Process for preparing lithium transition metal phosphate cathode materials

The method of forming lithium transition metal phosphate cathode materials within a conductive carbon matrix addresses inefficiencies and environmental concerns of existing LFP synthesis by using a solid organogel precursor mixture, resulting in a homogeneous and cost-effective product with improved properties.

JP2024537089AActive Publication Date: 2024-10-10ASPEN AEROGELS INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024519870
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-01
Filing Date
2023-03-30
Publication Date
2024-10-10
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Existing methods for preparing lithium ion battery cathode materials, such as lithium iron phosphate (LFP), are inefficient, costly, and environmentally harmful due to the use of expensive ores, toxic waste generation, and the need for extensive mechanical mixing and energy-intensive processes.

Method used

A method involving the formation of lithium transition metal phosphate cathode materials within a conductive carbon matrix using a solid organogel precursor mixture, which combines precursors in a fluid state, forms a solid organogel, and pyrolyzes it to create a homogeneous and conductive carbon matrix, reducing energy consumption and waste generation.

Benefits of technology

The method achieves a more homogeneous product with improved tap density and reduced impurities, providing a scalable and cost-effective synthesis of lithium transition metal phosphate cathode materials suitable for commercial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537089000001_ABST
    Figure 2024537089000001_ABST
Patent Text Reader

Abstract

The present disclosure is directed to a method for forming lithium transition metal phosphate and fluorophosphate materials within a conductive carbon matrix. The disclosed method is advantageous in that it utilizes inexpensive reactants, can reduce the formation of impurities during synthesis while providing a more homogeneous product, and can provide a cathode material with improved tap density compared to conventional lithium transition metal phosphates. The lithium transition metal phosphate and fluorophosphate materials prepared by the disclosed method are intimately mixed with carbon within a continuous three-dimensional conductive carbon matrix. The materials prepared according to the disclosed method are suitable for use in environments involving electrochemical reactions, for example as cathode materials in lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is a continuation of U.S. Provisional Patent Application No. 63 / 381777, filed November 1, 2022, U.S. Provisional Patent Application No. 63 / 381771, filed November 1, 2022, U.S. Provisional Patent Application No. 63 / 381694, filed October 31, 2022, U.S. Provisional Patent Application No. 63 / 381687, filed October 31, 2022, U.S. Provisional Patent Application No. 63 / 381681, filed October 31, 2022, U.S. Provisional Patent Application No. 63 / 381692, filed October 31, 2022, each of which is incorporated by reference in its entirety herein. This application claims priority to and benefit of U.S. Provisional Patent Application No. 3 / 381672, filed October 31, 2022, U.S. Provisional Patent Application No. 63 / 381666, filed October 18, 2022, U.S. Provisional Patent Application No. 63 / 416996, filed October 7, 2022, U.S. Provisional Patent Application No. 63 / 378756, filed October 7, 2022, U.S. Provisional Patent Application No. 63 / 352571, filed June 15, 2022, U.S. Provisional Patent Application No. 63 / 336640, filed April 29, 2022, and U.S. Provisional Patent Application No. 63 / 326353, filed April 1, 2022.

[0002] The present disclosure relates generally to cathode active materials for use in lithium-ion batteries and processes for making the same. [Background technology]

[0003] One of the most common forms of rechargeable batteries is the lithium-ion battery (LIB). LIBs are widely found in a variety of applications, from handheld electronics to automobiles. LIBs are a type of battery in which lithium ions migrate from the anode to the cathode during discharge and from the cathode to the anode during a charging cycle (recharging). Traditionally, the anode of a LIB is made of graphite and / or alloyed materials (e.g., Si), or oxides (e.g., Li), where the lithium ions intercalate into the graphite layers during the charging cycle. 4 Ti 5 O 12) to provide energy storage. LIB cathode materials are typically oxide compounds of nickel, cobalt, or manganese ("NCM"), or aluminum. NCM cathode materials are of interest because they have high charge capacities (approximately 200 milliamp hours per gram (mAh / g)) compared to other types of cathode materials. However, these materials can be expensive to prepare, require expensive ores to be obtained and processed to provide the necessary precursors, and can have adverse environmental impacts due to the generation of toxic waste materials during acquisition and processing.

[0004] Another LIB cathode material is lithium iron phosphate (e.g., LiFePO 4 Such LFP cathode materials have a lower theoretical charge capacity (about 170 mAh / g) than NCM cathode materials. Nevertheless, LFP has many commercial advantages, including but not limited to reduced environmental impact, as well as inexpensive precursors compared to ores for preparing NCMs. However, LFP has synthetic disadvantages that offset some of these advantages. For example, most previously reported synthetic processes involve extensive mechanical mixing of solid-phase precursor materials (e.g., via ball milling) to achieve the intimate contact between the precursors necessary to provide a homogenous product.

[0005] It would therefore be desirable in the art to provide a method for preparing lithium transition metal phosphate cathode active materials that is efficient, relatively inexpensive, and has a low environmental impact. Summary of the Invention

[0006] The present technology is generally directed to methods for preparing lithium transition metal phosphate cathode materials within a conductive carbon matrix.

[0007] Various solid and solution phase methods for forming lithium iron phosphate (LFP) materials have been previously reported, see, for example, U.S. Patent Application Publication No. 2011 / 0110838 to Wang et al., U.S. Patent Application Publication No. 2008 / 0099720 to Huang et al., U.S. Patent Application Publication Nos. 2010 / 0065787 and 2011 / 0091772 to Mishima et al., U.S. Patent No. 7,988,879 to Park et al., U.S. Patent No. 7,060,238 to Saidi et al., European Patent Application Publication No. 1,921,698 to Dong, and International Patent Application Publication No. WO2004 / 092065 to Barker et al.

[0008] The methods disclosed herein have advantages, at least in some aspects, over previously reported methods of preparing LFP materials that include an LFP within a conductive carbon matrix. Previously reported methods, for example, provide LFP cathode materials that include carbon, but the carbon is typically added using either carbon particles (e.g., carbon black) or pyrolysis of a mixture of an LFP precursor and sugar molecules. None of these conventional methods of introducing carbon into a cathode material provide a conductive matrix comparable to that provided according to the methods of the present disclosure.

[0009] Benefits of some or all of the embodiments described herein include the elimination of various process steps in LFP synthesis compared to more conventional methods by which LFP cathode materials are synthesized. For example, many conventional LFP processes use solution chemistry techniques that can generate large amounts of waste water (e.g., aqueous ammonia solutions). Waste water generation is almost entirely avoided in some of the embodiments of the present disclosure. Additionally, conventional solid-state reactions to produce LFPs (and largely avoid waste water generation) have the disadvantage of requiring significant energy input to mix and grind large amounts of dense solid-state powders. Also, due to the difficulty in achieving and maintaining a compositionally uniform mixture of the precursors, the product of the powder mixing is unlikely to be a homogenous and uniform LFP. Because embodiments of the present disclosure maintain intimate contact of the reactants in a viscous medium, the extent and duration of mixing and grinding is reduced compared to conventional techniques. This reduces the energy and process complexity required for the synthesis of LFPs. An additional advantage is that the present method only requires pyrolysis under an inert (e.g., nitrogen) atmosphere. In contrast, certain conventional methods require a reducing (hydrogen) atmosphere, adding to the complexity, cost, and danger of performing such synthesis. The disclosed methods surprisingly allow for control of the carbon content in lithium transition metal phosphate cathode materials in a conductive carbon matrix down to a range as low as 1-10% by weight, provide LFP active material utilization in the range of 85-90% (suitable for commercial products), and are scalable and inexpensive. Furthermore, in some embodiments, the methods disclosed herein provide lithium transition metal phosphates with improved tap density compared to conventional lithium transition metal phosphates, thereby improving the commercial viability of such materials in battery packs. The disclosed methods, and materials prepared thereby, have additional advantages, as further described herein below.

[0010] The methods disclosed herein generally include combining a group of precursors for synthesizing a lithium transition metal phosphate cathode material, providing one or more carbon precursors in a fluid state, mixing the group of precursors with one or more carbon precursors to form a precursor mixture, adding a gelation initiator to the precursor mixture, allowing the one or more carbon precursors to undergo gelation to form a solid organogel, and pyrolyzing the solid organogel to form the lithium transition metal phosphate cathode material in a conductive carbon matrix. The one or more carbon precursors are configured to form a solid organogel in the presence of the gelation initiator, and the solid organogel is configured to form a conductive carbon matrix upon pyrolysis. It is understood that the solid organogel produced by the disclosed methods is formed by gelation of the carbon precursors, and pyrolysis of the organogel produces a conductive carbon matrix. It is also understood that throughout this disclosure, in the context of the described methods, the terms "solid organogel" and "organogel" are intended to be interpreted to further include precursors for synthesizing lithium transition metal phosphate cathode materials and / or intermediate reaction products of these various precursors, unless the context makes clear otherwise that only organogel is described. In the disclosed methods, at least a first precursor of the group of precursors for synthesizing lithium transition metal phosphate cathode materials comprises a solid phase having a first density greater than 1 gram (g) / cubic centimeter (cc), and at least a second precursor of the group comprises a liquid phase having a second density, the second density being less than the first density. The solid organogel prevents the solid phase components of the group of precursors from separating (e.g., settling due to a density gradient between the solid and liquid phases) from the liquid phase components of the group of precursors. In particular, the solid organogel maintains uniform contact of the lithium transition metal phosphate groups of the precursors within the mixture so that the precursors can react to form lithium transition metal phosphate cathode materials (e.g., lithium iron phosphate (LFP)). Furthermore, the solid organogel can also contribute to the synthesis of commercially viable LFPs by converting them into the conductive carbon matrix necessary for their use as cathode materials.

[0011] As discussed above, the methods disclosed herein are advantageous in maintaining uniform contact between various precursor materials, e.g., the Fe precursor and lithium phosphate. Importantly, the solid organogel materials utilized in the methods are selected to maintain a solid state up to fairly high temperatures (e.g., up to at least about 300° C.), such that the solid organogel is capable of dissolving LiH 2 PO 4 Above the melting temperature of 2 PO 4 ) to maintain contact with LiH 2 PO 4 The organogel precursors are capable of reacting to LFP and not phase separating, even when melted into a liquid phase at the LFP synthesis reaction temperature. Because the organogel precursors and conditions are selected to allow for rapid gelation (e.g., less than 15 minutes, such as from a few seconds to about 15 minutes), the advantages of solid organogels with respect to maintaining contact between the precursors are quickly realized. Furthermore, in some embodiments, the method provides more intimate mixing and interaction of the precursor materials on a smaller scale (e.g., nano-sized solvated molecular scale) compared to methods that mix the components as solid-phase (e.g., micron-sized) particles. This more intimate mixing can mitigate the formation of impurities during synthesis and provide a more homogenous product. Surprisingly, such intimate mixing can achieve a reduction or even elimination of the costly grinding required in previously reported processes. Another advantage of the disclosed method is that gelation of the organogel precursor in the presence of a lithium transition metal phosphate precursor allows for the production of a cathode material that is intimately mixed with carbon within a continuous three-dimensional conductive carbon matrix after pyrolysis.

[0012] Thus, in one aspect, there is provided a method for preparing a lithium transition metal phosphate cathode material in a conductive carbon matrix, the method comprising: combining a group of precursors for synthesizing a lithium transition metal phosphate cathode material, wherein at least a first precursor of the group includes a solid phase having a first density greater than 1 gram (g) / cubic centimeter (cc) and at least a second precursor of the group includes a liquid phase having a second density, the second density being less than the first density; providing one or more carbon precursors in a fluid state, the one or more carbon precursors configured to form a solid organogel in the presence of a gelation initiator, the solid organogel configured to form a conductive carbon matrix upon pyrolysis; mixing a group of precursors with one or more carbon precursors to form a precursor mixture; adding a gelation initiator to the precursor mixture; allowing one or more carbon precursors to undergo gelation to form a solid organogel; and pyrolyzing the solid organogel to form a lithium transition metal phosphate cathode material within a conductive carbon matrix.

[0013] In some embodiments, a solid organogel forms within 5 seconds to 15 minutes after addition of the gelation initiator.

[0014] In some embodiments, the solid organogel comprises a porous network of interconnected solid polymeric structures.

[0015] In some embodiments, the porous network maintains contact between a first precursor of the group and a second precursor of the group.

[0016] In some embodiments, the contact is maintained at a temperature of at least about 300°C.

[0017] In some embodiments, the first precursor comprises iron, the second precursor comprises a lithium source and a phosphoric acid, and the lithium transition metal phosphate cathode material is lithium iron phosphate.

[0018] In some embodiments, the iron is provided as an iron(II) salt, an iron(III) salt, iron(II) oxide (FeO), iron(III) oxide (Fe 2 O 3 ), mixed iron oxide (Fe 3 O 4 ), or a combination thereof.

[0019] In some embodiments, the solid organogel comprises a phloroglucinol-furfural polymer or a resorcinol-furfural polymer, and the one or more carbon precursors are phloroglucinol or resorcinol and furfural. In some embodiments, the gelation initiator is an amine base or an acid.

[0020] In some embodiments, the solid organogel comprises a polyurethane polymer and the one or more carbon precursors comprise a polyol and an isocyanate. In some embodiments, the gelation initiator comprises an alkylamine.

[0021] In some embodiments, the organogel comprises a polyamic acid polymer and the gelation initiator comprises acetic anhydride, acetic acid, or a combination thereof.

[0022] In some embodiments, the group of precursors includes a microwave-sensitive precursor, and the pyrolyzing is performed by applying microwave radiation. In some embodiments, the microwave-sensitive precursor includes one or more of carbon, magnetite, and maghemite. In some embodiments, the microwave-sensitive precursor includes nanoparticles of one or more of magnetite and maghemite having a characteristic dimension of 20 nm to 100 nm.

[0023] In some embodiments, the first precursor comprises manganese, vanadium, or both, the second precursor comprises a lithium source and a phosphoric acid, and the lithium transition metal phosphate cathode material is a lithium manganese phosphate or a lithium vanadium phosphate.

[0024] In some embodiments, the method further comprises drying the lithium transition metal phosphate cathode material by applying microwave radiation.

[0025] In some embodiments, the solid phase having a first density greater than 1 gram comprises a ferromagnetic iron compound, a ferrimagnetic iron compound, or both.

[0026] In some embodiments, the ferromagnetic iron compound, ferrimagnetic iron compound, or both, are synthesized by a method comprising oxidizing an iron-containing anode in an electrochemical cell comprising a porous carbon substrate, an oxygen cathode, and an electrolyte in contact with both the iron-containing anode and the porous carbon substrate, wherein the oxidation produces particles of the ferromagnetic iron compound, ferrimagnetic iron compound, or both, having a characteristic dimension between 20 nm and 100 nm.

[0027] In some embodiments, the method further comprises removing particles by magnetic filtration.

[0028] In some embodiments, the method further comprises drying the particles by applying microwave radiation.

[0029] In some embodiments, operation of the electrochemical cell and formation of the ferromagnetic iron compound, the ferrimagnetic iron compound, or both, is carried out at a temperature between 15°C and 35°C.

[0030] In another aspect, there is provided a lithium transition metal phosphate cathode material prepared by the methods disclosed herein.

[0031] In yet another aspect, an energy storage system is provided that includes the lithium transition metal phosphate cathode material prepared by the methods disclosed herein.

[0032] In yet a further aspect, a composition is provided comprising nanoparticles comprising olivine-type lithium iron phosphate and integral with a conductive carbon matrix, the nanoparticles having a characteristic dimension of between 20 nm and 1000 nm and a characteristic dimension of between 10 meters. 2(m 2 ) / gram(g)~65m 2 In some embodiments, the characteristic dimension is between 30 nm and 70 nm and the specific surface area is between 20 m 2 / g~65m 2 In some embodiments, the characteristic dimension is between 30 nm and 60 nm and the specific surface area is between 22 m 2 / g~40m 2 In some embodiments, the characteristic dimension is between 20 nm and 40 nm and the specific surface area is between 60 m 2 / g~80m 2 / g.

[0033] In some embodiments, the nanoparticles further comprise magnetite, maghemite, or both.

[0034] In some embodiments, the nanoparticles further comprise manganese.

[0035] In some embodiments, the conductive carbon matrix comprises a carbonized organogel polymer matrix.

[0036] In yet another aspect, an energy storage system is provided comprising the composition disclosed herein.

[0037] The present disclosure includes, but is not limited to, the following aspects.

[0038] Aspect 1: A method for preparing a lithium transition metal phosphate cathode material in a conductive carbon matrix, the method comprising: combining a group of precursors for synthesizing the lithium transition metal phosphate cathode material, wherein at least a first precursor of the group includes a solid phase having a first density greater than 1 gram (g) / cubic centimeter (cc) and at least a second precursor of the group includes a liquid phase having a second density, the second density being less than the first density; providing one or more carbon precursors in a fluid state, the one or more carbon precursors configured to form a solid organogel in the presence of a gelation initiator, the solid organogel configured to form a conductive carbon matrix upon pyrolysis; mixing the group of precursors with the one or more carbon precursors to form a precursor mixture; adding said gelation initiator to said precursor mixture; allowing the one or more carbon precursors to undergo gelation to form the solid organogel; and pyrolyzing the solid organogel to form the lithium transition metal phosphate cathode material within the conductive carbon matrix.

[0039] Aspect 2: The method of aspect 1, wherein the solid organogel is formed within 5 seconds to 15 minutes after addition of the gelation initiator.

[0040] Example 3: The method of example 1 or example 2, wherein the solid organogel comprises a porous network of interconnected solid-phase polymeric structures.

[0041] Example 4: The method of any one of Examples 1 to 3, wherein the porous network maintains contact between the first precursor of the group and the second precursor of the group.

[0042] Embodiment 5: The method of any one of embodiments 1 to 4, wherein the contacting is maintained at a temperature of at least about 300° C.

[0043] Aspect 6: The method of any one of aspects 1-5, wherein the first precursor comprises iron, the second precursor comprises a lithium source and phosphoric acid, and the lithium transition metal phosphate cathode material is lithium iron phosphate.

[0044] Aspect 7: The method of any one of aspects 1-6, wherein the first precursor comprises iron, the second precursor comprises a lithium source and phosphoric acid, and the lithium transition metal phosphate cathode material is lithium iron phosphate.

[0045] Aspect 8: The iron is an iron(II) salt, an iron(III) salt, iron(II) oxide (FeO), iron(III) oxide (Fe 2 O 3 ), mixed iron oxide (Fe 3 O 4 8. The method according to any one of the preceding claims, wherein the compound is present in the form of:

[0046] Aspect 9: The method of any one of aspects 1 to 8, wherein the solid organogel comprises phloroglucinol-furfural polymer or resorcinol-furfural polymer and the one or more carbon precursors are phloroglucinol or resorcinol and furfural.

[0047] Aspect 10: The method of aspect 9, wherein the gelation initiator is an amine base or an acid.

[0048] Example 11: The method of any one of Examples 1 to 8, wherein the solid organogel comprises a polyurethane polymer and the one or more carbon precursors comprise a polyol and an isocyanate.

[0049] Aspect 12: The method of aspect 11, wherein the gelation initiator comprises an alkylamine.

[0050] Example 13: The method of any one of Examples 1 to 8, wherein the organogel comprises a polyamic acid polymer and the gelation initiator comprises acetic anhydride, acetic acid, or a combination thereof.

[0051] Example 14: The method of any one of Examples 1 to 13, wherein the group of precursors comprises a microwave-sensitive precursor and the pyrolyzing is carried out by applying microwave radiation.

[0052] Example 15: The method of example 14, wherein the microwave-sensitive precursor comprises one or more of carbon, magnetite, and maghemite.

[0053] Example 16: The method of example 14, wherein the microwave-sensitive precursor comprises nanoparticles of one or more of magnetite and maghemite having a characteristic dimension between 20 nm and 100 nm.

[0054] Aspect 17: The method of any one of the preceding aspects, wherein the first precursor comprises manganese, vanadium, or both, the second precursor comprises a lithium source and a phosphoric acid, and the lithium transition metal phosphate cathode material is a lithium manganese phosphate or a lithium vanadium phosphate.

[0055] Example 18: The method of any one of the preceding examples, wherein the method further comprises drying the lithium transition metal phosphate cathode material by applying microwave radiation.

[0056] Embodiment 19: The method of any one of the preceding embodiments, wherein the solid phase having the first density greater than 1 gram comprises a ferromagnetic iron compound, a ferrimagnetic iron compound, or both.

[0057] Aspect 20: The method of any one of the preceding aspects, wherein the ferromagnetic iron compound, the ferrimagnetic iron compound, or both, are synthesized by a process comprising oxidizing an iron-containing anode in an electrochemical cell comprising a porous carbon substrate, an oxygen cathode, and an electrolyte in contact with both the iron-containing anode and the porous carbon substrate, wherein the oxidizing produces particles of the ferromagnetic iron compound, the ferrimagnetic iron compound, or both, having a characteristic dimension between 20 nm and 100 nm.

[0058] Example 21: The method of example 20, wherein the method further comprises removing the particles by magnetic filtration.

[0059] Embodiment 22: The method of any one of the preceding embodiments, wherein the method further comprises drying the particles by applying microwave radiation.

[0060] Aspect 23: The method of aspect 20, wherein the operation of the electrochemical cell and the formation of the ferromagnetic iron compound, the ferromagnetic iron compound, or both, is performed at a temperature between 15°C and 35°C.

[0061] Embodiment 24: A lithium transition metal phosphate cathode material prepared by the methods disclosed herein.

[0062] Embodiment 25: An energy storage system comprising a lithium transition metal phosphate cathode material prepared by the methods disclosed herein.

[0063] Aspect 26. A composition comprising nanoparticles comprising olivine-type lithium iron phosphate and integral with a conductive carbon matrix, the nanoparticles having a characteristic dimension of between 20 nm and 1000 nm and a characteristic dimension of between 10 meters and 10 meters. 2 (m 2 ) / gram(g)~65m 2 The composition has a specific surface area of ​​100 / g.

[0064] Aspect 27: The characteristic dimension is 30 nm to 70 nm, and the specific surface area is 20 m 2 / g~65m 2 / g.

[0065] Aspect 28: The characteristic dimension is 30 nm to 60 nm, and the specific surface area is 22 m 2 / g~40m 2 / g.

[0066] Aspect 29: The characteristic dimension is between 20 nm and 40 nm, and the specific surface area is between 60 m 2 / g~80m 2 / g.

[0067] Aspect 30: The composition of any one of aspects 26-29, wherein the nanoparticles further comprise magnetite, maghemite, or both.

[0068] Aspect 31: The composition of any one of aspects 26 to 30, wherein the nanoparticles further comprise manganese.

[0069] Example 32: The composition of any one of Examples 26-31, wherein the conductive carbon matrix comprises a carbonized organogel polymer matrix.

[0070] Embodiment 33: An energy storage system comprising the composition disclosed herein.

[0071] These and other features, aspects, and advantages of the present disclosure will become apparent from a reading of the following detailed description in conjunction with the accompanying drawings, which are briefly described below. The present invention includes any combination of two, three, four, or more of the above-described aspects, as well as any combination of two, three, four, or more features or elements described in the present disclosure, whether or not such features or elements are expressly combined in the description of a particular embodiment herein. The present disclosure is intended to be read in its entirety, such that any separable features or elements of the disclosed invention, in any of its various embodiments, should be considered as intended to be combinable, unless the context clearly indicates otherwise.

[0072] To provide an understanding of aspects of the technology, reference is made to the accompanying drawings, which are not necessarily drawn to scale. The drawings are merely illustrative and should not be construed as limiting the technology. The disclosure described herein is illustrated by way of example, and not by way of limitation, in the accompanying drawings. [Brief description of the drawings]

[0073] [Figure 1] FIG. 1 is a schematic diagram of a conventional solid-state synthetic route to lithium iron phosphate in a carbon matrix. [Diagram 2] FIG. 2 is a schematic diagram of a slurry / sol-gel synthesis route to lithium iron phosphate in a carbon matrix, according to a non-limiting embodiment of the present disclosure. [Diagram 3] FIG. 3 illustrates a schematic of a system for oxidizing transition metals, including but not limited to, iron, using a carbon aerogel component, according to a non-limiting embodiment. [Figure 4] FIG. 4 illustrates a schematic of an electrochemical cell for oxidizing transition metals, including but not limited to, iron, using a carbon aerogel component, according to a non-limiting embodiment. [Figure 5A] FIG. 5A is a scanning electron micrograph at 100,000x magnification of a sample of nanoparticulate magnetite (Fe3O4) prepared by forced air anodization of iron, according to a non-limiting embodiment of the present disclosure. [Figure 5B] FIG. 5B is a powder X-ray diffraction (XRD) pattern of a sample of nanoparticulate magnetite prepared by forced air anodization of iron, according to a non-limiting embodiment of the present disclosure. [Figure 6] FIG. 6 is a schematic diagram of a semi-continuous method for preparing nanoparticulate magnetite from forced air anodic oxidation of iron and converting it to lithium iron phosphate within a carbon matrix, according to a non-limiting embodiment of the present disclosure. [Figure 7] 7A and 7B are scanning electron micrographs at two magnifications (1,490x and 5,050x, respectively) of a sample of lithium iron phosphate in a carbon matrix prepared according to a non-limiting embodiment of the present disclosure. [Figure 8] FIG. 8 is a powder X-ray diffraction (XRD) pattern of a sample of lithium iron phosphate in a carbon matrix prepared according to a non-limiting embodiment of the present disclosure. [Figure 9] 9A and 9B are scanning electron micrographs at two magnifications (10,000x and 49,900x, respectively) of a sample of lithium iron phosphate in a carbon matrix prepared according to a non-limiting embodiment of the present disclosure. [Figure 10]FIG. 10 is a powder XRD pattern of a sample of lithium iron phosphate in a carbon matrix prepared according to a non-limiting embodiment of the present disclosure. [Figure 11] 11A and 11B are scanning electron micrographs at two magnifications (10,000x and 100,000x, respectively) of a sample of lithium iron phosphate in a carbon matrix prepared according to a non-limiting embodiment of the present disclosure. [Figure 12] FIG. 12 is a powder XRD pattern of a sample of lithium iron phosphate in a carbon matrix prepared according to a non-limiting embodiment of the present disclosure. [Figure 13] 13A and 13B are scanning electron micrographs at two magnifications (2,000x and 20,000x, respectively) of a sample of lithium iron phosphate in a carbon matrix prepared according to a non-limiting embodiment of the present disclosure. [Figure 14] FIG. 14 is a powder XRD pattern of a sample of lithium iron phosphate in a carbon matrix prepared according to a non-limiting embodiment of the present disclosure. [Figure 15] 15A and 15B are scanning electron micrographs at two magnifications (2,000x and 50,000x, respectively) of a sample of lithium iron phosphate in a carbon matrix prepared according to a non-limiting embodiment of the present disclosure. [Figure 16] FIG. 16 is a powder XRD pattern of a sample of lithium iron phosphate in a carbon matrix prepared according to a non-limiting embodiment of the present disclosure. [Figure 17] FIG. 17 is a powder XRD pattern of a sample of lithium iron phosphate in a carbon matrix prepared according to a non-limiting embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0074] Before describing some example aspects of the present technology, it is to be understood that the technology is not limited to the details of construction or process steps set forth in the following description as the technology is capable of other aspects and of being practiced or carried out in various ways.

[0075] In general, the present technology is directed to a method for preparing a lithium transition metal phosphate cathode material within a conductive carbon matrix. In accordance with the present disclosure, it has surprisingly been found that the lithium transition metal phosphate cathode material prepared as disclosed herein provides a more homogeneous product without the need for a costly grinding step, and also provides a cathode material with improved tap density compared to conventional methods for preparing lithium transition metal phosphate. Furthermore, the disclosed method provides a lithium transition metal phosphate cathode material that is intimately mixed with carbon within a continuous three-dimensional conductive carbon matrix.

[0076] Thus, provided herein are methods for preparing lithium iron phosphate, lithium-transition metal-phosphate, and lithium vanadium fluorophosphate cathode materials in a conductive carbon matrix. As a general, non-limiting description, the disclosed methods generally include combining a group of precursors for synthesizing a lithium transition metal phosphate cathode material, providing one or more carbon precursors in a fluid state, mixing the group of precursors with one or more carbon precursors to form a precursor mixture, adding a gelation initiator to the precursor mixture, allowing the one or more carbon precursors to undergo gelation to form a solid organogel, and pyrolyzing the solid organogel to form a lithium transition metal phosphate cathode material in a conductive carbon matrix. Also provided are lithium transition metal phosphate cathode materials prepared by the disclosed methods, compositions comprising nanoparticles comprising olivine-type lithium iron phosphate and integral with a conductive carbon matrix, and energy storage systems comprising the lithium transition metal phosphate cathode materials or compositions described herein. Each of the components, materials, and products comprising the materials of the methods are further described herein below.

[0077] definition The following definitions are provided for terms used in this disclosure: This application uses the following terms that are defined below, unless the context in which the term appears otherwise requires a different meaning.

[0078] The articles "a" and "an" are used herein to refer to one or to more than one (ie, to at least one) of the grammatical object of the article.

[0079] The term "about" used throughout this specification is used to describe and explain small variations. For example, the term "about" can refer to ±10% or less, or ±5% or less, such as ±2% or less, ±1% or less, ±0.5% or less, ±0.2% or less, ±0.1% or less, or ±0.05% or less. All numerical values ​​herein are modified by the term "about", whether or not explicitly stated. Of course, a value modified by the term "about" includes the specific value. For example, "about 5.0" should include 5.0.

[0080] Any ranges cited herein are inclusive.

[0081] As used herein, the terms "comprise" and "comprising" and variations thereof mean the inclusion of the specified features, steps, or integers. The term is not to be interpreted as excluding the presence of other features, steps, or components. The present invention comprises, consists of, or consists essentially of the disclosed and claimed features.

[0082] In the context of the present disclosure, the term "framework" or "framework structure" refers to a network of interconnected oligomeric, polymeric, or colloidal particles that form the solid structure of a gel or xerogel. The polymers or particles (e.g., carbon) that make up the framework structure typically have a diameter of about 100 angstroms. However, the framework structure of the present disclosure can also include a network of interconnected oligomeric, polymeric, or colloidal particles of all diameter sizes that form the solid structure within a gel or xerogel.

[0083] In some embodiments, the gel material may be specifically referred to herein as a xerogel. As used herein, the term "xerogel" refers to a type of gel that contains an open, non-fluid colloidal or polymeric network that is formed by removing all swelling agents from a corresponding wet gel without taking precautions to avoid substantial volume loss or retard compaction. Xerogels are generally composed of compact structures. Xerogels undergo substantial volume loss during ambient pressure drying and generally have a volumetric density of about 0 to about 20 m, as measured by nitrogen adsorption analysis. 2 / g, etc. 0 to 100m 2 / g surface area.

[0084] As used herein, the term "gelation" or "gel transition" refers to the formation of a wet gel from a polymer system, such as the PF or polyimide described herein. At the point of polymerization, imidization, or drying described herein, defined as the "gel point", the sol loses flowability. Without intending to be bound by any particular theory, the gel point can be considered as the point at which the gelling solution exhibits resistance to flow. In the present context, gelation proceeds from an initial sol state (e.g., a liquid solution of an ammonium salt of a polyamic acid) through a highly viscous dispersion state, until the dispersion solidifies and the sol-gel (gel point) results in a wet gel (e.g., a polyimide gel). Such a time taken for a polymer in solution to transform into a form of gel that can no longer flow is referred to as the "phenomenal gelation time". Formally, gelation time is measured using rheology. At the gel point, the elastic properties of the solid gel begin to exceed the viscous properties of the fluid sol. The formal gel time is approximated as the time at which the complex moduli of the real and imaginary components of the gelling sol intersect. The two moduli are monitored as a function of time using a rheometer. Time is measured starting from the moment the last component of the sol is added to the solution. See, for example, the discussion of gelation in H.H. Winter, "Can the Gel Point of a Cross-linking Polymer Be Detected by the G'-G' Crossover?" Polym. Eng. Sci., 1987, 27, 1698-1702, S.-Y. Kim, D.-G. Choi and S.-M. Yang, "Rheological analysis of the gelation behavior of tetraethylorthosilane / vinyltriethoxysilane hybrid solutions," Korean J. Chem. Eng., 2002, 19, 190-196, and M. Muthukumar, "Screening effect on viscoelasticity near the gel point," Macromolecules, 1989, 22, 4656-4658.In some embodiments, gelation is induced by the addition of a suitable gelation initiator. In other embodiments, gelation may be induced, for example, by removal of the solvent from a solution containing the salt of the polyamic acid. Such solvent removal may be accomplished by a variety of drying techniques, including, but not limited to, spray drying.

[0085] As used herein, the term "wet gel" refers to a gel in which the mobile interstitial phase within a network of interconnected pores is composed primarily of a liquid phase, such as a conventional solvent or water. Examples of wet gels include, but are not limited to, alcogels, hydrogels, ketogels, carbon gels, and other wet gels known to those skilled in the art.

[0086] The term "carbon xerogel" as used herein refers to a porous carbon-based material. Some non-limiting examples of carbon xerogels include carbonized xerogels, such as carbonized polyimide gels. The term "carbonization" in the context of xerogels refers to an organogel (e.g., PF polymer or polyimide) that has been subjected to pyrolysis to decompose or convert the organogel composition to at least substantially pure carbon. As used herein, the terms "pyrolyze" or "pyrolysis", or "carbonization" refer to the heat-induced decomposition or conversion of an organic matrix to pure or substantially pure carbon. During such pyrolysis, as described herein below, reaction of various components present within the matrix occurs, simultaneously or subsequently forming the respective lithium transition metal phosphate or fluorophosphate cathode material within the carbon matrix.

[0087] As used herein, the term "average particle size" refers to a 50"means that half of the population of particles has a particle size above this point and half has a particle size below this point. Particle size can be measured by laser light scattering techniques or by microscopy techniques. Unless otherwise indicated, the average particle size reported herein is obtained by visual interpretation of SEM images using a calibrated scale bar and image processing software (such as ImageJ). Multiple particles are measured randomly, the results are averaged, and the standard deviation is calculated. For secondary particles and aggregates, laser diffraction particle size analysis is used.

[0088] In the context of this disclosure, the term "density" refers to a measure of the mass per unit volume of a material. The term "density" generally refers to the true or He true density of a material, the bulk density of a material or composition, or the tapped density of a material or composition. Density is typically expressed in kg / m 3 or g / cm 3 It is reported as:

[0089] The He true density of a material is the ratio of the mass of the material to the volume of the material, excluding pores within the material and voids between the particles of the material. He true density can be determined by methods known in the art, including but not limited to helium pycnometry.

[0090] The bulk density of a material is the ratio of the mass of the material to the volume of the material, including pores within the material and voids between the particles of the material. Bulk density, also referred to as "envelope density", may be determined by methods known in the art, including, but not limited to, Standard Test Method for Dimensions and Density of Preformed Block and Board-Type Thermal Insulation (ASTM C303, ASTM International, West Conshohocken, Pa.), Standard Test Methods for Thickness and Density of Blanket or Batt Thermal Insulations (ASTM C167, ASTM International, West Conshohocken, Pa.), or Determination of the apparent density of preformed pipe insulation (ISO 18098, International Organization for Standardization, Switzerland). In the context of this disclosure, unless otherwise stated, density measurements are taken according to the ASTM C167 standard.

[0091] In the context of this disclosure, the term "tap density" or "tapped density" of a material is the ratio of the mass of the material to the volume of the material measured when the material is vibrated or tapped under specified conditions. The tap density of a powder describes its random dense packing. Tap density values ​​are higher for more regularly shaped particles (e.g., spheres) compared to irregularly shaped particles. Tap density is defined as: where M=mass in grams and V f = cubic centimeters (cm 3 ) is the tapped volume in the equation M / V fThe tap density can be calculated using the formula: Tap density is generally measured by first gently introducing a known sample mass into a graduated cylinder and carefully leveling it without compressing the powder. The cylinder is then mechanically tapped by raising it and allowing it to fall under its own weight using a suitable mechanical tap density tester that provides a suitable fixed drop distance and nominal drop speed. Standard test methods for tap density measurement are described in MPIF-46, ASTM B-52722, and ISO3953. Unless otherwise indicated, the tap density of the materials described herein is obtained by the method of ASTM B-52722.

[0092] As used herein, the term "positive electrode" is used interchangeably with the term "cathode." Similarly, the term "negative electrode" is used interchangeably with the term "anode."

[0093] In the context of this disclosure, the term "electrical conductivity" refers to a measurement of a material's ability to conduct electric current or otherwise allow the flow of electrons through or within it. Electrical conductivity is specifically measured as the electrical conductance / susceptance / admittance of a material per unit size of the material. It is typically recorded as S / m (Siemens / meter) or S / cm (Siemens / centimeter). The electrical conductivity or resistivity of a material can be determined by methods known in the art, including, for example, but not limited to, in-line 4-point resistivity (using the dual configuration test method of ASTM F84-99). In the context of this disclosure, electrical conductivity measurements are obtained according to the ASTM F84-Resistivity (R) measurement, which is obtained by measuring the voltage (V) divided by the current (I), unless otherwise stated. In certain embodiments, the materials of the present disclosure have an electrical conductivity of about 10 S / cm or more, 20 S / cm or more, 30 S / cm or more, 40 S / cm or more, 50 S / cm or more, 60 S / cm or more, 70 S / cm or more, 80 S / cm or more, or in a range between any two of these values.

[0094] The term "substantially," as used herein, unless otherwise indicated, means, e.g., greater than about 95%, greater than about 99%, greater than about 99.9%, greater than 99.99%, or even as high as 100% of the referenced characteristic, amount, etc., relative to the particular context (e.g., substantially pure, substantially the same, etc.).

[0095] I. Method for preparing lithium transition metal phosphate cathode materials within a conductive carbon matrix In one aspect, a method for preparing a lithium transition metal phosphate cathode material within a conductive carbon matrix is ​​provided. As described herein above, many previously reported synthesis processes for preparing lithium transition metal phosphate cathode materials, such as lithium iron phosphate (LFP), involve extensive mechanical mixing of solid-phase precursor materials (e.g., via ball milling) to achieve the intimate contact between precursors necessary to provide a homogenous product. Furthermore, such solid-phase schemes utilize multiple energy-intensive steps. For example, FIG. 1 provides a schematic diagram of a typical solid-phase process method 100. With reference to FIG. 1, drying, mixing, grinding, calcination, and firing all require significant energy input, time, or both, increasing production costs. The energy-intensive steps are indicated by asterisks. In contrast, the methods disclosed herein are advantageous with respect to at least reducing the number of energy- and / or time-intensive steps. For example, FIG. 2 provides a schematic diagram of a process 200 according to a non-limiting embodiment using the slurry / sol-gel synthesis method described herein. Referring to Figure 2, the total number of steps, specifically the number of energy intensive steps, is reduced compared to the scheme of Figure 1. Furthermore, as discussed above, the disclosed method allows for more intimate mixing and interaction of the components on a smaller scale (e.g., nano-sized solvated molecular scale), which can mitigate the formation of impurities during synthesis and provide a more homogenous product. Another advantage of the disclosed method is that the organogel matrix formed during gelation inhibits phase separation of the reaction components, while the gelation of the organogel precursor in the presence of the lithium transition metal phosphate precursor allows for the production of a cathode material that is intimately mixed with carbon within a continuous three-dimensional conductive carbon matrix.

[0096] In another aspect, phase separation of the reaction components may be inhibited during removal of the liquid phase (e.g., water), immiscible solvent, precursor (e.g., aqueous phosphoric acid), or combinations thereof from the various solutions, suspensions, or emulsions disclosed herein. For example, the formation of a self-supporting solid phase comprising the various components during such removal by drying or concentrating the solution, suspension, or emulsion may serve the same purpose as a self-supporting solid-phase organogel formed by gelling a gelling precursor in the presence of a gelling initiator.

[0097] As a general, non-limiting description, the disclosed method generally includes combining a group of precursors for synthesizing a lithium transition metal phosphate cathode material, providing one or more carbon precursors in a fluid state, mixing the group of precursors with the one or more carbon precursors to form a precursor mixture, adding a gelation initiator to the precursor mixture, allowing the one or more carbon precursors to undergo gelation to form a solid organogel, and pyrolyzing the solid organogel to form the lithium transition metal phosphate cathode material within a conductive carbon matrix. Each of the individual components of the method and its preparation operations are further described herein below.

[0098] A. Lithium transition metal phosphate cathode material precursors The disclosed method includes combining a group of precursors for synthesizing a lithium transition metal phosphate cathode material, where at least a second precursor of the group includes a liquid phase having a second density, the second density being less than the first density.

[0099] 1. First Precursor At least a first precursor of the group of precursors comprises a solid phase having a first density greater than 1 gram (g) per cubic centimeter (cc). In some embodiments, the density is in the range of about 1 to about 5, such as about 1, about 2, about 3, about 4, or about 5 g / cc.

[0100] In some embodiments, the group of precursors includes a first precursor that is a transition metal salt or transition metal oxide. As used herein, the terms "transition metal salt" and "transition metal oxide" refer to any salt or oxide of a transition metal and may include a mixture of two or more transition metals. As used herein, the term "transition metal" refers to any metallic element in the d-block of the periodic table, which includes groups 3-12 of the periodic table, excluding the platinum group metals. The transition metal salt or oxide may include various oxidation states of the transition metal. With respect to oxides, these include, but are not limited to, the valence (e.g., 2 + , 3 + , 4 + , or 5 + ), the transition metal or metals present in the salt or oxide are generally in the (II) or (III) oxidation state. Suitable transition metals include, for example, vanadium, titanium, manganese, iron, cobalt, copper, and nickel. Particularly suitable transition metals include one or more of manganese, iron, and vanadium. The selection of a particular transition metal in the form of each salt, oxide, or mixed oxide can be determined by one of skill in the art based on the intended battery cell voltage or other performance parameters, availability, cost, toxicity, and other variables.

[0101] In some embodiments, the first precursor comprises a transition metal oxide. Transition metal oxides suitable for use in the disclosed methods (e.g., Fe 3 O 4 and / or Fe 2 O 3The particle size of the transition metal oxide (such as iron oxide) can vary. In general, small particle sizes, such as about 5 microns or less, are particularly preferred, as such particle sizes allow for intimate contact of the transition metal oxide with other reaction components (e.g., lithium and phosphate ions, as well as organogel precursor materials). In some embodiments, the transition metal oxide has an average particle size of about 5 microns or less, such as in the range of about 1 to about 5 microns. In some embodiments, the transition metal oxide can be synthesized (as described below) to have an average particle size of about 5 nanometers (nm) to about 200 nm, such as in the range of about 20 nm to about 100 nm. Alternatively, a transition metal oxide having an average particle size of about 5 microns or more may be milled to provide the desired particle size range. Such milling may be performed prior to mixing with the other reaction components, or may be performed in situ, as further described herein below.

[0102] The density of the transition metal oxide prior to use in the disclosed methods can vary. Generally, transition metal oxides with high tap densities are particularly preferred. As used herein, the term "high density" refers to a density of about 1.1 g / cm 3 "High tap density" refers to a material having a tap density of greater than about 0.8 to about 1.1 g / cm. Without wishing to be bound by any particular theory, it is believed that the high tap density transition metal oxide acts to template (e.g., via "isomorphous" reactions) the physical properties of the final lithium iron phosphate cathode material, resulting in a desirable high density product. High density cathode materials are considered desirable for battery applications because more power is generated (i.e., greater volumetric energy density is provided) per unit volume of cathode material. Surprisingly, in some embodiments, the disclosed methods provide for the production of high density cathode materials with a tap density of about 0.8 to about 1.1 g / cm. 3 In the range of about 0.8g / cm 3 Thus, the tap densities of the cathode materials of the present disclosure are within the range of commercial viability (i.e., comparable to that of previously available LFPs).

[0103] In some embodiments, the transition metal of the transition metal oxide comprises manganese, vanadium, iron, or a combination thereof, hi some embodiments, the transition metal of the transition metal oxide is manganese or vanadium.

[0104] In some embodiments, the transition metal of the transition metal oxide is manganese. Examples of suitable manganese oxides include, but are not limited to, MnO, MnO 2 , and Mn 2 O 3 In some embodiments, the transition metal oxide is manganese(II) oxide (MnO) or manganese(III) oxide (Mn 2 O 3 ).

[0105] In some embodiments, the transition metal oxide is V 2 O 3 , V.O. 2, , or V 2 O 5 In some embodiments, the transition metal oxide is vanadium oxide and the lithium vanadium phosphate cathode material is Li 3 Sc 2 (PO 4 ) 3 It has the following structural types.

[0106] In some embodiments, the transition metal of the transition metal oxide is iron. The oxidation state of the iron in the iron oxide can vary. For example, the iron oxide can be iron(II) oxide (FeO), iron(III) oxide (Fe 2 O 3 ), or combinations thereof (e.g., Fe 3 O 4 ).

[0107] In certain embodiments, the iron oxide is iron(III) oxide (Fe 2 O 3Iron(III) oxide is an inexpensive and readily available oxide that is stable to oxidation and therefore does not require special handling (e.g., to avoid oxidation, as may be the case with iron(II) oxide). Additionally, iron oxides having an average particle size of about 5 microns or less (e.g., Fe 2 O 3 ) is commercially available. Commercially available bulk Fe 2 O 3 (i.e., Fe with a grain size of greater than about 1 micron 2 O 3 ) can be ground to produce the desired nanoparticulate material, but this is a time-consuming and energy-intensive process. 2 O 3 The nanoparticulate iron(III) oxide, referred to herein as "nanoparticulate iron(III) oxide," may have an average particle size ranging from about 10 nanometers up to about 100 nanometers, such as in the range of about 30 to about 50 nanometers. However, such nanoparticulate iron(III) oxide is very expensive on a commercial scale. Surprisingly, in accordance with the present disclosure, it has been found that the nanoparticulate iron(III) oxide can be produced by the production of inexpensive and readily available iron(II) oxalate (FeC). 2 O 4 It has been found that FeC can be heated in air with the release of carbon dioxide to provide nanoporous iron(III) oxide. For example, it has been found that heating iron oxalate in an air atmosphere to a temperature in the range of about 350 to about 450° C. for a period of about 1 hour converts the iron oxalate to nanoporous iron(III) oxide. In particular, the iron(III) oxide particles produced by thermal decomposition of iron oxalate have an average particle size on the order of a few microns, but develop an internally permeable porosity with pore sizes on the order of 100 nm. Such particles are therefore referred to herein as "nanoporous." In some embodiments, FeC 2 O 4 . 2H 2 Fe obtained by thermal decomposition of O 2 O 3 is about 9.95m 2 / g BET nitrogen surface area.

[0108] In some embodiments, the iron oxide is magnetite (Fe 3 O 4 ) or maghemite (Fe 2 O 3 ), or in the form of a solid solution or mixture of both, with an average composition of Fe 3-x O 4 , (0≦x≦0.33), herein referred to as magnetic iron oxide nanoparticles (magnetic IONPs). Such IONPs can be purchased or prepared according to known methods. In some embodiments, IONPs are prepared by oxidation of iron with air in an electrochemical cell. In accordance with the present disclosure, it has been discovered that certain types of carbon aerogels or other porous carbon structures (e.g., carbonized polyurethane foam, a combination of carbon aerogel within the pores of carbonized polyurethane foam) can act as "air cathodes" to catalytically reduce oxygen at room temperature. When placed in an electrochemical cell with an aqueous electrolyte, oxygen can be reduced to hydroxide anions while oxidizing transition metals such as iron. In some embodiments, iron can be oxidized to produce iron hydroxide, magnetite, maghemite, or combinations thereof. The catalytic effect of the carbon aerogels described herein can be used to oxidize solid-state iron at room temperature (e.g., 5° C. to 25° C.).

[0109] 3 is a schematic diagram of a system 300 used to oxidize iron at room temperature according to one or more embodiments described herein. System 300 includes a porous conductive carbon element 304, a separator 308, an electrolyte 312, an iron-containing electrode 316, and a conductor 320. Without wishing to be bound by theory, it is believed that the carbon aerogel element 304 can reduce the activation energy for the reduction of oxygen, thereby allowing the electrically connected iron electrode to participate in the room temperature redox reaction.

[0110] In various embodiments, the porous conductive carbon element 304 (equivalently referred to as the "substrate") can be synthesized and / or produced according to techniques including pyrolysis of a polyimide aerogel. In some examples, the pyrolyzed polyimide aerogel can contain residual nitrogen or other heteroatoms (i.e., non-carbon atoms) that are not removed during synthesis or pyrolysis of the aerogel. By using the porous conductive carbon element 304 as a catalyst to oxidize the iron electrode 316, it is possible to obtain, without limitation, Fe(OH) 2 , Fe(OH) 3 , Fe 3 O 4 , and Fe 2 O 3 The process described herein can produce solid state iron oxide / hydroxide using air, water, and iron metal as the only reactants without producing significant amounts of waste water.

[0111] Although many of the embodiments described herein describe the use of carbon aerogel elements in electrochemical cells, the embodiments herein are not limited to those that include carbon aerogels. More generally, the porous conductive carbon element 304 can be any of a variety of porous carbon substrates that can act as an air cathode. Carbon aerogel materials (e.g., polyimide-derived carbon aerogels) are believed to support high oxidation rates of transition metals such as iron at room temperature, although other porous carbons may have the same effect under appropriate experimental conditions. Additional examples of porous carbon substrates that can be used in place of or in addition to carbon aerogel substrates include, but are not limited to, porous graphitic carbon substrates, carbon substrates made from carbon nanotubes, carbonized polymer foams (e.g., carbonized polyurethane foams), carbon fullerenes, graphene, graphene oxide, and / or activated carbon. In some examples, the specific surface area of ​​these substrates is at least 100 m 2 For example, the porous conductive carbon elements 304 of the present disclosure can have a specific surface area in the range of the non-pyrolyzed aerogel precursor (e.g., 100 m 2 / g~600m2 / g) The porous conductive carbon element 304 can be a carbon aerogel in monolithic form, particulate form, or a combination thereof.

[0112] In certain embodiments, a porous conductive carbon material or composition of the present disclosure has an electrical conductivity of about 1 Siemens (S) / centimeter (cm) or greater, about 5 S / cm or greater, about 10 S / cm or greater, 20 S / cm or greater, 30 S / cm or greater, 40 S / cm or greater, 50 S / cm or greater, 60 S / cm or greater, 70 S / cm or greater, 80 S / cm or greater, or in a range between any two of these values.

[0113] In some examples, the rate of the redox reaction (more specifically, the oxidation of iron metal) can be selected (e.g., increased or decreased compared to a reference reaction rate) by modifying one or more conditions under which the reaction is carried out. In some examples, the reaction rate can be increased by one or more of increasing the temperature at which the reaction is carried out, increasing the partial pressure of oxygen (thereby increasing the rate of hydroxy anion production), increasing the concentration of the electrolyte (e.g., from a 1 molar (M) solution to a multi-molar solution), and / or increasing the magnitude of the potential difference applied to the carbon aerogel / transition metal system 300. Similarly, the reaction rate can be decreased by limiting any of the aforementioned parameters. Also, the reaction rate, as well as the composition and morphology of the reaction product(s), can be affected by changing the pH of the electrolyte or the composition of the electrolyte. In addition, decreasing the concentration of the electrolyte (e.g., from 1 M to 0.2 M) and / or changing the electrolyte cation (e.g., Na + From K + It has been unexpectedly discovered that by modifying the cation exchange ratio (C) of the nanoparticles, the average diameter of the nanoparticles can be reduced from approximately 100 nm to as low as 5-20 nm. These nanoparticles can then be favorably reacted to form similarly sized lithium metal phosphate cathode materials with very high surface areas (as listed in Table 1 below).

[0114] In some instances, the reaction products can be influenced by excluding gases other than oxygen. For example, the presence of carbonate species in the reaction products can be reduced by using a mixture of gases that excludes pure oxygen or carbon dioxide. This in turn can reduce and / or eliminate the presence of undesirable reaction products (e.g., carbonates) in the iron oxide metal compounds.

[0115] The separator 308 is an electrically insulating material that provides a structure through which ions can travel. This combination prevents electrical shorting of the system 300 while allowing current flow via ion migration between the porous conductive carbon element 304 and the ferrous metal electrode 316. Examples of separator 308 can include cellulosic paper, fibrous polymer fabric, or felt, among others.

[0116] An electrolyte 312 disposed within the separator 308 facilitates ion transfer from the porous conductive carbon element 304 to the iron metal electrode 316. Examples of electrolytes include sodium chloride (NaCl), among others. (水溶液) ), ammonium chloride (NH 3 Cl (水溶液) )), sodium carbonate (NaCO 3(水溶液) ), and aqueous solutions of potassium chloride (KCl) (e.g., distilled water, deionized water, distilled deionized water, tap water). In some examples, the concentration of the electrolyte may be saturated with the solute. In other examples, the concentration of the electrolyte may be less than a saturated solution. In some examples, the concentration of the electrolyte may be selected according to various criteria, including, but not limited to, the desired reaction rate at the iron metal anode (higher concentrations generally accelerate the rate of oxidation), the morphology and / or composition of the oxide reaction product at the iron metal anode, among others.

[0117] Without wishing to be bound by theory, it has been observed that the presence of chloride in the electrolyte promotes the dissociation of the hydroxylated reaction products from the surface of the iron metal electrode 316. Thus, when using a chloride-containing electrolyte, as the reaction proceeds, fresh surfaces of the iron metal electrode 316 are naturally exposed, and the process can naturally convert the entire mass of the iron metal electrode 316 into the reaction products.

[0118] The iron metal electrode 316 may be an iron metal piece in electrical and ionic communication with the porous conductive carbon element 304, as illustrated in Figure 3. In some examples, the iron metal electrode 316 may include compositional components added to improve electrical conductivity, improve the oxidation reaction rate, or both.

[0119] The conductor 320 can be an electrical conductor, such as copper wire, aluminum wire, gold wire, and alloys thereof, that connects the carbon aerogel element 304 and the transition metal electrode 316. In some examples, the conductor 320 can also be used to apply an electrical potential to the system 300 that initiates and maintains the oxidation reaction at the iron metal electrode 316.

[0120] In some examples, the minimum applied potential applied from an external source through the conductor 320 varies depending on the iron metal selected for the iron electrode 316. The minimum applied potential required to promote an oxidation reaction at the iron metal oxide 316 may be an indication of the catalytic activity of the carbon catalyst used to reduce oxygen (e.g., to produce hydroxy anions) to the iron metal electrode 316. The maximum potential may be selected to avoid electrolysis (electrically induced decomposition) of the electrolyte.

[0121] 4 is a schematic diagram of an electrochemical cell 400 according to one embodiment of the disclosure. Electrochemical cell 400 is an alternative representation of some embodiments of system 300. Electrochemical cell 400 includes an electrode 404, an iron metal component 408, a conductor 412, a porous conductive carbon element 416, an oxidation reaction product layer 420, and an electrolyte 424.

[0122] Many of the elements shown in the electrochemical cell 400 of Figure 4 are homogenous to those described above in the context of the system 300 shown in Figure 3. The electrode 404 can be an electrical contact with which the iron metal component 408 (homogeneous with the iron metal electrode 316) is in electrical communication. The conductor 412 is homogenous to the conductor 320. The porous conductive carbon element 416 is homogenous to the porous conductive carbon element 304.

[0123] In addition to the elements already described in the context of Figure 3, Figure 4 illustrates diagrammatically the redox reaction that occurs within electrochemical cell 400 upon application of an external voltage having a magnitude of 1 volt (V). The magnitude of the minimum value of the applied voltage required to promote the oxidation reaction (the "onset voltage") may be determined by the particular transition metal (i.e., iron) of component 408 and the catalytic efficiency of the porous conductive carbon element 416. In some instances, oxidation of iron metal within electrochemical cell 400 may not occur at applied voltages having a magnitude below the minimum value.

[0124] In particular, Figure 4 illustrates generally the exposure of a porous conductive carbon element 416 to oxygen. In some examples, the oxygen may be gaseous, such as from air or a commercial gas mixture having a concentration of oxygen higher than that found in air. The oxygen may enter the porous conductive carbon element 416 pre-wetted with electrolyte 424. Upon encountering the porous conductive carbon element 416 that also contains and / or is coated with electrolyte 424, the oxygen may eventually be converted to hydroxy anions solvated by the electrolyte 424.

[0125] The hydroxy anions may then react with the iron oxide metal component 408 to form one or more of iron metal oxides, hydroxides, and / or other reaction products 420 resulting from the reaction of iron metal and hydroxy anions. These reaction products are indicated by the shaded regions 420 in FIG. 4. Although the reaction products 420 shown in FIG. 4 are in direct contact with the iron metal component 408, this need not be the case. Different electrolyte compositions as indicated above may result in different physical configurations in the reaction products 420. For example, the presence of chloride in the electrolyte 424 produces reaction products 420 that are separated from the iron metal component 408.

[0126] In some examples, oxygen is the cathode in the electrochemical cell 400. That is, oxygen that encounters the porous conductive carbon element 416 (which functions as an "air cathode") is reduced during operation of the electrochemical cell 400. - The arrow in FIG. 4 labeled "Oxygen Entering Carbon Aerogel Element 416" indicates that oxygen entering carbon aerogel element 416 is a recipient of electrons generated by operation of electrochemical cell 400. Since the amount of oxygen can be from an inexhaustible source (e.g., the Earth's atmosphere) or from a source having a number of moles equal to or greater than the number of moles of iron metal in electrode 408, iron metal electrode 408 can optionally be allowed to react to completion. In particular, iron metal electrode 408 can be allowed to react to completion if a fresh reactive surface is exposed upon separation of reaction product 420 from iron metal component 408. In other examples, iron metal electrode can be partially or completely reacted upon diffusion of hydroxyl ions through an adhesion layer of reaction product 420 to unreacted portions of iron metal electrode 408. The electrolytic reaction proceeds to oxidize iron metal 408 to form iron (II) hydroxide, Fe(OH). 2 and / or its partially oxidized form Fe(OH) 2 -xO x This produces "green rust", which is a ferric oxide nanoparticle that is oxidized to a metal oxide. In practice, this material falls to the bottom of the reaction chamber and can be removed, for example, by gravity or by pumping to a separate chamber. In the separate chamber, the (partially oxidized) iron hydroxide can be treated with air in basic conditions (e.g., pH>8) to obtain magnetic IONPs.

[0127] Operation of the electrochemical cell and formation of the iron oxide metal product (e.g., ferromagnetic iron compounds, ferrimagnetic iron compounds, or both) can be carried out at a variety of temperatures. In some embodiments, operation is carried out at a temperature between 15° C. and 35° C.

[0128] It should be noted that although the preparation of iron oxide metal products is described herein, the electrochemical / air oxidation process is not limited to iron. Other metals may be used, and one of skill in the art will recognize suitable metals and their oxidation products. Without wishing to be bound by theory, it is believed that for all metals (M) capable of forming stable divalent cations (e.g., Fe, Mn, Ni, Co, Cu, Zn, Sn, etc.), the immediate reaction product formed on the surface of the M anode is the corresponding metal double hydroxide salt, M(OH)2. With metals where +2 is the highest possible oxidation state (e.g., Zn), or when the metal is in an oxidation state higher than +2 (e.g., Ni, Co, Cu), it is not energetically favorable to form in air at low temperatures, and M(OH) 2 is also likely to be the final reaction product. In the particular case of Fe (and Mn), the +3 oxidation state is readily available in air at low temperatures, so M(OH) 2 tends to be an intermediate, leading to a higher oxidation state depending on the potential pH conditions described herein below.

[0129] The magnetic IONPs (e.g., magnetite, maghemite, and / or solid solutions thereof) are ferromagnetic and can be separated from the reaction mixture by magnetism (keeping in mind that iron hydroxide is paramagnetic). The recovered magnetite is then washed and dried for further processing, e.g., as an iron source in LFP synthesis.

[0130] The magnetic IONPs produced as described above have been subjected to XRD analysis and it has been confirmed that the observed XRD pattern matches that of the calculated cubic spinel. The magnetic particles produced in this way are in the form of nanoparticles, i.e. particles with sizes in the region of 20-100 nm when observed using a scanning electron microscope. Surprisingly, it was observed that the concentration of the electrolyte used in the process could affect the particle size of the particles produced.

[0131] In the specific example of Fe, Fe(OH) 2 and / or its partially oxidized form FeO x (OH) 2-x (i.e., "green rust") appears to be the first intermediate formed. In some embodiments, the iron hydroxide / iron oxide product is iron(I) hydroxide (Fe(OH) 2 ) or in a partially oxidized form (iron oxyhydroxide; FeO x (OH) 2-x ). Thus, in some embodiments, the method converts the iron hydroxide or iron oxyhydroxide into magnetite (Fe 3 O 4 ) or maghemite (Fe 2 O 3 In some embodiments, the oxidative conversion includes aeration under alkaline conditions. Without any specific further treatment at neutral pH, green rust slowly oxidizes to goethite, FeOOH. On the other hand, controlled oxidation with air at pH above 8 produces magnetite (FeOOH) with dehydration. 3 O 4 Further oxidation of magnetite with air gives maghemite (Fe 2 O 3 or the spinel representation of magnetite, Fe8 / 3V1 / 3O4, where V=vacancy). Similar transformations are expected due to the availability of the +3 oxidation state of manganese.

[0132] In some embodiments, the electrochemical air oxidation of iron is carried out in an alkaline environment, resulting in a non-magnetic iron oxide / hydroxide form. In other embodiments, the electrochemical air oxidation of iron is carried out as described herein above, and the resulting iron hydroxide or oxyhydroxide is isolated and then exposed to an aqueous environment having a pH greater than about 8, such as about 8, about 9, or about 10 up to about 11, about 12, about 13, or about 14, and then contacted with an oxygen source, such as air. In one embodiment, air is bubbled through the iron hydroxide / oxyhydroxide suspended or dissolved in an alkaline aqueous system. Such an alkaline aqueous system may be provided, for example, by an aqueous solution of a base, such as a carbonate or hydroxide.

[0133] In some embodiments, the iron hydroxide / iron oxide product does not require purification and / or washing to remove contaminants. In instances where sodium chloride is present in the electrolyte, the reaction products may include benign sodium chloride (NaCl), which can be simply removed by washing the reaction products with water. Sodium chloride is less of a pollutant to the environment and poses less of a threat to human health than the sulfates and ammonia produced by alternative processing techniques. When the electrolyte is ammonium chloride (NH 4 In the case of the example containing ammonium chloride, repair is also less problematic than in other processes. Ammonium chloride is converted to NH 3 It decomposes into a gaseous mixture of NH 4 The temperature of the gas mixture may be reduced below 338° C. after gas evolution so that Cl is recondensed into a solid form that can be recycled. 4 The Cl salt impurities do not require washing and therefore do not produce waste water.

[0134] In some embodiments, the IONPs are magnetic, such as magnetite, maghemite, or a solid solution or mixture thereof, and are separated from the electrolyte 424 by a magnetic process. In particular, when the oxide product 420 is exposed to a magnetic field (e.g., from a permanent magnet or electromagnet), the magnetic IONP products are attracted and held by the magnetic field. The held magnetite can then be washed, for example, with water, and then collected. For example, the magnetic field may be removed, or the magnetite may be physically separated from the magnet. The magnetic IONPs may optionally be dried by any suitable conventional means, or may be utilized in the disclosed methods described below in wet or partially dried form. Because magnetite and maghemite exhibit microwave sensitivity, these reaction products can be heated and thus dried using microwave radiation, which is more energy efficient than using indirect heating via an oven.

[0135] In some embodiments, the group of precursors includes precursors that have microwave sensitivity. In one particular embodiment, magnetite is a preferred transition metal oxide (i.e., a microwave susceptor) given the microwave sensitivity of magnetite. By receiving microwave energy and converting it to heat, magnetite allows for carbonization of the organogel and conversion of the reactants to LFPs without wasteful and energy-inefficient furnace treatment. As magnetite is consumed during the reaction and carbonization process, its microwave sensitivity decreases. However, during the consumption of magnetite, the organogel is increasingly converted to carbon. Since carbon is also a microwave susceptor, it gradually converts more microwave radiation into heat, thereby maintaining the conversion of the reactants to LFPs. The magnetic sensitivity (e.g., ferromagnetic, paramagnetic, or both) of these components also aids in microwave drying of the reagents and the finished LFPs without resorting to energy-intensive and inconvenient thermal drying.

[0136] In some embodiments, the iron oxide produced by the disclosed air anodization process is nanoparticulate. A scanning electron micrograph of the nanoparticulate iron oxide produced by air anodization described herein above is provided as FIG. 5A and shows an average (roughly cubic) particle size of about 60 nm. Surprisingly, the average particle size is reduced by reducing the concentration of electrolyte and / or changing the electrolyte anion to Na + From K + It was found that the solubility of Fe in water can be reduced by changing the solubility of Fe in water to Fe. The powder X-ray diffraction pattern is provided as FIG. 5B. 3-x O 4 (0≦x≦0.33) demonstrating the cubic structure of the product. In some embodiments, the IONP has the composition Fe 3-x O 4 (0≦x≦0.333). In such embodiments, the oxidation state of iron is 2.67-3. The nitrogen adsorption BET surface area of ​​the IONPs prepared as disclosed can vary, for example, with changes in the identity and concentration of the electrolyte. For example, according to the present disclosure, Fe IONPs obtained using 1M NaCl as the electrolyte have a BET surface area of ​​2.67-3. 3-x O 4 is 22.46m 2 / g, while Fe obtained with 0.2 M KCl as electrolyte 3-x O 4 is 40.22m 2 It was found to have a BET surface area of ​​100 nm / g. Thus, the process can be tailored to produce particles of different sizes depending on the intended end use. The term "size" in this case refers to the characteristic dimension of the particle. The characteristic dimension of a roughly spherical particle may be the diameter. In other cases, depending on the shape of the particle, the characteristic dimension may be one or more of the width, length, and / or depth.

[0137] Table 1 presents particle size and specific surface area data for iron oxides and corresponding LFPs of the present disclosure prepared therefrom under various experimental conditions described herein. Note that some examples include ball milling to unexpectedly approach specific surface areas as much as 10 times greater than commercially available materials. [Table 1]

[0138] The disclosed air anodization method of preparing magnetic IONPs, especially when combined with magnetic separation and washing, can be implemented in a semi-continuous or continuous process. A non-limiting flow diagram of a production scheme for the semi-continuous synthesis of magnetite is provided in Figure 6. Each of the processes shown in Figure 6 have been described herein in different contexts and do not require further explanation.

[0139] In some embodiments, the transition metal of the transition metal oxide is a combination of manganese and iron (e.g., iron-manganese mixed oxide). In some embodiments, the transition metal oxide is of the formula Fe 3-x Mn x O 4 In some embodiments, the resulting lithium transition metal phosphate cathode material is a mixed iron-manganese oxide having the formula LiFe 1-y Mn y O 4 has.

[0140] 2. Second Precursor i. Phosphate At least a second precursor of the group of precursors comprises a liquid phase having a second density, the second density being less than the first density (e.g., less than about 1, less than about 2, less than about 3, less than about 4, or less than about 5 g / cc).

[0141] In some embodiments, the precursor group is an aqueous solution of phosphoric acid (H 3 PO 4). Generally, an aqueous solution of phosphoric acid is provided by adding a desired volume of concentrated phosphoric acid to a desired volume of water. The volume of the aqueous solution and the amount (i.e., concentration) of phosphoric acid present in the solution can vary. Generally, phosphoric acid is prepared by adding LiMPO 4 Approximately 1:1 for the cathode family, Li 3 M 2 (PO 4 ) 3 The cathode family has a ratio of about 1:1.5 transition metal to phosphate (PO 4 3- In some embodiments, the volume of the aqueous solution is selected to provide a phosphate concentration in the range of about 0.1 to about 10 molar (i.e., moles per liter), or about 1 to about 5 molar, such as about 2 to 3 molar.

[0142] ii. Lithium ion source In some embodiments, the liquid phase includes a lithium ion source. Any lithium compound that is water soluble or capable of being dissolved in an aqueous phosphoric acid solution may be used. Examples of suitable lithium salts include, but are not limited to, lithium hydroxide, lithium carbonate, lithium acetate, lithium chloride, and the like. One particularly suitable lithium ion source is lithium carbonate (Li 2 ), which is relatively inexpensive and readily available. 2 CO 3 ). The lithium carbonate gradually dissolves in the aqueous phosphoric acid solution with the evolution of carbon dioxide gas. At least a portion of the lithium ions present may be associated with the phosphate ions as monobasic lithium phosphate. The amount of lithium ion source (e.g., lithium carbonate) added may vary. Generally, the lithium ion source is added in an amount sufficient to provide a molar ratio of lithium ions to phosphate and transition metal ions of about 1:1:1.

[0143] iii. Alternatives to the first or second precursor Although the first and second precursors are described above in terms of transition metal oxide and lithium / phosphate, respectively, it is contemplated herein that the identities of the first and second precursors may be reversed, and thus the description of the first and second precursors is not intended to be limited to the foregoing embodiments.

[0144] Additionally, other sources of transition metals (e.g., iron) are contemplated herein. For example, the transition metal can be iron, but the source can be other than the oxide. Such alternatives are described below.

[0145] Alternative Transition Metal Sources (Iron Oxalate) In some embodiments, the transition metal is iron and the source of iron is iron oxalate. Surprisingly, in accordance with the present disclosure, it has been found that iron oxalate can be used directly in the process without first being converted to iron(III) oxide. Thus, in another embodiment, the process comprises the steps of: 2 O 4 ), phosphoric acid aqueous solution (H 3 PO 4 ), and lithium carbonate as precursor groups. The resulting lithium iron phosphate cathode material within a conductive carbon matrix was found to have a nanoparticulate morphology comparable to that prepared by the sequential method, where iron oxalate is first converted to iron(III) oxide.

[0146] In some embodiments, the transition metal is iron and the source of iron is iron oxalate. However, in this sequence, the iron oxalate is first converted to iron phosphate, and the iron phosphate is reacted with lithium carbonate and one or more organogel precursor materials. Thus, in another embodiment, the method includes the steps of: 2 O 4 ) and phosphoric acid solution (H 3 PO 4 ) to form a compound of the formula Fe x (PO 4 ) yand combining the iron phosphate mixture with a lithium ion source. Without wishing to be bound by theory, it is believed that the chemical reactions occurring during mixing and pyrolysis can be represented by the following equation: (1) 3Fe 2 (C 2 O 4 ) 3 +2H 3 PO 4 →Fe x (PO 4 ) y +3H 2 C 2 O 4 , where x=y=1 (2) Iron x (PO 4 ) y + 1 / 2 Li 2 CO 3 +PAA / H 2 O→LFP / C, where x=y=1 (3) Iron x (PO 4 ) y +Li 3 PO 4 +PAA / H 2 O→LFP / C, where x=3, y=2.

[0147] Alternative Transition Metal Sources (Ferrous and Manganese Sulfates) In some embodiments, the transition metals are iron and manganese. In one permutation, iron sulfate and manganese sulfate are reacted together with oxalic acid to form a mixed oxalate, the mixed oxalate is converted to a mixed iron-manganese oxalate, and the mixed iron-manganese oxalate is reacted with lithium carbonate and phosphoric acid. Thus, in another embodiment, iron(II) sulfate, manganese(II) sulfate, and oxalic acid are combined in water to form a ferrous oxide of the formula Fe 1-x Mn x C 2 O 4 The formation of a precipitate of mixed iron-manganese oxalate and the phosphoric acid solution (H 3 PO 4) containing nanoporous mixed iron-manganese oxide suspended in water with the formula Fe 2-2x Mn 2x O 3t or Fe 3-x Mn x O 4 The method includes exposing the mixed iron-manganese oxalate to air at a temperature in the range of about 350 to about 450° C. for a period of time sufficient to convert the mixed iron-manganese oxalate to a nanoporous mixed iron-manganese oxide of 0.01% by mass, mixing the suspension for a period of time, and adding a source of lithium ions to the suspension to form a reaction mixture. The lithium manganese iron phosphate cathode material thus prepared has the formula LiFe, where x is [0≦x≦1]. 1-x Mn x PO 4 According to the present disclosure, the compound having the formula Fe 2-2x Mn 2x O 3 The nanoporous mixed iron-manganese oxides were found to have average particle sizes on the order of a few microns; however, high-resolution imaging reveals the presence of internal permeable porosity with pore diameters of approximately 100 nm. 1-x MnxC 2 O 4 .2H 2 Fe obtained by thermal decomposition of O 2 - 2x Mn 2x O 3 is about 11.93m 2 / g BET nitrogen surface area.

[0148] Without wishing to be bound by theory, it is believed that the chemical reactions occurring during mixing and pyrolysis can be represented by the following equation: (1) xFeSO 4 +1-xMnSO 4 +H 2 C 2 O 4 +H 2 O→Fe x Mn 1-x C 2 O 4(s) +H+ (aqueous solution)+SO 4 2- (水溶液) (2) Iron x Mn 1-x C 2 O 4 +air→Fe 2-2x Mn 2x O 3(ナノ多孔質) +CO 2 (350~450℃) (3) Iron 2-2x Mn 2x O 3(ナノ多孔質) +2H 3 PO 4 +Li 2 CO 3 +PAA / H 2 O → LMFP / C (ナノ粒子状)

[0149] In another permutation, iron sulfate and manganese sulfate are reacted together with oxalic acid to form a mixed oxalate salt, and the mixed oxalate salt is reacted with phosphoric acid and lithium carbonate. Thus, in another embodiment, the method comprises combining iron(II) sulfate, manganese(II) sulfate, and oxalic acid in water to form a compound of the formula Fe 1-x Mn x C 2 O 4 forming a mixture containing iron-manganese oxalate and lithium carbonate and phosphoric acid aqueous solution (H 3 PO 4 ) is added, and after pyrolysis, a LiFe 1-x Mn x PO 4 Without wishing to be bound by theory, it is believed that the chemical reactions occurring during mixing and pyrolysis can be represented by the following equation: (1) xFeSO 4 +1-xMnSO 4 +H 2 C 2 O 4 +H 2 O→Fe x Mn 1-x C 2 O4(s) +H + (aqueous solution)+SO 4 2- (水溶液) (2) Iron x Mn 1-x C 2 O 4 + 1 / 2 Li 2 CO 3 +H 3 PO 4 +PAA / H 2 O → LMFP / C (nanoparticle form)

[0150] In yet another permutation, iron sulfate and manganese sulfate are reacted together with oxalic acid to form a mixed oxalate, and the mixed oxalate is reacted with phosphoric acid to form an intermediate mixed iron-manganese phosphate. This mixed phosphate is then reacted with lithium phosphate. Thus, in another aspect, the method involves combining iron(II) sulfate, manganese(II) sulfate, and oxalic acid in water to form a lithium phosphate of the formula Fe 1-x Mn x C 2 O 4 The mixed iron-manganese oxalate precipitate is formed, and the mixed iron-manganese oxalate is converted into phosphoric acid (H 3 PO 4 ) to convert the mixed metal oxalates to mixed metal phosphates; adding lithium phosphate to obtain, after thermal decomposition, a mixture of the formula LiFe, where x is [0≦x≦1]. 1-x Mn x PO 4 Without wishing to be bound by theory, it is believed that the chemical reactions occurring during mixing and pyrolysis can be represented by the following equation: (1) xFeSO 4 +1-xMnSO 4 +H 2 C 2 O 4 +H 2 O→Fe x Mn 1-x C 2 O 4(s) +H +(aqueous solution)+SO 4 2- (水溶液) (2) 3Fe x Mn 1-x C 2 O 4 +2H 3 PO 4 →(Fe x Mn 1-x ) 3 (PO 4 ) 2 +3H 2 C 2 O 4 (3)(Fe x Mn 1-x ) 3 (PO 4 ) 2 +Li 3 PO 4 +PAA / H 2 O→3LiFe x Mn 1-x PO 4 / C

[0151] B. Carbon Precursors The method includes providing one or more carbon precursors in a fluid state, meaning that the mixture containing them can flow, does not have a fixed shape, and has low or no resistance to external stress. The one or more carbon precursors in a fluid state are configured to form a solid organogel in the presence of a gelation initiator, and the solid organogel is configured to form a conductive carbon matrix upon pyrolysis. In alternative aspects, the solid organogel can be formed through removing a liquid phase (e.g., solvent) from the solution. For example, in some aspects, partial or complete removal of the solvent by a drying method can result in the organogel in the absence of gelation induced by a gelation initiator. In general, the conductive carbon matrix includes a carbonized form of the organogel and / or its precursor material and surrounds the LMP particles and / or its precursor. The conductive carbon matrix can include graphitic carbon, amorphous carbon, or a mixture thereof. The conductive carbon matrix is ​​maintained despite particle size reduction upon any subsequent milling.

[0152] In some embodiments, the method includes mixing a group of lithium transition metal phosphate cathode material precursors with one or more carbon precursors to form a precursor mixture, adding a gelation initiator to the precursor mixture, and allowing the one or more carbon precursors to undergo gelation to form a solid organogel. As described herein above, such solid organogel is formed in the presence of precursors of lithium-transition metal-phosphate materials, and is therefore understood to include such precursors, their reaction products, and intermediates that ultimately result in lithium transition metal phosphate materials upon pyrolysis of a solid organogel containing such species.

[0153] "Carbon precursor" refers to a material capable of undergoing polymerization or other gelation reactions to produce a solid organogel, which can then be pyrolyzed to form a conductive carbon matrix. Generally, the solid organogel is porous in nature and capable of forming a conductive carbon matrix upon exposure to elevated temperature conditions as described herein below. In some embodiments, a catalyst or gelation initiator is utilized to initiate and / or complete the gelation. Suitable organogels include, but are not limited to, phloroglucinol-furfural aldehyde polymers, resorcinol-furfural aldehyde polymers, phenol-formaldehyde polymers, polyurethanes, melimine-aldehyde polymers, polyacrylamide polymers, polybenzoxazine polymers, polyamic acids, and polyimides. Each of these organogels and their respective precursor materials (i.e., carbon precursors), as well as gelation conditions, are further described herein below.

[0154] 1. Phloroglucinol-furfural, resorcinol-furfural, and phenol-formaldehyde polymers In some embodiments, the solid organogel is a phloroglucinol-furfural (PF) polymer. In such embodiments, the organogel precursor materials are phloroglucinol and furfural. In such embodiments, the method generally includes adding phloroglucinol and furfural to a reaction mixture, reacting the phloroglucinol and furfural, and forming an organic matrix comprising a PF organogel. Gelation of the phloroglucinol and furfural mixture occurs nearly instantaneously (e.g., 30 seconds or less, 15 seconds or less, 5 seconds or less). Thus, phloroglucinol and furfural are added individually to the reaction mixture in either order in succession. In some embodiments, phloroglucinol and furfural are each provided separately as an ethanol solution. No catalyst or initiator is required. However, in some embodiments, a gelation initiator is utilized. In some embodiments, the gelation initiator is an amine base or an acid. When phloroglucinol and furfural are combined, optionally with an initiator, gelation of the PF polymer occurs rapidly (e.g., in about 30 seconds or less). The resulting PF polymer contains a number of repeating units ("n"), which can vary depending on the reaction conditions and reactant ratios. In general, the resulting PF organogel has a rigid three-dimensional structure.

[0155] In another embodiment, the solid organogel is a resorcinol-furfural polymer. Such a polymer can be prepared as above, substituting phloroglucinol for resorcinol.

[0156] In yet other embodiments, the solid organogel is a phenol-formaldehyde (PF) polymer. Such a polymer can be prepared as above, substituting phenol for phloroglucinol and formaldehyde for furfural.

[0157] 2. Polyurethane polymer In some embodiments, the solid organogel includes or is a polyurethane polymer. In such embodiments, the precursor includes a polyol and an isocyanate. In some embodiments, the polyol is cellulose. In such embodiments, the gelation initiator includes an alkylamine (e.g., triethylamine).

[0158] 3. Polyamic acid In some embodiments, the organogel is a polyamic acid. Polyamic acids are polymer amides with repeating units that contain carboxylic acid groups, carboxamide groups, and aromatic or aliphatic moieties that contain the diamines and tetracarboxylic acids from which the polyamic acid is derived. A "repeating unit" as defined herein is a portion of a polyamic acid (or corresponding polyimide) whose repeats would generate a complete polymer chain (excluding terminal amino groups or unreacted anhydride ends) by linking the repeating units together consecutively along the polymer chain. Those skilled in the art will recognize that polyamic acid repeating units result from partial condensation of the carboxyl groups of a tetracarboxylic dianhydride with the amino groups of a diamine.

[0159] In some aspects, the polyamic acid is any commercially available polyamic acid. In other aspects, the polyamic acid is preformed ("preformed") and isolated, e.g., prepared, by reaction of a diamine and a tetracarboxylic dianhydride in an organic solvent according to conventional synthetic methods. In either case, whether purchased or prepared and isolated, suitable polyamic acids are in substantially pure form. Preformed, isolated, or commercially available polyamic acids can be in solid form, e.g., powder or crystalline form, or in liquid form.

[0160] Suitable polyamic acids, polyimides, and methods for preparing them are provided, for example, in U.S. Patent Application Publication No. US2022 / 0069290 to Zafiropoulos, and U.S. Patent Application No. 17 / 546,761 to Leventis, and U.S. Patent Application No. 17 / 546,529 to Begag, each of which is incorporated herein in its entirety.

[0161] In some embodiments, the polyamic acid is provided in the form of a water-soluble salt, which can then be precipitated from the reaction mixture as an insoluble polyamic acid by acidification of the reaction mixture, hi such embodiments, the organogel precursor material is an ammonium or alkali metal polyamic acid salt, and the method further comprises adding a gelation initiator to the reaction mixture.

[0162] In some embodiments, the organogel precursor material is a polyamic acid ammonium salt, including but not limited to ammonium salts with trialkylamines. In some embodiments, the ammonium salt is a salt of a polyamic acid with trimethylamine, triethylamine, tri-n-propylamine, tri-n-butylamine, N-methylpyrrolidine, N-methylpiperidine, diisopropylethylamine, or a combination thereof. In some embodiments, the ammonium salt is a salt of a polyamic acid with triethylamine. In some embodiments, the ammonium salt is a salt of a polyamic acid with diisopropylethylamine.

[0163] In some embodiments, the organogel precursor material is an alkali metal salt of a polyamic acid, such as the lithium, sodium, or potassium salt.

[0164] The gelation initiator is generally an acid or a substance that can be hydrolyzed to form an acid. One non-limiting example of a suitable acid is acetic acid. One non-limiting example of a suitable substance that can be hydrolyzed to form an acid is acetic anhydride. Thus, in some embodiments, the method includes adding acetic acid, acetic anhydride, natural protonated phosphate, or a combination thereof as a gelation initiator. In some embodiments, the method includes adding acetic anhydride, hydrolyzing the acetic anhydride, forming acetic acid, and inducing the gelation of the polyamic acid.

[0165] 4. Polyimide In some embodiments, the solid organogel comprises or is a polyimide. In some embodiments, the polyimide is formed from the imidization of a polyamic acid. Suitable polyimides and methods for preparing them are provided, for example, in U.S. Patent Application Publication No. US2022 / 0069290 to Zafiropoulos, U.S. Patent Application No. 17 / 546,761 to Leventis, and U.S. Patent Application No. 17 / 546,529 to Begag, each of which is incorporated herein in its entirety.

[0166] In some embodiments, imidizing the polyamic acid salt comprises thermally imidizing the corresponding polyamic acid. Irradiation of the wet gel polyamic acid material with microwave frequency energy is one particularly suitable thermal treatment.

[0167] In other aspects, imidizing the polyamic acid salt includes performing chemical imidization, which includes adding a gelation initiator to an aqueous solution of a salt of a polyamic acid to form a gelling mixture ("sol"), and allowing the gelling mixture to gel (e.g., in a mold, or cast onto a sheet, or in a variety of other formats such as beads). In such aspects, the gelation initiator is added to initiate and drive the imidization to form a polyimide wet gel from the polyamic acid salt.

[0168] The structure of the gelation initiator can vary, but generally it is at least partially soluble in the reaction solution, reactive with the carboxylate groups of the polyamic acid salt, and is an effective reagent for driving imidization of the polyamic acid carboxyl and amide groups while minimizing reactivity with aqueous solutions. One example of a suitable class of gelation initiators are carboxylic acid anhydrides, such as acetic anhydride, propionic anhydride, and the like. In some aspects, the gelation initiator is acetic anhydride.

[0169] In some embodiments, the amount of gelation initiator can vary based on the amount of tetracarboxylic dianhydride or polyamic acid. For example, in some embodiments, the gelation initiator is present in various molar ratios with the tetracarboxylic dianhydride. In some embodiments, the gelation initiator is present in various molar ratios with the polyamic acid. The molar ratio of gelation initiator to tetracarboxylic dianhydride or polyamic acid can vary depending on the desired reaction time, reagent structure, and desired material properties. In some embodiments, the molar ratio is about 2 to about 10, such as about 2, about 3, about 4, or about 5 to about 6, about 7, about 8, about 9, or about 10. In some embodiments, the ratio is about 2 to about 5.

[0170] The temperature at which the gelling reaction is permitted to proceed can vary, but is generally less than about 50°C, such as from about 10 to about 50°C, or from about 15 to about 25°C.

[0171] 5. Other polymer organogels In some embodiments, the solid organogel comprises a melamine-aldehyde polymer. In some embodiments, the solid organogel comprises a polyacrylamide polymer. In some embodiments, the solid organogel comprises a polybenzoxazine polymer. Such polymers, their precursors, and gelation initiators suitable for their formation are known to those of skill in the art.

[0172] 6. Concentration of Organogel Precursor Materials In some examples, the organogel precursor materials are collectively present in a concentration of the total mixture (i.e., including the lithium transition metal phosphate cathode material precursor) that approximates that of the carbon content of the resulting lithium metal phosphate material. For example, the organogel precursors can be present at approximately 1 weight percent (wt%) to 5 wt% of the lithium, transition metal, and phosphorus precursors in a stoichiometric 1:1:1 ratio.

[0173] C. Mixed The method includes mixing a group of precursors for synthesizing lithium transition metal phosphates with one or more carbon precursors in a fluid state for a period of time to form a precursor mixture, followed by adding a gelation initiator. The mixing is generally performed by stirring the mixture (i.e., as a suspension) at room temperature (e.g., approximately 20° C.) for a period of about 1 to about 12 hours, typically about 2 to about 4 hours. During this time, the particle size of the transition metal oxide is generally reduced from the initial particle size to a particle size in the range of about 1 to about 3 microns. Depending on the initial particle size, in some embodiments it may be desirable to perform active particle size reduction by milling, grinding, etc. In other embodiments, such particle size reduction is not performed beyond the described stirring. The mixture is generally mixed (e.g., by stirring) for a period of time sufficient to allow complete dissolution of the lithium ion source in the aqueous suspension.

[0174] D. Solid Organogels As described herein above, the method includes forming a solid organogel by subjecting one or more organogel precursor materials to gelation. As used herein in reference to an organogel, the term "solid" means that the organogel is self-supporting, e.g., a solid organogel is one that maintains a defined shape in the absence of any restraint.

[0175] The solid organogel, whether it comprises a PF polymer, a polyamic acid, a polyimide, or another polymer described herein, has a three-dimensional external (i.e., macro) and internal (e.g., micro, such as fibrils / pores) structure. In some embodiments, the solid organogel is a polyamic acid, a polyimide, or a combination thereof. For example, in certain embodiments, after gelation, the polyamic acid ammonium salts described herein above are converted partially to the corresponding polyamic acid and partially to the corresponding polyimide. The relative proportions of polyamic acid and polyimide can vary. The proportions of each can be determined by methods known in the art, such as nuclear magnetic resonance (NMR) and Fourier transform infrared spectroscopy (FTIR). Without wishing to be bound by theory, it is believed that a greater proportion of polyimide in the organic matrix results in a harder solid lithium metal phosphate material embedded in the carbon matrix after pyrolysis. Moreover, it has been surprisingly discovered, in accordance with the present disclosure, that in at least some embodiments, the presence of a relatively large amount of polyamic acid in an organic matrix provides a lithium transition metal phosphate / carbon matrix product having fewer impurities, greater uniformity in particle size, greater uniformity in morphology, or a combination thereof, as compared to a product obtained in the presence of a relatively large amount of polyimide. These differences can be inferred by a number of observational techniques, including, but not limited to, x-ray diffraction, electron microscopy, and acoustic densitometry.

[0176] The solid organogel is composed of lithium ions, transition metal oxide particles (e.g., iron(II or III) oxide), phosphoric acid (PO 4 3-) ions, and water in which they are suspended. At least a portion of the lithium ions and phosphate ions may be associated as lithium phosphate. In general, the various species present (lithium, and phosphate ions or salts thereof, transition metal oxide, and water) are held together in close proximity within the organogel. Without wishing to be bound by any particular theory, it is believed that this intimate physical contact facilitates the formation of the cathode material during pyrolysis and advantageously provides the cathode material with desirable physical properties. As described herein above, the use of the organogel inhibits phase separation of the precursor materials during the formation of the lithium transition metal phosphate cathode material. Because the formation of the cathode material is a diffusion-limited process, maintaining intimate contact between the lithium transition metal phosphate precursor materials is particularly important for the efficient and effective synthesis of the lithium transition metal phosphate cathode material. The viscosity of the organogel, the reaction mixture containing the organogel precursor materials, or both can be varied and is generally selected such that at room temperature and atmospheric pressure, the viscosity of the organogel is sufficient to prevent settling of solid phase materials (including, but not limited to, a transition metal source, such as a transition metal oxide, and liquid phase material(s)) from the reaction mixture due to density differences.

[0177] In some examples, the organogel precursor materials may gel almost instantly (e.g., in less than 30 seconds, less than 15 seconds, less than 5 seconds), thereby reducing the gelation time of other precursors (e.g., less than 1 gram / cm 3 A solid phase with a density of more than 1 g / cm 3 The gelation process prevents phase separation of the lithium iron phosphate cathode material (a liquid phase having a density of 100 nm). In some instances, gelation occurs via the polymerization reaction described above rather than through removal of the solvent. This can reduce the energy input required to produce the lithium iron phosphate cathode material by avoiding or reducing the need for energy-intensive drying processes. Notably, the solid aerogel produced by such gelation is distinct and separate from other solid phase materials utilized in previously reported syntheses of LFP materials in carbon matrices (e.g., non-gelling sugars or starches).

[0178] Additionally, as described herein above, the precursors and gelling conditions are selected such that the resulting organogel maintains the desired solid morphology, thereby maintaining intimate contact between the reactants during the thermal treatment (pyrolysis) required to convert the precursors to lithium transition metal phosphate cathode materials. In some embodiments, the solid organogel comprises a porous network of interconnected solid-phase polymeric structures, which is composed of a first precursor of the group and a second precursor of the group, e.g., iron oxide and a lithium / phosphate species (e.g., LiH 2 PO 4 ), especially lithium phosphate (LiH 2 PO 4 ) melt above 300° C. Thus, in some embodiments, the organogel maintains contact between the precursors at temperatures of at least about 300° C. This property of the disclosed organogels is also different and distinct from other solid phase materials utilized in previously reported syntheses of LFP materials in a carbon matrix (e.g., sugars or starches, which do not maintain structural rigidity upon heating).

[0179] E. Pyrolysis The solid organogel containing the lithium transition metal phosphate precursor material (e.g., lithium ions, one or more transition metal oxides, and phosphate ions) is then pyrolyzed (e.g., carbonized), which means that the organogel is pyrolyzed to 1) convert substantially all of the organogel material to carbon and form a conductive carbon matrix, and 2) optionally reduce transition metals of higher oxidation states to lower states (e.g., Fe 2 O 3 Fe(III) in LiFePO 4and 3) forming a lithium transition metal phosphate cathode material contained within a conductive carbon matrix. As used herein in the context of pyrolysis, "substantially all" means that greater than 95% of the organogel material is converted to carbon, such as 99%, or 99.9%, or 99.99%, or even 100% of the organogel is converted to carbon. Pyrolysis of the organogel converts it to a homogenous carbon matrix, and conversion to a carbon matrix means that the physical properties of the organogel (e.g., porosity, surface area, pore size, diameter, etc.) are substantially retained within the corresponding carbon matrix. Without wishing to be bound by theory, it is believed that carbonization helps promote good electrical conductivity of the resulting matrix while simultaneously initiating and driving to completion the reaction between the transition metal oxide, lithium ions, and phosphate ions to form the lithium-transition metal-phosphate cathode material within the conductive carbon matrix. Additionally, the organogel materials disclosed herein are rich in aromatic rings which upon pyrolysis result in a carbon matrix with high electrical conductivity.Furthermore, the uniform distribution of the lithium-transition metal-phosphate cathode material throughout a continuous three-dimensional conductive carbon matrix provides superior performance characteristics for batteries utilizing such cathode materials, as further described herein below.

[0180] Without wishing to be bound by theory, it is believed that during pyrolysis, the lithium-transition metal-phosphate cathode material inherits the morphology of the precursor transition metal oxide and is formed on the transition metal oxide by a templating process. This occurs as water evaporates from the slurry and loose precursor ions associate during evaporation, forming LiFePO 4 This process is believed to be distinct and separate from previously reported processes for the formation of

[0181] In embodiments in which the transition metal of the transition metal oxide is present in a higher oxidation state than that present in the lithium-transition metal-phosphate cathode materials described hereinabove, a portion of the carbon produced during pyrolysis may be converted to a higher oxidation state of the transition metal (e.g., Fe2 O 3 It is believed that it functions to reduce iron(III) present in ZnO to iron(II).

[0182] The temperature required for pyrolysis can vary. In some embodiments, the organogel matrix is ​​subjected to a treatment temperature of about 600°C or higher, such as about 600°C, about 650°C, about 700°C, about 750°C, about 800°C, about 850°C, about 900°C, or about 950°C, or a range between any two of these values, to carbonize the organogel matrix and complete the formation of the lithium-transition metal-phosphate cathode material. In some embodiments, the pyrolysis temperature is about 600 to about 800°C. Generally, pyrolysis is carried out under an inert or slightly reducing atmosphere to prevent combustion of the organic and / or carbon materials and to prevent reoxidation of the transition metal. Suitable atmospheres include, but are not limited to, nitrogen, argon, hydrogen, methane, or combinations thereof. In some embodiments, pyrolysis is carried out under nitrogen.

[0183] In some embodiments, the pyrolysis is carried out using microwave irradiation. Microwaves are low energy electromagnetic waves with wavelengths ranging from 0.001 to 0.3 meters and frequencies ranging from 1,000 to 300,000 MHz. A typical microwave device operates with microwaves at a frequency of 2450 MHz. In some embodiments, the group of precursors includes microwave-sensitive precursors and the pyrolysis is carried out by applying microwave radiation.

[0184] In some embodiments, the microwave-sensitive precursor comprises one or more of carbon, magnetite, and maghemite. In some embodiments, the precursor comprises magnetic iron oxide nanoparticles (magnetic IONPs), such as nanoparticulate magnetite or maghemite. In some embodiments, the microwave-sensitive precursor comprises one or more nanoparticles of magnetite and maghemite having a characteristic dimension between 20 nm and 100 nm.

[0185] In some embodiments, the magnetic IONPs are gradually converted to LiFe(PO 4 ), and as the organogel precursor is pyrolyzed to carbon, the microwave absorbing components change from a magnetic phase to a carbonized component. This is because LiFe(PO 4 ) itself does not respond strongly to microwave radiation, whereas the carbon materials described herein above heat efficiently upon exposure to microwave radiation.

[0186] The time required for completion of pyrolysis may vary and may depend on the temperature and the particular matrix components. Typically, the matrix is ​​subjected to pyrolysis conditions for a period ranging from about 4 to about 20 hours, such as about 8 hours. In some examples, microwave pyrolysis using a period that is from about 10 minutes to about 3 hours, such as from about 10 minutes to about 1 hour, or from about 1 hour to about 3 hours, may be more energy efficient and faster.

[0187] Another advantage of the disclosed method is that the carbon source (e.g., organogel such as polyamic acid or polyimide) has a high carbon yield, and therefore the weight percentage of carbon source required (approximately 20 wt%) relative to the total reactant composition is relatively low, resulting in high efficiency and cost savings. In particular, a small amount of carbon source is sufficient to reduce all higher oxidation state transition metal species (e.g., Fe(III) to Fe(II) in the case of iron(III) oxide precursor) during pyrolysis, leaving approximately 2-3% conductive carbon on the surface of the lithium-transition metal-phosphate.

[0188] Additionally, the carbon sources disclosed herein (e.g., organogels such as polyamic acids, polyimides, and other polymers mentioned above) contain abundant aromatic rings. Thus, these materials produce graphitic carbon coatings of lithium-transition metal-phosphates during pyrolysis. The graphitic carbon produced upon carbonization of these materials offers better electrical properties (e.g., higher electrical conductivity) than the saturated carbons found from the carbonization of other carbon sources such as sugars or starches.

[0189] F. Crushing In some embodiments, the lithium-transition metal-phosphate cathode material in a conductive carbon matrix is ​​optionally subjected to one or more grinding procedures to reduce particle size or provide a uniform distribution of particle size. Any suitable grinding technique may be utilized. In some embodiments, grinding may be performed using a ball mill. In some embodiments, grinding is performed in a stainless steel planetary ball mill at a speed ranging from about 100 to 400 rpm for a time ranging from about 30 minutes to about 48 hours.

[0190] The need for grinding, the type of grinding, and its duration can vary based on the nature of the conductive carbon matrix. For example, in some embodiments, cathode material particles prepared from pyrolysis of a polyimide organogel have a hard carbon matrix and may require grinding to provide a powder material (i.e., having a uniformly small particle size). In contrast, cathode material particles prepared from pyrolysis of a polyamic acid organogel tend to be softer and may require less grinding.

[0191] II. Characteristics of lithium transition metal phosphate cathode materials Following pyrolysis, the lithium-transition metal-phosphate cathode material in a conductive carbon matrix has the formula LiM(PO 4 ), or a lithium-transition metal-phosphate cathode material in a conductive carbon matrix has the formula Li 3 M(PO 4 ) 3 In embodiments where M is a combination of Fe and Mn, the stoichiometry of Fe to Mn can vary. For example, the molar ratio of Fe to Mn can range from about 0.1 to about 10, such as about 0.1, about 0.2, about 0.3, about 0.4, about 0.5, about 0.6, about 0.7, about 0.8, about 0.9, or about 1 to about 2, about 3, about 4, about 5, about 6, about 7, about 8, about 9, or about 10. In some embodiments, the molar ratio of Fe to Mn is about 4:1 to about 1:4, about 2:1 to about 1:2, or about 1:1.

[0192] In some embodiments, the lithium-transition metal-phosphate cathode material in a conductive carbon matrix has the formula LiM(PO 4 ) 、 The transition metal oxide source utilized in the method includes magnetite, maghemite, or a combination thereof. In some such embodiments, a residual amount of magnetite, maghemite, or a combination thereof may remain present in the lithium-transition metal-phosphate cathode material in a conductive carbon matrix. The residual amount may vary, but is generally present in an amount sufficient to impart magnetic susceptibility to the cathode material. The magnetic susceptibility imparted by the residual magnetic iron oxide material may vary, but is generally weak, but sufficient to be at least qualitatively observed through the interaction of a sample of the lithium-transition metal-phosphate cathode material in a conductive carbon matrix with a strong neodymium magnet. Quantitative measurements may be performed according to known methods for susceptibility measurements, including, but not limited to, Gouy's magnetic balance (wherein the sample is suspended between the poles of an electromagnet, and the change in weight when the electromagnet is turned on is proportional to the susceptibility) and Evans balance (which measures the force on the magnet itself).

[0193] In some embodiments, the lithium-transition metal-phosphate cathode material in a conductive carbon matrix has a density of about 0.6 to about 1.1 g / cm when prepared from magnetite, maghemite, or a combination thereof. 3 The tap density ranges from 0.01 to 0.1.

[0194] In some embodiments, the lithium-transition metal-phosphate cathode material is an olivine-type lithium iron phosphate. Accordingly, in another embodiment, a composition is provided that includes nanoparticles that include an olivine-type lithium iron phosphate and are integral with a conductive carbon matrix, the nanoparticles having a characteristic dimension of 20 nm to 1000 nm and a surface area of ​​10 meters. 2 (m 2 ) / gram(g)~65m 2In some embodiments, the characteristic dimension is between 30 nm and 70 nm and the specific surface area is between 20 m 2 / g~65m 2 In some embodiments, the characteristic dimension is between 30 nm and 60 nm and the specific surface area is between 22 m 2 / g~40m 2 In some embodiments, the characteristic dimension is between 20 nm and 40 nm and the specific surface area is between 60 m 2 / g~80m 2 / g.

[0195] In some embodiments, the nanoparticles further comprise magnetite, maghemite, or both.

[0196] In some embodiments, the nanoparticles further comprise manganese.

[0197] In some embodiments, the conductive carbon matrix comprises a carbonized organogel as described herein.

[0198] III. Method for forming lithium vanadium fluorophosphate cathode material within a conductive carbon matrix; fluorophosphate ion In another aspect of the present disclosure, a method for preparing a lithium vanadium fluorophosphate cathode material in a conductive carbon matrix is ​​provided. The method comprises: 4 2- The process is substantially similar to the process for forming the lithium transition metal phosphate cathode material described hereinabove, except that vanadium oxide is selected as the transition metal oxide. Each of the mixing, lithium ion source, organogel precursor material, gelling, solid organogel, and thermal decomposition thereof are as described hereinabove.

[0199] Vanadium oxide is vanadium(III) oxide (V 2 O 3 ), vanadium(IV) oxide (VO 2 ), vanadium(V) oxide(V 2 O5 ), or ammonium metavanadate (NH 4 VO 3 The oxide may be any readily available oxide of vanadium, such as

[0200] The fluorophosphate ion source may vary. For example, fluorophosphoric acid or a fluorophosphate salt, such as sodium monofluorophosphate or ammonium monofluorophosphate, may be utilized to provide the fluorophosphate ion. Alternatively, the fluorophosphate ion may be formed in situ from a lithium ion source, a phosphate ion source, and a fluoride ion source. The lithium, phosphate, and fluoride sources may be individual or may be provided in various combinations. For example, the method may utilize a lithium source as described herein above, along with separate sources of fluoride and phosphate, such as hydrofluoric acid or ammonium fluoride, and phosphoric acid, or an alkali metal or ammonium salt of phosphoric acid. Alternatively, the method may utilize a combined source of lithium and fluoride, such as lithium fluoride. Those skilled in the art will recognize the various combinations of lithium, fluoride, and phosphate that may be utilized to provide lithium and fluorophosphate ion in the reaction mixture, and all such combinations are contemplated herein. The order of addition of any such components (such as the source of lithium ions, the source of fluoride and phosphate ions, the source of fluorophosphate, etc.) may vary and may be sequential or simultaneous.

[0201] Following pyrolysis, the lithium vanadium fluorophosphate cathode material in a conductive carbon matrix has the formula LiVFPO 4 The resulting cathode material may optionally be ground as described above for the lithium transition metal phosphate material.

[0202] IV. Method for forming lithium vanadium fluorophosphate cathode material within a conductive carbon matrix; F - Fluoropolymers as a source In another aspect of the present disclosure, an alternative method is provided for preparing a lithium vanadium fluorophosphate cathode material in a conductive carbon matrix. The method is substantially similar to the method for forming the lithium vanadium fluorophosphate cathode material described hereinabove, except that the fluorophosphate ion source is replaced by phosphoric acid and the fluoride is provided in the form of a fluoropolymer. Each of the mixing, lithium ion source, organogel precursor material, gelling, solid organogel, and pyrolysis thereof are as described hereinabove. The method further includes adding a fluoropolymer to the precursor mixture prior to gelling.

[0203] Vanadium oxide is vanadium(III) oxide (V 2 O 3 ), vanadium(IV) oxide (VO 2 ), vanadium(V) oxide(V 2 O 5 ), or ammonium metavanadate (NH 4 VO 3 The oxide may be any readily available oxide of vanadium, such as

[0204] Examples of suitable fluoropolymers include, but are not limited to, polytetrafluoroethylene, polyvinylidene fluoride, and combinations thereof. Without wishing to be bound by theory, it is believed that such fluoropolymers are not chemically incorporated into the organogel polymer, but rather are physically incorporated (e.g., as a physical combination) into the organogel matrix, and then during pyrolysis, the fluoropolymer decomposes, liberating fluorine species that react with phosphate ions to form fluorophosphate salts in situ and / or react directly with vanadium oxide species to form the final intermediate species, with the fluorine in the intermediate coordinating with the vanadium. Such an alternative method is the formation of fluorophosphate (H 2 FPO 3 This addresses potential issues with fluorophosphate sources such as fluorophosphate, which is slowly converted to H 3 PO 4and hydrogen fluoride (HF). HF is volatile and toxic and can escape from the reaction mixture when dried, making it difficult to maintain the required 1:1:1:1 lithium:vanadium:phosphate:fluorine stoichiometry. The methods disclosed herein that use fluoropolymers avoid the need to use fluorophosphoric acid.

[0205] V. Method for Forming Lithium Vanadium Fluorophosphate Cathode Materials Within a Conductive Carbon Matrix; Fluoromonomers In another aspect of the present disclosure, a further alternative method is provided for preparing a lithium vanadium fluorophosphate cathode material within a conductive carbon matrix, the method being substantially similar to the method for forming a lithium vanadium fluorophosphate cathode material using a fluoropolymer described hereinabove, except that the fluoropolymer is replaced with a fluoromonomer, which is copolymerized with an organogel precursor material to form an organogel in which at least a portion of the hydrogen atom substituents are replaced with fluorine atoms.

[0206] Similar to the method for preparing lithium vanadium fluorophosphate cathode materials in a conductive carbon matrix using fluoropolymers disclosed above, this alternative method uses fluorinated monomers that are chemically incorporated into the organogel polymer. By "at least a portion of one or more organogel precursor materials includes fluorinated monomers" it is meant that a quantity of one or more organogel precursor materials is fluorinated. The amount of fluorinated monomer present as an organogel precursor material can vary, for example, from about 1% to about 100% of the total amount of organogel precursor material utilized. Furthermore, the degree of fluorination within the monomer (i.e., the number of fluorine substituents present on a given organogel precursor monomer structure) can vary. In some embodiments, the organogel is a polyimide, and some portion of the polyimide organogel precursor material (e.g., diamines and tetracarboxylic dianhydrides, or polyamic acids) bear one or more fluorine substituents. In some embodiments, the polyimide is formed in situ from organogel precursor materials that are phenylenediamines and tetracarboxylic dianhydrides, where the phenylenediamine, tetracarboxylic dianhydride, or both, carry one or more fluorine substituents. In certain embodiments, the fluorinated monomer is a 1,4-phenylenediamine carrying one or more fluorine atoms, such as 2,3,5,6-tetrafluorobenzene-1,4-diamine. Again, utilizing an organogel precursor material carrying fluoro substituents as the fluoride source avoids the loss of volatile and toxic HF gas during the initial stages of solvent evaporation and initial drying.

[0207] VI. Energy Storage Systems In another aspect of the present disclosure, an energy storage system is provided that includes the lithium transition metal phosphate cathode material described herein. In another aspect of the present disclosure, a composition is provided that includes nanoparticles that include olivine-type lithium iron phosphate and are integral with a conductive carbon matrix, the nanoparticles having a characteristic dimension of 20 nm to 1000 nm and a characteristic length of 10 meters. 2 (m 2 ) / gram(g)~65m 2An energy storage system is provided that includes a composition having a specific surface area of ​​100 nm to 150 nm / g.

[0208] Examples of energy storage systems include batteries, such as lithium ion batteries, that include the compositions or cathode materials described herein. Also disclosed herein are battery cells, battery modules, battery packs, electronic devices, and electric vehicles that include the compositions or cathode materials described herein.

[0209] In this application, certain U.S. patents, U.S. patent applications, and other materials (e.g., articles) are incorporated by reference. However, the text of such U.S. patents, U.S. patent applications, and other materials is incorporated by reference only to the extent that there is no conflict between such text and other descriptions and drawings set forth herein. In the event of such a conflict, any such conflicting text in the U.S. patents, U.S. patent applications, and other materials so incorporated by reference is not specifically incorporated by reference into this patent. Protection may be sought for any features disclosed in any one or more published documents referenced herein in combination with the present disclosure. All methods described herein may be performed in any suitable order unless otherwise indicated herein or otherwise clearly contradicted by context. The use of any and all examples or exemplary language (e.g., "etc.") provided herein is intended only to better describe the materials and methods and does not impose limitations on the scope unless otherwise claimed. No language in this specification should be construed as indicating any unclaimed element is essential to the practice of the disclosed materials and methods.

[0210] It will be readily apparent to those skilled in the relevant art that suitable modifications and adaptations to the compositions, methods, and applications described herein can be made without departing from the scope or aspects of any of them. The compositions and methods provided are exemplary and are not intended to limit the scope of the claimed aspects. All of the various aspects and options disclosed herein can be combined in all variations. The scope of the compositions, formulations, methods, and processes described herein includes all actual or potential combinations of the aspects, options, examples, and preferences herein.

[0211] Although the technology herein has been described with reference to specific embodiments, it is to be understood that these embodiments are merely illustrative of the principles and applications of the technology. It will be apparent to those skilled in the art that various modifications and variations can be made to the method and apparatus of the technology without departing from the spirit and scope of the technology. Thus, the technology is intended to cover modifications and variations that come within the scope of the appended claims and their equivalents.

[0212] Reference throughout this specification to "one aspect," "a particular aspect," "one or more aspects," or "an aspect" means that a particular feature, structure, material, or characteristic described in connection with the aspect is included in at least one aspect of the technology. Thus, the appearance of phrases such as "in one or more aspects," "in a particular aspect," "in one aspect," or "in an aspect" in various places throughout this specification does not necessarily refer to the same aspect of the technology. Furthermore, particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more aspects. The invention also broadly defines that the components, elements, steps, examples, and / or features referred to or shown herein individually or collectively may consist of any and all combinations of two or more of such components, elements, steps, examples, and / or features. In particular, one or more features in any of the aspects, examples, and embodiments described herein may be combined with one or more features from any other examples and embodiments described herein.

[0213] Aspects of the present technology are illustrated more fully with reference to the following examples. Before describing some exemplary aspects of the present technology, it is to be understood that the present technology is not limited to the details of configuration or process steps set forth in the following description. The present technology is capable of other embodiments and of being practiced or carried out in various ways.

[0214] Further modifications and alternative embodiments of the present invention will be apparent to those skilled in the art in view of this description. Thus, this description should be construed as merely illustrative and for the purpose of teaching those skilled in the art the general manner of carrying out the present invention. It is to be understood that the forms of the present invention shown and described herein are to be construed as exemplary embodiments. Elements and materials may be substituted for those illustrated and described herein, parts and processes may be reversed, and certain features of the present invention may be utilized independently, all as would become apparent to those skilled in the art after having the benefit of this description of the invention. Changes may be made to the elements described herein without departing from the spirit and scope of the present invention as set forth in the following claims.

[0215] Although certain exemplary aspects of the present invention have been described, the appended claims are not intended to be limited to only those aspects, and the claims are intended to be interpreted literally, intentionally, and / or to encompass equivalents.

[0216] The following examples are provided to illustrate certain aspects of the present technology and are not to be construed as limiting thereof. EXAMPLES

[0217] The present invention may be further illustrated by the following non-limiting examples which describe methods.

[0218] Example 1: Lithium iron phosphate (Fe) in a carbon matrix 2 O 3 Synthesis of furfuralaldehyde (phloroglucinol / furfuralaldehyde). Iron(III) oxide (Fe 2 O 3A sample of lithium iron phosphate in a carbon matrix was prepared using phloroglucinol-furfuralaldehyde polymer as the carbon source and iron(III) oxide (2.8 g, 13 mmol, particle size .about.5 microns) was added to deionized water (10 ml) and the suspension was stirred at room temperature for 5 min. Phosphoric acid (85% H 3 PO 4 2 ml, 26 mmol) was added and the suspension was stirred for 2 hours. 2 CO 3 0.96 g, 13 mmol) was added and the resulting suspension was stirred until carbon dioxide evolution ceased. In a separate container, phloroglucinol (1.68 g) was dissolved in 10 ml of ethanol. Furfuralaldehyde (1.68 ml) was added to the phloroglucinol solution and the solution was mixed for 5 minutes. After mixing, the solution was added all at once to the iron oxide / lithium / phosphate suspension. The suspension was stirred overnight at room temperature resulting in a viscous mixture. The solvents (ethanol and water) were evaporated by stirring at 100° C. A homogeneous dry powder was obtained, which was pyrolyzed under nitrogen using the temperature gradient provided in Table 2 to provide powdered lithium iron phosphate within a carbon matrix. [Table 2]

[0219] A sample of powdered lithium iron phosphate in a carbon matrix was analyzed by scanning electron microscopy. Micrographs at two magnifications (1,490x and 5,050x) are provided as Figures 7A and 7B, respectively. With reference to Figures 7A and 7B, the lithium iron phosphate is formed as primary particles with sizes ranging from submicron to several microns. The primary particles aggregate into secondary particles with diameters of tens of microns and are connected to each other through the carbon matrix. The sample was also subjected to powder X-ray diffraction (XRD) analysis, which revealed that the main phase of the material is olivine-type LiFePO 4 It was demonstrated that the zeolite was accompanied by a minor phase containing an unidentified impurity (FIG. 8).

[0220] Example 2: Lithium iron phosphate (Fe(OH)) in a carbon matrix3 / phloroglucinol / furfuralaldehyde) synthesis Iron(III) hydroxide (Fe(OH) 3 A sample of lithium iron phosphate in a carbon matrix was prepared using phosphate buffer, phosphate buffer, and phloroglucinol-furfuralaldehyde polymer as the carbon source. Iron(III) nitrate hydrate (Fe(NO 3 )-3.9H 2 Iron(III) hydroxide was prepared by dissolving 1.2 g (3.50 g, 8.7 mmol) of sodium hydroxide in deionized water (30 ml). To this solution was added a solution of sodium hydroxide (2.1 g; 52.5 mmol) in deionized water (15 ml), resulting in the instantaneous formation of an aqueous suspension of iron(III) hydroxide gel. The iron hydroxide gel was aged overnight in the mother liquor, then isolated and purified by cycles of centrifugation and resuspension in deionized water (total of 5 cycles). Phosphoric acid (85% H 3 PO 4 0.7ml, 8.7mmol), followed by lithium carbonate (Li 2 CO 3 0.32 g, 4.3 mmol) was added and the resulting suspension was stirred until carbon dioxide evolution ceased. In a separate vessel, phloroglucinol (1.05 g) was dissolved in 4 ml of ethanol. Furfuralaldehyde (0.57 ml) was added to the phloroglucinol solution and the solution was mixed for 5 minutes. After mixing, the solution was added all at once to the iron hydroxide / lithium / phosphate suspension. The suspension was stirred overnight at room temperature, resulting in a viscous mixture. The solvents (ethanol and water) were evaporated by stirring at 100° C. A homogeneous dry powder was obtained, which was pyrolyzed under nitrogen using the protocol described in Example 1 to provide lithium iron phosphate in a carbon matrix.

[0221] A sample of powdered lithium iron phosphate in a carbon matrix was analyzed by scanning electron microscopy. Micrographs at two magnifications (10,000x and 49,900x) are provided as Figures 9A and 9B, respectively. With reference to Figures 9A and 9B, the LFP was formed as fine crystalline matter with diameters of about 100 nm to about 1 micron, uniformly dispersed within the conductive carbon network. The secondary particle aggregates ranged in size from about 1 micron to several microns, and had an open framework structure that allowed electrolyte penetration. The sample was also subjected to powder X-ray diffraction (XRD) analysis, which revealed that the main phase of the material was olivine-type LiFePO 4 It was demonstrated that the iron impurity phase is approximately 2% with a minor phase containing approximately 2% iron (Figure 10). The iron impurity phase can be separated by magnetism or can be utilized as a ferromagnetic agent to increase the packing density of the particles in the cathode film, for example, during magnetic electrode film casting.

[0222] Example 3: Lithium iron phosphate (Fe(OH)) in a carbon matrix 3 / phloroglucinol / furfuralaldehyde) synthesis To evaluate the effect of residual carbon on particle size distribution and impurity profile, a second sample of lithium iron phosphate in a carbon matrix was prepared following the procedure of Example 2 but using twice the ratio of PF precursor to LFP precursor.

[0223] A sample of powdered lithium iron phosphate in a carbon matrix was analyzed by scanning electron microscopy at two magnifications (10,000x and 100,000x). Micrographs at each magnification are provided as Figures 11A and 11B, respectively. With reference to Figures 11A and 11B, the LFP was formed as fine crystalline material with diameters of about 100 nm to about 1 micron, uniformly dispersed within the conductive carbon network. The secondary particle aggregates ranged in size from about 1 micron to several microns, and had an open framework structure that allowed electrolyte penetration. The sample was also subjected to powder X-ray diffraction (XRD) analysis, which revealed that the primary phase of the material was olivine-type LiFePO 4It was demonstrated that the iron impurity phase is approximately 3% with a minor phase containing approximately 3% iron (FIG. 12). The iron impurity phase can be separated by magnetism or can be utilized as a ferromagnetic agent, for example, to increase the packing density of the particles in the cathode film during magnetic electrode film casting.

[0224] Example 4: Lithium iron phosphate (Fe) in a carbon matrix 2 O 3 Synthesis of PAA / Pyromellitic dianhydride / 1,4-phenylenediamine (PAA / Low PI gel) Iron(III) oxide (Fe 2 O 3 A sample of lithium iron phosphate in a carbon matrix was prepared using 10.38 g (65 mmol) of iron(III) oxide in deionized water (50 ml) and polyimide gel as the carbon source. The suspension was stirred at room temperature for 5 min. Phosphoric acid (85% H 3 PO 4 10 ml, 130 mmol) was added and the suspension was stirred for 2 hours. 2 CO 3 ;5.05 g, 68.2 mmol) was added and the resulting suspension was stirred until carbon dioxide evolution ceased. In a separate container, 1,4-phenylenediamine (PDA;2.0 g), pyromellitic dianhydride (PMDA;6.8 g), and triethylamine (9.3 ml) were added to deionized water (100 ml). The mixture was allowed to react overnight to form a polyamic acid triethylammonium salt solution. Acetic anhydride (11.3 ml) was added to this solution to initiate imidization. After mixing for 1 minute, the gelling solution was added in one portion to the iron suspension. The resulting reaction mixture was loosely capped and heated with stirring at 100 °C for 24 hours. During this time, the solvent evaporated and a homogeneous dry powder was obtained. The organic matrix consisted of a mixture of polyimide and polyamic acid enriched in polyamic acid. This dry powder was pyrolyzed using the protocol described in Example 1 to provide lithium iron phosphate within a carbon matrix.

[0225] A sample of powdered lithium iron phosphate in a carbon matrix was analyzed by scanning electron microscopy. Micrographs at two magnifications (2,000x and 20,000x) are provided as Figures 13A and 13B, respectively. With reference to Figures 13A and 13B, the LFP formed as agglomerates of submicron primary particles held together by a conductive carbon network into secondary particles approximately 10 microns in diameter. The sample was also subjected to powder X-ray diffraction (XRD) analysis, which revealed that the primary phase of the material was olivine-type LiFePO 4 It was demonstrated that the zeolite was oxidized to a zeolite with a minor phase containing an unidentified impurity (FIG. 14).

[0226] Example 5: Lithium iron phosphate (Fe) in a carbon matrix 2 O 3 Synthesis of PAA / Pyromellitic dianhydride / 1,4-phenylenediamine (PAA / Low PI gel) Iron(III) oxide (Fe 2 O 3 A sample of lithium iron phosphate in a carbon matrix was prepared using polyamic acid as the carbon source and iron(III) oxide (10.38 g, 65 mmol) was added to deionized water (50 ml) and the suspension was stirred at room temperature for 5 min. Phosphoric acid (85% H 3 PO 4 10 ml, 130 mmol) was added and the suspension was stirred for 2 hours. 2 CO 3;5.05 g, 68.2 mmol) was added and the resulting suspension was stirred until carbon dioxide evolution ceased. In a separate container, 1,4-phenylenediamine (PDA;2.0 g), pyromellitic dianhydride (PMDA;6.8 g), and triethylamine (9.3 ml) were added to deionized water (100 ml). The mixture was allowed to react overnight to form a polyamic acid triethylammonium salt solution. The gel precursor mixture was then added to the iron oxide suspension, followed immediately by acetic anhydride (11.3 ml). The resulting reaction mixture was loosely capped and heated with stirring at 100°C for 24 hours. During this time, the solvent evaporated and a homogeneous dry powder was obtained. The organic matrix consisted primarily of polyamic acid with a small amount of polyimide. Without wishing to be bound by theory, it is believed that the acidic environment caused hydrolysis of acetic anhydride to acetic acid and gelation of the insoluble polyamic acid with minimal imidization occurring. This dry powder was pyrolyzed using the protocol described in Example 1 to provide lithium iron phosphate within a carbon matrix.

[0227] A sample of powdered lithium iron phosphate in a carbon matrix was analyzed by scanning electron microscopy. Micrographs at two magnifications (2,000x and 50,000x) are provided as Figures 15A and 15B, respectively. With reference to Figures 15A and 15B, the LFP forms as agglomerates of uniform 2 micron primary particles that assemble into 10 micron secondary particles within a porous network that is permeable to the electrolyte. The sample was also subjected to powder X-ray diffraction (XRD) analysis, which revealed that the primary phase of the material is olivine LiFePO 4 It was demonstrated that the zeolite was oxidized to a zeolite with a minor phase containing an unidentified impurity (FIG. 16).

[0228] Example 6: Lithium iron phosphate (Fe) in a carbon matrix 2 O 3 Synthesis of PAA / Pyromellitic Dianhydride / 1,4-Phenylenediamine (PAA / Medium PI Gel) Iron(III) oxide (Fe 2 O 3A sample of lithium iron phosphate in a carbon matrix was prepared using polyamic acid as the carbon source and iron(III) oxide (10.38 g, 65 mmol) was added to deionized water (50 ml) and the suspension was stirred at room temperature for 5 min. Phosphoric acid (85% H 3 PO 4 10 ml, 130 mmol) was added and the suspension was stirred for 2 hours. 2 CO 3 ;5.05 g, 68.2 mmol) was added and the resulting suspension was stirred until carbon dioxide evolution ceased. In a separate container, 1,4-phenylenediamine (PDA;2.0 g), pyromellitic dianhydride (PMDA;6.8 g), and triethylamine (9.3 ml) were added to deionized water (100 ml). The mixture was allowed to react overnight to form a polyamic acid triethylammonium salt solution. Triethylamine (approximately 20 mL) was added to the iron oxide suspension to raise the pH to approximately 8.0 (from an initial 4.0). The gel precursor solution was then added all at once to the iron oxide suspension, followed by acetic anhydride (11.3 mL) to initiate chemical imidization. The resulting reaction mixture was loosely capped and heated with stirring at 100 °C for 24 h. During this time, the solvent evaporated and a homogeneous dry powder was obtained. The organic matrix consisted primarily of polyamic acid along with some polyimide. Without wishing to be bound by theory, it is believed that the relatively neutral environment resulted in increased imidization / gelation of the polyamic acid salt compared to Examples 4 and 5. This dry powder was pyrolyzed using the protocol described in Example 1 to provide lithium iron phosphate within a carbon matrix.

[0229] A sample of the product was subjected to powder X-ray diffraction (XRD) analysis, which confirmed that the material was LiFePO 4 (less than 70% by weight), unreacted Li 3 PO 4(about 30% by weight) mixture with the remainder being Fe (FIG. 17). This example surprisingly shows that at higher PI / PAA ratios in the organogel, a significant portion of the unreacted reagents is present in the final product. Without wishing to be bound by theory, it is believed that the rigid polyimide gel results in less efficient contact between the LFP precursors, resulting in less homogeneity of the reaction and lower product yields.

[0230] Example 7: Raman spectroscopy of carbon matrices The electronic structure of the in situ formed carbon of Examples 1-7 is evaluated by Raman spectroscopy. Without wishing to be bound by theory, it is believed that the carbon matrix formed according to the disclosed methods can be more conductive than particulate carbon added to lithium metal phosphate cathode materials.

[0231] Example 8: Analysis of carbon nanostructures The nanostructure of the carbon matrix of the cathode materials formed in Examples 1-7 is evaluated by dissolving the lithium metal phosphate from the carbon matrix. The remaining carbon material is analyzed to determine porosity, pore size, and carbon strut size. Specifically, He pycnometry, as well as N 2 The He true density is determined by surface and pore structure via adsorption isotherms. Mid- and long-term microstructural analysis is performed by SEM, TEM, Raman, and X-ray scattering. Also, elemental analysis of CHN is performed.

Claims

1. 1. A method for preparing a lithium transition metal phosphate cathode material in a conductive carbon matrix, the method comprising: combining a group of precursors for synthesizing the lithium transition metal phosphate cathode material, wherein at least a first precursor of the group includes a solid phase having a first density greater than 1 gram (g) per cubic centimeter (cc) and at least a second precursor of the group includes a liquid phase having a second density, the second density being less than the first density; providing one or more carbon precursors in a fluid state, the one or more carbon precursors configured to form a solid organogel in the presence of a gelation initiator, the solid organogel configured to form a conductive carbon matrix upon pyrolysis; mixing the group of precursors with the one or more carbon precursors to form a precursor mixture; adding said gelation initiator to said precursor mixture; allowing the one or more carbon precursors to undergo gelation to form the solid organogel; and pyrolyzing the solid organogel to form the lithium transition metal phosphate cathode material within the conductive carbon matrix.

2. 10. The method of claim 1, wherein the solid organogel is formed within 5 seconds to 15 minutes after addition of the gelation initiator.

3. 10. The method of claim 1, wherein the solid organogel comprises a porous network of interconnected solid-state polymeric structures.

4. The method of claim 3 , wherein the porous network maintains contact between the first precursor of the group and the second precursor of the group.

5. The method of claim 4 , wherein the contacting is maintained at a temperature of at least about 300° C.

6. the first precursor comprises iron; the second precursor comprises a lithium source and phosphoric acid; The method of claim 1 , wherein the lithium transition metal phosphate cathode material is lithium iron phosphate.

7. The iron may be an iron (II) salt, an iron (III) salt, iron (II) oxide (FeO), iron (III) oxide (Fe 2 O 3 ), mixed iron oxide (Fe 3 O 4 ), or a combination thereof.

8. 2. The method of claim 1, wherein the solid organogel comprises a phloroglucinol-furfural polymer or a resorcinol-furfural polymer and the one or more carbon precursors are phloroglucinol or resorcinol and furfural.

9. The method of claim 8, wherein the gelation initiator is an amine base or an acid.

10. The method of claim 1 , wherein the solid organogel comprises a polyurethane polymer and the one or more carbon precursors comprise a polyol and an isocyanate.

11. The method of claim 10 , wherein the gelation initiator comprises an alkyl amine.

12. 10. The method of claim 1, wherein the organogel comprises a polyamic acid polymer and the gelation initiator comprises acetic anhydride, acetic acid, or a combination thereof.

13. 10. The method of claim 1, wherein the group of precursors comprises a microwave-sensitive precursor and the pyrolyzing is carried out by applying microwave radiation.

14. 14. The method of claim 13, wherein the microwave-sensitive precursor comprises one or more of carbon, magnetite, and maghemite.

15. 15. The method of claim 14, comprising nanoparticles of one or more of magnetite and maghemite having a characteristic dimension between 20 nm and 100 nm.

16. the first precursor comprises manganese, vanadium, or both; the second precursor comprises a lithium source and phosphoric acid; 2. The method of claim 1, wherein the lithium transition metal phosphate cathode material is a lithium manganese phosphate or a lithium vanadium phosphate.

17. 10. The method of claim 1, further comprising drying the lithium transition metal phosphate cathode material by applying microwave radiation.

18. 2. The method of claim 1, wherein the solid phase having the first density greater than 1 gram comprises a ferromagnetic iron compound, a ferrimagnetic iron compound, or both.

19. the ferromagnetic iron compound, the ferrimagnetic iron compound, or both; The iron-containing anode is synthesized by a method comprising oxidizing an iron-containing anode in an electrochemical cell comprising a porous carbon substrate, an oxygen cathode, and an electrolyte in contact with both the iron-containing anode and the porous carbon substrate; 20. The method of claim 18, wherein the oxidizing produces particles of the ferromagnetic iron compound, the ferrimagnetic iron compound, or both, having a characteristic dimension between 20 nm and 100 nm.

20. 20. The method of claim 19, further comprising removing the particles by magnetic filtration.

21. 20. The method of claim 19, further comprising drying the particles by applying microwave radiation.

22. 20. The method of claim 19, wherein the operation of the electrochemical cell and the formation of the ferromagnetic iron compound, the ferromagnetic iron compound, or both, is performed at a temperature between 15°C and 35°C.

23. 13. A lithium transition metal phosphate cathode material prepared by the method of claim 1.

24. 13. An energy storage system comprising a lithium transition metal phosphate cathode material prepared by the method of claim 1.

25. A composition comprising nanoparticles comprising olivine-type lithium iron phosphate and integral with a conductive carbon matrix, said nanoparticles having a characteristic dimension between 20 nm and 1000 nm and a characteristic dimension between 10 meters and 100 meters. 2 (m 2 ) / gram (g) ~ 65m 2 The composition has a specific surface area of ​​100 / g.

26. The characteristic dimension is between 30 nm and 70 nm, and the specific surface area is between 20 m 2 / g ~ 65m 2 / g.

27. The characteristic dimension is between 30 nm and 60 nm, and the specific surface area is 22 m 2 / g to 40m 2 / g.

28. The characteristic dimension is between 20 nm and 40 nm, and the specific surface area is 60 m 2 / g ~ 80m 2 / g.

29. 26. The composition of claim 25, wherein the nanoparticles further comprise magnetite, maghemite, or both.

30. 26. The composition of claim 25, wherein the nanoparticles further comprise manganese.

31. 26. The composition of claim 25, wherein the conductive carbon matrix comprises a carbonized organogel polymer matrix.

32. 26. An energy storage system comprising the composition of claim 25.

Citation Information

Patent Citations

  • Carbon aerogel network lithium manganese ferric phosphate battery electrode material and preparation method

    CN106887586A

  • Manufacturing method of lithium battery electrode, lithium battery electrode, and lithium battery

    JP2005183032A

  • Electrode material for secondary battery, method for producing electrode material for secondary battery, and secondary battery

    WO2012133566A1