Solid electrolyte, production method for solid electrolyte, and battery

A solid electrolyte composition with a lithium salt, carbonate solvent, and metal oxide particles, enhanced by a binder and photopolymerization, addresses the issues of low transfer numbers and stability in existing electrolytes, enabling stable and conductive battery films.

JP2024157070AInactive Publication Date: 2024-11-07LINTEC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2021153979
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-09-22
Publication Date
2024-11-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing solid electrolytes using ionic liquid electrolytes have insufficient lithium ion transfer numbers and stability against lithium metal, particularly under severe conditions, and are difficult to form into solid electrolyte films due to low viscosity.

Method used

A solid electrolyte composition containing a lithium salt, carbonate-based solvent, and metal oxide particles with a viscosity of 7 mPa·s or more, enhanced by a binder with acrylic polymerizable compounds, is formed into a film through photopolymerization, improving thixotropy and stability.

Benefits of technology

The solution enables the formation of a solid electrolyte film with high lithium ion transfer number, ionic conductivity, and stability against lithium metal, facilitating the production of stable batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157070000001
    Figure 2024157070000001
  • Figure 2024157070000002
    Figure 2024157070000002
Patent Text Reader

Abstract

To provide a solid electrolyte that facilitates easy membrane formation, with high lithium-ion transference number, high ionic conductivity, and high stability against lithium metal.SOLUTION: A solid electrolyte comprises metal oxide particles and an electrolytic solution that contains a lithium salt and a carbonate solvent, the viscosity of the electrolytic solution at 23°C as measured in accordance with JIS Z 8803:2011 being 7 mPa s or higher.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solid electrolyte, a method for producing a solid electrolyte, and a battery. [Background technology]

[0002] Unlike liquid electrolytes, solid electrolytes are free from the risk of leakage and can form lightweight and flexible electrolyte membranes. Therefore, solid electrolytes are expected to be applied to secondary batteries using lithium ions, etc. For example, Patent Document 1 proposes a quasi-solid electrolyte that includes a metal oxide and an ion conductive material, and in which a specific ion conductive material is supported by metal oxide particles. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-059432 A Summary of the Invention [Problem to be solved by the invention]

[0004] The pseudo-solid electrolyte described in Patent Document 1 uses a mixture of either glymes or N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium bis(trifluoromethanesulfonyl)imide as an ion-conducting material, and a lithium salt containing lithium bis(fluorosulfonyl)imide. This ion-conducting material is an ionic liquid-based electrolyte. However, the solid electrolyte using an ionic liquid-based electrolyte does not have sufficient characteristics such as lithium ion transport number. In addition, in a more severe usage environment, the solid electrolyte using an ionic liquid-based electrolyte does not have sufficient characteristics such as stability against lithium metal. For this reason, further improvement is required in the characteristics of the solid electrolyte, such as more stable cycle discharge and charge performance. In addition, it has been found that it is difficult to obtain a solid electrolyte when the viscosity of the electrolyte is too low.

[0005] An object of the present invention is to provide a solid electrolyte which can be easily formed into a membrane and has high lithium ion transport number, ionic conductivity, and stability against lithium metal, a method for producing this solid electrolyte, and a battery including this solid electrolyte. [Means for solving the problem]

[0006] According to one aspect of the present invention, there is provided a solid electrolyte comprising an electrolyte solution containing a lithium salt and a carbonate-based solvent, and metal oxide particles, wherein the viscosity of the electrolyte solution at 23°C, as measured in accordance with JIS Z 8803:2011, is 7 mPa s or more.

[0007] In the solid electrolyte according to one aspect of the present invention, the lithium salt is preferably at least one selected from the group consisting of lithium bis(fluorosulfonyl)imide and lithium borofluoride.

[0008] In the solid electrolyte according to one aspect of the present invention, the carbonate-based solvent is preferably at least one selected from the group consisting of dimethyl carbonate and propylene carbonate.

[0009] In the solid electrolyte according to one aspect of the present invention, the molar ratio of the lithium salt to the carbonate-based solvent (lithium salt / carbonate-based solvent) contained in the electrolytic solution is preferably 1 / 4 or more and 1 / 1 or less.

[0010] In the solid electrolyte according to one aspect of the present invention, the metal oxide particles are preferably silica particles.

[0011] In the solid electrolyte according to one embodiment of the present invention, the specific surface area of ​​the metal oxide particles measured by a BET method is 160 m 2 / g or more 700m 2 It is preferable that the molecular weight is not more than 1 / g.

[0012] The solid electrolyte according to one aspect of the present invention preferably further contains a binder.

[0013] In the solid electrolyte according to the aspect of the present invention, the binder preferably contains an acrylic polymer.

[0014] In the solid electrolyte according to one embodiment of the present invention, the acrylic polymer contains a constitutional unit derived from an acrylic polymerizable compound, and the acrylic polymerizable compound has a reaction rate constant k p is 700 L·mol -1 ·s -1 It is preferable that the composition contains a monofunctional (meth)acrylate compound having the above structure.

[0015] In the solid electrolyte according to one aspect of the present invention, it is preferable that the acrylic polymerizable compound further contains a polyfunctional (meth)acrylate compound other than the monofunctional (meth)acrylate compound.

[0016] In the solid electrolyte according to one embodiment of the present invention, the polyfunctional (meth)acrylate compound is preferably at least one selected from the group consisting of 1,9-bis(acryloyloxy)nonane, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate.

[0017] In the solid electrolyte according to one embodiment of the present invention, the structural unit derived from the acrylic polymerizable compound includes at least one selected from the group consisting of a structural unit derived from the monofunctional (meth)acrylate compound and a structural unit derived from the polyfunctional (meth)acrylate compound, and when the total of the structural units derived from the monofunctional (meth)acrylate compound and the structural units derived from the polyfunctional (meth)acrylate compound is taken as 100 mol %, it is preferable that the content of the structural units derived from the monofunctional (meth)acrylate compound is 90 mol % or more and 100 mol % or less, and the content of the structural units derived from the polyfunctional (meth)acrylate compound is 0 mol % or more and 10 mol % or less.

[0018] According to one aspect of the present invention, there is provided a battery comprising the solid electrolyte according to the above aspect of the present invention.

[0019] According to one aspect of the present invention, there is provided a method for producing the solid electrolyte according to the aspect of the present invention, the method comprising the steps of: mixing the electrolytic solution, the metal oxide particles, the acrylic polymerizable compound, and a photopolymerization initiator to prepare a mixture; molding the mixture to obtain a molded product; and irradiating the molded product with ultraviolet light to obtain a solid electrolyte containing the acrylic polymer in which the acrylic polymerizable compound is cured. Effect of the Invention

[0020] According to one aspect of the present invention, there are provided a solid electrolyte that is easily formed into a membrane and has high lithium ion transport number, ionic conductivity, and stability against lithium metal, a method for producing the solid electrolyte, and a battery including the solid electrolyte. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present invention will be described below by taking an embodiment as an example, but the present invention is not limited to the content of the embodiment.

[0022] [Solid electrolyte] The solid electrolyte according to this embodiment will be described.

[0023] The solid electrolyte according to the present embodiment contains an electrolyte solution containing a lithium salt and a carbonate-based solvent, and metal oxide particles. The solid electrolyte according to the present embodiment has a viscosity of 7 mPa·s or more at 23° C., measured according to JIS Z 8803:2011. The solid electrolyte according to the present embodiment is easy to form into a membrane, and a solid electrolyte having high lithium ion transport number, high ionic conductivity, and high stability against lithium metal can be obtained. The reason for this is presumed to be as follows.

[0024] In the solid electrolyte according to the present embodiment, the thixotropy of the electrolyte is improved by containing the electrolyte and metal oxide particles. In addition, when the viscosity of the electrolyte at 23° C. is 7 mPa·s or more, the effect of improving the thixotropy is further enhanced. Therefore, it is possible to form a membrane of the electrolyte containing the metal oxide particles. By making this membrane possible, it is possible to suppress leakage of the electrolyte while suppressing the loss of the ionic conductivity of the electrolyte. From the above, it is presumed that the solid electrolyte according to the present embodiment can be easily formed into a membrane, and a solid electrolyte having high lithium ion transport number, ionic conductivity, and stability against lithium metal (among these properties, particularly high stability against lithium metal) can be obtained.

[0025] <Electrolyte> The electrolyte solution according to this embodiment is obtained by containing a lithium salt and a carbonate-based solvent.

[0026] (Lithium salts) Specific examples of the lithium salt according to this embodiment include lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium 2-trifluoromethyl-4,5-dicyanoimidazolate (LiTDI), lithium 4,5-dicyano-1,2,3-triazolate (LiDCTA), lithium bis(pentafluoroethylsulfonyl)imide (LiBETI), lithium borofluoride (LiBF4), lithium bis(oxalato)borate (LiBOB), lithium nitrate (LiNO3), lithium chloride (LiCl), lithium bromide (LiBr), and lithium fluoride (LiF).

[0027] Among these, the lithium salt is preferably at least one selected from lithium bis(fluorosulfonyl)imide and lithium fluoroborate, in terms of obtaining a solid electrolyte having high lithium ion transport number, ionic conductivity, and stability against lithium metal. The lithium salt may be either lithium bis(fluorosulfonyl)imide (LiFSI) or lithium fluoroborate (LiBF4), or these two may be used together. In the solid electrolyte, the lithium salt may exist as a cation of lithium metal and a counter ion of the cation. By using these lithium salts, the stability against lithium metal is further improved.

[0028] (Carbonate solvent) Specific examples of the carbonate-based solvent according to the present embodiment include dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC). Among these, the carbonate-based solvent is preferably at least one selected from dimethyl carbonate and propylene carbonate, in that a solid electrolyte having high lithium ion transport number, ionic conductivity, and stability against lithium metal can be obtained. The carbonate-based solvent may be one of dimethyl carbonate (DMC) and propylene carbonate (PC) alone, or these two may be used in combination. Here, the carbonate-based solvent in the present embodiment refers to a compound having a carbonate skeleton in its molecular structure.

[0029] (Molar ratio of lithium salt to carbonate solvent) In the electrolyte solution according to the present embodiment, the molar ratio of the lithium salt to the carbonate-based solvent (lithium salt / carbonate-based solvent) is preferably 1 / 4 or more and 1 / 1 or less. When this molar ratio is 1 / 4 or more, the stability to lithium metal is easily improved. On the other hand, when this molar ratio is 1 / 1 or less, the lithium salt is easily dissolved in the carbonate-based solvent. In terms of obtaining a solid electrolyte having high lithium ion transport number, ionic conductivity, and stability to lithium metal, this molar ratio may be 1 / 3 or more and 1 / 1 or less, or 1 / 2 or more and 1 / 1 or less.

[0030] Although the reason is unclear, the electrolyte according to the present embodiment is more stable to lithium metal when it is an electrolyte solution in which at least one lithium salt selected from lithium bis(fluorosulfonyl)imide and lithium borofluoride is combined with at least one carbonate-based solvent selected from dimethyl carbonate and propylene carbonate. In addition, when it is an electrolyte solution in which at least one lithium salt selected from lithium bis(fluorosulfonyl)imide and lithium borofluoride is combined with at least one carbonate-based solvent selected from dimethyl carbonate and propylene carbonate, the content of the lithium salt and the carbonate-based solvent is in the range of 1 / 4 to 1 / 1 in molar ratio, the stability to lithium metal is more excellent.

[0031] The content of the electrolytic solution in the solid electrolyte is preferably 75% by mass or more, more preferably 77% by mass or more, even more preferably 78% by mass or more, and even more preferably 79% by mass or more, based on the entire solid electrolyte, in order to obtain a solid electrolyte having high lithium ion transport number, ionic conductivity, and stability to lithium metal. Also, in the same respect, the content of the electrolytic solution in the solid electrolyte is preferably 90% by mass or less, more preferably 89% by mass or less, and even more preferably 88% by mass or less, based on the entire solid electrolyte.

[0032] (viscosity) In the solid electrolyte according to this embodiment, the viscosity of the electrolyte solution is 7 mPa·s or more. In order to facilitate the formation of a membrane of the solid electrolyte, the viscosity of the electrolyte solution is preferably 9 mPa·s or more, more preferably 11 mPa·s or more, even more preferably 20 mPa·s or more, even more preferably 30 mPa·s or more, and even more preferably 40 mPa·s or more.

[0033] The upper limit of the viscosity of the electrolyte is not particularly limited. For example, in consideration of obtaining a solid electrolyte having high lithium ion transport number, ionic conductivity, and stability to lithium metal, the upper limit of the viscosity of the electrolyte may be, for example, 500 mPa s or less, or 300 mPa s or less.

[0034] The viscosity of the electrolyte is measured at 23° C. in accordance with JIS Z 8803:2011. The viscosity of the electrolyte is preferably measured by, for example, a vibration viscometer. When measuring the viscosity of the electrolyte in a solid electrolyte, the electrolyte in the solid electrolyte is extracted, and the viscosity of the extracted electrolyte is measured by, for example, a vibration viscometer.

[0035] <Metal oxide particles> The solid electrolyte according to the present embodiment contains metal oxide particles. In the solid electrolyte according to the present embodiment, the electrolytic solution is supported on the metal oxide particles by containing the electrolytic solution and the metal oxide particles. Here, in the present embodiment, the supported state refers to a state in which the electrolytic solution is coated on at least a part of the surface of the metal oxide particles.

[0036] Metal oxide particles have a specific surface area of ​​160 m2 or more as measured by the BET method, which facilitates the formation of a solid electrolyte membrane. 2 / g or more 700m 2 The specific surface area (BET method) of the metal oxide particles is preferably 160 m 2 / g or more, the thixotropy is likely to be improved, and a film of an electrolyte solution containing metal oxide particles (i.e., a solid electrolyte) is likely to be formed. In addition, the specific surface area (BET method) is 700 m 2 When the specific surface area (BET method) of the metal oxide particles is less than 165 m / g, the metal oxide particles are easily mixed with the electrolytic solution, and a solid electrolyte membrane is easily formed. 2 / g or more is more preferable, and 170m 2 / g or more. 2 / g or less is more preferable, and 2 / g or less is more preferable. Here, the BET method is a method in which gas molecules (usually nitrogen gas) are adsorbed on solid particles, and the specific surface area of ​​the solid particles is measured from the amount of adsorbed gas molecules. The specific surface area can be measured using various BET measuring devices.

[0037] The metal oxide particles may be used alone, or two or more types of metal oxide particles having different specific surface areas may be used in combination. The type of metal oxide particles is not particularly limited, and examples thereof include silica particles, alumina particles, zirconia particles, ceria particles, magnesium silicate particles, calcium silicate particles, zinc oxide particles, antimony oxide particles, indium oxide particles, tin oxide particles, titanium oxide particles, iron oxide particles, magnesium oxide particles, aluminum hydroxide particles, magnesium hydroxide particles, potassium titanate particles, and barium titanate particles. The metal oxide particles may be used alone, or two or more types may be used in combination. Among these, the metal oxide particles are preferably at least one selected from silica particles, alumina particles, zirconia particles, magnesium oxide particles, and barium titanate particles in terms of improving thixotropy. The metal oxide particles are more preferably silica particles in terms of being lightweight and having a small particle diameter.

[0038] When silica particles are used as metal oxide particles, the silica particles may be wet silica particles or dry silica particles. Examples of wet silica particles include wet silica particles obtained by a precipitation method and a sol-gel method, which are obtained by a neutralization reaction between sodium silicate and a mineral acid. Examples of dry silica particles include combustion method silica particles (fumed silica particles) obtained by burning a silane compound, and deflagration method silica particles obtained by explosively burning metal silicon powder. When the silica particles are dry silica particles, the inclusion of moisture derived from the silica particles can be suppressed, so that deterioration of the electrolyte is easily suppressed. For this reason, from the viewpoint of suppressing deterioration of the electrolyte, the silica particles are preferably dry silica particles, and more preferably fumed silica particles.

[0039] The content of the metal oxide particles in the solid electrolyte is preferably 4% by mass or more, more preferably 5% by mass or more, and even more preferably 6% by mass or more, based on the entire solid electrolyte, in order to facilitate the formation of a solid electrolyte membrane. Also, from the same viewpoint, the content of the metal oxide particles in the solid electrolyte is preferably 16% by mass or less, more preferably 15% by mass or less, and even more preferably 14% by mass or less, based on the entire solid electrolyte.

[0040] <Binding agent> The solid electrolyte according to the present embodiment may or may not contain a binder. The solid electrolyte according to the present embodiment may contain a binder in order to facilitate the formation of a solid electrolyte membrane. When the solid electrolyte according to the present embodiment contains a binder, the type of the binder is not particularly limited. When the solid electrolyte according to the present embodiment contains a binder, it is preferable that the binder contains an acrylic polymer in order to facilitate the formation of a solid electrolyte membrane and to facilitate the improvement of stability against lithium metal.

[0041] (Acrylic polymer) In the solid electrolyte according to the present embodiment, the acrylic polymer contains a structural unit derived from an acrylic polymerizable compound. That is, the acrylic polymer is a resin polymerized using an acrylic polymerizable compound as a monomer, and contains a structural unit derived from the acrylic polymerizable compound in the main chain. Here, "derived from" means that the necessary structure is changed when the monomer is polymerized.

[0042] [Acrylic polymerizable compound] The acrylic polymerizable compound includes a (meth)acrylate compound. The acrylic polymerizable compound may include only a monofunctional (meth)acrylate compound, or may include both a monofunctional (meth)acrylate compound and a polyfunctional (meth)acrylate compound.

[0043] In this specification, "(meth)acrylic" is a notation used to represent both "acrylic" and "methacrylic", and the same applies to other similar terms. In this specification, the polyfunctional (meth)acrylate compound means a di- or higher functional (meth)acrylate compound.

[0044] ·Monofunctional (meth)acrylate compounds The solid electrolyte according to the present embodiment is an acrylic polymerizable compound having a reaction rate constant k p is 700 L·mol -1 ·s -1 In a similar manner, the acrylic polymerizable compound preferably contains a monofunctional (meth)acrylate compound having a reaction rate constant k p is 710 L mol -1 ·s -1 More preferably, it is 720 L·mol -1 ·s -1 The reaction rate constant k of the monofunctional (meth)acrylate compound contained in the acrylic polymerizable compound is more preferably equal to or greater than 1. p The upper limit is not particularly limited, and is, for example, 40,000 L·mol -1 ·s -1 May be less than 35000 L·mol -1 ·s -1 In this specification, the reaction rate constant k p is 700 L·mol -1 ·s -1 The monofunctional (meth)acrylate compound having the above reaction rate constant k may be referred to as component (A). p is 700 L·mol -1 ·s -1 It is believed that the use of the above monofunctional (meth)acrylate compound improves the reactivity of the monofunctional (meth)acrylate compound and increases the molecular weight, which makes it easier to form a solid electrolyte into a film.

[0045] Reaction rate constant k p is 700 L·mol -1·s -1 The monofunctional (meth)acrylate compound having the above reaction rate constant k is not particularly limited, and may be, for example, (meth)acrylic acid or alkyl (meth)acrylate. p is 700 L·mol -1 ·s -1 The monofunctional (meth)acrylate compound having the above structure is preferably an alkyl (meth)acrylate having an alkyl group having 1 to 3 carbon atoms. Specific examples include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, and isopropyl (meth)acrylate. Among these, the monofunctional (meth)acrylate compound having the above structure is preferably an alkyl (meth)acrylate having an alkyl group having 1 to 3 carbon atoms. p is 700 L·mol -1 ·s -1 More preferably, the monofunctional (meth)acrylate compound having a reaction rate constant k p is 700 L·mol -1 ·s -1 By using the above-mentioned monofunctional (meth)acrylate compound, it becomes easier to obtain a solid electrolyte having high lithium ion transport number, high ionic conductivity, and high stability against lithium metal.

[0046] · Polyfunctional (meth)acrylate compounds In the solid electrolyte according to the present embodiment, it is preferable that the acrylic polymerizable compound further contains a polyfunctional (meth)acrylate compound other than the monofunctional (meth)acrylate compound in order to facilitate the formation of a solid electrolyte membrane. When the acrylic polymerizable compound further contains a polyfunctional (meth)acrylate compound other than the monofunctional (meth)acrylate compound, a solid electrolyte having high lithium ion transport number, ionic conductivity, and stability against lithium metal is more easily obtained. In this specification, the polyfunctional (meth)acrylate compound may be referred to as component (B).

[0047] Multifunctional (meth)acrylate compounds have a reaction rate constant k p is 700 L L mol -1 ·s -1There is no particular limitation as long as it is a bifunctional or higher (meth)acrylate compound other than the above monofunctional (meth)acrylate compound. The polyfunctional (meth)acrylate compound is preferably a polyfunctional (meth)acrylate compound having no reactive group other than an acryloyl group, from the viewpoint of obtaining a solid electrolyte having high lithium ion transport number, ionic conductivity, and stability against lithium metal, and from the viewpoint of facilitating the formation of a solid electrolyte membrane.

[0048] Specific examples of the polyfunctional (meth)acrylate compound include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol diacrylate (1,9-bis(acryloyloxy)nonane), neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, dimethylol dicyclopentane di(meth)acrylate, and tricyclodecane dimethanol (meth)acrylate. difunctional (meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and pentaerythritol tri(meth)acrylate; tetrafunctional (meth)acrylate compounds such as diglycerol tetra(meth)acrylate and pentaerythritol tetra(meth)acrylate; pentafunctional (meth)acrylate compounds such as dipentaerythritol penta(meth)acrylate; and hexafunctional (meth)acrylate compounds such as dipentaerythritol hexa(meth)acrylate.

[0049] Among these, from the viewpoints of obtaining a solid electrolyte having high lithium ion transport number, ionic conductivity, and stability against lithium metal, and of facilitating the formation of a film of the solid electrolyte, the polyfunctional (meth)acrylate compound is preferably at least one selected from the group consisting of 1,9-bis(acryloyloxy)nonane, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate.

[0050] In the solid electrolyte according to the present embodiment, the structural unit derived from the acrylic polymerizable compound contained in the acrylic polymer preferably includes at least one selected from the group consisting of a structural unit derived from a monofunctional (meth)acrylate compound and a structural unit derived from a polyfunctional (meth)acrylate compound. The structural unit derived from the acrylic polymerizable compound more preferably includes a structural unit derived from a monofunctional (meth)acrylate compound. The structural unit derived from the acrylic polymerizable compound further preferably includes a structural unit derived from a monofunctional (meth)acrylate compound and a structural unit derived from a polyfunctional (meth)acrylate compound. In terms of facilitating the formation of a solid electrolyte membrane, the content of the structural unit derived from the monofunctional (meth)acrylate compound and the structural unit derived from the polyfunctional (meth)acrylate compound is preferably within the range shown below. In addition, when the content of the structural unit derived from the monofunctional (meth)acrylate compound and the structural unit derived from the polyfunctional (meth)acrylate compound is within the range shown below, a solid electrolyte having high lithium ion transport number, ionic conductivity, and stability to lithium metal is more easily obtained.

[0051] When the total of the constitutional units derived from the monofunctional (meth)acrylate compound and the constitutional units derived from the polyfunctional (meth)acrylate compound is 100 mol%, the content of the constitutional units derived from the monofunctional (meth)acrylate compound is preferably 90 mol% or more, more preferably 91 mol% or more, and even more preferably 93 mol% or more. The content of the constitutional units derived from the monofunctional (meth)acrylate compound is preferably 100 mol% or less, more preferably 99 mol% or less, and even more preferably 97 mol% or less.

[0052] When the total of the constitutional units derived from the monofunctional (meth)acrylate compound and the constitutional units derived from the polyfunctional (meth)acrylate compound is 100 mol%, the content of the constitutional units derived from the polyfunctional (meth)acrylate compound is preferably 0 mol% or more, more preferably 1 mol% or more, and even more preferably 3 mol% or more. The content of the constitutional units derived from the polyfunctional (meth)acrylate compound is preferably 10 mol% or less, more preferably 9 mol% or less, and even more preferably 7 mol% or less.

[0053] The content of the acrylic polymer in the solid electrolyte is preferably 3% by mass or more, more preferably 4% by mass or more, and even more preferably 5% by mass or more, based on the entire solid electrolyte, in order to facilitate the formation of a solid electrolyte membrane. In the same respect, the content of the metal oxide particles in the solid electrolyte is preferably 10% by mass or less, more preferably 9% by mass or less, and even more preferably 8% by mass or less, based on the entire solid electrolyte.

[0054] [Photopolymerization initiator] In the solid electrolyte according to the present embodiment, a photopolymerization initiator is preferably used to obtain an acrylic polymer. In the solid electrolyte according to the present embodiment, the acrylic polymer is obtained by polymerizing a binder composition containing an acrylic polymerizable compound and a photopolymerization initiator.

[0055] The photopolymerization initiator is not particularly limited, and may be a known compound used for the purpose of curing an acrylic polymerizable compound. The photopolymerization initiator is preferably a photopolymerization initiator that is sensitive to ultraviolet light. The photopolymerization initiator may be used alone or in combination of two or more kinds.

[0056] Specific examples of the photopolymerization initiator include α-ketol compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, and 1-hydroxycyclohexylphenyl ketone; acetophenone compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzoin ether compounds such as benzoin ethyl ether, benzoin isopropyl ether, and anisoin methyl ether; ketal compounds such as benzyl dimethyl ketal; and 2-naphthalenesulfonyl chloride. aromatic sulfonyl chloride compounds; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; benzophenone compounds such as benzophenone, benzoylbenzoic acid, and 3,3'-dimethyl-4-methoxybenzophenone; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone; camphorquinone; halogenated ketones; acylphosphinoxides; acylphosphonates; oligo[2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone], and the like.

[0057] The content of the binder in the solid electrolyte is preferably 3% by mass or more, more preferably 4% by mass or more, and even more preferably 5% by mass or more, based on the entire solid electrolyte, in order to facilitate the formation of a membrane from the solid electrolyte. Also, from the same viewpoint, the content of the binder in the solid electrolyte is preferably 10% by mass or less, more preferably 9% by mass or less, and even more preferably 8% by mass or less, based on the entire solid electrolyte.

[0058] The solid electrolyte according to the present embodiment contains the lithium salt according to the present embodiment described above, an electrolyte solution containing a carbonate-based solvent, metal oxide particles, and a binder containing an acrylic polymer. The solid electrolyte according to the present embodiment may contain other components as long as the object of the present invention is not impaired.

[0059] <Mass ratio of metal oxide, electrolyte, and binder> In terms of facilitating the formation of a solid electrolyte membrane, the solid electrolyte according to this embodiment preferably has the following contents when the total content of the electrolytic solution, the metal oxide particles, and the binder is taken as 100 mass %. In addition, in the total content of the electrolytic solution, the metal oxide particles, and the binder, if the contents of the electrolytic solution, the metal oxide particles, and the binder are within the following ranges, a solid electrolyte having high lithium ion transport number, ionic conductivity, and stability to lithium metal is more easily obtained. It is preferable that the content of the electrolyte is 77% by mass or more and 90% by mass or less, the content of the metal oxide particles is 4% by mass or more and 16% by mass or less, and the content of the binder is 3% by mass or more and 10% by mass or less. It is more preferable that the content of the electrolyte is 78% by mass or more and 89% by mass or less, the content of the metal oxide particles is 5% by mass or more and 15% by mass or less, and the content of the binder is 4% by mass or more and 9% by mass or less. It is more preferable that the content of the electrolyte is 79% by mass or more and 88% by mass or less, the content of the metal oxide particles is 6% by mass or more and 14% by mass or less, and the content of the binder is 5% by mass or more and 8% by mass or less.

[0060] [Method of manufacturing solid electrolyte] Next, a preferred method for producing the solid electrolyte according to the present embodiment will be described in the case where the solid electrolyte according to the present embodiment contains a binder containing an acrylic polymer. The method for producing the solid electrolyte according to the present embodiment is an example of a method for producing a solid electrolyte, and is not limited to the method described below.

[0061] The method for producing a solid electrolyte according to this embodiment includes the following steps. A step of preparing a mixture by mixing an electrolyte solution, metal oxide particles, an acrylic polymerizable compound, and a photopolymerization initiator (step 1) A step of forming the mixture to obtain a formed product (step 2) A step of irradiating the molded product with ultraviolet light to obtain a solid electrolyte containing an acrylic polymer in which the acrylic polymerizable compound is cured (step 3). The electrolyte contains a lithium salt and a carbonate-based solvent, and has a viscosity of 7 mPa·s or more at 23° C. as measured in accordance with JIS Z 8803:2011.

[0062] According to the preferred method for producing the solid electrolyte of this embodiment, the solid electrolyte can be easily formed into a membrane, and a solid electrolyte having high lithium ion transport number, ionic conductivity, and stability against lithium metal can be obtained. In addition, according to the preferred method for producing the solid electrolyte of this embodiment, the moldability for obtaining the solid electrolyte is improved by using an acrylic polymerizable compound and a photopolymerization initiator as a binder composition for obtaining an acrylic polymer. The reason for the improved moldability is considered as follows. In the method for producing the solid electrolyte of this embodiment, the solid electrolyte can be easily obtained without applying a strong shear force when mixing raw materials for obtaining the solid electrolyte. Therefore, in the method for producing the solid electrolyte of this embodiment, the moldability is improved.

[0063] (Process 1) Step 1 is a step of mixing raw materials for obtaining a solid electrolyte to obtain a mixture. In step 1, first, as raw materials for obtaining a solid electrolyte, an electrolyte solution containing the above-mentioned lithium salt and carbonate-based solvent, the above-mentioned metal oxide particles, and the above-mentioned acrylic polymerizable compound and photopolymerization initiator are prepared. As the electrolyte solution, an electrolyte solution having a viscosity of 7 mPa·s or more at 23°C is prepared. Next, these raw materials are weighed in the desired amount. Then, the weighed raw materials are mixed to prepare a mixture. The mixture may be prepared by stirring the raw materials using a known stirring device or the like. In the method for producing a solid electrolyte according to this embodiment, the mixture is prepared without applying a strong shear force.

[0064] In step 1, when the metal oxide particles, the electrolyte, and the acrylic polymerizable compound and photopolymerization initiator as the binder composition are mixed, for example, it is preferable to mix them in the following ratio: When the total content of the metal oxide particles, the electrolyte, and the binder composition is 100 mass%, the mixing ratio of the metal oxide particles, the electrolyte, and the binder composition is, for example, preferably, 4 mass% to 16 mass%, the electrolyte 77 mass% to 90 mass%, and the binder composition 3 mass% to 10 mass%, based on mass.

[0065] In the binder composition, when the total content of the acrylic polymerizable compound and the photopolymerization initiator is taken as 100 mol %, the content of the acrylic polymerizable compound is preferably, for example, 90 mol % or more and 99.9 mol % or less, and the content of the photopolymerization initiator is preferably 0.1 mol % or more and 10 mol % or less.

[0066] (Process 2) Step 2 is a step of obtaining a molded product from the mixture prepared in step 1. In step 2, the mixture prepared in step 1 is molded to obtain a molded product. The molding of the mixture is not particularly limited, and may be molded, for example, by applying the mixture to the surface of a support to form a coating film. The mixture may also be molded, for example, by compression molding in a mold exhibiting releasability. The mold exhibiting releasability may be, for example, a release film having a surface treated with a release agent.

[0067] (Step 3) Step 3 is a step of obtaining a solid electrolyte from the molded product obtained in step 2. In step 3, the molded product obtained in step 2 is irradiated with ultraviolet light, whereby the acrylic polymerizable compound is cured to form an acrylic polymer. Then, a solid electrolyte containing the above-mentioned electrolytic solution, the above-mentioned metal oxide particles, and the cured acrylic polymer is obtained. The device for irradiating the molded product with ultraviolet light is not particularly limited, and may be any device that cures the acrylic polymerizable compound. For example, the device for irradiating ultraviolet light may be a device equipped with an ultraviolet LED lamp, a device equipped with a high-pressure mercury lamp, or a device equipped with a metal halide lamp.

[0068] The conditions for irradiating the molded body with ultraviolet (UV) rays are not particularly limited, and may be any conditions under which the acrylic polymerizable compound can be cured. The maximum illuminance and integrated light quantity when irradiating the ultraviolet rays may be, for example, as follows. The maximum illuminance is, for example, 5 mW / cm 2 or more, 10 mW / cm 2 or more, 50 mW / cm 2 The maximum illuminance may be 1000 mW / cm or more. 2 may be less than 700 mW / cm 2 may be less than 500 mW / cm 2 The integrated light amount may be, for example, 50 mJ / cm 2 or more, 100 mJ / cm 2 or more, 500 mJ / cm 2 The integrated light amount may be 5000 mJ / cm or more.2 may be less than 3000 mJ / cm 2 or less than 2000 mJ / cm 2 It may be the following.

[0069] A solid electrolyte according to an example of the present embodiment is obtained through the above steps 1, 2, and 3. That is, the above steps provide a solid electrolyte that contains a lithium salt, an electrolyte solution containing a carbonate-based solvent, metal oxide particles, and a binder containing an acrylic polymer, and that has a viscosity of 7 mPa s or more at 23° C. as measured in accordance with JIS Z 8803:2011.

[0070] [battery] Next, the battery according to this embodiment will be described.

[0071] The battery according to the present embodiment includes the solid electrolyte according to the present embodiment. In the present embodiment, it is preferable that the solid electrolyte according to the present embodiment is included as a constituent material of the electrolyte layer of the battery. The battery is composed of an anode, a cathode, and an electrolyte layer disposed between the anode and the cathode. By adopting such a configuration, a battery excellent in each characteristic can be obtained. In addition, the battery is preferably a secondary battery, and more preferably a lithium ion secondary battery. The various members included in the lithium ion secondary battery according to the present embodiment are not particularly limited, and for example, materials generally used in batteries can be used.

[0072] The present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES

[0073] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The measurements and evaluations in the following examples and comparative examples were performed by the methods shown below.

[0074] [Measurement of electrolyte viscosity] The viscosity of the electrolyte was measured at 23°C using a vibration viscometer (VM-10A-L, manufactured by Sekonic Corporation) in accordance with JIS Z 8803:2011. The vibration viscometer was calibrated at 23°C using a standard solution for viscometer calibration in accordance with JIS Z 8809:2011. Three types of standard solutions for viscometer calibration, JS2.5, JS50, and JS200 manufactured by Nippon Grease Co., Ltd., were used.

[0075] [Measurement of ionic conductivity of solid electrolytes] The solid electrolyte membrane was cut into a circle with a diameter of 6 mm, sandwiched between two stainless steel plates as electrodes, and the impedance between the stainless steel plates was measured. For the measurement, an AC impedance method was used in which an AC voltage (applied voltage of 10 mV) is applied between the electrodes to measure the resistance component, and the ionic conductivity was calculated from the real impedance intercept of the obtained Cole-Cole plot. A potentiostat / galvanostat (VMP-300, manufactured by Biologic) was used for the measurement. Ionic conductivity (σ A ) was calculated using the following formula (F1). σ A =L A / (R A ×S A ) · · · (F1) In formula (F1), σ A is the ionic conductivity (unit: S cm -1 ), R A is resistance (unit: Ω), S A is the cross-sectional area of ​​the solid electrolyte membrane at the time of measurement (unit: cm 2 ), L A indicates the distance between electrodes (unit: cm). The measurement temperature was 25°C. The ionic conductivity (σ A ) was calculated.

[0076] [Measurement of ionic conductivity of electrolyte] A circular mesh cloth with a diameter of 19 mm (α-UX SCREEN 150-035 / 380TW, manufactured by NBC Meshtec Co., Ltd.) was used as a separator. The separator was impregnated with an electrolyte prepared by mixing the lithium salt and carbonate-based solvent used in the examples or comparative examples in a prescribed manner, and sandwiched between two stainless steel plates with a diameter of 16 mm as electrodes, and the impedance between the stainless steel plates was measured. For the measurement, an AC impedance method was used in which an AC voltage (applied voltage of 10 mV) is applied between the electrodes to measure the resistance component, and the ionic conductivity was calculated from the real impedance intercept of the obtained Cole-Cole plot. For the measurement, a potentiostat / galvanostat (VMP-300 manufactured by Biologic Co., Ltd.) was used. Ionic conductivity (σ B ) was calculated using the following formula (F2). σ B =L B / (R B ×S B ) · · · (F2) In formula (F2), σ B is the ionic conductivity (unit: S cm -1 ), R B is resistance (unit: Ω), S B is the cross-sectional area of ​​the electrode (unit: cm 2 ), L B indicates the distance between electrodes (unit: cm). The measurement temperature was 25°C. The ionic conductivity (σ B ) was calculated.

[0077] [Stability evaluation for lithium metal (dissolution and precipitation test)] The solid electrolyte membrane was cut into a circle with a diameter of 19 mm, and sandwiched between two lithium metal electrodes to prepare a lithium symmetric cell. The lithium metal electrode had a diameter of 16 mm. The current density was 3 mA / cm at a temperature of 25°C. 2 The oxidation current was 3 mAh / cm 2 After that, the reduction current was increased to 3 mAh / cm 2This series of operations was repeated 200 times, and the voltage change after 200 cycles was measured. This voltage measurement was used to investigate the dissolution and deposition behavior of lithium metal. It can be confirmed that the device is stable with respect to lithium metal when dissolution and deposition are repeated at a constant voltage without short circuits. The number of cycles in which the device operated at a potential within ±20mV of the voltage of the initial cycle was taken as the number of stable operation cycles, and the stability of each example with respect to lithium metal was compared.

[0078] [Lithium ion transport number measurement] The obtained solid electrolyte membrane was cut into a circle with a diameter of 6 mm, and sandwiched between two lithium plates as electrodes to prepare a cell. The cell was then connected to a potentiostat / galvanostat (VMP-300, manufactured by Biologic) and measurement was started after 2 hours or more had elapsed at 25°C. The measurement was first performed by complex impedance measurement, and the resistance value (R0) was calculated. Then, a voltage of 30 mV was applied and DC polarization measurement was performed. The initial current value (I0) and the steady-state current value (I S After checking the steady-state current, the complex impedance was measured again to obtain the resistance value (R S The lithium ion transport number (t + ) was calculated by the following formula (F3) (Evans' formula). t + =Is(ΔV-I0×R0) / I0(ΔV-I S ×R S ) · · · (F3) In formula (F3), ΔV is the applied voltage, R0, R S , I0 and I S is the same as above.

[0079] [Example 1] Lithium bis(fluorosulfonyl)imide (LiFSI) was prepared as the lithium salt. Dimethyl carbonate (DMC) was prepared as the carbonate-based solvent. Fumed silica particles (AEROSIL® 380, Nippon Aerosil Co., Ltd., specific surface area by BET method: 350 m) were prepared as the metal oxide particles. 2 / g-410m 2 / g) was prepared. To obtain the acrylic polymer that constitutes the binder, methyl acrylate (component (A)) and 1,9-bis(acryloyloxy)nonane (component (B)) were prepared as acrylic polymerizable compounds, and 1-hydroxycyclohexyl phenyl ketone was prepared as a photopolymerization initiator. Here, methyl acrylate (component (A)) corresponds to a monofunctional (meth)acrylate compound, and the reaction rate constant k p is 720 L·mol -1 ·s -1 It was.

[0080] In Table 1, methyl acrylate is represented as "MA" and 1,9-bis(acryloyloxy)nonane is represented as "1,9-NDDA." In the following examples, the same components (A) and (B) are represented in Table 1 in the same manner.

[0081] Lithium bis(fluorosulfonyl)imide (LiFSI) and dimethyl carbonate (DMC) were weighed out to a molar ratio of 1 / 2 (=LiFSI / DMC) and thoroughly stirred to prepare an electrolyte. Methyl acrylate and 1,9-bis(acryloyloxy)nonane were weighed out to a molar ratio of 95 / 5 (=methyl acrylate / 1,9-bis(acryloyloxy)nonane) and then mixed to prepare an acrylic polymerizable compound mixture. Furthermore, the acrylic polymerizable compound mixture and 1-hydroxycyclohexyl phenyl ketone as a photopolymerization initiator were mixed to a molar ratio of 97 / 3 (=acrylic polymerizable compound / photopolymerization initiator) to prepare a binder composition. Next, when the total of the fumed silica particles, the electrolyte, and the binder composition was taken as 100% by mass, the mixture was weighed out to be 15% by mass / 82% by mass / 3% by mass (=fumed silica particles / electrolyte solution / binder composition), and mixed thoroughly to obtain a mixture for forming a solid electrolyte membrane.

[0082] Thereafter, the mixture for forming the solid electrolyte membrane was compression molded on a release film (manufactured by Lintec Corporation, product name "PET38AL-5") to a thickness of 100 μm to obtain a molded product. This molded product was irradiated with ultraviolet (UV) rays [maximum illuminance: 180 mW / cm 2 , Accumulated light intensity: 1000mJ / cm 2 The measurement was performed using an illuminance actinometer manufactured by Eye Graphics (controller: EYE UV METER UVPF-A2, light receiver: EYE UV METER PD-365A2), and the binder composition was cured to obtain a solid electrolyte membrane containing a binder containing an acrylic polymer. In the solid electrolyte membrane of Example 1, when the total content of the fumed silica particles, the electrolyte, and the binder containing an acrylic polymer is taken as 100 mass%, the respective contents of the fumed silica particles, the electrolyte, and the binder containing an acrylic polymer are as shown in Table 1.

[0083] [Example 2] A solid electrolyte membrane was produced in the same manner as in Example 1, except that lithium bis(fluorosulfonyl)imide (LiFSI) and dimethyl carbonate (DMC) were weighed out to have a molar ratio of 1 / 3 (=LiFSI / DMC) and thoroughly stirred to prepare an electrolyte solution.

[0084] [Example 3] Lithium borofluoride (LiBF4) was prepared as the lithium salt. A solid electrolyte membrane was produced in the same manner as in Example 1, except that lithium borofluoride (LiBF4) and dimethyl carbonate (DMC) were weighed out to have a molar ratio of 1 / 2 (=LiBF4 / DMC) and thoroughly stirred to prepare an electrolyte solution.

[0085] [Example 4] Lithium borofluoride (LiBF4) was prepared as the lithium salt. A solid electrolyte membrane was produced in the same manner as in Example 1, except that lithium borofluoride (LiBF4) and dimethyl carbonate (DMC) were weighed out to have a molar ratio of 1 / 3 (=LiBF4 / DMC) and thoroughly stirred to prepare an electrolyte solution.

[0086] [Example 5] As a carbonate-based solvent, propylene carbonate (PC) was prepared. A solid electrolyte membrane was produced in the same manner as in Example 1, except that lithium bis(fluorosulfonyl)imide (LiFSI) and propylene carbonate (PC) were weighed out to have a molar ratio of 1 / 2 (=LiFSI / PC) and thoroughly stirred to prepare an electrolyte solution.

[0087] [Comparative Example 1] A solid electrolyte membrane was produced in the same manner as in Example 1, except that lithium bis(fluorosulfonyl)imide (LiFSI) and dimethyl carbonate (DMC) were weighed out to have a molar ratio of 1 / 12 (=LiFSI / DMC) and thoroughly stirred to prepare an electrolyte solution, but no membrane was obtained.

[0088] [Comparative Example 2] A solid electrolyte membrane was produced in the same manner as in Example 1, except that lithium bis(fluorosulfonyl)imide (LiFSI) and dimethyl carbonate (DMC) were weighed out to have a molar ratio of 1 / 6 (=LiFSI / DMC) and thoroughly stirred to prepare an electrolyte solution, but no membrane was obtained.

[0089] [Comparative Example 3] Lithium borofluoride (LiBF4) was prepared as the lithium salt. A solid electrolyte membrane was produced in the same manner as in Example 1, except that lithium borofluoride (LiBF4) and dimethyl carbonate (DMC) were weighed out to have a molar ratio of 1 / 12 (=LiBF4 / DMC) and thoroughly stirred to prepare an electrolyte solution, but no membrane was obtained.

[0090] [Comparative Example 4] Lithium borofluoride (LiBF4) was prepared as the lithium salt. A solid electrolyte membrane was produced in the same manner as in Example 1, except that lithium borofluoride (LiBF4) and dimethyl carbonate (DMC) were weighed out to have a molar ratio of 1 / 6 (=LiBF4 / DMC) and thoroughly stirred to prepare an electrolyte solution, but no membrane was obtained.

[0091] [Comparative Example 5] Lithium bis(fluorosulfonyl)imide (LiFSI) was prepared as the lithium salt. Tetraethylene glycol dimethyl ether (G4) was prepared as the solvent. Fumed silica particles (AEROSIL (registered trademark) 380, Nippon Aerosil Co., Ltd., specific surface area by BET method 350 m) were prepared as the metal oxide particles. 2 / g-410m 2 As a binder, polytetrafluoroethylene (PTFE) was prepared.

[0092] Lithium bis(fluorosulfonyl)imide (LiFSI) and tetraethylene glycol dimethyl ether (G4) were weighed out to a molar ratio of 1 / 1 (=LiFSI / G4) and thoroughly stirred to prepare an electrolyte solution. Next, the electrolyte solution and fumed silica particles were weighed out to a mass ratio of 80 / 20 (=electrolyte solution / fumed silica particles) and thoroughly mixed. Furthermore, 5 parts by mass of polytetrafluoroethylene (PTFE) were added to a total of 100 parts by mass of the electrolyte solution and the fumed silica particles, and thoroughly mixed using an agate mortar. Then, the mixture was compression molded on a fluororesin mold to obtain a solid electrolyte membrane. In the solid electrolyte membrane of Comparative Example 5, when the total content of the fumed silica particles, the electrolyte solution, and the binder was taken as 100% by mass, the respective contents of the fumed silica particles, the electrolyte solution, and the binder were as shown in Table 1.

[0093] [Comparative Example 6] As the lithium salt, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was prepared. A solid electrolyte membrane was produced in the same manner as in Example 1, except that lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and dimethyl carbonate (DMC) were weighed out to have a molar ratio of 1 / 6 (=LiTFSI / DMC) and thoroughly stirred to prepare an electrolyte solution, but no membrane was obtained.

[0094] [Comparative Example 7] As a carbonate solvent, diethyl carbonate (DEC) was prepared. A solid electrolyte membrane was produced in the same manner as in Example 1, except that lithium bis(fluorosulfonyl)imide (LiFSI) and diethyl carbonate (DEC) were weighed out to have a molar ratio of 1 / 6 (=LiFSI / DEC) and the electrolyte solution was prepared by thoroughly stirring. However, no membrane was obtained.

[0095] [Evaluation of electrolyte viscosity and solid electrolyte] The viscosity of the electrolyte solutions used in Examples 1 to 5 and Comparative Example 5 was measured according to the above-mentioned viscosity measurement method. In addition, the above-mentioned dissolution and deposition test, ion conductivity measurement, and lithium ion transport number measurement were performed on the solid electrolyte membranes obtained in Examples 1 to 5 and Comparative Example 5. The above-mentioned ion conductivity measurement of the electrolyte solution was performed for each Example and Comparative Example 5.

[0096] The composition of the solid electrolyte membrane of each example is shown in Table 1, and the results of the dissolution / precipitation test, ion conductivity measurement, and lithium ion transport number measurement are shown in Table 2. In Table 1, Li salt refers to lithium salt, and solvent refers to carbonate-based solvent.

[0097] [Table 1]

[0098] [Table 2]

[0099] In each of the comparative examples in which the viscosity of the electrolyte was less than 7 mPa·s, a solid electrolyte film could not be obtained.

[0100] As a result of the dissolution and deposition test, it can be seen that each Example operated stably for 200 cycles or more. In contrast, the Comparative Example operated for less than 200 cycles. In the Comparative Example, the voltage increased with the progress of cycles, and the device did not operate stably.

[0101] As for the results of the lithium ion transport number, it can be seen that the lithium ion transport number of each example exceeds 0.5. In general, the lithium ion transport number of an ionic liquid-based electrolyte tends to be low. For example, the lithium ion transport number of an ionic liquid-based electrolyte is 0.5 or less. And, the lithium ion transport number of Comparative Example 5 was 0.35. In contrast, it can be seen that the solid electrolyte of each example has an advantage.

[0102] From the above, it was found that the solid electrolyte membranes obtained in each Example were easily formed into a membrane. In addition, it was found that the properties of the transport number of lithium ions, ion conductivity, and stability against lithium metal were high compared to the solid electrolyte membrane obtained in Comparative Example 5. From this, it was confirmed that the solid electrolyte of the present invention is easy to form into a membrane of the solid electrolyte, and has high transport number of lithium ions, ion conductivity, and stability against lithium metal.

Claims

1. an electrolyte solution including a lithium salt and a carbonate-based solvent; Metal oxide particles; Contains The viscosity of the electrolyte at 23°C measured in accordance with JIS Z 8803:2011 is 7 mPa s or more; solid electrolyte.

2. The solid electrolyte according to claim 1, The lithium salt is at least one selected from the group consisting of lithium bis(fluorosulfonyl)imide and lithium borofluoride. solid electrolyte.

3. The solid electrolyte according to claim 1 or 2, The carbonate-based solvent is at least one selected from the group consisting of dimethyl carbonate and propylene carbonate. solid electrolyte.

4. The solid electrolyte according to any one of claims 1 to 3, The molar ratio of the lithium salt to the carbonate-based solvent contained in the electrolytic solution (lithium salt / carbonate-based solvent) is 1 / 4 or more and 1 / 1 or less. solid electrolyte.

5. The solid electrolyte according to any one of claims 1 to 4, The metal oxide particles are silica particles. solid electrolyte.

6. The solid electrolyte according to any one of claims 1 to 5, The specific surface area of ​​the metal oxide particles measured by the BET method is 160 m 2 / g or more 700m 2 / g or less, solid electrolyte.

7. The solid electrolyte according to any one of claims 1 to 6, Further containing a binder, solid electrolyte.

8. The solid electrolyte according to claim 7, The binder contains an acrylic polymer. solid electrolyte.

9. The solid electrolyte according to claim 8, the acrylic polymer contains a structural unit derived from an acrylic polymerizable compound, The acrylic polymerizable compound has a reaction rate constant k p is 700 L / mol -1 ・s -1 The monofunctional (meth)acrylate compound is solid electrolyte.

10. The solid electrolyte according to claim 9, The acrylic polymerizable compound further includes a polyfunctional (meth)acrylate compound other than the monofunctional (meth)acrylate compound. solid electrolyte.

11. The solid electrolyte according to claim 10, The polyfunctional (meth)acrylate compound is at least one selected from the group consisting of 1,9-bis(acryloyloxy)nonane, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate. solid electrolyte.

12. The solid electrolyte according to claim 10 or 11, the structural unit derived from the acrylic polymerizable compound includes at least one selected from the group consisting of a structural unit derived from the monofunctional (meth)acrylate compound and a structural unit derived from the polyfunctional (meth)acrylate compound, When the total of the structural units derived from the monofunctional (meth)acrylate compound and the structural units derived from the polyfunctional (meth)acrylate compound is 100 mol %, The content of the structural unit derived from the monofunctional (meth)acrylate compound is 90 mol % or more and 100 mol % or less, The content of the structural unit derived from the polyfunctional (meth)acrylate compound is 0 mol% or more and 10 mol% or less. solid electrolyte.

13. The solid electrolyte according to any one of claims 1 to 12 is provided. battery.

14. A method for producing the solid electrolyte according to any one of claims 8 to 12, comprising the steps of: mixing the electrolytic solution, the metal oxide particles, the acrylic polymerizable compound, and a photopolymerization initiator to prepare a mixture; shaping the mixture to obtain a shaped product; a step of irradiating the molded product with ultraviolet light to obtain a solid electrolyte containing the acrylic polymer in which the acrylic polymerizable compound is cured; Equipped with A method for producing a solid electrolyte.

Citation Information

Patent Citations

  • Pseudo solid electrolyte, and all-solid lithium secondary battery arranged by use thereof

    JP2017059432A