Additive manufacturing of oxide dispersion strengthened alloys of platinum group metals
The method of additively manufacturing ODS platinum alloys by powder bed fusion in an oxygen-containing atmosphere addresses the challenge of producing complex, high-temperature-resistant parts with enhanced hardness and creep resistance.
Patent Information
- Application Number
- JP2024510511
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-08-20
- Filing Date
- 2022-08-18
- Publication Date
- 2024-10-02
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There is a need for a method to additively manufacture oxide dispersion strengthened (ODS) platinum alloys for high-temperature applications, as conventional methods fail to produce parts with complex shapes and do not adequately enhance hardness, high-temperature strength, and creep resistance.
A method involving the use of a powder bed fusion process in an oxygen-containing atmosphere to form ODS platinum alloys by mixing platinum group metal and non-platinum group metal powders, ensuring uniform dispersion of oxides within the alloy, thereby enhancing hardness and creep resistance.
The method allows for the production of non-brittle, high-temperature-resistant ODS platinum alloys with complex shapes, offering improved hardness and creep resistance compared to conventional methods.
Smart Images

Figure 2024535701000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to methods of additively manufacturing articles comprising oxide dispersion strengthened alloys, and articles produced thereby. [Background technology]
[0002] Oxide dispersion strengthened (ODS) alloys have been manufactured for decades due to their beneficial properties such as strength retention at high temperatures and creep resistance. In some literature, they are also called dispersion hardened materials (e.g., DPH materials). These materials are sometimes called "metal matrix composites" because distinct discrete phases present within the grain boundaries of the alloy tend to increase the material's hardness, strength at high temperatures, and creep resistance.
[0003] For example, it is known that the addition of very small amounts of yttrium and / or zirconium to platinum alloys makes the structure of the platinum alloy more stable and significantly improves the recrystallization temperature. The dispersed second phases do not dissolve but remain at the grain boundaries. These yttrium and / or zirconium additions improve the properties of platinum at both room temperature and high temperatures. Furthermore, alloying both yttrium and zirconium is more effective than, for example, alloying only zirconium. Further improvements in the dispersion hardening of platinum are also made by oxidizing the elements yttrium and / or zirconium.
[0004] For example, ODS platinum alloys are known in the art and are particularly useful in high temperature applications because they have excellent chemical resistance, particularly to high temperature oxidation, retain mechanical properties at high temperatures, and have improved creep resistance.
[0005] Platinum alloys, i.e., non-ODS platinum alloys, are used in high temperature applications such as bushings for fiberglass production. It is desirable to additively manufacture platinum alloys to produce complex parts for such high temperature applications, e.g., bushings for fiberglass production. However, there is a desire to improve the working lifetime of such alloys used in high temperature applications, such as bushings for fiberglass production, due to, for example, the high turnover of conventional components in the glass manufacturing process. For example, conventionally manufactured bushings (i.e., often joined by welding, rather than by additive manufacturing) may typically require replacement after anywhere from 3 to 300 days of use. Summary of the Invention
[0006] The inventors have surprisingly found that ODS platinum alloys may be useful for similar applications, although methods for additively manufacturing such materials are currently unknown. Additively manufactured ODS platinum alloys may have significant advantages over conventionally manufactured ODS platinum alloys, for example, by allowing the manufacture of components having complex shapes and internal structures, while at the same time providing the advantages of increased hardness, high temperature strength and creep resistance of the material.
[0007] Conventional additive manufacturing of platinum group metal (PGM) alloys is known in the art, however, additively manufactured ODS PGM alloys are not known.
[0008] Therefore, there is a need to provide a method for additively manufacturing materials for high temperature applications that have improved high temperature properties such as hardness, high temperature strength and creep resistance compared to additively manufactured pure PGM alloys. [Problem to be solved by the invention]
[0009] The present invention seeks to address at least some of the problems associated with the prior art, or at least provide a commercially acceptable alternative solution.
[0010] The present invention provides methods of additively manufacturing articles comprising oxide dispersion strengthened alloys, additively manufactured articles and fiberglass manufactured bushings in accordance with the claims appended hereto. [Means for solving the problem]
[0011] Specifically, in one aspect, the present invention provides a method for additively manufacturing an article comprising an oxide dispersion strengthened alloy, the method comprising: providing a first powder comprising particles of one or more platinum group metals or alloys thereof; providing a second powder comprising particles of one or more non-platinum group metals or metalloids, or one or more alloys thereof; Providing a third powder by mixing the first powder and the second powder, wherein the third powder contains 0.01 to 1 wt % of the second powder based on the total weight of the third powder; and forming an article by powder bed fusion using the third powder in an atmosphere containing greater than 0 to 2 mole percent oxygen; The present invention provides a method comprising:
[0012] Each aspect or embodiment defined in this specification may be combined with other aspects or embodiments unless otherwise stated. In particular, any feature indicated as being preferred or advantageous may be combined with any other feature indicated as being preferred or advantageous.
[0013] The term "additive manufacturing" as used herein has its known and ordinary meaning in the art. More specifically, the term "additive manufacturing" as used herein may encompass a method of obtaining a three-dimensional object by adding material layer by layer to form a final product. Additive manufacturing may also be referred to as "3D printing."
[0014] The term "oxide dispersion strengthened alloy" (ODSA) as used herein has its usual meaning as known in the art. More specifically, the term "oxide dispersion strengthened alloy" as used herein may encompass a metal matrix having (small) oxide particles dispersed therein. Advantageously, the oxide particles may enhance high temperature strength and inhibit grain growth, thereby providing long term stable properties. Without wishing to be bound by theory, it is generally understood that the oxide particles are non-interfering with the lattice of the material, thereby reducing the movement of dislocations. This may prevent creep.
[0015] As used herein, terms such as "first powder," "second powder," "third powder," and the like are used as labels and do not indicate relative positions or the order in which the powders must be provided, unless otherwise specified.
[0016] The term "platinum group metals" (PGMs) as used herein includes the elements ruthenium (Ru), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir) and platinum (Pt) as commonly understood in the art. Thus, the term "non-platinum group metals" includes metal elements other than the PGMs. In other words, the term "non-platinum group metals" includes any metal element other than ruthenium (Ru), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir) and platinum (Pt).
[0017] The term "metalloid" as used herein, as common in the art, includes the elements boron, silicon, germanium, arsenic, antimony, tellurium, and polonium.
[0018] As used herein, the term "blend" may include a combination of two or more materials (e.g., PGMs) that are not in alloy form but are mixed. As used herein, the term "alloy" has its ordinary meaning in the art.
[0019] Unless otherwise specified, the term "mol % oxygen" as used herein means the mole % of oxygen molecules.
[0020] The term "power bed fusion" as used herein has its usual meaning as known in the art. In particular, the term "powder bed fusion" may encompass methods of melting and fusing material powders together layer by layer in an additive manufacturing process, for example using a laser or an electron beam, to obtain a final three-dimensional product. Common powder bed fusion processes include, but are not limited to, direct metal laser sintering (DMLS), electron beam melting (EBM), selective heat sintering (SHS), selective laser melting (SLM), selective laser sintering (SLS), etc. Alternatively, directed energy deposition (DED) methods such as direct laser deposition (DLD) may also be suitable for use as an alternative to the method of the present invention, i.e., powder bed fusion. In the present invention, SLM is typically and preferably used. However, other methods may be used, for example depending on the purpose of the final article and / or the materials used. All the steps described are known in the art, and the parameters used therein may be appropriately adjusted by the skilled person in routine use. Effect of the Invention
[0021] The inventors have surprisingly found that by forming articles by powder bed fusion in an atmosphere containing greater than 0 to 2 mol% oxygen, PGM-based ODSAs can be additively manufactured to be non-brittle and suitable for high temperature applications, which was not previously possible with PGM-based ODSAs. Without wishing to be bound by theory, it is believed that this is because the oxides of non-platinum group metals or metalloids are generated in-situ, layer by layer, during the additive manufacturing process, allowing the method to distribute one or more of the oxides uniformly throughout the article. This new method advantageously has many promising applications in a wide range of fields where articles, preferably with complex designs, need to withstand high temperatures. Such methods have not previously been envisioned or investigated using PGMs. Additively manufactured PGM-based ODSA articles offer significant improvements for use in high temperature applications compared to currently used additively manufactured articles, which are typically made from simple PGM alloys. The method of the present invention also advantageously allows PGM-based ODSA articles to be formed into complex shapes. This has not previously been possible on a large scale with PGM-based ODSAs, for example, without the extensive effort required for custom manufacturing, and therefore the additively manufactured articles described herein may have a longer lifespan in such high temperature applications. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The method includes providing a first powder comprising particles of one or more PGMs or alloys thereof. Alternatively, the particles of one or more PGMs may be in the form of a blend, i.e. a combination of two or more PGMs mixed together, but not in the form of an alloy. The PGM alloy may comprise at least one PGM and other elements suitable for forming an alloy therewith. However, preferably, the PGM alloy consists of two or more PGMs. Preferably, the first powder comprises particles of a Pt-based PGM alloy, i.e. a PGM alloy comprising Pt as the most abundant element. Preferably, the first powder consists essentially of particles of one or more PGMs or alloys thereof, more preferably of particles of one or more PGMs or alloys thereof. As used herein, the term "consists essentially of" may encompass materials in which, in addition to the essential elements, other non-specified elements may be present in the composition, provided that the essential properties of the composition are not significantly affected by their presence. It has been found that by selecting the elemental composition of the first powder in this way, additively manufactured articles can be formed with properties maximally optimized for high temperature applications, while taking into account costs.
[0023] It will be understood that there may be unavoidable impurities in the first powder. However, such impurities may typically be present in an amount of less than 1 wt%, preferably less than 0.5 wt%, more preferably less than 0.2 wt%, even more preferably less than 0.1 wt%, and even more preferably less than 0.01 wt%, based on the total weight of the first powder. Most preferably, the first powder is free of impurities within a practical range.
[0024] The method includes providing a second powder comprising particles of one or more non-platinum group metals or metalloids, or one or more alloys thereof. In general, the one or more non-platinum group metals or metalloids, or one or more alloys thereof, should have a lower oxidation temperature (i.e., the temperature at which the metal or metalloid oxidizes when heated in an oxygen-containing atmosphere) than the one or more PGMs or alloys thereof of the first powder. Preferably, the second powder comprises particles of one or more of cerium, tungsten, tantalum, hafnium, manganese, thorium, calcium, aluminum, zirconium and yttrium, or one or more alloys thereof. More preferably, the second powder comprises particles of zirconium and / or yttrium and / or alloys thereof, and even more preferably, zirconium and yttrium particles. In an alternative preferred embodiment, the second powder comprises particles of cerium and zirconium, or alloys thereof. While the invention can be practiced with any of the elements listed for the second powder, it was surprisingly found that the greatest improvement in hardness and creep resistance was achieved with zirconium and / or yttrium (i.e., zirconium and / or yttria are oxides in the resulting ODSA, e.g., zirconia, yttria, or yttria stabilized zirconia) compared to the respective one or more PGMs or alloys thereof. Also, zirconium and / or yttrium, particularly combinations of zirconium and yttrium, most preferably alloys thereof, work most effectively in the process of the invention (i.e., form oxides that are uniformly distributed within the final article). Also, the use of a combination of cerium and zirconium may be effective.
[0025] The second powder preferably consists essentially of particles of one or more non-platinum group metals or metalloids, or one or more alloys thereof, more preferably one or more non-platinum group metals or metalloids, or one or more alloys thereof. The second powder may be in the form of particles, for example, of single metal particles of each element, and / or in the form of blends or alloys thereof.
[0026] It will be understood that there may be unavoidable impurities in the second powder. However, such impurities may typically be present in an amount of less than 1 wt%, preferably less than 0.5 wt%, more preferably less than 0.2 wt%, even more preferably less than 0.1 wt%, and even more preferably less than 0.01 wt%, based on the total weight of the second powder. Most preferably, the second powder is free of impurities within a practical range.
[0027] The method includes providing a third powder by mixing a first powder with a second powder. Preferably, the third powder consists essentially of the first powder and the second powder, more preferably the first powder and the second powder. It will be understood that there may be unavoidable impurities in the third powder. However, such impurities may typically be present in an amount of less than 1 wt.%, preferably less than 0.5 wt.%, more preferably less than 0.2 wt.%, even more preferably less than 0.1 wt.%, and even more preferably less than 0.01 wt.%, based on the total weight of the third powder. Most preferably, the third powder is free of impurities within a practical range. The third powder is provided by mixing a first powder with a second powder, and it has been found that the more uniformly the second powder is dispersed within the first powder as a result of the mixing, the more uniformly the resulting oxide is dispersed within the additively manufactured article that may be formed, thereby resulting in an article that is more likely to exhibit the above-mentioned advantageous properties for high temperature applications. Thus, preferably, the third powder is homogeneous in that it comprises the second powder uniformly dispersed within the first powder.
[0028] The third powder contains 0.01 to 1 wt % of the second powder, for example, 0.01 to 1.0 wt % of the second powder, based on the total weight of the third powder. Preferably, the third powder contains 0.01 to 0.9 wt %, more preferably 0.01 to 0.8 wt %, and even more preferably 0.01 to 0.7 wt % of the second powder. In some preferred embodiments, the third powder contains 0.5 to 1.0 wt %, preferably 0.6 to 0.9 wt %, more preferably 0.65 to 0.75 wt %, and even more preferably about 0.7 wt % of the second powder. In other preferred embodiments, the third powder contains 0.01 to 0.1 wt %, preferably 0.01 to 0.05 wt %, more preferably 0.01 to 0.04 wt %, and most preferably about 0.015 wt % of the second powder, based on the total weight of the third powder. Alternatively, the third powder preferably comprises 0.01-0.05 wt.%, preferably 0.02-0.04 wt.%, more preferably about 0.03 wt.% of the second powder, based on the total weight of the third powder. Surprisingly, it has been found that such a weight ratio between the first and second powder advantageously provides a method by which additively manufactured articles can be produced having the most beneficial high temperature properties, such as hardness, strength and creep resistance. For example, it has been observed that using a third powder comprising about 0.7 wt.% yttria provides an advantage in tensile strength.
[0029] The method includes forming an article by powder bed fusion using a third powder in an atmosphere containing more than 0 mol% to 2 mol% oxygen. Thus, during powder bed fusion using a third powder in an atmosphere containing more than 0 mol% to 2 mol% oxygen, the particles of one or more non-platinum group metals or metalloids, or one or more alloys thereof, are typically at least partially oxidized in-situ. Preferably, the powder bed fusion is a selective laser melting process. Selective laser melting is known in the art. The parameters used therein can be adjusted appropriately by those skilled in the art in routine use. Without wishing to be bound by theory, it is believed that performing powder bed fusion in such a poisoned atmosphere containing more than 0 mol% to 2 mol% oxygen allows the oxides of one or more non-platinum group metals or metalloids to be uniformly distributed throughout the article, as the oxides are generated in-situ layer by layer during the additive manufacturing process. Thus, additively manufactured articles can be formed that have advantageously high and uniformly distributed hardness, strength and creep resistance.
[0030] The atmosphere may contain, for example, 0.01-2 mol% oxygen. Preferably, the atmosphere contains 0.05-2 mol% oxygen, more preferably 0.1-2 mol% oxygen, even more preferably 0.5-1.5 mol% oxygen, and most preferably 0.7-1.3 mol% oxygen. It has surprisingly been found that such oxygen concentrations allow the in-situ formation of oxides of one or more non-platinum group metals or metalloids, while at the same time reducing the risk of any PGMs also being oxidized. Without wishing to be bound by theory, it is believed that this is because, for example, the preferred elements cerium, tungsten, tantalum, hafnium, manganese, thorium, calcium, aluminum, zirconium and / or yttrium are susceptible to oxidation under the conditions of the present process. Preferably, the atmosphere consists of oxygen, one or more of nitrogen and argon, and unavoidable impurities, providing an otherwise inert atmosphere (i.e., other than the oxygen present).
[0031] The method may further include recovering the additively manufactured article. For example, the method may further include recovering the additively manufactured article from the powder bed fusion apparatus, such as by recovering the additively manufactured article from the remaining powder that was not sintered and / or melted during the process. Such steps would be known to one skilled in the art.
[0032] In a further aspect, the present invention provides a method of additively manufacturing an article comprising an oxide dispersion strengthened alloy, the method comprising: providing a first powder comprising particles of one or more platinum group metals or alloys thereof; providing a second powder comprising particles of one or more non-platinum group metals or metalloids, or one or more alloys thereof; providing a third powder by mixing the first powder and the second powder, wherein the third powder comprises 0.01-1 wt % of the second powder, based on a total weight of the third powder; providing an activated powder by heating the third powder in an atmosphere containing greater than 0-2 mole percent oxygen to a temperature sufficient to cause oxidation of at least a portion of the one or more non-platinum group metals or metalloids, or one or more alloys thereof, but not substantially causing oxidation of the one or more platinum group metals or alloys thereof; and forming an article by powder bed fusion using an activated powder in an inert atmosphere; Includes.
[0033] It will be appreciated that the definitions and preferences outlined above in relation to the first aspect apply, where appropriate, to this aspect as well.
[0034] As an alternative to the method of the first aspect, the method of the present aspect includes providing an activated powder by heating the third powder in an atmosphere containing more than 0 to 2 mol% oxygen to a temperature sufficient to cause at least a portion of the oxidation of the one or more non-platinum group metals or metalloids, or one or more alloys thereof, but not causing substantial oxidation of the one or more platinum group metals or alloys thereof. Thus, the method of the present aspect can provide an alternative solution to obtain a homogeneously distributed oxide within an additively manufactured article. While the method of the first aspect is preferred because it can more reliably achieve a homogeneous distribution of the oxide within an additively manufactured article, the method of the present aspect further overcomes the problems associated with the prior art by obtaining an additively manufactured PGM-based ODSA in which the oxide can be more homogeneously distributed such that an article having advantageous high temperature properties can be formed.
[0035] The atmosphere may contain, for example, 0.01 to 2 mol % of oxygen, preferably 0.05 to 2 mol % of oxygen, more preferably 0.1 to 2 mol % of oxygen, even more preferably 0.5 to 1.5 mol % of oxygen, and most preferably 0.7 to 1.3 mol % of oxygen.
[0036] The third powder is provided by mixing the first powder with the second powder, and it has been found that the more uniformly the second powder is dispersed within the first powder, the more likely the oxides formed in the activated powder during the heating step will be dispersed prior to the step of forming the article with the activated powder. Thus, the more likely the oxides in the additively manufactured article will be dispersed uniformly. Thus, the third powder is preferably homogenous, comprising the second powder uniformly dispersed within the first powder. As will be appreciated, in practice, the small particle size of the third powder may result in the activated powder containing a small amount of oxidized PGM. However, typically, the activated powder is substantially free of oxidized PGM, such as less than 0.1 wt. % based on the total weight of the activated powder. The activated powder may preferably contain less than 0.05 wt. % oxidized PGM, more preferably less than 0.01 wt. % oxidized PGM, based on the total weight of the activated powder.
[0037] Thus, the activated powder comprises oxides of one or more non-platinum group metals or metalloids, such as, for example, oxides of one or more of cerium, tungsten, tantalum, hafnium, manganese, thorium, calcium, aluminum, zirconium and yttrium, dispersed within the particles of one or more PGMs or alloys thereof from the first powder. However, it will be understood that not all of the one or more non-platinum group metals or metalloids, or one or more alloys thereof, in the third powder are completely oxidized. That is, the term "at least partial oxidation" as used herein may encompass a process in which at least a portion of one or more non-platinum group metals or metalloids, or one or more alloys thereof, respectively, forms an oxide of the element contained therein. Thus, small amounts of one or more non-platinum group metals or metalloids, such as, for example, cerium, tungsten, tantalum, hafnium, manganese, thorium, calcium, aluminum, zirconium and / or yttrium metals, or one or more alloys thereof, may be present in the activated powder. Preferably, greater than 50% by weight, more preferably greater than 70% by weight, even more preferably greater than 80% by weight, and even more preferably greater than 90% by weight, of the one or more non-platinum group metals or metalloids, or one or more alloys thereof (e.g., cerium, tungsten, tantalum, hafnium, manganese, thorium, calcium, aluminum, zirconium and / or yttrium) is oxidized in the activated powder, based on the total weight of the activated powder.
[0038] Preferably, the third powder is heated to a temperature of 400° C. to 950° C. for 2 hours or less, more preferably to a temperature of 500° C. to 950° C. for 2 hours or less. The preferred temperature may vary depending on the elements comprising the first and second powders.
[0039] Preferably, the third powder is heated for 1 hour or less, e.g., 10 seconds to 1 hour, more preferably, the third powder is heated for 10 seconds to 30 minutes. In some embodiments, the third powder is heated for 2 minutes or less, e.g., 30 seconds to 90 seconds. In other words, the third powder is heated for a time sufficient to cause at least a portion of the one or more non-platinum group metals or metalloids, or one or more alloys thereof, to oxidize, but not substantially oxidize, the one or more PGMs or alloys thereof.
[0040] The method of the present embodiment then comprises forming an article by powder bed fusion, i.e., conventional powder bed fusion, using an activated powder in an inert atmosphere, where the powder already comprises an oxide of one or more non-platinum group metals or metalloids, such as, for example, cerium, tungsten, tantalum, hafnium, manganese, thorium, calcium, aluminum, zirconium and / or yttrium. The inert atmosphere typically consists of nitrogen and / or argon, as well as any unavoidable impurities. As mentioned above, the oxides may be uniformly distributed in the activated powder, so that the oxides may be uniformly distributed in the PGM-based ODSA as a result. As a result, the advantageous properties of the additively manufactured article described above in relation to the first embodiment may also be achieved by the method of the present embodiment. Without wishing to be bound by theory, the above reasons apply mutatis mutandis to the method of the present embodiment.
[0041] The method of any embodiment may further include a heat treatment step, which preferably includes treating the article (i.e., the article formed by the method of the present invention) together with any unavoidable impurities at a temperature of 200° C. to 1600° C. for 1 hour to 20 hours in an atmosphere containing greater than 0 mol % to 2 mol % oxygen (e.g., about 10 hours at a temperature of about 1200° C. in a furnace with an atmosphere of about 0.5 mol % oxygen and balance argon). Without wishing to be bound by theory, it is believed that the additional heat treatment step may cause further oxidation of the grain refiner (i.e., the elements of the second powder, e.g., yttrium and zirconium), for example, if the grain refiner is not fully oxidized in-situ.
[0042] Preferably, in the method of the first two aspects disclosed herein, the particles of the second powder have a D90 of 10 μm or less. As will be understood by those skilled in the art, D90 refers to the value at 90% of the cumulative particle size distribution. D90 is based on volume. Typically, D90 is measured on a number basis and may be converted to a volume basis. D90 may be measured, for example, by laser diffraction. Suitable laser diffraction methods are known to those skilled in the art. In some embodiments, the particles of the second powder have a D90 of, for example, 0.1 to 10 μm. Preferably, the particles of the second powder have a D90 of 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. For example, the particles of the second powder may have a D90 of 0.1 to 5 μm, preferably 0.1 to 3 μm, and more preferably 0.1 to 1 μm. Also, the particles of the second powder may have a D90 of, for example, 0.5-10 μm, preferably 0.5-5 μm, more preferably 0.5-3 μm, and even more preferably 0.5-1 μm. Without wishing to be bound by theory, it is believed that such a particle size distribution allows the second powder to be more uniformly dispersed within the first powder to form the third powder, thereby helping to obtain additively manufactured articles with advantageous properties at high temperatures, at least for the same reasons as above. Without wishing to be bound by theory, this may be particularly advantageous in the method of the alternative embodiment, for example, since a smaller particle size of the particles of the second powder means that the surface area to volume ratio of the particles is increased. This may therefore in turn allow a higher weight percentage of material from the second powder to be oxidized in the heating step. Thus, an improved distribution of the oxide within the additively manufactured article may be achieved compared to conventional methods in which the materials may be mixed in bulk.
[0043] In a further aspect, the present invention provides a method of additively manufacturing an article comprising an oxide dispersion strengthened alloy, the method comprising: providing a first powder comprising particles of one or more platinum group metals or alloys thereof; providing an oxide powder comprising particles of one or more oxides of a non-platinum group metal or metalloid; Providing a mixed powder by mixing a first powder and an oxide powder, where the mixed powder contains 0.01 to 1 wt % of the oxide powder based on the total weight of the mixed powder; and forming an article by powder bed fusion using the mixed powder in an inert atmosphere; Includes.
[0044] It will be understood that the definitions and preferences outlined above in relation to the first and second aspects apply, where appropriate, to this aspect as well.
[0045] Alternatively to the methods of the first and second aspects, the method of this aspect includes providing an oxide powder comprising one or more oxide powders of a non-platinum group metal or metalloid, or mixtures thereof. That is, the method of this aspect includes providing preformed oxide particles rather than forming the oxide in-situ. Thus, in this aspect, it may be important that the mixed powder is well mixed. Thus, preferably, the mixed powder is homogenous as described herein with respect to the third powder. Preferably, the method includes mixing or blending the mixed powder, preferably in a mill, more preferably in a ball mill or rod mill, even more preferably in a ball mill. The mixed powder is mixed or blended, preferably for 1-60 minutes, preferably for 20-40 minutes, even more preferably for about 30 minutes. The inventors have surprisingly found that such mixing or blending may be particularly important for this aspect, for example to help avoid localised regions of oxide. Thus, it may be possible to form additively manufactured ODSA articles that are not brittle and have high hardness and tensile strength, for example. In other words, it is surprising that such articles can be additively manufactured in this way. The inventors have surprisingly discovered such a new additive manufacturing method using these starting materials.
[0046] The method of this aspect may therefore provide an alternative solution for obtaining a homogeneously distributed oxide within an additively manufactured article. The method of this aspect may for example be understood as an alternative to the second aspect, where for example a powder comprising a mixture of a first powder and one or more oxides of one or more non-platinum group metals or metalloids is not formed in-situ, but by mixing the first powder with a preformed oxide powder.
[0047] The methods of the first and second aspects described above are preferred because they may more reliably achieve a uniform distribution of oxides within an additively manufactured article. However, the method of this aspect may also be suitable. While the methods of the first and second aspects described above are preferred, the method of this aspect may also overcome problems associated with the prior art by obtaining an additively manufactured PGM-based ODSA in which the oxides may be more uniformly distributed such that an article having advantageous high temperature properties may be formed.
[0048] Preferably, the oxide powder particles have a D90 of 10 μm or less. D90 can be measured, for example, by laser diffraction. Suitable laser diffraction methods are known to those skilled in the art. In some embodiments, the oxide powder particles have a D90 of 0.01 to 10 μm, for example, 0.1 to 10 μm. Preferably, the oxide powder particles have a D90 of 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. For example, the oxide powder particles may have a D90 of 0.01 to 5 μm, preferably 0.1 to 3 μm, and even more preferably 0.1 to 1 μm. Also, the oxide powder particles may have a D90 of, for example, 0.5 to 10 μm, preferably 0.5 to 5 μm, more preferably 0.5 to 3 μm, and even more preferably 0.5 to 1 μm. Without wishing to be bound by theory, it is believed that such a particle size distribution allows the oxide powder to be more uniformly dispersed within the first powder to form a mixed powder, thereby helping to obtain additively manufactured articles having advantageous properties at high temperatures as discussed above, for at least the same reasons as above.
[0049] The method includes providing an oxide powder comprising particles of one or more oxides of a non-platinum group metal or metalloid, or mixtures thereof. Preferably, the oxide powder comprises particles of one or more oxides of cerium, tungsten, tantalum, hafnium, manganese, thorium, calcium, aluminum, zirconium and yttrium, or mixtures thereof. Preferably, the oxide powder comprises one or more of cerium oxide, zirconium oxide, yttrium oxide, zirconium-yttrium mixed oxide, and cerium-zirconium mixed oxide. Such oxides may provide particularly advantageous additively manufactured PGM-based ODSAs as described herein.
[0050] The oxide powder preferably consists essentially of particles of one or more oxides of non-platinum group metals or metalloids, or mixtures thereof, and more preferably consists of particles of one or more oxides of non-platinum group metals or metalloids, or mixtures thereof.
[0051] It will be understood that there may be unavoidable impurities in the oxide powder. However, such impurities may typically be present in an amount of less than 1 wt.%, preferably less than 0.5 wt.%, more preferably less than 0.2 wt.%, even more preferably less than 0.1 wt.%, and even more preferably less than 0.01 wt.%, based on the total weight of the oxide powder. Most preferably, the oxide powder is free of impurities within a practical range.
[0052] The method includes providing a mixed powder by mixing a first powder with an oxide powder. Preferably, the mixed powder consists essentially of the first powder and the oxide powder, more preferably the first powder and the oxide powder. It will be understood that unavoidable impurities may be present in the third powder. However, such impurities may typically be present in an amount of less than 1 wt%, preferably less than 0.5 wt%, more preferably less than 0.2 wt%, even more preferably less than 0.1 wt%, and even more preferably less than 0.01 wt%, based on the total weight of the mixed powder. Most preferably, the mixed powder is free of impurities within a practical range. The mixed powder is provided by mixing a first powder with an oxide powder, and it has been found that the more uniformly the oxide powder is dispersed within the first powder as a result of the mixing, the more uniformly the resulting oxide will be dispersed within the additively manufactured article that may be formed, thereby resulting in an article that is more likely to exhibit the above-mentioned advantageous properties for high temperature applications. Thus, preferably, the mixed powder is homogeneous in that it comprises the oxide powder dispersed uniformly within the first powder.
[0053] The mixed powder contains 0.01 to 1 wt % of oxide powder, for example, 0.01 to 1.0 wt % of oxide powder, based on the total weight of the mixed powder. Preferably, the mixed powder contains 0.01 to 0.9 wt %, more preferably 0.01 to 0.8 wt %, and even more preferably 0.01 to 0.7 wt % of oxide powder. In some preferred embodiments, the mixed powder contains 0.5 to 1.0 wt %, preferably 0.6 to 0.9 wt %, more preferably 0.65 to 0.75 wt %, and even more preferably about 0.7 wt % of oxide powder. In other preferred embodiments, the mixed powder contains 0.01 to 0.1 wt %, preferably 0.01 to 0.05 wt %, more preferably 0.01 to 0.04 wt %, and most preferably about 0.015 wt % of oxide powder, based on the total weight of the mixed powder. Alternatively, the mixed powder preferably comprises 0.01-0.05 wt.%, preferably 0.02-0.04 wt.%, more preferably about 0.03 wt.% of the oxide powder, based on the total weight of the mixed powder. Surprisingly, it has been found that such a weight ratio between the first powder and the oxide powder advantageously provides a method by which additively manufactured articles can be manufactured having the most beneficial high temperature properties, such as hardness, strength and creep resistance. For example, it has been observed that there is an advantage in tensile strength when using a mixed powder comprising about 0.7 wt.% yttria.
[0054] Preferably, the method of any of the embodiments disclosed herein further comprises forming a first powder by atomizing one or more PGMs or alloys thereof. Suitable atomization techniques are known in the art. As a result, a first powder having a preferred particle size distribution is provided. For example, the first powder may have a D90 of 90 μm or less, such as 70 μm or less, preferably 60 μm or less, more preferably 54 μm or less. Also, the first powder may have a D10 of 5 μm or more, such as 10 μm or more, preferably 15 μm or more. Without wishing to be bound by theory, it is believed that such a particle size distribution allows for a uniform distribution of the second powder or oxide powder within the first powder, thereby contributing to the advantageous effects described herein. Thus, preferably, the particles of the first powder have a D90 of 60 μm or less and the particles of the second powder or oxide powder have a D90 of 5 μm or less.
[0055] Preferably, the one or more PGMs comprise, more preferably consist essentially of, or consist of platinum, together with any unavoidable impurities. Preferably, the one or more PGMs or alloys thereof are PGM alloys, preferably comprise, more preferably consist essentially of, or consist of platinum and one or more of rhodium, ruthenium and iridium, together with any unavoidable impurities. In some embodiments, the platinum group metal alloy comprises, more preferably consists essentially of, or consists of 0.5-30 wt.% rhodium, preferably 2-30 wt.% rhodium, more preferably 5-30 wt.% rhodium, even more preferably 2-15 wt.% or 5-15 wt.% rhodium, even more preferably 8-12 wt.% rhodium, even more preferably about 10 wt.% rhodium; and the balance platinum, together with any unavoidable impurities. In yet another embodiment, the platinum group metal alloy comprises, more preferably consists essentially of, or consists of, 0.5-30 wt.% ruthenium, preferably 2-30 wt.% ruthenium; and the balance platinum, together with any unavoidable impurities. In yet another embodiment, the platinum group metal alloy comprises, more preferably consists essentially of, or consists of, 0.5-30 wt.% iridium, preferably 2-30 wt.% iridium; and the balance platinum, together with any unavoidable impurities. In yet another embodiment, the platinum group metal alloy comprises, more preferably consists essentially of, or consists of, 0.5-15 wt.% iridium; 0.5-15 wt.% rhodium, preferably 2-15 wt.% iridium and 2-15 wt.% rhodium; and the balance platinum, together with any unavoidable impurities. It has surprisingly been found that the above exemplified PGM alloys enable the formation of PGM-based ODSA additively manufactured articles with the most improved high temperature properties, such as high hardness, high strength and creep resistance.
[0056] Preferably, the third powder is provided by mixing the first powder and the second powder in a powder mixer, preferably for at least 30 minutes. Similarly, preferably, the mixed powder is provided by mixing the first powder and the oxide powder in a powder mixer, preferably for at least 30 minutes. Suitable powder mixers include, for example, a tubular mixer or a ball mill. Preferably, the third powder or the mixed powder is provided by mixing the first powder and the second powder or the oxide powder for 30 minutes to 12 hours, more preferably 1 hour to 6 hours, and even more preferably 2 hours to 4 hours. Without wishing to be bound by theory, it is believed that such a mixing process makes it possible to provide a sufficiently uniformly mixed (or homogenous) powder, thereby helping to achieve the advantageous effects related to the additively manufactured article described herein.
[0057] In some embodiments, the article is a bushing for fiberglass manufacturing. The term "bushing" can encompass, for example, a component that includes multiple nozzles through which molten glass can flow. The nozzles can be configured such that as molten glass pours into each nozzle, the molten glass can be directed out of a hole at the bottom of the nozzle. However, the shape and / or structure of the fiberglass bushing is not particularly limited and can take any shape known to those of skill in the art, for example. Fiberglass bushings are known to those of skill in the art.
[0058] In some embodiments, the articles are intended for high temperature applications. The articles described herein are particularly suited for such uses due to their high hardness, strength and creep resistance at high temperatures, as well as their ability to be manufactured into complex and specially designed shapes. Examples of high temperature applications include, for example, fiberglass manufacturing and space thruster nozzles.
[0059] However, it should be understood that the method of the present invention is not limited to oxide dispersion strengthened alloys. For example, each aspect or embodiment defined herein may be used to produce other dispersion strengthened alloys. Examples of other dispersion strengthened alloys to which the present invention may be applied include, for example, oxide, carbide, silicide, and nitride dispersion strengthened alloys or combinations thereof. In such methods, instead of or in addition to oxygen in the poisoned inert atmosphere, the atmosphere may contain, for example, nitrogen and / or carbon dioxide in an amount equivalent to the oxygen described in the above aspects and embodiments.
[0060] In a further aspect, the present invention provides an additively manufactured article produced by a method as described herein, the advantages of such an article being as described throughout this specification.
[0061] In a further aspect, the present invention provides a fiberglass manufacturing bushing comprising an additively manufactured article as described herein.
[0062] In a further aspect, the present invention provides a bushing for producing fiberglass comprising a platinum group metal-based oxide dispersion strengthened alloy, wherein the bushing is a continuous article. In other words, in a further aspect, the present invention provides a bushing for producing fiberglass comprising a platinum group metal-based oxide dispersion strengthened alloy, wherein the bushing does not include a weld. In a further aspect, the present invention provides a bushing for producing fiberglass comprising a platinum group metal-based oxide dispersion strengthened alloy, wherein the bushing comprises one or more nozzles and a body, wherein the one or more nozzles and the body are part of a continuous article and / or the one or more nozzles and the body are not joined by a weld joint.
[0063] The invention will now be described with reference to the following non-limiting drawings:
[0064] FIG. 1 is a flow chart of a method for additively manufacturing an article comprising an oxide dispersion strengthened alloy, according to one embodiment of the present invention.
[0065] FIG. 2 is a flow chart of a method of additively manufacturing an article comprising an oxide dispersion strengthened alloy in accordance with another embodiment of the present invention.
[0066] FIG. 3 is a flow chart of a method of additively manufacturing an article including an oxide dispersion strengthened alloy in accordance with yet another embodiment of the present invention.
[0067] Referring to FIG. 1, a flow chart of a method of additively manufacturing an article comprising an oxide dispersion strengthened alloy according to one embodiment of the present invention is shown (generally shown at 1). The method comprises: providing a first powder comprising particles of one or more platinum group metals or alloys thereof 5; providing a second powder comprising particles of one or more non-platinum group metals or metalloids, or one or more alloys thereof 10; providing a third powder by mixing the first powder with the second powder 15, where the third powder comprises 0.01-1 wt. % of the second powder, based on the total weight of the third powder; and forming the article by powder bed fusion with the third powder in an atmosphere comprising greater than 0-2 mol. % oxygen 20. Optionally, the method further comprises a step 25 of forming the first powder by atomizing the one or more platinum group metals or alloys thereof. Optionally, the method further comprises a step 30 of recovering the additively manufactured article.
[0068] Referring to Figure 2, a flow chart is shown (generally shown at 2) of a method of additively manufacturing an article comprising an oxide dispersion strengthened alloy according to another embodiment of the present invention. The method includes: providing a first powder comprising particles of one or more platinum group metals or alloys thereof 5; providing a second powder comprising particles of one or more non-platinum group metals or metalloids, or one or more alloys thereof 10; providing a third powder by mixing the first powder with the second powder 15, where the third powder comprises 0.01-1 wt% of the second powder, based on the total weight of the third powder; providing an activated powder by heating the third powder in an atmosphere comprising greater than 0-2 mol% oxygen to a temperature sufficient to cause oxidation of at least a portion of the one or more non-platinum group metals or metalloids, or one or more alloys thereof, but not substantially causing oxidation of the one or more platinum group metals or alloys thereof 35; and forming the article by powder bed fusion bonding using the activated powder in an inert atmosphere 40. Optionally, the method further comprises step 25 of forming a first powder by atomizing one or more platinum group metals or alloys thereof. Optionally, the method further comprises step 45 of recovering the additively manufactured article.
[0069] Referring to FIG. 3, a flow chart of a method of additively manufacturing an article comprising an oxide dispersion strengthened alloy according to another embodiment of the present invention is shown (generally shown at 3). The method includes: providing a first powder 5 comprising particles of one or more platinum group metals or alloys thereof; providing a powder 110 comprising particles of one or more oxides of one or more oxides of non-platinum group metals or metalloids, or mixtures thereof; providing a mixed powder by mixing the first powder with an oxide powder 115, where the mixed powder comprises 0.01-1 wt.% oxide powder based on the total weight of the mixed powder; and forming an article 120 by powder bed fusion using the mixed powder in an inert atmosphere. Optionally, the method further includes a step 25 of forming the first powder by atomizing one or more platinum group metals or alloys thereof. Optionally, the method further includes a step 50 of recovering the additively manufactured article.
[0070] The invention will now be described with reference to the following non-limiting examples.
[0071] Articles were additively manufactured according to embodiments of the present invention. In particular, articles were additively manufactured according to the third aspect, i.e. the aspect as defined in claim 6. The Vickers hardness, ultimate tensile strength (UTS) and elongation at break of the articles were tested using standard methods. The methods used were in accordance with ASTM E8 / E8M. The oxidation rate, which is the weight loss rate at 1550°C for 20 hours in air, was also measured. The results are compared to conventional materials in Table 1. "C" indicates that the material was cast (not by SLM). "S" indicates that the material was produced by SLM. The numbers indicate the relative amounts of the alloy components in weight percent. For example, Pt-Rh 10 is an alloy of platinum and rhodium, consisting of 10 weight percent rhodium and the balance platinum, as well as unavoidable impurities. The ODS alloys were produced using zirconia and yttria (i.e. zirconium oxide and yttrium oxide) to stabilize the alloy.
[0072] In particular, S-ODS-PtRh10 was produced as follows: 1.5 kg of PtRh10 powder was gas atomized and pre-sieved to a D10 of 15 μm and D90 of 54 μm. Yttria-stabilized zirconia oxide powder with a D90 of less than 2 μm and an amount of 0.7 wt% based on the total weight of the mixed powder was used as the second / oxide powder. This mixed powder was mixed in a tubular mixer with 2 kg of steel ball media for 30 minutes. The powder was collected and tested to ensure that the steel from the media did not contaminate the powder. SEM analysis was performed to ensure that the oxide was well dispersed in the Pt-Rh10. This material was then placed into an EOS M100 Additive Manufacturing System and articles were produced using standard Pt-Rh10 parameters.
[0073] [Table 1]
[0074] It can be seen that the hardness and tensile strength of additively manufactured articles produced according to the present invention are significantly higher than those of additively manufactured articles having the same platinum group metal composition but not stabilized by oxide. Moreover, the hardness and tensile strength of the articles according to the present invention are comparable to those of additively manufactured articles having a rhodium content significantly higher than that of the additively manufactured articles according to the present invention, for example 7% and 10% higher by weight. Moreover, surprisingly, the oxidation resistance of the articles according to the present invention is not significantly reduced compared to other additively manufactured articles. In other words, advantageously, the use of oxide stabilization works in the same way as increasing the rhodium content. Because rhodium is very expensive, the use of cheaper materials in the present invention can surprisingly result in comparable or higher hardness and tensile strength.
[0075] The foregoing detailed description has been provided for purposes of explanation and illustration and is not intended to limit the scope of the appended claims. Many variations in the presently preferred embodiments illustrated herein will be apparent to those of ordinary skill in the art and remain within the scope of the appended claims and their equivalents.
Claims
1. 1. A method of additively manufacturing an article comprising an oxide dispersion strengthened alloy, comprising: providing a first powder comprising particles of one or more platinum group metals or alloys thereof; providing a second powder comprising particles of one or more non-platinum group metals or metalloids, or one or more alloys thereof; Providing a third powder by mixing the first powder and the second powder, wherein the third powder comprises 0.01 to 1 wt. % of the second powder based on the total weight of the third powder; and forming an article by powder bed fusion using said third powder in an atmosphere containing greater than 0 to 2 mole percent oxygen; A method comprising:
2. 1. A method of additively manufacturing an article comprising an oxide dispersion strengthened alloy, comprising: providing a first powder comprising particles of one or more platinum group metals or alloys thereof; providing a second powder comprising particles of one or more non-platinum group metals or metalloids, or one or more alloys thereof; providing a third powder by mixing the first powder and the second powder, wherein the third powder comprises 0.01 to 1 wt % of the second powder based on the total weight of the third powder; providing an activated powder by heating said third powder in an atmosphere containing greater than 0 to 2 mole percent oxygen to a temperature sufficient to cause oxidation of at least a portion of one or more non-platinum group metals or metalloids, or one or more alloys thereof, but not substantially causing oxidation of one or more platinum group metals or alloys thereof; and forming an article by powder bed fusion using said activated powder in an inert atmosphere; A method comprising:
3. 3. The method of claim 1 or 2, wherein the second powder comprises particles of one or more of cerium, tungsten, tantalum, hafnium, manganese, thorium, calcium, aluminum, zirconium, and yttrium, or one or more alloys thereof.
4. The method according to any one of claims 1 to 3, wherein the second powder comprises particles of zirconium and / or yttrium and / or alloys thereof.
5. The method of any one of claims 2 to 4, wherein the third powder is heated to a temperature of from 400°C to 950°C for up to 2 hours.
6. 1. A method of additively manufacturing an article comprising an oxide dispersion strengthened alloy, comprising: providing a first powder comprising particles of one or more platinum group metals or alloys thereof; providing an oxide powder comprising one or more oxide powders of a non-platinum group metal or metalloid, or mixtures thereof; mixing the first powder and the oxide powder to provide a mixed powder, wherein the mixed powder contains 0.01 to 1 wt % of the oxide powder based on the total weight of the mixed powder; and forming an article by powder bed fusion using said mixed powder in an inert atmosphere; A method comprising:
7. 7. The method of claim 6, wherein the oxide powder comprises one or more oxide powders of cerium, tungsten, tantalum, hafnium, manganese, thorium, calcium, aluminum, zirconium, and yttrium, or mixtures thereof.
8. The method according to claim 6 or 7, wherein the oxide powder comprises one or more of cerium oxide, zirconium oxide, yttrium oxide, zirconium-yttrium mixed oxide and cerium-zirconium mixed oxide.
9. A method according to any one of the preceding claims, wherein the particles of the first powder have a D90 of 90 μm or less and / or the particles of the second powder or oxide powder have a D90 of 10 μm or less.
10. The method of any one of claims 1 to 9, further comprising forming the first powder by atomizing one or more platinum group metals or alloys thereof.
11. 11. The method according to any one of the preceding claims, wherein the one or more platinum group metals or alloys thereof are preferably platinum group metal alloys comprising platinum and one or more of rhodium, ruthenium and iridium and any unavoidable impurities.
12. The platinum group metal alloy is selected from the group consisting of: 0.5 to 30% by weight, preferably 5 to 15% by weight, more preferably 8 to 12% by weight, of rhodium; and the balance being platinum and any unavoidable impurities; The method of claim 11 , comprising:
13. The platinum group metal alloy is selected from the group consisting of: 0.5 to 30% by weight of ruthenium; and the balance being platinum and any unavoidable impurities; The method of claim 11 , comprising:
14. The platinum group metal alloy is selected from the group consisting of: 0.5 to 30% by weight of iridium; and the balance being platinum and any unavoidable impurities; The method of claim 11 , comprising:
15. The platinum group metal alloy is selected from the group consisting of: 0.5 to 15% by weight of iridium; 0.5 to 15% by weight of rhodium; and the balance being platinum and any unavoidable impurities; The method of claim 11 , comprising:
16. 16. The method according to any one of claims 1 to 15, wherein the third powder is provided by mixing the first powder and the second powder in a powder mixer, preferably for at least 30 minutes, or the mixed powder is provided by mixing the first powder and an oxide powder in a powder mixer, preferably for at least 30 minutes.
17. The method of any one of claims 1 to 16, wherein the article is a bushing for fiberglass manufacturing.
18. The method of any one of claims 1 to 17, wherein the article is for high temperature applications.
19. An additively manufactured article produced by the method of any one of claims 1 to 18.
20. 20. A bushing for fiberglass production comprising the additively manufactured article of claim 19.