Controlling the carbothermal reduction of rice husk ash (RHA) by-products to form nanostructured silicon carbide, silicon nitride, and silicon oxynitride nanocomposites by tailoring carbon and silica contents

By converting silica-deficient rice husk ash into nanostructured silicon carbide and nitride products without external carbon sources, the method addresses the challenges of carbon content variability and impurities, achieving high-purity materials suitable for electrochemical cells.

JP2024535761APending Publication Date: 2024-10-02THE RGT UNIV OF MICHIGAN
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2024515077
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-08
Filing Date
2022-09-08
Publication Date
2024-10-02

AI Technical Summary

Technical Problem

The commercial production of silicon carbide (SiC) and silicon nitride (Si3N4) from rice husk ash (RHA) is hindered by variability in carbon content and impurities, making it challenging to achieve high purity and uniformity in the final product.

Method used

A method involving the conversion of silica-deficient rice husk ash (SDRHA) with controlled silicon and carbon content is used, eliminating the need for external carbon sources and achieving carbothermal reduction at lower temperatures, resulting in nanostructured silicon carbide, silicon nitride, and silicon oxynitride products.

Benefits of technology

This method produces high-purity nanostructured materials with controlled morphology, enabling their use in electrochemical cells as electroactive materials, offering improved energy efficiency and reduced environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024535761000001_ABST
    Figure 2024535761000001_ABST
Patent Text Reader

Abstract

In various aspects, methods are provided for making silicon carbide or silicon nitride from rice husk ash (RHA) by-products. Silicon carbide (SiC), silicon nitride (Si3N4), and silicon oxynitride (Si2N2O, or non-stoichiometric SiN x O 4-x The treated silica-deficient rice husk ash product (SDRHA) comprising ≦about 65% by weight silicon oxide and ≧about 35% by weight carbon can be heated in an environment without an additional carbon source, but in an inert atmosphere having a temperature of ≧about 1,200° C. and ≦about 1,700° C., for a carbothermal reaction to form a product (e.g., a nanocomposite product) comprising at least one of: (wherein x is in the range of from greater than 0 to less than 4). A negative electroactive material comprising silicon oxynitride (Si2N2O) is also provided, which may be used in lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] government support This invention was made with Government support awarded by the National Science Foundation under Grant No. 1926199. The Government has certain rights in this invention.

[0002] This application claims the benefit of U.S. Provisional Application No. 63 / 241,820, filed September 8, 2021, the entire disclosure of which is incorporated herein by reference.

[0003] The present disclosure relates to a method for making at least one of silicon carbide (SiC), silicon nitride (Si3N4), and silicon oxynitride (Si2N2O) from rice husk ash (RHA) by-product. [Background technology]

[0004] This section presents background information related to the present disclosure, which is not necessarily prior art.

[0005] Rice is the second most consumed food worldwide and is usually marketed after milling to remove the rice husk or husk (RH), which constitutes approximately 20 wt.% of the rice as grown. RH is generally considered an agricultural waste product since it has no substantial direct commercial uses. However, the discovery that RH has approximately 15-20 wt.% amorphous SiO2 has led to various efforts to produce SiC and Si3N4 whiskers and particles. First, in 1975, it was found that RH produces SiC by heating it to SiC at 1200-1500 °C under an inert or reducing atmosphere. More recently, a typical process involves first coking or ashing RH prior to conversion to SiC or Si3N4.

[0006] However, commercial production of SiC and Si3N4 from RH has not yet been realized. Most RH is disposed of by incinerating rice husk ash (RHA), which is primarily used to fertilize soil to fertilize crops grown in the next season. The amount of SiO2, carbon, and residual mineral content from RH varies depending on the type of crop, the climate and location of cultivation, and the temperature and duration of combustion.

[0007] Generally, RHA contains 80-90 wt.% amorphous SiO2, while carbon and trace amounts of alkali elements such as K, S, Ca, and Mg make up the remaining mass. Considering the relatively high SiO2 content, only a limited number of studies have reported the synthesis of SiC and Si3N4 from RHA. Those reports typically use RHA as a SiO2 source with the further addition of an external carbon source. In one example, RHA was pyrolyzed with a phenolic resin carbon source as a preliminary step to generate SiC nanowires. The mixture of RHA and resin was embedded in graphite and then heated at 1600 °C. In another example, a template with a graphene carbon source and RHA was used to grow SiC whiskers with diameters of 30-120 nm.

[0008] Additionally, excess carbon and the co-formed CO gas are essential in the carbothermal nitridation to produce Si3N4. Typically, Si3N4 is synthesized by hydrothermal reaction by combining an external carbon source with RHA in the presence of a nitrogen-containing compound (such as NH4OH). In another example, carbothermal nitridation of RHA from Thailand, which has a naturally low silicon content (only 45 wt%), produced Si3N4 fibers and whiskers without the addition of additional carbon. However, typical RHA has a silica (SiO2) content of about 80-90 wt%, which is not a viable starting point for forming SiC or Si3N4 materials due to its low carbon content. This silica to carbon ratio, e.g., SiO2 to carbon ratio of 4:1 to 9:1, is rather unique to RHA feedstock worldwide and is not suitable for the formation of SiC and / or SiN4. x O 4-xThis leads to the conclusion that carbon must be added to adjust the stoichiometry to favor the formation of Summary of the Invention [Problem to be solved by the invention]

[0009] In addition to the variability of SiO2 and carbon content in agricultural waste materials, another obstacle impedes the commercial production of SiC and Si3N4 from RH and / or RHA. As discussed above, most agricultural sources often contain significant amounts of impurities that closely affect the phase and morphology, as well as the purity of the as-produced product. To address these variabilities in the composition of the precursor rice husk without the need for added carbon sources, it would be desirable to develop a method for processing RHA to form silicon carbide (SiC) and silicon nitride (Si3N4). [Means for solving the problem]

[0010] This section provides a general overview of the disclosure and is not an exhaustive disclosure of its entire scope or all of its components.

[0011] In a particular aspect, the present disclosure relates to a method for making silicon carbide or silicon nitride from rice husk ash (RHA) by-products. The method provides silicon carbide (SiC), silicon nitride (Si3N4), and silicon oxynitride (SiN x O 4-x and optionally a step of heating a silica-deficient rice hull ash product (SDRHA) comprising about 65% by weight or less of silicon oxide and about 35% by weight or more of carbon in an environment having a temperature of about 1,200° C. or more and an inert atmosphere and no additional carbon source, for a carbothermal reaction to form a product comprising at least one of the following: (wherein x is in the range of from greater than 0 to less than 4), e.g., SiNO).

[0012] In certain embodiments, the silica deficient rice hull ash (SDRHA) comprises from about 35% to about 60% carbon by weight.

[0013] In certain embodiments, the silica deficient rice hull ash (SDRHA) has a SiO2 to carbon ratio (SiO2:C) of about 1:8 to about 1:3.

[0014] In certain embodiments, the method further comprises removing silicon oxide from the rice husk ash (RHA) by-product by reacting the RHA with a hindered diol in the presence of a catalytic base to form a silica-deficient rice husk ash (SDRHA).

[0015] In a further embodiment, the hindered diol is selected from the group consisting of 2-methyl-2,4-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, and combinations thereof.

[0016] In a further embodiment, the catalytic base is selected from the group consisting of sodium hydroxide (NaOH), lithium hydroxide (LiOH), calcium hydroxide Ca(OH) 2 , potassium hydroxide (KOH), cesium hydroxide (CsOH), rubidium hydroxide (RbOH), and combinations thereof.

[0017] In a further embodiment, the hindered diol comprises 2-methyl-2,4-pentanediol and the catalytic base comprises sodium hydroxide (NaOH).

[0018] In certain embodiments, the temperature is from about 1,400°C to about 1,600°C.

[0019] In certain embodiments, the product is a nanocomposite.

[0020] In certain embodiments, the product comprises greater than or equal to about 75% by weight silicon carbide (SiC).

[0021] In certain embodiments, the product is a nanostructured silicon oxynitride (SiN x O 4-x(wherein x is greater than 0 and less than 4, e.g., Si2N2O), and the nanostructure includes at least one of silicon carbide (SiC) and silicon nitride (Si3N4) distributed therein.

[0022] In certain embodiments, the method further comprises, prior to heating, milling the rice hull ash (RHA) by-product with an acidic solution to obtain a refined rice hull ash (RHA) by-product; and subsequently removing silicon oxide from the refined rice hull ash (RHA) by-product by reacting the refined rice hull ash (RHA) with a hindered diol in the presence of a catalytic base to form a silica-deficient rice hull ash (SDRHA).

[0023] In certain embodiments, the method further comprises washing the refined rice husk ash (RHA) by-product with boiling water after milling to remove impurities.

[0024] In a particular embodiment, the present disclosure relates to an electroactive material for the negative electrode of an electrochemical cell circulating lithium ions, the electroactive material being silicon oxynitride (SiN x O 4-x (wherein x is greater than 0 and less than 4), such as Si2N2O.

[0025] In certain embodiments, the electroactive material is silicon oxynitride (SiNO, or nonstoichiometric SiN x O 4-x (wherein x is greater than 0 and less than 4).

[0026] In certain embodiments, the nanocomposite further comprises a pyrolyzed carbon-based material.

[0027] In certain embodiments, the nanocomposite is silicon oxynitride (SiNO, or nonstoichiometric SiN x O 4-x (wherein x is greater than 0 and less than 4).

[0028] In certain embodiments, silicon oxynitride (SiNO, or nonstoichiometric SiN x O 4-x (wherein x is in the range of from 0 to 4) is formed by heating a silica-deficient rice hull ash product (SDRHA) containing about 65% by weight or less of silicon oxide and about 35% by weight or more of carbon in an environment containing an inert atmosphere without an additional carbon source but having nitrogen present and having a temperature of about 1,200° C. to about 1,700° C. for a carbothermal reaction.

[0029] In certain embodiments, the silicon oxynitride comprises Si2N2O.

[0030] In certain embodiments, the silicon oxynitride is non-stoichiometric SiN x O 4-x Includes 、 x is greater than 0 and less than 4.

[0031] In certain further aspects, the present disclosure relates to an electrode comprising the electroactive material described above, which may further comprise graphite.

[0032] In certain further embodiments, the electrode further comprises a polymeric binder.

[0033] In certain other aspects, the present disclosure relates to an electroactive material for the negative electrode of an electrochemical cell circulating lithium ions, the electroactive material being silicon oxynitride (Si2N2O, or nonstoichiometric SiN x O 4-x (wherein x is greater than 0 and less than 4) and / or nanocomposites comprising silicon carbide (SiC).

[0034] In certain embodiments, the nanocomposite further comprises a pyrolyzed carbon-based material.

[0035] In certain embodiments, the nanocomposite comprises silicon carbide (SiC).

[0036] In certain embodiments, the nanocomposite is silicon oxynitride (SiNO, or nonstoichiometric SiN x O 4-x (wherein x is greater than 0 and less than 4).

[0037] In certain embodiments, the silicon oxynitride comprises Si2N2O.

[0038] In certain other embodiments, the silicon oxynitride is non-stoichiometric SiN x O 4-x and x is in the range of greater than 0 and less than 4.

[0039] In certain further aspects, the present disclosure relates to an electrode comprising the electroactive material described above, which may further comprise graphite.

[0040] In certain further embodiments, the electrode further comprises a polymeric binder.

[0041] Further areas of applicability will become apparent from the description provided herein. The description and specific examples in this summary are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure.

[0042] The drawings described herein are intended to illustrate only selected embodiments rather than every possible implementation and are not intended to limit the scope of the present disclosure. [Brief description of the drawings]

[0043] [Figure 1A] FIG. 1 is an XRD diagram of rice husk ash (RHA) and silica-deficient rice husk ash having 60 wt. % silica (SDRHA60). [Figure 1B] FIG. 1 is an SEM image of RHA. [Figure 1C] FIG. 1 is an SEM image of SDRHA60.

[0044] [Figure 2A] FIG. 1 is a diagram of an XPS survey scan. [Figure 2B] FIG. 1 is a TGA of RHA and SDRHA60. [Figure 2C] FIG. 1 is a diagram of N2 adsorption / desorption isothermal plots of RHA and SDRHA60.

[0045] [Figure 3A] FIG. 1 shows the XRD plots obtained from heating SDRHA60 at 1430-1500° C. / 8 h / Ar. [Figure 3B] FIG. 1 shows XRD plots from heating SDRHA60 at 1500° C. for various times. [Figure 3C] FIG. 13 shows heating of SDRHA40-60 at 1400° C. / 10 h / Ar.

[0046] [Figure 4A] 1 shows XRD plots from heating SDRHA60 at 1400 / 8h / N2, 1500°C / 4h / N2, and 1500°C / 8h / N2. [Figure 4B] FIG. 13 shows XRD plots from heating SDRHA60 at 1500° C. / N2 for various times.

[0047] [Diagram 5] FIG. 1 shows XRD plots from heating SDRHA60 under different ratios of N2 / H2 (95 / 5 and 85 / 15) at 1500° C. for various times.

[0048] [Figure 6A] FIG. 13 is a representative optical image of SiC with 13 wt.% carbon. [Figure 6B] FIG. 13 is a representative optical image of SiC without 13 wt.% carbon. [Figure 6C] FIG. 13 is a representative optical image of Si3N4 with 24 wt.% carbon. [Figure 6D] FIG. 13 is a representative optical image of Si3N4 without 24 wt.% carbon.

[0049] [Figure 7A] FIG. 2 is a representative TGA curve of a SiC composite. [Figure 7B] FIG. 13 is a representative TGA curve of a Si3N4 composite. [Figure 7C] FIG. 1 is a representative TGA curve of a Si2N2O composite. [Figure 7D] FIG. 13 shows representative FTIR spectra of SiC composites with and without carbon. [Figure 7E] FIG. 13 shows representative FTIR spectra of Si3N4 composites with and without carbon. [Figure 7F] FIG. 13 shows representative FTIR spectra of Si2N2O composites with different heat treatments.

[0050] [Figure 8A] FIG. 1 shows a representative XPS wide survey and elemental analysis, and core level spectrum of a SiC composite. [Figure 8B] FIG. 13 shows a representative XPS wide survey and elemental analysis and core level spectrum of a Si3N4 composite.

[0051] [Figure 9A] FIG. 13 is a representative SEM image of a SiC / C composite after oxidative removal of hard carbon. [Figure 9B] 1A-1C are representative SEM and EDX images of SiC after oxidative removal of hard carbon. [Figure 9C] FIG. 1 shows representative SEM and EDX images of Si3N4 after oxidative removal of hard carbon. [Figure 9D] FIG. 1 shows representative SEM and EDX images of Si2N2O after oxidative removal of hard carbon.

[0052] [Figure 10A] FIG. 13 shows representative isothermal plots of SiC with different heat treatments. [Figure 10B] FIG. 13 shows representative isothermal plots of Si3N4 with different heat treatments.

[0053] [Figure 11A] FIG. 1 is a capacitance-voltage (CV) curve of a SiC-C / Li half cell. [Figure 11B] FIG. 1 is a voltage-capacity curve of a SiC-C / Li half cell.

[0054] [Figure 12] FIG. 1 shows specific capacity versus cycle number of a SiC-C / Li half-cell.

[0055] [Figure 13] FIG. 13 shows XRD of pristine SiC / C composite and SiC / C after 600 cycles as anode material in a Li half cell.

[0056] [Figure 14] FIG. 13 shows a representative CV curve of a Si2N2O nanocomposite / Li half-cell.

[0057] [Figure 15A] FIG. 13 is a plot of specific capacity versus cycle number for a Si2N2O(88) / Li half-cell. [Figure 15B] FIG. 14 is a plot of specific capacity versus cycle number for a Si2N2O(84) / Li half-cell.

[0058] [Figure 16] FIG. 1 shows XRD of SiC / C before and after mixing with graphite.

[0059] [Figure 17A] FIG. 1 shows an SEM image of graphite. [Figure 17B] FIG. 1 shows an SEM image of SiC / C after mixing with 10 wt.% graphite.

[0060] [Figure 18A]FIG. 1 shows representative voltage profiles for the 1st and 2nd cycles at 0.1 C and the 1st cycle at 0.5 C, 1 C and 2 C for a graphite / Li half-cell; and specific capacity versus cycle number. [Figure 18B] FIG. 1 shows representative voltage profiles for the 1st and 2nd cycles at 0.1 C and the 1st cycle at 0.5 C, 1 C and 2 C for a SiC / C half-cell; and specific capacity versus cycle number. [Figure 18C] FIG. 1 shows representative voltage profiles for the 1st and 2nd cycles at 0.1 C and the 1st cycle at 0.5 C, 1 C and 2 C for SiC / C and 10 wt.% graphite half-cells; and specific capacity versus cycle number. [Figure 18D] FIG. 1 shows representative voltage profiles for the 1st and 2nd cycles at 0.1 C and the 1st cycle at 0.5 C, 1 C and 2 C for SiC / C and 30 wt.% graphite half-cells; and specific capacity versus cycle number.

[0061] [Figure 19A] FIG. 1 shows SEM images of cross sections of SiC / HC electrodes prepared according to certain embodiments of the present disclosure (top SEM image has a scale bar of 20 micrometers, magnified portion shown in bottom SEM has a scale bar of 2 micrometers). [Figure 19B] FIG. 1 shows a CV scan curve of a SiC / HC electrode. [Figure 19C] FIG. 1 shows charge / discharge curves of a SiC / HC electrode. [Figure 19D] FIG. 1 shows specific capacity versus cycle number for SiC / HC and SiC / O electrodes. [Figure 19E] FIG. 13 shows Nyquist plots (equivalent circuit model) of a SiC / HC half-cell before and after 300 and 600 cycles at 0.1 C (inset: equivalent circuit shown). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0062] Corresponding reference numerals indicate corresponding parts throughout the several views of the drawings.

[0063] Exemplary embodiments are presented so that this disclosure will be thorough and fully convey the scope to those skilled in the art. Many specific details are presented, such as examples of specific compositions, components, devices and methods, to achieve a complete understanding of the embodiments of the present disclosure. It will be apparent to those skilled in the art that specific details must be employed, that the exemplary embodiments may be implemented in many different forms, and that none of these should be construed as limiting the scope of the present disclosure. In some exemplary embodiments, well-known methods, well-known device structures, and well-known technologies are not described in detail.

[0064] The terminology used herein is intended to describe only certain example embodiments and is not intended to be limiting. As used herein, the singular forms "a," "an," and "the" may be intended to include the plural forms unless the context clearly dictates otherwise. The terms "comprises," "comprising," "including," and "having" are inclusive and thus specify the presence of a stated configuration, element, composition, step, integer, operation, and / or component, but do not preclude the presence or addition of one or more other configurations, integers, steps, operations, elements, components, and / or groups thereof. The open-ended term "comprising" should be understood as a non-limiting term used to describe and claim various embodiments set forth herein, although in certain aspects, this term may be understood to be a more restrictive, restrictive term such as "consisting of" or "consisting essentially of." Thus, for any embodiment reciting compositions, materials, components, elements, configurations, integers, operations, and / or steps, the present disclosure specifically includes embodiments that consist of or consist essentially of such recited compositions, materials, components, elements, configurations, integers, operations, and / or steps. In the case of "consisting of," alternative embodiments exclude any additional compositions, materials, components, elements, configurations, integers, operations, and / or steps, whereas in the case of "consisting essentially of," any additional compositions, materials, components, elements, configurations, integers, operations, and / or steps that would materially affect the basic and novel characteristics are excluded from such embodiments, but any compositions, materials, components, elements, configurations, integers, operations, and / or steps that do not materially affect the basic and novel characteristics may be included in the embodiments.

[0065] Any steps, processes, and operations described herein should not be construed as necessarily requiring them to be performed in the particular order discussed or illustrated, unless specifically identified as an order of performance. It should also be understood that additional or alternative steps may be employed, unless otherwise specified.

[0066] When a member, element, or layer is referred to as "on," "engaged with," "connected to," or "coupled to" another element or layer, it may be directly on, engaged with, connected to, or coupled to the other member, element, or layer, or there may be intervening elements or layers present. In contrast, when an element is referred to as "directly on," "directly engaged with," "directly connected to," or "directly coupled to" another element or layer, there may not be intervening elements or layers present. Other words used to describe relationships between elements should be interpreted similarly (e.g., "between" vs. "directly between," "adjacent" vs. "directly adjacent," etc.). As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.

[0067] Terms such as first, second, third, etc. may be used herein to describe various steps, elements, components, regions, layers, and / or sections, but these steps, elements, components, regions, layers, and / or sections should not be limited by these terms unless otherwise specified. These terms may be used only to distinguish one step, element, component, region, layer, or section from another step, element, component, region, layer, or section. Terms such as "first", "second", and other numerical terms, when used herein, do not imply any order or sequence unless clearly indicated by the context. Thus, without departing from the teachings of the exemplary embodiments, a first step, element, component, region, layer, or section discussed below can be referred to as a second step, element, component, region, layer, or section.

[0068] Spatial or temporal relationship terms, such as "in front of," "after," "inside," "outside," "below," "below," "lower," "on," "belowside," and the like, may be used herein for ease of description to describe the relationship of one element or structure to another element(s) or structure(s), as illustrated in the figures. Spatial or temporal relationship terms may be intended to encompass various orientations of a device or system in use or operation in addition to the orientation depicted in the figures.

[0069] Throughout this disclosure, numerical values ​​represent approximate measurements or range limits to include slight deviations from a given value and embodiments with just the stated value as well as those with the vicinity of the stated value. Except for the examples shown at the end of the detailed description, any numerical value of a parameter (e.g., amount or condition) in this specification, including the appended claims, should be understood as being modified by the term "about" in all cases, regardless of whether "about" is actually displayed before the numerical value. "About" indicates that the stated numerical value allows for some imprecision (somewhat close to the precision of the value; approximately or somewhat close to the value; approximately). When the imprecision introduced by "about" is not understood in this ordinary sense in the art, "about" as used herein indicates at least the deviation that may result from the ordinary method of measuring and using such parameters. For example, "about" may include deviations of 5% or less, optionally 4% or less, optionally 3% or less, optionally 2% or less, optionally 1% or less, optionally 0.5% or less, and in certain embodiments, optionally 0.1% or less.

[0070] Additionally, disclosure of a range includes disclosure of every value within the entire range, as well as divided ranges, including the endpoints and subranges given for that range.

[0071] Example embodiments will now be described more fully with reference to the accompanying drawings.

[0072] In various embodiments, the present disclosure relates to a method for forming silicon carbide (SiC), silicon nitride (Si3N4), and / or silicon oxynitride (Si2N2O) from silica-deficient rice husk / rice husk ash products. In various embodiments, the present disclosure contemplates rice husk as the preferred source of silicon and carbon, but other biogenic silica and carbon sources (biomass, e.g., coconut husk), including grasses that absorb SiO2 into their stems and seed shells (e.g., wheat, rice, corn, barley, oats, etc.), may also be used and processed as described herein. Rice husk (RH) has the highest silica content of any grass. Thus, ashes from these other biogenic sources are contemplated for alternative variations. Waste starting materials for producing SiC and Si3N4 can offer several advantages: (1) environmental benefits related to reduced carbon footprint; (2) economical disposal of waste materials; (3) improved properties resulting from reduced product particle size made possible by starting production using nanoscale mixtures, and (4) economies in energy and capital equipment costs due to reduced processing temperatures and times.

[0073] Combustion followed by stoichiometric alkaline treatment is a common conventional method (reaction 1) to extract SiO2 from RHA to produce silica-deficient RHA or SDRHA. Rice husk ash SiO2+M-OH -> SiO2 deficient rice husk ash (1).

[0074] However, this two-step process defeats the inherent advantage of intimately (nanoscale) mixed carbon and SiO2 that enables the low-cost production of SiC and Si3N4 from RHA. Furthermore, trace minerals present in the RHA remain in the SDRHA, leading to relatively high levels of impurities in the products formed.

[0075] The present disclosure provides a new method for forming silicon carbide (SiC), silicon nitride (Si3N4), and / or silicon oxynitride (Si2N2O) using acid-refined rice husk ash (RHA) processed to have a beneficially controlled silica content in a silica-deficient rice husk ash product (SDRHA). More specifically, the method advantageously enables a carbothermal reduction reaction to be performed using a silica-deficient rice husk ash product (SDRHA) having a beneficially controlled silicon and carbon content without the need to add an external carbon source. The method of the present invention is achieved by controlling the silica (SiO2) content in the silica-deficient rice husk ash product (SDRHA) to arrive at a SRDHA precursor having a sufficiently high carbon content such that the precursor can be heated at a relatively low temperature in a direct carbothermal reduction reaction to form a product comprising at least one of silicon carbide (SiC), silicon nitride (Si3N4), and silicon oxynitride (Si2N2O). In the past, in contrast to the techniques of the present invention, carbon had to be added to carefully adjust the stoichiometric ratio of SiO2:C. Furthermore, whereas in conventional methods the particle size of the reactants was at most micron-sized, in various embodiments the reactants used in the present disclosure may all be nanoscale, e.g., having at least one spatial dimension that is less than about 1 micrometer (i.e., 1,000 nm).

[0076] For example, rather than introducing additional carbon from an external source as has been required in the past, the SiO2:C ratio is optimized by removing SiO2 from the RHA by distillation to produce SDRHAs with different SiO2:C ratios while also removing typical impurities. The present disclosure provides a method for producing distillable spirosiloxanes by the reaction (2): [ka] The intention is to remove SiO2 from the RHA by forming a spirosiloxane (shown above) {[(CH3)2C(O)CH2CH(O)CH3)]2Si}, which is a nanocomposite mixture of SiO2:C approximately 90:10, with careful control of the molar ratio of C:SiO2 to allow for direct carbothermal reduction to form SiC, Si3N4, or Si2N2O, without the need for additional carbon addition and as a mechanism to maintain the original nanocomposite structure. Notably, extraction of SiO2 from the RHA to form spirosiloxanes can also be achieved with other hindered glycols, such as 2,2,4-trimethyl-1,3-pentanediol.

[0077] The RHA may be first washed with an acid. In one variation, the rice husk ash (RHA) may be milled with an acid (e.g., using milling or grinding media) for washing to remove impurities. The acid may be a dilute acid such as hydrochloric acid, sulfuric acid, phosphoric acid, and combinations thereof. In one variation, dilute hydrochloric acid may be used. In a particular variation, the dilute acid may be present in the solution at about 20% by weight or less, optionally about 12% by weight or less, optionally about 10% by weight or less, optionally about 1% by weight or more to about 12% by weight or less, in one variation, optionally about 1% by weight or more to about 10% by weight or less, or in another variation, optionally about 5% by weight or more to about 12% by weight or less.

[0078] The milled and acid washed RHA may then be washed with boiling water in at least one wash cycle, and possibly multiple wash cycles. The pre-washing of the RHA with acid and boiling water using milling is advantageous in that it removes typical product impurities found in the RHA compared to those found in conventional agricultural waste precursors, which can result in a very pure product after conventional carbothermal reduction. Milling the RHA in dilute acid followed by washing with boiling water results in an SDRHA with very low impurity levels to the extent that it is possible to process solar grade silicon (99.999% pure) from the SDRHA. In certain embodiments, the SDRHA has about 1% or less by weight of undesirable impurities, sometimes about 0.5% or less by weight, sometimes about 0.1% or less by weight, such as minerals, multi-metallic, boron, and aluminum, and in certain variations, it may be as low as about 0.01% by weight or less than about 1 ppm.

[0079] Thus, the disclosed method produces the desired SiC, Si3N4 and SiN after carbothermal reduction in the absence of an added carbon source. x O 4-x It is contemplated that the silicon and carbon content derived from the RHA is adjusted to form a silica deficient rice husk ash (SDRHA) having a range of silicon and carbon contents that can advantageously form a product (x ranging from 0 to 4).

[0080] In certain embodiments, the treated silica-deficient rice hull ash (SDRHA) comprises from about 10% to about 60% carbon by weight based on the total weight of the SDRHA, and optionally from about 40% to about 60% carbon by weight based on the total weight of the SDRHA. Thus, the treated SDRHA may have from about 20% to about 65% silicon by weight based on the total weight of the SDRHA, and optionally from about 35% to about 60% carbon by weight based on the total weight of the SDRHA.

[0081] The silicon to carbon content may reflect the ratio of moles of silicon dioxide or silica (SiO2) to moles of carbon. The SiO2:C ratio may be adjusted by reacting the initial acid-washed RHA material with a hindered diol in the presence of a catalytic base and removing excess SiO2 by distillation to produce a treated SDRHA having a desired silica to carbon ratio. For example, the treated SDRHA may have a SiO2 to carbon ratio (SiO2:C) of about 1:8 to about 1:3, and in some cases about 2:15 to about 13:35.

[0082] Suitable hindered diols for treating the RHA to adjust the silicon and carbon content may be selected from the group consisting of 2-methyl-2,4-pentanediol (hexylene glycol), 2,2,4-trimethyl-1,3-pentanediol, and combinations thereof. In certain embodiments, combinations of hindered diols may be used, including those just listed above, and optionally further including ethane-1,2-diol. In one embodiment, the hindered diol comprises 2-methyl-2,4-pentanediol (hexylene glycol).

[0083] Suitable catalytic bases may include those selected from the group consisting of sodium hydroxide (NaOH), lithium hydroxide (LiOH), calcium hydroxide Ca(OH)2, potassium hydroxide (KOH), cesium hydroxide (CsOH), rubidium hydroxide (RbOH), and combinations thereof.

[0084] In one particular variation, the SDRHA is formed from the RHA by using a hindered diol comprising 2-methyl-2,4-pentanediol and a catalytic base comprising sodium hydroxide (NaOH).

[0085] In various embodiments, the method includes the steps of: forming a silicon carbide (SiC), silicon nitride (Si3N4) and silicon oxynitride (SiN x O 4-x%, or more than about 65% by weight of silicon oxide and about 35% by weight of carbon, in an environment having a temperature of about 1,200° C. or more and an inert or reducing atmosphere and no additional carbon source, to form a product comprising at least one of the following: (a) a silica-deficient rice hull ash product (SDRHA) having about 65% by weight or less of silicon oxide and about 35% by weight or more of carbon, for a carbothermal reaction to form a product comprising at least one of the following: (a) a silica-deficient rice hull ash product (SDRHA) having about 65% by weight or less of silicon oxide and about 35% by weight or more of carbon, in an environment having a temperature of about 1,200° C. or more and an inert or reducing atmosphere and no more than about 1,700° C. The heating may be performed in a furnace, for example an electric arc furnace.

[0086] An environment free of external or additional carbon sources means that the only carbon source comes from the SDRHA used as precursor. Trace amounts of carbon may be present in the ambient air, for example as carbon monoxide (CO), but generally such amounts of carbon are limited, for example, to about 0.1% by weight or less. An inert or reducing atmosphere means that the gas atmosphere generally does not contain reactive non-carbon-containing oxidant species, such as oxygen-containing species (e.g., O2, NOx, etc.). Suitable inert or reducing atmospheres include, for example, nitrogen (N2), argon (Ar), and / or N2 / H2. In certain embodiments, the carbon source essentially consists of or consists of the SDRHA in the carbothermal reaction process.

[0087] The reactants may be provided with thermal energy and / or microwave energy to achieve carbothermal reduction. In certain variations, during the carbothermal reduction process, the environment is heated to a temperature of about 1,400° C. or more and about 1,600° C. or less, optionally in certain variations about 1,400° C. or more and about 1,500° C. or less. The reactants may be exposed to these temperatures for a duration of about 6 hours or more, optionally about 7 hours or more, optionally about 8 hours or more, optionally about 9 hours or more, and in certain variations, optionally about 10 hours or more.

[0088] After heating for carbothermal reduction, the product formed is about 50% by weight or more, optionally about 65% by weight or more, optionally about 75% by weight or more, and in certain embodiments, optionally about 80% by weight or more silicon carbide (SiC) or Si3N4 or SiN x O 4-x may be included in certain variations.

[0089] As described above, the RHA / SDRHA has a nanocomposite structure after processing, which is generally maintained after the heating and carbothermal reduction process that can form a composite or nanocomposite product. In certain variations, a nanocomposite is a structure that includes a primary phase or matrix with a plurality of nanostructures distributed therein. The nanostructures may include "nano-sized" or "nanometer-sized" particles having at least one spatial dimension that is less than about 1 μm (i.e., 1,000 nm), optionally less than about 0.5 μm (i.e., 500 nm), optionally less than about 0.4 μm (i.e., 400 nm), optionally less than about 0.3 μm (i.e., 300 nm), optionally less than about 0.2 μm (i.e., 200 nm), and in certain variations, optionally less than about 0.1 μm (i.e., 100 nm). Thus, the nanoparticle component has at least one spatial dimension that is greater than about 1 nm and less than about 1,000 nm (1 μm). It should be noted that as long as at least one dimension of the nanoparticle is within the nano-sized scale described above (e.g., diameter), one or more other axes may be much larger than nano-sized (e.g., length and / or width). In certain variations, the nanocomposite is a silicon oxynitride (SiN) nanoparticle having a plurality of nanostructures distributed therein. x O 4-x The nanostructure may include phases including silicon carbide (SiC) and silicon nitride (Si3N4), where x is in the range of 0 to 4. For example, whiskers appear as long rod-like structures intertwined with more rounded particles including the co-formed SiC and Si3N4 particles and residual carbon. The formed product may also include other components such as residual carbon (e.g., hard carbon) and / or unreacted or partially reacted silica (e.g., cristobalite). The product may be processed for oxidative removal of carbon in certain variants. Si2N2O and / or non-stoichiometric SiN present in the final product may be removed by oxidative removal of carbon. x O 4-xThe amount of oxygen (where x ranges from greater than 0 to less than 4) is related to the duration and / or temperature of heating in the carbothermal reduction reaction that is performed, with longer durations and / or higher temperatures resulting in less oxygen (thus favoring the formation of silicon carbide and silicon nitride rather than silicon oxynitride). By controlling or minimizing the amount of nitrogen present in the environment, the preferential formation of silicon carbide during the carbothermal reduction reaction can be controlled, such that a lower nitrogen content favors the formation of SiC, while a higher nitrogen content in the environment will favor the formation of Si3N4 as well as Si2N2O and / or non-stoichiometric SiN in addition to SiC. x O 4-x In one variation, the carbothermal reduction product formed by the method of the invention comprises about 75% by weight or more silicon carbide (SiC). In another variation, the carbothermal reduction product formed by the method of the invention comprises about 75% by weight or more silicon nitride (Si3N4). In yet another variation, the carbothermal reduction product formed by the method of the invention comprises about 75% by weight or more Si2N2O and / or non-stoichiometric SiN x O 4-x where x ranges from 0 to 4. In certain embodiments, composites formed according to certain embodiments of the present disclosure include Si2N2O and / or non-stoichiometric SiN x O 4-x as the major phase, for example at about 80 wt % or more, which can be produced by heating SDRHA under a N2 / H2 atmosphere.

[0090] In certain embodiments, the product formed by the methods of the present disclosure may be a mixture of SiC nanostructures, such as round or agglomerated particles of SiC, and axially shaped particles of SiC (e.g., whiskers, cylinders, wires, etc., having a distinct long axis). In certain variations, the nanostructures comprising SiC are about 10 mm in diameter. 2 / g or more, in some cases about 20m 2 / g or more, in some cases about 30m 2 / g or more, and in certain variants, in some cases about 40m 2The SiC may have a BET specific surface area (SSA) of about 44 m / g or more. In one variation, the SSA of the SiC is about 44 m 2 / g. Axial shaped particles (e.g., whiskers) of SiC may have diameters of about 100 nm to about 140 nm with lengths up to about 5 μm. Round or agglomerated particles of SiC may have average diameters of about 10 nm to about 200 nm.

[0091] In a particular variation, the nanostructure including Si3N4 has a thickness of about 10 m. 2 / g or more, in some cases about 20m 2 / g or more, and in certain variants, sometimes about 25m 2 In one variation, the SSA of Si3N4 is about 30 m / g or more when heated at 1400-1500° C. for 4-8 hours. 2 The Si3N4 particles may be in the form of irregular agglomerates mixed with many long whiskers having an average diameter of about 100 nm to about 200 nm and a length of several micrometers.

[0092] In certain other variations, the nanostructures comprising Si2N2O have a thickness of about 1 m. 2 / g or more, in some cases about 3m 2 / g or more, in some cases about 5m 2 / g or more, and in some variants, up to about 9m 2 In one variation, the SDRHA may have a BET specific surface area (SSA) of 100 / g or more. 65 When heated in a 95% N2-5% H2 atmosphere at 1500°C for 8 hours, the SSA of Si2N2O was approximately 10m 2 / g.

[0093] When carbon is present in the nanocomposite, the nanocomposite is about 150 m 2 / g or more, in some cases about 175m 2 / g or more, in some cases about 200m 2 / g or more, and in some variants, about 220m 2 / g or more.

[0094] The method of the present invention provides a more environmentally friendly and economical method that can remove trace impurities, for example, limiting the amount of alkali metals to reduce their presence as impurities, while advantageously adjusting the SiO2 content to enhance the carbon content while maintaining the microstructure in the nanocomposite product formed.

[0095] In certain variations, the present disclosure contemplates electroactive materials for electrodes of electrochemical cells, such as lithium ion batteries, formed according to certain aspects of the present disclosure. The electroactive materials may be used in the negative or positive electrodes. In certain variations, the electrodes may be porous composite electrodes, in which the electroactive materials and optional additional solid components are mixed together and distributed in a polymer binder to provide additional mechanical integrity to the electrode.

[0096] Suitable polymer binders may include polyvinylidene fluoride (PVdF), polyacrylic acid (PAA), polyamic acid, polyamide, polyimide, polysulfone, polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene, carboxymethylcellulose (CMC), ethylene propylene diene monomer (EPDM) rubber, nitrile butadiene rubber (NBR), styrene-butadiene rubber (SBR), lithium polyacrylate (LiPAA), sodium polyacrylate (NaPAA), lithium alginate, and / or sodium alginate. Additional particulate components may include conductive materials. In certain variations, the additional particulate material may be a carbon-containing material such as carbon black or graphite.

[0097] As will be appreciated by one of ordinary skill in the art, the electrochemical cell may further include, among other components, a negative electrode current collector in electrical communication with the negative electrode, a positive electrode, a positive electrode current collector in electrical communication with the positive electrode, an electrolyte, and an optional separator (when the electrolyte comprises a liquid electrolyte).

[0098] In one variation, the electroactive material is silicon carbide and / or silicon oxynitride (SiNO, and / or non-stoichiometric SiN x O 4-x (wherein x is greater than 0 and less than 4).

[0099] In certain embodiments, the electroactive material is silicon oxynitride (SiNO, and / or non-stoichiometric SiN x O 4-x The nanocomposite may further include a pyrolyzed carbon-based material (e.g., hard carbon). In certain variations, the electroactive material may include a product that is a composite including Si2N2O and one or more of hard carbon, SiC, and / or Si3N4 distributed therein. Thus, the nanocomposite may include a silicon oxynitride (Si2N2O and / or non-stoichiometric SiN x O 4-x Such nanocomposites may also include hard carbon and possibly trace amounts of silica (SiO2) or SiC. In certain embodiments, silicon oxynitride (Si2N2O) or nonstoichiometric SiN x O 4-x is formed by any of the processes described above. For example, the process may include heating a silica-deficient rice hull ash product (SDRHA) containing about 65% by weight or less silicon oxide and about 35% by weight or more carbon in an environment containing no additional carbon source but an inert atmosphere having nitrogen present and having a temperature of about 1,200° C. or more and about 1,700° C. or less.

[0100] In certain variations, the electroactive material has a high purity level (because the precursor RHA is acid washed and boiled) and may be, for example, silicon carbide (SiC) and / or silicon oxynitride (SiNO, and / or non-stoichiometric SiN x O 4-xwherein x is greater than 0 and less than 4.

[0101] In another variation, the electroactive material of the negative electrode may include SiC, hard carbon, or Si3N4 and hard carbon.

[0102] In a particular variation, an electroactive material for a negative electrode of an electrochemical cell for circulating lithium ions is provided. The electroactive material is silicon oxynitride (Si2N2O, or nonstoichiometric SiN x O 4-x where x is greater than 0 and less than 4. The electroactive material includes silicon oxynitride (Si2N2O, or nonstoichiometric SiN x O 4-x In certain other embodiments, the nanocomposite may include a nanocomposite having a phase comprising silicon oxynitride (Si2N2O, or nonstoichiometric SiN x O 4-x (wherein x is greater than 0 and less than 4) and further comprises at least one of silicon carbide (SiC) and silicon nitride (Si3N4) distributed in the phase comprising the compound.

[0103] In one variation, silicon oxynitride (SiNO, or non-stoichiometric SiN x O 4-x (wherein x is in the range of from 0 to 4) is formed by heating a silica-deficient rice hull ash product (SDRHA) containing about 65% by weight or less of silicon oxide and about 35% by weight or more of carbon in an environment containing an inert atmosphere without an additional carbon source but having nitrogen present and having a temperature of about 1,200° C. to about 1,700° C. for a carbothermal reaction.

[0104] In certain embodiments, the silicon oxynitride comprises Si2N2O. In certain other embodiments, the silicon oxynitride comprises non-stoichiometric SiN x O 4-x and x is in the range of greater than 0 and less than 4.

[0105] Electrodes including such electroactive materials may further include graphite. In certain variations, by way of non-limiting example, the electrodes may further include conductive materials such as carbon black particles. Additionally, the electrodes may also include a polymer binder in which the electroactive material and optional graphite particles, optional conductive particles such as carbon black, etc. may be mixed and / or distributed.

[0106] In yet another variation, an electroactive material for a negative electrode of an electrochemical cell for circulating lithium ions is provided, wherein the electroactive material is silicon oxynitride (Si2N2O, or nonstoichiometric SiN x O 4-x (wherein x is greater than 0 and less than 4) and / or silicon carbide (SiC). In certain variations, the nanocomposite includes silicon oxynitride (SiNO, or non-stoichiometric SiN x O 4-x (wherein x is greater than 0 and less than 4) and further comprises at least one of silicon carbide (SiC) and silicon nitride (Si3N4) distributed in the phase comprising the compound.

[0107] In certain variations, the nanocomposite further comprises a pyrolyzed carbon-based material. In one embodiment, the nanocomposite comprises silicon carbide (SiC). In such variations, silicon carbide (SiC) distributed in a hard carbon material (e.g., pyrolyzed carbon formed in a carbothermal process) can result. As a non-limiting example, SDRHA-derived SiC with hard carbon (HC-SiC / HC) or after oxidation of hard carbon (SiC / O) can result in lithium-ion batteries with gradually increasing capacity, as a non-limiting example, reaching more than 950 mAh / g and more than 740 mAh / g, respectively, after 600 cycles. It is believed that two different SiC morphologies, particles and whiskers, can result, which are believed to result from different simultaneous reaction mechanisms during carbothermal reduction. For example, in one variation, the BET specific surface area (SSA) is approximately 204 m for SiC / HC and 200 m for SiC / O.2 / g, and for SiC after oxidative removal of hard carbon at 500°C / 1h / O2 (forming SiC / O) is approximately 42m 2 / g. The broad pore size distribution of SiC / HC peaks at about 17-24 nm, whereas no peak is observed for SiC / O. Hard carbons typically exhibit a high degree of cross-linking that gives rise to the formation of nanopores within the disordered structure.

[0108] Comparing other known SiC-based electrodes with those formed according to certain embodiments of the present disclosure (SiC / HC composites derived from SDRHA), one or more of the following advantages are provided: (1) the electroactive material prepared according to certain embodiments of the present disclosure maintains a relatively high capacity compared to other reported SiC materials; (2) the electroactive material prepared according to certain embodiments of the present disclosure can be used at a commercial level, although it is easily manufactured by a "low temperature process" (e.g., 1450°C) of carbothermal reduction of agricultural waste, often landfilled; (3) RHA is a by-product of RH combustion, and the United States alone simultaneously produces 200 gigawatts and 200 kilotons of RHA annually. Assuming that rice cultivation fixes CO2, this process is at least carbon neutral, and may be carbon negative if the landfilled RHA produces CH4 / CO2 that is then released into the atmosphere.

[0109] SEM shows the microstructure of pristine and cycled SiC / HC and SiC / O electrodes, both with larger grain sizes (~2 to ~10 μm) after 600 cycles, indicating a stable and robust SEI layer remains upon extended cycling. Whiskers also remain, although not a dominant feature. Overall, the electrodes maintain their integrity on aging without significant volume change, suggesting that the cubic to hexagonal phase transition does not alter the pristine SiC electrode structure and / or morphology. Furthermore, post-mortem characterization of the cycled electrodes shows a partial phase transformation from cubic (3C) to hexagonal (6H) SiC, with no significant volume change or surface cracks seen in SEM. Elements Si, Li x Si or Li xNo C was observed, suggesting limited lithiation of SiC by intercalation rather than conversion or alloying reactions. These results are in stark contrast to Si electrodes, which suffer from pulverization and reduced cycle life due to the large volume changes that occur during cycling.

[0110] In another embodiment, the silicon oxynitride comprises Si2N2O. In yet another embodiment, the silicon oxynitride comprises non-stoichiometric SiN x O 4-x and x is in the range of greater than 0 and less than 4.

[0111] An electrode comprising such an electroactive material may further comprise graphite. The electrode may also further comprise a polymer binder.

[0112] Various embodiments of the present technology can be further understood by the specific examples contained herein, which are presented for the purpose of illustrating how to make and use the compositions, devices and methods according to the teachings of the present invention. EXAMPLES

[0113] (example)

[0114] (Example 1)

[0115] SDRHA was synthesized as described in Marchal, J. et al., "A Low Cost, Low Energy Route to Solar Grade Silicon from Rice Hull Ash (RHA), a Sustainable Source," Green Chemistry, 17(7), pp. 3931-3940 (2015), the relevant portions of which are incorporated herein by reference. In particular, the relevant portions of any further references described herein are expressly incorporated by reference. Briefly, rice hull ash (RHA) was first milled in dilute hydrochloric acid to remove impurities. RHA (200 g) was placed in a 2 L jar containing 200 g of milling media and 2 L of HCl solution (3.7 wt.% HCl). The grinding media was yttria-stabilized zirconia, spheres with a diameter of 3 mm. The RHA was milled for 48 hours. The acid-milled RHA was then collected by suction filtration through a Buchner funnel and then washed with 500 mL of DI water.

[0116] The acid milled RHA and 1 L of DI water were then introduced into a 2 L glass flask equipped with a stir bar and reflux condenser. The suspension was then boiled for 24 hours before isolation by filtration in a Buchner funnel. The boiling and filtering process was repeated once more. After the second filtration, the pH of the filtered water was neutral. The RHA was then dried at 100° C. / vacuum overnight.

[0117] A mixture of diol (250 mL of hexylene glycol (HG)) and catalyst (4.2 g of KOH (75 mmol)) was first heated to 190° C. in a 250 mL three-necked flask equipped with a stir bar to remove water for 3 hours. Dried RHA powder (approximately 50 g) was added to the HG+KOH solution. The mixture was heated to 200° C. in a Pyrex distillation apparatus. After 100 mL of HG was distilled, another 100 mL of HG was added.

[0118] Synthesis of SDRHA

[0119] FIG. 1A shows that the RHA contains amorphous SiO2 and carbon before and after SiO2 extraction, while EDX analysis shows that SiO2 and carbon are not present in the SDRHA (60 wt.% SiO2, SDRHA 60 The results confirm that the RHA morphology is intimately mixed at the nanoscale in the SDRHA (denoted as SDRHA). Thus, the prerequisites for effective carbothermal reduction at relatively low temperatures, e.g., milling of amorphous SiO2 and carbon sources in conventional manufacturing processes, are met without any special efforts. SEM images (Figures 1B and 1C) show that the RHA morphology is similar to that of the SDRHA. 60 It shows that the SDRHA 60 The majority of the particles in are in the 1-10 μm range. Furthermore, as discussed below, a highly porous network is visualized in the SEM images.

[0120] The as-received RHA used in the examples contains approximately 90 wt.% SiO2. The detailed SDRHA synthesis procedure was reported in Marchal, J. et al., "A Low Cost, Low Energy Route to Solar Grade Silicon from Rice Hull Ash (RHA), a Sustainable Source," Green Chemistry, 17(7), pp. 3931-3940 (2015). Briefly, the first step is to mill the as-received RHA in dilute acid, followed by washing with boiling water, which removes most of the mineral impurities. In the next step, the dried RHA is reacted with a hindered diol (hexylene glycol) using a catalytic amount of potassium hydroxide. As seen in the XPS wide survey in Figure 2A, the SDRHA 60The spectrum shows only the signature peaks of C 1s, Si 2s, Si 2p, and O 1s. Figure 2B shows the representative TGA of the acid washed / dried RHA and SDRHA after the distillation part at 25-600 °C under air, showing the respective SiO2 contents. No obvious mass loss was observed after the carbon oxidation was completed at approximately 480 °C, and 60 wt.% SiO2 was observed in SDRHA. 60 The BET SSA suggests that the remaining 2 / g to SDRHA 60 Approximately 345m 2 / g, while the BET SSA of SDRHA increased to about 440, about 420, about 370, and about 220 m 2 / g. Figure 2C shows typical N2 adsorption / desorption isotherms for RHA and SDRHA. The plot features correspond to type IV with H3 hysteresis in the IUPAC classification, which is probably due to the porous network in the soft aggregates of plate-like particles.

[0121] In one example, SDRHA 40-65 (having 40-65 wt. % silica) may be heated at 1400-1500 °C in an Ar, N2, or N2 / H2 atmosphere, which produces SiC, Si3N4, or Si2N2O and / or non-stoichiometric SiN, along with some residual carbon and in some cases of incomplete conversion to cristobalite. x O 4-x (x ranges from 0 to 4). SEM examination shows a mixture of particles and whiskers in these products, which are approximately 40 mm in diameter. 2 / g or more.

[0122] Synthesis of SiC, Si3N4 and Si2N2O composites

[0123] The treated SDRHA powders formed as above were placed in a graphite crucible and covered with an alumina disk, which was then heated to various temperatures and times at a heating rate of 10° C. / min under Ar, N2, or N2 / H2 mixtures.

[0124] Nanocomposites from SDRHA via carbothermal reduction

[0125] Carbothermal reduction studies. Conventional carbothermal reduction requires milling a SiO2 source with a carbon source as a first step. In contrast, SDRHA 40-65 contains SiO2 / C nanocomposites recovered from the distillative removal of SiO2. Therefore, they can be heated directly. Figure 3A shows the SDRHA at 1400-1500 °C under Ar. 60 Figure 3C shows the XRD of SiC obtained from heating 1500°C under Ar for 2, 4, 5, 6 and 8 hours. The peaks at 2θ 36°, 42°, 60° and 72° are associated with the (111), (200), (220) and (311) planes of β-SiC (3C-SiC, PDF 01-073-1708). The weak shoulder at 33.5° corresponds to stacking faults. Upon heating to 1450 and 1430°C, a peak assigned to the (101) plane of cristobalite at 2θ 22° appears, corresponding to approximately 5 and 20 wt.% cristobalite in the product, respectively. Figure 3B compares the XRD obtained from heat treatment at 1500°C under Ar for 2, 4, 5, 6 and 8 hours. No cristobalite or other SiO2 phases are seen for reaction times beyond 5 hours. When the heat treatment is limited to 4 hours, the main product is SiC with approximately 3 wt.% cristobalite. PDXL XRD analysis software was used to determine the crystalline phases listed in Table 1. [Table 1] The effect of SiO2 / C ratio was also investigated. Previous studies have shown that temperatures below 1400 °C are not favorable for the carbothermal reduction and nitridation of RHA. The known reactions involved in the carbothermal synthesis of SiC are as follows: SiO2(s)+C(s)→SiO(g)+CO(g) SiO(g)+3CO(g)→SiC(s)+2CO2(g) SiO(g)+2C(s)→SiC(s)+CO(g) CO2(g) + C(s) → 2CO(g).

[0126] Conventional carbothermal reduction requires excess carbon to promote complete conversion of SiO2 to SiC. The corresponding molar ratio of SiO2:C is lower than the stoichiometric ratio of 1:3. SDRHA prepared according to certain embodiments of the present disclosure 40,50,55,60 The materials exhibit SiO2:C molar ratios of 2:15, 1:5, 11:45, and 3:10, respectively, which meet the excess carbon criterion. 40,50 Heating in the SDRHA results in the formation of approximately 88 and 79 wt.% SiC, respectively, while heating in the SDRHA 60 yields approximately 16 wt.% (Table 2).

[0127] The trend for more carbon in the starting material to result in higher percentage of SiC in the product is consistent with previously reported studies in which excess carbon promoted increased yields of SiC, and is also consistent with reaction kinetics, where a higher concentration of a given reactant will make a given reaction proceed faster.

[0128] The detection of two crystalline SiO2 phases in the product heated at 1400 °C suggests an incomplete conversion of quartz to cristobalite, which has been reported to occur over temperatures between 1100 and 1400 °C. Furthermore, it is well recognized that carbon catalyzes the reduction of SiO2 to SiO, thereby initiating the steam-steam reaction between SiO and C / CO rather than solid-state reactions alone, ultimately leading to lower SiC formation temperatures. All these factors drive the trend shown in Table 2, with higher SiC yields resulting from higher initial carbon content at 1400 °C. [Table 2]

[0129] SDRHA heated under N2 60XRD analysis of the SiN4 confirmed the formation of α-Si3N4 shown in Figures 4A-4B. No peaks due to SiO2 or SiC were observed, and impurities commonly found in Si3N4 produced by carbothermal nitridation were observed, indicating that the SiN4 produced by SDRHA at 1400 °C / N2 / 8 h (Figure 4A) or 1500 °C / N2 / 4 h (Figure 4B) was 60 The XRD in Figure 4B shows the complete nitridation of SiO2 upon heating. However, the SiO2 / C ratio significantly affects the reaction. 65 It is shown that the products derived from (SiO2:C molar ratio = 13:35) include Si3N4, Si2N2O, SiC and cristobalite (Table 3). The intensity of the peak assigned to cristobalite at 2θ = 22° decreases with increasing heating time and is negligible (0%) after 8 hours, indicating complete carbonitridation of SiO2 by: 3SiO2(s)+6C(s)+2N2(g)→Si3N4(s)+6CO(g) 3SiO(g)+3C(s)+2N2(g)→Si3N4(s)+3CO(g)

[0130] The relative compositions of Si3N4 and SiC are due to the secondary reaction: 3SiC(s)+2N2(g)→Si3N4(s)+3C(s) Correlated with. [Table 3]

[0131] Similar to SiC and Si3N4, silicon oxynitride (Si2N2O) is another product of carbothermal reduction and nitridation reactions, which is a refractory material with high chemical and oxidation resistance. Theoretically, the stoichiometric SiO2:C molar ratio is: 2SiO2(s)+3C(s)+N2(g)→Si2N2O(s)+3CO(g) where prolonged treatment time results in further reduction of oxygen in Si2N2O to form Si3N4: 3Si2N2O(s)+3C(s)+N2(g)→2Si3N4(s)+3CO(g).

[0132] As mentioned above, residual additives are present in the product as external impurities. In certain embodiments, composites formed according to certain embodiments of the present disclosure having Si2N2O as the major phase (about 80 wt.% or more) are produced in this study by heating SDRHA under N2 / H2 atmosphere. In order to ensure sufficient oxygen is available from SiO2, SDRHA with a relatively high SiO2:C ratio was selected.

[0133] Figures 2A-2C. Figure 2A is an XPS survey scan, Figure 2B is TGA, and Figure 2C is RHA and SDRHA. 60 1 is a N2 adsorption / desorption isothermal plot of the above.

[0134] Figure 3A-3C. SDRHA at 1430-1500 °C / 8 h / Ar (Figure 3A). 60 and heating of SDRHA60 at 1500 °C for various times (Fig. 3B). Fig. 3C shows heating of SDRHA40-60 at 1400 °C / 10 h / Ar.

[0135] Figures 4A-4B. XRD obtained from heating of SDRHA60 at 1400 / 8h / N2, 1500 °C / 4h / N2, 1500 °C / 8h / N2 (Figure 4A), and heating of SDRHA65 at 1500 °C / N2 for various times (Figure 4B).

[0136] Figure 5 shows the SDRHA under different N2 / H2 mixing ratios (95 / 5 and 85 / 15). 65 Figure 4 shows a representative XRD pattern of the phases in the product from heating (SiO2:C molar ratio = 13:35). Similar to the Si3N4 product above, Si2N2O, Si3N4, SiC and cristobalite phases are present in the composite formed (Table 4). The longer the heating time, the more complete the reduction is, and the less cristobalite and more Si3N4 in the product. [Table 4]

[0137] The resulting SiC and Si3N4 powders are mixed with excess carbon and are dark gray in color (Figures 6A and 6C). The products of the process show a light grayish green color after oxidative removal of carbon (Figures 6B and 6D), which is typical of SiC and Si3N4 produced in conventional manufacturing.

[0138] 7A-7C show TGAs of representative products resulting from carbothermal reduction of SDRHA with SiC, Si3N4 and Si2N2O as the major phases, showing that excess carbon remains in all systems when heated to 1500°C / 8h. Thus, approximately 13 wt.% unreacted carbon remains in SiC, while as-produced Si3N4 retains approximately 24 wt.% carbon. Starting SDRHA for the synthesis of Si2N2O 65 contains a smaller amount of carbon, leaving a smaller amount of excess carbon in the composite (approximately 6 wt.%) than the former two systems.

[0139] FIG. 7D shows the FTIR of SiC with 13 wt.% carbon, with a peak at 790–1000 cm corresponding to the overlap of ν(Si–C) and ν(CC). -1 After oxidation at 500 °C / O2 / 1 h, a broad peak at 798 cm that can be assigned to ν(Si-C) is observed. -1 A strong absorption centered at approximately 800 cm appears, suggesting the formation of cubic phase SiC, which is consistent with the β-SiC phase assigned from the XRD results discussed above. -1 The increase in the intensity of the ν(Si-C) peak in is probably due to the exposure of SiC after removing the excess carbon.

[0140] In the spectrum of Si3N4 (Figure 7E), 800-1100 cm -1The broad bands at 926, 903, 885, 845 and 685 cm are associated with overlapping ν(Si-N) and ν(Si-O) peaks due to the oxidation of Si3N4 and SiO2-containing components on the surface of the Si3N4 particles. As with the SiC products, the removal of excess carbon increases the peak intensity. -1 The bands at 1090, 989, 910 and 679 cm are typical for α-Si3N4 and are in agreement with the XRD results. -1 The characteristic peaks of Si2N2O at 1500℃ / 6h / 95N2-5H2 are shown (Figure 7F). 65 The composite obtained from heating at 850 cm -1 Additional bands at 0.05 are shown, which are attributed to ν(Si-C) and ν(Si-O) due to the simultaneous formation of SiC and cristobalite phases in the system.

[0141] SDRHA heated at 1500℃ / 8h following oxidative removal of carbon 60 XPS was used to identify the elemental composition and oxidation state of SiC and Si3N4 obtained from the SiO2 / Si3N4 ...

[0142] For the Si3N4 composite, Si 2s, Si 2p, N 1s, C 1s, and O 1s peaks are seen in the XPS survey spectrum of Si3N4. In the core survey, peak fitting in the Si 2p region reveals a strong peak at approximately 101.5 eV attributed to Si3N4. The second component of the Si 2p peak at approximately 103.5 eV corresponds to the Si-O bond of SiO2, resulting from oxidation during carbon removal. One peak located at approximately 397.5 eV in the N 1s spectrum is assigned to the N-Si3 bond of Si3N4.

[0143] The SEM and EDS images in Figures 9A-9D show a cylindrical morphology. 60 SEM images of the as-synthesized SiC / C powder obtained from heating at 100°C and after removing excess hard carbon by oxidation at 500°C / 2h / O2 are shown, respectively. It can be seen that spherical particles coexist with fibrous whiskers in the SiC / C powder, and some of the spherical structures are due to the surrounding carbon particles in the composite. SiC particles with sizes in the range of 10-200 nm can be observed among the SiC whiskers with diameters of about 100-140 nm and lengths up to 5 μm.

[0144] The EDS map shows well-distributed Si and C. As discussed above, oxygen was also detected after carbon combustion. After removing the excess hard carbon by oxidation, the agglomerates are more clearly visible in the image. The non-uniform distribution of products with various morphologies is related to the multiple reaction mechanisms occurring during carbothermal reduction. The proposed growth mechanisms of SiC whiskers focus on non-uniform vapor-liquid-solid, birth-and-spread growth, and vapor-vapor growth. Specifically, solid-gas reactions produce whiskers, while the spherical morphology is mainly formed by solid-solid reactions under high SiO gas pressure. The nucleation and growth of SiC nanofibers are believed to result mainly from the gas-phase reaction between SiO and CO.

[0145] On the other hand, solid-gas reactions occur in the region where carbon consumes the resulting SiO in the surrounding diffusion path. Thus, the reaction occurs at the front of the whisker and can be terminated by colliding with other particles; thus, SiC whiskers show different widths and lengths in micrographs. Although the formation and growth of SiC polymorphs is still not fully understood, it is widely accepted that additives, starting materials, impurities, and growth conditions all affect the kinetics of SiC crystallization and the subsequent polymorph and phase differences.

[0146] Similar morphologies are seen in the Si3N4 and Si2N2O composites (Figures 9C-9D). Irregular agglomerates mixed with whiskers with diameters of about 100-200 nm and lengths of several microns dominate. These observations may suggest that SiC whiskers are formed first before nitridation.

[0147] 10A-10B show the N2 adsorption isotherms of SiC and Si3N4 obtained from heating at various temperatures. There is a gradual increase in the measured BET surface area (SSA) with decreasing synthesis temperature. The BET surface areas of SiC obtained from heating at 1450, 1500 and 1600 °C for 8 h followed by oxidative removal of carbon are 44, 27 and 10 m, respectively. 2 / g.

[0148] SDRHA at 1400 and 1500℃ / 8h / N2 60 BET studies performed on Si3N4 obtained by heating at 20 and 10 m, respectively, after oxidative removal of carbon. 2 The surface area of ​​the Si3N4 produced by heating at 1500°C for 4 hours is 28 m 2 The SSA of 1000 nm / g is shown. The decrease in specific surface area with increasing heating temperature and residence time is probably due to the growth and coalescence of fibrous and spherical SiC particles by a grain boundary diffusion mechanism. Without being limited to a particular theory, it is believed that SiC is formed first, followed by nitridation.

[0149] Several publications report the use of RH and / or RHA to make silicon non-oxide ceramics. Table 5 lists SiC production from RH and / or RHA that can be compared to the present technology in terms of surface area (SSA) and / or product dimensions, also briefly discussed above.

[0150] Most reported methods start with RH and prove to be not applicable to scale-up production, not to mention the energy consumed in pretreatment. In other studies using RHA as starting material, RHA generally serves as a SiO2 source given its high SiO2 content, so that an external carbon source must be added to the RHA to achieve the stoichiometric ratio for carbothermal reduction. In comparison, the method provided according to the present disclosure using treated SDRHA, an agricultural waste product whose by-product spirosiloxane also has great value, results in the highest surface area SiC with the fewest steps. [Table 5]

[0151] (Example 2)

[0152] Nanocomposites derived from SDRHA as electrode materials

[0153] Although traditionally considered electrochemically inactive, with some improvements, silicon carbide (SiC) has been recognized in recent years as a potential electrode material (electroactive material for the negative or positive electrodes) for lithium-ion batteries (LIBs). For example, carbon-coated SiC with a diameter of 50 nm obtained by coating Si nanoparticles with carbon using methane by CVD has an initial discharge capacity of approximately 1330 mAh / g and appears to retain a capacity of approximately 1200 mAh / g for 200 cycles. In another example, C / SiC nanowire (with a diameter of approximately 8-10 nm) composites synthesized by electrolyzing carbonized rice husks have a discharge capacity of 0.5-2 Ag / g. -1 Approximately 800mAhg after 400-600 cycles-1 It showed a capacity exceeding

[0154] As discussed above, for example, SDRHA at 1450°C / 8 hours / Ar with a ramp rate of 10°C per minute 60 When heated, SiC is formed which is mixed with 13 wt.% C.

[0155] The composite material is approximately 44m 2 / g SSA (with carbon: approx. 150m 2 / g or more), suggesting the possibility of using it as an anode / cathode material. The electrochemical performance of the SiC / Li half cell is shown in Figures 11A-11B. -1 The CV curves of the SiC / Li half-cell from 3 to 0.01 V at a scan rate of 1000 V are shown in FIG. 11A, and the voltage-capacity curves are shown in FIG. 11B. The CV curves of the first cycle are different from those of the subsequent cycles. In the first cathodic sweep, the peaks at 1.2 and 0.6 V are associated with the decomposition of the electrolyte and the formation of a solid electrolyte interface (SEI) layer on the cathode surface. The peaks disappear in the subsequent scans, indicating the formation of a stable SEI.

[0156] The long plateau from 0 to 2 V in the potential-capacity curve coincides with the peak of the CV curve. The two oxidation peaks at approximately 0.4 and 1 V in the anodic scan correspond to the Li + The intensity of the reduction peak at approximately 1.2 V is lower than that in the second and third cycles, suggesting irreversible lithiation of SiC during the first scan, which is consistent with the large irreversible capacity seen in the galvanostatic cycling results.

[0157] FIG. 12 shows a plot of the specific capacity versus cycle number of a SiC-C / Li half-cell cycled from 0.01 to 2.5 V at various C rates. The SiC-C / Li half-cell has a capacity of approximately 1200 mAhg at 0.1 C. -1 The initial discharge capacity is shown in Fig. 1. At high speed cycling at 2C, the capacity is approximately 200mAhg -1However, cycling at 0.1 C reduces the discharge capacity to approximately 959 and approximately 808 mAh g after 500 cycles. -1 Go back to.

[0158] The apparent observation of a gradual increase in capacity with cycling of the SiC cathode has also been reported in some earlier studies. Non-limiting theories on theorized explanations include: (1) Li + Intercalation causes a change in the crystal structure; (2) SiC is converted to Si, C and / or Li x S y A typical substitution reaction slowly converts to C; (3) the formation of a slow and complex SEI.

[0159] To investigate the mechanism of action of SiC as a cathode material, the coating on the SiC / C electrode after 600 cycles was scraped off the current collector using a razor blade in a dry room to remove the diffraction from Cu and obtain the active material for better analysis. The retrieved electrode was then immersed in NMP and rinsed with NMP using ultrasonic treatment to dissolve the PDVF. The resulting active material powder was then dried under vacuum / room temperature (RT) / 2 hours.

[0160] Figure 13 shows the XRD patterns of SiC / C before and after cycling, where the pristine SiC / C composite is mainly composed of β-phase belonging to the cubic (3C) system. The peaks at 2θ approximately 36°, 42°, 60° and 72° are associated with the diffraction from the (111), (200), (220) and (311) planes of cubic SiC, respectively. Analysis based on the Halder-Wagner method gives an estimated lattice parameter of 4.3518(19) Å, which is close to the reference 3C-SiC parameter (4.348 Å).

[0161] The peak of the (111) lattice plane shows a stronger residual diffraction signal compared to the peak intensity of the reference 3C-SiC DB card (PDF 01-073-1708, figure of merit = 0.528), indicating the presence of a SiC structure. <111> The peak intensity ratio of the (200) to (111) planes is 5.25, whereas that of the reference pattern is 17.5. The significant difference in peak intensity is probably due to a more favorable orientation along the (111) plane over the (200) plane resulting from competitive growth along the two directions. It is generally accepted that the surface energy of the {111} planes in β-SiC is lower than other lattice planes, which would favorably result in lower formation energy. <111> This results in β-SiC whiskers growing in the axial direction.

[0162] On the other hand, the low intensity peaks at angles lower than the (111) plane are due to the presence of stacking faults (marked with *). The occurrence of stacking faults is frequent in the growth of SiC whiskers, since stacking faults are easily inserted into the {111} planes perpendicular to the growth direction of SiC whiskers.

[0163] For the cycled SiC / C composite, the broad hump centered at 2θ approximately 25° is attributed to the amorphous carbon used in the electrode. In addition to the prominent 3C-SiC phase shown in the pristine SiC / C composite, the XRD pattern of the cycled SiC / C shows weak peaks at 2θ approximately 38°, 41°, 44°, 55°, and 64°, which are attributed to the (103), (104), (105), (107), and (109) planes of the 6H-SiC polytype (PDF01-074-1302, figure of merit = 2.72), respectively, within the hexagonal crystal structure system. The lattice parameter of the 3C-SiC phase increases slightly to 4.3533(6) Å after 600 cycles, suggesting a structural change upon cycling.

[0164] Several studies have reported the observation of SiC polytype transformation during charge / discharge in the literature. Kumari et al., "Nanosilicon Carbide: A New Lithium-Insertion Anode Material on the Horizon," RSC Adv., 3(35), pp. 15028-15034 (2013), https: / / doi.org / 10.1039 / C3RA40798E, were the first to reveal the presence of 8H-SiC phase after cycling pure 3C-SiC nanoparticles, which was published as being associated with a gradual increase in the capacity of SiC. A subsequent report by Li et al., “Bowl-like 3C-SiC Nanoshells Encapsulated in Hollow Graphitic Carbon Spheres for High-Rate Lithium-Ion Batteries,” Chem. Mater. 28(4), pp. 1179-1186 (2016), https: / / doi.org / 10.1021 / acs.chemmater.5b04750, showed a phase transformation to 6H-SiC when examining 3C-SiC nanoshells encapsulated in hollow graphitic carbon spheres as a cathode material, while the intermediate planar structural morphology during the polytype transformation was not observed in a DFT calculation study by Bijoy et al., “Exploring the Mechanism of Spontaneous and Lithium-Assisted Graphite Phase Formation in SiC Nanocrystallites for High-Capacity Li-Ion Battery Anodes.” Lithium-Assisted Graphitic Phase Formation in SiC Nanocrystallites of a High Capacity Li-Ion Battery Anode”, J. Phys. Chem. C, 121(28), pp. 15106-15113 (2017), https: / / doi.org / 10.1021 / acs.jpcc.7b04489.

[0165] (Example 3)

[0166] SiC / HC and SiC / O electrodes

[0167] SiO2 is extracted from the RHA by direct distillation of the spirosiloxane [(CH3)2C(O)CH2CH(O)CH3]2Si, and simultaneously obtains SDRHA by controlling the final SiO2:C molar ratio from 2:15 to 13:35 as described above. This finding enables the production of SiC by direct carbothermal reduction of RHA more quickly and at lower temperatures than conventional methods, because our approach takes advantage of the natural nanoscale mixing of SiO2 and carbon in the RHA without the conventional steps of carbon addition and lengthy milling processes.

[0168] SDRHA containing approximately 13 wt.% hard carbon was analyzed by isothermal TGA under O2. 60 (60wt.% SiO2, approximately 360m 2 By heating 1000g of SSA at 1450°C / 8h / Ar, a greyish product is obtained (hereafter denoted as SiC / HC). Both XRD and FTIR analyses show that the product is mainly composed of β-phase SiC belonging to the cubic (3C) system. It should be noted that the low intensity peaks at angles lower than the (111) plane are due to the presence of stacking faults (marked with *). Stacking faults frequently occur in the growth of SiC whiskers along the (111) plane perpendicular to the growth direction of the SiC whiskers.

[0169] The diffraction peaks seen at 2θ approximately 36°, 42°, 60° and 72° are associated with diffraction from the (111), (200), (220) and (311) planes of 3C-SiC, respectively. Analysis using the Halder-Wagner method gives a lattice parameter of 4.3518(19), which is close to the reference 3C-SiC parameter (4.348). The peak of the (111) lattice plane shows a stronger residual diffraction signal compared to the peak intensity of the reference 3C-SiC DB card (PDF 01-073-1708), indicating the presence of a SiC structure. <111> The peak intensity ratio for the (200) to (111) planes is 5.25, whereas that for the reference pattern is 17.5. The significant difference in peak intensities is likely due to a more favorable orientation along the (111) plane compared to the (200) plane, resulting from competitive growth along the two directions.

[0170] It is generally accepted that the surface energy of the (111) plane in 3C-SiC is lower than that of other lattice planes, which leads to a lower formation energy. <111> This results in 3C-SiC whiskers that grow selectively along the direction.

[0171] SEM images reveal two distinct SiC morphologies, particles and whiskers, which are believed to result from different reaction mechanisms occurring simultaneously during carbothermal reduction. The BET specific surface area (SSA) is approximately 204 m for SiC / HC. 2 / g, and for SiC after oxidative removal at 500°C / 1 h / O2 (hereafter referred to as SiC / O), it is approximately 42 m 2 / g. N2 adsorption / desorption isotherms show a broad pore size distribution with the SiC / HC peaking at about 17 to about 24 nm, and no peak seen for SiC / O. HC typically exhibits high cross-linking leading to the formation of nanopores within the disordered structure.

[0172] The SiO2 was removed from the RHA to recover the SDRHA, and the spirosiloxane was distilled. As discussed above, the synthesis of SiC can be achieved by carbothermal reduction of SDRHA with various SiO2:C ratios. Briefly, (60 wt.% SiO2) SDRHA powder is used as the starting material. As discussed above, the SDRHA is heated at 1450°C / 8h / Ar with a ramp rate of 10°C per minute, for example. 60 Upon heating, SiC mixed with 13 wt.% C or SiC / HC (85 wt.% SiC vs. 15 wt.% C) is formed. The excess hard carbon can be removed by oxidation at 500°C / 1h / O2.

[0173] SiC half cell assembly

[0174] 70wt.% SiC / HC or SiC / O as above, 20wt.% Super C 65 SiC / HC and SiC / O electrodes were prepared with carbon black and 10 wt.% poly(vinylidene fluoride) (PVDF) binder. 65 was dried overnight at 80°C / vacuum and dry mixed with a mortar and pestle, which was then mixed with a PVDF binder solution (5 wt.% solution in NMP) and 1.5 g of NMP in a 16 mL vial. The mixture was ball milled overnight with yttria-stabilized zirconia media (3 mm diameter) to obtain a uniform slurry, which was then coated onto a copper foil (16 μm thick) acting as a current collector at a controlled speed of 50 mm / s using a wire-wound rod coater. After drying at 80°C / vacuum / 2 hours, an electrode with a diameter of 18 mm was punched out. The porosity of the SiC positive electrode was calculated.

[0175] Half-cells (2023 coin cells) were assembled using either SiC / HC or SiC / O electrodes, with Li metal used as the counter electrode in a glove box. Metal Li (16 mm x 750 μm, Alfa Aesar) was milled to remove the oxide layer to expose a clean surface prior to cell assembly. CELGARD™ 2400 (19 mm) was used as the separator, and 1.1 M LiPF6 in EC:DC:DMC solvent (1:1:1 weight ratio) with 10 wt.% FEC additive was used as the electrolyte.

[0176] The data presented in the paper were averaged over three cells. The half-cells were galvanostatically cycled using a multi-channel Maccor test system at Li / Li + The experimental moles of Li in lithiated SiC were calculated from n Li =Q experimental / F×MSiC, where F is the Faraday constant and MSiC is 40.096 g / mol.

[0177] Electrochemical performance of SiC / HC and SiC / O

[0178] SiC has long been + It was considered electrochemically inert to SiC / HC and was considered as a matrix to reinforce the composite electrode and regulate the charge / discharge volume change. However, in recent years, some evidence has shown that the proposed SiC can be useful as an electroactive material, and therefore, SDRHA-derived SiC cathodes are tested here, especially since SDRHA-derived SiC cathodes are easily synthesized from sustainable materials. Figure 19A shows an SEM of a cross section of a representative SiC / HC cathode. The loading of active material is approximately 1 mg / cm. 2 is approximately 0.75mAh / cm 2 Both the SiC / HC and SiC / O half-cell electrodes were assembled with Li metal as the counter electrode.

[0179] FIG. 19B shows the CV curves of SiC / HC cycled from 3 to 0.01 V at 1 mV / s. In the first cathodic scan, peaks appear at approximately 1 V and approximately 0.72 V due to the reductive decomposition steps of two carbonates as the solid electrolyte interface (SEI) forms on the cathode surface. These steps disappear in the next scan, indicating a stable SEI. The two oxidation peaks appearing at approximately 0.2 V and approximately 1.2 V in the anodic scans of both SiC / HC and SiC / O are due to the Li + Extraction can be the cause. The reduction peak intensity at about 1.2 V is lower in the second and third sweeps, probably due to slow lithiation. A long plateau appears from 0 to 2 V in FIG. 19C, which shows the SiC / HC charge / discharge curves over 600 cycles. Further differential capacity analysis shows peaks at about 0.2 V and about 1.2 V, consistent with the CV results.

[0180] The discharge capacities of the initial SiC / HC and SiC / O half-cells are about 1200 and about 1040 mAh / g, respectively, indicating that the presence of HC promotes lithiation. However, the initial coulombic efficiencies (ICEs) are both about 25%, and the subsequent reversible discharge capacities are about 460 and about 410 mAh / g for SiC / HC and SiC / O, respectively. These relatively low ICEs can be attributed to SEI formation and irreversible reactions. The high SSA of the SiC / HC nanocomposite in this example leads to high Li-ionization during the initial cycles. + It is likely to be due to consumption.

[0181] FIG. 19D plots the galvanostatic cycling capacity of SiC / HC and SiC / O half-cells. The gradual increase in capacity with cycling is a distinctive feature of the SiC electrode. After 20 cycles at C / 2 and 40 cycles at 1C, the SiC / HC shows an increase in discharge capacity from approximately 250 to 270 mAh / g and from approximately 230 to 280 mAh / g, respectively. At 2C, the capacity is approximately 200 mAh / g. Cycling the SiC / HC half-cell at C / 10 reaches a discharge capacity of approximately 950 mAh / g (600 cycles). In comparison, the SiC / O half-cell without HC shows a lower discharge capacity of approximately 20 mAh / g from C / 2 to 2C; however, an increase also occurs. After 500 cycles at C / 10, the capacity reaches approximately 740 mAh / g.

[0182] The CE of SiC / HC and SiC / O half-cells at C / 10, C / 2, 1C, and 2C are approximately 85, 95, 97, and 99%, respectively. Although the relatively low CE and high overpotential observed in SiC / HC and SiC / O may not be well suited for high-energy density LIBs, conventional Si-based cathodes also exhibit poor CE in late cycles. However, the performance degradation of conventional Si-based cathodes is attributed to significant volume change, particle pulverization, and repeated SEI reformation. Further testing and characterization will be performed to further understand the origin of the typically low CE and gradual capacity increase of SiC-based cathodes.

[0183] To further investigate the lithiation mechanism of SiC, a post-mortem study was performed after 600 cycles. The recovered electrodes were first cleaned as follows. The SiC / HC and SiC / O half-cells after completing the 600 cycle test were de-crimped in a dry room. The recovered electrodes were rinsed and immersed in DEC solvent to remove electrolyte salt residues not specific to the SEI, followed by ultrasonic dissolution of the PDVF binder in NMP. The electrodes were then dried overnight at room temperature under vacuum. The coating on the SiC electrodes after 600 cycles was also scraped off the current collector using a razor blade in a dry room to obtain good analytical active material that eliminated the detection of Cu in the following characterization.

[0184] The XRD of SiC / HC before and after cycling is compared. The broad hump in the cycled SiC / HC centered at approximately 2θ 25° is due to the amorphous carbon used in the electrode. In addition to the peaks assigned to 3C-SiC, the XRD of the cycled SiC / HC shows weak peaks at approximately 2θ 38°, 41°, 44°, 55°, 64°, and 75°, which correspond to the (103), (104), (105), (107), (109), and (204) planes of 6H-SiC, respectively.

[0185] After 600 cycles, the lattice parameter of 3C-SiC increases from 4.3518(19) to 4.3533(6) Å, which may indicate a slight structural change.

[0186] The SiC / HC and SiC / O nanocomposite cathodes derived from RHA prepared according to certain embodiments of the present disclosure are potential alternatives to graphite and competitors to traditional Si-based cathodes in future LIB applications. SiC / HC showed a gradual increase in capacity to >950 mAh / g after 600 cycles, and a 10% increase in capacity as measured by GITT. -22 ~10 -14 cm 2 / s ambient environment Li + It has a diffusion coefficient.

[0187] Post-mortem characterization of cycled electrodes

[0188] XRD, 29SiNMR, XPS and SEM show a partial phase transformation from cubic (3C) to hexagonal (6H) SiC, with no significant volume change or surface cracks seen in SEM. No elemental Si, LixSi or LixC was observed, suggesting that SiC lithiation is limited by intercalation rather than conversion or alloying reactions. Computational modeling suggests that a cubic to hexagonal phase transition occurs at high Li contents, indicating that Li prefers the tetrahedral C sites due to electrostatic interactions.

[0189] Experimental data show that lithiated SiC can be charged to Li without significant volume change. 1.2~1.4 We show that the composition of SiC can be reached, resulting in a capacity approaching 1000 mAh / g. Thus, SiC represents a viable alternative to silicon as a negative electroactive material. For example, the conversion of Si to Li with a volume change of over 300% has been demonstrated. 4.4 Lithiation to Si occurs, meaning that batteries with Si cathodes must accommodate a significant proportion of this volume change.

[0190] Due to the roughly 40-60% porosity required in the host material (ignoring mechanical property issues), we can conclude that the actual capacity of a realistic Si-based cathode would be at best half of 3579 or 1300 mAh / g.

[0191] Furthermore, SiC can eliminate the need for surface passivation, which is otherwise partially required for Si-based cathodes.

[0192] (Example 4)

[0193] A postmortem study of SiC and graphite electrodes.

[0194] The electrodes containing SiC / HC and 30 wt.% graphite and the electrodes containing SiC / O and 30 wt.% graphite prepared as described above in Examples 1 and 2, which had been assembled into half-cells and had completed 600 lithiation / delithiation cycles, were then decrimped. The recovered electrodes were rinsed and immersed in DEC solvent to remove residual electrolyte salts. The electrodes were then sonicated in NMP to dissolve the PDVF binder. The electrodes were then vacuum dried at room temperature before characterization studies were performed.

[0195] XRD analysis of the SiC / HC and 30 wt.% graphite electrodes after 600 cycles shows that the most intense peak at 2θ approximately 26.5° is assigned to the (002) plane of graphite. In the magnified patterns, the peaks at 2θ approximately 36°, 42°, 60° and 72° are associated with diffraction from the (111), (200), (220) and (311) planes of 3C-SiC, respectively. Weaker peaks seen at 2θ approximately 38°, 45°, 55°, 60° and 67° are attributed to the (103), (104), (109) and (204) planes of 6H-SiC. Furthermore, the doublet peaks at 2θ approximately 48° and 49° are attributed to the lithiated graphite (LiC x ), indicating the intercalation of residual lithium in the graphite layers.

[0196] SEM images of the top and cross-section of the SiC / HC and 30 wt.% graphite (Formula BT™) electrodes after 600 cycles are examined. As expected, the electrode surface is covered with an SEI layer while no SiC whisker structure is visible. Similar to the cycled SiC / HC electrode, the cycled SiC / HC + 30 wt.% graphite electrode maintained its integrity and no cracks were observed. EDX images show the characteristic elements of Si, C and O distributed uniformly, as well as LiF, Li x PF y and Li x PF y O z The F and P elements associated with the species are shown.

[0197] For comparison, we examine the SEM image of the SiC / O+30wt.% graphite electrode after 600 cycles. Due to the smaller SSA and thus the thinner SEI on the surface, the fibrous SiC whiskers are more evident in the electrode without hard carbon (HC) particles. In addition, the graphite particles (approximately 10μm) are not clearly distinguishable from the electrode surface after cycling.

[0198] (Example 5)

[0199] SiN / O electrode

[0200] Although Si3N4 has been reported to exhibit very low capacities of 40–80 mAh / g, suggesting that it is relatively electrochemically inert, several studies have demonstrated the use of substoichiometric SiN4 rather than Si3N4. x In particular, it has been reported that extended cycling results in significantly higher capacity. In general, increasing the N content is detrimental to the reversible specific capacity, but improves cycling stability, since SiNx is considered a conversion-type cathode that is irreversibly reduced during the first cycle to form inactive Li3N. The resulting Li3N matrix has a capacity of approximately 10 at room temperature. -3 Scm -1 The high Li + Electrical conductivity drives electrochemical performance.

[0201] However, the SiN x O y There are few studies examining the feasibility of using SiN / SiO as a cathode. x N y Studies have been reported on the use of Si nanotubes covered with a LiN / SiOxNy shell, but the SiN / SiOxNy shell was considered as a mechanical stabilizer with no electrochemical activity. The only attempt reported so far was with Li x SiO y N z It is believed that the study was carried out on the nominal composition Li 12 SiO2N 0.4 A mixture of SiO2 and Li3N with a molar ratio of 1:4.2 was synthesized by high energy ball milling. This material had a capacity of 590 mAhg -1 Its initial discharge capacity is 460mAhg after 100 cycles. -1 Despite the unimpressive capacity, a wide voltage window was observed in this system, up to 3.7 V. However, it is not believed that Si2N2O has been used as a positive electrode active material in the past.

[0202] Carbothermal nitridation studies, as discussed above, have shown that a 95:5 mixture of N2 / H2 produces Si2N2O and / or nonstoichiometric SiN x O4-x It was found that the formation of 1 mVs was favored. Several Si2N2O composites were selected for the study of their electrochemical performance. Figure 14 shows the 1 mVs -1 Figure 1 shows the CV curves of a representative Si2N2O / Li half-cell from 3 to 0.01 V at a scan rate of 100 Hz. In the first cathodic sweep of the Si2N2O / Li half-cell, the reduction peak from 2 to 0.75 V is likely due to both reversible and irreversible lithiation. This is characteristic of the conversion reaction. In the subsequent lithiations, the conversion hump largely disappears, indicating that the conversion reaction is largely complete and irreversible during the initial cycles. The peak at approximately 0.5 V, associated with electrolyte decomposition and the formation of an SEI layer on the cathode surface, also disappears in the subsequent scans, indicating that a stable SEI has been formed.

[0203] 15A-15B show plots of specific capacity versus cycle number for Si2N2O / Li half-cells cycled from 2.5 to 0.01 V at various C-rates. 65 and Si2N2O with approximately 84 wt.% Si2N2O in the product by heating at 1500 °C / 10 h under N2 / H2 (85 / 15). 65 Si2N2O obtained by heating 100% Si2N2O with approximately 88 wt.% Si2N2O in the product was used in two cells (Table 4).

[0204] The Si2N2O(84) / Li half-cell showed an initial discharge capacity of about 800 mAh / g. At 1C, the charge capacity shows about 130 mAh / g after 40 cycles. At 2C, both the charge and discharge capacities increased to about 130 mAh / g after 40 cycles. When the C-rate was reduced back to 0.1C, the half-cell showed charge and discharge capacities of about 285 and about 226 mAh / g, respectively, after 240 cycles.

[0205] The Si2N2O(88) / Li half-cell shows a charge capacity recovered to about 228 mAh / g and a discharge capacity recovered to about 186 mAh / g after 40 cycles at 0.1 C, which is close to the charge / discharge capacity of the Si2N2O(84) / Li half-cell. After 270 cycles at 0.1 C, the charge and discharge capacities increase to about 376 and 264 mAh / g, respectively. Unlike the Si2N2O(84) / Li half-cell above, a higher charge capacity than the discharge capacity is seen over about 360 cycles at different C-rates. The presence of cristobalite and Si3N4 phases and / or the difference in SSA of the two systems probably led to the different performance upon cycling. The substoichiometric SiN x It is worth noting that the C-rate was calculated based on a capacity of 1200 mAh / g by referencing the film studies. Furthermore, the capacity increase seen in these preliminary tests is similar to that of SiC cathodes, despite the relatively low specific capacity.

[0206] (Example 6)

[0207] Electrodes with SiC / C containing graphite

[0208] Considering the excessive formation of solid electrolyte interface (SEI) layer due to the large surface area and unstable structure of Si-based cathode materials, graphite is often introduced to reduce unwanted electrolyte decomposition, help maintain the integrity of the cathode, and provide a pathway for electronic transition. In this example, graphite was mixed with SiC / C to increase the specific capacity and cycling stability compared to graphite-free or graphite-only batteries.

[0209] SiC / C (1450°C / Ar / 8h) was mixed with graphite in NMP solvent (weight ratios of 8:1 and 6:3). 65 The mixture was ball milled overnight with yttria-stabilized zirconia media (approximately 3 mm diameter, 3 g) before adding 5 wt.% poly(vinylidene fluoride) (PVDF) binder to prepare electrodes. 65The corresponding blend ratios of SiC+PVDF are 8:1:0.5:0.5 (hereafter referred to as SiC+10 wt.% graphite) and 6:3:0.5:0.5 (hereafter referred to as SiC+30 wt.% graphite) in the electrodes.

[0210] Figure 16 shows the XRD patterns of SiC / C before and after mixing with 10 wt.% graphite. In addition to the peaks attributable to 3C-SiC with stacking faults, a strong peak at 2θ approximately 26.5° is assigned to the (002) plane of graphite.

[0211] 17A-17B are SEM images of graphite (Formula BT™) and SiC / C after mixing. According to information provided by the supplier, the material is derived from natural graphite. Pure graphite particles include both spherical and ellipsoidal particles with an average diameter of approximately 10 μm. After ball milling the SiC / C, the fibrous SiC whiskers and the surrounding carbon particles maintain their respective morphology. The graphite particles are not clearly distinguished from the composite, probably due to their low content and / or particle size reduction during the ball milling process.

[0212] C 65 Electrodes were prepared by adding poly(vinylidene fluoride) (PVDF) binder solution (5 wt.% solution in NMP) to ball-milled SiC / C+graphite composites. The electrode slurry was ball-milled overnight in a glass vial with yttria-stabilized zirconia media (average diameter of about 3 mm, 6 g) to obtain a homogeneous mixture, and then coated onto copper foil current collectors using a wire-wound rod coater at a controlled speed of 50 mm / s. After drying at 80°C / vacuum / 2 h, they were die-cut into 18 mm circular electrodes for coin cells.

[0213] Half-cells were assembled to evaluate the electrochemical performance, with Li metal used as the counter electrode. Metal Li (16 mm diameter) was scraped to remove the oxide layer and expose a clean surface prior to cell assembly. CELGARD 2400 (19 mm diameter) was used as the separator, and 1.1 M LiPF6 in EC:DC:DMC (1:1:1 weight ratio) with 10 wt.% FEC added was used as the liquid electrolyte.

[0214] As a baseline for the reported results, a graphite / Li half-cell was charged and discharged from 0.01 to 2.5 V at different C rates (Figure 18A). As shown in the representative voltage profile of a graphite / Li half-cell, the Li charge on the graphite was + Intercalation of 0.25~0.01V vs. Li / Li + It is widely accepted that

[0215] The resulting initial discharge capacity of the graphite / Li half-cell is about 360 mAh / g, close to the theoretical 375 mAh / g. The specific capacity remains at about 350 mAh / g at 0.1C, decreasing to about 280 and about 170 mAh / g at 0.5C and 1C, respectively. When the C-rate is increased back to 0.1C, the retained charge and discharge capacities are about 370 and 300 mAh / g. No incremental increase in capacity is observed for the first five cycles at 0.1C, while a small gap is observed between the charge and discharge capacities in the graphite / Li half-cell. The charge capacity is larger than the discharge capacity, suggesting some excess lithium metal plating during cycling.

[0216] The SiC / C+graphite half-cell was charged and discharged from 0.01 to 2.5 V. Figures 18A, 18B, and 18C compare the representative voltage profiles and specific capacity versus cycle number for the first and second cycles of the SiC / C+graphite half-cell with the pristine SiC / C half-cell. As shown in Figure 18B, the SiC / C half-cell shows a first cycle irreversible capacity drop of over 70%. Such a significant first cycle irreversible capacity drop is common for silicon-based positive electrodes when discharged to potentials close to zero. Furthermore, the first discharge curves of the SiC / C half-cell show a large voltage profile from about 1.25 to 1 V and about 0.7 to 0.4 V vs. Li / Li. + These show a short plateau or hump associated with electrode passivation and SEI formation in LiPF 64 This is typical for silicon-based positive electrodes cycled using electrolyte-based systems. The voltage profile and efficiency of the first cycle are highly dependent on the electrolyte salt. In the second and subsequent cycles, the potential shows a sloping profile and these plateaus disappear, suggesting irreversible lithiation during the first cycle.

[0217] Just like the pristine SiC / C, plateaus at approximately 1.25-1 V and approximately 0.7-0.4 V appear in the first discharge curves of both SiC / C+graphite half-cells due to electrode passivation and SEI formation (FIGS. 18C and 18D). Furthermore, plateaus at 0.25-0.01 V vs. Li / Li in the second cycle + At , further long structureless features are seen, which are probably due to Li + This is due to the intercalation of Li. This indicates a potential contribution to capacity from graphite. Si-based positive electrodes are typically x It should be noted that the graph shows a long and flat voltage plateau around 0.25-0.1 V, which is due to the electrochemical lithiation of Si to form a Si alloy.

[0218] As seen in FIG. 18C, the reversible specific capacity of SiC / C+10 wt.% graphite is approximately 370 mAh / g at 0.1 C and decreases to approximately 210 mAh / g at 0.5 C. The specific capacity further decreases to approximately 130 mAh / g at 1 C. Back to 0.5 C, the capacity is approximately 210 mAh / g, which increases to approximately 220 mAh / g after 20 cycles. At 2 C, the capacity decreases from approximately 90 mAh / g to approximately 84 mAh / g. The battery was then charged / discharged at 0.1 C for a target of 500 cycles. After the first 15 cycles, the retained charge and discharge capacities are approximately 310 and approximately 390 mAh / g, with an upward slope.

[0219] Similarly, the SiC / C+30 wt.% graphite half-cell was charged and discharged according to the same C-rate from 0.01 to 2.5 V (FIG. 18D). The SiC / C+30 wt.% graphite half-cell shows a specific capacity of about 530 mAh / g at 0.1 C. When the C-rate is increased to 0.5 and 1 C, the specific capacities are about 450 and 310 mAh / g, respectively. When the C-rate is then decreased to 0.5 C, the cell shows a specific capacity of about 510 mAh / g. At 2 C, the specific capacity is about 190 mAh / g. After cycling back to 0.1 C for 15 cycles, the discharge capacity increases from about 740 to about 870 mAh / g, while the charge capacity increases from about 510 to about 560 mAh / g, again showing an upward slope.

[0220] Overall, the SiC / C+30wt.% graphite half-cell shows higher capacity than pristine SiC / C and SiC / C+10wt.% graphite at all C-rates. Similar to the SiC / C samples made without graphite addition, a gradual increase in capacity is shown in the SiC / C+graphite half-cell. A gap between charge and discharge capacity is observed not only in the SiC / C half-cell but also in the graphite half-cell, possibly due to the cycling programs at different C-rates.

[0221] We note that 30 wt.% graphite appears to improve capacity up to 5 times faster than the initial SiC half-cell, which is highly advantageous for use in electrochemical cells.

[0222] The foregoing description of the embodiments has been presented for purposes of illustration and description. It is not intended to be exhaustive or to limit the disclosure. Individual elements or components of a particular embodiment are generally not limited to that particular embodiment and, where applicable, may be interchangeable and used in selected embodiments even if not specifically shown or described. The same may also be modified in various ways. Such variations should not be considered as departures from the disclosure, and all such modifications are intended to be included within the scope of the disclosure.

Claims

1. A method for making silicon carbide or silicon nitride from rice husk ash (RHA) by-product, comprising: Silicon carbide (SiC), silicon nitride (Si 3 N 4 ), and silicon oxynitride (Si 2 N 2 heating a silica-deficient rice hull ash product (SDRHA) comprising about 65% by weight or less silicon oxide and about 35% by weight or more carbon in an environment having a temperature of about 1,200° C. or more and an inert atmosphere and no additional carbon source for a carbothermal reaction to form a product comprising at least one of the following: The above method.

2. 2. The method of claim 1, wherein the silica deficient rice hull ash (SDRHA) comprises from about 35% to about 60% by weight carbon.

3. Silica deficient rice husk ash (SDRHA) is about 1:8 to about 1:3 SiO 2 Ratio of carbon (SiO 2 2. The method of claim 1 , comprising:

4. 2. The method of claim 1, further comprising removing silicon oxide from rice hull ash (RHA) by-product to form silica deficient rice hull ash (SDRHA) by reacting RHA with a hindered diol in the presence of a catalytic base.

5. The method of claim 4, wherein the hindered diol is selected from the group consisting of 2-methyl-2,4-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, and combinations thereof.

6. The catalytic base is sodium hydroxide (NaOH), lithium hydroxide (LiOH), calcium hydroxide Ca(OH) 2 5. The method of claim 4, wherein the hydroxide is selected from the group consisting of potassium hydroxide (KOH), cesium hydroxide (CsOH), rubidium hydroxide (RbOH), and combinations thereof.

7. 5. The method of claim 4, wherein the hindered diol comprises 2-methyl-2,4-pentanediol and the catalytic base comprises sodium hydroxide (NaOH).

8. The method of claim 1 , wherein the temperature is from about 1,400° C. to about 1,600° C.

9. The method of claim 1 , wherein the product is a nanocomposite.

10. 10. The method of claim 1, wherein the product comprises at least about 75% by weight silicon carbide (SiC).

11. The product is a nanostructured silicon oxynitride (SiN x O 4-x (wherein x is in the range of from 0 to 4), and the nanostructure has a phase including silicon carbide (SiC) and silicon nitride (Si 3 N 4 10. The method of claim 1, further comprising at least one of:

12. Before heating, milling the rice husk ash (RHA) by-product with an acidic solution to obtain a refined rice husk ash (RHA) by-product; removing silicon oxide from the refined rice hull ash (RHA) by-product by reacting the RHA with a hindered diol in the presence of a catalytic base to form a silica-deficient rice hull ash (SDRHA); The method of claim 1 further comprising:

13. 13. The method of claim 12, further comprising washing the refined rice husk ash (RHA) by-product with boiling water after milling to remove impurities.

14. Silicon oxynitride (Si 2 N 2 O, or non-stoichiometric SiN x O 4-x 1. An electroactive material for a negative electrode of an electrochemical cell circulating lithium ions comprising:

15. Silicon oxynitride (Si 2 N 2 O, or non-stoichiometric SiN x O 4-x 15. The electroactive material of claim 14, comprising a nanocomposite having a phase comprising:

16. 16. The electroactive material of claim 15, wherein the nanocomposite further comprises a pyrolyzed carbon-based material.

17. The nanocomposite is made of silicon oxynitride (Si 2 N 2 O, or non-stoichiometric SiN x O 4-x (wherein x is in the range of from 0 to 4)) and silicon carbide (SiC) and silicon nitride (Si 3 N 4 20. The electroactive material of claim 15, further comprising at least one of the following:

18. Silicon oxynitride (Si 2 N 2 O, or non-stoichiometric SiN x O 4-x 16. The electroactive material of claim 15, wherein x is in the range of from 0 to 4, is formed by heating a silica-deficient rice hull ash product (SDRHA) comprising about 65% by weight or less of silicon oxide and about 35% by weight or more of carbon in an environment having an inert atmosphere without an additional carbon source but having nitrogen present and having a temperature of about 1,200° C. to about 1,700° C. for a carbothermal reaction.

19. Silicon oxynitride is Si 2 N 2 16. The electroactive material of claim 15 comprising O.

20. Silicon oxynitride is non-stoichiometric SiN x O 4-x 16. The electroactive material of claim 15 comprising: wherein x is in the range of from greater than 0 to less than 4.

21. 20. An electrode comprising the electroactive material of claim 15 and further comprising graphite.

22. 22. The electrode of claim 21 further comprising a polymer binder.

23. Silicon oxynitride (Si 2 N 2 O, or non-stoichiometric SiN x O 4-x 1. An electroactive material for a negative electrode of an electrochemical cell circulating lithium ions comprising a nanocomposite comprising: (wherein x is in the range of from greater than 0 to less than 4); and / or silicon carbide (SiC).

24. 24. The electroactive material of claim 23, wherein the nanocomposite further comprises a pyrolyzed carbon-based material.

25. 24. The electroactive material of claim 23, wherein the nanocomposite comprises silicon carbide (SiC).

26. The nanocomposite is made of silicon oxynitride (Si 2 N 2 O, or non-stoichiometric SiN x O 4-x (wherein x is in the range of from 0 to 4)) and silicon carbide (SiC) and silicon nitride (Si 3 N 4 24. The electroactive material of claim 23, further comprising at least one of the following:

27. Silicon oxynitride is Si 2 N 2 24. The electroactive material of claim 23 comprising O.

28. Silicon oxynitride is non-stoichiometric SiN x O 4-x 24. The electroactive material of claim 23 comprising: wherein x is in the range of from greater than 0 to less than 4.

29. 24. An electrode comprising the electroactive material of claim 23 and further comprising graphite.

30. 30. The electrode of claim 28 further comprising a polymer binder.

Citation Information

Patent Citations

  • Method for preparing silicon carbide through low-temperature electrolyzing

    CN102864462A

  • Manufacture of silicon carbide whiskers

    JP1983045195A

  • Preparation of silicon nitride

    JP1984035009A

  • Negative electrode material, and nonaqueous electrolyte secondary battery using the same

    JP1999102705A

  • Negative electrode and nonaqueous electrolyte battery

    JP2001135303A