Saturated phlodioxin derivative compound and its use as an additive for secondary batteries

The introduction of a saturated flodioxin derivative compound in the non-aqueous electrolyte composition for lithium-sulfur secondary batteries addresses the issue of lithium polysulfide elution, stabilizing electrodes and improving capacity retention and battery life.

JP2024537169AActive Publication Date: 2024-10-10SAMYANG CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024520860
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-06
Filing Date
2022-10-05
Publication Date
2024-10-10
Estimated Expiration
2042-10-05

AI Technical Summary

Technical Problem

Conventional lithium-sulfur secondary batteries suffer from the issue of lithium polysulfide elution, which leads to capacity loss, decreased ionic conductivity, and reduced electrode stability due to the diffusion of lithium polysulfide to the negative electrode, limiting their practical application to 70% of theoretical capacity.

Method used

A non-aqueous electrolyte composition for lithium-sulfur secondary batteries is developed, incorporating a saturated flodioxin derivative compound as an additive, produced through specific chemical reactions involving dianhydrosaccharide hexitol-ethylene glycol or alkylating agents, to stabilize the lithium electrode and enhance capacity retention.

Benefits of technology

The use of the flodioxin derivative compound significantly improves the stability of lithium electrodes, enhances capacity retention, and extends the battery life, achieving over 90% capacity retention rate in lithium-sulfur secondary batteries.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a saturated phlodioxine derivative compound and its use as an additive for secondary batteries. More specifically, the present invention relates to a novel compound having a structure in which a substituent is bonded to a saturated phlodioxine skeleton, which, when contained as an additive in a nonaqueous electrolyte composition for secondary batteries (particularly, a nonaqueous electrolyte composition for lithium-sulfur secondary batteries), can solve the problem of lithium polysulfide elution that exists in conventional electrolyte compositions and at the same time realize high capacity retention characteristics for various lithium salts, as well as a method for producing the compound, an electrolyte additive and nonaqueous electrolyte composition containing the compound, and a secondary battery (particularly, a lithium-sulfur secondary battery) containing the electrolyte composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a saturated phlodioxine derivative compound and its use as an additive for secondary batteries. More specifically, the present invention relates to a novel compound having a structure in which a substituent is bonded to a saturated phlodioxine skeleton, which, when contained as an additive in a nonaqueous electrolyte composition for secondary batteries (particularly, a nonaqueous electrolyte composition for lithium-sulfur secondary batteries), can solve the problem of lithium polysulfide elution that is present in conventional electrolyte compositions and at the same time realize high capacity retention characteristics for various lithium salts, as well as a method for producing the compound, an electrolyte additive and nonaqueous electrolyte composition containing the compound, and a secondary battery (particularly, a lithium-sulfur secondary battery) containing the electrolyte composition. [Background technology]

[0002] In recent years, the need for large-capacity batteries has increased with the development of portable electronic devices, electric vehicles, and large-capacity power storage systems. Lithium-sulfur secondary batteries are secondary batteries that use sulfur-based materials with S-S bonds (sulfur-sulfur bonds) as the positive electrode active material and lithium metal as the negative electrode active material. Sulfur, the main material of the positive electrode active material, has the advantages of being highly resourceful, non-toxic, and light in weight per atom.

[0003] In addition, the theoretical discharge capacity of the lithium-sulfur secondary battery is 1,672 mAh / g-sulfur, and the theoretical energy density is 2,600 Wh / kg, which are extremely higher than the theoretical energy densities of other battery systems currently being researched (Ni-MH battery: 450 Wh / kg, Li-FeS battery: 480 Wh / kg, Li-MnO2 battery: 1,000 Wh / kg, Na-S battery: 800 Wh / kg), and it is attracting attention as a battery with high energy density characteristics.

[0004] The most important problem to be solved for the practical use of lithium-sulfur secondary batteries is the decrease in battery life due to the elution of lithium polysulfide. x, x=8, 6, 4 or 2) is an intermediate product generated during the electrochemical reaction of lithium-sulfur secondary batteries, and has high solubility in organic electrolytes. Lithium polysulfide dissolved in the electrolyte gradually diffuses to the negative electrode and leaks out of the electrochemical reaction area of ​​the positive electrode, making it unable to participate in the electrochemical reaction of the positive electrode, ultimately resulting in capacity loss. In addition, the dissolution of lithium polysulfide increases the viscosity of the electrolyte, reducing ionic conductivity, and during continuous charge-discharge reactions, lithium polysulfide reacts with the negative electrode made of lithium metal material, causing lithium sulfide (Li2S) to adhere to the surface of the lithium metal, reducing reaction activity and potential characteristics.

[0005] Most of the research to solve these problems focuses on improving the positive electrode. Specifically, as a method for increasing the conductivity of the electrode, attempts have been made to minimize the decrease in conductivity of the electrode in which lithium sulfide has accumulated by adding a conductive material made of a carbon material, or to control the generation and accumulation of intermediate products and lithium sulfide by using a sulfur support having a nanostructure (e.g., Patent Documents 1 and 2).

[0006] However, the above-mentioned conventional technologies are difficult to put into practical use, and only up to 70% of the theoretical capacity can be used. Therefore, there is a need to develop a lithium-sulfur secondary battery that can delay the passivation of the electrodes by lithium sulfide and ensure high discharge capacity and life characteristics. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Korean Patent No. 10-1481234 [Patent Document 2] Korean Patent No. 10-2244915 Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a novel compound which, when incorporated as an additive in a nonaqueous electrolyte composition for a secondary battery (particularly a nonaqueous electrolyte composition for a lithium-sulfur secondary battery), can solve the problem of lithium polysulfide elution in conventional nonaqueous electrolytes used in secondary batteries (particularly lithium-sulfur secondary batteries), while improving the stability of lithium electrodes and achieving high capacity retention characteristics; a method for producing the compound; an electrolyte additive and nonaqueous electrolyte composition containing the compound; and a secondary battery (particularly a lithium-sulfur secondary battery) containing the electrolyte composition. [Means for solving the problem]

[0009] The present invention provides a compound represented by the following formula (1):

[0010] [ka] (In the formula, R1 and R2 are each independently selected from the group consisting of a hydrogen atom, a halogen atom, a substituted or unsubstituted C1-C30 alkyl group, a substituted or unsubstituted C2-C30 alkenyl group, a substituted or unsubstituted C2-C30 alkynyl group, a substituted or unsubstituted C1-C30 alkoxy group, a substituted or unsubstituted C3-C30 cycloalkyl group, a substituted or unsubstituted C1-C30 alkylene-O-C1-C30 alkyl group, a substituted or unsubstituted C3-C30 heterocycloalkyl group, a substituted or unsubstituted C6-C60 aryl group, a substituted or unsubstituted C1-C60 heteroaryl group, a substituted or unsubstituted C7-C60 aralkyl group, a substituted or unsubstituted C6-C60 aryloxy group, and a substituted or unsubstituted C6-C60 arylthio group, with the proviso that at least one of R1 and R2 is not a hydrogen atom.)

[0011] In one embodiment of the present invention, the compound represented by formula (1) may be selected from the group consisting of compounds represented by the following formulas (2) to (4).

[0012] [ka] [ka] [ka] (In the formula, R3 and R4 are each independently a substituted or unsubstituted C1-C30 alkyl group.)

[0013] More specifically, the compound represented by formula (2) may be selected from the group consisting of compounds represented by the following formulas (2-1) to (2-3): The compound represented by formula (3) is represented by the following formula (3-1) or (3-2): The compound represented by the formula (4) may be represented by the following formula (4-1) or (4-2).

[0014] [ka] [ka] [ka]

[0015] [ka] [ka]

[0016] [ka] [ka]

[0017] Another aspect of the present invention provides a method for producing a compound represented by formula (2), comprising the step of heating dianhydrosugar hexitol-ethylene glycol, a compound in which ethylene glycol is added to both terminal hydroxy groups of a dianhydrosugar hexitol, in the presence of an acid catalyst.

[0018] Yet another aspect of the present invention provides a method for producing a compound represented by the above formula (3) or (4), comprising the step of heating a compound represented by the following formula (A) or (B), respectively, and an alkylating agent in the presence of a base catalyst:

[0019] [ka] [ka]

[0020] Yet another aspect of the present invention provides an electrolyte additive comprising the compound represented by formula (1).

[0021] Yet another aspect of the present invention provides a non-aqueous electrolyte composition comprising: a non-aqueous electrolyte solvent; a lithium salt; and an electrolyte additive of the present invention, wherein the content of the electrolyte additive is 0.1 to 10 parts by weight, based on 100 parts by weight of a total amount of the electrolyte composition.

[0022] Yet another aspect of the present invention provides a secondary battery comprising: a positive electrode; a negative electrode; a separator; and the nonaqueous electrolyte composition of the present invention. Effect of the Invention

[0023] When the compound of formula (1) according to the present invention is used as an electrolyte additive in a non-aqueous electrolyte composition for a secondary battery (particularly, a non-aqueous electrolyte composition for a lithium-sulfur secondary battery), the problem of lithium polysulfide elution can be solved, and at the same time, the stability of the lithium electrode can be improved, and the capacity retention rate over cycles can be improved, thereby improving the battery life characteristics, as compared with conventional non-aqueous electrolyte compositions, and a secondary battery (particularly, a lithium-sulfur secondary battery) including the same can be provided.

[0024] According to one embodiment of the present invention, the compound of formula (1) can be produced from dianhydrosugar hexitol derived from natural resources. Therefore, by using the compound as an additive for secondary batteries, environmental friendliness in the field of secondary batteries can be improved. BEST MODE FOR CARRYING OUT THEINVENTION

[0025] The present invention will now be described in more detail.

[0026] [Compound of formula (1) and its production method] One aspect of the present invention relates to a compound represented by the following formula (1):

[0027] [ka] (In the formula, R1 and R2 are each independently selected from the group consisting of a hydrogen atom, a halogen atom, a substituted or unsubstituted C1-C30 alkyl group, a substituted or unsubstituted C2-C30 alkenyl group, a substituted or unsubstituted C2-C30 alkynyl group, a substituted or unsubstituted C1-C30 alkoxy group, a substituted or unsubstituted C3-C30 cycloalkyl group, a substituted or unsubstituted C1-C30 alkylene-O-C1-C30 alkyl group, a substituted or unsubstituted C3-C30 heterocycloalkyl group, a substituted or unsubstituted C6-C60 aryl group, a substituted or unsubstituted C1-C60 heteroaryl group, a substituted or unsubstituted C7-C60 aralkyl group, a substituted or unsubstituted C6-C60 aryloxy group, and a substituted or unsubstituted C6-C60 arylthio group, with the proviso that at least one of R1 and R2 is not a hydrogen atom.)

[0028] More specifically, in the formula (1), R1 and R2 are each independently selected from the group consisting of a hydrogen atom, a halogen atom, a substituted or unsubstituted C1-C12 alkyl group, a substituted or unsubstituted C2-C12 alkenyl group, a substituted or unsubstituted C2-C12 alkynyl group, a substituted or unsubstituted C1-C10 alkoxy group, a substituted or unsubstituted C3-C12 cycloalkyl group, a substituted or unsubstituted C1-C12 alkylene-O-C1-C12 alkyl group, a substituted or unsubstituted C3-C12 heterocycloalkyl group, a substituted or unsubstituted C6-C20 aryl group, a substituted or unsubstituted C1-C20 heteroaryl group, a substituted or unsubstituted C7-C20 aralkyl group, a substituted or unsubstituted C6-C20 aryloxy group, and a substituted or unsubstituted C6-C20 arylthio group, provided that at least one of R1 and R2 is not a hydrogen atom. More specifically, in the formula (1), R1 and R2 are each independently selected from the group consisting of a hydrogen atom, a halogen atom, a substituted or unsubstituted C1-C6 alkyl group, a substituted or unsubstituted C2-C6 alkenyl group, a substituted or unsubstituted C2-C6 alkynyl group, a substituted or unsubstituted C1-C6 alkoxy group, a substituted or unsubstituted C3-C6 cycloalkyl group, a substituted or unsubstituted C1-C6 alkylene-O-C1-C6 alkyl group, a substituted or unsubstituted C3-C6 heterocycloalkyl group, a substituted or unsubstituted C6-C10 aryl group, a substituted or unsubstituted C1-C10 heteroaryl group, a substituted or unsubstituted C7-C10 aralkyl group, a substituted or unsubstituted C6-C10 aryloxy group, and a substituted or unsubstituted C6-C10 arylthio group, provided that at least one of R1 and R2 is not a hydrogen atom.

[0029] In this specification, the term "substituted or unsubstituted" for any group means that the group is unsubstituted or substituted with one or more substituents selected from a halogen atom, a C1-C6 alkyl group, or a C1-C6 halogenated alkyl group.

[0030] In one embodiment, the compound represented by formula (1) may be selected from the group consisting of compounds represented by the following formulas (2) to (4).

[0031] [ka] [ka] [ka] (In the formula, R3 and R4 are each independently a substituted or unsubstituted C1-C30 alkyl group, more specifically a substituted or unsubstituted C1-C12 alkyl group, and more specifically a substituted or unsubstituted C1-C6 alkyl group.)

[0032] More specifically, the compound represented by formula (2) may be selected from the group consisting of compounds represented by the following formulas (2-1) to (2-3): The compound represented by the formula (3) may be a compound represented by the following formula (3-1) or (3-2): The compound represented by the formula (4) may be a compound represented by the following formula (4-1) or (4-2).

[0033] [ka] [ka] [ka]

[0034] [ka] [ka]

[0035] [ka] [ka] Another aspect of the present invention provides a method for producing a compound represented by formula (2), comprising the step of heating dianhydrosugar hexitol-ethylene glycol, a compound in which ethylene glycol is added to both terminal hydroxy groups of a dianhydrosugar hexitol, in the presence of an acid catalyst.

[0036] An anhydrosugar alcohol is generally referred to as a hydrogenated sugar or sugar alcohol, and is a substance obtained by removing one or more water molecules from a compound obtained by adding hydrogen to the reducing end group of a sugar. A dianhydrosugar hexitol is an anhydrosugar alcohol formed by removing two water molecules from inside a hexitol. It has a diol form with two hydroxyl groups in the molecule, and can be produced using hexitol derived from starch.

[0037] In one embodiment, the dianhydrosugar hexitol may be a 1,4:3,6-dianhydrohexitol, and more specifically may be isosorbide, isomannide, isoidide, or a mixture of two or more thereof.

[0038] In one embodiment, the dianhydrosugar hexitol-ethylene glycol may be prepared by an addition reaction of a dianhydrosugar hexitol with ethylene oxide having the following structure:

[0039] [Ethylene oxide] [ka]

[0040] In one embodiment, the addition reaction of the dianhydrosugar hexitol with ethylene oxide can be carried out, for example, at a temperature of 100° C. or higher, more specifically, 100° C. to 140° C., for 1 hour or longer, more specifically, 1 hour to 5 hours, but is not limited thereto.

[0041] In one embodiment, the addition reaction of the dianhydrosugar hexitol with ethylene oxide can be carried out using 2 or more moles of ethylene oxide per mole of the dianhydrosugar hexitol.

[0042] More specifically, in the addition reaction between the dianhydrosugar hexitol and ethylene oxide, the amount of ethylene oxide per mole of the dianhydrosugar hexitol may be 2 moles or more, 3 moles or more, 4 moles or more, or 5 moles or more, and may be 25 moles or less, 20 moles or less, 15 moles or less, or 10 moles or less. In the addition reaction between the dianhydrosugar hexitol and ethylene oxide, if the amount of ethylene oxide used per mole of the dianhydrosugar hexitol is less than 2 moles, it may not be possible to produce the compound of formula (1), whereas if it exceeds 25 moles, the economic efficiency may decrease due to an increase in production cost.

[0043] In one embodiment, the compound represented by the formula (2-1) can be produced by heating an addition reaction product of 1 mole of isosorbide and 2 moles or more of ethylene oxide in the presence of an acid catalyst.

[0044] In one embodiment, the compound represented by the formula (2-2) can be produced by heating an addition reaction product of 1 mole of isomannide and 2 moles or more of ethylene oxide in the presence of an acid catalyst.

[0045] In one embodiment, the compound represented by the formula (2-3) can be produced by heating an addition reaction product of 1 mole of isoidide and 2 moles or more of ethylene oxide in the presence of an acid catalyst.

[0046] In one embodiment, the acid catalyst may be an inorganic acid or an organic acid catalyst, and more specifically may be selected from, but is not limited to, sulfuric acid, hydrochloric acid, hydrobromic acid, phosphoric acid, methanesulfonic acid, benzenesulfonic acid, paratoluenesulfonic acid, or combinations thereof.

[0047] In one embodiment, the amount of the acid catalyst used in the addition reaction of the dianhydrosugar hexitol with ethylene oxide may be, for example, 0.01 parts by weight or more, 0.02 parts by weight or more, or 0.05 parts by weight or more, and may be 5 parts by weight or less, 2 parts by weight or less, or 1 part by weight or less, relative to 100 parts by weight of the dianhydrosugar hexitol, but is not limited thereto.

[0048] Yet another aspect of the present invention provides a method for producing a compound represented by formula (3) or (4), comprising the step of heating a compound represented by the following formula (A) or (B), respectively, with an alkylating agent in the presence of a base catalyst:

[0049] [ka] [ka] In one embodiment, the alkylating agent can be selected from, but is not limited to, an alkyl halide having the formula RX, where R is a substituted or unsubstituted C1-C30 alkyl group (more specifically, a substituted or unsubstituted C1-C12 alkyl group, even more specifically, a substituted or unsubstituted C1-C6 alkyl group), and X is a halogen atom (e.g., F, Cl, Br, or I), an aromatic sulfonate having a substituted or unsubstituted C1-C30 alkyl group, or a combination thereof.

[0050] More specifically, the alkyl halide may be methyl iodide, and the aromatic sulfonate having a substituted or unsubstituted C1-C30 alkyl group may be, but is not limited to, a toluenesulfonate having a C1-C30 alkyl group substituted with a halogen atom (e.g., F).

[0051] In one embodiment, the base catalyst may be selected from an inorganic base catalyst, an organic base catalyst, or a combination thereof, and more specifically, may be selected from, but is not limited to, sodium hydride, hydrogen iodide, hydrogen sulfide, aluminum hydride, or a combination thereof.

[0052] In one embodiment, the amount of the base catalyst used in the reaction of the compound represented by Formula (A) or (B) with an alkylating agent may be, for example, 1 part by weight or more, 2 parts by weight or more, or 5 parts by weight or more, and may be 80 parts by weight or less, 60 parts by weight or less, or 50 parts by weight or less, relative to 100 parts by weight of the compound of Formula (A) or (B), but is not limited thereto.

[0053] In one embodiment, the reaction of the compound represented by formula (A) or (B) with the alkylating agent can be carried out at a temperature of, for example, 40° C. or higher, more specifically, 40° C. to 80° C., for 5 hours or longer, more specifically, 5 hours to 15 hours, but is not limited thereto.

[0054] According to one embodiment of the present invention, the compound represented by the formula (1) can be effectively used as an electrolyte additive in a non-aqueous electrolyte composition for a secondary battery, particularly in a non-aqueous electrolyte composition for a lithium-sulfur secondary battery. This will be described later as another aspect of the present invention. However, the use of the compound of the present invention is by no means limited thereto, and the compound represented by the formula (1) can be used for various uses (for example, surfactants, penetration enhancers for cosmetic active ingredients, antibacterial agents, etc.) other than such electrolyte additives for secondary batteries.

[0055] [Electrolyte additive and non-aqueous electrolyte composition] Yet another aspect of the present invention relates to an electrolyte additive containing the compound represented by the formula (1).

[0056] In one embodiment, the electrolyte additive may consist solely of the compound represented by formula (1).

[0057] In one embodiment, the electrolyte additive may further include one or more components other than the compound represented by formula (1). As such additional components, components that can be used as additives for secondary batteries can be used without any particular limitation.

[0058] More specifically, the electrolyte additive may further contain a nitric acid (or nitrite)-based compound as a component other than the compound represented by formula (1). Such a nitric acid (or nitrite)-based compound can form a stable coating on the negative electrode (lithium-containing electrode) of a lithium-sulfur secondary battery, thereby improving the charge / discharge efficiency.

[0059] In one embodiment, the nitric acid (or nitrite) based compound may be selected from the group consisting of, but is not limited to, inorganic nitrate compounds (e.g., lithium nitrate (LiNO3) and lithium nitrite (LiNO2), etc.), organic nitrate compounds (e.g., nitromethane (CH3NO2), methyl nitrate (CH3NO3), etc.), or mixtures thereof.

[0060] In one embodiment, when the electrolyte additive contains the compound represented by formula (1) and other components (e.g., the nitric acid (or nitrite)-based compound), the content of the other components may be 0.1 to 2 parts by weight relative to 1 part by weight of the compound represented by formula (1) contained in the electrolyte additive, more specifically, 0.1 parts by weight or more, 0.2 parts by weight or more, or 0.3 parts by weight or more, and may be 2 parts by weight or less, 1.8 parts by weight or less, or 1.5 parts by weight or less, but is not limited thereto.

[0061] Yet another aspect of the present invention relates to a non-aqueous electrolyte composition comprising: a non-aqueous electrolyte solvent; a lithium salt; and the electrolyte additive of the present invention, wherein the content of the electrolyte additive is 0.1 to 10 parts by weight with respect to 100 parts by weight of a total amount of the electrolyte composition.

[0062] If the content of the electrolyte additive is less than 0.1 part by weight relative to 100 parts by weight of the total amount of the nonaqueous electrolyte composition of the present invention, when such an electrolyte composition is used, the effect of improving the life retention rate (or capacity retention rate) of the lithium-sulfur secondary battery may be insufficient. Conversely, if the content of the electrolyte additive exceeds 10 parts by weight, when such an electrolyte composition is used, the coating film may become thick, resulting in increased resistance and a decrease in the life retention rate (or capacity retention rate) of the lithium-sulfur secondary battery.

[0063] More specifically, the content of the electrolyte additive relative to 100 parts by weight of the total amount of the nonaqueous electrolyte composition of the present invention may be 0.1 parts by weight or more, 0.5 parts by weight or more, 1 part by weight or more, or 1.2 parts by weight or more, and may be 10 parts by weight or less, 9.5 parts by weight or less, 9 parts by weight or less, or 8.9 parts by weight or less.

[0064] The nonaqueous electrolyte solvent contained in the nonaqueous electrolyte composition of the present invention functions as a medium in which ions involved in the electrochemical reaction of the lithium-sulfur secondary battery can move.

[0065] In one embodiment, the non-aqueous electrolyte solvent may be a linear ether, a cyclic ether, or a combination thereof.

[0066] In one embodiment, the non-aqueous electrolyte solvent may be, for example, dimethyl ether, diethyl ether, dipropyl ether, dibutyl ether, diisobutyl ether, ethyl methyl ether, ethyl propyl ether, ethyl tert-butyl ether, dimethoxymethane, trimethoxymethane, dimethoxyethane, diethoxyethane, dimethoxypropane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, tetraethyl glycol dimethyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, dipropylene glycol dimethylene ether, butylene glycol ether, or diethylene The aryloxy group may be selected from the group consisting of, but is not limited to, glycol ethyl methyl ether, diethylene glycol isopropyl methyl ether, diethylene glycol butyl methyl ether, diethylene glycol tert-butyl ethyl ether, ethylene glycol ethyl methyl ether, dioxolane, methyl dioxolane, dimethyl dioxolane, vinyl dioxolane, methoxy dioxolane, ethyl methyl dioxolane, oxane, dioxane, trioxane, tetrahydrofuran, methyl tetrahydrofuran, dimethyl tetrahydrofuran, dimethoxy tetrahydrofuran, ethoxy tetrahydrofuran, dihydropyran, tetrahydropyran, furan, methyl furan, isosorbide dimethyl ether, or mixtures thereof.

[0067] In one embodiment, the lithium salt contained in the nonaqueous electrolyte composition of the present invention is selected from the group consisting of, but is not limited to, LiSCN, LiBr, LiI, LiPF6, LiBF4, LiSbF6, LiAsF6, LiCH3SO3, LiCF3SO3, LiClO4, LiBPh4, LiC(CF3SO2)3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(SFO2)2, LiN(CF3CF2SO2)2, Li2S, LiSn (wherein n=an integer of 1 to 8), or mixtures thereof. Here, Ph means phenyl.

[0068] In one embodiment, the molar concentration of the lithium salt in the nonaqueous electrolyte composition of the present invention may be 0.5 M to 5 M. If the molar concentration of the lithium salt in the electrolyte composition is less than 0.5 M, the capacity retention rate may decrease, whereas if it exceeds 5 M, the lithium salt may dissolve, resulting in a decrease in economic efficiency, which is not preferable.

[0069] More specifically, the molar concentration of the lithium salt in the nonaqueous electrolyte composition of the present invention may be 0.5M or more, 0.6M or more, 0.7M or more, 0.8M or more, 0.9M or more, or 1M or more, and may be 5M or less, 4.8M or less, 4.6M or less, 4.4M or less, or 4.2M or less.

[0070] [Secondary battery] Yet another aspect of the present invention relates to a secondary battery (particularly a lithium-sulfur secondary battery) comprising a positive electrode, a negative electrode, a separator, and the nonaqueous electrolyte composition of the present invention.

[0071] In one embodiment, the secondary battery of the present invention includes a positive electrode and a negative electrode arranged opposite each other; a separator provided between the positive electrode and the negative electrode; and a non-aqueous electrolyte composition according to the present invention impregnated in the positive electrode, the negative electrode, and the separator and having ion conductivity.

[0072] The positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector.

[0073] The positive electrode current collector may be any material that can be used as a current collector in this technical field, and specifically, it is preferable to use foamed aluminum, foamed nickel, or the like, which have good electrical conductivity.

[0074] The positive electrode active material layer may contain, as a positive electrode active material, elemental sulfur (S8), a sulfur-based compound, or a mixture thereof. Specific examples of the sulfur-based compound include Li2Sn (n=1), an organic sulfur compound, or a carbon-sulfur polymer (C2S x ) n :x=2.5~50, n=2).

[0075] Since such sulfur-based materials are not electrically conductive by themselves, the positive electrode active material layer is made of a conductive material.

[0076] The conductive material may be porous. Thus, the conductive material may be any material having porosity and conductivity, and may be, for example, a carbon-based material having porosity. Examples of such carbon-based materials include carbon black, graphite, graphene, activated carbon, and carbon fiber. In addition, metallic fibers such as metal mesh, metallic powders such as copper, silver, nickel, and aluminum, or organic conductive materials such as polyphenylene derivatives may be used. The conductive materials may be used alone or in combination.

[0077] In an embodiment, the positive electrode active material layer may further include a binder to improve the bond between the positive electrode active material and the conductive material and between the positive electrode active material layer and the positive electrode current collector.

[0078] The binder may include a thermoplastic resin or a thermosetting resin. For example, polyethylene, polyethylene oxide, polypropylene, polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), styrene-butadiene rubber, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer, polychlorotrifluoroethylene, vinylidene fluoride-pentafluoropropylene copolymer, propylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, ethylene-acrylic acid copolymer, etc. may be used alone or in combination, but are not limited thereto, and any material that can be used as a binder in the art may be used.

[0079] The positive electrode can be manufactured according to a conventional method, specifically, by mixing a positive electrode active material, a conductive material, and a binder in an organic solvent to form a composition for forming a positive electrode active material layer, applying the composition onto a positive electrode current collector, drying the composition, and optionally compressing the composition onto the positive electrode current collector to improve the electrode density. In this case, it is preferable to use an organic solvent that can uniformly disperse the positive electrode active material, the binder, and the conductive material and that is easy to evaporate. Specifically, the organic solvent can be selected from acetonitrile, methanol, ethanol, tetrahydrofuran, water, isopropyl alcohol, or a combination thereof.

[0080] The negative electrode may include a negative electrode current collector; and a negative electrode active material layer formed on the negative electrode current collector, or may be a lithium metal plate alone.

[0081] The negative electrode current collector is for supporting the negative electrode active material, and is not particularly limited as long as it has excellent electrical conductivity and is electrochemically stable in the voltage range of a lithium metal battery. For example, copper, stainless steel, aluminum, nickel, titanium, palladium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, silver, or the like, an aluminum-cadmium alloy, or the like can be used.

[0082] The negative electrode current collector may have fine irregularities on its surface in order to strengthen the bonding force with the negative electrode active material layer, and may be used in various forms such as a film, a sheet, a wheel, a mesh, a net, a porous body, a foam, or a nonwoven fabric.

[0083] The negative electrode active material layer contains lithium ions (Li + The lithium-containing compound may include a material capable of reversibly intercalating or deintercalating lithium ions; a material capable of reacting with lithium ions to reversibly form a lithium-containing compound; lithium metal; or a lithium alloy.

[0084] The lithium ion (Li + The material capable of reversibly absorbing or releasing lithium ions (Li) may be, for example, crystalline carbon, amorphous carbon, or a mixture thereof. + The material capable of reacting with lithium (Li) to reversibly form a lithium-containing compound may be, for example, tin oxide, titanium nitrate, or silicon. The lithium alloy may be, for example, an alloy of lithium (Li) and a metal selected from the group consisting of sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), aluminum (Al), and tin (Sn).

[0085] In a preferred embodiment, the negative electrode active material may be lithium metal, specifically in the form of a lithium metal thin film or lithium metal powder.

[0086] The method for forming the negative electrode active material layer is not particularly limited, and any layer or film forming method conventionally used in this technical field can be used. For example, methods such as compression, coating, and deposition can be used. In addition, the negative electrode of the present invention also includes a case where a battery is assembled without forming a lithium thin film on the negative electrode current collector, and a lithium metal thin film is formed on the metal plate by initial charging.

[0087] The nonaqueous electrolyte composition of the present invention is the same as described above, contains lithium ions, and is intended to cause an electrochemical oxidation reaction or reduction reaction between the positive electrode and the negative electrode via the lithium ions.

[0088] The nonaqueous electrolyte composition may be injected at an appropriate step during the manufacturing process of the electrochemical device depending on the manufacturing process and required properties of the final product, i.e., it may be applied before assembling the electrochemical device, or it may be applied in the final step of assembling the electrochemical device.

[0089] A separator may be further included between the positive electrode and the negative electrode. The separator is for physically separating the two electrodes in the secondary battery (particularly, the lithium-sulfur secondary battery) of the present invention, and any separator that has been conventionally used as a separator for a secondary battery (particularly, a lithium-sulfur secondary battery) may be used without any particular limitation. In particular, it is preferable to use a separator that has a small ion transfer resistance in the electrolyte composition and has good impregnation (humidification) with the electrolyte composition.

[0090] The separation membrane may be made of any porous material, and any porous material that has been conventionally used in electrochemical elements may be used. For example, a porous membrane or a nonwoven fabric may be used, but is not particularly limited thereto.

[0091] The specific example of the porous film is polyolefin-based porous film.The polyolefin-based porous film can be formed by using polyolefin-based polymers such as polyethylene (e.g., high-density polyethylene, linear low-density polyethylene, low-density polyethylene, ultra-high molecular weight polyethylene, etc.), polypropylene, polybutylene and polypentene alone, or can be formed by mixing these polymers.

[0092] The nonwoven fabric may be a polyolefin-based nonwoven fabric, or may be a nonwoven fabric formed by using, for example, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyether sulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalate, etc. alone or a nonwoven fabric formed from a polymer mixture thereof. The structure of the nonwoven fabric may be a spunbonded nonwoven fabric or a meltblown nonwoven fabric made of long fibers.

[0093] The thickness of the porous material is not particularly limited, but may be 1 to 100 μm, preferably 5 to 50 μm.

[0094] The size of the pores present in the porous material and the porosity are not particularly limited, but may be 0.001 to 50 μm and 10 to 95%, respectively.

[0095] The secondary battery (particularly, the lithium-sulfur secondary battery) according to the present invention can be manufactured through a process of laminating a separator and an electrode, stacking them, and folding them, in addition to a general winding process.

[0096] The shape of the secondary battery is not particularly limited, and the secondary battery can be manufactured in various shapes such as a cylindrical type, a laminated type, and a coin type.

[0097] The present invention will be described in more detail below with reference to examples and comparative examples, but the scope of the present invention is not limited thereto. Working Example

[0098] <Production of dianhydrosugar hexitol-ethylene glycol> In the following example of the preparation of dianhydrosugar hexitol-ethylene glycol, the stoichiometric addition reaction scheme of dianhydrosugar hexitol (isosorbide) and ethylene oxide is as follows:

[0099] [ka] (In the formula, m=1, n=1)

[0100] Production Example A1: Addition reaction using 5 moles of ethylene oxide to 1 mole of isosorbide 146g of isosorbide and 0.15g of phosphoric acid (85%) as an acid component were added to a pressurizable reactor, the reactor was replaced with nitrogen, heated to 100°C, and reduced pressure under vacuum to remove moisture in the reactor. Next, 88g of ethylene oxide was slowly added and reacted at a temperature of 100°C to 140°C for 2 to 3 hours. At this time, the reaction temperature was adjusted so that it did not exceed 140°C. After that, the reactor was cooled to 50°C, 0.3g of potassium hydroxide was added to the reactor, the reactor was replaced with nitrogen, the temperature was raised to 100°C, and the pressure was reduced under vacuum to remove moisture in the reactor. Next, 132g of ethylene oxide was slowly added and reacted at 100°C to 140°C for 2 to 3 hours. After the reaction was completed, the reactor was cooled to 50°C, 4.0g of Ambosol MP20 was added as an adsorbent, and the mixture was reheated and stirred at a temperature of 100°C to 120°C for 1 to 5 hours to remove the metal ions. At this time, the reactor was substituted with nitrogen or depressurized under vacuum. After confirming that no metal ions were detected, the reactor was cooled to 60°C to 90°C, and the residual by-products were removed to obtain 362g of a transparent liquid addition reaction product.

[0101] Production Example A2: Addition reaction using 10 moles of ethylene oxide to 1 mole of isosorbide The same method as in Production Example A1 was carried out except that the amount of ethylene oxide added in the second time was changed from 132 g to 352 g, and 551 g of a transparent liquid addition reaction product was obtained.

[0102] Preparation Example A3: Addition reaction using 2 moles of ethylene oxide to 1 mole of isosorbide The same method as in Production Example A1 was carried out except that the amount of ethylene oxide added in the first step was changed from 88 g to 44 g, and the amount added in the second step was changed from 132 g to 44 g, to obtain 227 g of a transparent liquid addition reaction product.

[0103] <Production of the compound of formula (2)> In the following compound preparation example, the reaction scheme for producing the target compound ((4aR,5R,7aR)-5-[(2S)-1,4-dioxan-2-yl]-2,3,4a,5,7,7a-hexahydrofuro[3,4-b][1,4]dioxine) from the dianhydrosugar hexitol-ethylene glycol is as follows:

[0104] [ka] (In the formula, m=1, n=1)

[0105] Example A1: Preparation of the target compound using the addition reaction product of Preparation Example A1 200 g of the addition reaction product obtained in Production Example A1 and 5 g of sulfuric acid were added to a three-neck glass reactor in which a vacuum pump and a micro-sublimation apparatus were connected in series, and the reaction was carried out while heating to 130°C. After heating and stirring for 1 hour, the pressure was slowly reduced to 50 mbar with a vacuum pump, decomposition gases and 1,4-dioxane were removed, and 35 g of the target compound in the form of needle crystals was obtained using a micro-sublimation apparatus. The analytical results of the target compound obtained are as follows: 1 H NMR (400 MHz, CDCl3): d 4.39 (td, J = 8.6, 4.0 Hz, 1H), 4.18 (t, J = 8.6 Hz, 1H), 3.96 (m, 1H), 3.96-3.83 (m, 5H), 3.81-3.74 (m, 3H), 3.71 (m, 1H), 3.66-3.58 (m, 2H), 3.50 (m, 1H), 3.33 (m, 1H). 13 C NMR (100 MHz, CDCl3): d 80.1, 74.7, 73.9, 72.4, 67.3, 66.6, 66.3, 64.6, 64.4, 59.6. Mass (ESI): 217.10 (M+1).

[0106] Example A2: Preparation of the target compound using the addition reaction product of Preparation Example A2 The same method as in Example A1 was carried out, except that 200 g of the addition reaction product obtained in Production Example A2 was used instead of the addition reaction product obtained in Production Example A1, to obtain 19 g of the target compound as needle crystals. The analytical results of the obtained target compound were the same as those of Example A1.

[0107] Example A3: Preparation of the target compound using the addition reaction product of Preparation A3 The same method as in Example A1 was carried out except that 200 g of the addition reaction product obtained in Production Example A3 was used instead of the addition reaction product obtained in Production Example A1, and 12 g of the target compound in the form of needle crystals was obtained. The analytical results of the target compound obtained were the same as those of Example A1.

[0108] <Production of compound of formula (3-1)> Example A4: Preparation of target compound using monohydroxyflodioxin In the following compound preparation examples, the reaction scheme for producing the target compound of formula (3-1) (5-(methoxymethyl)hexahydrofuro[3,4-b][1,4]dioxine) from monohydroxyfurodioxine is as follows:

[0109] [ka] 400 mL of tetrahydrofuran was added to a 1,000 mL flask, 80 g of the starting material ([hexahydrofuro[3,4-b][1,4]dioxin-5-yl]methanol) and 36 g of sodium hydride were added, and the flask was kept at 0° C. for 10 minutes. After stirring at 0° C. for 30 minutes, 90 g of methyl iodide was added, the temperature was raised to 60° C., and the reaction was carried out while stirring for 12 hours. After the reaction was completed, the resulting mixture was filtered and dried under vacuum to obtain 56 g of the target compound of the formula (3-1) (5-(methoxymethyl)hexahydrofuro[3,4-b][1,4]dioxin). 1H NMR (400 MHz, DMSO-d6): d 4.80 (td, 1H), 4.51 (t, 1H), 4.00-3.75 (m, 2H), 3.76-3.66 (m, 4H), 3.75 (m, 1H), 3.60-3.35 (m, 2H), 3.23 (s, 3H). 13 C NMR (100 MHz, DMSO-d6): d 91.1, 89.6, 86.1, 72.0, 62.7, 61.4, 61.1, 59.6. Mass (ESI): 174.2 (M+1).

[0110] <Production of compound of formula (3-2)> Example A5: Preparation of target compound using monohydroxyflodioxin The same method as in Example A4 was carried out except that 120 g of 2,2,2-trifluoroethyl p-toluenesulfonate was used instead of 90 g of methyl iodide, and 82 g of the target compound of the formula (3-2) (5-((2,2,2-trifluoroethoxy)methyl)hexahydrofuro[3,4-b][1,4]dioxine) was obtained. 1 H NMR (400 MHz, DMSO-d6): d 4.80 (td, 1H), 4.51 (td, 1H), 4.00-3.75 (m, 2H), 3.76-3.66 (m, 4H), 3.75 (m, 1H), 3.60-3.35 (m, 2H), 3.23 (s, 2H). 13 C NMR (100 MHz, DMSO-d6): d 128.5, 123.5, 91.1, 89.6, 86.1, 62.7, 61.4, 61.1, 51.6. Mass (ESI): 242.2 (M+1).

[0111] <Production of compound of formula (4-1)> Example A6: Preparation of target compound using dihydroxyflodioxin The same method as in Example A4 was carried out except that 90 g of 2,5-anhydro-3,4-O-(1,2-ethanediyl)mannitol was used instead of 80 g of [hexahydrofuro[3,4-b][1,4]dioxin-5-yl]methanol as the starting material, to obtain 66 g of the target compound of the formula (4-1) (5,7-bis(methoxymethyl)hexahydrofuro[3,4-b][1,4]dioxin). 1 H NMR (400 MHz, DMSO-d6): d 4.80 (td, 2H), 3.75 (m, 2H), 3.76-3.66 (m, 4H), 3.60-3.35 (m, 4H), 3.23 (s, 6H). 13 C NMR (100 MHz, DMSO-d6): d 88.9, 82.1, 72.3, 61.4, 59.6. Mass (ESI): 218.26 (M+1).

[0112] <Production of compound of formula (4-2)> Example A7: Preparation of target compound using dihydroxyflodioxin The same method as in Example A4 was carried out except that 90 g of 2,5-anhydro-3,4-O-(1,2-ethanediyl)mannitol was used instead of 80 g of [hexahydrofuro[3,4-b][1,4]dioxin-5-yl]methanol as a starting material, and 120 g of 2,2,2-trifluoroethyl p-toluenesulfonate was used instead of 90 g of methyl iodide, to obtain 83 g of the target compound of formula (4-2) (5,7-bis((2,2,2-trifluoroethoxy)methyl)hexahydrofuro[3,4-b][1,4]dioxin). 1 H NMR (400 MHz, DMSO-d6): d 4.92 (dd, 4H), 4.80 (td, 2H), 3.75 (m, 2H), 3.76-3.66 (m, 4H), 3.60-3.35 (m, 4H), 3.23 (s, 6H). 13C NMR (100 MHz, DMSO-d6): d 128.5, 121.6, 88.9, 82.1, 72.3, 61.4, 51.9. Mass (ESI): 354.25 (M+1).

[0113] <Production of non-aqueous electrolyte composition> Example B1: Preparation of an electrolyte composition containing, as additives, 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A1 An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 1.0 M LiN(CF3SO2)2 was mixed with 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A1 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to prepare 10 mL of the electrolyte composition.

[0114] Example B2: Preparation of an electrolyte composition containing 34.5 parts by weight of LiNO and 4.4 parts by weight of the target compound obtained in Example A2 as additives. An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 4.2 M LiN(CF3SO2)2 was mixed with 4.5 parts by weight of LiNO3 and 4.4 parts by weight of the target compound obtained in Example A2 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to produce 10 mL of the electrolyte composition.

[0115] Example B3: Preparation of an electrolyte composition containing 1 part by weight of CH3NO3 and 4.3 parts by weight of the target compound obtained in Example A3 as additives. An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 1.0 M LiN(CF3SO2)2 was mixed with 1.0 parts by weight of CH3NO3 and 4.3 parts by weight of the target compound obtained in Example A3 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to prepare 10 mL of the electrolyte composition.

[0116] Example B4: Preparation of an electrolyte composition containing, as additives, 0.5 parts by weight of LiNO2 and 0.7 parts by weight of the target obtained in Example A1 An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 0.4 M LiPF6 was mixed with 0.5 parts by weight of LiNO2 and 0.7 parts by weight of the target compound obtained in Example A1 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to produce 10 mL of the electrolyte composition.

[0117] Example B5: Preparation of an electrolyte composition containing, as additives, 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A1 An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane alone and 1.0 M LiN(CF3SO2)2 was mixed with 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A1 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to produce 10 mL of the electrolyte composition.

[0118] Example B6: Preparation of an electrolyte composition containing 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A1 as additives. An electrolyte solution containing a non-aqueous electrolyte solvent consisting of tetraethyl glycol dimethyl ether and 1,3-dioxolane (volume ratio = 25:75) and 1.0 M LiN(CF3SO2)2 was mixed with 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A1 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to prepare 10 mL of the electrolyte composition.

[0119] Example B7: Preparation of an electrolyte composition containing 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A4 as additives. An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 1.0 M LiN(CF3SO2)2 was mixed with 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A4 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to prepare 10 mL of the electrolyte composition.

[0120] Example B8: Preparation of an electrolyte composition containing 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A5 as additives. An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 1.0 M LiN(CF3SO2)2 was mixed with 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A5 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to prepare 10 mL of the electrolyte composition.

[0121] Example B9: Preparation of an electrolyte composition containing 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A6 as additives. An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 1.0 M LiN(CF3SO2)2 was mixed with 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A6 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to prepare 10 mL of the electrolyte composition.

[0122] Example B10: Preparation of an electrolyte composition containing 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A7 as additives. An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 1.0 M LiN(CF3SO2)2 was mixed with 1 part by weight of LiNO3 and 2 parts by weight of the target compound obtained in Example A7 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to prepare 10 mL of the electrolyte composition.

[0123] Comparative Example B1: Preparation of an electrolyte composition containing only 1 part by weight of LiNO3 as an additive An electrolyte composition of 10 mL was prepared by mixing 1 part by weight of LiNO3 as an additive with an electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 1.0 M LiN(CF3SO2)2 with respect to a total of 100 parts by weight of the electrolyte composition.

[0124] Comparative Example B2: Preparation of an electrolyte composition containing 0.09 parts by weight of additive (0.04 parts by weight of LiNO3 + 0.05 parts by weight of the target compound obtained in Example A1) An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 1.0 M LiN(CF3SO2)2 was mixed with 0.04 parts by weight of LiNO3 and 0.05 parts by weight of the target compound obtained in Example A1 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to produce 10 mL of the electrolyte composition.

[0125] Comparative Example B3: Preparation of an electrolyte composition containing 10.1 parts by weight of additive (35.5 parts by weight of LiNO + 4.6 parts by weight of the target compound obtained in Example A1) An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 1.0 M LiN(CF3SO2)2 was mixed with 5.5 parts by weight of LiNO3 and 4.6 parts by weight of the target compound obtained in Example A1 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to produce 10 mL of the electrolyte composition.

[0126] Comparative Example B4: Preparation of an electrolyte composition containing 0.09 parts by weight of additive (0.04 parts by weight of LiNO3 + 0.05 parts by weight of the target compound obtained in Example A4) An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 1.0 M LiN(CF3SO2)2 was mixed with 0.04 parts by weight of LiNO3 and 0.05 parts by weight of the target compound obtained in Example A4 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to produce 10 mL of the electrolyte composition.

[0127] Comparative Example B5: Preparation of an electrolyte composition containing 10.1 parts by weight of additive (35.5 parts by weight of LiNO + 4.6 parts by weight of the target compound obtained in Example A5) An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 1.0 M LiN(CF3SO2)2 was mixed with 5.5 parts by weight of LiNO3 and 4.6 parts by weight of the target compound obtained in Example A5 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to produce 10 mL of the electrolyte composition.

[0128] Comparative Example B6: Preparation of an electrolyte composition containing 0.09 parts by weight of additive (0.04 parts by weight of LiNO3 + 0.05 parts by weight of the target compound obtained in Example A6) An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 1.0 M LiN(CF3SO2)2 was mixed with 0.04 parts by weight of LiNO3 and 0.05 parts by weight of the target compound obtained in Example A6 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to prepare 10 mL of the electrolyte composition.

[0129] Comparative Example B7: Preparation of an electrolyte composition containing 10.1 parts by weight of additive (35.5 parts by weight of LiNO + 4.6 parts by weight of the target compound obtained in Example A7) An electrolyte solution containing a non-aqueous electrolyte solvent consisting of 1,2-dimethoxyethane and 1,3-dioxolane (volume ratio = 50:50) and 1.0 M LiN(CF3SO2)2 was mixed with 5.5 parts by weight of LiNO3 and 4.6 parts by weight of the target compound obtained in Example A7 as additives relative to 100 parts by weight of the total amount of the electrolyte composition to prepare 10 mL of the electrolyte composition.

[0130] <Manufacturing lithium-sulfur secondary batteries> Examples C1 to C10 and Comparative Examples C1 to C7 65 parts by weight of sulfur, 25 parts by weight of carbon black, and 10 parts by weight of polyethylene tellurene oxide were mixed with acetonitrile to prepare a composition for forming a positive electrode active material layer. At this time, the total content of sulfur, carbon black, and polyethylene oxide was 100 parts by weight. The composition for forming a positive electrode active material layer was coated on an aluminum current collector and dried to prepare a positive electrode. In addition, lithium metal having a thickness of 450 μm was used for the negative electrode. The prepared positive electrode and negative electrode were placed opposite each other, a polypropylene separator was placed between them, and the obtained electrolyte composition of each of Examples B1 to B10 and Comparative Examples B1 to B7 was filled therein to prepare the lithium-sulfur secondary batteries of Examples C1 to C10 and Comparative Examples C1 to C7.

[0131] <Charge and discharge characteristics of lithium-sulfur secondary batteries> The charge / discharge characteristics of the lithium-sulfur secondary batteries of Examples C1 to C10 and Comparative Examples C1 to C7 were measured by the following method, and the results are shown in Table 1 below.

[0132] Life evaluation at room temperature (discharge capacity) The lithium-sulfur secondary batteries manufactured in the examples and comparative examples were subjected to a life evaluation at room temperature. Specifically, the lithium-sulfur secondary batteries were discharged to 1.8 V at room temperature (25° C.) with a constant current mode of 0.36 mA, and charged at a constant current mode of 0.36 mA until the operating voltage reached 2.7 V 10 minutes after the completion of discharge. One charge and one discharge constitute one cycle, and the charge and discharge were repeated 100 times to measure the capacity retention rate (life retention rate) relative to the initial charge capacity at room temperature.

[0133] [Table 1-1] [Table 1-2]

[0134] As shown in Table 1, in the case of the secondary batteries using the electrolyte compositions of Examples B1 to B10 according to the present invention, the additive containing the compound of formula (1) according to the present invention was contained in the amount specified in the present invention, and therefore the life retention rate (capacity retention rate) was very high, at 90.0% or more, regardless of the type of lithium salt.

[0135] However, in the case of a secondary battery using the electrolyte composition of Comparative Example B1, which does not contain the compound of formula (1) of the present invention, the life retention rate was poor at 64.2%, in the case of secondary batteries using the electrolyte compositions of Comparative Examples B2, B4, and B6, in which the additive containing the compound of formula (1) of the present invention (specifically, the compound of formulas (2) to (4)) was used in an amount less than the amount specified in the present invention, the life retention rate was poor at less than 70%, and in the case of secondary batteries using the electrolyte compositions of Comparative Examples B3, B5, and B7, in which the additive containing the compound of formula (1) of the present invention (specifically, the compound of formulas (2) to (4)) was used in an amount greater than the amount specified in the present invention, the life retention rate was very poor at less than 60%.

Claims

1. A compound represented by the following formula (1): [Formula 1] (In the formula, R 1 and R 2 are each independently selected from the group consisting of a hydrogen atom, a halogen atom, a substituted or unsubstituted C1-C30 alkyl group, a substituted or unsubstituted C2-C30 alkenyl group, a substituted or unsubstituted C2-C30 alkynyl group, a substituted or unsubstituted C1-C30 alkoxy group, a substituted or unsubstituted C3-C30 cycloalkyl group, a substituted or unsubstituted C1-C30 alkylene-O-C1-C30 alkyl group, a substituted or unsubstituted C3-C30 heterocycloalkyl group, a substituted or unsubstituted C6-C60 aryl group, a substituted or unsubstituted C1-C60 heteroaryl group, a substituted or unsubstituted C7-C60 aralkyl group, a substituted or unsubstituted C6-C60 aryloxy group, and a substituted or unsubstituted C6-C60 arylthio group, with the proviso that R 1 and R 2 At least one of the is not a hydrogen atom.)

2. The compound according to claim 1, wherein the compound represented by formula (1) is selected from the group consisting of compounds represented by the following formulas (2) to (4): [Case 2] [C3] [C4] (In the formula, R 3 and R 4 are each independently a substituted or unsubstituted C1-C30 alkyl group.

3. The compound represented by formula (2) is selected from the group consisting of compounds represented by the following formulas (2-1) to (2-3): The compound represented by formula (3) is represented by the following formula (3-1) or (3-2): The compound according to claim 2, wherein the compound represented by formula (4) is represented by the following formula (4-1) or (4-2): [C5] [C6] [C7] [C8] [C9] [C10] [C11]

4. A method for producing a compound represented by formula (2), comprising the steps of: The method includes a step of heating dianhydrosugar hexitol-ethylene glycol, which is a compound in which ethylene glycol is added to both terminal hydroxy groups of a dianhydrosugar hexitol, in the presence of an acid catalyst. [C12]

5. 5. The method of claim 4, wherein the dianhydrosugar hexitol-ethylene glycol is produced by the addition reaction of a dianhydrosugar hexitol with ethylene oxide.

6. 6. The method according to claim 5, wherein the addition reaction of the dianhydrosugar hexitol with ethylene oxide is carried out using 2 or more moles of ethylene oxide per mole of the dianhydrosugar hexitol.

7. 5. The process of claim 4, wherein the acid catalyst is selected from sulfuric acid, hydrochloric acid, hydrobromic acid, phosphoric acid, methanesulfonic acid, benzenesulfonic acid, paratoluenesulfonic acid, or combinations thereof.

8. A method for producing a compound represented by formula (3) or (4), comprising the steps of: A method comprising the step of heating a compound represented by the following formula (A) or (B) and an alkylating agent in the presence of a base catalyst: [C13] [C14] (In the formula, R 3 and R 4are each independently a substituted or unsubstituted C1-C30 alkyl group. [C15] [C16]

9. 9. The method of claim 8, wherein the alkylating agent is selected from an alkyl halide having the formula R-X, where R is a substituted or unsubstituted C1-C30 alkyl group and X is a halogen atom, an aromatic sulfonate having a substituted or unsubstituted C1-C30 alkyl group, or a combination thereof.

10. 9. The method of claim 8, wherein the base catalyst is selected from an inorganic base catalyst, an organic base catalyst, or a combination thereof.

11. An electrolyte additive comprising a compound represented by the following formula (1): [C17] (In the formula, R 1 and R 2 are each independently selected from the group consisting of a hydrogen atom, a halogen atom, a substituted or unsubstituted C1-C30 alkyl group, a substituted or unsubstituted C2-C30 alkenyl group, a substituted or unsubstituted C2-C30 alkynyl group, a substituted or unsubstituted C1-C30 alkoxy group, a substituted or unsubstituted C3-C30 cycloalkyl group, a substituted or unsubstituted C1-C30 alkylene-O-C1-C30 alkyl group, a substituted or unsubstituted C3-C30 heterocycloalkyl group, a substituted or unsubstituted C6-C60 aryl group, a substituted or unsubstituted C1-C60 heteroaryl group, a substituted or unsubstituted C7-C60 aralkyl group, a substituted or unsubstituted C6-C60 aryloxy group, and a substituted or unsubstituted C6-C60 arylthio group, with the proviso that R 1 and R 2 At least one of the is not a hydrogen atom.)

12. The electrolyte additive according to claim 11, further comprising a nitric acid (or nitrite) based compound.

13. A non-aqueous electrolyte solvent; a lithium salt; and the electrolyte additive according to claim 11 or 12, The content of the electrolyte additive is 0.1 to 10 parts by weight based on 100 parts by weight of the total amount of the electrolyte composition.

14. A secondary battery comprising: a positive electrode; a negative electrode; a separator; and the nonaqueous electrolyte composition of claim 13.

15. 15. The secondary battery according to claim 14, which is a lithium-sulfur secondary battery.

Citation Information

Patent Citations

  • New 3,4-alkylenedioxy-2,5-dialkoxy-tetrahydrofuran and / or 3,4-arylendioxy-2,5-dialkoxy-tetrahydrofuran compounds useful for preparing e.g. 3,4-alkylenedioxythiophene and / or 3,4-arylenedioxythiophene and 3,4-alkylenedioxyselenophene

    DE102004029774A1

  • Sugar-modified cytostatic agents

    JP1999502860A

  • Nonaqueous electrolyte battery

    JP2000243438A

  • Flexible all-solid-state lithium-ion secondary battery and its manufacturing method

    JP2020524388A

  • Alkylation of alcohols, amines, thiols and their derivatives by cyclic sulfate intermediates