Electrophotographic photoreceptor, electrophotographic photoreceptor cartridge, and image forming device

By employing low-symmetry polyfunctional acrylates or methacrylates in the protective layer of electrophotographic photoreceptors, the issues of surface unevenness and image blurring are resolved, resulting in a smooth and mechanically durable photoreceptor with enhanced image quality.

JP2024168996APending Publication Date: 2024-12-05MITSUBISHI CHEM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023086156
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing electrophotographic photoreceptors face issues with surface unevenness and image blurring due to the use of certain polyfunctional acrylates or polyfunctional methacrylates in forming protective layers, leading to poor appearance and mechanical instability.

Method used

The use of specific polyfunctional acrylates or polyfunctional methacrylates with low symmetry structures, such as those represented by formulas (1) and (2), in forming a protective layer on a conductive support, which prevents crystal precipitation and maintains a smooth surface, thereby preventing image blurring and enhancing mechanical strength.

Benefits of technology

The proposed solution results in a smooth photoreceptor surface with high Martens hardness and elastic deformation rate, effectively preventing image blurring and ensuring good appearance and mechanical durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168996000001_ABST
    Figure 2024168996000001_ABST
Patent Text Reader

Abstract

To provide an electrophotographic photoreceptor which has good appearance with a smooth photoreceptor surface, is capable of preventing image blur, and yet offers high Martens hardness and elastic deformation rate.SOLUTION: An electrophotographic photoreceptor is provided, comprising a sequentially arranged photosensitive layer and protective layer containing a polymer having structures represented by formulas (1) and (2) below.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrophotographic photoreceptor used in copiers, printers, etc., and to an electrophotographic photoreceptor cartridge and an image forming apparatus using the same. [Background technology]

[0002] In printers and copiers, when a charged organic photoconductor (OPC) drum is irradiated with light, the part is discharged, an electrostatic latent image is generated, and an image is obtained by attaching toner to the electrostatic latent image. In such devices that use electrophotography, the photoconductor is the core material.

[0003] This type of organic photoreceptor has a wide range of material options and is easy to control the characteristics of the photoreceptor, so that "functionally separated photoreceptors" in which the functions of charge generation and transport are shared by different compounds are becoming mainstream. For example, a single-layer electrophotographic photoreceptor (hereinafter referred to as a single-layer photoreceptor) having a charge generation material (CGM) and a charge transport material (CTM) in the same layer, and a laminated electrophotographic photoreceptor (hereinafter referred to as a laminated photoreceptor) formed by laminating a charge generation layer containing a charge generation material (CGM) and a charge transport layer containing a charge transport material (CTM) are known. In addition, the charging method of the photoreceptor can be a negative charging method in which the photoreceptor surface is negatively charged, or a positive charging method in which the photoreceptor surface is positively charged. Combinations of layer structures and charging methods of photoreceptors currently in practical use include "negatively charged multi-layer photoreceptors" and "positively charged single-layer photoreceptors."

[0004] A "negatively charged laminated photoreceptor" generally has a structure in which an undercoat layer (UCL) made of a resin or the like is provided on a conductive substrate such as an aluminum tube, on which a charge generation layer (CGL) made of a charge generation material (CGM) and a resin or the like is provided, on which a charge transport layer (CTL) made of a hole transport material (HTM) and a resin or the like is provided.

[0005] On the other hand, a "positively charged single-layer photoreceptor" generally has a configuration in which an undercoat layer (UCL) made of a resin or the like is provided on a conductive substrate such as an aluminum tube, and a single-layer photosensitive layer made of a charge generating material (CGM), a hole transporting material (HTM), an electron transporting material (ETM), and a resin or the like is provided on top of the undercoat layer (UCL) (see, for example, Patent Document 1).

[0006] In either photoconductor, the surface of the photoconductor is charged by corona discharge or contact, and then the photoconductor is exposed to light to neutralize the surface charge, forming an electrostatic latent image due to the potential difference with the surrounding surface. Toner is then brought into contact with the photoconductor surface to form a toner image corresponding to the electrostatic latent image, which is then transferred to paper or the like and heated to melt and fix it to complete the print.

[0007] As described above, the basic structure of an electrophotographic photoreceptor is a photosensitive layer formed on a conductive support. In order to improve abrasion resistance, etc., a protective layer may be provided on the photosensitive layer.

[0008] As a technique for improving the mechanical strength or abrasion resistance of the photoreceptor surface, a photoreceptor has been disclosed in which a layer containing a compound having a chain-polymerizable functional group is formed as the outermost layer of the photoreceptor, and this is polymerized by applying energy such as heat, light, or radiation to form a hardened resin layer (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0009] [Patent Document 1] U.S. Pat. No. 9,417,538 [Patent Document 2] International Publication No. 2010 / 035683 (Patent Publication No. 5263296) Summary of the Invention [Problem to be solved by the invention]

[0010] As described above, a method for forming a protective layer using a polyfunctional acrylate or polyfunctional methacrylate as a curable resin is known as a method for improving the mechanical strength or abrasion resistance of the surface of a photoreceptor. However, when a protective layer is formed using a certain type of multifunctional acrylate or multifunctional methacrylate, there is a problem that unevenness occurs on the photoreceptor surface, resulting in poor appearance, as well as image deletion (image blur).

[0011] An object of the present invention is to provide a new electrophotographic photoreceptor which, with respect to an electrophotographic photoreceptor having a photosensitive layer and a protective layer in that order on a conductive support, has a smooth photoreceptor surface with a good appearance, can prevent image deletion, and yet has a high Martens hardness and elastic deformation rate. [Means for solving the problem]

[0012] The present invention solves the above problems by forming a protective layer using a compound having a specific structure among polyfunctional acrylates or polyfunctional methacrylates. That is, the gist of the present invention resides in the following [1] to [5].

[0013] [1] An electrophotographic photoreceptor having a photosensitive layer and a protective layer successively provided on a conductive support, the protective layer containing a polymer having structures represented by the following formulas (1) and (2):

[0014] [Formula (1)] TIFF2024168996000002.tif53170

[0015] In formula (1), l, m, n, and o are each an integer of 0 to 10, and l+m+n+o is greater than or equal to 1. R each independently represents an alkylene group having 1 to 8 carbon atoms which may have a substituent, an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent, or -O-(C=O)-(CX2) p- (wherein p is an integer of 1 to 6, and X is a hydrogen atom or a substituent). T represents a bond to any atom. Q represents a hydroxyl group or the following formula (3). Z 1 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and at least one of them is an alkyl group having 1 to 4 carbon atoms.

[0016] [Formula (2)] TIFF2024168996000003.tif49170

[0017] In formula (2), f, g, h, i, j, and k are each an integer of 0 to 10, and f+g+h+i+j+k is greater than or equal to 1. R each independently represents an alkylene group having 1 to 8 carbon atoms which may have a substituent, an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent, or -O-(C=O)-(CX2) p - (wherein p is an integer of 1 to 6, and X is a hydrogen atom or a substituent). T represents a bond to any atom. Q represents a hydroxyl group or the following formula (3). Z 1 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and at least one of them is an alkyl group having 1 to 4 carbon atoms.

[0018] [Formula (3)] TIFF2024168996000004.tif37170

[0019] In formula (3), Z 2 represents a bond to R in formula (1) or (2). 1 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. T represents a bond to any atom.

[0020] [2] An electrophotographic photoreceptor having a photosensitive layer and a protective layer successively provided on a conductive support, the protective layer containing a polymer of a compound a having a structure represented by the following formula (1') and a compound b having a structure represented by the following formula (2'):

[0021] [Formula (1')] TIFF2024168996000005.tif54170

[0022] In formula (1'), l, m, n, and o are each an integer of 0 to 10, and l+m+n+o is greater than or equal to 1. R each independently represents an alkylene group having 1 to 8 carbon atoms which may have a substituent, an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent, or -O-(C=O)-(CX2) p - (wherein p is an integer of 1 to 6, and X is a hydrogen atom or a substituent). Q represents a hydroxyl group or the following formula (3'). Z 1 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and at least one of them is an alkyl group having 1 to 4 carbon atoms.

[0023] [Formula (2')] TIFF2024168996000006.tif49170

[0024] In formula (2'), f, g, h, i, j, and k are each an integer of 0 to 10, and f+g+h+i+j+k is greater than or equal to 1. R each independently represents an alkylene group having 1 to 8 carbon atoms which may have a substituent, an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent, or -O-(C=O)-(CX2) p - (wherein p is an integer of 1 to 6, and X is a hydrogen atom or a substituent). Q represents a hydroxyl group or the following formula (3'). Z 1 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and at least one of them is an alkyl group having 1 to 4 carbon atoms.

[0025] [Formula (3')] TIFF2024168996000007.tif30170

[0026] In formula (3'), Z2 represents a bond to R in formula (1') or formula (2'). 1 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.

[0027] [3] R in at least one of the formulas (1), (2), (1') and (2') is an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent, or -O-(C=O)-(CX2) p - (wherein p is an integer of 1 to 6, and X represents a hydrogen atom or a substituent).

[0028] [4] An electrophotographic photoreceptor cartridge comprising the electrophotographic photoreceptor according to any one of [1] to [3]. [5] An image forming apparatus having the electrophotographic photoreceptor according to any one of [1] to [3]. Effect of the Invention

[0029] The electrophotographic photoreceptor of the present invention has a smooth surface and a good appearance, can prevent image deletion, and has a high Martens hardness and elastic deformation rate. [Brief description of the drawings]

[0030] [Figure 1] 1 is a diagram illustrating an example of the configuration of an image forming apparatus that can be configured using an electrophotographic photoreceptor according to an example of the present invention. [Diagram 2] 1 is a graph showing a general relationship between the indentation depth of an indenter and a load curve when measuring the Martens hardness and elastic deformation rate of a photoreceptor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] The following describes in detail the mode for carrying out the present invention (hereinafter, the embodiment of the invention). Note that the present invention is not limited to the following embodiment, and can be carried out in various modifications within the scope of the gist of the present invention.

[0032] <<The present electrophotographic photoreceptor>> An electrophotographic photoreceptor according to one embodiment of the present invention (also referred to as "the present electrophotographic photoreceptor") is an electrophotographic photoreceptor having a photosensitive layer and a protective layer, successively provided on a conductive support, and it is preferable that the protective layer contains a cured product obtained by curing a curable compound.

[0033] The present electrophotographic photoreceptor may optionally have layers other than the photosensitive layer and the protective layer. The electrophotographic photoreceptor may be charged by either a negative charging method in which the surface of the photoreceptor is negatively charged or a positive charging method in which the surface of the photoreceptor is positively charged.

[0034] In the present electrophotographic photoreceptor, the side opposite to the conductive support is the upper side or front side, and the conductive support side is the lower side or back side. From the viewpoint of obtaining the effects of the present invention more effectively, it is preferable that the protective layer is the outermost layer.

[0035] <Main protective layer> The protective layer of the present electrophotographic photoreceptor (also referred to as the "present protective layer") is preferably a layer containing a polymer having structures represented by the following formulas (1) and (2). When the protective layer contains polymers having structures represented by the following formulas (1) and (2), it may contain both a polymer having a structure represented by the following formula (1) and a polymer having a structure represented by the following formula (2), it may contain a polymer having both a structure represented by the following formula (1) and a structure represented by the following formula (2) in one polymer, or it may contain both of these two polymers.

[0036] [Formula (1)] TIFF2024168996000008.tif53170

[0037] [Formula (2)] TIFF2024168996000009.tif49170

[0038] The protective layer is also preferably a layer containing a polymer formed by polymerization of a compound a having a structure represented by the following formula (1') and a compound b having a structure represented by the following formula (2'). In other words, the protective layer contains a cured product formed by curing a curable compound, and the curable compound preferably contains a compound having a structure represented by the following formula (1') and a compound having a structure represented by the following formula (2'). When the protective layer contains a polymer formed by polymerization of a compound a having a structure represented by the following formula (1') and a compound b having a structure represented by the following formula (2'), the protective layer may contain both a polymer formed by polymerization of the compounds a and a polymer formed by polymerization of the compounds b, a polymer formed by polymerization of the compounds a and b, or both of these two polymers. Among these, it is preferable to contain a polymer formed by polymerization of the compound a and the compound b by polymerizing a mixture of the compound a and the compound b.

[0039] The mixture of the compound a and the compound b can be synthesized by, for example, mixing and reacting dipentaerythritol and pentaerythritol. In this case, it is preferable to further add, for example, ε-caprolactone to react. When ε-caprolactone is added, the linking group R in the formula (1), the formula (2), the following formula (1'), and the following formula (2') becomes -O-(C=O)-(CX2) p -(wherein p is an integer of 1 to 6, and X represents a hydrogen atom or a substituent) can be synthesized. When dipentaerythritol, pentaerythritol and ε-caprolactone are used, the amount of ε-caprolactone charged, i.e., the blending amount, is preferably 0.01 equivalent or more, more preferably 0.05 equivalent or more, and even more preferably 0.10 equivalent or more, relative to 1.0 equivalent of the total amount of dipentaerythritol and pentaerythritol charged, while it is preferably 2.0 equivalents or less, more preferably 1.0 equivalents or less, and even more preferably 0.5 equivalents or less.

[0040] [Formula (1')] TIFF2024168996000010.tif54170

[0041] [Formula (2')] TIFF2024168996000011.tif49170

[0042] As mentioned above, when a protective layer is formed using a certain type of multifunctional acrylate or multifunctional methacrylate, there is a problem that the appearance is poor due to the occurrence of unevenness on the photoreceptor surface, or the occurrence of unevenness in the film state, causing the surface to become partially rough, and that image flow (image blur) occurs. The former is presumed to be caused by the high crystallinity of the multifunctional acrylate or multifunctional methacrylate, which causes the crystals to precipitate on the photoreceptor surface. The latter is presumed to be caused by the structure and content balance of the multifunctional acrylate or multifunctional methacrylate, and if the symmetry of the structure is significantly disrupted, distortion occurs when polymerized, causing the film of the protective layer to become disordered, which in turn causes image flow. Compound a represented by the above formula (1') and compound b represented by the above formula (2') are each considered to be unlikely to precipitate crystals if they have a low symmetrical structure, but as mentioned above, there is a concern about image flow. By using compound a and compound b in combination, different structures are unlikely to be packed together, so that crystal precipitation is more suppressed and image flow is also unlikely to occur. In addition, compound b represented by the above formula (2') has a similar structure as a dimer of compound a represented by the above formula (1'), and is also preferable in that it does not adversely affect electrical properties even when used in combination. Therefore, when a protective layer is formed using the compound a and the compound b, crystals do not precipitate on the photoreceptor surface, the photoreceptor surface after curing becomes smooth, and image flow can be prevented. In other words, a photoreceptor whose protective layer contains a polymer obtained by polymerizing the compound a and the compound b does not precipitate crystals on the photoreceptor surface, the photoreceptor surface after curing becomes smooth, and image flow can be prevented. In other words, a photoreceptor whose protective layer contains a polymer having the structure represented by the formulas (1) and (2) does not precipitate crystals on the photoreceptor surface, the photoreceptor surface after curing becomes smooth, and image flow can be prevented.

[0043] [Formula (1) and Formula (1')] In the above formula (1) and formula (1'), l, m, n, and o are each an integer of 0 or more and 10 or less. Among them, it is preferable that any of l, m, n, and o is an integer of 1 or more, while it is preferable that l, m, n, and o are each an integer of 8 or less, more preferably an integer of 4 or less, and even more preferably an integer of 2 or less.

[0044] l+m+n+o means an equivalent amount of the linking chain R contained in the above formula (1) and the above formula (1'), and if it is 1 or more, it is preferable from the viewpoint of suppressing steric repulsion between groups having a C=O bond (e.g., (meth)acryloyl groups) arranged on the terminal side of the molecule and preventing detachment of the group having a C=O bond (e.g., (meth)acryloyl groups), and it is more preferable that it is 2 or more. On the other hand, if it is 20 or less, it is preferable from the viewpoint of the mechanical strength of the protective layer, and it is more preferable that it is 12 or less, more preferably 6 or less, and particularly preferably 4 or less.

[0045] In the above formula (1) and formula (1'), the presence of the linking chain R suppresses steric repulsion between groups having a C=O bond (for example, a (meth)acryloyl group) located at the terminal side of the molecule, and from the viewpoint of preventing the detachment of the group having a C=O bond (for example, a (meth)acryloyl group), R each independently represents an alkylene group having 1 to 8 carbon atoms which may have a substituent, an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent, and -O-(C=O)-(CX2) p - (wherein p is an integer of 1 to 6, and X represents a hydrogen atom or a substituent). Among them, from the viewpoint of ease of synthesis, an oxyalkylene group having 1 to 8 carbon atoms, which may have a substituent, or -O-(C=O)-(CX2) p - (wherein p is an integer of 1 to 6) is preferred, and -O-(C=O)-(CX2) p - (wherein p is an integer of 1 to 6, and X represents a hydrogen atom or a substituent) is more preferable. Here, the number of carbon atoms means only the number of carbon atoms in the main chain of the alkylene group or the oxyalkylene group, not including the number of carbon atoms in the substituent if the alkylene group or the oxyalkylene group has a substituent, or means the number of carbon atoms in the main chain of the alkylene group or the oxyalkylene group if the alkylene group or the oxyalkylene group has no substituent.

[0046] In the present invention, the phrase "may have a substituent" means that the group can have a substituent, and includes both the case where the group has a substituent and the case where the group does not have a substituent.

[0047] The alkylene group having 1 to 8 carbon atoms and the oxyalkylene group having 1 to 8 carbon atoms may have a substituent, but preferably has no substituent. When the alkylene group has a substituent, examples of the substituent include a methyl group, an ethyl group, and a dimethyl group. Among these, a methyl group is preferred from the viewpoints of availability of raw materials and ease of synthesis.

[0048] Examples of the alkylene group having 1 to 8 carbon atoms include -CH2-, -CH2-CH2-, -CH(CH3)-CH2-, -CH2-CH(CH3)-, -CH2-CH2-CH2-, -CH2-CH2-CH2-CH2-, etc. Among these, -CH2- and -CH2-CH2- are preferred, and -CH2- is more preferred. Examples of the oxyalkylene group having 1 to 8 carbon atoms include -O-CH2-, -O-CH2-CH2-, -O-CH(CH3)-CH2-, -O-CH2-CH(CH3)-, -O-CH2-CH2-CH2-, -O-CH2-CH2-CH2-CH2-, etc. Among these, -O-CH2-CH2- and -O-CH(CH3)-CH2- are preferred, and -O-CH2-CH2- is more preferred.

[0049] When the linking chain R is an oxyalkylene group having 1 to 8 carbon atoms, the number of the oxyalkylene groups in one molecule of the compound a having the structure represented by formula (1') is preferably 2 or more, more preferably 4 or more, while it is preferably 12 or less, more preferably 10 or less, and even more preferably 6 or less. The linking chain R is -O-(C=O)-(CX2) p -, then p is an integer of 1 or more and 6 or less. Among these, p is more preferably an integer of 1 or more and 5 or less. The linking chain R is -O-(C=O)-(CX2) p When -, X represents a hydrogen atom or a substituent. Examples of the substituent include the same ones as those that may be possessed by the above-mentioned alkylene group having 1 to 8 carbon atoms and the oxyalkylene group having 1 to 8 carbon atoms. Among these, X is preferably a hydrogen atom.

[0050] In the above formula (1), T represents a bond to an arbitrary atom, such as carbon, hydrogen, nitrogen, or oxygen.

[0051] In the above formula (1), Q is preferably a hydroxy group or the following formula (3) from the viewpoint of having polarity and suppressing the formation of a mixed layer. Furthermore, Q in the above formula (1') is preferably a hydroxy group or the following formula (3') from the viewpoint of having polarity and suppressing the formation of a mixed layer.

[0052] Z in the above formula (1) and formula (1') 1 Each of Z in the above formula (1) and formula (1') independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and at least one of them is preferably an alkyl group having 1 to 4 carbon atoms. 1 More preferably, two or more of Z are alkyl groups having 1 to 4 carbon atoms, and even more preferably, three or more of Z are alkyl groups having 1 to 4 carbon atoms. 1 It is particularly preferable that Z is an alkyl group having 1 to 4 carbon atoms. 1 The alkyl group with carbon number 1 to 4 is more effective in preventing acidic gases such as ozone from 1 This sterically prevents the unreacted carbon-carbon double bond to which the carboxylate is bonded from approaching, resulting in good gas resistance. In addition, Z in formula (1) and formula (1') 1 When is an alkyl group having 1 to 4 carbon atoms, the number of carbon atoms in the alkyl group is preferably 1 to 3, more preferably 1 to 2, and even more preferably 1, i.e., a methyl group.

[0053] [Formula (2) and Formula (2')] In the above formula (2) and formula (2'), f, g, h, i, j, and k are each an integer of 0 or more and 10 or less. Among them, it is preferable that any of f, g, h, i, j, and k is an integer of 1 or more, while it is preferable that each of f, g, h, i, j, and k is an integer of 8 or less, more preferably an integer of 4 or less, and even more preferably an integer of 2 or less.

[0054] f+g+h+i+j+k means an equivalent amount of the linking chain R contained in the above formula (2) and the above formula (2'), and is preferably 1 or more from the viewpoint of suppressing steric repulsion between groups having a C=O bond (e.g., (meth)acryloyl groups) arranged on the terminal side of the molecule and preventing detachment of the group having a C=O bond (e.g., (meth)acryloyl groups), more preferably 2 or more, and particularly preferably 4 or more. On the other hand, if it is 20 or less, it is preferable from the viewpoint of the mechanical strength of the protective layer, and is more preferably 18 or less, still more preferably 12 or less, and particularly preferably 6 or less.

[0055] In the above formula (2) and the above formula (2'), R each independently represents an alkylene group having 1 to 8 carbon atoms which may have a substituent, an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent, and -O-(C=O)-(CX2), from the viewpoint of suppressing steric repulsion between groups having a C=O bond (for example, a (meth)acryloyl group) located at the terminal side of the molecule and preventing elimination of the group having a C=O bond (for example, a (meth)acryloyl group). p - (wherein p is an integer of 1 to 6, and X represents a hydrogen atom or a substituent). Among them, from the viewpoint of ease of synthesis, an oxyalkylene group having 1 to 8 carbon atoms, -O-(C=O)-(CX2) p - (wherein p is an integer of 1 to 6) is preferred, and -O-(C=O)-(CX2) p - (wherein p is an integer of 1 to 6, and X represents a hydrogen atom or a substituent) is more preferable. Here, the number of carbon atoms means only the number of carbon atoms in the main chain of the alkylene group or the oxyalkylene group, not including the number of carbon atoms in the substituent if the alkylene group or the oxyalkylene group has a substituent, or means the number of carbon atoms in the main chain of the alkylene group or the oxyalkylene group if the alkylene group or the oxyalkylene group has no substituent.

[0056] The alkylene group having 1 to 8 carbon atoms and the oxyalkylene group having 1 to 8 carbon atoms may have a substituent, but preferably has no substituent. When the alkylene group has a substituent, examples of the substituent include a methyl group, an ethyl group, and a dimethyl group. Among these, a methyl group is preferred from the viewpoints of availability of raw materials and ease of synthesis.

[0057] Examples of the alkylene group having 1 to 8 carbon atoms include -CH2-, -CH2-CH2-, -CH(CH3)-CH2-, -CH2-CH(CH3)-, -CH2-CH2-CH2-, -CH2-CH2-CH2-CH2-, etc. Among these, -CH2- and -CH2-CH2- are preferred, and -CH2- is more preferred. Examples of the oxyalkylene group having 1 to 8 carbon atoms include -O-CH2-, -O-CH2-CH2-, -O-CH(CH3)-CH2-, -O-CH2-CH(CH3)-, -O-CH2-CH2-CH2-, -O-CH2-CH2-CH2-CH2-, etc. Among these, -O-CH2-CH2- and -O-CH(CH3)-CH2- are preferred, and -O-CH2-CH2- is more preferred. When the linking chain R is an oxyalkylene group having 1 to 8 carbon atoms, the number of the oxyalkylene groups in one molecule of the compound b having the structure represented by formula (2') is preferably 2 or more, more preferably 4 or more, while it is preferably 12 or less, more preferably 10 or less, and more preferably 6 or less.

[0058] The linking chain R is -O-(C=O)-(CX2) p -, then p is an integer of 1 or more and 6 or less. Among these, p is more preferably an integer of 1 or more and 5 or less. The linking chain R is -O-(C=O)-(CX2) p When -, X represents a hydrogen atom or a substituent. Examples of the substituent include the same ones as those that may be possessed by the above-mentioned alkylene group having 1 to 8 carbon atoms and the oxyalkylene group having 1 to 8 carbon atoms. Among these, X is preferably a hydrogen atom.

[0059] In the above formula (2), T represents a bond to an arbitrary atom, such as carbon, hydrogen, nitrogen, or oxygen.

[0060] In the above formula (2), Q is preferably a hydroxy group or the following formula (3) from the viewpoint of having polarity and suppressing the formation of a mixed layer. Furthermore, Q in the above formula (2') is preferably a hydroxy group or the following formula (3') from the viewpoint of having polarity and suppressing the formation of a mixed layer.

[0061] Z in the above formula (2) and formula (2') 1 Each of Z in the above formula (2) and formula (2') independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and it is preferable that at least one of them is an alkyl group having 1 to 4 carbon atoms. 1 More preferably, two or more of Z are alkyl groups having 1 to 4 carbon atoms, and even more preferably, four or more of Z are alkyl groups having 1 to 4 carbon atoms. 1 It is particularly preferable that Z is an alkyl group having 1 to 4 carbon atoms. 1 The alkyl group with carbon number 1 to 4 is more effective in preventing acidic gases such as ozone from 1 This sterically prevents the unreacted carbon-carbon double bond to which the carboxylate is bonded from approaching, resulting in good gas resistance. In addition, Z in formula (2) and formula (2') 1 When is an alkyl group having 1 to 4 carbon atoms, the number of carbon atoms in the alkyl group is preferably 1 to 3, more preferably 1 to 2, and even more preferably 1, i.e., a methyl group.

[0062] R in at least one of the formulas (1), (2), (1') and (2') is an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent, or -O-(C=O)-(CX2) p - (wherein p is an integer of 1 to 6, and X represents a hydrogen atom or a substituent) is preferable.

[0063] [Formula (3)] TIFF2024168996000012.tif37170

[0064] In formula (3), Z 1 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; Z 2 represents a bond to R in formula (1) or (2). T represents a bond to any atom. Z in formula (3) 1 When is an alkyl group having 1 to 4 carbon atoms, the number of carbon atoms in the alkyl group is preferably 1 to 3, more preferably 1 to 2, and even more preferably 1, i.e., a methyl group.

[0065] [Formula (3')] TIFF2024168996000013.tif30170

[0066] In formula (3'), Z 1 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; Z 2 represents a bond to R in formula (1') or formula (2'). Z in formula (3') 1 When is an alkyl group having 1 to 4 carbon atoms, the number of carbon atoms in the alkyl group is preferably 1 to 3, more preferably 1 to 2, and even more preferably 1, i.e., a methyl group.

[0067] Whether the protective layer of the electrophotographic photoreceptor is a layer containing the polymer having the linking chain R and the structures represented by the formulas (1) and (2) can be confirmed, for example, by the following method. The protective layer portion is isolated from the electrophotographic photoreceptor and subjected to pyrolysis GC / MS analysis to analyze the structure contained in the protective layer, and the linking chain R, the structure represented by the following formula (5), and the structure represented by the following formula (6) can be detected. The structure represented by the following formula (5) and the structure represented by the following formula (6) correspond to partial structures of the structure represented by the above formula (1) and the structure represented by the above formula (2).

[0068] [Formula (5)] TIFF2024168996000014.tif35170

[0069] In formula (5), Z 3 represents a bond to any atom.

[0070] [Formula (6)] TIFF2024168996000015.tif29170

[0071] In formula (6), Z 4 represents an alkyl group having 1 to 4 carbon atoms. T represents a bond to any atom.

[0072] [Equation (5) and Equation (6)] In the above formula (5), Z 3 represents a bond to an arbitrary atom, such as carbon, hydrogen, nitrogen, or oxygen. In the above formula (6), Z 4 represents an alkyl group having 1 to 4 carbon atoms. T represents a bond to an arbitrary atom. Such an arbitrary atom may be, for example, carbon, hydrogen, nitrogen, or oxygen. Z in formula (6) 4 When is an alkyl group having 1 to 4 carbon atoms, the number of carbon atoms in the alkyl group is preferably 1 to 3, more preferably 1 to 2, and even more preferably 1, i.e., a methyl group.

[0073] In the case where the compound has a structure represented by the formula (5), examples of the compound that can be detected by pyrolysis GC / MS analysis include pentaerythritol, methylpentaerythritol, dimethylpentaerythritol, trimethylpentaerythritol, tetramethylpentaerythritol, ethylpentaerythritol, diethylpentaerythritol, triethylpentaerythritol, tetraethylpentaerythritol, and dipentaerythritol. In addition, when the protective layer has a structure represented by formula (6), examples of compounds contained in the protective layer before curing (before polymerization) include acrylic acid, methacrylic acid, 2-ethylprop-2-enoic acid, 2-propylprop-2-enoic acid, 2-butylprop-2-enoic acid, methyl acrylate, methyl methacrylate, methyl 2-ethylprop-2-enoate, methyl 2-propylprop-2-enoate, methyl 2-butylprop-2-enoate, ethyl acrylate, ethyl methacrylate, ethyl 2-ethylprop-2-enoate, ethyl 2-propylprop-2-enoate, and ethyl 2-butylprop-2-enoate. The compounds contained in the protective layer before curing (before polymerization) may remain as unreacted compounds in the protective layer after curing. In such a case, the unreacted compounds are detected as a result of performing pyrolysis GC / MS analysis on the protective layer after curing, and it can be inferred that the protective layer is a layer containing a polymer having the structure represented by the formula (6).

[0074] [Molecular weight] From the viewpoints of solubility in a coating solution for forming a protective layer and mechanical strength of the protective layer, the molecular weight of the compound a having the structure represented by the above formula (1') is preferably 300 or more, more preferably 400 or more, and even more preferably 450 or more. On the other hand, it is preferably 1200 or less, more preferably 1000 or less, and even more preferably 900 or less. From the viewpoints of solubility in a coating solution for forming a protective layer and mechanical strength of the protective layer, the molecular weight of the compound b having the structure represented by the above formula (2') is preferably 500 or more, more preferably 600 or more, and even more preferably 700 or more. On the other hand, it is preferably 1400 or less, more preferably 1200 or less, and even more preferably 1000 or less.

[0075] [Functional group equivalent] With respect to the compound a represented by the formula (1') or the compound b represented by the formula (2'), it is preferable that the molecular weight X of the compound a or the compound b and the number Y of the acryloyl group and the methacryloyl group in one molecule satisfy the following formula (4). 120≦X / Y≦400 (4)

[0076] If the number of polar (meth)acryloyl groups or hydroxyl groups is large, the effect of suppressing the mixing by the polar groups described above is enhanced, and the formation of the mixed layer can be further suppressed. That is, by having a sufficient number of polar groups (acryloyl groups or methacryloyl groups) relative to the molecular weight, the formation of the mixed layer can be further suppressed. In addition, sufficient mechanical strength can be obtained to exhibit abrasion resistance. From this viewpoint, in the compound a or b represented by either of the formula (1') or (2'), the ratio (X / Y) of the molecular weight X of the compound a or b to the number Y of acryloyl groups and methacryloyl groups in one molecule, i.e., the functional group equivalent, is preferably 400 or less, more preferably 300 or less, even more preferably 200 or less, and even more preferably 180 or less. On the other hand, if the ratio (X / Y), i.e., the functional group equivalent, is large, it is believed that residual stress is small and cracks are less likely to occur, so the ratio (X / Y), i.e., the functional group equivalent, is preferably 120 or more, more preferably 130 or more, even more preferably 140 or more, and even more preferably 150 or more. The number Y of acryloyl groups and methacryloyl groups in one molecule is preferably 2 or more, more preferably 3 or more, and more preferably 4 or more. On the other hand, it is preferably 12 or less, more preferably 10 or less, even more preferably 8 or less, and particularly preferably 6 or less.

[0077] (metal oxide particles) The protective layer preferably contains metal oxide particles from the viewpoints of imparting charge transporting ability and improving mechanical strength.

[0078] As the metal oxide particles, metal oxide particles that can be used for electrophotographic photoreceptors can be used. Examples of the metal oxide particles include metal oxide particles containing one type of metal element such as titanium oxide, tin oxide, aluminum oxide, silicon oxide, zirconium oxide, zinc oxide, and iron oxide, and metal oxide particles containing multiple metal elements such as calcium titanate, strontium titanate, and barium titanate. Only one type of metal oxide particle may be used, or multiple types of particles may be mixed and used. Among these metal oxide particles, titanium oxide, tin oxide, aluminum oxide, silicon oxide, or zinc oxide is preferred, and titanium oxide and tin oxide are more preferred. Titanium oxide is particularly preferred.

[0079] The crystalline form of the titanium oxide particles may be any of rutile, anatase, brookite, and amorphous. In addition, the titanium oxide particles may have a plurality of different crystalline forms.

[0080] The surfaces of the metal oxide particles may be subjected to various surface treatments. For example, they may be treated with inorganic substances such as tin oxide, aluminum oxide, antimony oxide, zirconium oxide, silicon oxide, etc., or with organic substances such as stearic acid, polyols, and organosilicon compounds, etc. In particular, when titanium oxide particles are used, it is preferable that they are surface-treated with an organosilicon compound. Examples of the organosilicon compound include silicone oils such as dimethylpolysiloxane, organosilanes such as methyldimethoxysilane, silazanes such as hexamethyldisilazane, and silane coupling agents such as 3-methacryloyloxypropyltrimethoxysilane, 3-acryloyloxypropyltrimethoxysilane, vinyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, etc. In particular, from the viewpoint of improving the mechanical strength of the protective layer, 3-methacryloyloxypropyltrimethoxysilane, 3-acryloyloxypropyltrimethoxysilane, and vinyltrimethoxysilane, which have a chain polymerizable functional group, are preferred. The outermost surface of these surface-treated particles may be treated with a treating agent such as aluminum oxide, silicon oxide or zirconium oxide before being treated with such a treating agent.

[0081] The particle size of the metal oxide particles is preferably an average primary particle size of 500 nm or less, more preferably 100 nm or less, and even more preferably 50 nm or less, and more preferably 1 nm or more, and even more preferably 5 nm or more. This average primary particle size can be determined from the arithmetic mean value of particle sizes directly observed using a transmission electron microscope (hereinafter also referred to as TEM).

[0082] From the viewpoint of electrical properties, the content of the metal oxide particles in the protective layer is preferably 20 parts by mass or more, more preferably 60 parts by mass or more, and even more preferably 80 parts by mass or more, based on 100 parts by mass of the polymer contained in the protective layer, while from the viewpoint of maintaining the surface charge, the content is preferably 200 parts by mass or less, more preferably 160 parts by mass or less, and even more preferably 120 parts by mass or less.

[0083] (Other materials) In addition to the above materials, the protective layer may contain other materials as necessary. For example, the other materials may contain a "charge transport material" from the viewpoint of enhancing the charge transport ability, or a "polymerization initiator" to promote the polymerization reaction. Furthermore, as necessary, the protective layer may contain, for example, a stabilizer (heat stabilizer, ultraviolet absorber, light stabilizer, antioxidant, etc.), a dispersant, an antistatic agent, a colorant, a lubricant, etc. These may be used alone or in any ratio and combination of two or more kinds.

[0084] [Charge transport material] The charge transport material contained in the protective layer may be the same as the charge transport material used in the photosensitive layer described below.

[0085] From the viewpoint of improving the Martens hardness of the surface of the photoreceptor, the protective layer may contain a structure obtained by polymerizing a charge transport material having a chain-polymerizable functional group. Examples of the chain-polymerizable functional group of the charge transport material having the chain-polymerizable functional group include an acryloyl group, a methacryloyl group, a vinyl group, and an epoxy group. Among these, from the viewpoint of curability, an acryloyl group or a methacryloyl group is preferred. As the structure of the charge transport material portion of the charge transport material having the chain-polymerizable functional group, a carbazole derivative, an arylamine derivative, a stilbene derivative, a butadiene derivative, an enamine derivative, and a combination of a plurality of these compounds are preferred.

[0086] The content of the charge transport material in the protective layer of the electrophotographic photoreceptor is not particularly limited. From the viewpoint of electrical properties, the content is preferably 10 parts by mass or more, more preferably 30 parts by mass or more, and even more preferably 50 parts by mass or more, per 100 parts by mass of the polymer having the structure represented by the formula (1) or (2), or the polymer having the structure represented by the formula (1') or (2'), or the group represented by R', the structure represented by the formula (5), and the structure represented by the formula (6). Also, from the viewpoint of maintaining good surface resistance, the content is more preferably 300 parts by mass or less, more preferably 200 parts by mass or less, and even more preferably 150 parts by mass or less.

[0087] [Polymerization initiator] The polymerization initiator includes a thermal polymerization initiator, a photopolymerization initiator, and the like.

[0088] Examples of the thermal polymerization initiator include peroxide compounds such as 2,5-dimethylhexane-2,5-dihydroperoxide, and azo compounds such as 2,2'-azobis(isobutyronitrile).

[0089] Photopolymerization initiators can be classified into direct cleavage type and hydrogen abstraction type depending on the radical generation mechanism.

[0090] Examples of the direct cleavage type photopolymerization initiator include acetophenone or ketal compounds such as acetophenone, 2-benzoyl-2-propanol, 1-benzoylcyclohexanol, 2,2-diethoxyacetophenone, benzyl dimethyl ketal, and 2-methyl-4'-(methylthio)-2-morpholinopropiophenone; benzoin ether compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isobutyl ether, benzoin isopropyl ether, and O-tosylbenzoin; and acylphosphine oxide compounds such as diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and lithium phenyl(2,4,6-trimethylbenzoyl)phosphonate.

[0091] Examples of hydrogen abstraction type photopolymerization initiators include benzophenone-based compounds such as benzophenone, 4-benzoylbenzoic acid, 2-benzoylbenzoic acid, methyl 2-benzoylbenzoate, methyl benzoylformate, benzyl, p-anisyl, 2-benzoylnaphthalene, 4,4'-bis(dimethylamino)benzophenone, 4,4'-dichlorobenzophenone, and 1,4-dibenzoylbenzene, and anthraquinone-based or thioxanthone-based compounds such as 2-ethylanthraquinone, 2-isopropylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-dichlorothioxanthone. Other examples of photopolymerization initiators include camphorquinone, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, acridine-based compounds, triazine-based compounds, and imidazole-based compounds.

[0092] In order to efficiently absorb light energy and generate radicals, the photopolymerization initiator preferably has an absorption wavelength in the wavelength region of the light source used for light irradiation. From the viewpoint of preventing a decrease in the radical generation efficiency, it is preferable to contain an acylphosphine oxide compound, which has an absorption wavelength on the relatively long wavelength side among photopolymerization initiators. In this case, from the viewpoint of supplementing the curability of the surface of the protective layer, it is more preferable to use an acylphosphine oxide compound and a hydrogen abstraction initiator in combination. The content ratio of the hydrogen abstraction initiator to the acylphosphine oxide compound is not particularly limited. For example, from the viewpoint of supplementing the surface curability, it is preferable to contain 0.1 parts by mass or more of the hydrogen abstraction initiator to 1 part by mass of the acylphosphine oxide compound, and from the viewpoint of maintaining the internal curability, it is preferable to contain 5 parts by mass or less of the hydrogen abstraction initiator.

[0093] In addition, a substance having a photopolymerization promoting effect can be used alone or in combination with the above-mentioned photopolymerization initiator. Examples of substances having a photopolymerization promoting effect include triethanolamine, methyldiethanolamine, ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, (2-dimethylamino)ethyl benzoate, and 4,4'-dimethylaminobenzophenone.

[0094] The polymerization initiator may be used alone or in combination of two or more. The content of the polymerization initiator is preferably 0.5 to 40 parts by mass, more preferably 1 part by mass or more or 20 parts by mass or less, based on 100 parts by mass of the total content having radical polymerizability.

[0095] (Method of forming the protective layer) Next, the method for forming the protective layer will be described. The method for forming the protective layer is not particularly limited. For example, the protective layer can be formed by applying a coating liquid (referred to as the "coating liquid for forming the protective layer") in which the compound a having the structure represented by the formula (1') or the compound b having the structure represented by the formula (2'), the metal oxide particles as required, the polymerization initiator as required, the charge transport material as required, and other materials as required are dissolved in a solvent or dispersed in a dispersion medium on the photosensitive layer and curing the coating liquid.

[0096] [Solvent used in coating solution for forming protective layer] Examples of organic solvents used in the present protective layer forming coating solution include alcohols such as methanol, ethanol, propanol, and 2-methoxyethanol; ethers such as tetrahydrofuran; esters such as methyl formate; ketones such as acetone; aromatic hydrocarbons such as benzene and toluene; chlorinated hydrocarbons such as dichloromethane and chloroform; nitrogen-containing compounds such as n-butylamine; and aprotic polar solvents such as acetonitrile. Any combination and any ratio of mixed solvents from these can be used. In addition, even if an organic solvent does not dissolve the material for the protective layer of the present electrophotographic photoreceptor alone, it can be used if it can be dissolved by mixing it with the above organic solvent. In general, the use of a mixed solvent can reduce coating unevenness. When using a dip coating method in the coating method described below, it is preferable to select a solvent that does not dissolve the lower layer. From this viewpoint, it is preferable to contain alcohols that have low solubility in polycarbonate and polyarylate, which are suitable for use in the photosensitive layer.

[0097] The ratio of the organic solvent to the solid content used in the coating solution for forming a protective layer varies depending on the coating method of the coating solution for forming a protective layer, and may be appropriately changed so as to form a uniform coating film in the coating method to be used.

[0098] [Application method] The method of applying the coating solution for forming the present protective layer is not particularly limited, and examples thereof include spray coating, spiral coating, ring coating, and dip coating.

[0099] After forming the coating film by the above coating method, the coating film is dried. In this case, the temperature and time of drying are not important as long as necessary and sufficient drying is obtained. However, if the protective layer is coated only by air drying after the photosensitive layer coating, it is preferable to perform sufficient drying by the method described later in the photosensitive layer forming method.

[0100] [How to harden this protective layer] The protective layer can be formed by applying the coating solution for forming the protective layer and then curing the coating solution by applying external energy thereto. The external energy used in this case can include heat, light, and radiation.

[0101] Examples of methods for applying heat energy include heating methods using air, gases such as nitrogen, steam, various heat media, infrared rays, and electromagnetic waves. The heating can be performed from the coated surface side or the support side. The heating temperature is preferably 100°C or higher and 170°C or lower.

[0102] As the light energy, UV irradiation light sources that mainly emit light in the ultraviolet (UV) range, such as high-pressure mercury lamps, metal halide lamps, electrodeless lamp bulbs, light-emitting diodes, etc. It is also possible to select a visible light source according to the absorption wavelength of the chain polymerizable compound and photopolymerization initiator. The light irradiation dose was set to 10 J / cm from the viewpoint of curing. 2 More than 30 J / cm is preferable. 2 More preferably, 100 J / cm 2 More preferably, the electric field strength is 500 J / cm or more. 2 Less than 300 J / cm is preferable. 2 Less than 200 J / cm is more preferable. 2 The following are particularly preferred: On the other hand, examples of radiation energy include those using electron beams (EB).

[0103] Among these energies, light energy is preferred from the viewpoints of ease of reaction rate control, simplicity of the device, and long pod life.

[0104] After the protective layer is cured, a heating step may be added from the viewpoints of relieving residual stress, relieving residual radicals, and improving electrical properties. The heating temperature is preferably 60° C. or higher, more preferably 100° C. or higher, and is preferably 200° C. or lower, more preferably 150° C. or lower.

[0105] (layer thickness) From the viewpoint of abrasion resistance, the thickness of the protective layer is preferably 0.5 μm or more, more preferably 1 μm or more, and from the viewpoint of electrical properties, the thickness is preferably 5 μm or less, more preferably 3 μm or less. From the same viewpoint, the thickness of the protective layer is preferably 1 / 50 or more of the thickness of the photosensitive layer, more preferably 1 / 40 or more, and even more preferably 1 / 30 or more, while it is preferably 1 / 5 or less, more preferably 1 / 10 or less, and even more preferably 1 / 20 or less.

[0106] <Main photosensitive layer> The photosensitive layer in the present electrophotographic photoreceptor (also referred to as the "present photosensitive layer") may be any layer containing at least a charge generating material (CGM) and a charge transport material.

[0107] The photosensitive layer may be a single-layer type photosensitive layer containing both a charge generating material and a charge transporting material in the same layer, or may be a laminated type photosensitive layer separated into a charge generating layer and a charge transporting layer. Regardless of whether the photosensitive layer is a single-layer type or a multi-layer type, when a mixed layer is formed between the protective layer and the photosensitive layer, the concentration of the charge transport material in the mixed layer is lower than that of the photosensitive layer, and therefore the mechanism of the charge transport ability being reduced occurs in the same way. Therefore, the effect of the present invention can be enjoyed with either a single-layer type photosensitive layer or a multi-layer type photosensitive layer. However, in general, a single-layer type photosensitive layer has a hole transport material, an electron transport material, and a charge generating material in the same layer in addition to a binder resin, so that the proportion of low molecular weight components is high, and the glass transition point of the photosensitive layer is lower than that of a multi-layer type photosensitive layer. Therefore, since the photosensitive layer is easily softened by the heat generated during the heat drying and curing during the formation of the protective layer, it is considered that the single-layer type photosensitive layer is easier to form a mixed layer. From this viewpoint, it is considered that the effect of the present invention can be enjoyed more with a single-layer type photosensitive layer than with a multi-layer type photosensitive layer.

[0108] <Single-layer type photosensitive layer> When the photosensitive layer is a single-layer type photosensitive layer, it is preferable that the layer contains at least a charge generating material (CGM), a hole transporting material (HTM), an electron transporting material (ETM), and a binder resin.

[0109] (Charge generating material) The charge generating material used in the photosensitive layer may be, for example, various photoconductive materials such as inorganic photoconductive materials and organic pigments, etc. Among these, organic pigments are particularly preferred, and phthalocyanine pigments and azo pigments are more preferred.

[0110] In particular, when a phthalocyanine pigment is used as a charge generating material, specifically, metal-free phthalocyanine, phthalocyanines coordinated with metals such as copper, indium, gallium, tin, titanium, zinc, vanadium, silicon, germanium, or their oxides, halides, etc. are used. Examples of ligands to trivalent or higher metal atoms include oxygen atoms, chlorine atoms, hydroxyl groups, alkoxyl groups, etc. Among them, particularly highly sensitive X-type and τ-type metal-free phthalocyanine, A-type, B-type, D-type titanyl phthalocyanine, vanadyl phthalocyanine, chloroindium phthalocyanine, chlorogallium phthalocyanine, hydroxygallium phthalocyanine, etc. are suitable.

[0111] When an azo pigment is used, various known bisazo pigments and trisazo pigments are preferably used.

[0112] The charge generating material may be used alone or in any combination and ratio of two or more. When two or more charge generating materials are used in combination, the charge generating materials may be mixed after the charge generating materials are mixed, or may be mixed during the production and processing steps of the charge generating materials, such as synthesis, pigmentation, and crystallization.

[0113] From the viewpoint of electrical properties, it is desirable that the particle diameter of the charge generating material is small. Specifically, the particle diameter of the charge generating material is preferably 1 μm or less, more preferably 0.5 μm or less. The lower limit is 0.01 μm or more. Here, the particle diameter of the charge generating material means the particle diameter in the state in which it is contained in the photosensitive layer.

[0114] The amount of the charge generating material in the single-layer photosensitive layer is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, from the viewpoint of sensitivity, and is preferably 50% by mass or less, more preferably 20% by mass or less, from the viewpoint of sensitivity and chargeability.

[0115] (charge transport material) Charge transport materials are classified into hole transport materials having mainly hole transporting ability and electron transport materials having mainly electron transporting ability. However, when the present photosensitive layer is a single-layer type photosensitive layer, it is preferable that at least a hole transport material and an electron transport material are contained in the same layer.

[0116] [Hole transport material] The hole transport material (HTM) can be selected from known materials and can be used, for example, electron donating materials such as heterocyclic compounds such as carbazole derivatives, indole derivatives, imidazole derivatives, oxazole derivatives, pyrazole derivatives, thiadiazole derivatives, and benzofuran derivatives, aniline derivatives, hydrazone derivatives, arylamine derivatives, stilbene derivatives, butadiene derivatives, and enamine derivatives, as well as compounds in which a plurality of these compounds are bonded, and polymers having groups made of these compounds in the main chain or side chain.

[0117] Among these, carbazole derivatives, arylamine derivatives, stilbene derivatives, butadiene derivatives and enamine derivatives, as well as combinations of a plurality of these compounds, are preferred, with arylamine derivatives and enamine derivatives being more preferred.

[0118] From the viewpoint of electrical properties, the molecular weight of the hole transport substance is preferably 600 or more, more preferably 650 or more, even more preferably 700 or more, and particularly preferably 740 or more. On the other hand, from the viewpoint of ease of synthesis and stability of the compound, the molecular weight is preferably 1200 or less, more preferably 1000 or less, and even more preferably 900 or less.

[0119] The hole transport material may be used alone or in any combination of two or more kinds in any ratio.

[0120] Preferred examples of the structure of the hole transport material are shown below.

[0121] TIFF2024168996000016.tif70170

[0122] TIFF2024168996000017.tif76170

[0123] TIFF2024168996000018.tif107170

[0124] Among the above-mentioned hole transport materials, from the viewpoint of electrical properties, HTM31, HTM32, HTM33, HTM34, HTM35, HTM39, HTM40, HTM41, HTM42, HTM43, and HTM48 are preferred, and HTM39, HTM40, HTM41, HTM42, HTM43, and HTM48 are more preferred.

[0125] [Electron transport material] The electron transport material (ETM) can be selected from known materials. For example, there can be mentioned electron-withdrawing substances such as aromatic nitro compounds such as 2,4,7-trinitrofluorenone, cyano compounds such as tetracyanoquinodimethane, quinone compounds such as diphenoquinone, known cyclic ketone compounds, and perylene pigments (perylene derivatives). Among these, from the viewpoint of electrical properties, quinone compounds and perylene pigments (perylene derivatives) are preferred, and quinone compounds are more preferred. Among the quinone compounds, diphenoquinone or dinaphthylquinone is preferable from the viewpoint of electrical properties, and among them, dinaphthylquinone is more preferable.

[0126] From the viewpoint of electrical properties, the molecular weight of the electron transporting substance is preferably 400 or more, more preferably 410 or more, and even more preferably 420 or more, while it is preferably 1000 or less, more preferably 800 or less, and even more preferably 600 or less.

[0127] The electron transport material may be used alone or in any combination of two or more kinds in any ratio.

[0128] Preferred examples of the structure of the electron transport material are shown below.

[0129] TIFF2024168996000019.tif40170

[0130] Among the above electron transport materials, ET-2 and ET-5 are preferred from the viewpoint of electrical properties, with ET-2 being more preferred.

[0131] [Content of hole transport material and electron transport material] The ratio of the mass content of the electron transport material to the mass content of the hole transport material in the single-layer photosensitive layer is preferably 0.3 or more from the viewpoint of electron transportability, and more preferably 0.4 or more from the viewpoint of electrical properties. On the other hand, from the viewpoint of hole transportability, it is preferably 1.0 or less, and more preferably 0.9 or less from the viewpoint of suppressing precipitation of the electron transport material, and more preferably 0.8 or less from the viewpoint of adhesion.

[0132] From the viewpoint of hole transportability, the content of the hole transport material in the electrophotographic photoreceptor is preferably 50 parts by mass or more, more preferably 80 parts by mass or more, and even more preferably 90 parts by mass or more, relative to 100 parts by mass of the binder resin described below. On the other hand, the upper limit is more preferably 200 parts by mass or less, and even more preferably 150 parts by mass or less, from the viewpoint of suppressing precipitation.

[0133] (binder resin) Next, the binder resin used in the photosensitive layer will be described. Examples of the binder resin used in the photosensitive layer include vinyl polymers or copolymers thereof such as polymethyl methacrylate, polystyrene, and polyvinyl chloride; vinyl alcohol resins; polyvinyl butyral resins; polyvinyl formal resins; partially modified polyvinyl acetal resins; polyarylate resins; polyamide resins; polyurethane resins; polycarbonate resins; polyester resins; polyester carbonate resins; polyimide resins; phenoxy resins; epoxy resins; silicone resins; and partially crosslinked cured products thereof. The above resins may be modified with silicon reagents or the like. These may be used alone or in any ratio and combination of two or more.

[0134] The binder resin used in the present photosensitive layer preferably contains one or more types of polymers obtained by interfacial polymerization.

[0135] The binder resin obtained by the above interfacial polymerization is preferably a polycarbonate resin or a polyester resin, more preferably a polycarbonate resin or a polyarylate resin, and even more preferably a polycarbonate resin. In addition, a polymer made from an aromatic diol is particularly preferable.

[0136] (Other substances) In addition to the above materials, the photosensitive layer may contain additives such as well-known antioxidants, plasticizers, ultraviolet absorbers, electron-withdrawing compounds, leveling agents, and visible light shielding agents in order to improve film-forming properties, flexibility, coating properties, contamination resistance, gas resistance, and light resistance. The photosensitive layer may also contain various additives such as sensitizers, dyes, pigments (excluding the charge generating materials, hole transport materials, and electron transport materials described above), and surfactants, as necessary. Examples of surfactants include silicone oils and fluorine-based compounds. In the present invention, these may be used alone or in any ratio and combination of two or more of them.

[0137] In order to reduce the frictional resistance of the surface of the photosensitive layer, the photosensitive layer may contain a fluorine-based resin, a silicone resin, or the like, and may contain particles made of these resins or particles of an inorganic compound such as aluminum oxide.

[0138] (layer thickness) When the photosensitive layer is a single-layer type photosensitive layer, the thickness of the photosensitive layer is preferably 20 μm or more, more preferably 25 μm or more, from the viewpoint of dielectric breakdown resistance, and is preferably 50 μm or less, more preferably 40 μm or less, from the viewpoint of electrical properties.

[0139] <Laminated photosensitive layer> When the electrophotographic photoreceptor has a laminated photosensitive layer, for example, a charge transport layer (CTL) containing an electron transport material (ETM) and a hole transport material (HTM) is laminated on a charge generation layer (CGL) containing a charge generation material (CGM). In this case, it is possible to provide layers other than the charge generation layer (CGL) and the charge transport layer (CTL).

[0140] <Charge Generation Layer (CGL)> The charge generating layer usually contains a charge generating material (CGM) and a binder resin. The charge generating material (CGM) and the binder resin are the same as those described in the single-layer type photosensitive layer.

[0141] (Other Ingredients) In addition to the charge generating material and the binder resin, the charge generating layer may contain other components as necessary. For example, known additives such as antioxidants, plasticizers, ultraviolet absorbers, electron-withdrawing compounds, leveling agents, visible light shielding agents, and fillers may be contained in order to improve film-forming properties, flexibility, coating properties, stain resistance, gas resistance, light resistance, etc.

[0142] (composition ratio) In the charge generation layer, if the ratio of the charge generation substance is too high, the stability of the coating liquid may decrease due to aggregation of the charge generation substance, etc., while if the ratio of the charge generation substance is too low, it may result in a decrease in sensitivity as a photoreceptor. Therefore, the compounding ratio (mass) of the binder resin to the charge generation substance is preferably 10 parts by mass or more of the charge generation substance per 100 parts by mass of the binder resin, and more preferably 30 parts by mass or more, while it is preferably 1000 parts by mass or less, and more preferably 500 parts by mass or less, and from the viewpoint of film strength, it is more preferably 300 parts by mass or less, and even more preferably 200 parts by mass or less.

[0143] (layer thickness) The thickness of the charge generating layer is preferably 0.1 μm or more, more preferably 0.15 μm or more, and is preferably 10 μm or less, more preferably 6 μm or less.

[0144] <Charge transport layer (CTL)> The charge transport layer (CTL) usually contains a hole transport material (HTM) and a binder resin, and may further contain an electron transport material (ETM). The electron transport material (ETM), the hole transport material (HTM) and the binder resin are the same as those explained in the single-layer type photosensitive layer.

[0145] In the charge transport layer (CTL), the mixing ratio of the binder resin and the hole transport material (HTM) is preferably 20 parts by mass or more of the hole transport material (HTM) per 100 parts by mass of the binder resin, more preferably 30 parts by mass or more from the viewpoint of reducing the residual potential, and even more preferably 40 parts by mass or more from the viewpoint of stability and charge mobility during repeated use. On the other hand, from the viewpoint of the thermal stability of the photosensitive layer, it is preferable to mix 200 parts by mass or less of the hole transport material (HTM) per 100 parts by mass of the binder resin, more preferably 150 parts by mass or less from the viewpoint of compatibility between the hole transport material (HTM) and the binder resin, and particularly preferably 120 parts by mass or less from the viewpoint of the glass transition temperature.

[0146] (Other Ingredients) The charge transport layer may contain other components as necessary in addition to the electron transport material (ETM), hole transport material (HTM) and binder resin. For example, known additives such as antioxidants, plasticizers, ultraviolet absorbers, electron-withdrawing compounds, leveling agents, visible light shielding agents and fillers may be contained for the purpose of improving film-forming properties, flexibility, coatability, stain resistance, gas resistance, light resistance, etc.

[0147] (layer thickness) The thickness of the charge transport layer is not particularly limited, but from the viewpoints of electrical characteristics, image stability, and high resolution, it is preferably 5 μm or more and 50 μm or less, more preferably 10 μm or more or 35 μm or less, and even more preferably 15 μm or more or 25 μm or less.

[0148] <Method of forming photosensitive layer> In either the laminated type or the single layer type, the above layers can be formed as follows. The substance to be contained is dissolved or dispersed in a solvent to obtain a coating solution, which is then applied to a conductive support by a known method such as dip coating, spray coating, nozzle coating, bar coating, roll coating, or blade coating, and the steps of coating and drying are repeated in sequence to form each layer. However, the method is not limited to this.

[0149] The solvent or dispersion medium used to prepare the coating liquid is not particularly limited. Specific examples include alcohols such as methanol, ethanol, propanol, and 2-methoxyethanol, ethers such as tetrahydrofuran, 1,4-dioxane, and dimethoxyethane, aromatic hydrocarbons such as benzene, toluene, and xylene, and chlorinated hydrocarbons such as dichloromethane, chloroform, 1,2-dichloroethane, 1,1,2-trichloroethane, 1,1,1-trichloroethane, tetrachloroethane, 1,2-dichloropropane, and trichloroethylene. These may be used alone or in any combination of two or more of them.

[0150] The amount of the solvent or dispersion medium used is not particularly limited. Taking into consideration the purpose of each layer and the properties of the selected solvent and dispersion medium, it is preferable to appropriately adjust the solid content concentration, viscosity, and other physical properties of the coating liquid so that they fall within the desired range. The coating film is preferably dried to the touch at room temperature, and then heated and dried for 1 minute to 2 hours at a temperature in the range of 30° C. to 200° C., either stationary or with a fan. The heating temperature may be constant, or the temperature may be changed during drying.

[0151] <Conductive support> The conductive support of the present electrophotographic photoreceptor (also referred to as the "present conductive support") is not particularly limited as long as it supports a layer formed thereon and exhibits electrical conductivity. Examples of the conductive support that can be used include metal materials such as aluminum, aluminum alloys, stainless steel, copper, and nickel; resin materials that have been made conductive by the coexistence of conductive powders such as metal, carbon, and tin oxide; and resins, glass, and paper with conductive materials such as aluminum, nickel, and ITO (indium oxide tin oxide) vapor-deposited or applied to their surfaces. The conductive support may be in the form of a drum, cylinder, sheet, belt, or the like. The conductive support may be a conductive support made of a metal material on which a conductive material having an appropriate resistance value is applied in order to control the conductivity and surface properties, etc., or to cover defects.

[0152] When a metal material such as an aluminum alloy is used as the conductive support, the metal material may be provided with an anodized coating before use.

[0153] The average thickness of the anodic oxide coating is preferably 20 μm or less, and more preferably 7 μm or less.

[0154] When forming an anodized coating on a metal material, it is preferable to carry out a sealing treatment. The sealing treatment can be carried out by a known method.

[0155] The surface of the conductive support may be smooth, or may be roughened by using a special cutting method, by polishing, or by mixing particles of an appropriate particle size into the material constituting the support. In order to improve adhesion and blocking properties, an undercoat layer, which will be described below, may be provided between the conductive support and the photosensitive layer.

[0156] <Main undercoat layer> The present electrophotographic photoreceptor may have an undercoat layer (also referred to as "the present undercoat layer") between the present photosensitive layer and the present conductive support.

[0157] The undercoat layer may be made of, for example, a resin or a resin in which organic pigments or particles of metal oxides are dispersed. Examples of organic pigments used in the undercoat layer include phthalocyanine pigments, azo pigments, perylene pigments, etc. Among them, phthalocyanine pigments and azo pigments, specifically, the phthalocyanine pigments and azo pigments used as the charge generating material described above can be mentioned.

[0158] Examples of metal oxide particles used in the present undercoat layer include metal oxide particles containing one type of metal element, such as titanium oxide, aluminum oxide, silicon oxide, zirconium oxide, zinc oxide, iron oxide, etc., and metal oxide particles containing multiple metal elements, such as calcium titanate, strontium titanate, barium titanate, etc. In the undercoat layer, only one type of particle as above may be used, or multiple types of particles may be mixed in any ratio and combination.

[0159] Among the above-mentioned metal oxide particles, titanium oxide and aluminum oxide are preferred, and titanium oxide is particularly preferred. The titanium oxide particles may have their surfaces treated with any inorganic or organic material. The crystal type of the titanium oxide particles may be any of rutile, anatase, brookite, and amorphous. The titanium oxide particles may also include particles in a plurality of crystal states.

[0160] The particle size of the metal oxide particles used in the present undercoat layer is not particularly limited. In terms of the characteristics of the undercoat layer and the stability of the solution for forming the undercoat layer, the average primary particle size is preferably 10 nm or more, and 100 nm or less, more preferably 50 nm or less.

[0161] The binder resin used in the present undercoat layer may be selected from, for example, polyvinyl acetal resins such as polyvinyl butyral resins, polyvinyl formal resins, and partially acetalized polyvinyl butyral resins in which a part of butyral is modified with formal or acetal; insulating resins such as polyarylate resins, polycarbonate resins, polyester resins, phenoxy resins, acrylic resins, methacrylic resins, polyamide resins, polyurethane resins, epoxy resins, silicone resins, polyvinyl alcohol resins, styrene-alkyd resins, silicone-alkyd resins, and phenol-formaldehyde resins. However, the binder resins are not limited to these polymers. These binder resins may be used alone or in a mixture of two or more, or may be used in a cured form together with a curing agent. Among these, polyvinyl acetal resins, alcohol-soluble copolymerized polyamides, modified polyamides, etc. are preferred because they exhibit good dispersibility and coatability, and among these, alcohol-soluble copolymerized polyamides are particularly preferred.

[0162] The mixing ratio of the particles to the binder resin can be selected arbitrarily, but it is preferable to use the particles in the range of 10% by mass to 500% by mass in terms of the stability and coatability of the dispersion.

[0163] The thickness of the undercoat layer can be selected arbitrarily. In view of the characteristics of the electrophotographic photoreceptor and the coating property of the dispersion, the thickness is preferably 0.1 μm or more, and more preferably 20 μm or less. The undercoat layer may also contain a known antioxidant.

[0164] <Other layers> Furthermore, the present electrophotographic photoreceptor may have other layers as necessary, in addition to the present conductive support, the present photosensitive layer, the present protective layer and the present undercoat layer described above.

[0165] <Physical Properties of the Electrophotographic Photoreceptor> The electrophotographic photoreceptor can have the following physical properties.

[0166] (Martens hardness) In order to provide the electrophotographic photoreceptor with sufficient wear resistance for practical use, the Martens hardness is set to 355 N / mm 2 More preferably, it is 370N / mm 2 Above, 400N / mm 2 More preferably, it is equal to or greater than this. In the present invention, the Martens hardness of the photoreceptor means the Martens hardness measured from the surface side of the photoreceptor. The Martens hardness can be measured by the method described in the Examples below.

[0167] (Elastic deformation rate) In order to provide the electrophotographic photoreceptor with sufficient wear resistance for practical use, the elastic deformation rate is preferably 45% or more, more preferably 48% or more, and even more preferably 50% or more. In the present invention, the elastic deformation rate of the photoreceptor means the elastic deformation rate measured from the surface side of the photoreceptor. The elastic deformation rate can be measured by the method described in the Examples below.

[0168] <<This image forming device>> The present electrophotographic photoreceptor can be used to configure an image forming apparatus (the present image forming apparatus).

[0169] As shown in FIG. 1, the image forming apparatus includes an electrophotographic photoreceptor 1, a charging device 2, an exposure device 3, and a developing device 4, and may further include a transfer device 5, a cleaning device 6, and a fixing device 7 as necessary. The electrophotographic photoreceptor 1 is not particularly limited as long as it is the electrophotographic photoreceptor described above. As an example, Fig. 1 shows a drum-shaped photoreceptor in which the above-mentioned photosensitive layer is formed on the surface of a cylindrical conductive support. A charging device 2, an exposure device 3, a developing device 4, a transfer device 5, and a cleaning device 6 are arranged along the outer circumferential surface of the electrophotographic photoreceptor 1.

[0170] Examples of the charging device 2 include a non-contact corona charging device such as a corotron or scorotron, or a contact-type charging device (direct-type charging device) that charges the photoconductor surface by contacting a charging member to which a voltage is applied. Examples of contact charging devices include a charging roller and a charging brush. Note that FIG. 1 shows a roller-type charging device (charging roller) as an example of the charging device 2.

[0171] The exposure device 3 is not particularly limited in type as long as it can expose the electrophotographic photoreceptor 1 to light and form an electrostatic latent image on the photosensitive surface of the electrophotographic photoreceptor 1 . Moreover, the exposure may be performed by an internal exposure method of the photoconductor.

[0172] The type of toner T is arbitrary, and in addition to powder toner, polymerized toner produced by a suspension polymerization method, an emulsion polymerization method, or the like can be used.

[0173] The developing device 4 may have any configuration. The developing device 4 shown in Fig. 1 has a configuration in which the toner T is made into a thin layer by a regulating member (developing blade) 45, is triboelectrically charged to a predetermined polarity, and is carried by a developing roller 44 while being transported to contact the surface of the photoconductor 1. However, the configuration is not limited to this. The type of the transfer device 5 is not particularly limited, and any device using any method, such as electrostatic transfer methods such as corona transfer, roller transfer, and belt transfer, pressure transfer, and adhesive transfer, can be used.

[0174] There is no particular limitation on the cleaning device 6. For example, any cleaning device such as a brush cleaner or a blade cleaner can be used. If there is little or almost no toner remaining on the photoreceptor surface, the cleaning device 6 may not be necessary. The fixing device 7 may also have any configuration. In addition to the above-mentioned configuration, the image forming apparatus may be configured to perform, for example, a charge removal process.

[0175] Furthermore, the image forming apparatus may be further modified, for example, to be configured to perform processes such as a pre-exposure process and an auxiliary charging process, to be configured to perform offset printing, or even to be configured as a full-color tandem system using multiple types of toner.

[0176] <<This electrophotographic cartridge>> The present electrophotographic photoreceptor 1 can be combined with one or more of a charging device 2, an exposure device 3, a developing device 4, a transfer device 5, a cleaning device 6 and a fixing device 7 to form an integrated cartridge (referred to as "the present electrophotographic cartridge").

[0177] The present electrophotographic cartridge can be configured to be detachable from the main body of an electrophotographic device such as a copier or a laser beam printer. In that case, for example, when the present electrophotographic photoreceptor 1 or other members deteriorate, the electrophotographic photoreceptor cartridge can be removed from the main body of the image forming device and a new electrophotographic photoreceptor cartridge can be attached to the main body of the image forming device, thereby facilitating the maintenance and management of the image forming device.

[0178] <<Explanation of terms>> In the present invention, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In addition, when it is expressed as "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the intention that "greater than X is preferable" or "less than Y is preferable." EXAMPLES

[0179] Hereinafter, the embodiment of the present invention will be described in more detail with reference to examples. However, the following examples are provided to explain the present invention in detail, and the present invention is not limited to the examples shown below, and can be modified as desired without departing from the gist of the present invention. In the following examples and comparative examples, the term "parts" refers to "parts by mass" unless otherwise specified.

[0180] [Production Example 1: Production of reactant (M1)] Dipentaerythritol (8.00 g), methacrylic acid (24.38 g), toluene (24.00 g), hydroquinone (0.06 g), p-toluenesulfonic acid monohydrate (1.35 g), and copper(II) chloride (0.05 g) were charged into a 200 mL four-necked reaction vessel. Compressed air was blown into the reaction solution at 50 mL / min, the temperature was raised to reflux, and the reaction was carried out for 14 hours while distilling off the generated water, after which the temperature was lowered to 60°C and 30 mL of toluene and 140 mL of water were added. The organic layer was separated and washed twice with 0.5 N aqueous sodium hydroxide solution, then with 0.5 N aqueous hydrochloric acid solution, and further with 5% saline. Activated clay (11 g) was added to the obtained organic layer and stirred. After filtering off the activated clay, 4-methoxyphenol (20 mg) was added and concentrated under reduced pressure to obtain 20.45 g of a reaction product (M1) as a white crystal, the main component of which was a compound represented by the following formula (C1) (molecular weight: 662.73). The reaction product (M1) was analyzed by liquid chromatography-mass spectrometry (LC / MS), and the main component with the largest peak area was found to have m / z=663 ([M+H] + ) gave an ion peak of the formula (C1) below. The reaction product was analyzed by gel permeation chromatography (GPC) to find that it had a number average molecular weight (Mn) of 756, a weight average molecular weight (Mw) of 818, and Mw / Mn of 1.082.

[0181] TIFF2024168996000020.tif42170

[0182] [Production Example 2: Production of reactant (M2)] Instead of dipentaerythritol used in Production Example 1, pentaerythritol (7.00 g) was used, and methacrylic acid (26.56 g), toluene (21.00 g), hydroquinone (0.03 g), p-toluenesulfonic acid monohydrate (0.83 g), and copper (II) chloride (0.03 g) were charged and reacted for 9 hours in the same manner as in Production Example 1, to obtain 18.15 g of a reaction product (M2) containing as a main component a compound represented by the following formula (C2) (molecular weight: 408.45) as a white crystal. The reaction product (M2) was analyzed by liquid chromatography-mass spectrometry (LC / MS), and the main component with the largest peak area was found to have m / z=409 ([M+H] + ) gave an ion peak of the formula (C2) below. The reaction product was analyzed by gel permeation chromatography (GPC) to find that it had a number average molecular weight (Mn) of 508, a weight average molecular weight (Mw) of 542, and Mw / Mn of 1.067.

[0183] TIFF2024168996000021.tif38170

[0184] [Production Example 3: Production of reactant (M3)] The amounts of dipentaerythritol (5.30 g), methacrylic acid (17.94 g), toluene (15.90 g), hydroquinone (0.04 g), p-toluenesulfonic acid monohydrate (1.01 g), and copper (II) chloride (0.04 g) were changed to those of Production Example 1, and ε-caprolactone (7.85 g) was further added and reacted for 6 hours. In the same manner as in Production Example 1, 17.92 g of a reaction product (M3) containing as a main component a compound represented by the following formula (C3) (molecular weight: 776.87) was obtained as a pale yellow oil. The reaction product (M3) was analyzed by liquid chromatography-mass spectrometry (LC / MS), and the main component with the largest peak area was found to have m / z=777 ([M+H] + ) gave an ion peak of the formula (C3) below. The reaction product was analyzed by gel permeation chromatography (GPC) to find that it had a number average molecular weight (Mn) of 1111, a weight average molecular weight (Mw) of 1247, and Mw / Mn of 1.123.

[0185] TIFF2024168996000022.tif38170

[0186] [Production Example 4: Production of reactant (M4)] The same procedure as in Production Example 3 was repeated except that the amounts of dipentaerythritol (6.00 g), methacrylic acid (18.28 g), toluene (18.00 g), hydroquinone (0.04 g), p-toluenesulfonic acid monohydrate (1.02 g), copper (II) chloride (0.04 g), and ε-caprolactone (5.93 g) were used, and 17.90 g of a reaction product (M4) containing the compound represented by the formula (C3) (molecular weight: 776.87) as a main component was obtained as a pale yellow oil. The reaction product (M4) was analyzed by liquid chromatography-mass spectrometry (LC / MS), and the main component with the largest peak area was found to have m / z=777 ([M+H] + ) gave an ion peak of the formula (C3). The reaction product was analyzed by gel permeation chromatography (GPC) to find that it had a number average molecular weight (Mn) of 995, a weight average molecular weight (Mw) of 1108, and Mw / Mn of 1.113.

[0187] [Production Example 5: Production of reactant (M5)] The same procedure as in Production Example 3 was repeated except that the amounts of dipentaerythritol (7.00 g), methacrylic acid (21.33 g), toluene (21.00 g), hydroquinone (0.05 g), p-toluenesulfonic acid monohydrate (1.19 g), copper (II) chloride (0.04 g), and ε-caprolactone (3.14 g) were used to obtain 18.00 g of a reaction product (M5) containing a compound represented by the formula (C3) (molecular weight: 776.87) in a transparent oil in the form of some cloudy crystals. The reaction product was analyzed by gel permeation chromatography (GPC) to find that it had a number average molecular weight (Mn) of 856, a weight average molecular weight (Mw) of 955, and Mw / Mn of 1.116.

[0188] [Production Example 6: Production of reactant (M6)] The same procedure as in Production Example 3 was repeated except that the amounts of dipentaerythritol (7.50 g), methacrylic acid (22.85 g), toluene (22.50 g), hydroquinone (0.05 g), p-toluenesulfonic acid monohydrate (1.27 g), copper(II) chloride (0.04 g), and ε-caprolactone (1.68 g) were used, and 20.74 g of a reaction product (M6) containing a compound represented by the formula (C3) (molecular weight: 776.87) was obtained as white turbid crystals. The reaction product was analyzed by gel permeation chromatography (GPC) to find that it had a number average molecular weight (Mn) of 807, a weight average molecular weight (Mw) of 884, and Mw / Mn of 1.095.

[0189] [Production Example 7: Production of reactant (M7)] The amounts of pentaerythritol (6.50 g), methacrylic acid (24.66 g), toluene (19.50 g), hydroquinone (0.09 g), p-toluenesulfonic acid monohydrate (2.06 g), and copper (II) chloride (0.07 g) were changed to those of Production Example 2, and ε-caprolactone (2.72 g) was further added and reacted for 6 hours. In the same manner as in Production Example 2, 19.08 g of a reaction product (M7) containing a compound represented by the above formula (C2) (molecular weight: 408.45) and a compound represented by the following formula (C4) (molecular weight: 522.59) was obtained as pale yellow cloudy crystals. The reaction product (M7) was analyzed by liquid chromatography-mass spectrometry (LC / MS), and the main component with the largest peak area was identified as the formula (C2) by giving an ion peak at m / z=409 ([M+H]+). In addition, the peak with the second largest area after the formula (C2) peak was identified as the formula (C2) by giving an ion peak at m / z=523 ([M+H] + ) gave an ion peak of the formula (C4) below. The reaction product was analyzed by gel permeation chromatography (GPC) to find that it had a number average molecular weight (Mn) of 551, a weight average molecular weight (Mw) of 642, and Mw / Mn of 1.133.

[0190] TIFF2024168996000023.tif38170

[0191] [Production Example 8: Production of reactant (M8)] The same procedure as in Production Example 3 was repeated except that the amounts of dipentaerythritol (7.50 g), methacrylic acid (22.85 g), toluene (22.50 g), hydroquinone (0.05 g), p-toluenesulfonic acid monohydrate (1.27 g), copper(II) chloride (0.04 g), and ε-caprolactone (0.84 g) were used, and 18.96 g of a reaction product (M8) containing the compound represented by the formula (C3) (molecular weight: 776.87) was obtained as white turbid crystals. The reaction product was analyzed by gel permeation chromatography (GPC) to find that it had a number average molecular weight (Mn) of 779, a weight average molecular weight (Mw) of 849, and Mw / Mn of 1.090.

[0192] [Production Example 9: Production of reactant (M9)] The amounts of pentaerythritol (6.50 g), methacrylic acid (24.66 g), toluene (19.50 g), hydroquinone (0.09 g), p-toluenesulfonic acid monohydrate (2.06 g), and copper(II) chloride (0.07 g) were changed to the amounts of pentaerythritol (6.50 g), methacrylic acid (24.66 g), toluene (19.50 g), hydroquinone (0.09 g), p-toluenesulfonic acid monohydrate (2.06 g), and copper(II) chloride (0.07 g), and ε-caprolactone (1.36 g) was further added and reacted for 6 hours in the same manner as in Production Example 2, to obtain 17.58 g of a reaction product (M9) containing the compound represented by the formula (C4) (molecular weight: 522.59) as white turbid crystals. The reaction product was analyzed by gel permeation chromatography (GPC) to find that it had a number average molecular weight (Mn) of 520, a weight average molecular weight (Mw) of 586, and Mw / Mn of 1.127.

[0193] [Production Example 10: Production of reactant (M10)] The amounts of dipentaerythritol (5.71 g), methacrylic acid (23.22 g), toluene (20.19 g), hydroquinone (0.05 g), p-toluenesulfonic acid monohydrate (1.29 g), copper (II) chloride (0.04 g), and ε-caprolactone (3.42 g) were changed to Production Example 3, and pentaerythritol (1.02 g) was further added. In the same manner as in Production Example 3, 18.26 g of a reaction product (M10) containing the compound represented by the formula (C3) (molecular weight: 776.87) and the compound represented by the formula (C4) (molecular weight: 522.59) was obtained in the form of partially cloudy crystals in a pale yellow oil. The reaction product was analyzed by gel permeation chromatography (GPC) to find that it had a number average molecular weight (Mn) of 802, a weight average molecular weight (Mw) of 914, and Mw / Mn of 1.139.

[0194] [Production Example 11: Production of reactant (M11)] The amounts of dipentaerythritol (6.16 g), methacrylic acid (25.04 g), toluene (21.78 g), hydroquinone (0.06 g), p-toluenesulfonic acid monohydrate (1.39 g), copper (II) chloride (0.05 g), and ε-caprolactone (1.84 g) were changed to dipentaerythritol (6.16 g), methacrylic acid (25.04 g), toluene (21.78 g), hydroquinone (0.06 g), p-toluenesulfonic acid monohydrate (1.39 g), copper (II) chloride (0.05 g), and ε-caprolactone (1.84 g), and pentaerythritol (1.10 g) was further added. In the same manner as in Production Example 3, 20.16 g of a reaction product (M11) containing the compound represented by the formula (C3) (molecular weight: 776.87) and the compound represented by the formula (C4) (molecular weight: 522.59) was obtained in a partially cloudy crystal state in a pale yellow oil. The reaction product was analyzed by gel permeation chromatography (GPC) to find that it had a number average molecular weight (Mn) of 738, a weight average molecular weight (Mw) of 831, and Mw / Mn of 1.125.

[0195] [Production Example 12: Production of reactant (M12)] The amounts of dipentaerythritol (4.30 g), methacrylic acid (26.18 g), toluene (19.80 g), hydroquinone (0.06 g), p-toluenesulfonic acid monohydrate (1.45 g), copper (II) chloride (0.05 g), and ε-caprolactone (1.93 g) were changed to Production Example 3, and pentaerythritol (2.30 g) was further added. In the same manner as in Production Example 3, 16.04 g of a reaction product (M12) containing the compound represented by the formula (C3) (molecular weight: 776.87) and the compound represented by the formula (C4) (molecular weight: 522.59) was obtained as a pale yellow oil. The reaction product was analyzed by gel permeation chromatography (GPC) to find that it had a number average molecular weight (Mn) of 675, a weight average molecular weight (Mw) of 769, and Mw / Mn of 1.140.

[0196] [Production Example 13: Production of reactant (M13)] The amounts of dipentaerythritol (4.67 g), methacrylic acid (28.45 g), toluene (21.51 g), hydroquinone (0.07 g), p-toluenesulfonic acid monohydrate (1.58 g), copper (II) chloride (0.05 g), and ε-caprolactone (1.05 g) were changed to dipentaerythritol (4.67 g), methacrylic acid (28.45 g), toluene (21.51 g), hydroquinone (0.07 g), p-toluenesulfonic acid monohydrate (1.58 g), copper (II) chloride (0.05 g), and ε-caprolactone (1.05 g), and pentaerythritol (2.50 g) was further added. In the same manner as in Production Example 3, 17.42 g of a reaction product (M13) containing the compound represented by the formula (C3) (molecular weight: 776.87) and the compound represented by the formula (C4) (molecular weight: 522.59) was obtained in the form of partially cloudy crystals in a pale yellow oil. The reaction product was analyzed by gel permeation chromatography (GPC) to find that it had a number average molecular weight (Mn) of 635, a weight average molecular weight (Mw) of 715, and Mw / Mn of 1.125.

[0197] <Crystallization test> For the reaction products (M1) to (M13) obtained in Production Examples 1 to 13, a crystal precipitation test was carried out by the following method in order to confirm the ease of crystal precipitation. 0.40 g of each of the reactants (M1) to (M13) was dissolved in 1.60 g of a mixed solvent of methanol / 1-propanol / toluene = 7 / 1 / 2 to prepare a 20 wt% solution of each reactant. One drop of this solution was dropped with a poly dropper onto a sheet of aluminum-deposited PET film with a thickness of 75 μm, and air-dried at room temperature, and the time until crystals began to precipitate was measured. The reaction was observed for up to 10 minutes, and if crystals did not begin to precipitate even after 10 minutes, it was judged to have low crystallinity and difficult to precipitate. The evaluation criteria are shown below. In this example, a case of "○" was considered to be acceptable, and a case of "△" or less was considered to be unacceptable. If the time it takes for crystals to start precipitating in this test is less than 10 minutes, there is a risk that crystals will precipitate on the photoconductor surface when the protective layer is formed, making the surface less smooth and rough. Also, the shorter the time it takes for crystals to start precipitating, the higher the probability that crystals will precipitate on the photoconductor surface.

[0198] The evaluation results are shown in Table 1. In Table 1, "DPE" stands for dipentaerythritol, "PE" stands for pentaerythritol, and "CL" stands for ε-caprolactone. ○: More than 10 minutes until crystal precipitation begins △: Crystallization begins in 5 to 10 minutes ×: Crystallization begins in 1 minute or more but less than 5 minutes ××: Less than 1 minute until crystal precipitation begins

[0199] [Table 1]

[0200] (Preparation of Coating Solution P1 for Forming Undercoat Layer) 20 parts of D-type titanyl phthalocyanine, which shows a clear peak at a diffraction angle 2θ=27.3°±0.2° in powder X-ray diffraction using CuKα radiation, was mixed with 280 parts of 1,2-dimethoxyethane, and ground for 2 hours in a sand grind mill to carry out a fine dispersion treatment. 400 parts of a 1,2-dimethoxyethane solution containing 2.5% by mass of polyvinyl butyral (manufactured by Denki Kagaku Kogyo Co., Ltd., product name "Denka Butyral" #6000C) and 170 parts of 1,2-dimethoxyethane were further added and mixed to prepare coating solution P1 for forming an undercoat layer.

[0201] (Preparation of Coating Solution Q1 for Forming Single-Layer Photosensitive Layer) In powder X-ray diffraction using CuKα radiation, 2.6 parts of D-type titanyl phthalocyanine showing a clear peak at a diffraction angle 2θ=27.3°±0.2°, 1.3 parts of perylene pigment 1 having the structure shown below, 0.5 parts of polyvinyl butyral resin, 90 parts of the hole transport material shown below (HTM48, molecular weight 748), 70 parts of the electron transport material shown below (ET-2, molecular weight 424.2), 100 parts of polycarbonate resin having a biphenyl structure, and 0.05 parts of silicone oil (manufactured by Shin-Etsu Silicones: product name KF-96) as a leveling agent were added to 793.35 parts of a mixed solvent of tetrahydrofuran (hereinafter appropriately abbreviated as THF) and toluene (hereinafter appropriately abbreviated as TL) (THF 80% by mass, TL 20% by mass) and mixed to prepare a single-layer type photosensitive layer forming coating solution Q1 with a solid content concentration of 25% by mass.

[0202] TIFF2024168996000025.tif35170

[0203] TIFF2024168996000026.tif36150

[0204] TIFF2024168996000027.tif55170

[0205] (Preparation of protective layer forming coating solution S1) The reactant (M1) obtained in Production Example 1, which had been dissolved in advance in a mixed solvent of methanol / 1-propanol / toluene, was mixed with Irgacure OXE03 (manufactured by BASF Japan Ltd.) as a photopolymerization initiator and a dispersion slurry of titanium oxide particles (average primary particle size 40 nm, surface-treated with 3.5 mass % methyldimethoxysilane) to obtain a protective layer-forming coating solution S1 (solid concentration 27.0 mass %) having a reactant (M1) / titanium oxide particles / Irgacure OXE03 (mass ratio) = 100 / 60 / 3 and a solvent composition of methanol / 1-propanol / toluene (mass ratio) = 7 / 1 / 2.

[0206] (Preparation of protective layer forming coating solutions S2 to S13) Coating solutions S2 to S13 (solid content concentration 27.0 mass%) for forming protective layers were obtained in the same manner as the coating solution S1 for forming protective layers, except that the reaction product (M2) obtained in Production Example 2 to the reaction product (M13) obtained in Production Example 13 were used instead of the reaction product (M1).

[0207] <Preparation of single-layer photoreceptor> A single-layer photoreceptor was prepared according to the following procedure.

[0208] [Comparative Example 1] An aluminum cylinder with a diameter of 30 mm and a length of 244 mm, the surface of which had been machined, was dip-coated with coating solution P1 for forming an undercoat layer, so that an undercoat layer was formed with a film thickness of 0.4 μm after drying. Coating solution Q1 for forming a single-layer type photosensitive layer was dip-coated on the undercoat layer, and dried at 125° C. for 24 minutes, so that a single-layer type photosensitive layer was formed with a film thickness of 32 μm after drying. Coating solution S1 for forming a protective layer was ring-coated on the single-layer type photosensitive layer, and 365 nm LED light was applied at 1.3 W / cm while rotating the photoreceptor at 60 rpm under a nitrogen atmosphere. 2 A protective layer was provided so that the thickness after curing would be 2 μm, thereby preparing photoreceptor A1.

[0209] [Comparative Example 2] Photoreceptor A2 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S2.

[0210] [Comparative Example 3] Photoreceptor A3 was prepared in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S3.

[0211] [Comparative Example 4] Photoreceptor A4 was prepared in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S4.

[0212] [Comparative Example 5] Photoreceptor A5 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S5.

[0213] [Comparative Example 6] Photoreceptor A6 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S6.

[0214] [Comparative Example 7] Photoreceptor A7 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S7.

[0215] [Comparative Example 8] Photoreceptor A8 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S8.

[0216] [Comparative Example 9] Photoreceptor A9 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S9.

[0217] [Example 1] Photoreceptor A10 was produced in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S10.

[0218] [Example 2] Photoreceptor A11 was prepared in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S11.

[0219] [Example 3] Photoreceptor A12 was prepared in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S12.

[0220] [Example 4] Photoreceptor A13 was prepared in the same manner as photoreceptor A1, except that protective layer forming coating liquid S1 was changed to protective layer forming coating liquid S13.

[0221] <Evaluation of photoreceptor appearance> The surface conditions of the photoreceptors A1 to A13 obtained in the examples and comparative examples were visually observed. The evaluation criteria are shown below. The evaluation results are shown in Table 2. In this example, "◯" was considered to be pass, and "△" or lower was considered to be fail. ◯: The entire surface of the photoreceptor is smooth. △: There are irregularities or unevenness in some parts of the photoreceptor surface. ×: The entire surface of the photoreceptor is rough and uneven.

[0222] <Evaluation of image streaming> The photoreceptors A3 to A7 and A10 to A13 obtained in the examples and comparative examples were mounted on an electrophotographic printer, printed in an environment of a temperature of 32°C and a relative humidity of 80%, and the image was observed at room temperature and normal humidity. The evaluation criteria are shown below. The evaluation results are shown in Table 2. In this example, "○" was considered to be pass, and "△" or lower was considered to be fail. Incidentally, since the photoconductors A1, A2, A8, and A9 had unevenness on the entire surface thereof, it was not possible to evaluate image deletion. ◯: No image blurring (image blur) is observed. △: Image blurring is observed in some areas. ×: Significant image blurring (image blur) is observed.

[0223] <Martens hardness and elastic deformation rate measurement> The photoreceptors A5 to A7 and A10 to A13 obtained in the examples and comparative examples were measured from the surface side of the photoreceptor under the following measurement conditions using a microhardness tester (Fischer: FISCHERSCOPE HM2000) in an environment of 25°C temperature and 50% relative humidity. The Martens hardness and elastic deformation rate of each sample are shown in Table 2. In addition, since the entire surface of the photoconductors A1, A2, A8, and A9 was uneven, it was not possible to measure the Martens hardness and elastic deformation rate. As for the photoconductors A3 and A4, the evaluation of image deletion was poor, so the Martens hardness and elastic deformation rate were not measured.

[0224] (Martens hardness and elastic deformation rate measurement conditions) Indenter: Vickers square pyramid diamond indenter with facing angle of 136° Maximum pressing load: 0.2mN Load time: 10 seconds Unloading time: 10 seconds

[0225] The Martens hardness is calculated according to the following formula. Martens hardness (N / mm 2 ) = Maximum indentation load / Indentation area at maximum indentation load

[0226] The elastic deformation rate is a value defined by the following formula, and is the ratio of the work performed by the membrane due to its elasticity when removing the load to the total work required for pressing. Elastic deformation rate (%) = (We / Wt) x 100 In the above formula, the total work load Wt (nJ) indicates the area enclosed by ABDA in Figure 2, and the elastic deformation work load We (nJ) indicates the area enclosed by CBDC. The larger the elastic deformation rate, the less likely deformation will remain due to the load, and an elastic deformation rate of 100 means that no deformation will remain. In this embodiment, the Martens hardness is 350 N / mm 2 Anything above this was rated as "pass," and an elastic deformation rate of 45% or more was rated as "pass."

[0227] [Table 2]

[0228] <Consideration> In the reaction products (M1) and (M2) which do not contain either the compound having the structure represented by formula (1') or the compound having the structure represented by formula (2'), the time when crystals started to precipitate was less than 10 minutes in the crystal precipitation test. In the photoreceptors A1 and A2 of Comparative Examples 1 and 2 which used these reaction products, crystals precipitated on the photoreceptor surface, making the surface rough and resulting in poor appearance of the photoreceptor. Photoreceptors in such a state cannot be used in practice because the protective layer film is disturbed.

[0229] In the reaction products (M3) to (M9) containing only either the compound having the structure represented by formula (1') or the compound having the structure represented by formula (2'), the smaller the amount of ε-caprolactone charged, the more likely it was that crystals would precipitate. In addition, when compared with reaction products having the same amount of ε-caprolactone, the reaction products (M6) and (M8) containing only the compound having the structure represented by formula (2') were more likely to precipitate crystals than the reaction products (M7) and (M9) containing only the compound having the structure represented by formula (1').

[0230] In the photoreceptors A3 to A9 of Comparative Examples 3 to 9, which used the reactants (M3) to (M9), the crystal precipitation on the photoreceptor surface tended to be the same as in the case of the reactants being tested. When comparing the reactants (M5), (M6), and (M8) that contained only the compound having the structure represented by formula (2'), unevenness was observed in part of the film on the photoreceptor surface in all cases, and the photoreceptor appearance was the worst when the reactant (M8), which had the smallest amount of ε-caprolactone, was used. On the other hand, as for image blur (image blur), a comparison of the reactants (M3), (M4), and (M5) containing only the compound having the structure represented by formula (2') revealed that the image blur became worse as the amount of ε-caprolactone added increased.

[0231] The reaction products (M10) to (M13) containing both the compound having the structure represented by formula (1') and the compound having the structure represented by formula (2') did not precipitate crystals even after 10 minutes in the crystal precipitation test. The photoconductors A10 to A13 of Examples 1 to 4 using these reaction products had smooth photoconductor surfaces, good photoconductor appearances, and no image flow (image blur) was observed, which was good. It is considered that the inclusion of both the compound having the structure represented by formula (1') and the compound having the structure represented by formula (2') reduces the crystallinity of the reaction product, making it difficult for crystals to precipitate. Also, unlike the comparative example, it was found that regardless of the amount of ε-caprolactone added, crystals did not precipitate, and a photoconductor with a good surface condition and good image flow was obtained.

[0232] Regarding the Martens hardness and elastic deformation rate, when the photoreceptor A10 of Example 1 and the photoreceptor A5 of Comparative Example 5, both of which have the same molar ratio of ε-caprolactone added, 1, were compared, the photoreceptor A10 of Example 1, which used a reactant containing both the compound having the structure represented by formula (1′) and the compound having the structure represented by formula (2′), had higher Martens hardness and elastic deformation rate than the photoreceptor A5 of Comparative Example 5, which used a reactant containing only the compound having the structure represented by formula (2′). Furthermore, when comparing photoreceptor A12 of Example 3 with photoreceptor A13 of Example 4, photoreceptor A13 of Example 4, in which the molar ratio of ε-caprolactone charged was 0.25, had higher Martens hardness and elastic deformation rate. When reactants (M10) to (M13) containing both a compound having a structure represented by formula (1') and a compound having a structure represented by formula (2') are used, different structures are randomly and intricately combined to form a polymer when the protective layer is cured, which is thought to increase the Martens hardness and elastic deformation rate when made into a photoreceptor. The high Martens hardness and elastic deformation rate are expected to provide excellent mechanical strength and improve the printing durability of the photoreceptor.

[0233] From the results of the above Examples and Comparative Examples, as well as the results of tests conducted by the present inventors, it has been found that if the protective layer contains a polymer having a structure represented by the above formulas (1) and (2), i.e., if the protective layer is formed using a compound having a structure represented by the above formula (1') and a compound having a structure represented by the above formula (2'), then a photoreceptor can be obtained which has a smooth surface and good appearance, can prevent image deletion, and yet has high Martens hardness and elastic deformation rate.

[0234] The compounds having the structures represented by the formulas (1') and (2') react when the protective layer is cured, and the double bonds at the ends of the molecules are combined with reactive functional groups to polymerize, so that it is expected that there is a high possibility that the compounds will become copolymers in which polymers having the structures represented by the formulas (1) and (2) are randomly and complexly combined.

[0235] It is believed that by using the compound a and the compound b in combination, different structures become intertwined and packing becomes difficult, thereby suppressing crystal precipitation. In addition, l, m, n, and o in the formula (1'), and f, g, h, i, j, and k in the formula (2') are each independent integers, and have an asymmetric structure, except when they are all the same integer. In this case, compound a having a structure represented by formula (1') and compound b having a structure represented by formula (2') are preferable because their crystallinity is considered to be further suppressed. Therefore, when a protective layer is formed using the compound a and the compound b, crystals do not precipitate on the photoreceptor surface, the photoreceptor surface after curing becomes smooth, and image flow can be prevented. In other words, a photoreceptor whose protective layer contains a polymer obtained by polymerizing the compound a and the compound b does not precipitate crystals on the photoreceptor surface, the photoreceptor surface after curing becomes smooth, and image flow can be prevented. In other words, a photoreceptor whose protective layer contains a polymer having the structure represented by the formulas (1) and (2) does not precipitate crystals on the photoreceptor surface, the photoreceptor surface after curing becomes smooth, and image flow can be prevented. Thus, in Examples 1 to 4, R in the formulas (1') and (2') is -O-(C=O)-(CH2)5-, but it is believed that the same effect can be obtained even when the value of p is different or when R in the formulas (1') and (2') is an alkylene group having 1 to 8 carbon atoms which may have a substituent or an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent. [Explanation of symbols]

[0236] 1 Photoconductor (electrophotographic photoconductor) 2 Charging device (charging roller; charging section) 3 Exposure equipment (exposure section) 4. Developing device (developing section) 5. Transcription device 6 Cleaning device 7 Fixing device 41 Developer tank 42 Agitator 43 Supply roller 44 Developing roller 45 Regulatory Materials 71 Upper fixing member (pressure roller) 72 Lower fixing member (fixing roller) 73 Heating device T Toner P Recording paper (paper, medium)

Claims

1. An electrophotographic photoreceptor having a photosensitive layer and a protective layer in this order on a conductive support, The protective layer of the electrophotographic photoreceptor contains a polymer having a structure represented by the following formulas (1) and (2): [Formula (1)] In formula (1), l, m, n, and o each represent an integer of 0 to 10, and l+m+n+o represents 1 or more. Each R independently represents an alkylene group having 1 to 8 carbon atoms which may have a substituent, an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent, or -O-(C=O)-(CX 2 ) p - (wherein p is an integer of 1 to 6, and X is a hydrogen atom or a substituent). T represents a bond to any atom. Q represents a hydroxyl group or the following formula (3). Z 1 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and at least one of them is an alkyl group having 1 to 4 carbon atoms. [Formula (2)] In formula (2), f, g, h, i, j, and k each represent an integer of 0 to 10, and f+g+h+i+j+k is 1 or greater. Each R independently represents an alkylene group having 1 to 8 carbon atoms which may have a substituent, an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent, or -O-(C=O)-(CX 2 ) p - (wherein p is an integer of 1 to 6, and X is a hydrogen atom or a substituent). T represents a bond to any atom. Q represents a hydroxyl group or the following formula (3). Z 1 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and at least one of them is an alkyl group having 1 to 4 carbon atoms. [Formula (3)] (In formula (3), Z 2 represents a bond to R in formula (1) or (2). 1 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. T represents a bond to any atom.

2. An electrophotographic photoreceptor having a photosensitive layer and a protective layer in this order on a conductive support, The protective layer of the electrophotographic photoreceptor contains a polymer obtained by polymerizing a compound a having a structure represented by the following formula (1') and a compound b having a structure represented by the following formula (2'). [Formula (1')] In formula (1'), l, m, n, and o each represent an integer of 0 to 10, and l+m+n+o represents 1 or more. Each R independently represents an alkylene group having 1 to 8 carbon atoms which may have a substituent, an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent, or -O-(C=O)-(CX 2 ) p - (wherein p is an integer of 1 to 6, and X is a hydrogen atom or a substituent). Q represents a hydroxyl group or the following formula (3'): Z 1 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and at least one of them is an alkyl group having 1 to 4 carbon atoms. [Formula (2')] In formula (2'), f, g, h, i, j, and k each represent an integer of 0 to 10, and f+g+h+i+j+k is 1 or greater. Each R independently represents an alkylene group having 1 to 8 carbon atoms which may have a substituent, an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent, or -O-(C=O)-(CX 2 ) p - (wherein p is an integer of 1 to 6, and X is a hydrogen atom or a substituent). Q represents a hydroxyl group or the following formula (3'): Z 1 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and at least one of them is an alkyl group having 1 to 4 carbon atoms. [Formula (3')] (In formula (3'), Z 2 represents a bond to R in formula (1') or formula (2'). 1 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.

3. R in at least one of the formulas (1), (2), (1′) and (2′) is an oxyalkylene group having 1 to 8 carbon atoms which may have a substituent, or —O—(C═O)—(CX 2 ) p 3. The electrophotographic photoreceptor according to claim 1, wherein p is an integer of 1 to 6, and X represents a hydrogen atom or a substituent.

4. 3. An electrophotographic photoreceptor cartridge comprising the electrophotographic photoreceptor according to claim 1.

5. 3. An image forming apparatus comprising the electrophotographic photoreceptor according to claim 1.

Citation Information

Patent Citations

  • Foamed polyisocyanurate and construction material made of same

    JP1977063296A

  • Photo conductor overcoat comprising radical polymerizable charge transport molecules and hexa-functional urethane acrylates

    US9417538B2

  • Electrophotographic photoreceptor, image forming apparatus, and method for image formation

    WO2010035683A1