Method for producing cement clinker

The use of single-mode microwaves for localized heating in cement clinker production addresses the inefficiencies and environmental impact of conventional methods, enabling efficient and low-emission cement clinker production with improved quality.

JP2024153167APending Publication Date: 2024-10-29TOHOKU UNIV +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023066889
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The conventional method of producing cement clinker at high temperatures results in significant energy consumption and greenhouse gas emissions, with approximately 60% of raw material being limestone and 40% from fossil energy, necessitating a more efficient and environmentally friendly manufacturing process.

Method used

A method utilizing single-mode microwaves to directly and intensively heat cement clinker raw materials in a microwave irradiation device, focusing on localized energy concentration to produce cement clinker efficiently in a short time, reducing the risk of half-cooking and minimizing fossil energy use.

Benefits of technology

This approach allows for the production of cement clinker with reduced CO2 emissions and energy consumption, achieving high belite content and low free lime content, thereby improving the quality and efficiency of the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153167000003
    Figure 2024153167000003
  • Figure 2024153167000004
    Figure 2024153167000004
  • Figure 2024153167000001
    Figure 2024153167000001
Patent Text Reader

Abstract

To provide a novel method for producing a cement clinker.SOLUTION: A method for producing a cement clinker includes the following steps (a) to (c): (a) a step of filling a reaction tube in a microwave irradiation device with a cement clinker material; (b) a step of radiating a single-mode microwave on the cement clinker material and calcining it to obtain a calcined product; and (c) a step of grinding the calcined product to obtain a ground product.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing cement clinker. [Background technology]

[0002] Cement clinker is produced by putting cement clinker raw materials into a rotary kiln and burning them at a high temperature of around 1450°C (Patent Document 1). However, this production method emits CO2, of which about 60% comes from the raw material limestone (CaCO3), and the remaining 40% comes from fossil energy consumed in burning and crushing the clinker. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2007-169161 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, in order to achieve the goals of the Paris Agreement, Japan has set goals of achieving net-zero greenhouse gas emissions by 2050 and a 50% reduction in greenhouse gas emissions by 2030, so there is a demand for the development of new methods for producing cement clinker. An object of the present invention is to provide a novel method for producing cement clinker. [Means for solving the problem]

[0005] The present inventors have conducted various studies on heat sources for cement clinker raw materials, and have focused on the characteristic that microwaves have little energy loss and can directly heat the target object. They have found that, among microwaves, single-mode microwaves can locally concentrate energy (electric field or magnetic field, hereinafter the same) and can complete heating to a desired temperature in a short time. They have also found that by filling the cement clinker raw materials in a reaction tube provided in the cavity of a microwave irradiation device at a position where the energy intensity of the single-mode microwave is maximum and uniform, and then irradiating the raw materials with microwaves, the cement clinker raw materials are selectively and directly heated, and cement clinker can be efficiently produced in a short time without being in a half-baked state. In this specification, the term "half-baked state" refers to a state in which the content of free lime (hereinafter also referred to as "f.CaO") in the cement clinker exceeds 1 mass% due to insufficient burning.

[0006] That is, the present invention provides the following [1] to [4]. [1] The following steps (a) to (c); (a) charging a cement clinker raw material into a reaction tube of a microwave irradiation device; (b) irradiating the cement clinker raw material with single-mode microwaves to burn it and obtain a burned product; (c) A step of pulverizing the fired product to obtain a pulverized product. A method for producing cement clinker, comprising: [2] The method for producing cement clinker according to [1] above, comprising a step (d) of sequentially subjecting the pulverized product to steps (a) to (c) after the step (c). [3] The method for producing cement clinker according to [1] above, wherein the step (d) is carried out once or twice or more. [4] The method for producing cement clinker according to any one of the above [1] to [3], wherein the mixture is fired at a temperature of 1000°C or higher for 1 to 5 minutes per microwave irradiation. Effect of the Invention

[0007] According to the present invention, a new method for producing cement clinker can be provided. According to the present invention, it is possible to produce cement clinker efficiently in a short time without the cement clinker being in an under-baked state, and it is expected that the amount of CO2 generated from fossil energy will be significantly reduced compared to the conventional method for producing cement clinker using a furnace. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a diagram showing an example of a microwave irradiation device applicable to the present invention. [Diagram 2] FIG. 1 is a diagram showing the results of measuring the integrated calorific value of cement paste prepared using cement clinker. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The method for producing cement clinker of the present invention includes steps (a) to (c). Each step will be described below.

[0010] <Process (a)> This process is a process in which the cement clinker raw material is filled into the reaction tube of the microwave irradiation device. Microwaves are classified into multi-mode and single-mode according to the electromagnetic field distribution. For example, a microwave oven is known as a multi-mode microwave irradiating device. The inventors of the present invention tried to produce cement clinker using a multi-mode microwave irradiating device, and confirmed that the cement clinker was produced in an uncooked state, and therefore it was necessary to install a heating auxiliary material around the cement clinker raw material or to preheat the cement clinker raw material in advance. It was presumed that the reason for this is that the multi-mode microwave is oscillated in various directions in the multi-mode cavity, making it difficult to heat the cement clinker raw material in a concentrated manner. Therefore, the inventors of the present invention found that by selecting a single mode as the microwave, and then filling the cement clinker raw material at a position where the energy intensity of the microwave is maximum and uniform in the reaction tube provided in the single-mode cavity and irradiating the microwave, only the cement clinker raw material can be heated in a concentrated manner, and therefore cement clinker can be produced efficiently in a short time without being in an uncooked state.

[0011] (Cement clinker raw material) The cement clinker raw material is not particularly limited as long as it is a common raw material used in the production of cement clinker. Examples of the raw material include calcium-containing raw material (CaO source), silicon-containing raw material (SiO2 source), aluminum-containing raw material (Al2O3 source), and iron-containing raw material (Fe2O3 source). Examples of the calcium-containing raw material include limestone, quicklime, and slaked lime, and examples of the silicon-containing raw material include silica stone. Examples of the aluminum-containing raw material include clay, and examples of the iron-containing raw material include iron slag and iron cake. In addition, waste and by-products such as coal ash, construction soil, sludge, slag, and incineration ash can also be used as alternative raw materials. Examples of the construction soil include soil, earth and sand (e.g., boring waste soil generated by excavating the ground), and residual soil that are generated secondarily at construction sites and construction sites. Examples of the sludge include sewage sludge, water purification sludge, steelmaking sludge, and construction sludge. An example of the incineration ash is municipal waste incineration ash.

[0012] From the viewpoint of accelerating the burning reaction, various raw materials may be mixed and used as the cement clinker raw material. The mixing method is not particularly limited, and may be manual mixing or using a mixer. An industrial mixer may be used as the mixer. The cement clinker raw material may be pulverized, and a pulverizer may be used for pulverization. As the pulverizer, an industrial pulverizer, such as a ball mill or a disk mill, may be used.

[0013] (Microwave irradiation device)

[0014] An example of a microwave irradiation device applicable to the manufacturing method according to the present invention is shown in Fig. 1. In the description of the drawings, the same elements are given the same reference numerals, and duplicated descriptions are omitted. For convenience of illustration, the dimensional ratios of the drawings do not necessarily match those in the description. The microwave irradiation device 10 shown in Fig. 1(a) includes a microwave generator 1 that oscillates a single-mode microwave, a single-mode cavity 2 having a cylindrical space therein, and a reaction tube 3 that penetrates the single-mode cavity and is filled with cement clinker raw materials. Note that the microwave irradiation device may be a commercially available device, or may be manufactured according to the production scale, etc.

[0015] Examples of the microwave source in the microwave generator include magnetrons, klystrons, and solid-state semiconductor elements. Examples of the microwave generator using solid-state semiconductor elements include microwave generators using Gunn diodes, avalanche diodes (Impatt diodes), and the like. In addition, in the MHz band, an oscillator circuit using an LC circuit consisting of a coil and a capacitor can also be used. Examples of the oscillator circuit include a VCO (Voltage Controlled Oscillator) or a PLL (Phase Locked Loop) circuit that packages these elements and a frequency control mechanism. The microwave irradiation device may be equipped with a microwave amplifier that amplifies the output of the microwave oscillated by the microwave generator.

[0016] The shape of the single mode cavity is not particularly limited as long as it is cylindrical, and may be, for example, a cylindrical or elliptical shape, or a polygonal cylindrical shape in which the cross section perpendicular to the central axis of the cylinder is polygonal. That is, it is sufficient if the energy intensity of the single mode microwave is maximized and a uniform standing wave can be formed along the axis of the single mode cavity (for example, the central axis of the cylinder in the case of a cylindrical shape). The size of the single mode cavity can be appropriately selected depending on the manufacturing scale, etc.

[0017] The material of the single mode cavity is preferably one with low electrical resistivity, and is usually a metal. Examples include aluminum, copper, iron, magnesium, brass, stainless steel, and alloys thereof. In addition, the surface of a resin, ceramic, or metal may be coated with a substance with low electrical resistivity by plating, vapor deposition, or the like. Materials containing silver, copper, gold, tin, or rhodium can be used for the coating.

[0018] The reaction tube is not particularly limited as long as it is a bottomed tubular body, and may be, for example, a bottomed circular cylindrical body or a bottomed rectangular prism. The inner diameter of the reaction tube can be appropriately selected depending on the production scale, microwave frequency, etc., but for example, when a cylindrical reaction tube with a bottom is used for irradiation with microwaves in the 2.45 GHz frequency band, the inner diameter is preferably 25 mm or less, and more preferably 5 to 15 mm. The material of the reaction tube is not particularly limited as long as it has low microwave loss and high heat resistance, and examples of the material include glass, quartz, and polytetrafluoroethylene.

[0019] The cement clinker raw materials are filled inside the reaction tube where the energy intensity of the single mode microwave is maximum and uniform. For example, FIG. 1(b) shows an example of a method for filling the cement clinker raw materials at a position in the axial direction of the single mode cavity where the energy intensity of the single mode microwave is maximum and uniform. That is, a quartz rod 4 is installed at the bottom of the reaction tube 3 to raise the height, and the cement clinker raw materials 5 are placed on the top of the quartz rod 4. After that, the quartz rod 4 is further placed on the top to prevent the cement clinker raw materials from moving and pressurized, and the filling position of the cement clinker raw materials is adjusted.

[0020] <Process (B)> This process involves irradiating the raw cement clinker with single-mode microwaves to burn it and obtain a burned product. By irradiating the raw cement clinker with single-mode microwaves, it is possible to directly heat only the raw cement clinker, so that the raw cement clinker can be burned sufficiently without being left in an under-burned state.

[0021] Examples of microwave frequencies include the 2.45 GHz band, the 5.8 GHz band, and the 915 MHz band, but other frequency bands can also be used as appropriate.

[0022] The microwaves oscillated from the microwave generator into the single mode cavity form a single mode standing wave. The standing wave is not particularly limited, but for example, TM 0n0 Mode (n is an integer equal to or greater than 1), TE mn0 Among them, TM0n0 Mode (n is as defined above) is preferred, and TM 010 TM mode is more preferable. 010 The standing wave of the single mode has an advantage that the electric field strength is maximized along the axis of the single mode cavity (for example, the central axis of the cylinder in the case of a cylindrical type), making it easy to determine the installation position of the object to be processed. Whether or not a standing wave is formed can be determined based on a signal from an electric field monitor. If a standing wave is not formed, feedback control may be performed to form a standing wave by changing the frequency of the microwaves oscillated from the microwave generator or by adjusting the inner diameter of the cavity.

[0023] Single mode cavities are classified into a transmission line type and a resonator type, with the resonator type being preferred since it can provide a higher energy density. In this case, the Q value in the single mode is preferably 500 or more, more preferably 1000 or more, from the viewpoint of selectively and intensively heating the cement clinker raw material. Here, in this specification, the "Q value" refers to the ratio of the resonance frequency to the half-width, and the higher the Q value, the smaller the loss and the higher the energy amplification efficiency.

[0024] Microwave irradiation may be performed so that the free lime (hereinafter also referred to as "f.CaO") content in the cement clinker is 1 mass% or less. Here, in this specification, the "free lime content" is measured in accordance with the "Cement Association Standard Test Method JCAS I-01-1997 (Quantitative Method for Free Calcium Oxide A)". For example, the cement clinker raw material can be burned at a temperature of 1000°C or higher for preferably 1 to 5 minutes, more preferably 1 to 4 minutes, and even more preferably 1 to 3 minutes by irradiating with microwaves each time. The temperature at the time of microwave irradiation is preferably not higher than 2000°C, and more preferably not higher than 1700°C. The holding time at such a temperature is preferably within 30 seconds, and more preferably within 20 seconds. The temperature can be measured by a thermometer, a thermocouple, or a thermograph inserted in the reaction tube. The output of the microwave generator can be appropriately selected so as to achieve the above-mentioned irradiation conditions.

[0025] Microwave irradiation may be performed multiple times. When microwave irradiation is performed multiple times, it is preferable to irradiate the cement clinker raw materials with microwaves once, perform step (C) described below, and then perform step (d) from the viewpoint of efficiently producing cement clinker in a short time while preventing the cement clinker raw materials from being under-burned.

[0026] <Process (C)> This step is a step of pulverizing the burned material to obtain a pulverized material, thereby producing cement clinker. The fired product can be pulverized using, for example, a mortar or an industrial pulverizer. Specific examples of the pulverizer include those mentioned above. Grinding can also be performed using an industrial grinding machine using a diamond grinding wheel or the like. The pulverization time is set to 2000 to 4000 (cm2) when the Blaine specific surface area of ​​the pulverized product is measured in accordance with JIS R 5201 (Physical Testing Methods for Cement). 2 / g) as a guideline.

[0027] <Process (d)> This step is a step in which the content of f.CaO in the pulverized material obtained in step (c) is analyzed, and if the content of f.CaO exceeds 1 mass%, the pulverized material obtained in step (c) is sequentially subjected to steps (a) to (c). If the firing in step (b) is insufficient, the cement clinker will be in an unburned state, the content of alite will be low, and the content of f.CaO in the cement clinker will be high, resulting in insufficient early strength development and reduced cement quality. Therefore, this step is performed to obtain cement clinker rich in alite and with a content of f.CaO reduced to 1 mass% or less.

[0028] In this step, the pulverized material obtained in step (c) is filled into the reaction tube of a microwave irradiation device, irradiated with single-mode microwaves to obtain a fired material, and the fired material is pulverized. After pulverization, the f.CaO content of the pulverized material is analyzed to confirm whether the f.CaO content of the pulverized material is 1% by mass or less. If the f.CaO content exceeds 1% by mass, steps (a) to (c) are repeated until the f.CaO content of the pulverized material obtained in step (c) is 1% by mass or less. In this way, this step can be carried out once or twice or more times until the f.CaO content of the pulverized material obtained in step (c) is 1% by mass or less. The method of filling the pulverized material into the reaction tube, the microwave irradiation, and the operation of pulverizing the fired material in this step are as described above.

[0029] In this way, cement clinker can be produced. The cement clinker produced by the method of the present invention can be used for a variety of purposes depending on its mineral phase, etc., but is preferably used as Portland cement clinker. The Portland cement clinker is not particularly limited, but examples thereof include ordinary Portland cement clinker, high-early-strength Portland cement clinker, moderate-heat Portland cement clinker, and low-heat Portland cement clinker. Among these, ordinary Portland cement clinker and low-heat Portland cement clinker are preferred.

[0030] The mineral phase of the cement clinker preferably contains one or more minerals selected from alite (3CaO·SiO2: also referred to as "C3S"), belite (2CaO·SiO2: also referred to as "C2S"), aluminate (3CaO·Al2O3: also referred to as "C3A"), and ferrite (4CaO·Al2O3·Fe2O3: also referred to as "C4AF"), and more preferably contains at least alite and belite. The mineral phase contained in the cement clinker can be identified by performing Rietveld analysis using a powder X-ray diffraction (XRD) device and carrying out XRD measurement.

[0031] The cement clinker produced by the present invention is rich in belite, but has a reduced f.CaO content. It is known that when the burning temperature of the cement clinker raw materials is set low, the burning reaction of the cement clinker raw materials is slow, so the belite content is high and the residual f.CaO content is also likely to be high, while when the burning temperature is set high, the burning reaction of the cement clinker raw materials is accelerated, so the belite content in the cement clinker is low and the residual f.CaO content is also low. In other words, since an increase in belite and a decrease in f.CaO are contradictory characteristics, it has been difficult to increase the amount of belite while decreasing the amount of f.CaO in the past. However, the present inventors have unexpectedly found that a cement clinker rich in belite and with a reduced f.CaO content can be produced by irradiating and burning the cement clinker raw materials with single-mode microwaves. Specifically, for example, in the case of ordinary Portland cement clinker, the belite content is usually 20 mass% or more, preferably 21 mass% or more, and the f.CaO content can be 1 mass% or less, preferably 0.7 mass% or less. Also, in the case of low-heat Portland cement clinker, the belite content can be usually 60 mass% or more, preferably 63 mass% or more, and the f.CaO content can be usually 0.7 mass% or less, preferably 0.3 mass% or less. EXAMPLES

[0032] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0033] 1. Analysis of the chemical composition of cement clinker X-ray fluorescence analysis (calibration curve method) was performed using an X-ray fluorescence analyzer (ZSX primus II, Rigaku Corporation) to determine the contents of SiO2, Al2O3, Fe2O3, CaO, MgO, SO3, Na2O, K2O, TiO2, and other trace elements.

[0034] 2. Analysis of mineral phases in cement clinker Powder X-ray diffraction (XRD) measurements were performed using a Bruker AXS D8-Advance A-25 model, and Rietveld analysis was performed. The content of each mineral phase was calculated by fitting the theoretical profile of the minerals identified from the XRD pattern to the measured profile obtained from the powder XRD results.

[0035] Powder XRD measurement conditions ·X-ray used: CuKα Tube conditions: Tube voltage 40kV - Tube current 40mA Scanning range: 5~65° Step width: 0.023° / step Measurement time: 0.13 seconds / step Rietveld analysis software: TOPAS Version 5.0 (Bruker AXS)

[0036] 3. Analysis of free CaO (f.CaO) Measurements were made in accordance with the Cement Association Standard Test Method JCAS I-01-1997 (Quantitative Method for Free Calcium Oxide, Method A).

[0037] Example 1 To obtain cement clinker (OPC clinker) with the chemical composition shown in Table 1, each raw material reagent was placed in a plastic bag, mixed in the bag, and then mixed and ground for 60 seconds using a vibrating disk mill to prepare cement clinker raw material. Calcium carbonate reagent was used as the calcium source, and other reagents were oxides or carbonates. <Process (a)> In this process, a single-mode (cavity resonator) microwave irradiation device having the same configuration as that shown in Fig. 1(a) was used, and 0.5 g of cement clinker raw materials was filled into a cylindrical quartz reaction tube (inner diameter φ10 mm) with a bottom of this microwave irradiation device by the following method. That is, as shown in Fig. 1(b), a quartz rod was placed at the bottom of the reaction tube to raise it so that the cement clinker raw materials could be filled at a position where the energy intensity of the single-mode microwaves is maximum and uniform, and then the cement clinker raw materials were packed on the top surface of the quartz rod, and the quartz rod was placed on the top surface of the cement clinker raw materials to press them down. <Process (b)> Next, the cement clinker raw material in the reaction tube was irradiated with microwaves from a microwave generator and fired. The microwave irradiation conditions were a frequency of 2.45 GHz, 70 to 90 W, and a holding time of 2 minutes at 1000°C or higher. The temperature at this time was monitored by thermography. The maximum temperature during firing was 1700°C, and the holding time at this temperature was 15 seconds out of the above 2 minutes. The standing wave was TM 010 It is a single mode. <Process (c)> The calcined product was removed from the reaction tube, cooled, and then crushed in a mortar. The crushed product was subjected to wet titration analysis to determine the end point of the calcination. The content of f.CaO in the crushed product was 9% by mass, which exceeded 1% by mass, so the next step (d) was performed. <Process (d)> The pulverized material obtained in step (c) was filled into the reaction tube of a microwave irradiation device by the same operation as in step (a), irradiated with microwaves under the same conditions as in step (b) to be fired, and the fired material was pulverized by the same operation as in step (C) to obtain a pulverized material. When the pulverized material was subjected to wet titration analysis, it was found that the f.CaO content exceeded 1 mass%, so steps (a) to (C) were repeated to obtain a pulverized material. When the pulverized material was subjected to wet titration analysis, it was confirmed that the f.CaO content was 1 mass% or less. This pulverized material was collected as ordinary Portland cement clinker (OPC clinker). The mineral phase of the obtained ordinary Portland cement clinker (OPC clinker) was analyzed, and the results are shown in Table 2.

[0038] Example 2 A cement clinker raw material was prepared in the same manner as in Example 1, except that the CaO source was replaced with Ca(OH)2, the Al2O3 source was replaced with blast furnace slag, and CaF2 (1000 ppm CaF2 per 100 g of the mixed raw material) and CaSO4 (1 mass % CaSO4 per 100 g of the mixed raw material) were added as mineralizers, so as to obtain a cement clinker (OPC+clinker) having the chemical composition shown in Table 1. Next, this cement clinker raw material was subjected to steps (a) to (d) in the same manner as in Example 1 to obtain a pulverized product, which was then recovered as ordinary Portland cement clinker (OPC+clinker). The mineral phases of the resulting ordinary Portland cement clinker (OPC+clinker) were analyzed, and the results are shown in Table 2.

[0039] Example 3 A cement clinker raw material was prepared by the same operation as in Example 1 so as to obtain a cement clinker (LPC clinker) having the chemical composition shown in Table 1. Next, this cement clinker raw material was subjected to steps (a) to (d) by the same operation as in Example 1 to obtain a pulverized product, which was then recovered as low-heat Portland cement clinker (LPC clinker). The mineral phase of the obtained low-heat Portland cement clinker (LPC clinker) was analyzed, and the results are shown in Table 2.

[0040] Comparative Example 1 The cement clinker raw material prepared in Example 1 was placed in an electric furnace heated to an internal temperature of 1000° C. and fired at 1000° C. for 30 minutes, then heated to 1500° C. and fired at 1500° C. for 30 minutes. The fired product was removed from the electric furnace, cooled, coarsely crushed to 5 mm or less, and crushed in a disk mill for 150 seconds. The crushed material was collected as ordinary Portland cement clinker (OPC clinker) and the mineral phases were analyzed, the results of which are shown in Table 2.

[0041] Comparative Example 2 The cement clinker raw material prepared in Example 2 was placed in an electric furnace heated to an internal temperature of 1000°C, burned at 1000°C for 30 minutes, and then heated to 1400°C and burned at 1400°C for 30 minutes. A pulverized material was obtained in the same manner as in Comparative Example 1, except that the raw material was fired at 1400°C for 30 minutes. The ground material was collected as ordinary Portland cement clinker (OPC+clinker) and the mineral phases were analysed, the results of which are shown in Table 2.

[0042] Comparative Example 3 The cement clinker raw material prepared in Example 3 was placed in an electric furnace heated to an internal temperature of 1000°C, burned at 1000°C for 30 minutes, and then heated to 1450°C and burned at 1450°C for 30 minutes. A pulverized material was obtained in the same manner as in Comparative Example 1, except that the raw material was fired at 1450°C for 30 minutes. The ground material was collected as low-heat Portland cement clinker (LPC clinker) and the mineral phases were analyzed, the results of which are shown in Table 2.

[0043] [Table 1]

[0044] [Table 2]

[0045] Test Example Gypsum dihydrate was added to the cement clinker obtained in each Example and Comparative Example so that the SO3 content was 2.0 mass%, to produce cement. Note that the ordinary Portland cement clinker (OPC + clinker) obtained in Example 2 and Comparative Example 2 already had an SO3 content exceeding 2 mass%, so gypsum dihydrate with an SO3 content of 1.2 mass% was added. The guideline for grinding was to grind the clinker to a Blaine specific surface area of ​​3200 ± 100 (cm2) according to JIS R 5201 (Physical Testing Methods for Cement). 2 / g). Next, for each cement, cement and water were mixed at W / C=0.5 to prepare a cement paste, and the calorific value was measured. The calorific value was measured using an isothermal calorimeter (TA Air, manufactured by TA Instruments) and the integrated calorific value over 7 days (168 h) was measured. The results are shown in Figure 2 (a) to (c).

[0046] From the results in Figure 2, it was confirmed that the cement produced from the cement clinker obtained in the embodiment exhibited the same hydration reaction as the cement produced from the cement clinker obtained in the comparative example (a manufacturing method using a conventional furnace). It was also found that there was no difference in the time series changes in the integrated calorific value between the two. [Explanation of symbols]

[0047] 1 Microwave Generator 2 Single mode cavity 3 Reaction tube 4 quartz rod 5. Cement clinker raw materials 10 Microwave irradiation device

Claims

1. The following steps (a) to (c); (a) charging cement clinker raw material into a reaction tube of a microwave irradiation device; (b) irradiating the cement clinker raw material with single-mode microwaves to burn it and obtain a burned product; (c) A step of pulverizing the fired product to obtain a pulverized product. A method for producing cement clinker, comprising:

2. The method for producing cement clinker according to claim 1, further comprising a step (d) of subjecting the pulverized product to steps (a) to (c) in sequence after step (c).

3. 2. The method for producing cement clinker according to claim 1, wherein step (d) is carried out once or twice or more.

4. 2. The method for producing cement clinker according to claim 1, wherein the mixture is calcined at a temperature of 1000° C. or higher for 1 to 5 minutes per microwave irradiation.

Citation Information

Patent Citations

  • Process for producing cement clinker

    JP2007169161A