Reflective polarizing film, light source assembly including the same, and liquid crystal display device

The reflective polarizing film addresses the inefficiencies of conventional polymer-dispersed polarizers by optimizing refractive index differences and dispersion morphology, enhancing brightness and polarization efficiency through controlled polymer dispersion in a core layer.

JP2024539604APending Publication Date: 2024-10-29TORAY ADVANCED MATERIALS KOREA INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024521076
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-05
Filing Date
2022-09-22
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Conventional polymer-dispersed reflective polarizers exhibit lower brightness and polarization efficiency compared to multilayer reflective polarizers due to non-uniform dispersion morphology and refractive index mismatches, leading to significant scattering and reduced light transmission.

Method used

A reflective polarizing film with a core layer containing randomly arranged polymer dispersions, where the refractive index differences are controlled along the x, y, and z-axes, and the area percentage and thickness ratios of polymer dispersions are optimized to minimize scattering, ensuring uniform dispersion and improved light modulation.

Benefits of technology

The film achieves enhanced brightness and polarization characteristics by optimizing the refractive index mismatch and dispersion morphology, resulting in improved light transmission and polarization efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539604000001_ABST
    Figure 2024539604000001_ABST
Patent Text Reader

Abstract

The present invention relates to a reflective polarizing film, and more particularly to a reflective polarizing film having improved brightness and polarization degree, and a light source assembly and a liquid crystal display device including the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reflective polarizing film, and more particularly to a reflective polarizing film having improved brightness and polarization degree, and a light source assembly and a liquid crystal display device including the same. [Background technology]

[0002] Flat panel display technology is dominated by liquid crystal displays (LCD), which have already secured a market share in the TV sector, projection displays, and plasma displays (PDP), and it is expected that field emission displays (FED) and electroluminescent displays (ELD) will dominate their respective fields as related technologies improve. Currently, LCDs are being used in a wider range of applications, including notebook computers, personal computer monitors, LCD TVs, automobiles, and aircraft, and they account for around 80% of the flat panel market, with the demand for LCDs increasing sharply worldwide and the market currently enjoying a boom.

[0003] A conventional LCD uses a liquid crystal and electrode matrix between a pair of light-absorbing optical films. In an LCD, the liquid crystal portion has an optical state that can be changed by moving the liquid crystal portion in response to an electric field generated by applying a voltage to two electrodes. This process displays images using information-bearing "pixels" of polarized light in a particular direction. For this reason, LCDs include front and rear optical films that induce polarized light.

[0004] The optical films used in such LCDs do not necessarily have a high utilization efficiency of the light emitted from the backlight. This is because more than 50% of the light emitted from the backlight is absorbed by the rear optical film (absorptive polarizing film). Therefore, to increase the utilization efficiency of the backlight in LCDs, a reflective polarizer is installed between the optical cavity and the liquid crystal assembly.

[0005] 1 is a diagram illustrating the optical principle of a reflective polarizer. Specifically, P-polarized light from the optical cavity toward the liquid crystal assembly passes through a reflective polarizer and is transmitted to the liquid crystal assembly, and S-polarized light is reflected from the reflective polarizer to the optical cavity, and then reflected by the diffuse reflection surface of the optical cavity with the polarization direction of the light randomized, and then transmitted to the reflective polarizer again. This cycle is repeated, and eventually the S-polarized light is converted into P-polarized light that can pass through the polarizer of the liquid crystal assembly, passes through the reflective polarizer, and is transmitted to the liquid crystal assembly.

[0006] Examples of reflective polarizers exhibiting the above-mentioned functions include a multilayer reflective polarizer in which flat optical layers having an optically anisotropic refractive index and flat optical layers having an optically isotropic refractive index are alternately laminated, a cholesteric liquid crystal reflective polarizer containing a helical cholesteric liquid crystal in a specific direction, a polymer-dispersed reflective polarizer containing a discontinuous phase having an optically anisotropic or optically isotropic refractive index in a continuous phase having an optically isotropic or optically anisotropic refractive index, a sea-island dispersed reflective polarizer containing birefringent sea-island fibers in an isotropic base layer, and a wire-grid type reflective polarizer.

[0007] As an example of the polymer-dispersed reflective polarizer, a reflective polarizer in which a dispersant capable of achieving the function of a reflective polarizer by arranging a birefringent polymer stretched in the longitudinal direction inside a substrate layer has been proposed, and up to now, many efforts have been made to control the size of the dispersed birefringent polymer in order to improve the brightness and degree of polarization.

[0008] However, the polymer-dispersed reflective polarizers developed to date have problems such as a large luminance difference and poor polarization degree compared to multi-layer reflective polarizers. Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been devised to solve the above-mentioned problems, and aims to provide a reflective polarizing film that improves the brightness of conventional polymer-dispersed reflective polarizers and exhibits brightness characteristics close to those of multilayer reflective polarizers.

[0010] Another object of the present invention is to provide a reflective polarizing film that can improve the polarization degree as well as the luminance characteristics.

[0011] Another object of the present invention is to provide a light source assembly and a liquid crystal display device in which the reflective polarizing film according to the present invention is adopted, thereby improving the polarization degree of emitted light and increasing brightness. [Means for solving the problem]

[0012] In order to solve the above-mentioned problems, the present invention provides a reflective polarizing film comprising a core layer having a matrix and a number of polymer dispersions arranged randomly in the y-axis and z-axis directions, with the x-axis direction being the longitudinal direction among the matrix and the x-axis, y-axis, and z-axis directions being perpendicular to each other, and when the core layer is cut in the yz plane and divided into five regions in the z-axis direction with the same thickness, the difference between the area percentage of the polymer dispersion in the uppermost or lowermost region and the area percentage of the polymer dispersion in the central region among the five regions is 10% or less.

[0013] According to one embodiment of the present invention, the matrix and the polymer dispersion have refractive indices with a difference of less than 0.05 along the y-axis and z-axis directions and a difference of more than 0.1 along the x-axis direction.

[0014] In addition, the average thickness of the plurality of polymer dispersions may be 30 nm or more, more preferably 50 nm or more, on a surface obtained by cutting the core layer in the yz plane.

[0015] Additionally, the polymer dispersion located within the central region may have an average thickness of 110 nm or less.

[0016] Also, the average thickness d of the polymer dispersion contained in the uppermost region or the lowermost region I and the average thickness d of the polymer dispersion contained in the central region II Average thickness ratio (d II / d I ) may be 0.8 to 1.6.

[0017] In addition, the percentage of the polymer dispersion area in the total area of ​​the matrix and polymer dispersion in the top region or bottom region and the percentage of the polymer dispersion area in the total area of ​​the matrix and polymer dispersion in the central region may each independently be 40 to 55%.

[0018] The reflective polarizing film may have a haze of 30% or less, and the core layer may have a thickness of 150 μm or less.

[0019] The sheet may further include a skin layer integrally formed on at least one surface of the core layer.

[0020] The present invention also provides a light source assembly including a reflective polarizing film according to the present invention.

[0021] The present invention also provides a liquid crystal display device including a light source unit which is the light source assembly according to the present invention, and a display unit having a liquid crystal cell disposed on a light emitting surface of the light source unit. Effect of the Invention

[0022] The reflective polarizing film of the present invention has a greatly improved brightness and polarization degree, and can be widely used as a component of a liquid crystal display device such as a light source assembly, and can also be applied to glass windows and various polarized lighting industries. [Brief description of the drawings]

[0023] [Figure 1] FIG. 1 is a schematic diagram illustrating the principle of a reflective polarizer. [Diagram 2] 1A and 1B are a cross-sectional view and an enlarged cross-sectional view of a reflective polarizing film according to an embodiment of the present invention. [Diagram 3] 1A and 1B are a cross-sectional view and an enlarged cross-sectional view of a reflective polarizing film according to an embodiment of the present invention. [Figure 4] 2 is a schematic diagram illustrating the longitudinal arrangement of a polymer dispersion in a core layer of a reflective polarizing film according to an embodiment of the present invention. FIG. [Figure 5a] FIG. 2 is a schematic diagram illustrating the aspect ratio, thickness, and width of a polymer dispersion provided in a core layer in a reflective polarizing film according to an embodiment of the present invention. [Figure 5b] FIG. 2 is a schematic diagram illustrating the aspect ratio, thickness, and width of a polymer dispersion provided in a core layer in a reflective polarizing film according to an embodiment of the present invention. [Figure 5c] FIG. 2 is a schematic diagram illustrating the aspect ratio, thickness, and width of a polymer dispersion provided in a core layer in a reflective polarizing film according to an embodiment of the present invention. [Figure 6] FIG. 6(a) is a schematic diagram illustrating dispersion fusion and dispersion-matrix interfacial destruction that may occur during the process of producing a reflective polarizing film. FIG. 6(a) shows dispersion-forming components dispersed within a matrix-forming component, FIG. 6(b) shows dispersion-forming component fusion and dispersion-forming component / matrix-forming component interfacial destruction occurring after dispersion-forming components are dispersed within a matrix-forming component. [Figure 7a] 7A and 7B are schematic cross-sectional views of a portion of the central part of a cross section of a reflective polarizing film core layer according to an embodiment and a comparative example of the present invention, where FIG. 7A is a schematic cross-sectional view of region C of the reflective polarizing film core layer of Example 1, and FIG. 7B and FIG. 7C are schematic cross-sectional views of region C of the reflective polarizing film core layer of Example 2 and Comparative Example 1, respectively. [Figure 7b] 7A and 7B are schematic cross-sectional views of a portion of the central part of a cross section of a reflective polarizing film core layer according to an embodiment and a comparative example of the present invention, where FIG. 7A is a schematic cross-sectional view of region C of the reflective polarizing film core layer of Example 1, and FIG. 7B and FIG. 7C are schematic cross-sectional views of region C of the reflective polarizing film core layer of Example 2 and Comparative Example 1, respectively. [Figure 7c]7A and 7B are schematic cross-sectional views of a portion of the central part of a cross section of a reflective polarizing film core layer according to an embodiment and a comparative example of the present invention, where FIG. 7A is a schematic cross-sectional view of region C of the reflective polarizing film core layer of Example 1, and FIG. 7B and FIG. 7C are schematic cross-sectional views of region C of the reflective polarizing film core layer of Example 2 and Comparative Example 1, respectively. [Figure 8] 1 is a cross-sectional view of a liquid crystal display device according to an embodiment of the present invention. [Figure 9] 1 is an exploded perspective view of a liquid crystal display device according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, the embodiments of the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily carry out the present invention. The present invention may be embodied in various different forms and is not limited to the embodiments described herein. In the drawings, parts not related to the description will be omitted in order to clearly explain the present invention, and the same or similar components will be denoted with the same reference numerals throughout the specification. In addition, the present invention is not limited to the size and / or shape of a structure shown in the drawings. For example, the number and respective sizes of multiple polymer dispersions illustrated in FIG. 2 and FIG. 3, the intervals between the dispersions, the number and distribution of dispersions by region, and the shapes of the polymer dispersions illustrated in FIG. 5b and FIG. 5c are merely examples for explaining the present invention and are not illustrated to exactly correspond to the reflective polarizing film according to the present invention. In addition, the dotted line illustrated on one side of FIG. 3 is merely a schematic illustration of the longitudinal direction of the polymer dispersions and does not mean the length of the polymer dispersions inside the matrix not illustrated.

[0025] 2 and 3, a reflective polarizing film 1000 according to an embodiment of the present invention includes a core layer 100 including a matrix 110 and a number of polymer dispersions 120 randomly positioned within the matrix 110.

[0026] According to an embodiment of the present invention, a birefringent interface may be formed between the matrix 110 and the polymer dispersion 120 contained within the matrix. Specifically, the magnitude of the substantial match or mismatch of the refractive indexes along the spatial X, Y, and Z axes between the matrix 110 and the polymer dispersion 120 affects the degree of scattering of light polarized along that axis. In general, the scattering power varies in proportion to the square of the refractive index mismatch. Thus, the greater the degree of mismatch of the refractive index along a particular axis, the stronger the scattering of light polarized along that axis. Conversely, if the mismatch along a particular axis is small, the scattering of light polarized along that axis is less. If the refractive index of the matrix 110 along an axis substantially matches the refractive index of the polymer dispersion 120, incident light polarized in an electric field parallel to such axis will pass through the dispersion without being scattered, regardless of the size, shape, and density of the dispersion portions. Also, if the refractive indexes along that axis substantially match, the light will pass through the object without being substantially scattered. More specifically, the first polarized light (P polarized light) is transmitted without being affected by the birefringent interface formed at the boundary between the matrix 110 and the polymer dispersion 120, but the second polarized light (S polarized light) is modulated by the birefringent interface formed at the boundary between the matrix 110 and the polymer dispersion 120. Through this, the P polarized light is transmitted, while the S polarized light is modulated by light scattering, reflection, etc., resulting in the separation of the polarized light.

[0027] Therefore, the matrix 110 and the polymer dispersion 120 must form a birefringent interface to induce the light modulation effect, and therefore, when the matrix 110 is optically isotropic, the polymer dispersion 120 may have birefringence, and conversely, when the matrix 110 is optically birefringent, the polymer dispersion 120 may have optical isotropy. Specifically, when the refractive index of the polymer dispersion 120 in the x-axis direction is nX1, the refractive index of the polymer dispersion 120 in the y-axis direction is nY1, and the refractive index of the polymer dispersion 120 in the z-axis direction is nZ1, and the refractive index of the matrix 110 is nX2, nY2, and nZ2, in-plane birefringence between nX1 and nY1 may occur. More preferably, at least one of the refractive indexes of the X-, Y-, and Z-axes of the matrix 110 and the polymer dispersion 120 may be different, and more preferably, when the elongation axis is the X-axis, the difference in the refractive index in the Y-axis and Z-axis directions may be 0.05 or less, and the difference in the refractive index in the X-axis direction may be 0.1 or more. On the other hand, a refractive index difference of 0.05 or less is generally considered to be a match.

[0028] The matrix 110 may be made of any material that is used in a substrate layer of a typical polymer dispersed reflective polarizer, and may be made of any material, including, without limitation, polyethylene naphthalate (PEN), co-polyethylene naphthalate (co-PEN), polyethylene terephthalate (PET), polycarbonate (PC), polycarbonate (PC) alloy, polystyrene (PS), heat resistant polystyrene (PS), polymethyl methacrylate (PMMA), polybutylene terephthalate (PBT), polypropylene (PP), polyethylene (PE), acrylonitrile butadiene styrene (ABS), polyurethane (PU), polyimide (PI), polyvinyl chloride (PVC), styrene acrylonitrile blend (SAN), ethylene vinyl acetate (EVA), polyamide (PA), polyacetal (POM), phenol, epoxy (EP), urea (UF), melanin (MF), unsaturated polyester (UP), silicone (SI), and cycloolefin polymer. For example, polycarbonate (PC) alloy may be used.

[0029] In addition, the polymer dispersion 120 may be any dispersion material used in a typical polymer-dispersed reflective polarizer, and may be any of polyethylene naphthalate (PEN), co-polyethylene naphthalate (co-PEN), polyethylene terephthalate (PET), polycarbonate (PC), polycarbonate (PC) alloy, polystyrene (PS), heat-resistant polystyrene (PS), polymethyl methacrylate (PMMA), polybutylene terephthalate (PBT), polypropylene (PP), polyethylene (PE), acrylonitrile butadiene styrene (ABS), polyurethane (PU), polyimide (PI), polyvinyl chloride (PVC), styrene-acrylonitrile blend (SAN), ethylene vinyl acetate (EVA), polyamide (PA), polyacetal (POM), phenol, epoxy (EP), urea (UF), melanin (MF), unsaturated polyester (UP), silicone (SI), and cycloolefin polymer may be used alone or in combination, and one example may be PEN.

[0030] In addition, the plurality of polymer dispersions 120 may have a rod-like or fiber-like shape that is long in one direction. Accordingly, the aspect ratio of the plurality of polymer dispersions 120, which is the ratio between the length of the longitudinal main axis of the dispersion 120 and the length of the horizontal axis of the cross section perpendicular to the main axis, may be more than 10, for example, more than 100, more than 1,000, more than 10,000, or more than 100,000. The length of the horizontal axis means the diameter of the circle when the cross section is circular, and means the length of the longest line segment among two line segments that connect the circumference when the cross section is not circular. In addition, as shown in FIG. 5a, the cross-sectional aspect ratio of the cross section of the polymer dispersion 120 based on the cut surface that is the yz plane of the core layer 100, which is the ratio of the major axis length a to the minor axis length b (a / b), may also be more than 1, for example, more than 2. Here, the minor axis length b means the length of the minor axis when the axis that perpendicularly bisects the major axis is taken as the minor axis. Also, the cross-sectional aspect ratio may be 10 or less. However, if the cross-sectional aspect ratio exceeds 10, the rectilinearity of light may decrease due to light scattering, an increase in haze, etc., resulting in a decrease in brightness.

[0031] In addition, the multiple polymer dispersions 120 are arranged in the matrix 110 such that the x-axis direction is the longitudinal direction among the three mutually perpendicular x-axis, y-axis, and z-axis. However, here, being arranged such that the x-axis direction is the longitudinal direction does not mean that the longitudinal directions of all the polymer dispersions 120 are arranged parallel to the x-axis as shown in FIG. 2, but means that the direction of the main axis that is the longitudinal direction of the polymer dispersion 120 is closer to the x-axis direction than the y-axis or z-axis.

[0032] To explain this in detail with reference to Fig. 4, in the xz plane of the core layer 100, the first polymer dispersion 123 is arranged so that its longitudinal direction is parallel to the x-axis direction, while the second polymer dispersion 121 and the third polymer dispersion 122 may be arranged so that their longitudinal directions are inclined at a predetermined angle toward the z-axis direction. Although not shown in Fig. 4, it should be made clear that the polymer dispersions may also be arranged so as to be inclined at a predetermined angle toward the y-axis direction. However, the predetermined angle here may be, for example, less than (±) 45°, less than (±) 35°, less than (±) 25°, less than (±) 15°, less than (±) 10°, less than (±) 5°, less than (±) 3°, or less than (±) 1°.

[0033] In addition, the multiple polymer dispersions 120 are randomly arranged based on the y-axis and z-axis directions. That is, the multiple polymer dispersions 120 are randomly arranged in the y-axis and z-axis cross sections of the core layer 100 regardless of the size and shape of the cross section of the polymer dispersion.

[0034] In addition, in the reflective polarizing film 1000 of the present invention, when the surface of the core layer 100 cut in the yz plane is divided into five regions (A, B, C, D, E) having the same thickness in the z-axis direction, the difference between the area percentage of the polymer dispersion 121 located in the uppermost region A or the lowermost region E of the five regions and the area percentage of the polymer dispersion in the central region may be 10% or less, preferably 5% or less, more preferably 3% or less, and even more preferably 2% or less.

[0035] The inventors of the present invention have been continuously studying the reason why a polymer-dispersed reflective polarizer has inferior brightness characteristics compared to a multi-layer reflective polarizer in which optically isotropic layers and optically anisotropic layers are alternately laminated, and have found that the size of the polymer dispersion is not uniform depending on the position in the z-axis direction in the yz plane of the embodied polymer-dispersed reflective polarizer. In particular, the polymer dispersion located in the center based on the z-axis direction in the yz plane is thinner and relatively wider than the polymer dispersion located in the side portions based on the z-axis direction in the yz plane, but the interval between adjacent polymer dispersions is relatively large. As a result of conducting research based on the idea that the difference in morphology between polymer dispersions and the difference in spacing between dispersions depending on the position based on the z-axis direction in the yz plane would affect the brightness and polarization properties, it was found that when the difference in area percentage between the polymer dispersion 121 in the top region A or bottom region E and the polymer dispersion 122 in the central region C was embodied to be 10% or less in each region in the z-axis direction of the core layer, brightness and polarization were greatly improved compared to the conventional method, which led to the present invention.

[0036] Specifically, various factors may be involved in the reason why the difference in morphology between polymer dispersions and the difference in spacing between dispersions occur depending on the position in the yz plane of the core layer 100 with respect to the z-axis direction. As an example, it was discovered that during the manufacturing process, when the molten polymer dispersion-forming components and matrix-forming components are extruded together and cooled, the morphology of the polymer dispersions distributed in the central region C and the spacing between the dispersions change significantly compared to the polymer dispersions in the top region A and / or bottom region E due to differences in the cooling speed and cooling method between the top region A and / or bottom region E, which correspond to the surface portion in the thickness direction, and the central region C. In particular, as shown in Fig. 6, even if the dispersion state of the polymer dispersion-forming components is good immediately after extrusion regardless of the position in the z-axis direction (see Fig. 6(a)), if the cooling of the central region C is not performed properly and the solidification speed is slow, bonding between adjacent polymer dispersion-forming components occurs (see Fig. 6(b)), and in the worse case, the polymer dispersion-forming components that have been bonded to form one large mass are solidified while spreading in a direction parallel to the xy plane, resulting in the formation of a polymer dispersion that is thinner and more widely spread than the thickness of the polymer dispersion 121 located in the uppermost region A and / or the lowermost region E, which are the surface portions. It was also found that when the solidification of the polymer dispersion-forming components is slow, the matrix-forming components are transformed into a third substance due to a chemical reaction occurring at the interface between the polymer dispersion-forming components and the matrix-forming components, and the ratio of the complete matrix is ​​reduced. If cooling of the center is not performed properly in this manner, the weight ratio of the matrix will decrease in the center of the cross section of the core layer due to bonds between the polymer dispersion components and conversion of the matrix components into a third substance. As a result, the area ratio of the polymer dispersion to the sum of the areas of the polymer dispersion and the matrix in the cross section will increase, and the polymer dispersion may have a shape that is thin and widely spread out laterally (see Figure 6(c)).

[0037] That is, after extrusion, inadequate cooling of the center in the thickness direction can be one of the causes of structural and chemical deformation of the polymer dispersion and matrix distributed in the center, and when the reflective polarizing film is realized by controlling the factors that induce structural and chemical deformation, the difference in area percentage between the polymer dispersion 121 located in the uppermost region A or the lowermost region E and the polymer dispersion 122 located in the center region C can be realized to be 10% or less in each z-axis direction region of the core layer, and such a reflective polarizing film can exhibit excellent effects in terms of brightness and polarization degree properties. In other words, when the difference in area percentage of the polymer dispersion between the regions exceeds 10%, it may be the result of the matrix material in the region being modified into a third material, the third material being identified as a polymer dispersion and added to the area of ​​the polymer dispersion, and / or the degree or frequency of coalescence between the polymer dispersions is high, and the brightness and polarization degree properties of the reflective polarizing film may be significantly reduced in terms of physical properties.

[0038] Here, the area percentage of the polymer dispersion located in the specific region is the percentage of the polymer dispersion area relative to the matrix and the total area of ​​the polymer dispersion in the specific region, and the matrix and the total area of ​​the polymer dispersion in the specific region and the polymer dispersion area are the results of calculating the area percentage of the polymer dispersion using the SEM photograph taken in the specific region, which is an open program on the Internet, Image-J. At this time, it should be made clear that the area percentage of the polymer dispersion in the Image-J program is calculated based on the SEM photograph corrected for contrast, magnification, etc. so that the interface between the polymer dispersion and the matrix can be clearly seen in the taken SEM photograph.

[0039] In addition, the percentage of the polymer dispersion area of ​​the total area of ​​the matrix and polymer dispersion in each of the central region C and the uppermost region A or the lowermost region E in the yz cross section of the core layer 100 can satisfy 40 to 55%, more preferably 45 to 50%, thereby preventing the matrix component located in the central region from being degenerated into a third substance due to a chemical reaction at the interface between the matrix component and the polymer dispersion, and realizing a space between adjacent polymer dispersions that is not narrow, which can be advantageous in achieving the desired brightness and polarization properties. If the percentage of the polymer dispersion area of ​​the total area of ​​the matrix and polymer dispersion is less than 40% or exceeds 55%, one or all of the brightness and polarization properties may be significantly reduced. In particular, a percentage of the polymer dispersion area exceeding 55% may be the result of, in other words, modification at the interface between the polymer dispersion and the matrix to a third substance by chemical reaction, which is identified as the polymer dispersion and added to the area of ​​the polymer dispersion, and / or coalescence between polymer dispersions may have occurred.

[0040] According to an embodiment of the present invention, the polymer dispersion located in the uppermost region A or the lowermost region E of the core layer 100 in the z-axis direction may have an average thickness of 100 nm or less, more preferably, the polymer dispersion located in the uppermost region A or the lowermost region E may have an average thickness of 80 nm or less. Also, preferably, the average thickness may be 30 nm or more, more preferably, 50 nm or more. The light transmitted through the lower part of the reflective polarizing film 1000 undergoes optical modulation such as reflection and transmission at the interface between the matrix 110 and the multiple polymer dispersions 120, and constructive interference and destructive interference occur between the reflected and transmitted lights having different optical paths, so that some of the light passes through the upper part of the reflective polarizing film 1000 and is emitted, and the other part is lost through destructive interference, and the remaining part may be emitted to the lower surface or side surface of the reflective polarizing film 1000. Therefore, it is difficult for light incident from below the reflective polarizing film 1000 to exit upwards at a rate of 100%, which can reduce the degree of polarization and brightness. However, the polymer dispersion 121 located in the uppermost region A or the lowermost region E in the z-axis direction of the core layer 100 has an average thickness of 100 nm or less, which is advantageous in preventing the reduction in the degree of polarization and brightness. If the average thickness of the polymer dispersion located in the uppermost region A or the lowermost region E exceeds 100 nm, one or more physical properties of the degree of polarization and brightness may be reduced, and in particular, the polarization property may be significantly reduced. Here, the thickness of the polymer dispersion refers to the length of the longest line segment that connects the periphery of the cross section of the polymer dispersion in parallel with the z-axis direction corresponding to the thickness direction of the core layer 100 when the cross section of the polymer dispersion is placed on the cut surface of the core layer 100, which is the yz plane, and the average thickness of the polymer dispersion refers to the average value of the thicknesses of these polymer dispersions. To illustrate this with reference to FIG. 5b, the first polymer dispersion 124 has a thickness d1, the second polymer dispersion 125 has a thickness d2, the third polymer dispersion 126 has a thickness d3 and the fourth polymer dispersion 127 has a thickness d4.

[0041] The polymer dispersion 122 located in the central region C of the core layer 100 may have an average thickness of preferably 110 nm or less, more preferably 90 nm or less, and even more preferably 80 nm or less. Also, the thickness may be preferably 30 nm or more, and more preferably 50 nm or more, which may be advantageous in achieving desired levels of luminance and polarization properties.

[0042] Meanwhile, proper solidification of the central region C of the core layer 100 may be advantageous in achieving improved brightness and polarization properties by properly implementing the thickness ratio of the polymer dispersion located in the top region A or bottom region E and the central region of the core layer 100. Specifically, the average thickness (d I ) and the average thickness (d II ) thickness ratio (d II / d I ) is 0.8 to 1.6, and more preferably the thickness ratio (d II / d I ) can satisfy 0.8 to 1.1, and in the unlikely event that the thickness ratio (d II / d I ) does not satisfy the above-mentioned range, it may be difficult to simultaneously achieve increased brightness and polarization properties, specifically, the thickness ratio (d II / d I If the thickness ratio (d) is less than 0.8, it may be difficult to achieve improved luminance characteristics, and in particular, the degree of polarization may decrease significantly. II / d I If the ratio exceeds 1.6, the degree of polarization and brightness may be significantly reduced.

[0043] 5c, the polymer dispersion 120 may have widths W1, W2, W3, and W4 of 200 nm or less, preferably 150 nm or less, based on the cross section of the core layer 100, which is the yz plane, of 50% or more of the total number of polymer dispersions, and 60% or more, 70% or more, 80% or more, 85% or more, 90% or more, 95% or more, 98% or more, and 99% or more, thereby minimizing the light loss of the light transmitted through the core layer 100 in the z-axis direction and preventing a decrease in brightness. Here, the width of the polymer dispersion 120 refers to the widths W1, W2, W3, and W4 projected two-dimensionally when the polymer dispersion 120 is viewed in the z-axis direction, and is to be clearly distinguished from the length of the major axis of the polymer dispersion in the cross section of the core layer 100, which is the yz plane. As the width of the polymer dispersion 120 increases and / or the proportion of wider polymer dispersions increases, the average thickness of the polymer dispersion 120 is likely to decrease or the spacing between adjacent polymer dispersions is likely to decrease, which may result in a significant decrease in polarization degree and brightness.

[0044] Meanwhile, the reflective polarizing film 1000 according to an embodiment of the present invention may further include skin layers 211 and 212 disposed on both sides of the core layer 100 as shown in Fig. 2 and Fig. 3. The skin layers 211 and 212 complement the mechanical strength of the core layer 100 and protect the core layer 100 from external factors. In this case, a separate adhesive layer may be further provided between the core layer 100 and the skin layers 211 and 212, but preferably, the skin layers 211 and 212 may be integrally formed by co-extrusion with the core layer 100 without a separate adhesive layer. As a result, it is possible to prevent deterioration of optical properties due to the adhesive layer, and it is also advantageous to realize a thinner optical film.

[0045] Furthermore, unlike the conventional case where an unstretched skin layer is attached after stretching an optical layer, the skin layers 211 and 212 included in one embodiment of the present invention are co-extruded together with the core layer 100 and then stretched, so that they can be stretched in at least one axial direction. As a result, compared to an unstretched skin layer, the surface hardness can be improved, scratch resistance can be improved, and heat resistance can be improved.

[0046] The skin layers 211 and 212 may be made of a material that is commonly used for a skin layer to perform a supporting function of a reflective polarizing film, and preferably are made of polyethylene naphthalate (PEN), copolyethylene naphthalate (co-PEN), polyethylene terephthalate (PET), polycarbonate (PC), polycarbonate (PC) alloy, polystyrene (PS), heat-resistant polystyrene (PS), polymethyl methacrylate (PMMA), polybutylene terephthalate (PBT), polypropylene (PP), polyethylene (PE), acrylic, or the like. The materials that can be used include, but are not limited to, acrylamide butadiene styrene (ABS), polyurethane (PU), polyimide (PI), polyvinyl chloride (PVC), styrene acrylonitrile blend (SAN), ethylene vinyl acetate (EVA), polyamide (PA), polyacetal (POM), phenol, epoxy (EP), urea (UF), melamine (MF), unsaturated polyester (UP), silicone (SI) and cycloolefin polymer, either alone or in combination. More preferably, the same materials as those used for the matrix 110 described above can be used.

[0047] In the above-mentioned reflective polarizing film 1000, the thickness of the core layer 100 may be 20 to 150 μm, more preferably 50 to 120 μm, and the thickness of the skin layers 211, 212 may be 50 to 500 μm, but is not limited thereto. In addition, the number of polymer dispersions 120 in a unit area of ​​5 μm×5 μm in width and length on a surface obtained by cutting the core layer 100 in the yz plane may be 100 to 3,000, but is not limited thereto.

[0048] Also, the haze of the reflective polarizing film 1000 may be 30% or less. If the haze exceeds 30%, the brightness decreases, making it difficult to achieve the object of the present invention.

[0049] Hereinafter, a method for manufacturing the reflective polarizing film 1000 will be described. The reflective polarizing film 1000 according to an embodiment of the present invention can be manufactured through the steps of supplying a matrix component and a polymer dispersion component to an extrusion unit, inducing spreading in a flow control unit so that the polymer dispersion components contained in the matrix can be randomly arranged, cooling and smoothing, stretching the cooled and smoothed film, and heat fixing the stretched film.

[0050] First, in step (1), a matrix component and a polymer dispersion component may be supplied to an extrusion section. These components may be mixed and then supplied to a single extrusion section, or each component may be supplied to an independent extrusion section, in which case the extrusion section may be composed of two or more components. However, it is preferable that each component is mixed through sufficient stirring before being supplied to the extrusion section, and then supplied to a single extrusion section, which may be advantageous in achieving a uniform thickness of the polymer dispersion located in the uppermost region or the lowermost region of the core layer 100 as desired by the present invention. In this case, the extrusion section may be an extruder, which may further include a heating means for converting the supplied polymer component in a solid phase into a liquid phase.

[0051] On the other hand, in order for the polymer dispersion component to be arranged inside the matrix component, it is preferable that there is a difference in flowability between the matrix component and the polymer dispersion component, and for this purpose, it is preferable to design the viscosity between the two components to be different, and preferably, the flowability of the matrix component is designed to be better than that of the polymer dispersion component. As the matrix component and the polymer dispersion component pass through the mixing zone and the mesh filter zone, the polymer dispersion component can be randomly arranged within the matrix component due to the difference in viscosity.

[0052] The thickness and uniformity of the polymer dispersion can be primarily controlled by adjusting the process of step (1). Specifically, it may be advantageous to adjust the thickness and uniformity of the polymer dispersion by changing whether or not the two components are mixed in the extrusion section through sufficient stirring before being added to the extrusion section, the discharge rate during extrusion, the extruder rotation speed related to shear stress, and the type of extruder (single, coaxial twin, etc.).

[0053] Meanwhile, the skin layer is formed into an upper layer and a lower layer through separate extruders, and separate extruders can be used. When a single extruder is used, an S / M / S three-layer structure can be formed by forming an upper layer S and a lower layer S with a core layer M in the center through a flow path. The three-layer structure formed in a molten state is extruded through T-DIE and solidified on a cooling roll, so that the skin layer can be formed without a separate adhesive. The material of the skin layer can be the same or different, but is preferably the same as the material used in the matrix, and the thickness of the skin layer is preferably designed to maximize the optical properties.

[0054] Next, in step (2) of the present invention, the spreading can be induced by a flow control device so that the polymer dispersion components located inside the matrix can be randomly arranged. The flow control device can be a known flow control device, and one example is a coat hanger die. By inducing spreading through the flow control device in step (2), it is possible to secondarily further adjust the thickness and dispersity of the polymer dispersion.

[0055] Next, in step (3) of the present invention, a cooling and smoothing step can be performed. In this step, the film transported through the flow control section is cooled and solidified under conditions used in the manufacture of a typical reflective polarizing film, and the subsequent smoothing step can be performed by adopting or modifying the above. For example, the cooling and smoothing process can be performed using a casting roll. Preferably, one side of the film transported through the flow control section is cooled by contacting it with a main cooling roll, and at this time, the main cooling roll temperature can be set to 40° C. or less, more preferably 35° C. or less, and as another example, 20° C. or less. In the event that the temperature of the main cooling roll exceeds 40°C, bonding between the polymer dispersion forming components dispersed in a molten state in the matrix component is likely to occur in the central region among the five equally divided regions in the z-axis direction of the core layer 100, and as a result, the thickness of the solidified polymer dispersion may increase, or the thickness may decrease as the bonded polymer dispersion lumps spread in the left and right directions. In addition, the ratio of the matrix modified into a third substance by chemical reaction at the interface between the polymer dispersion and the matrix may increase, and the area percentage of the polymer dispersion may increase significantly. More preferably, the opposite side that does not contact the cooling roll is cooled together through an auxiliary cooling means, which may be cooling air, for example, and more preferably the temperature of the cooling air may be 30°C or less, more preferably 20°C or less.

[0056] Next, in step (4) of the present invention, the cooled film may be smoothed and stretched. A stretching process applied to a typical reflective polarizing film may be adopted or modified and performed on the film that has been smoothed so that problems such as breakage due to thickness deviation during stretching do not occur, and a refractive index difference between the matrix component and the polymer dispersion component may be induced to induce a light modulation phenomenon at the interface. The stretching may be uniaxial or biaxial, and more preferably uniaxial. In the case of uniaxial stretching, the stretching direction may be, for example, the x-axis direction. The stretching ratio may be 3 to 12 times.

[0057] Next, in step (5) of the present invention, the stretched film may be heat-set by a conventional method, preferably at 180 to 200° C. for 0.1 to 3 minutes using an IR heater.

[0058] Meanwhile, the reflective polarizing film 1000 may further include a structured surface layer on at least one surface. The structured surface layer performs a function of controlling the direction of light incident or exiting through the reflective polarizing film 1000. The structured surface layer may be any known structure having a structured surface known to have a function of controlling the direction of light, and may have a cross section in the shape of a lenticular, microlens, or prism, or a shape appropriately modified from these. Alternatively, the structured surface may have irregular unevenness generated by the protrusion of diffusion particles provided in the binder resin. Meanwhile, when diffusion particles are included, the direction of light can be controlled through the diffusion particles, so unevenness due to the protrusion of the diffusion particles is not necessarily required.

[0059] The structured surface layer may be provided on the upper and / or lower part of the reflective polarizing film 1000 via the skin layers 211, 212, or on the upper and / or lower part of the core layer 100 with the skin layers 211, 212 omitted, and in this case, it may be integrated with or without a separate adhesive layer.

[0060] The reflective polarizing film satisfying the physical properties according to the present invention described above can be used to improve light efficiency by being adopted in a light source assembly or a liquid crystal display device including the same. Light source assemblies are classified into direct-type light source assemblies in which a lamp is located at the bottom and edge-type light source assemblies in which a lamp is located at the side, and the like, and the reflective polarizing film according to the embodiment of the present invention can be adopted in any type of light source assembly. It can also be applied to a backlight assembly disposed below a liquid crystal panel or a front light assembly disposed above a liquid crystal panel. Below, as one example of various application examples, a case where the reflective polarizing film is applied to a liquid crystal display device including an edge-type light source assembly will be illustrated.

[0061] FIG. 7 is a cross-sectional view of a liquid crystal display device according to a preferred embodiment of the present invention. A liquid crystal display device 2700 includes a backlight unit 2400 and a liquid crystal panel assembly 2500. As shown in FIG.

[0062] The backlight unit 2400 includes a reflective polarizing film 2111 that modulates the optical characteristics of the emitted light. In this case, the functions and types of other known components included in the backlight unit and the positional relationship between the other components and the reflective polarizing film 2111 may vary depending on the purpose, and are not particularly limited in the present invention.

[0063] However, according to a preferred embodiment of the present invention, as shown in FIG. 7, the light guide plate 2415 may be configured and arranged to include a light source 2410, a light guide plate 2415 for guiding light emitted from the light source 2410, a reflective film 2320 arranged below the light guide plate 2415, and a reflective polarizing film 2111 arranged above the light guide plate 2415.

[0064] In this case, the light sources 2410 are disposed on both sides of the light guide plate 2415. The light sources 2410 may be, for example, light emitting diodes (LEDs), cold cathode fluorescent lamps (CCFLs), hot cathode fluorescent lamps (HCFLs), external electrode fluorescent lamps (EEFLs), etc. In another embodiment, the light sources 2410 may be disposed on only one side of the light guide plate 2415.

[0065] The light guide plate 2415 moves the light emitted from the light source 2410 through total internal reflection, and then emits the light upward through a scattering pattern formed on the lower surface of the light guide plate 2415. A reflective film 2420 is disposed under the light guide plate 2415 to reflect the light emitted downward from the light guide plate 2415 upward.

[0066] The reflective polarizing film 2111 is disposed on the light guide plate 2415. The reflective polarizing film 2111 has been described in detail above, so a repeated description will be omitted. Other optical sheets may be further disposed above or below the reflective polarizing film 2111. For example, an optical film capable of controlling the direction of light, such as by concentrating or diffusing light, a retardation film that changes the phase of light, and / or a protective film may be further installed. In this case, the optical film that controls the direction of light may be effective in the case where the reflective polarizing film does not have a separate structured surface layer as described above.

[0067] Additionally, the light source 2410 , the light guide plate 2415 , the reflective film 2420 and the reflective polarizing film 2111 may be housed by a bottom sash 2440 .

[0068] The liquid crystal panel assembly 2500 includes a first display panel 2511, a second display panel 2512, and a liquid crystal layer (not shown) interposed therebetween, and may further include polarizers (not shown) attached to the surfaces of the first display panel 2511 and the second display panel 2512, respectively.

[0069] The liquid crystal display device 2700 may further include a top sash 2600 that covers the edges of the liquid crystal panel assembly 2500 and surrounds the sides of the liquid crystal panel assembly 2500 and the backlight unit 2400 .

[0070] 8 is an example of an LCD device using a reflective polarizing film according to a preferred embodiment of the present invention, in which a reflector 3280 is inserted on a frame 3270, and a cold cathode fluorescent lamp 3290 is positioned on the upper surface of the reflector 3280. An optical film 3320 is positioned on the upper surface of the cold cathode fluorescent lamp 3290, and the optical film 3320 may be laminated in the order of a diffusion plate 3321, a reflective polarizing film 3322, and an absorbing polarizing film 3323, but the components included in the optical film and the lamination order between each component may be changed according to the purpose, some components may be omitted or may be provided in a plurality, and other types of optical films for controlling light not listed above may be further provided. Meanwhile, a liquid crystal display panel 3310 may be inserted into a mold frame 3300 and positioned on the upper surface of the optical film 3320.

[0071] Looking at the path of light in detail, the light irradiated from the cold cathode fluorescent lamp 3290 reaches the diffusion plate 3321 in the optical film 3320. The light transmitted through the diffusion plate 3321 passes through the reflective polarizing film 3322 to make the light travel direction perpendicular to the optical film 3320, and optical modulation occurs. Specifically, P-polarized light passes through the reflective polarizer without loss, but S-polarized light undergoes optical modulation (reflection, scattering, refraction, etc.) and is reflected again by the reflector 3280 on the rear side of the cold cathode fluorescent lamp 3290, and the nature of the light randomly changes to P-polarized light or S-polarized light, and then passes through the reflective polarizing film 3322 again. Then, the light passes through the absorbing polarizing film 3323 and reaches the LCD panel 3310. Meanwhile, the cold cathode fluorescent lamp 3290 can be replaced with other optical devices such as LEDs.

[0072] Meanwhile, in the present invention, the use of the reflective polarizing film has been described mainly with respect to liquid crystal displays, but the use is not limited thereto and can be widely used in flat display technologies such as projection displays, plasma displays, field emission displays, and electroluminescent displays, and can be widely used in glass windows, task lighting requiring polarization, and the like, without being limited thereto.

[0073] The present invention will be described in more detail through the following examples. However, the following examples should not be construed as limiting the scope of the present invention, but should be construed as being for the purpose of aiding in the understanding of the present invention.

[0074] <Example 1>

[0075] First, the dispersion component, matrix component, and skin layer component were extruded using a single compressor. Specifically, polyethylene naphthalate (PEN) with a refractive index of 1.65 as the dispersion component and polycarbonate alloy with a refractive index of 1.58 as the matrix component (containing 38% by weight of polycyclohexylene dimethylene terephthalate (PCTG) polymerized with terephthalate, ethylene glycol, and cyclohexane dimethylol in a 1:2 molar ratio, 60% by weight of polycarbonate, and 2% by weight of a heat stabilizer containing phosphate) were primarily dispersed and fed into the first extrusion section, and a raw material containing the same components as the matrix component was fed into the second extrusion section as the skin layer component, but the second extrusion section was manufactured so that the skin layer covered the upper and lower parts of the matrix with the same thickness using a flow channel.

[0076] The extrusion temperature of the matrix component and the dispersion component was set to 245℃, the polymer flow was corrected so that the IV difference between the two components was 0.013 by checking with the Cap.Rheometer, the dispersion component was induced to be randomly dispersed inside the matrix component by passing through a flow path with a filtration mixer, and then the skin layer component was laminated on both sides of the matrix component. Then, the spread was induced with a coat hanger die that corrected the flow rate and pressure gradient.

[0077] Specifically, the width of the die inlet was 200 mm, the thickness was 10 mm, the width of the die outlet was 1,260 mm, the thickness was 0.80 mm, and the flow rate was 1.0 m / min. After that, the main cooling was controlled to prevent deformation of the dispersion at 20°C, and 18°C ​​cooling air was supplied through an air blower to provide a cooling effect on the opposite side that does not contact the cooling roll, and a smoothing process was performed to prevent problems such as breakage due to thickness deviation when stretching with a casting roll, and the film was stretched 6 times in the MD direction.

[0078] Next, heat fixing was performed in a heater chamber at 180° C. for 2 minutes so that the thickness of the matrix including the skin layer did not exceed 25 μm, and the total thickness including the core layer did not exceed 125 μm, thereby producing a reflective polarizing film as shown in Table 1 below, which has a core layer in which polymer dispersions having a cross-sectional structure as shown in FIG. 2 are randomly dispersed inside the matrix. In this case, the refractive index of the dispersion component in the manufactured reflective polarizing film was (nx: 1.88, ny: 1.58, nz: 1.58), and the refractive index of the matrix component was 1.58.

[0079] <Example 2>

[0080] The same procedure as in Example 1 was carried out, but after the matrix forming components and polymer dispersion components uniformly dispersed in the single extruder were extruded using T-DIE, the temperature of the main cooling roll was changed to 38°C, and a reflective polarizing film was produced without using an air blower.

[0081] <Example 3>

[0082] The same procedure as in Example 1 was followed, but the extruder was changed to a co-rotation twin extruder with high shear stress to produce a reflective polarizing film.

[0083] <Example 4>

[0084] The same procedure as in Example 1 was followed, but in order to reduce shear stress, the screw speed of the single extruder was reduced by 30%, and the temperature of the main cooling roll during cooling after T-DIE extrusion was changed to 34°C. A reflective polarizing film was produced without using an air blower.

[0085] <Example 5>

[0086] The same procedure as in Example 3 was followed, but the screw rotation speed was increased by 1.5 times compared to Example 3 in order to increase the shear stress, and the temperature of the main cooling roll during cooling after T-DIE extrusion was set to 16°C to produce a reflective polarizing film.

[0087] <Example 6>

[0088] The same procedure as in Example 4 was carried out to produce a reflective polarizing film, except that the main cooling roll temperature was changed to 20° C. and an air blower was used to produce the reflective polarizing film.

[0089] <Example 7>

[0090] The same procedure as in Example 1 was carried out to produce a reflective polarizing film, but the overall thickness was kept the same, and the thickness of the core layer was changed to 120 μm, and the main cooling roll temperature during cooling was changed to 15° C.

[0091] <Comparative Example 1>

[0092] The same procedure as in Example 1 was followed, but the polymer was uniformly dispersed in the extruder, and the temperature of the main cooling roll was set to 82°C during cooling after extrusion with T-DIE, and a reflective polarizing film was produced without using an air blower.

[0093] <Comparative Example 2>

[0094] The same procedure as in Example 1 was followed, but the polymer was uniformly dispersed in the extruder, and the temperature of the main cooling roll was set to 100°C during cooling after extrusion with T-DIE. A reflective polarizing film was produced without using an air blower.

[0095] <Experimental Example 1>

[0096] The following physical properties were measured for the reflective polarizing films prepared in the Examples and Comparative Examples, and the results are shown in Tables 1 and 2 below.

[0097] 1. Hayes

[0098] The haze was measured using a haze and transmittance measuring instrument (a product of Nippon Denshoku Kogyo Co.) analytical equipment.

[0099] 2. Polymer dispersion thickness

[0100] The optical film of the embodiment was cut vertically so that the yz plane was the cut surface when the stretch direction of the optical film was the x-axis and the thickness direction was the z-axis, and then SEM photographs were taken of the cut surface. At this time, SEM photographs were taken of each of five regions equally spaced in the thickness direction of the core layer, and the thicknesses of the polymer dispersions located in region I of the top region A and region II of the central region C, which correspond to both sides of the five regions, were measured. Specifically, the thicknesses of the polymer dispersions located within a 5 μm×5 μm region and the intervals between the polymer dispersions were measured for each SEM photograph, and the average values ​​were calculated and shown. Meanwhile, the distance t between polymer dispersions means the shortest distance between adjacent polymer dispersions that overlap by 50% or more when projected two-dimensionally in the z-axis direction. For example, in the case of FIG. 7a, polymer dispersion A (218) and polymer dispersion B (218') correspond to adjacent polymer dispersions, and polymer dispersion C (218'') does not overlap by 50% or more when projected onto either polymer dispersion A (218) or polymer dispersion B (218'), so it does not correspond to an adjacent polymer dispersion and is excluded when calculating the distance between polymer dispersions based on these three polymers. Also, in the case of FIG. 7b, the distance between polymer dispersions is calculated between adjacent polymer dispersion D (219) and polymer dispersion E (219').

[0101] 3. Area Percentage of Polymer Dispersion

[0102] The area percentage of the polymer dispersion was calculated using Image-J, an open program on the Internet, based on the SEM images that were corrected for contrast, magnification, etc. so that the boundary between the polymer dispersion and the matrix was clear in the SEM images taken by region.

[0103] 4. Relative Luminance

[0104] The luminance of the reflective polarizing film was measured as follows. A test display was manufactured by assembling a panel on a 32" edge-type backlight unit having a reflective film, a light guide plate, a diffusion plate, a reflective polarizing film, and an absorptive polarizing film in that order, and then measuring the luminance at nine points on the panel using a Topcon BM-7 measuring device to calculate the average value. The luminance of Example 1 was set to 100, and the luminance of the remaining Examples and Comparative Examples was shown relatively.

[0105] 5. Degree of polarization

[0106] The polarization degree was measured at λ = 550 nm and λ = 650 nm using an OTSKA RETS-100 analytical equipment.

[0107] [Table 1]

[0108] [Table 2]

[0109] As can be seen from Tables 1 and 2 and Figures 6a to 6c,

[0110] It can be seen that the reflective polarizing films according to the examples have superior polarization degree and brightness compared to the reflective polarizing films according to the comparative examples.

[0111] Specifically, the polarization degree and brightness of Comparative Example 1 and Comparative Example 2 were significantly reduced compared to Example 1 and Example 2. This was presumably due to the fact that the central part of the core layer was not properly cooled, which caused bonding between the polymer dispersion forming components located in the central region of the core layer cross section, and the matrix forming components arranged adjacent to the polymer dispersion were converted into a third substance, resulting in matrix destruction in which the interface between the polymer dispersion and the matrix was not properly formed. It can be seen that the difference (%) (absolute value) in the area percentage of the polymer dispersion in Region II and Region I was reflected in the result being more than 10% in the comparative example.

[0112] Although one embodiment of the present invention has been described above, the concept of the present invention is not limited to the embodiment presented in this specification, and a person skilled in the art who understands the concept of the present invention may easily propose other embodiments by adding, changing, deleting, or adding components within the scope of the same concept, which may also be considered to fall within the scope of the concept of the present invention.

Claims

1. Matrix and a core layer having a plurality of polymer dispersions arranged randomly in the matrix in the y-axis and z-axis directions, the x-axis direction being a longitudinal direction among x-axis, y-axis and z-axis directions being perpendicular to each other; A reflective polarizing film, in which when a surface of the core layer cut in the y-z plane is divided into five regions having the same thickness in the z-axis direction, the difference between the area percentage of the polymer dispersion in the uppermost region or the lowermost region and the area percentage of the polymer dispersion in the central region is 10% or less.

2. 2. The reflective polarizing film of claim 1, wherein the matrix and the polymer dispersion have refractive indices in the y-axis and z-axis directions differing by 0.05 or less and the x-axis direction differing by 0.1 or more.

3. 2. The reflective polarizing film of claim 1, wherein the average thickness of the plurality of polymer dispersions on a surface cut in the yz plane of the core layer is 50 nm or more.

4. 2. The reflective polarizing film of claim 1, wherein the polymer dispersion located in the central region has an average thickness of 110 nm or less.

5. The average thickness (d I ) and the average thickness (d II ) between the average thickness ratio (d II / d I 2. The reflective polarizing film of claim 1, wherein the refractive index is 0.8 to 1.

6.

6. 2. The reflective polarizing film of claim 1, wherein the percentage of the polymer dispersion area of ​​the total area of ​​the matrix and polymer dispersion in the top region or the bottom region and the percentage of the polymer dispersion area of ​​the total area of ​​the matrix and polymer dispersion in the central region are each independently 40 to 55%.

7. The reflective polarizing film of claim 1 , wherein the reflective polarizing film has a haze of 30% or less, and the core layer has a thickness of 150 μm or less.

8. The reflective polarizing film of claim 1 , further comprising a skin layer integrally formed on at least one surface of the core layer.

9. A light source assembly comprising the reflective polarizing film of any one of claims 1 to 8.

10. A light source unit which is a light source assembly according to claim 9; and a display unit having a liquid crystal cell disposed on a light exit surface of the light source unit.

Citation Information

Patent Citations

  • Method for manufacturing composite optical body containing inorganic fiber

    JP2008545151A

  • Method of manufacturing diffusely-reflecting polarizer having nearly isotropic continuous phase

    JP2012137759A

  • Reflective polarizer and backlight unit containing same

    JP2018522274A

  • Composite Reflective Polarizing Film

    JP2019508727A

  • Method of manufacturing a diffusely reflecting polarizer having a substantially amorphous nano-composite continuous phase

    KR1020120074257A