Lithium secondary battery
Using single or pseudo-single particles as positive electrode active material with a tab-less structure addresses thermal stability issues in large lithium secondary batteries, improving safety and efficiency.
Patent Information
- Application Number
- JP2024520039
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-23
- Filing Date
- 2022-10-14
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2042-10-14
AI Technical Summary
Conventional can-shaped lithium secondary batteries face issues with thermal stability and safety due to increased volume, leading to heat and gas generation, which can cause fires or explosions, especially in large batteries used for electric vehicles.
The use of single particles or pseudo-single particles as positive electrode active material, combined with a tab-less structure and optimized particle size distribution, minimizes gas generation and improves thermal stability.
The solution enhances thermal stability and safety in large batteries by reducing particle cracking and resistance, allowing for high-capacity and efficient energy storage.
Smart Images

Figure 2024537842000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0136711 filed on October 14, 2021 and Korean Patent Application No. 10-2022-0121172 filed on September 23, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated as part of this specification.
[0002] The present invention relates to a lithium secondary battery, and more particularly to a lithium secondary battery that can achieve excellent thermal stability even when the volume is increased by applying a single-particle and / or pseudo-single-particle positive electrode active material. [Background technology]
[0003] 2. Description of the Related Art With technological advances in electric vehicles, portable electronic devices, and the like, the demand for lithium secondary batteries as energy sources is rapidly increasing.
[0004] Lithium secondary batteries are classified into can-type batteries, such as cylindrical or rectangular, and pouch-type batteries, depending on the material of the battery case. A can-type battery is formed by stacking a sheet-shaped positive electrode plate, a separator, and a negative electrode plate in order in a battery can, and then winding the stack in one direction to form a jelly-roll-type electrode assembly, and then sealing the battery can by covering the top of the battery can with a cap plate. The positive electrode plate and the negative electrode plate are provided with strip-shaped positive electrode tabs and negative electrode tabs, respectively, and the positive electrode tabs and negative electrode tabs are connected to electrode terminals to be electrically connected to an external power source. For reference, the positive electrode terminal is the cap plate, and the negative electrode terminal is the battery can. However, in the case of a conventional can-type battery having such a structure, current is concentrated in the strip-shaped electrode tabs, resulting in high resistance, a large amount of heat generation, and poor current collection efficiency.
[0005] Meanwhile, with the recent development of electric vehicle technology, the need for high-capacity batteries is increasing, and so there is a demand for the development of large-volume can-type batteries. Conventionally, small can-type batteries that have been commonly used, such as small cylindrical batteries with 1865 or 2170 form factors, have small capacities, so resistance and heat generation do not seriously affect the performance of the battery. However, if the specifications of conventional small can-type batteries are directly applied to large can-type batteries, serious problems may occur in the safety of the battery.
[0006] This is because as the size of a battery increases, the amount of heat and gas generated inside the battery also increases, and the heat and gas increase the temperature and pressure inside the battery, which can cause the battery to catch fire or explode. To prevent this, the heat and gas inside the battery must be properly discharged to the outside, and to this end, the cross-sectional area of the battery, which serves as a path for discharging heat to the outside of the battery, must increase in accordance with the increase in volume. However, since the increase in cross-sectional area is usually not sufficient to match the increase in volume, the larger the battery, the more heat generated inside the battery increases, which increases the risk of explosion and reduces output, etc. In addition, when fast charging at a high voltage, a large amount of heat is generated around the electrode tab in a short period of time, which can cause the battery to catch fire.
[0007] Therefore, in order to realize high capacity, there is a demand for the development of a can-type battery that has a large volume and is highly safe. Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention is intended to solve the above problems, and aims to provide a lithium secondary battery that can achieve excellent thermal stability even when the volume of a can-type battery is increased by applying a single particle or pseudo-single particle as a positive electrode active material. [Means for solving the problem]
[0009] According to one embodiment, the present invention provides a secondary battery including an electrode assembly in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate are wound in one direction, a battery can in which the electrode assembly is housed, and a sealing body for sealing an open end of the battery can, wherein the positive electrode plate includes a positive electrode active material including a single particle, a pseudo-single particle, or a combination thereof, and the D of the positive electrode active material is min The present invention provides a cylindrical lithium secondary battery having a particle size of 1.0 μm or more.
[0010] In addition, the positive electrode active material may include a lithium nickel-based oxide containing 80 mol % or more of Ni based on the total moles of transition metals, for example, a lithium nickel-based oxide represented by the following [Chemical Formula 1]. [Chemical formula 1] Li a Ni b Co c M 1 d M 2 e O2
[0011] In the above Chemical Formula 1, M 1 is Mn, Al or a combination of these, M 2 are Zr, W, Ti, Mg, Ca, Sr, and Ba, and 0.8≦a≦1.2, 0.83≦b<1, 0 <c<0.17、0<d<0.17、0≦e≦0.1である。
[0012] Meanwhile, the negative electrode plate may include a silicon-based negative electrode active material.
[0013] The negative electrode plate may include a silicon-based negative electrode active material and a carbon-based negative electrode active material, and the silicon-based negative electrode active material and the carbon-based negative electrode active material may be included in a weight ratio of 1:99 to 20:80.
[0014] Meanwhile, the secondary battery may be a cylindrical battery having a form factor ratio of 0.4 or more, for example, a 46110 cell, a 4875 cell, a 48110 cell, a 4880 cell, or a 4680 cell, where the form factor ratio is the diameter of the cylindrical battery divided by the height.
[0015] In addition, the secondary battery according to the present invention may be a battery in which each of the positive and negative electrode plates includes an uncoated portion on which no active material layer is formed, and at least a portion of the positive or negative electrode plate in the uncoated portion defines an electrode tab.
[0016] The positive plate uncoated portion and the negative plate uncoated portion are located along ends of one side of the positive plate and the negative plate that are parallel to the winding direction of the electrode assembly, respectively, and a current collecting plate is coupled to each of the positive plate uncoated portion and the negative plate uncoated portion, and the current collecting plate may be connected to an electrode terminal.
[0017] Meanwhile, the positive electrode plate uncoated portion and the negative electrode plate uncoated portion may be processed into a plurality of segment pieces that can be bent independently, at least some of the plurality of segment pieces defining the electrode tab and bent toward the winding center C of the electrode assembly. Also, at least some of the folded plurality of segment pieces may overlap on upper and lower ends of the electrode assembly, and the current collecting plate may be coupled onto the overlapping plurality of segment pieces.
[0018] Meanwhile, an insulating layer may be further formed on the positive electrode plate, covering a portion of the positive electrode active material layer and a portion of the uncoated portion along a direction parallel to the winding direction.
[0019] According to another embodiment, the present invention provides a battery pack including the lithium secondary battery according to the present invention, and a vehicle including the battery pack. Effect of the Invention
[0020] The lithium secondary battery according to the present invention applies a positive electrode active material consisting of a single particle and / or a pseudo-single particle as a positive electrode active material, and can minimize gas generation due to particle cracking during electrode manufacturing and internal cracking during charging and discharging, thereby achieving excellent safety even in a large battery with an increased volume.
[0021] The lithium secondary battery according to the present invention is also min By using a positive electrode active material having a particle size of 1.0 μm or more, it is possible to further improve the thermal stability of the battery. Research by the present inventors has shown that even if single particles and / or pseudo-single particles are used as the positive electrode active material, the effect of suppressing particle cracking and improving thermal stability after rolling varies depending on the particle size of the positive electrode active material. In particular, when particles with a particle size of less than 1.0 μm are contained in the positive electrode active material, the linear pressure increases in the rolling process, causing increased particle cracking and reduced thermal stability, making it impossible to ensure sufficient thermal stability when applied to large cylindrical batteries. Therefore, in the present invention, min By using a positive electrode active material with a particle size controlled to 1.0 μm or more, the thermal stability improvement effect can be maximized.
[0022] The lithium secondary battery according to the present invention is also 50 , D max By applying a positive active material with an appropriately adjusted particle size distribution (PSD), the increase in resistance caused by the application of single particles can be minimized, thereby achieving excellent capacity and output characteristics.
[0023] Furthermore, the lithium secondary battery according to the present invention may contain a silicon-based negative electrode active material having a large capacity as the negative electrode active material, and in this case, a higher energy density may be achieved.
[0024] In addition, the lithium secondary battery according to the present invention may have a structure in which the uncoated portions of the positive and negative electrode plates serve as electrode tabs, for example, a tab-less structure. Conventional batteries have a structure in which the electrode plates and electrode leads are connected via electrode tabs, but in this case, a large amount of current is concentrated on the electrode tab during charging, generating a lot of heat around the electrode tab. In particular, during fast charging, this phenomenon becomes severe, and there is a risk of the battery catching fire or exploding. In contrast, the lithium secondary battery according to the present invention may have a structure in which uncoated portions on which no active material layer is formed are formed at the ends of the positive and negative electrode plates, and the uncoated portions are connected to the electrode terminals by welding the uncoated portions to a current collecting plate having a wide cross-sectional area. A battery having such a structure has less current concentration compared to a conventional battery having electrode tabs, and therefore it is possible to effectively reduce heat generation inside the battery, thereby improving the thermal stability of the battery. [Brief description of the drawings]
[0025] [Figure 1] FIG. 4 is a diagram showing a stacked state of an electrode assembly according to the present invention before being wound. [Diagram 2] 2 is a cross-sectional view showing a structure of an electrode plate of an electrode assembly according to an embodiment of the present invention; [Diagram 3] 1 is a cross-sectional view showing the structure of a tabless-type battery according to one embodiment of the present invention; [Figure 4] FIG. 4 is a cross-sectional view showing the structure of a tabless-type battery according to another embodiment of the present invention. [Diagram 5] 2 is a diagram illustrating a structure of an electrode assembly according to an embodiment of the present invention; [Figure 6] 1 is a diagram for explaining a battery pack according to the present invention; [Figure 7] 1 is a diagram for explaining an automobile including a battery pack according to the present invention; [Figure 8] 1 is a SEM photograph of the positive electrode active material used in Example 1. [Figure 9] 1 is a SEM photograph of the positive electrode active material used in Example 2. [Figure 10] 1 is a SEM photograph of the positive electrode active material used in Comparative Example 2. [Figure 11] 1 is a graph showing hot box test results of 4680 cells manufactured according to Sample 1 of Example 1 and Comparative Example 1. [Figure 12] 1 is a graph showing the results of hot box tests of Samples 2 and 3 of Example 1, Samples 1 and 2 of Example 2, and 4680 cells of Comparative Example 2. [Figure 13] 1 is a cross-sectional SEM photograph of a positive electrode plate produced in Example 1. [Figure 14] 1 is a cross-sectional SEM photograph of a positive electrode plate produced in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The present invention will now be described in more detail.
[0027] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0028] In the present invention, the term "primary particle" refers to a particle unit that does not have grain boundaries when observed at a magnification of 5,000 to 20,000 times using a scanning electron microscope or an electron backscatter diffraction (EBSD) pattern analyzer. The term "average particle size of primary particles" refers to the arithmetic average value calculated after measuring the particle size of primary particles observed using a scanning electron microscope or an EBSD image.
[0029] In the present invention, the "secondary particle" is a particle formed by agglomeration of a plurality of primary particles. In order to distinguish from conventional secondary particles formed by agglomeration of tens to hundreds of primary particles, in the present invention, secondary particles formed by agglomeration of 10 or less primary particles are called pseudo-single particles.
[0030] In the present invention, "D min ", "D 50 " and "D max " is the particle size value of the volume cumulative distribution of the positive electrode active material measured using the laser diffraction method. min is the minimum particle size indicated by the cumulative volume distribution, and D 50 is the particle diameter when the cumulative volume is 50%, and D max is the maximum particle diameter shown in the volume cumulative distribution. The particle size value of the volume cumulative distribution can be measured, for example, by dispersing the positive electrode active material in a dispersion medium, introducing it into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000), irradiating it with ultrasonic waves of about 28 kHz at an output of 60 W, and then obtaining a volume cumulative particle size distribution graph.
[0031] The inventors have conducted extensive research to develop a large-scale battery that achieves high capacity and excellent safety, and as a result have discovered that the safety of large-scale batteries can be significantly improved by using, as a positive electrode active material, a single particle consisting of one primary particle and / or a pseudo-single particle, which is an aggregate of 10 or less primary particles, and have thus completed the present invention.
[0032] Specifically, the lithium secondary battery according to the present invention includes an electrode assembly in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate are wound in one direction, a battery can in which the electrode assembly is housed, and a seal body that seals an open end of the battery can.
[0033] The configuration of the lithium secondary battery of the present invention will be specifically described below.
[0034] electrode assembly The electrode assembly has a structure in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate are wound in one direction, and may be, for example, a jelly roll type electrode assembly.
[0035] FIG. 1 shows a laminated structure of an electrode assembly according to the present invention before being wound, and FIG. 2 shows a cross-sectional structure of an electrode plate (positive or negative electrode plate) according to the present invention.
[0036] Referring to FIG. 1 and FIG. 2, the electrode assembly of the present invention can be manufactured by winding up a laminate formed by stacking a separator 12, a positive electrode plate 10, a separator 12, and a negative electrode plate 11, in that order, at least once, in one direction X.
[0037] Here, the positive electrode plate 10 and the negative electrode plate 11 have a structure in which an active material layer 21 is formed on a sheet-shaped current collector 20, and may include a blank portion 22 in which the active material layer 21 is not formed in a portion of the current collector 20.
[0038] By using the positive electrode plate 10 and the negative electrode plate 11 including the uncoated portion 22 as described above, a battery having a tabless structure can be realized in which no separate electrode tab is provided, and at least a portion of the uncoated portion of the positive electrode plate 10 and the negative electrode plate 11 define the electrode tab.
[0039] Specifically, the uncoated portion 22 may be formed long along the winding direction X at an end of one side of the current collector 20. A current collecting plate may be bonded to each of the uncoated portions of the positive and negative electrode plates, and the current collecting plates may be connected to electrode terminals, thereby realizing a battery having a tab-less structure.
[0040] For example, a tab-less battery can be manufactured by the following method. First, a separator, a positive plate, a separator, and a negative plate are stacked in order so that the uncoated portions 22 of the positive plate 10 and the negative plate 11 are positioned in the opposite directions, and then the stack is wound in one direction to manufacture an electrode assembly. Then, the uncoated portions 22 of the positive plate and the negative plate are folded in the direction of the winding center C, and current collecting plates are welded to the uncoated portions of the positive plate and the negative plate, respectively, and the current collecting plates are connected to electrode terminals to manufacture a tab-less battery. Meanwhile, the current collecting plates have a larger cross-sectional area than strip-type electrode tabs, and since the resistance is inversely proportional to the cross-sectional area of the path through which the current flows, when a secondary battery is formed in the above-mentioned structure, the cell resistance can be significantly reduced.
[0041] On the other hand, the positive electrode plate and the negative electrode plate uncoated portions may be processed into a plurality of segmented pieces that can be bent independently, and at least a portion of the plurality of segmented pieces may be bent toward the winding center C of the electrode assembly.
[0042] The segments can be formed by processing the current collectors of the positive and negative plates through a metal foil cutting process such as laser notching, ultrasonic cutting, punching, etc.
[0043] When the uncoated portions of the positive and negative electrode plates are processed into multiple segmented pieces, the stress applied to the uncoated portions during bending can be reduced, preventing deformation or damage to the uncoated portions and improving the welding characteristics with the current collecting plates.
[0044] The current collecting plate and the uncoated portion are generally joined by welding, and in order to improve the welding characteristics, strong pressure must be applied to the welded area of the uncoated portion to bend it as flat as possible. However, during this bending process, the shape of the uncoated portion may become irregularly distorted and deformed, and the deformed portion may come into contact with the electrode of the opposite polarity, causing an internal short circuit or causing fine cracks in the uncoated portion. However, if the uncoated portions of the positive and negative electrode plates are processed into multiple segmented pieces that can be bent independently, the stress applied to the uncoated portion during bending is alleviated, minimizing deformation and damage to the uncoated portion.
[0045] In addition, when the uncoated portion is processed into segmented pieces as described above, overlaps occur between the segments during folding, which increases the weld strength with the current collecting plate and prevents the laser from penetrating into the electrode assembly and melting the separator or active material when using modern technology such as laser welding. Preferably, at least a portion of the folded segments may overlap on the upper and lower ends of the electrode assembly, and a current collecting plate may be bonded onto the overlapped segments.
[0046] Meanwhile, the electrode assembly according to the present invention may be formed in a structure in which an insulating layer 24 is further formed on the positive electrode plate 10, as shown in Fig. 5. Specifically, the insulating layer 24 may be formed to cover a portion of the positive electrode active material layer and a portion of the uncoated portion in a direction parallel to the winding direction of the electrode assembly.
[0047] In the case of a battery with a tabless structure using the uncoated portion 22c of the positive electrode plate 10 and the uncoated portion 22a of the negative electrode plate 11 as electrode tabs, an electrode assembly is formed such that the positive electrode plate 10 protrudes above the separator 12 and the negative electrode plate 11 protrudes below the separator 12, and the protruding positive electrode plate 10 and / or negative electrode plate 11 are folded and then combined with a current collecting plate. However, when the positive electrode plate 10 or the negative electrode plate 11 is folded as described above, the current collector of the positive electrode plate 10 or the negative electrode plate 11 is positioned adjacent to the electrode of the opposite polarity beyond the separator, which may cause an internal short circuit due to electrical contact between the positive electrode plate and the negative electrode plate. However, when an insulating layer 24 is formed to cover a part of the positive electrode active material layer and the uncoated portion as shown in FIG. 5, the insulating layer 24 can prevent electrical contact between the positive electrode plate 10 and the negative electrode plate 11, thereby preventing a short circuit inside the battery.
[0048] Preferably, the insulating layer 24 is provided on at least one side of the current collector of the positive electrode plate 10, and more preferably, on both sides of the positive electrode plate 10.
[0049] Also, the insulating layer 24 may be formed in a region of the positive electrode plate 10 that may face the active material layer 21a of the negative electrode plate 11. For example, in the uncoated portion 22c of the positive electrode plate 10, the insulating layer 24 may be formed to extend to an end of the uncoated portion 22c on a surface that faces the negative electrode plate 11 after being folded. However, in the case of a surface opposite to the surface that faces the negative electrode plate 11 after being folded, it is preferable that the insulating layer 24 is formed only to a part of the uncoated portion 22c, for example, to a portion in front of the folding point of the uncoated portion 22c. This is because if the insulating layer 24 is formed in the entire region of the uncoated portion on the surface opposite to the surface that faces the negative electrode plate 11, electrical contact with the current collecting plate is not possible, and the insulating layer 24 cannot function as an electrode tab.
[0050] Meanwhile, the insulating layer 24 may be any material or component that can be attached to the positive electrode plate while maintaining insulating performance. For example, the insulating layer may be an insulating coating layer or an insulating tape, and the insulating coating layer may include an organic binder and inorganic particles. Here, the organic binder may be, for example, styrene-butadiene rubber (SBR), and the inorganic particles may be, but are not limited to, alumina oxide.
[0051] Next, each component of the electrode assembly of the present invention will be described in more detail.
[0052] (1) Positive electrode plate The positive electrode plate may have a structure in which a positive electrode active material layer is formed on one or both sides of a long sheet-shaped positive electrode current collector, and the positive electrode active material layer may include a positive electrode active material and may optionally include a conductive material and / or a binder.
[0053] Specifically, the positive electrode plate may be manufactured by coating one or both sides of a long sheet-shaped positive electrode collector with a positive electrode slurry prepared by dispersing a positive electrode active material, a conductive material, and / or a binder in a solvent such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and then rolling the coated positive electrode slurry after removing the solvent from the positive electrode slurry by a drying process. Meanwhile, a positive electrode plate including a non-coated portion may be manufactured by not coating a part of the positive electrode collector, for example, one end of the positive electrode collector, with the positive electrode slurry when coating the positive electrode slurry.
[0054] As the positive electrode current collector, various positive electrode current collectors used in the art can be used. For example, as the positive electrode current collector, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. can be used. The positive electrode current collector can usually have a thickness of 3 to 500 μm, and fine irregularities can be formed on the surface of the positive electrode current collector to increase the adhesive strength of the positive electrode active material. The positive electrode current collector can be used in various forms, such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0055] In the present invention, the positive electrode plate contains a positive electrode active material consisting of a single particle consisting of one primary particle and / or a quasi-single particle which is an aggregate of 10 or less primary particles.
[0056] Conventionally, it has been common to use spherical secondary particles formed by agglomeration of tens to hundreds of primary particles as the positive electrode active material of a lithium secondary battery. However, in the case of a positive electrode active material in the form of secondary particles formed by agglomeration of many primary particles, there is a problem that the primary particles are easily broken during the rolling process during the manufacture of the positive electrode, and cracks are generated inside the particles during the charge and discharge process. When cracks occur in the particles of the positive electrode active material or inside the particles, the contact area with the electrolyte increases, and the generation of gas due to a side reaction with the electrolyte increases. If the generation of gas increases inside the battery, the pressure inside the battery increases, which may cause the battery to explode. In particular, when the volume of a cylindrical battery is increased, the amount of active material inside the battery increases due to the increase in volume, and the amount of gas generated also increases significantly, which increases the risk of the battery catching fire and / or exploding.
[0057] In contrast, positive electrode active materials in the form of single particles consisting of one primary particle or pseudo-single particles in which 10 or less primary particles are aggregated have higher particle strength than existing positive electrode active materials in the form of secondary particles in which tens to hundreds of primary particles are aggregated, and therefore hardly crack particles during rolling. In addition, in the case of positive electrode active materials in the form of single particles or pseudo-single particles, the number of primary particles constituting the particles is small, so there is little change due to volume expansion and contraction of the primary particles during charging and discharging, and therefore the occurrence of cracks inside the particles is significantly reduced.
[0058] Therefore, when a positive electrode active material consisting of single particles and / or pseudo-single particles is used as in the present invention, the amount of gas generation due to particle breakage and internal cracking can be significantly reduced, thereby achieving excellent safety even in large batteries.
[0059] Meanwhile, the monoparticles and / or pseudo-monoparticles are preferably included in an amount of 95% by weight to 100% by weight, preferably 98% by weight to 100% by weight, more preferably 99% by weight to 100% by weight, and even more preferably 100% by weight, based on the weight of the total positive electrode active material included in the positive electrode plate. When the content of the monoparticles and / or pseudo-monoparticles satisfies the above range, sufficient safety can be obtained when applied to a large battery. When the secondary particle type positive electrode active material is included in an amount exceeding 5% by weight of the total positive electrode active material, the side reaction with the electrolyte increases due to the fraction generated from the secondary particles during the manufacture and charging / discharging of the electrode, thereby reducing the effect of suppressing gas generation, and thus the effect of improving stability can be reduced when applied to a large battery.
[0060] On the other hand, the positive electrode active material containing the single particles and / or pseudo-single particles according to the present invention has a D min The D of the positive electrode active material can be 1.0 μm or more, 1.1 μm or more, 1.15 μm or more, 1.2 μm or more, 1.25 μm or more, 1.3 μm or more, or 1.5 μm or more. minIf the thickness is less than 1.0 μm, the voltage increases during the rolling process of the positive electrode plate, which makes it easy for particles to crack, and the thermal stability decreases, making it difficult to ensure sufficient thermal stability when applied to a large cylindrical battery.
[0061] On the other hand, considering the resistance and output characteristics, the D min can be 3 μm or less, 2.5 μm or less, or 2 μm or less. min If is too large, the lithium ion diffusion distance within the particle increases, which may result in a decrease in resistance and output characteristics.
[0062] For example, D of the positive electrode active material min can be 1.0 μm to 3 μm, 1.0 μm to 2.5 μm, or 1.3 μm to 2.0 μm.
[0063] On the other hand, the positive electrode active material is D 50 can be 5 μm or less, 4 μm or less, or 3 μm or less, for example, 0.5 μm to 5 μm, preferably 1 μm to 5 μm, and more preferably 2 μm to 5 μm. Positive electrode active materials in the form of single particles and / or pseudo-single particles have fewer interfaces between primary particles that serve as diffusion paths for lithium ions inside the particles, and therefore have a problem of inferior lithium mobility compared to positive electrode active materials in the form of secondary particles, resulting in increased resistance. Such an increase in resistance becomes more severe as the particle size increases, and the increased resistance adversely affects the capacity and output characteristics. Therefore, the D of the positive electrode active material 50 By adjusting the diameter to 5 μm or less, the lithium ion diffusion distance inside the positive electrode active material particles can be minimized, thereby suppressing an increase in resistance.
[0064] The positive electrode active material is D max The diameter of the positive electrode active material may be 12 μm to 17 μm, preferably 12 μm to 16 μm, and more preferably 12 μm to 15 μm. max When the D of the positive electrode active material satisfies the above range, better resistance characteristics and capacity characteristics are exhibited. maxIf D is too large, aggregation between single particles occurs, and the lithium migration path inside the aggregated particles becomes longer, which reduces the lithium mobility and increases the resistance. max If D is too small, excessive crushing will occur. min The grain size can be as small as less than 1 μm, which can cause grain cracking during rolling and reduce thermal stability.
[0065] On the other hand, the positive electrode active material may have a particle size distribution (PSD) represented by the following formula (1) of 3 or less, preferably 2 to 3, and more preferably 2.3 to 3.
[0066] Equation (1): Particle size distribution (PSD) = (D max -D min ) / D 50
[0067] When the positive electrode active material has the above particle size distribution, the electrode density of the positive electrode can be appropriately maintained, and particle cracking and an increase in resistance can be effectively suppressed.
[0068] Meanwhile, the positive electrode active material may have an average particle size of 5 μm or less, 4 μm or less, 3 μm or less, or 2 μm or less, for example, 0.5 μm to 5 μm, preferably 1 μm to 5 μm, and more preferably 2 μm to 5 μm. When the average particle size of the primary particles satisfies the above range, a positive electrode active material having excellent electrochemical properties and a single particle and / or pseudo-single particle form may be formed. If the average particle size of the primary particles is too small, the number of agglomerates of the primary particles forming the positive electrode active material increases, and the effect of suppressing the occurrence of particle cracks during rolling decreases. If the average particle size of the primary particles is too large, the lithium diffusion path inside the primary particles becomes long, increasing the resistance and decreasing the output characteristics.
[0069] In the present invention, the positive electrode active material preferably has a unimodal particle size distribution. In the past, in order to improve the electrode density of the positive electrode active material layer, bimodal positive electrode active materials have been used in which a large particle size positive electrode active material having a large average particle size and a small particle size positive electrode active material having a small average particle size are mixed. However, in the case of a positive electrode active material having a single particle or pseudo-single particle form, as the particle size increases, the lithium migration path becomes longer and the resistance increases significantly, so that when large particle size particles are mixed, a problem of reduced capacity and output characteristics may occur. Therefore, in the present invention, a positive electrode active material having a unimodal distribution is used to minimize the increase in resistance.
[0070] Meanwhile, the positive electrode active material may include a lithium nickel-based oxide, specifically, a lithium nickel-based oxide containing 80 mol% or more of Ni relative to the total moles of transition metals. Preferably, the lithium nickel-based oxide may contain Ni in an amount of 80 mol% or more and less than 100 mol%, 82 mol% or more and less than 100 mol%, or 83 mol% or more and less than 100 mol%. As described above, when a lithium nickel-based oxide with a high Ni content is used, a high capacity can be achieved.
[0071] More specifically, the positive electrode active material may include a lithium nickel-based oxide represented by the following [Chemical Formula 1].
[0072] [Chemical formula 1] Li a Ni b Co c M 1 d M 2 e O2
[0073] In the above Chemical Formula 1, M 1 can be Mn, Al or a combination thereof, preferably Mn or Mn and Al.
[0074] Said M 2is one or more selected from the group consisting of Zr, W, Y, Ba, Ca, Ti, Mg, Ta, and Nb, preferably can be one or more selected from the group consisting of Zr, Y, Mg, and Ti, and more preferably can be Zr, Y, or a combination thereof. M 2 The element is not necessarily included, but when included in an appropriate amount, it can play a role in promoting grain growth during firing or improving crystal structure stability.
[0075] Said a represents the lithium molar ratio in the lithium nickel-based oxide, and can be 0.8 ≦ a ≦ 1.2, 0.85 ≦ a ≦ 1.15, or 0.9 ≦ a ≦ 1.2. When the molar ratio of lithium satisfies the above range, the crystal structure of the lithium nickel-based oxide can be stably formed.
[0076] Said b represents the molar ratio of nickel among all the metals other than lithium in the lithium nickel-based oxide, and can be 0.8 ≦ b < 1, 0.82 ≦ b < 1, 0.83 ≦ b < 1, 0.85 ≦ b < 1, 0.88 ≦ b < 1, or 0.90 ≦ b < 1. When the molar ratio of nickel satisfies the above range, it shows a high energy density and enables the realization of a high capacity.
[0077] Said c represents the cobalt molar ratio among all the metals other than lithium in the lithium nickel-based oxide, and can be 0 < c < 0.2, 0 < c < 0.18, 0.01 ≦ c ≦ 0.17, 0.01 ≦ c ≦ 0.15, 0.01 ≦ c ≦ 0.12, or 0.01 ≦ c ≦ 0.10. When the molar ratio of cobalt satisfies the above range, good resistance characteristics and output characteristics can be realized.
[0078] Said d represents the molar ratio of the M 1 element among all the metals other than lithium in the lithium nickel-based oxide, and can be 0 < d < 0.2, 0 < d < 0.18, 0.01 ≦ d ≦ 0.17, 0.01 ≦ d ≦ 0.15, 0.01 ≦ d ≦ 0.12, or 0.01 ≦ d ≦ 0.10. M 1 When the molar ratio of the element satisfies the above range, the structure stability of the positive electrode active material is excellent.
[0079] The e is M among all metals other than lithium in the lithium nickel-based oxide. 2 It indicates the molar ratio of the elements and can be 0≦e≦0.1, or 0≦e≦0.05.
[0080] Meanwhile, the positive electrode active material according to the present invention may further include, if necessary, a coating layer on the surface of the lithium nickel-based oxide particles, the coating layer including one or more coating elements selected from the group consisting of Al, Ti, W, B, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb, Mo, Sr, Sb, Bi, Si, and S. Preferably, the coating element may be Al, B, Co, or a combination thereof.
[0081] When a coating layer is present on the surface of the lithium nickel-based oxide particles, the coating layer suppresses contact between the electrolyte and the lithium composite transition metal oxide, thereby providing the effect of reducing the elution of the transition metal and the generation of gas due to side reactions with the electrolyte.
[0082] The positive electrode active material can be contained in an amount of 80 to 99% by weight, preferably 85 to 99% by weight, and more preferably 90 to 99% by weight, based on the total weight of the positive electrode active material layer.
[0083] Next, the conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery that is constructed and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives. Of these, one type alone or a mixture of two or more types can be used. The conductive material can usually be contained in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, based on the total weight of the positive electrode active material layer.
[0084] The binder plays a role in improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and among these, one type alone or a mixture of two or more types can be used. The binder can be included in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, more preferably 1 to 10% by weight, based on the total weight of the positive electrode active material layer.
[0085] On one hand, an insulating layer that covers a part of the positive electrode active material layer and a part of the non-coated area can be further formed on the positive electrode plate according to the present invention. The insulating layer can be formed along a direction parallel to the winding direction of the electrode assembly.
[0086] (2) Negative electrode plate The negative electrode plate can have a structure in which a negative electrode active material layer is formed on one or both surfaces of a long sheet-like negative electrode current collector, and the negative electrode active material layer can contain a negative electrode active material, a conductive material, and a binder.
[0087] Specifically, the negative electrode plate can be manufactured by applying a negative electrode slurry produced by dispersing a negative electrode active material, a conductive material, and a binder in a solvent such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc. on one or both surfaces of a sheet-like negative electrode current collector, removing the solvent of the negative electrode slurry by a drying process, and then rolling. On the other hand, when applying the negative electrode slurry, a negative electrode plate including a non-coated area can be manufactured by a method of not applying the negative electrode slurry to a partial area of the negative electrode current collector, for example, one end of the negative electrode current collector.
[0088] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium can be used. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; silicon-based materials such as Si, Si-Me alloy (where Me is one or more selected from the group consisting of Al, Sn, Mg, Cu, Fe, Pb, Zn, Mn, Cr, Ti, and Ni), SiOy (where 0 < y < 2), and Si-C composite; lithium metal thin film; metal materials capable of alloying with lithium such as Sn and Al; etc. Any one or a mixture of two or more of these can be used.
[0089] Preferably, the negative electrode plate according to the present invention can contain a silicon-based negative electrode active material. The silicon-based negative electrode active material can be Si, Si-Me alloy (where Me is one or more selected from the group consisting of Al, Sn, Mg, Cu, Fe, Pb, Zn, Mn, Cr, Ti, and Ni), SiOy (where 0 < y < 2), Si-C composite, or a combination thereof, and preferably can be SiOy (where 0 < y < 2). Since the silicon-based negative electrode active material has a high theoretical capacity, when the silicon-based negative electrode active material is included, the capacity characteristics can be improved.
[0090] On the other hand, the silicon-based negative electrode active material can be doped with M b metal, where the M b metal can be a Group 1 metal element or a Group 2 metal element, and specifically can be Li, Mg, etc. Specifically, the silicon negative electrode active material can be Si, SiOy (where 0 < y < 2), Si-C composite, etc. doped with M b metal. In the case of the metal-doped silicon-based negative electrode active material, although the capacity of the active material decreases somewhat due to the doping element, since it has high efficiency, a high energy density can be realized.
[0091] Further, the silicon-based negative electrode active material can further include a carbon coating layer on the surface of the particles. Here, the amount of the carbon coating can be 20% by weight or less, preferably 1 to 20% by weight, based on the total weight of the silicon-based negative electrode active material.
[0092] In addition, the negative electrode plate can further contain a carbon-based negative electrode active material as a negative electrode active material as needed. The carbon-based negative electrode active material can be, for example, artificial graphite, natural graphite, graphitized carbon fiber, amorphous carbon, soft carbon, hard carbon, etc., but is not limited thereto.
[0093] On the other hand, when a mixture of a silicon-based negative electrode active material and a carbon-based negative electrode active material is used as the negative electrode active material, the mixing ratio of the silicon-based negative electrode active material and the carbon-based negative electrode active material may be 1:99 to 20:80, preferably 1:99 to 15:85, and more preferably 1:99 to 10:90, by weight.
[0094] The negative electrode active material can be contained in an amount of 80 to 99% by weight, preferably 85 to 99% by weight, and more preferably 90 to 99% by weight, based on the total weight of the negative electrode active material layer.
[0095] Meanwhile, as the negative electrode current collector, a negative electrode current collector generally used in the technical field can be used, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. The negative electrode current collector can usually have a thickness of 3 to 500 μm, and like the positive electrode current collector, the surface of the current collector can be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0096] The conductive material is used to impart electrical conductivity to the negative electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery to be constructed and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives. Of these, one type alone or a mixture of two or more types can be used. The conductive material can usually be contained in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, based on the total weight of the negative electrode active material layer.
[0097] The binder plays a role in improving the adhesion between the negative electrode active material particles and the adhesive strength between the negative electrode active material and the negative electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and among these, one type alone or a mixture of two or more types may be used. The binder may be included in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, more preferably 1 to 10% by weight, based on the total weight of the negative electrode active material layer.
[0098] (3) Separator The separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. Specifically, the separator may be a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, or the like, may be used. In addition, a coated separator containing a ceramic component or a polymeric substance may be used to ensure heat resistance or mechanical strength.
[0099] Lithium secondary battery Next, the lithium secondary battery according to the present invention will be described.
[0100] The lithium secondary battery according to the present invention may include an electrode assembly having a structure in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate are wound in one direction, a battery can in which the electrode assembly is housed, and a seal body that seals an open end of the battery can.
[0101] Preferably, the lithium secondary battery according to the present invention can be a cylindrical battery, and more preferably, a large cylindrical battery having a form factor ratio (defined as the value obtained by dividing the diameter of a cylindrical battery by its height, i.e., the ratio of the diameter (Φ) to the height (H)) of 0.4 or more. Here, the form factor refers to values indicating the diameter and height of a cylindrical battery.
[0102] Cylindrical batteries according to the present invention can be, for example, 46110 cells (diameter 46 mm, height 110 mm, form factor ratio 0.418), 4875 cells (diameter 48 mm, height 75 mm, form factor ratio 0.640), 48110 cells (diameter 48 mm, height 110 mm, form factor ratio 0.436), 4880 cells (diameter 48 mm, height 80 mm, form factor ratio 0.600), and 4680 cells (diameter 46 mm, height 80 mm, form factor ratio 0.575). In the form factor numbers, the first two digits indicate the diameter of the cell, and the next two or three digits indicate the height of the cell.
[0103] The lithium secondary battery according to the present invention uses a positive electrode active material in the form of a single particle and / or pseudo-single particle to significantly reduce the amount of gas generation compared to conventional batteries, thereby achieving excellent safety even in large cylindrical batteries with a form factor ratio of 0.4 or more.
[0104] Meanwhile, the lithium secondary battery according to the present invention may preferably be a battery having a tab-less structure that does not include an electrode tab, but is not limited thereto.
[0105] The tabless-structured battery may have a structure in which, for example, each of the positive and negative electrode plates includes an uncoated portion where no active material layer is formed, the uncoated positive and negative electrode plate portions are located at the upper and lower ends of the electrode assembly, respectively, current collecting plates are bonded to the uncoated positive and negative electrode plate portions, and the current collecting plates are connected to electrode terminals.
[0106] Fig. 3 shows a cross-sectional view of a battery having a tabless structure according to one embodiment of the present invention. Hereinafter, a lithium secondary battery according to one embodiment of the present invention will be described with reference to Fig. 3. However, Fig. 3 shows one embodiment of the present invention, and the structure of the lithium secondary battery of the present invention is not limited to the scope disclosed in Fig. 3.
[0107] The lithium secondary battery 140 according to an embodiment of the present invention includes a jelly-roll type electrode assembly 141, a battery can 142 in which the electrode assembly 141 is housed, and a seal 143 that seals an open end of the battery can 142.
[0108] Here, the positive and negative electrode plates of the electrode assembly may each include an uncoated portion where no active material layer is formed, and may be stacked and wound such that the positive and negative uncoated portions are located at the upper and lower ends of the electrode assembly, respectively. Since the electrode assembly has been described above, only the remaining components other than the electrode assembly will be described below.
[0109] The battery can 142 is a container having an opening at the top and is made of a conductive metal material such as aluminum or steel. The battery can accommodates the electrode assembly 141 in the inner space through the opening at the top, and also accommodates an electrolyte.
[0110] As the electrolyte used in the present invention, various electrolytes that can be used in lithium secondary batteries, such as organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes, can be used, and the type is not particularly limited.
[0111] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0112] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that can be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethyl alcohol and isopropyl alcohol, nitriles such as R-CN (R is a C2-C20 straight-chain, branched or cyclic hydrocarbon group that can contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of a battery and a low-viscosity straight-chain carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferred.
[0113] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 can be used as the lithium salt. The concentration of the lithium salt is preferably within a range of 0.1 to 5.0M, preferably 0.1 to 3.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0114] In addition to the electrolyte components, the electrolyte may further contain additives for the purpose of improving the life characteristics of the battery, suppressing the capacity reduction of the battery, and improving the discharge capacity of the battery. For example, the additives may be haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, which may be used alone or in combination, but are not limited thereto. The additives may be contained in an amount of 0.1 to 10% by weight, preferably 0.1 to 5% by weight, based on the total weight of the electrolyte.
[0115] The battery can 142 is electrically connected to the uncoated portion 146b of the negative plate and functions as a negative terminal that contacts an external power source and transmits a current applied from the external power source to the negative plate.
[0116] If necessary, a beading portion 147 and a crimping portion 148 may be provided at the upper end of the battery can 142. The beading portion 147 may be formed by pressing the periphery of the outer circumferential surface of the battery can 142 up to a distance D1. The beading portion 147 prevents the electrode assembly 141 accommodated inside the battery can 142 from being separated through the upper opening of the battery can 142, and may function as a support on which the sealed body 143 is placed.
[0117] The crimping portion 148 may be formed on the beading portion 147, and has an extended and bent shape so as to enclose the outer circumferential surface of the cap plate 143a disposed on the beading portion 147 and a part of the upper surface of the cap plate 143a.
[0118] Next, the sealing body 143 is for sealing the open end of the battery can 142, and includes a cap plate 143a, a first gasket 143b having insulating properties and providing airtightness between the cap plate 143a and the battery can 142, and may further include a connection plate 143c electrically and mechanically coupled to the cap plate 143a, if necessary. The cap plate 143a may be crimped onto a beading portion 147 formed on the battery can 142 and fixed by a crimping portion 148.
[0119] The cap plate 143a is a part made of a conductive metal material and covers an upper opening of the battery can 142. The cap plate 143a is electrically connected to the positive electrode plate of the electrode assembly 141 and is electrically insulated from the battery can 142 via a first gasket 143b. Therefore, the cap plate 143a can function as a positive electrode terminal of the secondary battery. The cap plate 143a may have a protrusion 143d protruding upward from a center C thereof, and the protrusion 143d may come into contact with an external power source so that a current can be applied from the external power source.
[0120] A first gasket 143b may be interposed between the cap plate 143a and the crimping portion 148 to ensure airtightness of the battery can 142 and to electrically insulate the battery can 142 from the cap plate 143a.
[0121] Meanwhile, the lithium secondary battery 140 according to the present invention may further include current collecting plates 144 and 145, if necessary. The current collecting plates are combined with the positive plate uncoated portion 146a and the negative plate uncoated portion 146b, and are connected to electrode terminals (i.e., positive and negative terminals).
[0122] Specifically, the lithium secondary battery 140 according to the present invention may include a first current collecting plate 144 coupled to an upper portion of the electrode assembly 141 and a second current collecting plate 145 coupled to a lower portion of the electrode assembly 141 .
[0123] A first current collecting plate 144 and / or a second current collecting plate 145 may further be included.
[0124] The first current collecting plate 144 is coupled to the upper part of the electrode assembly 141. The first current collecting plate 144 is made of a conductive metal material such as aluminum, copper, or nickel, and is electrically connected to the uncoated part 146a of the positive electrode plate. A lead 149 may be coupled to the first current collecting plate 144. The lead 149 may extend upwardly of the electrode assembly 141 and be coupled to the connection plate 143c, or may be directly coupled to the lower surface of the cap plate 143a. The coupling of the lead 149 to other components may be performed by welding. Preferably, the first current collecting plate 144 may be formed integrally with the lead 149. In this case, the lead 149 may have a long plate shape extending outward from the center of the first current collecting plate 144.
[0125] Meanwhile, the first current collecting plate 144 is coupled to an end of the uncoated portion 146a of the positive electrode plate, and the coupling may be performed by, for example, laser welding, resistance welding, ultrasonic welding, soldering, or the like.
[0126] The second current collecting plate 145 is coupled to the lower part of the electrode assembly 141. The second current collecting plate 145 is made of a conductive metal material such as aluminum, copper, or nickel, and is electrically connected to the uncoated portion 146b of the negative electrode plate. One surface of the second current collecting plate 145 may be coupled to the uncoated portion 146b of the negative electrode plate, and the opposite surface may be coupled to the inner bottom surface of the battery can 142. Here, the coupling may be performed by a method such as laser welding, resistance welding, ultrasonic welding, soldering, etc.
[0127] Meanwhile, the battery 140 according to the present invention may further include an insulating member (insulator) 146, if necessary. The insulating member 146 may be disposed to cover an upper surface of the first current collecting plate 144. By covering the first current collecting plate 144 with the insulating member 146, it is possible to prevent the first current collecting plate 144 and the inner peripheral surface of the battery can 142 from directly contacting each other.
[0128] The insulating member 146 has a lead hole 151 through which the lead 149 extending upward from the first current collecting plate 144 is pulled out. The lead 149 is pulled out upward through the lead hole 151 and coupled to the lower surface of the connecting plate 143c or the lower surface of the cap plate 143a.
[0129] The insulating member 146 may be made of an insulating polymer resin, such as polyethylene, polypropylene, polyimide, or polybutylene terephthalate.
[0130] Meanwhile, the battery 140 according to the present invention may further include a venting portion 152 formed on the bottom surface of the battery can 142, if necessary. The venting portion 152 corresponds to a region of the bottom surface of the battery can 142 that is thinner than the surrounding region. Since the venting portion 152 is thin, it is structurally weaker than the surrounding region. Therefore, when the pressure inside the battery 140 increases above a predetermined level, the venting portion 152 ruptures to release the gas inside the battery can 142 to the outside, thereby preventing the battery from exploding.
[0131] Fig. 4 shows a cross-sectional view of a battery having a tabless structure according to another embodiment of the present invention. Hereinafter, a battery according to another embodiment of the present invention will be described with reference to Fig. 4. However, Fig. 4 shows one embodiment of the present invention, and the structure of the battery according to the present invention is not limited to the scope disclosed in Fig. 4.
[0132] Referring to FIG. 4, a battery 170 according to another embodiment of the present invention has a different structure of the battery can and the sealed body compared to the battery 140 shown in FIG. 3, but the configuration of the electrode assembly and electrolyte is substantially the same.
[0133] Specifically, a battery 170 according to another embodiment includes a battery can 171 having a rivet terminal 172 penetrating therethrough. The rivet terminal 172 is installed on a partially closed surface (top surface in the drawing) of one end of the battery can 171. The rivet terminal 172 is riveted into a through hole (first opening at a first end) of the battery can 171 with an insulating second gasket 173 interposed therebetween. The rivet terminal 172 is exposed to the outside in the direction opposite to the direction of gravity.
[0134] The rivet terminal 172 includes a terminal exposing portion 172a and a terminal inserting portion 172b. The terminal exposing portion 172a is exposed to the outside of the closed surface of the battery can 171. The terminal exposing portion 172a may be located at an approximately central portion of the partially closed surface of the battery can 171. The maximum diameter of the terminal exposing portion 172a may be larger than the maximum diameter of the through hole formed in the battery can 171. The terminal inserting portion 172b may penetrate approximately the central portion of the partially closed surface of the battery can 171 to be electrically connected to the uncoated portion 146a of the positive electrode plate. The terminal inserting portion 172b may be rivet-coupled to the inner surface of the battery can 171. That is, an end of the terminal inserting portion 172b may have a shape that is bent toward the inner surface of the battery can 171. The maximum diameter of the end of the terminal inserting portion 172b may be larger than the maximum diameter of the through hole of the battery can 171.
[0135] A lower end surface of the terminal insertion portion 172b may be welded to the first current collecting plate 144 connected to the uncoated portion 146a of the positive electrode plate. An insulating cap 174 made of an insulating material may be interposed between the first current collecting plate 144 and the inner surface of the battery can 171. The insulating cap 174 covers an upper portion of the first current collecting plate 144 and an upper edge portion of the electrode assembly 141. This prevents the uncoated portion on the outer periphery of the electrode assembly 141 from coming into contact with the inner surface of the battery can 171 having a different polarity, causing a short circuit. The terminal insertion portion 172b of the rivet terminal 172 may be welded to the first current collecting plate 144 by penetrating the insulating cap 174.
[0136] The second gasket 173 is interposed between the battery can 171 and the rivet terminal 172 to prevent electrical contact between the battery can 171 and the rivet terminal 172, which have opposite polarities. This allows the upper surface of the rivet terminal 172, which has a substantially flat shape, to function as a positive terminal of the battery 170.
[0137] The second gasket 173 includes a gasket exposing portion 173a and a gasket inserting portion 173b. The gasket exposing portion 173a is interposed between the terminal exposing portion 172a of the rivet terminal 172 and the battery can 171. The gasket inserting portion 173b is interposed between the terminal inserting portion 172b of the rivet terminal 172 and the battery can 171. The gasket inserting portion 173b is deformed when the terminal inserting portion 172b is riveted, and can be closely attached to the inner surface of the battery can 171. The second gasket 173 may be made of, for example, a polymer resin having insulating properties.
[0138] The gasket exposing portion 173a of the second gasket 173 may extend to cover an outer circumferential surface of the terminal exposing portion 172a of the rivet terminal 172. When the second gasket 173 covers the outer circumferential surface of the rivet terminal 172, it is possible to prevent a short circuit from occurring during the process of connecting an electrical connecting component such as a bus bar to the upper surface of the battery can 171 and / or the rivet terminal 172. Although not shown in the drawings, the gasket exposing portion 173a may extend to cover not only the outer circumferential surface of the terminal exposing portion 172a but also a portion of the upper surface.
[0139] When second gasket 173 is made of a polymer resin, second gasket 173 can be joined to battery can 171 and rivet terminal 172 by thermal fusion. In this case, it is possible to strengthen the airtightness at the joining interface between second gasket 173 and rivet terminal 172 and at the joining interface between second gasket 173 and battery can 171. On the other hand, when gasket exposed portion 173a of second gasket 173 has a form that extends to the upper surface of terminal exposed portion 172a, rivet terminal 172 can be joined integrally with second gasket 173 by insert injection.
[0140] The remaining area 175 of the upper surface of the battery can 171 other than the area occupied by the rivet terminal 172 and the second gasket 173 corresponds to a negative terminal having a polarity opposite to that of the rivet terminal 172 .
[0141] The second current collecting plate 176 is coupled to the lower part of the electrode assembly 141. The second current collecting plate 176 is made of a conductive metal material such as aluminum, steel, copper, or nickel, and is electrically connected to the uncoated portion 146b of the negative electrode plate.
[0142] Preferably, the second current collecting plate 176 is electrically connected to the battery can 171. To this end, the second current collecting plate 176 may be fixed with at least a portion of an edge portion interposed between the inner surface of the battery can 171 and the first gasket 178b. In one example, at least a portion of the edge portion of the second current collecting plate 176 may be fixed to the beading portion 180 by welding while being supported by a lower end surface of the beading portion 180 formed at the lower end of the battery can 171. In a modified example, at least a portion of the edge portion of the second current collecting plate 176 may be directly welded to the inner wall surface of the battery can 171.
[0143] The second current collecting plate 176 may have a plurality of projections and recesses (not shown) formed radially on a surface facing the uncoated portion 146b. When the projections and recesses are formed, the second current collecting plate 176 may be pressed to press the projections and recesses into the uncoated portion 146b.
[0144] Preferably, the end of the second current collecting plate 176 and the uncoated portion 146b may be joined by welding, for example laser welding.
[0145] The sealing body 178 that seals the lower open end of the battery can 171 includes a cap plate 178a and a first gasket 178b. The first gasket 178b electrically separates the cap plate 178a from the battery can 171. A crimping portion 181 fixes the edge of the cap plate 178a and the first gasket 178b together. The cap plate 178a is provided with a vent portion 179. The configuration of the vent portion 179 is substantially the same as that of the above-mentioned embodiment.
[0146] Preferably, the cap plate 178a is made of a conductive metal material. However, the cap plate 178a does not have electrical polarity because the first gasket 178b is interposed between the cap plate 178a and the battery can 171. The seal 178 seals the open end of the lower part of the battery can 171 and functions to discharge gas when the internal pressure of the battery cell 170 increases above a critical value.
[0147] Preferably, the rivet terminal 172 electrically connected to the uncoated portion 146a of the positive electrode plate is used as a positive electrode terminal. Also, a portion 175 of the upper surface of the battery can 171 electrically connected to the uncoated portion 146b of the negative electrode plate via the second current collecting plate 176 other than the rivet terminal 172 is used as a negative electrode terminal. In this way, when two electrode terminals are located on the upper part of the battery, an electrical connection part such as a bus bar can be disposed only on one side of the battery 170. This can simplify the structure of the battery pack and improve the energy density. Also, since the portion 175 used as the negative electrode terminal has a substantially flat shape, a sufficient connection area can be secured when connecting an electrical connection part such as a bus bar. As a result, the battery 170 can reduce the resistance at the connection part of the electrical connection part to a preferable level.
[0148] When a lithium secondary battery is formed in a tabless structure as described above, current concentration is less than in conventional batteries with electrode tabs, so heat generation inside the battery can be effectively reduced, thereby improving the thermal stability of the battery.
[0149] The lithium secondary battery of the present invention as described above may be used to manufacture a battery pack. Fig. 6 is a schematic diagram of a battery pack according to an embodiment of the present invention. Referring to Fig. 6, a battery pack 3 according to an embodiment of the present invention includes an assembly to which secondary batteries 1 are electrically connected and a pack housing 2 that accommodates the assembly. Here, the secondary batteries 1 are the battery cells according to the above-described embodiment. For convenience of illustration, components such as a bus bar for electrically connecting the secondary batteries 1, a cooling unit, and external terminals are omitted in the drawings.
[0150] The battery pack 3 can be mounted on a vehicle. The vehicle can be, for example, an electric vehicle, a hybrid vehicle, or a plug-in hybrid vehicle. The vehicle can include a four-wheeled vehicle or a two-wheeled vehicle.
[0151] FIG. 7 is a diagram for explaining an automobile including the battery pack 3 of FIG.
[0152] Referring to FIG. 7, an automobile 5 according to an embodiment of the present invention includes a battery pack 3 according to an embodiment of the present invention, and is operated by receiving power from the battery pack 3.
[0153] The present invention will now be described in more detail with reference to specific examples.
[0154] [Example 1] It has a unimodal particle size distribution, D min = 1.78 μm, D 50 = 4.23 μm, D max = 13.1 μm, and the positive electrode active material is a mixture of single particles and pseudo-single particles (composition: Li[Ni 0.9 Co 0.06 Mn 0.03 Al 0.01 8 shows an SEM photograph of the positive electrode active material used in Example 1.
[0155] A positive electrode slurry was prepared by mixing the positive electrode active material, carbon nanotubes, and PVDF binder in a weight ratio of 97.8:0.6:1.6 in N-methylpyrrolidone, and the positive electrode slurry was applied to one side of an aluminum current collector sheet, dried at 120°C, and rolled to prepare a positive electrode plate.
[0156] Anode active material (graphite:SiO = 95:5 weight ratio mixture): conductive material (Super C): styrene-butadiene rubber (SBR): carboxymethyl cellulose (CMC) were mixed in water in a weight ratio of 96:2:1.5:0.5 to prepare anode slurry. The anode slurry was applied to one side of a copper current collector sheet, dried at 150°C, and rolled to prepare anode plate.
[0157] A separator was interposed between the positive and negative plates, and the plates were stacked in the order of separator / positive plate / separator / negative plate, and then wound up to prepare a jelly roll type electrode assembly. The electrode assembly prepared as above was inserted into a battery can, and an electrolyte was injected into the battery can to prepare a 4680 cell.
[0158] [Example 2] The positive electrode active material has a unimodal particle size distribution and is D min = 1.38 μm, D 50 = 4.69 μm, D max = 18.5 μm, and the positive electrode active material is a mixture of single particles and pseudo-single particles (composition: Li[Ni 0.9 Co 0.06 Mn 0.03 Al 0.01 ]O2) was used, a 4680 cell was manufactured in the same manner as in Example 1. FIG. 9 shows an SEM photograph of the positive electrode active material used in Example 2.
[0159] [Comparative Example 1] As a positive electrode active material, large particle size average particle size D 50 is 9μm, and the small particle average particle size D 50 The positive electrode active material (composition: Li[Ni 0.9 Co 0.05 Mn 0.04 Al 0.01 A 4680 cell was produced in the same manner as in Example 1, except that ]O2) was used.
[0160] [Comparative Example 2] The positive electrode active material has a unimodal particle size distribution and is D min = 0.892 μm, D 50 = 3.02 μm, D max = 11 μm, and the positive electrode active material is a mixture of single particles and pseudo-single particles (composition: Li[Ni 0.9 Co 0.06 Mn 0.03 Al 0.01 A 4680 cell was produced in the same manner as in Example 1, except that ]O2) was used.
[0161] FIG. 10 shows an SEM photograph of the positive electrode active material used in Comparative Example 2.
[0162] [Experimental Example 1] A hot box test was carried out on the 4680 cells manufactured according to Examples 1-2 and Comparative Examples 1-2.
[0163] Specifically, each of the 4680 cells manufactured according to Example 1 and Comparative Example 1 was placed in a hot box chamber at room temperature, and the temperature was raised to 130°C at a heating rate of 5°C / min and maintained for 30 minutes, after which the temperature change of the battery was measured. If no thermal runaway or ignition occurred during the test, it was indicated as Pass, and if thermal runaway and / or ignition occurred, it was indicated as Fail. In addition, for the accuracy of the test, the test was performed more than twice for the cells of Examples 1 and 2.
[0164] The measurement results are shown in Table 1 below and in Figures 11 and 12. Figure 11 is a graph showing the hot box test results of the 4680 cells manufactured according to Sample 1 of Example 1 and Comparative Example 1, and Figure 12 is a graph showing the hot box test results of the 4680 cells manufactured according to Samples 2 and 3 of Example 1, Samples 1 and 2 of Example 2, and Comparative Example 2.
[0165] [Table 1]
[0166] Referring to Table 1, FIG. 11 and FIG. 12, D min In the case of the cylindrical battery of Example 1, which uses a positive electrode active material having a single particle / pseudo-single particle form with a particle size of 1.0 μm or more, the voltage and temperature of the battery are stably maintained until 65 minutes have elapsed. minIt can be seen that the lithium secondary battery of Comparative Example 2, which uses a positive electrode active material having a single particle / quasi-single particle shape with a particle size of less than 1.0 μm, experienced a rapid increase in the temperature of the battery.
[0167] [Experimental Example 2] After rolling the positive electrode plates manufactured in Example 1 and Comparative Example 1, the positive electrode plates were cut using an ion milling device and the cross sections were photographed using an SEM to check the degree of cracking of the positive electrode active material particles. Fig. 13 shows an SEM cross-sectional image of the positive electrode plate manufactured in Example 1, and Fig. 14 shows an SEM cross-sectional image of the positive electrode plate manufactured in Comparative Example 1.
[0168] 13 and 14, the positive electrode plate of Example 1 had almost no cracks in the particles of the positive electrode active material even after rolling, whereas the positive electrode plate of Comparative Example 2, in which secondary particles were used, had many cracks in the particles of the positive electrode active material after rolling. [Explanation of symbols]
[0169] 10 Positive electrode plate 11 Negative plate 12 Separator 20 Current collector 21, 21a Active material layer 22, 22a, 22c, 146b Plain part 24 Insulating layer 140, 170 Cylindrical battery 141 Electrode assembly 142, 171 Battery can 143, 178 Sealed body 144 First current collecting plate 145, 176 Second current collecting plate 146 Insulators 152 Venting section 172 Rivet terminal 173 Second Gasket 147 Beading Section 148 Crimping section 149 Leads
Claims
1. A secondary battery comprising: an electrode assembly in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate are wound in one direction; a battery can in which the electrode assembly is housed; and a sealing body that seals an open end of the battery can, The positive electrode plate includes a positive electrode active material including a single particle, a pseudo-single particle, or a combination thereof, and the D of the positive electrode active material min The lithium secondary battery according to claim 1,
2. The positive electrode active material is D 50 The lithium secondary battery according to claim 1 , wherein the thickness of the first electrode is 5 μm or less.
3. The positive electrode active material is D max The lithium secondary battery according to claim 1, wherein the average particle diameter is 12 μm to 17 μm.
4. The lithium secondary battery according to claim 1 , wherein the positive electrode active material has a particle size distribution (PSD) represented by the following formula (1) of 3 or less. Formula (1): Particle size distribution (PSD) = (D max -D min ) / D 50
5. The lithium secondary battery according to claim 1 , wherein the positive electrode active material has a unimodal particle size distribution that exhibits a single peak in a volume cumulative particle size distribution graph.
6. The lithium secondary battery according to claim 1, wherein the single particle, pseudo-single particle, or a combination thereof is contained in an amount of 95% by weight to 100% by weight based on the total weight of the positive electrode active material contained in the positive electrode plate.
7. 2. The lithium secondary battery according to claim 1, wherein the positive electrode active material contains a lithium nickel-based oxide containing 80 mol % or more of Ni with respect to the total number of moles of transition metals.
8. The lithium secondary battery according to claim 1 , wherein the positive electrode active material comprises a lithium nickel-based oxide represented by the following Chemical Formula 1: [Chemical formula 1] Li a Ni b Co c M 1 d M 2 e O 2 In the above Chemical Formula 1, M 1 is Mn, Al or a combination thereof; M 2 are Zr, W, Ti, Mg, Ca, Sr, and Ba, and 0.8≦a≦1.2, 0.83≦b<1, 0<c<0.17, 0<d<0.17, and 0≦e≦0.
1.
9. 2. The lithium secondary battery according to claim 1, wherein the positive electrode active material has a primary particle having an average particle size of 0.5 μm to 5 μm.
10. The lithium secondary battery according to claim 1 , wherein the negative electrode plate comprises a silicon-based negative electrode active material.
11. The lithium secondary battery according to claim 1 , wherein the negative electrode plate comprises a silicon-based negative electrode active material and a carbon-based negative electrode active material.
12. The lithium secondary battery according to claim 11, wherein the silicon-based negative electrode active material and the carbon-based negative electrode active material are contained in a weight ratio of 1:99 to 20:
80.
13. 2. The lithium secondary battery according to claim 1, wherein the lithium secondary battery is a cylindrical battery having a form factor ratio of 0.4 or more, the form factor being a value obtained by dividing the diameter of a cylindrical battery by its height.
14. 14. The lithium secondary battery according to claim 13, wherein the lithium secondary battery is a 46110 cell, a 4875 cell, a 48110 cell, a 4880 cell or a 4680 cell.
15. each of the positive electrode plate and the negative electrode plate includes a plain portion on which no active material layer is formed; 2. The lithium secondary battery according to claim 1, wherein at least a portion of the uncoated portion of the positive or negative electrode plate defines an electrode tab.
16. the positive plate uncoated portion and the negative plate uncoated portion are formed on one end of one side of the positive plate and the negative plate along a direction in which the electrode assembly is wound, A current collecting plate is coupled to each of the positive electrode uncoated portion and the negative electrode uncoated portion, The lithium secondary battery according to claim 15 , wherein the current collecting plate is connected to an electrode terminal.
17. The positive electrode plate uncoated portion and the negative electrode plate uncoated portion are processed into a plurality of segmented pieces that can be bent independently, The lithium secondary battery according to claim 16 , wherein at least some of the plurality of segment pieces are bent toward the winding center of the electrode assembly.
18. At least a portion of the folded segments overlaps an upper end and a lower end of the electrode assembly, 18. The lithium secondary battery according to claim 17, wherein the current collecting plates are bonded onto the overlapping segments.
19. The lithium secondary battery according to claim 15 , further comprising an insulating layer formed on the positive electrode plate in a direction parallel to the winding direction, the insulating layer covering a portion of the positive electrode active material layer and a portion of the uncoated portion.
20. A battery pack comprising the lithium secondary battery according to any one of claims 1 to 19.
21. 21. A motor vehicle comprising the battery pack of claim 20.
Citation Information
Patent Citations
Secondary battery
JP2001148238A
Positive electrode active material for nonaqueous electrolyte secondary battery, production of positive electrode active material for nonaqueous electrolyte secondary battery, positive electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery
JP2021051909A
Method for producing positive electrode active material for secondary battery
JP2021516425A