Negative electrode active material for all-solid-state battery

The innovative design of the negative electrode active material for all-solid-state batteries, using stacked carbon fragments with internal and surface lithium-affinity substances, addresses conductivity and storage issues, enhancing performance and stability.

JP2024159495APending Publication Date: 2024-11-08HYUNDAI MOTOR CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024025200
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-02-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Conventional all-solid-state batteries face challenges with low lithium ion conductivity, storage properties, energy density, and life characteristics due to the interface reactions between graphite-based negative electrode materials and solid electrolytes, leading to reduced output and lithium precipitation.

Method used

A negative electrode active material is designed with flake carbon fragments stacked to form a predetermined shape, filled with a lithium-affinity first substance and coated with a lithium-affinity second substance, optimizing the internal lithium ion conductivity and preventing side reactions by ensuring uniform interfaces.

Benefits of technology

The solution enhances lithium ion conductivity, improves energy density, and extends the battery life by ensuring rapid lithium ion transmission and preventing lithium precipitation, enabling stable operation at various temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159495000001_ABST
    Figure 2024159495000001_ABST
Patent Text Reader

Abstract

To provide a negative electrode active material for an all-solid-state battery that has excellent lithium ion conductivity and storage property, and to provide a negative electrode active material for an all-solid-state battery that has excellent energy density and life characteristics.SOLUTION: A negative electrode active material for an all-solid-state battery according to the present invention may include: particles having a predetermined shape comprising a plurality of flake carbon fragments overlapped in multiple layers; a first material that fills a space between the flake carbon fragments and has lithium affinity; and a second material that coats at least a part of a surface of each particle and has lithium affinity. The shape of the particles may be spherical, elliptical, or rod-like. A shortest distance between any one flake carbon fragment and another flake carbon fragment adjacent thereto may be 10 nm to 100 nm. The first material may occupy 80% or more of the space between the flake carbon fragments.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an anode active material for an all-solid-state battery, and more particularly to an anode active material for an all-solid-state battery in which a lithium affinity material is deposited on the inside and surface of particles. [Background technology]

[0002] Structurally, a lithium secondary battery is composed of a positive electrode material, a negative electrode material, and an electrolyte that transports lithium ions, which are capable of exchanging lithium ions. Existing batteries include a separator that prevents physical contact between the positive and negative electrodes to prevent short circuits. An all-solid-state battery is a system in which a solid electrolyte plays the role of both the separator and the liquid electrolyte. Therefore, all-solid-state batteries have a significantly lower risk of explosion and are very safe. In addition, solid electrolytes theoretically have faster ion transfer properties than liquid electrolytes, so all-solid-state batteries are expected to be the next generation of high-power and high-energy batteries. Since all components of solid-state batteries are solid, electrons and ions are transferred through the interfaces between particles. Therefore, the interfaces between materials have a dominant influence on battery characteristics. To solve this problem, it is necessary to be able to control the transfer of ions and electrons at the interfaces, and in the process, a reversible reaction of storage and desorption of lithium ions is required. In particular, it is essential to solve this problem with graphite-based materials. Summary of the Invention [Problem to be solved by the invention]

[0003] An object of the present invention is to provide a negative electrode active material for an all-solid-state battery having excellent lithium ion conductivity and storage properties. Another object of the present invention is to provide a negative electrode active material for an all-solid-state battery that has excellent energy density and life characteristics. The object of the present invention is not limited to the object mentioned above. The object of the present invention will become clearer from the following description and can be realized by the means and combinations thereof described in the claims. [Means for solving the problem]

[0004] The negative electrode active material for an all-solid-state battery of the present invention may include particles having a predetermined shape formed by multiple overlapping of flake carbon fragments, a first material having lithium affinity that fills spaces between the flake carbon fragments, and a second material having lithium affinity that coats at least a portion of the surface of the particles. The particles may be spherical, ellipsoidal or rod-shaped in shape. The shortest distance between any one sliquified carbon fragment and another adjacent sliquified carbon fragment may be 10 nm to 100 nm.

[0005] The first material may occupy 80% or more of the space between the silica-like carbon pieces. The first material may include at least one selected from the group consisting of silver (Ag), magnesium (Mg), aluminum (Al), gallium (Ga), zinc (Zn), bismuth (Bi), tin (Sn), indium (In), antimony (Sb), lead (Pb), silicon (Si), germanium (Ge), and combinations thereof, or an alloy of these with lithium. The first material includes silicon (Si) or an alloy of silicon (Si) and lithium, and the first material may be amorphous.

[0006] The second material may cover 90% or more of the total surface of the particle. The second material may have a thickness of 20 nm to 1,000 nm. The second material may include at least one selected from the group consisting of silver (Ag), magnesium (Mg), aluminum (Al), gallium (Ga), zinc (Zn), bismuth (Bi), tin (Sn), indium (In), antimony (Sb), lead (Pb), silicon (Si), germanium (Ge), and combinations thereof, or an alloy of these with lithium. The second material includes silicon (Si) or an alloy of silicon (Si) and lithium, and the second material may be amorphous.

[0007] The negative electrode active material may have an average particle size (D50) of 1 μm to 20 μm. The negative electrode active material may include 40% to 90% by weight of the particles, and 10% to 60% by weight of the first material and the second material combined. The specific surface area of ​​the negative electrode active material is 0.5 m 2 / g~4m 2 / g. According to an embodiment of the present invention, a negative electrode active material for an all-solid-state battery includes secondary particles formed by pelletizing a plurality of primary particles, and the primary particles include a silica-like carbon fragment and a coating portion that is coated on a surface of the silica-like carbon fragment and includes a lithium affinity material.

[0008] The coating portion may include at least one selected from the group consisting of silver (Ag), magnesium (Mg), aluminum (Al), gallium (Ga), zinc (Zn), bismuth (Bi), tin (Sn), indium (In), antimony (Sb), lead (Pb), silicon (Si), germanium (Ge), and combinations thereof, or an alloy of these with lithium. The coating portion may cover 90% or more of the entire surface of the silica-like carbon pieces. The coating may have a thickness of 20 nm to 1,000 nm. The negative electrode active material may include 40% to 90% by weight of the silica-like carbon pieces and 10% to 60% by weight of the coating portion. Effect of the Invention

[0009] According to the present invention, it is possible to obtain a negative electrode active material for an all-solid-state battery having excellent lithium ion conductivity and storage properties. In addition, a negative electrode active material for an all-solid-state battery having excellent energy density and life characteristics can be obtained. The effects of the present invention are not limited to those mentioned above, and should be understood to include all effects that can be inferred from the following description. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 illustrates an all-solid-state battery according to the present invention. [Diagram 2] FIG. 1 is a diagram showing a first embodiment of a negative electrode active material according to the present invention. [Diagram 3] FIG. 2 is a diagram showing particles contained in a negative electrode active material. [Figure 4] FIG. 2 is a reference diagram for explaining the movement of lithium ions (Li+) between the negative electrode active material and the solid electrolyte in the negative electrode according to the present invention. [Figure 5a] FIG. 2 is a diagram showing a negative electrode active material at an early stage of charging. [Figure 5b] FIG. 13 is a diagram showing the negative electrode active material when charging has progressed sufficiently. [Figure 6] FIG. 2 is a diagram showing a second embodiment of a negative electrode active material according to the present invention. [Figure 7] FIG. 2 is a diagram showing primary particles contained in a negative electrode active material. [Figure 8] 8 is a cross-sectional view taken along line AA' in FIG. 7. [Figure 9] FIG. 7 is a cross-sectional view of the negative electrode active material according to FIG. [Figure 10] FIG. 13 is a diagram showing the results of analyzing a cross section of a negative electrode active material according to a manufacturing example using a scanning electron microscope. [Figure 11] FIG. 2 is a diagram showing the results of X-ray spectroscopy for the negative electrode according to Example 1. [Figure 12] 1 is a first charge / discharge graph of a half-cell including a negative electrode according to Example 1. [Figure 13] 1 is a first charge / discharge graph of a half cell including a negative electrode according to Comparative Example 1. [Figure 14] 1 is a high-rate charge / discharge graph of a half cell including a negative electrode according to Example 1. [Figure 15] 1 is a graph showing a high-rate charge / discharge of a half cell including a negative electrode according to Comparative Example 1. [Figure 16] FIG. 13 is a graph showing the measurement of the capacity retention rate of a completed battery according to Comparative Example 2. [Figure 17] FIG. 13 is a graph showing the measurement of the capacity retention rate of a fully charged battery according to Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The above objects, other objects, features and advantages of the present invention can be easily understood from the following preferred embodiments based on the accompanying drawings. However, the present invention is not limited to the embodiments described herein, and may be embodied in other forms. Rather, the embodiments described herein are provided so that the disclosure will be thorough and complete, and so that the concept of the present invention will be fully conveyed to those skilled in the art. In the description of each figure, like reference numerals are used for like elements. In the accompanying drawings, the dimensions of the structures are exaggerated for clarity of the present invention. Terms such as first and second can be used to describe various elements, but the elements should not be limited to the terms. The terms are used only for the purpose of distinguishing one element from another element. For example, the first element can be called the second element, and the second element can be called the first element, without departing from the scope of the present invention. A singular expression includes a plural expression unless the context clearly dictates otherwise.

[0012] In this specification, the terms "comprise" or "have" are intended to specify the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, and should be understood as not precluding the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof. In addition, when a layer, film, region, plate, or other part is said to be "on" another part, this includes not only the case where it is "directly on" the other part, but also the case where there is another part between them. Conversely, when a layer, film, region, plate, or other part is said to be "under" the other part, this includes not only the case where it is "directly under" the other part, but also the case where there is another part between them. Unless otherwise indicated, all numbers, values ​​and / or expressions expressing amounts of ingredients, reaction conditions, polymer compositions and formulations used herein should be understood in all cases to be modified by the term "about" since such numbers are inherently approximations reflecting, among other things, the various uncertainties of measurement that arise in obtaining such values. Also, when numerical ranges are disclosed in the following description, such ranges are continuous and include all values ​​from the minimum value to the maximum value, inclusive, unless otherwise indicated. Furthermore, when such ranges refer to integers, they include all integers from the minimum value to the maximum value, inclusive, unless otherwise indicated.

[0013] 1 is a diagram showing an all-solid-state battery according to the present invention. The all-solid-state battery may include an anode 10, a cathode 20, and a solid electrolyte layer 30 located between the anode 10 and the cathode 20. An anode current collector 40 may be attached to the anode 10, and a cathode current collector 50 may be attached to the cathode 20. The negative electrode 10 may have the shape of a sheet having at least two opposing main surfaces. Each of the two main surfaces may be not only a mathematically flat surface, but may also include a certain curved surface in part, and may have irregularities that occur during the manufacture of the negative electrode 10. In this sense, the shape of the sheet is not limited to a relatively thin rectangular parallelepiped. In the sheet-like negative electrode 10, the distance between two opposing main surfaces can be the thickness of the negative electrode 10. The length of the negative electrode 10 in a first direction (e.g., width direction) perpendicular to the thickness direction is greater than the thickness. Also, the length of the negative electrode 10 in a second direction (e.g., length direction) perpendicular to both the thickness direction and the first direction is greater than the thickness. The thickness of the negative electrode 10 is not particularly limited, but may be 1 μm to 100 μm. The thickness of the negative electrode 10 may refer to an average value obtained by measuring the measurement object at five points. The thickness of the negative electrode 10 may also refer to the thickness of the all-solid-state battery during discharge. The negative electrode 10 can include a negative electrode active material, a solid electrolyte, a binder, and the like.

[0014] 2 is a diagram showing a first embodiment of an anode active material 100 according to the present invention. The anode active material 100 may include particles 110 having a predetermined shape, a first material 120 filled inside the particles 110 and having an affinity for lithium, and a second material 130 coated on at least a portion of the surface of the particles 110 and having an affinity for lithium. Conventional solid-state batteries contain graphite-based negative electrode active materials. + ) is inserted and removed, and thus charging and discharging proceeds. In a lithium-ion battery using a liquid electrolyte, the inside and outside of the graphite-based negative electrode active material are impregnated with the liquid electrolyte, so there is no problem with the movement of lithium ions. However, in an all-solid-state battery using a solid electrolyte, lithium ions are smoothly conducted at the contact area between the surface of the graphite-based negative electrode active material and the solid electrolyte, but inside the graphite-based negative electrode active material, movement is possible only by diffusion, so the transmission path of lithium ions becomes very long. In other words, at room temperature or low temperature, where the rate of movement by diffusion is slow, the output of the all-solid-state battery is very low, and there is a problem that lithium is easily precipitated.

[0015] In addition, conventional all-solid-state batteries consist of a graphite-based negative electrode active material and a solid electrolyte, which are connected to carbon, a solid electrolyte, and lithium ions (Li + A solid electrolyte interphase layer is formed by the oxidation / reduction reaction of the lithium ions (Li + It also induces the formation of lithium dendrites on the surface of the solid electrolyte, shortening the life of the battery. The present invention is intended to solve such problems of conventional graphite-based negative electrode active materials, and is characterized in that a material having lithium affinity is sufficiently deposited inside and on the surface of the particles 110 to increase the lithium ion conductivity inside the negative electrode active material 100 and to prevent side reactions between the particles 110 and the solid electrolyte while making the interface between the negative electrode active material 100 and the solid electrolyte uniform, as will be described later.

[0016] 3 is a diagram showing the particle 110. The particle 110 may include a plurality of overlapping flake carbon fragments 111 and spaces 112 between the flake carbon fragments. The particles 110 may be formed by granulating the scaly carbon fragments 111 in a concentric, cabbage-like, or random manner. Although the particles 110 in FIG. 3 are spherical, the shape of the particles 110 is not limited thereto, and the shape of the particles 110 may be elliptical, rod-like, or the like. The scale-like carbon pieces 111 may be scale-like thin pieces. The shortest distance between any one of the scallop-like carbon fragments 111 and another adjacent one thereof may be 10 nm to 100 nm. Here, the shortest distance may refer to the distance between any one layer of the scallop-like carbon fragments 111 and another layer when the scallop-like carbon fragments 111 are piled up to form a series of layers. Also, the shortest distance may refer to the size of the space 112 based on the cross section of the scallop-like carbon fragments 111. If the shortest distance is less than 10 nm, it may be difficult for the first material 120 to be deposited in the space 112, and if it exceeds 100 nm, it may be difficult to evaporate lithium ions (Li + ) may lose its conductivity.

[0017] The spaces 112 may be pores in the particles 110 that are generated during the process of granulating the silica-like carbon fragments 111 by stacking them in layers. The spaces 112 may be formed continuously or discontinuously from the surface to the center of the particles 110. The first material 120 may fill the spaces 112 between the silicate carbon fragments 111. The first material 120 may also include a metal or metalloid having lithium affinity. Here, having lithium affinity may mean that it can form an alloy with lithium. A lithium alloy is formed by combining lithium ions (Li + ) and attracts lithium ions (Li + ) can increase the diffusion rate. As described above, the space 112 can be continuously formed from the surface to the center of the particle 110. Therefore, when the space 112 is filled with the first material 120, lithium ions (Li +) can migrate more easily. Therefore, the all-solid-state battery according to the present invention can be operated at room temperature or low temperature without problems such as output reduction and excessive precipitation of lithium. This will be described later.

[0018] The first material 120 may occupy 80% or more of the space 112 based on the total volume of the space 112. If the filling rate of the first material 120 is less than 80%, the lithium ions (Li + The upper limit of the filling rate of the first substance 120 is not particularly limited, and may be 100% or less, 99% or less, 95% or less, or 90% or less. The first material 120 may include at least one selected from the group consisting of silver (Ag), magnesium (Mg), aluminum (Al), gallium (Ga), zinc (Zn), bismuth (Bi), tin (Sn), indium (In), antimony (Sb), lead (Pb), silicon (Si), germanium (Ge), and combinations thereof, or an alloy of these with lithium. Preferably, the first material 120 may include silicon (Si) or an alloy of silicon (Si) and lithium. More preferably, the first material 120 may include amorphous silicon (Si) or an alloy of amorphous silicon (Si) and lithium. Since amorphous silicon expands isotropically, it is possible to minimize deformation and detachment of the first material 120, and to prevent lithium ions (Li ions) between the first material 120 and the particles 110. + ) can also be easily transmitted. The second material 130 may cover at least a portion of the surface of the particle 110. The second material 130 may prevent the particle 110 from contacting the solid electrolyte. If the particle 110 is exposed to the outside and contacts the solid electrolyte, the solid electrolyte may decompose due to the high electronic conductivity of the particle 110.

[0019] The second material 130 can include a metal or metalloid having an affinity for lithium. Since the second material 130 covers most of the surface of the particle 110, the lithium ions (Li +) can be inserted into the negative electrode active material 100 more quickly than when the second material 130 is not present. + ) is transmitted faster than the particle 110. The second material 130 may cover 90% or more of the total surface area of ​​the particles 110. The upper limit of the coverage rate of the second material 130 is not particularly limited, and may be 100% or less, 99% or less, or 95% or less. The thickness of the second material 130 may be 20 nm to 1,000 nm. The thickness of the second material 130 may be measured, for example, by observation using a transmission electron microscope (TEM). It is preferable to use a large number of samples, and for example, the thicknesses of the second material 130 formed on 10 or more, preferably 100 or more negative electrode active materials 100 may be measured and calculated as an average value. If the thickness is less than 20 nm, the second material 130 may not be able to sufficiently cover the surface of the particles 110, and if it exceeds 1,000 nm, the productivity may decrease and the physical properties of the negative electrode active material 100 may be adversely affected.

[0020] The second material 130 may include at least one selected from the group consisting of silver (Ag), magnesium (Mg), aluminum (Al), gallium (Ga), zinc (Zn), bismuth (Bi), tin (Sn), indium (In), antimony (Sb), lead (Pb), silicon (Si), germanium (Ge), and combinations thereof, or an alloy of these with lithium. Preferably, the second material 130 may include silicon (Si) or an alloy of silicon (Si) and lithium. More preferably, the second material 130 may include amorphous silicon (Si) or an alloy of amorphous silicon (Si) and lithium. Since amorphous silicon expands isotropically, it is possible to minimize deformation and detachment of the second material 130, and to prevent lithium ions (Li ions) between the second material 130 and the particles 110. + ) can also be easily transmitted.

[0021] The negative electrode active material 100 may include 40% to 90% by weight of the particles 110, and 10% to 60% by weight of the first material 120 and the second material 130. If the combined weight of the first material 120 and the second material 130 is less than 10% by weight, the first material 120 may not be able to sufficiently fill the spaces 112, or the second material 130 may not be able to sufficiently cover the surfaces of the particles 110. If the combined weight of the first material 120 and the second material 130 exceeds 60% by weight, the second material 130 may be too thick. The average particle size (D50) of the negative electrode active material 100 may be 1 μm to 20 μm. The average particle size (D50) can be measured using a commercially available laser diffraction scattering type particle size distribution measuring device, for example, a Microtrack particle size distribution measuring device. The average particle size can also be calculated by randomly extracting 200 particles from an electron microscope photograph. When the average particle size (D50) of the negative electrode active material 100 is 1 μm or more, the density of the negative electrode 10 can be increased, and therefore the discharge capacity per volume can be improved, and when it is 20 μm or less, the chargeability and cycle characteristics can be improved. The specific surface area of ​​the negative electrode active material 100 is 0.5 m 2 / g~4m 2 The specific surface area may be 0.1 to 1.0 μm / g. The specific surface area may be measured by the BET (Brunauer Emmett-Teller) method using nitrogen adsorption, and may be measured using a commonly used specific surface area measuring device (such as MOUNTECH's Macsorb HM (model 1210) or MicrotracBEL's Belsorp-mini). When the specific surface area is within the numerical range, it may be advantageous for suppressing the volume expansion of the negative electrode active material 100.

[0022] The method for manufacturing the negative active material 100 is not particularly limited. After preparing particles 110 in which silica-like carbon fragments 111 are stacked in a predetermined shape as shown in Fig. 3, metal or semi-metal elements corresponding to the first material 120 and the second material 130 are deposited on the particles 110 to manufacture the negative active material 100. The deposition may be, for example, a chemical vapor deposition (CVD) method or a physical vapor deposition (PVD) method, and considering the filling rate of the first material 120, the coverage rate of the second material 130, and the uniform thickness of the second material 130, it is preferable to deposit the negative active material 100 by the chemical vapor deposition method. The negative electrode 10 may include a solid electrolyte having lithium ion conductivity. The solid electrolyte may be an oxide-based solid electrolyte or a sulfide-based solid electrolyte. It is preferable to use a sulfide-based solid electrolyte having high lithium ion conductivity.

[0023] Sulfide-based solid electrolytes are 2 SP 2 S 5 , Li 2 SP 2 S 5 - LiI, Li 2 SP 2 S 5 -LiCl, Li 2 SP 2 S 5 -LiBr, Li 2 SP 2 S 5 -Li 2 O, Li 2 SP 2 S 5 -Li 2 O-LiI, Li 2 S-SiS 2 , Li 2 S-SiS 2 - LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 - LiI, Li2 S-SiS 2 -P 2 S 5 - LiI, Li 2 S.B. 2 S 3 , Li 2 SP 2 S 5 -Z m S n (where m and n are positive numbers, and Z is one of Ge, Zn, and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MO y (where x and y are positive numbers, and M is one of P, Si, Ge, B, Al, Ga, and In), Li 10 GeP 2 S 12 etc.

[0024] FIG. 4 shows the relationship between the lithium ion (Li ) between the negative electrode active material 100 and the solid electrolyte 200 in the negative electrode 10 according to the present invention. + 5A is a diagram showing the negative electrode active material 100 at the beginning of charging, and FIG 5B is a diagram showing the negative electrode active material 100 after charging has progressed sufficiently. During charging of the all-solid-state battery, lithium ions (Li + ) is inserted into the negative electrode active material 100 via a solid electrolyte 200 having lithium ion conductivity in the negative electrode 10 . Since the second material 130 covers most of the surface of the particle 110, the particle 110 does not come into contact with the solid electrolyte 200. Therefore, the surface of the negative electrode active material 100 is free of the particle 110, the solid electrolyte 200, and lithium ions (Li +) and the solid electrolyte interphase layer due to the oxidation and reduction reaction of electrons. The solid electrolyte interphase layer induces the depletion of lithium in the all-solid-state battery and the lithium ions (Li + However, the present invention is characterized in that it solves this problem by coating the surface of the particle 110 with the second material 130.

[0025] 4 and 5a, lithium ions (Li + ) reacts with the second material 130 to form an outer lithium alloy 130'. As charging continues, the lithium ion (Li + ) can diffuse and move inside the negative electrode active material 100. + ) is inserted into the particle 110. At this time, the first material 120 filled inside the particle 110 becomes lithium ions (Li + ) to form the inner lithium alloy 120' as shown in FIG. 5b. The inner lithium alloy 120' reacts with lithium ions (Li + ) transmission path, lithium ions (Li + ) diffusion rate increases. Then, lithium ion (Li + When the positive electrode 102 diffuses further into the negative electrode active material 100 and is inserted into the particles 110 until it reaches the capacity of the particles 110, charging is completed. In the negative electrode active material 100, lithium ions (Li + Since the transport path of the cations is short and the diffusion rate is fast, the solid-state battery according to the present invention can operate normally even when driven at room temperature or low temperature or when the output is high.

[0026] The negative electrode 10 may include a binder. The binder can adhere the negative electrode active material 100 and the solid electrolyte 200 together. The type of binder is not particularly limited, and may include, for example, butadiene rubber, nitrile butadiene rubber, hydrogenated nitrile butadiene rubber, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), carboxymethyl cellulose (CMC), and the like. The negative electrode 10 may contain 80% to 85% by weight of the negative electrode active material 100, 10% to 15% by weight of the solid electrolyte 200, and 1% to 5% by weight of a binder, although the content of each component may be appropriately adjusted in consideration of the capacity, efficiency, etc. of the intended all-solid-state battery.

[0027] 6 is a diagram showing a second embodiment of the negative electrode active material 100 according to the present invention. The negative electrode active material 100 may include secondary particles 140 formed by pelletizing a plurality of primary particles 150. Fig. 7 is a diagram showing a primary particle 150. Fig. 8 is a cross-sectional view taken along line AA' in Fig. 7. Fig. 9 is a cross-sectional view of the negative electrode active material 100 according to Fig. 6. The secondary particles 140 may be formed by granulating the primary particles 150 into a concentric circle shape, a cabbage shape, or randomly. Although the secondary particles 140 in Fig. 6 are spherical, the shape of the secondary particles 140 is not limited thereto, and the shape of the secondary particles 140 may be an ellipse, a rod shape, etc. The primary particles 150 may include a silica-like carbon fragment 111 and a coating portion 113 that is coated on the surface of the silica-like carbon fragment 111 and includes a lithiophilic material.

[0028] Since the silica-like carbon fragments 111 have been described above, a detailed description thereof will be omitted below. The coating portion 113 may cover 90% or more of the entire surface of the silica-like carbon pieces 111. The upper limit of the coverage of the coating portion 113 is not particularly limited, and may be 100% or less, 99% or less, or 95% or less. When the coverage of the coating portion 113 is 90% or more, the lithium affinity material may be sufficiently filled and / or coated inside and on the surface of the negative electrode active material 100, as shown in FIG. 9. The thickness of the coating portion 113 may be 20 nm to 1,000 nm. The thickness of the second material 130 may be measured, for example, by observation using a transmission electron microscope (TEM). It is preferable to use a large number of samples, and for example, the thicknesses of the coating portions 113 formed on 10 or more, preferably 100 or more primary particles 150 may be measured and calculated as an average value.

[0029] The negative electrode active material 100 may include 40% to 90% by weight of the silica-like carbon fragments 111 and 10% to 60% by weight of the coating portion 113. If the coating portion 113 is less than 10% by weight, the lithium affinity material may not be sufficiently filled and / or coated inside and on the surface of the negative electrode active material 100, and if it exceeds 60% by weight, the coating portion 113 may become too thick. The coating portion 113 may include at least one selected from the group consisting of silver (Ag), magnesium (Mg), aluminum (Al), gallium (Ga), zinc (Zn), bismuth (Bi), tin (Sn), indium (In), antimony (Sb), lead (Pb), silicon (Si), germanium (Ge), and combinations thereof, or an alloy of these with lithium. Preferably, the coating portion 113 may include silicon (Si) or an alloy of silicon (Si) and lithium. More preferably, the coating portion 113 may include amorphous silicon (Si) or an alloy of amorphous silicon (Si) and lithium. Since amorphous silicon expands isotropically, deformation and detachment of the coating portion 113 may be minimized, and lithium ions (Li +) can also be easily transmitted.

[0030] There is no particular limitation on the method for manufacturing the negative active material 100. After a lithium affinity material is deposited on the surface of the silica-like carbon fragments 111 to prepare primary particles 150, the primary particles 150 may be pelletized to manufacture the negative active material 100 in the form of secondary particles 140. The positive electrode 20 may have a sheet shape having at least two opposing main surfaces. Each of the two main surfaces may be not only a mathematically flat surface, but may also include a certain curved surface in part, and may have unevenness that occurs during the manufacture of the positive electrode 20. In this sense, the sheet shape is not limited to a relatively thin rectangular parallelepiped. In the sheet-like positive electrode 20, the distance between two opposing main surfaces can be the thickness of the positive electrode 20. The length of the positive electrode 20 in a first direction (e.g., width direction) perpendicular to the thickness direction is greater than the thickness. Also, the length of the positive electrode 20 in a second direction (e.g., length direction) perpendicular to both the thickness direction and the first direction is greater than the thickness. The thickness of the positive electrode 20 is not particularly limited, but may be 1 μm to 100 μm. The thickness of the positive electrode 20 may mean an average value when the measurement object is measured at five points. The thickness of the positive electrode 20 may also mean the thickness of the all-solid-state battery during discharge. The positive electrode 20 can include a positive electrode active material, a solid electrolyte, a conductive material, a binder, and the like.

[0031] The positive electrode active material is capable of absorbing and releasing lithium ions. The positive electrode active material is LiCoO 2 , LiMnO 2 , LiNiO 2 , LiVO 2 , Li 1+x Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 Rock salt layer type active materials such as LiMn 2 O 4 , Li(Ni 0.5 Mn 1.5 )O 4 Spinel-type active materials such as LiNiVO 4 , LiCoVO 4Inverse spinel type active materials such as, LiFePO 4 , LiMnPO 4 , LiCoPO 4 , LiNiPO 4 Olivine type active materials such as, Li 2 FeSiO 4 , Li 2 MnSiO 4 Silicon-containing active materials such as, LiNi 0.8 Co (0.2-x) Al x O 2 Rock salt layer type active materials in which part of the transition metal is replaced with a different metal as in Li 1+x Mn 2-x-y M y O 4 (M is at least one of Al, Mg, Co, Fe, Ni, and Zn, and 0 < x + y < 2), spinel type active materials in which part of the transition metal is replaced with a different metal, Li 4 Ti 5 O 12 It can contain lithium titanate such as Li The solid electrolyte can include an oxide-based solid electrolyte or a sulfide-based solid electrolyte.

[0032] It is preferable to use a sulfide-based solid electrolyte with high lithium ion conductivity. The sulfide-based solid electrolyte is not particularly limited, but Li 2 S-P 2 S 5 , Li 2 S-P 2 S 5 -LiI, Li 2 S-P 2 S 5 -LiCl, Li 2 S-P 2 S 5 -LiBr, Li 2 S-P 2 S 5 -Li 2 O, Li 2 S-P 2 S 5 -Li 2 O-LiI, Li 2 S-SiS 2 , Li 2S-SiS 2 - LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 - LiI, Li 2 S-SiS 2 -P 2 S 5 - LiI, Li 2 S.B. 2 S 3 , Li 2 SP 2 S 5 -Z m S n (where m and n are positive numbers, and Z is one of Ge, Zn, and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MO y (where x and y are positive numbers, and M is one of P, Si, Ge, B, Al, Ga, and In), Li 10 GeP 2 S 12 The solid electrolyte contained in the positive electrode 20 may be the same as or different from the solid electrolyte contained in the negative electrode 10.

[0033] The conductive material may include carbon black, conductive graphite, ethylene black, graphene, and the like. The binder may include butadiene rubber, nitrile butadiene rubber, hydrogenated nitrile butadiene rubber, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), carboxymethyl cellulose (CMC), etc. The binder included in the positive electrode 20 may be the same as or different from the binder included in the negative electrode 10.

[0034] The solid electrolyte layer 30 may have a sheet shape having at least two opposing main surfaces. Each of the two main surfaces may be not only a mathematically flat surface, but may also include a certain curved surface in part, and may have unevenness that occurs during the manufacture of the solid electrolyte layer 30. In this sense, the sheet shape is not limited to a relatively thin rectangular parallelepiped. In the sheet-like solid electrolyte layer 30, the distance between two opposing main surfaces may be the thickness of the solid electrolyte layer 30. The length of the solid electrolyte layer 30 in a first direction (e.g., width direction) perpendicular to the thickness direction is greater than the thickness. Also, the length of the solid electrolyte layer 30 in a second direction (e.g., length direction) perpendicular to both the thickness direction and the first direction is greater than the thickness. The thickness of the solid electrolyte layer 30 is not particularly limited, but may be 1 μm to 100 μm. The thickness of the solid electrolyte layer 30 may refer to the average value when the measurement object is measured at five points. The solid electrolyte layer 30 may include a solid electrolyte having lithium ion conductivity. The solid electrolyte may include at least one selected from the group consisting of oxide-based solid electrolytes, sulfide-based solid electrolytes, and combinations thereof. The solid electrolyte may be crystalline, amorphous, or a mixture thereof.

[0035] The oxide-based solid electrolyte is the perovskite type LLTO (Li 3x La 2 / 3-xTiO 3 ), phosphate-based NASICON-type LATP(Li 1+x Al x Ti 2-x (PO 4 ) 3 ) etc. Sulfide-based solid electrolytes are 2 SP 2 S 5 , Li 2 SP 2 S 5 - LiI, Li 2 SP 2 S 5 -LiCl, Li 2 SP 2 S 5 -LiBr, Li 2 SP 2 S 5 -Li 2 O, Li 2 SP 2 S 5 -Li 2 O-LiI, Li 2 S-SiS 2 , Li 2 S-SiS 2 - LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 - LiI, Li 2 S-SiS 2 -P 2 S 5 - LiI, Li 2 S.B. 2 S 3 , Li 2 SP 2 S 5 -Z m S n (where m and n are positive numbers, and Z is one of Ge, Zn, and Ga), Li 2 S-GeS 2 , Li 2 S-SiS2 -Li 3 PO 4 、Li 2 S - SiS 2 -Li x MO y (where x and y are positive numbers, and M is one of P, Si, Ge, B, Al, Ga, and In), Li 10 GeP 2 S 12 etc. can be included. Preferably, the solid electrolyte can include a sulfide - based solid electrolyte having an argyrodite - type crystal structure. The sulfide - based solid electrolyte having an argyrodite crystal structure contains Li 7-x PS 6-x Cl x (0 < x ≤ 2), Li 7-x PS 6-x Br x (0 < x ≤ 2), Li 7-x PS 6-x I x (0 < x ≤ 2) and can include at least one selected from the group consisting of these combinations.

[0036] The negative electrode current collector 40 can be a plate - shaped base material having electrical conductivity. Specifically, the negative electrode current collector 40 can be in the form of a sheet, thin film, or foil. The negative electrode current collector 40 can include a material that does not react with lithium. Specifically, the negative electrode current collector 40 can include at least one selected from the group consisting of nickel (Ni), copper (Cu), stainless steel, and combinations thereof. The thickness of the negative electrode current collector 40 is not particularly limited, and can be, for example, 1 μm to 500 μm. The positive electrode current collector 50 can include a plate - shaped base material having electrical conductivity. Specifically, the positive electrode current collector 50 can be in the form of a sheet, thin film, or foil. The positive electrode current collector 50 can include an aluminum thin plate (Aluminium foil). The thickness of the positive electrode current collector 50 is not particularly limited, and can be, for example, 1 μm to 500 μm.

[0037] Hereinafter, other aspects of the present invention will be described in more detail with reference to examples. The following examples are merely illustrative for the purpose of aiding in the understanding of the present invention, and are not intended to limit the scope of the present invention. Manufacturing Example Particles were prepared that were nearly spherical or elliptical in shape, with multiple overlapping silicate fragments. Silicon was deposited on the inside and surface of the particles using chemical vapor deposition. Specifically, the particles were placed in a chamber, the chamber was evacuated, and a reaction gas containing silicon was injected into the chamber. The inside of the chamber was heated to a predetermined temperature, and the silicon contained in the reaction gas was deposited as the first material and the second material on the inside and surface of the particles, respectively, to produce the negative electrode active material. The negative electrode active material according to this manufacturing example contains 70% by weight of particles and 30% by weight of the first material and the second material combined. Figure 10 shows the results of a scanning electron microscope analysis of a cross section of the negative active material according to a manufacturing example. The dark areas are particles formed by pelletizing the scallop-like carbon fragments, and the bright areas are the first and second materials. From this, it can be seen that the thickness of the second material coated on the surface of the particles was 20nm to 1,000nm, and was formed uniformly with almost no thickness deviation.

[0038] Comparative Manufacturing Example 1 The particles of the production example in which silicon was not deposited were designated as Comparative Production Example 1. Comparative Manufacturing Example 2 A negative electrode active material was prepared in the same manner as in Preparation Example, except that the negative electrode active material contained 95% by weight of the particles and 5% by weight of the first material and the second material combined. Example 1 The negative electrode active material according to the manufacturing example, the sulfide-based solid electrolyte, and the binder were put into a solvent to prepare a slurry. The slurry was applied onto a negative electrode current collector to form a negative electrode having a thickness of about 50 μm. Nitrile butadiene rubber (NBR) was used as the binder, and hexyl butyrate was used as the solvent.

[0039] 11 shows the results of X-ray spectroscopy for the negative electrode according to Example 1. The results on the bottom are for the negative electrode immediately after production, and the results on the top are for the negative electrode after two weeks have passed. Peaks due to the solid electrolyte and particles are observed, but no peaks due to silicon are observed, indicating that the silicon deposited on the negative electrode active material is amorphous. A solid electrolyte layer containing a sulfide-based solid electrolyte was laminated on the negative electrode, and lithium metal was laminated on the solid electrolyte layer to form a half cell. Comparative Example 1 A half cell was fabricated in the same manner as in Example 1, except that the negative electrode active material of Comparative Production Example 1 was used.

[0040] Experimental Example 1 Fig. 12 is a first charge / discharge graph of a half-cell including the negative electrode according to Example 1. Fig. 13 is a first charge / discharge graph of a half-cell including the negative electrode according to Comparative Example 1. The characteristics were evaluated at 30°C and 60°C, respectively. Comparative Example 1 shows relatively high reactivity in the initial charging reaction (>0.5 V). This is a reaction that forms an irreversible resistance layer, and is not visible in the results of Example 1. When evaluated at 30° C., the initial efficiency of Example 1 is about 91.8%, and the initial efficiency of Comparative Example 1 is about 89.5%. When evaluated at 60° C., the initial efficiency of Example 1 is about 90.0%, and the initial efficiency of Comparative Example 1 is about 88.2%. Experimental Example 2 Current density was set to 2mA / cm 2 The deposition capacity was increased to 3.5 mAh / cm and the charge / discharge characteristics were evaluated in the same manner as above. 2 was set to.

[0041] Fig. 14 is a graph showing high-rate charge / discharge of a half-cell including the negative electrode according to Example 1. Fig. 15 is a graph showing high-rate charge / discharge of a half-cell including the negative electrode according to Comparative Example 1. The characteristics were evaluated at 30°C and 60°C, respectively. 15, Comparative Example 1 shows a large difference in capacity according to temperature. At low temperatures where lithium movement is limited, lithium insertion is not smooth. This occurs because lithium movement between the particle surface and the solid electrolyte is not smooth. In addition, the solid electrolyte interface layer formed at the interface between the particle and the solid electrolyte acts as a resistor and can hinder lithium movement. 14, the temperature variation of lithium stored in the negative active material is significantly reduced in Example 1. This is because the first and second materials contribute to the rapid migration of lithium into the negative active material.

[0042] Example 2 A solid electrolyte layer containing a sulfide-based solid electrolyte was laminated on the negative electrode of Example 1, and a positive electrode containing a positive electrode active material, a solid electrolyte, a conductive material, and a binder was laminated on the solid electrolyte layer to form a complete battery. Nickel-cobalt-manganese oxide was used as the positive electrode active material. Comparative Example 2 A complete battery was fabricated in the same manner as in Example 2, except that the negative electrode active material of Comparative Preparation Example 2 was used.

[0043] Fig. 16 is a diagram showing the measurement of the capacity retention rate of a full battery according to Comparative Example 2. Fig. 17 is a diagram showing the measurement of the capacity retention rate of a full battery according to Example 2. It can be seen that Example 2, in which the contents of the first and second materials are high and silicon is sufficiently deposited inside and on the surfaces of the particles, has a much better capacity retention rate than Comparative Example 2 and operates stably. Although the experimental examples and examples of the present invention have been described in detail above, the scope of the present invention is not limited to the above experimental examples and examples, and many variations and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims are also included in the scope of the present invention. [Explanation of symbols]

[0044] 10 negative electrode 20 positive electrode 30 Solid electrolyte layer 40 Negative electrode current collector 50 Positive electrode current collector 100 Anode active material 110 particles 111 Lintous carbon fragment 112 Space 113 Coating Department 120 First substance 130 Second substance 140 Secondary particles 150 Primary particles 200 Solid electrolyte

Claims

1. A particle having a predetermined shape formed by multiple overlapping flake carbon fragments; a first substance having an affinity for lithium, the first substance being filled in the space between the silicate carbon fragments; and a second substance having lithium affinity and coating at least a portion of the surface of the particles.

2. The negative electrode active material for an all-solid-state battery according to claim 1 , wherein the particles have a spherical, elliptical or rod-shaped shape.

3. 2. The negative electrode active material for an all-solid-state battery according to claim 1, wherein the shortest distance between any one of the scale-like carbon fragments and another adjacent scale-like carbon fragment is 10 nm to 100 nm.

4. The negative electrode active material for an all-solid-state battery according to claim 1 , wherein the first material occupies 80% or more of the space between the silica-like carbon pieces.

5. 2. The negative electrode active material for an all-solid-state battery according to claim 1, wherein the first material comprises at least one selected from the group consisting of silver (Ag), magnesium (Mg), aluminum (Al), gallium (Ga), zinc (Zn), bismuth (Bi), tin (Sn), indium (In), antimony (Sb), lead (Pb), silicon (Si), germanium (Ge), and combinations thereof, or an alloy of any of these with lithium.

6. the first material comprises silicon (Si) or an alloy of silicon (Si) and lithium; The negative electrode active material for an all-solid-state battery according to claim 1 , wherein the first material is amorphous.

7. 2 . The negative electrode active material for an all-solid-state battery according to claim 1 , wherein the second material is coated on 90% or more of the entire surface of the particle.

8. 2. The negative electrode active material for an all-solid-state battery according to claim 1, wherein the second material has a thickness of 20 nm to 1,000 nm.

9. 2. The negative electrode active material for an all-solid-state battery according to claim 1, wherein the second material comprises at least one selected from the group consisting of silver (Ag), magnesium (Mg), aluminum (Al), gallium (Ga), zinc (Zn), bismuth (Bi), tin (Sn), indium (In), antimony (Sb), lead (Pb), silicon (Si), germanium (Ge), and combinations thereof, or an alloy of any of these with lithium.

10. the second material comprises silicon (Si) or an alloy of silicon (Si) and lithium; The negative electrode active material for an all-solid-state battery according to claim 1 , wherein the second material is amorphous.

11. 2. The negative electrode active material for an all-solid-state battery according to claim 1, wherein the average particle size (D50) of the negative electrode active material is 1 μm to 20 μm.

12. The negative electrode active material is 40% to 90% by weight of the particles; The negative electrode active material for an all-solid-state battery according to claim 1, wherein the sum of the first material and the second material is 10 wt % to 60 wt %.

13. The specific surface area of ​​the negative electrode active material is 0.5 m 2 / g to 4m 2 The negative electrode active material for an all-solid-state battery according to claim 1, wherein the molecular weight of the negative electrode active material is 1 / g.

14. The secondary particles are formed by pelletizing a plurality of primary particles, The primary particles are A sliver of carbon; a coating portion that is coated on a surface of the silica-like carbon pieces and that includes a lithium affinity material.

15. The negative electrode active material for an all-solid-state battery according to claim 14, wherein the shortest distance between any one of the scale-like carbon fragments and another adjacent scale-like carbon fragment is 10 nm to 100 nm.

16. 15. The negative electrode active material for an all-solid-state battery according to claim 14, wherein the coating portion contains at least one selected from the group consisting of silver (Ag), magnesium (Mg), aluminum (Al), gallium (Ga), zinc (Zn), bismuth (Bi), tin (Sn), indium (In), antimony (Sb), lead (Pb), silicon (Si), germanium (Ge), and combinations thereof, or an alloy of any of these with lithium.

17. The negative electrode active material for an all-solid-state battery according to claim 14, wherein the coating portion covers 90% or more of the entire surface of the silica-like carbon pieces.

18. The negative electrode active material for an all-solid-state battery according to claim 14, wherein the coating portion has a thickness of 20 nm to 1,000 nm.

19. The negative electrode active material is 40% to 90% by weight of the silica-like carbon fragments; The negative electrode active material for an all-solid-state battery according to claim 14, comprising: 10% by weight to 60% by weight of the coating portion.

20. The specific surface area of ​​the negative electrode active material is 0.5 m 2 / g to 4m 2 The negative electrode active material for an all-solid-state battery according to claim 14, characterized in that