosity of the third lithium metal layer 38 is preferably 10 to 40%, and more preferably 15 to 30%. A porosity of 10% or more allows lithium ions to pass through easily. A porosity of 40% or less tends to suppress the precipitation of dendrites. Therefore, a lithium secondary battery having a porosity in the above range tends to have even more excellent cycle characteristics. The porosity is measured by the method described in the Examples below.
[0023] The average pore diameter of the third lithium metal layer 38 is preferably 0.1 to 3 μm, and more preferably 0.5 to 1 μm, since this tends to further improve the charge / discharge cycle characteristics. When the average pore diameter is 0.1 μm or more, lithium ions can easily pass through. When the average pore diameter is 3 μm or less, the precipitation of dendrites tends to be suppressed. Therefore, a lithium secondary battery having an average pore diameter in the above range tends to have even more excellent cycle characteristics. The average pore diameter is measured by the method described in the Examples below.
[0024] The lithium metal content in the third lithium metal layer 38 may be 80% by weight or more, 95% by weight or more, 99% by weight or more, or 100% by weight.
[0025] The third lithium metal layer 38 may have a thickness of 2 to 50 μm.
[0026] The area ratio S of the negative electrode 30C calculated by the following formula (1) is preferably 60 area% or more, more preferably 70 area% or more, and even more preferably 80 area% or more, since this tends to further improve the charge-discharge cycle characteristics. The area ratio S is measured by the method described in the Examples below.
[0027] Area ratio S = {S3 / (S2+S3)} × 100... Equation (1) [In formula (1), S2 is the area of the second lithium metal layer on the main surface of the negative electrode of the lithium secondary battery on the third lithium metal layer side, and S3 is the area of the third lithium metal layer on the main surface of the negative electrode of the lithium secondary battery on the third lithium metal layer side.]
[0028] The total thickness of negative electrode 30C can be from 1 to 150 μm.
[0029] The negative electrode 30C may have a main body portion and a tab portion protruding from the main body portion.
[0030] The planar shape of the negative electrode 30C can take various shapes according to the final shape of the battery. For example, the negative electrode 30C does not need to have a tab portion. The main body portion may also have a circular shape.
[0031] (Mechanism of action) The lithium secondary battery 100 has a second lithium metal layer 36 and a third lithium metal layer, and the average particle size of the granular lithium metal 36a is larger than the average pore size of the third lithium metal layer 38. This allows the third lithium metal layer to suppress lithium metal nuclei from being generated and growing non-uniformly on the surface of the second lithium metal layer 36. As a result, the lithium secondary battery 100 is prevented from expanding the negative electrode, and has excellent cycle characteristics.
[0032] (positive electrode 10) The positive electrode 10 has a positive electrode current collector 12 and a positive electrode active material layer 14 provided on both sides of the positive electrode current collector 12 .
[0033] The positive electrode current collector 12 may be any conductive plate material, for example, a metal foil such as aluminum, copper, or nickel.
[0034] The positive electrode active material layer 14 contains a positive electrode active material, a conductive assistant, and a binder.
[0035] The positive electrode active material includes an active material capable of reversibly undergoing occlusion and release of lithium ions, desorption and insertion (intercalation) of lithium ions, or doping and dedoping of lithium ions and counter anions.
[0036] The positive electrode active material is, for example, a composite metal oxide. Examples of the composite metal oxide include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganate (LiMnO2), lithium manganese spinel (LiMn2O4), and a compound of the general formula: LiNi x Co y Mn z M a O2 (wherein in the general formula x + y + z + a = 1, 0 ≦ x < 1, 0 ≦ y < 1, 0 ≦ z < 1, 0 ≦ a < 1, and M is one or more elements selected from Al, Mg, Nb, Ti, Cu, Zn, Cr), lithium vanadium compound (LiV2O5), olivine-type LiMPO4 (where M represents one or more elements selected from Co, Ni, Mn, Fe, Mg, Nb, Ti, Al, Zr or VO), lithium titanate (Li4Ti5O 12 )、LiNi x Co y Al z O2 (0.9 < x + y + z < 1.1). The positive electrode active material may also be an organic substance. For example, examples of the organic positive electrode active material include polyacetylene, polyaniline, polypyrrole, polythiophene, and polyacene.
[0037] The conductive assistant enhances the electron conductivity between the positive electrode active materials. Examples of the conductive assistant include carbon powders such as carbon black, acetylene black, ketjen black, carbon nanotubes, carbon materials, metal fine powders such as copper, nickel, stainless steel, iron, mixtures of carbon materials and metal fine powders, and conductive oxides such as ITO. Carbon materials such as carbon black, acetylene black, and ketjen black are preferred as the conductive assistant.
[0038] The binder binds the active materials together. Any known binder can be used. An example of the binder is a fluororesin. Examples of the fluororesin include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkylvinyl ether copolymer (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), polychlorotrifluoroethylene (PCTFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), polyvinyl fluoride (PVF), etc.
[0039] Other examples of the binder are vinylidene fluoride-based fluororubbers such as vinylidene fluoride-hexafluoropropylene-based fluororubber (VDF-HFP-based fluororubber), vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene-based fluororubber (VDF-HFP-TFE-based fluororubber), vinylidene fluoride-pentafluoropropylene-based fluororubber (VDF-PFP-based fluororubber), vinylidene fluoride-pentafluoropropylene-tetrafluoroethylene-based fluororubber (VDF-PFP-TFE-based fluororubber), vinylidene fluoride-perfluoromethylvinylether-tetrafluoroethylene-based fluororubber (VDF-PFMVE-TFE-based fluororubber), and vinylidene fluoride-chlorotrifluoroethylene-based fluororubber (VDF-CTFE-based fluororubber). Further examples of the binder include cellulose, styrene-butadiene rubber, ethylene-propylene rubber, polyimide resin, polyamide-imide resin, and acrylic resin.
[0040] (Separator 20) The separator 20 has electrical insulation properties and a porous structure. An example of the separator 20 is a microporous film of resin. Examples of the resin are polyimide resins and polyolefin resins such as polyethylene and polypropylene. The resin may be a homopolymer, a copolymer, or a mixture of multiple polymers. The microporous film of resin can be produced by stretching a resin film (dry method) or removing a pore-forming agent or the like in the resin film (wet method), or the like.
[0041] Other examples of the separator 20 include nonwoven fabrics (paper) of various fibers. Examples of the fibers include the fibers of the above-mentioned resins, cellulose fibers, polyester fibers, polyamide fibers, polyacrylonitrile fibers, and glass fibers.
[0042] Yet another example of the separator 20 is a solid electrolyte. Examples of the solid electrolyte include a polymer solid electrolyte, an oxide-based solid electrolyte, and a sulfide-based solid electrolyte.
[0043] The separator 20 may be a single layer of the above materials, or may be a laminate of any two or more of the above materials. The separator 20 may further include a layer containing a material other than the above materials on one or both of its main surfaces. Such a material may be an inorganic material or an organic material. Examples of inorganic materials include metal oxides such as alumina, silica, zirconia, and titania, and solid electrolytes such as lithium ion conductors (LISICON, LLZ, LLTO).
[0044] (Non-aqueous electrolyte) The non-aqueous electrolyte is sealed in the exterior body 50 and impregnates the power generating element 90. The non-aqueous electrolyte includes, for example, a non-aqueous solvent and an electrolyte. The electrolyte is dissolved in the non-aqueous solvent.
[0045] The non-aqueous solvent contains, for example, a cyclic carbonate and a chain carbonate. The cyclic carbonate solvates the electrolyte. The cyclic carbonate is, for example, ethylene carbonate, propylene carbonate, and butylene carbonate. The cyclic carbonate preferably contains at least propylene carbonate. The chain carbonate reduces the viscosity of the cyclic carbonate. The chain carbonate is, for example, diethyl carbonate, dimethyl carbonate, and ethyl methyl carbonate. The non-aqueous solvent may also contain methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, and the like.
[0046] The electrolyte is, for example, a lithium salt. The electrolyte is, for example, LiPF6, LiClO4, LiBF4, LiCF3SO3, LiCF3CF2SO3, LiC(CF3SO2)3, LiN(FSO2)2, LiN(CF3SO2)2, LiN(CF3CF2SO2)2, LiN(CF3SO2)(C4F9SO2), LiN(CF3CF2CO)2, LiBOB, etc. The lithium salt may be used alone or in combination of two or more kinds.
[0047] (Exterior body 50) The power generating element 90 and the non-aqueous electrolyte are sealed inside the exterior body 50. The exterior body 50 prevents the non-aqueous electrolyte from leaking to the outside and prevents moisture and the like from entering the lithium secondary battery 100 from the outside.
[0048] Although not shown, the exterior body 50 can have a metal foil and resin layers laminated on both sides of the metal foil.
[0049] The metal foil may be, for example, aluminum foil. The resin layer may be a polymer film such as polypropylene. The materials constituting the resin layer may be different between the inside and outside. For example, the outside material may be a polymer with a high melting point, such as polyethylene terephthalate (PET) or polyamide (PA), and the inside polymer film may be made of polyethylene (PE), polypropylene (PP), or the like.
[0050] Although not shown in the figure, typically, leads connected to the tabs of the positive and negative electrodes communicate with the inside and outside of the exterior body. The leads can be made of conductive materials such as aluminum, nickel, and nickel-plated copper metal plates. In particular, it is preferable to use an aluminum metal plate for the lead connected to the positive electrode 10 side, and it is preferable to use a nickel metal plate or a nickel-plated copper metal plate for the lead connected to the negative electrode 30C side.
[0051] In this embodiment, both outermost layers of the power generating element 90 are negative electrodes 30C, but this is not limited thereto, and for example, both outermost layers of the power generating element 90 may be positive electrodes.
[0052] There is no particular limitation on the number of layers of the positive electrode (or negative electrode), and it may be, for example, one layer or multiple layers such as 10 layers or 20 layers.
[0053] [Method of manufacturing lithium secondary battery] The lithium secondary battery according to this embodiment includes the following steps (a) and (b), and performs step (b) two or more times. (a) preparing a lithium secondary battery precursor including a negative electrode having a current collector layer and a lithium metal foil, and a positive electrode; (b) charging the lithium secondary battery precursor at 0.01 to 0.5C until the charge rate reaches 10 to 100%, and then discharging the lithium secondary battery precursor at 0.2C to 2.5C.
[0054] (Step (a)) The lithium secondary battery precursor has a negative electrode, a positive electrode, and a separator disposed between the negative electrode and the positive electrode. These are impregnated with a non-aqueous electrolyte. The negative electrode current collector layer, lithium metal foil, positive electrode, and separator can be the same as those of the lithium secondary battery 100 according to the above embodiment.
[0055] (Step (b)) By carrying out step (b) two or more times, the second lithium metal layer and the third lithium metal layer according to the above embodiment are formed. EXAMPLES
[0056] The present disclosure will be described below based on examples and comparative examples. Note that the present disclosure is not limited to the following examples. [Preparation of lithium secondary batteries] Example 1 A copper foil with a thickness of 8 μm was prepared as a current collector layer. A lithium metal foil with a thickness of 20 μm was placed on one main surface of the current collector layer, and then cut into a predetermined shape to obtain a first laminate having a main body and a tab.
[0057] The positive electrode slurry was applied to one side of an aluminum foil having a thickness of 15 μm, and then cut into a predetermined shape having a body and a tab portion similar to those of the negative electrode. The positive electrode slurry was prepared by mixing a positive electrode active material, a conductive additive, a binder, and a solvent.
[0058] LiNi, a composite metal oxide, is used as the positive electrode active material. x Co y Mn z M a O2 (x=0.83, y=0.09, z=0.07, a=0.01, M=Al) was used. Carbon black was used as a conductive additive. Polyvinylidene fluoride (PVDF) was used as a binder. The mass ratio of the positive electrode active material, conductive additive, and binder was 95:2:3. The amount of the positive electrode active material supported in the dried positive electrode active material layer was 10 mg / cm. 2 The solvent was removed from the positive electrode slurry in a drying furnace to prepare a positive electrode.
[0059] The first laminate and the positive electrode were alternately laminated with a 10 μm thick polypropylene separator in between, and 11 sheets of the first laminate and 10 sheets of the positive electrode were laminated to produce a second laminate. Both outermost electrodes were made of the first laminate. Furthermore, a nickel negative electrode lead was attached to the tab portion of the first laminate in the second laminate, and an aluminum positive electrode lead was attached to the tab portion of the positive electrode of the second laminate, respectively, by an ultrasonic welding machine.
[0060] The second laminate was then inserted into a case and heat-sealed except for one peripheral location to form a closed portion. After that, a non-aqueous electrolyte was poured into the case. The non-aqueous electrolyte was prepared by adding 4M (mol / L) LiN(FSO2)2 as a lithium salt to a 1,2-dimethoxyethane solvent. The remaining location was then heat-sealed while reducing the pressure using a vacuum sealer to produce a lithium secondary battery precursor.
[0061] Next, using a secondary battery charge / discharge tester (manufactured by Hokuto Denko Corporation), the lithium secondary battery precursor was charged and discharged in an environment of 25°C, and two charge / discharge cycles were performed. A lithium secondary battery was obtained in this manner. Charging was performed by a constant current charging method at a rate C shown in Table 1 until the state of charge (SOC) reached the value shown in Table 1. Discharging was performed by a constant current discharging method at a rate C shown in Table 1 until the cell voltage reached 3.0 V. The negative electrode of the obtained lithium secondary battery had a structure of a current collector layer / Li metal foil (first lithium metal layer) / a second lithium metal layer containing granular lithium metal / a third lithium metal layer containing lithium metal and being porous.
[0062] (Examples 2 to 10, Comparative Examples 2 and 3) A lithium secondary battery was obtained in the same manner as in Example 1, except that the C rate during charging, the charge rate, and the C rate during discharging in the charge-discharge cycle were set to the values shown in Table 1. The negative electrode of the obtained lithium secondary battery had a structure of a current collector layer / Li metal foil (first lithium metal layer) / second lithium metal layer containing granular lithium metal / third lithium metal layer containing lithium metal and being porous.
[0063] Comparative Example 1 A lithium secondary battery was obtained in the same manner as in Example 1, except that the charge / discharge cycle was performed once. The negative electrode of the obtained lithium secondary battery had a structure of a current collector layer / Li metal foil (first lithium metal layer) / a third lithium metal layer that is porous and contains lithium metal / a second lithium metal layer that contains granular lithium metal.
[0064] [evaluation] <Examples 1 to 10 and Comparative Examples 1 to 3> (Cycle characteristics) The charge-discharge capacity retention rate after cycling of the lithium secondary battery was measured using a secondary battery charge-discharge tester (manufactured by Hokuto Denko Corporation). In an environment of 25°C, a charge-discharge cycle was set as one charge-discharge cycle in which the battery was charged at a constant current and constant voltage of 0.2C to 4.3V, and then discharged at a constant current of 1C to 3.0V. The number of cycles required for the capacity to drop to 80% or less of the initial capacity was measured. The results are shown in Table 1.
[0065] (Thickness change of negative electrode) After 100 cycles, the lithium secondary battery was disassembled and the thickness change of the negative electrode was measured. The thickness change rate was calculated by ("thickness of negative electrode after 100 cycles" - "thickness of negative electrode before first charge") / ("thickness of negative electrode before first charge") x 100. The results are shown in Table 1.
[0066] (Average pore size of the third lithium metal layer) The main surface of the third lithium metal layer of the negative electrode of the lithium secondary battery was observed (magnification: 2000 times) with a scanning electron microscope (manufactured by Hitachi High-Technologies, product name "SU8010") and an image was taken. The obtained image was binarized based on the color to distinguish between voids and non-voids in the third lithium metal layer. The voids in the image were extracted and all void diameters were measured, and the average value was adopted as the average void diameter. The results are shown in Table 1.
[0067] (Porosity of the third lithium metal layer) The main surface of the third lithium metal layer of the negative electrode of the lithium secondary battery was observed (magnification: 2000 times) with a scanning electron microscope (manufactured by Hitachi High-Technologies Corporation, product name "SU8010") and an image was taken. The obtained image was binarized based on the brightness to distinguish between voids and non-voids in the third lithium metal layer. The porosity was measured from the binarized image. The results are shown in Table 1.
[0068] (Average particle size of second lithium metal layer) The cross section of the second lithium metal layer of the negative electrode of the lithium secondary battery was observed (magnification: 5000 times) with a scanning electron microscope (manufactured by Hitachi High-Technologies, product name "SU8010") and images were taken. The obtained images were binarized based on brightness to identify the particles of the second lithium metal layer. The diameters of all particles in the images were measured, and the average value was adopted as the average particle diameter. The results are shown in Table 1.
[0069] (area ratio S) The main surface of the negative electrode of the lithium secondary battery on the side of the third lithium metal layer was observed (magnification: 500 times) with a scanning electron microscope (manufactured by Hitachi High-Technologies, product name "SU8010") and an image was taken. The obtained image was binarized based on the brightness to distinguish the second lithium metal layer from the third lithium metal layer. From the binarized image, the area S2 of the second lithium metal layer when the main surface was observed in a planar view and the area S3 of the third lithium metal layer when the main surface was observed in a planar view were obtained. From S2 and S3, the area ratio S was calculated by the following formula (1). The results are shown in Table 1.
[0070] Area ratio S = {S3 / (S2+S3)} × 100... Equation (1) [In formula (1), S2 is the area of the second lithium metal layer on the main surface of the negative electrode of the lithium secondary battery on the third lithium metal layer side, and S3 is the area of the third lithium metal layer on the main surface of the negative electrode of the lithium secondary battery on the third lithium metal layer side.]
[0071] [Table 1]
[0072] FIG. 3(a) is an SEM photograph (magnification: 5000 times) of a part of the cross section of the negative electrode of the lithium secondary battery obtained in the example. It can be seen that a second lithium metal layer containing granular lithium metal and a porous third lithium metal layer are formed. FIG. 3(b) is an SEM photograph (magnification: 2000 times) of the main surface of the negative electrode of the lithium secondary battery obtained in the example on the third lithium metal layer side. It can be seen that a second lithium metal layer containing granular lithium metal and a porous third lithium metal layer are formed. FIG. 3(c) is an SEM photograph (magnification: 500 times) of the main surface of the negative electrode of the lithium secondary battery obtained in the example on the third lithium metal layer side. It can be seen that a second lithium metal layer 36 and a third lithium metal layer 38 are present. [Explanation of symbols]
[0073] 10...positive electrode, 30C...negative electrode, 32...current collector layer, 34, 36, 38...lithium metal layers, 36a...granular lithium metal, 100...lithium secondary battery.
Claims
1. A lithium secondary battery comprising a negative electrode and a positive electrode, The negative electrode is A current collector layer; a first lithium metal layer made of lithium metal foil; a second lithium metal layer including granular lithium metal; a third lithium metal layer comprising lithium metal and being porous; in that order, a lithium secondary battery, wherein the average particle size of the granular lithium metal is larger than the average pore size of the third lithium metal layer.
2. 2. The lithium secondary battery according to claim 1, wherein the porosity of the third lithium metal layer is 10 to 40%.
3. 3. The lithium secondary battery according to claim 1, wherein the third lithium metal layer has an average pore size of 0.1 to 3 μm.
4. 3. The lithium secondary battery according to claim 1, wherein the granular lithium metal has an average particle size of 1 to 22 μm.
5. 3. The lithium secondary battery according to claim 1, wherein an area ratio S calculated by the following formula (1) is 60 area % or more. Area ratio S = {S3 / (S2+S3)} x 100 ... formula (1) [In formula (1), S2 is the area of the second lithium metal layer on the main surface of the negative electrode facing the third lithium metal layer, and S3 is the area of the third lithium metal layer on the main surface of the negative electrode facing the third lithium metal layer.]
6. (a) preparing a lithium secondary battery precursor including a negative electrode having a current collector layer and a lithium metal foil, and a positive electrode; (b) charging the lithium secondary battery precursor at 0.01 to 0.5 C until the charge rate reaches 10 to 100%, and then discharging the lithium secondary battery precursor at 0.2 C to 2.5 C; Equipped with A method for producing a lithium secondary battery, comprising carrying out the step (b) two or more times.
Citation Information
Patent Citations
Application of force in electrochemical cells
JP2014239047A
Sulfur-carbon composite, method for producing the same, positive electrode for lithium-sulfur battery including the same, and lithium-sulfur battery
JP2021521600A
Electrolyte solution, secondary battery, and module
WO2020246579A1
Secondary battery electrode and method for manufacturing secondary battery electrode