Deposition apparatus for metallic film

The film forming apparatus addresses the issue of gas bubbles obstructing electricity flow by using a convexly curved anode with through holes and vibration, ensuring uniform metal film deposition.

JP2024153365AActive Publication Date: 2024-10-29TOYOTA JIDOSHA KK
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023067220
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

Existing film forming apparatuses using insoluble anodes generate oxygen gas bubbles that adhere to the anode surface, obstructing the flow of electricity and preventing the stable formation of a uniform metal film.

Method used

A film forming apparatus with an anode featuring convexly curved surfaces and through holes, combined with a vibration mechanism, to facilitate the movement of gas bubbles away from the anode surface, ensuring uniform metal film deposition.

Benefits of technology

The apparatus stabilizes the formation of a metal film with uniform thickness by effectively managing gas bubbles, allowing for consistent metal film thickness across the base material surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153365000001_ABST
    Figure 2024153365000001_ABST
Patent Text Reader

Abstract

To provide a deposition apparatus for a metallic film that can stably deposit a metallic film with a uniform thickness.SOLUTION: A deposition apparatus 1 is an apparatus for depositing a metallic film F on a surface of a base material B. The deposition apparatus 1 comprises: a storage body 15 containing a plating solution L; a polymer electrolyte 13 covering an opening 15d of the storage body 15 formed in a position facing the base material B; an anode 11 arranged above the polymer electrolyte 13 within the storage body 15; and a power supply 14 that applies a voltage between the anode 11 and the substrate B. On an opposite surface 11f opposite to the polymer electrolyte 13 in a surface of the anode 11, there are a plurality of curved surfaces 11a that are curved convexly toward the polymer electrolyte 13. Between the plurality of curved surfaces 11a, there is an open hole 11b that penetrates the anode 11.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film forming apparatus for forming a metal film on a surface of a substrate. [Background technology]

[0002] For example, as this type of technology, Patent Document 1 proposes a film forming apparatus including an anode, a housing that contains a plating solution so that the plating solution contacts the anode, an electrolyte membrane that seals the plating solution in the housing, and a power source that applies a voltage between the anode and the substrate. The anode is an anode that is insoluble in the plating solution. When forming a metal film, a voltage is applied between the anode and the substrate in a state where the substrate is in contact with the electrolyte membrane, so that metal ions contained in the plating solution pass through the electrolyte membrane and are precipitated on the surface of the substrate. As a result, a metal film is formed on the surface of the substrate. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-152987 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, as shown in Patent Document 1, when an insoluble anode is used, oxygen gas is generated on the surface of the anode due to electrolysis of water contained in the plating solution. If oxygen gas generation continues, oxygen gas bubbles will adhere to the surface of the anode, and the attached bubbles will obstruct the flow of electricity from the anode to the substrate. As a result, it is expected that a metal coating with a uniform thickness cannot be stably formed.

[0005] The present invention has been made in consideration of such problems, and an object of the present invention is to provide a metal film forming apparatus that can stably form a metal film with a uniform thickness. [Means for solving the problem]

[0006] In view of the above problems, the present invention provides a metal coating deposition apparatus that deposits a metal coating on a surface of a substrate. The deposition apparatus includes a container that contains a plating solution, an electrolyte membrane that covers an opening of the container that is formed in a position facing the substrate, an anode that is insoluble in the plating solution and is disposed above the electrolyte membrane within the container, and a power source that applies a voltage between the anode and the substrate. A surface of the anode that faces the electrolyte membrane has a plurality of curved surfaces that are convexly curved toward the electrolyte membrane. Between the curved surfaces, a through hole penetrating the anode is formed.

[0007] According to the film forming apparatus of the present invention, a voltage is applied between the anode and the substrate by a power source while the electrolyte membrane is in contact with the substrate surface. As a result, metal ions contained in the plating solution contained in the container pass through the electrolyte membrane and are reduced on the substrate surface to deposit as metal. As a result, a metal film is formed on the substrate surface.

[0008] On the other hand, since the anode is an anode that is insoluble in the plating solution, the solvent of the plating solution is electrolyzed and gas is generated. The generated gas grows into bubbles while adhering to the surface of the anode. Since the surface of the anode facing the electrolyte membrane has a plurality of curved surfaces that are convexly curved toward the electrolyte membrane, the bubbles adhering to the curved surfaces move from the top of the curved surfaces toward the bottom (side surface) of the curved surfaces due to buoyancy in the plating solution. The migrated bubbles pass through the through holes formed between the curved surfaces. As a result, the attached bubbles are prevented from blocking the flow of electricity from the anode toward the substrate, and a metal coating with a uniform thickness can be stably formed.

[0009] The shape of the convexly curved surface formed on the anode is not particularly limited, and may be a rounded curved surface, as long as the bubbles generated during film formation can be moved along the curved surface. In a more preferred embodiment, the curved surface is a part of a sphere. During film formation, the electric field is likely to concentrate at the top of the curved surface of the anode, and bubbles are likely to be generated. As the bubbles grow, the bubbles generated on the surface of the top of each curved surface tend to move along the curved surface toward the bottom (side surface) of the curved surface due to buoyancy in the plating solution. As the bubbles move toward the bottom of the curved surface, the gradient of the spherical curved surface becomes larger, so that the bubbles that move from the top tend to move to the through-holes.

[0010] In a more preferred embodiment, the apex region of the curved surface is a surface that has been subjected to a water-repellent treatment. During film formation, the apex of the curved surface of the anode is prone to electrolysis and bubbles are likely to be generated. However, according to this embodiment, since the apex region has a water-repellent surface, it is difficult for fine bubbles to adhere uniformly to the apex region, and the generated bubbles tend to aggregate and grow. As a result, the grown bubbles tend to move from the state where they are attached to the apex region (surface) of the curved surface toward the bottom (side surface) of the curved surface due to buoyancy in the plating solution. As a result, the bubbles that have moved from the apex tend to move to the through-holes.

[0011] In a more preferred embodiment, the film forming apparatus includes a vibration device that vibrates the anode. According to this embodiment, by vibrating the anode, air bubbles attached to the anode can be easily moved along the surface of the anode.

[0012] In a more preferred embodiment, the vibration device vibrates the anode along the horizontal direction, and vibrates the anode with an amplitude equal to or greater than the hole width of the through hole along the horizontal direction in which the anode vibrates.

[0013] According to this embodiment, since the anode is vibrated with an amplitude equal to or greater than the width of the through hole, the position of the through hole can be moved to a different position with respect to the surface of the substrate, thereby forming a metal coating with a more uniform thickness on the surface of the substrate. Effect of the Invention

[0014] According to the present invention, a metal film having a uniform thickness can be stably formed. [Brief description of the drawings]

[0015] [Figure 1] 1 is a schematic cross-sectional view for explaining a metal film forming apparatus according to an embodiment of the present invention. [Figure 2A] FIG. 2 is a schematic perspective view of an anode of the film forming apparatus shown in FIG. [Figure 2B] FIG. 2B is a plan view of the anode shown in FIG. 2A. [Figure 2C] FIG. 2C is a partially enlarged cross-sectional view of the anode taken along line AA shown in FIG. 2B. [Figure 2D] FIG. 2D is a diagram for explaining the range of vibration of the anode shown in FIG. 2C. [Diagram 3] 2 is a schematic cross-sectional view for explaining a state during film formation of the film forming apparatus shown in FIG. 1. FIG. [Figure 4] FIG. 2D is a diagram for explaining the movement of gas (bubbles) attached to the anode shown in FIG. 2C. [Diagram 5] FIG. 1 is a diagram showing the results of the contact angle of water in Reference Examples 1 to 3, and an image of the growth and movement of bubbles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] First, a description will be given of a metal coating deposition apparatus 1 according to an embodiment of the present invention. Fig. 1 is a schematic cross-sectional view showing an example of a metal coating deposition apparatus according to an embodiment of the present invention.

[0017] 1. About the deposition device 1 1, the film formation apparatus 1 is an apparatus that forms a metal film F on the substrate B by electrolytic plating in a state in which an electrolyte membrane 13 is disposed between an anode 11 and the substrate B. Specifically, the film formation apparatus 1 includes the anode 11, the electrolyte membrane 13, and a power source 14 that applies a voltage between the anode 11 and the substrate B.

[0018] The film forming apparatus 1 further includes a mounting table 40 on which the substrate B is placed, a container 15 that contains the plating solution L, and a pair of linear actuators 70 that raise and lower the container 15. The linear actuator 70 has a rod 72 that moves linearly with respect to a main body 71, and the container 15 is fixed to the tip of the rod 72. In this embodiment, the anode 11 is disposed above the electrolyte membrane 13, and the mounting table 40 (i.e., the substrate B) is disposed below the electrolyte membrane 13.

[0019] The substrate B functions as a cathode. The substrate B is a plate-shaped substrate. In this embodiment, the substrate B is a rectangular substrate. The surface of the substrate B facing the electrolyte membrane 13 is a surface on which a film is formed and functions as a cathode. The material of the substrate B is not particularly limited as long as it functions as a cathode (i.e., a surface having electrical conductivity). The substrate B may be made of a metal material such as aluminum or copper. When forming a wiring pattern from the metal coating F, the substrate B is a substrate in which a base layer such as copper is formed on the surface of an insulating substrate such as resin. In this case, after the metal coating F is formed, the base layer other than the portion on which the metal coating F is formed is removed by etching or the like. This allows a wiring pattern to be formed by the metal coating F on the surface of the insulating substrate.

[0020] The plating solution L is a solution containing the metal of the metal film to be formed in an ionic state. Examples of the metal include copper, nickel, gold, and silver. The plating solution L is a solution in which these metals are dissolved (ionized) with an acid such as nitric acid, phosphoric acid, succinic acid, sulfuric acid, sulfamic acid, and pyrophosphoric acid. Water is used as the solvent for the solution, but the solvent may be alcohol or the like as long as the metal can be contained in an ionic state. For example, when the metal is copper, the plating solution L may be an aqueous solution containing copper sulfate, copper pyrophosphate, or the like.

[0021] The electrolyte membrane 13 is a membrane that can be impregnated (contained) with metal ions together with the plating solution L by contacting the electrolyte membrane 13 with the plating solution L. The electrolyte membrane 13 is a flexible membrane. The material of the electrolyte membrane 13 is not particularly limited as long as the metal ions of the plating solution L can migrate to the substrate B side when a voltage is applied from the power source 14. Examples of the material of the electrolyte membrane 13 include resins having an ion exchange function, such as fluororesins such as Nafion (registered trademark) manufactured by DuPont. The thickness of the electrolyte membrane 13 is preferably in the range of 5 μm to 200 μm. More preferably, the thickness is in the range of 20 μm to 60 μm.

[0022] The container 15 is made of a material insoluble in the plating solution L. The container 15 has a container space 15a for containing the plating solution L. A flat anode 11 is disposed in the container space 15a of the container 15. An opening 15d is formed on the substrate B side (lower side) of the container space 15a. The electrolyte membrane 13 is attached to the lower part of the container 15 by sandwiching the periphery of the electrolyte membrane 13 between the frame 17 and the container 15. This allows the electrolyte membrane 13 to cover the opening 15d of the container 15, and the plating solution L contained in the container space 15a of the container 15 to be sealed by the electrolyte membrane 13.

[0023] The linear actuator 70 moves the rod 72 linearly in the vertical direction relative to the main body 71, thereby raising and lowering the housing 15 so that the electrolyte membrane 13 and the substrate B can be brought into contact with and separated from each other. In this embodiment, the mounting table 40 is fixed and the housing 15 is raised and lowered, but the housing 15 may be fixed and the mounting table 40 may be raised and lowered. The linear actuator 70 is an electric actuator, and converts the rotational motion of a motor into linear motion by a ball screw or the like (not shown). However, instead of the electric actuator, a hydraulic or pneumatic actuator may be used.

[0024] The mounting table 40 includes a conductive material, and may have a recess formed therein for accommodating the substrate B. The mounting table 40 and the substrate B are electrically connected to each other, and the negative electrode of the power source 14 is connected to the mounting table 40.

[0025] The container 15 has a supply port 15b for supplying the plating solution L to the container space 15a. The container 15 has a discharge port 15c for discharging the plating solution L from the container space 15a. The supply port 15b and the discharge port 15c are holes communicating with the container space 15a. The supply port 15b and the discharge port 15c are formed on either side of the anode 11 of the container space 15a. The supply port 15b is connected to a supply path 51. The discharge port 15c is connected to a discharge path 52.

[0026] In this embodiment, the supply port 15b is formed at a position where the plating solution L flows onto the opposing surface 11f of the anode 11, and the discharge port 15c is formed at a position higher than the anode 11. As a result, as described later, air bubbles generated on the opposing surface 11f of the anode 11 are caused to flow by the plating solution L and move toward the through-holes 11b of the anode 11, which will be described later. The air bubbles that reach the through-holes 11b pass through the through-holes 11b due to the buoyancy of the plating solution L, and can flow from the upper surface (rear surface) side of the anode 11 to the discharge port 15c.

[0027] The film forming apparatus 1 further includes a tank 90, a pump 80, and a pressure regulating valve 54. As shown in FIG. 1, the tank 90 contains a plating solution L. The supply path 51 connects the tank 90 and the accommodation body 15. The supply path 51 is provided with a pump 80. The pump 80 supplies the plating solution L from the tank 90 to the accommodation body 15. The discharge path 52 connects the tank 90 and the accommodation body 15. The discharge path 52 is provided with a pressure regulating valve 54. The pressure regulating valve 54 regulates the pressure (liquid pressure) of the plating solution L in the accommodation space 15a to a predetermined pressure.

[0028] In this embodiment, the plating solution L is sucked from the tank 90 into the supply path 51 by driving the pump 80. The sucked plating solution L is pressure-fed from the supply port 15b to the accommodation space 15a. The plating solution L in the accommodation space 15a is returned to the tank 90 through the discharge port 15c. In this manner, the plating solution L contained in the accommodation body 15 can be circulated outside the accommodation body 15. The liquid pressure of the plating solution L in the accommodation body 15 is adjusted by the pressure regulating valve 54.

[0029] The anode 11 is attached in the accommodation space 15a of the accommodation body 15 via a vibration device 60. As shown in Fig. 3, during film formation described below, the anode 11 is accommodated in a state of being immersed in the accommodation space 15a, and a through hole 11b formed in the anode 11 described below is filled with a plating solution L. The anode 11 is electrically connected to the positive electrode of a power source 14. The negative electrode of the power source 14 is electrically connected to the substrate B via a mounting table 40.

[0030] In this embodiment, the anode 11 is an anode that is insoluble in the plating solution L. Therefore, even if a voltage from a power source 14 is applied between the anode 11 and the substrate B, the anode 11 does not dissolve. Examples of the material of the anode include titanium, a titanium alloy, and platinum. For example, when the material of the anode is titanium or a titanium alloy, the surface of the anode may be coated with iridium oxide or platinum. By carrying out such a coating, the reduction reaction of water is promoted, and metal is easily deposited on the surface of the substrate B.

[0031] In this embodiment, among the surfaces of the anode 11, a plurality of curved surfaces 11a curved in a convex shape toward the electrolyte membrane 13 are arranged on the surface facing the electrolyte membrane 13. As shown in Fig. 2A, the plurality of curved surfaces 11a, 11a, ... are arranged along two orthogonal directions on a horizontal plane, and in this embodiment, the plurality of curved surfaces 11a, 11a, ... are arranged, for example, in four rows in the short side direction and eight rows in the long side direction orthogonal to the short side direction. In this embodiment, through holes 11b penetrating the anode 11 are formed between the plurality of curved surfaces 11a, 11a.

[0032] Here, the shape of the curved surface 11a is not particularly limited as long as the oxygen gas bubbles attached to the surface can be moved to the through-hole 11b by the buoyancy of the plating solution L or the like by curving each curved surface 11a in a convex shape. In this embodiment, the curved surface 11a is a part of a spherical surface, specifically, a hemispherical curved surface. For example, the curved surface may be a part of the circumferential surface of a cylinder, the opposing surface of the anode may be a surface in which parts of the circumferential surface of the cylinder are arranged in one direction, and a slit-shaped through-hole may be formed between them.

[0033] 2A to 2C, the top region 11c of the curved surface 11a may be a surface that is more water repellent (hydrophobic) than other surfaces of the anode 11. In this embodiment, the top region 11c is a spherical surface region of the curved surface 11a, the center of which is an apex that protrudes toward the electrolyte membrane 13. As shown in FIG. 2B, in a plan view of the anode 11, the top region 11c may have a diameter that is, for example, in the range of 50% to 70% of the diameter of the curved surface 11a.

[0034] Specifically, the top region 11c (metal surface) is subjected to a water-repellent treatment. The water-repellent treatment may be a treatment to impart water-repellency to the metal surface by exposing it to plasma or irradiating it with a laser in an environment of a reactive gas derived from a water-repellent functional group. For example, examples of the water-repellent functional group include an alkyl group such as a saturated fluoroalkyl group (particularly a trifluoromethyl group), a silyl group such as an alkylsilyl group or a fluorosilyl group, or a phenyl group.

[0035] In addition, for example, a conductive film may be formed on top region 11c by interposing a conductive filler in a water-repellent resin, on the premise that the conductivity of top region 11c is ensured. For example, a film of a metal oxide (e.g., iridium oxide, ruthenium oxide, etc.) that is conductive and water-repellent may be formed on top region 11c. Furthermore, water-repellency may be imparted to top region 11c by providing a fine fractal structure having recesses and protrusions in top region 11c. For example, the contact angle of water with the surface of top region 11c of curved surface 11a is preferably 90° or more, and more preferably 100° or more.

[0036] Furthermore, a water-repellent treatment may be applied to the portion other than the top region 11c, and more preferably, a hydrophilic treatment is applied to the other region 11d of the curved surface 11a. For example, the other region 11d of the curved surface 11a may be provided with a functional group such as a hydroxyl group (-OH), a carbonyl group (-CO), or a carboxyl group (-COOH), so that the top region 11c has a hydrophilic surface. Specifically, the curved surface 11a may be masked except for the other region 11d, and the top region 11c may be exposed to plasma derived from the atmosphere or a reactive gas such as a hydrocarbon gas, thereby modifying the top region 11c to have a hydrophilic surface. In addition, a film made of a hydrophilic material may be formed by CVD or the like in a state in which the surface of the anode 11 except for the top region 11c is masked, or a film made of a hydrophilic material may be formed by a hydrophilic coating. For example, the water contact angle of the other region 11d is preferably 40° or less.

[0037] Furthermore, the film forming apparatus 1 includes a vibration device 60 that vibrates the anode 11. The vibration device 60 is not particularly limited as long as it vibrates the anode 11, and may be, for example, an ultrasonic vibration device.

[0038] In this embodiment, the vibration device 60 vibrates the anode 11 in the horizontal direction. The vibration device 60 vibrates the anode 11 with an amplitude equal to or greater than the hole width D of the through hole 11b along the horizontal direction in which the anode 11 vibrates. The vibration device 60 includes a main body 61 attached to the container 15, and a mover 62 attached between the main body 61 and the anode 11. The main body 61 is a power source for generating vibration, and the mover 62 slides horizontally relative to the main body 61 by the power from the main body 61. The mover 62 vibrates horizontally with a predetermined amplitude by the power from the main body 61.

[0039] More specifically, the anode 11 moves from the position shown in the upper diagram of FIG. 2D to one side in the horizontal direction (left side of the diagram) by a movement distance A1 as shown in the middle diagram by the vibration of the vibration device 60. Thereafter, the anode 11 moves to the other side in the horizontal direction (right side of the diagram) by a movement distance A1+A2 to the position shown in the lower diagram. Furthermore, the anode 11 moves to one side (left side of the diagram) by a movement distance A1+A2 to the position shown in the middle diagram. In this way, the anode 11 can be vibrated with an amplitude of (A1+A2) / 2 by the vibration device 60. In this embodiment, the amplitude condition of the vibration device 60 is set so that the amplitude of the anode 11 is equal to or greater than the horizontal hole width D of the through hole 11b.

[0040] A method for forming the metal film F of this embodiment will be described below. First, as shown in FIG. 1, the substrate B is placed on the mounting table 40. Next, the housing 15 is lowered toward the mounting table 40 by the linear actuator 70. As a result, the electrolyte membrane 13 attached to the housing 15 comes into contact with the substrate B.

[0041] Next, the pump 80 is driven. As a result, the pump 80 sucks the plating solution L contained in the tank 90, and the plating solution L is pumped into the accommodation space 15a of the accommodation body 15, filling the accommodation space 15a with the plating solution L. Furthermore, the supplied plating solution L passes through the accommodation space 15a of the accommodation body 15 and is returned to the tank 90. ​​In this manner, the plating solution L in the accommodation body 15 can be circulated. Since the pressure regulating valve 54 is provided downstream of the accommodation body 15, the liquid pressure of the plating solution L in the accommodation space 15a can be adjusted to a set pressure.

[0042] Next, as shown in Fig. 3, the vibration device 60 is driven to vibrate the anode 11. While circulating the plating solution L in the container 15 and vibrating the anode 11, a voltage is applied between the anode 11 and the substrate B. As a result, metal ions in the plating solution L in the container 15 can be passed through the electrolyte membrane 13, and metal derived from the metal ions can be deposited on the surface of the substrate B. By applying the voltage for a predetermined time, a metal coating F with a predetermined thickness can be formed on the surface of the substrate B.

[0043] Here, since the anode 11 is an anode insoluble in the plating solution L, the solvent of the plating solution L is electrolyzed to generate gas. For example, when the solvent is water, oxygen gas is generated. As shown in FIG. 4, the generated gas grows into bubbles P while adhering to the opposing surface 11f of the anode 11.

[0044] In this embodiment, the opposing surface 11f of the anode 11 facing the electrolyte membrane 13 has a plurality of curved surfaces 11a arranged thereon, each curved in a convex shape toward the electrolyte membrane 13. Therefore, the air bubbles P attached to each curved surface 11a of the anode 11 move from the top of the curved surface 11a toward the bottom (side surface) of the curved surface 11a due to buoyancy in the plating solution L. The moved air bubbles P pass through the through holes 11b formed between the curved surfaces 11a. As a result, the attached air bubbles P are prevented from interfering with the flow of electricity from the anode 11 toward the substrate B, and a metal film F with a uniform thickness can be stably formed.

[0045] In particular, during film formation, the electric field is likely to concentrate at the top of the curved surface 11a of the anode 11, and bubbles P are likely to be generated. As the curved surface 11a, which is a part of a sphere, approaches the bottom of the curved surface 11a, the gradient of the curved surface 11a becomes greater, so that bubbles P that have moved from the top of the curved surface 11a tend to move to the through-holes 11b while absorbing other bubbles P. In particular, when the curved surface 11a is a hemispherical curved surface, this effect can be more effectively achieved.

[0046] Furthermore, by subjecting the top region 11c to a water-repellent treatment, the top region 11c becomes a surface having water repellency. As a result, fine air bubbles are unlikely to adhere uniformly to the top region 11c of the curved surface 11a, and the generated air bubbles P tend to aggregate and grow. As a result, the grown air bubbles P tend to move from the state where they are attached to the top region 11c of the curved surface 11a toward the bottom (side surface) of the curved surface 11a due to buoyancy in the plating solution. As a result, the air bubbles P that have moved from the top region 11c tend to move to the through-holes 11b.

[0047] Furthermore, other region 11d of curved surface 11a, excluding top region 11c, is hydrophilic, so plating solution L can easily get between other region 11d of curved surface 11a and air bubbles P. Therefore, air bubbles P attached to top region 11c of curved surface 11a can easily move toward the bottom (side surface) of curved surface 11a due to buoyancy in the plating solution.

[0048] Furthermore, in this embodiment, since the metal coating is formed while vibrating the anode 11, the air bubbles P attached to the anode 11 can be easily moved along the surface of the anode 11. In particular, since the anode 11 is vibrated with an amplitude equal to or greater than the hole width D of the through-hole 11b, the position of the through-hole 11b can be moved to a different position with respect to the surface of the substrate B. This allows the metal coating F to be formed on the substrate B with a more uniform thickness.

[0049] When the film formation is completed, the plating solution L in the container 15 is discharged, and the linear actuator 70 is driven to raise the container 15 relative to the mounting table 40. This makes it possible to separate the substrate B from the electrolyte membrane 13. Thereafter, the substrate B on which the metal film F has been formed is removed from the mounting table 40, and a new substrate B is placed on the mounting table 40, and a metal film F is formed in the same manner.

[0050] Reference Examples 1 to 3 will be described below.

[0051] (Reference Example 1) A test specimen was prepared by coating the surface of a plate-shaped titanium substrate with iridium oxide as a water-repellent material. The contact angle of water with the test specimen surface (the surface coated with the material) was measured using the sessile drop method in accordance with JIS R 3257. The results are shown in Figure 5.

[0052] (Reference Example 2) A test specimen was prepared by coating the surface of a plate-shaped titanium substrate with a fluororesin as a water-repellent material. The contact angle of water with the surface of the test specimen (the surface coated with the material) was measured in the same manner as in Reference Example 1. The results are shown in Figure 5.

[0053] (Reference example 3) A plate-shaped titanium test specimen was prepared. The contact angle of water with respect to the surface of the test specimen (the titanium surface) was measured in the same manner as in Reference Example 1. The results are shown in FIG.

[0054] As shown in Fig. 5, the contact angle of the specimen of Reference Example 1 exceeds 90° (deg), and the contact angle of the specimen of Reference Example 2 is about 110°. Therefore, it was confirmed that water repellency was imparted to the surfaces of the specimens in Reference Examples 1 and 2. On the other hand, as shown in Fig. 5, the contact angle of the specimen of Reference Example 3 is about 75°, and is not a water repellent surface.

[0055] Next, a titanium expanded metal was prepared as the substrate of the anode, and the surface of this substrate was coated with the materials shown in Reference Examples 1 and 2 to prepare the anodes of Reference Examples 1 and 2. A titanium expanded metal was prepared as the anode of Reference Example 3. A current was passed through the anodes of Reference Examples 1 to 3 in a plating solution, and the generation of bubbles was confirmed.

[0056] As a result, as shown in Fig. 5, it was confirmed that in the anode of Reference Example 2, the bubbles grew faster and were easier to remove from the surface of the anode than in Reference Example 1. Furthermore, it was found that the surface of the anode of Reference Example 3 was uniformly covered with fine bubbles and that the bubbles were harder to remove than in Reference Examples 1 and 2. As a result, it was found that the higher the water repellency of the anode surface, the more the bubbles generated during film formation grew and the more easily they moved from the anode surface.

[0057] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to the above-described embodiments, and various design modifications can be made without departing from the spirit of the present invention as described in the claims. [Explanation of symbols]

[0058] 1: film forming device, 11: anode, 11a: curved surface, 11b: through hole, 13: electrolyte membrane, 15: container, 40: mounting table, 60: vibration device, B: substrate, L: plating solution

Claims

1. A film forming apparatus for forming a metal film on a surface of a substrate, comprising: A container containing a plating solution; an electrolyte membrane that covers an opening of the container and is formed at a position facing the base material; an anode that is disposed above the electrolyte membrane in the container and is insoluble in the plating solution; a power source that applies a voltage between the anode and the substrate; a surface of the anode facing the electrolyte membrane has a plurality of curved surfaces arranged convexly toward the electrolyte membrane; A metal film forming apparatus, wherein a through hole penetrating the anode is formed between the plurality of curved surfaces.

2. The metal film forming apparatus according to claim 1 , wherein the curved surface is a part of a sphere.

3. 3. The metal coating deposition apparatus according to claim 2, wherein the top area of ​​the curved surface is a surface that has been subjected to a water-repellent treatment.

4. The metal film forming apparatus according to claim 1 , further comprising a vibration device for vibrating the anode.

5. The metal coating deposition apparatus according to claim 4, wherein the vibration device vibrates the anode along a horizontal direction with an amplitude equal to or greater than the width of the through hole along the horizontal direction in which the anode vibrates.

Citation Information

Patent Citations

  • Plating method

    JP1988057797A

  • Electrode for electroplating

    JP1989208499A

  • Electroplating device

    JP1998140391A

  • Plating device and plating method

    JP2007113082A

  • Metal film deposition apparatus and deposition method

    JP2014051701A