Eco-friendly soil conditioner
The environmentally friendly ground improvement material, using slag and sodium silicate, addresses bleeding and pipe clogging issues under high pressure, ensuring long pot life and low emissions, suitable for diverse construction applications.
Patent Information
- Application Number
- JP2023081372
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional ground improvement materials face issues such as bleeding, material separation, pipe clogging, short pot life, high emissions, and environmental impact, particularly when subjected to high pressures during pumping, and they often rely on cement which exacerbates these problems.
An environmentally friendly ground improvement material composed of pulverized blast furnace slag, sodium silicate, water, and optionally an inert filler like light calcium carbonate, which does not contain cement, is formulated to thicken instantly, reducing bleeding and separation, and maintains long pot life even under high pressures, and includes an admixture to enhance pumpability.
The material effectively prevents pipe clogging at pressures up to 5-7 MPa, reduces emissions, and extends pot life, making it suitable for various construction methods while contributing to environmental sustainability through reduced CO2 emissions and carbon capture.
Smart Images

Figure 2024165292000001 
Figure 2024165292000002 
Figure 2024165292000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an environmentally friendly ground improvement material that produces little CO2 emissions and has a small environmental impact. [Background technology]
[0002] Conventionally, for the purpose of ground improvement, various materials have been proposed and put into practical use, which have sufficient fluidity when poured and exhibit appropriate strength after pouring so as not to interfere with excavation or driving of sheet piles, even in dewaterable or non-drainable soil (see, for example, Patent Documents 1 to 6).
[0003] However, the materials currently in practical use have the following problems. Cement slurry and chemical grout materials (LW Liquid: Labiles Wasserglas), which are mainly made of water glass and cement, have a high risk of bleeding and material separation, which can lead to blockage of pipes when pumped through them. In addition, physical properties such as volume and density change during use, making it difficult to ensure the desired performance. · Cement-bentonite liquid requires the addition of a large amount of bentonite to achieve high material separation resistance, which increases the cost. Increasing the amount of cement per unit volume to prevent bleeding and material separation shortens the pot life and makes the strength greater than necessary. In mechanical mixing methods for block, wall, and grid-type improvement, if lap construction is to be performed several days later, a retarder is added to the cement-based solidification material. However, if too much retarder is added, poor hardening will occur. On the other hand, if an insufficient amount of retarder is added, or if the lap construction is significantly delayed due to bad weather or construction problems, the strength of the previously improved area will increase, resulting in poor construction at the joints. - Materials that use cement have a large environmental impact due to their high CO2 emissions. · Because slag powder has latent hydraulic properties, replacing part or all of the cement with slag powder can improve chemical resistance and seawater resistance, and reduce CO2 emissions. However, as the ratio of slag powder increases, bleeding and material separation increase, and hardening and strength development delay become more pronounced. Water glass is used as an alkaline stimulant to promote strength development, but with conventional usage, it is not possible to suppress bleeding and material separation because a flock-like non-uniform gel is not produced. Also, even if all of the cement is replaced with slag powder, its contribution to achieving carbon neutrality is small.
[0004] Incidentally, the inventions disclosed in the above Patent Documents 1 to 6 have the following problems. The adhesive grout of Patent Document 1 uses cement, and therefore the pot life cannot be sustained for a long period of time. The soil improvement solidification material of Patent Document 2 does not clearly state the order of addition or the method of addition and stirring, and the viscosity cannot be adjusted. The fluidized sand of Patent Document 3 emits a lot of CO2 because it is mixed with a large amount of slaked lime. In addition, since sand uses natural resources, there are sustainability issues. In the geopolymer of Patent Document 4, the alkaline solution is pre-diluted with 20 to 60 volume percent water, and a floc-like non-uniform gel is not produced, resulting in significant bleeding and material separation during pumping. The slurries in Patent Documents 5 and 6 emit a large amount of CO2 because they contain cement. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6034530 [Patent Document 2] Patent No. 6968132 [Patent Document 3] Patent Publication No. 2021-25289 [Patent Document 4] Patent No. 6005408 [Patent Document 5] Patent No. 5590702 [Patent Document 6] Patent No. 6955967 Summary of the Invention [Problem to be solved by the invention]
[0006] In view of the problems associated with the above-mentioned conventional materials for ground improvement, the present applicants have previously proposed a thickening slag mortar and a manufacturing method thereof that can instantly thicken to reduce bleeding and material separation during pumping while maintaining a long usable time (see Patent Application No. 2023-2071).
[0007] The thickening slag mortar proposed by the applicants in this case can solve the problems associated with the above-mentioned conventional materials used for ground improvement. However, when using the various ground improvement methods for which the mortar is used, for example, a static compaction method in which a fluid material is injected into the ground (fluid material injection static compaction method), if (1) the pumping distance is long, (2) the discharge volume is increased, or (3) the fluid material is injected into the ground to compact it, the discharge pressure of the fluid material increases, promoting coagulation and pressurized dewatering, which can result in blockage of the pipes and make pumping impossible. In this case, pumpability can be improved by adding admixtures, but if the pressure during pumping rises to 5 MPa or more (5-7 MPa), the amount of pressurized dehydration increases, and there is still a risk that the piping will become clogged and pumping will become impossible.
[0008] The first object of the present invention is to provide an environmentally friendly ground improvement material that solves the problems of conventional materials intended for ground improvement, and that has the advantages of being able to maintain a long usable time while instantly thickening to reduce bleeding and material separation during pumping, and that does not cause pipe blockage even when the pressure during pumping rises to 5 MPa or more (5 to 7 MPa) and the amount of water dewatered under pressure increases, in order to solve the problems of conventional materials intended for ground improvement, which are characteristic of the thickening slag mortar proposed by the applicants described above.
[0009] A second object of the present invention is to provide an environmentally friendly ground improvement material that can reduce CO2 emissions. [Means for solving the problem]
[0010] In order to achieve the first object, the environmentally friendly ground improvement material of the present invention contains at least aggregate, ground granulated blast furnace slag, sodium silicate and water, does not contain cement, and is used by pumping at a pressure of 5 MPa or more, and satisfies the following conditions (1) to (2). (1) The aggregate paste ratio in the initial mixture is less than 100 vol.% and the aggregate paste ratio after dehydration under 7 MPa pressure is less than 80 vol.%. (2) The final dehydration rate in the 7 MPa pressure bleeding test is less than 15%.
[0011] In this case, the environmentally friendly ground improvement material according to claim 1 further satisfies the following condition (3). (3) After 0.5 hours, the vane shear strength is 6.8 kN / m 2 Less than
[0012] In order to achieve the second objective, the environmentally friendly ground improvement material is 3 CO2 emissions per unit can be -350 to 100 kg.
[0013] The environmentally friendly ground improvement material may further contain an inert filler, and the inert filler may be made of light calcium carbonate produced from an aqueous calcium hydroxide solution and carbon dioxide as raw materials.
[0014] The environmentally friendly soil improvement material may further contain an admixture for improving pumpability.
[0015] The fineness of the ground granulated blast furnace slag is 3500 to 5000 cm 2 / g. Effect of the Invention
[0016] The environmentally friendly ground improvement material of the present invention has the advantages of being able to maintain a long pot life while instantly thickening to reduce bleeding and material separation during pumping. Even if the pressure during pumping rises to 5 MPa or more (5 to 7 MPa) and the amount of pressurized dewatering increases, the material does not clog piping, and can therefore be widely used in various construction methods aimed at ground improvement.
[0017] In addition, depending on the application, an admixture for improving pumpability can be included as necessary, thereby further improving the pumpability.
[0018] In addition, according to the environmentally friendly ground improvement material of the present invention, 3 The CO2 emissions per unit of load are -350 to 100 kg, and in particular, the environmentally friendly ground improvement material further contains an inert filler, and the inert filler is light calcium carbonate produced from an aqueous calcium hydroxide solution and carbon dioxide as raw materials, thereby making it possible to suppress CO2 emissions and contribute to reducing the environmental load. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, an embodiment of the environmentally friendly ground improvement material of the present invention will be described.
[0020] The environmentally friendly ground improvement material of the present invention contains at least aggregate, ground granulated blast furnace slag, sodium silicate and water, but does not contain cement, and is used by pumping at a pressure of 5 MPa or more.
[0021] First, the constituent materials of the environmentally friendly soil improvement material of the present invention will be described. Table 1 shows the materials used in the property tests carried out on the environmentally friendly ground improvement material of the present invention (hereinafter in this specification, the materials may be referred to by the symbols in Table 1).
[0022] [Table 1]
[0023] [aggregate] The aggregate that serves as the base material for environmentally friendly ground improvement materials can be made from unused resources such as crushed stone screenings and crushed stone powder, as well as by-products such as crushed concrete sludge aggregate and fine blast furnace slag aggregate.By not using natural resources, the material contributes to sustainability. Blast furnace slag fine aggregate has latent hydraulic properties, which can increase the strength over the long term.
[0024] [Slag powder] The ground granulated blast furnace slag used was a gypsum-added product (premixed with anhydrite and gypsum). Ground granulated blast furnace slag has a specific surface area of 3500 to 5000 cm 2 / g is economical and easy to procure, but is not limited thereto, and a specific surface area of 5000 to 12000 cm 2 / g also has the same or higher reactivity with water glass, so that the use of this material can provide the same or higher performance.
[0025] [Inactive filler] As a filler, precipitated calcium carbonate is mixed in to replace part of the aggregate or solidifying agent. Precipitated calcium carbonate is a material used in carbon dioxide capture, utilization and storage (CCUS). It is a carbon dioxide capture, utilization and storage (CCS) material, which is manufactured by fixing CO2 derived from exhaust gas in a by-product-derived calcium source. In the case of ground improvement materials, CO2 is mineralized in the form of calcium carbonate and then stored underground as part of ground improvement work, so it is expected to be easier and cheaper to store than carbon dioxide capture and storage (CCS) technology, which injects CO2 into a reservoir deep underground. In addition, it has the advantage of eliminating concerns about the injected CO2 leaking outside the reservoir due to external forces such as earthquakes. In addition, light calcium carbonate derived from sources other than concrete sludge, such as by-products from the production of acetylene gas, by-products from steelmaking, waste concrete, etc., can also be used as the calcium source. The purity of the precipitated calcium carbonate used in the property test is 98%, and 431 kg-CO2 / t of CO2 is fixed. If the CO2 emissions during production, 50 kg-CO2 / t, are subtracted from this value, the net CO2 emission unit is -431+50=381 kg-CO2 / t. .
[0026] [Sodium silicate (alkaline stimulant)] The reaction between sodium silicate (Na2O·nSiO2), which is added as an alkaline stimulant, and the gypsum contained in the ground granulated blast furnace slag is as follows. Na2O·nSiO2+CaSO4→ CaO·nSiO2+2Na2SO4 Here, the amount of gelled matter produced is affected by the amount of gypsum and the Na2O concentration, while the strength of the gelled matter is affected by the amount of SiO2. Increasing the amount of SiO2 to increase the strength of the gelled matter improves the resistance to material separation, but reduces pumpability during ground improvement work. On the other hand, the hardening reaction occurs when the metal ions contained in the ground granulated blast furnace slag dissolve in an alkaline solution (Na2O) and polymerization proceeds. However, even if the amount of SiO2 is appropriate, if the amount of Na2O is insufficient, the dissolution of the metal ions will not proceed, and the material will not harden at room temperatures of around 15 to 20°C. Therefore, preliminary tests were conducted by varying the molar ratio (SiO2 / Na2O) of sodium silicate (Na2O·nSiO2) from 2 to 3.1 and the sodium oxide (Na2O) concentration from 9.2 to 14.5%. As a result, it was confirmed that within the above ranges, bleeding was suppressed, pot life was secured, and strength was developed at room temperature, but sodium silicate with SiO2 / Na2O (molar ratio) = 2.0 and Na2O concentration of 14.1 to 14.5% was used in the main tests because it allows the amount of additive to be reduced and is more economical.
[0027] [Admixture] Preliminary tests were conducted using several types of admixtures, and it was found that two types of admixtures whose main components are surfactants were highly effective in reducing the amount of dewatering under pressure when added in small amounts, and so they were used in the main tests.
[0028] Next, Table 2 shows a mix chart of the property tests conducted on the environmentally friendly ground improvement material of the present invention.
[0029] [Table 2] In Table 2, the admixtures were added in proportions relative to the water.
[0030] A mortar mixer (Marui mortar mixer (product number: MIC-362-1-01)) was used for mixing. The stirring speed was 140 rpm for rotation and 62 rpm for revolution. After the aggregate, ground granulated blast furnace slag, and light calcium carbonate were charged into the mortar mixer and stirred and mixed, water was charged and stirred for 30 seconds. Sodium silicate was then added and stirred for 30 seconds, after which the admixture was added and stirred for 90 seconds. For the mix without admixture, sodium silicate was added and stirred for 120 seconds. Here, the addition of sodium silicate produces a floc-like non-uniform gel, but stirring is intended to crush and refine the floc-like non-uniform gel and promote gelation. After kneading, a pressure bleeding test, a pumping test and a vane shear test were carried out. For practical use, for example, a mortar mixer manufactured by Kitagawa Iron Works (product name: WA series forced twin-shaft mixer) can be used.
[0031] The liquid powder ratio (wt%) is calculated by (WG+W) / (P+F). The aggregate paste ratio (vol%) is (S / ρ S ) / (P / ρ P +F / ρ F +WG / ρ WG +W / ρ W ) value. The filler replacement rate (wt%) is a value calculated by F / (S+P+F).
[0032] [Pressure bleeding test] In the pressurized bleeding test (JSCE-F 502, Japan Society of Civil Engineers, Standard Specifications for Concrete), a pressure of 3.5 MPa is applied to the top surface of the sample in the container for 10 minutes to measure the amount of dehydration. However, if the amount of dehydration falls below 2 ml / min after 3 minutes or more, the pressure is increased to 5 MPa and then released. Here, the test method of JSCE-F 502 is not suitable for examining a mixture that can be pumped at a pressure of 7 MPa, because the test pressure is too low. Therefore, in accordance with JSCE-F 502, a pressurized bleeding test was conducted in the following manner. The pressure on the top surface of the sample in the container is 5 MPa for 10 minutes and the amount of dehydration is measured. After 10 minutes, increase the pressure to 7MPa, measure the amount of water removed, and then release the pressure.
[0033] [Pump pressure test] The pumping test was carried out using a squeeze pump (Okasanki Kogyo Co., Ltd., model number: OPK-07M), with a hose (5 m) attached to the pump discharge port and an SGP pipe with an inner diameter of 16 mm attached to the end of the hose to create a pressure loss. The mixed material was put into the hopper and the pump was operated, and the material discharged from the end of the SGP pipe was returned to the hopper and circulated. The pump speed was gradually increased, and when the pumping pressure reached 0.5 MPa, the pump speed was kept constant, and if there were no abnormalities such as a sudden rise in pressure or blockage, the pump speed was further increased, and when the pumping pressure reached 1 MPa, the pump speed was kept constant, and if any abnormalities such as a sudden rise in pressure or blockage occurred, the pump was stopped.
[0034] [Vane shear test] The vane shear test was performed according to the Geotechnical Society standard JGS 1411-2012, and vane shear strength was calculated from the measured maximum torque value. The vane dimensions were width D = 20 mm x height H = 40 mm. To evaluate the sustainability of pumpability, vane shear strength was measured on samples immediately after mixing and after remixing every 0.5, 1, 3, and 24 hours.
[0035] [Property test 1] The materials were mixed according to the compositions No. 1 to No. 3 (comparative examples) and No. 4 (embodiment), and then subjected to a pressure bleeding test at a pressure of 7 MPa and a pumping test. The results are shown in Table 3.
[0036] [Table 3]
[0037] From Table 3, No. 1 to No. 3 (comparative examples) in which the aggregate paste ratio exceeds 100 vol% had low 60-second dehydration rates and final dehydration rates, but could not be pumped at a pumping pressure of 1 MPa in the pumping test. No. 4 (example) had the highest 60-second dehydration rate and final dehydration rate, but could be pumped at a pumping pressure of 1 MPa in the pumping test. When the aggregate paste ratio exceeds 100 vol%, the mixture is aggregate-rich and there is not enough paste, so even a small amount of pressurized dehydration causes the hose to become clogged and pumping becomes impossible. On the other hand, when the aggregate paste ratio is less than 100 vol%, that is, when the mixture is paste-rich, even if a small amount of pressurized dehydration occurs, excess paste continues to exist around the aggregate, so pumpability is maintained.
[0038] [Property test 2] Based on the results of property test 1, a pressure bleeding test and a pumping test were further carried out at a pressure of 7 MPa to investigate the blending conditions that contribute to reducing the amount of dehydration under pressure. The results are shown in Table 4.
[0039] [Table 4]
[0040] From Table 4, Nos. 5 to 6 (comparative examples) and Nos. 7 to 9 (embodiments) having a large liquid-powder ratio have a relatively large amount of pressurized dehydration compared to Nos. 10 to 25 (embodiments). Although the amount of water removed by pressure was increased, the addition of admixtures was found to have a suppressing effect on the amount of water removed by pressure. The amount of admixture that could be suppressed by pressure was reduced with less addition of BT2 than with BT1. It was found that when the liquid-powder ratio was 180wt% or more, it was necessary to add at least W x 0.25% for BT1 and at least W x 0.1% for BT2. In No. 12 (Example) using S3 as aggregate and No. 15 (Example) using S4, the amount of dehydration under pressure was suppressed without adding admixtures, and in particular, S4 was more effective in suppressing the amount of dehydration under pressure. By using S3 or S4 as aggregate, a paste-rich state is maintained without adding admixtures, so pumpability is maintained at a pressure of 7 MPa, but it was found that the risk of pipe clogging is further reduced by adding BT2 at W x 0.1% or more. The liquid powder ratio and aggregate paste ratio were recalculated by subtracting the final dewatering amount from the initial mix, and the results showed that No. 5 (comparative example) had an aggregate paste ratio of over 100% after pressure dewatering, making it aggregate-rich, and therefore pumpability was not maintained when pressurized at 7 MPa. No. 6 (comparative example) had an aggregate paste ratio of 88.7% after pressure dewatering, which did not exceed 100%, but there was little excess paste around the aggregate, so pumpability was not maintained when pressurized at 7 MPa, and there was a risk of the pipes becoming clogged.
[0041] [Property test 3] Table 5 shows the results of measuring the vane shear strength of samples immediately after mixing and after remixing every 0.5, 1, 3 and 24 hours. The x in the table indicates that the vane shear strength is 6.8 kN / m 2 This indicates that the measurement range was exceeded and the test could not be performed.
[0042] [Table 5]
[0043] From Table 5, the vane shear strength is 6.8 kN / m 2If this occurs, it is estimated that the fluidity will decrease significantly and pumpability will not be maintained, and there is an extremely high risk of pipes becoming clogged during ground improvement work. Among the mixtures using S2 as aggregate, No. 19 to No. 21 (Examples) with a liquid powder ratio of about 60% maintain fluidity for 30 minutes, but the fluidity decreases after one hour, so ground improvement work must be completed within 30 minutes. Construction vehicles should be allowed to pass through one hour after the completion of work. In such cases, No. 19 to No. 21 (Examples) are superior materials. On the other hand, when it is necessary to maintain fluidity for a long time (e.g., 3 hours or more) with a mixture using S2 as the aggregate, the filler replacement rate is set to about 20 wt% or more and the liquid powder ratio is set to about 80 wt% or more, as in No. 10 and No. 16 to No. 18 (Examples). No. 22 to No. 23 (Examples) using S3 as aggregate showed little change in vane shear strength even after 3 hours, even when the liquid powder ratio was about 60%, at a filler replacement rate of about 20wt% or more, and fluidity was maintained. No. 16 and No. 24 to No. 25 (Examples) without adding F and with a liquid powder ratio of 87 to 89wt% showed low vane shear strength even after 24 hours, and fluidity was maintained. On the other hand, as the ratio of F in P:F increases, the vane shear strength also tends to increase, and it is thought that the maintenance time of pumpability is shortened. S3 and S4 showed less change in vane shear strength compared to S2, and S4 showed even less change. In addition, in the case of a mix using S2 as the aggregate, as in No. 4 (Example), the filler replacement rate is about 20 wt% or more and the liquid powder ratio is about 40 wt% or more.
[0044] [CO2 storage and CO2 emissions] Table 6 shows the unconfined compressive strength of No. 4 and No. 7 to No. 25 (Examples), the amount of CO2 stored as CaCO3 by the execution of ground improvement work, and the amount of CO2 emitted by the ground improvement material. Here, the amount of CO2 stored is the value obtained by multiplying the amount of F mixed by the CO2 emission intensity. The amount of CO2 emitted is the total value obtained by multiplying the amount of F mixed by the CO2 emission intensity of each material.
[0045] [Table 6]
[0046] From Table 6, all the examples are 1MN / m 2 or more (1~21.5MN / m 2 ) of uniaxial compressive strength, and can be used appropriately according to the uniaxial compressive strength required for various construction methods aimed at ground improvement. Here, the strength ratio between the on-site and indoor ground improvement work is said to be about 1 / 5 to 1, and generally 1 / 3 is used. Therefore, when using the environmentally friendly ground improvement material of the present invention, the design strength is 1MN / m 2 ×1 / 5 ≒ 0.2MN / m 2 More than one degree can be applied. In addition, the amount of CO2 stored when F was added in the examples was 1 m 3 111-267kg-CO2 / m per use 3 This results in CO2 emissions. No. 24 to No. 25 (Examples) in which no F was added also had a CO2 content of 22 kg / m 3 This contributes to reducing CO2 emissions compared to ground improvement work that uses conventional cement-based solidification materials.
[0047] From the property tests 1 to 3, it can be said that the environmentally friendly ground improvement material of the present invention has the following effects. The environmentally friendly ground improvement material contains at least aggregate, ground granulated blast furnace slag, sodium silicate and water, but does not contain cement, and has resistance to material separation when pumped at a pressure of 5 MPa or more (5-7 MPa), allowing it to be pumped into the ground without clogging the piping. The fluidity maintenance time can be adjusted according to the time required from mixing the environmentally friendly ground improvement material to pressing it into the ground. By mixing light calcium carbonate as a filler to replace part of the aggregate or solidification material, CO2 derived from exhaust gas can be mineralized in the form of calcium carbonate (CaCO3) and then stored underground as part of the ground improvement work.
[0048] The above describes the environmentally friendly ground improvement material of the present invention based on its embodiment, but the present invention is not limited to the configuration described in the above embodiment, and the configuration can be changed as appropriate within the scope that does not deviate from the spirit of the present invention. [Industrial Applicability]
[0049] The environmentally friendly ground improvement material of the present invention can instantly thicken to reduce bleeding and material separation during pumping while maintaining a long pot life. In addition, the pressure during pumping can increase to 5 MPa or more (5 to 7 MPa), and even if the amount of pressurized dewatering increases, the pipes will not become clogged. In addition, CO2 emissions can be suppressed, so the material can be widely used in various construction methods aimed at ground improvement.
Claims
1. An environmentally friendly ground improvement material that contains at least aggregate, ground granulated blast furnace slag, sodium silicate, and water, does not contain cement, and is used by pumping at a pressure of 5 MPa or more, and satisfies the following conditions (1) and (2). (1) The aggregate paste ratio in the initial mix is less than 100 vol.% and the aggregate paste ratio after dehydration at 7 MPa is less than 80 vol.%. (2) The final dehydration rate in the 7 MPa pressure bleeding test is less than 15%.
2. The environmentally friendly ground improvement material according to claim 1, further satisfying the following condition (3). (3) After 0.5 hours, the vane shear strength is 6.8 kN / m 2 Less than
3. 1 m of the environmentally friendly ground improvement material 3 Hit CO 2 The environmentally friendly ground improvement material according to claim 1 or 2, wherein the discharge amount is −350 to 100 kg.
4. The environmentally friendly ground improvement material according to claim 1 or 2, further comprising an inert filler, the inert filler being made of light calcium carbonate produced using an aqueous calcium hydroxide solution and carbon dioxide as raw materials.
5. The environmentally friendly soil improvement material according to claim 1 or 2, further comprising an admixture for improving pumpability.
6. The fineness of the ground granulated blast furnace slag is 3500 to 5000 cm 2 The environmentally friendly ground improvement material according to claim 1 or 2, wherein the average molecular weight of the soil is 1000 or more.
Citation Information
Patent Citations
Accumulating circuit
JP1980090702A
Winding structure of dual-gap magnetic head
JP1985005408A
Caliper rotation type disc brake
JP1985034530A
Mixed material for fluidized sand, manufacturing method thereof, improved fluidized sand composition and manufacturing method thereof
JP2021025289A
Blast furnace slag-containing cement slurry composition and method for preparing soil cement slurry using the same
JP6955967B2