Secondary batteries and their use

The secondary battery design addresses poor low-temperature performance by optimizing electrolytic solution composition and electrode structure, enhancing lithium ion transport and reducing impedance for improved capacity retention.

JP2024538462AActive Publication Date: 2024-10-22SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD

Patent Information

Application Number
JP2024523526
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-14
Filing Date
2022-12-16
Publication Date
2024-10-22
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

Lithium-ion batteries exhibit poor dynamic characteristics and low capacity retention in low-temperature environments, limiting their large-scale use.

Method used

A secondary battery design comprising a specific composition of electrolytic solution with cyclic and chain ester solvents, optimized conductivity, viscosity, and additive ratios, along with a positive and negative electrode structure, to enhance lithium ion transport and reduce impedance.

Benefits of technology

The optimized battery design improves dynamic characteristics and capacity retention at low temperatures, preventing lithium elution and maintaining high performance under cold conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538462000001_ABST
    Figure 2024538462000001_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of batteries, and more specifically, to a secondary battery. The secondary battery according to the present application includes a positive electrode plate, a negative electrode plate, and an electrolyte, the electrolyte includes an organic solvent, the organic solvent includes a cyclic ester solvent and a chain ester solvent, and the parameters of the secondary battery satisfy the following relational expression (1). The secondary battery has good dynamic characteristics at low temperatures by adjusting the electrolyte and the negative electrode plate to make them act synergistically, and has good capacity retention and low impedance under low temperature conditions.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims priority to a Chinese patent application bearing application number 202211260215.8 and entitled "Secondary Battery" filed with the State Intellectual Property Office of the People's Republic of China on October 14, 2022, the entire contents of which are incorporated herein by reference. [Technical field]

[0002] The present application relates to the technical field of batteries, and more particularly to secondary batteries. [Background technology]

[0003] Secondary batteries, such as lithium-ion batteries, have become the most popular energy storage system due to their characteristics of high specific energy, long life, and environmental friendliness, and are currently widely used in the fields of home appliances, electric vehicles, energy storage, etc. With the popularity of new energy vehicles and the rapid development of the energy storage market, the requirements for the performance of lithium-ion batteries are constantly improving, and the development of low-cost, highly safe, and widely applicable lithium-ion batteries is currently an urgent need for the development of the lithium battery industry.

[0004] Secondary batteries have drawbacks such as low capacity retention and high impedance in low-temperature environments, which limits their large-scale use. Therefore, it is necessary to improve the dynamic characteristics of secondary batteries at low temperatures. Summary of the Invention [Problem to be solved by the invention]

[0005] Therefore, the technical problem to be solved by the present application is to provide a lithium ion battery that overcomes the drawbacks of the prior art, such as poor dynamic characteristics at low temperatures, of lithium ion batteries. [Means for solving the problem]

[0006] To this end, the present application provides the following technical solutions:

[0007] The present application relates to a secondary battery including a positive electrode plate, a negative electrode plate, and an electrolyte, the negative electrode plate including a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the electrolyte including an organic solvent, the organic solvent including a cyclic ester solvent and a chain ester solvent, A secondary battery is provided that satisfies the following relational formula (1):

number

[0008] Preferably, the secondary battery comprises: (1) the mass ratio β of the cyclic ester solvent to the chain ester solvent is 0.25 to 0.85, preferably 0.33 to 0.82; (2) the electrical conductivity σ of the electrolyte is 9 to 13, preferably 9.5 to 12.5; (3) the viscosity η of the electrolyte is 2 to 5, preferably 2.5 to 4.5; (4) The weight value Mel. of the electrolyte is 11 to 16, preferably 13 to 15.

[0009] Preferably, the value of PD is from 1.1 to 1.65, preferably from 1.2 to 1.6.

[0010] Preferably, the chain ester solvent comprises at least one of a chain carbonate and a chain carboxylate, The chain carbonate includes at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, and methyl propyl carbonate, The chain carboxylate includes at least one of ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, and ethyl butyrate.

[0011] Preferably, the cyclic ester solvent comprises at least one of ethylene carbonate, propylene carbonate, and butylene carbonate.

[0012] Preferably, the electrolyte further comprises an additive, the additive comprising at least one of a silicon-containing additive, a cyclic carbonate additive, or a sulfur-containing additive.

[0013] Preferably, the additive is (a) the silicon-containing additive includes at least one of tris(trimethylsilyl) phosphite, tris(trimethylsilyl) phosphate, tris(trimethylsilyl) borate, trimethylfluorosilane, and heptamethyldisilazane, and the silicon-containing additive is 0.1 to 4 mass% with respect to the mass of the electrolyte; (b) the cyclic carbonate additive includes at least one of vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, and difluoroethylene carbonate, and the content of the cyclic carbonate additive is 0.05 to 3 mass% relative to the mass of the electrolytic solution; (c) The sulfur-containing additive includes at least one of 1,3-propane sultone and vinyl sulfate, and the sulfur-containing additive is present in an amount of 0.05 to 3 mass % relative to the mass of the electrolyte.

[0014] Preferably, the electrolyte additive comprises a silicon-containing additive and a sulfur-containing additive, and the content of the silicon-containing additive relative to the mass of the electrolyte is W si %, and the content of the sulfur-containing additive is W s %, and 0.3≦W si +W s ≦4, 0.1≦W si / W s Satisfy ≦5.

[0015] Preferably, the electrolyte further comprises a lithium salt additive, the lithium salt additive comprising at least one of lithium bisfluorosulfonylimide, lithium bistrifluoromethanesulfonylimide, lithium difluorooxalyl borate, lithium difluorophosphate, and lithium difluorooxalyl phosphate; The lithium salt additive in the electrolyte solution is 0.1 to 5% by mass.

[0016] Preferably, the positive electrode plate includes a positive electrode current collector and a positive electrode active material layer provided on the positive electrode current collector, the positive electrode active material layer including a positive electrode active material, The positive electrode active material is Li a Fe 1-y Mn y Includes PO4 (0.9≦a≦1.1, 0≦y≦1).

[0017] The active material layer in the negative electrode plate contains at least one of graphite and silicon-based materials.

[0018] The present application also provides an electric device including the above-mentioned secondary battery. Effect of the Invention

[0019] The technical solution of this application has the following advantages: The secondary battery according to the present application includes a positive plate, a negative plate, and an electrolyte, the electrolyte includes an organic solvent, the organic solvent includes a cyclic ester solvent and a chain ester solvent, and the secondary battery satisfies the relational formula (1). The secondary battery has good dynamic characteristics at low temperatures, good capacity retention rate and low impedance under low temperature conditions, and generally does not cause lithium elution, by optimizing the composition and content of the electrolyte and adjusting the active material layer of the negative plate. The electrolyte is one of the main components of a lithium ion battery and is one of the factors that affect the performance of the secondary battery. The solvent is an important component of the electrolyte and greatly affects the performance of the secondary battery, such as the cycle, impedance, and dynamic characteristics. The present application optimizes the electrolyte, the negative plate, and the battery capacity, and comprehensively designs parameters such as the composition of the electrolyte solvent, the viscosity of the electrolyte, the electrical conductivity, and the battery capacity, thereby greatly improving the dynamic characteristics of the secondary battery at low temperatures, reducing the impedance of the secondary battery, and increasing the low-temperature capacity retention rate. Among these, cyclic ester solvents have a high dielectric constant and a high viscosity, while chain ester solvents have a low dielectric constant and a low viscosity. Controlling the ratio of the cyclic ester solvent to the chain ester solvent within an appropriate range contributes to improving the dynamic characteristics of the secondary battery. In the secondary battery according to the present application, the viscosity of the electrolyte affects the migration speed of lithium ions in the electrolyte, and if the viscosity of the electrolyte is within the range of the present application, the transport of lithium ions is further improved, the impedance of the secondary battery is reduced, and the cycle characteristics of the battery are improved. In addition to satisfying the following relational formula (1), the small viscosity of the electrolyte promotes the transport of lithium ions in the electrolyte, and the dynamic characteristics are further improved. By limiting the electrical conductivity of the electrolyte, it is possible to more reliably prevent phenomena such as lithium elution during high current operation. The amount of electrolyte injected into a secondary battery is affected by the design capacity of the battery. If the amount is too small, it is difficult to completely impregnate the positive and negative electrodes, which will affect the degree of lithium ion deintercalation during the charge and discharge process, and affect problems such as impedance, capacity, cycle, and lithium elution of the secondary battery. If the amount is too large, side reactions will increase, causing gas generation and swelling. If the compression density PD of the negative electrode active material layer in the negative electrode plate is too small, the energy density of the battery will be affected and the application process of the negative electrode slurry will be difficult to control, and if the compression density PD is too high, the electrolyte will be difficult to impregnate into the negative electrode active material layer, which will affect the dynamic properties of the battery. By setting an appropriate compression density PD, the dynamic properties and energy density of the battery can be further improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The following examples are provided for a better understanding of the present application, and are not limited to the best embodiment, and are not intended to limit the content and scope of protection of the present application; any products identical or similar to those of the present application that someone obtains based on the present application or as a result of combining the features of the present application with other prior art shall be included within the scope of protection of the present application.

[0021] The present application relates to a battery comprising a positive electrode plate, a negative electrode plate, and an electrolyte, the negative electrode plate including a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the electrolyte including an organic solvent, the organic solvent including a cyclic ester solvent and a chain ester solvent, A secondary battery is provided that satisfies the following relational formula (1):

number

[0022] In some embodiments of the present application,

number

[0023] In some embodiments of the present application, the mass ratio β of the cyclic ester solvent to the chain ester solvent is 0.25 to 0.85. For example, it may be 0.25, 0.30, 0.33, 0.35, 0.38, 0.40, 0.43, 0.45, 0.47, 0.50, 0.53, 0.55, 0.57, 0.60, 0.63, 0.65, 0.67, 0.70, 0.72, 0.74, 0.78, 0.80, 0.82, 0.85, or a range consisting of any two of these values. When the mass ratio P of the cyclic ester solvent to the chain ester solvent is in the above range, the viscosity of the electrolyte and the conductivity of the electrolyte are relatively stable, the diffusion of lithium ions at low temperatures is facilitated, the dynamic behavior of lithium ions is maintained, and the risk of lithium elution is reduced.

[0024] In some embodiments of the present application, the mass ratio β of the cyclic ester solvent to the chain ester solvent is 0.33 to 0.82.

[0025] In some embodiments of the present application, the value of the conductivity σ of the electrolyte is 9 to 13. For example, it may be 9, 9.3, 9.5, 9.7, 10.0, 10.4, 10.7, 11.0, 11.3, 11.5, 11.7, 12.0, 12.2, 12.4, 12.5, 12.7, 13.0, or a range consisting of any two of these values. When the conductivity of the electrolyte is in the above range, the lithium ions in the electrolyte can diffuse quickly, and the lithium ions released from the positive electrode can reach the negative electrode faster, which can increase the potential of the negative electrode, effectively improve the dynamic properties of the lithium ions, and further improve the lithium elution at low temperatures.

[0026] In some embodiments of the present application, the electrolytic solution has a conductivity σ value of 9.5 to 12.5.

[0027] The conductivity of the electrolyte can be measured by a DDSJ-308A type conductivity meter.

[0028] In some embodiments of the present application, the viscosity η of the electrolyte is 2 to 5. For example, it may be 2, 2.2, 2.4, 2.6, 2.8, 3.0, 3.3, 3.5, 3.7, 3.9, 4.0, 4.2, 4.4, 4.6, 4.8, 5.0, or a range consisting of any two of these values. When the viscosity η of the electrolyte is in the above range, the larger the η, the higher the viscosity of the electrolyte, which adversely affects the diffusion of lithium ions at low temperatures, reduces the dynamic behavior of lithium ions, and brings about the risk of lithium elution.

[0029] In some embodiments of the present application, the viscosity η of the electrolyte is 2.5 to 4.5.

[0030] In this application, the viscosity of the electrolyte may be measured using a 1835 Ubbelohde viscometer.

[0031] In some embodiments of the present application, the weight value of the electrolyte, Mel. teeth It is 11 to 16. For example, it may be 11, 11.2, 11.5, 11.7, 12, 12.2, 12.4, 12.8, 13, 13.3, 13.5, 13.7, 14, 14.3, 14.5, 14.7, 15, 15.5, 16, or a range consisting of any two of these values. When the weight of the electrolyte is in the above range, the amount of circulating gas generated by the battery is within an appropriate range, and the battery internal pressure is prevented from excessively increasing, causing the explosion-proof valve to burst and the battery to break down, and the black spots of bubbles generated at the interface of the negative electrode plate can be reduced, and the electrolyte can move lithium ions well, improving the cycle characteristics and dynamic characteristics of the battery.

[0032] In some embodiments of the present application, the weight value Mel. of the electrolyte is 13 to 15. When Mel. is in this range, the electrolyte can transfer lithium ions better, while the amount of gas generated by the battery is less, and the overall performance of the battery is better.

[0033] In some embodiments of the present application, the Mel. / Cap. value is 3-6.

[0034] In some embodiments of the present application, the value of the PD is 1.1 to 1.65. When the PD is in the above range, the compressed density affects the movement of lithium ions in the negative electrode, and if the compressed density is too high, the diffusion speed of lithium ions decreases, and especially at low temperatures, the low-temperature performance is affected, causing lithium elution, and if the compressed density is too high, it affects the impregnation of the electrolyte.

[0035] In some embodiments of the present application, the value of PD is 1.2 to 1.6.

[0036] In some embodiments herein, the linear ester solvent comprises at least one of a linear carbonate and a linear carboxylate.

[0037] In some embodiments of the present application, the linear carbonate includes at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, and methyl propyl carbonate.

[0038] In some embodiments of the present application, the linear carboxylate comprises at least one of ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, and ethyl butyrate.

[0039] In some embodiments herein, the cyclic ester solvent comprises at least one of ethylene carbonate, propylene carbonate, and butylene carbonate.

[0040] In some embodiments herein, the electrolyte further comprises an additive, the additive comprising at least one of a silicon-containing additive, a cyclic carbonate additive, or a sulfur-containing additive.

[0041] In some embodiments herein, the silicon-containing additive comprises at least one of tris(trimethylsilyl) phosphite, tris(trimethylsilyl) phosphate, tris(trimethylsilyl) borate, trimethylfluorosilane, or heptamethyldisilazane.

[0042] In some embodiments of the present application, the silicon-containing additive is present in an amount of 0.1 to 4% by weight based on the weight of the electrolyte.

[0043] In some embodiments herein, the cyclic carbonate additive comprises at least one of vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, or difluoroethylene carbonate.

[0044] In some embodiments of the present application, the cyclic carbonate additive is present in an amount of 0.05 to 3% by mass relative to the mass of the electrolyte.

[0045] In some embodiments herein, the sulfur-containing additive comprises at least one of 1,3-propane sultone or vinyl sulfate.

[0046] In some embodiments of the present application, the sulfur-containing additive is present in an amount of 0.05 to 3% by weight based on the weight of the electrolyte.

[0047] In some embodiments of the present application, the electrolyte additive comprises a silicon-containing additive and a sulfur-containing additive, and the content of the silicon-containing additive relative to the mass of the electrolyte is W si %, and the content of the sulfur-containing additive is W s %, and 0.3≦W si +W s ≦4. When the electrolyte contains a silicon-containing additive and a sulfur-containing additive at the same time, they can form an SEI film with a relatively low impedance, and lithium ions can pass through the SEI film quickly. When the total content of the two is within the above range, the film formation state is better, and the quality and thickness of the formed protective film are both good, and the diffusibility of lithium ions is improved.

[0048] In some embodiments of the present application, the electrolyte additive comprises a silicon-containing additive and a sulfur-containing additive, and the content of the silicon-containing additive relative to the mass of the electrolyte is W si %, and the content of the sulfur-containing additive is W s %, and 0.1≦W si / W s ≦5. W si / W s When the amount of the protective film is within the above range, the composition and thickness of the protective film formed can be further optimized, and the overall characteristics of the battery can be further improved.

[0049] In some embodiments of the present application, the electrolyte further comprises a lithium salt additive, and the lithium salt additive comprises at least one of lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium difluorooxalyl borate, lithium difluorophosphate, and lithium difluorooxalyl phosphate. When the electrolyte comprises the lithium salt additive, the impedance of the membrane can be further reduced, the stability of membrane formation can be improved, the diffusivity of lithium ions can be improved, and cycle characteristics can be considered.

[0050] In some embodiments of the present application, the lithium salt additive in the electrolyte is 0.1 to 5% by weight.

[0051] In some embodiments of the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode active material layer provided on the positive electrode current collector, The positive electrode active material is Li a Fe 1-y Mn y Includes PO4 (0.9≦a≦1.1, 0≦y≦1).

[0052] In some embodiments of the present application, the positive electrode active material may further include a doping element. The type of the doping element is not limited as long as it can improve the performance of the positive electrode active material.

[0053] In some embodiments of the present application, the positive electrode active material has a coating layer on its surface.

[0054] In some embodiments of the present application, the coating layer includes a coating element, and the coating element is not limited as long as it can improve the stability of the positive electrode active material.

[0055] In some embodiments of the present application, a carbon material layer is included on a surface of the positive electrode active material, the carbon material layer including amorphous carbon.

[0056] Phosphate-based positive electrode active materials are widely used in lithium batteries due to their advantages of low cost and high safety. However, phosphate-based positive electrode active materials have poor low-temperature mechanical properties, so by combining the phosphate-based positive electrode active material with the electrolyte and negative electrode plate of the present application, the low-temperature performance of the battery can be significantly improved, and the electrolyte, the phosphate-based positive electrode active material, and the negative electrode plate of the present application all have good compatibility, and the impedance of the film formed can be reduced, the stability can be improved, and the cycle characteristics can be taken into consideration, and the lithium elution at low temperatures can be effectively improved.

[0057] If specific experimental steps or conditions are not described in the examples, they can be carried out according to the conventional experimental steps or conditions described in the literature in the field. If the manufacturers of the reagents or instruments used are not specified, they are all ordinary reagent products that can be purchased on the market. Example 1

[0058] This embodiment provides a lithium ion secondary battery, which has a designed theoretical capacity Cap. of 3.5 Ah, and includes a positive electrode plate, a negative electrode plate, and an electrolyte. Positive electrode plate: Positive electrode active material LiFePO4, conductive agent SP, binder PVDF (HSV900 manufactured by Arkema, same below) were mixed in a mass ratio of 96:2:2, NMP was added, and the system was stirred under vacuum until it became homogeneous to obtain a positive electrode slurry. The positive electrode slurry was applied onto an aluminum foil positive electrode current collector, baked, and cold pressed to obtain a compressed density of 2.45 g / cm. 3 Thus, a positive electrode plate having the positive electrode active material layer was obtained. Negative electrode plate: Graphite, conductive agent SP, thickener CMC, binder SBR (Zeon Corporation 451B, same below) were mixed in a mass ratio of 96.2:1.2:1.2:1.4, deionized water was added, and the mixture was stirred under vacuum until the system became homogeneous to obtain a negative electrode slurry. The negative electrode slurry was applied onto the copper foil of the negative electrode current collector, dried, and cold pressed to obtain a compressed density of 1.55 g / cm. 3 Thus, a negative electrode plate having the negative electrode active material layer was obtained. Electrolyte: Ethylene carbonate (EC, cyclic ester solvent), methyl ethyl carbonate (EMC, chain carbonate solvent), and dimethyl carbonate (DMC, chain carbonate solvent) were mixed in a ratio of 30:40:30 to obtain an organic solvent, LiPF6 was added to the organic solvent, and after uniform mixing, vinylene carbonate, vinyl sulfate, lithium difluorophosphate, and tris(trimethylsilyl) phosphate were added to obtain an electrolyte. Here, the content of LiPF6 was 12 mass%, the content of vinylene carbonate was 1 mass%, the content of vinyl sulfate was 1.5 mass%, the content of lithium difluorophosphate was 0.5 mass%, the content of tris(trimethylsilyl) phosphate was 1 mass%, the mass ratio β of the cyclic ester solvent to the chain ester solvent was 0.43, the conductivity of the electrolyte was 11.28 mS / cm, and the viscosity of the electrolyte was 3.46 mPa·s. A positive electrode plate, a separator (14PP manufactured by Sungyuan Materials Co., Ltd.), and a negative electrode plate were stacked in this order, and the separator was placed between the positive and negative electrodes, and the stack was wound to obtain an electrode assembly. The electrode assembly was packaged in an aluminum plastic film, dried, and 14 g of electrolyte was poured into it, packaged, left to stand, formed, and hot pressed to obtain a secondary battery. Example 2

[0059] The compressed density of the negative electrode active material layer is 1.6 g / cm 3 Other than that, the results were the same as in Example 1. Example 3

[0060] The compressed density of the negative electrode active material layer is 1.45 g / cm 3 Other than that, the results were the same as in Example 1. Example 4

[0061] In the manufacturing method, the electrolyte solution was specifically a mixture of ethylene carbonate (EC, cyclic ester solvent), methyl ethyl carbonate (EMC, chain carbonate solvent), dimethyl carbonate (DMC, chain carbonate solvent), and ethyl acetate (EA, chain carboxylate solvent) in a ratio of 30:30:30:10. The obtained electrolyte solution had a mass ratio β of cyclic ester solvent to chain ester solvent of 0.43, a conductivity of 11.44 mS / cm, and a viscosity of 3.32 mPa s, which were the same as those in Example 1. Example 5

[0062] In the manufacturing method, the electrolyte solution was specifically a mixture of ethylene carbonate (EC, cyclic ester solvent), methyl ethyl carbonate (EMC, chain carbonate solvent), and dimethyl carbonate (DMC, chain carbonate solvent) in a ratio of 27:40:33. The obtained electrolyte solution had a mass ratio β of cyclic ester solvent to chain ester solvent of 0.37, a conductivity of 11.09 mS / cm, and a viscosity of 3.37 mPa s, which were the same as those in Example 1. Example 6

[0063] In the manufacturing method, the electrolyte solution was specifically a mixture of ethylene carbonate (EC, cyclic ester solvent), methyl ethyl carbonate (EMC, chain carbonate solvent), and dimethyl carbonate (DMC, chain carbonate solvent) in a ratio of 25:45:30. The obtained electrolyte solution had a mass ratio β of cyclic ester solvent to chain ester solvent of 0.33, a conductivity of 10.75 mS / cm, and a viscosity of 3.3 mPa s, which were the same as those in Example 1. Example 7

[0064] In the manufacturing method, the electrolyte solution was specifically a mixture of ethylene carbonate (EC, cyclic ester solvent), methyl ethyl carbonate (EMC, chain carbonate solvent), and dimethyl carbonate (DMC, chain carbonate solvent) in a ratio of 32:40:28. The obtained electrolyte solution had a mass ratio β of cyclic ester solvent to chain ester solvent of 0.47, a conductivity of 11.52 mS / cm, and a viscosity of 3.48 mPa s, which were the same as those in Example 1. Example 8

[0065] In the production method, the electrolyte did not contain vinyl sulfate, and the obtained electrolyte had a mass ratio β of the cyclic ester solvent to the chain ester solvent of 0.43, a conductivity of 11.18 mS / cm, and a viscosity of 3.34 mPa s, which were the same as in Example 1. Example 9

[0066] In the production method, the electrolyte did not contain vinyl sulfate and tris(trimethylsilyl) phosphate, and the obtained electrolyte had a mass ratio β of the cyclic ester solvent to the chain ester solvent of 0.43, a conductivity of 11.02 mS / cm, and a viscosity of 3.4 mPa s, which were the same as in Example 1. Example 10

[0067] In the production method, the electrolyte did not contain vinyl sulfate, lithium difluorophosphate, or tris(trimethylsilyl) phosphate, and the obtained electrolyte had a mass ratio β of cyclic ester solvent to chain ester solvent of 0.43, a conductivity of 10.85 mS / cm, and a viscosity of 3.42 mPa s, which were the same as in Example 1. Example 11

[0068] In the production method, specifically, 0.5% lithium difluorophosphate, 1% tris(trimethylsilyl) phosphate, and 1.5% vinyl sulfate were added to the electrolyte, and the obtained electrolyte had a mass ratio β of the cyclic ester solvent to the chain ester solvent of 0.43, a conductivity of the electrolyte of 11.12 mS / cm, and a viscosity of the electrolyte of 3.39 mPa s, which were the same as those in Example 1. Example 12

[0069] In the production method, specifically, 1.0% vinylene carbonate, 0.5% lithium difluorophosphate, 0.2% vinyl sulfate, and 1% tris(trimethylsilyl) phosphate were added to the electrolyte, and the obtained electrolyte had a mass ratio β of the cyclic ester solvent to the chain ester solvent of 0.43, a conductivity of the electrolyte of 11.14 mS / cm, and a viscosity of the electrolyte of 3.41 mPa s, which were the same as those in Example 1. Example 13

[0070] In the production method, specifically, 1.0% vinylene carbonate, 0.5% lithium difluorophosphate, 0.7% vinyl sulfate, and 1.6% tris(trimethylsilyl)phosphate were added to the electrolyte, and the obtained electrolyte had a mass ratio β of the cyclic ester solvent to the chain ester solvent of 0.43, a conductivity of 11.25 mS / cm, and a viscosity of 3.38 mPa s, which were the same as in Example 1. Example 14

[0071] In the production method, specifically, 1.0% vinylene carbonate, 0.5% lithium difluorophosphate, 2% vinyl sulfate, and 0.15% tris(trimethylsilyl)phosphate were added to the electrolyte, and the obtained electrolyte had a mass ratio β of the cyclic ester solvent to the chain ester solvent of 0.43, a conductivity of the electrolyte of 11.21 mS / cm, and a viscosity of the electrolyte of 3.36 mPa s, which were the same as those in Example 1. Example 15

[0072] In the production method, the electrolyte was prepared by adding 1.0% vinylene carbonate, 0.5% lithium difluorophosphate, 1.5% vinyl sulfate, and 3% tris(trimethylsilyl)phosphate. The obtained electrolyte had a mass ratio β of the cyclic ester solvent to the chain ester solvent of 0.43, a conductivity of 11.33 mS / cm, and a viscosity of 3.33 mPa s, which were the same as those in Example 1. Example 16

[0073] In the production method, specifically, 1.0% vinylene carbonate, 0.5% lithium difluorophosphate, 2.5% vinyl sulfate, and 3% tris(trimethylsilyl) phosphate were added to the electrolyte, and the obtained electrolyte had a mass ratio β of the cyclic ester solvent to the chain ester solvent of 0.43, a conductivity of the electrolyte of 11.32 mS / cm, and a viscosity of the electrolyte of 3.35 mPa s, which were the same as those in Example 1. Example 17

[0074] The manufacturing method was the same as in Example 1, except that the mass of the electrolyte was different; specifically, the amount of electrolyte injected was 13 g. Example 18

[0075] The manufacturing method was the same as in Example 1, except that the amount of electrolyte injected was specifically 16 g. Example 19

[0076] The manufacturing method differs in the compressed density of the negative electrode. Specifically, the density of the negative electrode active material layer is 1.68 g / cm 3 Other than that, the results were the same as in Example 1. Comparative Example 1

[0077] In the manufacturing method, the electrolyte solution was specifically a mixture of ethylene carbonate (EC, cyclic ester solvent), methyl ethyl carbonate (EMC, chain carbonate solvent), and dimethyl carbonate (DMC, chain carbonate solvent) in a ratio of 40:30:30. The obtained electrolyte solution had a mass ratio β of cyclic ester solvent to chain ester solvent of 0.67, a conductivity of 12.01 mS / cm, and a viscosity of 3.74 mPa s, which were the same as those in Example 1. Comparative Example 2

[0078] In the manufacturing method, the electrolyte solution was specifically a mixture of ethylene carbonate (EC, cyclic ester solvent), methyl ethyl carbonate (EMC, chain carbonate solvent), and dimethyl carbonate (DMC, chain carbonate solvent) in a ratio of 40:40:20. The obtained electrolyte solution had a mass ratio β of cyclic ester solvent to chain ester solvent of 0.67, a conductivity of 11.84 mS / cm, and a viscosity of 4.05 mPa s, which were the same as those in Example 1. Comparative Example 3

[0079] In the manufacturing method, the electrolyte was specifically a mixture of ethylene carbonate (EC, cyclic ester solvent), methyl ethyl carbonate (EMC, chain carbonate solvent), and dimethyl carbonate (DMC, chain carbonate solvent) in a ratio of 40:15:45. The obtained electrolyte had a mass ratio β of the cyclic ester solvent to the chain ester solvent of 0.67, a conductivity of the electrolyte of 12.19 mS / cm, and a viscosity of 3.66 mPa s, which were the same as those in Example 1. Comparative Example 4

[0080] In the manufacturing method, the electrolyte was specifically a mixture of ethylene carbonate (EC, cyclic ester solvent), methyl ethyl carbonate (EMC, chain carbonate solvent), and dimethyl carbonate (DMC, chain carbonate solvent) in a ratio of 48:26:26. The obtained electrolyte had a mass ratio β of cyclic ester solvent to chain ester solvent of 0.92, a conductivity of 12.13 mS / cm, and a viscosity of 4.43 mPa s, which were the same as those in Example 1. Comparative Example 5

[0081] In the production method, specifically, 3.5% vinylene carbonate, 0.5% lithium difluorophosphate, 1% tris(trimethylsilyl) phosphate, and 1.5% vinyl sulfate were added to the electrolyte, and the obtained electrolyte had a mass ratio β of the cyclic ester solvent to the chain ester solvent of 0.43, a conductivity of 10.97 mS / cm, and a viscosity of 3.68 mPa s, which were the same as in Example 12. Comparative Example 6

[0082] The manufacturing method was the same as in Example 1, except that the mass of the electrolyte was different; specifically, the amount of electrolyte injected was 10 g. Comparative Example 7

[0083] In the manufacturing method, the electrolyte solution was specifically a mixture of ethylene carbonate (EC, cyclic ester solvent), methyl ethyl carbonate (EMC, chain carbonate solvent), and dimethyl carbonate (DMC, chain carbonate solvent) in a ratio of 20:40:40. The obtained electrolyte solution had a mass ratio β of cyclic ester solvent to chain ester solvent of 0.25, a conductivity of 10.48 mS / cm, and a viscosity of 3.11 mPa s, which were the same as those in Example 1. In each of the Examples and Comparative Examples, the conductivity of the electrolyte is measured at 25°C using a conductivity meter, and the viscosity of the electrolyte is measured at 25°C using a viscometer. Test Example

[0084] This test example provides performance test results of the lithium ion secondary batteries according to the examples and comparative examples, and is specifically as follows. Test method for battery capacity retention rate: The battery was fully charged to the upper limit voltage, and discharged to the lower limit voltage at a discharge current of 1C at a temperature of 25°C, and the discharge capacity was taken as C0. It was fully charged again to the upper limit voltage at 25°C, and the temperature was adjusted to -20°C, and the battery was discharged to the lower limit voltage at a discharge current of 1C, and the discharge capacity was taken as C1. The capacity retention rate of a lithium-ion secondary battery at -20°C is C1 / C0. Battery DCR (impedance) test method: Adjust the remaining capacity to 50% SOC at 25℃ with a discharge current of 1C, adjust the temperature to -25℃, discharge at 0.36C for 10s, and calculate the discharge DCR at -25℃ using the formula △U / I, where △U is the change in voltage before and after discharge, and I is the discharge current. Battery lithium dissolution test method: Adjust the temperature to -10℃, charge to the upper voltage limit with a charging current of 0.13C, discharge to the lower voltage limit with a discharging current of 1C, perform 10 charge and discharge cycles, adjust the temperature to 25℃, charge to the upper voltage limit with a charging current of 1C, disassemble the battery, and observe whether lithium dissolution occurs at the interface. If the area of ​​the lithium dissolution area on the negative plate surface is less than 2%, it is considered that there is no lithium dissolution; if the area of ​​the lithium dissolution area on the negative plate surface is 2% or more but less than 5%, it is considered that there is slight lithium dissolution; if the area of ​​the lithium dissolution area on the negative plate surface is 5% to 50%, it is considered that there is lithium dissolution; if the area of ​​the lithium dissolution area on the negative plate surface is more than 50%, it is considered that there is serious lithium dissolution. [Table 1] TIFF2024538462000006.tif167170

[0085] From the experimental results shown in Table 1, when the parameters of the organic solvent, the negative electrode plate, and the electrode assembly in the secondary battery satisfy a specific relationship, the secondary battery has a good capacity retention rate and low impedance under low temperature conditions, and the lithium dissolution phenomenon hardly occurs, although slight lithium dissolution was observed individually (Example 15).

[0086] Specifically, when comparing Comparative Example 1, Examples 4 to 6, and Comparative Example 4,

number

[0087] Compared with Example 1,

number

[0088] Comparing Examples 1 to 3 with Example 19, when the compression density is too high,

number

[0089] In Examples 17 to 18 and Comparative Example 6, the change in the amount of electrolyte injected is different from that in Example 1. When the amount of electrolyte injected is too low,

number

[0090] The data from Example 1, Examples 8 to 16, and Comparative Example 5 show that the difference in additives does not have a large effect on the viscosity and conductivity of the electrolyte, and that even when a certain additive is used in excess, lithium dissolves, as in Comparative Example 5. Secondary batteries manufactured with different additive systems do not essentially dissolve lithium at low temperatures, but have different capacity retention rates and impedances. Moreover, under the cooperative action of the cyclic carbonate additive, silicon-containing additive, sulfonate ester additive, and lithium salt additive, parameters such as the electrolyte, the active material layer of the negative electrode plate, and the weight of the electrolyte in the secondary battery are rationally designed and rationally quantified,

number

[0091] From the data of Example 1 and Examples 12 to 16, it is clear that 0.3≦W si +W s ≦4, 0.1≦W si / W s If ≦5, the secondary battery has better overall performance.

[0092] Obviously, the above examples are merely illustrative and are not intended to limit the embodiments. Those skilled in the art can make other different forms of changes or modifications based on the above description. It is not necessary and cannot be possible to cover all the embodiments here. Any obvious changes or modifications thus made are also included in the scope of protection of the present application.

Claims

1. A secondary battery including a positive electrode plate, a negative electrode plate, and an electrolyte, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the electrolytic solution includes an organic solvent, the organic solvent includes a cyclic ester solvent and a chain ester solvent, A secondary battery characterized by satisfying the following relational formula (1): [0010] (Here, Mel. is the weight of the electrolyte in the secondary battery, and the unit of weight is g, σ is the conductivity value of the electrolyte, the unit of conductivity being mS / cm; Cap. is the value of the theoretical capacity designed for the secondary battery, and the unit of the designed theoretical capacity is Ah; PD is the value of the compressed density of the negative electrode active material layer, and the unit of compressed density is g / cm 3 and η is the viscosity value of the electrolyte, the unit of viscosity being mPa s; β is the mass ratio of the cyclic ester solvent to the chain ester solvent in the electrolyte.

2. (1) the mass ratio β of the cyclic ester solvent to the chain ester solvent is 0.25 to 0.85; (2) the electrical conductivity σ of the electrolyte is 9 to 13; (3) the viscosity η of the electrolyte is 2 to 5; (4) The secondary battery according to claim 1, wherein the weight value Mel. of the electrolyte is 11 to 16.

3. 2. The secondary battery according to claim 1, wherein a mass ratio β of the cyclic ester solvent to the chain ester solvent is 0.33 to 0.

82.

4. 2. The secondary battery according to claim 1, wherein the electrolytic solution has a conductivity σ of 9.5 to 12.

5.

5. 2. The secondary battery according to claim 1, wherein the viscosity η of the electrolyte is 2.5 to 4.

5.

6. 2. The secondary battery according to claim 1, wherein the weight value of the electrolyte is 13 to 15 Mel.

7. 7. The secondary battery according to claim 1, wherein the PD value is 1.1 to 1.

65.

8. The chain ester solvent contains at least one of a chain carbonate and a chain carboxylate, The chain carbonate includes at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, and methyl propyl carbonate, 2. The secondary battery according to claim 1, wherein the chain carboxylate includes at least one of ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, and ethyl butyrate.

9. The secondary battery according to claim 1 , wherein the cyclic ester solvent contains at least one of ethylene carbonate, propylene carbonate, and butylene carbonate.

10. 2. The secondary battery according to claim 1, wherein the electrolyte further comprises an additive, the additive comprising at least one of a silicon-containing additive, a cyclic carbonate additive, or a sulfur-containing additive.

11. The additive is (a) the silicon-containing additive includes at least one of tris(trimethylsilyl) phosphite, tris(trimethylsilyl) phosphate, tris(trimethylsilyl) borate, trimethylfluorosilane, or heptamethyldisilazane, and the silicon-containing additive is 0.1 to 4 mass% relative to the mass of the electrolyte; (b) the cyclic carbonate additive includes at least one of vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, and difluoroethylene carbonate, and the cyclic carbonate additive is present in an amount of 0.05 to 3% by mass relative to the mass of the electrolyte; (c) the sulfur-containing additive includes at least one of 1,3-propane sultone and vinyl sulfate, and the sulfur-containing additive is 0.05 to 3 mass% relative to the mass of the electrolyte. The secondary battery according to claim 10,

12. The electrolyte additive includes a silicon-containing additive and a sulfur-containing additive, and the content of the silicon-containing additive relative to the mass of the electrolyte is W si %, and the content of the sulfur-containing additive is W s %, and 0.3≦W si +W s ≦4, 0.1≦W si / W s The secondary battery according to claim 10 , wherein the above satisfies the condition ≦5.

13. The electrolyte solution further comprises a lithium salt additive, the lithium salt additive comprising at least one of lithium bisfluorosulfonylimide, lithium bistrifluoromethanesulfonylimide, lithium difluorooxalyl borate, lithium difluorophosphate, and lithium difluorooxalyl phosphate; 2. The secondary battery according to claim 1, wherein the lithium salt additive in the electrolyte is 0.1 to 5 mass %.

14. the positive electrode plate includes a positive electrode current collector and a positive electrode active material layer provided on the positive electrode current collector, the positive electrode active material layer including a positive electrode active material, The positive electrode active material is Li a Fe 1-y Mn y P.O. 4 2. The secondary battery according to claim 1, wherein a is an integer of 0.9≦a≦1.1, 0≦y≦1.

15. An electric device comprising the secondary battery according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Lithium ion secondary battery

    JP2020077576A

  • Lithium iron phosphate battery

    US20200020980A1

Cited By

  • Electrolytes, lithium secondary batteries, and power consumption devices

    JP2026518424A