Composite substrate for surface acoustic wave device

The composite substrate with a piezoelectric single crystal thin film and intervening layer addresses energy leakage and spurious noise issues, enhancing the reliability and frequency characteristics of surface acoustic wave devices.

JP2024162125AActive Publication Date: 2024-11-21SHIN ETSU CHEMICAL CO LTD

Patent Information

Application Number
JP2023077370
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-21
Estimated Expiration
2043-05-09

AI Technical Summary

Technical Problem

Existing composite substrates for surface acoustic wave devices suffer from energy leakage and spurious noise due to elastic wave interactions at the bonding interface, leading to increased loss and deteriorated frequency characteristics.

Method used

A composite substrate comprising a piezoelectric single crystal thin film, a supporting substrate, and an intervening layer with controlled thickness and attenuation properties, optimized for low loss and high reliability.

Benefits of technology

The solution reduces passband loss and suppresses spurious noise, ensuring high reliability and improved frequency performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162125000005
    Figure 2024162125000005
  • Figure 2024162125000006
    Figure 2024162125000006
  • Figure 2024162125000007
    Figure 2024162125000007
Patent Text Reader

Abstract

To provide a composite substrate for a surface acoustic wave device having less loss in a filter passband, fewer spurious components, and excellent performance and reliability.SOLUTION: A composite substrate for a surface acoustic wave device includes a piezoelectric single crystal thin film, a support substrate, and at least one type of intervening layer disposed between the piezoelectric single crystal thin film and the support substrate, and the intervening layer is in contact with the piezoelectric single crystal thin film, the total thickness of the intervening layer is equal to or less than twice the wavelength of the surface acoustic wave, and the attenuation of longitudinal waves of the intervening layer calculated at frequencies between 40 GHz and 60 GHz using the Brillouin oscillation method is equal to or less than 8×10-2 (nm-1 THz-2).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite substrate for a surface acoustic wave device, which comprises a piezoelectric single crystal thin film and a supporting substrate. [Background technology]

[0002] Mobile phones and other devices use surface acoustic wave (SAW) devices, which have interdigital transducers (IDTs) formed on a piezoelectric substrate to excite surface acoustic waves, as frequency adjustment and selection components. Surface acoustic wave devices are required to be small, have low insertion loss, and block unwanted waves, and lithium tantalate (LiTaO 3 ;LT) and lithium niobate (LiNbO 3 Piezoelectric materials such as ZnO (LiNb) are used.

[0003] On the other hand, under the communication standards for 4th generation and later mobile phones, the piezoelectric materials used in surface acoustic wave devices must have sufficiently small temperature-induced characteristic variations. Also, to prevent unnecessary noise from spilling out between bands, filters, duplexers, and multiplexers must have as small an insertion loss as possible, and the shoulder characteristics of filters must be extremely steep, so that the resonators that make up the filters must have a high Q (Quality Factor). Filters are also required to be able to handle a wide bandwidth depending on the band used.

[0004] Regarding materials used in such surface acoustic wave devices, composite substrates made of piezoelectric materials and other materials have been considered. For example, Patent Document 1 discloses an acoustic wave device having a piezoelectric film, the acoustic wave device including a support substrate, a high acoustic velocity film formed on the support substrate and having a bulk wave acoustic velocity faster than the acoustic wave acoustic velocity propagating through the piezoelectric film, a low acoustic velocity film laminated on the high acoustic velocity film and having a bulk wave acoustic velocity slower than the bulk wave acoustic velocity propagating through the piezoelectric film, the piezoelectric film laminated on the low acoustic velocity film, and an IDT electrode formed on one surface of the piezoelectric film.

[0005] Furthermore, Patent Document 2 includes a support substrate, a medium layer laminated on the support substrate, a piezoelectric body laminated on the medium layer through which a bulk wave propagates, and an IDT electrode formed on one surface of the piezoelectric body. The medium layer includes a low-velocity medium in which the propagation speed of the bulk wave, which is the main component of the elastic wave, is lower than the sound velocity of the elastic wave propagating through the piezoelectric body, and a high-velocity medium in which the propagation speed of the bulk wave, which is the main component of the elastic wave, is higher than the sound velocity of the elastic wave propagating through the piezoelectric body. When the sound velocity of the main vibration mode when the medium layer is formed of the high-velocity medium is VH and the sound velocity of the main vibration mode when the medium layer is formed of the low-velocity medium is VL, the medium layer is formed such that VL < the sound velocity of the main vibration mode < VH in the elastic wave device in which the medium layer is formed, and the thickness of the medium layer is 1λ or more when the period of the IDT is λ. An elastic wave device is disclosed, which is characterized by the above.

Prior Art Documents

Patent Documents

[0006]

Patent Document 1

Patent Document 2

Summary of the Invention

Problems to be Solved by the Invention

[0007] However, when a surface acoustic wave filter is manufactured using the composite substrate of Patent Document 1 or Patent Document 2, the energy of the acoustic wave leaks from the piezoelectric body to the low-velocity medium and remains there, causing a problem that noise called spurious or ripple occurs within the passband of the surface acoustic wave filter or at higher frequencies. This noise is generated by wave reflection at the bonding interface between the piezoelectric crystal film and the support substrate, or by acoustic waves being trapped in an intervening layer between the piezoelectric crystal film and the support substrate, and is undesirable because it deteriorates the frequency characteristics of the surface acoustic wave filter and causes an increase in loss in the passband of the filter.

[0008] The present invention has been made in view of the above circumstances, and has an object to provide a composite substrate for a surface acoustic wave device which has small loss in the filter passband, few spurious components, excellent performance, and high reliability. [Means for solving the problem]

[0009] As a result of intensive research, the inventors have found that a filter having a piezoelectric single crystal thin film, a support substrate, and at least one intermediate layer between the piezoelectric single crystal thin film and the support substrate, and by specifying the total thickness of the intermediate layer and the attenuation of longitudinal waves, can reduce loss in the passband of the filter and obtain high reliability, and have completed the present invention. The gist of the present invention is as follows. [1] A composite substrate comprising a piezoelectric single crystal thin film, a support substrate, and at least one intermediate layer provided between the piezoelectric single crystal thin film and the support substrate, the intermediate layer being in contact with the piezoelectric single crystal thin film, the total thickness of the intermediate layer being equal to or less than twice the wavelength of a surface acoustic wave, and the attenuation of a longitudinal wave of the intermediate layer calculated at a frequency of 40 GHz to 60 GHz by the Brillouin oscillation method being equal to or less than 8×10 -2 (nm -1 THz -2 ) or less. [2] The composite substrate for surface acoustic wave devices according to [1], wherein the sound velocity of the shear wave in the intermediate layer is faster than the sound velocity of the slow shear wave in the piezoelectric single crystal thin film. [3] The piezoelectric single-crystal thin film contains iron at 120 ppm or less, and the volume resistivity of the piezoelectric single-crystal thin film is 2×10 11 Ω·cm or less, which is the composite substrate for surface acoustic wave devices described in [1] or [2]. [4] The intermediate layer is either SiOx (1.8 < x < 2.05) or SiOyNz (0.02 < z / (y + z) < 0.1), which is the composite substrate for surface acoustic wave devices described in any one of [1] to [3]. [5] The main component of the piezoelectric single-crystal thin film is lithium tantalate or lithium niobate, which is the composite substrate for surface acoustic wave devices described in any one of [1] to [4]. [6] The support substrate is any one of a silicon substrate, a sapphire substrate, an alumina substrate, a silicon carbide substrate, an aluminum nitride substrate, a silicon nitride substrate, and a quartz substrate, which is the composite substrate for surface acoustic wave devices described in any one of [1] to [5]. [7] The support substrate consists of a Si single crystal and a polysilicon layer formed on the Si single crystal, which is the composite substrate for surface acoustic wave devices described in any one of [1] to [5]. [8] The content of Li ions in the intermediate layer is 1×10 17 atom / cm 3 or less, which is the composite substrate for surface acoustic wave devices described in any one of [1] to [7]. [Effect of the Invention]

[0010] According to the present invention, it is possible to provide a composite substrate for surface acoustic wave devices with a small loss in the filter passband and high reliability. [Brief Description of the Drawings]

[0011] [Figure 1] FIG. 1 is a diagram showing an example of the spectrum of Brillouin vibration of a SiO1.7 thin film. [Diagram 2] FIG. 2 is a diagram showing a waveform obtained by Fourier-transforming only the reflected light by ultrasonic waves (longitudinal waves) in the thin film. [Diagram 3]FIG. 3 is a diagram showing the dependency relationship between the LSAW sound velocity of a thin film and the value obtained by normalizing the thin film thickness to the wavelength of ultrasonic waves (thin film thickness / wavelength), and the calculation results of the sound velocity of elastic waves obtained by the finite element method. [Figure 4] FIG. 4 shows an example of the calculation result of the displacement distribution of elastic waves in which the energy is concentrated on the surface layer of a thin film having a SiO1.7 thin film / (111)Si substrate structure. [Diagram 5] FIG. 5 is a diagram showing an example of a cross-sectional TEM photograph of the composite substrate produced in Example 1. [Figure 6] FIG. 6 is a diagram showing a composite substrate having Al fine electrodes formed on the surface. [Figure 7] FIG. 7 is a diagram showing the resonant waveform (input impedance (Zin) and Q value) of the SAW obtained in Example 1. [Figure 8] FIG. 8 is a diagram showing the resonant waveform (input impedance (Zin) and Q value) of the SAW obtained in Example 2. [Figure 9] FIG. 9 is a diagram showing the resonant waveform (input impedance (Zin) and Q value) of the SAW obtained in Comparative Example 1. [Figure 10] FIG. 10 is a diagram showing the resonant waveform (input impedance (Zin) and Q value) of the SAW obtained in Comparative Example 2. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The composite substrate for surface acoustic wave devices of the present invention will be described in detail below, but the present invention is not limited to the embodiments. In addition, a numerical range defined by the symbol "~" includes both the upper and lower limits of the numerical range.

[0013] [Composite substrates for surface acoustic wave devices] The composite substrate for a surface acoustic wave device of the present invention is a composite substrate comprising a piezoelectric single crystal thin film, a support substrate, and at least one intermediate layer provided between the piezoelectric single crystal thin film and the support substrate, the intermediate layer being in contact with the piezoelectric single crystal thin film, the total thickness of the intermediate layer being equal to or less than twice the thickness of the wavelength of the surface acoustic wave, and the attenuation of the longitudinal wave of the intermediate layer calculated at a frequency of 40 GHz to 60 GHz by the Brillouin oscillation method is equal to or less than 8×10 -2 (nm -1 THz -2 ) or less.

[0014] (Piezoelectric single crystal thin film) The piezoelectric single crystal thin film in the surface acoustic wave device composite substrate according to an embodiment of the present invention is not particularly limited as long as it can be used as a piezoelectric film. 3 :LT), or lithium niobate (LiNbO 3 By using the above-mentioned components as the main components of the piezoelectric single crystal thin film, an acoustic wave device with large electromechanical coupling can be obtained. In the present invention, the main component of the piezoelectric single crystal thin film is lithium tantalate or lithium niobate means that 50 mass % or more of the components constituting the piezoelectric single crystal thin film is lithium tantalate or lithium niobate. In addition, the components of the piezoelectric single crystal thin film may contain iron, magnesium, etc., in addition to lithium tantalate and lithium niobate.

[0015] In addition, it is preferable that the piezoelectric single crystal thin film contains 120 ppm or less of iron. By containing a small amount of iron in the piezoelectric single crystal thin film, the electric field at which the polarization of the piezoelectric single crystal thin film is destroyed, i.e., the coercive electric field, increases, making it difficult for the polarization to be destroyed. From the above viewpoint, the iron content is more preferably 10 ppm or more and 120 ppm or less, and even more preferably 50 ppm or more and 100 ppm or less.

[0016] In addition, the initial volume resistivity of the piezoelectric single crystal thin film is 2×10 11It is preferable that the initial volume resistivity of the piezoelectric single crystal thin film is 2×10 11 By setting the resistivity to Ω·cm or less, the constant temperature resistance of the composite substrate for surface acoustic wave devices of the present invention can be improved. The initial volume resistivity of the piezoelectric single crystal thin film is 2×10 10 Ω cm or more 2×10 11 It is more preferable that the resistance is less than 2×10 10 Ω cm or more 1×10 11 It is more preferable that the resistivity is Ω·cm or less.

[0017] (Support substrate) The support substrate in the surface acoustic wave device composite substrate according to one embodiment of the present invention can be any of a silicon substrate, a sapphire substrate, an alumina substrate, a silicon carbide substrate, an aluminum nitride substrate, a silicon nitride substrate, and a quartz substrate. A surface acoustic wave resonator manufactured using a composite substrate for surface acoustic wave devices using the above-mentioned substrate as a supporting substrate has a high Q value, and out-of-band spurious emissions are further suppressed, resulting in a surface acoustic wave device with excellent temperature characteristics.

[0018] The support substrate may be made of a single crystal Si and a polysilicon layer formed on the single crystal Si. By appropriately adjusting the thickness of the polysilicon layer as the support substrate, out-of-band spurious emissions can be further suppressed. The thickness of the polysilicon layer is preferably 0.2 μm or more and 2 μm or less, more preferably 0.5 μm or more and 1.9 μm or less, and further preferably 0.5 μm or more and 1.2 μm or less.

[0019] (intervening layer) The composite substrate for a surface acoustic wave device of the present invention includes an intervening layer between the piezoelectric single crystal thin film and the support substrate, and the intervening layer is provided in contact with the piezoelectric single crystal thin film. In the composite substrate for a surface acoustic wave device according to an embodiment of the present invention, the intervening layer is preferably either SiOx (1.8 < x < 2.05) or SiOyNz (0.02 < z / (y + z) < 0.1). Further, the composite substrate for a surface acoustic wave device of the present invention includes at least one intervening layer. The intervening layer may be a single layer, or may be two or more layers. In the case of two or more layers, each layer may be composed of the same material or different materials.

[0020] Also, the content of Li ions in the intervening layer is preferably 1×10 17 atom / cm 3 or less. Li ions mainly diffuse from the piezoelectric single crystal thin film into the intervening layer. By setting the content of Li ions in the intervening layer to 1×10 17 atom / cm 3 or less, softening of the intervening layer can be prevented, and spurious signals inside and outside the band can be suppressed.

[0021] Furthermore, when the intervening layer is a single layer, the thickness of the intervening layer, and when there are two or more layers, the total thickness thereof, is equal to or less than twice the thickness of the surface acoustic wave wavelength of the intervening layer. When the thickness of the intervening layer exceeds twice the thickness of the surface acoustic wave wavelength of the intervening layer, elastic waves are likely to be trapped in the intervening layer, resulting in a problem of increased spurious signals outside the band. The total thickness of the intervening layer is preferably equal to or less than twice the thickness of the surface acoustic wave wavelength, and more preferably equal to or less than once the thickness.

[0022] Also, the longitudinal wave attenuation of the intervening layer calculated by the Brillouin vibration method at a frequency of 40 GHz to 60 GHz is 8×10 -2 (nm -1 ·THz -2 ) or less. When the acoustic attenuation of the longitudinal wave in the intermediate layer is large, the acoustic wave is easily trapped in the intermediate layer. In this case, the surface acoustic wave resonator made of the composite substrate for a surface acoustic wave device of the present invention has a problem of large spurious out-of-band. -2 (nm -1 THz -2 ) or less, the Q value of the surface acoustic wave resonator is high, and out-of-band spurious can be further suppressed. The attenuation of the longitudinal wave in the intermediate layer is 2×10 -2 (nm -1 THz -2 ) or less, and preferably 0.5×10 -2 (nm -1 THz -2 ) or less is more preferable.

[0023] In addition, the sound velocity of the shear waves in the intervening layer is preferably faster than the sound velocity of the slow shear waves in the piezoelectric single crystal thin film. By making the shear wave (bulk wave) velocity in the intervening layer faster than the slow shear wave (bulk wave) in the piezoelectric single crystal thin film, the loss in the passband of the surface acoustic wave filter obtained using the composite substrate for surface acoustic wave devices can be improved. If the shear wave velocity in the intervening layer is slower than the slow shear wave in the piezoelectric single crystal thin film, there is a concern that the acoustic wave will be easily trapped in the intervening layer. Note that, since the piezoelectric single crystal thin film is an anisotropic material, there are two types of shear waves in the piezoelectric single crystal thin film: fast shear waves and slow shear waves.

[0024] For example, LiTaO 3 In the case of 46° rotated Y-cut LiTaO 3 The slow shear wave is 3330 m / s. 1.85 , or SiO 1.94 N 0.06 In the case of SiO 1.85 , or SiO 1.94 N 0.06 The sound velocities of the shear waves in SiO are 3850 m / s and 3750 m / s, respectively. 1.85 , or SiO 1.94 N 0.06The sound velocity of the shear wave in SiO is described in detail later. For example, see Tatsuya Omori1, Kensuke Sakamoto, Satoshi Suzuki, Jun-ichi Kushibiki, Satoru Matsuda, and Ken-ya Hashimoto, “Characterization of Elastic Properties of SiO 2 This can be obtained from the shear wave sound velocity measurement value of the LSAW of the piezoelectric single crystal thin film by a linear convergent beam ultrasonic microscope described in “Thin Films by Ultrasonic Microscopy” and analysis by the finite element method. The intermediate layer is SiO 1.85 , or SiO 1.94 N 0.06 The piezoelectric single crystal thin film was LiTaO 3 This allows the sound velocity of the transverse waves in the intervening layer to be faster than the sound velocity of the slow transverse waves in the piezoelectric single crystal thin film.

[0025] In addition, the attenuation of the longitudinal wave in the intermediate layer calculated at frequencies from 40 GHz to 60 GHz by the Brillouin oscillation method was found to be 0.01%. 1.85 The attenuation is 1.2×10 -2 (nm -1 THz -2 ), SiO 1.94 N 0.06 The attenuation is 0.1×10 -2 (nm -1 THz -2 ) and the attenuation of the longitudinal wave is 8×10 -2 (nm -1 THz -2 ) can be as follows:

[0026] Here, as the Brillouin oscillation method, the method described in H. Ogi et.al., “Elastic constant and Brillouin oscillations in sputtered vitreous SiO2 thin films”, PHISICAL REVIEW B 78, 13204 (2008) can be used. 1.7In this case, the SiO 1.7 1 shows an example of the spectrum of Brillouin oscillations of a thin film.

[0027] The SiO used in the measurement of Figure 1 1.7 The thin film (hereinafter simply referred to as "thin film") is made of SiO.sub.2 having the same composition and the same manufacturing method as the intermediate layer. 1.7 A thin film is formed on a Si substrate to a thickness of 1055 nm (the thickness is defined as d), and then a SiO 1.7 An Al film was formed on the thin film to a thickness of 10 nm. The method for producing the thin film is not particularly limited, but may be, for example, a CVD method. 1.7 Ultra-high frequency ultrasonic waves are generated by irradiating a structure consisting of a thin film and a Si substrate with an extremely short pulse of light. In addition, a delayed pulse of light with a reference wavelength (λ) of 400 nm is irradiated. The longitudinal wave sound velocity of the thin film can be obtained by detecting the light diffracted by the ultrasonic waves within the thin film.

[0028] At this time, the density of the thin film and the refractive index at 400 nm are obtained in advance. The refractive index (n) of the thin film at 400 nm is 1.728 by the prism coupler method. The density (ρ) of the thin film was determined by XPS (X-ray photoelectron spectroscopy) to be 2300 kg / m 3 The first half of the Brillouin spectrum shown in Figure 1 shows the reflected light intensity due to diffraction by ultrasonic waves (longitudinal waves) inside the thin film. By performing a Fourier transform on only the reflected light due to the ultrasonic waves (longitudinal waves) inside the thin film, the frequency of the ultrasonic waves (longitudinal waves) inside the thin film shown in Figure 2 can be obtained. From Figure 2, the frequency (f) of the ultrasonic waves (longitudinal waves) inside the thin film can be calculated to be 54.5 GHz.

[0029] At this time, the sound velocity vl of the ultrasonic wave (longitudinal wave) in the thin film can be calculated by the following formula (1). vl=f×λ / (2×n)...Equation (1) The sound velocity of the ultrasonic waves (longitudinal waves) in the thin film shown in Figure 2, calculated using formula (1), was 6325 m / s. The elastic constant C11 of the thin film was calculated using vl = √(C11 / ρ), and was found to be 92 GPa.

[0030] Next, SiO 1.7 A method for determining the sound velocity of a shear wave in a film using a linear convergent beam acoustic microscope and the finite element method is described. First, for example, the above-mentioned Tatsuya Omori1, Kensuke Sakamoto, Satoshi Suzuki, Jun-ichi Kushibiki, Satoru Matsuda, and Ken-ya Hashimoto, “Characterization of Elastic Properties of SiO 2 Using a linear convergent beam ultrasonic microscope described in “Thin Films by Ultrasonic Microscopy”, the LSAW sound velocity of the thin film was measured by changing the frequency from 160 MHz to 275 MHz, and the dependency of the value obtained by normalizing the thin film thickness to the ultrasonic wavelength (thin film thickness / wavelength) was obtained. The relationship diagram is shown in Figure 3.

[0031] The LSAW sound velocity (vertical axis) measured by a linear convergent beam ultrasonic microscope in Fig. 3 is the SiO 1.7 A thin film was formed on a Si(111)-oriented substrate with a thickness of 2830 nm. The SiO 1.7 This was achieved by propagating LSAW on the surface of the thin film / Si substrate structure.

[0032] On the other hand, a two-dimensional finite element method was used to calculate the SiO 1.7 A ZnO film and an Al electrode, which are sufficiently thin compared to the electrode period, are placed on the surface of the thin film of the thin film / (111)Si substrate structure. <110> The elastic wave is excited in a direction shifted 45 degrees clockwise from the direction of the electrode, and the wavelength determined by the electrode period is changed in the model of the finite element method calculation. 1.7 The relationship between the acoustic velocity of the thin film / (111)Si substrate and the intermediate layer normalized by the wavelength was calculated. 1.7Since the elastic constant C12 of the thin film is an unknown quantity, a tentative value was input for C12, and C12 was determined so as to match the measurement results of the LSAW sound velocity using a linear convergent beam acoustic microscope in Figure 3. The other constants (C11, ρ) were calculated using the values ​​mentioned above.

[0033] The C12 calculated above was 20 GPa. 1.7 Figure 3 shows the results of elastic wave sound velocity calculations using the finite element method when the elastic constant C12 of the thin film is 20 GPa. As an example, in a calculation model using the finite element method when the elastic wave wavelength is 18 μm, the elastic wave is 1.7 Figure 4 shows an example of the calculated displacement distribution of waves with energy concentrated on the surface layer of a thin film with a thin film / (111)Si substrate structure.

[0034] From the above considerations, SiO 1.7 The shear wave acoustic velocity Vs (=√((C11-C12) / ρ)) of the thin film alone was calculated to be Vs = 3960 m / s. In the calculation model using the finite element method of the present application described above, the elastic constants of the Si substrate, ZnO film, and Al film were taken from the values ​​given in the Surface Acoustic Wave Data Book (edited by the Japan Electronics Industry Association), (p.66 (ZnO), p.165 (Si), p.172 (Al)).

[0035] In addition, in the study of this application, as an original attempt of this application, attention was focused on the fact that the reflected light intensity due to diffraction by ultrasonic waves (longitudinal waves) in the thin film layer, which is the first half of the Brillouin spectrum shown in Figure 1, attenuates exponentially with time. That is, in the envelope of the reflected light intensity shown by the dotted line in Figure 1, if the amplitude intensity at time 0 psec is A0 and the amplitude intensity at the time when the ultrasonic waves reach Si is A, the attenuation constant (β) of the ultrasonic waves (longitudinal waves) in the thin film is described by formula (2). A=A0·exp(-β·f 2 ·d) ·········································Formula (2) In the case of Figure 2, A0 was 0.03 and A was 0.004. From the above, the damping constant β is calculated from equation (3). β=-1 / (f 2 d) In(A / A0) Equation (3) In the case of Figure 2, β is 10.8×10 -2 (nm -1 THz -2 ) was.

[0036] For the various intermediate layers described above, the attenuation of longitudinal waves was calculated at frequencies of 40 GHz to 60 GHz by the Brillouin oscillation method using the same method as above. When the acoustic attenuation of the longitudinal waves in the intermediate layer is large, the acoustic waves tend to be trapped in the intermediate layer. In this case, it was confirmed that the surface acoustic wave resonator made of the composite substrate for surface acoustic wave devices has a problem of large out-of-band spurious. On the other hand, if the intermediate layer according to the present invention has a high acoustic velocity and little attenuation of longitudinal waves, the acoustic waves cannot be concentrated excessively on the intermediate layer, and the wave energy can be concentrated on the piezoelectric single crystal thin film. Therefore, the Q value of the surface acoustic wave resonator using the composite substrate for surface acoustic wave devices according to the present invention is high, and out-of-band spurious is further suppressed, which is preferable. EXAMPLES

[0037] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.

[0038] Example 1 A polysilicon layer of 1.7 μm was formed on the surface of a high-resistivity silicon substrate having a diameter of 150 mm and a (111) orientation.

[0039] Next, a melt having a composition in which the amount of lithium was reduced based on the amount of lithium contained in the lithium tantalate crystal of the congruent composition was prepared, and an iron-substituted lithium tantalate crystal was grown from the melt having the adjusted composition. The amount of added iron was adjusted so that the iron content in the iron-substituted lithium tantalate crystal was 95 mass ppm, and a 6-inch iron-containing 42° Y-cut lithium tantalate (LT) substrate was prepared. The iron-containing 42° Y-cut lithium tantalate (LT) substrate was subjected to a reduction treatment to reduce the volume resistivity to 2.2×10 10 The resistance was adjusted to Ω·cm.

[0040] Next, hydrogen molecular ions were implanted into the surface of a 6-inch iron-containing lithium tantalate (LT) substrate to be bonded. The dose was 9×10 16 atm / cm 2 The accelerating voltage was 160 KeV. Next, a 0.4 μm thick layer of SiO was applied to the 6-inch iron-containing lithium tantalate (LT) substrate ion-implanted with hydrogen molecular ions. 1.85 The intermediate layer was formed by CVD. Next, the silicon substrate on which the polysilicon layer was formed was immersed in a 0.4 μm thick SiO 1.85 The iron-containing LT substrate with the intervening layer was subjected to surface activation treatment by plasma treatment. 1.85 The iron-containing LT substrate was bonded to the substrate with an intermediate layer of the material interposed therebetween to form a joint.

[0041] Next, the bonded body was heat-treated at 350°C under nitrogen to prevent the introduction of crystal defects due to misalignment of the bonding interface. The heat-treated bonded body was then heated to 110°C, and a wedge was driven into one end of the ion-implanted part of the iron-containing lithium tantalate (LT) substrate to separate it into the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the silicon substrate and the remaining iron-containing lithium tantalate (LT) substrate. The thickness of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the silicon substrate after separation was measured using a spectrophotometer and found to be 0.52 μm. Next, the composite substrate consisting of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the silicon substrate was heated at 500°C for 6 hours.

[0042] Furthermore, the surface layer of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film of the composite substrate was polished by 20 nm, and the thickness of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the silicon substrate was measured using a spectrophotometer, finding it to be 0.5 μm. FIG. 5 shows an example of a cross-sectional TEM observation photograph of the composite substrate of Example 1 produced by the above method, and FIG. 5(b) is a further enlarged photograph of a part of FIG. 5(a).

[0043] The intermediate layer (SiO 1.85 The amount of Li in the SiO 1.85 The amount of Li in the layer is up to 2×10 16 atom / cm 3 In addition, the intermediate layer (SiO 1.85 The composition ratio of each layer was determined by X-ray photoelectron spectroscopy (XPS).

[0044] Furthermore, the intermediate layer (SiO 1.85 The density of the layer was determined by XPS (X-ray photoelectron spectroscopy) and found to be 2240 g / cm 3 In addition, the intervening layer (SiO 1.85 The longitudinal wave velocity and attenuation of the intermediate layer (SiO 1.85 The longitudinal wave velocity in the layer is 6200 m / s, and the acoustic attenuation rate is 1.2 × 10 at 55 GHz. -3 (nm -1 THz -2 ) was. In addition, the intermediate layer (SiO 1.85 The shear wave velocity of the intervening layer (SiO 1.85 The shear wave velocity of the single layer was 3,850 m / s.

[0045] Next, an Al film was sputtered to a thickness of 0.14 μm on the surface of the composite substrate obtained above, and after applying a resist, a resist pattern with a line width of about 0.5 μm was formed by i-line exposure. Next, the Al was etched by dry etching to form the first layer of a one-port SAW resonator. At this time, the wavelength of the surface acoustic wave was 2 μm, and the intermediate layer (SiO 1.85 The thickness of the layer is 0.2 wavelengths. Furthermore, a second layer of pads with an Al film thickness of 0.6 μm was formed on the above composite substrate by the lift-off method. Figure 6 shows the composite substrate with the Al microelectrodes formed on its surface.

[0046] Next, the electrical characteristics of the one-port SAW resonator on the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate prepared above were measured using a network analyzer. The obtained SAW resonance waveform (input impedance (Zin) and Q value) is shown in Figure 7. In addition, the resonant frequency (fr), anti-resonant frequency (fa), and electromechanical coupling coefficient (k 2 ), maximum Q value (Qmax), input impedance amplitude (ΔZ), fractional bandwidth value (fractional bandwidth = (antiresonant frequency - resonant frequency) / resonant frequency), and spurious intensity between 2400 and 2800 MHz are shown in Table 1.

[0047] [Table 1]

[0048] Next, the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate with the one-port SAW resonator pattern created above was placed on a hot plate heated to 350°C for 10 minutes, then placed on a cooling plate at room temperature to cool, and the electrical characteristics of the one-port SAW resonator were measured again with a network analyzer. The resulting characteristics were the same as those in Table 1. Furthermore, this process of hot plate heating at 350°C, cooling, and measurement was repeated for a total of four hours with a cumulative heating time of 350°C, and the electrical characteristics of the one-port SAW resonator after each cumulative heating time were not different from those in Table 1.

[0049] Example 2 In Example 1, the thickness is 0.4 μm and the composition is SiO 1.85 Instead of an intermediate layer of 0.3 μm thickness and composition SiO 1.94 N 0.06A composite substrate was prepared by bonding an iron-containing lithium tantalate (LT) piezoelectric single crystal thin film to a silicon substrate in the same manner as in Example 1, except that an intermediate layer of

[0050] The intervening layer (SiO 1.94 N 0.06 The amount of Li in the SiO 1.94 N 0.06 The amount of Li in the layer is 1×10 14 atom / cm 3 In addition, the intermediate layer (SiO 1.94 N 0.06 The composition ratio of each layer was determined by X-ray photoelectron spectroscopy (XPS).

[0051] In addition, the LT layer of a composite substrate consisting of an iron-containing lithium tantalate (LT) piezoelectric single crystal thin film bonded to a silicon substrate was removed, and the intermediate layer (SiO 1.94 N 0.06 The density of the intermediate layer (SiO 1.94 N 0.06 The density of the layer is 2210g / cm 3 In addition, the LT layer of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate was removed, and the intermediate layer (SiO 1.94 N 0.06 The longitudinal wave velocity and attenuation of the intermediate layer (SiO 1.94 N 0.06 The longitudinal wave velocity in the layer is 6190 m / s, and the acoustic attenuation rate is 1.2 × 10 at 55 GHz. -3 (nm -1 THz -2 ) was. In addition, the intermediate layer, SiO 1.94 N 0.06 The shear wave velocity of the layer alone was calculated by combining the linear convergent beam acoustic microscope and finite element method analysis described above. 1.94 N0.06 The shear wave velocity of the layer alone was 3750 m / s.

[0052] Next, the electrical characteristics of the one-port SAW resonator on the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate prepared above were measured using a network analyzer. The obtained SAW resonance waveform (input impedance (Zin) and Q value) is shown in Figure 8. At this time, the wavelength of the surface acoustic wave was 2 μm, and the intermediate layer (SiO 1.94 N 0.06 The thickness of the layer is 0.15 wavelengths. In addition, the resonant frequency (fr), anti-resonant frequency (fa), and electromechanical coupling coefficient (k 2 ), maximum Q value (Qmax), input impedance amplitude (ΔZ), fractional bandwidth, and spurious intensity between 2400 and 2800 MHz are shown in Table 1.

[0053] [Table 2]

[0054] Next, an iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to a silicon substrate with a one-port SAW resonator pattern made in the same manner as in Example 1 was placed on a hot plate heated to 350°C for 10 minutes, then placed on a cooling plate at room temperature to cool, and the electrical characteristics of the one-port SAW resonator were measured again with a network analyzer. The resulting characteristics were the same as those in Table 2. Furthermore, this hot plate heating at 350°C, cooling, and measurement were repeated for a total of four hours of cumulative heating at 350°C, and the electrical characteristics of the one-port SAW resonator after each cumulative heating time were not different from those in Table 2.

[0055] Comparative Example 1 A polysilicon layer of 1.7 μm was formed on the surface of a high-resistivity silicon substrate having a diameter of 150 mm and a (111) orientation.

[0056] Next, the amount of lithium in the melt was adjusted to a composition in which it was reduced based on the amount of lithium contained in the lithium tantalate crystal of the congruent composition, and an iron-substituted lithium tantalate crystal was grown from the melt of the adjusted composition. A 6-inch iron-containing 42° Y-cut lithium tantalate (LT) substrate was prepared by adding iron so that the iron content in the iron-substituted lithium tantalate crystal was 95 mass ppm. The iron-containing 42° Y-cut lithium tantalate (LT) substrate was subjected to a reduction treatment to reduce the volume resistivity to 2.2×10 10 The resistance was adjusted to Ω·cm.

[0057] Next, hydrogen molecular ions were implanted into the surface of a 6-inch iron-containing lithium tantalate (LT) substrate to be bonded. The dose was 9×10 16 atm / cm 2 The accelerating voltage was 160 KeV. Next, a 0.4 μm thick layer of SiO was applied to the 6-inch iron-containing lithium tantalate (LT) substrate ion-implanted with hydrogen molecular ions. 1.7 The intermediate layer was formed by CVD. Next, the silicon substrate on which the polysilicon layer was formed was immersed in a 0.4 μm thick SiO 1.7 The iron-containing LT substrate with the interposed layer was subjected to surface activation treatment by plasma treatment. Furthermore, the silicon substrate with the polysilicon layer and the SiO 1.7 The iron-containing LT substrate was bonded to the substrate with an intermediate layer of the material interposed therebetween to form a joint.

[0058] Next, the bonded body was heat-treated at 350°C under nitrogen to prevent the introduction of crystal defects due to misalignment of the bonding interface. The heat-treated bonded body was then heated to 110°C, and a wedge was driven into one end of the ion-implanted part of the iron-containing lithium tantalate (LT) substrate to separate it into the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the support substrate and the remaining iron-containing lithium tantalate (LT) substrate. The thickness of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the silicon substrate after separation was measured using a spectrophotometer and found to be 0.52 μm. Next, the composite substrate consisting of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film bonded to the silicon substrate was heated at 500°C for 6 hours.

[0059] Furthermore, the surface layer of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film of the composite substrate was polished by 20 nm, and the thickness of the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the silicon substrate was measured using a spectrophotometer, finding it to be 0.5 μm.

[0060] The intermediate layer (SiO 1.7 The amount of Li in the SiO 1.7 The amount of Li in the layer is up to 2×10 17 atom / cm 3 The intermediate layer (SiO 1.7 The composition ratio of each layer was determined by X-ray photoelectron spectroscopy (XPS).

[0061] In addition, the intermediate layer (SiO 1.7 The density of the layer was determined by XPS (X-ray photoelectron spectroscopy) and found to be 2240 g / cm 3 In addition, the intervening layer (SiO 1.7 The longitudinal wave velocity and attenuation of the intermediate layer (SiO 1.7 The longitudinal wave velocity in the layer is 6325 m / s, and the acoustic attenuation rate is 10.8 × 10 at 55 GHz. -2 (nm -1 THz -2 ) was. In addition, the intermediate layer (SiO 1.7 The shear wave velocity of the intervening layer (SiO 1.7 The shear wave velocity of the single layer was 3,960 m / s.

[0062] Next, an Al film was sputtered to a thickness of 0.14 μm on the surface of the composite substrate obtained above, and a resist was applied, and then a resist pattern with a line width of about 0.5 μm was formed by i-line exposure. Then, the Al was etched by dry etching to form the first layer of a one-port SAW resonator. Furthermore, a second layer pad part of an Al film with a thickness of 0.6 μm was formed on the above composite substrate by a lift-off method. At this time, the wavelength of the surface acoustic wave was 2 μm, and the intermediate layer (SiO 1.7 The thickness of the layer is 0.2 wavelengths.

[0063] Next, the electrical characteristics of the one-port SAW resonator on the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate prepared above were measured using a network analyzer. The obtained SAW resonance waveform (input impedance (Zin) and Q value) is shown in Figure 9. In addition, the resonant frequency (fr), anti-resonant frequency (fa), and electromechanical coupling coefficient (k 2 ), maximum Q value (Qmax), input impedance amplitude (ΔZ), fractional bandwidth, and spurious intensity between 2400 and 2800 MHz are shown in Table 3.

[0064] [Table 3]

[0065] Next, the iron-containing lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate with the one-port SAW resonator pattern created above was placed on a hot plate heated to 350°C for 10 minutes, then placed on a cooling plate at room temperature to cool, and the electrical characteristics of the one-port SAW resonator were measured again with a network analyzer. The resulting characteristics were the same as those in Table 3. Furthermore, this 350°C hot plate heating, cooling, and measurement were repeated for a total of 4 hours of cumulative heating at 350°C, and the electrical characteristics of the one-port SAW resonator after each cumulative heating time were not different from those in Table 3.

[0066] Comparative Example 2 A polysilicon layer of 1.7 μm was formed on the surface of a high-resistance silicon substrate with a diameter of 150 mm.

[0067] Next, an iron-free lithium tantalate crystal was grown on the lithium tantalate crystal of the congruent composition. A 6-inch iron-free lithium tantalate (LT) substrate with a 42° Y-cut was prepared by processing a non-iron-containing lithium tantalate crystal. The volume resistivity of the non-iron-containing 42° Y-cut lithium tantalate (LT) substrate was reduced to 2.2× 10 The resistance was adjusted to Ω·cm.

[0068] Next, hydrogen molecular ions were implanted into the surface to be bonded of a 6-inch iron-free lithium tantalate (LT) substrate. The dose was 9×10 16 atm / cm 2 The accelerating voltage was 160 KeV.

[0069] Next, a 0.4μm thick layer of SiO was applied to the ion-implanted surface of a 6-inch iron-free lithium tantalate (LT) substrate. 2 The intermediate layer was formed by CVD. Next, the silicon substrate on which the polysilicon layer was formed was immersed in a 0.4 μm thick SiO 2 The iron-free LT substrate with the intervening layer was subjected to surface activation treatment by plasma treatment. 2 The iron-free LT substrate was bonded to the substrate with an intermediate layer of the material interposed therebetween to form a joint.

[0070] Next, the surface of the bonded body (bonded substrate) was removed by grinding and polishing. The thickness of the iron-free lithium tantalate (LT) piezoelectric single crystal thin film layer bonded to the silicon substrate after thinning was measured by a spectrophotometer and found to be 0.5 μm.

[0071] The intermediate layer (SiO 2The amount of Li in the SiO 2 The amount of Li in the layer is up to 5×10 19 atom / cm 3 The intermediate layer (SiO 2 The composition ratio of each layer was determined by X-ray photoelectron spectroscopy (XPS).

[0072] In addition, the LT layer of the composite substrate manufactured by the above method was removed, and the intermediate layer (SiO 2 The density of the intermediate layer (SiO 2 The density of the layer is 2100g / cm 3 In addition, the LT layer of the composite substrate was removed, and the intermediate layer (SiO 2 The longitudinal wave velocity and attenuation of the intermediate layer (SiO 2 The longitudinal wave velocity in the layer is 5400 m / s, and the acoustic attenuation rate is 5×10 at 55 GHz. -1 (nm -1 THz -2 ) was. In addition, the intermediate layer, SiO 2 The shear wave velocity of the layer alone was determined by combining the above-mentioned linear convergent beam ultrasonic microscope and finite element method analysis. 2 The shear wave velocity of the layer alone was 3150 m / s.

[0073] Next, the electrical characteristics of the one-port SAW resonator on the iron-free lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate created above were measured using a network analyzer. The obtained SAW resonance waveform (input impedance (Zin) and Q value) is shown in Figure 10. In addition, the resonant frequency (fr), anti-resonant frequency (fa), and electromechanical coupling coefficient (k 2 ), maximum Q value (Qmax), input impedance amplitude (ΔZ), specific bandwidth, and spurious intensity between 2400 and 2800 MHz are shown in Table 4. At this time, the wavelength of the surface acoustic wave is 2 μm, and the intermediate layer (SiO2 The thickness of the layer is 0.2 wavelengths.

[0074] [Table 4]

[0075] Next, the iron-free lithium tantalate (LT) piezoelectric single crystal thin film substrate bonded to the silicon substrate with the one-port SAW resonator pattern created above was placed on a hot plate heated to 350°C for 10 minutes, then placed on a cooling plate at room temperature to cool, and the electrical characteristics of the one-port SAW resonator were measured again with a network analyzer. The resulting characteristics were the same as those in Table 4. Furthermore, this process of hot plate heating at 350°C, cooling, and measurement was repeated for a total of four hours with a cumulative heating time of 350°C, and the electromechanical coupling coefficient (k 2 ) starts to decrease from the value in Table 3, and after a cumulative heating time of 4 hours, the electromechanical coupling coefficient (k 2 ) had decreased to 5%.

Claims

1. A composite substrate comprising a piezoelectric single crystal thin film, a support substrate, and at least one intermediate layer provided between the piezoelectric single crystal thin film and the support substrate, The intermediate layer is in contact with the piezoelectric single crystal thin film, the total thickness of the intermediate layer is equal to or less than twice the wavelength of the surface acoustic wave, and the attenuation of the longitudinal wave of the intermediate layer calculated at a frequency of 40 GHz to 60 GHz by the Brillouin oscillation method is equal to or less than 8×10 -2 (nm -1 ・THz -2 ) or less.

2. 2. The composite substrate for surface acoustic wave devices according to claim 1, wherein the sound velocity of the shear wave of said intermediate layer is faster than the sound velocity of the slow shear wave of said piezoelectric single crystal thin film.

3. The piezoelectric single crystal thin film contains iron at 120 ppm or less, The volume resistivity of the piezoelectric single crystal thin film is 2×10 11 3. The composite substrate for a surface acoustic wave device according to claim 1, wherein the resistivity is Ω·cm or less.

4. 3. The composite substrate for a surface acoustic wave device according to claim 1, wherein the intermediate layer is any one of SiOx (1.8<x<2.05) and SiOyNz (0.02<z / (y+z)<0.1).

5. 3. The composite substrate for surface acoustic wave devices according to claim 1, wherein the main component of said piezoelectric single crystal thin film is lithium tantalate or lithium niobate.

6. 3. The composite substrate for a surface acoustic wave device according to claim 1, wherein the support substrate is any one of a silicon substrate, a sapphire substrate, an alumina substrate, a silicon carbide substrate, an aluminum nitride substrate, a silicon nitride substrate, and a quartz substrate.

7. 3. The composite substrate for a surface acoustic wave device according to claim 1, wherein the supporting substrate is made of a silicon single crystal and a polysilicon layer formed on the silicon single crystal.

8. The content of Li ions in the intermediate layer is 1×10 17 atom / cm 3 3. The composite substrate for a surface acoustic wave device according to claim 1, wherein:

Citation Information

Patent Citations

  • Composite substrate for surface acoustic wave device, manufacturing method and surface acoustic wave device

    CN113872557A

  • Composite substrate for surface acoustic wave device and manufacturing method thereof

    JP2021005785A

  • Composite substrate for surface acoustic wave device and method for manufacturing the same

    JP2021180465A

  • Apparatus for supplying matter to be incinerated to incinerator

    JP1982013025A

  • Control system of electronically controlled washer

    JP1983061789A

Cited By

  • Oxide single crystal composite substrate and method for manufacturing same

    WO2026126658A1