Dispersing recovery method of metallic compound particulate in ferrous material, analysis method of metallic compound particulate in ferrous material, and electrolyte for electrolytic extraction of ferrous material
By using a solvent with a specific Hansen solubility parameter distance in the electrolytic solution and applying ultrasonic waves, the method stabilizes the dispersion and recovery of metal compound fine particles, addressing incomplete recovery and aggregation issues in electrolytic extraction, thereby enhancing the accuracy of quantitative analysis.
Patent Information
- Application Number
- JP2023073601
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Existing electrolytic extraction methods for metal compound fine particles in steel materials result in incomplete recovery and aggregation, leading to inaccurate quantitative analysis due to particles remaining in the electrolytic solution.
The method involves immersing a steel material and a counter electrode in an electrolytic solution, applying ultrasonic waves to detach particles, and using a solvent with a Hansen solubility parameter distance Ra of 8.0 (J/cm 3 ) 1/2 to stabilize dispersion and recovery, ensuring the particles remain dispersed for analysis.
This approach allows for stable dispersion and recovery of metal compound fine particles without loss, improving the accuracy of quantitative analysis by preventing agglomeration and enabling effective size measurement and component analysis.
Smart Images

Figure 2024158416000003 
Figure 2024158416000004 
Figure 2024158416000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for dispersing and recovering fine metal compound particles in a steel material, a method for analyzing fine metal compound particles in a steel material, and an electrolytic solution for electrolytic extraction of a steel material. [Background technology]
[0002] The size, quantity, and chemical composition of inclusions and precipitates (hereinafter referred to as metal compound particles) contained in steel materials have a significant effect on the properties of the steel material. For example, relatively large metal compound particles with a particle size on the order of several tens of micrometers are considered to be harmful and degrade the properties of steel materials. On the other hand, in recent years, technology has been developed to improve various properties of steel materials by actively using metal compound particles on the order of a micrometer or smaller to control the structure of steel. Accordingly, there is an increasing need to appropriately perform quantitative analysis and particle size distribution measurement of tiny metal compound particles in steel materials.
[0003] To meet these needs, it is necessary to prepare a solution in which metal compound fine particles are stably dispersed in a solvent. Therefore, attempts have been made to prepare a dispersion liquid in which metal compound fine particles are dispersed by carrying out a step of extracting and separating the metal compound fine particles from a steel material and a step of dispersing the extracted and separated metal compound fine particles in a liquid.
[0004] As a method for extracting and separating metal compound particles in steel, electrolytic extraction using a non-aqueous electrolyte is known. In electrolytic extraction, a steel material is used as an anode, a platinum electrode is used as a cathode, and the anode and cathode are immersed in a non-aqueous electrolyte, and electrolysis is performed to dissolve the iron, which is the matrix of the steel material, and extract the metal compound particles.
[0005] The electrolytic extraction method of steel materials using a non-aqueous electrolyte has the advantage that metal compound fine particles can be selectively extracted by selecting a solvent and potential according to the substance to be extracted. For example, Non-Patent Document 1 describes a non-aqueous solvent electrolyte solution containing 10% acetylacetone (AA) or 4% methyl salicylate-1% salicylic acid (MS) as an iron chelating agent and 1% tetramethylammonium chloride (TMAC) as a supporting electrolyte as an electrolyte solution used in the electrolytic extraction method of steel materials. In these electrolyte solutions, the extracted metal compound fine particles may aggregate in the electrolyte solution, so in order to measure the size of the metal compound fine particles, it is necessary to disperse the metal compound fine particles in the dispersion solution by immersing a steel sample in a suitable dispersion solution and applying ultrasonic waves.
[0006] However, in the past, it was thought that most of the metal compound fine particles were attached to the surface of the steel material immediately after electrolytic extraction and were recovered in this state in the dispersion solution. However, recently, however, a problem has become apparent in which some of the metal compound fine particles fall off from the surface of the steel material during the electrolytic extraction process and remain in the electrolytic solution, and not all of them are recovered in the dispersion solution, resulting in low quantitative analysis values in the subsequent analysis stage. [Prior art documents] [Non-patent literature]
[0007] [Non-Patent Document 1] "Sample Analysis Course: Steel Analysis", edited by the Japan Society for Analytical Chemistry, Maruzen Publishing Co., Ltd., published on September 15, 2011, p.91, p.101 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above circumstances, and has as its object to provide a method for dispersing and recovering metal compound fine particles in steel material, which is capable of stably dispersing and recovering metal compound fine particles extracted from steel material by electrolytic extraction without loss, a method for analyzing metal compound fine particles in steel material, and an electrolytic solution for electrolytic extraction of steel material. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention employs the following configuration. [1] An electrolysis step of immersing an electrode including a steel material and a counter electrode in an electrolytic solution to electrolyze the steel material; a dispersion step of applying ultrasonic waves to the electrolytic solution while the steel material is immersed in the electrolytic solution to detach metal compound fine particles from the surface of the steel material, thereby dispersing the metal compound fine particles in the electrolytic solution. [2] The method for dispersing and recovering metal compound fine particles in a steel material according to [1], wherein the electrolytic solution has a function of dispersing the metal compound fine particles. [3] Following the electrolysis step, the Hansen solubility parameter distance Ra (Equation (1)) between the electrolytic solution and all of the metal compound fine particles to be dispersed and recovered is 8.0 (J / cm 3 ) 1 / 2 A method for dispersing and recovering metal compound fine particles in a steel material according to [1], comprising a dispersion liquid preparation step of adding an arbitrary solvent so as to obtain the following: R a = [4(δ d1 -δ d2 ) 2 +(δ p1 -δ p2 ) 2 +(δ h1 -δ h2 ) 2 ] 1 / 2 …(1) However, δ in formula (1) d1 is the London dispersion force of the metal compound fine particles, δ p1 is the dipole-dipole force of the metal compound fine particles, δ h1is the hydrogen bonding strength of the metal compound fine particles, δ d2 is the London dispersion force of the solvent, δ p2 is the dipole-dipole force of the solvent, δ h2 is the hydrogen bonding strength of the solvent. [4] An electrolysis step of immersing an electrode including a steel material and a counter electrode in an electrolytic solution to electrolyze the steel material; a dispersion step of applying ultrasonic waves to the electrolytic solution while the steel material is immersed in the electrolytic solution to detach metal compound fine particles from the surface of the steel material, thereby dispersing the metal compound fine particles in the electrolytic solution, The Hansen solubility parameter distance Ra (Equation (1)) between the electrolyte and all of the metal compound fine particles to be dispersed and recovered is 8.0 (J / cm 3 ) 1 / 2 A method for dispersing and recovering metal compound fine particles in a steel material, comprising the following solvent: R a = [4(δ d1 -δ d2 ) 2 +(δ p1 -δ p2 ) 2 +(δ h1 -δ h2 ) 2 ] 1 / 2 …(1) However, δ in formula (1) d1 is the London dispersion force of the metal compound fine particles, δ p1 is the dipole-dipole force of the metal compound fine particles, δ h1 is the hydrogen bonding strength of the metal compound fine particles, δ d2 is the London dispersion force of the solvent, δ p2 is the dipole-dipole force of the solvent, δ h2 is the hydrogen bonding strength of the solvent. [5] The method for dispersing and recovering metal compound fine particles in a steel material according to [1] or [4], wherein the electrolytic solution contains a complexing agent that forms a complex with iron. [6] A method for analyzing metal compound microparticles in a steel material, comprising an analysis step of analyzing the electrolytic solution containing the metal compound microparticles obtained by the method for dispersing and recovering metal compound microparticles in a steel material described in [1] or [4]. [7] The analyzing step includes a step of subjecting the electrolytic solution in which the metal compound fine particles are dispersed to a field flow fractionation method, thereby separating the metal compound fine particles according to particle size; and analyzing the components of the metal compound fine particles separated by particle size. [8] The analyzing step includes a step of removing a liquid phase component from the electrolytic solution in which the metal compound fine particles are dispersed, while leaving the metal compound fine particles in the electrolytic solution, thereby preparing a sample for observation by an electron microscope containing the metal compound fine particles; The method for analyzing metal compound fine particles in a steel material according to [6], further comprising a step of observing the sample under an electron microscope. [9] An electrolytic solution for immersing an electrode containing a steel material and a counter electrode in the solution, electrolyzing the steel material to extract metal compound fine particles contained in the steel material, and dispersing the metal compound fine particles; The electrolytic solution has a Hansen solubility parameter distance R a (Equation (1)) is 8.0 (J / cm 3 ) 1 / 2 Electrolyte solution for electrowinning of steel materials, comprising a solvent in which the concentration is less than 100%. R a = [4(δ d1 -δ d2 ) 2 +(δ p1 -δ p2 ) 2 +(δ h1 -δ h2 ) 2 ] 1 / 2 …(1) However, δ in formula (1) d1 is the London dispersion force of the metal compound fine particles, δ p1 is the dipole-dipole force of the metal compound fine particles, δ h1 is the hydrogen bonding strength of the metal compound fine particles, δ d2 is the London dispersion force of the solvent, δ p2 is the dipole-dipole force of the solvent, δ h2 is the hydrogen bonding strength of the solvent.
[10] An electrolytic solution for electrowinning of steel materials according to [9], having a relative dielectric constant of 30 or more at 25°C. Effect of the Invention
[0010] According to the present invention, it is possible to provide a method for dispersing and recovering metal compound fine particles in steel material, which is capable of stably dispersing and recovering metal compound fine particles extracted from steel material by electrolytic extraction without loss, a method for analyzing metal compound fine particles in steel material, and an electrolytic solution for electrolytic extraction of steel material. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing the main parts of a field-flow fractionation device. [Figure 2A] Figure 2A shows the Hansen space and Hansen solubility sphere created when determining the Hansen solubility parameter of AlN. [Figure 2B] Figure 2B shows the Hansen space and Hansen solubility sphere created when determining the Hansen solubility parameter of TiN. [Diagram 3] Figure 3 shows the electrolysis potential-current curves when LSV measurements were performed using various pellet samples as the working electrode (WE) (electrolysis solution: 5 vol.% acetylacetone (AA)-1 mass% tetramethylammonium chloride (TMAC)-79 vol.% N,N'-dimethylformamide (DMF)-16 vol.% water). [Figure 4] FIG. 4 is a graph showing the results of FFF-ICP mass spectrometry in Example 1 and Comparative Example 1, and shows the ion intensity at m / z=27. [Diagram 5] FIG. 5 is a graph showing the results of FFF-ICP mass spectrometry in Example 1 and Comparative Example 1, and shows the ion intensity at m / z=93. [Figure 6] FIG. 6 is a photograph showing AlN and NbN remaining in the electrolytic solution used in the comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The inventors of the present invention have paid attention to the Hansen solubility parameter while investigating an electrolytic solution capable of electrolytically extracting metal compound particles contained in steel materials and stably dispersing the extracted metal compound particles without agglomeration. Hansen solubility parameter δ t is an index used to predict the solubility of a substance. It is a further decomposition of the solubility parameter (cohesive energy density) defined by Hildebrand into three components and can be expressed by the following formula (A).
[0013] δ t =(δ d 2 +δ p 2 +δ h 2 ) 1 / 2 …(A)
[0014] In formula (A), δ d is the London dispersion force between molecules, δ p is the dipole-dipole force between molecules, δ h is the hydrogen bonding strength between molecules.
[0015] In general, the solubility parameter is defined by regarding the intermolecular forces in a solution as the parameter of dissolving power, and the energy required to mix two components, ΔE M can be expressed as the difference between the cohesive energy when component 1 and component 2 exist as pure substances and the cohesive energy when they are a mixture of component 1 and component 2. In other words, if the solubility parameters of two substances are known, the closer these values are, the smaller the energy required for mixing will be, and the easier it will be to dissolve.
[0016] The three parameters in formula (A) can be considered as coordinates in a three-dimensional space (Hansen space). When the Hansen solubility parameters of two substances are placed in the Hansen space, it is suggested that the closer the distance between the two points, the easier it is for them to dissolve in each other. The distance between the two points is the Hansen solubility parameter distance R shown in formula (B) below. aIt can be expressed as:
[0017] R a = [4(δ d1 -δ d2 ) 2 +(δ p1 -δ p2 ) 2 +(δ h1 -δ h2 ) 2 ] 1 / 2 …(B)
[0018] δ in formula (B) d1 is the London dispersion force of component 1, δ p1 is the dipole-dipole force of component 1, δ h1 is the hydrogen bond strength of component 1, δ d2 is the London dispersion force of component 2, δ p2 is the dipole-dipole force of component 2, δ h2 is the hydrogen bonding strength of component 2.
[0019] Hansen Solubility Parameter Distance R a As mentioned above, the Hansen solubility parameter R is used to predict the solubility of a substance, particularly to evaluate the compatibility between organic materials, but the inventors have investigated its use as a parameter to evaluate the coagulation of metal compound particles contained in steel materials. As a result, the Hansen solubility parameter distance R between the target metal compound particles and the solvent of the selected candidate electrolyte solution was a It has been found that when the molecular weight of the metal compound falls within a predetermined range, the metal compound fine particles are dispersed in the solvent without agglomerating.
[0020] Hansen Solubility Parameter Distance R aThe electrolytic solution containing a solvent having a specific range allows for electrolytic extraction of steel materials, and allows the electrolytically extracted metal compound fine particles to be dispersed in the electrolytic solution as they are. The electrolytic solution in which the metal compound fine particles are dispersed can be used as it is as a sample for various analytical methods. That is, the conventional electrolytic solution allows for electrolytic extraction, but the metal compound fine particles are aggregated, so that it is necessary to transfer the steel material after electrolytic extraction from the electrolytic solution to another dispersion solvent and then disperse the metal compound fine particles in the dispersion solvent. However, in the present invention, the metal compound fine particles can be dispersed in the electrolytic solution without agglomeration, making such an operation unnecessary, and the electrolytic solution in which the metal compound fine particles are dispersed can be used as a sample for various analytical methods, for example, as a test solution for the field flow fractionation method, as a sample for preparing a sample by the support film method of a transmission electron microscope, and further as a sample for component analysis of the metal compound fine particles. As a result, even if some of the metal compound microparticles fall off from the surface of the steel material during the electrolysis process and remain in the electrolytic solution, the entire amount of the electrolytically extracted metal compound microparticles can be dispersed and recovered, preventing low quantitative analysis values in the subsequent analysis stage and improving the accuracy of size measurement of the metal compound microparticles and the quantitative accuracy of number density distribution evaluation.
[0021] The following describes embodiments of the present invention, namely, a method for dispersing and recovering metal compound microparticles in steel material (hereinafter sometimes referred to as the dispersion and recovery method), a method for analyzing metal compound microparticles in steel material (hereinafter sometimes referred to as the analysis method), and an electrolytic solution for electrolytic extraction of steel material.
[0022] The dispersion and recovery method of this embodiment includes an electrolysis process in which an electrode containing a steel material and a counter electrode are immersed in an electrolytic solution to electrolyze the steel material, and a dispersion process in which, while the steel material is immersed in the electrolytic solution, ultrasonic waves are applied to the electrolytic solution to detach metal compound fine particles from the surface of the steel material and disperse the metal compound fine particles in the electrolytic solution.
[0023] The electrolytic solution used in the electrolysis step and the dispersion step must contain a solvent that disperses the metal compound fine particles to be dispersed and recovered. More specifically, the electrolytic solution must have a Hansen solubility parameter distance Ra between the electrolytic solution and all of the metal compound fine particles to be dispersed and recovered, as shown in the following formula (1), of 8.0 (J / cm 3 ) 1 / 2 It is preferred to include a solvent that is:
[0024] R a = [4(δ d1 -δ d2 ) 2 +(δ p1 -δ p2 ) 2 +(δ h1 -δ h2 ) 2 ] 1 / 2 …(1)
[0025] However, δ in formula (1) d1 is the London dispersion force of metal compound particles, δ p1 is the dipole-dipole force of the metal compound particles, δ h1 is the hydrogen bond strength of the metal compound particles, δ d2 is the London dispersion force of the solvent, δ p2 is the dipole-dipole force of the solvent, δ h2 is the hydrogen bonding strength of the solvent.
[0026] More specifically, for each metal compound particle, the Hansen solubility parameter distance R between the metal compound particle and the selected candidate solvent is a The Hansen solubility parameter distance R for each metal compound particle is calculated. a All of the above are 8.0(J / cm 3 ) 1 / 2 It is preferable to select a candidate solvent that can be used for the electrolytic solution in the following cases:
[0027] As a prerequisite, the Hansen solubility parameters of the metal compound particles and the solvent are understood.
[0028] The Hansen solubility parameters of the solvents can be any known ones, examples of which are shown in Table 1.
[0029] [Table 1]
[0030] In addition, the Hansen solubility parameter of a mixed solvent containing two or more solvents can be calculated using the following formula.
[0031] For example, for a two-component mixed solvent consisting of a% by volume of solvent A and b% by volume (a+b=100%) of solvent B, the London dispersion force of the mixed solvent δ dM , dipole-dipole force δ pM , hydrogen bond strength δ hM are calculated by the following formulas (C) to (E), respectively. In the case of a ternary mixed solvent, they are similarly multiplied by the volume fraction.
[0032] δ dM =(a×δ dA +b×δ dB ) / (a+b) …(C) δ pM =(a×δ pA +b×δ pB ) / (a+b) …(D) δ hM =(a×δ hA +b×δ hB ) / (a+b) …(E)
[0033] In formulas (C) to (E), δ dA is the London dispersion force of solvent A, δ pA is the dipole-dipole force of solvent A, δ hA is the hydrogen bonding strength of solvent A, and δ dB is the London dispersion force of solvent B, δ pB is the dipole-dipole force of solvent B, δ hB is the hydrogen bonding strength of solvent B.
[0034] The Hansen solubility parameter of the metal compound fine particles may be a known one or may be determined experimentally. An example is shown in Table 2. The units of the values in Table 2 are (J / cm 3 ) 1 / 2 It is.
[0035] [Table 2]
[0036] When the Hansen solubility parameter of metal compound particles is measured by an experiment, it may be measured by a known method. Specifically, for example, metal compound particles with a known primary particle size are added to each of the 28 types of solvents shown in Table 1, whose Hansen solubility parameters are known, and ultrasonic treatment is performed. After leaving the mixture to stand for a certain period of time (for example, 1 hour), the dispersibility of each particle, that is, whether it is dispersed or aggregated, is evaluated. The dispersibility is evaluated by using a sedimentation method or a dynamic light scattering method (for example, a Zetasizer NanoS device manufactured by Malvern).
[0037] In the case of the sedimentation method, the dispersibility is judged by measuring the Stokes diameter from the sedimentation velocity of the particles due to gravity or centrifugal force in various solvents, and if the Stokes diameter is close to the known primary particle diameter, it is evaluated as being dispersed. In the case of the dynamic light scattering method, the dispersibility is judged as being dispersed if the hydrodynamic diameter measured by a dynamic light scattering device is close to the known primary particle diameter. As the solvents for evaluating the dispersibility of metal compound microparticles, if there are at least four types of solvents that are evaluated as dispersing by the above procedure, and if the total number of solvents, including those evaluated as dispersing and those not evaluated as dispersing, is 20 or more, the Hansen solubility parameter of the metal compound microparticles can be determined with good reproducibility.
[0038] Next, the Hansen solubility parameters of the 28 types of solvents are plotted in the Hansen space. At this time, the Hansen space is made such that it is possible to distinguish between solvents in which metal compound particles are dispersed and solvents in which metal compound particles are aggregated. Then, a Hansen solubility sphere that includes all the plots of the solvents in which metal compound particles are dispersed is calculated using the least squares method. The position of the center of gravity of the Hansen solubility sphere in the Hansen space is taken as the Hansen solubility parameter of the metal compound particles. The above calculation using the Hansen space can be performed using commercially available software (software name: HSPiP, provided by: Pirika.com). The Hansen solubility parameters of the metal compound particles listed in Table 2 were calculated using the above method.
[0039] Once the Hansen solubility parameters of the solvent and metal compound particles to be selected are determined, the Hansen solubility parameter distance R between the metal compound particles and the candidate solvent for each metal compound particle that can be electrolytically extracted from the steel material is calculated. a is calculated using the above formula (1).
[0040] Next, the calculated Hansen solubility parameter distance R a All are 8.0 (J / cm 3 ) 1 / 2 Then, determine whether the total Hansen solubility parameter distance R a is 8.0(J / cm 3 ) 1 / 2 A candidate solvent is selected as a solvent for the available electrolyte solution if:
[0041] Hansen solubility parameter distance R, which is the criterion for selecting a solvent a Upper limit (8.0(J / cm 3 ) 1 / 2The values below) were determined by experiments. Specifically, various metal compound particles were added to various solvents, dispersed by applying ultrasonic vibration, and then left to stand for about 12 hours to observe whether they dispersed or settled, and the dispersion evaluation results were obtained. The dispersion evaluation results thus obtained and the Hansen solubility parameter distance R a When comparing and matching, the Hansen solubility parameter distance R a is 8.0(J / cm 3 ) 1 / 2 In the following combinations, the metal compound particles are dispersed in the solvent and reach 8.0 (J / cm 3 ) 1 / 2 It was found that in combinations of more than 100, the metal compound particles settle in the solvent (i.e., do not disperse). Therefore, the Hansen solubility parameter distance R a Upper limit (8.0(J / cm 3 ) 1 / 2 (see below) can be used as a threshold value for determining whether or not metal compound fine particles that may be contained in steel materials are dispersed in a solvent.
[0042] Hansen Solubility Parameter Distance R a The smaller the distance, the better the dispersibility of the metal compound particles in the solvent. a The upper limit is more preferably 5.0 (J / cm 3 ) 1 / 2 and even more preferably 3.0 (J / cm 3 ) 1 / 2 However, the Hansen solubility parameter distance R a If the distance R is too small, the metal compound particles may dissolve in the solvent. a is 1.0 (J / cm 3 ) 1 / 2 It may be more than that.
[0043] In this embodiment, there is a possibility that a plurality of solvents may be selected as available solvents. In that case, the selection criteria for further narrowing down the solvents may be the Hansen solubility parameter distance R aIt is preferable to select a solvent that has a smaller solubility than the solvent that has a smaller solubility. As another selection criterion for narrowing down the selection, a solvent that is easy to handle in the analysis step after the electrolysis step and the dispersion and recovery step, for example, in the field flow fractionation method or in observation with an electron microscope may be selected. A solvent that does not adversely affect the human body or the environment may also be selected.
[0044] In addition, it is preferable to select a solvent having an appropriate relative dielectric constant as the solvent for the electrolytic solution of this embodiment in order to improve the efficiency of the electrolysis process. r It is advisable to select a solvent having a relative dielectric constant ε of 30 or more, more preferably 32.7 or more. This allows the supporting electrolyte to be sufficiently dissolved in the electrolytic solution, making it possible to improve the efficiency of electrolytic extraction. r Even if the dielectric constant is less than 30, the electrolysis process can be carried out, but the electrolysis process may require a long time. There is no particular need to specify an upper limit for the dielectric constant, but since the dielectric constant of water is about 78.54, the dielectric constant condition is set to 78.54 or less. If the candidate solvent is a mixed solvent, the weighted average weighted by the volume fraction of the dielectric constant of each solvent that makes up the mixed solvent should be used as the dielectric constant of the mixed solvent.
[0045] Furthermore, the electrolytic solution of the present embodiment preferably contains a complexing agent that forms a complex with iron. As the complexing agent that forms a complex with iron, known agents such as acetylacetone, salicylic acid, maleic anhydride, citric acid, and phthalic acid can be used. In addition, the Hansen solubility parameter distance R a is 8.0(J / cm 3 ) 1 / 2 If the solvent described below contains a complexing agent that forms a complex with iron, it can be used as is.
[0046] Furthermore, the electrolytic solution of the present embodiment preferably contains an electrolyte.As the electrolyte, it is preferable to contain one or more of lithium chloride, sodium chloride, potassium chloride, magnesium chloride, calcium chloride, strontium chloride, tetramethylammonium chloride, lithium hydroxide, sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, strontium hydroxide, tetramethylammonium hydroxide, tetraethylammonium chloride, tetrabutylammonium chloride, tetrabutylammonium tetrafluoroborate, and tetrabutylammonium hexafluorophosphate.By containing these electrolytes, it is possible to impart electrical conductivity to the electrolytic solution, and it can be used as an electrolytic solution for electrolytic extraction.
[0047] The electrolyte content in the electrolytic solution is preferably in the range of 0.001 to 5.0% by mass, more preferably in the range of 0.1 to 1.0% by mass. If the electrolyte content is 0.001% by mass or more, a current necessary and sufficient for electrolysis can be applied. If the electrolyte content is 5.0% by mass or less, the electrolysis speed does not become too fast.
[0048] In addition, it may be difficult to extract all of the metal compound fine particles that may be contained in the steel material by a single electrolysis process. Therefore, the electrolysis conditions are usually set to optimal conditions for each metal compound fine particle. Therefore, in the selection method of this embodiment, a solvent for the electrolytic solution may be selected for one or more types of metal compound fine particles that can be simultaneously extracted by a single electrolysis among the metal compound fine particles that may be contained in the steel material that is the actual analysis target.
[0049] Furthermore, the Hansen solubility parameter distance Ra (J / cm) between the metal compound particles to be analyzed in the steel material and the solvent was determined as the solvent for the electrolytic solution. 3 ) 1 / 2A solvent may be selected in which the Hansen solubility parameter distance Ra between the metal compound fine particles not to be analyzed in the steel material and the solvent exceeds 8.0, and the metal compound fine particles having the Hansen solubility parameter distance Ra between the metal compound fine particles and the solvent is 8.0 or less. Here, the metal compound fine particles having the Hansen solubility parameter distance Ra between the metal compound fine particles and the solvent is 8.0 or less may be, for example, particles to be measured for particle size, and the metal compound fine particles having the Hansen solubility parameter distance Ra exceeding 8.0 may be particles for which particle size measurement is not required.
[0050] The metal compound particles not subject to analysis are separated by the Hansen solubility parameter Ra (J / cm 3 ) 1 / 2 Since the solubility of the metal compound particles exceeds 8.0, the metal compound particles do not disperse in the electrolyte solution but aggregate and settle. On the other hand, the metal compound particles to be analyzed remain dispersed in the electrolyte solution, so that the metal compound particles to be analyzed can be separated from the metal compound particles not to be analyzed by filtering the metal compound particles with a filter having an appropriate pore size.
[0051] That is, the Hansen solubility parameter distance Ra (J / cm 3 ) 1 / 2 Metal compound fine particles not to be analyzed, which have a particle size distribution greater than 8.0, aggregate in the electrolytic solution and remain on the filter during the filtration process, so that they are less likely to contaminate the filtrate. This makes it possible to accurately and easily carry out particle size measurement and elemental analysis of metal compound fine particles for the purpose of particle size measurement.
[0052] There is no particular restriction on the steel material to which the selection method of the present embodiment can be applied, and there is also no particular restriction on the target metal compound fine particles, although carbides and / or nitrides are preferred.
[0053] (Electrolysis process) The electrolysis process is a process for electrolyzing a steel material to extract metal compound fine particles from the steel material. The electrolysis process according to this embodiment can be applied to a general electrolytic extraction method for steel materials using an electrolytic solution. That is, in the electrolysis process according to this embodiment, an anode containing the steel material and a cathode are immersed in an electrolytic solution containing a selected solvent, and the steel material is electrolyzed in the electrolytic solution. For example, a platinum electrode may be used as the cathode.
[0054] The electrolysis conditions may be either constant potential conditions or constant current conditions. By adopting a predetermined potential and current during electrolysis, it is possible to selectively dissolve only the iron matrix without dissolving the target metal compound fine particles.
[0055] After the electrolysis process, the iron matrix is removed from the surface of the steel material, and as a result, fine metal compound particles are extracted and attached to the surface. In some cases, some of the fine metal compound particles fall off the surface of the steel material and are dispersed in the electrolytic solution.
[0056] (Dispersion and recovery process) After the electrolysis process is completed, a dispersion and recovery process is performed. In the dispersion and recovery process, while the steel material is still immersed in the electrolytic solution, ultrasonic waves are applied to the electrolytic solution to detach the metal compound fine particles from the surface of the steel material, and the metal compound fine particles are dispersed in the electrolytic solution. In other words, the electrolytic solution is used as it is as the dispersion liquid. The application of ultrasonic waves promotes the dissociation of the metal compound fine particles from the steel material. The application time of ultrasonic waves is preferably, for example, within 2 minutes, and more preferably within 1 minute.
[0057] The metal compound particles that appear on the surface of the steel material by the electrolysis process are dispersed in the electrolytic solution through the dispersion and recovery process. The solvent of the electrolytic solution is a solution that is soluble in all of the metal compound particles that may be contained in the steel material, or in the steel material that is the actual analysis target, and has a Hansen solubility parameter distance R a is 8.0(J / cm 3 ) 1 / 2Since the above-mentioned range is satisfied, the metal compound fine particles can be kept in a stably dispersed state for a long period of time, and aggregation of the metal compound fine particles can be prevented.
[0058] A dispersant may be added to the electrolytic solution in the dispersion and recovery step. Examples of dispersants include sodium dodecyl sulfate (hereinafter referred to as SDS) and sodium cholate (hereinafter referred to as SC). The concentration of the dispersant may be about 50 to 3000 ppm. The dispersant is not limited to SDS and SC. By adding these dispersants to the electrolytic solution, the dispersion stability over a long period of time is improved, and a stable dispersion state can be maintained for one day or more.
[0059] (Analysis process) Next, the analysis method of the present embodiment will be described. In the analysis method of the present embodiment, an analysis step is performed to analyze the electrolytic solution containing the metal compound fine particles obtained in the dispersion and recovery step. A specific example of the analysis step will be described below.
[0060] (First example) As a first example of the analysis step, application to a field flow fractionation method (hereinafter, referred to as FFF method) can be mentioned. In the first example, the field flow fractionation method is applied to the electrolytic solution obtained by the above-mentioned dispersion and recovery step, thereby performing a fractionation step of fractionating the metal compound fine particles by particle size, and an analysis step of analyzing the components of the metal compound fine particles fractionated by particle size.
[0061] An example of an FFF device applicable to this example is shown in Figure 1. This FFF device includes a separation cell 16 through which the developing solution flows, a permeable membrane 21 disposed in the separation cell 16, a cross-flow inlet section (not shown) that introduces the cross-flow 14 into the separation cell 16, a sample inlet section (not shown) that introduces a test solution 15 (electrolytic solution after the dispersion and recovery step) into the separation cell 16, and a control means (not shown) that controls the flow of the developing solution and the cross-flow 14 in the separation cell 16. The cross-flow 14 is a flow of the developing solution from top to bottom in Figure 1.
[0062] The separation cell 16 is composed of an upper housing 16a and a lower housing 16b arranged with a predetermined distance between them. The internal space of the separation cell 16 is a channel section 16c through which the developing solution flows. The lower housing 16b is composed of a mesh-like member. A permeable membrane 21 is laminated on the channel section 16c side of the lower housing 16b. The permeable membrane 21 allows liquid components such as the solvent of the electrolytic solution and the developing solution to pass through but does not allow metal compound fine particles to pass through. Furthermore, an ICP mass spectrometer (not shown) is connected to the right side of the separation cell 16 in the figure.
[0063] Next, a separation step and an analysis step are carried out. In the separation step, the electrolytic solution obtained by the above-mentioned dispersion and recovery method is used as the test solution for the FFF method. The electrolytic solution may contain a dispersant. Examples of the dispersant include SDS and SC. The concentration of the dispersant may be about 50 to 3000 ppm.
[0064] In the separation process, first, a flow of developing solution called cross flow 14 is generated in the FFF device. In addition, developing solution is also caused to flow from the left and right sides of the separation cell 16. As a result, the flows of developing solution flowing in opposite directions from both the left and right sides are guided by the flow of cross flow 14 to form a flow toward the permeable membrane 21. After this flow is stabilized, a test solution 15 (electrolyte solution) containing metal compound fine particles is added to the developing solution.
[0065] Then, the metal compound fine particles are carried by the flow of the developing solution and locally concentrated near the permeable membrane 21. If the flow of the developing solution is maintained for a predetermined time, the metal compound fine particles gradually diffuse with Brownian motion. The large particles 20 are pressed against the permeable membrane 21 by the flow of the cross flow 14, while the relatively small medium particles 19 and small particles 18 are suspended in the separation cell 16 due to Brownian motion. The smaller the particles 18, the more likely they are to float upwards. This operation is called focusing. By achieving this state, the metal compound fine particles are rearranged by size in the separation cell 16.
[0066] Thereafter, while maintaining the cross flow 14, the flow of the developing solution that has been pushed from the left and right sides of the separation cell 16 is changed to form a channel flow 17 made of the developing solution. The channel flow 17 is a laminar flow, and has a flow velocity distribution as shown in Fig. 1. That is, the flow velocity is the fastest at the center in the thickness direction of the channel portion 16c, and the flow velocity decreases with increasing distance from the center. That is, the flow velocity is high in the region where small particles 18 exist, and low in the region where large particles 20 exist.
[0067] At this time, when the pressure of the cross flow 14, which serves to retain the metal compound particles near the permeable membrane 21, is gradually reduced, the metal compound particles that were retained near the separation membrane 21 are carried along by the laminar flow of the channel flow 17 and are gradually discharged to the right in the order of small particles to large particles.
[0068] The separation principle of FFF may be a combination of the pressing force of the cross-flow liquid and Brownian motion, or it may utilize gravity, an electric field, a magnetic field, a temperature gradient, or the like.
[0069] Next, the analysis process will be described. The metal compound particles separated by size by the FFF method are guided by the channel flow 17 to an ICP mass spectrometer installed outside the FFF device. The metal compound particles arrive at the ICP mass spectrometer in ascending order of particle size. The metal compound particles that arrive there are decomposed to the atomic level by the thermal energy of the plasma, then ionized and introduced into the mass spectrometer. The mass spectrometer obtains a mass spectrum specific to each metal compound particle. Also, a chart of the amount of each ion that changes over time can be obtained, with the amount of each ion detected on the vertical axis and the detection time on the horizontal axis.
[0070] A laser light irradiation and detection device may also be placed between the FFF device and the ICP mass spectrometer. The light intensity of the scattered laser light is obtained from photodetectors installed at multiple angles in the laser light irradiation and detection device. In the case of small particles, the angle dependency is very small and the phenomenon of omnidirectional scattering is exhibited. On the other hand, as the particles become coarser, the forward scattering phenomenon becomes stronger, and therefore the size of the metal compound microparticles can be uniquely determined by taking the slope of this angle dependency.
[0071] Since the metal compound particles are dispersed in the electrolyte solution without coagulation or sedimentation, an appropriate amount of the metal compound particles can be introduced into the FFF device, which allows the metal compound particles to be reliably detected by an ICP mass spectrometer or a laser light detector installed downstream of the FFF device.
[0072] In addition, even after the electrolytic solution is introduced into the FFF device, the metal compound fine particles are maintained in a dispersed state without agglomeration. As a result, in the FFF method, the metal compound fine particles are appropriately sorted by size in the separation cell 16, and can be extracted in order from small particles to large particles, and analysis can be performed by particle size using an ICP mass spectrometer or the like. In addition, the particle size distribution of the electrolytic solution may be measured using a laser diffraction particle size distribution measuring device. Also, the electrolytic solution may be directly introduced into the ICP mass spectrometer, and the particle size and elemental composition may be analyzed by the single particle method.
[0073] Prior to the analysis step, the electrolytic solution may be filtered through a filter, and the filtrate may be used for the analysis. The pore size of the filter may be appropriately selected. As an example, the pore size of the filter is preferably 2.0×dm or more and 2.5 dm or less, with the predetermined value dm (μm). The predetermined value dm (μm) may be determined, for example, as a value that causes problems in the subsequent particle size measurement or elemental analysis if particles with a particle size of dm (μm) or more are present. Examples of problems in particle size measurement or elemental analysis include clogging of the pipe for transporting particles and clogging of the nebulizer of the ICP mass spectrometer. When the pore size of the filter is less than 2.0×dm (μm), the proportion of particles with a particle size of less than dm (μm) remaining on the filter increases, and the particle size of the metal compound fine particles to be measured cannot be measured accurately. When the pore size of the filter exceeds 2.5×dm (μm), the proportion of particles with a particle size of dm (μm) or more mixed into the filtrate increases, causing problems in particle size measurement and elemental analysis. dm can be appropriately selected, for example, within the range of 1 to 5 μm.
[0074] (Second example) Next, a second example of the analysis step will be described. In the second example, a sample preparation step is performed in which a sample for observation with an electron microscope containing metal compound fine particles is prepared by removing liquid phase components from the electrolytic solution obtained by the above-mentioned dispersion and recovery step while leaving metal compound fine particles in the electrolytic solution, and an observation step is performed in which the sample is observed with an electron microscope.
[0075] In the sample preparation process, for example, on a support film for observation with a transmission electron microscope, liquid components are removed while leaving metal compound fine particles in the electrolytic solution. The electrolytic solution contains liquid components, such as a solvent and a complexing agent, in addition to the metal compound fine particles, which are solid components. In the test observation process, the electrolytic solution is heated or depressurized to evaporate the liquid components, or the electrolytic solution is kept at room temperature, about 25°C, to volatilize the liquid components. By removing the liquid components, the metal compound fine particles remain in a dispersed state on the support film for observation.
[0076] Next, in the observation step, the metal compound fine particles together with the support film are introduced into a transmission electron microscope to observe the morphology of the metal compound fine particles, measure the particle size, etc. In addition, a qualitative analysis or composition analysis of the metal compound fine particles may be performed by an elemental analysis device such as EDS attached to the transmission electron microscope.
[0077] Since the metal compound fine particles are dispersed in the electrolytic solution, they remain dispersed even after the liquid components are removed in the sample preparation process. This prevents the metal compound fine particles on the support film from agglomerating with each other. This allows the metal compound fine particles to be observed with a transmission electron microscope while still spaced apart from each other, making it easier to grasp the shape of the metal compound fine particles and allowing accurate particle size measurement and other appropriate morphological observation of the metal compound fine particles.
[0078] The method for dispersing and recovering metal compound fine particles according to the present embodiment is not limited to the above embodiment, and may be modified as follows. That is, the electrolysis step is performed using an electrolysis solution that does not have the function of dispersing metal compound fine particles. Next, another solvent is added to the electrolysis solution after the electrolysis step (dispersion adjustment step). As a result, the Hansen solubility parameter distance Ra (Equation (1)) between the electrolysis solution and all of the metal compound fine particles to be dispersed and recovered is 8.0 (J / cm 3 ) 1 / 2 The dispersion liquid is as follows. When adding another solvent, it is preferable to leave the steel material after the electrolysis process immersed in the electrolytic solution. Then, ultrasonic waves are applied to this dispersion liquid to detach the metal compound fine particles from the surface of the steel material, and a dispersion process is performed in which the metal compound fine particles are dispersed in the dispersion liquid.
[0079] Electrolytic extraction is possible with electrolytes that do not have the function of dispersing metal compound particles (for example, electrolytes with a dielectric constant of 30 or more at 25°C), but the Hansen solubility parameter distance Ra (Equation (1)) between the electrolyte and all of the metal compound particles to be dispersed and recovered is 8.0 (J / cm 3 ) 1 / 2An example of such an electrolyte is an electrolyte that is
[0080] By carrying out the above-mentioned operations, it becomes possible to stably disperse and recover the fine metal compound particles extracted from the steel material by electrolytic extraction without loss. EXAMPLES
[0081] (Preparation and verification experiments) Metal compound fine particles with known primary particle diameters were added to the 28 types of solvents shown in Table 1, whose Hansen solubility parameters are known, and ultrasonic treatment was performed. AlN particles (Sigma-Aldrich, primary particle diameter: 100 nm or less) and TiN particles (Fujifilm Wako Pure Chemical Industries, primary particle diameter: 1.2 to 1.8 μm) were used as the metal compound fine particles.
[0082] After the ultrasonic treatment, the particles were allowed to stand for a certain period of time (e.g., 1 hour), and then the dispersibility of each particle, i.e., whether it was dispersed or aggregated, was evaluated. The dispersibility was evaluated using a dynamic light scattering (DLS) device (Malvern, Zetasizer NanoS).
[0083] Next, the Hansen solubility parameters of 28 types of solvents were plotted in Hansen space. At this time, the Hansen space was set up so that solvents in which metal compound particles were dispersed could be distinguished from solvents in which metal compound particles were aggregated. A Hansen solubility sphere that encompassed all the plots of solvents in which metal compound particles were dispersed was calculated using the least squares method. The position of the center of gravity of the Hansen solubility sphere in the Hansen space was taken as the Hansen solubility parameter of the metal compound particles. The above calculations using the Hansen space were performed using commercially available software (software name: HSPiP, provided by: Pirika.com).
[0084] The results of the evaluation using the analysis method using the Hansen dissolving sphere are shown in Figures 2A and 2B. Figure 2A shows the Hansen space and Hansen dissolving sphere created when determining the Hansen solubility parameter of AlN, and Figure 2B shows the Hansen space and Hansen dissolving sphere for TiN. The spherical plots in Figures 2A and 2B show the solvent in which AlN or TiN remains dispersed, and the rectangular plots show the solvent in which AlN or TiN has aggregated. A sphere (Hansen dissolving sphere) was created so that all the spherical plots are included inside and the radius is the smallest. The inside of the Hansen dissolving sphere contains a solvent with good dispersibility. The coordinates of the center point of the Hansen dissolving sphere determined for AlN and TiN, respectively, were used as the Hansen solubility parameters of AlN and TiN.
[0085] As a result, the Hansen solubility parameter of AlN is δ d1 = 14.63, δ p1 = 16.26, δ h1 = 16.83. The Hansen solubility parameter of TiN is δ d1 = 19.31, δ p1 = 16.82, δ h1 =20.47.
[0086] Next, a search was conducted for a solvent that would minimize the Hansen solubility parameters and distances of AlN and TiN. In addition, a search was conducted for a solvent with a relative dielectric constant of 30 or more at 25°C and a dipole moment of 1.5D or more. As a result, an electrolyte solution with the composition 5% by volume acetylacetone (AA) - 1% by mass tetramethylammonium chloride (TMAC) - 79% by volume N,N'-dimethylformamide (DMF) - 16% by volume water was selected. The Hansen solubility parameter distance R between AlN and the electrolyte solution, and between TiN and the electrolyte solution, a are 8.0(J / cm 3 ) 1 / 2 The results were as follows.
[0087] Next, the conditions under which the electrolytic extraction of AlN and TiN is possible using the selected electrolytic solution were confirmed.
[0088] An electrolysis cell was constructed with a working electrode (WE), a counter electrode (CE), a reference electrode (RE) and an electrolyte. A potentiostat (HA-7000) manufactured by Hokuto Denko was connected to the electrolysis cell to perform a Linear Sweep Voltammetry (LSV) measurement test.
[0089] The working electrodes (WE) were pellet samples containing various nitrides, carbides, and sulfides, in addition to carbon steel as the steel sample. The pellet samples were obtained by mixing various nitride, carbide, and sulfide reagents with graphite powder in a weight ratio of 1:1 and pressurizing them. The nitrides, carbides, and sulfides used were TiN, AlN, NbN, NbC, TiC, and MnS.
[0090] A silver-silver chloride (Ag / AgCl) electrode was used as the reference electrode (RE), and a Pt plate (manufactured by Nilaco, 99.9999%) was used as the counter electrode (CE).
[0091] The electrolyte used was the previously selected electrolyte solution with a composition of 5% by volume acetylacetone (AA)-1% by mass tetramethylammonium chloride (TMAC)-79% by volume N,N'-dimethylformamide (DMF)-16% by volume water. r was 44.29.
[0092] The preliminary electrolytic treatment of the steel sample used as the working electrode (WE) was performed under the following conditions: Before the LSV measurement, constant current electrolysis was performed at 500 mA and 450 C using a 10% AA-based electrolyte ((10% acetylacetone-1% tetramethylammonium chloride-methanol solution)), and then the surface was washed with methanol to remove the oxide layer and contaminants on the surface of the steel sample.
[0093] Before the LSV measurement, Ar gas was blown into the electrolyte for 20 minutes to saturate the electrolyte with Ar gas and create an inert atmosphere in the system. During the measurement, the flow rate was reduced so that the electrodes did not vibrate, and the inert atmosphere was maintained. In addition, in order to maintain the uniformity of the composition of the electrolyte during the measurement, stirring was performed with a stirrer at a level that did not vibrate the electrodes. The reason for avoiding electrode vibration is to keep the distance between the electrodes constant during the LSV measurement and ensure the reproducibility of the data obtained.
[0094] The potential scanning range was set to -1000 to +1500 mV (vs. Ag / AgCl), and LSV measurements were performed while increasing the potential stepwise by 100 mV each. Each potential was held for 5 minutes, and the average current value for the last 10 seconds during which the current was most stable was measured as the current value at each potential.
[0095] Similarly, LSV measurements were performed using various pellet samples instead of steel samples as the working electrode (WE). The measurement results are shown in Figure 3. The curves shown in Figure 3 are electrolysis potential-current curves.
[0096] As shown in Figure 3, it was revealed that iron is electrolyzed at -600mV (vs. Ag / AgCl), while nitrides and carbides such as AlN and TiN are electrolyzed at about +400mV (vs. Ag / AgCl). Therefore, it was predicted that the selected electrolyte would enable AlN and TiN to be extracted from steel samples without dissolving them, and to be dispersed in the electrolyte as is.
[0097] Example 1 A hot-rolled steel sheet (C: 0.15 mass%, Si: 0.22 mass%, Mn: 1.2 mass%, Al: 0.015 mass%, S: 0.009 mass%, Nb: 0.06 mass%, balance: Fe and impurities) was prepared as a test material. Observation with a transmission electron microscope (TEM) confirmed that fine AlN and NbN were precipitated in this hot-rolled steel sheet.
[0098] The steel plate was subjected to an electrolysis process. The steel material cut out from the steel plate was used as the anode, and a platinum electrode was used as the cathode, and the plate was immersed in an electrolytic solution. The electrolytic solution was the previously selected electrolytic solution with a composition of 5% by volume acetylacetone (AA)-1% by mass tetramethylammonium chloride (TMAC)-79% by volume N,N'-dimethylformamide (DMF)-16% by volume water. The electrolysis conditions were constant current conditions, with a current of 500 mA and 3600 coulombs.
[0099] Next, in the dispersion and recovery process, ultrasonic waves were applied to the electrolytic solution in which the steel material after the electrolysis process was immersed, and the fine particles attached to the steel sheet surface were dispersed in the electrolytic solution. Furthermore, the electrolytic solution after dispersion was centrifuged at a rotation speed of 1000 rpm for 1 minute, and coarse precipitates were precipitated and removed. In this way, the test solution of Example 1 was prepared.
[0100] The electrolyte used in Example 1 had a Hansen solubility parameter distance R a is 6.1(J / cm 3 ) 1 / 2 and the Hansen solubility parameter distance R a is 6.7(J / cm 3 ) 1 / 2 Both are 8.0 (J / cm 3 ) 1 / 2 It was to be the following.
[0101] Comparative Example 1 An electrolysis step was carried out in the same manner as in Example 1 above, except that a 10% AA-based electrolytic solution ((10% acetylacetone-1% tetramethylammonium chloride-methanol solution)) was used as the electrolytic solution.
[0102] Thereafter, in the dispersion recovery process, the steel sample after electrolytic extraction was immersed in a dispersion recovery liquid (45% dimethyl sulfoxide (DMSO)-45% ethylene glycol (EG)-10% methanol solution) and ultrasonic waves were applied to disperse the fine particles exposed on the surface of the steel sample into the dispersion recovery liquid. Furthermore, the dispersion recovery liquid after dispersion was centrifuged at a rotation speed of 1000 rpm for 1 minute to settle and remove coarse precipitates. In this way, the test liquid of Comparative Example 1 was prepared.
[0103] The electrolyte used in Comparative Example 1 had a Hansen solubility parameter distance R a is 10.4(J / cm 3 ) 1 / 2 , the Hansen solubility parameter distance R between AlN and a is 6.0(J / cm 3 ) 1 / 2 The Hansen solubility parameter distance R between the dispersion recovery liquid used in Comparative Example 1 and AlN and NbN was a is the R for the dispersion recovery liquid and AlN a is 7.2(J / cm 3 ) 1 / 2 and R for the dispersion recovery liquid and NbN a is 5.5(J / cm 3 ) 1 / 2 Both are 8.0 (J / cm 3 ) 1 / 2 or less, and the dispersibility was considered to be good.
[0104] Next, FFF-ICP mass spectrometry was performed on the test solutions of Example 1 and Comparative Example 1 after standing for 1 hour. The particles were separated by size using the FFF method, and ions of m / z=27 and m / z=93 were detected by mass spectrometry. The ion of m / z=27 was derived from aluminum, and the ion of m / z=93 was derived from niobium. The results are shown in FIG. 4.
[0105] 4 and 5, the detected amounts of ions with m / z=27 and m / z=93 were small in Comparative Example 1, whereas the detected amounts of ions with m / z=27 and m / z=93 were clearly larger in Example 1 than in the Comparative Example. This is believed to be because in Example 1, the steel sample electrolyzed in the electrolysis step was not transferred to another dispersion liquid, but was left immersed in the electrolytic solution during the dispersion and recovery step, and therefore the loss of AlN and NbN was significantly reduced.
[0106] In addition, in Comparative Example 1, the dispersibility of AlN in the electrolytic solution was good, while the dispersibility of NbN in the electrolytic solution was poor. Although there was a difference in dispersibility between AlN and NbN in the electrolytic solution, in Comparative Example 1, the operation of transferring from the electrolytic solution to the dispersion solution was performed, so that some of the NbN and AlN remained in the electrolytic solution, which was thought to be the reason for the low analytical value.
[0107] To verify this point, the 10% AA-based electrolyte after the electrolysis process used in Comparative Example 1 was subjected to suction filtration using a 0.2 μm filter, and it was found that a large number of AlN particles and NbN particles had fallen off into the electrolyte, as shown in FIG. 6.
[0108] From the above results, it was found that the use of the electrolytic solution of Example 1 significantly improves the quantitative evaluation of fine particles in steel materials by FFF-ICP-MS. [Explanation of symbols]
[0109] 14...cross flow, 15...test liquid, 16...separation cell, 16a...upper housing, 16b...lower housing, 16c...channel portion, 17...channel flow, 18...small particles, 19...medium particles, 20...large particles, 21...permeable membrane.
Claims
1. an electrolysis step of immersing an electrode including a steel material and a counter electrode in an electrolytic solution to electrolyze the steel material; a dispersion step of applying ultrasonic waves to the electrolytic solution while the steel material is immersed in the electrolytic solution to detach metal compound fine particles from the surface of the steel material, thereby dispersing the metal compound fine particles in the electrolytic solution.
2. 2. The method for dispersing and recovering fine metal compound particles in a steel material according to claim 1, wherein the electrolytic solution has a function of dispersing the fine metal compound particles.
3. Following the electrolysis step, the Hansen solubility parameter distance Ra (Equation (1)) between the electrolytic solution and all of the metal compound fine particles to be dispersed and collected is 8.0 (J / cm 3 ) 1/2 2. The method for dispersing and recovering metal compound fine particles in a steel material according to claim 1, further comprising a dispersion liquid preparation step of adding an optional solvent so as to obtain the following dispersion liquid: R a = [4(δ d1 -δ d2 ) 2 + (δ p1 -δ p2 ) 2 + (δ h1 -δ h2 ) 2 ] 1/2 …(1) However, δ in formula (1) d1 is the London dispersion force of the metal compound fine particles, δ p1 is the dipole-dipole force of the metal compound fine particles, δ h1 is the hydrogen bonding strength of the metal compound fine particles, δ d2 is the London dispersion force of the solvent, δ p2 is the dipole-dipole force of the solvent, δ h2 is the hydrogen bonding strength of the solvent.
4. an electrolysis step of immersing an electrode including a steel material and a counter electrode in an electrolytic solution to electrolyze the steel material; a dispersion step of applying ultrasonic waves to the electrolytic solution while the steel material is immersed in the electrolytic solution to detach metal compound fine particles from the surface of the steel material, thereby dispersing the metal compound fine particles in the electrolytic solution, The Hansen solubility parameter distance Ra (Equation (1)) between the electrolytic solution and all of the metal compound fine particles to be dispersed and collected is 8.0 (J / cm 3 ) 1/2 A method for dispersing and recovering metal compound fine particles in a steel material, comprising the following solvent: R a = [4(δ d1 -δ d2 ) 2 + (δ p1 -δ p2 ) 2 + (δ h1 -δ h2 ) 2 ] 1/2 …(1) However, δ in formula (1) d1 is the London dispersion force of the metal compound fine particles, δ p1 is the dipole-dipole force of the metal compound fine particles, δ h1 is the hydrogen bonding strength of the metal compound fine particles, δ d2 is the London dispersion force of the solvent, δ p2 is the dipole-dipole force of the solvent, δ h2 is the hydrogen bonding strength of the solvent.
5. 5. The method for dispersing and recovering fine metal compound particles in a steel material according to claim 1, wherein the electrolytic solution contains a complexing agent that forms a complex with iron.
6. A method for analyzing metal compound fine particles in a steel material, comprising an analysis step of analyzing the electrolytic solution containing the metal compound fine particles obtained by the method for dispersing and recovering metal compound fine particles in a steel material according to claim 1 or 4.
7. The analyzing step includes a step of performing a field flow fractionation method on the electrolytic solution in which the metal compound fine particles are dispersed, thereby separating the metal compound fine particles according to particle size; 7. The method for analyzing fine metal compound particles in steel material according to claim 6, further comprising a step of analyzing components of the fine metal compound particles separated by particle size.
8. The analyzing step includes a step of removing a liquid phase component from the electrolytic solution in which the metal compound fine particles are dispersed, while leaving the metal compound fine particles in the electrolytic solution, thereby preparing a sample for observation with an electron microscope, which contains the metal compound fine particles; The method for analyzing fine particles of a metal compound in a steel material according to claim 6, further comprising a step of observing the sample with an electron microscope.
9. an electrolytic solution in which an electrode containing a steel material and a counter electrode are immersed, the steel material is electrolyzed to extract metal compound fine particles contained in the steel material, and the metal compound fine particles are dispersed; The electrolytic solution has a Hansen solubility parameter distance R a (Equation (1)) is 8.0 (J / cm 3 ) 1/2 Electrolyte solution for electrowinning of steel materials, comprising a solvent in which the concentration is less than 100%. R a = [4(δ d1 -δ d2 ) 2 + (δ p1 -δ p2 ) 2 + (δ h1 -δ h2 ) 2 ] 1/2 …(1) However, δ in formula (1) d1 is the London dispersion force of the metal compound fine particles, δ p1 is the dipole-dipole force of the metal compound fine particles, δ h1 is the hydrogen bonding strength of the metal compound fine particles, δ d2 is the London dispersion force of the solvent, δ p2 is the dipole-dipole force of the solvent, δ h2 is the hydrogen bonding strength of the solvent.
10. 10. The electrolytic solution for electrowinning of steel materials according to claim 9, which has a relative dielectric constant of 30 or more at 25°C.
Citation Information
Cited By
Method for preparing high-purity metallic iron through ultrasonic circulation electrodeposition method
CN120797075A