Toner, image formation device, image formation method, and method for manufacturing printed matter

A toner with amorphous polyester resin, wax, and hydrophobically treated silica additives addresses the challenge of low-temperature fixability and heat-resistant storage stability, ensuring charging stability and preventing abnormal images.

JP2024163517APending Publication Date: 2024-11-22RICOH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023079209
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The challenge lies in achieving both low-temperature fixability and heat-resistant storage stability in toners while maintaining charging stability and preventing abnormal images, especially when titanium oxide is not used as an external additive.

Method used

A toner formulation containing an amorphous polyester resin, wax, and external additives, where the external additive is silica partially coated with a hydroxide of a metal element, with a hydrophobicity of 55% (MeOH%) or more, and optimized circularity and volume resistivity.

Benefits of technology

The toner achieves both low-temperature fixability and heat-resistant storage stability, ensuring charging stability and preventing abnormal images, thereby enhancing image quality and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163517000006
    Figure 2024163517000006
  • Figure 2024163517000007
    Figure 2024163517000007
  • Figure 2024163517000008
    Figure 2024163517000008
Patent Text Reader

Abstract

To provide a toner which achieves both low temperature fixability and heat resistant storage property, and achieves charge stability and suppression of an abnormal image.SOLUTION: A toner contains an amorphous polyester resin, a wax and an external additive, wherein at least a part of the external additive contains silica coated with a hydroxide of a metallic element, and a degree of hydrophobicity of the silica is 55 (MeOH%) or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner, an image forming apparatus, an image forming method, and a method for producing a printed matter. [Background technology]

[0002] In recent years, in order to suppress volatile fine particles in addition to the conventional energy saving, it is important to improve the low-temperature fixability of toner, but it is also necessary to achieve a high-temperature storage stability. It is also important to maintain a stable charge level for a long period of time and maintain image quality. From this perspective, not only the design of the toner base formulation but also the selection of external additives is important. On the other hand, there has been a trend in recent years to adopt safer materials, and there has been a search for external additives to replace the titanium oxide that has been used traditionally.

[0003] Patent Document 1 describes that excellent image density, charge amount, and charge stability can be achieved by using aluminum hydroxide, an external additive treated with an organic substance, and silica particles in combination. Patent Document 2 describes that a toner with high long-term environmental charging performance can be realized by using a composition made of aluminum hydroxide and silica, a fine powder whose surface has been silane-treated, and small-particle silica having an average primary particle size smaller than that of the fine powder. Summary of the Invention [Problem to be solved by the invention]

[0004] If titanium oxide is not used, it becomes difficult to control the charge amount, and it becomes difficult to ensure a stable charge amount over a long period of use. In addition, changes in the physical properties of the external additives may lead to the occurrence of abnormal images due to poorly cleaned toner. An object of one embodiment of the present invention is to provide a toner which has both low-temperature fixability and heat-resistant storage stability, and which achieves charge stability and suppression of abnormal images. [Means for solving the problem]

[0005] In order to solve the above problem, one embodiment of the present invention is A toner comprising an amorphous polyester resin, a wax, and an external additive, The external additive contains silica at least a part of which is coated with a hydroxide of a metal element, The toner has a hydrophobicity of the silica of 55 (MeOH%) or more. Effect of the Invention

[0006] According to one embodiment of the present invention, it is possible to provide a toner which achieves both low-temperature fixability and heat-resistant storage stability, and which achieves charge stability and suppression of abnormal images. [Brief description of the drawings]

[0007] [Figure 1] 1 is a schematic diagram illustrating an example of a portion of an image forming apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 4 is a schematic diagram showing another example of a portion of an image forming apparatus according to an embodiment of the present invention. [Diagram 3] 1 is a schematic diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram showing another example of a portion of an image forming apparatus according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The embodiments of the present invention will be described in detail below.

[0009] (toner) The present invention relates to A toner comprising an amorphous polyester resin, a wax, and an external additive, The external additive contains silica at least a part of which is coated with a hydroxide of a metal element, The toner has a hydrophobicity of the silica of 55 (MeOH%) or more.

[0010] The toner of the present invention can achieve both low-temperature fixability and heat-resistant storage stability, and can also realize charge stability and suppression of abnormal images.

[0011] The toner preferably has an average circularity of 0.930 to 0.960. When the average circularity is in the above range, it is easy to achieve both transferability and cleanability in an appropriate range.

[0012] The average circularity of the toner can be measured using a known particle measuring device, for example, a wet flow type particle size / shape analyzer FPIA-3000 and analysis software FPIA-3000 Data Processing Program for FPIA version 00-10 (manufactured by Sysmex Corporation). Specifically, for example, 0.1 to 0.5 mL of a 10% aqueous solution of alkylbenzene sulfonate Neogen SC-A (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and 0.1 to 0.5 g of toner or toner base particles are added to a 100 mL glass beaker, and then the mixture is stirred with a micro spatula and 80 mL of ion-exchanged water is added. Next, the mixture is dispersed at 20 kHz, 50 W / 10 cm using an ultrasonic disperser UH-50 (manufactured by SMT Co., Ltd.). 3 After dispersing for 1 minute under the above conditions, the sample is dispersed for a total of 5 minutes to obtain a measurement sample. -3 cm 3 Using the measurement sample, the average circularity of particles having a circle-equivalent diameter in the desired range can be measured. The average circularity of the toner particles may be determined by the average circularity of the base particles of the toner.

[0013] The toner preferably further contains a crystalline polyester resin and / or an aromatic petroleum resin. The toner contains a crystalline polyester resin, so that good low-temperature fixability can be ensured. Furthermore, by containing an aromatic petroleum resin, the toner can have improved grindability and improved heat resistance while maintaining low-temperature fixability.

[0014] <External additives> The toner of the present invention contains an external additive, and thus the wax in the toner is covered with the external additive, thereby suppressing the deterioration of transferability and durability caused by the wax. In addition, the toner surface is covered with fine particles of the external additive, thereby reducing the contact area between the resin particles contained in the toner particles, thereby improving the fluidity, storage stability, developability, transferability, and durability of the toner.

[0015] The external additive contained in the toner of the present invention contains silica (hereinafter, sometimes referred to as "silica") at least a part of which is covered with a hydroxide of a metal element. By containing such silica as an external additive in the toner, it is possible to ensure charging stability and suppress the occurrence of abnormal images.

[0016] The hydrophobicity of the silica at least partially coated with a hydroxide of a metal element is 55 (MeOH%) or more. If the hydrophobicity of the silica is less than 55 (MeOH%), the silica cannot have an appropriate cleaning performance, and abnormal images are likely to occur.

[0017] The degree of hydrophobicity can be measured, for example, by the following method. First, 50 ml of ion-exchanged water and 0.2 g of sample are placed in a beaker, and methanol is added dropwise while stirring. As the methanol concentration in the beaker increases, the sample gradually sinks, and the mass fraction of methanol in the mixed solution of methanol and water at the end point when the entire sample has sunk is taken as the degree of hydrophobicity (MeOH%).

[0018] The silica at least partially coated with a hydroxide of a metal element preferably has a volume resistivity of 1.0E+11 (Ω·cm) or less. When the volume resistivity of the silica is 1.0E+11 (Ω·cm) or less, charging stability can be maintained at a higher level.

[0019] The volume resistivity can be measured, for example, by the following method. First, in a cell consisting of a fluororesin container containing two electrodes with a surface area of ​​2.5 cm x 4 cm spaced 0.2 cm apart, a measurement sample is filled between the two electrodes, and tapped 10 times at a drop height of 1 cm and a tapping speed of 30 times / min. Next, a DC voltage of 1,000 V is applied between the two electrodes filled with the measurement sample, and the resistance value r [Ω] after 30 seconds is measured using a high resistance meter 4329A (manufactured by Yokogawa Hewlett-Packard Co., Ltd.). The volume resistivity [Ω·cm] of the sample can be calculated by inputting the measured resistance value r into the following formula: (Formula) r×(2.5×4) / 0.2

[0020] It is preferable that at least a part of the silica at least partly coated with a hydroxide of a metal element is coated with an alkylsilane, which makes it easy to achieve both a certain level of hydrophobicity and a certain level of volume resistivity, thereby maintaining a higher level of charging stability and suppression of abnormal images.

[0021] The hydroxide of the metal element is preferably at least one hydroxide of aluminum, zinc, iron and magnesium, since the hydroxide of these metal elements makes it easy to control the volume resistivity of the silica within a desired range.

[0022] The average particle size of the silica at least partially coated with a hydroxide of a metal element is preferably 10 nm to 30 nm. By having the average particle size of the silica in the above range, the coating state of the toner surface can be optimized, and it becomes easier to achieve both low-temperature fixability and heat-resistant storage stability. Note that the average particle size of the silica coated with a hydroxide of a metal element may be the average primary particle size of the silica particles before being coated with the hydroxide of a metal element.

[0023] The average primary particle diameter of the silica particles can be determined, for example, by obtaining an SEM image of the silica particles using a field emission scanning electron microscope (SU8230, manufactured by Hitachi High-Technologies Corporation) and measuring the number average particle diameter by image analysis. Specifically, for example, a silica particle sample is dispersed in tetrahydrofuran, the solvent is removed on a substrate, the sample is dried, and the sample is observed with the above-mentioned SEM to obtain an image, and the maximum length of the primary particle of each particle is measured under the following measurement conditions. The average value of 50 particles is calculated to obtain the average primary particle diameter of the silica particles. [SEM measurement conditions] Accelerating voltage: 2.0 kV WD(Working Distance):5.0mm Observation magnification: 100,000 times

[0024] The toner of the present invention may contain other fine particles as an external additive in addition to the silica at least a part of which is coated with a hydroxide of a metal element.

[0025] As the other fine particles, one or more of inorganic fine particles, inorganic oxide fine particles, and resin fine particles may be used. The inorganic fine particles, inorganic oxide fine particles, and resin fine particles each preferably have an average primary particle diameter of 5 nm to 2 μm. The content of the other fine particles in the toner varies depending on the type, but is preferably in the range of 0.01 to 5% by mass of the toner particles. The other fine particles preferably have a surface that has been subjected to a hydrophobic treatment, and fine particles of an inorganic oxide such as silica that has been subjected to a hydrophobic treatment are preferably used.

[0026] Examples of the inorganic fine particles include silica, alumina, barium titanate, magnesium titanate, calcium titanate, strontium titanate, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, pengallo, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, silicon nitride, etc. These may be used alone or in combination of two or more.

[0027] Examples of the resin fine particles include resin fine particles made of polystyrene, methacrylate or acrylate copolymers, silicone, benzoguanamine, nylon, or the like obtained by soap-free emulsion polymerization, suspension polymerization, or dispersion polymerization, or polymer particles made of a thermosetting resin.

[0028] The hydrophobic treatment agent used in the hydrophobic treatment is not particularly limited and can be appropriately selected depending on the purpose. Examples of the hydrophobic treatment agent include dimethyldichlorosilane, trimethylchlorosilane, methyltrichlorosilane, allyldimethyldichlorosilane, allylphenyldichlorosilane, benzyldimethylchlorosilane, bromomethyldimethylchlorosilane, α-chloroethyltrichlorosilane, p-chloroethyltrichlorosilane, chloromethyldimethylchlorosilane, chloromethyltrichlorosilane, p-Chlorophenyltrichlorosilane, 3-chloropropyltrichlorosilane, 3-chloropropyltrimethoxysilane, vinyltriethoxysilane, vinylmethoxysilane, vinyl-tris(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, vinyltriacetoxysilane, divinyldichlorosilane, dimethylvinylchlorosilane, octyl-trichlorosilane, decyl-trichlorosilane, nonyl-trichlorosilane, (4-t-propylphenyl (4-t-butylphenyl)-trichlorosilane, dipentyl-dichlorosilane, dihexyl-dichlorosilane, dioctyl-dichlorosilane, dinonyl-dichlorosilane, didecyl-dichlorosilane, didodecyl-dichlorosilane, dihexadecyl-dichlorosilane, (4-t-butylphenyl)-octyl-dichlorosilane, dioctyl-dichlorosilane, didecenyl-dichlorosilane, dinonenyl-dichlorosilane, di-2-ethylhexyl-dic Examples of the chlorosilane include dichlorosilane, di-3,3-dimethylpentyl-dichlorosilane, trihexyl-chlorosilane, trioctyl-chlorosilane, tridecyl-chlorosilane, dioctyl-methyl-chlorosilane, octyl-dimethyl-chlorosilane, (4-t-propylphenyl)-diethyl-chlorosilane, octyltrimethoxysilane, hexamethyldisilazane, hexaethyldisilazane, diethyltetramethyldisilazane, hexaphenyldisilazane, and hexatlyldisilazane. In addition, titanate-based coupling agents and aluminum-based coupling agents can also be used.

[0029] A general powder mixer is used to mix the above-mentioned external additive and toner base particles, but a mixer equipped with a jacket or the like so that the internal temperature can be adjusted is preferred. For example, a V-type mixer, a rocking mixer, a Loedige mixer, a Nauta mixer, a Henschel mixer, or the like is preferably used.

[0030] The inorganic fine particles, inorganic oxide fine particles, and resin fine particles may be contained (internal added) in the toner. By adding the inorganic fine particles, inorganic oxide fine particles, and resin fine particles internally to the toner, the effect of improving transferability and durability can be obtained, and the grindability of the toner can be improved. In addition, by using both external and internal addition, the externally added inorganic fine particles and resin fine particles can be prevented from being embedded inside the toner, so that excellent transferability can be stably obtained and durability is also improved.

[0031] <Amorphous polyester resin> The amorphous polyester resin contained in the toner of the present invention is not particularly limited and any known one can be used, but it is preferable that the toner contains at least bisphenol A and ethylene glycol as diol components. By containing bisphenol A as the diol component, the toner can have good heat resistance. In addition, by containing ethylene glycol as the diol component, the toner can maintain good dispersibility with a wax having a low SP value. As a result, the durability of the toner can be improved.

[0032] As the monomer unit constituting the amorphous polyester resin, a monomer unit of a dihydric alcohol may be used in addition to bisphenol A and ethylene glycol. Examples of the dihydric alcohol include propylene glycol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, diethylene glycol, triethylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 2-ethyl-1,3-hexanediol, hydrogenated bisphenol A, and diols obtained by polymerizing cyclic ethers such as ethylene oxide and propylene oxide with bisphenol A.

[0033] Further, as a means for crosslinking the amorphous polyester resin, it is also possible to use a polyhydric alcohol having a valence of three or more in combination. Examples of the trihydric or higher polyhydric alcohol include sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, such as dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentatriol, glycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxybenzene.

[0034] Examples of the acid component that forms the amorphous polyester resin include benzenedicarboxylic acids such as phthalic acid, isophthalic acid, and terephthalic acid, or their anhydrides; alkyldicarboxylic acids such as succinic acid, adipic acid, sebacic acid, and azelaic acid, or their anhydrides; unsaturated dibasic acids such as maleic acid, citraconic acid, itaconic acid, alkenylsuccinic acid, fumaric acid, and mesaconic acid; and unsaturated dibasic acid anhydrides such as maleic anhydride, citraconic anhydride, itaconic anhydride, and alkenylsuccinic anhydride.

[0035] Furthermore, as the acid component that forms the amorphous polyester resin, a polyvalent carboxylic acid having a valence of three or more can also be used. Examples of such a polyvalent carboxylic acid include trimellitic acid, pyromellic acid, 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxy-2-methyl-2-methylenecarboxypropane, tetra(methylenecarboxy)methane, 1,2,7,8-octanetetracarboxylic acid, and EMPO trimer acid, as well as anhydrides and partial lower alkyl esters thereof.

[0036] The acid value of the amorphous polyester resin is preferably 0.1 mgKOH / g to 100 mgKOH / g, more preferably 0.1 mgKOH / g to 70 mgKOH / g, and even more preferably 0.1 mgKOH / g to 50 mgKOH / g. In the present invention, the molecular weight distribution of the amorphous polyester resin can be measured by gel permeation chromatography (GPC) using THF as a solvent.

[0037] <Crystalline polyester resin> The toner of the present invention preferably further contains a crystalline polyester resin, which can provide better low-temperature fixability.

[0038] The melting point of the crystalline polyester resin is preferably 100 to 120° C. When the melting point of the crystalline polyester resin is 100° C. or higher, the glass transition temperature of a non-crystallized portion present in the crystalline polyester resin increases in accordance with the melting point, and the glass transition temperature of the non-crystallized portion becomes closer to the glass transition temperature of the amorphous polyester resin, increasing compatibility and improving low-temperature fixability. When the melting point of the crystalline polyester resin is 120° C. or lower, the melting due to the amount of heat during fixing is sufficient, so that low-temperature fixability can be easily ensured.

[0039] The crystalline polyester resin is (I) a polycarboxylic acid consisting of a linear unsaturated aliphatic dicarboxylic acid or a reactive derivative thereof (such as an acid anhydride, a lower alkyl ester having 1 to 4 carbon atoms, or an acid halide); (II) a polyhydric alcohol consisting of a linear aliphatic diol; can be produced by subjecting the above to a polycondensation reaction in a conventional manner. If necessary, a small amount of another polycarboxylic acid can be added to the polycarboxylic acid (I).

[0040] Examples of the other polyvalent carboxylic acids include (i) Branched unsaturated aliphatic dicarboxylic acid (ii) Saturated aliphatic dicarboxylic acids and saturated aliphatic polycarboxylic acids such as saturated aliphatic tricarboxylic acids (iii) Aromatic polycarboxylic acids such as aromatic dicarboxylic acids and aromatic tricarboxylic acids etc.

[0041] The amount of the other polycarboxylic acids (i) to (iii) added is usually 30 mol % or less, and preferably 10 mol % or less, based on the amount of the polycarboxylic acid (I), and can be appropriately adjusted and added within the range in which the resulting polyester resin has crystallinity.

[0042] Specific examples of the other polyvalent carboxylic acids include divalent carboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, sebacic acid, citraconic acid, phthalic acid, isophthalic acid, and terephthalic acid; and trivalent or higher polyvalent carboxylic acids such as trimellitic anhydride, 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-cyclohexanetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methylenecarboxypropane, and 1,2,7,8-octanetetracarboxylic acid.

[0043] If necessary, a small amount of other polyhydric alcohols can be added to the polyhydric alcohol (II), and in addition to aliphatic branched-chain dihydric alcohols and cyclic dihydric alcohols, polyhydric alcohols having a valence of three or more can be added.

[0044] The amount of the other polyhydric alcohol added is 30 mol % or less, preferably 10 mol % or less, based on the amount of the polyhydric alcohol (II), and can be appropriately adjusted within the range in which the resulting polyester has crystallinity.

[0045] Examples of the other polyhydric alcohols include 1,4-bis(hydroxymethyl)cyclohexane, polyethylene glycol, bisphenol A ethylene oxide adduct, bisphenol A propylene oxide adduct, and glycerin.

[0046] The crystalline polyester resin preferably has a sharp peak in its molecular weight distribution from the viewpoint of low-temperature fixability, and the molecular weight is preferably relatively low. The molecular weight of the crystalline polyester resin is preferably in the range of a weight average molecular weight (Mw) of 5,500 to 6,500, a number average molecular weight (Mn) of 1,300 to 1,500, and an Mw / Mn ratio of 2 to 5 in the molecular weight distribution of the o-dichlorobenzene soluble matter by gel permeation chromatography (GPC).

[0047] The molecular weight distribution of the crystalline polyester resin is based on a molecular weight distribution diagram with logM (M is molecular weight) on the horizontal axis and mass% on the vertical axis. In the case of the crystalline polyester resin used in the present invention, the molecular weight distribution diagram preferably has a maximum value of the molecular weight peak in the range of 3.5 to 4.0 (mass%), and the half-value width of the maximum value of the peak is preferably 1.5 or less.

[0048] The content of the crystalline polyester resin in the toner base particles is preferably 5.0% by mass or less. By setting the content of the crystalline polyester resin in the toner base particles to 5.0% by mass or less, adhesion to the photoreceptor due to recrystallization after toner formation can be suppressed, and image blurring can be suppressed.

[0049] <Aromatic petroleum resin> The toner of the present invention preferably contains an aromatic petroleum resin. By containing an aromatic petroleum resin, it is possible to improve the grindability of the toner and to improve the heat resistance while maintaining the low-temperature fixability. The aromatic petroleum resin is a resin synthesized using styrene, vinyltoluene, indene, etc., which are C9 fractions of petroleum, as raw materials. In particular, styrene-based copolymers of styrene or α-methylstyrene are preferred.

[0050] The weight average molecular weight of the aromatic petroleum resin is preferably from 2000 to 3500. When the weight average molecular weight is 2000 or more, durability in an actual machine can be easily ensured, and when the weight average molecular weight is 3500 or less, good toner grindability can be easily ensured.

[0051] The styrene-based copolymer is not particularly limited, but examples thereof include styrene and its substitute polymers such as polystyrene, poly-p-styrene, and polyvinyltoluene, styrene-α-methylstyrene copolymer, styrene-p-chlorostyrene copolymer, styrene-propylene copolymer, styrene-vinyltoluene copolymer, styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer, styrene-butyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-ethyl methacrylate copolymer, styrene-butyl methacrylate copolymer, styrene-α-chloromethyl methacrylate copolymer, styrene-acrylonitrile copolymer, styrene-vinyl methyl ether copolymer, styrene-vinyl methyl ketone copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-maleic acid copolymer, and styrene-maleic acid ester copolymer. Among them, it is particularly preferable to contain a styrene-α-methylstyrene copolymer.

[0052] The glass transition temperature (Tg) of the styrene copolymer is preferably 60° C. or higher, and more preferably 65 to 85° C. When the Tg of the styrene resin is 60° C. or higher, the heat-resistant storage stability can be improved. The Tg can be measured using a differential scanning calorimeter (Q-200, manufactured by TA Instruments). As a specific measurement method, for example, about 5.0 mg of the target sample is placed in an aluminum sample container, the sample container is placed on a holder unit, and set in an electric furnace, and the temperature is raised from -80°C to 150°C at a rate of 10°C / min in a nitrogen atmosphere to obtain a DSC curve. From the obtained DSC curve, the glass transition temperature (Tg) of the target sample is determined using an analysis program in the differential scanning calorimeter.

[0053] When the toner of the present invention contains an aromatic petroleum resin and the crystalline polyester, the mass ratio of the crystalline polyester to the aromatic petroleum resin is preferably 1.0 or more and 1.2 or less. The aromatic petroleum resin disperses in the toner to improve the grindability of the toner, but has a certain glass transition temperature or higher, and therefore may impair low-temperature fixability. On the other hand, the crystalline polyester resin improves low-temperature fixability, but may impair the grindability of the toner due to the presence of a crystallized portion. In addition, since the crystalline polyester resin is generally partially compatible with the amorphous polyester resin, the proportion of the crystallized portion in the toner may be slightly less than the amount added to the toner. Therefore, when the toner of the present invention contains an aromatic petroleum resin and the crystalline polyester, it is preferable that the mass proportions of both materials in the toner be approximately the same in order to appropriately bring out the respective effects of both materials. When the mass ratio of the crystalline polyester to the aromatic petroleum resin is within the above range, the effects of both materials, which have opposing effects on the toner grindability and low-temperature fixability, can be appropriately brought out, and the toner grindability and low-temperature fixability can be achieved at a high level.

[0054] The content of the aromatic petroleum resin in the toner base particles is preferably 3.0% by mass or more. By making the content of the aromatic petroleum resin in the toner base particles 3.0% by mass or more, it is possible to improve the wax dispersibility and improve the durability while maintaining a certain level of toner grindability.

[0055] <Wax> The wax contained in the toner of the present invention is not particularly limited, and can be appropriately selected from known waxes. Examples of waxes include natural waxes such as vegetable waxes such as carnauba wax, cotton wax, wood wax, and rice wax; animal waxes such as beeswax and lanolin; mineral waxes such as ozokerite and cerusin; and petroleum waxes such as paraffin, microcrystalline, and petrolatum. In addition to these natural waxes, synthetic hydrocarbon waxes such as Fischer-Tropsch wax, polyethylene, and polypropylene; synthetic waxes such as esters, ketones, and ethers; and the like can also be used.

[0056] Further, fatty acid amide compounds such as 12-hydroxystearic acid amide, stearic acid amide, phthalimide anhydride, and chlorinated hydrocarbons; homopolymers or copolymers of polyacrylates such as poly-n-stearyl methacrylate and poly-n-lauryl methacrylate, which are low molecular weight crystalline polymer resins (for example, copolymers of n-stearyl acrylate and ethyl methacrylate); and crystalline polymers having long alkyl groups in their side chains may be used. Among these, hydrocarbon waxes such as paraffin wax, microcrystalline wax, Fischer-Tropsch wax, polyethylene wax, and polypropylene wax are preferred.

[0057] The melting point of the wax is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 60° C. or higher and lower than 95° C. When the melting point of the wax is 60° C. or higher, the release agent is unlikely to melt at low temperatures, and the heat-resistant storage stability of the toner can be maintained.When the melting point of the wax is lower than 95° C., the release agent is sufficiently melted by heating during fixing, and sufficient offset properties can be obtained.

[0058] The wax is preferably a hydrocarbon wax. Hydrocarbon waxes are preferred because they have almost no compatibility with the amorphous polyester resin and the crystalline polyester resin and can function independently of each other, and therefore do not impair the softening effect of the crystalline polyester resin as a binder resin or the offset property of the release agent.

[0059] The wax is more preferably a hydrocarbon wax having a melting point of 60°C or higher and lower than 95°C. A hydrocarbon wax with a melting point of 60°C or higher and lower than 95°C can effectively act as a release agent between the fixing roller and the toner interface, thereby improving high-temperature offset resistance without applying a release agent such as oil to the fixing roller.

[0060] The content of the wax in the toner is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 2% by mass to 10% by mass, and more preferably 3% by mass to 8% by mass, in the toner. When the wax content in the toner is 2% by mass or more, high-temperature offset resistance and low-temperature fixability during fixing can be exhibited, and when it is 10% by mass or less, heat-resistant storage stability can be maintained and image fogging, etc. can be prevented from occurring. When the wax content is within the above range, high image quality and fixing stability can be further improved.

[0061] <Coloring agent> The toner of the present invention preferably contains a colorant. As the colorant used in the toner of the present invention, all known dyes and pigments can be used. For example, carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ochre, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, anthrazan yellow BGL, isoindolinone yellow, red iron oxide, red lead, vermilion, kaolin, etc. Domium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachlor Orthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Carmine BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Permanent Red F5R, Brilliant Carmine 6B, Pogment Scarlet Red 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkaline Blue Lake, Peacock Couleur Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake,Malachite green lake, phthalocyanine green, anthraquinone green, titanium oxide, zinc oxide, lithopone, and mixtures thereof. The content of the colorant in the toner is preferably from 1 to 15% by mass, and more preferably from 3 to 10% by mass.

[0062] In the production of the toner, a master batch in which the colorant is mixed with a resin may be used. The resin kneaded with the colorant to prepare the master batch may be the same as the resin described above. The resin kneaded with the colorant may be used alone or in combination of two or more.

[0063] The master batch can be obtained by mixing and kneading the resin and colorant for preparing the master batch with high shear force. In this case, an organic solvent can be used to enhance the interaction between the colorant and the resin. In addition, a method called a flushing method can be used in which an aqueous paste of a colorant containing water is mixed and kneaded with a resin and an organic solvent, the colorant is transferred to the resin side, and the water and organic solvent components are removed. According to the flushing method, the wet cake of the colorant can be used as it is, so there is no need to dry it, and it can be used preferably. For mixing and kneading in the flushing method, a high shear dispersing device such as a three-roll mill is preferably used. The amount of the master batch used is preferably 0.1 to 20 parts by mass with respect to 100 parts by mass of the resin.

[0064] In preparing the master batch, it is preferable to disperse the colorant in a resin. The resin for preparing the master batch preferably has an acid value of 30 mgKOH / g or less and an amine value of 1 to 100, and more preferably has an acid value of 20 mgKOH / g or less and an amine value of 10 to 50. When the resin for preparing the master batch has an acid value of 30 mgKOH / g or less, the chargeability does not decrease even under high humidity conditions, and the dispersibility of the colorant is sufficient, and when the amine value is 1 to 100, the dispersibility of the colorant is sufficient. The acid value of the resin for preparing the master batch can be measured by the method described in JIS K0070, and the amine value can be measured by the method described in JIS K7237.

[0065] A dispersant can be used to improve the dispersibility of the colorant. From the viewpoint of the dispersibility of the colorant, the dispersant preferably has high compatibility with the resin. Examples of the dispersant include commercially available products such as "Ajisper PB821" and "Ajisper PB822" (manufactured by Ajinomoto Fine-Techno Co., Ltd.), "Disperbyk-2001" (manufactured by BYK-Chemie Co., Ltd.), and "EFKA-4010" (manufactured by EFKA Co., Ltd.).

[0066] From the viewpoint of dispersibility of the colorant, the mass average molecular weight of the dispersant is preferably 500 to 100,000, more preferably 3,000 to 100,000, further more preferably 5,000 to 50,000, and particularly preferably 5,000 to 30,000, as the molecular weight of the maximum value of the main peak in styrene-equivalent mass in gel permeation chromatography. When the molecular weight is 500 or more, the polarity is not too high and the dispersibility of the colorant is not easily reduced, and when it is 100,000 or less, the affinity with the solvent is not too high and the dispersibility of the colorant is not easily reduced.

[0067] The dispersant is preferably blended in the toner in a ratio of 0.1 to 10% by mass relative to the colorant. When the blending ratio of the dispersant is 0.1% by mass or more of the colorant, the dispersibility of the colorant becomes sufficient, and when the blending ratio is 10% by mass or less, the chargeability is less likely to decrease under high humidity conditions.

[0068] <Charge control agent> The toner of the present invention may contain a charge control agent as necessary. Any known charge control agent can be used, but in color toners, white or light-colored ones are preferred. When using a colored charge control agent, the content is preferably small in order to prevent the toner from being mixed with the color and becoming dull.

[0069] Examples of the charge control agent include nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus simple substances or compounds, tungsten simple substances or compounds, fluorine-based activators, metal salicylic acid salts, and metal salts of salicylic acid derivatives. Specifically, for example, the nigrosine dye Bontron 03, the quaternary ammonium salt Bontron P-51, the metal-containing azo dye Bontron S-34, the oxynaphthoic acid metal complex E-82, the salicylic acid metal complex E-84, the phenol condensate E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), the quaternary ammonium salt molybdenum complexes TP-302 and TP-415 (all manufactured by Hodogaya Chemical Co., Ltd.), the quaternary ammonium salt Copy Charge PSY VP2038, the triphenylmethane derivative Copy Blue PR, the quaternary ammonium salt Copy Charge NEG VP2036, and Copy Charge NX. Examples of suitable pigments include VP434 (all manufactured by Hoechst), LRA-901, the boron complex LR-147 (manufactured by Nippon Carlit), copper phthalocyanine, perylene, quinacridone, azo pigments, and other polymeric compounds having functional groups such as sulfonic acid groups, carboxyl groups, and quaternary ammonium salts.

[0070] The charge control agent can be melt-kneaded together with the resin, the release agent, and the master batch. The amount of the charge control agent used is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 5 parts by mass, per 100 parts by mass of the resin. When the amount of the charge control agent used is within the above range, the chargeability of the toner does not become too high, so that the effect of the charge control agent does not decrease, the electrostatic attraction force with the developing roller is kept at an appropriate level, and the fluidity of the developer and the image density are less likely to decrease. The amount of the charge control agent used can be appropriately adjusted depending on the type of resin used in the toner, the presence or absence of additives used as necessary, and the toner production method including the dispersion method.

[0071] <Other ingredients> The toner may contain other components as appropriate depending on the purpose. Examples of other components include a flowability improver, a cleaning property improver, a magnetic material, and a metal soap.

[0072] The flowability improver refers to a substance that increases hydrophobicity by performing surface treatment on a component that may be contained in the toner, thereby making it possible to prevent deterioration of flowability and charging characteristics even under high humidity conditions. Examples of the flow improver include silane coupling agents, silylation agents, silane coupling agents having a fluoroalkyl group, organic titanate coupling agents, aluminum coupling agents, silicone oils, and modified silicone oils.

[0073] The cleaning improver is used to remove the developer remaining on the electrostatic latent image carrier or intermediate transfer body after transfer. Examples of the cleaning improver include polymer fine particles produced by soap-free emulsion polymerization, such as fatty acid metal salts such as zinc stearate, calcium stearate, and stearic acid, polymethyl methacrylate fine particles, polystyrene fine particles, etc. The polymer fine particles preferably have a relatively narrow peak width in the particle size distribution, and preferably have a mass average particle size of 0.01 to 1 μm.

[0074] The magnetic material is not particularly limited and may be appropriately selected from known materials depending on the purpose, and examples thereof include iron powder, magnetite, ferrite, etc. Among these, a material having a color tone that is unlikely to be mixed with the toner is preferable, a light-colored material is more preferable, and a white material is even more preferable.

[0075] (Toner manufacturing method) The method for producing the toner in the present invention is not particularly limited, and the toner can be produced by a melt-kneading pulverization method, a polymerization method using an isocyanate group-containing prepolymer, a method of dissolving in a solvent, removing the solvent and pulverizing, or a melt spray method.

[0076] For example, a melt kneading method, a polymerization method (suspension polymerization method / emulsion polymerization method) in which a monomer composition containing a specific crystalline polymer and a polymerizable monomer is directly polymerized in an aqueous phase, a polyaddition reaction method in which a composition containing a specific crystalline polymer and an isocyanate group-containing prepolymer is directly elongated / crosslinked with amines in an aqueous phase, a method in which the material is dissolved in a solvent, desolvated, and pulverized, and the like can be used. In the toner of the present invention, the main component of the resin is preferably a polyester resin.

[0077] In the melt-kneading pulverization method, examples of an apparatus for melting and kneading the toner include a batch-type two-roll mixer, a Banbury mixer, a continuous twin-screw extruder, a KTK-type twin-screw extruder manufactured by Kobe Steel, Ltd., a TEM-type twin-screw extruder manufactured by Toshiba Machine Co., Ltd., a twin-screw extruder manufactured by KCK Corporation, a PCM-type twin-screw extruder manufactured by Ikegai Iron Works, a KEX-type twin-screw extruder manufactured by Kurimoto Iron Works, a continuous single-screw kneader, and a Co-kneader manufactured by Buss.

[0078] In the above-mentioned polymerization method and polyaddition reaction method using an isocyanate group-containing prepolymer, it is essential to forcibly perform emulsification (formation of droplets) by applying mechanical energy to the aqueous phase. Examples of the means for applying such mechanical energy include means for applying strong stirring or ultrasonic vibration energy using a homomixer, ultrasonic waves, Manton-Gaulin, etc.

[0079] The toner raw materials are coarsely pulverized using a hammer mill, a rotoplex, or the like, and then pulverized to an appropriate size using a fine pulverizer using a jet stream or a mechanical fine pulverizer, and it is preferable that the pulverized material is pulverized to a mass average particle size of 3 to 15 μm. Furthermore, it is preferable that the particle size of the pulverized material is adjusted to a mass average particle size of 5 to 20 μm using an air classifier, or the like.

[0080] The softening temperature (T 1 / 2The glass transition temperature (Tg): the temperature at which half of the sample flows out under a given load when heated) is preferably 115 to 140°C. From the viewpoint of toner storage stability, the glass transition temperature (Tg) of the toner is preferably 55 to 70°C, more preferably 57 to 70°C. If the toner Tg is 55°C or higher, the toner is less likely to deteriorate in a high-temperature atmosphere and offset is less likely to occur during fixing. Also, if the toner Tg is 70°C or lower, the fixing property of the toner is less likely to decrease.

[0081] As a method for coating the toner base particles with the external additive, the toner base particles and the external additive are mixed and stirred using a mixer, so that the external additive can be coated on the surfaces of the toner base particles while disintegrating the external additive. At this time, the external additive is uniformly and firmly attached to the toner base particles, thereby improving the durability of the toner.

[0082] (Developer) The developer using the toner of the present invention may be either a one-component developer or a two-component developer. The two-component developer has the toner of the present invention and a carrier. The carrier is not particularly limited and can be appropriately selected depending on the purpose, but is preferably one having a core material and a resin layer covering the core material.

[0083] The material of the core material is not particularly limited and can be appropriately selected according to the purpose. For example, manganese-strontium (Mn-Sr)-based materials and manganese-magnesium (Mn-Mg)-based materials having a density of 50 emu / g or more and 90 emu / g or less are preferable. From the viewpoint of ensuring image density, highly magnetized materials such as iron powder (100 emu / g or more) and magnetite (75 emu / g or more and 120 emu / g or less) are preferable. In addition, weakly magnetized materials such as copper-zinc (Cu-Zn)-based materials (30 emu / g or more and 80 emu / g or less) are preferable because they can weaken the contact of the toner with the photoconductor in a spiked state, which is advantageous for improving image quality. These materials may be used alone or in combination of two or more types.

[0084] The volume average particle diameter of the core material is preferably 25 μm or more and 200 μm or less.

[0085] The material of the resin layer is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include amino resins, polyvinyl resins, polystyrene resins, halogenated olefin resins, polyester resins, polycarbonate resins, polyethylene resins, polyvinyl fluoride resins, polyvinylidene fluoride resins, polytrifluoroethylene resins, polyhexafluoropropylene resins, copolymers of vinylidene fluoride and acrylic monomers, copolymers of vinylidene fluoride and vinyl fluoride, fluoro terpolymers such as terpolymers of tetrafluoroethylene, vinylidene fluoride and non-fluorinated monomers, silicone resins, etc. These may be used alone or in combination of two or more.

[0086] The mixture ratio of the toner and the carrier in the two-component developer is preferably 2.0% by mass to 12.0% by mass, more preferably 2.5% by mass to 10.0% by mass.

[0087] (Toner storage unit) In this specification, the toner storage unit refers to a unit having a function of storing toner and storing the toner. Examples of the toner storage unit include a toner storage container, a developing unit, a developing device, and a process cartridge. The toner storage container refers to a container that stores toner. The developing unit and developing device refer to a device having a means for storing toner and developing the toner. The process cartridge is a cartridge that integrates at least an image carrier and a developing unit, contains toner, and is detachably mountable to an image forming apparatus. The process cartridge may further include one or more of a charging unit, an exposure unit, and a cleaning unit.

[0088] The toner storage unit of the present invention stores the toner of the present invention. By mounting the toner storage unit of the present invention in an image forming apparatus and forming an image using the toner of the present invention, it is possible to obtain an excellent image with excellent low-temperature fixing properties and heat-resistant storage stability, and with few abnormalities.

[0089] (Process cartridge) The process cartridge according to one embodiment of the present invention has at least an electrostatic latent image carrier that carries an electrostatic latent image, and a developing means. The developing means can form a toner image by developing the electrostatic latent image carried on the electrostatic latent image carrier with the toner of the present invention. The process cartridge may further include other means as necessary. Examples of the other means include a charging means, an exposure means, a transfer means, a cleaning means, and a discharging means.

[0090] The developing means has at least a developer container that contains the toner or developer of the present invention, and a developer carrier that supports and transports the toner or developer contained in the developer container. The developing means may further include a layer thickness regulating member for regulating the thickness of the toner layer carried on the developer carrying member.

[0091] The process cartridge of the present invention is preferably detachably mountable to the main body of an image forming apparatus such as various electrophotographic apparatus, facsimile machines, printers, etc.

[0092] (Image forming method and image forming apparatus) The image forming apparatus of the present invention comprises: An electrostatic latent image carrier; an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image bearing member; a developing means for developing the electrostatic latent image with the toner of the present invention to form a toner image; a transfer means for transferring the toner image onto a recording medium; and a fixing unit for fixing the toner image transferred onto the recording medium.

[0093] The image forming apparatus of the present invention may further include other means such as a discharging means, a cleaning means, a recycling means, and a control means, if necessary.

[0094] The image forming method of the present invention comprises the steps of: an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image with the toner of the present invention to form a toner image; a transfer step of transferring the toner image onto a recording medium; a fixing step of fixing the toner image transferred onto the recording medium; Includes.

[0095] The image forming method of the present invention may further include other steps such as a static elimination step, a cleaning step, a recycling step, and a control step, if necessary.

[0096] <Electrostatic latent image forming process and electrostatic latent image forming means> The electrostatic latent image forming step is a step of forming an electrostatic latent image on an electrostatic latent image bearing member. The electrostatic latent image forming unit is a unit that forms an electrostatic latent image on an electrostatic latent image carrier. The electrostatic latent image forming step is suitably carried out by the electrostatic latent image forming means.

[0097] The electrostatic latent image carrier (hereinafter, sometimes referred to as "electrophotographic photoreceptor" or "photoreceptor") is not particularly limited in terms of material, shape, structure, size, etc., and can be appropriately selected from known ones. The electrostatic latent image bearing member preferably has a drum shape. Examples of the material of the electrostatic latent image carrier include inorganic photoconductors such as amorphous silicon and selenium, and organic photoconductors (OPC) such as polysilane and phthalopolymethine. Among these, organic photoconductors (OPC) are preferred because they can provide higher definition images. Examples of the organic photoreceptor include a laminated type photoreceptor having a laminated structure in which a layer (charge generation layer) in which a charge generation material such as metal-free phthalocyanine or titanyl phthalocyanine is dispersed in a binder resin and a layer (charge transport layer) in which a charge transport material is dispersed in a binder resin are stacked on a support such as an aluminum drum, and a single-layer type photoreceptor having a single-layered photosensitive layer in which both a charge generation material and a charge transport material are dispersed in a binder resin on a support. In the single-layer type photoreceptor, a hole transport material and an electron transport material can also be added to the photosensitive layer as charge transport materials. An undercoat layer may be provided between the support and the multi-layer charge generating layer or the single-layer photosensitive layer.

[0098] In the electrostatic latent image forming step, the electrostatic latent image can be formed, for example, by uniformly charging the surface of the electrostatic latent image bearing member by the electrostatic latent image forming unit, and then exposing the surface to light in an imagewise manner. The electrostatic latent image forming means can include, for example, at least a charging means (charger) that uniformly charges the surface of the electrostatic latent image carrier, and an exposure means (exposure device) that imagewise exposes the surface of the electrostatic latent image carrier.

[0099] The charging can be carried out, for example, by applying a voltage to the surface of the electrostatic latent image bearing member using the charger. The charger is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charger include a contact charger known per se having a conductive or semiconductive roll, brush, film, rubber blade, or the like, and a non-contact charger utilizing corona discharge such as a corotron or scorotron.

[0100] The charger is preferably one which is disposed in contact or non-contact with the electrostatic latent image bearing member and charges the surface of the electrostatic latent image bearing member by applying DC and AC voltages in a superimposed manner. The charger is preferably a charging roller arranged in close proximity to the electrostatic latent image carrier without contacting the electrostatic latent image carrier via a gap tape, and is preferably one that charges the surface of the electrostatic latent image carrier by applying a DC voltage and an AC voltage superimposed on the charging roller.

[0101] The exposure can be carried out, for example, by exposing the surface of the electrostatic latent image bearing member imagewise using the exposure unit. The exposure device is not particularly limited as long as it can expose the surface of the electrostatic latent image carrier charged by the charger in the shape of an image to be formed, and can be appropriately selected depending on the purpose. Examples of the exposure device include various exposure devices such as a copying optical system, a rod lens array system, a laser optical system, and a liquid crystal shutter optical system. In the image forming apparatus and image forming method of the present invention, a backlight system in which exposure is performed imagewise from the back side of the electrostatic latent image bearing member may be adopted.

[0102] <Developing step and developing means> The developing step is a step of developing the electrostatic latent image with the toner of the present invention to form a toner image. The developing means is a means for developing the electrostatic latent image with the toner of the present invention to form a toner image. The developing step is suitably carried out by the developing means. In the developing step, the toner image can be formed, for example, by developing the electrostatic latent image with the toner, and can be performed by the developing unit. The developing means preferably has at least a developing unit or developing device that contains the toner and can apply the toner to the electrostatic latent image in a contact or non-contact manner, and more preferably has a developing unit or developing device equipped with a toner container. The developing unit or device may be for single color or for multiple colors. The developing unit or developing device preferably includes, for example, a device having a stirrer that stirs the toner by friction to charge the toner, and a rotatable magnet roller.

[0103] <Transfer process and transfer means> The transfer step is a step of transferring the toner image onto a recording medium. The transfer unit is a unit for transferring the toner image onto a recording medium. The transfer step is suitably carried out by the transfer means. In the transfer step, a toner image is preferably primarily transferred onto an intermediate transfer member, and then the toner image is secondarily transferred onto the recording medium. In addition, it is more preferable that the transfer step includes a first transfer step in which the toner is a toner of two or more colors, preferably a full-color toner, and the toner image is transferred onto an intermediate transfer body to form a composite transfer image, and a second transfer step in which the composite transfer image is transferred onto a recording medium. The transfer means used in the transfer step (the first transfer means in the first transfer step, and the second transfer means in the second transfer step) preferably has at least a transfer device that peels and charges the toner image formed on the electrostatic latent image carrier (photoconductor) onto the recording medium. The number of the transfer means may be one or more. Examples of the transfer device include a corona transfer device using corona discharge, a transfer belt, a transfer roller, a pressure transfer roller, and an adhesive transfer device. The recording medium is not particularly limited and can be appropriately selected from known recording media (recording paper).

[0104] <Fixing process and fixing means> The fixing step is a step of fixing the toner image transferred onto the recording medium. The fixing unit is a unit for fixing the toner image transferred onto the recording medium. The fixing step is suitably carried out by the fixing means. The fixing step may be carried out for each color developer each time it is transferred to the recording medium by the fixing means, or may be carried out simultaneously for each color developer in a layered state. The fixing means is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a known heating and pressurizing means, such as a combination of a heating roller and a pressure roller, or a combination of a heating roller, a pressure roller and an endless belt.

[0105] The charge removing step is a step of removing electricity by applying a charge removing bias to the electrostatic latent image bearing member, and can be suitably performed by a charge removing unit. The charge removing means is not particularly limited as long as it can apply a charge removing bias to the electrostatic latent image bearing member, and can be appropriately selected from known charge removers. For example, a charge removing lamp is preferably used.

[0106] The cleaning step is a step of removing the toner remaining on the electrostatic latent image bearing member, and can be suitably performed by a cleaning unit. The cleaning means is not particularly limited as long as it can remove the toner remaining on the electrostatic latent image carrier, and can be appropriately selected from among known cleaners. Suitable examples of the cleaning means include magnetic brush cleaners, electrostatic brush cleaners, magnetic roller cleaners, blade cleaners, brush cleaners, and web cleaners.

[0107] The recycling step is a step of recycling the toner removed by the cleaning step to the developing means, and can be suitably performed by a recycling means. The recycling means is not particularly limited, and examples thereof include known transport means.

[0108] The control step is a step of controlling each of the steps, and each of the steps can be suitably performed by a control means. The control means is not particularly limited as long as it can control the movement of each of the means, and can be appropriately selected depending on the purpose. For example, the control means includes devices such as a sequencer and a computer.

[0109] FIG. 1 is a schematic explanatory diagram showing an example of a part of an image forming apparatus according to an embodiment of the present invention. The image forming apparatus 100A includes a photoconductor drum 10, a charging roller 20, an exposure device, a developing device 40, an intermediate transfer belt 50, a cleaning device 60 having a cleaning blade, and a discharging lamp .

[0110] The intermediate transfer belt 50 is an endless belt stretched around three rollers 51 arranged on the inside, and can move in the direction of the arrow in Fig. 1. Some of the three rollers 51 also function as transfer bias rollers capable of applying a transfer bias (primary transfer bias) to the intermediate transfer belt 50. A cleaning device 90 having a cleaning blade is arranged near the intermediate transfer belt 50. Furthermore, a transfer roller 80 capable of applying a transfer bias (secondary transfer bias) for transferring a toner image to a transfer paper 95 is arranged facing the intermediate transfer belt 50.

[0111] In addition, a corona charging device 58 for applying an electric charge to the toner image transferred to the intermediate transfer belt 50 is disposed around the intermediate transfer belt 50, between the contact point between the photosensitive drum 10 and the intermediate transfer belt 50 and the contact point between the intermediate transfer belt 50 and the transfer paper 95, in the direction of rotation of the intermediate transfer belt 50.

[0112] The developing device 40 is composed of a developing belt 41, a black developing unit 45K, a yellow developing unit 45Y, a magenta developing unit 45M, and a cyan developing unit 45C, which are arranged around the developing belt 41 and contain the toner of the present invention. The developing units 45K, 45Y, 45M, and 45C, which contain the toner of the present invention, each include a developer container 42K, 42Y, 42M, and 42C, developer supply rollers 43K, 43Y, 43M, and 43C, and developing rollers (developer carriers) 44K, 44Y, 44M, and 44C. The developing belt 41 is an endless belt stretched by a plurality of belt rollers, and can move in the direction of the arrow in FIG. 1. Furthermore, a part of the developing belt 41 is in contact with the photosensitive drum 10.

[0113] Next, a part of an example of a method for forming an image with the toner of the present invention using the image forming apparatus 100A will be described. First, the surface of the photoconductor drum 10 is uniformly charged using the charging roller 20, and then the photoconductor drum 10 is exposed to exposure light L using an exposure device to form an electrostatic latent image. Next, the electrostatic latent image formed on the photoconductor drum 10 is developed with toner supplied from the developing device 40 to form a toner image. Furthermore, the toner image formed on the photoconductor drum 10 is transferred (primary transfer) onto the intermediate transfer belt 50 by the transfer bias applied from the roller 51, and then transferred (secondary transfer) onto the transfer paper 95 by the transfer bias applied from the transfer roller 80. Meanwhile, the photoconductor drum 10 from which the toner image has been transferred onto the intermediate transfer belt 50 is discharged by the discharge lamp 70 after the toner remaining on the surface is removed by the cleaning device 60.

[0114] 2 is a schematic diagram showing another example of a part of an image forming apparatus according to an embodiment of the present invention. Image forming apparatus 100B has the same configuration as image forming apparatus 100A, except that image forming apparatus 100B does not include developing belt 41 and has black developing unit 45K, yellow developing unit 45Y, magenta developing unit 45M, and cyan developing unit 45C disposed directly opposite each other around photoconductor drum 10.

[0115] 3 is a schematic diagram showing an example of an image forming apparatus according to an embodiment of the present invention. The image forming apparatus 100C is a tandem type color image forming apparatus, and includes a copying machine main body 150, a paper feed table 200, a scanner 300, and an automatic document feeder (ADF) 400. Intermediate transfer belt 50, provided in the center of copying machine main body 150, is an endless belt stretched around three rollers 14, 15, and 16, and can move in the direction of the arrow in Fig. 3. Near roller 15, a cleaning device 17 having a cleaning blade for removing toner remaining on intermediate transfer belt 50 after a toner image has been transferred to recording paper, is disposed. Facing intermediate transfer belt 50 stretched around rollers 14 and 15, yellow, cyan, magenta, and black image forming units 120Y, 120C, 120M, and 120K are arranged in parallel along the conveying direction.

[0116] An exposure device 21 is disposed near the image forming unit 120. A secondary transfer belt 24 is disposed on the side of the intermediate transfer belt 50 opposite to the side on which the image forming unit 120 is disposed. The secondary transfer belt 24 is an endless belt stretched over a pair of rollers 23, and the recording paper transported on the secondary transfer belt 24 and the intermediate transfer belt 50 can come into contact with each other between the rollers 16 and 23.

[0117] Further, disposed near the secondary transfer belt 24 is a fixing device 25 including a fixing belt 26, which is an endless belt stretched over a pair of rollers, and a pressure roller 27 disposed so as to be pressed against the fixing belt 26. Further, disposed near the secondary transfer belt 24 and the fixing device 25 is a sheet inverting device 28 for inverting the recording paper when images are formed on both sides of the recording paper.

[0118] Next, an example of a method for forming a full-color image using the toner of the present invention and the image forming apparatus 100C will be described. First, a color original is placed on the platen 130 of the automatic document feeder (ADF) 400, or the automatic document feeder 400 is opened and a color original is placed on the contact glass 32 of the scanner 300, and the automatic document feeder 400 is closed. When the start switch is pressed, if an original is set on the automatic original feeder 400, the original is transported and moved onto the contact glass 32, whereas if an original is set on the contact glass 32, the scanner 300 is driven and the first traveling body 33 equipped with a light source and the second traveling body 34 equipped with a mirror travel immediately. At this time, the light irradiated from the first traveling body 33 is reflected from the original surface by the second traveling body 34, and then received by the reading sensor 36 via the imaging lens 35, whereby the original is read and image information of black, yellow, magenta and cyan is obtained. The image information for each color is transmitted to the image forming means 18 in the image forming unit 120 for each color, and a toner image for each color is formed.

[0119] Fig. 4 is a schematic diagram showing another example of a part of an image forming apparatus according to an embodiment of the present invention. As shown in Fig. 4, each of the image forming units 120 for each color shown in Fig. 3 includes a photoconductor drum 10, a charging roller 160 for uniformly charging the photoconductor drum 10, an exposure device for exposing the photoconductor drum 10 to exposure light L based on image information for each color to form an electrostatic latent image for each color, a developing device 61 for developing the electrostatic latent image with a developer for each color to form a toner image for each color, a transfer roller 62 for transferring the toner image onto the intermediate transfer belt 50, a cleaning device 63 having a cleaning blade, and a static elimination lamp 64.

[0120] The toner images of each color formed by the image forming units 120 of each color shown in FIG. 3 are transferred in sequence (primary transfer) onto the intermediate transfer belt 50 moving while being stretched around rollers 14, 15, and 16, and are superimposed to form a composite toner image. Meanwhile, in the paper feed table 200, one of the paper feed rollers 142 is selectively rotated to feed recording paper from one of the paper feed cassettes 144 provided in multiple stages in the paper bank 143, which is separated one by one by the separation roller 145 and sent to the paper feed path 146, transported by the transport roller 147 and guided to the paper feed path 148 in the copying machine main body 150, where it is stopped by hitting the registration roller 49. Alternatively, the paper feed roller is rotated to feed recording paper on the manual feed tray 54, which is separated one by one by the separation roller 52 and guided to the manual feed path 53, where it is stopped by hitting the registration roller 49.

[0121] The registration roller 49 is generally used while being grounded, but may be used with a bias applied thereto in order to remove paper dust from the recording paper. Next, the registration roller 49 is rotated in synchronization with the composite toner image formed on the intermediate transfer belt 50, thereby feeding the recording paper between the intermediate transfer belt 50 and the secondary transfer belt 24, and the composite toner image is transferred (secondary transfer) onto the recording paper. Any toner remaining on the intermediate transfer belt 50 after the composite toner image has been transferred is removed by the cleaning device 17.

[0122] The recording paper onto which the composite toner image has been transferred is transported by secondary transfer belt 24, and then the composite toner image is fixed by fixing device 25. Next, the transport path of the recording paper is switched by switching claw 55, and the recording paper is discharged onto paper discharge tray 57 by discharge rollers 56. Alternatively, the transport path of the recording paper is switched by switching claw 55, the sheet is inverted by sheet inverting device 28, an image is formed on the back side in the same manner, and then the recording paper is discharged onto paper discharge tray 57 by discharge rollers 56. EXAMPLES

[0123] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. However, "parts" refers to "parts by mass" unless otherwise specified.

[0124] (Preparation of inorganic additive 1) 100g of hydrophilic silica particles (Aerosil 200: manufactured by Nippon Aerosil Co., Ltd., average primary particle diameter 12nm) was dispersed in 2L of water and heated to 85°C. Next, an aluminum chloride aqueous solution was added in an amount equivalent to 10% by mass of Al2O3 relative to the silica particles, and the mixture was adjusted to pH 5.5 with an aqueous sodium hydroxide solution, and then the mixture was stirred for 30 minutes and filtered, and the residue on the filter was washed with water to obtain a washed cake. Next, the washed cake was dried at 120°C and then pulverized with a media-type fine grinder. Finally, 40g of the obtained powder was put into a small mixer, 10g of isobutyltrimethoxysilane was added, mixed for 15 minutes, and then re-dried at 120°C to produce inorganic external additive 1 (average particle size 12nm).

[0125] (Preparation of inorganic additive 2) 100g of hydrophilic silica particles (Aerosil 200: manufactured by Nippon Aerosil Co., Ltd., average primary particle diameter 12nm) was dispersed in 2L of water and heated to 85°C. Next, an aluminum chloride aqueous solution was added in an amount equivalent to 10% by mass of Al2O3 relative to the silica particles, and the mixture was adjusted to pH 5.5 with an aqueous sodium hydroxide solution, and then the mixture was stirred for 30 minutes and filtered, and the residue on the filter was washed with water to obtain a washed cake. Next, the washed cake was dried at 120°C and then pulverized with a media-type fine grinder. Finally, 40g of the obtained powder was put into a small mixer, 12g of isobutyltrimethoxysilane was added, mixed for 15 minutes, and then re-dried at 120°C to produce inorganic external additive 2 (average particle size 12nm).

[0126] (Preparation of inorganic additive 3) 100g of hydrophilic silica particles (Aerosil 200: manufactured by Nippon Aerosil Co., Ltd., average primary particle diameter 12nm) was dispersed in 2L of water and heated to 85℃. Next, an aluminum chloride aqueous solution was added in an amount equivalent to 10% by mass of Al2O3 relative to the silica particles, and the mixture was adjusted to pH 5.5 with an aqueous sodium hydroxide solution, and then the mixture was stirred for 30 minutes and filtered, and the residue on the filter was washed with water to obtain a washed cake. Next, the washed cake was dried at 120℃ and pulverized with a media-type fine pulverizer to produce inorganic external additive 3 (average particle diameter 12nm).

[0127] (Preparation of inorganic additive 4) 100g of hydrophilic silica particles (Aerosil 200: manufactured by Nippon Aerosil Co., Ltd., average primary particle diameter 12nm) was dispersed in 2L of water and heated to 85°C. Next, an aqueous zinc chloride solution was added in an amount equivalent to 10% by mass in terms of ZnO relative to the silica particles, and the pH was adjusted to 8.0 with an aqueous sodium hydroxide solution. The mixture was then stirred for 30 minutes, filtered, and the residue on the filter was washed with water to obtain a washed cake. Next, the washed cake was dried at 120°C and pulverized with a media-type fine grinder. Finally, 40g of the obtained powder was put into a small mixer, 10g of isobutyltrimethoxysilane was added, mixed for 15 minutes, and then re-dried at 120°C to produce inorganic external additive 4 (average particle size 12nm).

[0128] (Preparation of inorganic additive 5) 100g of hydrophilic silica particles (Aerosil 200: manufactured by Nippon Aerosil Co., Ltd., average primary particle diameter 12nm) was dispersed in 2L of water and heated to 85°C. Next, an aqueous magnesium chloride solution was added in an amount equivalent to 10% by mass in terms of MgO relative to the silica particles, and the mixture was adjusted to pH 5.0 with an aqueous sodium hydroxide solution. The mixture was then stirred for 30 minutes, filtered, and the residue on the filter was washed with water to obtain a washed cake. Next, the washed cake was dried at 120°C and pulverized with a media-type fine grinder. Finally, 40g of the obtained powder was put into a small mixer, 10g of isobutyltrimethoxysilane was added, mixed for 15 minutes, and then re-dried at 120°C to produce inorganic external additive 5 (average particle size 12nm).

[0129] (Preparation of inorganic additive 6) 100g of hydrophilic silica particles (Aerosil 200: manufactured by Nippon Aerosil Co., Ltd., average primary particle diameter 12nm) was dispersed in 2L of water and heated to 85°C. Next, an aqueous solution of iron chloride was added in an amount equivalent to 10% by mass in terms of FeO relative to the silica particles, and the pH was adjusted to 8.5 with an aqueous solution of sodium hydroxide. The mixture was then stirred for 30 minutes, filtered, and the residue on the filter was washed with water to obtain a washed cake. Next, the washed cake was dried at 120°C and pulverized with a media-type fine grinder. Finally, 40g of the obtained powder was put into a small mixer, 10g of isobutyltrimethoxysilane was added, mixed for 15 minutes, and then re-dried at 120°C to produce inorganic external additive 6 (average particle size 12nm).

[0130] (Preparation of inorganic additive 7) 100g of hydrophilic silica particles (Aerosil 90: manufactured by Nippon Aerosil Co., Ltd., average primary particle diameter 25nm) was dispersed in 2L of water and heated to 85°C. Next, an aluminum chloride aqueous solution was added in an amount equivalent to 10% by mass of Al2O3 relative to the silica particles, and the mixture was adjusted to pH 5.5 with an aqueous sodium hydroxide solution, and then the mixture was stirred for 30 minutes and filtered, and the residue on the filter was washed with water to obtain a washed cake. Next, the washed cake was dried at 120°C and then pulverized with a media-type fine grinder. Finally, 40g of the obtained powder was put into a small mixer, 10g of isobutyltrimethoxysilane was added, mixed for 15 minutes, and then re-dried at 120°C to produce inorganic external additive 7 (average particle size 25nm).

[0131] (Preparation of inorganic additive 8) 100g of hydrophilic silica particles (Aerosil 300: manufactured by Nippon Aerosil Co., Ltd., average primary particle diameter 8nm) was dispersed in 2L of water and heated to 85°C. Next, an aluminum chloride aqueous solution was added in an amount equivalent to 10% by mass of Al2O3 relative to the silica particles, and the mixture was adjusted to pH 5.5 with an aqueous sodium hydroxide solution, and then the mixture was stirred for 30 minutes and filtered, and the residue on the filter was washed with water to obtain a washed cake. Next, the washed cake was dried at 120°C and then pulverized with a media-type fine grinder. Finally, 40g of the obtained powder was put into a small mixer, 10g of isobutyltrimethoxysilane was added, mixed for 15 minutes, and then re-dried at 120°C to produce inorganic external additive 8 (average particle size 8nm).

[0132] (Preparation of inorganic additive 9) 100g of hydrophilic silica particles (Aerosil 50: manufactured by Nippon Aerosil Co., Ltd., average primary particle diameter 35nm) was dispersed in 2L of water and heated to 85°C. Next, an aluminum chloride aqueous solution was added in an amount equivalent to 10% by mass of Al2O3 relative to the silica particles, and the mixture was adjusted to pH 5.5 with an aqueous sodium hydroxide solution, and then the mixture was stirred for 30 minutes and filtered, and the residue on the filter was washed with water to obtain a washed cake. Next, the washed cake was dried at 120°C and then pulverized with a media-type fine grinder. Finally, 40g of the obtained powder was put into a small mixer, 10g of isobutyltrimethoxysilane was added, mixed for 15 minutes, and then re-dried at 120°C to produce inorganic external additive 9 (average particle size 35nm).

[0133] (Preparation of inorganic external additive 10) 100g of hydrophilic silica particles (Aerosil 200: manufactured by Nippon Aerosil Co., Ltd., average primary particle diameter 12nm) was dispersed in 2L of water and heated to 85°C. Next, an aluminum chloride aqueous solution was added in an amount equivalent to 10% by mass of Al2O3 relative to the silica particles, and the mixture was adjusted to pH 5.5 with an aqueous sodium hydroxide solution, and then the mixture was stirred for 30 minutes and filtered, and the residue on the filter was washed with water to obtain a washed cake. Next, the washed cake was dried at 120°C and then pulverized with a media-type fine grinder. Finally, 40g of the obtained powder was put into a small mixer, 10g of isobutyltrimethoxysilane was added, mixed for 15 minutes, and then re-dried at 120°C to produce inorganic external additive 10 (average particle size 12nm).

[0134] (Average primary particle size) The average primary particle size of the silica particles used in preparing the inorganic external additives 1 to 10 was measured by the following method. A field emission scanning electron microscope (SU8230, Hitachi High-Technologies Corporation) was used to obtain SEM images of the silica particles, and the number-average particle diameter was measured by image analysis. First, a sample of silica particles was dispersed in tetrahydrofuran, and then the solvent was removed on a substrate to dry it. The sample was observed with the above-mentioned SEM to obtain an image, and the maximum length of the primary particles for each particle was measured under the following measurement conditions. The average value of 50 particles was calculated, and this was taken as the average primary particle diameter of the silica particles. [SEM measurement conditions] Accelerating voltage: 2.0 kV WD(Working Distance):5.0mm Observation magnification: 100,000 times

[0135] (Measurement of hydrophobicity) The hydrophobicity of the prepared inorganic external additives 1 to 10 was measured by the following method. 0.2 g of each of the inorganic external additives 1 to 10 was added to a beaker containing 50 ml of ion-exchanged water, and methanol was added dropwise while stirring. As the methanol concentration in the beaker increased, the added external additive gradually settled, so the mass fraction of methanol in the mixed solution of methanol and water at the end point when the entire amount had settled was taken as the hydrophobicity (MeOH%) of each inorganic external additive.

[0136] (Measurement of volume resistivity) The volume resistivity of the prepared inorganic external additives 1 to 10 was measured by the following method. In a cell consisting of a fluororesin container containing two electrodes with a surface area of ​​2.5 cm × 4 cm spaced 0.2 cm apart, inorganic external additives 1 to 10 were filled between the two electrodes, and tapping was performed 10 times at a drop height of 1 cm and a tapping speed of 30 times / min. Next, a direct current voltage of 1,000 V was applied between the two electrodes filled with the inorganic external additive, and the resistance value r [Ω] after 30 seconds was measured using a high resistance meter 4329A (manufactured by Yokogawa Hewlett-Packard Co., Ltd.). The volume resistivity [Ω·cm] of each of the inorganic external additives 1 to 10 was calculated by inputting each measured resistance value r into the following formula. (Formula) r×(2.5×4) / 0.2

[0137] Details of the inorganic external additives 1 to 10 obtained above are shown in Table 1. [Table 1]

[0138] (Production of amorphous polyester resin) The monomer species and tetrabutoxy titanate as a condensation catalyst shown in Table 2 below were placed in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, and reacted at 230°C for 6 hours under a nitrogen stream while distilling off the water produced. Next, the reaction was carried out for 1 hour under a reduced pressure of 5 mmHg to 20 mmHg to obtain amorphous polyester resins used in the production of toner base particles 1 to 5 below. In Table 2, the "25 mol %" shown for bisphenol A (2,2) ethylene oxide indicates the proportion in the alcohol component when the acid component is 50 mol % and the alcohol component is 50 mol %. [Table 2]

[0139] (Production of Crystalline Polyester Resin) Fumaric acid and 1,6-hexanediol were charged into a 5 L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple so that the OH / COOH ratio of the mixture was 0.9, and reacted with titanium tetraisopropoxide (500 ppm relative to the resin component) at 180°C for 10 hours, then heated to 200°C and reacted for 3 hours, and further reacted at a pressure of 8.3 kPa for 2 hours to obtain a crystalline polyester resin with a melting point of 103°C. This crystalline polyester resin was used to prepare the following toner base particles 1 to 5.

[0140] (Preparation of toner base particles 1) Amorphous polyester resin: 86.4 parts Crystalline polyester resin: 4.8 parts Aromatic petroleum resin (FTR-2140: Mitsui Chemicals Inc.): 4.8 parts Hydrocarbon wax (Sasol Wax C80: manufactured by Sasol): 4.0 parts Carbon black (Mitsubishi Chemical #44): 10 parts

[0141] According to the above recipe, the toner raw materials were premixed using a Henschel mixer (FM20B, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and then melted and kneaded at a temperature of 120° C. in a twin-screw kneader (PCM-30, manufactured by Ikegai Iron Works Co., Ltd.). The obtained kneaded material was rolled to a thickness of 2.7 mm with a roller, cooled to room temperature with a belt cooler, and coarsely pulverized to 200 μm to 300 μm with a hammer mill. Next, it was finely pulverized with a supersonic jet pulverizer Labojet (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), and then classified with an air classifier (manufactured by Nippon Pneumatic Mfg. Co., Ltd., MDS-I) while appropriately adjusting the louver opening so that the mass average particle size was 5.8±0.2 μm, and toner base particles 1 were obtained.

[0142] (Preparation of toner base particles 2) The toner base particles 1 were subjected to a spheronization treatment using hot air to prepare toner base particles 2.

[0143] (Preparation of toner base particles 3) Amorphous polyester resin: 91.2 parts Aromatic petroleum resin (FTR-2140: Mitsui Chemicals Inc.): 4.8 parts Hydrocarbon wax (Sasol Wax C80: manufactured by Sasol): 4.0 parts Carbon black (Mitsubishi Chemical #44): 10 parts

[0144] According to the above recipe, the toner raw materials were premixed using a Henschel mixer (FM20B, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and then melted and kneaded at a temperature of 120° C. in a twin-screw kneader (PCM-30, manufactured by Ikegai Iron Works Co., Ltd.). The obtained kneaded product was rolled to a thickness of 2.7 mm with a roller, cooled to room temperature with a belt cooler, and coarsely pulverized to 200 μm to 300 μm with a hammer mill. Next, it was finely pulverized with a supersonic jet pulverizer Labojet (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), and then classified with an air classifier (manufactured by Nippon Pneumatic Mfg. Co., Ltd., MDS-I) while appropriately adjusting the louver opening so that the mass average particle size was 5.8±0.2 μm, and toner base particles 3 were obtained.

[0145] (Preparation of toner base particles 4) Amorphous polyester resin: 91.2 parts Crystalline polyester resin: 4.8 parts Hydrocarbon wax (Sasol Wax C80: manufactured by Sasol): 4.0 parts Carbon black (Mitsubishi Chemical #44): 10 parts

[0146] According to the above recipe, the toner raw materials were premixed using a Henschel mixer (FM20B, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and then melted and kneaded at a temperature of 120°C using a twin-screw kneader (PCM-30, manufactured by Ikegai Iron Works Co., Ltd.). The kneaded product obtained was rolled to a thickness of 2.7 mm using a roller, cooled to room temperature using a belt cooler, and coarsely pulverized to 200 μm to 300 μm using a hammer mill. Next, the product was finely pulverized using a supersonic jet pulverizer Labojet (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), and then classified using an air classifier (MDS-I, manufactured by Nippon Pneumatic Mfg. Co., Ltd.) while appropriately adjusting the louver opening so that the mass average particle size was 5.8 ± 0.2 μm, to obtain toner base particles 4.

[0147] (Preparation of Toner Base Particles 5) Amorphous polyester resin: 86.4 parts Crystalline polyester resin: 4.8 parts Aromatic petroleum resin (FTR-2140: Mitsui Chemicals Inc.): 4.8 parts Ester wax (WE-10: NOF Corp.): 4.0 parts Carbon black (Mitsubishi Chemical #44): 10 parts

[0148] According to the above recipe, the toner raw materials were premixed using a Henschel mixer (FM20B, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and then melted and kneaded at a temperature of 120° C. in a twin-screw kneader (PCM-30, manufactured by Ikegai Iron Works Co., Ltd.). The obtained kneaded product was rolled to a thickness of 2.7 mm using a roller, cooled to room temperature using a belt cooler, and coarsely pulverized to 200 μm to 300 μm using a hammer mill. Next, the mixture was finely pulverized using a supersonic jet mill Labojet (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), and then classified using an air classifier (manufactured by Nippon Pneumatic Mfg. Co., Ltd., MDS-I) while appropriately adjusting the louver opening so that the mass average particle size became 5.8±0.2 μm, thereby obtaining toner base particles 5.

[0149] (Measurement of average circularity) Using a wet flow type particle size / shape analyzer FPIA-3000 and analysis software FPIA-3000 Data Processing Program for FPIA version 00-10 (Sysmex Corporation), the average circularity of toner base particles 1 to 5 was determined by the following method. 0.1-0.5 mL of a 10% aqueous solution of alkylbenzene sulfonate Neogen SC-A (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and 0.1-0.5 g of toner base particles were added to a 100 mL glass beaker, and then the mixture was stirred with a micro spatula and 80 mL of ion-exchanged water was added. Next, an ultrasonic disperser UH-50 (manufactured by SMT Co., Ltd.) was used to disperse the mixture at 20 kHz, 50 W / 10 cm. 3 After dispersing for 1 minute under the above conditions, the particles were dispersed for a total of 5 minutes to obtain a measurement sample. -3 cm 3 The average circularity of the toner base particles was measured using the measurement sample. The average circularity of the toner base particles was determined as the average circularity of the toner using the toner base particles.

[0150] Table 3 shows the details of the toner base particles 1 to 5 obtained above. [Table 3]

[0151] (Examples 1 to 13, Comparative Examples 1 to 2) Toners 1 to 15 were prepared by mixing 100 parts by mass of toner base particles with 1 part by mass of HDK-2000 (Clariant Co., Ltd.) as hydrophobic silica particles and 0.5 parts by mass of inorganic external additives in a Henschel mixer. Table 4 shows the combinations of toner base particles 1 to 5 and inorganic external additives 1 to 10 used in toners 1 to 15.

[0152] [Table 4]

[0153] (Toner Developer 1-15) Toner 1-15: 5 mass % and 95 mass % of the coated ferrite carrier were uniformly mixed for 5 minutes at 48 rpm using a Turbula mixer (manufactured by Willy & Bachofen (WAB)) to prepare toner developers 1-15.

[0154] The toners 1 to 15 and toner developers 1 to 15 prepared above were used to evaluate low-temperature fixing property, heat-resistant storage stability, charge stability, and the presence or absence of abnormal images by the following evaluation methods.

[0155] (Evaluation of low temperature fixability) Toner developers 1 to 15 were placed in a Ricoh Co., Ltd. copying machine (RICOH MPC 6003) and images were output. The amount of adhesion was 0.4 mg / cm 2 A solid image was output on paper (Ricoh Co., Ltd., Type 6200) through exposure, development, and transfer processes. The fixing linear speed was 256 mm / sec. The fixing temperature was output in 5°C increments, and the lowest temperature at which cold offset did not occur (lowest fixing temperature: low-temperature fixability) was measured. The NIP width of the fixing device was 11 mm. Among the following evaluation criteria, ◎ and ◯ were judged to be sufficient results for practical use, and × was judged to be insufficient results for the present invention. -Evaluation criteria for low temperature fixability- ◎: Less than 120℃ ○: 120℃ or higher but less than 130℃ ×: 130℃ or higher

[0156] (Evaluation of heat resistance storage stability) Toners 1 to 15 were stored for 24 hours under 50°C conditions, and the penetration was measured according to JIS K2235 (25°C). A penetrometer VR-5610 (Shimadzu Corporation) was used as the penetration measurement device. Among the following evaluation criteria, ◎ and ◯ were judged to be sufficient results for practical use, and × was judged to be insufficient results according to the present invention. -Evaluation criteria for heat resistance storage stability- ◎:25mm or more ○: 20mm or more and less than 25mm ×: Less than 20mm

[0157] (Evaluation of charging stability) The toner developers 1 to 15 were placed in a Ricoh copier imajio MF-6550 with low-temperature fixing property, and 100,000 copies of a test chart with an image area of ​​6% were made, and the degree of decrease in the amount of charge was evaluated. Among the following evaluation criteria, the evaluations of ◎ and ◯ were judged to be sufficient results for practical use, and the evaluation of × was judged to be insufficient results according to the present invention. - Evaluation criteria for charging stability - ◎: Very little decrease in charge amount and excellent durability ○: Less loss of charge and better durability than conventional toners ×: Durability is as poor as or lower than that of conventional toners.

[0158] (Evaluation of abnormal images) Toner developers 1 to 15 were placed in a Ricoh copier imajio MF-6550 with low-temperature fixing properties, and 200,000 copies of a test chart with an image area of ​​6% were made in a high-temperature, high-humidity environment (27°C, 80%) using paper: Askul Super White+, and the presence or absence of abnormal images with black streaks was evaluated. Among the following evaluation criteria, ◎ and ◯ were judged to be sufficient results for practical use, and × was judged to be insufficient results for the present invention. -Evaluation criteria for the presence or absence of abnormal images- ◎: The rate of abnormal images occurring is less than 10% ○: Abnormal image occurrence rate is 10% or more but less than 20% ×: Abnormal image occurrence rate is 20% or more

[0159] The evaluation results for each toner are as follows. [Table 5]

[0160] The toners used in Examples 1 to 13 were evaluated as having low-temperature fixing ability, heat-resistant storage stability, charge stability, and the presence or absence of abnormal images as being "A" or "B," and were therefore sufficient for practical use. The toner of Comparative Example 1 did not contain silica at least partly covered with a hydroxide of a metal element, and therefore could not ensure charging stability, and was prone to producing abnormal images. The toner of Comparative Example 2 contained silica at least partially coated with a hydroxide of a metal element, but since the hydrophobicity of the silica was lower than 55 (MeOH%), it did not have adequate cleaning performance and was prone to producing abnormal images.

[0161] For example, aspects of the present invention are as follows. <1> A toner comprising an amorphous polyester resin, a wax, and an external additive, The external additive contains silica at least a part of which is coated with a hydroxide of a metal element, The toner, wherein the hydrophobicity of the silica is 55 (MeOH%) or more. <2> The volume resistivity of the silica is 1.0E+11 (Ω·cm) or less. <1> The toner according to claim 1. <3> The toner has an average circularity of 0.930 to 0.960. <1> or <2> The toner according to claim 1. <4> At least a portion of the silica is coated with an alkylsilane. <1> from <3> 2. The toner according to claim 1 . <5> The hydroxide of the metal element is at least one hydroxide of aluminum, zinc, iron and magnesium. <1> from <4> 2. The toner according to claim 1 . <6> The average particle size of the silica is 10 to 30 nm. <1> from <5> 2. The toner according to claim 1 . <7> The toner further contains a crystalline polyester resin and / or an aromatic petroleum resin. <1> from <6> 2. The toner according to claim 1 . <8> An electrostatic latent image carrier; an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image bearing member; The above <1> from <7> a developing unit for developing the electrostatic latent image with the toner according to any one of claims 1 to 4 to form a toner image; a transfer means for transferring the toner image onto a recording medium; a fixing unit for fixing the toner image transferred onto the recording medium; An image forming apparatus comprising: <9> an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; The above <1> from <7> a developing step of developing the electrostatic latent image with the toner according to any one of claims 1 to 4 to form a toner image; a transfer step of transferring the toner image onto a recording medium; a fixing step of fixing the toner image transferred onto the recording medium; An image forming method comprising the steps of: <10> The above <9> 2. A method for producing a printed matter, comprising forming the toner image on the recording medium by the image forming method according to claim 1.

[0162] the above <1> from <7> Any of the above toners <8> The image forming apparatus <9> The image forming method and the above <10> According to the method for producing a printed matter, the conventional problems can be solved and the object of the present invention can be achieved. [Explanation of symbols]

[0163] 10 Electrostatic latent image carrier (photoconductor drum) 17 Cleaning equipment 18 Image forming means 20 Charging roller 21 Exposure equipment 24 Secondary transfer belt 25 Fixing device 26 Fixing belt 27 Pressure roller 40 Developing device 41 Developing belt 42K, 42Y, 42M, 42C Developer storage unit 43K, 43Y, 43M, 43C Developer supply roller 44K, 44Y, 44M, 44C Developing roller 45K Black Development Unit 45Y Yellow Development Unit 45M Magenta Development Unit 45C Cyan Development Unit 58 Corona charging device 60 Cleaning Equipment 61 Developing device 62 Transfer roller 63 Cleaning Equipment 80 Transfer roller 90 Cleaning Equipment 95 Transfer paper 100A, 100B, 100C image forming device 120 Image forming unit 160 Charging roller [Prior art documents] [Patent documents]

[0164] [Patent Document 1] JP 2022-146467 A [Patent Document 2] JP 2021-128245 A

Claims

1. A toner comprising an amorphous polyester resin, a wax, and an external additive, The external additive contains silica at least a part of which is coated with a hydroxide of a metal element, The toner, wherein the hydrophobicity of the silica is 55 (MeOH %) or more.

2. 2. The toner according to claim 1, wherein the volume resistivity of said silica is 1.0E+11 (Ω·cm) or less.

3. 3. The toner according to claim 1, wherein the average circularity of the toner is 0.930 to 0.

960.

4. 3. The toner according to claim 1, wherein at least a portion of the silica is coated with an alkylsilane.

5. 3. The toner according to claim 1, wherein the hydroxide of the metal element is at least one hydroxide of aluminum, zinc, iron and magnesium.

6. 3. The toner according to claim 1, wherein the average particle size of the silica is from 10 to 30 nm.

7. 3. The toner according to claim 1, further comprising a crystalline polyester resin and / or an aromatic petroleum resin.

8. An electrostatic latent image carrier; an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image bearing member; a developing unit for developing the electrostatic latent image with the toner according to claim 1 or 2 to form a toner image; a transfer means for transferring the toner image onto a recording medium; a fixing unit for fixing the toner image transferred onto the recording medium; An image forming apparatus comprising:

9. an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image with the toner according to claim 1 or 2 to form a toner image; a transfer step of transferring the toner image onto a recording medium; a fixing step of fixing the toner image transferred onto the recording medium; An image forming method comprising the steps of:

10. A method for producing a printed matter, comprising forming the toner image on the recording medium by the image forming method according to claim 9.

Citation Information

Patent Citations

  • JP2022‐146467A

  • JP2021‐128245A