Iron-based composite phosphate positive electrode material and its manufacturing method, positive electrode sheet, and sodium ion battery
By controlling the viscosity of the solid-liquid ratio and processing iron-based composite phosphate particles, the method addresses production costs and environmental issues, enhancing the electrochemical performance and safety of sodium ion batteries.
Patent Information
- Application Number
- JP2024521066
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-03-14
- Filing Date
- 2023-03-08
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-08
AI Technical Summary
Existing sodium ion battery cathode materials like Na4Fe3(PO4)2P2O7 face issues with high production costs and environmental pollution due to water-soluble salts, making them unsuitable for large-scale industrial production.
A method is developed to control the viscosity of the solid-liquid ratio during the mixing and polishing process, followed by drying and sintering, to produce uniformly sized nanospherical iron-based composite phosphate particles for the cathode material.
The method results in a cathode material with excellent electrochemical performance, improving cycle and safety performance of sodium ion batteries.
Smart Images

Figure 2024536424000001_ABST
Abstract
Description
[Technical field]
[0001] (CROSS-REFERENCE TO RELATED APPLICATIONS) This disclosure claims priority to a Chinese patent application bearing application number CN202210247605.5 and entitled "Iron-based composite phosphate positive electrode material and its manufacturing method, positive electrode sheet and sodium ion battery," filed with the China Patent Office on March 14, 2022, the entire contents of which are incorporated herein by reference.
[0002] The present disclosure relates to the technical field of sodium-ion battery materials, in particular to an iron-based composite phosphate positive electrode material and its manufacturing method, a positive electrode sheet and a sodium-ion battery. [Background technology]
[0003] In recent years, great efforts have been made to develop clean energy sources such as solar energy, wind energy, and water energy. However, these clean energy sources have disadvantages such as high variability, low stability, and intermittent supply, so they need to be integrated and converted into large-scale energy storage devices in order to be utilized rationally. Among existing energy storage technologies, secondary batteries are considered to be one of the ideal choices for large-scale energy storage technology due to their excellent flexibility and high energy conversion efficiency.
[0004] Lithium-ion batteries have been very successful in the fields of portable electronic devices and electric vehicles due to their high energy density and good cycle stability, but due to the scarcity and uneven distribution of lithium resources, they cannot meet the requirements for cheap large-scale energy storage. However, sodium-ion batteries have a similar working principle to lithium-ion batteries, but the storage capacity is more abundant and distributed over a wider area.
[0005] Considering the important characteristic that the value cost of large-scale energy storage devices is greater than the energy density, sodium-ion batteries are considered to be one of the potential candidates for large-scale energy storage systems.
[0006] Currently, many positive electrode materials for sodium-ion batteries have been reported, but very few have shown good electrochemical performance, such as vanadium-based phosphates, iron-based phosphates and Prussian blue analogues.
[0007] Furthermore, in the process of commercializing the experimental results, these materials also face some serious problems, such as the high toxicity and high cost of vanadium-based materials, and the structural instability of Prussian blue analogues. In iron-based phosphates, Na4Fe3(PO4)2P2O7 is low-cost, environmentally friendly, and has a theoretical capacity (129 mAh g -1 ) and high average operating voltage (3.1V S.Na + This material combines all the advantages of iron-based phosphates, including a high thermal conductivity (Tc / Na) and a low volume expansion coefficient (4% reduction), making it the most promising material for the positive electrode of sodium-ion batteries.
[0008] However, Na4Fe3(PO4)2P2O7 uses water-soluble salts in the synthesis process, which is expensive and causes serious environmental pollution due to decomposition products. Considering the production cost of raw materials, it is not favorable for industrial development. Therefore, finding a more economical production process is helpful for mass production of Na4Fe3(PO4)2P2O7. Summary of the Invention [Means for solving the problem]
[0009] One objective of the present disclosure is to provide a method for preparing an iron-based composite phosphate positive electrode material, in which the viscosity of the solution is controlled using a suitable solid-liquid ratio to achieve solution of solid reactants in the grinding process, obtain uniform reaction function, and then dry and sinter to obtain the final product.
[0010] Another object of the present invention is to provide an iron-based composite phosphate positive electrode material produced by the method for producing the iron-based composite phosphate positive electrode material.
[0011] Another object of the present invention is to provide a positive electrode sheet comprising said positive electrode material.
[0012] Another object of the present invention is to provide a sodium ion battery including the positive electrode sheet.
[0013] In order to achieve the above objectives of the present disclosure, in particular, the following technical solutions are adopted: The present disclosure provides a method for producing an iron-based composite phosphate cathode material, the method comprising: The method includes the steps of: uniformly mixing a sodium source, a phosphorus source, a carbon source, and water, and then mixing with iron phosphate to obtain a first mixed system; grinding the first mixed system to obtain a second mixed system, and drying and sintering the second mixed system; In the first mixture system, Na element, Fe element, (PO4) 3- The total mass of the carbon sources is 30% to 40% of the mass of the water, and the viscosity of the second mixture system is 300 Pa.S or more.
[0014] Optionally, the sodium source comprises at least one of sodium acetate, sodium nitrate, sodium oxalate, sodium citrate, and sodium phosphate.
[0015] Optionally, the phosphorus source comprises at least one of sodium dihydrogen phosphate, sodium phosphate, and phosphoric acid.
[0016] Optionally, the carbon source comprises at least one of citric acid, glucose, sucrose, and polyethylene glycol.
[0017] Optionally, the molar ratio of the phosphorus source, the sodium source and the carbon source is 1:(2.8-3.2):(1-10).
[0018] Optionally, the molar ratio of Fe to P in the iron phosphate is 0.97-1.
[0019] Optionally, the iron phosphate comprises micron-scale particles and / or nano-scale aggregates.
[0020] Optionally, in the second mixture system, the particle size D90 of said iron phosphate is between 0.05 and 0.15 μm.
[0021] Optionally, the viscosity of the second mixture system is 300-400 Pa.S.
[0022] Optionally, the drying comprises spray drying.
[0023] Optionally, the drying temperature is 80 to 120° C., and the drying time is 5 to 10 hours.
[0024] Optionally, the sintering step includes performing a first sintering step at a temperature of 290 to 310°C, and then increasing the temperature to 550 to 600°C to perform a second sintering step.
[0025] Optionally, the time of the first sintering process is 3-5 h, and the time of the second sintering process is 10-12 h.
[0026] Optionally, the heating rate is 2-5° C. / min.
[0027] The iron-based composite phosphate positive electrode material is manufactured by the above-mentioned method for manufacturing the iron-based composite phosphate positive electrode material.
[0028] Optionally, the iron-based composite phosphate positive electrode material is a spherical particle having a particle size of 100-200 nm.
[0029] The present disclosure further provides a positive electrode sheet comprising the positive electrode material.
[0030] The present disclosure further provides a sodium ion battery comprising the positive electrode sheet. Effect of the Invention
[0031] Compared with the prior art, the beneficial effects of the present disclosure are as follows: (1) The present disclosure achieves the solution of solid reactants in the grinding process by controlling the viscosity of the solution using an appropriate solid-liquid ratio, obtaining a uniform reaction function, and then drying and sintering to obtain an iron-based composite phosphate positive electrode material, which is a nano-spherical particle with a uniform size of 100-200 nm and has excellent electrochemical performance.
[0032] (2) The iron-based composite phosphate positive electrode material prepared in this disclosure can be applied to sodium-ion batteries to further improve the cycle performance and safety performance of the batteries. [Brief description of the drawings]
[0033] In order to more clearly describe the specific embodiments of the present disclosure or the technical solutions of the prior art, the following briefly introduces drawings necessary for describing the specific embodiments or the prior art. Obviously, the drawings described below are some embodiments of the present disclosure, and those skilled in the art can obtain other drawings based on these drawings without creative efforts. [Figure 1] 1 is a scanning electron microscope image (SEM image) of the iron-based composite phosphate positive electrode material obtained in Example 1 of the present disclosure. [Diagram 2] 1 is a charge / discharge curve graph of a battery made of the iron-based composite phosphate positive electrode material obtained in Example 1 of the present disclosure; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to examples. Those skilled in the art should understand that the following examples are only for illustrating the present disclosure and should not be considered as limiting the scope of the present disclosure. If no specific conditions are shown in the examples, conventional conditions or conditions recommended by the manufacturers are followed. Reagents or equipment without manufacturer names are all conventional products available on the market.
[0035] According to one aspect of the present disclosure, a method for producing an iron-based composite phosphate cathode material according to the present disclosure includes: The method includes the steps of: uniformly mixing a sodium source, a phosphorus source, a carbon source, and water, and then mixing with iron phosphate to obtain a first mixed system; grinding the first mixed system to obtain a second mixed system, and drying and sintering the second mixed system; In the first mixture system, Na element, Fe element, (PO4) 3- The total mass of the carbon sources is 30% to 40% of the mass of the water, and the viscosity of the second mixture system is 300 Pa.S or more.
[0036] The present disclosure uses an appropriate solid-liquid ratio to control the viscosity of the solution to achieve the solution of solid reactants in the polishing process, obtain uniform reaction function, and then dry and sinter to obtain iron-based composite phosphate Na4Fe3(PO4)2P2O7 cathode material, which is a nano-spherical particle with a uniform size of 100-200 nm.
[0037] In one embodiment, the first mixture system includes Na element, Fe element, (PO4) 3- The total mass of (phosphate) and carbon source is 30% to 40% of the mass of the water, specifically including but not limited to 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38% or 39%.
[0038] In one embodiment, the viscosity of the second mixture system is 300 Pa.S or more, specifically 310 Pa.S or more. . Examples of viscosity ranges include, but are not limited to, 320 Pa.S, 330 Pa.S, 350 Pa.S, 360 Pa.S, 380 Pa.S, 400 Pa.S, 420 Pa.S, 450 Pa.S, and 500 Pa.S. In one embodiment, the viscosity of the second mixture system is 300 to 500 Pa.S.
[0039] The term "polishing" refers to a method of dispersing particles finely by mechanical force. For example, a sanding method is adopted, and the sanding medium includes at least one of sandstone, glass beads, zirconia beads, and zirconium silicate beads.
[0040] In one embodiment, the sodium source includes at least one of sodium acetate, sodium nitrate, sodium oxalate, sodium citrate, and sodium phosphate.
[0041] In one embodiment, the phosphorus source comprises at least one of sodium dihydrogen phosphate, sodium phosphate, and phosphoric acid.
[0042] In one embodiment, the carbon source comprises at least one of citric acid, glucose, sucrose, and polyethylene glycol.
[0043] In one embodiment, the molar ratio of the phosphorus source, the sodium source and the carbon source is 1:(2.8 to 3.2):(1 to 10).
[0044] In one embodiment, the molar ratio of the phosphorus source, sodium source and carbon source is 1:3:1, 1:3:2, 1:3:3, 1:3:4, 1:3:5, 1:3:6, 1:3:7, 1:3:10.
[0045] In one embodiment, the iron phosphate has a molar ratio of Fe to P of 0.97 to 1. For example, it may be 0.98 or 0.99.
[0046] In one embodiment, the iron phosphate is a crystalline or amorphous particle. The iron phosphate comprises micron-scale particles and / or nano-scale aggregates. The preferred type is the nano-scale aggregates.
[0047] In one embodiment, the iron phosphate micron-scale particles have a particle size of 1-20 μm, including but not limited to 2 μm, 3 μm, 5 μm, 6 μm, 7 μm, 10 μm, 11 μm, 13 μm, 15 μm, 17 μm, or 20 μm.In one embodiment, the iron phosphate micron-scale particles have a particle size of 20-200 nm, including but not limited to 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 70 nm, 80 nm, 100 nm, 120 nm, 150 nm, 170 nm, 180 nm, or 200 nm.
[0048] In one embodiment, the particle size D90 of the iron phosphate in the second mixture system is 0.05 to 0.15 μm.
[0049] In one embodiment, the iron phosphate has a particle size D90 of .06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.1 μm, 0.11 μm, 0.12 μm, 0.13 μm, 0.14 μm or 0.15 μm.
[0050] In one embodiment, the drying comprises spray drying.
[0051] In one embodiment, the drying temperature is 80 to 120° C., and the drying time is 5 to 10 hours. In one embodiment, the drying temperature is 85° C., 90° C., 95° C., 100° C., 105° C., 110° C., or 115° C. The drying time is 6 hours, 7 hours, 8 hours, 9 hours, or 9.5 hours.
[0052] In one embodiment, the sintering includes performing a first sintering process under conditions of 290 to 310° C., and then increasing the temperature to 550 to 600° C. to perform a second sintering process. In one embodiment, the temperature of the first sintering process is 292° C., 295° C., 298° C., 300° C., 302° C., 305° C., or 309° C. In one embodiment, the temperature of the second sintering process includes, but is not limited to, 555° C., 560° C., 565° C., 570° C., 575° C., 580° C., 585° C., 590° C., 595° C., or 600° C.
[0053] In one embodiment, the time of the first sintering process is 3 to 5 hours, and the time of the second sintering process is 10 to 12 hours. In one embodiment, the time of the first sintering process includes, but is not limited to, 3 hours, 3.5 hours, 4 hours, or 4.5 hours. The time of the second sintering process includes, but is not limited to, 10.5 hours, 11 hours, or 11.5 hours.
[0054] Optionally, the temperature rise rate is 2 to 5° C. / min, for example, 2.5° C. / min, 3° C. / min, 4° C. / min, or 4.5° C. / min.
[0055] In one embodiment, the sintering is carried out under protective gas conditions. Protective gases include nitrogen, inert gases, etc. Inert gases include argon, neon, etc.
[0056] In the present disclosure, the above sintering conditions result in iron-based composite phosphate cathode materials with better electrochemical performance.
[0057] According to another aspect of the present disclosure, the present disclosure also relates to an iron-based composite phosphate positive electrode material produced by the method for producing the iron-based composite phosphate positive electrode material.
[0058] In one embodiment, the iron-based composite phosphate positive electrode material is a spherical particle having a particle size of 100 to 200 nm. In one embodiment, the particle size of the iron-based composite phosphate positive electrode material includes, but is not limited to, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, or 200 nm.
[0059] According to another aspect of the present disclosure, the present disclosure also relates to a positive electrode sheet comprising the positive electrode material.
[0060] According to another aspect of the present disclosure, the present disclosure also relates to a sodium ion battery including the positive electrode sheet.
[0061] The battery of the present disclosure has excellent cycle performance and safety performance.
[0062] Hereinafter, the present disclosure will be further interpreted and explained in combination with specific examples and comparative examples.
[0063] FIG. 1 is a scanning electron microscope image (SEM image) of the iron-based composite phosphate positive electrode material obtained in Example 1 of the present disclosure.
[0064] FIG. 2 is a charge / discharge curve graph of the battery made of the iron-based composite phosphate positive electrode material obtained in Example 1 of the present disclosure.
[0065] Example 1 The method for producing the iron-based composite phosphate positive electrode material includes the steps of: The method includes the steps of: adding sodium dihydrogen phosphate, sodium acetate, and citric acid monohydrate into 5 kg of deionized water with a molar ratio of 1:3:2, and continuing to stir until a clear solution is formed; taking a certain proportion of iron phosphate solid and adding it to the above clear solution to control the total solid content at 35%, where the iron phosphate is a nanoscale aggregate with a particle size of 50-100 nm; sanding, dispersing iron phosphate in the solution, the solution viscosity gradually increases, and stopping the sanding when the solution viscosity reaches 300 Pa.S; spray drying the above solution, the spray drying temperature is 95°C, the time is 8h, and then high-temperature calcination in N2 atmosphere, the heating rate is 2°C / min, the temperature is kept constant at 300°C for 5h, and the temperature is kept constant at 550°C for 12h, and after natural cooling, an iron-based composite phosphate positive electrode material is obtained.
[0066] The results of SEM analysis of the morphology of the material are shown in FIG. 1, and the material is in the form of nano-spherical particles with a uniform size of 100 to 200 nm.
[0067] Example 2 The method for producing the iron-based composite phosphate positive electrode material includes the steps of: The method includes the steps of: adding sodium dihydrogen phosphate, sodium acetate, and citric acid monohydrate into 5 kg of deionized water with a molar ratio of 1:3:5, and continuing to stir until a clear solution is formed; taking a certain proportion of iron phosphate solid and adding it to the above clear solution to control the total solid content at 40%, where the iron phosphate is a nanoscale aggregate with a particle size of 20-95 nm; sanding, dispersing iron phosphate in the solution, the solution viscosity gradually increases, and stopping the sanding when the solution viscosity reaches 350 Pa.S; spray drying the above solution, the spray drying temperature is 120°C, the time is 10h, and then high-temperature calcination in an inert N2 atmosphere, the heating rate is 5°C / min, the temperature is kept constant at 300°C for 4h, and the temperature is kept constant at 600°C for 10h, and after natural cooling, an iron-based composite phosphate positive electrode material is obtained.
[0068] Example 3 The method for producing the iron-based composite phosphate positive electrode material includes the steps of: The method includes the steps of: adding sodium dihydrogen phosphate, sodium acetate, and citric acid monohydrate into 5 kg of deionized water with a molar ratio of 1:3:10, and continuing to stir until a clear solution is formed; taking a certain proportion of iron phosphate solid and adding it to the above clear solution to control the total solid content to 30%, where the iron phosphate is a nanoscale aggregate with a particle size of 75-95 nm; sanding, dispersing the iron phosphate in the solution, the solution viscosity gradually increases, and stopping the sanding when the solution viscosity reaches 400 Pa.S; spray drying the above solution, the spray drying temperature is 80°C, the time is 6h, and then high-temperature calcination in an inert N2 atmosphere, the heating rate is 2.5°C / min, the temperature is kept constant at 290°C for 4.5h, and the temperature is kept constant at 585°C for 11h, and after natural cooling, an iron-based composite phosphate positive electrode material is obtained.
[0069] Example 4 In the preparation method of the iron-based composite phosphate positive electrode material, the sodium source is sodium oxalate, the phosphorus source is sodium phosphate, the carbon source is glucose and citric acid, and the molar ratio of sodium oxalate, sodium phosphate, glucose and citric acid is 0.5:1:1:2.5, other conditions are the same as those in Example 1.
[0070] Example 5 In the preparation method of the iron-based composite phosphate positive electrode material, the sodium source is sodium citrate, the phosphorus source is phosphoric acid, the carbon source is polyethylene glycol, glucose, and sucrose, and the molar ratio of sodium citrate, phosphoric acid, polyethylene glycol, glucose, and sucrose is 1:1:0.1:1:1.5, except that the other conditions are the same as those in Example 1.
[0071] Comparative Example 1 In the preparation method of the iron-based composite phosphate positive electrode material, the total solid content is controlled at 25%, and the sanding is stopped when the solution viscosity reaches 250 Pa.S, except that the other conditions are the same as in Example 1.
[0072] Comparative Example 2 In the preparation method of the iron-based composite phosphate positive electrode material, the total solid content is controlled at 45%, and the sanding is stopped when the solution viscosity reaches 280 Pa.S, except that the other conditions are the same as in Example 1.
[0073] Experimental Example The positive electrode materials of the examples and comparative examples were weighed, mixed with acetylene black and PVDF, respectively, and the positive electrode material, the mass ratio of acetylene black to PVDF was 70:20:10, was applied to an aluminum foil having a diameter of 19 mm, and then the aluminum foil was vacuum dried at 120°C for 12 hours to obtain a positive electrode sheet. Metallic sodium was used as the counter electrode, 1 mol / L NaClO4 ethylene carbonate / diethyl carbonate (volume ratio 1:1) was used as the electrolyte, and the separator was Cellgard2035, and assembled into a button battery of model number CR2016 in a glove box. A constant current charge / discharge test of the above battery was performed, and the current density was 26 mA / g. The test results are shown in FIG. 2. In the voltage range of 2.0 to 4.3 V, the reversible specific capacity is 109 mAh / g.
[0074] The results of performance tests on the initial efficiency and capacity retention rate for the batteries of the examples and comparative examples are shown in Table 1.
[0075] [Table 1]
[0076] As can be seen from Table 1, in the present disclosure, by controlling the viscosity of the solution using an appropriate solid-liquid ratio, the solid reactants are turned into solution in the grinding process, and a uniform reaction function is obtained, and the iron-based composite phosphate positive electrode material obtained by further drying and sintering has excellent initial efficiency and capacity retention. The solid-liquid ratio and solution viscosity of Comparative Example 1 and Comparative Example 2 are not within the scope of protection of the present disclosure, and the capacity retention of the obtained positive electrode material is much lower than that of the positive electrode material of the present application.
[0077] Finally, it should be noted that the above embodiments are only for illustrating the technical solutions of the present disclosure, and are not intended to limit the same. Although the present disclosure has been described in detail with reference to the above embodiments, those skilled in the art can still modify the technical solutions described in the above embodiments, or make equivalent replacements for some or all of the technical features therein, and such modifications or replacements do not cause the essence of the corresponding technical solutions to depart from the scope of the technical solutions of the embodiments of the present disclosure.
Claims
1. The method includes the steps of: uniformly mixing a sodium source, a phosphorus source, a carbon source, and water, and then mixing with iron phosphate to obtain a first mixed system; grinding the first mixed system to obtain a second mixed system, and drying and sintering the second mixed system; In the first mixture system, Na element, Fe element, (PO 4 ) 3- and the total mass of the carbon source is 30% to 40% of the mass of the water, and the viscosity of the second mixture system is 300 Pa.S or more; A method for producing an iron-based composite phosphate cathode material.
2. the sodium source comprises at least one of sodium acetate, sodium nitrate, sodium oxalate, sodium citrate, and sodium phosphate; Preferably, the phosphorus source comprises at least one of sodium dihydrogen phosphate, sodium phosphate, and phosphoric acid; Preferably, the carbon source comprises at least one of citric acid, glucose, sucrose and polyethylene glycol; Preferably, the molar ratio of the phosphorus source, the sodium source and the carbon source is 1:(2.8-3.2):(1-10); A method for producing the iron-based composite phosphate positive electrode material according to claim 1.
3. The molar ratio of Fe to P in the iron phosphate is 0.97 to 1; Preferably, the iron phosphate comprises micron-scale particles and / or nano-scale aggregates. A method for producing the iron-based composite phosphate positive electrode material according to claim 1.
4. The particle size D90 of the iron phosphate in the second mixture is 0.05 to 0.15 μm. A method for producing the iron-based composite phosphate positive electrode material according to claim 1.
5. The viscosity of the second mixture is 300 to 400 Pa.S. A method for producing the iron-based composite phosphate positive electrode material according to claim 1.
6. The drying comprises spray drying; Preferably, the drying temperature is 80 to 120° C. and the drying time is 5 to 10 h. A method for producing the iron-based composite phosphate positive electrode material according to claim 1.
7. The sintering step includes carrying out a first sintering process at a temperature of 290 to 310° C., and then increasing the temperature to 550 to 600° C. and carrying out a second sintering process; Preferably, the time of the first sintering treatment is 3 to 5 h, and the time of the second sintering treatment is 10 to 12 h; Preferably, the heating rate is 2 to 5 ° C. / min. A method for producing the iron-based composite phosphate positive electrode material according to claim 1.
8. An iron-based composite phosphate positive electrode material produced by the method for producing an iron-based composite phosphate positive electrode material according to any one of claims 1 to 7, Preferably, the iron-based composite phosphate positive electrode material is a spherical particle having a particle size of 100 to 200 nm. Iron-based composite phosphate cathode material.
9. The iron-based composite phosphate positive electrode material according to claim 8, Positive electrode sheet.
10. The electrode sheet according to claim 9 , Sodium ion battery.
Citation Information
Patent Citations
Method for preparing lithium iron phosphate membrane electrode
CN103647049A
Preparation method of rate type lithium iron phosphate
CN111554922A
Method for preparing Na4Fe3 (PO4) 2 (P2O7) by homogeneous phase method and application
CN113060713A
Small particle electrode material composition and method for forming the small particle electrode material composition
JP2011508378A
Lithium secondary battery positive electrode active material and method for producing the same