All-solid battery
The all-solid-state battery's innovative design with reinforced margin portions addresses the issue of path breakage due to volumetric expansion, improving long-term charge-discharge cycle characteristics by maintaining structural integrity.
Patent Information
- Application Number
- JP2023074749
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
The connection between the ion conduction path and the electron conduction path within the electrode layer of all-solid-state batteries is prone to breakage due to volumetric expansion and contraction of the active material during charging and discharging, leading to deterioration of long-term charge-discharge cycle characteristics.
The all-solid-state battery design includes a solid electrolyte layer with alternating first and second internal electrode layers, surrounded by margin portions with a Vickers hardness of 3 GPa or more, where the ratio of the margin hardness to the electrode layer hardness is greater than 1, and these layers are stacked in a rectangular parallelepiped shape with specific margin configurations to reinforce the structure.
This design effectively suppresses deterioration in long-term charge-discharge cycle characteristics by reinforcing the battery structure through strong margin portions, enhancing the battery's durability and performance.
Smart Images

Figure 2024159026000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an all-solid-state battery. [Background technology]
[0002] Currently, lithium ion secondary batteries are used in various fields such as consumer devices, industrial machines, and automobiles. However, existing lithium ion secondary batteries contain electrolyte, and therefore there is a risk of electrolyte leakage, smoke, fire, etc. For this reason, the development of all-solid-state lithium ion secondary batteries that employ a solid electrolyte that is stable in the air is being actively carried out. As a representative solid electrolyte, an all-solid-state battery that employs a phosphate-based solid electrolyte containing a NASICON-type crystal structure is known (for example, see Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2021-108258 [Patent Document 2] JP 2021-140899 A [Patent Document 3] Patent Publication No. 2022-63272 Summary of the Invention [Problem to be solved by the invention]
[0004] One of the factors that may cause deterioration in the cycle characteristics of all-solid-state batteries is that the volume expansion and contraction of the active material that accompanies charging and discharging may easily cause the ionic and electronic conductive paths in the electrode layer to become disconnected.
[0005] The present invention has been made in consideration of the above problems, and has an object to provide an all-solid-state battery capable of suppressing deterioration of long-term charge-discharge cycle characteristics. [Means for solving the problem]
[0006] The all-solid-state battery according to the present invention comprises a solid electrolyte layer, a first internal electrode layer provided on a first main surface of the solid electrolyte layer and including an electrode active material and a solid electrolyte, a first marginal portion provided around the first internal electrode layer on the first main surface, a second internal electrode layer provided on a second main surface of the solid electrolyte layer and including an electrode active material and a solid electrolyte, and a second marginal portion provided around the second internal electrode layer on the second main surface, the Vickers hardness Hv of the first marginal portion is 3 GPa or more, the ratio of the Vickers hardness Hv of the first marginal portion to the Vickers hardness Hv of the first internal electrode layer is greater than 1, and the ratio of the Vickers hardness Hv of the second marginal portion to the Vickers hardness Hv of the second internal electrode layer is greater than 1, and the Vickers hardness Hv is a hardness calculated by reading the length of the diagonal line of the indentation after pressing an indenter into the target area for 15 seconds under a load of 3 gf (= 0.029 N).
[0007] In the above-mentioned all-solid-state battery, a laminated chip is provided in which the solid electrolyte layer, the first internal electrode layer, the solid electrolyte layer, and the second internal electrode layer are alternately stacked multiple times to have an approximately rectangular parallelepiped shape, the first internal electrode layer is extended to a first end face of the approximately rectangular parallelepiped shape, and the second internal electrode layer is extended to a second end face opposite the first end face of the approximately rectangular parallelepiped shape, and the second marginal portion is provided in a region where the first internal electrode layers face each other without the second internal electrode layer therebetween in the vicinity of the first end face, and the first marginal portion may be provided in a region where the second internal electrode layers face each other without the first internal electrode layer therebetween in the vicinity of the second end face.
[0008] In the above all-solid-state battery, a laminated chip is provided in which the solid electrolyte layer, the first internal electrode layer, the solid electrolyte layer, and the second internal electrode layer are alternately stacked multiple times to have an approximately rectangular parallelepiped shape, the first internal electrode layer is extended to a first end face of the approximately rectangular parallelepiped shape, and the second internal electrode layer is extended to a second end face opposite the first end face of the approximately rectangular parallelepiped shape, and the first marginal portion is provided in a region of the laminated chip from two side faces other than the upper face, lower face, first end face, and second end face in the stacking direction to the first internal electrode layer, and the second marginal portion is provided in a region of the laminated chip from the two side faces to the second internal electrode layer.
[0009] In the all-solid-state battery, the solid electrolyte layer, the first marginal portion, and the second marginal portion may contain a phosphate-based solid electrolyte having a NASICON-type crystal structure.
[0010] In the all-solid-state battery, the phosphate-based solid electrolyte in the first marginal portion and the second marginal portion may be glass.
[0011] In the all-solid-state battery, the first marginal portion and the second marginal portion may contain at least any one of a Li-BO based compound, a Li-Si-O based compound, a Li-CO based compound, a Li-SO based compound, and a Li-PO based compound. Effect of the Invention
[0012] According to the present invention, it is possible to provide an all-solid-state battery capable of suppressing deterioration of long-term charge-discharge cycle characteristics. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a basic structure of an all-solid-state battery. [Diagram 2] FIG. 2 is a partial cross-sectional perspective view of a stacked-type all-solid-state battery in which a plurality of battery units are stacked. [Diagram 3] 3 is a cross-sectional view taken along line AA in FIG. 2. [Figure 4] FIG. 3 is a cross-sectional view taken along line BB in FIG. [Diagram 5] 1A is an enlarged view of a cross section of a side margin, and FIG. 1B is an enlarged view of a cross section of a first end margin. [Figure 6] FIG. 1 is a diagram illustrating a flow of a method for producing an all-solid-state battery. [Figure 7] 1(a) and (b) are diagrams illustrating the lamination process. [Figure 8] FIG. 1 is a diagram illustrating a lamination process. [Figure 9] FIG. 5 is a YZ cross-sectional view of an all-solid-state battery according to a second embodiment. [Figure 10] 1(a) and (b) are diagrams illustrating the lamination process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment will be described with reference to the drawings.
[0015] (First embodiment) FIG. 1 is a schematic cross-sectional view showing the basic structure of an all-solid-state battery 100. As illustrated in FIG. 1, the all-solid-state battery 100 has a structure in which a solid electrolyte layer 30 is sandwiched between a first internal electrode layer 10 and a second internal electrode layer 20. The first internal electrode layer 10 is formed on a first main surface of the solid electrolyte layer 30. The second internal electrode layer 20 is formed on a second main surface of the solid electrolyte layer 30. For example, the first internal electrode layer 10, the second internal electrode layer 20, and the solid electrolyte layer 30 are sintered bodies obtained by sintering powder materials.
[0016] When the all-solid-state battery 100 is used as a secondary battery, one of the first internal electrode layer 10 and the second internal electrode layer 20 is used as a positive electrode, and the other is used as a negative electrode. In this embodiment, as an example, the first internal electrode layer 10 is used as a positive electrode layer, and the second internal electrode layer 20 is used as a negative electrode layer.
[0017] The solid electrolyte layer 30 has a NASICON-type crystal structure and is mainly composed of an oxide-based solid electrolyte having ion conductivity. The solid electrolyte of the solid electrolyte layer 30 is, for example, an oxide-based solid electrolyte having lithium ion conductivity. The solid electrolyte is, for example, a phosphate-based solid electrolyte. The phosphate-based solid electrolyte having a NASICON-type crystal structure has a high electrical conductivity and is stable in the air. The phosphate-based solid electrolyte is, for example, a phosphate containing lithium. The phosphate is not particularly limited, but examples thereof include a composite lithium phosphate salt with Ti (for example, LiTi2(PO4)3). Alternatively, Ti can be partially or completely replaced with a tetravalent transition metal such as Ge, Sn, Hf, or Zr. In addition, in order to increase the Li content, it may be partially replaced with a trivalent transition metal such as Al, Ga, In, Y, or La. More specifically, for example, Li 1+x Al x Ge 2-x (PO4)3 and Li 1+x Al x Zr 2-x (PO4)3, Li 1+x Al x Ti 2-x (PO4)3 and the like. For example, Li-Al-Ge-PO4-based (LAGP-based) materials to which the same transition metal as that contained in the phosphate having an olivine crystal structure contained in the first internal electrode layer 10 and the second internal electrode layer 20 is added in advance are preferred. For example, when the first internal electrode layer 10 and the second internal electrode layer 20 contain a phosphate containing Co and Li, it is preferred that the solid electrolyte layer 30 contains a Li-Al-Ge-PO4-based material to which Co is added in advance. In this case, the effect of suppressing the elution of the transition metal contained in the electrode active material into the electrolyte can be obtained. When the first internal electrode layer 10 and the second internal electrode layer 20 contain a phosphate containing a transition element other than Co and Li, it is preferred that the solid electrolyte layer 30 contains a Li-Al-Ge-PO4-based material to which the transition metal is added in advance.
[0018] The first internal electrode layer 10 used as the positive electrode contains a substance having an olivine crystal structure as an electrode active material. It is preferable that the second internal electrode layer 20 also contains the electrode active material. An example of such an electrode active material is a phosphate containing a transition metal and lithium. The olivine crystal structure is a crystal that natural olivine has, and can be identified by X-ray diffraction.
[0019] A typical example of an electrode active material having an olivine crystal structure is LiCoPO4 containing Co. Phosphates in which the transition metal Co is substituted in this chemical formula can also be used. Here, the ratio of Li and PO4 can vary depending on the valence. Note that it is preferable to use Co, Mn, Fe, Ni, etc. as the transition metal.
[0020] The electrode active material having an olivine type crystal structure acts as a positive electrode active material in the first internal electrode layer 10 acting as a positive electrode. For example, when only the first internal electrode layer 10 contains an electrode active material having an olivine type crystal structure, the electrode active material acts as a positive electrode active material. When the second internal electrode layer 20 also contains an electrode active material having an olivine type crystal structure, the second internal electrode layer 20 acting as a negative electrode exhibits the effects of increasing the discharge capacity and increasing the operating potential with discharge, which are presumed to be based on the formation of a partial solid solution state with the negative electrode active material, although the mechanism of action is not completely clear.
[0021] When both the first internal electrode layer 10 and the second internal electrode layer 20 contain an electrode active material having an olivine crystal structure, each electrode active material preferably contains a transition metal that may be the same or different from each other. "May be the same or different from each other" means that the electrode active materials contained in the first internal electrode layer 10 and the second internal electrode layer 20 may contain the same type of transition metal, or may contain different types of transition metals. The first internal electrode layer 10 and the second internal electrode layer 20 may contain only one type of transition metal, or may contain two or more types of transition metals. Preferably, the first internal electrode layer 10 and the second internal electrode layer 20 contain the same type of transition metal. More preferably, the electrode active materials contained in both electrodes have the same chemical composition. Since the first internal electrode layer 10 and the second internal electrode layer 20 contain the same type of transition metal or contain electrode active materials of the same composition, the similarity of the compositions of the two internal electrode layers is increased. Therefore, even if the terminals of the all-solid-state battery 100 are attached with the positive and negative terminals reversed, depending on the application, there is an effect that the battery can withstand practical use without malfunction.
[0022] The second internal electrode layer 20 contains a negative electrode active material. By containing the negative electrode active material in only one electrode, it becomes clear that the one electrode acts as a negative electrode and the other electrode acts as a positive electrode. It is also possible to contain a material that is known as a negative electrode active material in both electrodes. For the negative electrode active material of the electrode, reference can be made to conventional techniques in secondary batteries as appropriate, and examples thereof include compounds such as titanium oxide, lithium titanium composite oxide, lithium titanium composite phosphate, carbon, and lithium vanadium phosphate.
[0023] In the preparation of the first internal electrode layer 10 and the second internal electrode layer 20, in addition to these electrode active materials, a solid electrolyte having ion conductivity, a conductive material (conductive assistant), etc. are added. For these members, a paste for the internal electrode can be obtained by uniformly dispersing a binder and a plasticizer in water or an organic solvent. As the conductive assistant, a carbon material or the like may be included. As the conductive assistant, a metal may be included. Examples of the metal of the conductive assistant include Pd, Ni, Cu, Fe, and alloys containing these. The solid electrolyte included in the first internal electrode layer 10 and the second internal electrode layer 20 can be the same as the main component solid electrolyte of the solid electrolyte layer 30, for example.
[0024] Fig. 2 is a partial cross-sectional perspective view of a stacked-type all-solid-state battery 100a in which a plurality of battery units are stacked. Fig. 3 is a cross-sectional view taken along line AA in Fig. 2. Fig. 4 is a cross-sectional view taken along line BB in Fig. 2. The all-solid-state battery 100a includes a stacked chip 60 having a substantially rectangular parallelepiped shape. In the stacked chip 60, a first external electrode 40a is provided so as to contact a first end face of the four faces other than the upper and lower faces at the ends in the stacking direction, and a second external electrode 40b is provided so as to contact a second end face opposite the first end face.
[0025] 2 to 4, the X-axis direction is the direction in which the first end face and the second end face of the laminated chip 60 face each other, and is the direction in which the first external electrode 40a and the second external electrode 40b face each other. The Y-axis direction is the width direction of the first internal electrode layer 10 and the second internal electrode layer 20, and is the direction in which two of the four side faces of the laminated chip 60 other than the two end faces face each other. The Z-axis direction is the stacking direction, and is the direction in which the upper face and the lower face of the laminated chip 60 face each other. The X-axis direction, the Y-axis direction, and the Z-axis direction are mutually perpendicular.
[0026] In the following description, components having the same composition ranges and the same thickness ranges as those of the all-solid-state battery 100 are denoted by the same reference numerals and detailed description thereof will be omitted.
[0027] In the all-solid-state battery 100a, a plurality of first internal electrode layers 10 and a plurality of second internal electrode layers 20 are alternately stacked with a solid electrolyte layer 30 interposed therebetween. The edges of the plurality of first internal electrode layers 10 in the X-axis direction are drawn to the first end face of the laminated chip 60, and are not drawn to the second end face. The edges of the plurality of second internal electrode layers 20 in the X-axis direction are drawn to the second end face of the laminated chip 60, and are not drawn to the first end face. Thereby, the first internal electrode layer 10 and the second internal electrode layer 20 are alternately conducted to the first external electrode 40a and the second external electrode 40b. The solid electrolyte layer 30 extends from the first external electrode 40a to the second external electrode 40b. In this way, the all-solid-state battery 100a has a structure in which a plurality of battery units are stacked.
[0028] A cover layer 50 is laminated on the upper end surface of the laminated portion of the first internal electrode layer 10, the solid electrolyte layer 30, and the second internal electrode layer 20. The cover layer 50 is in contact with the uppermost internal electrode layer (either the first internal electrode layer 10 or the second internal electrode layer 20) and is in contact with a part of the solid electrolyte layer 30. A cover layer 50 is also laminated on the lower end surface of the laminate. The cover layer 50 is in contact with the lowermost internal electrode layer (either the first internal electrode layer 10 or the second internal electrode layer 20) and is in contact with a part of the solid electrolyte layer 30. For example, the cover layer 50 is a sintered body obtained by sintering a powder material.
[0029] 3, the region where the first internal electrode layer 10 connected to the first external electrode 40a and the second internal electrode layer 20 connected to the second external electrode 40b face each other is a region that generates battery capacity. Therefore, this region is referred to as a battery capacity region 70. In other words, the battery capacity region 70 is a region where two adjacent internal electrode layers connected to different external electrodes face each other.
[0030] The region where the first internal electrode layers 10 connected to the first external electrode 40a face each other without the second internal electrode layer 20 connected to the second external electrode 40b being interposed therebetween is called the first end margin 80a. The region where the first internal electrode layers 10 connected to the second external electrode 40b face each other without the first internal electrode layer 10 connected to the first external electrode 40a being interposed therebetween is called the second end margin 80b. In other words, the end margin is a region where internal electrode layers connected to the same external electrode face each other without the internal electrode layer connected to a different external electrode being interposed therebetween. The first end margin 80a and the second end margin 80b are regions that do not produce battery capacity.
[0031] 4, in the laminated chip 60, the regions extending from the two side surfaces of the laminated chip 60 to the first internal electrode layer 10 and the second internal electrode layer 20 are referred to as side margins 90. In other words, the side margins 90 are regions provided so as to cover the ends of the multiple first internal electrode layers 10 and second internal electrode layers 20 laminated in the laminate extending to the two side surfaces.
[0032] 5(a) is an enlarged view of a cross section of the side margin 90. The side margin 90 has a structure in which the solid electrolyte layers 30 and the margins are alternately stacked in the stacking direction of the first internal electrode layers 10 and the second internal electrode layers 20 in the battery capacity region 70. A first margin 95a is provided in the same layer as the first internal electrode layer 10. A second margin 95b is provided in the same layer as the second internal electrode layer 20. With this configuration, the step between the battery capacity region 70 and the side margin 90 is suppressed.
[0033] FIG. 5(b) is an enlarged view of the cross section of the first end margin 80a. In comparison with the side margin 90, in the first end margin 80a, the internal electrode layer extends to the end face of the first end margin 80a for every other one of the multiple internal electrode layers stacked. That is, in the first end margin 80a, the first internal electrode layer 10 extends to the end face, and the second internal electrode layer 20 does not extend to the end face. In the same layer as the second internal electrode layer 20, a second margin 95b is provided. Also, in the layer in which the first internal electrode layer 0 extends to the end face of the first end margin 80a, the first margin 95a is not stacked. According to this configuration, the step between the battery capacity region 70 and the first end margin 80a is suppressed. In addition, in the second end margin 80b, the second internal electrode layer 20 extends to the end face, and the first internal electrode layer 10 does not extend to the end face. In the second end margin 80b, in the same layer as the first internal electrode layer 10, a first marginal portion 95a is provided.
[0034] In an all-solid-state battery including a solid electrolyte, a sintering process is performed by heat treatment to obtain desired electrical properties and mechanical strength properties. In addition, from the viewpoint of extending the life of an all-solid-state battery, it is desirable to pack the electrode active material, solid electrolyte, and conductive assistant in the internal electrode layer as densely as possible so that they have many contacts with each other, and then to form the contacts more effectively through a sintering process. One of the factors that deteriorate the cycle characteristics of an all-solid-state battery is that the connection of the ion conductive path and the electron conductive path in the internal electrode layer is easily broken due to the volume expansion and contraction of the electrode active material accompanying charging and discharging.
[0035] For example, a technology has been disclosed that uses an external force in a direction that presses down an element placed inside from the exterior side. However, in an all-solid-state battery using a solid electrolyte, it is more preferable to reinforce it by batch firing. In addition, in a rectangular all-solid-state battery in which internal electrode layers and solid electrolyte layers are alternately stacked, the thickness of the internal electrode layers is designed to be sufficiently thin relative to the dimensions in the X-axis direction and the Y-axis direction, so that the effect of the volume change of the internal electrode layers is likely to be noticeable in the X-axis direction and the Y-axis direction, which is likely to lead to a deterioration of the long-term charge-discharge cycle characteristics.
[0036] Therefore, the all-solid-state battery 100a according to this embodiment has a configuration capable of suppressing the deterioration of the long-term charge-discharge cycle characteristics. In this embodiment, the margin portion adjacent to the internal electrode layer has a strong configuration, and the deterioration of the long-term charge-discharge cycle characteristics is suppressed by the reinforcement by pressing from the margin portion.
[0037] Specifically, the Vickers hardness Hv of the first marginal portion 95a and the second marginal portion 95b is 3 GPa or more, the ratio of the Vickers hardness Hv of the first marginal portion 95a to the Vickers hardness Hv of the first internal electrode layer 10 (Vickers hardness of the first marginal portion 95a / Vickers hardness of the first internal electrode layer 10) is greater than 1, and the ratio of the Vickers hardness Hv of the second marginal portion 95b to the Vickers hardness Hv of the second internal electrode layer 20 (Vickers hardness of the second marginal portion 95b / Vickers hardness of the second internal electrode layer 20) is greater than 1. The Vickers hardness Hv here can be calculated by reading the length of the diagonal line of the indentation after pressing an indenter into the target location for 15 seconds under a load of 3 gf (=0.029 N).
[0038] With this configuration, the first margin portion 95a and the second margin portion 95b become strong, and the first internal electrode layer 10 and the second internal electrode layer 20 are reinforced by being pressed against the first internal electrode layer 10 and the second internal electrode layer 20, thereby suppressing deterioration of the long-term charge-discharge cycle characteristics.
[0039] In order to provide sufficient strength to the first marginal portion 95a, the Vickers hardness Hv of the first marginal portion 95a is preferably 5 GPa or more, and more preferably 7 GPa or more. In order to provide sufficient strength to the second marginal portion 95b, the Vickers hardness Hv of the second marginal portion 95b is preferably 5 GPa or more, and more preferably 7 GPa or more.
[0040] From the viewpoint of sufficiently increasing the strength of the first marginal portion 95a relative to the first internal electrode layer 10, the ratio of the Vickers hardness Hv of the first marginal portion 95a to the Vickers hardness Hv of the first internal electrode layer 10 is preferably 2 or more, and more preferably 4 or more. From the viewpoint of sufficiently increasing the strength of the second marginal portion 95b relative to the second internal electrode layer 20, the ratio of the Vickers hardness Hv of the second marginal portion 95b to the Vickers hardness Hv of the second internal electrode layer 20 is preferably 2 or more, and more preferably 4 or more.
[0041] The strength of the first marginal portion 95a and the second marginal portion 95b can be adjusted by the material used for the first marginal portion 95a and the second marginal portion 95b. For example, inorganic materials such as alumina, zirconia, quartz glass, silicate glass (soda-lime glass, aluminosilicate glass, borosilicate glass, etc.), NASICON-type phosphate-based crystal material, and NASICON-type phosphate-based glass ceramics can be used as the material for the first marginal portion 95a and the second marginal portion 95b. Table 1 shows the approximate Vickers hardness Hv of each material. These materials may be used in combination. [Table 1]
[0042] Since the Vickers hardness may vary depending on the sintering state, the Vickers hardness Hv may be improved by adding a sintering aid to the first marginal portion 95a and the second marginal portion 95b. For example, the sintering aid may be one or more glass components such as Li-BO based compounds, Li-Si-O based compounds, Li-CO based compounds, Li-SO based compounds, and Li-PO based compounds.
[0043] In addition, in consideration of the ease of forming an interface bond between the first marginal portion 95a and the first internal electrode layer 10 during sintering, and the ease of forming an interface bond between the second marginal portion 95b and the second internal electrode layer 20 during sintering, it is preferable that the material of the first marginal portion 95a and the second marginal portion 95b is a material of the same system as the solid electrolyte material of the first internal electrode layer 10 and the second internal electrode layer 20. For example, it is preferable that the solid electrolyte layer 30, the first marginal portion 95a, and the second marginal portion 95b are mainly composed of a phosphate-based solid electrolyte containing a NASICON-type crystal structure. For example, it is preferable to use a Li-Al-Ge-PO4-based material, a Li-Al-Ti-PO4-based material, a Li-Al-Zr-PO4-based material, or the like as the material of the first marginal portion 95a and the second marginal portion 95b.
[0044] In addition, in the XZ cross section of Figure 3, the length in the X-axis direction of the first margin 95a and the second margin 95b at each end margin is preferably 0.2 mm or more and 10 mm or less, more preferably 0.5 mm or more and 6 mm or less, and even more preferably 1 mm or more and 5 mm or less.
[0045] In addition, in the YZ cross section of Figure 4, the length in the Y-axis direction of the first margin portion 95a and the second margin portion 95b in each side margin 90 is preferably 0.2 mm or more and 10 mm or less, more preferably 0.5 mm or more and 6 mm or less, and even more preferably 1 mm or more and 5 mm or less.
[0046] Next, a description will be given of a method for manufacturing the all-solid-state battery 100a illustrated in Fig. 2. Fig. 6 is a diagram illustrating a flow of the method for manufacturing the all-solid-state battery 100a.
[0047] (Process for producing raw powder for solid electrolyte layer) First, a raw material powder for the solid electrolyte layer constituting the above-mentioned solid electrolyte layer 30 is prepared. For example, raw materials, additives, etc. are mixed, and a solid-phase synthesis method or the like is used to prepare raw material powder for an oxide-based solid electrolyte. The obtained raw material powder can be dry-milled to adjust to a desired average particle size. For example, a planetary ball mill using 5 mmφ ZrO2 balls is used to adjust to a desired average particle size.
[0048] (Cover layer raw powder preparation process) The raw material powder of the ceramics constituting the above-mentioned cover layer 50 is prepared. For example, the raw material powder for the cover layer can be prepared by mixing the raw materials, additives, etc. and using a solid-phase synthesis method or the like. The obtained raw material powder can be adjusted to a desired average particle size by dry pulverizing. For example, the desired average particle size is adjusted using a planetary ball mill using 5 mmφ ZrO2 balls.
[0049] (Process for preparing raw powder for blank areas) The raw material powder constituting the above-mentioned first marginal portion 95a and second marginal portion 95b is prepared. For example, the raw material powder for the marginal portion can be prepared by mixing raw materials, additives, etc., and using a solid-phase synthesis method, etc. The obtained raw material powder can be adjusted to a desired average particle size by dry pulverizing. For example, the desired average particle size is adjusted using a planetary ball mill using 5 mmφ ZrO2 balls.
[0050] (Electrode layer paste preparation process) Next, the internal electrode paste for producing the first internal electrode layer 10 and the second internal electrode layer 20 is separately produced. For example, the internal electrode paste can be obtained by uniformly dispersing a conductive assistant, an electrode active material, a solid electrolyte material, a sintering assistant, a binder, a plasticizer, and the like in water or an organic solvent. The above-mentioned solid electrolyte paste may be used as the solid electrolyte material. A carbon material or the like is used as the conductive assistant. A metal may be used as the conductive assistant. Examples of the metal of the conductive assistant include Pd, Ni, Cu, Fe, and alloys containing these. Pd, Ni, Cu, Fe, alloys containing these, and various carbon materials may also be used.
[0051] The sintering aid in the internal electrode paste contains one or more glass components such as Li-BO based compounds, Li-Si-O based compounds, Li-CO based compounds, Li-SO based compounds, and Li-PO based compounds.
[0052] (External electrode paste manufacturing process) Next, an external electrode paste for producing the above-mentioned first external electrode 40a and second external electrode 40b is prepared. For example, the external electrode paste can be obtained by uniformly dispersing a conductive material, a glass frit, a binder, a plasticizer, etc. in water or an organic solvent.
[0053] (Solid electrolyte green sheet manufacturing process) The raw material powder for the solid electrolyte layer is uniformly dispersed in an aqueous or organic solvent together with a binder, a dispersant, a plasticizer, etc., and wet-pulverized to obtain a solid electrolyte slurry having a desired average particle size. At this time, a bead mill, a wet jet mill, various kneaders, a high-pressure homogenizer, etc. can be used, and it is preferable to use a bead mill from the viewpoint of simultaneously adjusting the particle size distribution and dispersing. A binder is added to the obtained solid electrolyte slurry to obtain a solid electrolyte paste. The obtained solid electrolyte paste is coated to produce a solid electrolyte green sheet 51. The coating method is not particularly limited, and a slot die method, a reverse coat method, a gravure coat method, a bar coat method, a doctor blade method, etc. can be used. The particle size distribution after wet-pulverization can be measured, for example, using a laser diffraction measurement device using a laser diffraction scattering method.
[0054] (Lamination process) As illustrated in FIG. 7(a), the internal electrode paste 52 is printed on one side of the solid electrolyte green sheet 51. The blank portion paste 53 is printed on the peripheral area of the solid electrolyte green sheet 51 where the internal electrode paste 52 is not printed. The blank portion paste 53 can be formed by applying raw material powder for the blank portion in the same manner as in the solid electrolyte green sheet preparation process. As illustrated in FIG. 7(b), the printed solid electrolyte green sheets 51 are alternately shifted and stacked. As illustrated in FIG. 8, a laminate is obtained by pressing the cover sheets 54 from above and below in the stacking direction. In this case, a green chip having a substantially rectangular parallelepiped shape is obtained so that the internal electrode paste 52 for the first internal electrode layer 10 is exposed on one end face of the laminate and the internal electrode paste 52 for the second internal electrode layer 20 is exposed on the other end face. The cover sheet 54 can be formed by applying raw material powder for the cover layer in the same manner as in the solid electrolyte green sheet preparation process. The cover sheet 54 is formed to be thicker than the solid electrolyte green sheet 51. The thickness may be increased during coating, or may be increased by stacking a plurality of coated sheets.
[0055] (Firing process) Next, the green chip thus obtained is fired to obtain the laminated chip 60. The firing conditions are not particularly limited, and may be set in an oxidizing or non-oxidizing atmosphere, with the maximum temperature preferably being 400°C to 1000°C, more preferably 500°C to 900°C, etc. Before the maximum temperature is reached, a step of maintaining the temperature lower than the maximum temperature in an oxidizing atmosphere may be provided in order to sufficiently remove the binder. In order to reduce the process cost, it is desirable to fire at a temperature as low as possible. After firing, a reoxidation treatment may be performed. Then, the first external electrode 40a and the second external electrode 40b are formed by applying and curing a paste for external electrodes on two end faces of the laminated chip 60.
[0056] Second embodiment In the first embodiment, the side margin 90 has a laminated structure of a solid electrolyte layer and a blank portion, but is not limited thereto. In the second embodiment, an example in which the entire side margin 90 is a blank portion will be described.
[0057] FIG. 9 is a YZ cross-sectional view of the all-solid-state battery according to the second embodiment. The cross-section of FIG. 9 corresponds to the cross-section of line BB in FIG. 2. In this embodiment, the side margin 90 is provided from the upper surface to the lower surface of the laminated chip 60. In this embodiment, the solid electrolyte layer 30 does not extend to the inside of the side margin 90, and the entire side margin 90 is a margin. The side margin 90 has the same configuration as the first margin 95a or the second margin 95b described in the first embodiment. Therefore, in this embodiment, the Vickers hardness Hv of the entire side margin 90 is 3 Ga or more, the ratio of the Vickers hardness Hv of the side margin 90 to the Vickers hardness Hv of the first internal electrode layer 10 is greater than 1, and the ratio of the Vickers hardness Hv of the side margin 90 to the Vickers hardness Hv of the second internal electrode layer 20 is greater than 1. In this embodiment, in the side margin 90, the area adjacent to the first internal electrode layer 10 in the same layer serves as the first margin, and the area adjacent to the second internal electrode layer 20 in the same layer serves as the second margin.
[0058] The side margin 90 of this embodiment can be obtained by carrying out the lamination process illustrated in FIG. 10(a) and FIG. 10(b) instead of the lamination process described in the first embodiment. Specifically, as illustrated in FIG. 10(a), a laminated portion is obtained by alternately laminating solid electrolyte green sheets 51 and internal electrode pastes 52 having the same width as the solid electrolyte green sheets 51. Next, side margin sheets 55 formed from the margin paste 53 described in the first embodiment are attached to both ends of the laminated portion in the Y-axis direction. In this manner, a green chip having an approximately rectangular parallelepiped shape can be obtained. The obtained green chip is fired to obtain a laminated chip 60. EXAMPLES
[0059] Example 1 A laminated all-solid-state battery was produced according to the above embodiment. A first internal electrode paste for a first internal electrode layer (positive electrode layer) was applied and formed on a first solid electrolyte green sheet by a screen printing method. A margin paste for a first margin was printed around the first internal electrode paste on the first solid electrolyte green sheet. A second internal electrode paste for a second internal electrode layer (negative electrode layer) was applied and formed on a second solid electrolyte green sheet by a screen printing method. A margin paste for a second margin was printed around the second internal electrode paste on the second solid electrolyte green sheet. The first internal electrode paste for the positive electrode layer and the second internal electrode paste for the negative electrode layer were made to have the same thickness. A plurality of first solid electrolyte green sheets and a plurality of second solid electrolyte green sheets were laminated so that the positive electrode layer and the negative electrode layer were alternately drawn out to the left and right. The green chip of the laminated all-solid-state battery was obtained by cutting to a predetermined size. The green chip was sintered by degreasing and baking, and external electrodes were formed by coating and curing a paste for external electrodes, resulting in a stacked all-solid-state battery.
[0060] In Example 1, LiCoPO4 was used as the positive electrode active material of the first internal electrode layer, TiNb2O7 was used as the negative electrode active material of the second internal electrode layer, glass LAGP was used as the solid electrolyte of the first internal electrode layer and the second internal electrode layer, carbon black was used as the conductive assistant of the first internal electrode layer and the second internal electrode layer, and glass LAGP was used as the solid electrolyte of the solid electrolyte layer. 1.5 Al 0.5 Ge 1.5 P3O 12 ) was used.
[0061] Example 2 In Example 2, the first marginal portion and the second marginal portion are made of glass LAGP (Li 1.5 Al 0.5 Ge 1.5 P3O 12 ) and alumina were used. The other conditions were the same as in Example 1.
[0062] Example 3 In Example 3, the first marginal portion and the second marginal portion are made of glass LAGP (Li 1.5 Al 0.5 Ge 1.5 P3O 12 ) and zirconia were used. The other conditions were the same as in Example 1.
[0063] Example 4 In Example 4, the first marginal portion and the second marginal portion are made of glass LAGP (Li 1.5 Al 0.5 Ge 1.5 P3O 12 ) and crystalline LZP (LiZr2P3O 12 The other conditions were the same as in Example 1.
[0064] Example 5 In Example 5, the first margin portion and the second margin portion are made of crystalline LAGP (Li 1.5 Al 0.5 Ge 1.5 P3O 12 ) and a sintering aid (Li3PO4). The other conditions were the same as in Example 1.
[0065] Comparative Example 1 In Comparative Example 1, the first margin portion and the second margin portion are made of crystalline LAGP (Li 1.5 Al 0.5 Ge 1.5 P3O 12 ) and a sintering aid (Li3BO4) were used. The hardness was adjusted by adjusting the mixing ratio of the sintering aid, glass LAGP, etc. in the first internal electrode layer and the second internal electrode layer. The other conditions were the same as in Example 1.
[0066] Comparative Example 2 In Comparative Example 2, the first marginal portion and the second marginal portion are made of crystalline LAZP(Li 1.3 Al 0.3 Zr 1.7 P3O 12 ) and a sintering aid (Li3BO4). The other conditions were the same as in Example 1.
[0067] Comparative Example 3 In Comparative Example 3, the first marginal portion and the second marginal portion were made of crystalline LAZP(Li 1.3 Al 0.3 Zr 1.7 P3O 12 ) was used. In the first internal electrode layer and the second internal electrode layer, the mixing ratio of the sintering aid, glass LAGP, etc. was adjusted to adjust the hardness. The other conditions were the same as in Example 1.
[0068] (Vickers hardness) For each of the all-solid-state batteries of Examples 1 to 5 and Comparative Examples 1 to 3, a cross-section was processed by a cross-section polisher (CP), and then the Vickers hardness Hv (margin) of the first marginal portion and the second marginal portion was measured according to JIS R 1610, and the Vickers hardness Hc (electrode layer) of the first internal electrode layer and the second internal electrode layer was measured. In addition, the ratio of the Vickers hardness Hv (marginal portion) to the Vickers hardness Hv (electrode layer) was measured. The Vickers tester used was MMT-X3 manufactured by Matsuzawa Co., Ltd., and the indenter was pressed into the target portion for 15 seconds under a load of 3 gf (= 0.029 N), and the length of the diagonal line of the indentation was read, and the Vickers hardness (Hv) was calculated. The results are shown in Table 2. [Table 2]
[0069] The Vickers hardness Hv (margin portion) was 10.77 GPa in Example 1, 8.69 GPa in Example 2, 6.12 GPa in Example 3, 5.40 GPa in Example 4, 3.17 GPa in Example 5, 3.13 GPa in Comparative Example 1, 2.24 GPa in Comparative Example 2, and 1.17 GPa in Comparative Example 3.
[0070] The Vickers hardness Hv (electrode layer) was 1.94 GPa in Example 1, 1.80 GPa in Example 2, 1.76 GPa in Example 3, 1.89 GPa in Example 4, 1.88 GPa in Example 5, 3.48 GPa in Comparative Example 1, 1.80 GPa in Comparative Example 2, and 3.25 GPa in Comparative Example 3.
[0071] The Vickers hardness Hv (margin portion) / Vickers hardness (electrode layer) was 5.55 in Example 1, 4.83 in Example 2, 3.48 in Example 3, 2.86 in Example 4, 1.69 in Example 5, 0.90 in Comparative Example 1, 1.24 in Comparative Example 2, and 0.36 in Comparative Example 3.
[0072] (Long-term charge / discharge cycle characteristics) The capacity retention rate after 100 cycles was measured for each of the all-solid-state batteries of Examples 1 to 5 and Comparative Examples 1 to 3. The charge-discharge test was carried out at room temperature and at a current of 10 μA / cm 2 After charging to 3.4 V at a current density of 100 V, a 10-minute break was taken, followed by discharging to 0 V at the same current density, and the measurement was repeated for 100 cycles. The capacity retention rate was defined as the value obtained by dividing the discharge capacity after 100 cycles by the initial discharge capacity, and a capacity retention rate after 100 cycles of 80% or more was judged as very good (◎), a rate between 70% and 80% was judged as good (◯), a rate between 50% and 70% was judged as fair (△), and a rate less than 50% was judged as poor (×).
[0073] In all of Examples 1 to 5, the long-term charge-discharge cycle characteristics were judged to be very good "◎", good "◯", or somewhat good "△". This is believed to be because the Vickers hardness Hv (margin part) was 3 GPa or more, the Vickers hardness Hv (margin part) / Vickers hardness Hv (electrode layer) exceeded 1, the margin part adjacent to the internal electrode layer had a strong structure, and was reinforced by the pressing from the margin part. In contrast, in all of Comparative Examples 1 to 3, the long-term charge-discharge cycle characteristics were judged to be poor "×". In Comparative Examples 1 and 3, this is believed to be because the Vickers hardness Hv (margin part) / Vickers hardness Hv (electrode layer) did not exceed 1. In Comparative Example 2, this is believed to be because the Vickers hardness Hv (margin part) was less than 3 GPa.
[0074] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]
[0075] 10 First internal electrode layer 20 Second internal electrode layer 30 Solid electrolyte layer 40a First external electrode 40b 2nd external electrode 50 Cover Layer 51 Solid electrolyte green sheet 52 Internal electrode paste 53 Margin paste 54 Cover Sheet 60 Stacked Chips 70 battery capacity area 80a First End Margin 80b Second End Margin 90 Side Margin 95a First margin 95b Second margin 100,100a solid state battery
Claims
1. A solid electrolyte layer; a first internal electrode layer provided on a first main surface of the solid electrolyte layer and including an electrode active material and a solid electrolyte; a first margin provided around the first internal electrode layer on the first main surface; a second internal electrode layer provided on a second main surface of the solid electrolyte layer and including an electrode active material and a solid electrolyte; a second margin provided around the second internal electrode layer on the second main surface, the first marginal portion and the second marginal portion have a Vickers hardness Hv of 3 GPa or more, a ratio of the Vickers hardness Hv of the first marginal portion to a Vickers hardness Hv of the first internal electrode layer is greater than 1, and a ratio of the Vickers hardness Hv of the second marginal portion to a Vickers hardness Hv of the second internal electrode layer is greater than 1; The Vickers hardness Hv is a hardness calculated by reading the length of the diagonal line of an indentation after pressing an indenter into a target location for 15 seconds under a load of 3 gf (=0.029 N).
2. a laminated chip in which the solid electrolyte layer, the first internal electrode layer, the solid electrolyte layer, and the second internal electrode layer are alternately laminated a plurality of times, the laminated chip having a substantially rectangular parallelepiped shape, the first internal electrode layer being drawn out to a first end face of the substantially rectangular parallelepiped shape, and the second internal electrode layer being drawn out to a second end face opposite the first end face of the substantially rectangular parallelepiped shape, the second marginal portion is provided in a region in the vicinity of the first end surface where the first internal electrode layers face each other without the second internal electrode layer therebetween, The all-solid-state battery according to claim 1 , wherein the first marginal portion is provided in a region in the vicinity of the second end face where the second internal electrode layers face each other without the first internal electrode layer therebetween.
3. a laminated chip in which the solid electrolyte layer, the first internal electrode layer, the solid electrolyte layer, and the second internal electrode layer are alternately laminated a plurality of times, the laminated chip having a substantially rectangular parallelepiped shape, the first internal electrode layer being drawn out to a first end face of the substantially rectangular parallelepiped shape, and the second internal electrode layer being drawn out to a second end face opposite the first end face of the substantially rectangular parallelepiped shape, the first marginal portion is provided in a region of the laminated chip from two side surfaces other than the top surface, the bottom surface, the first end surface, and the second end surface in a lamination direction to the first internal electrode layer, The all-solid-state battery according to claim 1 , wherein the second marginal portion is provided in an area of the laminated chip from the two side surfaces to the second internal electrode layer.
4. 2. The all-solid-state battery according to claim 1, wherein the solid electrolyte layer, the first marginal portion, and the second marginal portion contain a phosphate-based solid electrolyte having a NASICON-type crystal structure.
5. The all-solid-state battery according to claim 4 , wherein the phosphate-based solid electrolyte in the first marginal portion and the second marginal portion is glass.
6. 2. The all-solid-state battery according to claim 1, wherein the first marginal portion and the second marginal portion contain at least one of a Li-B-O based compound, a Li-Si-O based compound, a Li-C-O based compound, a Li-S-O based compound, and a Li-P-O based compound.
Citation Information
Patent Citations
All-solid battery
JP2021108258A
All-solid battery and manufacturing method thereof
JP2021140899A
Exterior material for all-solid-state battery, manufacturing method thereof, and all-solid-state battery