CURABLE COMPOSITION, PROTECTIVE FILM, OPTICAL ELEMENT, AND LIQUID CRYSTAL DISPLAY DEVICE

A curable composition with a polyorganosiloxane and redox catalyst simplifies the formation of adhesive layers for optical material protection films in liquid crystal displays, enhancing productivity and reducing costs by omitting heat or energy ray curing.

JP2024541128AActive Publication Date: 2024-11-07LG CHEM LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024513952
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-25
Filing Date
2022-10-26
Publication Date
2024-11-07
Estimated Expiration
2042-10-26

AI Technical Summary

Technical Problem

Existing surface protection films for optical materials in liquid crystal displays require a curing process using heat or energy rays to form an adhesive layer, which is inefficient and increases production costs.

Method used

A curable composition that includes a polyorganosiloxane component and a redox catalyst, allowing the adhesive layer to be formed without heat or energy ray curing, thereby simplifying the manufacturing process and reducing costs.

Benefits of technology

The curable composition achieves appropriate mold release peeling force and residual adhesion rate, improving productivity and reducing costs by eliminating the need for heat or energy ray curing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541128000001
    Figure 2024541128000001
  • Figure 2024541128000002
    Figure 2024541128000002
  • Figure 2024541128000003
    Figure 2024541128000003
Patent Text Reader

Abstract

The present application aims to provide a curable composition that forms a cured product having appropriate demolding strength and residual adhesion rate, and cures a pressure-sensitive adhesive composition that forms a pressure-sensitive adhesive layer without a curing process using heat or energy rays.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to a curable composition, a protective film, an optical element, and a liquid crystal display device. [Background technology]

[0002] In the manufacturing process of optical materials such as polarizing plates and retardation plates, which are materials constituting liquid crystal displays, a surface protection film is bonded to protect the surface of the optical material. The surface protection film is used only in the process of manufacturing the optical material, and is peeled off and removed from the optical material when the optical material is attached to a liquid crystal display.

[0003] In general, a surface protection film has a pressure-sensitive adhesive layer formed on one side of an optically transparent polyalkylene terephthalate resin film, and a release film is bonded onto the pressure-sensitive adhesive layer to protect the pressure-sensitive adhesive layer. An example of such a surface protection film is known from Patent Document 1 (Korea Patent Publication No. 10-2016-0143501).

[0004] Thus, the release film has generally been used as a coating substrate while protecting the pressure-sensitive adhesive layer.

[0005] Meanwhile, the pressure-sensitive adhesive layer of the surface protection film is generally made of an acrylic composition containing an acrylic compound, and the acrylic composition contains a compound that causes a curing reaction by heat or energy rays, and is formed by curing the acrylic composition by appropriate heat or energy ray irradiation depending on the conditions. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Republic of Korea Patent Publication No. 10-2016-0105354 Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present application is to provide a curable composition capable of forming a cured product having suitable demolding strength and residual adhesion rate.

[0008] Another object of the present application is to provide a curable composition that cures the acrylic composition that forms the pressure-sensitive adhesive layer without a curing process using heat or energy rays. [Means for solving the problem]

[0009] In the present application, when a physical property is affected by the temperature, the physical property is measured at room temperature unless otherwise specified. Also, unless otherwise specified, the unit of temperature is Celsius (°C).

[0010] The term "room temperature" as used in this application means a natural temperature that is not heated or cooled, and may mean, for example, any temperature within a range of 10°C to 30°C, such as a temperature of about 15°C or higher, about 18°C ​​or higher, about 20°C or higher, about 23°C or higher, about 27°C or lower, or 25°C.

[0011] The term a to b used in this application means a range between a and b, including a and b. For example, including a to b parts by weight is the same as including within the range of a to b parts by weight.

[0012] The term relative humidity as used in this application is the ratio of the amount of water vapor currently contained in a unit volume of air to the maximum saturated water vapor pressure that a unit volume of air can contain, expressed as a percentage (%), and can be expressed as RH%.

[0013] The term weight average molecular weight (M w ) and number average molecular weight (M n) may be measured using GPC (Gel permeation chromatography), specifically, it may be measured by the following physical property measurement method. Also, the polydispersity index (PDI) of the terms used in this application is 、 weight average molecular weight (M w ) divided by the number average molecular weight (M n ), a value (M w / M n ), which means the molecular weight distribution of the polymer. Specifically, the number average molecular weight (M n ) and the weight average molecular weight (M w ) are obtained by placing the analysis target in a 20 mL vial, diluting it with a THF (tetrahydrofuran) solvent to a concentration of about 20 mg / mL, filtering the calibration standard sample and the sample to be analyzed through a syringe filter (pore size: 0.2 μm), and then measuring. Also, the analysis program may use ChemStation of Agilent technologies. By comparing the elution time of the sample with the calibration curve, the number average molecular weight (M n ) and the weight average molecular weight (M w ) can be determined. Here, the polydispersity index (PDI) may be the value obtained by dividing the measured weight average molecular weight (M w ) by the number average molecular weight (M n ).

[0014] <GPC measurement conditions> Equipment: 1200 series of Agilent technologies Column: Use TL Mix.A&B of Agilent technologies Solvent: THF Column temperature: 40 °C Sample concentration: 20 mg / mL, 10 μl injection Use MP: 364000, 91450, 17970, 4910, 1300 as standard samples

[0015] The term "substitution" as used in the present application means that a hydrogen atom bonded to a carbon atom of a compound is changed to another substituent, and the position of the substitution is not particularly limited as long as it is a position at which a hydrogen atom is substituted, i.e., a position at which a substituent can be substituted, and when two or more substituents are substituted, the substituents may be the same or different.

[0016] The term "substituent" as used in this application means an atom or an atomic group replacing one or more hydrogen atoms on a hydrocarbon parent chain. The substituents are described below but are not limited thereto, and the substituents may be further substituted with the substituents described below or may not be substituted with any substituents unless otherwise specified in this application.

[0017] Unless otherwise specified, the term alkyl or alkylene group used in this application may be a straight-chain or branched alkyl or alkylene group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 6 carbon atoms, or may be a cyclic alkyl or alkylene group having 3 to 20 carbon atoms, 3 to 16 carbon atoms, 3 to 12 carbon atoms, 3 to 8 carbon atoms, or 3 to 6 carbon atoms. Here, the cyclic alkyl or alkylene group includes an alkyl or alkylene group having only a ring structure and an alkyl or alkylene group containing a ring structure. For example, a cyclohexyl group and a methylcyclohexyl group are both cyclic alkyl groups. Also, for example, the alkyl group or alkylene group is specifically methyl(ren), ethyl(ren), n-propyl(ren), isopropyl(ren), n-butyl(ren), isobutyl(ren), tert-butyl(ren), sec-butyl(ren), 1-methyl-butyl(ren), 1-ethyl-butyl(ren), n-pentyl(ren), isopentyl(ren), neopentyl(ren), tert-pentyl(ren), n-hexyl(ren), 1-methylpentyl(ren), 2-methylpentyl(ren), 4-methyl-2-pentyl(ren), 3,3-dimethyl(ren), 4-methyl-2-pentyl ... Examples of arylalkyl include, but are not limited to, butyl(ren), 2-ethylbutyl(ren), n-heptyl(ren), 1-methylhexyl(ren), n-octyl(ren), tert-octyl(ren), 1-methylheptyl(ren), 2-ethylhexyl(ren), 2-propylpentyl(ren), n-nonyl(ren), 2,2-dimethylheptyl(ren), 1-ethylpropyl(ren), 1,1-dimethylpropyl(ren), isohexyl(ren), 2-methylpentyl(ren), 4-methylhexyl(ren), and 5-methylhexyl(ren).Specific examples of the cycloalkyl group or cycloalkylene group include cyclopropyl(ren), cyclobutyl(ren), cyclopentyl(ren), 3-methylcyclopentyl(ren), 2,3-dimethylcyclopentyl(ren), cyclohexyl(ren), 3-methylcyclohexyl(ren), 4-methylcyclohexyl(ren), 2,3-dimethylcyclohexyl(ren), 3,4,5-trimethylcyclohexyl(ren), 4-tert-butylcyclohexyl(ren), cycloheptyl(ren), and cyclooctyl(ren), but are not limited thereto.

[0018] Unless otherwise specified, the term alkenyl or alkenylene group used in this specification may be a straight-chain or branched non-cyclic alkenyl or alkenylene group having 2 to 20, 2 to 16, 2 to 12, 2 to 8, or 2 to 6 carbon atoms, or a cyclic alkenyl or alkenylene group having 3 to 20, 3 to 16, 3 to 12, 3 to 8, or 3 to 6 carbon atoms. Here, if an alkenyl or alkenylene group having a ring structure is included, it corresponds to a cyclic alkenyl or alkenylene group. Also, for example, ethenyl(ren), n-propenyl(ren), isopropenyl(ren), n-butenyl(ren), isobutenyl(ren), tert-butenyl(ren), sec-butenyl(ren), 1-methyl-butenyl(ren), 1-ethyl-butenyl(ren), n-pentenyl(ren), isopentenyl(ren), neopentenyl(ren), tert-pentenyl(ren), n-hexenyl(ren), 1-methylpentenyl(ren), 2-methylpentenyl(ren), 4-methyl-2-pentenyl(ren), 3,3-dimethylbutenyl(ren), 2-ethylbutenyl(ren), Non-limiting examples of suitable aryl groups include but are not limited to phenyl(ren), n-heptenyl(ren), 1-methylhexenyl(ren), n-octenyl(ren), tert-octenyl(ren), 1-methylheptenyl(ren), 2-ethylhexenyl(ren), 2-propylpentenyl(ren), n-nonylenyl(ren), 2,2-dimethylheptenyl(ren), 1-ethylpropenyl(ren), 1,1-dimethylpropenyl(ren), isohexenyl(ren), 2-methylpentenyl(ren), 4-methylhexenyl(ren), and 5-methylhexenyl(ren).Specific examples of the cycloalkenyl group or cycloalkenylene group include, but are not limited to, cyclopropenyl(ylene), cyclobutenyl(ylene), cyclopentenyl(ylene), 3-methylcyclopentenyl(ylene), 2,3-dimethylcyclopentenyl(ylene), cyclohexenyl(ylene), 3-methylcyclohexenyl(ylene), 4-methylcyclohexenyl(ylene), 2,3-dimethylcyclohexenyl(ylene), 3,4,5-trimethylcyclohexenyl(ylene), 4-tert-butylcyclohexenyl(ylene), cycloheptenyl(ylene), and cyclooctenyl(ylene).

[0019] The term alkynyl or alkynylene group used in this specification, unless otherwise specified, may be a straight-chain or branched non-cyclic alkynyl or alkynylene group having 2 to 20 carbon atoms, or 2 to 16 carbon atoms, or 2 to 12 carbon atoms, or 2 to 8 carbon atoms, or 2 to 6 carbon atoms, or a cyclic alkynyl or alkynylene group having 3 to 20 carbon atoms, or 3 to 16 carbon atoms, or 3 to 12 carbon atoms, or 3 to 8 carbon atoms, or 3 to 6 carbon atoms. Here, if an alkynyl or alkynylene group having a ring structure is included, it corresponds to a cyclic alkynyl or alkynylene group. Also, for example, ethynyl(ren), n-propynyl(ren), isopropynyl(ren), n-butynyl(ren), isobutynyl(ren), tert-butynyl(ren), sec-butynyl(ren), 1-methyl-butynyl(ren), 1-ethyl-butynyl(ren), n-pentynyl(ren), isopentynyl(ren), neopentynyl(ren), tert-pentynyl(ren), n-hexynyl(ren), 1-methylpentynyl(ren), 2-methylpentynyl(ren), 4-methyl-2-pentynyl(ren), 3,3-dimethylbutynyl(ren), 2-ethyl Examples of aryl groups include, but are not limited to, butynyl(ren), n-heptynyl(ren), 1-methylhexynyl(ren), n-octynyl(ren), tert-octynyl(ren), 1-methylheptynyl(ren), 2-ethylhexynyl(ren), 2-propylpentynyl(ren), n-nonynyl(ren), 2,2-dimethylheptynyl(ren), 1-ethylpropynyl(ren), 1,1-dimethylpropynyl(ren), isohexynyl(ren), 2-methylpentynyl(ren), 4-methylhexynyl(ren), and 5-methylhexynyl(ren).Specific examples of the cycloalkynyl group or cycloalkynylene group include, but are not limited to, cyclopropynyl(ren), cyclobutynyl(ren), cyclopentynyl(ren), 3-methylcyclopentynyl(ren), 2,3-dimethylcyclopentynyl(ren), cyclohexynyl(ren), 3-methylcyclohexynyl(ren), 4-methylcyclohexynyl(ren), 2,3-dimethylcyclohexynyl(ren), 3,4,5-trimethylcyclohexynyl(ren), 4-tert-butylcyclohexynyl(ren), cycloheptynyl(ren), and cyclooctynyl(ren).

[0020] The alkyl group, alkylene group, alkenyl group, alkenylene group, alkynyl group, and alkynylene group may be optionally substituted with one or more substituents. In this case, the substituent may be at least one selected from the group consisting of halogen (chlorine (Cl), iodine (I), bromine (Br), and fluorine (F)), aryl group, heteroaryl group, epoxy group, alkoxy group, cyano group, carboxyl group, acryloyl group, methacryloyl group, acryloyloxy group, methacryloyloxy group, carbonyl group, and hydroxy group, but is not limited thereto.

[0021] The term aryl group used in the present application means an aromatic ring obtained by removing one hydrogen from an aromatic hydrocarbon ring, and the aromatic hydrocarbon ring may include a monocyclic or polycyclic ring. The number of carbon atoms in the aryl group is not particularly limited, and unless otherwise specified, it may be an aryl group having 6 to 30 carbon atoms, 6 to 26 carbon atoms, 6 to 22 carbon atoms, 6 to 20 carbon atoms, 6 to 18 carbon atoms, or 6 to 15 carbon atoms. The term arylene group used in the present application means that the aryl group has two bonding positions, that is, a divalent group. The above description of the aryl group may be applied, except that each of these is a divalent group. Examples of the aryl group include, but are not limited to, a phenyl group, a phenylethyl group, a phenylpropyl group, a benzyl group, a tolyl group, a xylyl group, or a naphthyl group.

[0022] The term heteroaryl group used in the present application refers to an aromatic ring containing at least one heteroatom other than carbon, and specifically, the heteroatom may contain one or more atoms selected from the group consisting of nitrogen (N), oxygen (O), sulfur (S), selenium (Se) and tellurium (Te). In this case, the atoms constituting the ring structure of the heteroaryl group may be called ring atoms. The heteroaryl group may also contain a monocyclic or polycyclic ring. The heteroaryl group is not particularly limited in number of carbon atoms, but may be a heteroaryl group having 2 to 30 carbon atoms, or 2 to 26 carbon atoms, or 2 to 22 carbon atoms, or 2 to 20 carbon atoms, or 2 to 18 carbon atoms, or 2 to 15 carbon atoms, unless otherwise specified. In another example, the heteroaryl group is not particularly limited in number of ring atoms, but may be a heteroaryl group having 5 to 30, 5 to 25, 5 to 20, 5 to 15, 5 to 10, or 5 to 8 ring atoms. Examples of the heteroaryl group include a thiophene group, a furan group, a pyrrole group, an imidazolyl group, a thiazolyl group, an oxazolyl group, an oxadiazolyl group, a triazolyl group, a pyridyl group, a bipyridyl group, a pyrimidyl group, a triazinyl group, an acridyl group, a pyridazinyl group, a pyrazinyl group, a quinolinyl group, a quinazolinyl group, a quinoxalinyl group, a phthalazinyl group, a pyridopyrimidinyl group, a pyridopyrazinyl group, a pyrazinopyrazinyl group, an isoquinolinyl group, an indole group, a carbazolyl group, a benzoxazolyl group, a benzimidazolyl group, a benzothiazolyl group, a benzocarbazolyl group, a dibenzocarbazolyl group, a benzothiophene group, a dibenzothiophene group, a benzofuran group, a dibenzofuran group, a benzosilole group, a dibenzosilole group, a phenanthrolinyl group, group), an isoxazolyl group, a thiadiazolyl group, a phenothiazinyl group, a phenoxazine group, and condensed structures thereof, but are not limited thereto.

[0023] In addition, the term "heteroarylene group" used in this application means that the heteroaryl group has two bonding positions, i.e., is a divalent group. The above description of the heteroaryl group may be applied, except that each of these is a divalent group.

[0024] The aryl group or heteroaryl group may be optionally substituted with one or more substituents, which may be at least one selected from the group consisting of halogens (chlorine (Cl), iodine (I), bromine (Br), fluorine (F)), aryl groups, heteroaryl groups, epoxy groups, alkoxy groups, cyano groups, carboxyl groups, acryloyl groups, methacryloyl groups, acryloyloxy groups, methacryloyloxy groups, carbonyl groups, and hydroxy groups, but are not limited thereto.

[0025] A curable composition according to one embodiment of the present application may include a polyorganosiloxane component and a redox catalyst.

[0026] The term "curable composition" as used in the present application may include components that can be converted to resin through a curing reaction or polymerization reaction, as well as components generally known as resins. In addition, the curable composition may have adhesive or cohesive properties by itself, or may have adhesive or cohesive properties through a reaction such as a curing reaction.

[0027] The curable composition may be a solvent-based curable composition, a water-based curable composition, or a solventless curable composition.

[0028] The curable composition may be of an active energy ray (e.g., ultraviolet ray) curable type, a moisture curable type, a heat curable type, or a room temperature curable type. When the curable composition is of an active energy ray curable type, the curing of the curable composition is performed by irradiation of an active energy ray such as ultraviolet ray, when the curable composition is of a moisture curable type, the curing of the curable composition is performed by a method of maintaining the curable composition under appropriate humidity, when the curable composition is of a heat curable type, the curing of the curable composition is performed by a method of applying appropriate heat, or when the curable composition is of a room temperature curable type, the curing of the curable composition may be performed by a method of maintaining the curable composition at room temperature.

[0029] The curable composition according to an embodiment of the present application can cure an acrylic composition. In addition, the curable composition can cure the acrylic composition to form a cured product without the need for irradiation with heat or energy rays.

[0030] The term acrylic composition as used in this application can mean a composition that contains 55% by weight or more, 55% by weight or more, 65% by weight or more, 75% by weight or more, 85% by weight or more, 95% by weight or more, 99% by weight or more, or 100% by weight of acrylic compounds based on the total weight.

[0031] Furthermore, the term acrylic compound (or (meth)acrylate) used in this application is a term that includes acrylate and methacrylate, and specifically means acrylic acid, methacrylic acid, a derivative of acrylic acid, or a derivative of methacrylic acid.

[0032] The term acrylic compound (or (meth)acrylate) used in this application can be represented by a compound represented by the following chemical formula A.

[0033] [Chemical formula A] [ka]

[0034] In the above chemical formula A, R1 may be hydrogen or an alkyl group having 1 to 20 carbon atoms. R2 may be hydrogen or a halogen atom (fluoro (F), chloro (Cl), iodine (I), bromo (Br)), an alkyl group substituted or unsubstituted with the above-mentioned substituents, an alkenyl group substituted or unsubstituted with the above-mentioned substituents, an alkynyl group substituted or unsubstituted with the above-mentioned substituents, an aryl group substituted or unsubstituted with the above-mentioned substituents, a heteroaryl group substituted or unsubstituted with the above-mentioned substituents, or a hydroxy group.

[0035] In chemical formula A, when R1 is hydrogen and R2 is hydrogen, it is acrylic acid, and when R1 is a methyl group and R2 is hydrogen, it is methacrylic acid.

[0036] In addition, in the chemical formula A, when R1 is hydrogen and R2 is not hydrogen, it is an acrylic acid derivative, and when R1 is a methyl group and R2 is not hydrogen, it is a methacrylic acid derivative.

[0037] Examples of compounds of formula A include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, and stearyl (meth)acrylate, phenyl (meth)acrylate, aryl (meth)acrylates including 3-phenoxypropyl (meth)acrylate, and nonylphenol ethylene oxide modified (meth)acrylate, methoxymethyl (meth)acrylate, ethoxymethyl (meth)acrylate, propoxymethyl (meth)acrylate, ... Ether-based (meth)acrylates including butoxymethyl (meth)acrylate, isobutoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, oxiranyl (meth)acrylate, oxetanyl (meth)acrylate, tetrahydrofuranyl (meth)acrylate, tetrahydro-2H-pyranyl (meth)acrylate, oxiranylmethyl (meth)acrylate (or glycidyl (meth)acrylate), oxetanylethyl (meth)acrylate, tetrahydrofuranylmethyl (meth)acrylate (or tetrahydrofurfuryl (meth)acrylate), 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2,3-dihydroxypropyl (meth)acrylate, 2,Examples of the hydroxyl group-containing (meth)acrylates include, but are not limited to, 2-dihydroxyethyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, alkyloxypolyethylene glycol mono(meth)acrylate, and alkyloxypolypropylene glycol mono(meth)acrylate.

[0038] The curable composition according to one embodiment of the present application may contain a polyorganosiloxane component in an amount of 50% by weight or more, 52% by weight or more, 54% by weight or more, 56% by weight or more, 58% by weight or more, 60% by weight or more, 62% by weight or more, 64% by weight or more, 66% by weight or more, or 68% by weight or more, or 95% by weight or less, 94% by weight or less, 93% by weight or less, or 92% by weight or less, based on the total weight. When the polyorganosiloxane component is contained within the above range, an excellent residual adhesion rate as well as an appropriate release force can be ensured.

[0039] In the curable composition according to one embodiment of the present application, the polyorganosiloxane component may include a first polyorganosiloxane component represented by the following chemical formula 1. By including the first polyorganosiloxane component represented by the following chemical formula 1, the curable composition can ensure not only an appropriate release force but also an excellent residual adhesion rate.

[0040] [Chemical formula 1] [ka]

[0041] In Chemical Formula 1, R, R and R 10may each independently be an alkenyl group having 2 to 20 carbon atoms, 2 to 18 carbon atoms, 2 to 16 carbon atoms, 2 to 14 carbon atoms, 2 to 12 carbon atoms, 2 to 10 carbon atoms, 2 to 8 carbon atoms, 2 to 6 carbon atoms, or 2 to 4 carbon atoms, an isocyanate group, or an amine group. The first polyorganosiloxane component represented by Chemical Formula 1 can ensure an excellent level of curing properties by having at least three functional groups be alkenyl groups, isocyanate groups, or amine groups.

[0042] In Chemical Formula 1, R2, R3, R4, R5, R6, R8, and R9 may each independently be an alkyl group having 1 to 20 carbon atoms, 1 to 18 carbon atoms, 1 to 16 carbon atoms, 1 to 14 carbon atoms, 1 to 12 carbon atoms, 1 to 10 carbon atoms, 1 to 8 carbon atoms, 1 to 6 carbon atoms, 1 to 4 carbon atoms, or 1 to 3 carbon atoms; an alkenyl group having 2 to 20 carbon atoms, 2 to 18 carbon atoms, 2 to 16 carbon atoms, 2 to 14 carbon atoms, 2 to 12 carbon atoms, 2 to 10 carbon atoms, 2 to 8 carbon atoms, 2 to 6 carbon atoms, or 2 to 4 carbon atoms; an isocyanate group, or an amine group.

[0043] In addition, in Chemical Formula 1, m and n may each independently be a number within the range of 1 to 10,000, 1 to 8,000, 1 to 6,000, 1 to 4,000, 1 to 3,000, 1 to 2,000, or 1 to 1,000. Specifically, in Chemical Formula 1, m may be within the range of 1 to 5,000, 10 to 4,500, 50 to 5,000, 100 to 4,500, 500 to 4,000, or 1,000 to 3,000. In addition, in Chemical Formula 1, n may be within the range of 1 to 100, 2 to 75, 3 to 50, or 4 to 25.

[0044] The first polyorganosiloxane component of the curable composition according to one embodiment of the present application has a weight average molecular weight of 100,000 g / mol or more, 125,000 g / mol or more, 150,000 g / mol or more, 175,000 g / mol or more, 200,000 g / mol or more, 225,000 g / mol or more, 250,000 g / mol or more, 275,000 g / mol or more, or 300,000 g / mol or more, or 1,000,000 g / mol or more. g / mol or less, 950,000g / mol or less, 900,000g / mol or less, 850,000g / mol or less, 800,000g / mol or less, 750,000g / mol or less, 700,000g / mol or less, 650,000g / mol or less, 600,000g / mol or less, 550,000g / mol or less, 500,000g / mol or less, 450,00g / mol or less, or 400,000g / mol or less. When the first polyorganosiloxane component has a weight average molecular weight within the above range, an appropriate viscosity can be ensured, and therefore excellent coating properties can be ensured.

[0045] The first polyorganosiloxane component of the curable composition according to one embodiment of the present application may have a polydispersity index (PDI) in the range of 1 to 5, 1.25 to 3.5, or 1.5 to 2.5. If the first polyorganosiloxane component does not have a polydispersity index within the above range, the content of components having a molecular weight smaller than the desired weight average molecular weight increases, which may cause a problem of reduced physical properties of the cured product.

[0046] In the curable composition according to one embodiment of the present application, the polyorganosiloxane component may contain the first polyorganosiloxane component in an amount of 70% by weight or more, 75% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or 95% by weight or more, or 99.9% by weight or less, 99% by weight or less, or 98% by weight or less, based on the total weight of the polyorganosiloxane component. When the first polyorganosiloxane component is contained within the above range, it is possible to ensure not only an appropriate release force but also an excellent residual adhesion rate.

[0047] In the curable composition according to one example of the present application, the polyorganosiloxane component may include a second polyorganosiloxane component represented by the following chemical formula 2. By including the second polyorganosiloxane component represented by the following chemical formula 2, the curable composition can improve crosslink density and ensure excellent durability.

[0048] [Chemical formula 2] [ka]

[0049] In Chemical Formula 2, R 11 ~R 19 may each independently be an alkyl group having 1 to 20 carbon atoms, 1 to 18 carbon atoms, 1 to 16 carbon atoms, 1 to 14 carbon atoms, 1 to 12 carbon atoms, 1 to 10 carbon atoms, 1 to 8 carbon atoms, 1 to 6 carbon atoms, 1 to 4 carbon atoms, or 1 to 3 carbon atoms.

[0050] In addition, in Chemical Formula 2, a and b may each independently be a number within a range of 1 to 10,000, 1 to 8,000, 1 to 6,000, 1 to 4,000, 1 to 3,000, 1 to 2,000, or 1 to 1,000. Specifically, in Chemical Formula 2, a and b may each independently be a number within a range of 2 to 500, 5 to 250, 10 to 200, 15 to 150, 20 to 100, or 25 to 50.

[0051] The second polyorganosiloxane component of the curable composition according to one embodiment of the present application may have a weight average molecular weight of 1,000 g / mol or more, 1,500 g / mol or more, 2,000 g / mol or more, 2,500 g / mol or more, 3,000 g / mol or more, 3,500 g / mol or more, 4,000 g / mol or more, 4,500 g / mol or more, 5,000 g / mol or more, 5,500 g / mol or more, 6,000 g / mol or more, 6,500 g / mol or more, or 7,000 g / mol or more. g / mol or more, 7,000 g / mol or more, 7,500 g / mol or more, or 8,000 g / mol or more, or 50,000 g / mol or less, 45,000 g / mol or less, 40,000 g / mol or less, 35,000 g / mol or less, 30,000 g / mol or less, 25,000 g / mol or less, 20,000 g / mol or less, 15,000 g / mol or less, or 12,000 g / mol or less. When the second polyorganosiloxane component has a weight average molecular weight within the above range, excellent curability can be ensured.

[0052] The second polyorganosiloxane component of the curable composition according to one embodiment of the present application may have a polydispersity index (PDI) in the range of 1 to 5, 1.25 to 3.5, or 1.5 to 2.5. When the second polyorganosiloxane component has a polydispersity index in the above range, excellent curability, uniform crosslink density and curability can be ensured.

[0053] The curable composition according to one embodiment of the present application may contain the second polyorganosiloxane component in an amount of 0.1 parts by weight or more, 0.25 parts by weight or more, 0.5 parts by weight or more, 0.75 parts by weight or more, 1 part by weight or more, 1.25 parts by weight or more, 1.5 parts by weight or more, 1.75 parts by weight or more, or 2 parts by weight or more, or 10 parts by weight or less, 8 parts by weight or less, 6 parts by weight or less, or 4 parts by weight or less, relative to 100 parts by weight of the first polyorganosiloxane component. When the second polyorganosiloxane component is contained within the above range, it is possible to improve the appropriate crosslink density and ensure excellent durability.

[0054] The curable composition according to one embodiment of the present application may include a redox catalyst as described above.

[0055] In the manufacturing process of optical materials such as polarizing plates and retardation plates, which are materials constituting liquid crystal displays, a surface protection film is used to protect the surface of the optical material. The surface protection film includes a release layer and an adhesive layer, and the adhesive layer is generally made of an acrylic composition containing an acrylic compound. Here, in order to manufacture the adhesive layer, a process of curing the acrylic composition using heat or energy rays is performed.

[0056] The curable composition according to an embodiment of the present application may perform a surface protection function and may form a cured product capable of curing an acrylic compound forming an adhesive layer. The curable composition may omit a curing process using heat or energy rays on an acrylic composition to form an adhesive layer, thereby simplifying the process and improving productivity and reducing costs.

[0057] The redox catalyst of the curable composition according to one embodiment of the present application may include at least one selected from the group consisting of metal naphthenate salts such as cobalt(II) naphthenate, metal acetate hydrate salts such as cobalt(II) acetate tetrahydrate, metal alkanoate salts such as cobalt(II) 2-ethylhexanoate, metal sulfate hydrate salts such as iron(II) sulfate hydrate, metal acetylacetonate salts such as iron(II) acetylacetonate, metal halogenide salts such as copper(I) chloride, and metal alkoxide salts such as titanium(IV) isopropoxide. In the redox catalyst, the metal salt may be a salt of a transition metal, and examples of the transition metal include, but are not limited to, titanium (Ti), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), molybdenum (Mo), lead (Pd), silver (Ag), or cadmium (Cd).

[0058] The curable composition according to one embodiment of the present application may contain a redox catalyst in an amount of 0.01 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, 0.2 parts by weight or more, 0.3 parts by weight or more, 0.4 parts by weight or more, 0.5 parts by weight or more, 0.6 parts by weight or more, 0.7 parts by weight or more, or 0.8 parts by weight or more, or 80 parts by weight or less, 75 parts by weight or less, 70 parts by weight or less, 65 parts by weight or less, 60 parts by weight or less, 55 parts by weight or less, 50 parts by weight or less, or 45 parts by weight or less, based on 100 parts by weight of the polyorganosiloxane component. When the redox catalyst is contained within the above range, it is possible to ensure an excellent residual adhesion rate as well as an appropriate release force while curing the acrylic compound forming the pressure-sensitive adhesive layer.

[0059] The curable composition according to one embodiment of the present application may contain a redox catalyst in an amount of 0.01 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, 0.2 parts by weight or more, 0.3 parts by weight or more, 0.4 parts by weight or more, 0.5 parts by weight or more, 0.6 parts by weight or more, 0.7 parts by weight or more, or 0.8 parts by weight or more, or 80 parts by weight or less, 75 parts by weight or less, 70 parts by weight or less, 65 parts by weight or less, 60 parts by weight or less, 55 parts by weight or less, 50 parts by weight or less, or 45 parts by weight or less, based on 100 parts by weight of the first polyorganosiloxane component. In particular, when the redox catalyst is contained within the above range in combination with the first polyorganosiloxane component, the acrylic compound forming the pressure-sensitive adhesive layer can be efficiently cured while ensuring an excellent residual adhesion rate as well as an appropriate release force.

[0060] The curable composition according to an embodiment of the present application may further include a metal catalyst for carrying out a reaction to form a cured product. The metal catalyst may include at least one selected from the group consisting of aluminum, bismuth, lead, mercury, tin, zinc, platinum, silver, and zirconium as a central metal element. In addition, the metal catalyst may have a siloxane group, an ester group, an ether group, or a carboxy group bonded to the central metal element. The metal catalyst may be, for example, Bis[1,3-bis(2-ethenyl)-1,1,3,3-tetramethyldisiloxane]platinum (CAS No. 81032-58-8), dibutyltin dilaurate, or dimethyltin diacetate, but is not particularly limited thereto, and any metal catalyst that can be generally used in the art may be used without limitation.

[0061] Considering the components contained in the curable composition, the metal catalyst is preferably a platinum catalyst containing platinum (Pt) as a central metal element. In addition, the curable composition may contain the platinum catalyst in an amount of 0.1 parts by weight or more, 0.5 parts by weight or more, 1 parts by weight or more, 1.5 parts by weight or more, 2 parts by weight or more, 2.5 parts by weight or more, or 3 parts by weight or more, or 10 parts by weight or less, 9 parts by weight or less, 8 parts by weight or less, 7 parts by weight or less, 6 parts by weight or less, 5 parts by weight or less, or 4 parts by weight or less, based on 100 parts by weight of the polyorganosiloxane component. In addition, when the content ratio of the platinum catalyst satisfies the above range, the reaction of forming a cured product can be effectively carried out while reducing side reactions.

[0062] The curable composition according to one embodiment of the present application may further include one or more additives as exemplified below in order to secure further physical properties. However, the additives may be any additives that are generally usable in the art, and are not necessarily limited to the additives exemplified below.

[0063] The curable composition according to an embodiment of the present application may further include a dispersant. The dispersant may be, for example, polyamidoamine and its salt, polycarboxylic acid and its salt, modified polyurethane, modified polyester, modified poly(meth)acrylate, (meth)acrylic copolymer, naphthalenesulfonic acid formalin condensate, polyoxyethylene alkyl phosphate, polyoxyethylene alkylamine, pigment derivative, etc., but may be any dispersant known in the art without limitation. For example, Disperbyk-1799 (BYK) may be used.

[0064] The curable composition according to one embodiment of the present application may further include a plasticizer. The type of the plasticizer is not particularly limited, and may be, for example, one or more selected from phthalic acid compounds, phosphoric acid compounds, adipic acid compounds, sebacic acid compounds, citric acid compounds, glycolic acid compounds, trimellitic acid compounds, polyester compounds, epoxidized soybean oil, chlorinated paraffin, chlorinated fatty acid esters, fatty acid compounds, and vegetable oils.

[0065] The phthalic acid compound may be at least one of dimethyl phthalate, diethyl phthalate, dibutyl phthalate, dihexyl phthalate, di-n-octyl phthalate, di-2-ethylhexyl phthalate, diisooctyl phthalate, dicapryl phthalate, dinonyl phthalate, diisononyl phthalate, didecyl phthalate, diundecyl phthalate, dilauryl phthalate, ditridecyl phthalate, dibenzyl phthalate, dicyclohexyl phthalate, butyl benzyl phthalate, octyl decyl phthalate, butyl octyl phthalate, octyl benzyl phthalate, n-hexyl n-decyl phthalate, n-octyl phthalate, and n-decyl phthalate. The phosphoric acid compound may be at least one of tricresyl phosphate, trioctyl phosphate, triphenyl phosphate, octyl diphenyl phosphate, cresyl diphenyl phosphate, and trichloroethyl phosphate. The adipic acid compound may be at least one of dibutoxyethoxyethyl adipate (DBEEA), dioctyl adipate, diisooctyl adipate, di-n-octyl adipate, didecyl adipate, diisononyl adipate (DINA), diisodecyl adipate (DIDP), n-octyl n-decyl adipate, n-heptyl adipate, and n-nonyl adipate. The sebacic acid compound may be at least one of dibutyl sebacate, dioctyl sebacate, diisooctyl sebacate, and butyl benzyl. The citric acid compound may be at least one of triethyl citrate, acetyl triethyl citrate, tributyl citrate, acetyl tributyl citrate, and acetyl trioctyl citrate. The glycolic acid compound may be at least one of methylphthalyl ethyl glycolate, ethylphthalyl ethyl glycolate, and butylphthalyl ethyl glycolate.The trimellitic acid compound may be at least one of trioctyl trimellitate and tri-n-octyl n-decyl trimellitate.The polyester compound may be a reaction product of a diol selected from butanediol, ethylene glycol, propane 1,2-diol, propane 1,3 diol, polyethylene glycol, glycerol, a diacid (selected from adipic acid, succinic acid, succinic anhydride) and a hydroxy acid (e.g., hydroxystearic acid).

[0066] The curable composition according to an embodiment of the present application may further include a reaction accelerator as necessary. The reaction accelerator may function to accelerate the curing reaction of the curable composition. The type of the reaction accelerator is not particularly limited, and for example, dimethyl-p-toluidine (N,N-Dimethyl-p-toluidine; DMPT) may be used.

[0067] The curable composition according to an embodiment of the present application may further include a viscosity modifier, such as a thixotropy-imparting agent, a diluent, a surface treatment agent, a dispersion stabilizer, a reaction control agent, or a coupling agent, for adjusting the viscosity, for example, to increase or decrease the viscosity, or to adjust the viscosity by shear force, as necessary. The thixotropy-imparting agent may adjust the viscosity by shear force of the curable composition. Examples of thixotropy-imparting agents that can be used include fumed silica. The diluent is generally used to reduce the viscosity of the curable composition, and various types of diluents known in the art may be used without limitation as long as they can exhibit the above-mentioned action. The surface treatment agent is for surface treatment of the filler composition introduced into the cured product of the curable composition, and various types of diluents known in the art may be used without limitation as long as they can exhibit the above-mentioned action. The dispersion stabilizer may be used to stabilize the dispersibility between the components in the curable composition, and various types of diluents known in the art may be used without limitation as long as they can exhibit the above-mentioned action. The reaction control agent may be used to control chemical reactions such as the curing of the curable composition, and various types of reaction control agents known in the art may be used without limitation as long as they can exhibit the above-mentioned effects. In the case of a coupling agent, for example, it may be used to improve the dispersibility between components in the curable composition, and specifically, a silane coupling agent may be used, for example, KBM403 or KBM-5103 from Shin-Etsu Co., Ltd. In addition, various types of reaction control agents known in the art may be used without limitation as long as they can exhibit the above-mentioned effects.

[0068] The curable composition according to an example of the present application may be dispersed in a solvent. The term "dispersion" as used in the present application means a state in which a solute is dissolved in a solvent, and also means a state in which a solute is uniformly spread even if it is not dissolved in the solvent.

[0069] Considering the composition of the curable composition, the solvent may be an organic solvent. The organic solvent is not particularly limited as long as it is one generally used in the art, and may be tetrahydrofuran, methyl ethyl ketone, toluene, heptane, or a mixture thereof.

[0070] The solvent may be used in an amount sufficient to disperse the curable composition. Specifically, the amount of the solvent may be, but is not particularly limited to, 500 parts by weight or more, 600 parts by weight or more, 700 parts by weight or more, 800 parts by weight or more, 900 parts by weight or more, 1,000 parts by weight or more, 1,100 parts by weight or more, 1,200 parts by weight or more, 1,300 parts by weight or more, 1,400 parts by weight or more, or 1,500 parts by weight or more based on 100 parts by weight of the curable composition.

[0071] The curable composition according to one embodiment of the present application can cure an acrylic composition through a combination of a polyorganosiloxane component and a redox catalyst as described above, and can ensure excellent curing properties for the acrylic composition and have various physical properties. In addition, the curable composition can cure an acrylic composition without relying on heat and / or active energy rays, and can ensure excellent curing properties even during such curing, and can have various physical properties.

[0072] The curable composition according to one embodiment of the present application can cure the acrylic composition at a cure temperature of 10° C. or more, 12.5° C. or more, 15° C. or more, 17.5° C. or more, 20° C. or more, or 60° C. or less, 57.5° C. or less, 55° C. or less, 52.5° C. or less, or 50° C. or less.

[0073] The curable composition according to one embodiment of the present application has a residual adhesion rate (A d The residual adhesion rate (A) may be 80% or more, 81% or more, 82% or more, 83% or more, 84% or more, or 85% or more. d The upper limit of the residual adhesion rate (A) according to general formula 1 is not particularly limited, but may be 100% or less, less than 100%, or 99% or less. dSpecifically, the residual adhesion rate according to the following general formula 1 can be measured by the following physical property measuring method. That is, the curable composition can ensure an excellent level of the residual adhesion rate according to the following general formula 1 by appropriately curing the acrylic composition.

[0074] [General formula 1] Residual adhesion rate (A d )=A f / A i ×100(%)

[0075] In the general formula 1, A i is the 25°C peel strength of the cured acrylic composition measured at the interface of a PET (polyethylene terephthalate) film at a peel angle of 180° and a peel speed of 0.3 m / min, and A f A i After measuring the peel strength at 25°C, the cured acrylic composition was attached to the interface of the PET film again and measured at a peel angle of 180° and a peel speed of 0.3 m / min.

[0076] The curable composition according to one embodiment of the present application is an acrylic composition that is appropriately cured to have a peel strength of 50 gf / inch (19.3 kg / s) at 25°C measured at a peel angle of 180° and a peel speed of 0.3 m / min on the interface of a PET (polyethylene terephthalate) film. 2 ) or less, 45 gf / inch or less, 40 gf / inch or less, or 35 gf / inch or less, or 10 gf / inch or more, 11 gf / inch or more, 12 gf / inch or more, 13 gf / inch or more, 14 gf / inch or more, or 15 gf / inch or more. Specifically, the 25°C release peel force measured here may be measured by the following physical property measurement method.

[0077] In the curable composition according to one embodiment of the present application, the acrylic composition is appropriately cured, so that the unreacted content (T1 and T2) according to the following general formulas 2 and 3 can be satisfied within the respective specified ranges.

[0078] Regarding the cured product of the acrylic composition obtained by curing the curable composition, the unreacted content (T1) according to the following general formula 2 may be 60% or less, 58% or less, 56% or less, 54% or less, 52% or less, 50% or less, 48% or less, or 46% or less. The lower limit of the unreacted content (T1) is not particularly limited because the lower the content, the better the curing properties, but may be 0.01% or more, 0.1% or more, or 1% or more. When the unreacted content (T1) according to the following general formula 2 satisfies the above numerical range, the acrylic composition can have excellent curing properties even without irradiation of heat or energy rays, and can have a desired release force and residual adhesion rate after curing.

[0079] [General formula 2] T1 = 100 × (W A -W B ) / W A

[0080] In the general formula 2, W A is the initial weight of the cured product obtained by curing the acrylic composition at 25°C, and W B means the post-weight of the cured acrylic composition after storing the cured acrylic composition having the initial weight measured in an oven at 150° C. for 1 hour. Here, the cured acrylic composition may be formed by leaving it at 25° C. for a curing time sufficient for curing, and specifically, the curing time may be, for example, 10 hours or more, 11 hours or more, or 12 hours or more, or 30 hours or less, 25 hours or less, or 20 hours or less. The curing time may be 12 hours or 20 hours. In addition, T1 in the general formula 2 may be specifically measured by the following physical property measuring method.

[0081] Regarding the cured product of the acrylic composition obtained by curing the curable composition, the unreacted content (T2) according to the following general formula 3 may be 50% or less, 48% or less, 46% or less, 44% or less, 42% or less, or 40% or less. The lower limit of the unreacted content (T2) is not particularly limited because the lower limit has better curing properties, but may be 0.01% or more, 0.1% or more, or 1% or more. When the unreacted content (T2) according to the following general formula 3 satisfies the above numerical range, the acrylic composition maintains excellent curing properties even without irradiation of heat or energy rays, and has the desired curing properties after curing.

[0082] [General formula 3] T2 = 100 × (W C -W D ) / W C

[0083] In the general formula 3, W C is the initial weight of the cured product obtained by curing the acrylic composition at 50°C, and W D means the post-weight of the cured acrylic composition after storing the cured acrylic composition of which initial weight was measured in an oven at 150° C. for 1 hour. Here, the cured acrylic composition may be formed by leaving it for a sufficient curing time to cure sufficiently, and specifically, the curing time may be, for example, 10 hours or more, 11 hours or more, 12 hours or more, or 30 hours or less, 25 hours or less, or 20 hours or less. The curing time may be 12 hours or 20 hours. In addition, T2 in the general formula 3 may be specifically measured by the following physical property measurement method.

[0084] The acrylic composition according to one embodiment of the present application may include an acrylic polymer component and an acrylic monomer component. The acrylic polymer component may include a polymer in which one or more acrylic compounds are polymerized (or copolymerized). For example, the polymer is obtained by adding a photoinitiator to a composition containing an alkyl group-containing (meth)acrylate and a hydroxyl group-containing (meth)acrylate, followed by photoinitiation. In addition, specifically, the polymer may be obtained in which the weight ratio (K1 / K2) of the alkyl group-containing (meth)acrylate (K1) and the hydroxyl group-containing (meth)acrylate (K2) is 1 or more, 1.25 or more, or 1.5 or more, or 3 or less, 2.5 or less, or 2 or less.

[0085] The acrylic monomer component may include one or more acrylic compounds. For example, the acrylic monomer component may include an alkyl group-containing (meth)acrylate and a hydroxyl group-containing (meth)acrylate. For example, the acrylic monomer component may include an alkyl group-containing (meth)acrylate in an amount of 50% by weight or more, 55% by weight or more, 60% by weight or more, 65% by weight or more, or 70% by weight or more, or 90% by weight or less, 85% by weight or less, 80% by weight or less, or 75% by weight or less, based on the total weight of the acrylic monomer component. Also, the acrylic monomer component may include a hydroxyl group-containing (meth)acrylate in an amount of 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 25 parts by weight or more, or 50 parts by weight or less, 45 parts by weight or less, 40 parts by weight or less, or 35 parts by weight or less, based on 100 parts by weight of an alkyl group-containing (meth)acrylate.

[0086] In the acrylic composition, the acrylic polymer component and the acrylic monomer component may be included in an appropriate content ratio so that the cured product (which can form an adhesive layer) has a desired adhesive strength and excellent durability while being easily cured by the release layer. Specifically, the acrylic polymer component may be included in an amount of 5 wt% or more, 6 wt% or more, 7 wt% or more, 8 wt% or more, 9 wt% or more, or 20 wt% or less, 19 wt% or less, 18 wt% or less, 17 wt% or less, 16 wt% or less, 15 wt% or less, 14 wt% or less, 13 wt% or less, 12 wt% or less, or 11 wt% or less based on the total weight of the acrylic composition. Specifically, the acrylic monomer component may be included in an amount of 300 parts by weight or more, 350 parts by weight or more, 400 parts by weight or more, 450 parts by weight or more, 500 parts by weight or more, 550 parts by weight or more, 600 parts by weight or more, 650 parts by weight or more, 700 parts by weight or more, 750 parts by weight or more, 800 parts by weight or more, or 850 parts by weight or more, or 1,500 parts by weight or less, 1,400 parts by weight or less, 1,300 parts by weight or less, 1,200 parts by weight or less, 1,100 parts by weight or less, or 1,000 parts by weight or less, relative to 100 parts by weight of the acrylic polymer component.

[0087] In addition, the acrylic composition may further contain an additive as necessary, and the additive may include at least one selected from the group consisting of a metal catalyst, a dispersant, a plasticizer, an initiator, and a reaction accelerator. The metal catalyst, the dispersant, the plasticizer, and the reaction accelerator may be appropriately selected and used in the above examples. The initiator may include a peroxide compound, and the peroxide compound may be a substance that initiates a polymerization reaction of the acrylic composition. The peroxide compound may be, for example, methyl ethyl ketone peroxide. peroxide, MEKP), ketone peroxide compounds such as cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, methylcyclohexanone peroxide, methylacetoacetate peroxide, and acetylacetone peroxide, hydroperoxide compounds such as tert-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, paramenthane hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, and 1,1,3,3-tetramethylbutyl hydroperoxide, diacyl peroxide compounds such as acetyl peroxide, isobutyl peroxide, octanoyl peroxide, decanoyl peroxide, laurinoyl peroxide, 3,3,5-trimethylhexanoyl peroxide, succinic acid peroxide, benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, and meta-toluoyl peroxide, benzoyl peroxide, The peroxide compound may be, but is not limited to, an acyl peroxide compound such as BPO. One or more peroxide compounds may be used.

[0088] A protective film according to an example of the present application may include a substrate film and a cured product of the curable composition according to an example of the present application. The protective film may include a substrate film, a pressure-sensitive adhesive layer, and a release layer, and the curable composition according to an example of the present application may be formed as a release layer, and the pressure-sensitive adhesive layer may be formed by curing an acrylic composition.

[0089] Specifically, the protective film may be a protective film for optical elements. For example, it may be used as a protective film for optical elements such as a polarizing plate, a polarizer, a polarizer protective film, a retardation film, a viewing angle compensation film, and a brightness enhancement film. The terms polarizer and polarizing plate used in this specification refer to objects that are distinguished from each other. That is, a polarizer refers to a film, sheet, or element itself that exhibits a polarizing function, and a polarizing plate refers to an optical element that includes other elements together with the polarizer. Other elements that may be included in the optical element together with the polarizer include, but are not limited to, a polarizer protective film or a retardation layer.

[0090] In addition, the protective film may be effectively used as a surface protective film for protecting the surfaces of optical elements such as polarizing plates, retardation plates, optical compensation films, reflective sheets, and brightness enhancement films used in various optical devices or components and display devices or components, for example, LCDs, but the use is not limited to the protective film.

[0091] The substrate film included in the protective film according to one embodiment of the present application may be a general film or sheet known in the art. Examples of the substrate film include polyester films such as polyethylene terephthalate or polybutylene terephthalate, polytetrafluoroethylene films, polyethylene films, polypropylene films, polybutene films, polybutadiene films, poly(vinyl chloride) films, and polyimide films. Such films may be composed of a single layer or may be laminated with two or more layers, and may further include a functional layer such as an antifouling layer or an antistatic layer in some cases. In addition, from the viewpoint of improving adhesion to the substrate, one or both sides of the substrate may be subjected to a surface treatment such as a primer treatment.

[0092] The thickness of the base film is not particularly limited and may be appropriately selected depending on the application, and may usually be formed to a thickness of 5 μm to 500 μm, 5 μm to 250 μm, or 5 μm to 100 μm.

[0093] The adhesive layer included in the protective film according to an embodiment of the present application may be formed by curing an adhesive composition. The adhesive composition may be the above-mentioned acrylic composition, and the adhesive layer may be formed by curing the acrylic composition. Specifically, the adhesive layer may be formed by applying the composition onto a release layer described later and then curing the composition. Here, the acrylic composition is the same as described above, so detailed description is omitted. The application method of the acrylic composition is not particularly limited as long as it is a method commonly used in the industry, and may include, for example, knife coating, roll coating, or reverse coating. In addition, when forming the adhesive layer, it is preferable to perform the process after sufficiently removing bubble-inducing components such as volatile components and reaction residues in the acrylic composition. This can prevent problems such as a decrease in elastic modulus due to a low crosslink density or molecular weight of the adhesive layer, and an increase in the size of bubbles present between the glass plate and the adhesive layer at high temperatures, which causes scattering bodies to form inside.

[0094] The thickness of the pressure-sensitive adhesive layer contained in the protective film is not particularly limited and may be, for example, 2 μm to 100 μm or 5 μm to 50 μm.

[0095] The pressure-sensitive adhesive layer of the protective film according to one embodiment of the present application has a residual adhesion rate (A d The residual adhesion rate (A) may be 80% or more, 81% or more, 82% or more, 83% or more, 84% or more, or 85% or more. d The upper limit of the residual adhesion rate (A) according to general formula 1 is not particularly limited, but may be 100% or less, less than 100%, or 99% or less. d Specifically, the residual adhesion rate may be measured by the following physical property measuring method. In addition, when the pressure-sensitive adhesive layer of the protective film has a residual adhesion rate within the above range, a protective film having excellent reworkability can be ensured.

[0096] [General formula 1] Residual adhesion rate (Ad )=A f / A i ×100(%)

[0097] In the general formula 1, A i is the 25°C peel strength of the pressure-sensitive adhesive layer measured at a peel angle of 180 degrees and a peel speed of 0.3 m / min on the interface of a PET (polyethylene terephthalate) film, and A f A i After measuring the peel strength at 25° C., the adhesive layer was again attached to the interface of the PET film and measured at a peel angle of 180° and a peel speed of 0.3 m / min.

[0098] The adhesive layer of the protective film according to one embodiment of the present application has a peel strength of 50 gf / inch (19.3 kg / s) at 25°C measured at a peel angle of 180° and a peel speed of 0.3 m / min on the interface of a PET (polyethylene terephthalate) film. 2 ) or less, 45 gf / inch or less, 40 gf / inch or less, or 35 gf / inch or less, or 10 gf / inch or more, 11 gf / inch or more, 12 gf / inch or more, 13 gf / inch or more, 14 gf / inch or more, or 15 gf / inch or more. Specifically, the 25°C peel strength measured here may be measured by the following physical property measurement method. Furthermore, when the pressure-sensitive adhesive layer of the protective film has a 25°C peel strength within the above range, separation from the adherend is prevented, and the surface of the adherend is protected, while the surface of the adherend is not damaged when the protective film is peeled off in the process.

[0099] The release layer included in the protective film according to one embodiment of the present application is obtained by curing the curable composition according to one embodiment of the present application described above. Here, the method for curing the curable composition is not particularly limited, and may be cured through an appropriate aging process or in an appropriate high temperature environment or light irradiation environment. The thickness of the release layer included in the protective film is not particularly limited, and may be, for example, 10 nm to 10 μm, 10 nm to 1 μm, or 10 nm to 100 nm.

[0100] The adhesive layer of the protective film according to an example of the present application may be determined by the composition and content ratio of the curable composition according to an example of the present application forming the release layer, and the curing characteristics of the acrylic composition and the physical properties according to the curing characteristics may be determined. Here, the adhesive layer may be formed by curing the acrylic composition as described above, and at this time, the curing temperature may be 10°C or more, 12.5°C or more, 15°C or more, 17.5°C or more, 20°C or more, or 60°C or less, 57.5°C or less, 55°C or less, 52.5°C or less, or 50°C or less. However, this means that the acrylic composition can be cured at the above curing temperature due to the cured product of the curable composition according to an example of the present application (i.e., the release layer), and the curing reaction may also be performed at a temperature higher than the above curing temperature, such as 60°C or more, 65°C or more, 70°C or more, 75°C or more, or 80°C or more.

[0101] In particular, the acrylic composition undergoes an excellent curing reaction in the above temperature range without high temperature or active energy rays (eg, ultraviolet rays) due to the redox catalyst contained in the release layer.

[0102] The curing properties of the acrylic composition applied to the release layer may be measured by measuring the unreacted content (TML, total mass loss). The curing properties of the acrylic composition can be determined by the unreacted content (T1 and T2) according to the following general formulas 2 and 3, and when the unreacted content (T1 and T2) is within a specified range, it can be evaluated that the curing properties are excellent.

[0103] Regarding the curing properties of the acrylic composition, the unreacted content (T1) according to the following general formula 2 may be 60% or less, 58% or less, 56% or less, 54% or less, 52% or less, 50% or less, 48% or less, or 46% or less. The lower limit of the unreacted content (T1) is not particularly limited because the lower limit has better curing properties, but may be 0.01% or more, 0.1% or more, or 1% or more. When the unreacted content (T1) according to the following general formula 2 satisfies the above numerical range, the acrylic composition can ensure excellent curing properties even without irradiation of heat or energy rays, and can ensure desired release force and residual adhesion rate after curing.

[0104] [General formula 2 T1 = 100 × (W A -W B ) / W A

[0105] In the general formula 2, W A is the initial weight of the cured product obtained by curing the acrylic composition at 25°C, and W B means the post-weight of the cured acrylic composition after storing the cured acrylic composition having the initial weight measured in an oven at 150° C. for 1 hour. Here, the cured acrylic composition may be formed by leaving it at 25° C. for a curing time sufficient for curing, and specifically, the curing time may be, for example, 10 hours or more, 11 hours or more, or 12 hours or more, or 30 hours or less, 25 hours or less, or 20 hours or less. In addition, T1 in the general formula 2 may be specifically measured by the following physical property measuring method.

[0106] Regarding the curing properties of the acrylic composition, the unreacted content (T2) according to the following formula 3 may be 50% or less, 48% or less, 46% or less, 44% or less, 42% or less, or 40% or less. The lower limit of the unreacted content (T2) is not particularly limited since the lower limit has better curing properties, but may be 0.01% or more, 0.1% or more, or 1% or more. When the unreacted content (T2) according to the following formula 3 satisfies the above numerical range, the acrylic composition can ensure excellent curing properties even without irradiation with heat or energy rays, and can also ensure desired release force and residual adhesion rate after curing.

[0107] [General formula 3] T2 = 100 × (W C -W D ) / W C

[0108] In the general formula 3, W C is the initial weight of the cured product obtained by curing the acrylic composition at 50°C, and W D means the post-weight of the cured acrylic composition after storing the cured acrylic composition having the initial weight measured in an oven at 150° C. for 1 hour. Here, the cured acrylic composition may be formed by leaving it for a curing time sufficient for curing, and specifically, the curing time may be, for example, 10 hours or more, 11 hours or more, or 12 hours or more, or 30 hours or less, 25 hours or less, or 20 hours or less. In addition, T2 in the general formula 3 may be specifically measured by the following physical property measuring method.

[0109] The optical element according to one example of the present application may have the protective film attached to a surface thereof. For example, a pressure-sensitive adhesive layer of the protective film may be attached to the surface of the optical element, thereby protecting the optical element with the surface-protecting base film.

[0110] Examples of the optical element included in the optical element include a polarizer, a polarizing plate, a polarizer protective film, a retardation layer, a viewing angle compensation layer, etc. As the polarizer, a general type known in the art, such as a polyvinyl alcohol polarizer, may be used without limitation.

[0111] A polarizer is a functional film or sheet capable of extracting only light vibrating in one direction from light that is incident while vibrating in various directions. Such a polarizer may be, for example, a form in which a dichroic dye is adsorbed and aligned on a polyvinyl alcohol-based resin film. The polyvinyl alcohol-based resin constituting the polarizer is obtained, for example, by gelling a polyvinyl acetate-based resin. In this case, the polyvinyl acetate-based resin that can be used may include not only a homopolymer of vinyl acetate, but also a copolymer of vinyl acetate and other monomers that can be copolymerized with the above. Examples of monomers that can be copolymerized with the vinyl acetate include, but are not limited to, one or a mixture of two or more of unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and acrylamides having an ammonium group. The gelation degree of the polyvinyl alcohol-based resin may usually be about 85 mol% to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may be further modified, for example, polyvinyl formal or polyvinyl acetal modified with aldehydes may be used. The degree of polymerization of the polyvinyl alcohol resin may be usually about 1,000 to 10,000, preferably about 1,500 to 5,000.

[0112] A film of the polyvinyl alcohol-based resin may be formed and used as a raw film of a polarizer. The method of forming the polyvinyl alcohol-based resin is not particularly limited, and a general method known in this field may be used. The thickness of the raw film formed from the polyvinyl alcohol-based resin is not particularly limited, and may be appropriately controlled within a range of, for example, 1 μm to 150 μm. Considering ease of stretching, the thickness of the raw film may be controlled to 10 μm or more. The polarizer may be manufactured through a process of stretching (e.g., uniaxial stretching) the polyvinyl alcohol-based resin film as described above, a process of dyeing the polyvinyl alcohol-based resin film with a dichroic dye and adsorbing the dichroic dye, a process of treating the polyvinyl alcohol-based resin film adsorbed with the dichroic dye with a boric acid aqueous solution, and a process of washing with water after treating with the boric acid aqueous solution. As the dichroic dye, iodine or a dichroic organic dye may be used.

[0113] The polarizing plate may include, for example, the polarizer and another optical film attached to one or both sides of the polarizer. Examples of the other optical film include the above-mentioned polarizer protective film, retardation layer, viewing angle compensation layer, and antiglare layer.

[0114] The polarizer protective film is a concept that is different from the protective film including the pressure-sensitive adhesive layer, and is a protective film for a polarizer. The polarizer protective film may be formed as a multilayer film in which protective films composed of, for example, cellulose-based films such as triacetyl cellulose, acrylic films, polyester-based films such as polycarbonate films or polyethylene terephthalate films, polyethersulfone-based films and / or polyethylene films, polypropylene films, polyolefin films having a cyclo- or norbornene structure, or polyolefin-based films such as ethylene propylene copolymers are laminated. The thickness of the protective film is not particularly limited, and may be formed to a normal thickness.

[0115] A surface treatment layer may be present on the surface of the optical element protected by the protective film in the optical element. The surface treatment layer may have a surface energy of, for example, 30 mN / m or less. That is, a surface treatment layer having a surface energy of 30 mN / m or less may be formed on the surface of the optical element protected by the protective film in the optical element, and the adhesive layer of the protective film may be attached to the surface treatment layer. The method of measuring the surface energy is not particularly limited, and a known method of measuring surface energy may be applied. For example, the contact angle of the surface of the optical element may be measured and the surface energy may be calculated from the contact angle, or the surface energy may be measured using a known surface energy measuring device.

[0116] Examples of the surface treatment layer include a high hardness layer, an anti-glare layer such as an AG (Anti-glare) layer or an SG (Semi-glare) layer, or a low reflection layer such as an AR (Anti-reflection) layer or an LR (Low reflection) layer.

[0117] The high hardness layer may be a layer having a pencil hardness of 1H or more or 2H or more under a load of 500 g. The pencil hardness may be measured, for example, according to the ASTM D 3363 standard using a pencil lead specified in KS G2603.

[0118] The high hardness layer may be, for example, a resin layer having high hardness. The resin layer may include, for example, a room temperature curable, moisture curable, thermosetting, or active energy ray curable resin composition in a cured state. In one example, the resin layer may include a thermosetting or active energy ray curable resin composition, or an active energy ray curable resin composition in a cured state. In the description of the high hardness layer, the term "cured state" refers to a case where the resin composition is converted into a hard state through a crosslinking reaction or a polymerization reaction of the components contained in each of the resin compositions. In addition, the room temperature curable, moisture curable, thermosetting, or active energy ray curable resin composition may refer to a composition in which the cured state is induced at room temperature or in the presence of appropriate moisture by application of heat or irradiation of active energy rays.

[0119] Various resin compositions capable of meeting the aforementioned range of pencil hardness in a cured state are known in the art, and an average technician can easily select an appropriate resin composition.

[0120] In one example, the resin composition may include, as a main component, an acrylic compound, an epoxy compound, a urethane compound, a phenolic compound, or a polyester compound, etc. Here, the "compound" may be a monomeric, oligomeric, or polymeric compound.

[0121] In one example, the resin composition may be an acrylic resin composition having excellent optical properties such as transparency and excellent resistance to yellowing, such as an active energy ray-curable acrylic resin composition.

[0122] The active energy ray-curable acrylic composition may contain, for example, an active energy ray-polymerizable polymer component and a reactive diluent monomer.

[0123] The polymer component may be a component known in the art as a so-called active energy ray polymerizable oligomer, such as urethane acrylate, epoxy acrylate, ether acrylate, or ester acrylate, or a polymer of a mixture containing a monomer, such as a (meth)acrylic acid ester monomer. The (meth)acrylic acid ester monomer may be an alkyl (meth)acrylate, a (meth)acrylate having an aromatic group, a heterocyclic (meth)acrylate, or an alkoxy (meth)acrylate. In this field, various polymer components for producing an active energy ray curable composition are known, and such compounds may be selected as necessary.

[0124] The reactive dilution monomer that may be contained in the active energy ray curable acrylic composition may be a monomer having one or more active energy ray curable functional groups, such as an acryloyl group or a methacryloyl group. The reactive dilution monomer may be, for example, the (meth)acrylic acid ester monomer or a polyfunctional acrylate.

[0125] The selection of the components for producing the active energy ray-curable acrylic composition and the blending ratio of the selected components are not particularly limited, and may be adjusted in consideration of the desired hardness and other physical properties of the resin layer.

[0126] As an antiglare layer such as an AG layer or an SG layer, for example, a resin layer having an uneven surface or a resin layer containing particles, in which the particles have a refractive index different from that of the resin layer, may be used.

[0127] As the resin layer, for example, the resin layer used for forming the high hardness layer may be used. When forming an antiglare layer, it is not necessary to adjust the components of the resin composition so that the resin layer can exhibit high hardness, but the resin layer may be formed so that it can exhibit high hardness.

[0128] The method of forming the uneven surface on the resin layer is not particularly limited. For example, the uneven structure may be realized by contacting a coating layer of the resin composition with a mold having a desired uneven structure and curing the resin composition, or by blending particles of an appropriate particle size into the resin composition, coating and curing the mixture.

[0129] The antiglare layer may be embodied using particles having a refractive index different from that of the resin layer.

[0130] In one example, the difference in refractive index between the particles and the resin layer may be, for example, 0.03 or less or 0.02 to 0.2. If the difference in refractive index is too small, it is difficult to induce haze, and conversely, if it is too large, a lot of scattering occurs in the resin layer, increasing the haze, but this may induce a decrease in light transmittance and contrast characteristics, so appropriate particles may be selected in consideration of this.

[0131] The shape of the particles contained in the resin layer is not particularly limited, and may be, for example, spherical, elliptical, polyhedral, amorphous or other shapes. The particles may have an average diameter of 50 nm to 5,000 nm. In one example, the particles may be particles having irregularities formed on the surface. Such particles may have, for example, an average surface roughness (Rz) of 10 nm to 50 nm or 20 nm to 40 nm, and / or the maximum height of the irregularities formed on the surface may be about 100 nm to 500 nm or 200 nm to 400 nm, and the width between the irregularities may be 400 nm to 1200 nm or 600 nm to 1000 nm. Such particles have excellent compatibility with the resin layer and excellent dispersibility therein.

[0132] The particles include various inorganic or organic particles, such as inorganic particles including silica, amorphous titania, amorphous zirconia, indium oxide, alumina, amorphous zinc oxide, amorphous cerium oxide, barium oxide, calcium carbonate, amorphous barium titanate, and barium sorbate, and organic particles including crosslinked or non-crosslinked organic materials such as acrylic resin, styrene resin, urethane resin, melamine resin, benzoguanamine resin, epoxy resin, and silicone resin, but are not limited thereto.

[0133] The uneven structure formed in the resin layer or the content of the particles is not particularly limited. For example, the shape of the uneven structure and the content of the particles may be adjusted so that the haze of the resin layer is about 5% to 15%, 7% to 13%, or about 10% in the case of an AG layer, and may be adjusted so that the haze is about 1% to 3% in the case of an SG layer. The haze may be measured using a hazemeter such as HR-100 or HM-150 from Sepoong Co., Ltd. according to the manufacturer's manual.

[0134] A low reflection layer such as an AR layer or an LR layer may be formed by coating a low refractive index material. Various low refractive index materials capable of forming a low reflection layer are known, and all of these may be appropriately selected and used in the optical element. The low reflection layer may be formed by coating a low refractive index material so that the reflectance is about 1% or less.

[0135] The formation of the surface treatment layer may be carried out in accordance with Korean Patent Publication Nos. 2007-0101001, 2011-0095464, 2011-0095004, 2011-0095820, 2000-0019116, 2000-0009647, 2000-0018983, 2003-0068335, 2002-0 Known materials such as Nos. 066505, 2002-0008267, 2001-0111362, 2004-0083916, 2004-0085484, 2008-0005722, 2008-0063107, 2008-0101801, or 2009-0049557 may also be used.

[0136] The surface treatment layer may be formed alone or in combination of two or more. An example of the combination is a case where a high-hardness layer is first formed on the surface of the base layer, and then a low-reflection layer is formed on the surface of the high-hardness layer.

[0137] A liquid crystal display (LCD) device according to an embodiment of the present application may include a liquid crystal panel, and the optical elements described above may be attached to one or both sides of the liquid crystal panel.

[0138] The type of liquid crystal panel included in the liquid crystal display device is not particularly limited. For example, without being limited to the type, all known liquid crystal panels including various F manual matrix types including TN (Twisted Neumatic) type, STN (SuperTwisted Neumatic) type, F (ferroelectric) type and PD (polymer dispersed LCD) type, various active matrix types including two terminal type and three terminal type, in-plane switching type (IPS mode) panel and vertical alignment type (VA mode) panel may be applied. In addition, the types of other components included in the liquid crystal display device and their manufacturing methods are not particularly limited, and general components in this field may be adopted and used without restrictions. Effect of the Invention

[0139] The present application can provide a curable composition capable of forming a cured product having suitable demolding peel strength and residual adhesion rate.

[0140] In addition, the present application can provide a curable composition that cures the acrylic composition that forms the pressure-sensitive adhesive layer without a curing process using heat or energy rays. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0141] The present application will be described below through examples and comparative examples, but the scope of the present application is not limited to the following contents.

[0142] <Production of Curable Composition> Example 1. A compound represented by the following formula 1A (KS-847H from Shinetsu Silicon Co., Ltd.) was used as the first polyorganosiloxane component, and the weight average molecular weight (Mw ) was in the range of approximately 300,000 to 400,000 g / mol.

[0143] [Chemical formula 1A] [ka]

[0144] In Chemical Formula 1A, m is about 1,000 to 2,000, and n is about 5 to 20.

[0145] A compound represented by the following formula 2A (X-92-122 from Shin-Etsu Silicone Co., Ltd.) was used as the second polyorganosiloxane component, and the weight average molecular weight (M w ) was in the range of approximately 8,000 to 12,000 g / mol.

[0146] [Chemical formula 2A] [ka]

[0147] In Chemical Formula 2A, a is about 25-45, and b is about 25-45.

[0148] The first polyorganosiloxane component (PS1), the second polyorganosiloxane component (PS2), a platinum catalyst (Ptc, PL-50L, Shin-Etsu Silicone Co., Ltd.) and a redox catalyst (Rc, iron (III) acetylacetonate, Sigma-Aldrich Co., Ltd.) were added to an organic solvent in a weight ratio of 5:0.1:0.15:2 (PS1:PS2:Ptc:Rc) to prepare a curable composition dispersed in an organic solvent.

[0149] The organic solvent used was a mixture of tetrahydrofuran (THF), methylethyl ketone (MEK), toluene (T) and n-heptane (H), and was used in a sufficient amount to adequately disperse the curable composition.

[0150] Example 2. In Example 2, the first polyorganosiloxane component (PS1), the second polyorganosiloxane component (PS2), platinum catalyst (Ptc, Shin-Etsu Silicone Co., Ltd. PL-50L) and redox catalyst (Rc, iron (III) acetylacetonate, Sigma-Aldrich Co., Ltd.) used in Example 1 were added to an organic solvent in a weight ratio of 5:0.1:0.15:0.04 (PS1:PS2:Ptc:Rc), except that a curable composition dispersed in an organic solvent was prepared in the same manner as in Example 1.

[0151] Example 3. In Example 3, the first polyorganosiloxane component (PS1), the second polyorganosiloxane component (PS2), platinum catalyst (Ptc, Shin-Etsu Silicone Co., Ltd. PL-50L) and redox catalyst (Rc, iron (III) acetylacetonate, Sigma-Aldrich Co., Ltd.) used in Example 1 were added to an organic solvent in a weight ratio of 5:0.1:0.15:0.2 (PS1:PS2:Ptc:Rc), except that a curable composition dispersed in an organic solvent was prepared in the same manner as in Example 1.

[0152] Example 4. In Example 4, the first polyorganosiloxane component (PS1), the second polyorganosiloxane component (PS2), platinum catalyst (Ptc, Shin-Etsu Silicone Co., Ltd. PL-50L) and redox catalyst (Rc, iron (III) acetylacetonate, Sigma-Aldrich Co., Ltd.) used in Example 1 were added to an organic solvent in a weight ratio of 5:0.1:0.15:1 (PS1:PS2:Ptc:Rc), except that a curable composition dispersed in an organic solvent was prepared in the same manner as in Example 1.

[0153] Comparative Example 1 In Comparative Example 1, the first polyorganosiloxane component (PS1), the second polyorganosiloxane component (PS2) and a platinum catalyst (Ptc, Shin-Etsu Silicone Co., Ltd. PL-50L) used in Example 1 were added to an organic solvent in a weight ratio of 5:0.1:0.15 (PS1:PS2:Ptc), except that a curable composition dispersed in an organic solvent was prepared in the same manner as in Example 1.

[0154] Comparative Example 2 In Comparative Example 2, the first polyorganosiloxane component (PS1), the second polyorganosiloxane component (PS2), platinum catalyst (Ptc, Shin-Etsu Silicone Co., Ltd. PL-50L) and redox catalyst (Rc, iron (III) acetylacetonate, Sigma-Aldrich Co., Ltd.) used in Example 1 were added to an organic solvent in a weight ratio of 5:0.1:0.15:5 (PS1:PS2:Ptc:Rc), except that a curable composition dispersed in an organic solvent was prepared in the same manner as in Example 1.

[0155] Example 5. In Example 5, the first polyorganosiloxane component (PS1), the second polyorganosiloxane component (PS2), platinum catalyst (Ptc, Shin-Etsu Silicone Co., Ltd. PL-50L) and redox catalyst (Rc, cobalt (III) naphthenate) used in Example 1 were added to an organic solvent in a weight ratio of 5:0.1:0.15:2 (PS1:PS2:Ptc:Rc), except that a curable composition dispersed in an organic solvent was prepared in the same manner as in Example 1.

[0156] <Protective film manufacturing> Using each of the curable compositions prepared in Examples 1 to 5 and Comparative Examples 1 and 2, protective films were prepared.

[0157] Each of the curable compositions prepared in Examples 1 to 5 and Comparative Examples 1 and 2 was applied to one side of each substrate film and cured at 150° C. for 3 minutes to form a release layer on the substrate film. At this time, the thickness of the release layer was about 50 to 80 nm, and the substrate film used was a PET (polyethylene terephthalate) film having a thickness of about 50 μm.

[0158] Then, an acrylic composition was applied to the release layer to a thickness of about 20 to 30 μm, and the acrylic composition was cured to produce a protective film having an adhesive layer formed thereon. In this case, the acrylic composition used was acrylic composition A or acrylic composition B.

[0159] The acrylic composition A was prepared by mixing 2-ethylhexyl acrylate (2-EHA) and hydroxyethyl acrylate (HEA) in a weight ratio of 6:4 (2-EHA:HEA) and then polymerizing the mixture to obtain an acrylic polymer component (AP), an acrylic monomer component (AM) obtained by mixing hydroxyethyl acrylate (HEA) and butyl acrylate (BA) in a weight ratio of 3:1 (HEA:BA), and a curing agent, 1,6-hexanediol diacrylate (HDDA), in a weight ratio of 10:85:1 (AP:AM:HDDA), to which an initiator (cumene hydroperoxide, CHP) was added in an amount of about 1 part by weight based on the total weight of the mixture, and a reducing agent (N,N-dimethyl-p-toluidine, DMPT) was added in an amount of about 0.6 parts by weight based on the total weight of the mixture.

[0160] The acrylic composition B is prepared by mixing 2-ethylhexyl acrylate (2-EHA) and hydroxyethyl acrylate (HEA) in a weight ratio of 6:4 (2-EHA:HEA) and polymerizing the mixture, and mixing the mixture with an initiator (methyl ethyl ketone peroxide, SUO-1000) in a weight ratio of 10:85:5 (AP:AM:SUO-1000) with an initiator initiator (methyl ethyl ketone peroxide, SUO-1000) in a weight ratio of 10:85:5 (AP:AM:SUO-1000) with an initiator initiator (methyl ethyl ketone peroxide, SUO-1000) in a weight ratio of 10:85:5 (AP:AM:SUO-1000). The mixture was prepared by adding about 2 parts by weight of a reducing agent (N,N-dimethyl-p-toluidine, DMPT) to the mixture and about 0.6 parts by weight of a reducing agent (N,N-dimethyl-p-toluidine, DMPT) to the mixture.

[0161] Table 1 below shows examples of protective films using the curable compositions, in which the curable composition serves as the release layer of the protective film and the acrylic composition serves as the adhesive layer of the protective film.

[0162] [Table 1]

[0163] <Physical property measurement method> 1. Method for measuring the unreacted material content (TML, total mass loss) ratio (1) 25℃ curing conditions When preparing the protective film, the acrylic composition applied on the release layer was left at 25° C. for 12 or 20 hours to form a pressure-sensitive adhesive layer. A portion of the formed pressure-sensitive adhesive layer was appropriately cut, and a PET (polyethyleneterephthalate) film was attached to both sides of the cut pressure-sensitive adhesive layer to prepare a measurement sample.

[0164] The weight (W A ) was measured and left in an oven at 150° C. for 1 hour. The weight (W B ) was measured. Then, the content of unreacted material (T1) was measured according to the following general formula 2.

[0165] [General formula 2] T1 = 100 × (W A -W B )W A

[0166] In Examples 6 to 9 and Comparative Examples 3 and 4, the acrylic composition applied on the release layer was left at 25°C for 12 hours to measure the unreacted content (T1). In Example 10 and Comparative Example 5, the acrylic composition applied on the release layer was left at 25°C for 20 hours to measure the unreacted content (T1).

[0167] (2) 50℃ curing conditions When preparing the protective film, the acrylic composition applied on the release layer was left for 20 hours at 25° C. to form a pressure-sensitive adhesive layer. A portion of the formed pressure-sensitive adhesive layer was appropriately cut, and a PET (polyethyleneterephthalate) film was attached to both sides of the cut pressure-sensitive adhesive layer to prepare a measurement sample.

[0168] The weight (W C ) was measured and left in an oven at 150° C. for 1 hour. The weight (W D ) was measured. Then, the content of unreacted material (T2) was measured according to the following general formula 3.

[0169] [General formula 3] T2 = 100 × (W C -W D )W C

[0170] The results are shown in Tables 2 and 3 below.

[0171] [Table 2]

[0172] [Table 3]

[0173] 2.Method of measuring release force and residual adhesion rate A standard tape (TESA7475, TESA) having a PET (polyethylene terephthalate) interface was laminated on the adhesive layer of the protective film prepared above, and stored at 70°C for about 24 hours. After that, the standard tape was peeled off at a peel angle of 180° and a peel speed of 0.3 m / min at 25°C using a physical property measuring device (AR-1000, Cheminstruments), and the release force (A i The release force (A i ) are summarized in Table 4 below.

[0174] After measuring the release force, a standard tape (TESA7475, TESA) having a PET (polyethylene terephthalate) interface was laminated on the pressure-sensitive adhesive layer and stored at 70° C. for about 24 hours. The standard tape was then peeled off at a peel angle of 180° and a peel speed of 0.3 m / min at 25° C. using a physical property measuring device (AR-1000, Cheminstruments), and the post-release peel force (A f ) was measured.

[0175] The residual adhesion rate was measured according to the following general formula 1.

[0176] [General formula 1] Residual adhesion rate (A d )=A f / A i ×100(%)

[0177] In the general formula 1, A i is the above-mentioned release peel force (A i ), and A f is the post-release peel force (A f )

[0178] The results are shown in Table 4 below.

[0179] [Table 4]

Claims

1. comprising a polyorganosiloxane component and a redox catalyst; The acrylic composition can be cured; The unreacted content (T 1 The cured product of the acrylic composition has a peel strength of 50 gf / inch (19.3 kg / s) at 25° C., measured at a peel angle of 180° and a peel speed of 0.3 m / min at the interface of a PET film. 2 ) A curable composition which satisfies the following: [General formula 2] T 1 = 100 × (W A -W B ) / W A In the general formula 2, W A is the initial weight of the cured product obtained by curing the acrylic composition at 25° C. for 12 hours or 20 hours, and W B means the post-weight of the cured acrylic composition after storing the cured acrylic composition, the initial weight of which has been measured, in an oven at 150° C. for 1 hour.

2. 2. The curable composition of claim 1, wherein the polyorganosiloxane component comprises a first polyorganosiloxane component represented by the following chemical formula 1: [Chemical formula 1] [Case 1] In Chemical Formula 1, R 1 , R 7 and R 10 each independently represents an alkenyl group having 2 to 20 carbon atoms, an isocyanate group, or an amine group, R 2 , R 3 , R 4 , R 5 , R 6 , R 8 and R 9 each independently represents an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an isocyanate group, or an amine group, m and n are each independently a number in the range of 1 to 10,000.

3. The first polyorganosiloxane component is contained in an amount of 70% by weight or more based on the total weight of the polyorganosiloxane component, and the first polyorganosiloxane component has a weight average molecular weight (M w 3. The curable composition of claim 2, wherein

4. The curable composition according to claim 1 , wherein the polyorganosiloxane component comprises a second polyorganosiloxane component represented by the following chemical formula 2: [Chemical formula 2] [Case 2] In Chemical Formula 2, R 11 ~R 19 are each independently an alkyl group having 1 to 20 carbon atoms, a and b are each independently a number in the range of 1 to 10,000.

5. The second polyorganosiloxane component has a weight average molecular weight (M w 5. The curable composition of claim 4, wherein

6. The curable composition according to claim 1, wherein the redox catalyst comprises at least one selected from the group consisting of naphthenate metal salts, acetate hydrate metal salts, alkanoate metal salts, sulfate hydrate metal salts, acetylacetonate metal salts, halogenide metal salts, and alkoxide metal salts.

7. The curable composition according to claim 1, comprising a redox catalyst in the range of 0.01 to 80 parts by weight per 100 parts by weight of the polyorganosiloxane component.

8. The curable composition of claim 1 further comprising a platinum catalyst.

9. The curable composition of claim 2, comprising a redox catalyst in the range of 0.01 to 80 parts by weight per 100 parts by weight of the first polyorganosiloxane component.

10. The curable composition according to claim 1 , which forms a cured product by curing the acrylic composition without exposure to heat or energy rays.

11. The acrylic composition comprises an acrylic compound, The curable composition of claim 10 , wherein the acrylic compound comprises an alkyl group-containing (meth)acrylate and a hydroxy group-containing (meth)acrylate.

12. The cured product of the acrylic composition has a residual adhesion rate (A d 2. The curable composition according to claim 1, wherein the proportion of 100% or more of the copolymer is 80% or more. [General formula 1] Residual adhesion rate (A d ) = A f / A i ×100(%) In the general formula 1, A i is the 25°C peel strength of the cured acrylic composition measured at the interface of a PET (polyethylene terephthalate) film at a peel angle of 180° and a peel speed of 0.3 m / min, and A f is the above A i After measuring the peel strength at 25° C., the cured acrylic composition was attached to the interface of the PET film again and measured at a peel angle of 180° and a peel speed of 0.3 m / min.

13. The adhesive layer includes a base film, a pressure-sensitive adhesive layer, and a release layer. A protective film, wherein the release layer comprises a cured product of the curable composition according to claim 1 .

14. An optical element having the protective film according to claim 13 attached to one or both surfaces thereof.

15. A liquid crystal display device having an optical element according to claim 14 attached to one or both sides of a liquid crystal panel.

Citation Information

Patent Citations

  • Thermosetting silicone composition

    JP2009263552A

  • Method for manufacturing image display

    JP2012219180A

  • Method for manufacturing a laminate film, adhesive composition kit, and reaction initiator composition

    JP2014043099A

  • Method for producing optical component, adhesive composition kit, and coating composition

    WO2013172284A1

  • Battery module

    KR1020160105354A