Election ballot sheet and method for producing the same
A ballot paper with a coating layer of acrylic polymer, clay, and polyethylene particles stabilizes paper passability, addressing variations in conventional papers, ensuring consistent feeding and accurate counting.
Patent Information
- Application Number
- JP2023078112
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional election ballot papers experience variations in paper passability during mass production, particularly in their ability to be fed by counting machines, despite having the same composition.
An election ballot paper with a coating layer containing specific proportions of acrylic polymer, clay, heavy calcium carbonate, and polyethylene particles, along with controlled friction coefficients and surface roughness, is developed to stabilize paper passability.
The solution effectively suppresses variations in paper passability, ensuring consistent feeding and accurate counting by counting machines, while maintaining excellent flexibility and recyclability.
Smart Images

Figure 2024162530000001 
Figure 2024162530000002 
Figure 2024162530000003
Abstract
Description
[Technical field]
[0001] The present invention relates to election ballots and methods for producing same. [Background technology]
[0002] Due to their purpose, election ballots are required to have various characteristics, such as ease of counting by machine. In order to meet such demands, papers having various characteristics have been proposed. For example, Patent Document 1 proposes an election ballot paper that is recyclable and has excellent paper feedability. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 7049733 Summary of the Invention [Problem to be solved by the invention]
[0004] On the other hand, the present inventors have found that when conventional election ballots are mass-produced, their characteristics may vary even if they have the same composition. The present inventors have found that, among these characteristics, the paper feedability in particular may be prone to variation.
[0005] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide election ballot papers in which variation in paper feedability is suppressed. [Means for solving the problem]
[0006] The present inventors have found that the above problems can be solved by using an election ballot paper having a coating layer containing a specific polyethylene particle, etc., and have completed the present invention. Specifically, the present invention provides the following.
[0007] (1) An election ballot paper comprising a substrate and a coating layer provided on one or both sides of the substrate, the coating layer comprises a continuous phase made of an acrylic polymer, clay, ground calcium carbonate, and polyethylene particles; The content of the clay is 25% by mass or more and 55% by mass or less with respect to the coating layer, The content of the ground calcium carbonate is 5% by mass or more and 30% by mass or less with respect to the coating layer, The volume average particle size of the ground calcium carbonate is 0.05 μm or more and 2.00 μm or less, The particle size of the polyethylene particles in accordance with JIS Z8832:2010 is 8.0 μm or more and 11.0 μm or less, The density of the polyethylene particles according to JIS K6922-2 is 950 kg / m 3 More than 1000kg / m 3 is as follows: The static friction coefficient of the coating layer in accordance with JIS P8147:2010 is 0.30 or more and 0.50 or less, The coating layer has a dynamic friction coefficient in accordance with JIS P8147:2010 of 0.20 or more and 0.35 or less, The arithmetic mean height of the coating layer in accordance with JIS B0601:2001 is 0.50 μm or more and 0.90 μm or less, The total content of the dye contained in the substrate and the coating layer is 0.1% by mass or less with respect to the substrate and the coating layer. Election ballot paper.
[0008] (2) An election ballot paper as described in (1), in which at least a portion of the surface of the coating layer is provided with a halftone dot printed area using offset ink.
[0009] (3) An election ballot as described in (2), wherein the dot percentage of the dot printed portion is between 10% and 50%.
[0010] (4) An election ballot paper as described in (1) or (2), wherein the base material contains a thermoplastic resin and an inorganic substance powder in a mass ratio of 50:50 to 10:90.
[0011] (5) The election ballot paper described in (4), wherein the thermoplastic resin is a polypropylene-based resin.
[0012] (6) The election ballot paper described in (1), wherein the ground calcium carbonate is a surface-treated ground calcium carbonate.
[0013] (7) The election ballot paper described in (4), wherein the volume average particle diameter of the clay is 0.05 μm or more and 2.00 μm or less.
[0014] (8) The election ballot paper described in (4), wherein the acrylic polymer is a (meth)acrylic acid alkyl ester copolymer.
[0015] (9) The election ballot paper according to (8), wherein the (meth)acrylic acid alkyl ester copolymer is one or more selected from the group consisting of methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, isooctyl acrylate, nonyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, 2-hydroxymethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, and 2-hydroxypropyl methacrylate.
[0016] (10) An election ballot paper as described in (1) or (2) having an opacity of 95% or more in accordance with JIS P 8149:2000.
[0017] (11) A step of obtaining a substrate by extrusion molding a resin composition containing a polyolefin resin and an inorganic substance powder in a mass ratio of 50:50 to 10:90; A step of applying an aqueous emulsion containing an acrylic polymer, clay, ground calcium carbonate, and polyethylene particles to one or both sides of the substrate and drying the emulsion to provide a coating layer; The content of the clay is 25% by mass or more and 55% by mass or less with respect to the coating layer, The content of the ground calcium carbonate is 5% by mass or more and 30% by mass or less with respect to the coating layer, The volume average particle size of the ground calcium carbonate is 0.05 μm or more and 2.00 μm or less, The particle size of the polyethylene particles in accordance with JIS Z8832:2010 is 8.0 μm or more and 11.0 μm or less, The density of the polyethylene particles according to JIS K6922-2 is 950 kg / m 3 More than 1000kg / m 3 is as follows: The static friction coefficient of the coating layer in accordance with JIS P8147:2010 is 0.30 or more and 0.50 or less, The coating layer has a dynamic friction coefficient in accordance with JIS P8147:2010 of 0.20 or more and 0.35 or less, The arithmetic mean height of the coating layer in accordance with JIS B0601:2001 is 0.50 μm or more and 0.90 μm or less, The total content of the dye contained in the substrate and the coating layer is 0.1% by mass or less with respect to the substrate and the coating layer. How election ballots are manufactured.
[0018] (12) The method according to (11), wherein the substrate is biaxially stretched after extrusion molding. Effect of the Invention
[0019] According to the present invention, an election ballot paper is provided in which variation in paper feedability is reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, an embodiment of the present invention will be described in detail, but the present invention is not particularly limited thereto.
[0021] <Election ballot paper> An election ballot paper according to one aspect of the present invention includes a substrate and a coating layer provided on one or both sides of the substrate.
[0022] As explained in Patent Publication No. 7049733, by adjusting the composition of the coating layer and the physical properties of the halftone dot printed area on the surface of the coating layer to meet specified conditions, election ballot papers can be obtained that have excellent paper feedability, writability, and fold recovery, as well as excellent recyclability.
[0023] However, the present inventors have found that there is a possibility that variations in paper feed properties may occur for mass-produced election ballots, even if they have the same composition. It was then unexpectedly discovered that such variations could be suppressed by blending polyethylene particles that meet certain requirements. Although the reason for this is unclear, it is presumed that blending the polyethylene particles into the coating layer creates appropriate roughness and friction on the surface of the coating layer, preventing excessive adhesion between sheets of paper and more reliably suppressing double feeding, etc., thereby suppressing variations in paper feedability.
[0024] In the present invention, an "election ballot" is a form used in any election on which voters write the representatives, etc., they have selected. The election ballot paper in the present invention includes ballot papers that comply with the "Regulations Concerning Ballot Papers, etc." (Notification No. 3 of the Election Administration Commission, November 1, 2004).
[0025] In the present invention, "paper feedability" refers to the ease with which election ballots can be fed through a counting machine or the like. For example, "high paper feedability" and "good paper feedability" include the ease with which election ballots can be fed and the ability to accurately count ballots using a counting machine or the like (few or no missed counts).
[0026] In the present invention, "variation in paper feedability is suppressed" encompasses little or no difference in the degree of paper feedability between different lots of election ballot papers of the same composition. For example, if there is no or only a small difference in the number of election ballots that cannot be counted properly, even if the lots are different for election ballots of the same composition, it can be determined that variation in paper feedability is suppressed.
[0027] The paper feed property and the variation in the paper feed property can be evaluated by the method shown in the examples.
[0028] The structure of the election ballot paper of the present invention will now be described in detail. In the following, unless otherwise specified, the specifications regarding mass refer to dry mass.
[0029] (1) Base material The structure of the substrate in the election ballot paper of the present invention is not particularly limited, and any structure conventionally known in the papermaking field can be used.
[0030] Examples of substrates include plastic sheets whose main component is a resin-based material, sheets made of pulp-based materials (paper substrates such as glassine paper, coated paper, fine paper, dust-free paper, and impregnated paper), synthetic paper, and combinations of these (laminated paper).
[0031] From the viewpoint of making it easier to achieve the effects of the present invention, the mass ratio of thermoplastic resin to inorganic substance powder (thermoplastic resin:inorganic substance powder) of the substrate can be preferably 50:50 to 10:90, more preferably 45:55 to 20:80, and even more preferably 40:60 to 25:75. When the configuration of the substrate satisfies the above requirements, the substrate has excellent impact resistance and moldability.
[0032] From the viewpoint of making it easier to achieve the effects of the present invention, the lower limit of the amount of the thermoplastic resin contained is preferably 20% by mass or more, and more preferably 25% by mass or more, relative to the base material.
[0033] From the viewpoint of making it easier to achieve the effects of the present invention, the upper limit of the content of the thermoplastic resin is preferably 45% by mass or less, and more preferably 40% by mass or less, relative to the base material.
[0034] From the viewpoint of making it easier to achieve the effects of the present invention, the lower limit of the content of the inorganic substance powder is preferably 55% by mass or more, and more preferably 60% by mass or more, relative to the base material.
[0035] From the viewpoint of making it easier to obtain the effects of the present invention, the upper limit of the content of the inorganic substance powder is preferably 80% by mass or less, and more preferably 75% by mass or less, relative to the base material.
[0036] Examples of the components of the substrate layer will be described in detail below.
[0037] (1-1)Thermoplastic resin The thermoplastic resin constituting the substrate is not particularly limited, and any resin that can be used in the papermaking field can be adopted. The thermoplastic resin can be used alone or in combination of two or more kinds.
[0038] Examples of thermoplastic resins include the following: Polyolefin resins (polypropylene resins, polyethylene resins, polymethyl-1-pentene, ethylene-cyclic olefin copolymers, etc.); Functional group-containing polyolefin resins (ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, metal salts of ethylene-methacrylic acid copolymers (ionomers), ethylene-acrylic acid alkyl ester copolymers, ethylene-methacrylic acid alkyl ester copolymers, maleic acid modified polyethylene, maleic acid modified polypropylene, etc.); Thermoplastic polyester resins (aromatic polyester resins (polyamide resins such as nylon-6, nylon-6,6, nylon-6,10, nylon-6,12, etc.; polyethylene terephthalate and its copolymers, polyethylene naphthalate, polybutylene terephthalate, etc.), aliphatic polyester resins (polybutylene succinate, polylactic acid, etc.), etc.); Polycarbonate resins (aromatic polycarbonates, aliphatic polycarbonates, etc.); Polystyrene resins (atactic polystyrene, syndiotactic polystyrene, acrylonitrile-styrene (AS) copolymers, acrylonitrile-butadiene-styrene (ABS) copolymers, etc.); Polyvinyl chloride resins (polyvinyl chloride, polyvinylidene chloride, etc.); Polyphenylene sulfide; Polyether resins, etc. (polyethersulfone, polyetherketone, polyetheretherketone, etc.).
[0039] Among the thermoplastic resins, in view of ease of molding, performance, economics, etc., it is preferable to use polyolefin-based resins, aromatic polyester-based resins, or aliphatic polyester-based resins, and it is particularly preferable to use polyolefin-based resins.
[0040] In the present invention, the term "polyolefin resin" refers to a polyolefin resin containing an olefin component unit as a main component. "Containing an olefin component unit as the main component" means that the olefin component unit is contained in the polyolefin resin at 50% by mass or more (preferably 75% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, and most preferably 100% by mass). The method for producing the polyolefin resin used in the present invention is not particularly limited, and may be any method using a Ziegler-Natta catalyst, a metallocene catalyst, a radical initiator (oxygen, peroxide, etc.), or the like.
[0041] From the viewpoint of a balance between mechanical strength and heat resistance, etc., the base material preferably contains a polypropylene-based resin and / or a polyethylene-based resin among polyolefin-based resins, more preferably contains a polypropylene-based resin, and most preferably contains only a polypropylene-based resin as a resin component.
[0042] The polypropylene resin may be a resin containing 50% by mass or more of propylene component units. More specific examples of polypropylene-based resins include propylene homopolymers, copolymers of propylene and other α-olefins (copolymerizable with propylene), etc. Examples of the "other α-olefins" include α-olefins having 4 to 10 carbon atoms (ethylene, 1-butene, isobutylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 3,4-dimethyl-1-butene, 1-heptene, 3-methyl-1-hexene, etc.). Of these, propylene homopolymer is particularly preferred.
[0043] Propylene homopolymers include linear or branched polypropylenes exhibiting various stereoregularities (isotactic, syndiotactic, atactic, hemiisotactic, etc.).
[0044] The propylene copolymer may be any of a random copolymer, a block copolymer, a binary copolymer, a ternary copolymer, etc. Specific examples include an ethylene-propylene random copolymer, a butene-1-propylene random copolymer, an ethylene-butene-1-propylene random terpolymer, an ethylene-propylene block copolymer, etc.
[0045] Examples of polyethylene resins include resins containing 50% by mass or more of ethylene component units, such as high density polyethylene (HDPE), low density polyethylene (LDPE), medium density polyethylene (MDPE), linear low density polyethylene (LLDPE), ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, ethylene-propylene-butene 1 copolymer, ethylene-butene 1 copolymer, ethylene-hexene 1 copolymer, ethylene-4 methylpentene 1 copolymer, and ethylene-octene 1 copolymer.
[0046] (1-2) Inorganic substance powder The inorganic powder constituting the substrate is not particularly limited, and any resin that can be used in the papermaking field can be used. The inorganic powder can be used alone or in combination of two or more kinds.
[0047] The inorganic powder may be synthetic or derived from natural minerals, and examples of the inorganic powder include powders of carbonates, sulfates, silicates, phosphates, borates, oxides, or hydrates of metals (calcium, magnesium, aluminum, titanium, iron, zinc, etc.). More specific examples include calcium carbonate, magnesium carbonate, zinc oxide, titanium oxide, silica, alumina, clay, talc, kaolin, aluminum hydroxide, magnesium hydroxide, aluminum silicate, magnesium silicate, calcium silicate, aluminum sulfate, magnesium sulfate, calcium sulfate, magnesium phosphate, barium sulfate, silica sand, carbon black, zeolite, molybdenum, diatomaceous earth, sericite, shirasu, calcium sulfite, sodium sulfate, potassium titanate, bentonite, and graphite. Of these, calcium carbonate powder is preferred.
[0048] The calcium carbonate may be either heavy calcium carbonate or light calcium carbonate. From the viewpoint of easily realizing good writability, it is preferable that the base material contains heavy calcium carbonate, and it is more preferable that the inorganic substance powder contained in the base material is made of heavy calcium carbonate.
[0049] In addition, "heavy calcium carbonate" is calcium carbonate obtained by mechanically crushing (dry method, wet method, etc.) natural raw materials whose main component is CaCO3 (limestone, etc.). "Light calcium carbonate" is calcium carbonate prepared by a synthetic method (such as chemical precipitation reaction). Therefore, heavy calcium carbonate and light calcium carbonate are clearly distinguished.
[0050] The shape of the inorganic powder is not particularly limited, and may be any of particles, flakes, granules, fibers, etc. Furthermore, these shapes may be uniform shapes obtained by synthesis methods, etc., or may be irregular shapes obtained by pulverizing natural minerals, etc.
[0051] The inorganic powder is preferably in the form of particles or fibers.
[0052] When the inorganic powder is particulate, its average particle size according to JIS M-8511 is preferably 0.01 μm to 50.0 μm, more preferably 1.0 μm to 10.0 μm, and even more preferably 1.0 μm to 5.0 μm. In particular, it is preferable that the particle size distribution does not contain any particles having a particle size exceeding 50.0 μm. When the average particle size satisfies the above requirements, an increase in viscosity during kneading with a thermoplastic resin is easily suppressed, and molding processability is easily improved.
[0053] In the present invention, the "average particle size according to JIS M-8511" means a value calculated from the measurement results of the specific surface area by the air permeability method according to JIS M-8511. As a measuring device, for example, a specific surface area measuring device SS-100 type manufactured by Shimadzu Corporation can be preferably used.
[0054] When the inorganic powder is fibrous, the average fiber length is preferably 3.0 μm or more and 20.0 μm or less, the average fiber diameter is preferably 0.2 μm or more and 1.5 μm or less, and the aspect ratio is usually 10 or more and 30 or less.
[0055] In the present invention, the terms "average fiber length" and "average fiber diameter" refer to values measured using an electron microscope. The aspect ratio refers to the ratio of the average fiber length to the average fiber diameter (average fiber length / average fiber diameter).
[0056] The inorganic powder may be surface-treated in advance to enhance its dispersibility or reactivity. Examples of the surface treatment method include physical methods (plasma treatment, etc.) and chemical methods (methods using coupling agents or surfactants). Examples of the coupling agent include a silane coupling agent, a titanium coupling agent, etc. Examples of the surfactant include an anionic, cationic, nonionic, and amphoteric surfactant, and examples of the surfactant include a higher fatty acid, a higher fatty acid ester, a higher fatty acid amide, and a higher fatty acid salt.
[0057] (1-3) Other additives in the substrate In addition to the above-mentioned components, the base material may or may not contain other additives as necessary, such as dyes, lubricants, plasticizers, coupling agents, flow improvers, dispersants, antioxidants, UV absorbers, flame retardants, stabilizers, antistatic agents, and foaming agents. These additives may be used alone or in combination of two or more. The types and contents of these additives can be appropriately set depending on the effects to be obtained.
[0058] However, when a dye is blended in the substrate, the total content of the dye contained in the substrate and the coating layer is adjusted to 0.1% by mass or less based on the substrate and the coating layer. For example, the content of the dye is preferably 0.1% by mass or less, and more preferably 0% by mass, relative to the substrate (that is, the substrate does not contain any dye).
[0059] In the present invention, the term "colorant" includes any component that is blended for the purpose of coloring in the papermaking field. Examples of colorants include disazo yellow, brilliant carmine 6B, phthalocyanine blue, lake red C, carbon black, titanium white, etc.
[0060] (1-4) Other configurations of the substrate Other configurations of the substrate are not particularly limited.
[0061] The layer structure of the substrate may be a single layer or a multilayer. When the substrate is multilayered, any layer may be provided according to the purpose (such as a sealant layer for improving adhesion between the substrate and the coating layer, a protective layer, a shielding layer, or an adhesive layer on the substrate surface on which no coating layer is provided). However, when the substrate has multiple layers, at least one of the layers must satisfy the requirements for the substrate of the present invention, and preferably all of the layers satisfy the requirements for the substrate of the present invention.
[0062] The substrate may be a stretched sheet or an unstretched sheet. In the case of a stretched sheet, it may be stretched uniaxially, e.g., longitudinally or transversely, or biaxially.
[0063] The size of the substrate is not particularly limited, and may be any size appropriate for an election ballot. For example, the size of a typical election ballot is 128 mm long by 80 mm wide, and the size of the substrate may be of such a size.
[0064] The thickness of the substrate is not particularly limited, and is usually from 10 μm to 300 μm, preferably from 25 μm to 200 μm.
[0065] The substrate may be subjected to a surface treatment on one or both sides as required. The surface treatment may be applied to the entire surface or a part of the surface of the substrate. Preferred surface treatments include treatment by an oxidation method, treatment by a roughening method, and primer treatment, from the viewpoint of improving adhesion to a coating layer provided on the surface of the substrate. Examples of the oxidation method include corona discharge treatment, flame treatment, plasma treatment, glow discharge treatment, chromic acid treatment (wet), flame treatment, hot air treatment, ozone / ultraviolet light irradiation treatment, and the like. Examples of the roughening method include a sandblasting method and a solvent treatment method.
[0066] (2) Coating layer The coating layer is provided on one or both sides of the substrate. The coating layer may be provided on the entire surface of the substrate, or may be provided on a part of the surface. However, from the viewpoint of easily achieving the effects of the present invention, it is preferable that the coating layer is provided on the entire surface of the substrate. The coating layer of the election ballot of the present invention may represent the area where a voter makes marks using a writing instrument.
[0067] In the coating layer, clay, ground calcium carbonate, and polyethylene particles are present in a continuous phase made of an acrylic polymer so as to satisfy the requirements of the present invention, thereby forming fine irregularities with appropriate hardness without impairing the smoothness of the paper surface. The inventor has discovered that election ballot papers having such a coating layer can achieve not only good writability, fold recovery, etc., but also suppression of variation in paper feedability. The inventors also found that such a coating layer has good adhesion and bonding properties to the above-mentioned substrate (particularly, to a substrate containing a polypropylene-based resin).
[0068] The thickness of the coating layer (thickness in a dry state) is not particularly limited, and is usually from 1 μm to 10 μm, preferably from 2 μm to 8 μm, and more preferably from 3 μm to 5 μm. When the thickness of the coating layer is within the above range, the coating layer functions satisfactorily as an ink receiving layer, and is likely to exhibit ink receiving properties (good coloring, color development, etc.). Furthermore, the election ballot paper is likely to have good properties such as water resistance, antistatic surface, and adhesion to ink.
[0069] The thickness of the coating layer (thickness in a dry state) can be, for example, 1% or more and 15% or less of the thickness of the substrate.
[0070] The components of the coating layer will be described in detail below.
[0071] (2-1) Acrylic polymer that forms the continuous phase The acrylic polymer of the coating layer serves as a continuous phase, in other words, a matrix. The acrylic polymer may be any of those conventionally used in the papermaking field. The acrylic polymer may be used alone or in combination of two or more.
[0072] Examples of acrylic polymers include polymers obtained from (meth)acrylic acid, (meth)acrylic acid esters, (meth)acrylamide, and (meth)acrylonitrile as main monomer components. In the present invention, the term "(meth)acrylic" is used to mean both "acrylic" and "methacrylic".
[0073] The monomer components constituting the acrylic polymer may be used alone or in combination. That is, the acrylic polymer may be a homopolymer constituted of only one type of monomer component, or a copolymer in which a plurality of monomer components are combined.
[0074] Examples of monomer components constituting the acrylic polymer include one or more selected from the group consisting of the following components (acrylic acid, methacrylic acid). Acrylic acid alkyl esters having an alkyl group with 1 to 18 carbon atoms (such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, t-butyl acrylate, hexyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, isooctyl acrylate, nonyl acrylate, lauryl acrylate, stearyl acrylate, palmityl acrylate, and cyclohexyl acrylate); Methacrylic acid alkyl esters having an alkyl group of 1 to 18 carbon atoms (such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, t-butyl methacrylate, hexyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, nonyl methacrylate, lauryl methacrylate, stearyl methacrylate, palmityl methacrylate, and cyclohexyl methacrylate); Alkyl esters of (meth)acrylic acid having a hydroxyl group on the side chain (2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, monohydroxyethyl phthalate acrylate, etc.); Polyethylene glycol having an ethylene glycol unit in the molecule (n is preferably 3 or more and 20 or less). Diacrylate, trimethylolpropane EO modified (n is preferably 3 or more and 20 or less). Triacrylate, phenol EO modified (n is preferably 3 or more and 20 or less). Acrylate; Alkenyloxyalkyl esters of (meth)acrylic acid (such as allyloxyethyl acrylate and allyloxyethyl methacrylate); Alkyl esters having an alkoxyl group on the side chain of (meth)acrylic acid (methoxybutyl acrylate, methoxybutyl methacrylate, methoxyethyl acrylate, methoxyethyl methacrylate, ethoxybutyl acrylate, ethoxybutyl methacrylate, etc.); Alkenyl esters of (meth)acrylic acid (such as allyl acrylate and allyl methacrylate); Alkyl esters of acrylic acid having an epoxy group on the side chain (e.g., glycidyl acrylate, glycidyl methacrylate, methyl glycidyl acrylate, methyl glycidyl methacrylate, etc.); Mono- or di-alkylaminoalkyl esters of (meth)acrylic acid (diethylaminoethyl acrylate, diethylaminoethyl methacrylate, methylaminoethyl acrylate, methylaminoethyl methacrylate, etc.); Silicone-modified (meth)acrylic acid esters having a silyl group, an alkoxysilyl group, a hydrolyzable alkoxysilyl group, or the like as a side chain; Acrylamide, methacrylamide; (Meth)acrylamides having a methylol group (such as N-methylol acrylamide and N-methylol methacrylamide); (Meth)acrylamides having an alkoxymethylol group (N-alkoxymethylol acrylamide (e.g., N-isobutoxymethylol acrylamide, etc.), N-alkoxymethylol methacrylamide (e.g., N-isobutoxymethylol methacrylamide, etc.), etc.); (Meth)acrylamides having alkoxyalkyl groups (such as N-butoxymethyl acrylamide and N-butoxymethyl methacrylamide); and Various acrylic monomers (acrylonitrile, methacrylonitrile, etc.).
[0075] The acrylic polymer may be one in which a crosslinked structure is introduced by a photocuring reaction, etc. Such an acrylic polymer makes it easy to increase the film strength of the coating layer. From the viewpoint of introducing a crosslinked structure, a difunctional or polyfunctional acrylic monomer, specifically a polyfunctional (meth)acrylate, may be used as a monomer component. Examples of polyfunctional (meth)acrylates include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, the above-mentioned polyethylene glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphoric acid di(meth)acrylate, allylated cyclohexyl di(meth)acrylate, isocyanurate di(meth)acrylate, and trimethylolpropane tri(meth)acrylate. dipentaerythritol tri(meth)acrylate, propionic acid modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, propionic acid modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, caprolactone modified dipentaerythritol hexa(meth)acrylate, and the like.
[0076] Other monomer components that form copolymers with the above-mentioned monomer components include vinyl monomers (vinyl acetate, vinyl chloride, vinylidene chloride, vinyl lactate, vinyl butyrate, vinyl versatate, vinyl benzoate, etc.), ethylene, butadiene, styrene, etc.
[0077] Particularly preferred examples of the acrylic polymer include (meth)acrylic acid alkyl ester copolymers.
[0078] Preferred examples of the (meth)acrylic acid alkyl ester copolymer include one or more selected from the group consisting of methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, isooctyl acrylate, nonyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, 2-hydroxymethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, and 2-hydroxypropyl methacrylate.
[0079] The content of the acrylic polymer is not particularly limited as long as a continuous phase made of the acrylic polymer can be sufficiently formed and the clay, ground calcium carbonate, and polyethylene particles can be sufficiently blended. The lower limit of the content of the acrylic polymer is preferably 15% by mass or more, and more preferably 30% by mass or more, based on the coating layer. The upper limit of the content of the acrylic polymer is preferably 50% by mass or less, and more preferably 45% by mass or less, based on the coating layer.
[0080] (2-2) Clay The content of the clay is 25% by mass or more and 55% by mass or less with respect to the coating layer.
[0081] The lower limit of the clay content is 25% by mass or more, preferably 28% by mass or more, and more preferably 30% by mass or more, relative to the coating layer, from the viewpoint of easily improving the printability of the coating layer and further, making it easier for the polyethylene particles to exert the effect of suppressing variations in paper feed performance.
[0082] The upper limit of the clay content is 55% by mass or less, preferably 52% by mass or less, and more preferably 50% by mass or less, relative to the coating layer, from the viewpoints of easily forming a continuous phase consisting of an acrylic polymer and further imparting sufficient water resistance to the coating layer and easily obtaining a good appearance.
[0083] In the present invention, the term "clay" includes clay minerals having a layered structure and clay minerals not having a layered structure (imogolite, allophane, etc.). Clays can be used alone or in combination of two or more kinds.
[0084] Examples of clay minerals having a layered structure include swelling minerals (smectite, vermiculite, montmorillonite, bentonite, illite, hectorite, halloysite, saponite, beidellite, stevensite, nontronite, smectite, mica, brittle mica, sericite, illite, glauconite, hydrotalcite, etc.), and non-swelling minerals (kaolin minerals (kaolinite, sapphire), serpentine, pyrophyllite, talc, chlorite, zeolite, etc.).
[0085] The clay may be any of natural clay, synthetic clay, and organo-clay.
[0086] The organized clay is not particularly limited, but is preferably a clay (natural product, synthetic product, etc.) that has been organized with an organizing agent.
[0087] The organizing agent may be any agent capable of organifying clay, such as hexyl ammonium ion, octyl ammonium ion, 2-ethylhexyl ammonium ion, dodecyl ammonium ion, lauryl ammonium ion, octadecyl ammonium ion, dioctyl dimethyl ammonium ion, trioctyl ammonium ion, dioctadecyl dimethyl ammonium ion, trioctyl ammonium ion, dioctadecyl dimethyl ammonium ion, trioctyl ammonium ion, dioctadecyl dimethyl ammonium ion, trioctadecyl ammonium ion, and the like.
[0088] From the viewpoint of easily achieving the effects of the present invention, the clay preferably contains kaolin clay (clay containing kaolinite as a main component), and more preferably consists of kaolin clay.
[0089] The particle size of the clay is not particularly limited and can be appropriately set depending on the thickness of the coating layer to be formed, etc. From the viewpoint of easily achieving the effects of the present invention and further easily achieving good dispersibility in the coating layer, adhesion to the substrate, printability, and antistatic properties, the volume average particle size (MV) of the clay is preferably 0.05 μm or more and 2.00 μm or less, more preferably 0.10 μm or more and 1.70 μm or less, and even more preferably 0.20 μm or more and 1.50 μm or less.
[0090] In the present invention, the term "volume average particle size" (MV) refers to the 50% diameter (D50) in the volume-based cumulative fraction in particle size distribution measurement based on a laser diffraction scattering method.
[0091] The more uniform the particle size of the clay, the more likely it is that the in-plane properties of the coating layer will become uniform, which is preferable.
[0092] The shape of the clay is not particularly limited, and may be any of spherical, elliptical, flat, irregular, and the like. However, from the viewpoint of dispersibility in the coating layer, for example, the aspect ratio (major axis / minor axis) is preferably 20 or less, more preferably 18 or less, and further preferably 15 or less.
[0093] The specific gravity of the clay is not particularly limited, but from the viewpoint of dispersibility in the coating layer, it is preferably 1.5 or more and 3.0 or less, and more preferably 2.0 or more and 2.8 or less.
[0094] (2-3) Ground calcium carbonate As the heavy calcium carbonate contained in the coating layer, the same one as explained in the above section "(1-2) Inorganic substance powder" can be used. However, the ground calcium carbonate contained in the coating layer has a volume average particle size (MV) of 0.05 μm or more and 2.00 μm or less.
[0095] As a result of the inventor's investigation, it was found that when the volume average particle diameter of heavy calcium carbonate exceeds 2.00 μm, the adhesion between the substrate and the coating layer is reduced compared to the case where the same amount of light calcium carbonate is used. This is presumably because, with heavy calcium carbonate having a volume average particle diameter of more than 2.00 μm, the anchor effect due to the unevenness of the particle surface is difficult to manifest, and the adhesion is reduced due to the falling off of the particles, etc. On the other hand, it was also found that when the volume average particle size of heavy calcium carbonate is in the range of 0.05 μm to 2.00 μm, the adhesiveness is improved compared to the case of using light calcium carbonate of the same particle size. This is thought to be because the particles of heavy calcium carbonate having such a volume average particle size are less likely to fall off, and the anchor effect due to the irregular shape of the particles can be well expressed.
[0096] The lower limit of the volume average particle diameter of the heavy calcium carbonate is 0.05 μm or more, preferably 0.07 μm or more, more preferably 0.10 μm or more, and even more preferably 0.20 μm or more, from the viewpoint of fully exerting the anchoring effect and further facilitating improvement in the smoothness of the coating layer and the glossiness of the sheet.
[0097] The upper limit of the volume average particle size of the ground calcium carbonate is 2.00 μm or less, preferably 1.50 μm or less, more preferably 1.00 μm or less, and even more preferably 0.50 μm or less, from the viewpoint of easily improving the adhesion between the substrate and the coating layer.
[0098] The content of the ground calcium carbonate is from 5% by mass to 30% by mass with respect to the coating layer.
[0099] The lower limit of the content of heavy calcium carbonate is 5% by mass or more, preferably 6% by mass or more, more preferably 8% by mass or more, and even more preferably 9% by mass or more, relative to the coating layer, from the viewpoints of easily improving the quick-drying properties of the ink on the coating layer and the suitability for offset printing, and furthermore, making it easier for the polyethylene particles to exert an effect of suppressing variations in paper feed performance.
[0100] The upper limit of the content of heavy calcium carbonate is 30% by mass or less, preferably 29% by mass or less, more preferably 27% by mass or less, and even more preferably 25% by mass or less, of the coating layer, from the viewpoints of easily forming a continuous phase consisting of an acrylic polymer, easily smoothing the surface of the coating layer, and further, not easily impairing the effect of the polyethylene particles in suppressing variations in paper feed performance.
[0101] The surface of the heavy calcium carbonate may be previously treated in order to enhance its dispersibility and reactivity. The surface treatment method may be the same as that described in the above section "(1-2) Inorganic substance powder." From the viewpoint of easily achieving the effects of the present invention, the surface treatment method is preferably a surface treatment with a fatty acid (such as a higher fatty acid).
[0102] (2-4) Polyethylene particles The polyethylene particles contained in the coating layer generate appropriate roughness and friction on the surface of the coating layer, which can improve the passability of election ballot papers and suppress the variation in the passability.
[0103] In the present invention, the "polyethylene particles" include ethylene homopolymers, ethylene copolymers, and the like.
[0104] The particle size of the polyethylene particles according to JIS Z8832:2010 is 8.0 μm or more and 11.0 μm or less. When the particle diameter of the polyethylene particles is within this range, the polyethylene particles can form appropriate irregularities on the surface of the coating layer, producing roughness sufficient to suppress variations in paper feed properties.
[0105] The lower limit of the particle size of the polyethylene particles in accordance with JIS Z8832:2010 is 8.0 μm or more, preferably 8.5 μm or more, and more preferably 9.0 μm or more, from the viewpoint of easily producing better roughness.
[0106] The upper limit of the particle size of the polyethylene particles according to JIS Z8832:2010 is 11.0 μm or less, preferably 10.5 μm or less, and more preferably 10.0 μm or less, from the viewpoint of easily producing better roughness and hardly impairing printing characteristics.
[0107] The density of polyethylene particles according to JIS K6922-2 is 950kg / m 3 More than 1000kg / m 3 The following is the result. When the density of the polyethylene particles is within this range, the polyethylene particles can form unevenness with an appropriate hardness on the surface of the coating layer, and the variation in paper feed performance can be effectively suppressed.
[0108] The lower limit of the density of polyethylene particles according to JIS K6922-2 is 950 kg / m3 from the viewpoint of easily producing a better roughness. 3 More than 955kg / m 3 More preferably, 960 kg / m 3 That's all.
[0109] The upper limit of the density of polyethylene particles according to JIS K6922-2 is 1000 kg / m3 from the viewpoint of easily producing better roughness. 3 Less than or equal to 990 kg / m 3 Less than or equal to 980 kg / m 3 The following is the result.
[0110] The lower limit of the content of the polyethylene particles is preferably 1.0% by mass or more, more preferably 1.5% by mass or more, and even more preferably 2.0% by mass or more, based on the coating layer, from the viewpoint of easily achieving an effect of improving paper feedability.
[0111] From the viewpoint of easily forming appropriate unevenness, the upper limit of the content of the polyethylene particles is preferably 20.0% by mass or less, more preferably 18.0% by mass or less, and even more preferably 15.0% by mass or less, relative to the coating layer.
[0112] As the polyethylene particles, commercially available products can be used. A commercially available polyethylene particle suitable for use in the present invention is "Chemipearl (registered trademark) W310" (Mitsui Chemicals, Inc., particle size 9.5 μm, density 970 kg / m 3 ) are mentioned.
[0113] (2-5) Other additives in the coating layer In addition to the above-mentioned components, the coating layer may or may not contain other additives as necessary. Examples of other additives include surfactants, crosslinking agents, pH adjusters, thickeners, flow improvers, defoamers, foam inhibitors, release agents, penetrating agents, dyes, fluorescent brighteners, UV absorbers, antioxidants, preservatives, antifungal agents, water-resistant agents, ink fixing agents, hardeners, and weather-resistant materials. These additives may be used alone or in combination of two or more. The types and contents of these additives can be appropriately set depending on the effects to be obtained.
[0114] Examples of the crosslinking agent include aldehyde compounds, melamine compounds, isocyanate compounds, zirconium compounds, titanium compounds, amide compounds, aluminum compounds, boric acid, borates, carbodiimide compounds, and oxazoline compounds.
[0115] However, when a dye is blended in the coating layer, the total content of the dye contained in the substrate and coating layer is adjusted to 0.1% by mass or less based on the substrate and coating layer. For example, the content of the dye is preferably 0.1% by mass or less, and more preferably 0% by mass, relative to the coating layer (that is, the coating layer does not contain any dye).
[0116] From the viewpoint of easily achieving the effects of the present invention, it is preferable that the coating layer does not substantially contain or does not contain any fine particles other than clay, heavy calcium carbonate, and polyethylene particles (particularly, fine particles having a volume average particle size of 0.05 μm to 2.00 μm). Examples of such fine particles include polymer fine particles ((meth)acrylic acid ester resin particles, such as polymethyl methacrylate particles), zinc pyrithione, zinc oxide, etc.
[0117] (2-6) Physical properties of election ballots and coating layers In one form of the invention, the election ballot and / or coating layer have the following physical characteristics: A coating layer having such physical properties can be obtained by appropriately blending various components into the coating layer as specified in the present invention.
[0118] (2-6-1) Static friction coefficient The static friction coefficient of the coating layer in accordance with JIS P8147:2010 is 0.30 or more and 0.50 or less. Too high a static friction coefficient can impair the passability of the election ballot paper, whereas too low a static friction coefficient can impair the writeability of the election ballot paper.
[0119] The lower limit of the static friction coefficient is 0.30 or more, preferably 0.33 or more, and more preferably 0.35 or more.
[0120] The upper limit of the static friction coefficient is 0.50 or less, preferably 0.48 or less, and more preferably 0.45 or less.
[0121] (2-6-2) Coefficient of kinetic friction The coating layer has a dynamic friction coefficient in accordance with JIS P8147:2010 of 0.20 or more and 0.35 or less. If the coefficient of dynamic friction is too high, it may impair the passability of the election ballot paper, whereas if the coefficient of dynamic friction is too low, it may impair the writeability of the election ballot paper.
[0122] The lower limit of the dynamic friction coefficient is 0.20 or more, preferably 0.23 or more, and more preferably 0.25 or more.
[0123] The upper limit of the dynamic friction coefficient is 0.35 or less, preferably 0.34 or less, and more preferably 0.33 or less.
[0124] (2-6-3) Arithmetic mean height The arithmetic mean height of the coating layer in accordance with JIS B0601:2001 is 0.50 μm or more and 0.90 μm or less. If the arithmetic mean height is too high, it may impair the passability of the election ballot paper, whereas if the arithmetic mean height is too low, it may impair the writeability of the election ballot paper.
[0125] The lower limit of the arithmetic mean height is 0.50 μm or more, preferably 0.53 μm or more, and more preferably 0.55 μm or more.
[0126] The upper limit of the arithmetic mean height is 0.90 μm or less, preferably 0.88 μm or less, and more preferably 0.85 μm or less.
[0127] (2-6-4) Opacity The opacity of the election ballot paper in accordance with JIS P 8149:2000 is preferably 95% or more, more preferably 96% or more. In election ballots, it is necessary to prevent characters from showing through the side on which the voter has written (showing through), so the higher the opacity, the better.
[0128] (3) Halftone Printing Department In a preferred embodiment of the present invention, at least a part of the surface of the coating layer may be provided with a halftone dot printed portion using offset ink.
[0129] In the present invention, the "halftone dot printed portion" refers to a portion consisting of halftone dots offset printed using offset ink.
[0130] In the present invention, "offset printing" refers to a printing method in which ink applied to a plate is transferred to an intermediate transfer medium (such as a blanket), and then printed on a substrate (the coating layer in the present invention).
[0131] In the present invention, the "offset ink" refers to ink used in offset printing.
[0132] The offset printing conditions used to form the halftone dot printing section are not particularly limited, and any conventionally known offset printing machine, agent (primer treatment agent, etc.), and various processes (primer treatment process, printing process, drying process, etc.) can be used.
[0133] The dot percentage of the dot printed portion is preferably 10% or more and 50% or less, more preferably 15% or more and 45% or less, from the viewpoint of preventing deterioration of paper feed properties.
[0134] In the present invention, "dot percentage" is also known as "dot area ratio" and means the area of dots per unit area (unit: %). A dot percentage of a dot-printed area of 100% means that the dot-printed area is completely covered with ink (so-called solid color).
[0135] From the viewpoint of preventing deterioration of paper passing properties, the lower limit of the area (printed area) that the halftone dot printed portion occupies on the surface of the coat layer is preferably 10% or more, and more preferably 15% or more. The upper limit of the area is preferably 50% or less, more preferably 45% or less.
[0136] The diameter of the dots constituting the halftone dot printing portion may be uniform or non-uniform, however, from the viewpoint of preventing deterioration of paper feedability and printing efficiency, it is preferable that the diameter of the dots constituting the halftone dot printing portion is uniform.
[0137] The diameter of the dots constituting the halftone dot printing portion is, for example, 0.5 μm or more and 5 μm or less.
[0138] <How election ballots are manufactured> The method for producing the election ballot paper of the present invention is not particularly limited and any method can be adopted, but in a preferred embodiment, it may include the following steps. (Step 1) A step of obtaining a substrate by extrusion molding a resin composition containing a polyolefin resin and an inorganic substance powder in a mass ratio of 50:50 to 10:90. (Step 2) A step of forming a coating layer by applying and drying an aqueous emulsion containing an acrylic polymer, clay, ground calcium carbonate, and polyethylene particles to one or both sides of the substrate. (Step 3) Optionally, a step of providing a halftone dot printing portion using offset ink on at least a part of the surface of the coating layer.
[0139] (1) Regarding step 1 The method for forming the substrate is not particularly limited, and examples of the method include a method in which each component constituting the substrate is formed into a sheet shape using a molding machine (such as an extrusion molding machine) to obtain the substrate.
[0140] The components constituting the base material may be mixed before being charged into the molding machine from the hopper, or may be mixed simultaneously with molding by the molding machine.
[0141] The components constituting the base material are preferably melt-kneaded using a twin-screw kneader from the viewpoint of achieving uniform dispersion and the effect of high shear stress.
[0142] The molding temperature in step 1 tends to produce an odor more easily as the temperature is higher, so it is preferably not more than the melting point of the polyolefin resin + 55°C, more preferably not less than the melting point of the polyolefin resin + 55°C, and even more preferably not less than the melting point of the polyolefin resin + 10°C and not more than the melting point of the polyolefin resin + 45°C.
[0143] The substrate may be stretched (longitudinally and / or transversely stretched). Stretching reduces the density of the substrate, resulting in a substrate with good whiteness. The stretching may be any of uniaxial stretching, biaxial stretching (sequential biaxial stretching, simultaneous biaxial stretching, etc.), and multiaxial stretching (stretching by a tubular method, etc.). Among these, biaxial stretching is preferred from the viewpoint of easily achieving the effects of the present invention.
[0144] (2) Regarding step 2 As a method for providing a coating layer on one or both sides of a substrate, a coating liquid containing each component constituting the coating layer is applied to the substrate surface, followed by drying.
[0145] The form of the coating liquid is not particularly limited, but may be one in which each component constituting the coating layer is dispersed or dissolved in a solvent, such as water or an organic solvent. The coating liquid in the present invention is preferably an aqueous emulsion in which the components constituting the coat layer are dispersed in water.
[0146] The method for producing the aqueous emulsion is not particularly limited, and any conventional method such as emulsion polymerization can be used.
[0147] As the surfactant optionally used in the emulsion polymerization, anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, etc. may be used alone or in combination of two or more. Among these, nonionic surfactants and cationic surfactants are preferred.
[0148] Examples of the nonionic surfactant include polyoxyethylene alkyl ether, polyoxyethylene alkyl phenyl ether, polyoxyethylene alkyl ester, sorbitan alkyl ester, polyoxyethylene sorbitan alkyl ester, etc. Among these, polyoxyethylene alkyl phenyl ether is preferred.
[0149] Examples of the cationic surfactant include dodecyltrimethylammonium chloride, stearyltrimethylammonium chloride, and N-2-ethylhexylpyridinium chloride.
[0150] The amount of the surfactant in the aqueous emulsion may be, for example, from 1% by mass to 5% by mass relative to the polyolefin resin (total amount).
[0151] Polymerization initiators optionally used in emulsion polymerization include persulfates (potassium persulfate, ammonium persulfate, etc.), water-soluble types (hydrogen peroxide, t-butyl hydroperoxide, azobisamidinopropane hydrochloride, etc.), oil-soluble types (benzoyl peroxide, diisopropyl peroxydicarbonate, cumyl peroxyneodecanoate, cumyl peroxyoctoate, azobisisobutyronitrile, etc.), etc. Among these, the water-soluble types are preferred.
[0152] The amount of the polymerization initiator in the aqueous emulsion may be, for example, 0.01% by mass or more and 0.50% by mass or less with respect to the polyolefin resin (total amount).
[0153] The conditions for the emulsion polymerization reaction are not particularly limited, and the reaction is usually carried out at a temperature of 35 to 90° C. for 3 to 40 hours with stirring.
[0154] At the start or end of emulsion polymerization, a basic substance may be added to adjust the pH to 5 to 9 to improve the emulsion's shelf stability, freezing stability, chemical stability, etc. Examples of basic substances include ammonia, ethylamine, diethylamine, triethylamine, ethanolamine, triethanolamine, dimethylethanolamine, caustic soda, caustic potassium, etc.
[0155] The aqueous emulsion may contain a protective colloid (a water-soluble polymer such as gelatin or polyvinyl alcohol).
[0156] The coating liquid may be prepared by dispersing each component together with a solvent using a stirrer or disperser (eg, wet colloid mill, edged turbine, paddle blade, etc.) at a rotation speed of 500 to 3000 rpm for 1 to 5 minutes. However, since clay and heavy calcium carbonate may aggregate, a dispersant may be added as necessary. Since clay and heavy calcium carbonate have approximately the same specific gravity, clay and heavy calcium carbonate are unlikely to be unevenly distributed in the coating liquid and can be easily dispersed uniformly.
[0157] Examples of the coating method include a method in which a coating liquid is applied by an appropriate method (microgravure, roll coating, blade coating, bar coating, brush coating, spray coating, dipping, etc.) and then the coating layer is dried and cured. The temperature for drying or curing the coating layer may be, for example, 90°C or higher and 120°C or higher.
[0158] (3) Regarding step 3 As a method for providing a halftone dot printed portion on at least a part of the surface of the coating layer, any device and conditions employed in offset printing can be used.
[0159] (4) Other processes After step 2 or step 3, the resulting paper can be used as an election ballot. The election ballot may be subjected to a quality inspection process, a packaging process, etc., as necessary. EXAMPLES
[0160] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0161] <Preparation of election ballots> The election ballots were prepared in the following manner:
[0162] (1) Preparation of materials The materials for the substrate and the coating layer were prepared as follows.
[0163] (1-1) Substrate material Polyolefin resin: Polypropylene homopolymer (melting point 160°C) Inorganic powder: Heavy calcium carbonate powder (average particle size measured by air permeability method according to JIS M-1511: 2.2 μm)
[0164] (1-2) Coating layer material The coating layer in each example contains one each of the following acrylic polymer, clay, ground calcium carbonate, and polyethylene particles.
[0165] (1-2-1) Acrylic polymer Acrylic polymer-1: (meth)acrylic acid alkyl ester copolymer containing n-butyl acrylate, methyl methacrylate, 2-ethylhexyl acrylate, methacrylic acid, vinyl acetate, and a rosin derivative in a ratio (mass ratio) of 26:16:44:8:6:3. Acrylic polymer-2: styrene-acrylic acid ester copolymer containing styrene, benzyl acrylate, butyl acrylate, 1,6-hexanediol dimethacrylate, and 2-hydroxyethyl methacrylate in a ratio of 84.0:26.0:32.0:0.1:0.9 (mass ratio)
[0166] (1-2-2) Clay Clay: Kaolin clay (volume average particle size 0.29 μm, specific gravity 2.5)
[0167] (1-2-3) Ground calcium carbonate Heavy calcium carbonate-1: Volume average particle size 0.01 μm, specific gravity 2.6 Heavy calcium carbonate-2: Volume average particle size 0.15μm, specific gravity 2.6 Heavy calcium carbonate-3: Volume average particle size 3.00 μm, specific gravity 2.6
[0168] (1-2-4) Polyethylene particles Polyethylene particle-1: "Chemipearl (registered trademark) W310" (Mitsui Chemicals, Inc.), particle size 9.5 μm, density 970 kg / m 3 Polyethylene particle-2: "Chemipearl (registered trademark) W308" (Mitsui Chemicals, Inc.), particle size 6.0 μm, density 970 kg / m 3 Polyethylene particle-3: "Chemipearl (registered trademark) W410" (Mitsui Chemicals, Inc.), particle size 9.5 μm, density 920 kg / m 3
[0169] The polyethylene particles are commercially available as liquid reagents, each of which contains approximately 40% by mass of polyethylene. Therefore, in this example, the solid content of polyethylene was calculated and the composition was adjusted to contain the amount (dry mass) shown in the "Polyethylene Particles" column of Tables 1 to 3. The amount (dry mass) of "Chemipearl (registered trademark)" added is shown in parentheses in the "Polyethylene Particles" column.
[0170] (2) Preparation of the substrate The substrate materials were fed into an extrusion molding machine (T-die extrusion molding machine equipped with a twin screw, φ20 mm, L / D=25) in the ratios shown in the "Substrate" section of Tables 1 to 3, kneaded at a temperature of 220°C or less, and then formed into a sheet using a T-die at a molding temperature of 220°C. The sheet was then biaxially stretched (3.5 times vertically x 5 times horizontally) while being taken up by a take-up machine, to obtain a sheet-shaped substrate (128 mm vertically x 80 mm horizontally, 200 μm thick).
[0171] (3) Coating of the Coating Layer Acrylic polymer, clay, ground calcium carbonate, and polyethylene particles were mixed with a dispersion medium (water) in the proportions shown in the "Coat Layer" section of Tables 1 to 3, and stirred at 3000 rpm for 3 minutes using an edged turbine to obtain an aqueous emulsion. The obtained aqueous emulsion was applied to the entire surface of one side of each substrate by the microgravure method, and then dried at 110°C to obtain a substrate (corresponding to an election ballot paper) provided with a coating layer (film thickness 4 μm). The numerical values for the composition of the "coat layer" in the table are values of dry mass.
[0172] (4) Halftone printing For some of the obtained election ballot papers, a halftone dot print was made using offset ink (oil-based, blue) on the entire surface of the coating layer by offset printing. The dot percentage for the halftone printing area was set to 30%. The offset printing machine used was "RMGT920" (manufactured by Ryobi MHI Graphic Technology Co., Ltd.).
[0173] <Evaluation of Election Ballots> Various measurements and evaluations were carried out on each election ballot paper using the following methods. The results are shown in the "Results" section of the table.
[0174] (1) Physical property measurements The following physical properties were measured for the surface of each coating layer. -Static friction coefficient according to JIS P8147:2010 Dynamic friction coefficient according to JIS P8147:2010 ·Arithmetic mean height according to JIS B0601:2001 In addition, the following physical properties of the election ballots were measured: ·Opacity according to JIS P 8149:2000
[0175] (2) Variation in paper feedability Using a commercially available ballot counting machine, the passability of the election ballots was evaluated with reference to the method described in JP 2008-307835 A. Specifically, five sets of double-ply election ballots were created by applying a very light amount of glue to the center of the election ballot and then stacking another election ballot on top of it. The election ballots (500 in total), including these double-ply election ballots, were counted using the above-mentioned counting machine, and the number of election ballots that could not be counted properly was identified.
[0176] The above series of steps was performed 10 times (10 lots) for each election ballot, and the average number of election ballots that could not be counted correctly was calculated using the following formula. Average number of election ballots that were not properly counted (number of ballots) = Total number of election ballots that were not properly counted / 10
[0177] For each election ballot, the variability of threadability was evaluated based on the average number of election ballots that could not be counted properly, using the following criteria: A: The average number of election ballots that could not be counted properly was less than one. B: The average number of election ballots that could not be counted properly was between two and three. C: The average number of election ballots that could not be counted properly was four or more.
[0178] [Table 1]
[0179] [Table 2]
[0180] [Table 3]
[0181] As shown in the table, election ballots meeting the requirements of the present invention had reduced variability in feedability.
[0182] In each of the above examples, when ground calcium carbonate that had been surface-treated with a higher fatty acid was used as the ground calcium carbonate blended in the coating layer, better effects tended to be achieved.
[0183] In this example, the amount of polyethylene particles blended into the coating layer was set to 2.0% by mass relative to the coating layer, but it was found that a range of 1.0% by mass or more and 20.0% by mass or less is preferable from the viewpoint of stably suppressing variations in paper feed performance.
[0184] Although no data is shown, when the volume average particle diameter of the kaolin clay is within the range of 0.05 μm or more and 2.00 μm or less, appropriate roughness due to the polyethylene particles is easily generated, and further, the printability, etc. of the coating layer tends to be stable.
[0185] In this example, the presence or absence of a halftone dot printed portion did not have a significant effect on suppressing variations in paper feed performance. From the viewpoint of not impairing the effects of the present invention, it was confirmed that the halftone dot percentage of the halftone dot printed portion is preferably in the range of 10% to 50%.
[0186] None of the election ballots in this example contain any pigment. However, it was confirmed that the effect of the present invention is not significantly affected if the total amount of pigment contained in the substrate and coating layer is 0.1% by mass or less relative to the substrate and coating layer.
Claims
1. An election ballot paper comprising a substrate and a coating layer provided on one or both sides of the substrate, the coating layer comprises a continuous phase made of an acrylic polymer, clay, ground calcium carbonate, and polyethylene particles; The content of the clay is 25% by mass or more and 55% by mass or less with respect to the coating layer, The content of the ground calcium carbonate is 5% by mass or more and 30% by mass or less with respect to the coating layer, The volume average particle size of the ground calcium carbonate is 0.05 μm or more and 2.00 μm or less, The particle size of the polyethylene particles in accordance with JIS Z8832:2010 is 8.0 μm or more and 11.0 μm or less, The density of the polyethylene particles according to JIS K6922-2 is 950 kg / m 3 More than 1000kg / m 3 is as follows: The coating layer has a static friction coefficient in accordance with JIS P8147:2010 of 0.30 or more and 0.50 or less, The coating layer has a dynamic friction coefficient in accordance with JIS P8147:2010 of 0.20 or more and 0.35 or less, The coating layer has an arithmetic mean height in accordance with JIS B0601:2001 of 0.50 μm or more and 0.90 μm or less, The total content of the dye contained in the substrate and the coating layer is 0.1% by mass or less with respect to the substrate and the coating layer. Election ballot paper.
2. The election ballot paper according to claim 1 , wherein at least a portion of the surface of the coating layer is provided with a halftone dot printed portion using offset ink.
3. 3. The election ballot paper according to claim 2, wherein the halftone dot percentage of the halftone dot printed portion is between 10% and 50%.
4. The election ballot paper according to claim 1 or 2, wherein the base material comprises a thermoplastic resin and an inorganic substance powder in a mass ratio of 50:50 to 10:
90.
5. 5. The election ballot of claim 4, wherein the thermoplastic resin is a polypropylene-based resin.
6. 2. The election ballot of claim 1, wherein the ground calcium carbonate is a surface-treated ground calcium carbonate.
7. 5. The election ballot paper according to claim 4, wherein the volume average particle size of the clay is 0.05 μm or more and 2.00 μm or less.
8. 5. The election ballot of claim 4, wherein the acrylic polymer is a (meth)acrylic acid alkyl ester copolymer.
9. The (meth)acrylic acid alkyl ester copolymer is one or more selected from the group consisting of methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, isooctyl acrylate, nonyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, 2-hydroxymethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, and 2-hydroxypropyl methacrylate. The election ballot paper of claim 8.
10. 3. The election ballot paper according to claim 1 or 2, having an opacity of 95% or more in accordance with JIS P 8149:2000.
11. A step of obtaining a substrate by extrusion molding a resin composition containing a polyolefin resin and an inorganic substance powder in a mass ratio of 50:50 to 10:90; A step of applying an aqueous emulsion containing an acrylic polymer, clay, ground calcium carbonate, and polyethylene particles to one or both sides of the substrate and drying the emulsion to provide a coating layer; The content of the clay is 25% by mass or more and 55% by mass or less with respect to the coating layer, The content of the ground calcium carbonate is 5% by mass or more and 30% by mass or less with respect to the coating layer, The volume average particle size of the ground calcium carbonate is 0.05 μm or more and 2.00 μm or less, The particle size of the polyethylene particles in accordance with JIS Z8832:2010 is 8.0 μm or more and 11.0 μm or less, The density of the polyethylene particles according to JIS K6922-2 is 950 kg / m 3 More than 1000kg / m 3 is as follows: The coating layer has a static friction coefficient in accordance with JIS P8147:2010 of 0.30 or more and 0.50 or less, The coating layer has a dynamic friction coefficient in accordance with JIS P8147:2010 of 0.20 or more and 0.35 or less, The coating layer has an arithmetic mean height in accordance with JIS B0601:2001 of 0.50 μm or more and 0.90 μm or less, The total content of the dye contained in the substrate and the coating layer is 0.1% by mass or less with respect to the substrate and the coating layer. How election ballots are manufactured.
12. The method according to claim 11 , wherein the substrate is biaxially stretched after extrusion.
Citation Information
Patent Citations
Election ballot paper and its manufacturing method
JP7049733B1