Shaft body of pencil or cosmetics

A shaft material composition for pencils and cosmetics, composed of naturally derived extenders, binders, and pigments, addresses environmental concerns and aesthetic challenges by ensuring easy cutting, drop resistance, and water resistance, while enabling customizable coloration of the shaft appearance.

JP2024152297AInactive Publication Date: 2024-10-25MITSUBISHI PENCIL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023066409
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing pencil and cosmetic shaft materials face environmental burdens due to high energy consumption and dye waste in impregnation, and difficulty in achieving desired aesthetic treatments, especially at the cut cross section, while alternative materials often rely on thermoplastic or thermosetting resins that also contribute to environmental impact.

Method used

A shaft material composition for pencils and cosmetics comprising naturally derived extenders, binders, and pigments, with a natural origin index of 75% or more, allowing for easy cutting, drop resistance, and water resistance without the need for painting, and enabling coloration of the cut cross section.

Benefits of technology

The solution provides pencils and cosmetics with ease of cutting, drop resistance, and water resistance, while minimizing environmental impact, and allowing for customizable coloration of the shaft appearance, including the cut cross section, using environmentally friendly materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152297000001
    Figure 2024152297000001
Patent Text Reader

Abstract

To provide a shaft body of a pencil lead (including a color pencil lead) which is easy to sharpen and has falling resistance and water resistance just like a conventional wood shaft, has low environmental impact, and allows an appearance including a cutting cross-section to be made into any color without coating, or a shaft body of a cosmetic such as a rod-like cosmetic such as an eye liner, an eyebrow and an eye shadow.SOLUTION: There is provided a shaft body of a pencil or a cosmetic obtained by coating a pencil lead or a rod-like cosmetic with a shaft body material composition, in which the shaft body material composition contains at least a naturally derived extender, a naturally derived binder, and a pigment.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] To provide a pencil lead or a cosmetic shaft which has the same ease of sharpening, drop resistance, and water resistance as conventional wooden shafts, imposes little burden on the environment, and allows the appearance, including the cut cross section, to be colored in any desired color without painting. [Background technology]

[0002] Conventionally, natural wood, such as American red cedar, has been used for the shafts of pencils, stick-shaped cosmetics, and the like, because it provides a pleasant feel to the user and is soft and easy to sharpen with a knife or pencil sharpener. However, in recent years, forests have been decreasing due to deforestation and other indiscriminate harvesting, and this situation has drawn attention to the problem of environmental destruction. As a result, it has become difficult to obtain red cedar and other wood materials, and alternative materials are being developed. Furthermore, when coloring the shaft body made of the above-mentioned natural wood, the most common methods are to impregnate the natural wood itself with a liquid containing a dye, or to apply paint to the surface after forming the shaft body. However, the former method requires a large amount of energy during impregnation and generates waste dye liquid, which places a high burden on the environment, while the latter method leaves the cross section of the pencil lead or stick-shaped cosmetic product in its normal wood color when cut to expose the pencil lead or stick-shaped cosmetic product.

[0003] Conventionally, the following techniques 1) to 7) have been known as techniques for substitute materials for the barrels of pencils, stick-shaped cosmetics, and the like, and techniques for coloring these barrels. 1) A method for producing a plate-shaped material for pencil shafts, which comprises adding caustic soda or a soluble substance with the same effect to old newspapers, pulp wood chips, sawdust, or other plant fibrous materials, boiling and dissolving the mixture in water to make a liquid, forming the liquid into a plate, drying the plate, and then uniformly infiltrating one or more types of cellulose acetate, stearin, lacquer, urea resin, etc. into the inside of the plate and applying appropriate pressure to make the plate (see, for example, Patent Document 1).

[0004] 2) A pencil characterized in that the rod-shaped outer peripheral surface of a core material containing a thermoplastic resin, a lubricant, and graphite or a pigment has alternately continuous convex and concave stripes formed integrally along the axial direction, and a shaft material containing a thermoplastic resin, cellulose fibers, and a foaming agent is formed on the outside of the core material so as to closely contact the uneven surface of the stone material, and part of the cellulose fibers in the shaft material are mixed in and embedded in the uneven surface of the rod-shaped outer peripheral surface of the core material (see, for example, Patent Document 2).

[0005] 3) A pencil in which a lead is inserted into a pencil shaft obtained by mixing fine cellulose powder particles obtained by grinding with a resin, molding the mixture by extrusion or injection molding, and forming the molded body into a pencil shaft, in order to provide a pencil which can be sharpened with a pencil sharpener without any problems and which can be manufactured inexpensively because the shaft has excellent workability (see, for example, Patent Document 3);

[0006] 4) A method for producing a substantially rod-shaped composite from a core surrounded by at least one polymer obtained by plasticizing the polymer and extruding it onto a continuous core, characterized in that at least one natural polymer based on lignin is used and that slip agents based on natural oils and / or waxes are added to the plasticized polymer before or during extrusion, and further in that natural fibers are added to the plasticized polymer before or during extrusion, said method being for producing writing tools, such as pencils or colored pencils, for producing cosmetic pencils, composites that are coated, for example by applying a paint (see, for example, patent document 4);

[0007] 5) A wood substitute material for wooden-shaft pencils, comprising at least one polymer binder, at least one organic filler, at least one inorganic filler, at least one compatibilizer, at least one wax, at least one coloring pigment, and at least one additive, wherein the at least one compatibilizer forms a chemical bond between the at least one polymer binder and the at least one organic filler, the ratio of the at least one compatibilizer to the at least one wax is in the range of 1:2 to 1:6, and the total of the organic filler and the inorganic filler is 80% by weight or less (see, for example, Patent Document 5);

[0008] 6) A rigid fiberboard used as a pencil shaft, the fiberboard comprising fibers selected from the group consisting of natural fibers, synthetic fibers and mixtures thereof, a binder, a filler, a lubricant and a waterproofing agent, the natural fibers being cellulose fibers obtained from a source selected from the group consisting of wood pulp, linters, denim fibers, newspapers, cardboard boxes, kraft paper bags, bleached paper, kraft paper, cotton waste and mixtures thereof, the binder being selected from the group consisting of thermosetting resin binders and water-soluble gums and mixtures thereof, the water-soluble gums being selected from the group consisting of guar gum, carboxymethylcellulose and hydroxyethylcellulose and mixtures thereof, the filler being an inorganic particulate material selected from the group consisting of perlite, vermiculite, glass microbubbles and mixtures thereof, and further comprising at least one dye; a pencil comprising a marking core and a shaft encasing the core, the shaft being molded from a fiberboard comprising fibers, a binder, a filler, a lubricant and a waterproofing agent (see, for example, Patent Document 6);

[0009] 7) A hollow cylindrical biodegradable pencil-shaped synthetic cosmetic shaft that is molded using a biodegradable thermoplastic material consisting of a starch ester in which the hydrogen of the reactive hydroxyl group of the same starch molecule is substituted with a short-chain acyl group and a long-chain acyl group, and a reinforcing filler as a base material, in order to provide a synthetic pencil-shaped biodegradable cosmetic shaft that has excellent physical properties such as rigidity, machinability, and resistance to oil and grease penetration, and a good feel when used, and that is easily decomposed after disposal, can be burned with a low amount of heat, and does not generate harmful substances when incinerated, as well as a method for producing the same (see, for example, Patent Document 7); etc. are known.

[0010] However, in the above Patent Document 1, the plant fiber material needs to be dissolved by boiling, and in the above Patent Documents 2 to 5, a thermoplastic or thermosetting resin is used, so heating is essential during coloring, molding or curing, and so there is still a problem of a heavy burden on the environment. In addition, the above Patent Documents 6 and 7 use natural fibers and starch esters, but there is still a problem of a heavy burden on the environment, and the aesthetic treatment of the appearance, including the cut cross section, is still not sufficient. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP Patent Publication No. 37-2728 (Claims, etc.) [Patent Document 2] JP 60-204399 A (Claims, etc.) [Patent Document 3] JP 6-255296 A (Claims, etc.) [Patent Document 4] JP Patent Publication No. 2002-529273 (Claims, etc.) [Patent Document 5] Patent Publication No. 2011-528046 (Claims, etc.) [Patent Document 6] JP 5-96899 A (Claims, etc.) [Patent Document 7] JP 2001-192502 A (Claims, etc.) Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention is intended to solve the above-mentioned conventional problems, and has an object to provide a pencil lead or a cosmetic shaft that has the same ease of sharpening, drop resistance, and water resistance as conventional wooden shafts, has a low environmental impact, and further, the appearance, including the cut cross section, can be made any color without painting. [Means for solving the problem]

[0013] As a result of intensive research into the above-mentioned problems in the conventional art, the inventors have discovered that the above-mentioned desired pencil or cosmetic barrel can be obtained by covering a pencil lead or a rod-shaped cosmetic with a barrel material composition, where the barrel material composition contains at least an extender having specific physical properties, a binder, and a pigment, and have thus completed the present invention.

[0014] In other words, the pencil or cosmetic barrel of the present invention is a pencil or cosmetic barrel formed by covering a pencil lead or a rod-shaped cosmetic with a barrel material composition, and is characterized in that the barrel material composition contains at least a naturally derived filler, a naturally derived binder, and a pigment. The shaft material composition preferably has a natural origin index (excluding water) of 75% or more. The pencil of the present invention is a pencil comprising at least a pencil lead and a barrel formed by covering the pencil lead, characterized in that the barrel has the above-mentioned configuration, and the stick-shaped cosmetic of the present invention is a stick-shaped cosmetic comprising at least a stick-shaped cosmetic material and a barrel formed by covering the stick-shaped cosmetic material, characterized in that the barrel has the above-mentioned configuration. Effect of the Invention

[0015] According to the present invention, it is possible to provide a pencil lead or cosmetic barrel that has the same ease of sharpening, drop resistance, and water resistance as conventional wooden barrels, has a low environmental impact, and the appearance, including the cut cross section, can be made any color without painting, as well as a pencil, stick-shaped cosmetic product, and the like that are equipped with this barrel. The objects and advantages of the invention will be realized and obtained by means of the elements and combinations particularly pointed out in the claims. Both the foregoing general description and the following detailed description are exemplary and explanatory but are not restrictive of the invention as claimed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The following describes in detail the embodiments of the present invention. However, please note that the technical scope of the present invention is not limited to the embodiments described in detail below, but extends to the inventions described in the claims and their equivalents. The present invention can be implemented based on the contents disclosed in this specification and common technical knowledge in the relevant field (including design matters and obvious matters).

[0017] The pencil or cosmetic barrel of the present invention is a pencil or cosmetic barrel formed by covering a pencil lead or a rod-shaped cosmetic with a barrel material composition, and is characterized in that the barrel material composition contains at least a naturally derived filler, a naturally derived binder, and a pigment.

[0018] Examples of the naturally occurring filler used in the present invention include sawdust, wood flour, powdered cellulose, and naturally occurring inorganic powders obtained from naturally occurring wood. The sawdust that can be used is not particularly limited, and may be derived from broadleaf wood or coniferous wood. Specific tree species of sawdust used in the present invention include cedar, pine, larch, red pine, Abies sachalinensis, cypress, beech, horse chestnut, konara oak, Japanese oak, oak, linden, birch, Japanese elm, lauan, and Japanese hemlock. In particular, cedar, cypress sapwood, beech, horse chestnut, and Japanese oak are preferably used. In addition, waste generated during the manufacture of these wood materials may be effectively utilized. Furthermore, at least one type of sawdust (one type or a combination of two or more types, the same applies below) can be used. The size of the sawdust is preferably an average particle size of 10 mesh or more from the standpoint of dispersibility and moldability, and more preferably 200 mesh or less from the standpoint of the energy costs involved in crushing.

[0019] Examples of wood flour that can be used include at least one of wood flours obtained from each of the tree species exemplified above for sawdust, wood flour obtained from the above sawdust or waste wood, sander powder, etc. In order to further improve dispersibility and moldability, the upper limit of the average particle size of the wood flour is preferably, for example, 2000 μm or less, and the lower limit is preferably, for example, 100 μm or more, but microfibrillated fibrous wood may also be used. The average particle size in the present invention can be a value measured according to a laser diffraction / scattering method.

[0020] The powdered cellulose that can be used is preferably a cellulose powder obtained by finely pulverizing cellulose fibers of natural plants, and has an average particle size of 100 μm or less, preferably in the range of 10 to 50 μm. As the powdered cellulose, for example, a crystalline cellulose powder having a certain particle size distribution produced by purifying and drying the undecomposed residue obtained after acid hydrolysis of selected pulp, followed by pulverization and sieving, may be used, or a commercially available product such as "KC Flock" (manufactured by Nippon Paper Chemicals Co., Ltd.), "Ceolas" (manufactured by Asahi Kasei Chemicals Co., Ltd.), or "Avicel" (manufactured by FMC Corporation) may be used.

[0021] As the naturally occurring inorganic powder that can be used, at least one of talc, calcium carbonate, huntite, kaolin, sericite, bentonite, titanium oxide, and the like can be used. The upper limit of the average particle size of these inorganic powders is preferably, for example, 50 μm or less, and the lower limit is preferably, for example, 1 μm.

[0022] The content of these naturally occurring fillers is preferably 60 to 90% by mass, more preferably 70 to 80% by mass, based on the total amount of the shaft material composition. By making the content of these naturally occurring fillers 60% by mass or more, usable machinability can be achieved, and by making it 90% by mass or less, usable strength can be achieved. Furthermore, since the proportion of inorganic powder among these naturally derived fillers is 60 mass % or less, the drop resistance of the barrel is improved, and when made into a pencil or cosmetic product, it is possible to prevent breakage inside the pencil lead or stick-shaped cosmetic product.

[0023] The naturally occurring binder used in the present invention may be at least one of cellulose fibers (including nanofibers), methylcellulose or a salt thereof, carboxymethylcellulose or a salt thereof, hydroxymethylpropylcellulose or a salt thereof, cellulose acetate or a salt thereof, sodium alginate, etc. Examples of the salts of the above celluloses include sodium, ammonium, calcium, etc. These binders are preferably water-soluble, and more preferably ammonium carboxymethylcellulose in order to impart water resistance.

[0024] The content of these naturally occurring binders is preferably 10 to 40 mass %, and more preferably 20 to 30 mass %, based on the total amount of the shaft material composition. By making the content of this naturally occurring binder 10% by mass or more, usable strength can be achieved, and by making it 40% by mass or less, usable machinability can be achieved.

[0025] In addition to the above-mentioned naturally derived filler and naturally derived binder, the shaft material composition of the present invention may further contain a crosslinking agent that crosslinks the binder in order to further enhance the effects of the present invention and to impart water resistance. The crosslinking agent for crosslinking the binder is preferably one having a carboxylic acid group for ester-crosslinking the binder, and specific examples thereof include succinic acid, malic acid, maleic acid, tartaric acid, citric acid, and polyacrylic acid. The content of these crosslinking agents is preferably 0.1 to 5 mass%, and more preferably 0.5 to 2 mass%, of the total amount of the shaft material composition in order to exhibit water resistance, to prevent a decrease in strength due to moisture absorption, and to prevent discoloration of the material.

[0026] Examples of the pigments used in the present invention include inorganic pigments and organic pigments. In the present invention, the above-mentioned natural body materials and natural binders are used to form the shafts of pencils or cosmetics that are environmentally friendly, so it is preferable to use pigments that are environmentally friendly. Therefore, it is not preferable to use resin particle pigments, white plastic pigments, hollow resin particles, thermochromic pigments, photochromic particles, and composite particles thereof that contain pigments.

[0027] Examples of inorganic pigments that can be used include at least one of carbon black, titanium black, zinc white, red iron oxide, aluminum, chromium oxide, iron black, cobalt blue, iron oxide yellow, viridian, zinc sulfide, lithopone, cadmium yellow, vermilion, cadmium red, yellow lead, molybdate orange, zinc chromate, strontium chromate, white carbon, clay, talc, ultramarine, precipitated barium sulfate, baryte powder, calcium carbonate, white lead, dark blue, Prussian blue, manganese violet, aluminum powder, brass powder, titanium oxide, zinc oxide, silica powder, and lithopone.

[0028] Examples of organic pigments that can be used include azo lakes, insoluble azo pigments, chelate azo pigments, phthalocyanine pigments, perylene and perinone pigments, nitroso pigments, etc. More specifically, CI Pigment Blue 15, CI Pigment Blue 17, CI Pigment Blue 27, CI Pigment Red 5, CI Pigment Red 22, CI Pigment Red 38, CI Pigment Red 48, CI Pigment Red 49, CI Pigment Red 53, CI Pigment Red 57, CI Pigment Red 81, CI Pigment Red 104, CI Pigment Red 146, CI Pigment Red 245, CI Pigment Yellow 1, CI Pigment Yellow 3, CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Red 146, CI Pigment Red 245, CI Pigment Yellow 1, CI Pigment Yellow 3, CI Pigment Yellow 146, CI Pigment Yellow 245 ... and at least one of CI Pigment Yellow 14, CI Pigment Yellow 17, CI Pigment Yellow 34, CI Pigment Yellow 55, CI Pigment Yellow 74, CI Pigment Yellow 95, CI Pigment Yellow 166, CI Pigment Yellow 167, CI Pigment Orange 5, CI Pigment Orange 13, CI Pigment Orange 16, CI Pigment Violet 1, CI Pigment Violet 3, CI Pigment Violet 19, CI Pigment Violet 23, CI Pigment Violet 50, and CI Pigment Green 7. Among these pigments, it is preferable to use inorganic pigments, particularly iron oxide, iron oxide yellow, red iron oxide, titanium oxide, etc., from the viewpoints of light resistance and heat resistance. The average particle size of these pigments is preferably 0.1 to 2 μm in order to prevent a decrease in strength and to achieve sufficient coloring power. In the present invention (including examples), the "average particle size" is the D50 value measured using a particle size analyzer (Microtrac HRA9320-X100 (manufactured by Nikkiso Co., Ltd.)).

[0029] The content of these pigments is preferably 0.2 to 5 mass %, and more preferably 0.5 to 2 mass %, based on the total amount of the shaft material composition, in order to avoid a decrease in strength and to obtain good color development. Furthermore, the shaft material composition of the present invention may contain, in addition to the above-mentioned naturally derived fillers, naturally derived binders, crosslinking agents, and pigments, antibacterial agents, preservatives, fragrances, etc., as necessary.

[0030] From the viewpoint of further exerting the effects of the present invention and from the viewpoint of the burden on the environment, it is preferable that these shaft material compositions have a natural origin index (excluding water) of 75% or more. The "natural index (excluding water)" refers to an index indication according to ISO 16128, and by making this natural index (excluding water) 75% or more, and more preferably 85% or more, it is possible to obtain pencil leads or cosmetic barrels that have an even smaller impact on the environment. The natural index (excluding water) of this shaft material composition can be set to 75% or more by appropriately selecting the above-mentioned natural extenders, natural binders, and pigments.

[0031] The shaft of the pencil or cosmetic of the present invention is prepared by dry-mixing the blended composition consisting of the above-mentioned natural body material, natural binder, pigment, etc., using a kneading machine such as a Henschel mixer, planetary mixer, kneader, etc., and then adding water (purified water, distilled water, etc.) so that the moisture content is 40 to 80%, kneading to obtain a slurry, which is further kneaded while heating and degassing to obtain a clay-like mixture with a moisture content of about 30 to 60%, and this mixture is coated with the above-mentioned material on the outer periphery of the pencil lead or cosmetic to be coated using a die of a specified diameter using an extrusion molding machine, etc., and dried to obtain a pencil or cosmetic. Alternatively, the kneaded mixture is molded into a round bar or plate shape using a die of a specified diameter or a T-die using an extrusion molding machine, etc., and dried to produce a molded body, which is then processed to insert the pencil lead or cosmetic. Furthermore, the physical properties of the barrel can be widely controlled by combining the pressing pressure, moisture content, natural extenders and binders during extrusion molding, etc., so that it is possible to obtain barrels that are suitable for pencils or cosmetics and that satisfy the desired texture, strength, moldability, and color appearance including the cut cross section.

[0032] In the present invention, the composition and form of the pencil lead to be covered with the shaft material composition are not particularly limited, and examples thereof include baked pencil leads (including baked color pencil leads) and non-baked pencil leads (including non-baked color pencil leads). Examples of baked pencil leads include baked pencil leads obtained by mixing, dispersing, kneading, and extruding a thin wire-shaped core obtained by subjecting the core obtained by heat treatment up to the baking temperature to a baking temperature, and impregnating the core with oils and waxes such as silicone oil, liquid paraffin, spindle oil, squalane, and α-olefin oligomers.

[0033] Furthermore, the composition and form of the rod-shaped cosmetic to be coated with the shaft material composition are not particularly limited, and examples include compositions used for applications such as eyeliner, eyebrow, lip liner, concealer pencil, eyeshadow pencil, etc., such as cosmetics obtained by kneading waxes or clays such as oils and fats, waxes, fatty acids, and hydrocarbons as binders, colorants, and bodying agents, and shaping the mixture into a rod shape, and these may be baked or non-baked rod-shaped cosmetics.

[0034] The pencil lead or cosmetic barrel of the present invention configured in this manner has the same ease of sharpening, drop resistance, and water resistance as conventional wooden barrels, the appearance, including the cut cross section, can be made any color, it has a low environmental impact, and can be used without improving the molding machines used in molding conventional pencils and cosmetics, resulting in a pencil lead or cosmetic barrel that can be easily manufactured.

[0035] The pencil of the present invention is characterized in that at least the shaft is formed by covering and molding the pencil lead as described above, and the stick-shaped cosmetic of the present invention is characterized in that at least the shaft is formed by covering and molding the stick-shaped cosmetic material as described above, and the stick-shaped cosmetic of the present invention is characterized in that .... In the present invention, the pencil lead and stick-shaped cosmetic material can be formed into any shape, for example, a cross-sectional shape that is circular (including oval), a polygonal shape such as a triangular or hexagonal shape, or a tubular shape, and therefore pencils and stick-shaped cosmetics of various shapes can be made by various processing methods such as coating and molding and cutting. EXAMPLES

[0036] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these examples. The pencil leads used in Examples 1 to 9 and Comparative Examples 1 to 3 were obtained by the following method. Graphite 60% by mass and clay 40% by mass were dry mixed in a Henschel mixer, and then purified water was added to the mixture so that the moisture content was 40%. The obtained slurry was heated and kneaded while being degassed to obtain a clay-like mixture with a moisture content of about 30%. This was molded in a die with a diameter of 2.5 mm using a hydraulic plunger type extrusion molding machine, and the molded body was dried in a 60°C environment and then fired at 800 to 1400°C for 12 to 24 hours to obtain a core body with a diameter of 2.0 mm. The obtained core body was impregnated with α-olefin oligomer to obtain a pencil lead with a diameter of 2.0 mm and a hardness of HB.

[0037] Example 1 Cedar wood sawdust (16 mesh) 69% by mass Black iron oxide 1% by mass Ammonium carboxymethylcellulose 30% by mass The natural origin index (excluding water) of this shaft material composition was 91.5%. The above blended composition was dry-mixed in a Henschel mixer, and then purified water was added to give a moisture content of 50%, followed by kneading. The obtained slurry was kneaded while being heated and deaerated to obtain a clay-like mixture with a moisture content of about 40%. This was then extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine to coat the material around a pencil lead with a diameter of 2.0 mm and hardness of HB. This molded body was dried in an environment of 60°C and then heated at 180°C to make the binder insoluble in water, thereby obtaining a pencil with a black appearance.

[0038] Example 2 Huntsmanite powder (average particle size 2 μm) 89% by mass Black iron oxide 1% by mass Cellulose powder (average particle size 45 μm) 10% by mass The natural origin index (excluding water) of this shaft material composition was 99.0%. The above blended composition was dry-mixed in a Henschel mixer, and then purified water was added to give a moisture content of 50%, followed by kneading. The obtained slurry was kneaded while being heated and deaerated to obtain a clay-like mixture with a moisture content of about 40%. This was then extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine to coat the material around a pencil lead with a diameter of 2.0 mm and hardness of HB. The molded product was dried in an environment of 60°C to obtain a pencil having a black appearance.

[0039] Example 3 Talc (average particle size 8 μm) 29% by mass Cellulose powder (average particle size 45 μm) 60% by mass Black iron oxide 1% by mass Ammonium carboxymethylcellulose 10% by mass The natural origin index (excluding water) of this shaft material composition was 96.5%. The above blended composition was dry mixed in a Henschel mixer, and then purified water was added to the mixture so that the moisture content was 50%. The obtained slurry was heated and kneaded while being deaerated to obtain a clay-like mixture with a moisture content of about 40%. This was then extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine to coat the material on the outer periphery of a pencil core with a diameter of 2.0 mm and hardness of HB. The molded product was dried in a 60°C environment and heated at 180°C to make the binder insoluble in water, resulting in a pencil with a black appearance.

[0040] Example 4 Talc (average particle size 8 μm) 28.5% by mass Cellulose powder (average particle size 45 μm) 60% by mass CI Pigment Red 245 1.5% by mass Ammonium carboxymethylcellulose 10% by mass The natural origin index (excluding water) of this shaft material composition was 97.0%. The above blended composition was dry mixed in a Henschel mixer, and then purified water was added to the mixture so that the moisture content was 50%. The obtained slurry was heated and kneaded while being deaerated to obtain a clay-like mixture with a moisture content of about 50%. This was then extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine to coat the material on the outer periphery of a pencil lead with a diameter of 2.0 mm and hardness of HB. The molded product was dried in a 60°C environment and heated at 180°C to make the binder insoluble in water, and a pencil with a red appearance was obtained.

[0041] Example 5 Talc (average particle size 8 μm) 28% by mass Cellulose powder (average particle size 45 μm) 60% by mass Iron oxide yellow 2% by mass Ammonium carboxymethylcellulose 10% by mass The natural origin index (excluding water) of this shaft material composition was 95.5%. The above blended composition was dry mixed in a Henschel mixer, and then purified water was added to the mixture so that the moisture content was 50%. The obtained slurry was heated and kneaded while being deaerated to obtain a clay-like mixture with a moisture content of about 40%. This was then extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine to coat the material on the outer periphery of a pencil lead with a diameter of 2.0 mm and hardness of HB. The molded product was dried in a 60°C environment and heated at 180°C to make the binder insoluble in water, resulting in a pencil with a yellow appearance.

[0042] Example 6 Talc (average particle size 8 μm) 28% by mass Cellulose powder (average particle size 45 μm) 60% by mass CI Pigment Yellow 3 0.5% by mass CI Pigment Red 22 0.4% by mass Bengara 1.1% by mass Ammonium carboxymethylcellulose 10% by mass The natural origin index (excluding water) of this shaft material composition was 95.5%. The above blended composition was dry mixed in a Henschel mixer, and then purified water was added to the mixture so that the moisture content was 50%. The obtained slurry was heated and kneaded while being deaerated to obtain a clay-like mixture with a moisture content of about 40%. This was then extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine to coat the material on the outer periphery of a pencil lead with a diameter of 2.0 mm and hardness of HB. The molded product was dried in an environment of 60°C and heated at 180°C to make the binder insoluble in water, and a pencil with a brown appearance was obtained.

[0043] Example 7 Talc (average particle size 8 μm) 29% by mass Cellulose powder (average particle size 45 μm) 60% by mass Iron oxide black 1% by mass Sodium carboxymethylcellulose 10% by weight The natural origin index (excluding water) of this shaft material composition was 94.1%. The above blended composition was dry mixed in a Henschel mixer, and then a 5% aqueous solution of succinic acid was added to the mixture so that the moisture content was 50%, followed by kneading. The resulting slurry was heated and kneaded while being deaerated to obtain a clay-like mixture with a moisture content of about 40%. This was then extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine, and the material was coated on the outer periphery of a pencil core with a diameter of 2.0 mm and hardness of HB. This molded product was dried in an environment of 60°C, and then heated at 180°C to crosslink the binder, resulting in a pencil with a black appearance.

[0044] Example 8 Talc (average particle size 8 μm) 29% by mass Cellulose powder (average particle size 45 μm) 60% by mass Iron oxide black 1% by mass Methylcellulose 10% by weight The natural origin index (excluding water) of this shaft material composition was 96.5%. The above blended composition was dry mixed in a Henschel mixer, and then purified water was added to the mixture so that the moisture content was 50%. The obtained slurry was heated and kneaded while being deaerated to obtain a clay-like mixture with a moisture content of about 40%. This was extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine to coat the material on the outer periphery of a pencil lead with a diameter of 2.0 mm and hardness of HB. The molded body was dried in a 60°C environment to obtain a pencil with a black appearance.

[0045] Example 9 Talc (average particle size 8 μm) 29% by mass Cellulose powder (average particle size 45 μm) 60% by mass Black iron oxide 1% by mass Methylcellulose 10% by weight The natural origin index (excluding water) of this shaft material composition was 94.1%. The above blended composition was dry mixed in a Henschel mixer, and then a 5% aqueous solution of succinic acid was added to the mixture so that the moisture content was 50%. The obtained slurry was heated and kneaded while being deaerated to obtain a clay-like mixture with a moisture content of about 40%. This was then extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine to coat the material on the outer periphery of a pencil core with a diameter of 2.0 mm and hardness of HB. This molded product was dried in an environment of 60°C, and then heated at 180°C to crosslink the binder, obtaining a pencil with a black appearance.

[0046] Example 10 Preparation of Solid Cosmetics 20 parts beeswax Ozokerite 10 parts Microcrystalline wax 10 parts Carnauba wax 8 parts 7 parts Vaseline 5 parts lanolin Liquid Paraffin 7 parts Isopropyl myristate 4 parts The above blended materials were dissolved, to which 10 parts of iron oxide and 19 parts of red iron oxide were added, stirred and dispersed, then kneaded in a mixer, cooled to room temperature, and then extruded to obtain a 2.0 mm brown solid cosmetic preparation.

[0047] Talc (average particle size 8 μm) 29% by mass Cellulose powder (average particle size 45 μm) 60% by mass Black iron oxide 1% by mass Methylcellulose 10% by weight The natural origin index (excluding water) of the above shaft material composition was 96.5%. The above blended composition was dry mixed in a Henschel mixer, and then purified water was added to a moisture content of 50% and kneaded. The obtained slurry was heated and kneaded while being deaerated to obtain a clay-like mixture with a moisture content of about 40%. This was then coated onto the above solid cosmetic material with a diameter of 2.0 mm using a hydraulic plunger type extrusion molding machine with a die with a diameter of 9.0 mm. The molded product was dried in an environment of 60°C to obtain a bar-shaped cosmetic material with a black appearance.

[0048] Comparative Example 1 Pencil (A pencil made by cutting an incense cedar board impregnated with 2% paraffin wax by weight, and coating the pencil core with the above-mentioned 2.0 mm diameter and HB hardness. The surface of the shaft is colored with paint containing black iron oxide.)

[0049] Comparative Example 2 This pencil is made from known recycled natural materials, and uses a thermoplastic resin as the binder, which is a non-natural material, and the barrel surface is coated with a thermoplastic resin that contains a coloring agent. The barrel has the following composition, and the natural index is 70.0%. Polypropylene (PP) 20% by mass Wood flour 70% by weight Maleic anhydride grafted polypropylene 1% by weight Amide wax 3% by weight Stearic acid 1% by weight Boron nitride 5% by weight

[0050] Comparative Example 3 Talc (average particle size 8 μm) 30% by mass Cellulose powder (average particle size 45 μm) 60% by mass Ammonium carboxymethylcellulose 10% by mass The natural origin index (excluding water) of this shaft material composition was 97.5%. The above blended composition was dry mixed in a Henschel mixer, and then purified water was added to the mixture so that the moisture content was 50%. The obtained slurry was heated and kneaded while being deaerated to obtain a clay-like mixture with a moisture content of about 40%. This was then extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine to coat the material on the outer periphery of a pencil lead with a diameter of 2.0 mm and hardness of HB. The molded product was dried in an environment of 60°C and heated at 180°C to make the binder insoluble in water, and a pencil with a white appearance was obtained.

[0051] The pencils and stick-shaped cosmetics of Examples 1 to 10 and Comparative Examples 1 to 3 obtained above were evaluated for their natural origin index, ease of sharpening, and appearance including the cut cross section, using the evaluation method described below. The results are shown in Table 1 below.

[0052] (natural origin index) The natural origin index (excluding water) of the shaft bodies of Examples 1 to 10 and Comparative Examples 1 to 3 was determined by calculating the composition ratio as a percentage from the weight ratio of the raw materials blended into the shaft material excluding the core, using the weight excluding water of the natural raw materials and the naturally derived parts of the naturally derived raw materials defined in ISO 16128. The higher this value, the higher the ratio of animal and plant-derived materials and the less petroleum-derived materials used, indicating a smaller burden on the environment.

[0053] (Method of evaluating ease of cutting) For the pencils and stick-shaped cosmetics of Examples 1 to 10 and Comparative Examples 1 to 3, the tips were trimmed to a diameter of 2 mm using a pencil sharpener, and then the pencil was sharpened by rotating the pencil on the side opposite the sharpener by hand using a pencil sharpener installed in a fixture connected to a rotation moment measuring device until the lead was sharpened. The peak value of the rotation moment during this period was measured, and the ease of sharpening (cuttability) was evaluated according to the following evaluation criteria. If this value is less than 0.1 N, it can be said to be easily cut, and if it exceeds 0.2 N·m, it is said to be hard and difficult to cut. Evaluation criteria: ○: Easily cut (less than 0.1 N m) △: Abrasion (0.1N m or more but less than 0.2N m) ×: Difficult to cut (0.2N·m or more)

[0054] (Method of evaluating appearance including cut cross section) For the pencils and stick-shaped cosmetics of Examples 1 to 10 and Comparative Examples 1 to 3, a pencil sharpener was used to expose the cut surfaces, and the colors of the shaft and the cut surfaces were observed. The appearance, including the cut surfaces, was evaluated according to the following evaluation criteria. Evaluation criteria: ○: Both the shaft and the cut surface are of the desired color △: The shaft surface is a random color, but the cut surface is not colored. ×: Not colored and not colored in any particular way

[0055] [Table 1]

[0056] Considering the evaluation results in Table 1, it was confirmed that Examples 1 to 10 within the scope of the present invention have the same easy-to-cut property as Comparative Examples 1 to 3, but have low environmental impact, and can easily make the appearance, including the cut cross section, any color. In addition, in Examples 1, 3 to 10, the inorganic powder ratio in the body material is set to 60% or less while maintaining a high natural origin index, and when evaluated by performing free drop 10 times from a height of 75 cm onto a concrete floor, no damage was observed in the pencil or cosmetic body, and the pencil core or stick-shaped cosmetic, and it was confirmed that they have sufficient drop resistance. Furthermore, in Examples 1, 3 to 7, and 9, the naturally derived binder was made insoluble by using carboxymethylcellulose ammonium, or crosslinked with a crosslinking agent having a carboxylic acid group that forms ester crosslinks, when the water resistance (water resistance after immersing the manufactured pencil in purified water for 24 hours) was evaluated, it was confirmed that it did not disintegrate, and it was confirmed that it can exhibit sufficient water resistance. [Industrial Applicability]

[0057] It is possible to obtain pencil or cosmetic barrels suitable for pencil leads (including colored pencil leads) and stick-shaped cosmetics such as eyeliner, eyebrow pencil, and eyeshadow.

Claims

1. The shaft of a pencil or cosmetic product is formed by covering a pencil lead or a rod-shaped cosmetic product with a shaft material composition, the shaft material composition containing at least a naturally derived filler, a naturally derived binder, and a pigment.

2. 2. The pencil or cosmetic barrel according to claim 1, characterized in that the barrel material composition has a natural origin index (excluding water) of 75% or more.

3. A pencil comprising at least a pencil lead and a shaft body formed by covering the pencil lead, the shaft body being the shaft body according to claim 1 or 2.

4. 3. A stick-shaped cosmetic comprising at least a stick-shaped cosmetic material and a shaft body formed by covering the stick-shaped cosmetic material, wherein the shaft body is the shaft body according to claim 1 or 2.

Citation Information

Patent Citations

  • JP1962-002728B

  • pencil

    JP1985204399A

  • Rigid fiberboard

    JP1993096899A

  • Pencil

    JP1994255296A

  • Synthetic shaft for biodegradable pencil-shaped cosmetic and method for manufacturing the same

    JP2001192502A