Nonaqueous electrolyte secondary battery, battery pack, and battery module

The non-aqueous electrolyte secondary battery addresses uneven salt concentration and positive electrode potential issues by using a specific electrolyte composition and pressure application, achieving low output resistance and high cycle capacity retention.

JP2024165642AActive Publication Date: 2024-11-28PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023082005
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-28
Estimated Expiration
2043-05-18

AI Technical Summary

Technical Problem

In non-aqueous electrolyte secondary batteries with wide electrode bodies, uneven salt concentration and increased positive electrode potential lead to capacity deterioration due to pressure applied in the electrode plate lamination direction, causing transition metal elution and deposition on the negative electrode.

Method used

A non-aqueous electrolyte secondary battery design with a wound electrode body, using a specific electrolyte composition of LiPF6 and LiBF4 with a controlled A/B ratio, and applying pressure in the electrode plate stacking direction to maintain a sufficient LiF film on the positive electrode active material, reducing output resistance and suppressing cycle deterioration.

Benefits of technology

The solution results in a battery with low output resistance and improved cycle characteristics, maintaining a capacity retention rate of 90% or more through controlled electrolyte distribution and reduced transition metal elution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165642000001_ABST
    Figure 2024165642000001_ABST
Patent Text Reader

Abstract

To provide a nonaqueous electrolyte secondary battery which includes a wide electrode body and is subjected to pressure in the electrode plate stacking direction of the electrode body, and which has low output resistance and suppresses deterioration of cycle characteristics, and to provide a battery pack and a battery module including the same.SOLUTION: A nonaqueous electrolyte secondary battery includes a wound-type electrode body and an electrolyte, and a positive electrode plate includes a positive electrode active material layer, and a negative electrode plate includes a negative electrode active material layer, at least one of the positive electrode active material layer and the negative electrode active material layer has a dimension of 150 mm or more in a winding axis direction of an electrode body, the electrolyte includes an electrolyte salt and LiFSO3, the electrolyte salt comprises at least one of LiPF6 and LiBF4, a ratio A / B of a total concentration A (mol / L) of LiPF6 and LiBF4 to a concentration B (mol / L) of LiFSO3 in the electrolyte is 5 or more and 12 or less, and the electrode body is subjected to a pressure of 0.5 MPa or more in a stacking direction of the electrode plates.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery, and further to a battery pack and a battery module including the same. [Background technology]

[0002] For the purpose of improving the input / output characteristics and impedance characteristics after endurance testing in a nonaqueous electrolyte secondary battery, Patent Document 1 proposes a nonaqueous electrolyte solution containing LiPF6 and LiFSO3, and Patent Document 2 proposes setting the ratio of the molar content of FSO3 to the molar content of PF6 within a specific range. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-152956 A [Patent Document 2] JP 2011-187440 A Summary of the Invention [Problem to be solved by the invention]

[0004] In non-aqueous electrolyte secondary batteries that include wide electrode bodies (e.g., active material layers with a longitudinal dimension of 15 cm or more), when pressure is applied to the electrode body in the direction of electrode plate stacking, salt concentration unevenness is likely to occur during high-rate cycles, leading to a large increase in the positive electrode potential and a tendency for capacity degradation to occur. When an electrolyte containing LiFSO3 is used, SO3F - is adsorbed on the surface of the positive electrode active material, which tends to inhibit the formation of the LiF film derived from the electrolyte salt, and when the cell size is large, the salt concentration unevenness due to high-rate charging cycles becomes significant, and the salt concentration at the end of the plate tends to decrease. As a result, the potential at the end of the positive plate increases, and the positive electrode active material and the highly acidic SO3F -This is presumably because the potential reaches a point at which the transition metal reacts with the positive electrode active material, which has an insufficient LiF coating, dissolves out of the positive electrode active material, and accumulates on the negative electrode plate.

[0005] An object of the present disclosure is to provide a nonaqueous electrolyte secondary battery that includes a wide electrode assembly and is subjected to pressure in the electrode plate stacking direction of the electrode assembly, and that has low output resistance and suppressed deterioration of cycle characteristics, as well as a battery pack and a battery module that include the same. [Means for solving the problem]

[0006] The present disclosure provides the following nonaqueous electrolyte secondary battery, battery pack, and battery module. [1] A battery comprising an electrode body and an electrolyte solution, The electrode body is a wound electrode body in which a positive electrode plate and a negative electrode plate are wound with a separator interposed therebetween, The positive electrode plate includes a positive electrode active material layer, The negative electrode plate includes a negative electrode active material layer, At least one of the positive electrode active material layer and the negative electrode active material layer has a dimension of 150 mm or more in the winding axis direction of the electrode body, The electrolyte solution contains an electrolyte salt and LiFSO3, The electrolyte salt contains at least one of LiPF6 and LiBF4, When the total concentration of LiPF6 and LiBF4 in the electrolyte is A (mol / L) and the concentration of LiFSO3 is B (mol / L), the A / B ratio, which is the ratio of A to B, is 5 to 12, A nonaqueous electrolyte secondary battery, wherein a pressure of 0.5 MPa or more is applied to the electrode assembly in a stacking direction of the electrode plates. [2] The nonaqueous electrolyte secondary battery according to [1], wherein the A / B ratio is 6.7 or more and 10 or less. [3] The nonaqueous electrolyte secondary battery according to [1] or [2], wherein a total concentration A of LiPF6 and LiBF4 in the electrolyte is 1 to 1.5 mol / L. [4] The nonaqueous electrolyte secondary battery according to any one of [1] to [3], wherein the concentration B of LiFSO3 in the electrolyte is 0.1 to 0.25 mol / L. [5] The nonaqueous electrolyte secondary battery according to any one of [1] to [4], wherein the electrode body has a length parallel to the winding axis of 180 mm or more. [6] A battery pack comprising the nonaqueous electrolyte secondary battery according to any one of [1] to [5]. [7] A battery module comprising the nonaqueous electrolyte secondary battery according to any one of [1] to [5]. Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a nonaqueous electrolyte secondary battery that includes a wide electrode assembly and is subjected to pressure in the electrode plate stacking direction of the electrode assembly, the nonaqueous electrolyte secondary battery having low output resistance and suppressed deterioration in cycle characteristics, as well as a battery pack and a battery module including the same. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic diagram showing an example of the configuration of a nonaqueous electrolyte secondary battery according to this embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing an example of the configuration of the electrode body in this embodiment. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing an example of the configuration of the electrode body in this embodiment. [Figure 4] FIG. 4 is a schematic diagram showing an example of the configuration of the electrode body in this embodiment. [Diagram 5] FIG. 5 is a perspective view showing an example of a battery pack according to the present embodiment. [Figure 6] FIG. 6 is a perspective view showing an example of a battery module in the present embodiment. [Figure 7] FIG. 7 is a schematic diagram for explaining a method for restraining a battery in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings, but the present invention is not limited to the following embodiment. In all of the drawings, the scale of each component is appropriately adjusted to make it easier to understand, and the scale of each component shown in the drawings does not necessarily match the scale of the actual component.

[0010] In this specification, elements expressed in the singular form include the plural form unless otherwise specified. For example, a "particle" can mean not only "one particle" but also "an aggregate of particles (powder, powder, particle group)."

[0011] FIG. 1 is a schematic diagram showing an example of the configuration of a battery in this embodiment. The battery 100 can be used for any purpose. For example, the battery 100 may be used as a main power source or a power source for power assist in an electric vehicle or the like. A battery module or a battery pack may be formed by connecting a plurality of batteries 100. The battery module and the battery pack will be described later. The battery 100 may have a rated capacity of, for example, 1 to 300 Ah.

[0012] The battery 100 includes an electrode assembly 50 and an electrolyte. As shown in FIG. 1, the battery 100 may further include an exterior body 90. The exterior body 90 houses the electrode assembly 50 and an electrolyte (not shown). The exterior body 90 is rectangular (flattened rectangular parallelepiped). The exterior body 90 may be made of, for example, an aluminum (Al) alloy. A pressure of 0.5 MPa or more is applied to the electrode assembly 50 in the electrode plate stacking direction (D-axis direction in FIG. 1). The pressure may be applied from the outside of the electrode assembly 50. The pressure applied to the electrode assembly may be an area indicated by the electrode assembly area S shown in FIG. 4. FIG. 4 will be described later. The electrode assembly 50 may be in a state of being restrained within the exterior body 90. The force that restrains the electrode assembly 50 may be the above pressure. The force that restrains the electrode assembly 50 may be, for example, a force that restrains a plurality of batteries and inter-cell separators in a battery module described later.

[0013] The exterior body 90 may include, for example, a sealing plate 91 and an exterior can 92. The sealing plate 91 closes the opening of the exterior can 92. For example, the sealing plate 91 and the exterior can 92 may be joined by laser processing or the like. The exterior body 90 may have any shape. The exterior body 90 may be, for example, in a pouch shape. That is, the exterior body 90 may be a pouch made of an Al laminate film or the like.

[0014] The sealing plate 91 is provided with a positive electrode terminal 81 and a negative electrode terminal 82. The sealing plate 91 may further be provided with an injection port (not shown), a gas exhaust valve (not shown), and the like. An electrolyte may be injected into the exterior body 90 from the injection port. The injection port may be closed by, for example, a sealing plug. The positive electrode current collecting member 71 connects the positive electrode terminal 81 and the electrode body 50. The positive electrode current collecting member 71 may be, for example, an Al plate. The negative electrode current collecting member 72 connects the negative electrode terminal 82 and the electrode body 50. The negative electrode current collecting member 72 may be, for example, a copper (Cu) plate.

[0015] The electrode body 50 is a wound type electrode body in which a positive electrode plate and a negative electrode plate are wound with a separator interposed therebetween. The positive electrode plate, the negative electrode plate, and the separator may form a laminate having, for example, a band-like planar shape. A wound body may be formed by spirally winding the band-like laminate. The wound body may be, for example, cylindrical. A flat electrode body 50 may be formed by radially compressing the cylindrical wound body. The dimension of the electrode body 50 in the winding axis direction (hereinafter also referred to as the width direction) (W-axis direction in FIG. 1) may be, for example, 180 mm or more, or may be 180 mm or more and 300 mm or less.

[0016] FIG. 2 is a schematic diagram showing an example of the configuration of the electrode body in this embodiment. The electrode body 50 in FIG. 2 is a wound type electrode body having a winding axis R parallel to the W-axis direction. The electrode body 50 includes a laminate 40. The electrode body 50 may be substantially composed of the laminate 40. The laminate 40 includes a positive electrode plate 10, a negative electrode plate 20, and a separator 30. At least a part of the separator 30 is interposed between the positive electrode plate 10 and the negative electrode plate 20. The separator 30 separates the positive electrode plate 10 and the negative electrode plate 20. The positive electrode plate 10 and the negative electrode plate 20 may each be bonded to the separator 30. The laminate 40 may include one separator 30 alone. The laminate 40 may include two separators 30. For example, the positive electrode plate 10 may be sandwiched between two separators 30. For example, the negative electrode plate 20 may be sandwiched between two separators 30. The laminate 40 may be formed, for example, by laminating a separator 30 (first separator), a negative electrode plate 20, a separator 30 (second separator), and a positive electrode plate 10 in this order.

[0017] FIG. 3 is a schematic cross-sectional view showing an example of the configuration of the electrode body in this embodiment. FIG. 3 shows a cross section perpendicular to the winding axis. The electrode body 50 includes a curved portion 51 and a flat portion 52. At the curved portion 51, the laminate 40 is curved. At the curved portion 51, the laminate 40 may be arc-shaped. At the flat portion 52, the laminate 40 is flat. The flat portion 52 is sandwiched between the two curved portions 51. The flat portion 52 connects the two curved portions 51. The thickness of the laminate 40 indicates the total thickness of the positive electrode plate 10, the negative electrode plate 20, and the separator 30 included in the laminate 40. The laminate 40 may have a thickness of, for example, 100 to 400 μm, or may have a thickness of 1 to 300 μm. The thickness of the laminate 40 is the thickness in the electrode body stacking direction (D-axis direction in FIG. 3).

[0018] In the electrode body 50, the positive electrode plates 10 may have any number of layers. The number of layers of the positive electrode plates 10 indicates the number of times that a straight line that cuts the electrode body 50 in the layering direction intersects with the positive electrode plates 10. The layering direction indicates the direction in which the positive electrode plates 10, the negative electrode plates 20, and the separators 30 are layered in the electrode body 50. The layering direction in the wound electrode body 50 is parallel to the thickness direction of the positive electrode plates 10, the negative electrode plates 20, and the separators 30 in the flat portion 52 (the D-axis direction in FIG. 3).

[0019] As shown in FIG. 4, the electrode body 50 can be produced by stacking a positive electrode plate 10 and a negative electrode plate 20 with a separator 30 between them so that the aluminum foil of the positive electrode plate and the copper foil of the negative electrode plate are exposed at both ends, and then winding the laminate around one end of the laminate as the winding axis R.

[0020] The positive electrode plate 10 may have a number of laminations of, for example, 2 to 100. The negative electrode plate 20 may have a number of laminations of, for example, 2 to 100. The separator 30 may have a number of laminations of, for example, 4 to 200. The number of laminations of the negative electrode plate 20 and the separator 30 may be counted in the same manner as the number of laminations of the positive electrode plate 10.

[0021] The positive electrode plate 10 includes a positive electrode active material layer. In Fig. 1, the dimension of the positive electrode active material layer in a direction parallel to the winding axis direction (W axis direction) of the electrode body 50 is 150 mm or more, and may be, for example, 180 mm or more, 200 mm or more, or 220 mm or more, or may be 300 mm or less. The positive electrode active material layer will be described later.

[0022] The negative electrode plate 20 includes a negative electrode active material layer. In Fig. 1, the dimension of the negative electrode active material layer in a direction parallel to the winding axis direction (W-axis direction) of the electrode body 50 is 150 mm or more, and may be, for example, 180 mm or more, 200 mm or more, or 220 mm or more, or may be 300 mm or less. The negative electrode active material layer will be described later.

[0023] The positive electrode plate 10 includes a positive electrode core material 11 and a positive electrode active material layer 12 (see FIG. 2). The positive electrode active material layer 12 may be disposed on the surface of the positive electrode core material 11. The positive electrode active material layer 12 may be disposed on only one side of the positive electrode core material 11. The positive electrode active material layer 12 may be disposed on both the front and back sides of the positive electrode core material 11. The positive electrode core material 11 is a conductive sheet. The positive electrode core material 11 may include, for example, pure Al foil, Al alloy foil, or the like. The positive electrode core material 11 may have a thickness of, for example, 10 to 30 μm. The positive electrode core material 11 may be exposed at one end in the width direction (W-axis direction in FIG. 2) of the electrode body 50. A positive electrode current collecting member 71 may be joined to the exposed portion of the positive electrode core material 11 (see FIG. 1). The thickness of the positive electrode plate 10 may be, for example, 20 to 290 μm, 50 to 250 μm, or 100 to 200 μm. The longitudinal dimension of the positive electrode plate 10 may be, for example, 0.5 to 10 m, or 1 to 5 m.

[0024] The thickness of the positive electrode active material layer 12 indicates the total thickness of the positive electrode active material layers 12 included in the laminate 40. For example, when the positive electrode active material layers 12 are formed on both sides of the positive electrode plate 10, the thickness of the positive electrode active material layer 12 indicates the total thickness of the positive electrode active material layers 12 on both sides (two). The positive electrode active material layer 12 may have a thickness of, for example, 10 to 260 μm, may have a thickness of 20 to 60 μm, or may have a thickness of 30 to 50 μm. The thickness of the positive electrode active material layer 12 on one side (one) may have a thickness of, for example, 5 to 130 μm, may be 10 to 30 μm, or may be 15 to 25 μm.

[0025] The positive electrode active material layer 12 may contain a lithium transition metal composite oxide. The lithium transition metal composite oxide may contain at least one selected from the group consisting of LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(NiCoMn)O2, Li(NiCoAl)O2, and LiFePO4. For example, in the composition formula of "Li(NiCoMn)O2", the sum of the composition ratios in parentheses is 1. That is, "C Ni +C Co +C Mn =1" relationship is satisfied. For example, "C Ni" indicates the composition ratio of Ni. The composition ratio of each component is arbitrary as long as the sum of the composition ratios is 1. The positive electrode active material layer 12 may contain positive electrode active material particles. The positive electrode active material particles may contain any component. The positive electrode active material particles may contain the above-mentioned lithium transition metal composite oxide.

[0026] The positive electrode active material layer 12 may further contain, for example, a conductive material, a binder, and the like, in addition to the positive electrode active material particles. For example, the positive electrode active material layer 12 may be substantially composed of, by mass fraction, 0.1 to 10% of a conductive material, 0.1 to 10% of a binder, and the remainder being positive electrode active material particles. The conductive material may contain, for example, a carbon material, and the like. The binder may contain any component. The binder may contain, for example, polyvinylidene fluoride (PVdF), and the like. The packing density (after compression) of the positive electrode active material layer 12 is, for example, 2.0 g / cm. 3 More than 4.0g / cm 3 It may be the following:

[0027] The negative electrode plate 20 includes a negative electrode core material 21 and a negative electrode active material layer 22 (see FIG. 2). The negative electrode active material layer 22 may be disposed on the surface of the negative electrode core material 21. The negative electrode active material layer 22 may be disposed on only one side of the negative electrode core material 21. The negative electrode active material layer 22 may be disposed on both the front and back sides of the negative electrode core material 21. The negative electrode core material 21 is a conductive sheet. The negative electrode core material 21 may include, for example, a pure Cu foil, a Cu alloy foil, or the like. The negative electrode core material 21 may have a thickness of, for example, 5 to 30 μm. In the width direction (W-axis direction in FIG. 2) of the negative electrode plate 20, the negative electrode core material 21 may be exposed at one end. A negative electrode current collecting member 72 may be joined to the exposed portion of the negative electrode core material 21 (see FIG. 1). The thickness of the negative electrode plate 20 may be, for example, 20 to 290 μm, 50 to 250 μm, or 100 to 200 μm. The longitudinal dimension of the negative electrode plate 20 may be, for example, 0.5 to 10 m, or 1 to 5 m.

[0028] The thickness of the negative electrode active material layer 22 indicates the total thickness of the negative electrode active material layers 22 included in the laminate 40. For example, when the negative electrode active material layers 22 are formed on both sides of the negative electrode plate 20, the thickness of the negative electrode active material layers 22 indicates the total thickness of the negative electrode active material layers 22 on both sides (two). The negative electrode active material layers 22 may have a thickness of, for example, 10 to 260 μm, may have a thickness of 40 to 80 μm, or may have a thickness of 50 to 70 μm. The thickness of the negative electrode active material layer 22 on one side (one) may have a thickness of, for example, 5 to 130 μm, may be 20 to 40 μm, or may be 25 to 35 μm. The packing density (after compression) of the negative electrode active material layers 22 is, for example, 1.0 g / cm. 3 More than 1.8g / cm 3 It may be the following:

[0029] The negative electrode active material layer 22 is made of, for example, graphite, silicon, silicon oxide, tin, tin oxide, and Li4Ti5O 12 The negative electrode active material layer 22 may contain at least one selected from the group consisting of the negative electrode active material. The negative electrode active material layer 22 may contain negative electrode active material particles. The negative electrode active material particles may contain the above-mentioned negative electrode active material. The negative electrode active material layer 22 may be substantially composed of negative electrode active material particles. The negative electrode active material particles may be, for example, composite particles. The negative electrode active material particles may contain, for example, a substrate particle and a coating. The coating may cover the surface of the substrate particle. The substrate particle may contain, for example, graphite, etc. The coating may contain, for example, amorphous carbon, etc.

[0030] The negative electrode active material layer 22 may further contain a conductive material, a binder, and the like in addition to the negative electrode active material particles. For example, the negative electrode active material layer 22 may be substantially composed of 0 to 10% by mass of a conductive material, 0.1 to 10% by mass of a binder, and the remainder being negative electrode active material particles. The conductive material may contain any component. The conductive material may contain, for example, a carbon material. The binder may contain any component. The binder may contain, for example, at least one selected from the group consisting of carboxymethyl cellulose (CMC) and styrene butadiene rubber (SBR).

[0031] The separator 30 includes a resin film. The separator 30 may be substantially composed of a resin film. The separator 30 may have a single-layer structure made of one resin film, or may have a multi-layer structure made of two or more resin films. When the separator 30 has a multi-layer structure, the resin films may be different types of resin films. The resin film may be substantially made of, for example, a polyolefin-based material. The polyolefin-based material may include, for example, at least one selected from the group consisting of polyethylene (PE) and polypropylene (PP). When the separator 30 has a multi-layer structure, the separator 30 may have a three-layer structure made of, for example, a resin film made of PP / a resin film made of PE / a resin film made of PP. The resin film may have a thickness of, for example, 10 to 50 μm, may have a thickness of 10 to 30 μm, or may have a thickness of 10 to 20 μm. The resin film may be porous.

[0032] The electrolyte is a liquid electrolyte. The electrolyte contains an electrolyte salt and LiFSO3. The electrolyte salt may be dissolved in a solvent described later in the electrolyte.

[0033] The electrolyte salt contains at least one of LiPF6 and LiBF4. The electrolyte salt may contain LiPF6 alone, may contain LiBF4 alone, or may contain both LiPF6 and LiBF4. When the total concentration of LiPF6 and LiBF4 in the electrolyte is A (mol / L) and the concentration of LiFSO3 is B (mol / L), the A / B ratio, which is the ratio of A to B, is 5 to 12. By setting A / B within the above range, at least one of LiPF6 and LiBF4 is sufficiently present relative to LiFSO3, a sufficient LiF film is formed on the surface of the positive electrode active material, and the elution of the active material transition metal caused by LiFSO3 is unlikely to occur, and as a result, it is presumed that a battery that can exhibit low output resistance and good cycle characteristics can be obtained. The A / B ratio is preferably 5 to 10, more preferably 6.7 to 10, from the viewpoint of output resistance and cycle characteristics.

[0034] The total concentration A of LiPF6 and LiBF4 in the electrolyte may be, for example, 1.0 to 1.5 mol / L. The concentration B of LiFSO3 in the electrolyte may be, for example, 0.1 to 0.25 mol / L.

[0035] The electrolytic solution may contain a solvent. The solvent is aprotic. The solvent may contain any component. The solvent may contain at least one selected from the group consisting of carbonate-based solvents, 1,2-dimethoxyethane (DME), methyl formate (MF), methyl acetate (MA), methyl propionate (MP), and γ-butyrolactone (GBL). The solvent preferably contains a carbonate-based solvent. Examples of carbonate-based solvents include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC).

[0036] The battery of the present disclosure can have a capacity retention rate of 90% or more in an evaluation of cycle characteristics. When the cycle capacity retention rate is 90% or more, the battery can have good cycle characteristics. The evaluation of cycle characteristics is performed according to the method described in the Examples section below.

[0037] The method for manufacturing a battery may include, for example, an accommodation step of accommodating the electrode body in an exterior body, and an electrolyte injection step. In the accommodation step, the aluminum foil of the positive current collecting member and the aluminum plate for external current collection of the electrode body are welded, and the copper foil of the negative current collecting member and the copper plate for external current collection of the electrode body are welded, and the battery is inserted into the outer case of the aluminum laminate film. In the electrolyte injection step, the above-mentioned electrolyte can be injected. After the electrolyte injection, the battery can be obtained by sealing and welding the can.

[0038] (Battery pack) Fig. 5 is a perspective view of a battery pack 200. The battery pack 200 shown in Fig. 5 includes batteries 100 and inter-cell separators 201. The batteries 100 and the inter-cell separators 201 are arranged alternately along the Y-axis direction (first direction).

[0039] The batteries 100 are rectangular battery cells, and a plurality of batteries 100 are provided along the Y-axis direction. The plurality of batteries 100 are electrically connected to each other via bus bars (not shown).

[0040] Inter-cell separators 201 are provided between multiple batteries 100. The inter-cell separators 201 prevent unintended electrical conduction between adjacent batteries 100. The inter-cell separators 201 ensure electrical insulation between adjacent batteries 100.

[0041] (Battery module) 6 is a perspective view of a battery module 300. As shown in FIG 3, the battery module 300 includes batteries 100, inter-cell separators 201, binding members 301, and end plates 302.

[0042] The batteries 100 and inter-cell separators 201 arranged alternately along the Y-axis direction (first direction) are pressed by the end plates 302 and are restrained between the two end plates 302.

[0043] The end plates 302 are disposed at both ends in the Y-axis direction. The end plates 302 are fixed to a base such as a case that houses the battery module 300. The restraining member 301 connects the two end plates 302 to each other and restrains the multiple batteries 100 and the inter-cell separators 201 along the Y-axis direction.

[0044] When a compressive force in the Y-axis direction is applied to the laminate of batteries 100, inter-cell separators 201, and end plates 302, restraining members 301 are fixed to end plates 302, and the compressive force is then released, causing a tensile force to act on restraining members 301 connecting the two end plates 302. In reaction to this, restraining members 301 press the two end plates 302 in a direction that brings them closer to each other. In this way, a battery module 300 is constructed.

[0045] A battery pack is constructed by housing the battery modules 300 in a pack case (cell-module-pack structure). Alternatively, the battery pack 200 shown in Fig. 5 may be directly supported by the wall of the pack case (cell-to-pack structure). EXAMPLES

[0046] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.

[0047] <Example 1> [Preparation of positive electrode plate] A positive electrode active material layer mixture having a composition of LiNiCoMnO2:AB:pVdF=100:1:1wt% was mixed with NMP to prepare a positive electrode mixture slurry. The mixture was applied onto an aluminum foil positive electrode current collector, dried, compressed to a specified thickness, and cut to a specified width to prepare a positive electrode plate consisting of a portion where the positive electrode active material layer was formed on the aluminum foil and a portion where the active material layer was not formed in the width direction. The width where the positive electrode active material layer was formed was set to 150 mm. [Preparation of negative electrode plate] Graphite was used as the negative electrode active material. A negative electrode active material layer mixture having a mixture composition of graphite:SBR:CMC=100:1:1wt% was mixed with water to prepare a negative electrode mixture slurry. The negative electrode mixture slurry was applied onto the copper foil of the negative electrode current collector, dried, compressed to a predetermined thickness, and cut to a predetermined width to prepare a negative electrode plate composed of a portion on the copper foil where the negative electrode active material layer was formed and a portion where the active material layer was not formed. The width where the negative electrode active material layer was formed was set to 154 mm. [Preparation of electrode body] An electrode body having the configuration shown in Fig. 4 was fabricated as follows: A positive electrode plate and a negative electrode plate were laminated with a separator consisting of three layers of polypropylene / polyethylene / polypropylene in between so that the positive electrode aluminum foil and the negative electrode copper foil were exposed at both ends to produce a laminate, and the laminate was wound around one end of the laminate as a winding axis to produce the electrode body.

[0048] [Preparation of non-aqueous electrolyte secondary battery] The aluminum foil of the positive current collector was welded to the aluminum plate for external current collection, and the copper foil of the negative current collector was welded to the copper plate for external current collection. These were then inserted into the outer shell of an aluminum laminate film, and the following electrolyte 1 was poured in, and the laminate film was sealed. (electrolyte 1) Solvent: EC / EMC (volume ratio 1:3) LiPF6 concentration (concentration A): 1mol / L LiFSO3 concentration (concentration B): 0.1mol / L

[0049] Next, as shown in FIG. 7, both side surfaces of the battery perpendicular to the winding axis of the electrode body were sandwiched between stainless steel restraint plates, and the four corners of these restraint plates were fastened with screws and nuts. The load was adjusted so that a restraint pressure of 0.5 MPa was applied to the electrode body area S (the width direction is the width for forming the positive electrode active material layer) shown in FIG. 4, and the battery was restrained to produce a nonaqueous electrolyte secondary battery.

[0050] <Comparative Example 1> A nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1, except that in the production of the positive electrode plate, the width over which the positive electrode active material layer was formed was 100 mm, in the production of the negative electrode plate, the width over which the negative electrode active material layer was formed was 104 mm, and the electrolyte solution 1 was changed to the following electrolyte solution 2. (electrolyte 2) Solvent: EC / EMC (volume ratio 1:3) LiPF6 concentration (concentration A): 1mol / L LiFSO3: None

[0051] <Comparative Example 2> A nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1, except that in the production of the positive electrode plate, the width over which the positive electrode active material layer was formed was 100 mm, in the production of the negative electrode plate, the width over which the negative electrode active material layer was formed was 104 mm, and the electrolyte solution 1 was changed to the following electrolyte solution 3. (Electrolyte 3) Solvent: EC / EMC (volume ratio 1:3) LiPF6 concentration (concentration A): 1mol / L LiFSO3 concentration (concentration B): 0.08mol / L

[0052] <Comparative Example 3> A nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1, except that in the production of the positive electrode plate, the width over which the positive electrode active material layer was formed was 100 mm, in the production of the negative electrode plate, the width over which the negative electrode active material layer was formed was 104 mm, and the electrolyte solution 1 was changed to the following electrolyte solution 4. (electrolyte 4) Solvent: EC / EMC (volume ratio 1:3) LiPF6 concentration (concentration A): 1mol / L LiFSO3 concentration (concentration B): 0.1mol / L

[0053] <Comparative Example 4> A nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1, except that in the production of the positive electrode plate, the width over which the positive electrode active material layer was formed was 100 mm, in the production of the negative electrode plate, the width over which the negative electrode active material layer was formed was 104 mm, and the electrolyte solution 1 was changed to the following electrolyte solution 5. (electrolyte 5) Solvent: EC / EMC (volume ratio 1:3) LiPF6 concentration (concentration A): 1mol / L LiFSO3 concentration (concentration B): 0.2mol / L

[0054] <Comparative Example 5> A nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1, except that in the production of the positive electrode plate, the width over which the positive electrode active material layer was formed was 100 mm, in the production of the negative electrode plate, the width over which the negative electrode active material layer was formed was 104 mm, and the electrolyte solution 1 was changed to the following electrolyte solution 6. (electrolyte 6) Solvent: EC / EMC (volume ratio 1:3) LiPF6 concentration (concentration A): 1mol / L LiFSO3 concentration (concentration B): 0.25mol / L

[0055] <Comparative Example 6> A nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1, except that the electrolyte solution 1 in Example 1 was changed to the electrolyte solution 2.

[0056] <Comparative Example 7> A nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1, except that the electrolyte solution 1 in Example 1 was changed to the electrolyte solution 3.

[0057] <Example 2> A nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1, except that the electrolyte solution 1 in Example 1 was changed to the electrolyte solution 7 below. (electrolyte 7) Solvent: EC / EMC (volume ratio 1:3) LiPF6 concentration (concentration A): 1mol / L LiFSO3 concentration (concentration B): 0.15mol / L

[0058] <Example 3> A nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1, except that the electrolyte solution 1 in Example 1 was changed to the electrolyte solution 5.

[0059] <Comparative Example 8> A nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1, except that the electrolyte solution 1 in Example 1 was changed to the electrolyte solution 6.

[0060] <Example 4> A nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1, except that the electrolyte solution 1 in Example 1 was changed to the electrolyte solution 8 below. (electrolyte 8) Solvent: EC / EMC (volume ratio 1:3) LiPF6 concentration (concentration A): 1.5mol / L LiFSO3 concentration (concentration B): 0.25mol / L

[0061] <Example 5> A nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1, except that the electrolytic solution 1 in Example 1 was changed to the following electrolytic solution 9. (electrolyte 9) Solvent: EC / EMC (volume ratio 1:3) Concentration A=1.0mol / L LiPF6 concentration: 0.9mol / L LiBF4 concentration: 0.1mol / L LiFSO3 concentration (concentration B): 0.2mol / L

[0062] <Comparative Example 9> A nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example 1, except that the electrolyte solution 1 in Example 1 was changed to electrolyte solution 7, and the battery was not restrained.

[0063] <Initial activation of non-aqueous electrolyte secondary batteries> After preparing a non-aqueous electrolyte secondary battery by the method described in each Example, the battery was initially activated by charging it at a current value of C / 10 at 4.2 Vccccv in a 25°C environment, storing it at 60°C for 24 hours, and discharging it to 3 V at a current value of C / 10.

[0064] <Evaluation method for non-aqueous electrolyte secondary batteries> [Output resistance measurement] Charge the battery to SOC50% at a current value of C / 3 in a 25°C environment, and measure the battery voltage after 30 minutes of rest (=V0). Then, discharge the battery for 10 seconds at a current value of 2C in a 25°C environment. Measure the battery voltage at the 10th second (=V1) and calculate it using the following formula: Resistance = (V0-V1) / 2C current value The output resistance of the battery was calculated according to the following formula: The output resistance of Comparative Examples 1 to 5 is shown in Table 1 as a relative value with Comparative Example 1 set to 100%, and the output resistance of Examples 1 to 5 and Comparative Examples 6 to 9 is shown as a relative value with Comparative Example 6 set to 100%.

[0065] [Evaluation of cycle characteristics] After the output resistance was measured, a cycle test was carried out. The cycle test conditions were: charging at 4.2Vcccv at a current value of 2C in a 25°C environment, discharging to 3V at a current value of C / 2, and repeating this cycle of charging and discharging. The cycle capacity retention rate was determined as the retention rate of the discharge capacity at the 500th cycle relative to the discharge capacity at the 1st cycle. Capacity retention rate = (500th cycle discharge capacity / 1st cycle discharge capacity) x 100 (%) The results are shown in Table 1.

[0066] [Table 1]

[0067] In Comparative Examples 1 to 5, the width of the positive electrode active material layer was 100 mm, and the electrode body width was relatively narrow, so that when the LiFSO3 concentration increased, the output resistance was reduced and the cycle capacity retention rate was improved, but no specific effect due to the A / B ratio was observed. This is presumed to be because, because the electrode body width was relatively narrow, even in a relatively high-rate charging cycle of 2C, the salt concentration was less likely to be uneven in the width direction of the electrode body, and as a result, the potential of the positive electrode was less likely to increase, and the elution of transition metals from the positive electrode active material was small, and the cycle capacity retention rate was slightly improved along with the resistance reduction effect due to the addition of LiFSO3. In Comparative Examples 1 to 5, at least no decrease in the cycle retention rate was observed.

[0068] In Comparative Examples 6 to 8 and Examples 1 to 5, the width of the positive electrode active material layer was 150 mm, and in Comparative Examples 6 to 8 and Examples 1 to 5, in which the electrode body width was relatively wide, the increase in LiFSO3 concentration tended to reduce the output resistance and improve the cycle capacity retention rate. In Examples 1 to 3, when the A / B ratio was in the range of 5 to 10, a specific output resistance reduction effect was achieved, and a cycle capacity retention rate of 90% or more was obtained. In the A / B ratio range of Examples 1 to 3, a reduction in the output resistance of LiFSO3 and an improvement in the cycle capacity retention rate were achieved. On the other hand, in Comparative Example 8, in which the concentration of LiFSO3 was relatively high and the A / B ratio was 4.0, the cycle capacity retention rate was significantly reduced. This is presumably because the width of the positive electrode active material layer was as wide as 150 mm, and the salt concentration unevenness in the width direction of the cell became noticeable due to the influence of the relatively high-rate charging cycle of 2C, and the positive electrode potential during charging increased. In contrast, in Examples 1 to 3, the LiPF6 concentration was sufficient relative to the LiFSO3 concentration, so that a sufficient LiF coating was formed on the surface of the positive electrode active material, and as a result, it is presumed that the transition metal elution of the positive electrode active material was suppressed and the cycle capacity retention rate was maintained at a high level. On the other hand, in Comparative Example 8, the LiPF6 concentration was low relative to the LiFSO3 concentration, so it is predicted that the LiF coating on the surface of the positive electrode active material was insufficient, and as a result, the positive electrode active material and the highly acidic SO3F - It is presumed that the reaction potential reached 1000 mV, and where the LiF coating was insufficient, the transition metal of the positive electrode active material was dissolved and deposited on the negative electrode, resulting in a decrease in the capacity retention rate. In Examples 1 to 3, in which the A / B ratio was in the range of 5 to 10, a cycle capacity retention rate of 90% or more was obtained along with a reduction in output resistance. Also, good results were obtained in Examples 4 and 5.

[0069] In Comparative Example 9, where the battery was not restrained, the A / B ratio was 6.7, but the output resistance was high and the cycle capacity retention rate was also low. This is presumably because, since the battery was not restrained, the electrolyte flow was smooth, making it difficult for uneven salt concentration to occur during the cycle test, but because the battery was not restrained, the gap between the electrodes was likely to widen, resulting in higher resistance and greater capacity degradation during the cycle test. [Explanation of symbols]

[0070] 10 positive electrode plate, 11 positive electrode core material, 12 positive electrode active material layer, 20 negative electrode plate, 21 negative electrode core material, 22 negative electrode active material layer, 30 separator, 40 laminate, 50 electrode body, 51 curved portion, 52 flat portion, 71 positive electrode current collecting member, 72 negative electrode current collecting member, 81 positive electrode terminal, 82 negative electrode terminal, 90 exterior body, 91 sealing plate, 92 exterior can, 100 battery, 111 negative electrode external terminal, 112 positive electrode external terminal, 113 restraining plate, 114 screw, 200 battery pack, 201 inter-cell separator, 300 battery module, 301 restraining member, 302 end plate, W width direction, R winding axis, S electrode body area.

Claims

1. An electrode assembly and an electrolyte solution are included. The electrode body is a wound electrode body in which a positive electrode plate and a negative electrode plate are wound with a separator interposed therebetween, The positive electrode plate includes a positive electrode active material layer, The negative electrode plate includes a negative electrode active material layer, At least one of the positive electrode active material layer and the negative electrode active material layer has a dimension of 150 mm or more in a winding axis direction of the electrode body, The electrolyte solution contains an electrolyte salt and LiFSO 3 and The electrolyte salt is LiPF 6 and LiBF 4 At least one of the following is included: LiPF in the electrolyte 6 and LiBF 4 The total concentration of LiFSO is A (mol / L). 3 When the concentration of is B (mol / L), the A / B ratio, which is the ratio of A to B, is 5 or more and 12 or less, A nonaqueous electrolyte secondary battery, wherein a pressure of 0.5 MPa or more is applied to the electrode assembly in a direction in which the electrodes are stacked.

2. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the A / B ratio is 6.7 or more and 10 or less.

3. LiPF in the electrolyte 6 and LiBF 4 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the total concentration A is 1 to 1.5 mol / L.

4. LiFSO in the electrolyte 3 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the concentration B is 0.1 to 0.25 mol / L.

5. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the electrode body has a length parallel to the winding axis of 180 mm or more.

6. A battery pack comprising the nonaqueous electrolyte secondary battery according to claim 1.

7. A battery module comprising the nonaqueous electrolyte secondary battery according to claim 1 .

Citation Information

Patent Citations

  • Non-aqueous electrolyte secondary battery and battery module

    JP2022168455A

  • Lithium-ion batteries, battery modules, battery packs and power consumption devices

    JP2023514769A

  • Nonaqueous electrolyte and nonaqueous electrolyte secondary battery

    JP2011187440A

  • Nonaqueous electrolyte and nonaqueous electrolyte secondary battery

    JP2013152956A