Electrolyte and secondary battery containing same
The use of a specific electrolyte solution with tailored solvents forms a stable inorganic-based solid electrolyte interface, addressing lithium metal battery instability and enhancing long-term stability and performance.
Patent Information
- Application Number
- JP2023529120
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-08
- Filing Date
- 2022-11-04
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2042-11-04
AI Technical Summary
Lithium metal batteries face instability due to high chemical/electrochemical reactivity, leading to the formation of a solid electrolyte interphase layer that causes local current density differences and reduces battery stability, capacity, and coulombic efficiency.
An electrolyte solution comprising a lithium salt, a first solvent with Lewis basicity ≥0.40, and a second solvent with Lewis basicity ≤0.20 is used to form an inorganic-based solid electrolyte interface on the negative electrode, stabilizing the battery during charging and discharging.
The solution enhances battery stability by minimizing desorption at the solid electrolyte interface, allowing for stable operation over a long period and improving life characteristics.
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrolyte solution and a secondary battery containing the same. [Background technology]
[0002] 2. Description of the Related Art With the rapid development of the electrical, electronic, communication and computer industries, the demand for high performance and high stability secondary batteries is increasing sharply.
[0003] A secondary battery has a structure in which an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode is stacked or wound, and the electrode assembly is placed in a battery case into which an electrolyte is injected.
[0004] 2. Description of the Related Art Recently, in order to realize a secondary battery having a high capacity and a high energy density, various researches have been conducted on a lithium metal battery (LMB) using lithium metal as a negative electrode active material.
[0005] The lithium metal-containing anode used in the lithium metal battery has a large capacity relative to its volume or mass, making it an efficient material for reducing the volume and weight of the battery. It also has the lowest reduction potential among anode materials for lithium secondary batteries, which allows it to obtain a high battery voltage.
[0006] However, the lithium metal battery can easily react with electrolytes, impurities, and lithium salts due to the high chemical / electrochemical reactivity of lithium metal to form a solid electrolyte interphase (SEI) layer that does not have electrochemical activity on the surface of the electrode, and the solid electrolyte interphase layer that does not have electrochemical activity can form lithium dendrite on the surface of the lithium metal by causing a local current density difference. In addition, the lithium dendrite increases the contact area of the lithium metal with the electrolyte and increases the reactivity, which can cause problems such as a decrease in the stability of the secondary battery as well as a decrease in the capacity, coulombic efficiency, and life characteristics of the secondary battery.
[0007] As a solution to this problem, efforts have been made to form a solid electrolyte interface with high electrochemical activity on the negative electrode containing lithium metal at the beginning of charging and discharging. Also, in order to efficiently improve the performance of secondary batteries, attempts to form an inorganic-based solid electrolyte interface on the surface of the negative electrode containing lithium metal rather than an organic-based interface have become mainstream, and research to further improve the performance of secondary batteries using this has been continuously required. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Korean published patent no. 2017-0028391 [Non-patent literature]
[0009] [Non-Patent Document 1] Ditchfield, R et al., The Journal of Chemical Physics 54, 724-728 (1971) Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been devised to solve the above-mentioned problems of the prior art, and provides a method for producing lithium ions (Li ions) in an electrolyte solution by comprising: a first solvent and a second solvent, the first solvent and the second solvent each having a specific Lewis basicity among Kamlet-Taft parameters. + The present invention aims to provide an electrolyte solution that can create a solvated environment in which anions are present around the negative electrode containing lithium metal, form a mechanically strong inorganic-based solid electrolyte interface on the negative electrode containing lithium metal, and ensure the stability of the secondary battery even during long-term charging and discharging, while also improving the life characteristics. [Means for solving the problem]
[0011] According to an embodiment of the present invention, there is provided an electrolyte solution comprising: a lithium salt; a first solvent; and a second solvent, wherein, among Kamlet-Taft parameters of the first solvent and the second solvent, Lewis basicity is represented as β1 and β2, respectively, β1 is 0.40 or more, and β2 is 0.20 or less.
[0012] According to another embodiment of the present invention, there is provided a secondary battery including a negative electrode, a positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, the electrolyte including a lithium salt, a first solvent, and a second solvent, the first solvent and the second solvent having Lewis basicity β1 and β2, respectively, the β1 being 0.40 or more and the β2 being 0.20 or less. Effect of the Invention
[0013] The electrolyte according to the present invention can form an inorganic-based solid electrolyte interface having high electrochemical activity on a lithium metal-containing anode, thereby minimizing detachment of the solid electrolyte interface even when a large volume change occurs during charging and discharging of the secondary battery. This can further enhance the stability of the anode, enabling the anode to operate stably for a long period of time.
[0014] In addition, the secondary battery according to the present invention can have a further improved life characteristic by containing an electrolyte solution having the above-mentioned characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described in detail with reference to the following examples. The examples are not limited to the following examples, and may be modified in various ways without departing from the spirit and scope of the invention.
[0016] In this specification, when a part "comprises" a certain component, this does not mean that it excludes other components, but that it may further include other components, unless otherwise specified to the contrary.
[0017] In addition, all numerical ranges indicating the physical properties, dimensions, etc. of the components described in this specification should be understood to be modified in all cases by the term "approximately" unless otherwise specified.
[0018] [Electrolyte] The electrolyte according to an embodiment of the present invention includes a lithium salt; a first solvent; and a second solvent. The first solvent and the second solvent have Kamlet-Taft parameters β1 and β2, respectively, of which Lewis basicity is β1 or more and β2 is 0.40 or less.
[0019] Normally, the electrolyte contains lithium ions (Li +) and enables the reversible charging and discharging of lithium ions. In addition, since the electrolyte is in direct contact with the positive and negative electrodes and a chemical reaction occurs, the selection of the electrolyte is an important variable for stabilizing the surfaces of the positive and negative electrodes and can have a significant impact on the performance of the secondary battery.
[0020] Such electrolytes contain lithium ions (Li + The electrolyte contains a lithium salt, which acts as a path through which the lithium ions (Li + ) is surrounded by the solvent, resulting in solvation.
[0021] Here, the term "solvation" means that the lithium salt is dissolved in a solvent to form lithium ions (Li + ), and the lithium ion (Li + This refers to the phenomenon in which the solvent surrounds the molecule.
[0022] Conversely, the term "non-solvated" refers to a state in which the lithium salt is not dissolved by a solvent in the electrolyte, and lithium ions (Li + ) does not undergo solvation.
[0023] If the electrolyte can dissolve the lithium salt well and can store lithium ions (Li + ) is solvated (e.g., the first solvent), lithium ions (Li + As a result of solvation around the negative electrode, a weak organic-based solid electrolyte interphase (SEI) layer is formed, which is prone to cracking during repeated charging and discharging. In this process, the solid electrolyte interphase layer brings about a local current density difference, forming resin-like lithium on the negative electrode surface, which not only makes it difficult to ensure stability when charging and discharging are repeated, but may also limit the improvement of the life characteristics of the secondary battery.
[0024] In the present invention, the electrolyte contains two or more mixed solvents including a first solvent and a second solvent, and among the Kamlet-Taft parameters of the first solvent and the second solvent, β1 and β2, which represent Lewis basicity, satisfy specific ranges, so that lithium ions (Li + ) can be controlled to a high degree of solvation, and an inorganic-based solid electrolyte interface with high electrochemical activity can be formed on the negative electrode containing lithium metal. Furthermore, the stability of the secondary battery can be ensured even during long-term charging and discharging, and the life characteristics can be improved. Specifically, the secondary battery has excellent life characteristics such as the ratio of the discharge capacity at a specific cycle to the discharge capacity at the first cycle, and the battery can be maintained for a specific number of cycles or more at 0.2C charging and discharging.
[0025] Specifically, in the electrolyte solution of the present invention, by including a first solvent in which the β1 satisfies 0.4 or more, the lithium salt can be dissolved well and the lithium ions (Li + ) is easily transferred, and by including a second solvent having β2 of 0.2 or less, the second solvent acts as a cosolvent for the first solvent to facilitate the transfer of lithium ions (Li + By further stabilizing the solvation of the lithium ion battery, a mechanically strong inorganic-based stable solid electrolyte interface layer can be created, and the formation of resin-like lithium on the surface of the anode can be minimized, which aids in stable charging and discharging. In this case, the stability of the anode, especially the anode containing lithium metal, can be further enhanced, enabling the anode to operate for a long period of time.
[0026] According to an embodiment of the present invention, in order to achieve a desired level of solvation of lithium ions, a first solvent and a second solvent having specific levels of Kamlet Taft parameters β1 and β2 can be selected and used.
[0027] The Kamlet-Taft parameter is a parameter determined from the difference in absorbance wavelength when light of a specific wavelength band is irradiated in a solvent using a UV spectrometer.
[0028] Among the Kamlet-Taft parameters, Lewis basicity (β) is, for example, obtained by measuring the maximum absorption wavelength (λ) of 4-nitroaniline and N,N-diethyl-4-nitroaniline added to the first solvent and the second solvent, respectively, using a UV spectrometer. max ) is the basicity calculated using lithium ions (Li + ) can be a measure representing the degree of solvation of the first and second solvents.
[0029] Specifically, in the electrolyte, lithium ions (Li + ) acts as a Lewis acid that requires electrons, and the first solvent and the second solvent act as Lewis bases that provide electrons, so that the first solvent and the second solvent each have the lithium ion (Li + ) may be bonded to the lithium ion (Li ). Therefore, the first and second solvents may have different maximum absorption wavelengths depending on the degree of bonding. + ), i.e., the degree to which it bonds with lithium ions (Li + ) can be seen.
[0030] In one embodiment of the present invention, the Lewis basicity of the Kamlet-Taft parameters can be determined by measuring absorbance in a wavelength band of about 300 to 500 nm using, for example, a Shimadzu UV-2600 spectrometer.
[0031] Specifically, the Lewis basicity of the Kamlet-Taft parameters is measured by adding 4-nitroaniline to the solvent (first solvent, second solvent) at about 1×10 -4 Add the solution so that the concentration is M, and then measure the maximum absorption wavelength (λ max(4) ) and N,N-diethyl-4-nitroaniline was added to 1X10 -4Add the solution so that the concentration is M, and then measure the maximum absorption wavelength (λ max(n) ) can be calculated respectively.
[0032] Then, the λ max(4) and λ max(n) respectively in kK (kilokaiser, 1kK=1000cm -1 After conversion to units of 1, the Lewis basicity (β) can be calculated using the following equations 1-1 and 1-2.
[0033] [Formula 1-1] λ max(N) (kK)=λ max(n) (kK)X1.035+2.64
[0034] In the above formula 1-1, Said λ max(n) is a 1X10 mixture of the above solvent and N,N-diethyl-4-nitroaniline. -4 The maximum absorbance wavelength (λ max(n) ) and The above 1.035 and 2.64 are the results of dissolving 4-nitroaniline in various non-polar solvents at approximately 1X10 -4 Add the solution so that the concentration is M, and then measure the maximum absorption wavelength (λ max(4) ) and N,N-diethyl-4-nitroaniline was added to 1X10 -4 Add the solution so that the concentration is M, and then measure the maximum absorption wavelength (λ max(n) ) are calculated, and max(4) and λ max(n) These are the gradient and y-intercept obtained by linear regression of
[0035] [Formula 1-2] TIFF2024536952000001.tif2367
[0036] In the above formula 1-2, Said λ max(N) is as defined in formula 1-1 above, Said λ max(4) is a 1X10 mixture of the above solvent and 4-nitroaniline. -4 The maximum absorbance wavelength (λ max(n) ).
[0037] For example, 4-nitroaniline and N,N-diethyl-4-nitroaniline are added to the first solvent, respectively, and their maximum absorption wavelengths are determined, and the Lewis basicity (β1) of the first solvent can be calculated using the above formulas 1-1 and 1-2.
[0038] In addition, 4-nitroaniline and N,N-diethyl-4-nitroaniline are added to the second solvent to determine their respective absorption wavelengths, and the Lewis basicity (β2) of the second solvent can be calculated using the formulas 1-1 and 1-2.
[0039] According to an embodiment of the present invention, the Kamlet-Taft parameter β1, which represents the Lewis basicity of the first solvent, is 0.40 or more, and the Kamlet-Taft parameter β2, which represents the Lewis basicity of the second solvent, is 0.20 or less. By including two mixed solvents having different Lewis basicities, it is possible to create a solvation environment in which anions are distributed around lithium ions, thereby further improving the performance, particularly the life characteristics, of the secondary battery.
[0040] Each component of the electrolyte solution of the present invention will be specifically described below.
[0041] Lithium salts The electrolyte according to one embodiment of the present invention may include a lithium salt. The lithium salt is a lithium ion (Li + ) can act as a passageway through which they can move.
[0042] The lithium salt is not particularly limited in the present invention, and any lithium salt that can be generally used in electrolytes for secondary batteries may be used without limitation.
[0043] Specifically, the lithium salt may include at least one selected from the group consisting of LiPF6, LiAsF6, LiFSI, LiTFSI, LiCF3SO3, LiN(CF3SO2)2, LiBF4, LiBF6, LiSbF6, LiN(C2F5SO2)2, and LiSO3CF3. More specifically, the lithium salt may include at least one selected from the group consisting of LiPF6, LiAsF6, LiFSI, LiTFSI, and LiBF4. When the lithium salt is used, it is easily dissolved and dissociated in the first solvent, and ion migration, solubility, and chemical stability can be further improved.
[0044] Specifically, based on the total volume of the first solvent and the second solvent, the concentration may be, for example, 1 to 8 mol, for example, 1 to 7 mol, for example, 1 to 6 mol, for example, 1 to 5 mol, for example, 2 to 5 mol, for example, 1 to 4 mol, for example, 2 to 4 mol, or for example, 1 to 3 mol. If the concentration of the lithium salt is below the above range, it may be difficult to ensure ion conductivity suitable for driving the secondary battery, and if the concentration of the lithium salt exceeds the above range, the viscosity of the electrolyte increases, causing the lithium ions (Li + ) may decrease in mobility, and the decomposition reaction of the lithium salt itself may increase, resulting in a decrease in the performance of the secondary battery.
[0045] First Solvent An electrolyte according to an embodiment of the present invention may include a first solvent.
[0046] The first solvent dissolves the lithium salt well and converts the lithium ions (Li + ) can play a role in guiding them to move smoothly.
[0047] In the electrolyte according to one embodiment of the present invention, the first solvent may have a Lewis basicity β1 of, for example, 0.40 or more, for example, 0.45 or more, for example, 0.50 or more, for example, 0.55 or more, or for example, 0.60 or more, of Kamlet Taft Peromito. Specifically, the β1 may be, for example, 0.45 or more to 1.00 or less, for example, 0.50 or more to 1.00 or less, for example, 0.55 or more to less than 1.00, for example, 0.55 or more to 0.90 or less, for example, 0.55 or more to 0.80 or less, or for example, 0.55 or more to 0.75 or less, or for example, 0.55 or more to 0.70 or less. When the β1 satisfies the above range, the first solvent dissolves the lithium salt well and converts lithium ions (Li + ) can be made to move more smoothly.
[0048] The first solvent may include, for example, one or more selected from the group consisting of ether-based solvents, ester-based solvents, linear carbonate-based solvents, cyclic carbonate-based solvents, and amide-based solvents.
[0049] The ether-based solvent may include, but is not limited to, one or more selected from the group consisting of, for example, dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, ethyl propyl ether, dimethoxyethane (e.g., 1,2-dimethoxyethane), diethoxyethane, methoxyethoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, triethylene glycol methyl ethyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, tetraethylene glycol methyl ethyl ether, polyethylene glycol dimethyl ether, polyethylene glycol diethyl ether, polyethylene glycol methyl ethyl ether, 1,3-dioxolane, tetrahydrofuran, and 2-methyltetrahydrofuran.
[0050] The ester-based solvent may include at least one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone, but is not limited thereto.
[0051] The linear carbonate solvent may include, but is not limited to, one or more selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), and ethyl propyl carbonate (EPC).
[0052] The cyclic carbonate solvent may include, but is not limited to, one or more selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, vinylethylene carbonate, and halides thereof.
[0053] Moreover, the halide may be, for example, fluoroethylene carbonate (FEC), but is not limited thereto.
[0054] The amide solvent may include, but is not limited to, at least one selected from the group consisting of N-methyl-2-pyrrolidone (NMP), dimethylacetamide (DMAC), and dimethylformamide (DMF).
[0055] When the electrolyte solution contains the first solvent, the lithium salt is dissolved well and the lithium ions (Li + ) can be more smoothly moved, which can be advantageous in improving the performance of the secondary battery.
[0056] Second Solvent The electrolyte according to an embodiment of the present invention may include a second solvent.
[0057] The second solvent acts as a cosolvent for the first solvent and has a smaller Kamlet-Taft parameter than the first solvent, and is therefore more effective in dispersing lithium ions (Li + ) and limits the solvation area of the first solvent, so that lithium ions (Li + This allows anions to participate in the solvation of the electrolyte. This allows a mechanically strong inorganic-based, stable solid electrolyte interface layer to be created, and by minimizing the formation of resin-like lithium on the surface of the anode, a relatively stable lithium anode can be maintained even with sustained charging and discharging, ultimately improving the performance of the secondary battery.
[0058] In order to have such characteristics, it may be very important to adjust the Kamlet-Taft parameters β2, which indicates Lewis basicity, of the second solvent to a specific value.
[0059] Specifically, in the electrolytic solution, the β2 may be, for example, 0.20 or less, for example, 0.19 or less, or for example, 0.18 or less. Specifically, the β2 may be, for example, -0.30 or more to 0.20 or less, for example, -0.25 or more to 0.20 or less, for example, -0.20 or more to 0.20 or less, for example, -0.10 or more to 0.20 or less, for example, 0 or more to 0.20 or less, for example, more than 0 to 0.20 or less, for example, 0.01 or more to 0.20 or less, for example, 0.02 or more to 0.20 or less, for example, 0.10 or more to 0.20 or less, for example, 0.12 or more to 0.19 or less, or for example, 0.12 or more to 0.18 or less. When the β2 satisfies the above-mentioned numerical range, the solvation structure targeted in the present invention can be maintained and a mechanically strong inorganic-based solid electrolyte interface can be formed in the anode. Therefore, detachment of the solid electrolyte interface can be minimized despite a large volume change during charging and discharging of the secondary battery, thereby further enhancing the stability of the anode, thereby enabling the anode to operate stably for a long period of time.
[0060] In addition, the difference between β1 and β2 (β1-β2) may be, for example, 0.30 or more, for example, 0.35 or more, for example, 0.40 or more, for example, 0.42 or more, for example, 0.43 or more, or for example, 0.44 or more. Specifically, the difference between β1 and β2 (β1-β2) may be, for example, 0.30 or more to 1.00 or less, for example, 0.35 or more to 1.00 or less, for example, 0.40 or more to 1.00 or less, for example, 0.42 or more to 1.00 or less, for example, 0.44 or more to less than 1.00, for example, 0.44 or more to 0.90 or less, or for example, 0.44 or more to 0.87 or less. When the difference between β1 and β2 (β1-β2) satisfies the above range, it may be more advantageous to realize the effect aimed at in the present invention.
[0061] Meanwhile, according to an embodiment of the present invention, the Kamlet-Taft parameter of the second solvent, which indicates the polarizability of the solvent, may be 0.15 or more.
[0062] In order to achieve the intended effect of the present invention, the second solvent must stabilize the electrolyte environment mainly composed of dipole-shaped cations and anions, and be well mixed in the electrolyte solution without layer separation. The TIFF2024536952000002.tif98 value can be an index for determining the degree of mixing of the second solvent in the electrolyte.
[0063] The above The TIFF2024536952000003.tif98 value can be determined by irradiating a solvent with light of a specific wavelength band, for example, a wavelength band of about 400 to 700 nm, using a UV spectrometer and measuring the maximum absorbance.
[0064] For example, a zwitterionic dye (Reichardt's dye), 2,6-Diphenyl-4-(2,4,6-triphenyl-1-pyridinio)phenolate, was dissolved in a solvent (second solvent, water, tetramethylsilane (TMS)) at 1X10-4 Add the solution so that the concentration is M, and measure the maximum absorption wavelength (λ max ) and calculate the polarizability of the solvent using the following equations 2-1 and 2-2. You can get TIFF2024536952000004.tif1517.
[0065] [Formula 2-1] TIFF2024536952000005.tif1849
[0066] In the above formula 2-1, λ max is dissolved in a solvent, e.g., 1x10 2,6-diphenyl-4-(2,4,6-triphenyl-1-pyridinio)phenolate in a second solvent, water, or tetramethylsilane (TMS). -4 This is the maximum absorption wavelength for the solvent when it is added to achieve a concentration of M, and the 28591 is a constant, which is the product of the Planck constant (h), the speed of light (c), and the Avogadro number (NA). T (30) represents the electron transition energy per mole and therefore has the above constant value.
[0067] [Formula 2-2] TIFF2024536952000006.tif24102
[0068] In the above formula 2-2, E T (30, solvent) is E when the solvent is the second solvent T (30) E T (30, water) is E when the solvent is water. T (30) E T (30, TMS) is the E when the solvent is tetramethylsilane (TMS). T (30).
[0069] According to an embodiment of the present invention, the second solvent The TIFF2024536952000007.tif98 value may be, for example, 0.15 or more, for example, 0.16 or more, for example, 0.15 or more to less than 1.00, for example, 0.15 or more to 0.90 or less, for example, 0.15 or more to 0.80 or less, for example, 0.15 or more to 0.70 or less, for example, 0.15 or more to 0.60 or less, for example, 0.15 or more to 0.50 or less, for example, 0.15 or more to 0.40 or less, for example, 0.15 or more to 0.30 or less, for example, 0.15 or more to 0.25 or less, or for example, 0.15 or more to 0.20 or less. When the TIFF2024536952000008.tif98 value satisfies the above numerical range, the second solvent can be well mixed in the electrolyte without phase separation, thereby realizing the intended effect of the present invention.
[0070] In particular, according to an embodiment of the present invention, the second solvent has a Kamlet-Taft parameter β2, which represents Lewis basicity, of 0.20 or less, and a polarizability parameter β2, which represents the polarizability of the solvent, of 0.20 or less. If the TIFF2024536952000009.tif98 value is 0.15 or more, it may be more advantageous to realize the effects aimed at in the present invention.
[0071] Meanwhile, according to yet another embodiment of the present invention, the LUMO (Lowest Unoccupied Molecular Orbital) energy level of the second solvent is, for example, more than -1.0 eV and less than 0 eV, for example, -0.95 eV or more and less than 0 eV, for example, -0.95 eV or more and -0.01 eV or less, for example, -0.95 eV or more and -0.05 eV or less, for example, -0.95 eV or more and -0.08 eV or less, for example, -0.95 eV or more and -0.09 eV or less, for example, -0.95 eV or more and -0.10 eV or less, for example, -0.95 eV or more and -0.15 eV or less, For example, it may be -0.95 eV or more to -0.16 eV or less, for example, -0.95 eV or more to -0.17 eV or less, for example, -0.95 eV or more to -0.18 eV or less, for example, -0.95 eV or more to -0.20 eV or less, for example, -0.95 eV or more to -0.30 eV or less, for example, -0.95 eV or more to -0.40 eV or less, for example, -0.95 eV or more to -0.50 eV or less, or for example, -0.90 eV or more to -0.50 eV or less. When the LUMO energy level of the second solvent satisfies the above numerical range, a stable electrolyte environment can be maintained without a decrease in the amount of solvent in the electrolyte even during continuous charging and discharging due to the high LUMO energy level.
[0072] The LUMO energy level of the second solvent is an energy level calculated by calculation of the extended Gaussian type basis (basis) using the Gaussian 16, Revision A.03 program, as in Ditchfield, R et al., The Journal of Chemical Physics 54, 724-728 (1971). For example, the LUMO energy level is an energy level calculated by the theory of B3LYP / 6-31G+(d,p) level of density functional theory (DFT), Grimme dispersion (D3BJ) and ultrafine integration using the program (Parr, RG & Yang, W. Density-functional theory of atoms and molecules (Oxford Univ. Press [ua], 1994). Frisch, MJ et al. Gaussian 16 Rev. C. 01. (2016)).
[0073] The second solvent may include, for example, one or more selected from the group consisting of furan, anisole, ethoxybenzene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,2-difluorobenzene, and fluorobenzene.
[0074] According to yet another embodiment of the present invention, the second solvent may be a non-fluorinated solvent, for example, the second solvent may include one or more selected from the group consisting of furan, anisole, and ethoxybenzene.
[0075] In this case, even in a long-term charge-discharge environment, the lithium ion (Li + ) does not undergo solvation (non-solvation), and a stable electrolyte environment can be maintained during charging and discharging, and stability can be maintained especially when a negative electrode containing lithium metal is used and / or when the negative electrode is combined with a positive electrode to be used as a complete secondary battery, thereby providing excellent performance of the secondary battery and further having an advantage in terms of cost efficiency.
[0076] Meanwhile, according to an embodiment of the present invention, the contents of the first solvent and the second solvent are adjusted to maintain an optimal electrolyte environment, thereby further improving the performance of the secondary battery.
[0077] Specifically, the amount of the second solvent may be the same as or greater than the amount of the first solvent.
[0078] More specifically, the volume ratio of the first solvent to the second solvent may be, for example, 1:1 to 1:3, for example, 1:1 to 1:2, for example, 1:2 to 1:3, for example, 1:1.5 to 1:2.5, or for example, 1:2. When the volume ratio of the first solvent to the second solvent satisfies the above range, the concentration of the electrolyte solution is reduced while lithium ions (Li + Since the degree of solvation of the above-mentioned solvent can be controlled, when the solvent having the above-mentioned volume ratio is applied to a secondary battery, the stable solvation structure targeted by the present invention can be maintained.
[0079] According to one embodiment of the present invention, the first solvent may be one or more, and the second solvent may be one or more. Specifically, the first solvent may be one, and the second solvent may be one. That is, the types of solvents contained in the electrolytic solution may be two or more, or three or more, and specifically, may be two, but are not limited thereto.
[0080] [Additives] The electrolyte according to an embodiment of the present invention may include an additive.
[0081] The additives may include various commonly used additives as long as they do not impair the effects of the present invention, and may be added in various amounts depending on the desired properties and applications.
[0082] Specifically, the electrolyte may further include a nitric acid compound, for example, at least one selected from the group consisting of lithium nitrate (LiNO3), potassium nitrate (KNO3), cesium nitrate (CsNO3), magnesium nitrate (MgNO3), barium nitrate (BaNO3), lithium nitrite (LiNO2), potassium nitrite (KNO2), and cesium nitrite (CsNO2).
[0083] Other examples include fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinyl ethyl carbonate (VEC), lithium fluoride (LiF), and lithium sulfide (LiS x , 2≦x≦8), and additives such as lithium phosphate difluoride (LiPO2F2).
[0084] The additive may be included in an amount of, for example, more than 0 wt % to 30 wt %, for example, 1 wt % to 30 wt %, or for example, 5 wt % to 20 wt %, based on the total weight of the electrolyte solution. If the content of the additive is too high, the performance of the secondary battery may be deteriorated.
[0085] [Secondary battery] According to one embodiment of the present invention, there is provided a secondary battery including the electrolytic solution.
[0086] The secondary battery includes a negative electrode, a positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, the electrolyte including a lithium salt, a first solvent, and a second solvent, and the first solvent and the second solvent have Lewis basicities β1 and β2, respectively, of Kamlet-Taft parameters, and the β1 may be 0.40 or more and the β2 may be 0.20 or less.
[0087] Specifically, the positive electrode may include a positive electrode current collector and a positive electrode active material applied to one or both sides of the positive electrode current collector.
[0088] The positive electrode current collector is not particularly limited as long as it supports a positive electrode active material, does not induce chemical changes in the secondary battery, and has high electrical conductivity.
[0089] The positive electrode current collector may be, for example, stainless steel, aluminum, nickel, titanium, palladium, baked carbon, copper or stainless steel whose surface has been treated with carbon, nickel, silver, or the like, or an aluminum-cadmium alloy.
[0090] The positive electrode current collector may have fine projections and recesses on its surface to strengthen the bonding force with the positive electrode active material, and may be in various forms such as a film, a sheet, a foil, a mesh, a net, a porous body, a foam, a nonwoven fabric, etc.
[0091] The positive electrode active material may include a positive electrode active material, and optionally a conductive material and a binder.
[0092] The positive electrode active material is, for example, LiMn2O4, V2O5, LiCoO2, LiNiO2, LiFePO4, Li4Ti5O 12 , LiNi x Co y Mn z O2(x+y+z=1) and LiNi x Co y Al z O2(x+y+z=1).
[0093] The conductive material is used to improve electrical conductivity, and may be any electronically conductive material that does not cause chemical changes in the secondary battery.
[0094] The conductive material may be, for example, carbon black, graphite, carbon fiber, carbon nanotubes, metal powder, conductive metal oxide, organic conductive material, etc., and currently commercially available conductive materials may include acetylene black series (e.g., products of Chevron Chemical Company or Gulf Oil Company), Ketjen Black EC series (products of Armak Company), Vulcan XC-72 (products of Cabot Company), and SUPER P, etc.
[0095] In addition, the positive electrode active material may further include a binder having a function of fixing the positive electrode active material to the positive electrode current collector and binding between the active materials. As the binder, various types of binders may be used, such as polyvinylidene fluoride-hexafluoropropylene (PVDF-co-HFP), polyvinylidene fluoride (PVDF, poly(vinylidene fluoride), polyacrylonitrile, polymethyl methacrylate, styrene butadiene rubber (SBR), carboxyl methyl cellulose (CMC), poly(acrylic acid, PAA), poly(vinyl alcohol, PVA), etc.
[0096] Meanwhile, the negative electrode may include a negative electrode current collector and a negative electrode active material located on the negative electrode current collector, or the negative electrode may include a lithium metal thin film.
[0097] The negative electrode current collector is for supporting the negative electrode active material, and is not particularly limited as long as it has excellent conductivity and is electrochemically stable in the voltage region of the secondary battery. For example, copper, stainless steel, nickel, titanium, palladium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, silver, or the like, aluminum-cadmium alloy, or the like may be used.
[0098] The negative electrode current collector may have fine projections and recesses on its surface to strengthen the bonding force with the negative electrode active material, and may be in various forms such as a film, a sheet, a foil, a mesh, a net, a porous body, a foam, a nonwoven fabric, etc.
[0099] The negative electrode active material is lithium (Li + The intercalation or deintercalation of lithium ions may include a material capable of reversibly intercalating or deintercalating lithium ions, a material capable of reversibly forming a lithium-containing compound by reacting with lithium ions, lithium metal, or a lithium alloy.
[0100] The lithium ion (Li + The material capable of reversibly absorbing and releasing . ) may be, for example, crystalline carbon, amorphous carbon, or a mixture thereof.
[0101] The lithium ion (Li + The material capable of reacting with ZnO to reversibly form a lithium-containing compound may be, for example, tin oxide, titanium nitrate, or silicon.
[0102] The lithium alloy may be, for example, an alloy of lithium (Li) and a metal including one or more selected from the group consisting of sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), aluminum (Al), and tin (Sn).
[0103] Specifically, the negative electrode active material may be lithium metal, preferably in the form of a lithium metal thin film or lithium metal powder.
[0104] The method for forming the negative electrode active material is not particularly limited, and may be a layer or film forming method commonly used in the art, such as compression bonding, coating, or deposition. In addition, the negative electrode of the present invention may include a case where a thin metallic lithium film is formed on a metal plate by initial charging after assembling a battery without a thin lithium film on a current collector.
[0105] The electrolyte contains lithium ions and serves to cause an electrochemical oxidation or reduction reaction between the positive electrode and the negative electrode using the lithium ions as a medium, as described above.
[0106] The electrolyte may be injected at an appropriate stage in the manufacturing process of the electrochemical device depending on the manufacturing process and required properties of the final product, i.e., before assembly of the electrochemical device or at the final stage of assembly of the electrochemical device.
[0107] Meanwhile, a separator may be further included between the positive electrode and the negative electrode.
[0108] The separator membrane is for physically separating the two electrodes in the secondary battery of the present invention, and any separator membrane that is usually used in lithium secondary batteries can be used without any particular limitation. In particular, a separator membrane that has low resistance to the ion movement of the electrolyte and excellent electrolyte humidification capacity is preferred.
[0109] The separator may be made of a porous substrate. The porous substrate may be any porous substrate typically used in electrochemical devices, such as, but not limited to, a polyolefin-based porous membrane or nonwoven fabric.
[0110] Examples of the polyolefin-based porous membrane include membranes formed of polyolefin-based polymers such as polyethylene (e.g., high density polyethylene, linear low density polyethylene, low density polyethylene, ultra-high molecular weight polyethylene), polypropylene, polybutylene, and polypentene, either alone or in combination.
[0111] The nonwoven fabric may include, in addition to polyolefin-based nonwoven fabric, nonwoven fabrics formed of polymers such as polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyether sulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalate, each of which may be used alone or in combination. The structure of the nonwoven fabric may be a spunbonded nonwoven fabric or a meltblown nonwoven fabric made of long fibers.
[0112] The thickness of the porous substrate is not particularly limited, but may be 1 to 100 um or 5 to 50 um.
[0113] The size and porosity of the pores in the porous substrate are not particularly limited. For example, the size of the pores in the porous substrate may be 0.001 to 50 μm, and the porosity may be 10 to 95%.
[0114] In addition to the general winding process, the secondary battery according to the present invention can be manufactured by laminating (stack) and folding processes of the separator and the electrodes.
[0115] The shape of the secondary battery is not particularly limited, and may include various shapes such as a cylindrical type, a laminated type, and a coin type.
[0116] In addition, the secondary battery according to the embodiment of the present invention can last for 120 cycles or more at a charge / discharge rate of 0.2 C-rate.
[0117] The secondary battery according to an embodiment of the present invention includes the electrolyte, thereby improving the life characteristics of the secondary battery.
[0118] [Battery module] According to an embodiment of the present invention, a battery module including the secondary battery as a unit battery can be provided.
[0119] The battery module can be used as a power source for medium to large devices that require high temperature stability, long cycle characteristics, and high capacity characteristics.
[0120] Examples of the medium- to large-sized devices include, but are not limited to, power tools that are powered by battery-powered motors; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs); electric two-wheeled vehicles, including electric bicycles (E-bikes) and electric scooters (E-scooters); electric golf carts; and power storage systems.
[0121] The above contents will be described in detail with reference to the following examples. However, the following examples are only for illustrating the present invention, and the scope of the examples is not limited to these examples.
[0122] <Example 1> Electrolyte and secondary battery production 1 LiFSI was prepared as the lithium salt. In addition, 1,2-dimethoxyethane (DME) with a Kamlet-Taft parameter β1 of 0.62, which indicates the Lewis basicity, was prepared as the first solvent, and anisole with a Kamlet-Taft parameter β2 of 0.18, which indicates the Lewis basicity, was prepared as the second solvent.
[0123] The first solvent and the second solvent were mixed in a volume ratio of 1:2 to prepare a mixed solvent, which was then mixed with 3.0 mol of LiFSI per total volume (L) of the mixed solvent to prepare an electrolyte solution.
[0124] In the manufacture of the secondary battery, a LiFePO4 electrode with a thickness of 90 um was used as the positive electrode (LFP), and a lithium metal thin film with a thickness of 20 um was used as the negative electrode (Li). In this case, the positive electrode (LFP) was an electrode in which a slurry was prepared by mixing LiFePO4 as a positive electrode active material, Super P as a conductive material, and polyvinylidene fluoride (PVDF, poly(vinylidene fluoride)) as a binder in a weight ratio of 93.5:4:2.5, and then cast on a 20 um aluminum foil as a current collector.
[0125] The prepared positive and negative electrodes were placed facing each other, a polyethylene separator was interposed between them, and 80 ul of the electrolyte was poured therein to prepare a secondary battery.
[0126] <Example 2> Electrolyte and secondary battery production 2 An electrolyte solution and a secondary battery using the same were manufactured in the same manner as in Example 1, except that a second solvent having β2 of 0.17 was used.
[0127] <Example 3> Electrolyte and secondary battery production 3 An electrolyte solution and a secondary battery using the same were manufactured in the same manner as in Example 1, except that a second solvent having a molecular weight of β2 of 0.12 was used and 1.0 mol of LiFSI was used per total volume (L) of the mixed solvent of the first solvent and the second solvent.
[0128] <Example 4> Electrolyte and secondary battery production 4 An electrolyte solution and a secondary battery using the same were manufactured in the same manner as in Example 1, except that a second solvent having β2 of −0.25 was used.
[0129] <Example 5> Preparation of electrolyte and secondary battery 5 An electrolyte solution and a secondary battery using the same were manufactured in the same manner as in Example 1, except that a second solvent with β2 of 0.02 was used.
[0130] <Example 6> Preparation of electrolyte and secondary battery 6 An electrolyte solution and a secondary battery using the same were manufactured in the same manner as in Example 1, except that a second solvent having β2 of 0.04 was used.
[0131] <Example 7> Preparation of electrolyte and secondary battery 7 An electrolyte solution and a secondary battery using the same were manufactured in the same manner as in Example 1, except that a second solvent having β2 of 0.12 was used and 2.0 mol of LiFSI was used per total volume (L) of the mixed solvent of the first solvent and the second solvent.
[0132] <Comparative Example 1> Electrolyte and Secondary Battery Production 8 An electrolyte solution and a secondary battery using the same were manufactured in the same manner as in Example 1, except that a second solvent having β2 of 0.55 was used.
[0133] <Comparative Example 2> Electrolyte and Secondary Battery Production 9 An electrolyte solution and a secondary battery using the same were manufactured in the same manner as in Example 1, except that the first and second solvents having β1 of 0.18 and β2 of −0.25 were used.
[0134] <Experimental Example 1> Kamlet-Taft parameters: Lewis basicity (β(β1, β2)) Among the Kamlet-Taft parameters, Lewis basicity (β(β1, β2)))) was determined by measuring absorbance in the wavelength range of approximately 300 to 500 nm using a Shimadzu UV-2600 spectrometer.
[0135] Specifically, 1X10 4-nitroaniline was added to the solvent (first solvent, second solvent) for which the (β(β1, β2)) value is to be measured. -4 Add the solution so that the concentration is M, and then measure the maximum absorption wavelength (λ max(4) ) and N,N-diethyl-4-nitroaniline was added to 1X10 -4 Add the solution so that the concentration is M, and then measure the maximum absorption wavelength (λ max(n) ) were calculated respectively.
[0136] Said λ max(4) and λ max(n) respectively in kK (kilokaiser, 1kK=1000cm -1 ) units, and the Lewis basicity (β(β1, β2)) was calculated using the following formulas 1-1 and 1-2.
[0137] [Formula 1-1] λ max(N) (kK)=λ max(n) (kK)X1.035+2.64
[0138] In the above formula 1-1, Said λ max(n) is a 1X10 mixture of the above solvent and N,N-diethyl-4-nitroaniline. -4 The maximum absorbance wavelength (λ max(n) ), and the above 1.035 and 2.64 are the results of dissolving 4-nitroaniline in various non-polar solvents at about 1×10-4 Add the solution so that the concentration is M, and then measure the maximum absorption wavelength (λ max(4) ) and N,N-diethyl-4-nitroaniline was added to 1X10 -4 Add the solution so that the concentration is M, and then measure the maximum absorption wavelength (λ max(n) ) are calculated, and max(4) and λ max(n) These are the gradient and y-intercept obtained by linear regression of
[0139] [Formula 1-2] TIFF2024536952000010.tif1747
[0140] In the above formula 1-2, Said λ max(N) is as defined in the above formula 1-1, and the λ max(4) is a 1X10 mixture of the above solvent and 4-nitroaniline. -4 The maximum absorbance wavelength (λ max(n) ).
[0141] <Experimental Example 2> Polarizability of the solvent TIFF2024536952000011.tif1517Kamlet-Taft parameters, solvent polarizability TIFF2024536952000012.tif1517 was determined by measuring absorbance in the wavelength range of approximately 400 to 700 nm using a Shimadzu UV-2600 spectrometer.
[0142] Specifically, a zwitterionic dye (Reichardt's dye), 2,6-diphenyl-4-(2,4,6-triphenyl-1-pyridinio)phenolate, was added to the solvent (second solvent, water, tetramethylsilane (TMS)) at a concentration of 1X10 -4Add the solution so that the concentration is M, and measure the maximum absorption wavelength (λ max ) were calculated respectively.
[0143] The maximum absorption wavelength (λ max ) and calculate the polarizability of the solvent using the following equations 2-1 and 2-2. I asked for TIFF2024536952000013.tif1517.
[0144] [Formula 2-1] TIFF2024536952000014.tif1744In the above formula 2-1, λ max is dissolved in a solvent, e.g., 1x10 2,6-diphenyl-4-(2,4,6-triphenyl-1-pyridinio)phenolate in a second solvent, water, or tetramethylsilane (TMS). -4 is the maximum absorbance wavelength for the solvent when it is added to give a concentration of M, [Formula 2-2] TIFF2024536952000015.tif28118 In the above formula 2-2, E T (30, solvent) is E when the solvent is the second solvent T (30), and E T (30, water) is E when the solvent is water. T (30), and E T (30, TMS) is the E when the solvent is tetramethylsilane (TMS). T (30).
[0145] <Experimental Example 3> LUMO Energy Level The LUMO energy level was calculated using the Gaussian 16, Revision A.03 program, based on the B3LYP / 6-31G+(d,p) level theory of density functional theory (DFT), Grimme dispersion (D3BJ) and ultrafine integration (Parr, RG & Yang, W. Density-functional theory of atoms and molecules (Oxford Univ. Press[ua], 1994). Frisch, MJ et al. Gaussian 16 Rev.C.01.(2016)).
[0146] <Experimental Example 4> Evaluation of charge / discharge and life (cycle) characteristics of secondary batteries The secondary batteries according to Examples 1 to 7 and Comparative Examples 1 and 2 were each charged for 5 cycles at 0.1C, 0.25C, 0.5C, 0.75C, 1C, 2C, and 3C until the voltage reached 3.8V, and then discharged to 2.0V at the same C-rate to evaluate the charge / discharge rate.
[0147] After the experiment, the charge / discharge characteristics of the secondary battery were evaluated by comparing how much the discharge capacity at 0.1C was maintained at a high C-rate for each electrolyte, and the lifespan characteristic (%) of the secondary battery was calculated as shown in the following [Formula A]: [Formula A] Secondary battery life characteristics (%) = Discharge capacity at 120th cycle / Discharge capacity at 1st cycle x 100 (%) The results obtained in the above Evaluation Examples 1 to 4 are summarized in Table 1 below.
[0148] [Table 1]
[0149] As can be seen from Table 1, the secondary batteries of Examples 1 to 7, in which the electrolyte solution in which the β1 of the first solvent is 0.40 or more and the β2 of the second solvent is 0.20 or less was used, had a ratio of the discharge capacity at the 120th cycle to the discharge capacity at the 1st cycle of almost 85% or more, and were confirmed to have excellent life characteristics by lasting for more than 120 cycles at 0.2C charge / discharge.
[0150] Conversely, in the case of the secondary battery according to Comparative Example 1, in which an electrolyte solution in which the β1 of the first solvent was 0.40 or more but the β2 of the second solvent was 0.55 was used, cycling using LFP was impossible. In the case of Comparative Example 2, in which an electrolyte in which the β1 of the first solvent was low at 0.18 but the β2 of the second solvent was 0.20 or less was used, it was impossible to fabricate a full cell due to layer separation of the electrolyte, and it was impossible to analyze the performance of the secondary battery.
[0151] From the above results, it was confirmed that in the case of the electrolyte solutions according to Examples 1 to 7 of the present invention, an inorganic-based solid electrolyte interface having high electrochemical activity is formed in the negative electrode, enabling the negative electrode to operate stably for a long period of time, thereby improving the performance of the secondary battery.
Claims
1. A lithium salt; A first solvent; a second solvent, The Lewis basicity of the Kamlet-Taft parameters of the first and second solvents is β 1 and β 2 Expressed as: Said β 1 is 0.40 or more, Said β 2 is 0.20 or less.
2. 2. The electrolyte solution according to claim 1, wherein a volume ratio of the first solvent to the second solvent is 1:1 to 1:
3.
3. Said β 1 and the β 2 The difference between 1 -β 2 2. The electrolyte according to claim 1, wherein the σ is 0.30 or more.
4. 2. The electrolyte solution according to claim 1, wherein the first solvent comprises at least one selected from the group consisting of ether-based solvents, ester-based solvents, linear carbonate-based solvents, cyclic carbonate-based solvents, and amide-based solvents.
5. Said β 2 The electrolyte according to claim 1, wherein the electrolytic solution is −0.25 to 0.
20.
6. Among the Kamlet-Taft parameters of the second solvent, 2. The electrolyte of claim 1 comprising a solvent having a value of 0.15 or greater.
7. The electrolyte according to claim 1, wherein the second solvent has a LUMO (Lowest Unoccupied Molecular Orbital) energy level of more than -1.0 eV and less than 0 eV.
8. 2. The electrolyte of claim 1, wherein the second solvent comprises at least one selected from the group consisting of furan, anisole, ethoxybenzene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropylether, 1,2-difluorobenzene, and fluorobenzene.
9. The electrolyte of claim 1 , wherein the second solvent is a non-fluorinated solvent.
10. The lithium salt is LiPF 6 , LiAsF 6 , LiFSI, LiTFSI, LiCF 3 SO 3 , LiN(CF 3 SO 2 ) 2 , LiBF 4 , LiBF 6 , LiSbF 6 , LiN (C 2 F 5 SO 2 ) 2 , and LiSO 3 CF 3 The electrolyte solution according to claim 1, comprising one or more selected from the group consisting of:
11. The electrolyte according to claim 1 , wherein the electrolyte contains 1 to 8 mol of the lithium salt based on a total volume of the first solvent and the second solvent.
12. The battery includes a negative electrode, a positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte; The electrolyte A lithium salt; A first solvent; a second solvent, The Lewis basicity of the Kamlet-Taft parameters of the first and second solvents is β 1 and β 2 Expressed as: Said β 1 is 0.40 or more, Said β 2 A secondary battery, wherein the resistance is 0.20 or less.
Citation Information
Patent Citations
Electrolytic solution for lithium ion battery
JP1997022722A
Energy storage device, its module and automobile using it
JP2006172775A
Electrolyte solution and battery
JP2006294374A
Nonaqueous electrolyte secondary battery
JP2007335406A
Nonaqueous electrolyte battery
JP2008218381A