Display apparatus

The use of a microcrystalline semiconductor layer with a recessed buffer layer in thin film transistors addresses mobility and oxidation issues, enhancing electrical performance and manufacturing efficiency in display devices.

JP2024153903AInactive Publication Date: 2024-10-29SEMICON ENERGY LAB CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024129777
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2007-07-26
Filing Date
2024-08-06
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Thin film transistors using amorphous semiconductor films have low carrier mobility, leading to low driving ability and increased electrical capacitance, which impedes the trend toward thinner picture frames and higher power consumption, while polycrystalline semiconductor films have complex manufacturing processes with low yield and high cost, and microcrystalline semiconductor films are prone to oxidation, affecting electrical characteristics.

Method used

A thin film transistor structure using a microcrystalline semiconductor layer with a buffer layer on a gate insulating layer, featuring a recessed buffer layer design to reduce leakage current and oxidation, and a plasma CVD method for film formation without the need for additional crystallization processes.

Benefits of technology

The proposed structure enhances electrical characteristics, reduces leakage current, and improves yield and cost-effectiveness in manufacturing display devices, allowing for high mobility and reliable operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153903000001_ABST
    Figure 2024153903000001_ABST
Patent Text Reader

Abstract

To provide a display apparatus having a protection circuit formed of small-sized thin film transistors with high withstand voltage.SOLUTION: A protection circuit for a display apparatus uses a thin-film transistor in which an amorphous semiconductor layer, a microcrystalline semiconductor layer, a gate insulating layer disposed in contact with the microcrystalline semiconductor layer, and a gate electrode layer are overlapped with each other. Since the microcrystal semiconductor layer has high current drive capability, the transistor can be made smaller in size. Moreover, since the protection circuit has the amorphous semiconductor layer, its withstand voltage can be improved. The display apparatus in the present invention is a liquid crystal display apparatus or a light emitting apparatus.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a display device having a thin film transistor. Regarding the device. [Background technology]

[0002] In recent years, semiconductor thin films (thickness: several nm to several hundred nm) formed on substrates with insulating surfaces have been ) is a technology that is attracting attention for constructing thin-film transistors. Thin-film transistors are IC In particular, they are widely used in electronic devices such as liquid crystal displays. There is an urgent need to develop such devices as switching elements for image display devices.

[0003] In semiconductor elements such as thin film transistors, there is a risk of band-forming that can lead to element deterioration or dielectric breakdown. How to suppress charging is an important issue in the manufacturing process of semiconductor devices. In particular, with the trend toward higher integration, the thickness of various insulating films, such as gate insulating films, is decreasing. Therefore, insulation breakdown due to charging has become a more serious problem.

[0004] The causes and circumstances in which charging occurs are extremely complex and diverse. In addition to investigating the cause and environment of aging, In addition, we have devised ways to improve resistance to deterioration or insulation breakdown caused by charging. In order to prevent deterioration or breakdown due to charging, a diode (protection diode) is required. It is effective to secure a discharge path by using a protection circuit composed of a diode. By ensuring a discharge path, the charge accumulated in the insulating film is discharged near the semiconductor element. This prevents the semiconductor elements from being deteriorated or destroyed by the energy of the discharge. This prevents electrostatic discharge (ESD) that can occur when Cut.

[0005] In addition, by providing a protection circuit, even if noise is input together with the signal and power supply voltage, However, it is possible to prevent malfunction of the circuit due to the noise, and deterioration of the semiconductor element due to the noise is also prevented. Or destruction can be prevented.

[0006] In image display devices such as liquid crystal display devices, amorphous semiconductor films are mainly used as switching elements. A thin film transistor using a polycrystalline semiconductor film or a thin film transistor using a polycrystalline semiconductor film is used. do.

[0007] As a method for forming a polycrystalline semiconductor film, a pulsed excimer laser beam is irradiated by an optical system. The amorphous semiconductor film is processed into a linear shape, and then irradiated with a linear beam while scanning it to crystallize it. The technology is known.

[0008] In addition, thin-film transistors using amorphous semiconductor films are used as switching elements for image display devices. In addition to thin film transistors using stannous or polycrystalline semiconductor films, thin film transistors using microcrystalline semiconductor films 2. Description of the Related Art Transistors are known (see, for example, Patent Documents 1 to 4).

[0009] As a method for manufacturing a thin film transistor using a microcrystalline semiconductor film, A silicon film is formed, a metal film is formed on the amorphous silicon film, and a diode lens is formed on the metal film. A technology has been developed to convert an amorphous silicon film into a microcrystalline silicon film by irradiating the film with a laser. According to this manufacturing method, the metal film formed on the amorphous silicon film is a diode. It only serves to convert the light energy of the laser into heat energy, and is removed in the subsequent process. In other words, the amorphous silicon film was heated only by conductive heating from the metal film. This heat causes a microcrystalline silicon film to be formed (see, for example, Non-Patent Document 1). [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Japanese Patent Application Publication No. 4-242724 [Patent Document 2] JP 2005-49832 A [Patent Document 3] U.S. Patent No. 4,409,134 [Patent Document 4] U.S. Patent No. 5,591,987 [Non-patent literature]

[0011] [Non-Patent Document 1] Toshiaki Arai et al., SID '07 DIGEST, 2007, pp.1370-1373 Summary of the Invention [Problem to be solved by the invention]

[0012] In a thin film transistor using an amorphous semiconductor film, the mobility of carriers is low. Therefore, a protection circuit is made of a thin film transistor using an amorphous semiconductor film. When forming a large transistor, it is necessary to form a large transistor in order to provide sufficient electrostatic discharge protection. This has the problem that it is necessary to make the size of the display smaller, which hinders the creation of a narrower frame. By forming a transistor, a scanning line electrically connected to the gate electrode and a source electrode or drain electrode are formed. The electrical capacitance between the signal line electrically connected to the drain electrode increases, resulting in increased power consumption. There is also the problem of an increase in

[0013] A thin film transistor using a polycrystalline semiconductor film is a thin film transistor using an amorphous semiconductor film. Its mobility is two orders of magnitude higher than that of other semiconductors, and it is possible to integrate the pixel section of a liquid crystal display and its surrounding driving circuits on the same substrate. However, a thin film transistor using a polycrystalline semiconductor film can be formed on an amorphous substrate. Compared to thin-film transistors using semiconductor films, the manufacturing process is more complicated due to the crystallization of the semiconductor film. This results in low yields and high costs.

[0014] On the other hand, there is a problem that the surfaces of the crystal grains in the microcrystalline semiconductor film are easily oxidized. The crystal grains in the channel formation region are easily oxidized during the manufacturing process of the thin film transistor, and the crystal grains An oxide film is formed on the surface of the grains. This oxide film impedes the movement of carriers and However, there is a problem that the electrical characteristics of the transistor are deteriorated (for example, the mobility is reduced).

[0015] In addition, thin-film transistors used in protection circuits are often subjected to high voltages and A large current may flow.

[0016] In order to manufacture a display device with a small number of steps and high yield, the thin film formed in the pixel A thin film transistor and a thin film transistor which constitutes a protection circuit and is formed on the same substrate as the thin film transistor. The film transistors are preferably formed simultaneously.

[0017] In view of the above problems, the present invention provides a thin film transistor having good electrical characteristics and high reliability. It is an object of the present invention to manufacture a display device having such a structure with high yield and low cost. [Means for solving the problem]

[0018] One aspect of the present invention is a display device, comprising: a semiconductor layer of a thin film transistor that constitutes a protection circuit; A microcrystalline semiconductor layer is used as a buffer layer. The structure of the thin film transistor is described below.

[0019] The thin film transistor of the present invention is an inverted staggered type, and has a gate insulating layer covering the gate electrode. a microcrystalline semiconductor layer (semi-amorphous) functioning as a channel formation region on the gate insulating layer; A buffer layer is provided over the microcrystalline semiconductor layer, and the buffer A pair of source and drain regions is provided on the silicon layer, and the The source electrode and the drain electrode are opposed to each other. In the region where the source region and the drain region are exposed, a part of the buffer layer is exposed. is doing.

[0020] Alternatively, the source and drain regions are formed so as to expose parts of the source and drain regions. It is preferable that the semiconductor device has a pair of source and drain electrodes in contact with the drain region. This is to reduce the leakage current between the source region and the drain electrode. The drain region is a region in contact with the source electrode and the drain electrode, and a region between the source electrode and the drain electrode. The source electrode and the drain electrode are not in contact with each other. The ends of the source and drain regions are formed.

[0021] The display device of the present invention is a display device having an input terminal and a pixel portion, At least one protection circuit is provided between the pixel and the pixel unit, and the protection circuit includes at least The thin film transistor has a gate electrode and the first gate a gate insulating layer provided to cover the gate electrode; and a microcrystalline semiconductor provided on the gate insulating layer. a buffer layer provided on the microcrystalline semiconductor layer; and a The side surfaces of the source region and the drain region are substantially flush with the side surfaces of the recessed portion of the buffer layer. a drain region, a source electrode provided on and in contact with the source region, and a drain electrode provided in contact with the source region in the buffer layer. The region overlapping the drain region is thicker than the region overlapping the channel forming region, A protective insulating layer is provided on the source electrode and the drain electrode, and the protective insulating layer has a first opening and and a second opening, the first opening reaching the source electrode or the drain electrode. the second opening is provided so as to reach above the gate electrode, An electrode that connects the first opening and the second opening is provided on the protective insulating layer. It is characterized by:

[0022] The edges of the source and drain electrodes do not match the edges of the source and drain regions. The ends of the source region and the drain region are formed outside the ends of the source electrode and the drain electrode. As a result, the distance between the ends of the source electrode and the drain electrode increases, so that the source electrode In addition, the leakage current between the drain electrodes can be reduced, and short circuits can be prevented. In addition, an electric field is concentrated at the ends of the source electrode, the drain electrode, and the source region and the drain region. The present invention reduces leakage current between the gate electrode and the source and drain electrodes without causing a breakdown in the gate electrode. It is possible.

[0023] The buffer layer has a recess in a part thereof, and the side surface of the recess and the source region and the drain region The buffer layer has a recess in a portion thereof, and the ends of the source and drain regions are aligned. The leakage path distance is large, reducing the leakage current between the source and drain regions As a result, the off-current can be reduced.

[0024] In addition, a buffer layer is provided between the microcrystalline semiconductor layer and the source and drain regions. The microcrystalline semiconductor layer functions as a channel formation region. The microcrystalline semiconductor layer and the source and drain regions are formed on the semiconductor layer. Since a buffer layer with a recess is provided between the gate region and the semiconductor layer, the mobility is high and the leakage current is low. It is possible to form thin film transistors with small current and high withstand voltage. By reducing the leakage current, the off-current can be reduced.

[0025] The buffer layer can be formed of an amorphous semiconductor, and further, can be formed of nitrogen, hydrogen, or halide. It is preferable that the amorphous semiconductor layer contains at least one of nitrogen, hydrogen, or halogen. By including any one of halogens, crystal grains included in the microcrystalline semiconductor layer are oxidized. It is possible to reduce the occurrence of

[0026] The buffer layer can be formed by a plasma CVD method, a sputtering method, or the like. In addition, after forming the amorphous semiconductor layer, the amorphous semiconductor layer is irradiated with nitrogen plasma, hydrogen plasma or ha The amorphous semiconductor layer can be nitrogenized, hydrogenated, or halogenated by exposing it to halogen plasma. can.

[0027] By providing a buffer layer on the surface of the microcrystalline semiconductor layer, the crystal grains ( In particular, it can reduce oxidation of the surface, and reduce the deterioration of the electrical characteristics of thin film transistors. It is possible.

[0028] The microcrystalline semiconductor layer can be formed directly on the substrate. The film can be formed by using a plasma CVD method with a source gas such as orthogonal orthogonal. The microcrystalline semiconductor layer manufactured using the above method has semiconductor crystal grains with a size of about 0.5 nm to 20 nm. The amorphous semiconductor layer also contains a microcrystalline semiconductor. Unlike the conventional method, it is not necessary to provide a crystallization process such as a laser crystallization method after the semiconductor layer is formed. By using a microcrystalline semiconductor layer, the number of manufacturing steps of a thin film transistor can be reduced. This makes it possible to improve the yield of the display device and reduce the cost. In this study, the film (layer) obtained by film formation is called a microcrystalline semiconductor film (layer), and The film (layer) in which crystals are grown by irradiating laser light with an energy density that is not large enough to cause the laser to explode is then subjected to LPSA. In addition, plasma using microwaves with frequencies of 1 GHz or higher is called an electron-dense film. The frequency is high, which makes it easy to dissociate the silicon hydride gas used as the source gas. Compared with the microwave plasma CVD method using a frequency of 100 MHz or more and a frequency of 100 MHz or less, it is easy to form a microcrystalline semiconductor layer. This allows the film formation speed to be increased, and therefore the number of display devices can be increased. Productivity can be increased.

[0029] Further, the present invention relates to a display device using a thin film transistor having a microcrystalline semiconductor layer in a protection circuit. The mobility of a thin film transistor using a microcrystalline semiconductor layer is approximately 1 cm.2 / V· sec or more 20cm 2 / V·sec or less, and is a thin-film transistor using an amorphous semiconductor layer. Therefore, a part or the whole of the driver circuit can be placed in the same place as the pixel section. It is also possible to form the display panel on a substrate.

[0030] In addition, the element substrate may be formed with only the pixel electrodes of the display element. Alternatively, the pixel electrode may be formed by etching after the conductive layer that will become the pixel electrode is formed. It can be in a state before it is installed, or it can take any form.

[0031] In this specification, the liquid crystal display device refers to an image display device or a light source (illumination device). Also refers to connectors, such as FPC (Flexible Printed Circuit). circuit) or TAB (Tape Automated Bonding) Tape or TCP (Tape Carrier Package) attached Module, a module with a printed wiring board attached to the end of TAB tape or TCP, or The display element is directly mounted with an IC (integrated circuit) using the COG (Chip On Glass) method. The mounted modules are all included in the liquid crystal display device.

[0032] In this specification, LPSAS refers to a process in which a microcrystalline semiconductor layer is subjected to laser processing (LAPSAS) after film formation. A crystalline semiconductor obtained by the LP process. Refers to...

[0033] In the formation of the microcrystalline semiconductor layer in the present invention, microcrystalline silicon ( Semi-Amorphous Silicon (hereinafter referred to as "SAS") layers are deposited. After that, the surface side of the microcrystalline semiconductor layer is irradiated with laser light. The amorphous silicon layer is irradiated with an energy density that does not melt the amorphous silicon layer. LP is a solid-phase crystallization process that uses radiation heating to form a semi-amorphous silicon layer without melting it. That is, the deposited semi-amorphous silicon layer becomes liquid phase. This is a technique that utilizes the critical region where growth cannot occur, and in that sense it can be called "critical growth." can.

[0034] The laser light acts on the interface between the semi-amorphous silicon layer and the gate insulating layer. This allows the crystals formed in the semi-amorphous silicon layer to be used as seeds. Then, a semi-amorphous silicon layer having improved crystallinity can be formed by solid phase crystal growth. Typically, the crystals formed on the surface side of the semi-amorphous silicon layer act as nuclei. Solid-phase crystal growth proceeds from the surface toward the interface with the gate insulating layer, forming substantially columnar crystals. Alternatively, the crystals formed in the semi-amorphous silicon layer are used as nuclei, and the nuclei are The solid phase crystal growth is performed on the interface between the surface of the semi-amorphous silicon layer and the gate insulating layer. This allows the formation of a semi-amorphous silicon layer with improved crystallinity. Solid-phase crystal growth by laser does not enlarge the grain size, but increases the direction of laser irradiation (layer thickness). The crystal growth proceeds in the direction perpendicular to the crystal plane.

[0035] In the above LP process, the laser beam is focused into a long rectangular shape (formed into a linear laser beam). For example, semi-amorphous silicon on a 730 mm x 920 mm glass substrate The layer can be processed in one laser beam scan. In this case, a linear laser beam The overlap rate should be 0 to 90%, preferably 0 to 67%. This reduces the processing time per substrate, improving productivity. However, the shape of the laser beam is not limited to a linear shape, and may be a planar shape. In addition, LP processing is not limited to the size of the glass substrate, but can be applied to substrates of various sizes. By performing the LP treatment, the interface region between the microcrystalline semiconductor layer and the gate insulating layer can be The crystallinity of the resulting semiconductor is improved, thereby improving the electrical characteristics of a transistor having a bottom gate structure. It is possible.

[0036] This critical growth eliminates the surface irregularities ( No protruding ridges are formed, and the silicon surface after LP processing is smooth. .

[0037] As described above, the laser beam is directly applied to the semi-amorphous silicon layer after film formation. The crystalline silicon layer obtained by the above process is different from the conventional as-deposited microcrystalline silicon layer. The microcrystalline silicon layer modified by conductive heating (see Non-Patent Document 1) is The growth mechanisms and the film properties of the layers formed are significantly different.

[0038] In this specification, the amorphous semiconductor layer is formed by adding nitrogen, hydrogen, fluorine, or chlorine. It is preferable to include it. Effect of the Invention

[0039] The present invention provides a thin film transistor having excellent electrical characteristics and high reliability. The display device can be manufactured with high yield and low cost. [Brief description of the drawings]

[0040] [Figure 1] 1A to 1C are diagrams illustrating an example of a structure of a thin film transistor used in the present invention. [Diagram 2] 1A to 1C are diagrams illustrating an example of a display device to which the present invention can be applied. [Diagram 3] FIG. 2 is a diagram illustrating an example of a circuit configuration of a protection circuit to which the present invention is applied. [Figure 4] 2A to 2C illustrate an example of a manufacturing method of a thin film transistor used in the present invention. [Diagram 5] 2A to 2C illustrate an example of a manufacturing method of a thin film transistor used in the present invention. [Figure 6] FIG. 2 is a top view of a plasma CVD apparatus used for producing a thin film transistor according to the present invention. [Figure 7] FIG. 2 is a diagram for defining the taper angle in this specification. [Figure 8] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 9] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 10] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 11] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 12] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 13] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 14] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 15] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 16] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 17] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 18] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 19] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 20] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 21] 1A and 1B are diagrams illustrating a liquid crystal display device to which the present invention can be applied. [Figure 22] 1A to 1C are diagrams illustrating an example of a method for manufacturing a light-emitting device to which the present invention can be applied. [Diagram 23] 1A to 1C are diagrams illustrating a light-emitting device to which the present invention can be applied. [Figure 24] FIG. 1 is a block diagram illustrating a configuration of a display device to which the present invention can be applied. [Diagram 25] FIG. 1 is an equivalent circuit diagram illustrating a driver circuit of a display device to which the present invention can be applied. [Figure 26] FIG. 2 is an equivalent circuit diagram illustrating a driver circuit of a display device that can be used in the present invention. [Figure 27] 1A and 1B are a top view and a cross-sectional view illustrating a liquid crystal display panel of the present invention. [Figure 28] 1A and 1B are a top view and a cross-sectional view illustrating a light-emitting display panel of the present invention. [Figure 29] 1A to 1C are diagrams illustrating electronic devices using a display device of the present invention. [Diagram 30] 1A to 1C are diagrams illustrating electronic devices using a display device of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0041] The present invention will be described below with reference to the drawings. The present invention is not limited to the above description without departing from the spirit and scope of the present invention. It will be readily understood by those skilled in the art that various changes in form and detail may be made. Therefore, the present invention should not be construed as being limited to the following description of the embodiments. In describing the configuration of the present invention with reference to the drawings, the same elements are designated by different reference numerals. This is also used commonly between the drawings.

[0042] (Embodiment 1) In this embodiment, one embodiment of the present invention will be described with reference to the drawings.

[0043] First, the configuration of the semiconductor display device of the present invention will be described with reference to FIG. 1 shows a top view of a substrate 130 on which a semiconductor display device is formed. The input terminal 132 and the input terminal 133 are formed on the substrate 130. The pixel circuit is supplied with signals and power for displaying an image.

[0044] The present invention is not limited to the embodiment shown in Fig. 2. Either or both of a driver circuit and a signal line driver circuit may be formed.

[0045] The input terminals 132 on the scanning line side and the input terminals 133 on the signal line side are formed on the substrate 130. The pixel section 131 is connected to the pixel section 133 by wiring extending vertically and horizontally. It is connected to circuits 134 to 137.

[0046] The pixel portion 131 and the input terminal 132 are connected to each other by a wiring 139. 134 is disposed between the pixel section 131 and the input terminal 132 and is connected to a wiring 139. By providing the protection circuit 134, the thin film transistors and the like included in the pixel portion 131 are It is possible to protect various semiconductor elements and prevent them from being deteriorated or destroyed. Although the wiring 139 is shown as one wiring in the figure, it is set in parallel with the wiring 139. All of the multiple wirings connected to the wiring 139 have the same connection relationship as the wiring 139. 39 functions as a scanning line.

[0047] On the scanning line side, a protection circuit is provided between the input terminal 132 and the pixel section 131. A protection circuit is provided not only on the input terminal 134 but also on the opposite side of the input terminal 132 across the pixel section 131. (See the protection circuit 135 in FIG. 2).

[0048] On the other hand, the pixel section 131 and the input terminal 133 are connected by a wiring 138. The protection circuit 136 is disposed between the pixel section 131 and the input terminal 133 and is connected to the wiring 138. By providing the protection circuit 136, the thin film transistor of the pixel portion 131 It can protect various semiconductor elements such as photodiodes and photodiodes from deterioration or destruction. In addition, although the wiring 138 is shown as one wiring in the figure, the wiring 138 and All of the multiple wirings arranged in parallel have the same connection relationship as the wiring 138. The wiring 138 functions as a signal line.

[0049] In addition, on the signal line side, a protection circuit provided between the input terminal 133 and the pixel section 131 136, but also on the opposite side of the input terminal 133 across the pixel unit 131. Good (see protection circuit 137 in FIG. 2).

[0050] It is not necessary to provide all of the protection circuits 134 to 137. However, at least one protection circuit 134 is required. When an excessive current is generated in the scanning line, This is because the gate insulating layer of the thin film transistor may be destroyed, resulting in a large number of point defects.

[0051] In addition, by providing not only the protection circuit 134 but also the protection circuit 136, excessive current in the signal line is prevented. Therefore, the reliability is improved compared to the case where only the protection circuit 134 is provided. The protection circuit 136 improves the efficiency of the thin film transistor formation. It is also possible to prevent damage caused by static electricity that may occur in a subsequent rubbing step or the like.

[0052] Furthermore, the provision of the protection circuits 135 and 137 further improves reliability. In addition, the yield can be increased. 37 is provided on the opposite side to the input terminals 132 and 133. These are various semiconductor elements that are generated during the manufacturing process of the display device (for example, the rubbing process). This contributes to preventing deterioration and destruction of the

[0053] In FIG. 2, the signal line driving circuit and the scanning line driving circuit formed separately from the substrate 130 are The substrate 130 is mounted by a known method such as the OG method or the TAB method. However, this is not limited to this. The scanning line driving circuit and the pixel section are formed on the substrate 130, and the signal line driving circuit is formed separately. Alternatively, a part of the scanning line driver circuit or a part of the signal line driver circuit may be mounted. is formed on the substrate 130 together with the pixel portion 131, and other portions of the scanning line driving circuit or signal lines Other parts of the driver circuit may be mounted. and the input terminal 132 on the scanning line side, A protection circuit may be provided between the gate 2 and a part of the scanning line driving circuit on the substrate 130. A protection circuit may be provided between a part of the operating circuit and the pixel section 131, or a protection circuit may be provided on both of them. A part of the signal line driver circuit may be connected to the pixel section 131 and the input terminal 1 on the signal line side. 33, the input terminal 133 on the signal line side and the signal A protection circuit may be provided between a part of the signal line driving circuit and the pixel section 1. A protection circuit may be provided between the power supply 1 and the power supply 31, or a protection circuit may be provided between the power supply 1 and the power supply 31. Since there are various types of drive circuits, the number and location of the protection circuits must be determined according to the type of drive circuit. stipulate.

[0054] Next, a specific circuit configuration of the protection circuits 134 to 137 in FIG. An example of the above will be described with reference to FIG. 3. N-type transistors have higher mobility than p-type transistors, Therefore, in the following explanation, n-type transistors are generally used. Only the case where a resistor is provided will be described.

[0055] The protection circuit shown in FIG. 3A includes a protection diode 151 using a plurality of thin film transistors. The protection diode 151 has n-type thin film transistors 1 to 154 connected in series. The n-type thin film transistor 151a and the n-type thin film transistor 151b are One of the source electrode and the drain electrode of the n-type thin film transistor 151a and is connected to the gate electrode of the second-type thin film transistor 151b and is connected to the potential V ss is maintained. The other of the source electrode and the drain electrode of the n-type thin film transistor 151a is The n-type thin-film transistor 151b is connected to one of the source electrode and the drain electrode of the n-type thin-film transistor 151c. The other of the source electrode and the drain electrode of the transistor 151b is connected to a protection diode 152. Similarly to the protective diode 151, the other protective diodes 152 to 154 are also Each of the thin film transistors is connected in series. One end of the thin film transistor is connected to the gate electrodes of the plurality of thin film transistors.

[0056] In the present invention, the thin film transistors of the protection diodes 151 to 154 are The number and polarity of the protection diodes are not limited to the configuration shown in FIG. 151 may be composed of three thin film transistors connected in series.

[0057] The protection diodes 151 to 154 are connected in series in order. The node 152 and the protection diode 153 are connected to a wiring 155. The wiring 55 is electrically connected to the semiconductor element to be protected. The wiring connected to 55 is limited to the wiring between the protection diode 152 and the protection diode 153. That is, the wiring 155 is not connected between the protection diode 151 and the protection diode 152. or between the protection diode 153 and the protection diode 154. It may be possible to do so.

[0058] One end of the protective diode 154 is connected to the power supply potential V dd In addition, the protection Each of the diodes 151 to 154 is connected so that a reverse bias voltage is applied. There are.

[0059] The protection circuit shown in FIG. 3B includes a protection diode 160, a protection diode 161, a capacitance element The resistor element 164 is a two-terminal resistor. One end of the wire 165 is connected to a potential V in is supplied to the other end, and the potential V ss Supplied by The resistor element 164 is connected to a potential V inWhen the power supply is stopped, the potential of the wiring 165 is V ss The resistance value is sufficiently larger than the wiring resistance of the wiring 165. The protection diode 160 and the protection diode 161 are diodes The device uses a gate-connected n-type thin-film transistor.

[0060] The protection diode shown in FIG. 3 is further constructed by connecting multiple thin film transistors in series. It may be the same.

[0061] Let us now consider the case where the protection circuit shown in Figure 3 operates. The source electrodes of the electrodes 151, 152, 156, 161, 170, 171, 174, and 175 At the drain electrode, the potential V ss The side that is held by the resistor is the drain electrode. The protection diodes 153, 154, 157, 160, 172, 173, 1 At the source and drain electrodes of 76 and 177, the potential V dd The side that is held by the saw The other electrode is the source electrode, and the other electrode is the drain electrode. The threshold voltage of the transistor is V th This indicates that.

[0062] In addition, protection diodes 151, 152, 156, 161, 170, 171, 174, 1 75 is the potential V in is the potential V ss When the voltage is higher, a reverse bias voltage is applied and current begins to flow. On the other hand, protection diodes 153, 154, 157, 160, 172, 173, 176 , 177 is the potential V in is the potential V dd When the voltage is lower than the The flow is poor.

[0063] Here, the potential V out is approximately the potential V ss and potential V dd A protection zone is set up between The operation of the protection circuit will now be described.

[0064] First, the potential V in is the potential V dd Consider the case where the potential is higher than V in is the potential V dd twist If the voltage is also high, the protection diodes 153, 154, 157, 160, 172, 173, and 176 , 177 potential difference between the gate electrode and the source electrode V gs =V in -V dd >V th When When V in Assuming that is abnormally high At this time, the protection diodes 151 and 1 52, 156, 161, 170, 171, 174, and 175 have n-type thin film transistors Then, the protection diodes 153, 154, 157, 160, 172, Through 173, 176, and 177, the wirings 155, 158, 165, 179A, and 179B The potential is V dd Therefore, the potential V in is the potential V dd abnormally higher than Even if this happens, the potential of the wirings 155, 158, 165, 179A, and 179B will be V d d It will never be higher than that.

[0065] On the other hand, the potential V in is the potential V ss If the voltage is lower than the threshold voltage, the protection diodes 151 and 152 , 156, 161, 170, 171, 174, 175, potential between gate electrode and source electrode difference V gs =V ss -V in >V th At this time, the n-type thin film transistor is turned on. Here, V in Since it is assumed that the voltage is abnormally low, the n-type thin film transistor turns on. At this time, the protection diodes 153, 154, 157, 160, 172, 173, and 176 Then, the n-type thin film transistor 177 is turned off. , 152, 156, 161, 170, 171, 174, 175, through wiring 155, 1 The potential of 58, 165, 179A, and 179B is V ss Therefore, the power consumption may be affected by noise, etc. Place V in is the potential V ss Even if it becomes abnormally low, wiring 155, 158, 165, 1 The potential of 79A and 179B is V ss Furthermore, the capacitance element 1 62, 163 are the input potential V in It reduces the potential of the noise by reducing the pulse noise. This serves to mitigate the sudden changes in

[0066] In addition, the potential V in But, V ss -V th From V dd +V th In the case of The n-type thin film transistor in the protection diode is turned off, and the potential V in is the potential V out fart is entered.

[0067] By disposing the protection circuits as described above, the wirings 155, 158, 165, and 179 The potential of A and 179B is approximately V ssand potential V dd Therefore, The wirings 155, 158, 165, 179A, and 179B are at potentials that are significantly outside this range. In other words, the wirings 155, 158, 165, 179A, 1 79B to prevent the potential from becoming abnormally high or low, and This prevents the circuit from being destroyed or deteriorated, and protects the subsequent circuits.

[0068] Furthermore, as shown in FIG. 3B, a protection circuit having a resistor element 164 is provided at the input terminal. By doing so, when no signal is being input, the potential of all wiring to which a signal is applied is kept constant. (Here, the potential V ss ) when no signal is being input. It also functions as a short ring that can short the wires together. It is possible to prevent electrostatic destruction caused by a potential difference occurring between wirings. Since the resistance of 4 is sufficiently large compared to the wiring resistance, the signal applied to the wiring when the signal is input is The number is the potential V ss It is possible to prevent the temperature from dropping to the level below the threshold.

[0069] Here, as an example, the protective diodes 160 and 161 in FIG. Threshold voltage V th A case where an n-type thin film transistor with a capacitance of 0 is used will be described.

[0070] First, V in >V dd In this case, the protection diode 160 is V gs =V in -V dd > 0 and turns on. The protective diode 161 turns off. Therefore, the potential of the wiring 165 becomes V ddAnd V out =V dd It becomes.

[0071] On the other hand, V in <V ss In this case, the protection diode 160 is turned off. Do 161 is V gs =V ss -V in >0, and the line 165 is turned on. V ss And V out =V ss It becomes.

[0072] In this way, V in <V ss or V dd <V in Even if V ss <V out <V dd Therefore, V in If too large or too Even if the V out This can prevent the amount of Therefore, if the potential V in is the potential V ss If it is lower than However, the potential of the wiring 165 is V ss Furthermore, the capacitance of the The capacitor 162 and the capacitance element 163 are connected to the input potential V in It reduces the pulse noise of the It acts to mitigate sudden changes in position.

[0073] As described above, by disposing the protection circuit, the potential of the wiring 165 is set to the potential V ss And electricity Place V dd Therefore, the wiring 165 is not significantly out of this range. This prevents the input voltage from reaching a certain level, and the circuit downstream of the protection circuit (the input section is V ou t In addition, the input (circuits electrically connected to the By providing a protection circuit to the terminal, when no signal is input, all signals The potential of the wiring is kept constant (here, potential V ss ), that is, the signal can be kept at the input When not in use, it functions as a shorting ring that can short wires together. Therefore, it is possible to prevent electrostatic damage caused by the potential difference between wiring. In addition, since the resistance value of the resistor element 164 is sufficiently large, when a signal is input, the wiring 165 This can prevent a decrease in the potential of the signal applied to the

[0074] The protective circuit shown in FIG. 3C includes a protective diode 160 and a protective diode 161. Each of these is replaced by two n-type thin-film transistors.

[0075] The protection circuits shown in FIG. 3B and FIG. 3C use a diode as a protection diode. Although the present invention uses n-type thin film transistors connected to each other, the present invention is not limited to this configuration.

[0076] The protection circuit shown in FIG. 3D includes protection diodes 170 to 177 and a resistance element 17 8. The resistor element 178 is connected in series between the wiring 179A and the wiring 179B. Each of the protection diodes 170 to 173 is a diode-connected n-type thin film transistor. Each of the protection diodes 174 to 177 is a diode-connected The device uses n-type thin-film transistors.

[0077] The protection diode 170 and the protection diode 171 are connected in series, and one end is connected to a potential V ss and the other end is held at potential V in The protection diode 1 is connected to the wiring 179A. 72 and a protection diode 173 are connected in series, and one end is connected to a potential V dd held in other The end is at potential V in The protection diode 174 and the protection diode 179 are connected to the wiring 179A. The leads 175 are connected in series, with one end connected to a potential V ss and the other end is held at potential V out of The protection diode 176 and the protection diode 177 are connected in series. One end is connected to a potential V dd and the other end is held at potential V out Connect to wire 179B. This is being continued.

[0078] The protection circuit shown in FIG. 3E includes a resistance element 180, a resistance element 181, and a protection diode. In FIG. 3E, a diode connection is used as the protection diode 182. However, the present invention is not limited to this configuration. A plurality of thin film transistors connected in series may be used. 181 and a protection diode 182 are connected in series to a wiring 183 .

[0079] The resistor element 180 and the resistor element 181 reduce abrupt changes in the potential of the wiring 183. In addition, the protection diode 182 can prevent the semiconductor element from being deteriorated or destroyed. This prevents a reverse bias current from flowing through the wiring 183 due to a change in potential. can be done.

[0080] The protection circuit shown in Figure 3(A) can be replaced with the configuration shown in Figure 3(F). In particular, the protection circuit used in the present invention has a high withstand voltage, and therefore uses a configuration as shown in FIG. There can be.

[0081] In addition, when only a resistance element is connected in series to a wiring, the sudden fluctuation of the wiring potential is mitigated. This makes it possible to prevent deterioration or destruction of the semiconductor element. When connecting in series with a wire, it is possible to prevent a reverse current from flowing in the wire due to a change in potential. can.

[0082] The protection circuit used in the present invention is not limited to the configuration shown in FIG. As long as the circuit configuration functions as described above, the design can be modified as appropriate.

[0083] The protection diode of the protection circuit of the present invention is a diode-connected thin film The thin film transistor is a high voltage thin film transistor. Therefore, in conventional protection circuits, a voltage high enough to destroy the protection circuit itself is applied. Even in such a case, the protection circuit of the present invention prevents the wiring from being exposed to an abnormally high or low potential. Here, the protection diode of the protection circuit is The constituent thin film transistors will be described with reference to FIG.

[0084] FIG. 1 shows an example of a top view and a cross-sectional view of the protection diode 160 etc. shown in FIG. The thin film transistor constituting the protection diode shown in FIG. 102, a first insulating layer 104 covering the first conductive layer 102, and the first insulating layer 1 04, and a buffer layer 108 on the LPSAS layer 106; A doped semiconductor layer 110 is provided on the buffer layer 108, and a second conductive layer is provided on the doped semiconductor layer 110. The second conductive layer 112 has a second insulating layer 114 over the second conductive layer 112. A third conductive layer 116 is formed on layer 114. Each layer is patterned into a desired shape. The third conductive layer 116 is formed through the first opening 118 and the second opening 119 in the second insulating layer 114. The first conductive layer 102 and the second conductive layer 112 are electrically connected to each other through the opening 120. do.

[0085] At least one of the source electrode and the drain electrode is The other pole is enclosed (U-shaped) (see Figure 1). The electrodes of the thin-film transistors used in the device protection circuit are U-shaped as shown in Figure 1. This makes it possible to increase the channel width of the thin film transistor, and an excessive current flows. Therefore, it is a protection circuit with excellent original function. A path can be established.

[0086] Next, a method for manufacturing the protection diode shown in FIG. Generally, n-type thin-film transistors have higher mobility than p-type. If all the thin-film transistors formed in the semiconductor device are made to have the same polarity, the number of manufacturing steps can be reduced. Therefore, a method for fabricating an n-type thin film transistor will be described here. Reveal.

[0087] First, a first conductive layer 102 is formed on a substrate 100. The substrate 100 is made of barium borate. Glass made of fluorinated glass, aluminoborosilicate glass, or aluminosilicate glass. In addition to non-alkali glass substrates and ceramic substrates manufactured by the deposition method and float method, A heat-resistant plastic substrate capable of withstanding the processing temperatures in the manufacturing process can be used. Alternatively, a metal substrate such as a stainless steel alloy substrate having an insulating layer on its surface may be used. That is, a substrate having an insulating surface is used as the substrate 100. In the case of semiconductor devices, the size of the board is divided into first generation (e.g., 320 mm x 400 mm), 2nd generation (e.g., 400mm x 500mm), 3rd generation (e.g., 550mm x 650mm m), 4th generation (e.g., 680mm x 880mm, or 730mm x 920mm), 5th generation (e.g., 1000mm x 1200mm or 1100mm x 1300mm), 6th Generation (e.g., 1500mm x 1800mm), 7th generation (e.g., 1900mm x 22 00mm), 8th generation (e.g., 2160mm x 2460mm), 9th generation (e.g., 2 400mm x 2800mm), 10th generation (e.g., 2850mm x 3050mm), etc. can be used.

[0088] The first conductive layer 102 functions as a gate electrode. The first conductive layer 102 is made of titanium, Molybdenum, chromium, tantalum, tungsten, aluminum, copper, neodymium, scandium The plate is made of a metal material such as aluminum or an alloy material that contains these as its main component. If an Al-Ta alloy is used, hillocks can be suppressed by adding tantalum. In addition, an Al-Nd alloy containing neodymium is used. By using this method, not only hillocks are suppressed but also wiring with low resistance can be formed, which further improves the In addition, semiconductors such as polycrystalline silicon doped with impurity elements such as phosphorus are also preferred. A conductor or an AgPdCu alloy may be used. It may be a single layer or a multilayer. For example, aluminum Two-layer laminate structure with a molybdenum layer laminated on a tungsten layer, and a molybdenum layer laminated on a copper layer A two-layer laminate structure with a titanium nitride layer or a tantalum nitride layer laminated on a copper layer. It is preferable to use a laminated structure. A metal layer that functions as a barrier layer on a layer with low electrical resistance. By stacking the metal layers, the electrical resistance is low and the metal layer that can diffuse into the microcrystalline semiconductor layer can be prevented. The diffusion of metal elements can be prevented. A two-layer laminate structure or a 50 nm thick tungsten layer and a 500 nm thick aluminum layer The titanium nitride layer may be a three-layered structure consisting of a titanium-silicon alloy layer and a titanium nitride layer with a thickness of 30 nm. In addition, when a three-layer laminate structure is used, tungsten is replaced by tungsten nitride in the first conductive layer. Alternatively, the second conductive layer may be made of aluminum instead of the aluminum-silicon alloy layer. A layer of an alloy of aluminum and titanium may be used, or titanium may be used instead of the titanium nitride layer of the third conductive layer. For example, a molybdenum layer may be formed on an Al-Nd alloy layer. In this way, a conductive layer having excellent heat resistance and low resistance can be formed.

[0089] The first conductive layer 102 is formed by forming a conductive layer on the substrate 100 by sputtering or vacuum deposition. A mask is formed on the conductive layer by photolithography or inkjet printing. The conductive layer can be etched using the mask. Conductive nanopaste made of gold, copper, etc. is ejected onto a substrate using the inkjet method and then baked. In addition, in order to improve the adhesion between the first conductive layer 102 and the substrate 100 and As a barrier metal to prevent diffusion to the underlayer, a nitride layer of the above metal material is formed on the substrate 100. The second conductive layer 102 may be provided between the first conductive layer 102 and the second conductive layer 103. Using a resist mask, the conductive layer formed on the substrate 100 is etched to form a first conductive layer. Form 102.

[0090] In addition, since a semiconductor layer and a wiring layer are formed on the first conductive layer 102 in a later process, a step is formed on the first conductive layer 102. In order to prevent the wiring from breaking at the part having the wire, the end is processed to have a tapered shape. In addition, the scanning lines can be formed at the same time in this process. A capacitance line having a scanning line can also be formed. .

[0091] Next, a first insulating layer 104, a microcrystalline semiconductor layer 105, a barrier layer 106, and a GaN layer 108 are formed on the first conductive layer 102. a buffer layer 107 and an impurity semiconductor layer 109 to which an impurity element imparting one conductivity type is added; Layers for forming the conductive layer 111 are formed in order, and a resist pattern is formed on the conductive layer 111 using a multi-tone mask. A mask 140 is formed (see FIG. 4(A)). 04. It is preferable to form the microcrystalline semiconductor layer 105 and the buffer layer 107 in succession. More preferably, the first insulating layer 104, the microcrystalline semiconductor layer 105, the buffer layer 107, and the A pure semiconductor layer 109 is successively formed. At least the first insulating layer 104, the microcrystalline semiconductor layer The dielectric layer 105 and the buffer layer 107 are successively formed without being exposed to the atmosphere. Each layer interface can be formed without being contaminated by impurity elements floating in the air or by chemical components. This reduces the variation in the electrical characteristics of thin-film transistors, improving reliability. High quality semiconductor devices can be manufactured with high yield.

[0092] The first insulating layer 104 functions as a gate insulating layer. The first insulating layer 104 is formed by CVD. Silicon oxide, silicon nitride, silicon oxynitride, or silicon nitride oxide is formed by a deposition method or a sputtering method. It may be formed as a single layer or may be formed by laminating these layers. The first insulating layer 104 may be formed of a mixture of silicon nitride or silicon nitride oxide and silicon oxide or silicon oxynitride. It is preferable that the insulating layer is formed by laminating silicon nitride and silicon oxide in this order from the substrate side. The silicon carbide is formed by absorbing impurity elements contained in the substrate 100 into the LPSAS layer 106. Silicon oxide and silicon oxynitride have a high effect of preventing the interface between the microcrystalline semiconductor layer and the semiconductor layer. Alternatively, the first insulating layer 104 may be made of silicon oxide or silicon oxynitride. , silicon nitride or silicon nitride oxide, and silicon oxide or silicon oxynitride in this order from the substrate side. Alternatively, the first insulating layer 104 may be formed by stacking layers. It may be formed of a single layer of silicon or silicon nitride oxide. It is preferable to form the first insulating layer 104 by using a microwave plasma CVD method. Silicon oxynitride and silicon nitride oxide formed by the microwave plasma CVD method have a dense film quality and are therefore pressure-resistant. This can improve the reliability of the thin film transistor to be formed later.

[0093] The first insulating layer 104 is preferably a two-layer structure in which silicon oxynitride is laminated on silicon nitride oxide. The thickness of this laminated film is 50 nm or more, preferably 50 nm or more and 200 nm or less. Silicon oxynitride is formed by oxidizing alkali metals contained in the substrate 100 to the LPSAS layer 10. In addition, silicon oxynitride can be prevented from being mixed into the first conductive layer 102. This prevents hillocks that may occur when aluminum is used for the first conductive layer 102. It is possible to prevent oxidation of the material.

[0094] Silicon oxynitride is a material whose composition contains more oxygen than nitrogen. The concentration ranges are 55-65 atomic % for oxygen, 1-20 atomic % for nitrogen, and 25- 35 atomic % and hydrogen in the range of 0.1 to 10 atomic %. Silicon oxynitride The element is a substance whose composition contains more nitrogen than oxygen, and its concentration range is Oxygen 15-30 atomic %, Nitrogen 20-35 atomic %, Silicon 25-35 atomic %, Hydrogen is contained in the range of 15 to 25 atomic %.

[0095] After the first insulating layer 104 is formed and before the microcrystalline semiconductor layer 105 is formed, A layer for improving adhesion of the layer 105 and preventing oxidation due to LP is formed on the first insulating layer 104. By this treatment, the microcrystalline semiconductor layer 105 to be formed thereon is preferably It improves adhesion and prevents oxidation during LP.

[0096] The microcrystalline semiconductor layer 105 will become an LPSAS layer 106 in a later process. The crystalline semiconductor layer 105 is a semiconductor having an intermediate structure between an amorphous structure and a crystalline structure (including a single crystal and a polycrystal). A microcrystalline semiconductor is a semiconductor that has a third state that is stable in terms of free energy. Conductive, crystalline, with short-range order and lattice distortion, with a grain size of approximately 0. It is possible to disperse the particles in the non-single crystal semiconductor to a size of 0.5 to 20 nm. Microcrystalline silicon, a typical example of a crystalline semiconductor, has a Raman spectrum similar to that of single-crystalline silicon. Shown: 520.6cm -1 It is shifted to the lower frequency side than 481 cm. -1 Below Upper 520.6cm -1 The Raman spectrum of microcrystalline silicon has a peak between In addition, at least one hydrogen or halogen atom is added to terminate the dangling bond. In addition, helium, argon, krypton, neon, etc. By adding rare gas elements, the lattice distortion is further promoted, resulting in increased stability and good microcrystallinity. A semiconductor layer is obtained. Such a microcrystalline semiconductor is disclosed, for example, in Patent Document 3. As shown.

[0097] Note that the half-width of the peak of the Raman spectrum can be used to determine the It is possible to calculate the grain size of the crystal grains. The grains are not believed to be round in shape.

[0098] The microcrystalline semiconductor layer 105 is formed by a high-frequency plasma CVD method having a frequency of several tens to several hundreds of MHz. Alternatively, it can be formed by a microwave plasma CVD method with a frequency of 1 GHz or more. Representative examples include SiH 4 , Si 2 H 6 It can be formed by diluting silicon hydride such as In addition to silicon hydride and hydrogen, helium, argon, krypton and neon are also used. It may also be formed by diluting with one or more selected rare gas elements. The flow rate ratio of hydrogen to silicon is 5 to 200 times, preferably 50 to 150 times. , and more preferably 100 times. Note that instead of silicon hydride, SiH 2 Cl 2 , Si HCl 3 , SiCl 4 or SiF 4 etc. can be used.

[0099] In addition, the microcrystalline semiconductor layer must be formed by intentionally adding an impurity element for the purpose of controlling valence electrons. Since it exhibits weak n-type electrical conductivity, it functions as the channel formation region of a thin-film transistor. An impurity element that imparts p-type conductivity is added to the microcrystalline semiconductor layer simultaneously with or after the film formation. By doing so, the threshold voltage V th It is preferable to control the p-type impurity element. A typical example is boron, and B 2 H 6 , B.F. 3 Impurity gases such as 1ppm to 1000ppm pm, preferably at a ratio of 1 to 100 ppm, is mixed into silicon hydride. And the concentration of boron is, for example, 1×10 14 ~6×10 16 cm -3 It would be better to say:

[0100] The oxygen concentration of the microcrystalline semiconductor layer is set to 1×10 19 cm -3 Less than or equal to 5×10 18 cm -3 The following nitrogen and carbon concentrations are 5×10 18 cm -3 Below, preferably 1×1 0 18 cm -3 The following is preferable: By reducing the carbon concentration, the channel formation region of the microcrystalline semiconductor layer becomes an n-type semiconductor. In addition, if the concentration of these substances varies between elements, the threshold voltage Voltage V th Therefore, by reducing the concentration of these elements, The threshold voltage V th It is possible to reduce the variation in the

[0101] The microcrystalline semiconductor layer 105 has a thickness of 2 nm to 50 nm, preferably 10 nm to 30 nm. The microcrystalline semiconductor layer 105 is formed as a channel formation region of a thin film transistor. By setting the thickness of the microcrystalline semiconductor layer 105 to 2 nm or more and 50 nm or less, a thin film The transistor can be made a fully depleted type. Since the film formation speed is 1 / 10 to 1 / 100 of the film formation speed of the high-quality semiconductor layer, it is preferable to form it thinly. By forming the semiconductor thin, the throughput can be improved. Because it is made up of microcrystals, it has a smaller electrical resistance than amorphous semiconductors. In a thin-film transistor using a microcrystalline semiconductor, the horizontal axis represents the gate voltage and the vertical axis represents the source- The slope of the rising portion of the curve showing the current-voltage characteristics of the drain current becomes steeper. Therefore, a thin film transistor using a microcrystalline semiconductor for a channel formation region is a switching element. The device has excellent response as a semiconductor and can operate at high speed. By using a microcrystalline semiconductor in the formation region, the threshold voltage V th Suppression of fluctuations It is possible to make the threshold voltage V th By suppressing the fluctuation of Therefore, a display device with less noise can be manufactured.

[0102] In addition, the microcrystalline semiconductor has a higher carrier mobility than the amorphous semiconductor. A switching element in a display device is formed of a microcrystalline semiconductor in a channel formation region. When a thin film transistor having a channel region is used, the area of ​​the thin film transistor is Therefore, the area of ​​the protection circuit can be reduced, and the display device can be made smaller. Edging becomes possible.

[0103] The buffer layer 107 is formed using the same material as the microcrystalline semiconductor layer 105. The amorphous semiconductor layer is made of SiH 4 , Si 2 H 6 Hydrogenated silicon such as The silicon hydride can be formed by using a plasma CVD method. It is used by diluting it with one or more rare gas elements selected from argon, krypton, and neon. By this, an amorphous semiconductor layer can be formed. 10 times or less, preferably 1 to 10 times or less, more preferably 1 to 5 times or less The amorphous semiconductor layer containing hydrogen can be formed by using the above-mentioned silicon hydride. and nitrogen or ammonia to form an amorphous semiconductor layer containing nitrogen. In addition, the above silicon hydride and a gas containing fluorine or chlorine (F 2 , Cl 2 , H.F. By using an amorphous semiconductor layer containing fluorine or chlorine, an amorphous semiconductor layer containing fluorine or chlorine can be formed. Instead of silicon hydride, SiH 2 Cl 2 , SiHCl 3 , SiCl 4 , Si F 4 The thickness of the amorphous semiconductor layer is 100 nm or more and 50 nm or less. 0 nm or less, preferably 150 nm to 400 nm, and more preferably 200 The thickness is from 1 nm to 300 nm.

[0104] The buffer layer 107 is formed by ionizing hydrogen or a rare gas using an amorphous semiconductor as a target. Alternatively, the insulating layer may be formed of an amorphous semiconductor by sputtering in a vacuum. Ammonia, Nitrogen or N 2 By including O in the atmosphere, an amorphous semiconductor containing nitrogen is formed. In addition, a gas containing fluorine or chlorine (F 2 , Cl 2 , HF, HCl, etc.) to form an amorphous semiconductor layer containing fluorine or chlorine. It is possible.

[0105] The buffer layer 107 is formed on the surface of the microcrystalline semiconductor layer 105 by a plasma CVD method or After forming an amorphous semiconductor layer by sputtering, the surface of the amorphous semiconductor layer is immersed in hydrogen. The surface of the amorphous semiconductor layer is treated with a nitrogen plasma or a halogen plasma to convert the surface of the amorphous semiconductor layer into hydrogen. Alternatively, the surface of the amorphous semiconductor layer may be irradiated with helium. Treatment with Zr, neon plasma, argon plasma, krypton plasma, or the like may also be used.

[0106] The buffer layer 107 is formed of an amorphous semiconductor. The amorphous semiconductor layer does not include crystal grains. For this reason, high-frequency plasma CV with a frequency of several tens to several hundreds of MHz is used. When it is formed by the D method or the microwave plasma CVD method, it is an amorphous semiconductor that does not contain crystal grains. It is preferable to control the film formation conditions so as to form a conductive layer.

[0107] The buffer layer 107 is partially depleted in the subsequent process of forming the source and drain regions. The thickness of the buffer layer 108 is such that the buffer layer 108 is etched to have a recess, but a portion of the buffer layer 108 overlapping the recess remains. It is preferable to form the recess by the thickness of the remaining portion (portion overlapping the recess) after etching. The thickness of the film after etching is preferably about half of the thickness before etching. The film thickness before etching is, as described above, 100 nm or more and 500 nm or less, and preferably is 150 nm or more and 400 nm or less, and more preferably 200 nm or more and 300 nm or less The thickness of the buffer layer 108 in the portion overlapping with the impurity semiconductor layer 109 is Since it is not reduced in the process of forming the source and drain regions, nm or less, preferably 150 nm or more and 400 nm or less, and more preferably 20 As described above, the amorphous semiconductor that becomes the buffer layer 108 has a thickness of 0 nm or more and 300 nm or less. By making the layer sufficiently thick, the LPSAS layer 106 can be formed stably. Thus, the buffer layer 108 functions as a film that prevents the LPSAS layer 106 from being etched. It functions as such.

[0108] The buffer layer 107 does not contain impurities that impart one conductivity type, such as phosphorus or boron. In particular, boron is added to the LPSAS layer 106 to control the threshold voltage. It is preferable that phosphorus contained in the impurity semiconductor layer 110 does not mix with the buffer layer 108. For example, if the buffer layer 108 contains phosphorus, the LPSAS layer 106 and the buffer A PN junction is formed between the buffer layer 108 and the layer 108. When the buffer layer 108 contains boron, A PN junction is formed between the buffer layer 108 and the impurity semiconductor layer 110. Alternatively, The inclusion of both boron and phosphorus creates recombination centers, which can cause leakage current. Since the buffer layer 108 does not contain these impurities that impart one conductivity type, the leakage current This can eliminate the region where leakage current occurs, thereby reducing the leakage current. Between the SiO 2 layer and the LPSAS layer 106, impurities such as phosphorus or boron that impart one conductivity type are added. By providing the buffer layer 108 which is an amorphous semiconductor layer that is not interposed between the channel formation region and the The LPSAS layer 106 is a semiconductor layer that serves as a source region and a drain region. This can prevent the diffusion of impurities contained in each of them.

[0109] The surface of the microcrystalline semiconductor layer 105 is provided with an amorphous semiconductor layer and / or a semiconductor layer containing hydrogen, nitrogen, or halogen. By forming an amorphous semiconductor layer including the microcrystalline semiconductor layer 105, the surface of the crystal grains included in the microcrystalline semiconductor layer 105 can be automatically It is possible to prevent spontaneous oxidation. In particular, in the region where the amorphous semiconductor contacts the crystal grains, Cracks caused by distortion of the crystal lattice are likely to occur. When oxygen comes into contact with these cracks, the crystal grains The buffer layer 107 is formed on the surface of the microcrystalline semiconductor layer 105. By having the above structure, it is possible to prevent the oxidation of the crystal grains. However, since the crystals grow in a way that increases the crystal surface area, The crystals tend to grow upward in a needle-like shape. The etching residues generated during the formation of the source and drain regions are deposited on the LPSAS layer 106. This prevents the mixing of electrical properties between elements. As a result, highly reliable thin film transistors can be manufactured with high yield.

[0110] The buffer layer 107 is formed of an amorphous semiconductor or a material containing hydrogen, nitrogen, or It is formed from an amorphous semiconductor containing halogen. Therefore, the energy gap of the amorphous semiconductor The energy gap is larger than that of microcrystalline semiconductors (the energy gap of amorphous semiconductors is 1.6 to 1. The energy gap of the electron transport material is 1.8 eV, and the energy gap of the microcrystalline semiconductor is 1.1 to 1.5 eV. It has high electrical resistance and low mobility (1 / 5 to 1 / 10 of that of microcrystalline semiconductors). In the thin film transistor to be formed, the impurity semiconductor layer 109 and the microcrystalline semiconductor layer 105 The buffer layer 107 formed between the microcrystalline semiconductor layer 1 and the buffer layer 107 functions as a high resistance region. Therefore, the buffer layer 108 functions as a channel formation region. Therefore, the off-current of the thin film transistor can be reduced. When such a thin film transistor is used as a switching element in a liquid crystal display device, The contrast of the liquid crystal display device can be improved.

[0111] When an n-type thin film transistor is formed, the impurity semiconductor layer 109 is typically an impurity. All you need to do is add phosphorus as a pure element, and the PH 3 Impurities that give one conductivity type, such as In addition, when forming a p-type thin film transistor, A typical impurity element is boron, and silicon hydride is 2 H 6 Impurity gases such as The impurity semiconductor layer 109 can be formed using a microcrystalline semiconductor or an amorphous semiconductor. The impurity semiconductor layer 109 is formed to a thickness of 2 nm to 50 nm. It is preferable that the thickness of the impurity semiconductor layer 109 is approximately the same as that of the LPSAS layer 106. By forming a thin film, the throughput can be improved.

[0112] In the present invention, as described above, the first insulating layer 104 to the impurity semiconductor layer 109 are continuously formed. It is preferable to deposit these layers successively. The microwave plasma CVD method will now be described with reference to FIG. Not only the microwave plasma CVD method but also the high frequency plasma CVD method may be applied. FIG. 1 is a schematic diagram showing a cross section of a microwave plasma CVD apparatus. 10, a load chamber 200, an unload chamber 205, a first reaction chamber 201 to a fourth reaction chamber 202, The common chamber 210 is provided with a gate valve 212 to each chamber. 217, and the processes in each chamber are configured so as not to interfere with each other. The plate 220 is mounted in the cassette 218 and the cassette 219 in the load chamber 200 and the unload chamber 205. The first reaction chamber 201 to the fourth reaction chamber 204 are filled with the liquid, and the liquid is transferred to the first reaction chamber 201 to the fourth reaction chamber 204 by the transfer means 211 of the common chamber 210. In this system, a reaction chamber can be assigned to each deposition type, and multiple Different films can be formed in succession without exposure to the atmosphere.

[0113] In each of the first reaction chamber 201 to the fourth reaction chamber 204, a first insulating layer 104, A microcrystalline semiconductor layer 105, a buffer layer 107, and an impurity semiconductor layer 109 are stacked. In this case, by switching the source gas, multiple layers of different types can be continuously laminated. In this case, after the first insulating layer 104 is formed, silane or the like is added to the reaction chamber. silicon hydride is introduced, the residual oxygen and silicon hydride are reacted, and the reactant is discharged outside the reaction chamber. As a result, the concentration of residual oxygen in the reaction chamber can be reduced. In addition, the concentration of oxygen contained in the microcrystalline semiconductor layer 105 can be reduced. This can prevent oxidation of the crystal grains.

[0114] Alternatively, the insulating layer 104 in the first reaction chamber 201 and the third reaction chamber 203 may be formed by the insulating layer 104. A layer, a microcrystalline semiconductor layer, and an amorphous semiconductor layer are formed in the second reaction chamber 202 and the fourth reaction chamber In step 204, the impurity semiconductor layer 109 is formed. Only the impurity semiconductor layer 109 is formed. As a result, impurity elements that impart one conductivity type remaining in the chamber are mixed into other layers. This can be prevented.

[0115] As shown in Figure 6, a microwave plasma CVD device with multiple chambers connected is used. Thus, the first insulating layer 104, the microcrystalline semiconductor layer 105, the buffer layer 107, and the impurity semiconductor The layer 109 can be continuously formed, and mass production (productivity) can be improved. Even if one reaction chamber is undergoing maintenance or cleaning, the remaining reaction chambers can be used. This allows for film formation in a short time, improving the tact time of film formation. The interfaces of the layers can be formed without being contaminated by impurity elements that can be a source of contamination. Therefore, the variation in the electrical characteristics of the thin film transistors can be reduced.

[0116] In addition, the first insulating layer 104 is formed in the first reaction chamber 201 and then finely sintered in the second reaction chamber 202. The crystalline semiconductor layer 105 and the buffer layer 107 are formed, and the impurity semiconductor layer is formed in the third reaction chamber 203. In addition, since the deposition rate of the microcrystalline semiconductor layer is slow, a plurality of anti-reflection films can be formed. For example, a microcrystalline semiconductor layer may be formed in the first reaction chamber 201. The edge layer 104 is formed, and the microcrystalline semiconductor layer 10 is grown in the second reaction chamber 202 and the third reaction chamber 203. 5, a buffer layer 107 is formed in the fourth reaction chamber 204, and a fifth reaction chamber (not shown) is formed in the fifth reaction chamber 205. In this manner, the impurity semiconductor layer 110 may be formed by simultaneously using a plurality of reaction chambers. By forming a microcrystalline semiconductor layer on the substrate, throughput can be improved. Preferably, the interior walls of each reaction chamber are coated with a layer of the type to be deposited.

[0117] By using the microwave plasma CVD apparatus with the configuration shown in Figure 6, the composition of each reaction chamber can be varied. It is possible to deposit similar layers or a single type of layer, and the layers can be deposited successively without exposure to the atmosphere. Therefore, the interface is free from residues of previously formed layers and impurity elements floating in the air. A laminated film can be formed without being contaminated.

[0118] The microwave plasma CVD apparatus shown in FIG. 6 has separate load and unload chambers. These may be integrated into one room to form a load / unload room. In addition, a spare chamber may be provided in the microwave plasma CVD apparatus. This allows the heating time for each reaction chamber to be shortened, making it possible to This can improve the investment.

[0119] Next, the film forming process will be described. The film forming process is carried out by using gas supplied from a gas supply unit according to the purpose. Select the gas to be supplied.

[0120] Here, the first insulating layer 104 is formed in a two-layer structure by laminating layers. A silicon nitride oxide layer is formed as the insulating layer 104, and a silicon oxynitride layer is formed on the silicon nitride oxide layer. The method of forming the film will be described as an example.

[0121] First, the inside of the processing vessel of the reaction chamber of the microwave plasma CVD device is heated with fluorine radicals. The introduction of fluorine radicals was performed using a plasma Carbon fluoride, nitrogen fluoride or fluorine is introduced into the generator, dissociated, and introduced into the reaction chamber. The introduction of fluorine radicals enables cleaning of the inside of the reaction chamber. .

[0122] After cleaning with fluorine radicals, a large amount of hydrogen is introduced into the reaction chamber. The concentration of residual fluorine in the reaction chamber can be reduced by reacting the residual fluorine with hydrogen. This makes it possible to reduce the amount of fluorine that gets mixed into the protective layer that is later formed on the inner wall of the reaction chamber. Therefore, the thickness of the protective layer can be reduced.

[0123] Next, a silicon oxynitride layer is deposited as a protective layer on the surface of the inner wall of the processing vessel of the reaction chamber. In this case, the pressure in the treatment vessel is set to 1 Pa or more and 200 Pa or less, preferably 1 Pa or more and 100 Pa or less. a or less, and the gases used for plasma ignition are helium, argon, xenon and crypto In addition to the rare gases, hydrogen or other rare gases may be introduced. In particular, it is preferable to use helium gas as the gas for plasma ignition. It is more preferable to use a mixed gas of helium and hydrogen.

[0124] Helium has a high ionization energy of 24.5 eV, but has a metastable state at about 20 eV. Therefore, ionization is possible at about 4 eV during discharge. The discharge is low and easy to maintain. Therefore, the generated plasma can be maintained uniformly. This enables power saving.

[0125] In addition, oxygen gas may be introduced as a gas for plasma ignition. By introducing oxygen gas into the processing chamber, plasma can be easily ignited.

[0126] Next, turn on the microwave generator and set the output of the microwave generator to 500 W or more. The plasma is generated at a power of 4000 W or more and 6000 W or less, preferably 4000 W or more and 6000 W or less. Next, the source gas is introduced into the processing vessel through the gas pipe. By introducing silane, nitrous oxide and ammonia, the inner walls of the processing vessel, gas pipes, dielectric A silicon oxynitride layer is formed as a protective layer on the surface of the substrate and the support table. Nitrogen may be introduced instead of ammonia. The thickness of the protective layer is 500 to 2000 nm. The mixture is formed so that the

[0127] Next, the supply of the raw material gas is stopped, the pressure in the processing vessel is reduced, and the microwave generating device is turned on. After the power is turned off, the substrate is placed on the support table in the processing chamber.

[0128] Next, a nitride oxide film is formed on the substrate as the first insulating layer 104 by the same process as the protective layer described above. A silicon layer is deposited.

[0129] After the silicon oxynitride layer is deposited to a desired thickness, the supply of the source gas is stopped, and the inside of the processing vessel is degassed. The pressure is released and the microwave is turned off.

[0130] Next, the pressure in the treatment vessel is increased to 1 Pa or more and 200 Pa or less, preferably 1 Pa or more and 100 Pa or less. a or less, and the plasma ignition gases are helium, argon, xenon and krypton. The raw material gases dinitrogen monoxide, rare gas and silane are introduced. Next, turn on the microwave generator and set the output of the microwave generator to 50. The plasma is generated at a power of 0 W or more and 6000 W or less, preferably at a power of 4000 W or more and 6000 W or less. Next, the source gas is introduced into the processing vessel from the gas pipe, and the source gas is deposited on the silicon oxynitride film of the substrate. A silicon oxynitride layer is formed. Next, the supply of the source gas is stopped, and the pressure in the processing vessel is reduced. Then, the microwave generator is turned off to finish the film formation process.

[0131] Through the above steps, the protective layer on the inner wall of the reaction chamber is made into a silicon nitride oxide layer, and silicon nitride oxide is deposited on the substrate. By successively forming the silicon oxynitride layer and the silicon oxide nitride layer, impurities in the upper silicon oxide nitride layer are prevented from being mixed. It is possible to reduce the contamination of elements. By depositing these layers using the microwave plasma CVD method, the plasma density was increased to Therefore, a film with high pressure resistance can be formed. When the layer is used as a gate insulating layer of a thin film transistor, the variation in the threshold voltage of the thin film transistor is It is also possible to reduce adhesion. In addition, the resistance to static electricity is improved, It is possible to fabricate a transistor that is not easily destroyed even when a high voltage is applied. It is possible to fabricate thin film transistors that are less susceptible to damage during hot carrier application. Therefore, it is possible to fabricate a transistor with less defects.

[0132] The first insulating layer 104 is made of an oxynitride film formed by a microwave plasma CVD method. When the silicon layer is a single layer, the above-mentioned method for forming a protective layer and the method for forming a silicon oxynitride layer are used. In particular, the flow ratio of nitrous oxide to silane is set to 100 to 300, preferably When the thickness is set to 150 times or more and 250 times or less, a silicon oxynitride layer with high voltage resistance can be formed. do.

[0133] Next, a microcrystalline semiconductor layer and a buffer layer are formed by a microwave plasma CVD method. A method for successively forming a thin film of a semiconductor layer and an amorphous semiconductor layer that functions as a gate insulating film will be described. The inside of the reaction chamber is cleaned in the same manner as in the formation of the insulating layer. Next, a protective layer and The silicon layer is deposited by depositing an amorphous semiconductor layer having a thickness of 0.2 μm to 0.4 μm. Here, the pressure in the processing vessel is set to 1 Pa or more and 200 Pa or less, preferably The pressure is between 1 Pa and 100 Pa, and the gas for plasma ignition is helium, argon, At least one of rare gases such as xenon and krypton is introduced. Hydrogen may be introduced.

[0134] Next, turn on the microwave generator and set the output to 500W or more. The plasma is generated at a power of 4000 to 6000 W or less, preferably 4000 to 6000 W. Next, the source gas is introduced into the processing vessel through the gas pipe. By introducing silicon hydride gas and hydrogen gas, the inner wall of the processing vessel, the gas pipe, the dielectric plate and the support are A microcrystalline silicon layer is formed as a protective layer on the surface of the holder. Silicon hydride gas and hydrogen gas are also used. and one or more rare gas elements selected from helium, argon, krypton, and neon. The silicon hydride can be diluted with hydrogen to form a microcrystalline semiconductor layer. The flow rate ratio is 5 times or more and 200 times or less, preferably 50 times or more and 150 times or less, and more preferably The thickness of the protective layer is 500 nm or more and 2000 nm or less. Before turning on the microwave generator, the above-mentioned rare gases and other gases are added to the processing vessel. Alternatively, silicon hydride gas and hydrogen gas may be introduced.

[0135] The silicon hydride gas is selected from the group consisting of helium, argon, krypton and neon. and diluting the semiconductor layer with one or more rare gas elements to form an amorphous semiconductor layer as a protective layer. can.

[0136] Next, the supply of the raw material gas is stopped, the pressure in the processing vessel is reduced, and the power of the microwave generator is turned on. After the source is turned off, the substrate is introduced onto the support stage within the processing vessel.

[0137] Next, the surface of the first insulating layer 104, which functions as a gate insulating layer and is formed on the substrate, is immersed in water. By performing hydrogen plasma treatment before forming a microcrystalline semiconductor layer, Reducing lattice distortion at the interface between the first insulating layer 104 and the LPSAS layer 106 It is possible to improve the interface properties between the first insulating layer 104 and the LPSAS layer 106. As a result, the electrical characteristics of the thin film transistor formed can be improved.

[0138] In the hydrogen plasma treatment, the amorphous protective layer formed in the treatment chamber is The semiconductor layer or the microcrystalline semiconductor layer is also subjected to hydrogen plasma treatment, so that the protective layer is etched. A small amount of semiconductor is deposited on the surface of the first insulating layer 104. This becomes the nucleus for crystal growth and a microcrystalline semiconductor layer is formed. As a result, the first insulating layer 104 and the L It is possible to reduce the lattice distortion at the interface with the PSAS layer 106, and the first insulating layer 1 The interface properties between the SiO2 layer 04 and the LPSAS layer 106 can be improved. The electrical characteristics of the thin film transistor can be improved.

[0139] Next, a microcrystalline semiconductor is deposited on the substrate in the same manner as the above-mentioned protective layer. The film thickness is set to 2 nm or more and 50 nm or less, preferably 10 nm or more and 30 nm or less. Silicon is used as the crystalline semiconductor.

[0140] Note that the crystal growth of the microcrystalline semiconductor layer is from the bottom to the top of the layer, and needle-like crystals are formed. This is because the crystal grows so that the crystal face becomes larger. Even when the microcrystalline semiconductor layer grows, the rate at which the microcrystalline semiconductor layer is formed is faster than the rate at which the amorphous semiconductor layer is formed. The speed is between 1% and 10% of the actual speed.

[0141] After the microcrystalline semiconductor layer is deposited to a desired thickness, the supply of the source gas is stopped, and the processing vessel is The pressure inside the chamber was reduced, the microwave generator was turned off, and the deposition process of the microcrystalline semiconductor layer was started. End the process.

[0142] Next, the microcrystalline semiconductor layer is irradiated with laser light from the surface side of the microcrystalline semiconductor layer. The following explains this.

[0143] In the formation of the microcrystalline semiconductor layer in the present invention, after depositing the microcrystalline semiconductor layer on the gate insulating layer, Preferably, the surface side of the microcrystalline semiconductor layer is irradiated with laser light. That is, the LP process of the present invention is performed by irradiating the silicon layer with an energy density that does not melt the silicon layer. The principle is to grow the semi-amorphous silicon layer in a solid phase without melting it by radiative heating. That is, the deposited semi-amorphous silicon layer does not become liquid. This utilizes the boundary region, and in that sense it can also be called "critical growth."

[0144] The above laser light is allowed to act on the interface between the semi-amorphous silicon layer and the gate insulating layer. As a result, the crystals on the surface side of the semi-amorphous silicon layer can be used as nuclei. Then, solid phase crystal growth proceeds from the surface toward the interface with the gate insulating layer, and approximately columnar crystals grow. The solid-phase crystal growth by LP treatment does not increase the grain size, but increases the thickness of the layer. Improves the crystallinity in the

[0145] The above LP process is performed by concentrating the light into a long rectangular shape (forming it into a linear laser beam), for example, A semi-amorphous silicon layer on a 30mm x 920mm glass substrate was laser-beam-deposited in one go. This can be done by processing the image with a MUSCANN. In this case, the linear laser beams are overlapped. The overlap rate is set to 0 to 90%, preferably 0 to 67%. This reduces the processing time per substrate and improves productivity. The shape of the laser beam is not limited to a linear shape, and a planar shape can also be used for processing. In addition, the LP process is not limited to the size of the glass substrate, and can be used with substrates of various sizes. By performing the LP treatment, the interface between the microcrystalline semiconductor layer and the gate insulating layer can be The crystallinity of the region is improved, improving the electrical characteristics of transistors with a bottom gate structure. Can.

[0146] This "critical growth" technique eliminates the surface irregularities ( No convex structures called ridges are formed, and the silicon surface remains smooth after LP processing. .

[0147] Therefore, the laser beam is directly applied to the semi-amorphous silicon layer after deposition. The LPSAS layer of the present invention is different from the conventional microcrystalline silicon layer that is simply deposited. A microcrystalline silicon layer that has been modified by conductive heating after deposition (see Non-Patent Document 1) is The growth mechanism and the film quality of the layer formed are obviously different.

[0148] After forming the LPSAS layer, the amorphous semiconductor layer was heated at 300°C or higher for 4 hours by plasma CVD. The film is formed at a temperature of 00°C or less. This film formation process supplies hydrogen to the LPSAS layer, The effect is the same as that of hydrogenating the PSAS layer. By depositing an amorphous semiconductor layer, hydrogen is diffused into the LPSAS layer to form dangling bonds. It is possible to terminate the

[0149] Next, the pressure in the processing vessel is lowered and the flow rate of the source gas is adjusted. The flow rate is significantly reduced from the film formation conditions of the microcrystalline semiconductor layer. 1 to 20 times, preferably 1 to 10 times, more preferably 1 to 5 times Alternatively, hydrogen gas is not introduced into the processing vessel, and silicon hydride gas is introduced. By reducing the flow rate of hydrogen relative to the silicon hydride in this manner, The deposition rate of the amorphous semiconductor layer formed as the buffer layer can be improved. The silicon hydride gas is selected from the group consisting of helium, argon, krypton and neon. The microwave generator is then turned on and the microwave is The output of the microwave generator should be between 500W and 6000W, preferably between 4000W and 6000W. The amorphous semiconductor layer can be formed by generating plasma at a concentration of 1000 .mu.m or less. Since the deposition rate of conductors is higher than that of microcrystalline semiconductors, the pressure in the processing vessel should be set low. In this case, the thickness of the amorphous semiconductor layer is set to 100 nm or more and 400 nm or less.

[0150] After the amorphous semiconductor layer is deposited to a desired thickness, the supply of the source gas is stopped and the inside of the processing chamber is The pressure in the chamber is reduced, the microwave generator is turned off, and the deposition process of the amorphous semiconductor layer is started. Exit the process.

[0151] Note that the microcrystalline semiconductor layer 105 and the amorphous semiconductor layer to be the buffer layer 107 are irradiated with plasma. Specifically, the flow rate ratio of hydrogen to silicon hydride is gradually decreased. The microcrystalline semiconductor layer 105 and the amorphous semiconductor layer which becomes the buffer layer 107 are stacked. By such a method, impurities are formed at the interface between the microcrystalline semiconductor layer 105 and the buffer layer 107. This allows the formation of an interface with little distortion, and the thin film transistor that will be formed later The electrical characteristics of the transistor can be improved.

[0152] The plasma generated by microwave plasma CVD equipment with a frequency of 1 GHz or more is electron-dense. Since the concentration is high, many radicals are generated from the source gas and supplied to the substrate 220. The radical reaction on the surface is promoted, and the film formation speed of the microcrystalline semiconductor can be increased. A microwave plasma CVD apparatus comprising a plurality of microwave generators and a plurality of dielectric plates. The device can stably generate plasma over a large area. It is possible to form a layer having a high uniformity in terms of film quality even in mass production. This can increase productivity.

[0153] In addition, a microcrystalline semiconductor layer and an amorphous semiconductor layer are successively formed in the same processing vessel. It is possible to form an interface with little distortion and to reduce atmospheric components that may be mixed into the interface. This is preferable because it is possible to

[0154] In the respective processes for forming the insulating layer and the semiconductor layer, the inner wall of the reaction chamber is heated to 50 If a protective layer with a thickness of 0 nm or more and 2000 nm or less is formed, the above cleaning process In addition, the step of forming a protective layer can be omitted.

[0155] Next, a resist mask 140 is formed (see FIG. 4(A)). is a mask having multiple regions of different thicknesses, and is used in photolithography using a multi-tone mask. The film is formed by a lithography technique or an inkjet method.

[0156] Next, the microcrystalline semiconductor layer, the amorphous semiconductor layer, and the impurity semiconductor layer are formed using a resist mask 140. Etching is performed in a state where the layer and the conductive layer are formed. 05, the buffer layer 107, the impurity semiconductor layer 109, and the conductive layer 111 are separated for each element (FIG. 4(B)).

[0157] In this etching process, the microcrystalline semiconductor layer, the amorphous semiconductor layer, and the impurity semiconductor layer The etching is performed so that the end of the laminated layer has a tapered shape. The taper angle is 3 The angle is 0° to 90°, preferably 40° to 80°. The end has a tapered shape. By performing etching so as to form the impurity semiconductor layer 109 and the microcrystalline semiconductor layer 105, Not only can it be prevented that the layers are in direct contact with each other, but also the distance between these layers at the ends can be reduced. Therefore, the leakage current at the end portion can be reduced.

[0158] In addition, by making the ends tapered, the covering of the layer formed on them in the subsequent process can be improved. Therefore, it is possible to prevent the wiring from being broken at the step. .

[0159] The taper angle is the angle θ shown in FIG. 7. FIG. 7 shows a substrate 190 having a tapered end. A layer 191 having a taper shape is formed. The layer 191 has a taper angle of θ.

[0160] Next, a resist mask 142 is formed over the conductive layer 111 (see FIG. 4C). The resist mask 142 is formed by ashing the resist mask 140 with oxygen plasma or the like. It can be formed by carrying out the above steps.

[0161] The conductive layer 111 is made of aluminum, copper, silicon, titanium, neodymium, scandium, etc. Elements that improve heat resistance, such as tungsten, molybdenum, chromium, tantalum, or tungsten Or an aluminum alloy containing an element for preventing hillocks (used for the first conductive layer 102) It is formed in a single layer or multilayer using an impurity that gives one conductivity type. Crystalline silicon doped with an impurity that gives one conductivity type may be used. The layer on the side in contact with the semiconductor layer is made of titanium, tantalum, molybdenum, tungsten or A multilayer structure is formed by forming a nitride of these elements and forming aluminum or an aluminum alloy on it. The upper and lower surfaces of the aluminum or aluminum alloy may be laminated. Layered structure sandwiched between tantalum, molybdenum, tungsten or nitrides of these elements For example, a three-layer structure in which an aluminum layer is sandwiched between molybdenum layers may be used as the conductive layer. It is preferable to use this structure.

[0162] The conductive layer 111 is formed by a sputtering method, a vacuum deposition method, or the like. 111 is printed by screen printing or inkjet printing using conductive nanopaste such as silver, gold, or copper. It may be formed by discharging using a jet method or the like and baking.

[0163] The resist mask 142 is ash-treated with oxygen plasma or the like on the resist mask 140. The formation of the void can be achieved by performing a void forming process.

[0164] Next, the conductive layer 111 is etched using the resist mask 142 to form a conductive layer 111. Next, a resist mask 142 is used to dope the semiconductor substrate 100 with an impurity that provides one conductivity type. The impurity semiconductor layer 109 and the buffer layer 107 are etched to form a source region and The impurity semiconductor layer 110 constituting the drain region and the buffer layer 108 are formed (see FIG. 5(A)). Note that the buffer layer 108 is only partially etched. It covers the surface of the LPSAS layer 106. Also, as is clear from FIG. The ends of the source and drain regions formed by the semiconductor layer 110 and the patterned The end of the conductive layer 111 is substantially aligned with the end of the conductive layer 111 .

[0165] Next, a part of the conductive layer 111 is further etched while leaving the resist mask 142. The second conductive layer 112 is formed by forming a source electrode or a drain electrode. The conductive layer 111 functions as an inner electrode. Here, the conductive layer 111 is wet-etched using a mask. The ends of the conductive layers 111 are selectively etched by wet etching. As a result, the conductive layer is isotropically etched, and the area of ​​the conductive layer is larger than that of the resist mask 142. A small second conductive layer 112 can be formed. The end of the second conductive layer 112 and the impurity The impurity semiconductor layer 110 is disposed outside the end of the second conductive layer 112. The end of the conductive layer 110 is formed (see FIG. 5(B)). The second conductive layer 112 functioning as a source electrode and a drain electrode is removed. It also functions as a route.

[0166] The end of the second conductive layer 112 and the end of the impurity semiconductor layer 110 do not coincide with each other. As a result, the distance between the ends of the second conductive layer 112 becomes large, and the source electrode or the drain electrode By making the distance between one of the electrodes and the other of the source electrode or drain electrode sufficiently large, This reduces the leakage current and prevents short circuits. The buffer layer 108 between the first conductive layer 102 and the second conductive layer 112 The distance between the MOSFET and the MOSFET is sufficiently large. This suppresses the occurrence of parasitic capacitance and reduces leakage current. This allows the fabrication of thin-film transistors that are highly reliable, have small off-currents, and have high withstand voltages. It can be manufactured.

[0167] By the above steps, the channel-etch type thin film transistor of the present invention can be formed. Cut.

[0168] The thin film transistor shown in this embodiment has a first conductive layer 10 functioning as a gate electrode. A first insulating layer 104 that functions as a gate insulating layer is formed on the first insulating layer 102, and a second insulating layer 104 that functions as a channel forming region is formed on the second insulating layer 102. the LPSAS layer 106, the buffer layer 108, and the impurity semiconductor layer 109 which will become the source and drain regions; A conductor layer 110 and a second conductive layer 112 functioning as a source electrode and a drain electrode are laminated. The surface of the LPSAS layer 106 which functions as a channel forming region is a buffer. It is covered with a layer 108 .

[0169] The LPSAS layer 106 functions as a channel forming region, and the impurity element 107 provides one conductivity type. A buffer layer 108 is provided between the impurity semiconductor layer 110 to which silicon is added, and the LPSAS The surface of the layer 106 is covered with a buffer layer 108. The buffer layer 108 is formed of an amorphous semiconductor layer or the like having a higher electrical resistance than the microcrystalline semiconductor layer. The buffer layer 108 is formed of the LPSAS layer 106 and the second conductive layer 112. Therefore, it is possible to reduce the leakage current generated in the thin film transistor. Not only can this be achieved, but it also prevents the thin film transistor from deteriorating due to the application of high voltage. The buffer layer 108 can also etch the surface of the LPSAS layer 106 with hydrogen. Therefore, the LPSAS layer 106 is covered with an amorphous semiconductor layer terminated with a SiO 2 . Furthermore, it is possible to prevent the etch that occurs when forming the impurity semiconductor layer 110. Therefore, the present invention can prevent the mixing of the coating residue into the LPSAS layer 106. The thin film transistors used in the present invention have high electrical characteristics and excellent voltage resistance. become.

[0170] In addition, a portion of the buffer layer 108 has a recess (groove), and the region other than the recess serves as a source region. The buffer layer 108 is covered with an impurity semiconductor layer 110 which is to become the source and drain regions. The recess formed ensures that the leakage path between the source and drain regions is long enough. Therefore, the leakage current between the source region and the drain region can be reduced. In addition, by etching a portion of the buffer layer 108 so as to have a recess, the source region Etching that occurs in the process of forming the impurity semiconductor layer 110 that will become the drain and upper regions. The residues can be easily removed. Therefore, the source region and The leakage current that may occur in the drain region can be reduced. The recesses 8 are formed in the step of forming the impurity semiconductor layer 110 which will become the source and drain regions. Therefore, the side surfaces of the source and drain regions are formed by the buffer layer. It is provided so as to be approximately flush with the side surface of the recess of 108 .

[0171] When the LPSAS layer 106 is oxidized, the mobility of the thin film transistor decreases, and the sub- The threshold value increases, which deteriorates the electrical characteristics of the thin film transistor. Since hydrogen and fluorine are mixed in the buffer layer 108, oxygen does not enter the buffer layer 108. 08, and oxidation of the LPSAS layer 106 can be prevented.

[0172] Furthermore, by providing the buffer layer 108, the occurrence of a parasitic channel can be prevented. .

[0173] In addition, the ends of the source electrode and the drain electrode and the ends of the source region and the drain region are The mismatched shapes may cause one end of the source or drain electrode to overlap with the other end of the source or drain electrode. Since the drain electrode has a sufficient distance between the source electrode and the other end of the drain electrode, The leakage current between one of the electrodes and the other of the source electrode or the drain electrode is reduced, and the This can prevent short circuits.

[0174] In addition, in the above-mentioned FIGS. 5(A) and 5(B), the buffer layer has a recess (groove) in a part thereof. After forming 108, a sufficiently large distance is provided between the end of the source electrode and the end of the drain electrode. However, the present invention is not limited to this example. The conductive layer that will become the conductive layer 112 of the second insulating layer is etched and separated to expose the impurity semiconductor layer 110. After that, one end of the source electrode or the drain electrode and the other end of the source electrode or the drain electrode are Then, etching may be performed to increase the distance between the edge of the semiconductor layer and the The conductor layer is etched to separate the source and drain regions, and a buffer layer is then formed. A recess (groove) may be formed in a part of 108. The distance between one end of the in-electrode and the other end of the source or drain electrode is increased. After the etching, the mask is removed and the second conductive layer 112 is used as a mask. The etching may be performed by

[0175] The end portions of the impurity semiconductor layer 110, which is the source region and the drain region, and the buffer layer The edges of the recess formed in 108 coincide (see FIG. 1). This is because the recess is This is because they are formed in the same process as when etching the compound semiconductor layer 110. .

[0176] Next, as shown in FIG. 5C, the second conductive layer 112, the impurity semiconductor layer 110, and the LPS A second insulating layer 114 is formed on the AS layer 106 and the first insulating layer 104. The edge layer 114 can be formed in the same manner as the first insulating layer 104. 114 is a measure of the amount of impurity elements that can be a source of contamination, such as organic matter, metals, and water vapor, suspended in the air. Since the purpose of the buffer layer 1 is to prevent the intrusion of oxygen, it is preferable to form the buffer layer 1 densely. The carbon, nitrogen, and oxygen concentrations in 08 are 1×10 19 cm -3 Below, and further 5×10 18 cm - 3 It is preferable that:

[0177] Next, a first opening 118 and a second opening 120 are formed in the second insulating layer 114, and The third conductive layer 116 is formed in the first opening 118. 1 and 2, and is connected to the first conductive layer 102 at the second opening 120. The third conductive layer 116 is formed on the entire surface, similar to the second conductive layer 112, and then is formed by a resist. The third conductive layer 116 may be patterned using a photomask or the like. It is preferable that the third conductive layer 116 is formed at the same time as the pixel electrode to be formed. A case where the electrode is formed in the same layer as the electrode will be described.

[0178] The third conductive layer 116 is made of indium oxide with tungsten oxide, tungsten oxide Indium zinc oxide containing titanium oxide, indium oxide containing titanium oxide Indium tin oxide, indium tin oxide (hereinafter referred to as ITO), indium zinc oxide A conductive material having light-transmitting properties, such as indium tin oxide doped with silicon oxide, is used. can be done.

[0179] The third conductive layer 116 may be made of a material containing a conductive polymer. The third conductive layer formed using the conductive composition can be formed using the conductive composition. The layer 116 has a sheet resistance of 10000 Ω / □ or less and is transparent at a wavelength of 550 nm. It is preferable that the light efficiency is 70% or more. It is preferable that the sheet resistance is lower. The resistivity of the conductive polymer contained in the conductive composition is preferably 0.1 Ω·cm or less. It is.

[0180] As the conductive polymer, a so-called π-electron conjugated conductive polymer can be used. For example, polyaniline or its derivatives, polypyrrole or its derivatives, poly Examples of the material include thiophene or a derivative thereof, and a copolymer of two or more of these.

[0181] The above description has been given of the case where the third conductive layer 116 is formed in the same layer as the pixel electrode. However, the present invention is not limited thereto. The third conductive layer 116 is a first conductive layer 102 and a second conductive layer 103. The conductive layer 112 may be formed using the same material and method as the conductive layer 112. The thin film transistor used in the protection circuit of the present invention is the same as the thin film transistor used in the pixel circuit. They are formed on the same substrate by the same process. The material is used to form a pixel electrode that is connected to a thin film transistor used in a pixel circuit. By forming them simultaneously, the number of manufacturing steps can be reduced and the yield can be improved. Cut.

[0182] Also, as shown in FIG. 1, the third conductive layer 116 connects the first conductive layer 102 and the second conductive layer 116. The diode used in the protection circuit of the present invention is formed by diode-connecting the conductive layer 112. A connected thin film transistor (protection diode) can be formed.

[0183] In the above description, the gate electrode and the scanning line are formed in the same process, and the source electrode or The above description is directed to a case where the drain electrode and the signal line are formed in the same process. The electrodes and the wiring connected to the electrodes may be formed in separate steps.

[0184] In this embodiment, the LPSAS layer 106 is provided. In the thin-film transistor, instead of the LPSAS layer, a microcrystalline A semiconductor layer may be included.

[0185] Through the above steps, a channel-etch type thin film transistor can be formed. The channel-etch type thin film transistor requires fewer manufacturing steps and can reduce costs. In addition, by forming a channel formation region using a microcrystalline semiconductor layer, the 2 / V Therefore, the field effect mobility of this thin film transistor can be obtained by using the pixel As a switching element for the pixel, a driving circuit for the scanning line (gate line) is further formed. It can be used as an element.

[0186] As described in this embodiment, a thin film transistor having good electrical characteristics and high reliability is obtained. A thin film transistor can be fabricated. By providing a protection circuit, the electric charge on the interlayer insulation layer, etc. is discharged, and the signal or power supply voltage is In addition, it is possible to reduce noise input to the wiring and prevent deterioration or destruction of the semiconductor element. Therefore, it is possible to provide a protection circuit with a higher withstand voltage and smaller parasitic capacitance than conventional circuits. In the conventional protection circuit, when a large current or a high voltage flows that is large enough to destroy the protection circuit itself, Even if a voltage is applied, the protection circuit described in this embodiment can be provided to prevent the semiconductor device from being damaged. It is possible to effectively prevent damage to the conductive elements and manufacture a display device with higher reliability.

[0187] In this embodiment, a multi-tone mask is used to form the mask. Of course, it is also possible to form a thin film transistor without using a mask.

[0188] (Embodiment 2) In this embodiment mode, a liquid crystal display having a protection circuit using the thin film transistor described in Embodiment 1 is A liquid crystal display device will now be described.

[0189] First, about VA (Vertical Alignment) type LCD devices The VA method is a method in which the liquid crystal molecules are perpendicular to the panel surface when no voltage is applied. In this embodiment, the pixels are divided into several regions ( The molecules are divided into subpixels, and each subpixel is designed to fall in a different direction. This is called multi-domain or multi-domain design. In the following explanation, A liquid crystal display device with a unique design will now be described.

[0190] FIG. 9 is a plan view of the substrate side on which pixel electrodes are formed, and corresponds to the cutting line AB in FIG. FIG. 8 shows a cross-sectional structure of the device. FIG. 10 is a plan view of the substrate on which the counter electrode is formed. The following description makes reference to these drawings.

[0191] FIG. 8 shows a state in which the substrate 300 and the opposing substrate 301 are opposed to each other and liquid crystal is injected. On the substrate 300, a thin film transistor 328 and a The pixel electrode 324 and the storage capacitor 330 are disposed on the substrate 301. do.

[0192] In the position where the spacer 342 is to be formed on the substrate 301, a light-shielding layer 332 and a first colored The colored layer 334, the second colored layer 336, the third colored layer 338, and the counter electrode 340. By adopting this structure, the height of the protrusions 344 for controlling the alignment of the liquid crystal and the spacers 342 The pixel electrode 324 has an alignment layer 348 on it, and the counter electrode 340 has a height different from that of the pixel electrode 324. On top of that is an alignment layer 346. A liquid crystal layer 350 is disposed between the alignment layer 346 and the alignment layer 348. can be done.

[0193] In FIG. 8, a post spacer (columnar spacer) is used as the spacer 342. The spacer is not limited to this. Bead spacers (spherical spacers) may be scattered as spacers. The spacer 342 may be provided on the pixel electrode 324 of the substrate 300.

[0194] On the substrate 300, a thin film transistor 328 and a pixel connected to the thin film transistor 328 are provided. The pixel electrode 324 and the wiring 318 are connected to each other through an insulating layer. 320 and an opening 323 through the insulating layer 322. The insulating layer 320 is The thin film transistor 328, the wiring 318, and the storage capacitor 330 are provided so as to cover the thin film transistor 328, the wiring 318, and the storage capacitor 330. The insulating layer 322 is provided to cover the insulating layer 320. The thin film transistor functions as a protection diode as described in the first embodiment. The storage capacitor 330 may be a thin film transistor. A conductive layer formed in the same process as the gate electrode and scanning line of the thin film transistor 328 is formed. A conductive layer is formed in the same process as the source electrode and signal line of the stator 328, and a thin film is formed. It is constructed by sandwiching the gate insulating layer of transistor 328 .

[0195] A pixel electrode 324 having an alignment layer 348, a liquid crystal layer 350, and a counter electrode having an alignment layer 346. The liquid crystal element is provided by overlapping with the electrode 340 .

[0196] 9 shows a plan view of the substrate 300 side. The pixel electrode 324 is the third conductor in the first embodiment. The pixel electrode 324 is formed using the same material as the conductive layer 116. The pixel electrode 324 is provided with a slit 325. The slits 325 are used to control the alignment of the liquid crystal.

[0197] FIG. 9 shows a thin film transistor 329 and a pixel electrode 3 connected to the thin film transistor 329. 26 and the storage capacitor 331 are respectively a thin film transistor 328, a pixel electrode 324, and a storage capacitor. The thin film transistor 328 and the thin film transistor The stator 329 is connected to the wiring 316. The pixel electrode 32 is composed of the pixel electrode 324 and the pixel electrode 326. The area of ​​4 and the area of ​​the pixel electrode 326 are sub-pixels.

[0198] FIG. 10 shows a plan view of the substrate 301 side. A counter electrode 340 is formed on the light-shielding layer 332. The counter electrode 340 is preferably formed using the same material as the pixel electrode 324. The counter electrode 340 has a protrusion 344 for controlling the alignment of the liquid crystal. In FIG. 10, the spacer 342 is formed in accordance with the position of the light shielding layer 332. Only the spacers 342 and the projections 344 are hatched.

[0199] An equivalent circuit of the pixel structure described above is shown in FIG. The transistor 329 is connected to the wiring 302 and the wiring 316 which both function as scanning lines. In FIG. 11, the potential of the wiring 304 functioning as a capacitance line and the potential of the wiring 305 functioning as a capacitance line are By making the potential of the wiring 305 different from that of the liquid crystal element 351, the operation of the liquid crystal element 352 can be made different. That is, the potentials of the wiring 304 and the wiring 305 can be individually controlled. This allows precise control of the alignment of the liquid crystal to achieve a wide viewing angle.

[0200] When a voltage is applied to the pixel electrode 324 having the slit 325, The slit 325 and the protrusion 34 on the substrate 301 side cause distortion of the electric field (oblique electric field). 4 and 5 are arranged so that they interdigitate with each other, effectively generating a diagonal electric field and distributing the liquid crystal. Since the orientation can be controlled, the orientation of the liquid crystal can be varied depending on the location. In other words, by creating a multi-domain display, the viewing angle of the LCD panel is expanded.

[0201] Next, a VA type liquid crystal display device having a different configuration from the above is shown in FIG. This will be explained with reference to FIGS.

[0202] FIG. 13 is a plan view of the substrate on which pixel electrodes are formed, and a cut line CD in FIG. The corresponding cross-sectional structure is shown in FIG. 12. Also, FIG. 14 is a plan view of the substrate side on which the counter electrode is formed. The following description will make reference to these drawings.

[0203] In the pixel structure of the liquid crystal display device shown in FIGS. 12 to 15, one pixel has a plurality of pixel electrodes. A thin film transistor is connected to each pixel electrode. Each thin-film transistor is driven by a different gate signal. That is, the signals applied to the individual pixel electrodes can be controlled independently. (See Figure 15).

[0204] The pixel electrode 424 is connected to a thin film transistor 428 through a wiring 418 in an opening 423. The pixel electrode 426 is connected to the thin film 419 through the opening 427. The gate electrode of the thin film transistor 428 is connected to the gate electrode of the thin film transistor 429. A wiring 402 functioning as a scan line is connected to a gate electrode of a thin film transistor 429. The wiring 403, which functions as a scanning line, can be supplied with different gate signals. On the other hand, the signal line is connected to a thin film transistor 428 and a thin film transistor 429. The wiring 416 is shared. A thin-film transistor similar to the thin-film transistor functioning as a protection diode described in the first embodiment. A resistor can be used as appropriate.

[0205] The thin film transistor 428 is connected to a storage capacitor 430. A storage capacitor 431 is connected to the resistor 429 .

[0206] The pixel electrode 424 and the pixel electrode 426 have different shapes and are separated by a slit 425. A pixel electrode 426 is provided so as to surround the outer side of the pixel electrode 424 that spreads in a V shape. The timing of the voltage applied to the pixel electrodes 424 and 426 is controlled by a thin film transistor. The alignment of the liquid crystal is controlled by changing the polarity of the resistor 428 and the thin film transistor 429. The equivalent circuit of this pixel structure is shown in FIG. The thin film transistor 429 is connected to a wiring 402 that functions as a scan line. The wiring 402 and the wiring 403 are connected to each other to provide different gate signals. In this way, the operation timing of the thin film transistor 428 and the thin film transistor 429 are made different from each other. It is possible.

[0207] A light-shielding layer 432, a colored layer 436, and a counter electrode 440 are formed on a substrate 401 that is an opposing substrate. In addition, a flattening layer 437 is formed between the colored layer 436 and the counter electrode 440. This prevents the alignment of the liquid crystal from being disturbed. FIG. 14 shows a plan view of the opposing substrate side. The opposing electrode 440 is The pixel 441 is shared between the pixels 441 and 442. The electrode 424 and the slit 425 on the pixel electrode 426 side are arranged so as to interdigitate with each other. This effectively generates an oblique electric field and controls the alignment of the liquid crystal. The orientation of the liquid crystal can be varied depending on the location, enabling a wide viewing angle to be achieved. can.

[0208] A pixel electrode 424 having an alignment layer 448, a liquid crystal layer 450, and a counter electrode having an alignment layer 446. The first liquid crystal element 451 is provided by overlapping with the electrode 440. A pixel electrode 426 having a layer 448, a liquid crystal layer 450, and a counter electrode 444 having an alignment layer 446. 40 overlaps with each other to provide a second liquid crystal element 452. In the pixel structure shown in FIG. 15, a first liquid crystal element 451 and a second liquid crystal element 452 are provided in one pixel. This results in a multi-domain structure.

[0209] The present invention can also be applied to a liquid crystal display device of the in-plane switching mode. This method expresses gradation by applying an electric field horizontally to the liquid crystal molecules. According to the in-plane switching method, the viewing angle can be expanded to about 180 degrees. A liquid crystal display device of the in-plane switching mode using this technique will be described below with reference to FIGS.

[0210] FIG. 16 shows a first pixel electrode 507, a thin film transistor 528, and a thin film transistor 52 The substrate 500 on which the second pixel electrode 524 connected to the substrate 8 is provided is opposed to the substrate 501. The substrate 501 includes a light-shielding layer 532, a colored layer 536, and a flattening layer 537. 537. The substrate 500 has pixel electrodes, but the substrate 501 does not have pixel electrodes. A liquid crystal layer 550 is provided between a substrate 500 and a substrate 501 .

[0211] The substrate 500 includes a first pixel electrode 507 and a capacitance line connected to the first pixel electrode 507. The thin film transistor 528 is connected to the wiring 504. 28 is the same as the thin film transistor functioning as the protection diode described in the first embodiment. The first pixel electrode 507 may be formed as described in the embodiment. The same material as that of the third conductive layer shown in FIG. 1 can be used. The first pixel electrode 507 and the wiring 504 are partitioned into a shape roughly corresponding to a pixel. has a gate insulating layer 506.

[0212] The source electrode and drain electrode of the thin film transistor 528 and the wiring 5 connected thereto 16 and a wiring 518 are formed on the gate insulating layer 506. The wiring 516 is The wiring 516 is a signal line through which a video signal is input to the device. At the same time, it is connected to the source region 510 and is connected to one of the source electrode and the drain electrode. The wiring 518 is connected to the other of the source electrode and the drain electrode, and the second pixel electrode 5 It is connected to 24.

[0213] A second insulating layer 520 is provided on the wiring 516 and the wiring 518. On the layer 520, an opening 523 is provided in the second insulating layer 520, and the wiring 518 is connected to the opening 523. The second pixel electrode 524 is formed in the same manner as in the first embodiment. The third conductive layer is formed using the same material as that of the third conductive layer described above.

[0214] As described above, the thin film transistor 528 and the thin film transistor 528 A second pixel electrode 524 is connected to the first pixel electrode 522. 07 and the second pixel electrode 524.

[0215] 17 is a plan view showing the configuration of the pixel electrode. 25 is provided. Slit 525 is for controlling the alignment of the liquid crystal. In this case, an electric field is generated between the first pixel electrode 507 and the second pixel electrode 524. A gate insulating layer 506 is provided between the base electrode 507 and the second pixel electrode 524. The thickness of the insulating layer 506 is generally 50 nm to 200 nm, and the thickness is about 2 μm to 10 μm. Since it is sufficiently thin compared to the liquid crystal layer, which is less than 1 μm, the An electric field is generated in the direction parallel to the substrate. This electric field controls the alignment of the liquid crystal. The liquid crystal molecules are rotated horizontally using an electric field in a certain direction. In this case, the liquid crystal molecules are rotated horizontally in any state. Since the screen is horizontal, there is almost no change in contrast depending on the viewing angle. In addition, the first pixel electrode 507 and the second pixel electrode 524 Since both electrodes have light transmitting properties, a high aperture ratio can be achieved.

[0216] Next, a liquid crystal display device of the in-plane switching mode, which has a different configuration from the above, is shown in FIG. 8 and 19.

[0217] 18 and 19 show the pixel structure of an IPS type liquid crystal display device. The cross-sectional structure corresponding to the cutting line GH shown in FIG. 19 is shown in FIG. The following description will be given with reference to FIG. 18 and FIG.

[0218] FIG. 18 illustrates a thin film transistor 628 and a second pixel connected to the thin film transistor 628. The figure shows a state in which a substrate 600 having an electrode 624 and a substrate 601 are opposed to each other and liquid crystal is injected. A light-shielding layer 632, a coloring layer 636, a planarizing layer 637, etc. are formed on the substrate 601. The substrate 600 has a pixel electrode, but the substrate 601 does not have a pixel electrode. A liquid crystal layer 650 is provided between the plates 601 .

[0219] The substrate 600 includes a wiring 609 serving as a common potential line and a thin film transistor 628. The line 609 is formed simultaneously with the scanning line 602 of the thin film transistor 628 in the same process. The first pixel electrode is also formed in the same process as the scanning line 602, and the The shape is compartmentalized.

[0220] A wiring 616 connected to one of the source electrode and the drain electrode of the thin film transistor 628 A wiring 618 is formed on the gate insulating layer 606. The wiring 616 is It is a signal line through which video signals are input, and it is a wiring that extends in one direction, and at the same time, it is also a source The wiring 618 is connected to the region 610 and is connected to one of the source electrode and the drain electrode. The other of the source electrode and the drain electrode is connected to the second pixel electrode 624. The thin film transistor 628 is a wiring that is connected to the protective diode described in the first embodiment. A thin film transistor similar to the thin film transistor that functions as the gate can be appropriately used. do.

[0221] A second insulating layer 620 is provided on the wiring 616 and the wiring 618. On the second insulating layer 620, an opening 623 is formed in the second insulating layer 620, and the wiring 618 is connected to the opening 623. The second pixel electrode 624 is the same as that in the first embodiment. The second conductive layer is formed using the same material as that of the third conductive layer described above. The pixel electrode 624 is disposed between the comb-shaped electrode (first pixel electrode) formed at the same time as the wiring 609. The second pixel electrode 624 is provided so that a horizontal electric field is generated. The electrodes are arranged so as to interdigitate with the comb-shaped electrodes (first pixel electrodes) formed at the same time as 609. do.

[0222] An electric field is generated between the potential applied to the second pixel electrode 624 and the potential of the wiring 609. The electric field controls the alignment of the liquid crystal. Rotate the liquid crystal molecules horizontally. In this case, the liquid crystal molecules are horizontal in any state, so the viewing angle is There is almost no change in contrast depending on the angle. Therefore, it is possible to realize a wide viewing angle. can be done.

[0223] As described above, the thin film transistor 628 and the thin film transistor 628 are connected to the substrate 600. A second pixel electrode 624 is provided to be connected to the wiring 609 and the wiring 616. The gate insulating layer 606 is provided between the gate insulating layer 606 and the capacitance electrode 615 formed at the time of the formation of the gate insulating layer 606. The capacitance electrode 615 and the second pixel electrode 624 are connected through an opening 623.

[0224] The present invention can also be applied to a TN type liquid crystal display device. The configuration of a TN type liquid crystal display device will be described below.

[0225] 20 and 21 show the pixel structure of a TN type liquid crystal display device. The cross-sectional structure corresponding to the cutting line IJ in FIG. 21 is shown in FIG. The following description will be given with reference to FIGS. 20 and 21. FIG.

[0226] The pixel electrode 724 is connected to the thin film transistor 728 through the wiring 718 via the opening 723. The wiring 716 functioning as a data line is connected to a thin film transistor 728. The thin film transistor 728 functions as a protection diode described in Embodiment 1. A thin film transistor similar to the thin film transistor can be used as appropriate.

[0227] The pixel electrode 724 is formed using the same material as the third conductive layer described in the first embodiment. do.

[0228] The substrate 701, which is the counter substrate, has a light-shielding layer 732, a colored layer 736, and a counter electrode 740. In addition, a flattening layer 737 is provided between the colored layer 736 and the counter electrode 740, and the alignment of the liquid crystal is controlled. The liquid crystal layer 750 is provided between the pixel electrode 724 and the counter electrode 740. There are.

[0229] The pixel electrode 724, the liquid crystal layer 750, and the counter electrode 740 are overlapped to form a liquid crystal pixel. A child is formed.

[0230] In addition, a colored layer that becomes a color filter or a shielding layer (black matrix) is formed on the substrate 700. In addition, the surface of the substrate 700 on which the thin film transistors and the like are provided may be different from the surface of the substrate 700 on which the thin film transistors and the like are provided. A polarizing plate is attached to the opposite surface (back surface), and a counter electrode 740 of the substrate 701 and the like are provided. A polarizing plate is attached to the opposite side (reverse side) of the film.

[0231] The counter electrode 740 can be made of the same material as the pixel electrode 724. 724, a liquid crystal layer 750, and a counter electrode 740 are overlapped to form a liquid crystal element. do.

[0232] In the drawings referred to in the above explanation, the gate electrodes and the scanning lines are formed in the same layer. Similarly, the source electrode or drain electrode and the signal line are formed from the same layer.

[0233] Through the above steps, a liquid crystal display device can be manufactured. The thin film transistor of the device functions as a protection diode as described in the first embodiment. The off-state current of the thin film transistor is the same as that of the thin film transistor. Since the liquid crystal display device described in this embodiment has a small current and high reliability of electrical characteristics, , it is possible to provide a high contrast and high visibility.

[0234] (Embodiment 3) The present invention can be applied not only to liquid crystal display devices but also to light emitting devices. Next, a manufacturing process of the light emitting device will be described with reference to FIGS. A light-emitting element that utilizes electroluminescence is used as the light-emitting element. The light-emitting element that utilizes the sense is characterized by whether the light-emitting material is an organic compound or an inorganic compound. Generally, the former are called organic EL elements and the latter are called inorganic EL elements.

[0235] In an organic EL element, electrons and positive electrodes are released from a pair of electrodes by applying a voltage to the light-emitting element. The holes are then injected into a layer containing a light-emitting organic compound, and a current is passed through them. Recombination of carriers (electrons and holes) creates an excited state in light-emitting organic compounds The light is emitted when the excited state returns to the ground state. Therefore, it is called a current-excited light-emitting element.

[0236] Inorganic EL elements are classified into dispersion type inorganic EL elements and thin film type inorganic EL elements depending on the element structure. Dispersion-type inorganic EL elements have a light-emitting layer in which particles of light-emitting material are dispersed in a binder. The emission mechanism is a donor-acceptor mechanism that utilizes the donor and acceptor levels. Thin-film inorganic EL elements are made by sandwiching a light-emitting layer between dielectric layers, The light emission mechanism is localized light emission that utilizes the inner-shell electron transition of metal ions. In this embodiment, the light emitting element is an organic EL element. The protective die described in the first embodiment is used as a thin film transistor for controlling the driving of the light emitting element. Using a thin film transistor with a structure similar to that of a thin film transistor that functions as an electrode explain.

[0237] As described in the first embodiment, the steps of FIG. 4 and FIG. 5 are performed to obtain the structure shown in FIG. 22(A). In FIG. 22(A), a thin film transistor 800 is formed on a substrate 800. An insulating layer 803 that functions as a protective layer is provided on the insulating layers 801 and 802. The insulating layer 804 is provided to flatten the upper surface. 4 is formed using organic resin such as acrylic, polyimide, polyamide, or siloxane It is preferable to do so.

[0238] A conductive layer 805 is provided over the insulating layer 804. The conductive layer 805 functions as a pixel electrode. When the thin film transistor of the pixel is an n-type, it is preferable to form a cathode as the pixel electrode. However, in the case of p-type, it is preferable to form an anode. Well-known materials such as Ca, Al, CaF, MgAg, and AlLi may be used.

[0239] Next, as shown in FIG. 22B, a partition wall 80 is formed on the end of the conductive layer 805 and on the insulating layer 804. The partition wall 806 has an opening, and the conductive layer 805 is exposed in the opening. The partition wall 806 is formed using an organic resin, an inorganic insulating material, or an organic polysiloxane. In particular, a photosensitive material is used to form an opening on the conductive layer 805, and the sidewall of the opening is continuous. It is preferable to form the inclined surface so as to have a certain curvature.

[0240] Next, a light-emitting layer 807 is formed so as to be in contact with the conductive layer 805 in the opening of the partition wall 806. The light-emitting layer 807 may be composed of a single layer or a plurality of layers laminated together. It's fine if you're there.

[0241] Then, a conductive layer 808 is formed so as to cover the light-emitting layer 807. The conductive layer 808 is a common electrode. The conductive layer 808 is referred to as the third conductive layer 116 in the first embodiment. The conductive layer 80 can be formed of a light-transmitting conductive layer using a light-transmitting conductive material. A titanium nitride layer or a titanium layer may be used as the conductive layer 808. In the opening of the partition wall 806, the conductive layer 805, the light-emitting layer 807 and the conductive The conductive layers 808 are overlapped to form a light-emitting element 809. In order to prevent oxygen, hydrogen, moisture, carbon dioxide, and the like from entering the conductive layer 808 and the partition wall 806, It is preferable to form a protective layer 810 on the insulating layer 810. The protective layer 810 may be a silicon nitride layer, a nitride oxide layer, or the like. A silicon carbide layer, a DLC layer, etc. can be used.

[0242] In reality, after completing the process up to Figure 22(B), the structure is airtight and cannot be exposed to the outside air. Protective film with low gas content (laminate film, UV-curable resin film, etc.) or cover It is preferable to provide further packaging (encapsulation) with a material.

[0243] Next, the configuration of the light emitting element will be described with reference to FIG. The cross-sectional structure of a pixel will be described using an n-type transistor as an example.

[0244] The light emitting element only needs to have at least one of the anode and cathode transparent in order to extract light. Then, a thin film transistor and a light emitting element are formed on the substrate, and light is emitted from the surface opposite the substrate. The top emission structure extracts light from the surface on the substrate side, the bottom emission structure extracts light from the surface on the substrate side, and the bottom emission structure extracts light from the substrate side and the substrate side. There is a light emitting device with a dual emission structure that emits light from both the surface opposite the plate. This can be applied to any of the above injection structures.

[0245] FIG. 23(A) shows a light-emitting element having a top emission structure. When 821 is an n-type light emitting element and light emitted from the light emitting element 822 exits to the anode 825 side, 23A is a cross-sectional view of a cathode 823 of a light-emitting element 822 and a driving transistor. 821 are electrically connected, and a light-emitting layer 824 and an anode 825 are stacked in this order on a cathode 823. The cathode 823 may be a conductive layer that has a small work function and reflects light. Known materials can be used. For example, calcium, aluminum, calcium fluoride, The light-emitting layer 824 is preferably made of a material such as a silver-magnesium alloy or a lithium-aluminum alloy. It can be made up of a single layer or multiple layers stacked together. In the case where the cathode 823 is composed of a plurality of layers, an electron injection layer, an electron transport layer, an emitter layer, and an electron transport layer are disposed on the cathode 823. The light-emitting layer, the hole transport layer, and the hole injection layer are laminated in this order. Note that it is not necessary to provide all of these layers. The anode 825 is formed using a conductive material that transmits light, for example, oxide. Tungsten-containing indium oxide, tungsten oxide-containing indium zinc oxide, Indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium Tin oxide (ITO), indium zinc oxide or indium tin oxide doped with silicon oxide A light-transmitting conductive layer such as a transparent conductive layer may be used.

[0246] The region where the light-emitting layer 824 is sandwiched between the cathode 823 and the anode 825 corresponds to the light-emitting element 822. In the case of the pixel shown in FIG. 23(A), the light emitted from the light emitting element 822 is indicated by a white arrow. The light is emitted toward the anode 825 as indicated by the mark.

[0247] FIG. 23B shows a light-emitting element having a bottom emission structure. The driving transistor 831 is an n-type transistor. 8 is a cross-sectional view of a pixel when light emitted from a light-emitting element 832 is emitted toward a cathode 833. In FIG. 23B, a light-transmitting conductive film is electrically connected to the driving transistor 831. A cathode 833 of the light-emitting element 832 is formed on the cathode layer 837, and a light-emitting layer is formed on the cathode 833. In addition, when the anode 835 has a light-transmitting property, A light reflecting or blocking layer 836 may be formed to cover the anode. The cathode 833 may be a conductive layer having a small work function, as in the case of FIG. Known materials can be used. However, the thickness of the film is such that light can be transmitted through it (preferably For example, an aluminum film having a thickness of 20 nm is can be used as the cathode 833. The light-emitting layer 834 can be formed in the same manner as in FIG. It can be made up of a single layer or multiple layers stacked together. The anode 835 does not need to transmit light, but may have light-transmitting properties as in FIG. The shielding layer 836 may be formed of a conductive material that reflects light, for example. For example, a metal layer that reflects light can be used, but is not limited to this. Resins and the like can also be used.

[0248] The region where the light-emitting layer 834 is sandwiched between the cathode 833 and the anode 835 corresponds to the light-emitting element 832. In the case of the pixel shown in FIG. 23B, the light emitted from the light emitting element 832 is a white The light is emitted toward the cathode 833 as indicated by the arrow.

[0249] FIG. 23C shows a light-emitting element having a dual emission structure. A light-emitting element 842 is formed on a light-transmitting conductive layer 847 electrically connected to the photoresist 841. A cathode 843 is formed, and a light-emitting layer 844 and an anode 845 are laminated in this order on the cathode 843. The cathode 843 can be a conductive layer having a small work function, as in the case of FIG. A known material can be used. However, the thickness of the film must be such that light can pass through it. For example, aluminum having a thickness of 20 nm can be used as the cathode 843. The light-emitting layer 844 may be composed of a single layer or a plurality of layers, as in FIG. The anode 845 may be configured so that layers are laminated. Similarly, the insulating film 11 can be formed using a light-transmitting conductive material.

[0250] The overlapping portion of the cathode 843, the light-emitting layer 844, and the anode 845 constitutes the light-emitting element 842. In the case of the pixel shown in FIG. 23C, the light emitted from the light emitting element 842 is a white outline. As shown by the arrows, the light is emitted to both the anode 845 side and the cathode 843 side.

[0251] Although the organic EL element has been described as the light-emitting element here, inorganic light-emitting elements may also be used. An EL element can also be used.

[0252] In this embodiment, a thin film transistor (a driving transistor) for controlling driving of a light emitting element is used. In the above example, the driving transistor and the light-emitting element are directly connected. A current control transistor may be connected between the first and second terminals.

[0253] Note that the light emitting device described in this embodiment is not limited to the structure shown in FIG. Various modifications based on the technical concept of the present invention are possible. For example, in Figs. 22 and 23, Although the first insulating layer and the second conductive layer have a laminated structure, they may be a single layer.

[0254] Through the above steps, a light-emitting device can be manufactured. The thin film transistor to be used is the thin film transistor functioning as a protection diode described in the first embodiment. Therefore, the off-current of the thin film transistor is small. Since the light-emitting device described in this embodiment has high reliability in electrical characteristics, The light source can be made to have high light transmittance and high visibility.

[0255] (Embodiment 4) Next, the display device described in the second embodiment or the light-emitting device described in the third embodiment is mounted One embodiment of a display panel or a light-emitting panel to be mounted will be described with reference to the drawings.

[0256] In the display device or light-emitting device of the present invention, as shown in FIG. The driving circuit and the scanning line driving circuit are provided on a separate substrate (for example, a semiconductor substrate or an SOI substrate, etc.). However, it is also possible to form the pixel circuit and the pixel circuit on the same substrate without providing a separate circuit. Good too.

[0257] In this embodiment, the liquid crystal display device and the light emitting device are collectively called a display device. .

[0258] The method for connecting the separately formed substrate is not particularly limited, and may be a known COG method. The method may be a soldering method, a wire bonding method, a TAB method, or the like. There is no particular limitation as long as electrical connection is possible. Alternatively, a memory or the like may be formed separately and connected to the pixel circuit.

[0259] FIG. 24 is a block diagram of a display device according to the present invention. The display device shown in FIG. A pixel section 850 having a plurality of pixels each having the above-mentioned, and a scanning line driver circuit 852 for selecting each pixel; and a signal line driver circuit 853 for controlling input of a video signal to a selected pixel.

[0260] The signal line driver circuit 853 shown in FIG. 5. The shift register 854 receives a clock signal (CLK) and a start pulse signal The clock signal (CLK) and the start pulse signal (SP) are input. When the input is input, a timing signal is generated in the shift register 854, and the analog shift The signal is input to switch 855.

[0261] The display device of the present invention is not limited to the form shown in FIG. The signal line driver circuit is not limited to a form having only a shift register and an analog switch. In addition to shift registers and analog switches, it also has buffers, level shifters, source followers, and The shift register and analog switch are not necessarily required. For example, a signal line selection circuit such as a decoder circuit may be provided instead of a shift register. You can use another circuit that can select, or you can use a latch instead of the analog switch. good.

[0262] Also, a video signal is supplied to the analog switch 855. The analog switch 855 outputs the video signal according to the input timing signal. The signal is then sampled and supplied to the signal line of the subsequent stage.

[0263] The scanning line driver circuit 852 shown in FIG. In some cases, a level shifter may be provided. Then, a clock signal (CLK) and a start pulse signal (SP) are input to the shift register 856. The selection signal is generated by inputting the selection signal. The signal is buffered and amplified in the 1 / 2-bit 1 / 4-bit 1 / 8-bit 1 / 16 ... The gates of all pixel transistors are connected together. Since all the transistors must be turned on at the same time, the buffer 857 must pass a large current. A flushable one is used.

[0264] In a full-color display device, the video signal corresponds to R (red), G (green), and B (blue) In the case where the signals are sampled in sequence and supplied to the corresponding signal lines, a shift register 854 and an analog The number of terminals for connecting the log switch 855 is the number of terminals for connecting the analog switch 855 and the pixel unit 85 This is equivalent to about 1 / 3 of the number of terminals required to connect the 0 signal line. Therefore, By forming the analog switch 855 on the same substrate as the pixel portion 850, Compared to when it is formed on a different substrate from 850, the terminals used to connect the separately formed substrate are This reduces the number of connections, reduces the probability of connection failure, and increases yields.

[0265] The scanning line driver circuit 852 in FIG. However, the present invention is not limited to this, and the scanning line driver circuit 85 may be formed of only a shift register 856. 2 may be constructed.

[0266] Note that the configuration shown in FIG. 24 is merely one mode of the display device of the present invention, and is not limited to the signal line drive. The configuration of the circuit and the scanning line driver circuit is not limited to this.

[0267] Next, a shift register including thin film transistors using microcrystalline semiconductor layers all having the same polarity is An embodiment of the shift register of this embodiment will be described with reference to Figs. 25 and 26. Fig. 25 shows the shift register of this embodiment. The shift register shown in FIG. 25 includes flip-flops 851_i (i=1 to n) are combined together. The first clock signal, the second clock signal, It operates by inputting a clock signal, a start pulse signal, and a reset signal.

[0268] The connection relationship of the shift register in FIG. 25 will be described. The shift register in FIG. The flip-flop 851_i (i=1 to n) in the second stage is connected to the first wiring 881 shown in FIG. is connected to the seventh wiring 867_i-1, and the second wiring 882 shown in FIG. 26 is connected to the seventh wiring 867_i+1. 26 is connected to the fifth wiring 865.

[0269] In addition, the fourth wiring 884 shown in FIG. 26 is the second wiring in the odd-numbered flip-flops. In the even-numbered flip-flops, the first wiring 862 is connected to the third wiring 863. 6 is connected to the fourth wiring 864.

[0270] However, the first wiring 881 of the first-stage flip-flop 851_1 shown in FIG. 26 of the n-th flip-flop 851_n. The line 882 is connected to the sixth wiring 866 .

[0271] The first wiring 861, the second wiring 862, the third wiring 863, and the sixth wiring 866 , may be referred to as a first signal line, a second signal line, a third signal line, and a fourth signal line, respectively. Furthermore, the fourth wiring 864 and the fifth wiring 865 are respectively connected to the first power supply line and the second power supply line. It may also be called.

[0272] Next, the details of the flip-flop shown in FIG. 25 are shown in FIG. 26. The flip-flop is a first transistor 871, a second transistor 872, a third transistor a fourth transistor 873, a fourth transistor 874, a fifth transistor 875, a sixth transistor The semiconductor device includes a first transistor 876, a seventh transistor 877, and an eighth transistor 878. In the embodiment, a first transistor 871, a second transistor 872, a third transistor a fourth transistor 873, a fourth transistor 874, a fifth transistor 875, a sixth transistor The seventh transistor 876, the seventh transistor 877, and the eighth transistor 878 are n-channel When the gate-source voltage (Vgs) exceeds the threshold voltage (Vth), The flip-flop shown in FIG. 25 is connected as follows: In the following description, the first electrode refers to a source electrode or a drain electrode. The term "electrode" refers to one of the source electrode and the drain electrode, and the second electrode refers to the other of the source electrode and the drain electrode.

[0273] A first electrode of the first transistor 871 is connected to a fourth wiring 884. The second electrode of the resistor 871 is connected to a third wiring 883 .

[0274] A first electrode of the second transistor 872 is connected to a sixth wiring 886. The second electrode of the resistor 872 is connected to a third wiring 883 .

[0275] A first electrode of the third transistor 873 is connected to a fifth wiring 885. The second electrode of the transistor 873 is connected to the gate electrode of the second transistor 872. The gate electrode of the transistor 873 is connected to a fifth wiring 885 .

[0276] A first electrode of the fourth transistor 874 is connected to a sixth wiring 886. The second electrode of the transistor 874 is connected to the gate electrode of the second transistor 872, and the fourth The gate electrode of the transistor 874 is connected to the gate electrode of the first transistor 871. .

[0277] A first electrode of the fifth transistor 875 is connected to a fifth wiring 885. The second electrode of the fifth transistor 875 is connected to the gate electrode of the first transistor 871. The gate electrode of the transistor 875 is connected to a first wiring 881 .

[0278] A first electrode of the sixth transistor 876 is connected to a sixth wiring 886. The second electrode of the sixth transistor 876 is connected to the gate electrode of the first transistor 871. The gate electrode of the transistor 876 is connected to the gate electrode of the second transistor 872. .

[0279] A first electrode of the seventh transistor 877 is connected to a sixth wiring 886. The second electrode of the seventh transistor 877 is connected to the gate electrode of the first transistor 871. The gate electrode of the transistor 877 is connected to the second wiring 882. A first electrode of the eighth transistor 878 is connected to a sixth wiring 886. The electrode is connected to the gate electrode of the second transistor 872 and the gate electrode of the eighth transistor 878. The gate electrode is connected to a first wiring 881 .

[0280] The first wiring 881, the second wiring 882, the third wiring 883, and the fourth wiring 884 may be referred to as a first signal line, a second signal line, a third signal line, and a fourth signal line, respectively. Furthermore, the fifth wiring 885 may be called the first power supply line and the sixth wiring 886 may be called the second power supply line. good.

[0281] The circuits shown in FIGS. 24 to 26 are constructed using transistors using a microcrystalline semiconductor layer. For example, the driver circuit can be made of amorphous semiconductor. When comparing the case where a dielectric layer is used and the case where a microcrystalline semiconductor layer is used, In the case of the MOS type, the mobility of the transistor is larger, so that the driving circuit (e.g., the scanning line driving circuit 8 It is possible to increase the driving frequency of the shift register 856) of the scanning line 52. Since the driving circuit 852 can be operated at high speed, the frame frequency can be increased. Alternatively, it is also possible to insert a black screen.

[0282] When increasing the frame frequency, the screen data is generated according to the direction of the image movement. It is desirable to perform motion compensation and interpolate the data. By increasing the frame frequency and interpolating image data, the display characteristics of moving images are improved. For example, the frequency is doubled (for example, 120 Hz, 100 Hz). Hz) or more, and more preferably four times that (for example, 240 Hz, 200 Hz) or more. This can reduce the blurring and image retention in moving images. The circuit 852 also operates at a higher drive frequency to increase the frame frequency. It is possible.

[0283] When inserting a black screen, image data or data for black display is supplied to the pixel unit 850. As a result, it becomes similar to impulse driving, and image retention can be reduced. In that case, the scanning line driving circuit 852 can also be operated at a high driving frequency. This allows for black screen insertion.

[0284] Furthermore, the channel width of the transistor of the scan line driver circuit 852 is increased, and By arranging the scanning line driver circuit, a higher frame frequency can be realized. For example, the frame frequency can be set to 8 times (e.g. 480 Hz, 400 Hz) or more. When a plurality of scanning line driving circuits are arranged, a scanning circuit for driving the even-numbered scanning lines is provided. The scanning line driving circuit for driving the odd-numbered scanning lines is arranged on one side, and the scanning line driving circuit for driving the odd-numbered scanning lines is arranged on the opposite side. By placing it on the side, the frame frequency can be increased.

[0285] Note that the circuits shown in FIGS. 24 to 26 can be implemented using transistors using microcrystalline semiconductors. By configuring the display device in this manner, the layout area can be reduced. For example, the frame can be made smaller when an amorphous semiconductor layer is used and when a microcrystalline semiconductor layer is used. The transistor movement is smaller when a microcrystalline semiconductor layer is used than when a Because the resolution is large, the channel width of the transistor can be made small. This makes it possible to narrow the frame of the device.

[0286] 26. In addition, the second transistor 872 in FIG. 26 is connected to the third wiring 883 via a low-level signal During this period, the second transistor 872 is in an on state. Therefore, a strong stress is applied to the second transistor 872, and the transistor characteristics are deteriorated. When the transistor characteristics deteriorate, the threshold voltage gradually increases. As a result, the current value becomes smaller. Therefore, even if the transistor deteriorates, In order to be able to supply sufficient current, the channel width of the second transistor 872 is large. Alternatively, it is preferable that the circuit operation is not hindered even if the transistor deteriorates. For example, a transistor 872 may be connected in parallel with the second transistor 872. 871 and the second transistor 872 are alternately turned on. It is preferable to make the material less susceptible to deterioration.

[0287] However, when comparing the case where an amorphous semiconductor layer is used with the case where a microcrystalline semiconductor layer is used, Therefore, the microcrystalline semiconductor layer is less likely to deteriorate. In the case of using the above, the channel width of the transistor can be reduced. By using a thin film transistor similar to that shown in form 1, deterioration can be significantly reduced. This allows the device to operate normally without the need for a compensation circuit for deterioration. This makes it possible to reduce the layout area.

[0288] Next, the appearance of a liquid crystal display panel and a light-emitting panel corresponding to one embodiment of the liquid crystal display device of the present invention will be described. The cross section will be described with reference to Figs. 27 and 28. Fig. 27(A) shows a first substrate A transistor 910 having a microcrystalline semiconductor layer and a liquid crystal element 913 are formed on a substrate 901. 9 shows a top view of a panel sealed between a second substrate 906 and the panel with a sealant 905. FIG. 27B corresponds to a cross-sectional view taken along line MN in FIG. 27A. FIG. 28 shows the cross-sectional view of the light-emitting device. In addition, in Fig. 28, only the parts different from Fig. 27 are given reference numerals.

[0289] A pixel portion 902 and a scanning line driver circuit 904 are provided on a first substrate 901. In this manner, a sealant 905 is provided. A second substrate 906 is provided on the pixel portion 902 and the scanning line driver circuit 904. 904 is a liquid crystal 904 formed by a first substrate 901, a sealant 905, and a second substrate 906. 908 or a filler 931. Also, the sealant 90 on the first substrate 901 A polycrystalline semiconductor layer is formed on a separately prepared substrate in a region different from the region surrounded by 5. In this embodiment, a signal line driver circuit 903 formed of polycrystalline silicon is mounted. A signal line driver circuit having a transistor using a semiconductor layer is attached to a first substrate 901. An example in which a signal line driver circuit is formed using transistors using single crystal semiconductors will be described. In FIG. 27, multiple elements included in the signal line driver circuit 903 are A transistor 909 formed using a crystalline semiconductor layer is illustrated as an example.

[0290] A pixel portion 902 and a scanning line driver circuit 904 provided on a first substrate 901 are In FIG. 27B, the transistors included in the pixel portion 902 are In this embodiment, the transistor 910 is a driving transistor. In the light emitting device, the transistor 910 is assumed to be a current control transistor. The transistor 910 may be a microcrystalline It corresponds to a transistor using a semiconductor layer.

[0291] In addition, the pixel electrode 912 of the liquid crystal element 913 is connected to the wiring 918 of the transistor 910. Furthermore, the wiring 918 is electrically connected to the lead wiring 914. A counter electrode 917 of the liquid crystal element 913 is formed on the second substrate 906. The overlapping portion of the pixel electrode 912, the counter electrode 917, and the liquid crystal 908 constitutes the liquid crystal element 9 Equivalent to 13.

[0292] The pixel electrode of the light emitting element 930 is a source electrode or a drain electrode of the transistor 910. The light emitting element is electrically connected to the rain electrode via a wiring. The common electrode of the transistor 930 is electrically connected to a light-transmitting conductive material layer. The configuration of the element 930 is not limited to that shown in this embodiment. The configuration of the light emitting element 930 is determined according to the direction of the emitted light, the polarity of the transistor 910, etc. It can be changed as appropriate.

[0293] The first substrate 901 and the second substrate 906 may be made of glass, metal (typical examples include For the material, stainless steel, ceramics, plastics, etc. can be used. The materials used are FRP (Fiberglass-Reinforced Plastics). ) plate, PVF (polyvinyl fluoride) film, polyester film or acrylic A PVF film or polyvinyl chloride film can be used instead of aluminum foil. It is also possible to use a sheet having a structure in which the sheet is sandwiched between polyester films.

[0294] The spacer 911 is a bead spacer, and is disposed between the pixel electrode 912 and the counter electrode 917. The insulating film is selectively etched to control the distance between the electrodes (cell gap). Alternatively, a spacer obtained by etching may be used. It's fine.

[0295] In addition, a signal line driver circuit 903 and a scanning line driver circuit 904 or a pixel portion 9 Various signals and potentials given to the .02 are transmitted from the FPC 907 through the wiring 914. is being supplied.

[0296] In this embodiment, the connection terminal 916 is the same as the pixel electrode 912 of the liquid crystal element 913. The lead wiring 914 is formed from the same conductive layer as the wiring 918. It has been made.

[0297] The connection terminal 916 is electrically connected to a terminal of the FPC 907 via an anisotropic conductive layer 919. is connected to

[0298] Although not shown, the liquid crystal display device shown in this embodiment has an alignment layer and a polarizing plate. It may further include a color filter and a shielding layer.

[0299] In addition, a signal line driver circuit 903 and a scanning line driver circuit 904 or a pixel portion 9 Various signals and potentials applied to the MOSFET 02 are not shown in the cross-sectional view shown in FIG. are supplied from the FPC 907 via wiring 914 and 915.

[0300] In this embodiment, the connection terminal 916 is formed from the same conductive layer as the pixel electrode 912. The lead wiring 915 is formed from the same conductive layer as the wiring 918.

[0301] The second substrate, which is the substrate positioned in the direction in which light is extracted from the light emitting element 930, must be transparent. In that case, glass plates, plastic plates, polyester films or aluminum plates must be used. A substrate made of a light-transmitting material such as a plastic film is used.

[0302] In addition, the filler 931 can be an inert gas such as nitrogen or argon, or an ultraviolet-curing resin. It can be made of PVC (polyvinyl chloride), acrylic, Polyimide, epoxy resin, silicone resin, PVB (Polyvinyl Butyral) or EVA ( In this embodiment, nitrogen is used as the filler. It is best to use the element.

[0303] If necessary, a polarizing plate, a circular polarizing plate (including an elliptical polarizing plate), a positioning plate, etc. may be provided on the light-emitting surface of the light-emitting element. An optical film such as a retardation plate (λ / 4 plate, λ / 2 plate) or a color filter may be provided as appropriate. The polarizing plate or the circular polarizing plate may be provided with an anti-reflection layer.

[0304] This embodiment can be implemented in combination with the configurations described in other embodiments. .

[0305] (Embodiment 5) The liquid crystal display device obtained by the present invention is used in an active matrix type liquid crystal module. That is, the present invention can be applied to any electronic device that incorporates such a display unit. Electronic devices include cameras such as video cameras and digital cameras, head-mounted Displays (goggle-type displays), car navigation systems, projectors, car TV, personal computers, personal digital assistants (mobile computers, mobile phones, (e.g. electronic books) and others. An example is shown in Figure 29.

[0306] FIG. 29(A) is a television device. The display module is as shown in FIG. Then, the TV set can be completed by installing the FPC in the housing. The display panel mounted on the display unit is also called the display module. 3 is formed, and other auxiliary equipment such as a speaker unit 959 and an operation switch are provided. In this manner, the television device is completed.

[0307] As shown in FIG. 29(A), a display panel 952 using a display element is assembled in a housing 951. The receiver 955 receives general television broadcasts, and the modem 954 receives One-way (from sender to receiver) by connecting to a wired or wireless communication network Or it can be two-way (between sender and receiver, or between receivers). The revision device is operated by a switch built into the housing or a separate remote control 956 This can be done by the remote control device 956, which also has a display for displaying the information to be output. A display unit 957 may be provided.

[0308] In addition to the main screen 953, the television device also has a sub-screen 958 as a second display panel. The display may be formed of a digital camera and may be added with a configuration for displaying the channel, volume, etc. In the main screen 953 and the sub-screen 958, one is a liquid crystal display panel and the other is a light-emitting display panel. In addition, in order to prioritize low power consumption, a light-emitting display panel may be used. In the case where the sub-screen 958 is formed by a liquid crystal display panel, for example, The sub screen 958 may be configured to be able to blink.

[0309] FIG. 30 is a block diagram showing the main components of a television device. The display panel has pixels. A signal line driving circuit 972 and a scanning line driving circuit 973 are formed in the same manner as in other embodiments. The connection may be made as described above.

[0310] As for the configuration of other external circuits, on the video signal input side, a signal received by a tuner 974 A video signal amplifier circuit 975 amplifies the video signal, and the signal output from the video signal amplifier circuit 975 is a video signal processing circuit 976 which converts the video signals into color signals corresponding to the colors, green and blue; It has a control circuit 977 for converting the input specifications of the driver IC. The control circuit 977 outputs signals to the scanning line side and the signal line side. In this case, a signal division circuit 978 is provided on the signal line side to divide the input digital signal into m parts. The power supply may be configured to be supplied via the power supply.

[0311] Of the signals received by the tuner 974, the audio signal is sent to an audio signal amplifier circuit 979. The output of the control circuit 98 is supplied to a speaker 983 via an audio signal processing circuit 980. 1 receives control information for a receiving station (receiving frequency) and volume from an input unit 982, and A signal is sent to the audio signal processing circuit 980.

[0312] Of course, the present invention is not limited to television devices, and may be used with monitors of personal computers. In addition, it is also used in large-area displays such as information display boards at train stations and airports, and advertising display boards on the street. It can also be used for various purposes as a display medium.

[0313] FIG. 29B shows an example of a mobile phone 961. This mobile phone 961 has a display unit The display unit 962 includes an operation unit 963 and the like. By applying the liquid crystal display device described in the above embodiment, mass productivity can be improved.

[0314] The portable computer shown in FIG. 29C includes a main body 966, a display unit 967, etc. By applying the liquid crystal display device described in the above embodiment to the display portion 967, Mass productivity can be improved. [Explanation of symbols]

[0315] 100 Substrates 102 Conductive layer 104 Insulating layer 105 Microcrystalline semiconductor layer 106 LPSAS layers 107 Buffer Layer 108 Buffer Layer 109 Impurity Semiconductor Layer 110 Impurity semiconductor layer 111 Conductive layer 112 Conductive layer 114 Insulating layer 116 Conductive Layer 118 Opening 120 Opening 130 Substrate 131 Pixel section 132 Input terminal 133 Input terminal 134 Protection circuit 135 Protection circuit 136 Protection circuit 137 Protection circuit 138 Wiring 139 Wiring 140 Mask 142 Mask 151 Protection Diode 151a n-type thin film transistor 151b n-type thin film transistor 152 Protection Diode 153 Protection Diode 154 Protection Diode 155 Wiring 160 Protection Diode 161 Protection Diode 162 Capacitive element 163 Capacitive element 164 Resistance element 165 Wiring 170 Protection Diode 171 Protection Diode 172 Protection Diode 173 Protection Diode 174 Protection Diode 175 Protection Diode 176 Protection Diode 177 Protection Diode 178 Resistance element 179A Wiring 179B Wiring 180 Resistance element 181 Resistance element 182 Protection Diode 183 Wiring 186 Transistors 190 Substrate 191 layers 200 Road Room 201 Reaction chamber 202 Reaction chamber 203 Reaction chamber 204 Reaction chamber 205 Unloading Room 210 Common room 211 Means of transport 212 Gate valve 218 Cassette 219 Cassette 220 Substrate 300 Substrates 301 Substrate 302 Wiring 304 Wiring 305 Wiring 316 Wiring 318 Wiring 320 Insulating layer 322 Insulating layer 323 Opening 324 Pixel electrode 325 Slit 326 Pixel electrode 328 Thin Film Transistor 329 Thin Film Transistor 330 Holding capacity section 331 Holding capacity section 332 Light blocking layer 334 Colored layer 336 Colored layer 338 Colored layer 340 Counter Electrode 342 Spacer 344 Protrusion 346 Orientation Layer 348 Orientation Layer 350 Liquid crystal layer 351 Liquid Layer Element 352 Liquid crystal element 401 Substrate 402 Wiring 403 Wiring 416 Wiring 418 Wiring 419 Wiring 423 Opening 424 Pixel electrode 425 Slit 426 Pixel electrode 427 Opening 428 Thin Film Transistor 429 Thin Film Transistor 430 Holding capacity section 431 Holding capacity section 432 Light blocking layer 436 Colored layer 437 Planarization layer 440 Counter Electrode 441 Slit 446 Orientation Layer 448 Orientation Layer 450 Liquid crystal layer 451 Liquid crystal element 452 Liquid crystal element 500 boards 501 Substrate 504 Wiring 506 Gate Insulation Layer 507 Pixel electrode 510 Source Region 516 Wiring 518 Wiring 520 Insulating layer 523 Opening 524 Pixel electrode 525 Slit 528 Thin Film Transistor 532 Light blocking layer 536 Colored layer 537 Planarization layer 550 Liquid crystal layer 600 Substrates 601 Substrate 602 scan lines 606 Gate Insulation Layer 607 Pixel electrode 609 Wiring 610 Source Region 615 Capacitive electrode 616 Wiring 618 Wiring 620 Insulating layer 623 Opening 624 Pixel electrode 628 Thin Film Transistor 632 Light blocking layer 633 Opening 636 Colored layer 637 Planarization layer 650 Liquid crystal layer 700 Substrates 701 Substrate 716 Wiring 718 Wiring 723 Opening 724 Pixel electrode 728 Thin Film Transistor 732 Light blocking layer 736 Colored layer 737 Planarization layer 740 Counter Electrode 750 Liquid crystal layer 800 boards 801 Thin Film Transistor 803 Insulation layer 804 Insulating layer 805 Conductive layer 806 Bulkhead 807 Light-emitting layer 808 Conductive layer 809 Light emitting element 810 protective layer 821 Driving Transistor 822 Light emitting element 823 Cathode 824 Light-emitting layer 825 Anode 831 Driving Transistor 832 Light emitting element 833 Cathode 834 Light-emitting layer 835 Anode 836 Shielding layer 837 Conductive Layer 841 Drive transistor 842 Light emitting element 843 Cathode 844 Light-emitting layer 845 Anode 847 Conductive Layer 850 pixels 851 Flip-flop 852 Scanning line driver circuit 853 Signal Line Driver Circuit 854 Shift Register 855 Analog Switch 856 Shift Register 857 Buffer 861 Wiring 862 Wiring 863 Wiring 864 Wiring 865 Wiring 866 Wiring 867 Wiring 871 Transistor 872 Transistors 873 Transistor 874 Transistor 875 Transistors 876 Transistors 877 Transistors 878 Transistor 881 Wiring 882 Wiring 883 Wiring 884 Wiring 885 Wiring 886 Wiring 901 Board 902 Pixel section 903 Signal line driver circuit 904 Scanning line driver circuit 905 Sealing material 906 Substrate 907 FPC 908 Liquid crystal 909 Transistor 910 Transistor 911 Spacer 912 Pixel electrode 913 Liquid crystal element 914 Wiring 915 Wiring 916 Connection terminal 917 Counter Electrode 918 Wiring 919 Anisotropic conductive layer 930 Light emitting element 931 Filling material 940 Wiring 951 Case 952 Display Panel 953 Main screen 954 Modem 955 Receiver 956 Remote Controlled Device 957 Display section 958 Sub Screen 959 Speaker section 961 Mobile Phones 962 Display section 963 Operation section 966 Main Unit 967 Display section 971 Pixel section 972 Signal line driver circuit 973 Scanning line driver circuit 974 Tuner 975 Video signal amplifier circuit 976 Video signal processing circuit 977 Control Circuit 978 Signal splitting circuit 979 Audio signal amplifier circuit 980 Audio signal processing circuit 981 Control circuit 982 Input section 983 Speaker

Claims

[Claim 1] A display device having an input terminal and a pixel unit, At least one protection circuit is provided between the input terminal and the pixel unit, the protection circuit includes at least one thin film transistor; The thin film transistor is A gate electrode; a gate insulating layer provided to cover the gate electrode; a microcrystalline semiconductor layer provided on the gate insulating layer; a buffer layer provided on the microcrystalline semiconductor layer; a source region and a drain region provided on a portion of the buffer layer, the side surfaces of the source region and the drain region being substantially flush with the side surfaces of the recessed portion of the buffer layer; a source electrode provided on and in contact with the source region, and a drain electrode provided on and in contact with the drain region; In the buffer layer, a region overlapping with the source region and the drain region is thicker than a region overlapping with a channel formation region; A protective insulating layer is provided on the source electrode and the drain electrode, the protective insulating layer has a first opening and a second opening; the first opening is provided to reach the source electrode or the drain electrode, the second opening is provided so as to reach above the gate electrode; a first opening and a second opening, the first opening being electrically connected to the second opening, the second opening being electrically connected to the first opening;

Citation Information

Patent Citations

  • Thin film transistor and manufacture thereof

    JP1991278466A

  • Thin-film transistor and its manufacture

    JP1994342909A

  • Thin-film transistor

    JP1999121761A

  • Active matrix display and manufacturing method thereof

    JP2003057673A

  • Thin-film transistor for display device, substrate and display device using the same therein, and method of manufacturing the same