Sensor element and odor measurement device

The sensor element with a tailored odorant-receiving layer and permeable layer addresses deformation issues in chemiresistor sensors, enhancing sensitivity and accuracy in odorant detection.

JP2024169367APending Publication Date: 2024-12-05SANYO CHEM IND LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024082772
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-05-21
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Chemiresistor-type odor sensors face challenges in distinguishing between odorant-induced deformations and deformations caused by external physical forces, leading to erroneous measurements due to turbulence and wind pressure changes when high gas flow rates are used.

Method used

A sensor element design incorporating an odorant-receiving layer with specific resin and filler compositions, along with a porosity range and an odorant-permeable layer, to mitigate external force-induced deformations and enhance sensitivity.

Benefits of technology

The design reduces deformation due to external forces, improving measurement sensitivity and accuracy by stabilizing the odorant-receiving layer, allowing for precise odorant detection and identification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169367000001_ABST
    Figure 2024169367000001_ABST
Patent Text Reader

Abstract

To provide a sensor element which mitigates deformation of an odor substance receptive layer due to external physical force and offers improved measurement sensitivity.SOLUTION: A sensor element (31) is provided, comprising an odor substance receptive layer (315) containing a resin composition, metal wiring (313) in contact with the odor substance receptive layer (315), and an odor substance-permeable layer (317) covering the odor substance receptive layer (315) on a side opposite the side in contact with the metal wiring. In a cross-section of the odor substance receptive later, a first porosity representing a proportion of area occupied by pores is 3% to 20%, inclusive. In a cross-section of the odor substance-permeable layer, a second porosity representing a proportion of area occupied by pores is 3% or less. An odor measurement method is of the chemiresistor type.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an odor measuring device. [Background technology]

[0002] With recent developments in information processing technology, if it were possible to somehow quantify the sense of smell, which is one of the five human senses that cannot be adequately measured mechanically, it is expected that this technology could be used in a wide range of industrial fields, including the medical field, the environmental field, the field of biogas utilization, the field of safety, the field of food, and the field of marketing. Such technology relating to the sense of smell can be used for a variety of purposes, for example, as follows: Medical field: Nursing care, assistance, preventive diagnosis and disease testing, etc. ·Environmental field: Odor control in factories, etc. - Biogas utilization: Fermentation process management, wastewater treatment management, etc. Safety field: Predicting landslides and floods, detecting deterioration of engine oil and machine operating oil, etc. Food industry: Detection of the maturity state of plants (e.g. vegetables and grains) and meat, process management of fermented foods such as alcoholic beverages, plant cultivation management, and quality control during food production, storage, and distribution. Marketing field: Cosmetics, body odor countermeasures, scented environments, product scent production, etc.

[0003] The invention described in Patent Document 1 proposes a mechanism for detecting the adsorption of odor components on the surface of a conductive polymer by replacing the semiconductor of a semiconductor gas sensor with a conductive polymer. Patent Document 1 reports that it is possible to detect odor components that are easily thermally decomposed and substances that do not cause an oxidation-reduction reaction on the surface of the detection part of the sensor.

[0004] Patent Document 2 also focuses on the property that the electrical resistance of a mixture of an organic polymer and a conductive material changes when exposed to an organic gas. Patent Document 2 describes that when a plurality of combinations of organic polymer / conductive material in which the organic polymer composition is different from that of the above mixture is prepared and these are used as an electrical resistance array in a sensor, the electrical resistance changes when exposed to the same organic gas are different for each combination. Patent Document 2 reports that this can be used to identify odors by attributing the pattern of electrical resistance changes to the type of odor (= organic gas mixture).

[0005] Furthermore, Patent Document 3 reports that the response speed of the sensor is improved by adding a plasticizer to the above organic polymer. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 11-23508 [Patent Document 2] Special Publication No. 11-503231 [Patent Document 3] Patent Publication No. 2002-519633 Summary of the Invention [Problem to be solved by the invention]

[0007] Chemiresistor-type odor sensors detect the deformation of the odorant receptive layer caused by the adsorption of odorants through changes in stress and electrical resistance, and are odor sensors with excellent repeatability. However, in chemiresistor-type odor sensors, it may be difficult to distinguish between deformation of the odorant receptive layer caused by external stress such as local turbulence and deformation caused by odorant adsorption.

[0008] For example, an odor measuring device equipped with a chemiresistor-type odor sensor can increase the amount of odorant that comes into contact with the odor sensor element and improve sensitivity by sending gas containing the odorant to be measured to the odor sensor at high speed. However, when the flow rate of the gas sent to the sensor is increased, deformation of the odorant receiving layer that is not caused by the adsorption of the odorant (e.g., deformation due to physical external forces) may occur. For example, if a large amount of air containing the odorant is sent to the odor sensor or the flow rate of the carrier gas is changed, turbulence and changes in wind pressure may occur around the odor sensor. These turbulence and changes in wind pressure may affect the odor sensor as physical external forces. Such deformation may cause the concentration of the odorant to be measured erroneously.

[0009] One aspect of the present invention aims to provide a sensor element or the like that reduces deformation of an odorant receiving layer caused by external physical force and improves measurement sensitivity. [Means for solving the problem]

[0010] A sensor element for an odor measuring device according to one embodiment of the present invention comprises an odorant receiving layer comprising a resin composition including a resin (A) and a filler (B), a first metal wiring in contact with at least a portion of the odorant receiving layer, a second metal wiring spaced from the first metal wiring and in contact with at least a portion of the odorant receiving layer, and an odorant permeation layer covering the surface of the odorant receiving layer opposite the side in contact with the first metal wiring and the second metal wiring, wherein a first porosity indicating the proportion of the area occupied by voids in the cross section of the odorant receiving layer is 3% or more and 20% or less, a second porosity indicating the proportion of the area occupied by voids in the cross section of the odorant permeation layer is 3% or less, and the odor measurement method is a chemiresistor type. Effect of the Invention

[0011] According to one aspect of the present invention, a sensor element or the like can be provided in which deformation of an odorant receiving layer caused by external physical force is mitigated, thereby improving measurement sensitivity. [Brief description of the drawings]

[0012] [Figure 1] 1 is a schematic diagram showing an example of the configuration of an odor sensor according to one embodiment of the present invention. [Diagram 2] This is an SEM image of a cross section of a sensor element. [Diagram 3] FIG. 2 is a top view showing an example of the configuration of a sensor element. [Figure 4] 4 is a cross-sectional view showing an example of the configuration of the sensor element shown in FIG. 3. [Diagram 5] 1 is a schematic diagram showing an example of the configuration of an odor measurement device according to one embodiment of the present invention. [Figure 6] 1 is a functional block diagram showing an example of the configuration of an odor measurement device. [Figure 7] 11 is a flowchart showing an example of a process flow in which the estimation device generates an estimation model. [Figure 8] 1 is a functional block diagram showing an example of the configuration of an odor measurement device. [Figure 9] 11 is a flowchart showing an example of a process flow in which the estimation device estimates an odor substance. [Figure 10] FIG. 2 is a top view showing an example of the configuration of a sensor element of the present invention. [Figure 11] FIG. 2 is a top view showing an example of the configuration of a sensor element of the present invention. [Figure 12] FIG. 2 is a perspective view showing an example of the configuration of a sensor element of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] An embodiment of the present invention will be described below, but the present invention is not limited thereto. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more and B or less."

[0014] [1. Sensor element 31] As a result of investigations aimed at achieving the above object, the present inventors arrived at the present invention.

[0015] The sensor element 31 for an odor measuring device according to one embodiment of the present invention includes an odorant receiving layer 315 containing a resin composition, a first metal wiring 313A and a second metal wiring 313B each in contact with at least a portion of the odorant receiving layer 315, and an odorant permeable layer 317. Here, the resin composition contains a resin (A) and a filler (B). The first metal wiring 313A is spaced apart from the second metal wiring 313B.

[0016] The odorant permeation layer 317 covers the surface of the odorant reception layer 315 opposite the side in contact with the first metal wiring 313A and the second metal wiring 313B. For example, the odorant permeation layer 317 may be provided so as to completely cover the side of the odorant reception layer 315 opposite the side in contact with the first metal wiring 313A and the second metal wiring 313B. The odorant permeation layer 317 and the odorant reception layer 315 are in contact on a surface different from the surface including the contact surface of the odorant reception layer 315 with the first metal wiring 313A and the second metal wiring 313B. The odorant permeation layer 317 is not in contact with the first metal wiring 313A and the second metal wiring 313B.

[0017] [2-1. Odor-permeable layer] The odorant-permeable layer 317 of the sensor element 31 may include any of butyral, polymethyl methacrylate, polyurethane, polyvinyl alcohol, polyvinyl chloride, polyester, polyvinylidene fluoride, cellulose acetate, polyvinylpyrrolidone, paraffin and polypropylene.

[0018] The odorant permeable layer 317 containing this composition may be a layer that allows the odorant to reach the odorant receiving layer 315 described below. The odorant permeable layer 317 may also function as a protective layer that reduces the rate at which the odorant receiving layer 315 deteriorates due to humidity in the measurement environment.

[0019] The odorant permeable layer 317 may be a thin film having a thickness of 0.1 μm or more and 20 μm or less, with the lower limit of the thickness being more preferably 0.5 μm or more and the upper limit of the thickness being more preferably 20 μm or less. The thickness of the odorant permeable layer 317 may be within the above numerical range throughout the entire odorant permeable layer 317, or the average value of the entire thickness of the odorant permeable layer 317 may be within the above numerical range. When creating the odorant permeable layer 317, the area of ​​the film to be coated is regulated by the electrode shape, etc., and the evaporation residue and the amount of the solution of the odorant permeable layer 317 to be dispensed are controlled to control the thickness of the odorant permeable layer 317. The odorant that has permeated the odorant permeable layer 317 can reach the odorant receiving layer 315, but the odorant that cannot permeate the odorant permeable layer 317 cannot reach the odorant receiving layer 315. If the thickness of the odorant permeable layer 317 is excessively thick, less odorant reaches the odorant receiving layer 315, resulting in a decrease in measurement sensitivity. Furthermore, if the odorant permeation layer 317 inhibits the volume change of the odorant receiving layer 315, the change in electrical conductivity of the odorant receiving layer 315 caused by the odorant being adsorbed by the odorant receiving layer 315 will be small, and the measurement sensitivity will decrease. On the other hand, if the thickness of the odorant permeation layer 317 is insufficient, the odorant receiving layer 315 cannot be sufficiently protected. Therefore, it is preferable that the thickness of the odorant permeation layer 317 of the sensor element 31 according to the present invention is within the above-mentioned range.

[0020] The lower the second porosity, which indicates the proportion of the area occupied by voids in the cross section of the odorant permeable layer 317, the less effective it is at protecting the odorant receiving layer 315 from external physical forces (e.g., air flow) that affect the odorant receiving layer 315. Therefore, the second porosity, which indicates the proportion of the area occupied by voids in the cross section of the odorant permeable layer 317, is 3% or less, and preferably 2.0% or less. In addition, the second porosity is preferably 0.5% or more. Such an odorant permeable layer 317 can form a sensor element 31 that is highly durable against external physical forces.

[0021] <Method for measuring the thickness of the odorant permeable layer 317> The method for measuring the thickness of the odorant permeation layer 317 will be described below with reference to FIG. 2. FIG. 2 is a scanning electron microscope (SEM) image of the cross section of the sensor element 31 including the odorant reception layer 315 and the odorant permeation layer 317, observed at 25,000 times magnification. The cross section of the sensor element 31 including the odorant reception layer 315 and the odorant permeation layer 317 is formed, for example, using a cross-section polisher, specifically IB-19530CP (product name manufactured by JEOL Ltd.). The lines indicated by symbols L1 to L20 in FIG. 2 indicate the length from the boundary between the odorant reception layer 315 and the odorant permeation layer 317 at each location to the surface of the odorant permeation layer 317. Hereinafter, the length from the boundary between the odorant reception layer 315 and the odorant permeation layer 317 to the surface of the odorant permeation layer 317 is referred to as the cross-sectional length of the odorant permeation layer 317. The boundary between the odorant receiving layer 315 and the odorant permeable layer 317 can be determined, for example, using SEM reflection observation, electron image SEM-EDX, or STEM.

[0022] The thickness of the odorant-permeable layer 317 may be the average value of the cross-sectional length at multiple points of the odorant-permeable layer 317. The measurement points of the cross-sectional length that are the calculation basis for the thickness of the odorant-permeable layer 317 may be two points, the thickest and the thinnest, or may be 10 points arbitrarily selected from the odorant-permeable layer 317, or may be even more. As an example, the average value of the cross-sectional lengths at 20 points indicated by symbols L1 to L20 in the example shown in FIG. 2 may be the thickness of the odorant-permeable layer 317. The thickness of the odorant-permeable layer 317 may be the average value of the cross-sectional lengths at multiple points that fall within the above-mentioned numerical range.

[0023] [2-2. Odor Receptor Layer] The odorant receiving layer 315 of the sensor element 31 contains a resin composition including a resin (A) and a filler (B). This resin composition may further contain a surfactant (C). This resin composition is applied onto a sensor element substrate, heated and dried to a dry solid, and then used as the odorant receiving layer 315. The electrical resistance value of this resin composition changes depending on the adsorption of odorants, etc. In other words, the sensor element 31 is an odor detection device equipped with such a resin composition, and the odor measurement method of the sensor element 31 is a chemiresistor type.

[0024] The higher the first porosity, which indicates the proportion of the area occupied by voids in the cross section of the odorant receiving layer 315, the greater the degree to which the sensor element is deformed under the influence of external physical forces, and the lower the durability of the odorant receiving layer 315 against the external physical forces. On the other hand, if the first porosity is low, the amount of deformation due to the adsorption of the odorant is small, and the sensitivity of the sensor element is reduced. Therefore, the first porosity, which indicates the proportion of the area occupied by voids in the cross section of the odorant receiving layer 315, is 3% or more and 20% or less. The first porosity is more preferably 8% or more. Moreover, the first porosity is more preferably 15% or less. Such an odorant receiving layer 315 has excellent durability against external physical forces. In addition, the sensor element 31 having such an odorant receiving layer 315 requires a short time for multiple measurements and is highly convenient.

[0025] The resin (A), the filler (B), and the surfactant (C) will be described later with specific examples.

[0026] <Resin composition> In this specification, "odor substance" refers in a broad sense to a substance that can be adsorbed to the odor substance receiving layer 315. Therefore, it also includes substances that are not generally considered to be the cause of odor. "Odor" often contains multiple odor substances that cause it, and there are also substances that are not recognized as odor substances or unknown odor substances. One embodiment of the present invention focuses on the fact that the amount of odor substance adsorbed to the odor substance receiving layer 315 varies depending on the type of odor substance.

[0027] In addition, even when the term "odor substance" is simply used in this specification, it may mean a "collection of odor substances" that may contain multiple odor substances, rather than an individual odor substance.

[0028] Examples of "odor substances" include, but are not limited to, hexane, ethyl acetate, methanol, diethyl carbonate, toluene, d-limonene, bornan-2-one, cis-3-hexenol, β-phenylethyl alcohol, citral, L-carvone, γ-undecalactone, eugenol, linalyl acetate, menthol, benzaldehyde, vanillin, hexanal, ethanol, pentyl valerate, linalool, and 2-propanol.

[0029] In addition, in this specification, the term "odor substance receiving layer" refers to a layer that adsorbs the odor substance to be recognized. The odor substance receiving layer 315 is formed from the above-mentioned resin composition. The odor substance receiving layer 315 can be provided as a part of the sensor element 31 described below.

[0030] It is believed that the sensor described in the cited document 1 can detect odors consisting of single compounds. On the other hand, many odors are mixtures of multiple substances. The sensor described in the cited document 1 does not have a function to distinguish odor components in the detection unit, so the odor discrimination performance for mixtures is insufficient. In the cited document 2, it is shown that it is possible to recognize odors as mixtures by making the response of the detection unit to various compounds different through each conductive polymer by utilizing the difference in the chemical structure of the conductive polymer used in the detection unit. However, the chemical structure of the conductive polymer is limited, and it is difficult to separate the response of the detection unit to any odor component with high sensitivity, and it is difficult to distinguish between odors consisting of similar components. In the cited document 3, a method is proposed in which a mixture consisting of an organic polymer, a plasticizer, and a conductive substance is used as a detection material in the detection unit, and the penetration of odor components into the organic polymer is detected as a change in the electrical resistance of the mixture. By utilizing the fact that the odor components that penetrate are different when organic polymers of different compositions are used, it is possible to recognize odors as mixtures by using multiple detection units consisting of the above detection material containing organic polymers of different compositions in parallel to form an array. However, in the case of the above organic polymers and organic polymers containing plasticizers, even if multiple combinations of organic polymers and conductive materials are prepared, the difference in chemical properties between the organic polymers is small, so the odor discrimination performance is insufficient. These conventional techniques cannot accurately detect, for example, real odor patterns in which multiple substances interact with each other or real odor patterns caused by substances with unknown compositions.

[0031] The electrical conductivity of the resin composition described above changes depending on the amount of odorant adsorbed to the resin composition. In addition, the adsorption process of odorants to the resin composition described above differs for each odorant. Therefore, by using such a resin composition, the sensor element 31 according to one embodiment of the present invention can improve the odor discrimination performance. For example, it can discriminate a real odor pattern in which multiple substances interact with each other or a real odor pattern caused by a substance whose composition is unknown.

[0032] <Resin (A)> The resin (A) contained in the resin composition according to one embodiment of the present invention is not particularly limited, and may be a urethane resin, a polyalkylene oxide, an acrylic resin, a fluorine-containing resin, a vinyl polymer resin, a silicone resin, a polyamide resin, a polypropylene resin, paraffin wax, a polyester resin, or the like.

[0033] <Filler (B)> The resin composition according to one embodiment of the present invention contains a filler (B). In this specification, the filler (B) is a conductive carbon material, more specifically, a carbon material having a volume resistivity of 0.1 Ω·cm or less. The above-mentioned resin composition is in a state in which the filler (B) is dispersed in the resin (A). The fillers (B) come into contact with each other to form a conductive path, which makes the resin composition conductive.

[0034] Examples of the filler (B) include conductive carbon materials such as carbon black, carbon nanotubes, and graphene, pigments, silica, and metal powders.

[0035] Commercially available carbon black products include Ketjen Black EC (product name of Akzo Co., Ltd., Netherlands), Ketjen Black EC-300J (product name of Lion Specialty Chemicals Co., Ltd.), Ketjen Black EC-600JD (product name of Lion Specialty Chemicals Co., Ltd.), Seast G116, 116 (product names of Tokai Carbon Co., Ltd.), Niteron #10 (product name of Nippon Steel Chemical Co., Ltd.), Denka Black (product name of Denka Co., Ltd.), Toka Black (product name of Tokai Carbon Co., Ltd.), and SUPER C-65 (product name of MTI Corporation, USA).

[0036] Commercially available carbon nanotubes include VGCF-H (product name manufactured by Showa Denko KK).

[0037] Commercially available graphene products include those manufactured by Sigma-Aldrich.

[0038] The conductive carbon material is preferably in the form of fibers or spheres.

[0039] In the case of a fibrous form, the fiber diameter is preferably 0.1 to 10 μm, more preferably 0.1 to 5 μm, and the fiber length is preferably 0.1 to 10 μm, more preferably 1 to 10 μm.

[0040] When it is spherical, the primary particle size is preferably 10 nm to 200 nm, and more preferably 20 nm to 150 nm.

[0041] In addition, the conductive carbon material preferably has a primary particle diameter of 100 nm or less from the viewpoint of conductivity in the resin composition and sensor sensitivity. The particle diameter of the conductive carbon material can be determined by a known method. For example, the particle diameter of the conductive carbon material can be measured by observing with a transmission electron microscope (TEM) and analyzing the image using an image processing device (for example, a digital microscope VHX-700F manufactured by Keyence). When the conductive carbon material is a known or commercially available product, the particle diameter may be a literature value or a catalog value.

[0042] When carbon black is used as the filler (B), the lower the carbon black content, the higher the resistance value of the odorant receiving layer 315 and the lower the elastic modulus. The odorant receiving layer 315 with a lower elastic modulus is more susceptible to deformation under the influence of physical external forces. On the other hand, the higher the carbon black content, the worse the dispersibility of the carbon black in the odorant receiving layer 315 becomes, and the lower the measurement sensitivity of the odorant becomes. Therefore, when the filler (B) is carbon black, the carbon black content in the odorant receiving layer 315 may be preferably 10 to 60% by weight, when the total amount of the resin (A) and the filler (B) is 100% by weight. The carbon black content in the odorant receiving layer 315 may more preferably be 10 to 55% by weight, when the total amount of the resin (A) and the filler (B) is 100% by weight.

[0043] The resin composition may further contain other components other than the above-mentioned resin (A), filler (B) and surfactant (C) within the range in which the effects of the present invention can be obtained. Examples of other components include a solvent (D). The other components can be suitably used within the range in which both the effects of the present invention and the effects of the other components can be obtained.

[0044] The solvent (D) can be blended into the resin composition from the viewpoint of increasing the compatibility between the resin (A) and the filler (B), increasing the dispersibility of the surfactant (C) in the resin composition, or increasing the coatability of the resin composition. Examples of the solvent (D) include N-methylpyrrolidone (hereinafter also referred to as NMP), propylene glycol monomethyl ether acetate, ethyl butyrate, butyl butyrate, ethyl acetate, N,N-dimethylformamide, N,N-dimethylacetamide, toluene, and xylene. The content of the solvent (D) in the resin composition can be determined appropriately.

[0045] <Surfactant (C)> The resin composition according to one embodiment of the present invention may contain a surfactant (C) as described below. The surfactant (C) acts as a dispersant for the filler (B). The surfactant (C) can be appropriately selected from known surfactants within the range in which the resin composition exerts the above-mentioned function.

[0046] The surfactant (C) is not particularly limited, but preferably has an HLB value of 8 to 18, more preferably 9 to 17, and particularly preferably 10 to 16. By using a surfactant (C) having such an HLB value, odor discrimination performance is improved.

[0047] The "HLB value" here is an index showing the balance between hydrophilicity and lipophilicity, and is known as a value calculated by the Oda method described, for example, in "Introduction to Surfactants" [published by Sanyo Chemical Industries, Ltd. in 2007, written by Takehiko Fujimoto], page 212, and is not a value calculated by the Griffin method.

[0048] The HLB value can be calculated from the ratio of the organic value to the inorganic value of an organic compound.

[0049] HLB=10×Inorganic / Organic Here, the inorganic and organic values ​​in the above formula represent index values ​​expressing organic and inorganic properties proposed by Fujita et al., and can be calculated using the values ​​in the table on page 213 of the aforementioned "Introduction to Surfactants."

[0050] Examples of the ionic surfactant include anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants.

[0051] Examples of the anionic surfactant include alkali metal salts of carboxylic acids having 10 to 24 carbon atoms, alkali metal salts of alkylsulfonic acids having 14 to 24 carbon atoms, and amine salts of polyether acid esters.

[0052] Examples of the carboxylic acid having 10 to 24 carbon atoms include decanoic acid, undecanoic acid, dodecanoic acid, tridecanoic acid, tetradecanoic acid, hexadecanoic acid, heptadecanoic acid, octadecanoic acid, pentadecanoic acid, nonadecanoic acid, icosanoic acid, henicosanoic acid, docosanoic acid, tricosanoic acid, and tetracosanoic acid.

[0053] Examples of the alkyl group contained in the alkylsulfonic acid having 14 to 24 carbon atoms include a tetradecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, an octadecyl group, a nonadecyl group, an icosyl group, a henicosyl group, a docosyl group, a tricosyl group, and a tetracosyl group.

[0054] Examples of the alkali metal contained in the alkali metal salt include sodium and potassium.

[0055] Examples of the cationic surfactant include halide salts of quaternary ammonium having an alkyl group having 12 to 24 carbon atoms.

[0056] Examples of the quaternary ammonium having an alkyl group having 12 to 24 carbon atoms include tetrapropylammonium, tetrabutylammonium, tetrapentylammonium, tetrahexylammonium, dimethyldioctylammonium, didecyldimethylammonium, decyltrimethylammonium, dodecyltrimethylammonium, tridecyltrimethylammonium, hexadecyltrimethylammonium, methyltrioctylammonium, octyltrimethylammonium, tributylmethylammonium, octadecyltrimethylammonium, tetradecyltrimethylammonium, nonadecyltrimethylammonium, icosyltrimethylammonium, henicosyltrimethylammonium, heptadecyltrimethylammonium, and pentadecyltrimethylammonium.

[0057] The halide salts include, for example, fluoride salts, chloride salts, bromide salts, and iodide salts.

[0058] Examples of amphoteric surfactants include dimethyl(3-sulfopropyl)ammonium inner salts having an alkyl group with 10 to 22 carbon atoms, and N-alkyl-N,N-dimethylglycines having an alkyl group with 10 to 22 carbon atoms.

[0059] Examples of dimethyl(3-sulfopropyl)ammonium hydroxide inner salts having an alkyl group having 10 to 22 carbon atoms include decyldimethyl(3-sulfopropyl)ammonium hydroxide inner salt, undecyldimethyl(3-sulfopropyl)ammonium hydroxide inner salt, dodecyldimethyl(3-sulfopropyl)ammonium hydroxide inner salt, tridecyldimethyl(3-sulfopropyl)ammonium hydroxide inner salt, tetradecyldimethyl(3-sulfopropyl)ammonium hydroxide inner salt, pentadecyldimethyl(3-sulfopropyl)ammonium hydroxide inner salt, Examples of such ammonium hydroxide inner salt include hexadecyldimethyl(3-sulfopropyl)ammonium hydroxide inner salt, heptadecyldimethyl(3-sulfopropyl)ammonium hydroxide inner salt, octadecyldimethyl(3-sulfopropyl)ammonium hydroxide inner salt, nonadecyldimethyl(3-sulfopropyl)ammonium hydroxide inner salt, icosyldimethyl(3-sulfopropyl)ammonium hydroxide inner salt, henicosyldimethyl(3-sulfopropyl)ammonium hydroxide inner salt, and docosyldimethyl(3-sulfopropyl)ammonium hydroxide inner salt.

[0060] Examples of N-alkyl-N,N-dimethylglycines having an alkyl group having 10 to 22 carbon atoms include N-dodecyl-N,N-dimethylglycine and N-octadecyl-N,N-dimethylglycine.

[0061] Examples of nonionic surfactants include higher alcohol ethylene oxide adducts.

[0062] Examples of higher alcohols include 1-hexyl alcohol, 1-heptyl alcohol, 1-octyl alcohol, 1-nonyl alcohol, 1-decyl alcohol, 1-undecyl alcohol, 1-dodecyl alcohol, 1-tridecyl alcohol, 1-tetradecyl alcohol, 1-pentadecyl alcohol, 1-hexadecyl alcohol, 1-heptadecyl alcohol, and 1-octadecyl alcohol.

[0063] The number of moles of ethylene oxide added is preferably 5 to 50, more preferably 5 to 40, and even more preferably 5 to 30, from the viewpoint of odor discrimination performance.

[0064] The resin (A) and the filler (B) may or may not be compatible with each other.

[0065] The weight ratio of the resin (A) to the surfactant (C) in the resin composition [(A) / (C)] is preferably 4.0 to 50.0 from the viewpoint of the coating stability of the resin composition and the stability of the filler (B) in the resin composition. From the viewpoint of the stability of the filler (B) in the resin composition, the weight ratio (A) / (C) is more preferably more than 4.0, more preferably 4.5 or more, and more preferably 5.0 or more. From the viewpoint of the coating stability of the resin composition, the weight ratio (A) / (C) is more preferably 40.0 or less, more preferably 30.0 or less, and most preferably 20.0 or less.

[0066] <Method of producing resin composition> A specific example of the method for producing a resin composition according to one embodiment of the present invention is as follows.

[0067] The resin composition is obtained as a slurry by mixing the resin (A) and the filler (B) and kneading them uniformly with a stirrer. When mixing the resin (A) and the filler (B), a surfactant (C) and a solvent (D) may be added as necessary. As the stirrer, for example, a centrifugal mixer is used. As the centrifugal mixer, for example, ARE-310 (trade name of Thinky Corporation) or HR003-04A / V (trade name of Samsung Industries Co., Ltd.) can be mentioned. The resin composition is obtained as a slurry having a desired porosity by mixing the resin (A) and the filler (B) and kneading them with a stirrer at a rotation speed of, for example, 2000 rpm and a rotation time of about 10 to 60 minutes. When the surfactant (C) and the solvent (D) are added as necessary to the resin composition, the solvent (D) is distilled off from the resin composition. The solvent (D) may be removed by distillation from a resin composition formed by uniformly mixing, or may be removed by distillation from a coating film formed during the production of the sensor element 31.

[0068] [2. Sensor element 31] The above-mentioned resin composition exhibits different changes in electrical conductivity over time when odorant A is adsorbed to the resin composition than when odorant B, which is different from odorant A, is adsorbed to the resin composition. By utilizing this property, a sensor element 31 capable of detecting and identifying odorants can be realized.

[0069] The outline and effects of a sensor element 31 to which a resin composition according to one embodiment of the present invention is applied will be described below.

[0070] The sensor element 31 includes an odorant receiving layer 315 containing the above-mentioned resin composition, a first metal wiring 313A, a second metal wiring 313B, and an odorant permeable layer 317. In the following description, when there is no need to distinguish between the first metal wiring 313A and the second metal wiring 313B, they may be referred to as metal wiring 313.

[0071] Here, the first metal wiring 313A and the second metal wiring 313B will be described with reference to Fig. 3 and Fig. 4. Fig. 3 is a top view showing an example of the configuration of sensor element 31, and Fig. 4 is a cross-sectional view showing an example of the configuration of sensor element 31 shown in Fig. 3.

[0072] The first metal wiring 313A and the second metal wiring 313B are metal wirings that function as electrodes for measuring changes in the electrical conductivity of the odorant receiving layer 315 (i.e., the resin composition). That is, the first metal wiring 313A and the second metal wiring 313B are spaced apart from each other, and the odorant receiving layer 315 is in contact with at least a portion of the first metal wiring and at least a portion of the second metal wiring. In one example, the first metal wiring 313A and the second metal wiring 313B are metal wirings that are not in direct contact with each other, and may be metal wirings that are approximately parallel to each other, as shown in FIG. 3.

[0073] As shown in FIG. 3, the metal wiring 313 including the first metal wiring 313A and the second metal wiring 313B may be disposed on a substrate 311. The substrate 311 may be a substrate such as glass epoxy generally used for electronic circuits. The substrate 311 is not limited to glass epoxy, and may be a substrate of paper phenol, glass composite, polyimide, PET, glass ceramic, alumina, or aluminum. The metal wiring 313 may be a metal wiring such as copper or gold. The thickness of each of the first metal wiring 313A and the second metal wiring 313B as viewed from a direction perpendicular to the surface of the substrate is preferably 10 μm to 2 mm, and more preferably 10 μm to 1 mm. The height, i.e., thickness, of each of the first metal wiring 313A and the second metal wiring 313B as viewed from a direction parallel to the surface of the substrate is preferably 1 μm to 100 μm, and more preferably 10 μm to 50 μm. The distance between first metal wiring 313A and second metal wiring 313B is preferably 1 μm to 3 mm, and more preferably 1 μm to 1.5 mm. The length of metal wiring 313 is preferably 100 μm to 50 mm, and more preferably 500 μm to 30 mm.

[0074] FIG. 4 shows the AA cross section of FIG. 3. The odorant receiving layer 315 may be in contact with at least a part of the first metal wiring 313A and at least a part of the second metal wiring 313B. The odorant receiving layer 315 is arranged to completely cover the first metal wiring 313A and the second metal wiring 313B, for example, as shown in FIG. 3 and FIG. 4. At least a part of the odorant receiving layer 315 may be a thin film having a thickness of 1 μm to 50 μm. With this configuration, the change in the electrical conductivity of the odorant receiving layer 315 caused by the odorant being adsorbed by the odorant receiving layer 315 can be detected as an electrical signal with high accuracy. In addition, when the odorant receiving layer 315 is produced, the area of ​​the film to be applied is regulated by the electrode shape, etc., and the evaporation residue and the amount of the odor permeation layer solution to be dispensed are controlled, thereby controlling the thickness of the odorant receiving layer 315.

[0075] The maximum peak height of the surface of the odorant receiving layer 315 covered by the odorant permeation layer 317 described below may be 50 μm or less. The surface of the odorant receiving layer 315 covered by the odorant permeation layer 317 is the surface that receives the odorant. If the smoothness of this surface is low, it is difficult to ensure the uniformity of the thickness of the odorant permeation layer 317 arranged to cover the odorant receiving layer 315. As described above, if the maximum peak height of the surface of the odorant receiving layer 315 covered by the odorant permeation layer 317 is 50 μm or less, it becomes easy to apply the odorant permeation layer 317 smoothly to the surface.

[0076] When the electrical conductivity of the odorant receiving layer 315 (ie, the electrical conductivity of the sensor element 31) is low, it is desirable that the distance between the first metal wiring 313A and the second metal wiring 313B be a predetermined distance (eg, 500 μm) or less.

[0077] The sensor element 31 can detect and distinguish various odorants by applying a resin composition that exhibits different changes in electrical conductivity over time when odorant A is adsorbed and when odorant B, which is different from odorant A, is adsorbed. In the odor sensor 30 described later, a plurality of sensor elements 31 each having a substrate 311 provided with a configuration for detecting an odorant (metal wiring 313 and an odorant receiving layer 315) may be arranged. Each substrate 311 may be provided with a plurality of sets including an odorant receiving layer 315 of the same composition. When a plurality of sensor elements 31 are arranged, a constant voltage power supply and a voltmeter are provided for each sensor element 31. In the odor sensor 30, one configuration for detecting an odorant (metal wiring 313 and an odorant receiving layer 315) may be arranged on each substrate 311. Alternatively, in the odor sensor 30, a plurality of sets of a configuration for detecting an odorant (metal wiring 313 and an odorant receiving layer 315) may be arranged on one substrate 311. In the latter case, a constant voltage power supply and a voltmeter are connected to each of the sets provided on the substrate 311.

[0078] The composition of each of the multiple odorant receiving layers 315 included in the odor sensor 30 may be the same or different. When the odor sensor 30 includes odorant receiving layers 315 with the same composition, the same odorant can be detected in each of the multiple odorant receiving layers 315. When the odor sensor 30 includes odorant receiving layers 315 with different compositions, each of the multiple odorant receiving layers 315 responds differently to the odorant. In this way, by providing multiple sets of configurations for detecting odorants, the accuracy of odorant identification in the odor sensor 30 can be improved.

[0079] [3. Odor Sensor 30] The outline and effects of the odor sensor 30 to which the sensor element 31 is applied will be described below with reference to Fig. 5. Fig. 5 is a block diagram showing an example of the configuration of the odor sensor 30 to which the sensor element 31 is applied.

[0080] The odor sensor 30 includes a sensor element 31 that detects odor substances, a constant-voltage power supply 32 (power supply), and a voltmeter 33 (measuring device).

[0081] The first metal wiring 313A and the second metal wiring 313B of the sensor element 31 are connected by a lead wire W. An example in which a constant voltage power supply 32 and a voltmeter 33 are provided on the lead wire W is shown in FIG.

[0082] The constant voltage power supply 32 is a power supply for supplying power to the sensor element 31. The constant voltage power supply 32 supplies a constant voltage via lead wires to the sensor element 31. The voltage value supplied by the constant voltage power supply 32 is 0.5V to 10V, for example, 2.5V.

[0083] The voltmeter 33 measures the potential difference generated between the first metal wiring 313A and the second metal wiring 313B when a constant voltage supplied from the constant voltage power supply 32 is supplied to the odorant receiving layer 315.

[0084] In addition, the odor sensor 30 includes an amplifier (not shown) in front of the voltmeter 33 in the circuit for measuring odor substances, and the amplifier amplifies the acquired signal and supplies it to the voltmeter 33.

[0085] In addition, the odor sensor 30 is equipped with a reference circuit in addition to the circuit for measuring odorous substances, and the voltmeter 33 acquires the difference (potential difference) between the value acquired in the circuit for measuring odorous substances and the value acquired in the reference circuit as a voltage value.

[0086] Although not a required component, the odor sensor 30 may further include a housing 34. The housing 34 is a container capable of containing air containing an odor substance. When the odor sensor 30 includes the housing 34, the sensor element 31 is disposed within the housing 34.

[0087] The housing 34 has an inlet 341 for introducing an odorant and an outlet 342 for discharging air containing the odorant. The odorant may be introduced by introducing filter paper or the like soaked in the odorant into the housing 34 from the inlet 341, or by introducing air containing the odorant into the housing 34 from the inlet 341. The housing 34 is a container for containing air containing the odorant at a predetermined concentration (e.g., 200 ppm) or more.

[0088] Although not essential, an airflow generating fan 35 may be provided at the exhaust port 342 of the housing 34. The airflow generating fan 35 is for generating an airflow inside the housing 34 and discharging the gas inside the housing 34 from the exhaust port 342 to the outside of the housing 34.

[0089] The odor sensor 30 may include a constant current source (power supply) (not shown) instead of the constant voltage power supply 32, and an ammeter (measuring device) (not shown) instead of the voltmeter 33. In this case, the constant current source functions as a power supply for supplying power to the sensor element 31, and applies a constant current to the sensor element 31 via a lead wire. Meanwhile, the ammeter measures the value of the current flowing between the first metal wiring 313A and the second metal wiring 313B when a constant current is applied to the odorant receiving layer 315. Both the first metal wiring 313A and the second metal wiring 313B can function as electrodes. Hereinafter, when the metal wiring 313 functions as an electrode, it may be referred to as "electrode 313".

[0090] The odor sensor 30 outputs a measurement value that indicates the change over time in the electrical conductivity of the sensor element 31 before and after an odor substance is adsorbed to the sensor element 31. This makes it possible to detect and identify various odor substances.

[0091] 4. Odor measuring device 100 The odor sensor 30 described above can output the change over time in the electrical conductivity of the sensor element 31 for each odor substance when various odor substances are adsorbed to the sensor element 31. By applying this odor sensor 30, it is possible to compare the change over time in the electrical conductivity of the sensor element 31 when odor substance A is adsorbed to the sensor element 31 with the change over time in the electrical conductivity of the sensor element 31 when odor substance B is adsorbed to the sensor element 31. Based on such a comparison result, it is possible to realize an odor measurement device 100 that can estimate the odor substance adsorbed to the sensor element 31.

[0092] Furthermore, the odor measuring device 100 can estimate odor substances with high accuracy by using the estimation model 22 generated by machine learning. The estimation model 22 can be generated using learning data including a combination of measurement values ​​measured when each of a plurality of odor substances is adsorbed to at least one sensor element 31, and identification information unique to the odor substance that provided the measurement value.

[0093] The following describes the outline and effects of an odor measuring device 100 that uses the odor sensor 30. The odor measuring device 100 is a device that estimates the odor substance adsorbed to a sensor element 31 based on a change in electrical conductivity that occurs in the sensor element 31 to which the above-mentioned resin composition is applied.

[0094] The odor measuring device 100 of this embodiment is separately provided with a sensor chamber 60 including a plurality of sensor elements 31A (hereinafter also referred to as a "sensor element group 31A"), and a target sample receiving section 50 into which a target sample containing an odorant is introduced and into which gas containing the odorant generated from the target sample is enclosed. In this embodiment, each sensor element 31 included in the sensor element group 31A will be simply referred to as a "sensor element 31".

[0095] The odor measuring device 100 of this embodiment employs a configuration in which the gas containing an odorant inside the target sample receiving section 50 and a gas other than the gas containing the odorant are used to push the gas toward the sensor chamber 60. In this embodiment, the gas inside the target sample receiving section 50 when the target sample is introduced into the target sample receiving section 50 (i.e., the gas containing the odorant to be detected) is referred to as the first gas. Meanwhile, the gas for pushing the first gas toward the sensor chamber 60 is referred to as the second gas.

[0096] Fig. 1 is a schematic diagram of an odor measurement device 100. As shown in Fig. 1, the odor measurement device 100 includes an odor sensor 30, a target sample receiving section 50, a sensor chamber 60, a gas supply section 80, and an estimation device 10. The odor measurement device 100 may further include an adjustment section 51. The odor measurement device 100 may further include an estimation device 10a.

[0097] 1 shows, as an example, an example in which gas flows from gas supply unit 80 to target sample receiving unit 50 and sensor chamber 60 in that order. Gas supply unit 80, target sample receiving unit 50, and sensor chamber 60 are each connected by a tube.

[0098] [Target sample receiving section 50] The target sample receiving section 50 can receive a target sample containing an odorant and hold a first gas. The target sample receiving section 50 has a first port 501 through which the second gas entering the inside passes, and a second port 502 through which the first gas and the second gas leaving the inside can pass. In FIG. 1, the first port 501 is installed at the upper part of the target sample receiving section 50 and the second port 502 is installed at the lower part of the target sample receiving section 50, but is not limited to this. For example, the positions of the first port 501 and the second port 502 can be appropriately set depending on the type and combination of odor components contained in the first gas. For example, the positions of the first port 501 and the second port 502 may be changed depending on whether the weight per unit volume of the odor components contained in the first gas (i.e., specific gravity) is heavier or lighter than that of the second gas. Furthermore, the target sample receiving section 50 may include an airflow generating fan 35 therein, as in FIG.

[0099] The target sample receiving section 50 includes a sample inlet 503 for receiving a liquid or solid target sample. The target sample receiving section 50 may include a placement section (not shown) for placing the target sample. When the target sample is liquid, the placement section may be a cup for holding the liquid, and when the target sample is solid, the placement section may be a petri dish on which the solid is placed. The target sample may be introduced into the target sample receiving section 50 in a gaseous state as a first gas from the sample inlet 503. In this way, since the target sample receiving section 50 can receive a liquid or solid target sample, it is possible to adjust the concentration of the odorant in the first gas. For example, even if the odorant is the same, it is easy to adjust the concentration of the odorant in the first gas.

[0100] A material inactive to odorants may be disposed on the inner surface of the target sample receiving portion 50. A material inactive to odorants is a material that does not significantly change the concentration of each odorant contained in the gas sent to the sensor chamber 60. For example, a material inactive to odorants is a material in which odorants are unlikely to be adsorbed or dissolved. Examples of materials inactive to odorants include glass, metal, and resin. When metal is used, stainless steel (SUS) is preferable, and when resin is used, fluorine-based resin, polypropylene (PP), polyethylene (PE), ABS resin, and polyethylene terephthalate (PET) are preferable.

[0101] If the inner surface of target sample receiving portion 50 is made of a material that adsorbs odorous substances contained in the first gas, the odorous substances may be adsorbed to various portions, which may affect subsequent measurements.

[0102] In this way, the inner surface of the target sample receiving portion 50 is made of a material that is inactive against odorants, thereby reducing the risk that the material of the inner surface will react with the odorants contained in the first gas, or that the odorants will be adsorbed onto the inner surface. This reduces the risk that the odorants contained in the first gas supplied to the sensor chamber 60 will change while contained in the target sample receiving portion 50, or that the concentration of the odorants will be diluted.

[0103] Even if the target sample is a liquid or solid, the odor measurement device 100 is provided with the target sample receiving section 50, thereby making the concentration of the first gas uniform in the target sample receiving section 50 before the first gas is sent to the sensor chamber 60. Furthermore, by providing the target sample receiving section 50, the odor measurement device 100 is able to push the first gas into the sensor chamber 60 at a constant flow rate. As a result, even when measurements are repeated, the odor measurement device 100 can send the first gas to the sensor chamber 60 under the same conditions each time, thereby enabling repeated and stable measurements to be performed.

[0104] The volume of the target sample receiving section 50 is preferably 1 to 200 times the volume of the sensor chamber 60. In particular, the volume of the target sample receiving section 50 is preferably larger than the volume of the sensor chamber 60. The volume of the target sample receiving section 50 is more preferably 2 or more times the volume of the sensor chamber 60, and more preferably 4 or more times. In addition, the volume of the target sample receiving section 50 is preferably 100 or less times the volume of the sensor chamber 60, and more preferably 60 or less times. By having the volume of the target sample receiving section 50 be 1 or more times the volume of the sensor chamber 60, the concentration of the odor substance in the sensor chamber 60 is appropriately adjusted, and the measurement result by the sensor provided in the sensor chamber 60 is stably output. In addition, by having the volume of the target sample receiving section 50 be 200 or less times the volume of the sensor chamber 60, it is easy to adjust the temperature and humidity in the target sample receiving section 50, so that the measurement result by the sensor is stably output and the size of the odor measuring device 100 can be kept compact.

[0105] If the volume of the target sample receiving section 50 is less than one time the volume of the sensor chamber 60, the odorant generated in the target sample receiving section 50 may be diluted in the sensor chamber 60, and the measurement sensitivity of the sensor may decrease. If the volume of the target sample receiving section 50 is more than 200 times the volume of the sensor chamber 60, the volume of the target sample receiving section 50 is too large, so the uniformity of the concentration, temperature, and humidity of the first gas may decrease, and when measurements are repeated, the first gas may not be sent to the sensor chamber 60 under the same conditions. Furthermore, the overall size of the odor measuring device 100 may become large.

[0106] FIG. 1 shows an example in which the volume of the target sample receiving portion 50 is eight times the volume of the sensor chamber 60 .

[0107] For example, if the inner surface of the tube 93 is made of a material that adsorbs odorous substances contained in the first gas, the odorous substances may be adsorbed to various parts, which may affect the subsequent measurement. Therefore, it is preferable that a material that is inactive to odorous substances is arranged on the inner surface of the tube 93 that guides the first gas from the target sample receiving section 50 to the sensor chamber 60, similar to the inner surface of the target sample receiving section 50. Examples of materials that are inactive to odorous substances include glass, metal, and resin. When metal is used, stainless steel (SUS) is preferable, and when resin is used, fluorine-based resin, polypropylene (PP), polyethylene (PE), ABS resin, and polyethylene terephthalate (PET) are preferable.

[0108] The target sample receiving section 50 may be configured to be detachable from the tubes 92 and 93. In this manner, since the target sample receiving section 50 is detachable, when the previous measurement is completed and the next measurement is to be performed, a new target sample receiving section 50 can be attached without purging the inside of the target sample receiving section 50. This allows the odor measuring device 100 to perform multiple measurements in a short period of time.

[0109] Furthermore, because the target sample receiving section 50 is detachable, the target sample receiving section 50 into which the target sample has been introduced can be maintained at a desired temperature using a heat retention chamber separate from the odor measurement device 100. This allows the odor measurement device 100 to adjust the temperature of the target sample receiving section 50, even if it is not possible to provide the adjustment section 51 described below in the odor measurement device 100. As the heat retention chamber, for example, a water bath, a dry bath, a heat jacket, a silicon heater, a forward air dryer, a thermo-hygrostat, a sprayer, or the like may be used.

[0110] [Adjustment section 51] The adjustment unit 51 adjusts at least one of the temperature and humidity of the first gas contained in the target sample receiving section 50. When the adjustment unit 51 adjusts the temperature, the adjustment unit 51 is, for example, a heater or a cooler. In this case, the adjustment unit 51 may be configured to cover the entire target sample receiving section 50. When the adjustment unit 51 adjusts the humidity, the adjustment unit 51 is, for example, a humidifier or a dehumidifier. The adjustment unit 51 may adjust at least one of the temperature and humidity for each type of first gas, or may change at least one of the temperature and humidity at predetermined time intervals during measurement of the same first gas. As the adjustment unit 51, for example, a water bath, a dry bath, a heat jacket, a silicon heater, a wind dryer, a thermohygrostat, a sprayer, or the like capable of changing at least one of the temperature and humidity may be used.

[0111] By the adjustment section 51 adjusting at least one of the temperature and humidity of the first gas in the target sample receiving section 50, the odor measuring device 100 can send the first gas to the sensor chamber 60 using conditions according to, for example, the type of the first gas (weight of the gas, volatility, etc.). Furthermore, this allows the odor measuring device 100 to send the first gas at a stable concentration to the sensor chamber 60, improving the measurement accuracy.

[0112] [Sensor Chamber 60] The sensor chamber 60 is a space for storing the sensor element 31 for measuring odor substances. The sensor chamber 60 is connected to the second port 502 of the target sample receiving portion 50. Specifically, the sensor chamber 60 includes a gas supply port 601 and a gas exhaust port 602, and the second port 502 of the target sample receiving portion 50 is connected to the gas supply port 601.

[0113] The sensor chamber 60 includes a plurality of sensor elements 31A capable of outputting a measurement result according to an odor substance contained in the first gas. The plurality of sensor elements 31A may be sensor elements 31 each having a different resin composition as a substance receiving layer. That is, the plurality of sensor elements 31A may have different sensitivities and specificities to the odor substance. The sensor chamber 60 in FIG. 1 includes, as an example, a sensor element 31 and a sensor element 31b, but is not limited thereto. The sensor chamber 60 in FIG. 1 also includes a sensor element 31c having a resin composition different from the sensor elements 31 and 31b as a substance receiving layer. The sensor element 31 and the sensor element 31b are capable of outputting a measurement result according to the same odor substance contained in the first gas, but the measurement results output by each of them are different. The measurement result according to the odor substance is, for example, a measurement result according to the concentration of the odor substance. In the following description, when there is no particular distinction between the sensor elements 31, 31b, 31c and the sensor element 31d described later, they are collectively referred to as "sensor element 31".

[0114] The sensor elements 31 each having a different resin composition as a substance receiving layer may be installed in any combination and arrangement in the sensor chamber 60. Furthermore, the sensor chamber 60 may be installed with a plurality of sensor elements 31 each having the same resin composition as a substance receiving layer.

[0115] Here, the sensor element 31 and the sensor element 31b may be sensor elements capable of outputting measurement results corresponding to different odor substances. For example, the sensor chamber 60 may be provided with a sensor element 31 capable of outputting measurement results corresponding to an odor substance contained in a first gas, and a sensor element 31b capable of outputting measurement results corresponding to a second odor substance different from the odor substance contained in the first gas. For example, the odor sensor 30 may include sensor elements 31 and 31b having different resin compositions used in the odor substance receiving layer 315.

[0116] By providing multiple sensor elements 31 in which resin compositions with different odorant adsorption properties are used in the odorant receiving layer 315, the odor measuring device 100 can simultaneously perform estimations for multiple odorants. Note that as a sensor element 31 according to one embodiment of the present invention, a sensor element 31 that does not contain a surfactant (C) in the odorant receiving layer 315 and a sensor element 31 that contains a surfactant (C) in the odorant receiving layer 315 may be used in combination.

[0117] Furthermore, by using the odor measurement device 100, it is possible to obtain a first change pattern indicating a change in the electrical conductivity of the sensor element 31 and a second change pattern indicating a change in the electrical conductivity of the sensor element 31b for each known odor substance. The estimation model 22 may be generated by machine learning using both the first change pattern and the second change pattern. The odor measurement device 100 estimates odor substances using the estimation model 22 generated in this way, and therefore is able to more precisely identify each odor substance.

[0118] 1 includes a plurality of sensor elements 31A arranged in a 4×4 array, as an example. The number of sensor elements 31A and the manner in which the sensor elements 31A are arranged are not limited. The total number of sensor elements 31A included in the sensor chamber 60 is also not particularly limited, and may be, for example, 2, 8, 16, or 64. The total number of sensor elements 31A may be 8 or more and 16 or less.

[0119] The material of the inner surface of the sensor chamber 60 is preferably a material that is inactive to odorants, similar to the target sample receiving section 50. Examples of materials that are inactive to odorants include glass, metal, and resin. When metal is used, stainless steel (SUS) is preferable, and when resin is used, fluororesin, polypropylene (PP), polyethylene (PE), ABS resin, and polyethylene terephthalate (PET) are preferable. When the material of the inner surface of the sensor chamber 60 is a material that adsorbs odorants contained in the first gas, the odorants adsorbed in the sensor chamber may reduce the amount of change in output from the sensor element 31 in a subsequent measurement, and the odor measuring device 100 may not be able to perform an accurate measurement.

[0120] [Multiple sensor elements 31A (sensor element group 31A)] The sensor elements 31A may include a thin film. As an example, the odorant receiving layer 315 and the odorant permeable layer 317 in FIG. 3 and FIG. 4 are thin films.

[0121] As an embodiment for sending the first gas containing an odorant into the sensor chamber 60, for example, a vacuum pump may be installed on the gas exhaust port 602 side of the sensor chamber 60, and the gas may be drawn using the vacuum pump to send the odorant into the sensor chamber 60 from the gas supply port 601 side of the sensor chamber 60. However, if the sensor elements 31 and 31b have a thin film, the thin film may expand if the pressure inside the sensor chamber 60 is negative, and the sensor elements 31 and 31b may not be able to output a stable measurement result. In the odor measurement device 100 according to this embodiment, the gas supply unit 80 pushes the gas from the first port 501 side of the sensor chamber 60 and the target sample receiving unit 50 to send the first gas into the sensor chamber 60, so the pressure inside the sensor chamber 60 is positive. Therefore, the odor measurement device 100 can obtain a stable measurement result even if multiple sensor elements 31A have thin films. In contrast, if the gas supply unit 80 sends the first gas into the sensor chamber 60 by pushing the gas from the sensor chamber 60 and the first port 501 side of the target sample receiving unit 50, the pressure inside the sensor chamber 60 will be positive. Therefore, it is preferable for the odor measurement device 100 according to this embodiment to adopt a configuration in which the gas supply unit 80 sends the first gas into the sensor chamber 60 by pushing the gas from the sensor chamber 60 and the first port 501 side of the target sample receiving unit 50. This allows the odor measurement device 100 to obtain stable measurement results even if multiple sensor elements 31A are equipped with thin films.

[0122] The thin film of the plurality of sensor elements 31A may also contain a filler, a resin composition, and a surfactant.

[0123] [Gas supply unit 80] The gas supply unit 80 is connected to the first port 501 of the target sample receiving portion 50, and by sending a second gas into the inside of the target sample receiving portion 50, the first gas is sent from within the target sample receiving portion 50 toward the sensor chamber 60.

[0124] A valve 81 may be provided between the gas supply unit 80 and the target sample receiving unit 50. By opening and closing the valve 81, start and stop of gas supply from the gas supply unit 80 may be adjusted.

[0125] In this way, the gas supply unit 80 pushes the gas from the first port 501 side of the target sample receiving unit 50 to send the first gas into the sensor chamber 60, so the pressure inside the sensor chamber 60 is positive. This allows the odor measurement device 100 to obtain stable measurement results. In addition, since the second gas can be sent by opening and closing the valve 81, the odor measurement device 100 can send the first gas from the target sample receiving unit 50 toward the sensor chamber 60 at any timing. This allows the odor measurement device 100 to improve the reproducibility of the waveform shape output by each sensor element 31 when repeatedly measuring odor substances contained in the first gas using the sensor element group 31A.

[0126] The second gas may be an inert gas or air. Examples of the inert gas include argon and nitrogen. When the second gas is an inert gas, the gas supply unit 80 may be a gas cylinder.

[0127] Furthermore, when the second gas is air, the gas supply unit 80 may be a pump. In this case, in order to remove components that react with the first gas contained in the target sample receiving unit 50, the odor measuring device 100 may be provided with, for example, an activated carbon filter, a dehumidifier, a silica gel column, or a dust filter on the first port 501 side of the target sample receiving unit 50.

[0128] The odor measuring device 100 may further include a mass flow controller on the side of the first port 501 of the target sample receiving section 50, more specifically, between the valve 81 and the gas supply section 80. The odor measuring device 100 employing this configuration can send the first gas from the target sample receiving section 50 to the sensor chamber 60 at a constant flow rate, and the multiple sensor elements 31A can provide stable outputs.

[0129] 1 shows a configuration in which the first gas and the second gas leaving the inside of the target sample receiving part 50 pass through the tube 93 and the sensor chamber 60, but the configuration is not limited to this. Since the target sample receiving part 50 of the odor measurement device 100 has a larger volume than the sensor chamber 60, it is not necessary to send the entire amount of the first gas inside the target sample receiving part 50 to the sensor chamber 60 during measurement. Furthermore, when the inside of the target sample receiving part 50 is purged with the second gas after the measurement, it is not necessary for the target sample receiving part 50 and the sensor chamber 60 to be connected. Therefore, the odor measurement device 100 may be configured such that a valve (not shown) is arranged in the tube 93 so that the first gas and the second gas leaving the inside of the target sample receiving part 50 can be exhausted without passing through the sensor chamber 60.

[0130] [Estimation device 10] The estimation device 10 is a device that estimates an odor substance detected by the odor sensor 30. The estimation device 10 is, for example, a computer, and includes a CPU and a memory (not shown). The estimation device 10 is connected to the odor sensor 30 so that it can communicate with the odor sensor 30. Specifically, the estimation device 10 performs estimation of the odor substance by analyzing the measurement value acquired from the odor sensor 30. If the sensor chamber 60 further includes a sensor element 31c in which a resin composition different from that of the sensor element 31 and the sensor element 31b is used in the substance receiving layer 315, the estimation device 10 may further acquire and analyze a measurement value measured by a voltmeter by supplying a constant voltage to the sensor element 31c. The estimation device 10 may also display the measurement value itself, a waveform in which the measurement value is plotted, and an estimation result of an unknown odor substance based on an estimation model. The estimation device 10 may also display a numerical value and a graph indicating the change in the presence ratio of each odor substance for a gas containing multiple odor substances. The estimation device 10 may also generate an estimation model 22 used to estimate an odor substance.

[0131] <Generation of Estimation Model 22> Next, the configuration of the odor measuring device 100 that performs the process of generating the estimation model 22 used to estimate odor substances, and the process of generating the estimation model 22 will be described with reference to FIGS. 6 and 7. FIG.

[0132] The estimation model 22 is generated by machine learning using learning data including a combination of measurement values ​​measured by the voltmeter 33 when each of a plurality of odor substances is adsorbed to at least one sensor element 31, and identification information unique to the odor substance that gave the measurement value. Here, the identification information unique to the odor substance may be, for example, the name, CAS number, and chemical formula of the odor substance.

[0133] (Configuration of the Estimation Device 10 (Generation of Estimation Model 22)) Fig. 6 is a functional block diagram showing an example of the configuration of the odor measuring device 100. For ease of explanation, the same reference numerals are given to members having the same functions as those described in Fig. 1, and the explanation thereof will not be repeated.

[0134] As shown in FIG. 6, the estimation device 10 includes an input unit 15, a control unit 1, and a storage unit 2.

[0135] The input unit 15 is for accepting various input operations from a user, and may be, for example, a keyboard, a mouse, a touch panel, or the like.

[0136] The control unit 1 includes a measurement value acquiring unit 11 (acquiring unit), a change pattern analyzing unit 12 (analyzing unit), a learning control unit 13, and an estimation model generating unit .

[0137] The measurement value acquiring unit 11 acquires a measurement value from the voltmeter 33. Furthermore, the measurement value acquiring unit 11 uses the acquired measurement value to calculate a value (e.g., resistance value, impedance, etc.) indicating the electrical conductivity of the sensor element 31. The measurement value acquiring unit 11 may acquire the measurement value from the voltmeter 33 at a predetermined time interval (e.g., 0.1 second interval).

[0138] The change pattern analysis unit 12 analyzes the change over time in the electrical conductivity of at least one sensor element 31. Using the resistance value calculated by the measurement value acquisition unit 11, the change pattern analysis unit 12 calculates a value indicating the amount of change in the electrical conductivity of the sensor element 31 due to the adsorption of an odorant. The change pattern analysis unit 12 generates data indicating a change pattern indicating the time change in the calculated amount of change in electrical conductivity. When the generated change pattern is a known odorant, the change pattern analysis unit 12 may store the generated change pattern in the change pattern database 21 (learning data) in association with identification information specific to the known odorant.

[0139] The learning control unit 13 reads out the change pattern database 21 from the storage unit 2 and controls the generation of the estimation model 22 by machine learning. Here, the change pattern database 21 is a database that includes combinations of measurement values ​​measured when multiple odor substances are adsorbed to the sensor element 31 and identification information unique to the known odor substances that provided the measurement values. The learning control unit 13 inputs the change pattern read out from the change pattern database 21 to the estimation model generation unit 14. In addition, the learning control unit 13 compares the identification information of the odor substance corresponding to the change pattern input to the estimation model generation unit 14 with the estimation result output from the estimation model generation unit 14, and outputs a correction instruction according to the comparison result to the estimation model generation unit 14.

[0140] The estimation model generation unit 14 generates the estimation model 22 by a machine learning algorithm using the change patterns stored in the change pattern database 21. The estimation model generation unit 14 may be configured to generate the estimation model 22 by using a known supervised machine learning algorithm. Examples of machine learning algorithms that can be applied to the estimation model generation unit 14 include the k-nearest neighbor method, logistic regression, support vector machine, random forest, and neural network.

[0141] Feature extraction method When generating an estimation model by machine learning, the data on which the model is based may be the measurement value itself, or may be data extracted from the feature of the measurement value, such as a statistical quantity of the measurement value, a differential integral value, a peak detection value, or an autocorrelation value. Examples of the statistical quantity include an average value, a variance value, a maximum value, a minimum value, a difference between a maximum value and a minimum value, and a standard deviation. Examples of the differential integral include a slope and an area. Examples of the peak detection value include the number of peaks and the height. Examples of the autocorrelation value include a step difference.

[0142] Pretreatment method When generating an estimation model by machine learning, the base data may be used for machine learning as it is, or the base data may be pre-processed as necessary. When pre-processing is performed, the pre-processing may be performed before feature extraction, after feature extraction, or both before and after feature extraction. The pre-processing may be performed by a known method, and may include correction, noise removal, standardization, data conversion, smoothing, data expansion, and other methods. Correction may be performed based on the measurement results of multiple elements, commercially available sensors (for example, temperature sensors, humidity sensors, and the like), and standard gases. For example, correction may be performed by output ratio calculation, independent component analysis (ICA), statistical calculation, integration, addition, subtraction, division, and other methods. Examples of noise removal include removal of outliers and white noise. Examples of standardization include normalization and regularization. Examples of data transformation include trend removal, frequency conversion, logarithmic conversion, and the like. Examples of smoothing include moving average, difference, and the like. Examples of data augmentation include adding the same sample data (for example, assuming a normal distribution) and adding new sample data (for example, adding using a vector mixture ratio).

[0143] Machine learning algorithms Machine learning algorithms applicable to the estimation model generation unit 14 include regression analysis, classification, tree, time series analysis, neural network, clustering, etc. Examples of regression analysis include logistic regression, Lasso, elastic net, support vector regression (SVR), linear, Ridge, ensemble regression, etc. Examples of classification include k-nearest neighbor method, support vector classification (SVC), Naibe Bayes classifier, stochastic gradient descent (SGD), kernel approximation, etc. Examples of trees include decision trees, regression trees, random forests, boosting (lightGBM, XGboost), stacking, etc. Examples of time series include AR, MA, ARIMA, state space, etc. Examples of neural networks include multi-layer perceptrons (MLPs), convolutional neural networks (CNNs), recurrent neural networks (RNNs), residual neural networks (ResNets), transformers, graph neural networks (GNNs), etc. Examples of clustering include Gaussian mixture models (GMMs), k-means methods (kmeas), minikmeans, variational Gaussian mixture models (VBGMMs), kernel approximations, etc.

[0144] (Process for generating estimation model 22) The process of generating the estimation model 22 using the odor measurement device 100 will be described below with reference to Fig. 7. Fig. 7 is a flow chart showing an example of the process flow in which the estimation device 10 of the odor measurement device 100 generates the estimation model 22. The estimation model 22 is generated by machine learning using learning data including a combination of measurement values ​​measured by the voltmeter 33 when each of a plurality of odor substances is adsorbed to at least one sensor element 31, and identification information unique to the odor substance that gave the measurement value. Here, the identification information unique to the odor substance may be, for example, the name, CAS number, and chemical formula of the odor substance.

[0145] First, the measurement value acquiring unit 11 acquires the voltage value V0 measured by the odor sensor 30 before the odor substance is introduced into the target sample receiving unit 50, and calculates the resistance value R0. The resistance value R0 is preferably 500 to 3000 Ω, more preferably 800 to 2800 Ω, and most preferably 1000 to 2500 Ω. Then, the odor substance is introduced into the target sample receiving unit 50 (step S1).

[0146] Meanwhile, the input unit 15 receives an input of the name of the known odor substance introduced into the target sample receiving unit 50 (step S2). The process of step S2 may be performed before step S1.

[0147] Next, the measurement value acquiring unit 11 acquires data (waveform or pattern of change over time) of the amount of change (ΔV) in the voltage value V before and after the odor substance is adsorbed and desorbed to the sensor element 31 (step S3).

[0148] Next, the change pattern analysis unit 12 associates the change (ΔV) data (waveform or change pattern over time) in the voltage value V before and after the odor substance adsorption and desorption with the name of the input known odor substance and stores it in the change pattern database (step S4).

[0149] If no change pattern has been stored for a given type of existing odor substance (NO in step S5), that is, if there is still insufficient data to use for machine learning, the process returns to step S1.

[0150] If a change pattern is stored for a predetermined type of existing odor substance (YES in step S5), the learning control unit 13 reads out the change pattern for the known odor substance stored in the change pattern database 21 and inputs it to the estimation model generation unit 14. The estimation model generation unit 14 generates an estimation model 22 by machine learning based on the time-dependent change pattern (or feature amount extracted from the change pattern) stored in the change pattern database 21 (step S6).

[0151] The estimation model generating unit 14 stores the estimation model 22 generated by a predetermined machine learning in the storage unit 2 (step S7).

[0152] 6 and 7, the estimation device 10 generates the estimation model 22, but is not limited to this. For example, the estimation device 10 may provide an external computer different from the estimation device 10, which has the same functions as the learning control unit 13 and the estimation model generation unit 14, with the same data as the change pattern database 21 to generate the estimation model 22.

[0153] <Identification of odor substances> Next, the configuration of the odor measuring device 100a that estimates an odor substance using the estimation model 22 and the estimation process will be described with reference to FIGS.

[0154] (Configuration of Estimation Device 10a (Execution of Estimation Process)) Fig. 8 is a functional block diagram showing an example of the configuration of an odor measuring device 100a. For ease of explanation, the same reference numerals are given to members having the same functions as those described in Fig. 1 and Fig. 6, and the description thereof will not be repeated.

[0155] As shown in Fig. 8, the estimation device 10a includes a control unit 1a, a storage unit 2a, and an output unit 18. Here, Fig. 8 shows a configuration example in which the estimation device 10 shown in Fig. 6 is used for odor substance estimation processing. That is, the estimation device 10 shown in Fig. 6 and the estimation device 10a shown in Fig. 8 may be computers having the same hardware configuration.

[0156] The output unit 18 is for presenting the estimation result to the user, and may be, for example, a display, a speaker, a lamp, or the like.

[0157] The control unit 1 a includes a measurement value acquiring unit 11 (acquiring unit), a change pattern analyzing unit 12 (analyzing unit), an estimating unit 16, and an output control unit 17.

[0158] The estimation unit 16 uses the estimation model 22 to estimate the odor substance from the analysis results obtained by analyzing the measurement values ​​obtained from the odor sensor 30.

[0159] The output control unit 17 controls the output unit 18 to output the estimation result.

[0160] (Estimation process) Hereinafter, specific processing performed by each part of the control unit 1a will be described with reference to Fig. 9. Fig. 9 is a flow chart showing an example of the flow of processing performed by the estimation device 10a to estimate an odor substance.

[0161] First, the measurement value acquiring unit 11 acquires the voltage value V0 measured by the odor sensor 30 before the odor substance is introduced into the target sample receiving unit 50, and calculates the resistance value R0. After that, an unknown odor substance (regardless of its properties) is introduced into the target sample receiving unit 50 (step S11).

[0162] Next, the measurement acquisition unit 11 acquires data (waveform or pattern of change over time) of the change (ΔV) in the voltage value V before and after the adsorption and desorption of the unknown (i.e., the target) odor substance to the sensor element 31 (step S12).

[0163] Next, the estimation unit 16 estimates the unknown odor substance from the time-dependent change pattern (or the feature amount extracted from the change pattern) based on the estimation model 22 (step S13).

[0164] The output control unit 17 controls the output unit to output the estimation result (step S14).

[0165] In the above embodiment, the estimation device 10 that generates the estimation model 22 and the estimation device 10a that estimates odor substances using the estimation model 22 have been described. Note that the estimation device 10 and the estimation device 10a may be separate devices or may be a single device.

[0166] <Configuration example of sensor element 31c> FIG. 10 is a top view showing an example of the configuration of one sensor element 31c included in the sensor element group 31A. The sensor element 31c includes an electrode 313, which is a metal wiring arranged on the substrate 311, and a circular odorant receiving layer 315c formed on the electrode 313. The electrode 313 includes a first metal wiring 313C and a second metal wiring 313D. The first metal wiring 313C and the second metal wiring 313D are metal wirings that function as electrodes for measuring changes in the electrical conductivity of the odorant receiving layer 315c. In FIG. 10, the metal wiring 313a and the metal wiring 313d are arranged on the front side of the substrate 311 (i.e., the front side of the paper) and are in contact with the odorant receiving layer 315c. On the other hand, the metal wiring 313b and the metal wiring 313c are connected to the metal wiring 313a and the metal wiring 313d, respectively, on the front side of the substrate 311 and penetrate the substrate 311 toward the back side. Therefore, the metal wiring 313b and the metal wiring 313c are not in contact with the odorant receiving layer 315c. The diameter R of the odorant receiving layer 315c is 0.2 mm or more and 5 mm or less. In FIG. 10, the shape of the odorant receiving layer 315c provided in the sensor element 31c is elliptical as an example, but is not limited to this. When the shape of the odorant receiving layer 315c is elliptical, the average of the minor axis and the major axis may be 0.2 mm or more and 5 mm or less. The shape of the odorant receiving layer 315c may also be a perfect circle.

[0167] As shown in FIG. 10, the metal wiring 313a and the metal wiring 313d are in contact with the odorant receiving layer 315c but are not in contact with the odorant permeable layer 317.

[0168] 11 is a top view showing an example of the configuration of one sensor element 31d included in the sensor element group 31A. The sensor element 31d comprises an electrode 313 (first metal wiring 313C, second metal wiring 313D) arranged on the substrate 311, and a strip-shaped odorant receiving layer 315d formed on the electrode 313. The length W of the short width of the odorant receiving layer 315d is 0.2 mm or more and 5 mm or less. In the following description, when there is no particular distinction between the odorant receiving layers 315c and 315d, they will be collectively referred to as "odorant receiving layer 315."

[0169] The electrodes of the sensor elements 31 included in the sensor element group 31A each have a first electrode and a second electrode, and the first and second electrodes may be arranged in parallel lines, parallel curves, a comb shape, or a concentric circle shape. Regardless of which shape is adopted, the first and second electrodes are preferably arranged in line symmetry or point symmetry with each other. By arranging the first and second electrodes in this way, the odor measuring device 100 can measure odor substances contained in the gas with high accuracy.

[0170] The sensor element 31c in FIG. 10 has a first metal wiring 313C and a second metal wiring 313D. As an example, the first metal wiring 313C is a first electrode composed of a metal wiring 313a and a metal wiring 313b, and the two metal wirings are arranged in a T-shape so as to be perpendicular to each other. The second metal wiring 313D is a second electrode composed of two metal wirings 313c and 313d like the first metal wiring 313C, and is configured so as to be arranged in a T-shape so as to be perpendicular to each other. The first metal wiring 313C and the second metal wiring 313D are arranged in parallel lines so that the metal wiring 313a and the metal wiring 313c face each other.

[0171] The first metal wiring 313C and the second metal wiring 313D are arranged in a T-shape, so that the first metal wiring 313C and the second metal wiring 313D can be arranged at a suitable distance, and the resistance value of the electrodes can be stabilized. For example, if the electrodes are arranged in a comb shape, the distance between the electrodes is short, and the resistance value of the electrodes may become too small. In addition, since the first metal wiring 313C and the second metal wiring 313D are arranged in a T-shape, in the application process of the manufacturing method of the sensor element 31 described later, there is no uneven part of the electrode that can hinder the slurry from spreading in the area where the slurry spreads, so the slurry spreads easily. In addition, since the slurry spreads easily, the thickness of the odorant receiving layer 315 after drying is uniform.

[0172] 12 is a perspective view showing an example of the configuration of one sensor element 31c included in the sensor element group 31A. As shown in FIG. 12, in the sensor element 31c, the first metal wiring 313C and the second metal wiring 313D are connected to pins 316 at the ends where the first metal wiring 313C and the second metal wiring 313D do not face each other. The pins 316 are conductive members for electrically connecting the first metal wiring 313C and the second metal wiring 313D to other members of the odor sensor 30. Although not shown, the sensor elements 31c and 31d shown in FIG. 10 and FIG. 11 also include the pins 316 shown in FIG. 12.

[0173] <Method of manufacturing sensor element 31> The following describes a method for manufacturing a variety of types of sensor elements 31 used in the odor measuring device 100. The odorant receiving layer 315 of the sensor element 31 may use slurries having various compositions as its raw material.

[0174] (Slurry preparation process) First, a plurality of types of slurries with different mixing ratios of the filler and the resin composition are prepared. The mixing ratio of the filler and the resin composition may be appropriately set according to the desired sensitivity and detection specificity of the odorant receiving layer 315. The slurry may contain a solvent, an additive, and a surfactant in addition to the filler and the resin composition. When preparing / kneading a slurry of the resin composition containing the filler and the resin composition, NMP as a solvent may be added to the mixture of the filler and the resin composition in multiple batches, and kneading may be repeated. Note that by increasing the number of times of kneading, the first porosity in the cross section of the odorant receiving layer 315 decreases.

[0175] (Electrode placement process) Next, electrodes are arranged on the substrate. The electrodes may include a first electrode and a second electrode. The first electrode and the second electrode may be arranged in a parallel straight line shape, a parallel curved line shape, a comb shape, or a concentric circle shape. In addition, the first electrode and the second electrode are preferably arranged in line symmetry or point symmetry with each other, regardless of which shape is adopted. Furthermore, it is more preferable that the first electrode and the second electrode are arranged in a parallel straight line shape or a parallel curved line shape. It is particularly preferable that the first electrode and the second electrode are arranged in a shape as shown in FIG. 10 and FIG. 11. Specifically, it is preferable that the first metal wiring 313C is composed of two metal wirings (313a and metal wiring 313c) arranged perpendicular to each other in a T-shape, the second metal wiring 313D is composed of two metal wirings (313c and metal wiring 313d) arranged perpendicular to each other in a T-shape, and the first metal wiring 313C and the second metal wiring 313D are arranged in parallel lines such that the metal wiring 313a and the metal wiring 313c face each other. By arranging the first metal wiring and the second metal wiring in this way, the odor measuring device 100 can measure odor substances contained in the gas with high accuracy.

[0176] As an example, in Figures 10 and 11, a pair of electrodes (first metal wiring 313C and second metal wiring 313D) is arranged on a single substrate 311, but multiple pairs of electrodes may be arranged side by side on a single substrate.

[0177] (Area definition process) Next, coating regions for coating each of the multiple types of slurries are defined on the substrate on which the electrodes are disposed. The coating regions may be defined, for example, by disposing a resist. Furthermore, in the coating step, when the slurry is dropped from a nozzle, the coating regions may be defined in accordance with the nozzle diameter. The resist M is disposed so as to define the coating region 330. In the coating region 330, the substrate 311 is exposed.

[0178] The size of the coating area 330 may be specified to be the same for each of the multiple types of slurries. That is, even if the slurries have different mixture ratios of the filler and the resin composition, the area of ​​the coating area 330 for coating the slurries may be uniform. This reduces the variation in the area of ​​the multiple types of odorant receiving layers 315 after drying, even if multiple types of slurries with different mixture ratios are used.

[0179] The coated area 330 is circular as an example, but the shape of the coated area 330 is not limited thereto. The coated area 330 may be circular or strip-shaped. This forms a circular or strip-shaped odorant receiving layer 315.

[0180] When the shape of the coating region 330 is circular, the diameter of the circle may be 0.2 mm or more and 5 mm or less, and when the shape of the coating region 330 is strip-shaped, the length of the strip in the short direction may be 0.2 mm or more and 5 mm or less. This forms a circular odorant receiving layer 315c with a diameter of 0.2 mm or more and 5 mm or less, and a circular odorant receiving layer 315d with a strip length in the short direction of 0.2 mm or more and 5 mm or less.

[0181] The method for applying the resist M is not particularly limited, but examples include a method of silk-screening the solder resist in a specified area and then UV-curing the solder resist, a method of attaching a resist film to a substrate, and a method of curing only the resist in a specified area and removing the uncured portion.

[0182] (coating process) Next, each of the multiple types of slurries is applied to the application region 330. The method of applying the slurry can be a conventionally known method, and the slurry may be dropped from a nozzle, sprayed, or spin-coated. The method of applying the slurry is particularly preferably a method of dropping the slurry from a nozzle, and a desired application shape can be obtained by using, for example, a SUS metal needle nozzle (inner diameter 0.1 mmΦ, outer diameter 0.23 mm) on an IMAGE MASTER 350 PC Smart manufactured by Musashi Engineering Co., Ltd.

[0183] (drying process) Finally, the slurry applied to the application area 330 is dried to form the odorant receiving layer 315. The method for drying the slurry is not particularly limited, but for example, a method can be used in which the slurry is heated at 100°C for 1 hour at normal pressure, and then heated at 100°C for 1 hour while reducing the pressure in a vacuum dryer.

[0184] (Odor permeable layer adjustment process) By kneading various resin compositions with NMP, a solution containing the resin for the odorant-permeable layer 317 is prepared. Note that by repeating the kneading process many times, the second porosity in the cross section of the odorant-permeable layer 317 decreases.

[0185] (Superposition of odorant permeable layer 317) A solution of resin for the odorant permeable layer 317 is applied onto the dried odorant receiving layer 315. At this time, care is taken to ensure that no gaps are formed between the odorant receiving layer 315 and the odorant permeable layer 317. After application, the layer is dried using a circulating air dryer.

[0186] <Example of software implementation> The control block (particularly the control unit 1) of the estimation device 10, 10a may be realized by a logic circuit (hardware) formed on an integrated circuit (IC chip) or the like, or may be realized by software.

[0187] In the latter case, the estimation device 10, 10a includes a computer that executes instructions of a program, which is software that realizes each function. The computer includes, for example, one or more processors, and a computer-readable recording medium that stores the program. The object of the present invention is achieved by the processor reading the program from the recording medium and executing it in the computer. The processor may be, for example, a CPU (Central Processing Unit). The recording medium may be a "non-transient tangible medium", such as a ROM (Read Only Memory), a tape, a disk, a card, a semiconductor memory, a programmable logic circuit, or the like. The device may further include a RAM (Random Access Memory) that expands the program. The program may be supplied to the computer via any transmission medium (such as a communication network or a broadcast wave) that can transmit the program. Note that one aspect of the present invention may also be realized in the form of a data signal embedded in a carrier wave, in which the program is embodied by electronic transmission.

[0188] 〔summary〕 The sensor element for an odor measuring device according to aspect 1 of the present disclosure comprises an odorant receiving layer comprising a resin composition including a resin (A) and a filler (B), a first metal wiring in contact with at least a portion of the odorant receiving layer, a second metal wiring spaced from the first metal wiring and in contact with at least a portion of the odorant receiving layer, and an odorant permeation layer covering the surface of the odorant receiving layer opposite the side in contact with the first metal wiring and the second metal wiring, wherein a first porosity indicating the proportion of the area occupied by voids in the cross section of the odorant receiving layer is 3% or more and 20% or less, a second porosity indicating the proportion of the area occupied by voids in the cross section of the odorant permeation layer is 3% or less, and the odor measurement method is a chemiresistor type.

[0189] A sensor element for measuring odors according to aspect 2 of the present disclosure may be such that in aspect 1 above, the maximum peak height of the odorant receiving layer on the surface covered by the odorant permeation layer is 50 μm or less.

[0190] A sensor element for an odor measuring device according to aspect 3 of the present disclosure is, in aspect 1 or 2 above, wherein the filler (B) is a conductive carbon material and may account for 10 to 50% by weight when the total amount of the resin (A) and the filler (B) is 100% by weight.

[0191] A sensor element for an odor measuring device according to aspect 4 of the present disclosure, in any one of aspects 1 to 3 above, may include an odorant-permeable layer that contains any one of butyral, polymethyl methacrylate, polyurethane, polyvinyl alcohol, polyvinyl chloride, polyester, polyvinylidene fluoride, cellulose acetate, polyvinylpyrrolidone, paraffin and polypropylene.

[0192] An odor measuring device according to a fifth aspect of the present disclosure includes a plurality of sensor elements for use in the odor measuring device according to any one of the first to fourth aspects. EXAMPLES

[0193] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited thereto. In the following, % means % by weight, and parts means parts by weight, unless otherwise specified.

[0194] The odor sensor 31 is exposed to a flow of air containing odorants. At this time, if the amount of odorant-containing air fed to the odor sensor 31 is large or the flow rate of the carrier gas is changed, turbulence or changes in wind pressure may occur. This turbulence or change in wind pressure may affect the odor sensor 31 as a physical external force. Therefore, in this embodiment, the resistance to changes in wind pressure and measurement sensitivity of odor sensors 31 (Examples 1 to 81) having an odorant-permeable layer 317 on the odorant receiving layer 315 were compared with the resistance to changes in wind pressure and measurement sensitivity of odor sensors (Comparative Examples 1 to 9) not having an odorant-permeable layer 317.

[0195] <Preparation of Examples 1 to 81> <Preparation of Resin> Resin A1: Butyral resin (manufactured by Kuraray Co., Ltd.) was used. Resin A2: Methyl methacrylate polymer (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used. Resin A3: Polyurethane resin A3 was obtained using polyoxyethylene glycol and 4,4'-diphenylmethane diisocyanate according to the method described below.

[0196] Specifically, a heating / cooling device, a thermometer, a temperature control device, a polymerization catalyst introduction tube, and a nitrogen introduction tube were attached to a reaction vessel equipped with an agitator blade, an agitator, a nitrogen inlet, and an outlet. This reaction vessel had a seal structure capable of reducing the pressure inside the reaction vessel. 10,000 parts of polyoxyethylene glycol having a number average molecular weight of 10,000 and 250 parts of 4,4'-diphenylmethane diisocyanate were added to the reaction vessel, and dibutyltin dilaurate was further added as a reaction solvent and a reaction catalyst. Thereafter, the inside of the reaction vessel was placed under normal pressure and nitrogen atmosphere, the temperature inside the reaction vessel was raised to 65°C, and the inside of the reaction vessel was stirred for 10 hours while maintaining the temperature, and the polyoxyethylene glycol and 4,4'-diphenylmethane diisocyanate were reacted. Subsequently, after stirring, 5 parts of 1-butanol were added as a reaction terminator to the inside of the reaction vessel, and the stirring inside the reaction vessel was continued for another 1 hour. As a result, a polyurethane resin was obtained. The reaction solvent used was dimethylformamide (DMF). Resin A4: Polyvinyl chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used. Resin A5: Silicone resin, DOWSIL TM RSN-0255 Flake Resin (manufactured by DOW Corporation) was used. Resin A6: Cellulose acetate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used. Resin A7: Polyvinylpyrrolidone K 90 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used. Resin A8: W#850 (manufactured by Kureha Corporation) was used as a vinylidene fluoride homopolymer. Resin A9: San-Estar 4610 (manufactured by Sanyo Chemical Industries, Ltd.) was used as the polyethylene butylene adipate. Resin A10: Polypropylene A10 was obtained by pyrolyzing commercially available polypropylene.

[0197] Specifically, a heating / cooling device, a thermometer, a temperature control device, a polymerization catalyst introduction tube, and a nitrogen introduction tube were attached to a reaction vessel equipped with an agitator, an agitator, a nitrogen inlet, and an outlet. This reaction vessel had a seal structure capable of reducing the pressure inside the reaction vessel. Polypropylene Vistamaxx 3000 (manufactured by ExxonMobil Corporation) was charged into the reaction vessel, and then the inside of the reaction vessel was placed under normal pressure and nitrogen atmosphere, the temperature inside the reaction vessel was raised to 280° C., and the inside of the reaction vessel was stirred for 10 hours while maintaining the temperature, and heated under a nitrogen atmosphere while removing hydrogen, to obtain polypropylene (A10) having a weight average molecular weight of 10,000. Resin A11: HNP-9 (manufactured by Nippon Seiro Co., Ltd.) was used as the paraffin wax.

[0198] <Preparation of resin composition for odorant receiving layer> <Resin composition E1> The following components were weighed out in the following amounts into a sample bottle to obtain a mixture. The filler was Denka Black (manufactured by Denka Co., Ltd.), and the surfactant was Disparlon DA-325 (manufactured by Kusumoto Chemicals Co., Ltd.), an amine salt of polyether phosphate ester.

[0199] Resin A1 72 parts by weight Filler: 20 parts by weight Surfactant: 8 parts by weight NMP 400 parts by weight The mixture was stirred (kneaded) at 2000 rpm for 20 minutes using a planetary centrifugal mixer (ARE-310 manufactured by Thinky Corporation) to obtain a slurry, which was a resin composition E1.

[0200] <Resin Compositions E2 - E10> Resin Compositions E2 - E10 were obtained in the same manner as Resin Composition E1, except that A2 - A10 were used as the resin.

[0201] <Preparation of E11> Resin Composition E11 was obtained in the same manner as Resin Composition E1, except that 82 parts by weight of resin were used instead of 72 parts by weight of Resin A1, and 10 parts by weight of Denka Black were used instead of 20 parts by weight.

[0202] <Preparation of E12> Resin Composition E12 was obtained in the same manner as Resin Composition E1, except that 42 parts by weight of resin were used instead of 72 parts by weight of Resin A1, and 50 parts by weight of Denka Black were used instead of 20 parts by weight.

[0203] <Preparation of E13> Resin Composition E13 was obtained in the same manner as Resin Composition E1, except that 87 parts by weight of resin were used instead of 72 parts by weight of Resin A1, and 5 parts by weight of Denka Black were used instead of 20 parts by weight.

[0204] <Preparation of E14> Resin Composition E14 was obtained in the same manner as Resin Composition E1, except that 32 parts by weight of resin were used instead of 72 parts by weight of Resin A1, and 60 parts by weight of Denka Black were used instead of 20 parts by weight.

[0205] <Preparation of E25> Resin Composition E25 was obtained in the same manner as Resin Composition E1, except that the number of kneading times was increased (60 minutes at 2000 revolutions per minute).

[0206] <Preparation of E26> Resin Composition E26 was obtained in the same manner as Resin Composition E1, except that the number of kneading times was decreased (10 minutes at 2000 revolutions per minute).

[0207] <Preparation of E27> Resin Composition E27 was obtained in the same manner as Resin Composition E1, except that the number of kneading times was increased (90 minutes at 2000 revolutions per minute).

[0208] <Preparation of Resin Composition for Odor Substance Permeation Layer> <Preparation of E15> The following components were weighed into a sample bottle in the following amounts to obtain a mixture.

[0209] Resin A1 100 parts by weight NMP 1900 parts by weight The mixture was stirred at 2000 revolutions per minute for 20 minutes using a rotation-revolution mixer (ARE-310 manufactured by Shinki Co., Ltd.) to obtain a slurry. Further, the slurry was ultrasonically dispersed at 40 kHz for 20 minutes using an ultrasonic cleaner (MCS-3 manufactured by AS ONE Corporation) to obtain resin composition E15. Note that when the number of times and time of ultrasonic dispersion are increased, the second porosity decreases.

[0210] <Preparation of E16 - E24> Resin compositions E16 to E24 were obtained in the same manner as resin composition E15, except that A2 - A4, A6 - A11 were used as the resin.

[0211] <Preparation of E28> Resin composition E28 was obtained in the same manner as resin composition E15, except that the ultrasonic dispersion time of the slurry was reduced to 5 minutes at 40 kHz.

[0212]

Table 1

[0213] <Preparation of Examples 1 - 10> Using a device with a SUS metal needle nozzle (inner diameter 0.1 mmΦ, outer diameter 0.23 mm) attached to IMAGE MASTER350PCSmart manufactured by Musashi Engineering Co., Ltd., each of resin compositions E1 - E10 was dropped onto a sensor substrate to coat the metal wiring portion. After coating, it was dried for 3 hours in a circulating air dryer heated to 100 °C to prepare an odor substance receiving layer. After drying, it was cooled to room temperature to prepare sensor elements F1 - F10.

[0214] Next, the resin composition E15 was dropped onto the applied sensors F1 to F10, and after dropping, the sensor was dried for 3 hours in a circulating air dryer heated to 100°C to prepare an odorant permeable layer. After drying, the sensor was cooled to room temperature to prepare sensor elements F11 to F20 corresponding to Examples 1 to 10. The surface smoothness of the odorant receiving layer 315 was adjusted as follows.

[0215] (Method for adjusting the surface smoothness of the odorant receptor layer) The depth of the "groove" (i.e., the depression that defines the area to which the slurry is applied) in the substrate onto which the odorant receptive layer slurry is applied was adjusted to a volume that would accommodate the amount of slurry to be applied. If the slurry does not fit into the "groove," the center of the slurry will rise due to surface tension, and the center of the "groove" will protrude compared to the periphery after drying.

[0216] <Preparation of Examples 11 to 19> Resin compositions E16 to E24 were dropped onto the sensor element F1, and after dropping, the sensor element was dried for 3 hours in a circulating air dryer heated to 100°C to prepare an odorant-permeable layer. After drying, the sensor elements were cooled to room temperature to prepare sensor elements F21 to F29 corresponding to Examples 11 to 19.

[0217] <Preparation of Example 20> A sensor element F30 corresponding to Example 20 was obtained in the same manner as in F11, except that the resin composition E11 was used instead of the resin composition E1.

[0218] <Preparation of Example 21> A sensor element F31 corresponding to Example 21 was obtained in the same manner as in F11, except that the resin composition E12 was used instead of the resin composition E1.

[0219] <Preparation of Example 22> A sensor element F32 corresponding to Example 22 was obtained in the same manner as in F11, except that the resin composition E25 was used instead of the resin composition E1.

[0220] <Preparation of Comparative Examples 1 to 10> Sensor elements F1 to F10 corresponding to Comparative Examples 1 to 10 were produced in the same manner as in the above <Production of Examples 1 to 10>. Comparative Examples 1 to 10 were completed at this point, and the odor permeable layer 317 was not coated.

[0221] <Preparation of Comparative Example 11> A sensor element F33 corresponding to Comparative Example 11 was obtained in the same manner as in F11, except that the resin composition E13 was used instead of the resin composition E1.

[0222] <Preparation of Comparative Example 12> A sensor element F34 corresponding to Comparative Example 12 was obtained in the same manner as in F11, except that the resin composition E14 was used instead of the resin composition E1.

[0223] <Preparation of Comparative Examples 13 and 14> Moreover, a sensor element F35 corresponding to Comparative Example 13 was obtained in the same manner as in F11, except that the resin composition E26 was used instead of the resin composition E1.

[0224] Moreover, a sensor element F36 corresponding to Comparative Example 14 was obtained in the same manner as in F11, except that the resin composition E27 was used instead of the resin composition E1.

[0225] <Preparation of Comparative Example 15> Sensor element F37 corresponding to Comparative Example 15 was obtained in the same manner as in F11, except that resin composition E28 was used instead of resin composition E15.

[0226] <Preparation of Comparative Example 16> Sensor element F38 corresponding to Comparative Example 16 was obtained in the same manner as sensor element F11, except that a substrate having a groove depth of 50 μm, which was too large to accommodate the slurry to be applied, was used.

[0227] <Construction of an odor sensor> A housing was prepared that had a target sample receiving section equipped with an inlet for introducing a specimen (odor substance) and an aluminum block thermostatic bath for temperature control, a nitrogen gas cylinder for gas supply, a mass flow controller, and a sensor chamber. The volume of the target sample receiving section was designed to be five times the volume of the sensor chamber. Lead wires for taking out the sensor terminals to the outside were soldered to the sensor elements F1 to F38, and the sensor elements F1 to F38 were installed in their respective sensor chambers. A 5V constant voltage power supply and a 300Ω fixed resistor were connected in series to the ends of the lead wires taken out of the sensor chamber for each of the sensor elements F1 to F38, and a voltmeter was connected to measure the voltage across both terminals of the sensor element. In this way, odor sensors corresponding to Examples 1 to 22 and Comparative Examples 1 to 16, each having the sensor elements F1 to F38, were constructed.

[0228] <Method of measuring first porosity and second porosity> The cross section of the sensor element, including the odorant receiving layer and the odorant permeation layer, was observed and photographed using a scanning electron microscope (SEM). The SEM observation conditions were as follows: Manufacturer:HITACHI Equipment: S-4800 Acceleration voltage: 1.0V Current value: 10μA.

[0229] When acquiring SEM images, the contrast was adjusted between 3225 and 3275, and the brightness was adjusted between 2025 and 2075 using the built-in application.

[0230] The SEM image obtained by SEM was binarized using image analysis software. ImageJ was used for the binarization process. In this binarization process, the image was processed in the order of "Gaussian Blur", "16bit", and "unsharp Mask", and then binarized using "threshold". The threshold value was set to 50 in grayscale to extract the area corresponding to the voids in the SEM image, and the first porosity, which is the ratio of the area occupied by the voids to the area shown in the SEM image of the odorant receiving layer 315, was calculated. Similarly, the second porosity, which is the ratio of the area occupied by the voids to the area shown in the SEM image of the odorant permeation layer 317, was calculated.

[0231] <Method for measuring the maximum peak height on the surface of the odorant receiving layer 315> The surface smoothness of the odorant receiving layer 315 of the odor sensor 31 was measured using a one-shot 3D measuring device, and analyzed using the built-in analysis software. Specifically, a circle with a radius of 1 mm was set as the analysis range, starting from the center of the surface of the odorant receiving layer of the odor sensor, and the maximum height "Sp" was obtained. The measurement conditions using the one-shot 3D measuring device were as follows: Manufacturer: KEYENCE Equipment:VR-5000 Camera magnification: 12x Analysis software: VRAnalyzer2.

[0232] <Number average molecular weight, weight average molecular weight measurement method> The number average molecular weight and weight average molecular weight of the substances used in the present invention can be measured by GPC (gel permeation chromatography). The measurement conditions for GPC in the present invention are as follows. Apparatus: High temperature gel permeation chromatography ("AllianceGPCV2000", Waters, Inc.) -Detection device: Refractive index detector Solvent: orthodichlorobenzene Reference material: Polystyrene Sample concentration: 3mg / ml Column stationary phase: PLgel 10 μm, MIXED-B 2 columns in series (Polymer Laboratories, Inc.) Column temperature: 135℃

[0233] <Verification method> [Measurement of wind pressure change resistance] For each odor sensor, we measured the resistance to wind pressure changes. Wind pressure changes were generated by pumping nitrogen into the chamber at high speed.

[0234] Specifically, for each odor sensor, nitrogen as a carrier gas was flowed from the carrier gas inlet into the housing in which the sensor element was installed at a flow rate of 5 L / min using a gas flow regulator, and then discharged to the outside. During this time, the measured value of the voltmeter connected to the sensor element was recorded by a computer. In this way, the resistance value of each sensor element in the odor sensor was calculated. For each sensor element of each odor sensor, the rate of change in resistance R 100 seconds after the start of the nitrogen flow relative to the output resistance R0 before the nitrogen flow was calculated.

[0235] The resistance to wind pressure changes of each odor sensor element was judged based on the rate of change in resistance R. Specifically, if the rate of resistance change was greater than 1%, it was judged to have high resistance, if it was between 0.5% and 1%, it was judged to have medium resistance, and if it was less than 0.5%, it was judged to have low resistance.

[0236] [Sensor element sensitivity measurement] For each odor sensor, 5 mL of ethanol as a sample was placed in the inlet of the odor sensor. After that, nitrogen as a carrier gas was flowed from the gas supply port into the sensor chamber in which the sensor element was installed at a flow rate of 1 L / min using a gas flow regulator, and then discharged to the outside. During this time, the measurement value of the voltmeter connected to the sensor element was recorded by a computer. In this way, the resistance value of each sensor element in the odor sensor was calculated. For each sensor element of each odor sensor, the rate of change in resistance R during sample introduction relative to the output resistance R0 before sample introduction was calculated.

[0237] The sensitivity of each odor sensor element was judged based on the rate of change in resistance R. Specifically, if the rate of change was greater than 20%, it was judged to be high sensitivity, if it was between 10% and 20%, it was judged to be medium sensitivity, and if it was less than 10%, it was judged to be low sensitivity.

[0238] <Result> First, the results when the odor sensors according to Examples 1 to 22 were used are shown in Table 2. As shown in Table 2, it was confirmed that the odor sensors having sensor elements F11 to F32 provided with an odorant-permeable layer (the odor sensors according to Examples 1 to 22) had medium or higher resistance to changes in wind pressure. It was also confirmed that all of the odor sensors according to Examples 1 to 22 had medium or higher sensor element sensitivity. In particular, it was confirmed that the odor sensors according to Examples 1 to 19 had high resistance to changes in wind pressure and also had high sensor element sensitivity.

[0239] [Table 2]

[0240] <Comparative Example> Next, Table 3 shows the results when odor sensors equipped with sensor elements F1 to 10 and F33 to 38 according to Comparative Examples 1 to 10 were used.

[0241] [Table 3]

[0242] As shown in Table 3, it was confirmed that the odor sensors according to the comparative examples (odor sensors according to comparative examples 1 to 10) having sensor elements F1 to F10 that do not have an odorant-permeable layer have resistance that varies greatly with wind pressure and have low resistance to wind pressure.

[0243] In addition, it was confirmed that the odor sensor of Comparative Example 12, which has sensor element F34 in which the filler contained in the odorant receiving layer exceeds 50 weight % relative to the total weight of the odorant receiving layer, has high resistance to wind pressure but low sensor element sensitivity.

[0244] In addition, it was confirmed that the odor sensor according to Comparative Example 13, which has a sensor element F35 having an odorant receiving layer using the resin composition E26, has a first porosity of more than 20%. It was confirmed that the odor sensor according to Comparative Example 13 has low resistance to wind pressure.

[0245] In addition, it was confirmed that the odor sensor according to Comparative Example 14, which has a sensor element F36 having an odorant receiving layer using resin composition E27, had a first porosity of less than 3%. It was confirmed that the odor sensor according to Comparative Example 14 had high resistance to wind pressure, but had low sensor element sensitivity.

[0246] In addition, the odor sensor according to Comparative Example 15, which has a sensor element F37 having an odorant-permeable layer using resin composition E28 with a shorter ultrasonic dispersion time than resin composition E15, was confirmed to have a second porosity of more than 4%. It was confirmed that the odor sensor according to Comparative Example 15 has low resistance to wind pressure.

[0247] It was confirmed that the odor sensor according to Comparative Example 16, which has a sensor element F38 fabricated using a substrate with a groove depth of 50 μm, which is a volume that does not accommodate the slurry to be applied, has a maximum peak height exceeding 50 μm. It was confirmed that the odor sensor according to Comparative Example 16 has low resistance to wind pressure and has medium sensor sensitivity.

[0248] As described above, it has been confirmed that a sensor element having the configuration of the present invention can provide an odor sensor that combines high resistance to wind pressure and high sensor sensitivity, compared to a sensor element that does not satisfy this configuration. [Industrial Applicability]

[0249] The present invention is useful as an odor identification sensor for medical use, gas detection, agriculture, and other industrial and daily uses. For example, farmers can use the odor identification sensor to determine the maturity of fragrant crops and manage the optimal harvest timing. In addition, the odor identification sensor can be used to digitize the odors of products such as food and cosmetics, helping to improve the efficiency of product development and stabilize quality. [Explanation of symbols]

[0250] 10, 10a Estimation device 11 Measurement value acquisition unit (acquisition unit) 12 Change pattern analysis section (analysis section) 16 Estimation part 30 Odor Sensor 31A Multiple sensor elements (sensor element group) 31, 31b, 31c Sensor element 32 Constant voltage power supply (power supply) 33 Voltmeter (measuring instrument) 100, 100a Odor measuring device 313A, 313C 1st metal wiring 313B, 313D 2nd metal wiring 315, 315c, 315d Odorant receptor layer 317 Odor-permeable layer 50 Target sample receiving section 51 Adjustment part 60 Sensor Chamber 80 Gas supply section 91, 92, 93, 94 Body 501 1st mouth 502 2nd mouth 503 Sample inlet

Claims

1. An odorant receiving layer comprising a resin composition comprising a resin (A) and a filler (B); A first metal wiring in contact with at least a portion of the odorant receiving layer, and a second metal wiring spaced apart from the first metal wiring and in contact with at least a portion of the odorant receiving layer; an odorant permeable layer covering the surface of the odorant receiving layer opposite to the side in contact with the first metal wiring and the second metal wiring; Equipped with A first porosity, which indicates the ratio of an area occupied by voids in a cross section of the odorant receiving layer, is 3% or more and 20% or less; In the cross section of the odorant-permeable layer, a second porosity indicating the ratio of the area occupied by voids is 3% or less; A sensor element for an odor measuring device that uses a chemiresistor type odor measuring method.

2. 2. A sensor element for an odor measuring device as described in claim 1, wherein the maximum peak height of the odorant receiving layer on the surface covered by the odorant permeation layer is 50 μm or less.

3. The filler (B) is a conductive carbon material, 2. The sensor element for an odor measuring device according to claim 1, wherein the amount of said resin (A) and said filler (B) is 10 to 50% by weight, assuming that the total amount of said resin (A) and said filler (B) is 100% by weight.

4. The sensor element for an odor measuring device described in claim 1, wherein the odorant-permeable layer includes any one of butyral, polymethyl methacrylate, polyurethane, polyvinyl alcohol, polyvinyl chloride, polyester, polyvinylidene fluoride, cellulose acetate, polyvinylpyrrolidone, paraffin and polypropylene.

5. A plurality of sensor elements for an odor measuring device according to any one of claims 1 to 4 are provided. Odor measuring device.

Citation Information

Patent Citations

  • Odor sensor

    JP1999023508A

  • Sensor array for detecting analytes in fluids

    JP1999503231A

  • Sensors based on polymers / plasticizers

    JP2002519633A