Exterior material for power storage device and power storage device

The exterior material for power storage devices, featuring a hydrophobic insulating adhesive layer and sealant composition, addresses insulation failures under heat and pressure, ensuring effective insulation and preventing short circuits, thus enhancing safety and performance.

JP2024168082APending Publication Date: 2024-12-05TOPPAN HOLDINGS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023084484
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing exterior materials for power storage devices, such as lithium ion batteries, fail to maintain adequate insulation properties when subjected to heated and pressurized conditions, leading to potential short circuits due to the flow of sealants and adhesives, which can crush and cause electrical contact between the metal layer and the electrodes.

Method used

An exterior material comprising a base material layer, a barrier layer with a metal layer, an adhesive layer containing hydrophobic insulating inorganic fillers, and a sealant layer, designed to prevent flow and maintain insulation under heat and pressure, using a composition that includes modified polyolefin resin and polyfunctional isocyanate compounds to enhance adhesion and moisture barrier properties.

Benefits of technology

The material ensures excellent insulation properties even under heated and pressurized conditions, preventing short circuits and maintaining structural integrity by minimizing the flow of adhesive and sealant layers, thereby enhancing safety and performance of power storage devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168082000001_ABST
    Figure 2024168082000001_ABST
Patent Text Reader

Abstract

To provide an exterior material for a power storage device and a power storage device, which has excellent insulation properties even when used under heated and pressurized conditions as an exterior bag for the power storage device.SOLUTION: An exterior material for a power storage device includes at least a base layer, a barrier layer including a metal layer, an adhesive layer, and a sealant layer in this order, and the adhesive layer includes a hydrophobic insulating inorganic filler. The content of the hydrophobic insulating inorganic filler may be 0.5 to 20 mass%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an exterior material for an electricity storage device and an electricity storage device. [Background technology]

[0002] Secondary batteries such as lithium ion batteries are widely used in portable electronic devices, electric vehicles and hybrid electric vehicles that use electricity as a power source, etc. A lithium ion battery generally comprises a battery cell including a positive electrode and a negative electrode, and an outer bag that houses the battery cell, and the outer bag is obtained by using an outer casing material. In such lithium secondary batteries, the battery capacity and the current used can become large, and therefore the exterior material is required to have better insulating properties in order to ensure higher safety. For example, Patent Document 1 below proposes that in order to obtain an outer casing material for a battery having excellent insulating properties, the outer casing material for a battery is formed by laminating an outer layer including a heat-resistant resin film, a metal foil layer, an adhesive layer, and an inner layer including a thermoplastic resin film, and that insulating particles are contained in the adhesive layer, the insulating particles being either inorganic particles having an average particle size of 0.1 μm to 4 μm, organic particles having an average particle size of 0.1 μm to 4 μm, or a mixture of these, and the amount of insulating particles added to the adhesive layer is 1 to 30 mass %. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-127258 A Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, lithium secondary batteries include all-solid-state batteries that use a solid electrolyte, and such power storage devices, such as all-solid-state batteries, are sometimes constrained in a pressurized state via an exterior material in a direction perpendicular to the surface of a battery cell that includes a positive electrode, a solid electrolyte, and a negative electrode. This is to increase the adhesion between the positive electrode or negative electrode and the solid electrolyte, thereby reducing the resistance between the positive electrode or negative electrode and the solid electrolyte, and thereby to achieve and maintain sufficient battery performance of the power storage device. However, when the exterior material described in Patent Document 1 is used as an exterior bag for a battery cell, the battery cell may heat up, and when the exterior material is pressurized in a heated state for a long period of time, the sealant layer may be crushed and further flow, which may result in a short circuit between the metal layer of the exterior material and the positive electrode or negative electrode of the battery cell. Therefore, the exterior material described in Patent Document 1 has room for improvement in terms of insulation properties when used as an exterior bag for an electricity storage device under a heated and pressurized state.

[0005] The present disclosure has been made in consideration of the above-mentioned problems, and aims to provide an outer casing material for an energy storage device and an energy storage device that have excellent insulating properties even when used under heated and pressurized conditions as an outer bag for the energy storage device. [Means for solving the problem]

[0006] In order to solve the above problems, the present disclosure provides an exterior material for an electricity storage device comprising, in this order, at least a base material layer, a barrier layer including a metal layer, an adhesive layer, and a sealant layer, wherein the adhesive layer contains a hydrophobic insulating inorganic filler.

[0007] The above-mentioned exterior material has excellent insulating properties even when used in a heated and pressurized state as an exterior bag for an electricity storage device. The inventors of the present disclosure speculate as follows about the reason why the above effects are obtained. That is, in the exterior material of the present disclosure, the adhesive layer generally becomes a viscous fluid under a long-term heating and pressurizing condition, but since the adhesive layer is adjacent to a barrier layer including a metal layer, the adhesive layer becomes less likely to flow than the sealant layer due to friction with the barrier layer. In addition, since the hydrophobic insulating inorganic filler has hydrophobicity, the affinity with other components in the adhesive layer increases, and the cohesive force of the adhesive layer is improved. Therefore, even when the adhesive layer is heated and pressurized, the adhesive layer becomes less likely to flow. Furthermore, since the adhesive layer contains a hydrophobic insulating inorganic filler, unevenness is easily generated on the surface of the adhesive layer on the sealant layer side, the contact area between the adhesive layer and the sealant layer is increased, and the adhesion between the adhesive layer and the sealant layer is improved, so that the sealant layer becomes less likely to flow even when heated and pressurized. As a result, even when the exterior material is heated and pressurized, the adhesive layer and the sealant layer become less likely to flow. Furthermore, the hydrophobic insulating inorganic filler is less likely to deform even under long-term heating and pressure conditions compared to the insulating organic filler, and even if the adhesive layer is compressed by heating and pressure, the adhesive layer and the sealant layer (hereinafter, these are also collectively referred to as the "insulating layer") can ensure a thickness at least equal to the size of the hydrophobic insulating inorganic filler. In addition, since moisture having electrical conductivity is less likely to adhere to the hydrophobic insulating inorganic filler, a decrease in the electrical resistance of the adhesive layer can be suppressed, and a decrease in the insulating properties of the adhesive layer can be suppressed. From the above, the inventors of the present disclosure speculate that the exterior material will have excellent insulating properties even when used under heated and pressurized conditions as an exterior bag for a battery cell of an electricity storage device.

[0008] In the exterior packaging material for a power storage device, it is preferable that the composition contains the hydrophobic insulating inorganic filler, a resin, and a polyfunctional isocyanate compound, and the resin is a modified polyolefin resin. In this case, the modified polyolefin resin and the polyfunctional isocyanate compound contained in the composition react with each other, so that the adhesive layer obtained using the composition is less likely to flow even under a heated and pressurized condition for a long period of time, and the insulating layer including the adhesive layer can be more sufficiently prevented from being crushed. Therefore, the exterior material can have better insulating properties even when used under a heated and pressurized condition as an exterior bag for a battery cell of an electricity storage device. Furthermore, since the adhesive layer is obtained using a composition containing a modified polyolefin, the adhesion of the adhesive layer to the barrier layer and the sealant layer is further improved. Furthermore, when the composition further contains a polyfunctional isocyanate compound, the seal strength can be further improved while the moisture barrier property can be further improved.

[0009] In the packaging material for an electricity storage device, the sealant layer preferably has an MFR of 20 g / 10 min or less. By setting the MFR of the sealant layer to 20 g / 10 min or less to make the sealant layer less likely to flow even when heated and pressurized, the sealant layer is less likely to be crushed even when the packaging material is used as an outer bag under heated and pressurized conditions, and the thickness of the insulating layer including the sealant layer can be sufficiently ensured, resulting in better insulation properties.

[0010] In the packaging material for an electricity storage device, the sealant layer preferably has a melting point of 160° C. or higher. By setting the melting point of the sealant layer to 160°C or higher, the flow of the sealant layer can be sufficiently suppressed even under heating and pressure. This makes it possible to more sufficiently suppress the insulating layer including the adhesive layer from being crushed. This allows the exterior material to have better insulating properties even when used under heating and pressure as an exterior bag for a battery cell of an electricity storage device.

[0011] In the packaging material for a power storage device, the hydrophobic insulating inorganic filler preferably has an average particle size of 1 to 20 μm. In this case, the packaging material can have better insulating properties even when used under heated and pressurized conditions as an outer bag for a battery cell of an electricity storage device, compared to when the average particle size of the hydrophobic insulating inorganic filler is less than 1 μm. Also, the hydrophobic insulating inorganic filler can be maintained in a well-dispersed state in the composition, the cohesive force of the adhesive layer is less likely to decrease, and the adhesion strength of the adhesive layer to the barrier layer and sealant layer and the seal strength of the sealant layer are less likely to decrease.

[0012] The packaging material for a power storage device preferably has a dielectric breakdown voltage of 100 V or more when heated and pressed at 150° C. and 3 MPa for 24 hours. In this case, even if the heating and pressurizing conditions are severe, the exterior material can have better insulating properties when used under heated and pressurized conditions as an exterior bag for a battery cell of an electricity storage device.

[0013] In the exterior packaging material for an electricity storage device, the modified polyolefin resin is preferably an acid-modified polyolefin resin. According to this packaging material, the adhesive layer has improved adhesion to the barrier layer, and the adhesive layer is less likely to flow even when the packaging material is heated and pressurized. Furthermore, the improved adhesion of the adhesive layer to the barrier layer also improves heat resistance.

[0014] In the exterior packaging material for an electricity storage device, the polyfunctional isocyanate compound preferably includes an isocyanurate-type polyfunctional isocyanate compound. According to this exterior material, since the polyfunctional isocyanate compound contains an isocyanurate-type polyfunctional isocyanate compound, the adhesive layer can have excellent adhesion and heat resistance, and can have high sealing strength, heat resistance, and excellent barrier properties.

[0015] In the packaging material for a power storage device, the content of the hydrophobic insulating inorganic filler in the composition is preferably 0.5 to 20 mass %. In this case, the thickness of the insulating layer including the adhesive layer is more easily maintained uniformly even when the exterior material is used under heating and pressure as an exterior bag for a battery cell of a power storage device, compared to when the content of the hydrophobic insulating inorganic filler in the composition is less than 0.5% by mass. Also, compared to when the content of the filler in the composition exceeds 20% by mass, the decrease in the cohesive force of the adhesive layer is suppressed, and the decrease in the seal strength and adhesion is more suppressed. Also, the decrease in the brittleness of the adhesive layer can be more suppressed.

[0016] The packaging material for an electricity storage device may include a corrosion prevention treatment layer on one or both surfaces of the barrier layer. This exterior material improves the adhesion of the adhesive layer to the corrosion prevention treatment layer and suppresses flow of the adhesive layer, allowing the exterior material to have better insulating properties even when used under heated and pressurized conditions as an exterior bag for battery cells in an energy storage device.

[0017] In the packaging material for an electricity storage device, the electricity storage device may be an all-solid-state battery.

[0018] The present disclosure also provides an energy storage device comprising a battery cell having a positive electrode, an electrolyte, and a negative electrode in that order, and an outer bag that houses the battery cell, the outer bag having the above-mentioned outer casing material for a energy storage device. According to the energy storage device disclosed herein, even when the outer casing material is used as an outer bag in a heated and pressurized state, it has excellent insulating properties, and therefore even when the energy storage device is heated while being pressurized in a direction perpendicular to the interface between the battery cell and the outer casing material, it is possible to prevent a short circuit between the positive or negative electrode in the battery cell and the metal layer of the outer casing material.

[0019] The power storage device may be an all-solid-state battery. Effect of the Invention

[0020] According to the present disclosure, it is possible to provide an exterior material for an electricity storage device and an electricity storage device that have excellent insulating properties even when used in a heated and pressurized state as an exterior bag for the electricity storage device. [Brief description of the drawings]

[0021] [Figure 1] 1 is a cross-sectional view showing a first embodiment of an exterior material for an electricity storage device according to the present disclosure. [Diagram 2] 4 is a cross-sectional view showing a second embodiment of an exterior material for an electricity storage device according to the present disclosure. FIG. [Diagram 3] 1 is a perspective view showing an embodiment of a power storage device according to the present disclosure. [Figure 4] FIG. 4 is a cross-sectional view showing the battery cell of FIG. [Diagram 5]FIG. 2 is a plan view showing a folded cut piece before cutting out a test piece for measuring seal strength used in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. In the drawings, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted.

[0023] [First embodiment of exterior material for power storage device] First, a first embodiment of the exterior material for an electricity storage device according to the present disclosure will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view showing the first embodiment of the exterior material for an electricity storage device according to the present disclosure. The exterior material for a storage battery device (hereinafter also simply referred to as "exterior material") 10 shown in Figure 1 is an exterior material used for a storage battery device, and comprises, in this order, a base material layer 11, a first adhesive layer 12a, a barrier layer 14, a second adhesive layer 12b as an adhesive layer, and a sealant layer 16.

[0024] The second adhesive layer 12b contains a hydrophobic insulating inorganic filler. The second adhesive layer 12b is obtained by using an adhesive as a composition containing a hydrophobic insulating inorganic filler.

[0025] The barrier layer 14 has a first anti-corrosion treatment layer 14a and a second anti-corrosion treatment layer 14b on both sides of the metal layer 14c. The first anti-corrosion treatment layer 14a is disposed between the substrate layer 11 and the metal layer 14c, and the second anti-corrosion treatment layer 14b is disposed between the metal layer 14c and the second adhesive layer 12b. Although FIG. 1 shows the case where the corrosion prevention treatment layers 14a, 14b are provided on both sides of the metal layer 14c, only one of the corrosion prevention treatment layers 14a, 14b may be provided.

[0026] In the exterior packaging material 10, the base material layer 11 is the outermost layer and the sealant layer 16 is the innermost layer. That is, the exterior packaging material 10 is used with the base material layer 11 facing the exterior side of the electricity storage device and the sealant layer 16 facing the interior side of the electricity storage device.

[0027] The exterior material 10 has excellent insulating properties even when used under heated and pressurized conditions as an exterior bag for an electricity storage device.

[0028] Each layer constituting the packaging material 10 will now be described in detail.

[0029] <Base material layer> The base layer 11 provides heat resistance in the sealing process when manufacturing the electricity storage device and plays a role in suppressing the occurrence of pinholes that may occur during molding and distribution. In particular, in the case of an exterior material for a large-scale electricity storage device, the base layer 11 can also provide scratch resistance, chemical resistance, insulation, and the like.

[0030] The base layer 11 is preferably a layer formed of an insulating resin, such as polyester resin, polyamide resin, polyimide resin, polyamideimide resin, polyetherketone resin, polyphenylene sulfide resin, polyetherimide resin, polysulfone resin, fluororesin, phenol resin, melamine resin, urethane resin, allyl resin, silicone resin, epoxy resin, furan resin, acetyl cellulose resin, or the like.

[0031] Among these resins, polyester resin and polyamide resin are preferable for the base layer 11 because of their excellent moldability. Examples of polyester resin include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of polyamide resin include nylon 6, nylon 6,6, a copolymer of nylon 6 and nylon 6,6, nylon 6, nylon 9T, nylon 10, polymetaxylylene adipamide (MXD6), nylon 11, and nylon 12.

[0032] The base layer 11 may contain additives such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, a dehydrating agent, a crystal nucleating agent, and a tackifier, as necessary.

[0033] The substrate layer 11 may be in the form of a stretched or unstretched film, or in the form of a coating film. The substrate layer 11 may be a single layer or a multilayer, and in the case of a multilayer, different resins may be used in combination. When the substrate layer 11 is a film, the substrate layer 11 may be a layer obtained by co-extrusion of multiple layers, or a layer obtained by laminating multiple layers with an adhesive. When the substrate layer 11 is a coating film, the substrate layer 11 may be a layer obtained by coating a coating liquid the number of times that the layers are laminated, or a layer obtained by combining a film and a coating film to form a multilayer may be used.

[0034] When these resins are used in the form of a film, the base layer 11 is preferably a biaxially stretched film. When the base layer 11 is a biaxially stretched film, examples of the stretching method include sequential biaxial stretching, tubular biaxial stretching, and simultaneous biaxial stretching. From the viewpoint of obtaining better deep-draw formability, the biaxially stretched film is preferably one stretched by the tubular biaxial stretching method.

[0035] The thickness of the substrate layer 11 is preferably 6 to 40 μm, and more preferably 10 to 30 μm. When the thickness of the substrate layer 11 is 6 μm or more, the pinhole resistance and insulating properties of the packaging material 10 tend to be improved. When the thickness of the substrate layer 11 is 40 μm or less, the total thickness of the packaging material 10 can be reduced.

[0036] In order to suppress deformation of the base layer 11 during sealing, the melting point of the base layer 11 is higher than the melting point of the sealant layer 16, and is preferably higher than the melting point of the sealant layer 16 by 30° C. or more.

[0037] <First adhesive layer> The first adhesive layer 12a is a layer that bonds the base material layer 11 and the metal layer 14c. The first adhesive layer 12a is obtained by using a first adhesive layer forming composition (adhesive). The first adhesive layer forming composition contains, for example, a base agent such as polyester polyol, polyether polyol, acrylic polyol, carbonate polyol, etc., and a bifunctional or higher isocyanate compound (polyfunctional isocyanate compound). The above-mentioned various polyols can be used alone or in combination of two or more types depending on the function and performance required for the exterior material 10. In addition, as the first adhesive layer forming composition that forms the first adhesive layer 12a, in addition to the above-mentioned first adhesive layer forming composition, a first adhesive layer forming composition containing a base agent such as an epoxy resin and a curing agent can also be used, but the first adhesive layer forming composition is not limited thereto.

[0038] The composition for forming the first adhesive layer may contain various additives such as flame retardants, slip agents, antiblocking agents, antioxidants, light stabilizers, dehydrating agents, crystal nucleating agents, and tackifiers depending on the performance required for the first adhesive layer 12a.

[0039] The thickness of the first adhesive layer 12a is not particularly limited, but from the viewpoint of obtaining desired adhesive strength, conformability, processability, and the like, the thickness is, for example, preferably 1 to 10 μm, and more preferably 2 to 7 μm.

[0040] <Barrier layer> (metal layer) The metal layer 14c has a water vapor barrier property that prevents moisture from penetrating into the inside of the electricity storage device. The metal layer 14c may also have extensibility for deep drawing. As the metal layer 14c, for example, various metal foils such as aluminum, stainless steel, copper, etc., or metal vapor deposition films, films provided with such vapor deposition films, etc. can be used. As the film provided with a vapor deposition film, for example, an aluminum vapor deposition film can be used. As the metal layer 14c, a metal foil is preferable, and an aluminum foil is more preferable, in terms of mass (specific gravity), moisture resistance, processability, and cost.

[0041] As the aluminum foil, a soft aluminum foil that has been annealed can be preferably used from the viewpoint of imparting desired ductility during molding, but it is more preferable to use an aluminum foil containing iron for the purpose of imparting further pinhole resistance and ductility during molding. The content of iron in the aluminum foil is preferably 0.1 to 9.0 mass%, more preferably 0.5 to 2.0 mass%, in 100 mass% of the aluminum foil. When the iron content is 0.1 mass% or more, an exterior material 10 having better pinhole resistance and ductility can be obtained. When the iron content is 9.0 mass% or less, an exterior material 10 having better flexibility can be obtained. As the aluminum foil, an untreated aluminum foil may be used, but it is preferable to use an aluminum foil that has been degreased in terms of imparting corrosion resistance. When the aluminum foil is degreased, the degreased treatment may be performed on only one side of the aluminum foil, or on both sides.

[0042] The thickness of the metal layer 14c is not particularly limited, but is preferably 9 to 200 μm, more preferably 15 to 100 μm, in consideration of barrier properties, pinhole resistance, and processability.

[0043] (First corrosion prevention treatment layer and second corrosion prevention treatment layer) The first anti-corrosion treatment layer 14a and the second anti-corrosion treatment layer 14b are layers provided to prevent the corrosion of the metal layer 14c. The first anti-corrosion treatment layer 14a prevents the metal layer 14c from being corroded by the corrosive gas contained in the atmosphere, and also plays a role of increasing the adhesive strength between the metal layer 14c and the first adhesive layer 12a. The second anti-corrosion treatment layer 14b prevents the metal layer 14c from being corroded by the electrolyte or the gas (e.g., hydrogen sulfide gas) generated inside the battery, thereby further improving the resistance to the electrolyte or the gas generated inside the battery, and also plays a role of increasing the adhesive strength between the metal layer 14c and the second adhesive layer 12b. The first and second anti-corrosion treatment layers 14a and 14b can maintain the reliability of the exterior material 10 for a longer period of time. The first anti-corrosion treatment layer 14a and the second anti-corrosion treatment layer 14b may be layers of the same configuration or layers of different configurations. The first and second corrosion prevention treatment layers 14a, 14b (hereinafter also simply referred to as "corrosion prevention treatment layers 14a, 14b") are formed, for example, by subjecting the metal foil constituting the metal layer 14c to degreasing treatment, hydrothermal conversion treatment, anodizing treatment, chemical conversion treatment, or a combination of these treatments.

[0044] Examples of the degreasing treatment include acid degreasing and alkaline degreasing. Examples of the acid degreasing include a method using an inorganic acid such as sulfuric acid, nitric acid, hydrochloric acid, or hydrofluoric acid alone, or a method using a mixture of these. In addition, it is preferable to perform a treatment using an acid degreasing agent in which a fluorine-containing compound such as monosodium ammonium difluoride is dissolved in the inorganic acid as described above. This treatment not only provides a degreasing effect for aluminum, but also allows the formation of aluminum fluoride, which is a passive state, particularly when an aluminum foil is used for the metal layer 14c. Therefore, this treatment is effective in terms of corrosion resistance. Examples of the alkaline degreasing include a method using sodium hydroxide or the like.

[0045] An example of the hydrothermal modification treatment is boehmite treatment in which an aluminum foil is immersed in boiling water containing triethanolamine. An example of the anodization treatment is alumite treatment.

[0046] The chemical conversion treatment may be of the immersion type or the coating type. Examples of the immersion type chemical conversion treatment include chromate treatment, ceria sol treatment, zirconium treatment, titanium treatment, vanadium treatment, molybdenum treatment, calcium phosphate treatment, strontium hydroxide treatment, cerium treatment, ruthenium treatment, or various chemical conversion treatments consisting of a mixture of these. On the other hand, examples of the coating type chemical conversion treatment include a method in which a coating agent having corrosion prevention properties is applied onto the metal layer 14c.

[0047] When forming at least a part of the corrosion prevention layer by any of these corrosion prevention treatments, namely, hydrothermal conversion treatment, anodizing treatment, and chemical conversion treatment, it is preferable to perform the above-mentioned degreasing treatment in advance. Note that, when using a degreased metal foil such as a metal foil that has been subjected to an annealing process as the metal layer 14c, there is no need to perform a degreasing treatment again in forming the corrosion prevention layers 14a and 14b.

[0048] The coating agent used in the spray-type chemical conversion treatment preferably contains trivalent chromium. The coating agent may also contain at least one polymer selected from the group consisting of cationic polymers and anionic polymers, which will be described later.

[0049] Among the above treatments, particularly in hydrothermal conversion treatment and anodization treatment, the aluminum foil surface is dissolved by a treatment agent to form an aluminum compound (boehmite, alumite) with excellent corrosion resistance. Therefore, a form in which a co-continuous structure is formed from the metal layer 14c using the aluminum foil to the corrosion prevention treatment layers 14a, 14b is obtained, so the above treatment is included in the definition of chemical conversion treatment. On the other hand, as described later, it is also possible to form the corrosion prevention treatment layers 14a, 14b only by a pure coating method that is not included in the definition of chemical conversion treatment. As an example of this method, a method using a sol of a rare earth element oxide such as cerium oxide with an average particle size of 100 nm or less can be mentioned, which has an aluminum corrosion prevention effect (inhibitor effect) and is also environmentally friendly. By using this method, it is possible to impart a corrosion prevention effect to metal foils such as aluminum foils even by a general coating method.

[0050] Examples of the rare earth element oxide sol include sols using various solvents such as water-based, alcohol-based, hydrocarbon-based, ketone-based, ester-based, ether-based, etc. Among these, water-based sols are preferred.

[0051] In order to stabilize the dispersion of the rare earth oxide sol, inorganic acids such as nitric acid, hydrochloric acid, phosphoric acid, etc. or their salts, and organic acids such as acetic acid, malic acid, ascorbic acid, lactic acid, etc. are usually used as dispersion stabilizers. Among these dispersion stabilizers, phosphoric acid in particular is expected to provide the following in the exterior packaging material 10: (1) stabilization of the dispersion of the sol, (2) improvement of adhesion to the metal layer 14c by utilizing phosphoric acid's aluminum chelating ability, (3) imparting corrosion resistance by capturing aluminum ions (passivation formation), and (4) improvement of the cohesive force of the corrosion prevention treatment layers (oxide layers) 14a, 14b by easily causing dehydration condensation of phosphoric acid even at low temperatures.

[0052] The corrosion prevention layers 14a and 14b formed from the rare earth oxide sol are aggregates of inorganic particles, and therefore may lose their cohesive strength even after the drying and curing process. Therefore, it is preferable that the corrosion prevention layers 14a and 14b in this case are compounded with an anionic polymer or a cationic polymer to compensate for the cohesive strength.

[0053] The corrosion prevention treatment layers 14a, 14b are not limited to the above-mentioned layers. For example, they may be formed using a treatment agent in which phosphoric acid and a chromium compound are mixed with a resin binder (such as aminophenol), as in the case of coating-type chromate, which is a known technology. By using this treatment agent, a layer having both corrosion prevention function and adhesion can be formed. In addition, although it is necessary to consider the stability of the coating liquid, the corrosion prevention treatment layers 14a, 14b can be formed into a layer having both corrosion prevention function and adhesion by using a coating agent in which a rare earth element oxide sol and a polycationic polymer or a polyanionic polymer are previously mixed into a one-component solution.

[0054] The mass per unit area of ​​the corrosion prevention layers 14a and 14b is 0.005 to 0.200 g / m2 regardless of whether the layer has a multi-layer structure or a single-layer structure. 2 is preferable, and 0.010 to 0.100 g / m 2 It is more preferable that the mass per unit area is 0.005 g / m 2 If the mass per unit area is 0.200 g / m or more, it is easy to impart a corrosion prevention function to the metal layer 14c. 2 Even if the thickness exceeds 100 mm, the corrosion prevention function does not change much. On the other hand, when a rare earth oxide sol is used, if the coating is thick, the heat curing during drying may be insufficient, which may result in a decrease in cohesive force. The thickness of the corrosion prevention layers 14a and 14b can be calculated from their specific gravity.

[0055] From the viewpoint of easily maintaining the adhesion between the sealant layer 16 and the barrier layer 13, the corrosion prevention treatment layers 14a, 14b may be, for example, in an embodiment containing cerium oxide, 1 to 100 parts by mass of phosphoric acid or a phosphate salt per 100 parts by mass of the cerium oxide, and a cationic polymer, or may be formed by subjecting the metal layer 14c to a chemical conversion treatment, or may be formed by subjecting the metal layer 14c to a chemical conversion treatment and contain a cationic polymer.

[0056] <Second adhesive layer> The second adhesive layer 12b is a layer that bonds the metal layer 14c and the sealant layer 16. The second adhesive layer 12b is obtained by using a composition (adhesive) containing a hydrophobic insulating inorganic filler. The composition may contain a resin.

[0057] (Hydrophobic insulating inorganic filler) The hydrophobic insulating inorganic filler is an insulating inorganic filler having hydrophobicity, and is obtained by surface-treating a non-hydrophobic insulating inorganic filler with an organosilicon compound. By surface-treating the non-hydrophobic insulating inorganic filler with an organosilicon compound, the surface of the non-hydrophobic insulating inorganic filler is hydrophobized, and the non-hydrophobic insulating inorganic filler is imparted with hydrophobicity. The filler is an inorganic filler because it is less likely to deform when heated and pressurized for a long period of time compared to organic fillers.

[0058] Examples of non-hydrophobic insulating inorganic fillers include silica and talc, of which silica is preferred from the viewpoints of insulation properties and particle size control.

[0059] An example of the organosilicon compound is alkoxysilane. The alkoxysilane may have an alkyl group such as a methyl group. In this case, the non-hydrophobic insulating inorganic filler and the alkoxysilane are more likely to react with each other.

[0060] The average particle size of the hydrophobic insulating inorganic filler is not particularly limited, but is preferably 1 μm or more. In this case, compared to when the average particle size of the hydrophobic insulating inorganic filler is less than 1 μm, the exterior material 10 can have better insulating properties even when used under heated and pressurized conditions as an exterior bag for a battery cell of an energy storage device. The average particle size of the hydrophobic insulating inorganic filler is more preferably 3 μm or more, and further preferably 5 μm or more.

[0061] The average particle size of the hydrophobic insulating inorganic filler is preferably 20 μm or less. In this case, the hydrophobic insulating inorganic filler can maintain a good dispersion state in the composition, the cohesive force of the second adhesive layer 1b is less likely to decrease, and the adhesion strength of the second adhesive layer 12b to the barrier layer 13 and the sealant layer 16 and the sealing strength of the sealant layer 16 are less likely to decrease. The average particle size of the hydrophobic insulating inorganic filler is more preferably 15 μm or less, and particularly preferably 10 μm or less.

[0062] The average particle size of the hydrophobic insulating inorganic filler can be obtained by taking an enlarged photograph of a plurality of hydrophobic insulating inorganic fillers using an electron microscope, then determining the particle size of each hydrophobic insulating inorganic filler by image analysis, and calculating the average value of these particle sizes. Specifically, the particle size of each hydrophobic insulating inorganic filler can be calculated by taking the area S of each hydrophobic insulating inorganic filler obtained by image analysis as the area of ​​a circle, and calculating the radius r (r=(S / π) 1 / 2 ) is doubled.

[0063] In the composition for forming the second adhesive layer, the content of the hydrophobic insulating inorganic filler in the total solid content, i.e., the content of the hydrophobic insulating inorganic filler in the second adhesive layer 12b, is not particularly limited, but is preferably 0.5 mass% or more. In this case, compared to when the content of the hydrophobic insulating inorganic filler in the total solid content is less than 0.5 mass %, the thickness of the insulating layer including the second adhesive layer 12b is more easily maintained uniformly even when the exterior material 10 is used under heating and pressure as an exterior bag for a battery cell of an energy storage device. The content of the hydrophobic insulating inorganic filler in the total solid content is more preferably 1 mass % or more, and further preferably 2 mass % or more.

[0064] The content of the hydrophobic insulating inorganic filler in the total solid content is preferably 20 mass % or less. In this case, the decrease in the cohesive force of the second adhesive layer 12b is suppressed, and the decrease in the seal strength and adhesion is further suppressed, compared to when the content of the hydrophobic insulating inorganic filler in the total solid content exceeds 20 mass %. Also, the decrease in the brittleness of the second adhesive layer 12b can be further suppressed. The content of the hydrophobic insulating inorganic filler in the total solid content is more preferably 15 mass % or less, and further preferably 10 mass % or less.

[0065] (resin) The resin is not particularly limited, but preferably contains a modified polyolefin resin. The modified polyolefin resin can disperse the hydrophobic insulating inorganic filler in the resin more satisfactorily. In addition, the resin containing the modified polyolefin resin can provide high adhesion to the barrier layer 13 and the sealant layer 16, and can improve the laminate strength of the exterior packaging material 10. Examples of the modified polyolefin resin include hydroxyl-modified polyolefin resin, glycidyl-modified polyolefin resin, acid-modified polyolefin resin, etc. Among them, from the viewpoint of adhesion to the barrier layer 13 and the sealant layer 16, the acid-modified polyolefin resin is preferred. The acid-modified polyolefin resin is a polyolefin resin graft-modified with an unsaturated carboxylic acid derivative derived from an unsaturated carboxylic acid, an unsaturated sulfonic acid, an acid anhydride of an unsaturated carboxylic acid, an ester of an unsaturated carboxylic acid, or the like.

[0066] Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, tetrahydrophthalic acid, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic acid.

[0067] Examples of the acid anhydrides of unsaturated carboxylic acids include acid anhydrides of unsaturated carboxylic acids such as maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic anhydride.

[0068] Examples of the esters of unsaturated carboxylic acids include esters of unsaturated carboxylic acids such as methyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, dimethyl maleate, monomethyl maleate, diethyl fumarate, dimethyl itaconate, diethyl citraconate, dimethyl tetrahydrophthalate, and dimethyl bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylate.

[0069] Examples of polyolefin resins include polyethylene-based resins such as low-density polyethylene (LDPE or LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), and ethylene-α-olefin copolymers; and polypropylene-based resins such as homopolypropylene, block polypropylene, random polypropylene, and propylene-α-olefin copolymers. Among these, polypropylene-based resins are preferred from the viewpoint of heat resistance.

[0070] The acid-modified polyolefin resin is preferably a polyolefin resin modified with maleic anhydride, from the viewpoint of obtaining excellent adhesion between the barrier layer 13 and the second adhesive layer 12b. Suitable modified polyolefin resins include, for example, "ADMER" manufactured by Mitsui Chemicals, Inc., "MODIC" manufactured by Mitsubishi Chemical Corporation, "TOYOTAC" manufactured by Toyobo Co., Ltd., and "SUNSTACK" manufactured by Sanyo Chemical Industries, Ltd. Such modified polyolefin resins have excellent reactivity with various metals and polymers having various functional groups, and thus the reactivity can be utilized to impart adhesion to the second adhesive layer 12b.

[0071] When the resin composition for forming the sealant layer that forms the sealant layer 16 contains a polyolefin resin as a resin, it is preferable to use a polyolefin resin similar to that polyolefin resin. For example, when the resin composition for forming the sealant layer contains a polypropylene-based resin as a resin, it is preferable that the acid-modified polyolefin resin of the composition for forming the second adhesive layer is an acid-modified polypropylene-based resin. In this case, the second adhesive layer 12b can have high adhesion to the sealant layer 16 and can also improve the heat resistance of the exterior material 10.

[0072] When the resin contains a modified polyolefin resin, the composition for forming the second adhesive layer preferably further contains a polyfunctional isocyanate compound as a curing agent. In this case, the second adhesive layer 12b further contains a polyfunctional isocyanate compound, so that the second adhesive layer 12b can have excellent adhesion and heat resistance, and can have high seal strength, heat resistance, and excellent barrier properties. Examples of the polyfunctional isocyanate compound include diisocyanates such as tolylene diisocyanate, xylylene diisocyanate or hydrogenated products thereof, hexamethylene diisocyanate, 4,4'-diphenylmethane diisocyanate or hydrogenated products thereof, and isophorone diisocyanate; or polyisocyanates such as adducts obtained by reacting these isocyanates with polyhydric alcohols such as trimethylolpropane, biuret forms obtained by reacting these isocyanates with water, or isocyanurate forms (isocyanurate-type polyfunctional isocyanate compounds) which are trimers; and blocked polyisocyanates obtained by blocking these polyisocyanates with alcohols, lactams, oximes, or the like. Among them, the polyfunctional isocyanate compound preferably contains an isocyanurate (isocyanurate-type polyfunctional isocyanate compound). When the polyfunctional isocyanate compound contains an isocyanurate, the second adhesive layer 12b can have excellent adhesion and heat resistance, and the exterior material 10 can have high seal strength and heat resistance.

[0073] The amount of the polyfunctional isocyanate compound may be, for example, 3 parts by mass or less per 100 parts by mass of the modified polyolefin resin (solid content).

[0074] When the resin contains an acid-modified polyolefin resin as the modified polyolefin resin, it is preferable that the resin further contains a carbodiimide compound as a curing agent. By further containing a carbodiimide compound in the composition for forming the second adhesive layer, the heat resistance of the exterior material 10 can be further improved compared to when the composition for forming the second adhesive layer does not contain a carbodiimide compound. This is because the crosslink density increases due to the reaction between the carbodiimide compound and the acid-modified polyolefin resin. Examples of the carbodiimide compound include N,N'-di-o-toluylcarbodiimide, N,N'-diphenylcarbodiimide, N,N'-di-2,6-dimethylphenylcarbodiimide, N,N'-bis(2,6-diisopropylphenyl)carbodiimide, N,N'-dioctyldecylcarbodiimide, N-triyl-N'-cyclohexylcarbodiimide, N,N'-di-2,2-di-t-butylphenylcarbodiimide, N-triyl-N'-phenylcarbodiimide, N,N'-di-p-nitrophenylcarbodiimide, N,N'-di-p-aminophenylcarbodiimide, N,N'-di-p-hydroxyphenylcarbodiimide, N,N'-di-cyclohexylcarbodiimide, and N,N'-di-p-toluylcarbodiimide. These can be used alone or in combination of two or more.

[0075] The amount of the carbodiimide compound may be, for example, 3 parts by mass or less per 100 parts by mass of the modified polyolefin resin (solid content).

[0076] The composition for forming the second adhesive layer may further contain various additives such as flame retardants, slip agents, antiblocking agents, antioxidants, light stabilizers, tackifiers, dehydrating agents, and crystal nucleating agents, as necessary.

[0077] In addition, as the second adhesive layer forming composition for forming the second adhesive layer 12b, for example, a polyurethane adhesive containing a polyester polyol made of hydrogenated dimer fatty acid and diol, a polyisocyanate, and a hydrophobic insulating inorganic filler can be used. Examples of the second adhesive layer forming composition include polyurethane resins in which a bifunctional or higher isocyanate compound is reacted with a base material such as polyester polyol, polyether polyol, acrylic polyol, or carbonate polyol, and epoxy resins in which an amine compound or the like is reacted with a base material having an epoxy group, which are preferable from the viewpoint of heat resistance.

[0078] The second adhesive layer 12b may be composed of a single layer or may be composed of multiple layers. When the second adhesive layer 12b is composed of multiple layers, all layers may contain the hydrophobic insulating inorganic filler, or only some layers may contain the hydrophobic insulating inorganic filler.

[0079] The thickness of the second adhesive layer 12b is not particularly limited, but is preferably 0.2 to 30 μm. In this case, sufficient adhesion can be obtained compared to when the thickness of the second adhesive layer 12b is less than 0.2 μm. Also, the volumetric energy density of the electricity storage device can be further increased compared to when the thickness of the second adhesive layer 12b exceeds 30 μm. The thickness of the second adhesive layer 12b is more preferably 0.2 to 10 μm.

[0080] <Sealant layer> The sealant layer 16 is a layer that imparts heat-sealing sealability to the exterior material 10, and is a layer that is disposed on the inside and heat-sealed (thermally fused) when assembling the electricity storage device. The sealant layer 16 is obtained using a resin composition for forming a sealant layer that contains a resin.

[0081] (Resin composition for forming sealant layer) (resin) Examples of the resin contained in the resin composition for forming the sealant layer include polyolefin resins and polyester resins. These resins constituting the sealant layer 16 (hereinafter also referred to as "base resins") may be used alone or in combination of two or more.

[0082] Examples of polyolefin resins include polyethylene resins such as low-density polyethylene (LDPE or LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), and ethylene-α-olefin copolymers; polypropylene resins such as homopolypropylene, block polypropylene, and propylene-α-olefin copolymers; and polybutene. Of the polyolefin resins, polypropylene resins are preferred from the viewpoints of heat resistance and flexibility, and homopolypropylene and block polypropylene, which have particularly high melting points, are preferred.

[0083] Examples of polyester resins include polyethylene terephthalate (PET) resin, polybutylene terephthalate (PBT) resin, polyethylene naphthalate (PEN) resin, polybutylene naphthalate (PBN) resin, and copolymers thereof.

[0084] (Hydrophobic insulating inorganic filler) The resin composition for forming a sealant layer may or may not contain a hydrophobic insulating inorganic filler, but it is preferable that it contains the hydrophobic insulating inorganic filler.

[0085] The average particle size of the hydrophobic insulating inorganic filler is not particularly limited, but is preferably 1 μm or more. In this case, compared to when the average particle size of the hydrophobic insulating inorganic filler is less than 1 μm, the exterior material 10 can have better insulating properties even when used under heated and pressurized conditions as an exterior bag for a battery cell of an energy storage device. The average particle size of the hydrophobic insulating inorganic filler is more preferably 3 μm or more, and further preferably 5 μm or more.

[0086] The average particle size of the hydrophobic insulating inorganic filler is preferably 20 μm or less, in which case the hydrophobic insulating inorganic filler can maintain a good dispersion state in the composition, the cohesive force of the sealant layer 16 is less likely to decrease, and the adhesive strength of the sealant layer 16 to the second adhesive layer 12b and the sealing strength of the sealant layer 16 are less likely to decrease. The average particle size of the hydrophobic insulating inorganic filler is more preferably 15 μm or less, and particularly preferably 10 μm or less.

[0087] The content of the hydrophobic insulating inorganic filler in the resin composition for forming the sealant layer is not particularly limited, but is preferably 0.5% by mass or more. In this case, compared to when the content of the hydrophobic insulating inorganic filler in the resin composition for forming the sealant layer is less than 0.5 mass %, the thickness of the insulating layer including the sealant layer 16 is more easily maintained uniformly even when the exterior material 10 is used under heating and pressure as an exterior bag for a battery cell of an electricity storage device. The content of the hydrophobic insulating inorganic filler in the resin composition for forming a sealant layer is more preferably 1% by mass or more, and further preferably 2% by mass or more. The content of the hydrophobic insulating inorganic filler in the resin composition for forming a sealant layer is preferably 20% by mass or less. In this case, the decrease in the cohesive force of the sealant layer 16 is suppressed, and the decrease in the seal strength and adhesion are further suppressed, compared to when the content of the hydrophobic insulating inorganic filler in the resin composition for forming the sealant layer exceeds 20% by mass. Also, the decrease in the brittleness of the sealant layer 16 can be further suppressed. The content of the hydrophobic insulating inorganic filler in the resin composition for forming a sealant layer is more preferably 15% by mass or less, and further preferably 10% by mass or less.

[0088] The sealant layer 16 may be either a monolayer film or a multilayer film. When the sealant layer 16 is a multilayer film, all layers may contain the hydrophobic insulating inorganic filler, or only some layers may contain the hydrophobic insulating inorganic filler. For example, when the sealant layer 16 is a two-layer film, all of the two layers may contain the hydrophobic insulating inorganic filler, or only the layer of the two-layer film on the second adhesive layer 12b side may contain the hydrophobic insulating inorganic filler, or only the layer of the two-layer film on the opposite side to the second adhesive layer 12b may contain the hydrophobic insulating inorganic filler.

[0089] The sealant layer 16 may also contain additives such as slip agents, antiblocking agents, antioxidants, light stabilizers, flame retardants, dehydrating agents, tackifiers, and crystal nucleating agents. The content of these additives is preferably 5 parts by mass or less, assuming that the total mass of the sealant layer 16 is 100 parts by mass.

[0090] The MFR of the sealant layer 16 is not particularly limited, but is preferably 20 g / 10 min or less. By setting the MFR of the sealant layer 16 to 20 g / 10 min or less to make the sealant layer 16 less likely to flow even when heated and pressurized, the sealant layer 16 is less likely to be crushed even when the packaging material 10 is used as an outer packaging bag in a heated and pressurized state, and the thickness of the insulating layer including the sealant layer 16 can be sufficiently ensured, making it possible to have better insulating properties. The MFR of the sealant layer 16 is preferably 18 g / 10 min or less, and more preferably 15 g / 10 min or less. The MFR of the sealant layer 16 may be 0.1 g / 10 min or more, or may be 0.3 g / 10 min or more. The MFR of the sealant layer 16 is obtained by measuring the melt flow rate using a melt flow rate measuring device (manufactured by Toyo Seiki Seisakusho, measuring temperature: 230° C.) in accordance with JIS K7210.

[0091] The melting point of the sealant layer 16 is not particularly limited, but is preferably 160° C. or higher. By setting the melting point of the sealant layer 16 to 160°C or higher, it is possible to suppress the flow of the sealant layer 16 as much as possible even under a heated and pressurized state. This makes it possible to more sufficiently suppress the insulating layer including the second adhesive layer 12b from being crushed. This allows the exterior material 10 to have better insulating properties even when used under a heated and pressurized state as an exterior bag for a battery cell of an electricity storage device. When differential scanning calorimetry (DSC) measurement is performed on the sealant layer 16, if one peak appears corresponding to the melting point of the sealant layer 16, the melting point refers to the temperature at the apex of that peak. If multiple peaks appear corresponding to the melting point of the sealant layer 16, the melting point refers to the temperature at the apex of the peak (main peak) that has the greatest intensity among the multiple peaks. The melting point of the sealant layer 16 is more preferably 161° C. or higher, and particularly preferably 162° C. or higher.

[0092] The thickness of the sealant layer 16 is not particularly limited, but is preferably in the range of 20 to 150 μm, more preferably in the range of 30 to 150 μm, and further preferably in the range of 40 to 100 μm. When the thickness of the sealant layer 16 is 20 μm or more, the sealing strength of the exterior material 10 is further improved. When the thickness of the sealant layer 16 is 150 μm or less, the volumetric energy density of the electricity storage device can be further increased.

[0093] <Exterior materials> In the exterior packaging material 10, when heated and pressurized for 24 hours under conditions of 150° C. and 3 MPa, the dielectric breakdown voltage is preferably 100 V or more, more preferably 0.5 kV or more, and particularly preferably 1 kV or more. In this case, even under severe heating and pressurizing conditions, the exterior material 10 can have better insulating properties when used under heated and pressurized conditions as an exterior bag for battery cells of an electricity storage device. The dielectric breakdown voltage when heated and pressurized under conditions of 150° C. and 3 MPa for 24 hours may be 5 kV or less.

[0094] [Second embodiment of exterior material for power storage device] Next, a second embodiment of the exterior packaging material for an electricity storage device according to the present disclosure will be described with reference to Fig. 2. Fig. 2 is a cross-sectional view showing the second embodiment of the exterior packaging material for an electricity storage device according to the present disclosure. As shown in FIG. 2, the packaging material 20 of this embodiment differs from the packaging material 10 of the first embodiment which has a second adhesive layer 12b obtained using an adhesive, in that the packaging material 20 of this embodiment has an adhesive resin layer 15 obtained using a resin composition for forming an adhesive resin layer containing a resin and a hydrophobic insulating inorganic filler as an adhesive layer between the barrier layer 13 and the sealant layer 16. The exterior material 20 shown in FIG. 2 may further include a second adhesive layer 12b between the barrier layer 13 and the adhesive resin layer 15.

[0095] The adhesive resin layer 15 may be either a single-layer film or a multilayer film. When the adhesive resin layer 15 is a multilayer film, all layers may contain the hydrophobic insulating inorganic filler, or only some layers may contain the hydrophobic insulating inorganic filler.

[0096] The thickness of the adhesive resin layer 15 is not particularly limited, but is preferably 5 to 30 μm. When the thickness of the adhesive resin layer 15 is 5 μm or more, sufficient adhesion is obtained. When the thickness of the adhesive resin layer 15 is 30 μm or less, the total thickness of the exterior material 10 becomes small, and when a battery is produced using the exterior material 10, a decrease in the volumetric energy density of the battery can be suppressed. The thickness of the adhesive resin layer 15 may be the same as or less than that of the sealant layer 16 from the viewpoints of stress relaxation and moisture permeability.

[0097] [Exterior material manufacturing method] Next, there will be described an example of a method for manufacturing the exterior packaging material 10 shown in Fig. 1. Note that the method for manufacturing the exterior packaging material 10 is not limited to the following method.

[0098] The manufacturing method of the exterior material 10 includes the steps of forming a barrier layer 13 by laminating corrosion prevention treatment layers 14a, 14b on both sides of a metal layer 14c, respectively, a step of bonding the base material layer 11 and the barrier layer 13 using a first adhesive layer 12a to obtain a first laminate, a step of further laminating a sealant layer 16 onto the barrier layer 13 of the first laminate via a second adhesive layer 12b to produce a second laminate, and a step of aging the obtained second laminate, if necessary.

[0099] (Laminating process of corrosion prevention treatment layer onto metal layer) This step is a step of forming the corrosion prevention treatment layers 14a and 14b on both sides of the metal layer 14c, respectively, to form the barrier layer 13. As described above, examples of the method include subjecting the metal layer 14c to a degreasing treatment, a hydrothermal conversion treatment, an anodizing treatment, or a chemical conversion treatment, or applying a coating agent having corrosion prevention properties.

[0100] Furthermore, when the corrosion prevention treatment layers 14a, 14b are multi-layered, the corrosion prevention treatment layers 14a, 14b can be formed, for example, by applying a coating liquid (coating agent) constituting the lower corrosion prevention treatment layer (metal layer 14c side) to the metal layer 14c and baking it to form a first layer, and then applying a coating liquid (coating agent) constituting the upper corrosion prevention treatment layer to the first layer and baking it to form a second layer, and repeating the operation of forming the first and second layers as necessary.

[0101] The degreasing treatment can be carried out by a spray method or a dipping method. The hydrothermal conversion treatment and the anodizing treatment can be carried out by a dipping method. The chemical conversion treatment can be carried out by appropriately selecting a method such as a dipping method, a spray method, or a coating method according to the type of chemical conversion treatment.

[0102] The coating agent having corrosion prevention properties can be applied by a method such as gravure coating, reverse coating, roll coating, or bar coating.

[0103] As described above, the various treatments may be performed on either one or both sides of the metal foil constituting the metal layer 14c, but in the case of one-sided treatment, the treated side is preferably the side on which the sealant layer 16 is laminated. If required, the above treatments may also be performed on the surface of the base layer 11.

[0104] The amount of coating agent applied to form the first layer and the second layer is 0.005 to 0.200 g / m 2 , or 0.010 to 0.100 g / m 2 may be also possible.

[0105] Furthermore, when dry curing is required, the drying can be performed at a base material temperature in the range of 60 to 300° C. depending on the drying conditions of the corrosion prevention treatment layers 14a and 14b used.

[0106] (Laminating process of substrate layer and barrier layer) This step is a step of bonding the barrier layer 13 and the base layer 11 via the first adhesive layer 12a to obtain a first laminate. Examples of the bonding method include a method of bonding the two layers using a composition for forming the first adhesive layer 12a described above using techniques such as dry lamination, non-solvent lamination, and wet lamination. The first adhesive layer 12a has a dry coating amount of 1 to 10 g / m 2 or 2 to 7 g / m 2 It may be set in the range.

[0107] (Laminating process of the second adhesive layer and the sealant layer) In this step, the sealant layer 16 is bonded to the second corrosion prevention treatment layer 14b side of the first laminate via the second adhesive layer 12b to obtain a second laminate. Examples of the bonding method include wet lamination and dry lamination.

[0108] For example, when the sealant layer 16 is bonded by dry lamination, a composition for forming the second adhesive layer 12b is applied onto the second corrosion prevention treatment layer 14b, and the composition is dried at a predetermined temperature to remove the solvent, and then the sealant layer 16 is laminated. Examples of the method for applying the composition for forming the second adhesive layer include gravure coating, reverse coating, roll coating, and bar coating. The preferred dry application amount of the composition for forming the second adhesive layer may be appropriately set according to the thickness of the second adhesive layer 12b.

[0109] The second adhesive layer-forming composition can be obtained by dissolving or dispersing a resin, a hydrophobic insulating inorganic filler, etc., in a solvent. It is preferable to first disperse the hydrophobic insulating inorganic filler in a solvent, and then mix the resin and curing agent into the second adhesive layer-forming composition.

[0110] The composition for forming the second adhesive layer preferably further contains a dispersant. In this case, the dispersant can increase the dispersibility of the hydrophobic insulating inorganic filler and can easily suppress a decrease in the function (e.g., adhesion strength) of the second adhesive layer 12b. As the dispersant, for example, a surfactant such as metal soap (zinc stearate, etc.) is used. When the resin contains a modified polyolefin resin, the modified polyolefin resin can also function as the dispersant. From the viewpoint of increasing the dispersibility of the hydrophobic insulating inorganic filler, it is preferable to disperse the hydrophobic insulating inorganic filler using a dispersing device such as a bead mill.

[0111] The average particle size of the hydrophobic insulating inorganic filler in the composition for forming the second adhesive layer is not particularly limited, but is preferably 20 μm or less. By making the average particle size of the hydrophobic insulating inorganic filler 20 μm or less, the dispersion state of the hydrophobic insulating inorganic filler can be maintained well, and the decrease in the cohesive force of the second adhesive layer 12b as a coating film after film formation can be suppressed. In addition, the hydrophobic insulating inorganic filler is less likely to fall off from the second adhesive layer 12b. Furthermore, the height of the convex portion from the surface of the second adhesive layer 12b is not too large, and air bubbles are less likely to enter between the sealant layer 16 and the second adhesive layer 12b when the sealant layer 16 is attached. The average particle size of the hydrophobic insulating inorganic filler is more preferably 15 μm or less, and particularly preferably 10 μm or less. The average particle size of the hydrophobic insulating inorganic filler is preferably 1 μm or more. In this case, aggregation between particles is less likely to occur and aggregates are less likely to form during dispersion, and the average particle size is more stable, compared to when the average particle size of the hydrophobic insulating inorganic filler is less than 1 μm.

[0112] In the second adhesive layer-forming composition, the content of the hydrophobic insulating inorganic filler in the total solid content is preferably 20 mass % or less. In this case, the viscosity (thixotropy) of the composition for forming the second adhesive layer does not increase too much compared to when the content of hydrophobic insulating inorganic filler in the total solids of the composition for forming the second adhesive layer exceeds 20 mass %, and the composition for forming the second adhesive layer becomes more suitable for coating.

[0113] The sealant layer 16 can be produced, for example, by a melt extrusion molding machine using a T-die, using the above-mentioned resin composition for forming the sealant layer for forming the sealant layer 16. In the melt extrusion molding machine, the processing speed can be set to 80 m / min or more from the viewpoint of productivity.

[0114] When forming the sealant layer 16 containing a hydrophobic insulating inorganic filler, a master batch may be prepared by mixing a resin and a hydrophobic insulating inorganic filler in advance, and the master batch may be mixed with the above-mentioned base resin when performing extrusion lamination or the like to obtain a resin composition for forming a sealant layer. In this case, the base resin used is one having properties, such as MFR, similar to those of the resin contained in the master batch. The resin to be mixed with the hydrophobic insulating inorganic filler when preparing the master batch may be a modified polyolefin resin. As the modified polyolefin resin, an acid-modified polyolefin resin is particularly preferred from the viewpoint of improving dispersibility in the base resin. Furthermore, the concentration of the masterbatch in the resin composition for forming a sealant layer may be, for example, 5 to 50% by mass. When the concentration of the masterbatch in the resin composition for forming a sealant layer is 5% by mass or more, the masterbatch can be sufficiently dispersed in the sealant layer 16. When the concentration of the masterbatch in the resin composition for forming a sealant layer is 50% by mass or less, the masterbatch is sufficiently dispersed by kneading during extrusion, and defects such as film breakage are unlikely to occur.

[0115] In addition, it is preferable that the resin composition for forming the sealant layer further contains a dispersant when forming the sealant layer 16. In this case, the dispersant can increase the dispersibility of the hydrophobic insulating inorganic filler and also makes it easier to suppress a decrease in the function of the sealant layer 16 (for example, adhesion strength, sealing strength, etc.). As the dispersant, for example, a surfactant such as metal soap (zinc stearate, etc.) is used. When the resin contains a modified polyolefin resin, the modified polyolefin resin can also function as the dispersant.

[0116] The average particle size of the hydrophobic insulating inorganic filler in the resin composition for forming the sealant layer is not particularly limited, but is preferably 20 μm or less. By making the average particle size of the hydrophobic insulating inorganic filler 20 μm or less, the dispersion state of the hydrophobic insulating inorganic filler can be well maintained. The average particle size of the hydrophobic insulating inorganic filler is more preferably 15 μm or less, and particularly preferably 10 μm or less. The average particle size of the hydrophobic insulating inorganic filler is preferably 1 μm or more. In this case, aggregation between particles is less likely to occur and aggregates are less likely to form during dispersion, and the average particle size is stable, compared to when the average particle size of the hydrophobic insulating inorganic filler is less than 1 μm.

[0117] (Aging process) This step is a step of aging (curing) the second laminate. By aging the second laminate, it is possible to promote adhesion between the metal layer 14c / the second corrosion prevention treatment layer 14b / the second adhesive layer 12b / the sealant layer 16. The aging treatment can be carried out at a temperature in the range of room temperature to 100°C. The aging time is, for example, 1 to 10 days.

[0118] In this manner, the exterior packaging material 10 shown in FIG. 1 can be manufactured.

[0119] Next, a description will be given of an example of a method for manufacturing the exterior material 20 shown in Fig. 2. Note that the method for manufacturing the exterior material 20 is not limited to the following method.

[0120] The manufacturing method of the exterior material 20 includes the steps of forming anti-corrosion treatment layers 14a, 14b on both sides of a metal layer 14c to form a barrier layer 13, bonding the base material layer 11 and the barrier layer 13 together using a first adhesive layer 12a to obtain a first laminate, further laminating an adhesive resin layer 15 and a sealant layer 16 on the barrier layer 13 of the first laminate to obtain a second laminate, and, if necessary, heat treating the obtained second laminate. The process up to the step of bonding the base layer 11 and the barrier layer 13 to obtain the first laminate can be carried out in the same manner as the manufacturing method of the packaging material 10 described above.

[0121] (Laminating process of adhesive resin layer and sealant layer) This step is a step of forming an adhesive resin layer 15 and a sealant layer 16 on the second corrosion prevention treatment layer 14b of the first laminate formed in the previous step to obtain a second laminate. Examples of the method include a method of sand laminating the adhesive resin layer 15 together with the sealant layer 16 using an extrusion laminator, and a thermal lamination method such as co-extrusion in which the adhesive resin layer 15 and the sealant layer 16 are extruded. In forming the adhesive resin layer 15 and the sealant layer 16, for example, the above-mentioned resin composition for forming an adhesive resin layer and the resin composition for forming a sealant layer are used.

[0122] When forming the adhesive resin layer 15, a master batch may be prepared by mixing a resin with a hydrophobic insulating inorganic filler in advance, and the master batch may be mixed with the above-mentioned base resin to obtain a resin composition for forming the adhesive resin layer. In this case, the base resin used is one having properties, such as MFR, similar to those of the resin contained in the master batch. The resin to be mixed with the hydrophobic insulating inorganic filler when preparing the master batch may be a modified polyolefin resin. As the modified polyolefin resin, an acid-modified polyolefin resin is particularly preferable from the viewpoints of being easily mixed with the base resin and improving the adhesion between the barrier layer 13 and the adhesive resin layer 15. Furthermore, the concentration of the masterbatch in the resin composition for forming an adhesive resin layer may be, for example, 5 to 50% by mass. When the concentration of the masterbatch in the resin composition for forming an adhesive resin layer is 5% by mass or more, the masterbatch can be sufficiently dispersed in the adhesive resin layer 15. When the concentration of the masterbatch in the resin composition for forming an adhesive resin layer is 50% by mass or less, the masterbatch is sufficiently dispersed by kneading during extrusion, and defects such as film breakage are unlikely to occur.

[0123] In addition, it is preferable that the resin composition for forming the adhesive resin layer further contains a dispersant when forming the adhesive resin layer 15. In this case, the dispersant can increase the dispersibility of the hydrophobic insulating inorganic filler and also makes it easier to suppress a decrease in the function (e.g., adhesion strength, etc.) of the adhesive resin layer 15. As the dispersant, for example, a surfactant such as metal soap (zinc stearate, etc.) is used. When the resin contains a modified polyolefin resin, the modified polyolefin resin can also function as the dispersant.

[0124] The method for forming the sealant layer 16 is the same as the method for forming the sealant layer 16 in the method for producing the exterior packaging material 10.

[0125] This process produces a second laminate in which the layers are stacked in the following order: base layer 11 / first adhesive layer 12a / first corrosion prevention treatment layer 14a / metal layer 14c / second corrosion prevention treatment layer 14b / adhesive resin layer 15 / sealant layer 16, as shown in Figure 2.

[0126] (Heat treatment process) This step is a step of heat-treating the second laminate. Heat-treating the second laminate can improve adhesion between the metal layer 14c, the second corrosion prevention treatment layer 14b, the adhesive resin layer 15, and the sealant layer 16. As a method of heat treatment, it is preferable to treat at a temperature at least equal to or higher than the melting point of the adhesive resin layer 15.

[0127] In this manner, the exterior material 20 shown in FIG. 2 can be manufactured.

[0128] [Electricity storage device] Next, an embodiment of the power storage device of the present disclosure will be described with reference to Fig. 3 and Fig. 4. Fig. 3 is a perspective view of the embodiment of the power storage device of the present disclosure, and Fig. 4 is a cross-sectional view showing the battery cell of Fig. 3. 3, the power storage device 50 includes a battery cell 52 and an exterior bag 54 that holds the battery cell 52 and has metal terminals 53 therebetween. The power storage device 50 may further include two metal terminals (current extraction terminals) 53 extending from the battery cell 52 for extracting current to the outside.

[0129] As shown in FIG. 4, the battery cell 52 includes a positive electrode 52a, an electrolyte 52c, and a negative electrode 52b in this order.

[0130] The exterior bag 54 has an exterior material 10. In the exterior material 10, the base material layer 11 is the outermost layer and the sealant layer 16 is the innermost layer. The exterior bag 54 is formed by folding one exterior material 10 in half and heat-sealing the peripheral portions, or by stacking two exterior materials 10 and heat-sealing the peripheral portions, so that the base material layer 11 is on the outer side of the electricity storage device 50 and the sealant layer 16 is on the inner side of the electricity storage device 50. The metal terminal 53 is held by the peripheral edge of the exterior bag 54. The metal terminal 53 may be held by the exterior material 10 via a tab sealant.

[0131] According to the energy storage device 50, even when the exterior material 10 is used in a heated and pressurized state as the exterior bag 54, the energy storage device 50 has excellent insulating properties, so that even when the energy storage device 50 is heated in a state where it is pressurized in a direction perpendicular to the interface between the battery cell 52 and the exterior material 10, a short circuit between the positive electrode 52a or negative electrode 52b in the battery cell 52 and the metal layer 14c of the exterior material 10 can be prevented.

[0132] The electrolyte 52c may be, for example, a solid electrolyte. In this case, the power storage device 50 is an all-solid-state battery. Examples of the solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes.

[0133] Metal terminal 53 is a part of the current collector taken out from exterior material 10, and is made of metal foil such as copper foil or aluminum foil. In addition, in the electricity storage device 50, the exterior packaging material 20 may be used in place of the exterior packaging material 10. EXAMPLES

[0134] The present disclosure will be described more specifically below based on examples, but the present disclosure is not limited to the following examples.

[0135] [Materials used] The materials used in the examples and comparative examples are shown below. <Base material layer> A nylon (Ny) film (manufactured by Toyobo Co., Ltd.) having a thickness of 15 μm was used.

[0136] <Composition for forming the first adhesive layer> As the composition for forming the first adhesive layer, a polyurethane adhesive (manufactured by Toyo Ink Co., Ltd.) containing a polyester polyol-based base agent and an adduct-based curing agent of tolylene diisocyanate was used.

[0137] <Materials for forming the first corrosion prevention treatment layer (base layer side) and the second corrosion prevention treatment layer (sealant layer side)> As materials for forming the first corrosion prevention treatment layer (base layer side) and the second corrosion prevention treatment layer (sealant layer side), the following (CL-1) and (CL-2) were used. (CL-1): "Sodium polyphosphate stabilized cerium oxide sol" obtained by using distilled water as a solvent and adjusting the solid concentration to 10% by mass. The sodium polyphosphate-stabilized cerium oxide sol was obtained by mixing 10 parts by mass of sodium phosphoric acid with 100 parts by mass of cerium oxide. (CL-2): A composition consisting of 90% by mass of "polyallylamine (manufactured by Nittobo Co., Ltd.)" and 10% by mass of "polyglycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation)" obtained by adjusting the solid content concentration to 5% by mass using distilled water as a solvent.

[0138] <Metal layer> A soft aluminum foil having a thickness of 40 μm that had been annealed and degreased (manufactured by Toyo Aluminum Co., Ltd., "Material 8079") was used.

[0139] <Composition for forming adhesive layer> As the adhesive layer-forming composition, a second adhesive layer-forming composition (adhesive) and an adhesive resin layer-forming resin composition (adhesive resin) were prepared as follows. (Composition for forming second adhesive layer) The composition for forming the second adhesive layer was prepared by dispersing the hydrophobic insulating inorganic filler described below in a solvent consisting of methylcyclohexane and methyl ethyl ketone as necessary, and then adding the acid-modified polyolefin resin-containing liquid, polyfunctional isocyanate compound-containing liquid, and carbodiimide compound-containing liquid described below.

[0140] (Resin composition for forming adhesive resin layer) Using a twin-screw extruder, the following hydrophobic insulating inorganic filler was dispersed as necessary in an adhesive resin (random polypropylene (PP)-based acid-modified polypropylene resin composition, manufactured by Mitsui Chemicals, Inc.) to prepare a resin composition for forming an adhesive resin layer.

[0141] (1) Acid-modified polyolefin resin-containing liquid Manufactured by Nippon Paper Industries Co., Ltd., Product name: 150S, Acid-modified polyolefin resin: Maleic anhydride-modified polypropylene (2) Liquid containing polyfunctional isocyanate compound Manufactured by Tosoh Corporation, product name: Coronate HXR, multifunctional isocyanate compound: hexamethylene diisocyanate (HDI)-based polyisocyanurate resin (3) Carbodiimide compound-containing liquid Manufactured by Nisshinbo Chemical Inc., Product name: V-03 (4) Hydrophobic insulating inorganic filler A: Hydrophobic silica filler (product name "Silohobic 100", manufactured by Fuji Silysia Chemical Ltd., average particle size: 2.7 μm, surface treated with an organosilicon compound) B: Hydrophobic silica filler (product name "Silohobic 704", Fuji Silysia Chemical Ltd., average particle size: 6.2 μm, surface treated with organic silicon compound) C: Hydrophobic silica filler (product name "Silohobic 4004", manufactured by Fuji Silysia Chemical Ltd., average particle size: 8.0 μm, surface treated with an organosilicon compound)

[0142] <Resin composition for forming sealant layer> A sealant layer-forming resin composition containing a polypropylene-polyethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F744NP) was prepared using a twin-screw extruder.

[0143] [Creating exterior materials] (Examples 1 and 3-4) First, a first and a second corrosion prevention treatment layer were formed on both sides of a metal layer by the following procedure. That is, the above-mentioned (CL-1) was applied to both sides of the metal layer in a dry coating amount of 70 mg / m 2 The mixture was applied by microgravure coating so that the thickness of the coating was 200 mm, and then baked in a drying unit at 200° C. to obtain a first layer. Next, (CL-2) was applied on the obtained first layer in a dry coating amount of 20 mg / m 2 The second layer was obtained by applying the first and second layers by microgravure coating so that the first and second layers were coated on both sides of the metal layer as the first and second corrosion prevention layers, respectively, to obtain a barrier layer. This composite layer exhibits corrosion prevention performance by combining the two types of materials, (CL-1) and (CL-2).

[0144] Next, the first corrosion prevention treatment layer side of the barrier layer obtained as described above was attached to the base layer by dry lamination using a composition for forming a first adhesive layer (polyurethane adhesive). Specifically, lamination of the barrier layer and the base layer was performed by applying a polyurethane adhesive to the surface of the first corrosion prevention treatment layer opposite the metal layer so that the thickness after curing was 5 μm, drying at 80° C. for 1 minute, laminating the base layer thereon, and aging at 60° C. for 72 hours. In this way, a first laminate including the barrier layer and the base layer was obtained.

[0145] Next, the first laminate obtained as described above was set on the unwinding section of the extrusion laminator, and the second adhesive layer forming composition, in which the type, content and average particle size of the hydrophobic insulating inorganic filler in the total solid content of the second adhesive layer forming composition were as shown in Table 1, was applied on the second corrosion prevention treatment layer so that the thickness after curing was 20 μm, and after drying at 100 ° C. for 1 minute, it was laminated with a sealant layer and aged at 40 ° C. for 72 hours. This sealant layer was produced by extruding the sealant layer forming resin composition under processing conditions of 270 ° C. and 100 m / min.

[0146] In this way, an exterior material (substrate layer / first adhesive layer / first corrosion prevention treatment layer / metal layer / second corrosion prevention treatment layer / second adhesive layer / sealant layer) was produced.

[0147] Example 2 In the same manner as in Example 1, a first laminate including a barrier layer and a base layer was obtained.

[0148] Next, the first laminate obtained as described above was set on the unwinding section of an extrusion laminator, and an adhesive resin composition having a hydrophobic insulating inorganic filler type, content and average particle size as shown in Table 1 and a resin composition for forming a sealant layer were co-extruded on the second corrosion prevention treatment layer under processing conditions of 270°C and 100m / min to laminate an adhesive resin layer (thickness 20μm) and a sealant layer (thickness 60μm) in this order, thereby obtaining a second laminate.

[0149] The second laminate thus obtained was subjected to a heat treatment so that the maximum temperature of the second laminate reached was 190° C. In this manner, an exterior material (substrate layer / first adhesive layer / first corrosion prevention treatment layer / metal layer / second corrosion prevention treatment layer / adhesive resin layer / sealant layer) was produced.

[0150] (Examples 3 to 4) In the composition for forming the second adhesive layer, the type, content and average particle size of the hydrophobic insulating inorganic filler in the total solid content were as shown in Table 1, and in the composition for forming the second adhesive layer, the amount of the polyfunctional isocyanate compound per 100 parts by mass of acid-modified polyolefin was 1 part by mass as shown in Table 1. An exterior material (substrate layer / first adhesive layer / first corrosion prevention treatment layer / metal layer / second corrosion prevention treatment layer / second adhesive layer / sealant layer) was prepared in the same manner as in Example 1.

[0151] Comparative Example 1 An exterior material (substrate layer / first adhesive layer / first corrosion prevention treatment layer / metal layer / second corrosion prevention treatment layer / second adhesive layer / sealant layer) was prepared in the same manner as in Example 1, except that in the composition for forming the second adhesive layer, the content of hydrophobic insulating inorganic filler in the total solids was 0 mass% as shown in Table 1, in the composition for forming the second adhesive layer, the amount of polyfunctional isocyanate compound per 100 mass parts of acid-modified polyolefin was 0 mass parts as shown in Table 1, and the MFR of the sealant layer was 30 g / 10 minutes as shown in Table 1.

[0152] Comparative Example 2 An exterior material (substrate layer / first adhesive layer / first corrosion prevention treatment layer / metal layer / second corrosion prevention treatment layer / adhesive resin layer / sealant layer) was prepared in the same manner as in Example 2, except that the content of hydrophobic insulating inorganic filler in the adhesive resin composition was 0 mass% as shown in Table 1, the amount of polyfunctional isocyanate compound in the composition for forming the second adhesive layer was 0 mass parts per 100 mass parts of acid-modified polyolefin as shown in Table 1, and the MFR of the sealant layer was 30 g / 10 min as shown in Table 1.

[0153] <Evaluation> (1) Heat sealability (1-1) Preparation of test specimens The exterior materials obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were cut to a size of 50 mm (TD) x 100 mm (MD) to obtain cut pieces. The cut pieces were folded in two so as to sandwich a chemically treated aluminum foil cut to a size of 50 mm x 50 mm, and the end opposite to the folded part was heat sealed over a width of 10 mm at 180°C / 0.6 MPa / 10 seconds. Then, a 15 mm width was cut out along the MD so as to include the center part in the longitudinal direction (TD) of the heat sealed part (see FIG. 5) to prepare a test piece. (1-2) Seal strength (room temperature) The test pieces prepared as described above were subjected to a T-peel test to peel the exterior material from the chemically treated aluminum foil at a room temperature (25°C) environment and a tensile speed of 50 mm / min using a tensile tester (manufactured by Shimadzu Corporation), and the seal strength (burst strength) was measured. (1-3) Evaluation The heat sealability was evaluated based on the seal strength (burst strength) obtained in (1-2) above, according to the following criteria. The seal strength and evaluation results are shown in Table 1. (standard) A: Seal strength is 20N / 15mm or more B: Seal strength is 15N / 15mm or more and less than 20N / 15mm C: Seal strength is less than 15N / 15mm

[0154] (2) Adhesion The exterior materials obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were cut to a width of 15 mm and a length of 120 mm to prepare test pieces. A T-peel test for peeling between the metal layer and the sealant layer was then performed on these test pieces using a tensile tester (manufactured by Shimadzu Corporation) at room temperature and a tensile speed of 50 mm / min to measure the laminate strength. The adhesion between the metal layer and the sealant layer was evaluated based on the obtained laminate strength and on the following criteria. The laminate strength and the evaluation results are shown in Table 1. (standard) A: Lamination strength is 10N / 15mm or more, or peeling is not possible B: Lamination strength is 3N / 15mm or more and less than 10N / 15mm C: Lamination strength is less than 3N / 15mm

[0155] (3) Insulation properties after heating and pressurization The packaging materials obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were cut into test pieces with a size of 100 mm x 100 mm. The test pieces were sandwiched between two electrodes with a size of 20 mm x 20 mm, and heated and pressed for 24 hours under conditions of 150°C and 3 MPa, after which the dielectric breakdown voltage in the direction perpendicular to the surface of the test piece was measured. The insulation properties of the packaging materials after heating and pressing were judged from the measured dielectric breakdown voltage based on the following criteria. The results are shown in Table 1. (standard) ○: Dielectric breakdown voltage is 50V or more ×: Breakdown voltage is less than 50V

[0156] [Table 1]

[0157] The results shown in Table 1 show that in Examples 1 to 4, the insulation voltage after heating and pressing was higher than 100V, whereas in Comparative Examples 1 and 2, the insulation voltage after heating and pressing was lower than 10V.

[0158] From the above, it was confirmed that the exterior packaging material for an electricity storage device according to the present disclosure has excellent insulating properties even when used under heated and pressurized conditions as an exterior bag for an electricity storage device.

[0159] The outline of this disclosure is as follows. [1] An exterior packaging material for an electricity storage device comprising, in this order, at least a base material layer, a barrier layer including a metal layer, an adhesive layer, and a sealant layer, wherein the adhesive layer contains a hydrophobic insulating inorganic filler. [2] The exterior packaging material for a storage battery device according to [1], wherein the composition contains the hydrophobic insulating inorganic filler, a resin, and a polyfunctional isocyanate compound, and the resin is a modified polyolefin resin. [3] The packaging material for a storage battery device according to [1] or [2], wherein the MFR of the sealant layer is 20 g / 10 min or less. [4] The packaging material for a power storage device according to any one of [1] to [3], wherein the sealant layer has a melting point of 160° C. or higher. [5] The packaging material for a power storage device according to any one of [1] to [4], wherein the hydrophobic insulating inorganic filler has an average particle size of 1 to 20 μm. [6] The packaging material for a power storage device according to any one of [1] to [5], which has a dielectric breakdown voltage of 100 V or more when heated and pressurized under conditions of 150° C. and 3 MPa for 24 hours. [7] The exterior packaging material for a storage battery device according to [2], wherein the modified polyolefin resin is an acid-modified polyolefin resin. [8] The exterior packaging material for a storage battery device according to [2], wherein the polyfunctional isocyanate compound includes an isocyanurate-type polyfunctional isocyanate compound. [9] The packaging material for a power storage device according to any one of [1] to [8], wherein the content of the hydrophobic insulating inorganic filler in the adhesive layer is 0.5 to 20 mass %.

[10] The packaging material for a power storage device according to any one of [1] to [9], wherein the barrier layer further comprises a corrosion prevention treatment layer on one or both surfaces of the metal layer.

[11] The exterior packaging material for a power storage device according to any one of [1] to

[10] , wherein the power storage device is an all-solid-state battery.

[12] An electricity storage device comprising: a battery cell having a positive electrode, an electrolyte, and a negative electrode in this order; and an outer bag that houses the battery cell, the outer bag having the outer casing for an electricity storage device according to any one of [1] to

[10] .

[13] The power storage device according to

[12] , which is an all-solid-state battery. [Explanation of symbols]

[0160] Reference Signs List: 10, 20...outer packaging material (outer packaging material for electricity storage device), 11...base material layer, 12b...second adhesive layer (adhesive layer), 13...barrier layer, 14c...metal layer, 15...adhesive resin layer (adhesive layer), 16...sealant layer, 50...electricity storage device, 52...battery cell, 52a...positive electrode, 52b...negative electrode, 52c...electrolyte, 54...outer packaging bag.

Claims

1. An exterior material for a storage battery device, comprising at least a base layer, a barrier layer including a metal layer, an adhesive layer, and a sealant layer in this order, The adhesive layer comprises a hydrophobic insulating inorganic filler.

2. the adhesive layer contains the hydrophobic insulating inorganic filler, a resin and a polyfunctional isocyanate compound, The packaging material for an electricity storage device according to claim 1 , wherein the resin is a modified polyolefin resin.

3. The packaging material for an electricity storage device according to claim 1 , wherein the sealant layer has an MFR of 20 g / 10 min or less.

4. The packaging material for an electricity storage device according to claim 1 , wherein the sealant layer has a melting point of 160° C. or higher.

5. 2. The packaging material for a power storage device according to claim 1, wherein the hydrophobic insulating inorganic filler has an average particle size of 1 to 20 μm.

6. 2 . The packaging material for an electricity storage device according to claim 1 , which has a dielectric breakdown voltage of 100 V or more when heated and pressed under conditions of 150° C. and 3 MPa for 24 hours.

7. The exterior packaging material for an electricity storage device according to claim 2 , wherein the modified polyolefin resin is an acid-modified polyolefin resin.

8. The exterior packaging material for an electricity storage device according to claim 2 , wherein the polyfunctional isocyanate compound includes an isocyanurate-type polyfunctional isocyanate compound.

9. 2. The packaging material for a power storage device according to claim 1, wherein a content of the hydrophobic insulating inorganic filler in the adhesive layer is 0.5 to 20 mass %.

10. The packaging material for an electricity storage device according to claim 1 , wherein the barrier layer further comprises a corrosion prevention treatment layer on one or both surfaces of the metal layer.

11. The exterior packaging material for a power storage device according to claim 1 , wherein the power storage device is an all-solid-state battery.

12. a battery cell having a positive electrode, an electrolyte, and a negative electrode in this order; an exterior bag that houses the battery cell; The outer bag comprises the outer casing material for an electricity storage device according to any one of claims 1 to 10.

13. The power storage device according to claim 12 , which is an all-solid-state battery.

Citation Information

Patent Citations

  • Exterior material for battery and lithium secondary battery

    JP2014127258A