Liquid crystal compound, liquid crystal composition thereof, and liquid crystal display device

A liquid crystal compound with enhanced optical and dielectric anisotropy, low rotational viscosity, and high UV stability addresses the limitations of existing compounds, improving display reliability and performance in high-resolution displays.

JP2024542038AActive Publication Date: 2024-11-13JIANGSU HECHENG DISPLAY TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024525741
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-01
Filing Date
2022-09-26
Publication Date
2024-11-13
Estimated Expiration
2042-09-26

AI Technical Summary

Technical Problem

Existing liquid crystal compounds used in liquid crystal displays suffer from low dielectric anisotropy, high rotational viscosity, low UV stability, and poor temperature resistance, which affect display reliability and performance, especially in high-resolution displays.

Method used

Development of a liquid crystal compound with high clearing point, large optical anisotropy, and equal or higher absolute value of dielectric anisotropy, combined with low rotational viscosity and high UV stability, achieved through specific structural modifications in the terminal group of the compound.

Benefits of technology

The new liquid crystal compound maintains appropriate rotational viscosity while enhancing optical anisotropy and dielectric anisotropy, ensuring high contrast, fast response speed, and improved reliability in liquid crystal displays, even after UV exposure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542038000001_ABST
    Figure 2024542038000001_ABST
Patent Text Reader

Abstract

The present invention provides a liquid crystal compound of general formula F, a liquid crystal composition containing the liquid crystal compound, and a liquid crystal display device containing the liquid crystal composition. The liquid crystal compound of the present invention has a high clearing point, a large optical anisotropy, and an equivalent or higher absolute value of dielectric anisotropy while maintaining a suitable rotational viscosity, so that the liquid crystal composition containing the compound of general formula F of the present invention has a large optical anisotropy, a small rotational viscosity, a high VHR(UV) and a long low-temperature storage time while maintaining a suitable clearing point, a suitable absolute value of dielectric anisotropy, and a suitable VHR(initial), and the liquid crystal display device containing the liquid crystal composition of the present invention has a high contrast, a fast response speed, high reliability and high low-temperature storage stability. [Case 1] TIFF2024542038000219.tif26170
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of liquid crystals, and in particular to a liquid crystal compound, a liquid crystal composition comprising said liquid crystal compound, and a liquid crystal display device comprising said liquid crystal composition. [Background technology]

[0002] Liquid crystal display devices can be used in various home appliances such as clocks and calculators, measuring instruments, automotive panels, word processors, computers, printers, televisions, etc. Depending on the type of display mode, liquid crystal display devices can be divided into types such as PC (phase change), TN (twist nematic), STN (super twisted nematic), ECB (electrically controlled birefringence), OCB (optically compensated bend), IPS (in-plane switching), VA (vertical alignment), etc. Depending on the driving method of the device, liquid crystal display devices can be divided into PM (passive matrix) type and AM (active matrix) type. PM can be divided into static and multiplex types. AM can be divided into types such as TFT (thin film transistor) and MIM (metal insulator metal). TFT types include amorphous silicon and polycrystal silicon. The latter can be divided into high-temperature and low-temperature types depending on the manufacturing process. Depending on the type of light source, LCD elements can be divided into reflective types that use natural light, transmissive types that use backlight, and semi-transmissive types that use both natural light and backlight.

[0003] A liquid crystal display element contains a liquid crystal composition having a nematic phase, and the liquid crystal composition has suitable characteristics. By improving the characteristics of the liquid crystal composition, an AM element having good characteristics can be obtained. The relationship between the characteristics of the liquid crystal composition and the characteristics of the AM element is summarized in Table 1 below.

[0004] [Table 1]

[0005] In the application of liquid crystal display devices, the impact of contrast on visual effects is very important. Generally speaking, the higher the contrast, the clearer and more prominent the image is, and the more vivid and beautiful the color is; whereas, if the contrast is low, the whole screen is dull. High contrast contributes greatly to the clarity of the image, the expression of details, and the expression of gradation. High-contrast products have advantages in terms of black-and-white contrast, clarity, completeness, etc. Contrast also has a great impact on the display effect of dynamic video. Because the light-dark transformation in dynamic images is fast, the higher the contrast, the easier it is for the human eye to distinguish such a transformation process.

[0006] With the improvement of the resolution of liquid crystal displays, 4K and 8K resolution liquid crystal displays are gradually emerging, and liquid crystal panels are required to have a small aperture ratio and high light transmittance. Negative liquid crystal compositions have high light transmittance, and the advantage of high light transmittance is more prominent especially in PSA mode and NFFS mode, but the structure of negative liquid crystal determines that they have a large rotational viscosity and a small voltage holding ratio. In order to improve the shortage of conventional negative liquid crystals and provide liquid crystal compositions that meet market demand, it is urgent to develop negative liquid crystal compounds with small rotational viscosity and high voltage holding ratio.

[0007] Chinese patent application CN1942461A and German patent application DE10101022A1 disclose liquid crystal compounds that can solve the above problems to some extent, and Chinese patent application CN107973766A uses ring substitution on the end group structure of this type of compound based on the prior art, but the currently disclosed compounds have problems such as small absolute value of dielectric anisotropy, large rotational viscosity, and low low temperature compatibility.More serious is the low UV stability of benzofuran and benzothiophene compounds, which, as is well known, need to be exposed to a certain amount of UV light during the manufacturing process of liquid crystal panels, and generally, the illuminance of ultraviolet light with a wavelength of 365 nm is about 6000-1000 MJ, and the VHR(UV) of conventional benzofuran and benzothiophene compounds is low after UV light irradiation, which reduces the reliability of the display and causes image retention.

[0008] Therefore, how to obtain a liquid crystal compound and a liquid crystal composition containing the same that can solve or partially solve the above problems remains a problem to be solved in the art. Summary of the Invention [Problem to be solved by the invention]

[0009] In view of the shortcomings of the prior art, the present invention aims to provide a liquid crystal compound having a high clearing point, a large optical anisotropy, and an equivalent or higher absolute value of dielectric anisotropy while maintaining an appropriate rotational viscosity.

[0010] Furthermore, the present invention aims to provide a liquid crystal composition containing the above liquid crystal compound, which has large optical anisotropy, small rotational viscosity, high VHR(UV) and long low-temperature storage time while maintaining a suitable clearing point, a suitable absolute value of dielectric anisotropy and a suitable VHR(initial).

[0011] Another object of the present invention is to provide a liquid crystal display device containing the above liquid crystal composition. [Means for solving the problem]

[0012] In order to achieve the above object of the invention, the present invention provides a liquid crystal compound represented by general formula F: [ka] During the ceremony, R F1 is -H, a halogen, a linear or branched alkyl group containing 1 to 12 (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12) carbon atoms; [ka] [ka] or [ka] wherein one or two or more non-adjacent -CH2- groups in a linear or branched alkyl group containing 1 to 12 carbon atoms may each be independently replaced by -C≡C-, -O-, -CO-, -CO-O- or -O-CO-, and one or more -H groups in the linear or branched alkyl group containing 1 to 12 carbon atoms may each be independently replaced by -F or -Cl, ring [ka] And ring [ka] are each independently [ka] or [ka] represents [ka] and [ka] one or more -CH2- in the ring may be replaced by -O-, and one or more single bonds in the ring may be replaced by a double bond; [ka] and [ka] one or more -H in each ring may be independently replaced by -CN, -F, or -Cl, and one or more -CH= in the ring may be replaced by -N=; X F represents -O-, -S- or -CO-; L F1 and L F2 each independently represents -H, -F, -Cl, -CF3, or -OCF3; Z F1 and Z F2 each independently represents a single bond, -O-, -CO-O-, -O-CO-, -CHO-, -OCH-, -CH=CH-, -C≡C-, -CHCH-, -CFCF-, -(CH)-, -CFO-, or -OCF-, n F1 and n F2 Each independently represents 0, 1, or 2; n F1 If represents 2, the ring [ka] may be the same or different, n F2 If represents 2, the ring [ka] may be the same or different, Z F2 may be the same or different, and n F3 represents an integer from 0 to 4.

[0013] In some embodiments of the present invention, preferably, LF1 and L F2 each independently represents -F or -Cl.

[0014] In some embodiments of the present invention, the compound of general formula F is [ka] [ka] is selected from the group consisting of compounds During the ceremony, X F1 and X F2 each independently represents -CH2- or -O-.

[0015] In some embodiments of the present invention, in order to obtain a large absolute value of the dielectric anisotropy while maintaining a suitable clearing point, a suitable optical anisotropy, and a suitable rotational viscosity, F preferably represents -S-.

[0016] In some embodiments of the present invention, preferably, n F3 represents 0 or 1, and more preferably, n F3 represents 0.

[0017] In some embodiments of the present invention, preferably, Z F1 and Z F2 each independently represents a single bond, -CH2O- or -OCH2-, and more preferably Z F1 and Z F2 Each of them represents a single bond.

[0018] In some embodiments of the present invention, n F1 and n F2 At least one of n represents 0, and more preferably F1 and n F2 Both represent 0.

[0019] In some embodiments of the present invention, preferably, R F1represents a linear or branched alkyl group containing 1 to 10 carbon atoms, a linear or branched alkoxy group containing 1 to 9 carbon atoms, or a linear or branched alkenyl group containing 2 to 10 carbon atoms, and more preferably R F1 represents a linear or branched alkyl group containing 1 to 8 carbon atoms, a linear or branched alkoxy group containing 1 to 7 carbon atoms, or a linear or branched alkenyl group containing 2 to 8 carbon atoms.

[0020] In some embodiments of the present invention, in the compound of formula F-1, the compound of formula F-2, the compound of formula F-3, the compound of formula F-4, the compound of formula F-5, the compound of formula F-6, the compound of formula F-26, and the compound of formula F-27, R F1 represents a straight or branched chain alkoxy group containing 1 to 7 carbon atoms.

[0021] In some embodiments of the present invention, the compound of formula F-1 is [ka] The compound is selected from the group consisting of:

[0022] In some embodiments of the present invention, the compound of formula F-2 is [ka] The compound is selected from the group consisting of:

[0023] In some embodiments of the present invention, the compound of formula F-5 is [ka] The compound is selected from the group consisting of:

[0024] In some embodiments of the present invention, the compound of formula F-6 is [ka] The compound is selected from the group consisting of:

[0025] In some embodiments of the present invention, the compound of formula F-9 is [ka] The compound is selected from the group consisting of:

[0026] The liquid crystal compound of the present invention has a large absolute value of dielectric anisotropy, and is particularly applicable to VA-TFT, IPS or FFS display devices, and has an absolute value of dielectric anisotropy of 10 or more (e.g., 10.5), preferably 12 or more (e.g., 13, 14), preferably 15 or more (e.g., 15.8, 16, 16.4), and is applicable to liquid crystal compositions having high requirements for the absolute value of dielectric anisotropy. Furthermore, when such a compound of the present invention is applied to a liquid crystal composition, it has high miscibility, high low-temperature storage stability, low rotational viscosity and high VHR(UV), and has high reliability even after ultraviolet treatment.

[0027] In another aspect, the present invention provides a liquid crystal composition comprising at least one liquid crystal compound of general formula F above.

[0028] In some embodiments of the present invention, it is preferable to adjust the content of the compound of general formula F so that the liquid crystal composition of the present invention has large optical anisotropy, small rotational viscosity, high VHR(UV) and long low-temperature storage time while maintaining a suitable clearing point, a suitable absolute value of dielectric anisotropy and a suitable VHR(initial).

[0029] In some embodiments of the present invention, the weight percentage of the compound of general formula F in the liquid crystal composition is 0.1% to 30% (all values ​​in between are not included), for example, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 8%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 20%, 22%, 24%, 25%, 26%, 28%, 30%, or a range of values ​​between any two thereof.

[0030] In some embodiments of the present invention, in order to obtain large optical anisotropy, small rotational viscosity, high VHR(UV) and long low-temperature storage time, it is preferred that the liquid crystal composition contains at least two (e.g., two, three) compounds of general formula F.

[0031] In some embodiments of the present invention, the liquid crystal composition further comprises at least one compound of general formula N, [ka] During the ceremony, R N1 and R N2 are each independently a straight-chain or branched-chain alkyl group containing 1 to 12 (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12) carbon atoms; [ka] or [ka] one or two or more non-adjacent -CH2- groups in a linear or branched alkyl group containing 1 to 12 carbon atoms may each be independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -CO-O- or -O-CO-; ring [ka] And ring [ka] are each independently [ka] or [ka] represents [ka] one or more -CH2- in the ring may be replaced by -O-, and one or more single bonds in the ring may be replaced by a double bond; [ka] one or more -H in the ring may be independently replaced by -F, -Cl or -CN, and one or more -CH= in the ring may be independently replaced by -N=; Z N1 and Z N2 each independently represents a single bond, -CO-O-, -O-CO-, -CHO-, -OCH-, -CH=CH-, -C≡C-, -CHCH-, -CFCF-, -(CH)-, -CFO-, or -OCF-, L N1 and L N2 each independently represents -H, an alkyl group having 1 to 3 carbon atoms, or a halogen; and n N1 represents 0, 1, 2 or 3; n N2 represents 0 or 1, and 0≦n N1 +n N2 ≦3, n N1 = 2 or 3, the ring [ka] may be the same or different, Z N1 may be the same or different.

[0032] In some embodiments of the present invention, L N1 and L N2 Both represent -H.

[0033] In some embodiments of the present invention, the compound of general formula N is [ka] [ka] [ka] The compound is selected from the group consisting of:

[0034] In some embodiments of the present invention, preferably, R N1 and R N2 each independently represents a linear or branched alkyl group having 1 to 10 carbon atoms, a linear or branched alkoxy group having 1 to 9 carbon atoms, or a linear or branched alkenyl group having 2 to 10 carbon atoms, and more preferably R N1 and R N2 each independently represents a linear or branched alkyl group containing 1 to 8 carbon atoms, a linear or branched alkoxy group containing 1 to 7 carbon atoms, or a linear or branched alkenyl group containing 2 to 8 carbon atoms.

[0035] In some embodiments of the present invention, the compound of general formula N is preferably selected from the group consisting of a compound of general formula N-1, a compound of general formula N-2, a compound of general formula N-3, a compound of general formula N-9, a compound of general formula N-12, a compound of general formula N-13, a compound of general formula N-19, a compound of general formula N-21, a compound of general formula N-24, a compound of general formula N-27, and a compound of general formula N-30.

[0036] In some embodiments of the present invention, in order to obtain large optical anisotropy, a high clearing point, a small rotational viscosity, suitable VHR (initial), high VHR (UV) and long low-temperature storage time, it is preferable that the compound of general formula N is selected from the group consisting of compounds of general formulas N-2, N-3, N-9, N-12 and N-13.

[0037] In some embodiments of the present invention, in order to obtain large optical anisotropy, small rotational viscosity, high VHR(UV) and long low-temperature storage time, it is preferable that the compound of general formula N is selected from the group consisting of compounds of general formulas N-1, N-19, N-21, N-24, N-27 and N-30.

[0038] In some embodiments of the present invention, it is preferable to adjust the content of the compound represented by general formula N so that the liquid crystal composition of the present invention has a suitable clearing point, a suitable absolute value of dielectric anisotropy, a suitable VHR (initial), a large optical anisotropy, a small rotational viscosity, a high VHR (UV) and a long low-temperature storage time.

[0039] In some embodiments of the present invention, the weight percentage of the compound of general formula N in the liquid crystal composition is 0.1% to 70% (including all values ​​therebetween), for example, 0.1%, 1%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 37%, 38%, 40%, 42%, 44%, 46%, 48%, 49%, 50%, 52%, 53%, 54%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 64%, 66%, 68%, 70%, or a range of values ​​between any two thereof.

[0040] In some embodiments of the present invention, the liquid crystal composition further comprises at least one compound of general formula M, [ka] During the ceremony, R M1 and R M2 are each independently a straight-chain or branched-chain alkyl group containing 1 to 12 (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12) carbon atoms; [ka] [ka] one or two or more non-adjacent -CH2- groups in a linear or branched alkyl group containing 1 to 12 carbon atoms may each be independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -CO-O- or -O-CO-; ring [ka] ,ring [ka] And ring [ka] are each independently [ka] or [ka] represents [ka] one or more -CH2- in the ring may be replaced by -O-, and one or more single bonds in the ring may be replaced by a double bond; [ka] at most one -H may be replaced by halogen; Z M1 and Z M2 each independently represents a single bond, -CO-O-, -O-CO-, -CHO-, -OCH-, -C≡C-, -CH=CH-, -CHCH- or -(CH)-; n M represents 0, 1 or 2; n M If =2, the ring [ka] may be the same or different, Z M2 may be the same or different.

[0041] In some embodiments of the present invention, preferably, R M1 and R M2 each independently represents a linear or branched alkyl group having 1 to 10 carbon atoms, a linear or branched alkoxy group having 1 to 9 carbon atoms, or a linear or branched alkenyl group having 2 to 10 carbon atoms, and more preferably R M1 and R M2 each independently represents a linear or branched alkyl group containing 1 to 8 carbon atoms, a linear or branched alkoxy group containing 1 to 7 carbon atoms, or a linear or branched alkenyl group containing 2 to 8 carbon atoms.

[0042] In some embodiments of the present invention, preferably, R M1 and R M2 each independently represents a linear alkenyl group having 2 to 8 carbon atoms, and more preferably R M1 and R M2 each independently represents a linear alkenyl group having 2 to 5 carbon atoms.

[0043] In some embodiments of the present invention, preferably, R M1 and R M2 One of them is a straight-chain alkenyl group containing 2 to 5 carbon atoms, and the other is a straight-chain alkyl group containing 1 to 5 carbon atoms.

[0044] In some embodiments of the present invention, preferably, R M1 and R M2 each independently represents a linear alkoxy group having 1 to 8 carbon atoms, and more preferably R M1 and R M2 each independently represents a linear alkoxy group containing 1 to 5 carbon atoms.

[0045] In some embodiments of the present invention, preferably, R M1 and R M2 One of them is a linear alkoxy group containing 1 to 5 carbon atoms, and the other is a linear alkyl group containing 1 to 5 carbon atoms.

[0046] In some embodiments of the present invention, when reliability is important, it is preferable to use R M1 and R M2 are all alkyl groups. When it is important to reduce the volatility of the compound, it is preferable to use R M1 and R M2 are both alkoxy groups, and when a reduction in viscosity is important, R M1 and R M2 At least one of the groups is an alkenyl group.

[0047] As used herein, the term "comprising 1 to r carbon atoms" (where r is an integer greater than 1) may include any integer between 1 and r (including the end values ​​1 and r) carbon atoms, such as including 2 carbon atoms, including (r-1) carbon atoms, or including r carbon atoms. For example, "comprising 1 to 12 carbon atoms" may include 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12 carbon atoms.

[0048] As used herein, the term "an integer between y1 and y2" may be any integer within this range, including the end values ​​y1 and y2. For example, an "integer between 0 and 12" may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12.

[0049] The alkenyl group of the present invention is preferably selected from groups represented by any one of formulas (V1) to (V9), and particularly preferably selected from groups represented by formulas (V1), (V2), (V8) and (V9). The groups represented by formulas (V1) to (V9) are: [ka] and In the formula, * represents the bonding site in the linked ring structure.

[0050] The alkenyloxy group of the present invention is preferably selected from groups represented by any one of formulas (OV1) to (OV9), and particularly preferably selected from groups represented by formulas (OV1), (OV2), (OV8) and (OV9). The groups represented by formulas (OV1) to (OV9) are: [ka] and In the formula, * represents the bonding site in the linked ring structure.

[0051] In some embodiments of the present invention, the compound of general formula M is [ka] [ka] The compound is selected from the group consisting of:

[0052] In some embodiments of the present invention, in order to obtain a large optical anisotropy, a suitable clearing point, a small rotational viscosity, a suitable VHR (initial), a high VHR (UV) and a long low-temperature storage time, the compound of general formula M is preferably selected from the group consisting of a compound of general formula M-1, a compound of general formula M-4, a compound of general formula M-11 and a compound of general formula M-13.

[0053] In some embodiments of the present invention, the content of the compound of general formula M needs to be appropriately adjusted depending on the required performance such as solubility at low temperature, transition temperature, electrical reliability, birefringence, process compatibility, drop marks, image sticking, and dielectric anisotropy.

[0054] Regarding the content of the compound of general formula M, when it is necessary to keep the viscosity of the liquid crystal composition of the present invention low and the response time short, it is preferable to make the lower limit high and the upper limit high; furthermore, when it is necessary to keep the clearing point of the liquid crystal composition of the present invention high and the temperature stability good, it is preferable to make the lower limit high and the upper limit high; and in order to keep the driving voltage low and to increase the absolute value of the dielectric anisotropy, it is preferable to make the lower limit low and the upper limit low.

[0055] In some embodiments of the present invention, it is preferable to adjust the content of the compound represented by general formula M so that the liquid crystal composition of the present invention has a suitable clearing point, a suitable absolute value of dielectric anisotropy, a suitable VHR (initial), a large optical anisotropy, a small rotational viscosity, a high VHR (UV) and a long low-temperature storage time.

[0056] In some embodiments of the present invention, the weight percentage of the compound of general formula M in the liquid crystal composition is 0.1% to 70% (including all values ​​therebetween), for example, 0.1%, 1%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%, 35%, 36%, 37%, 38%, 40%, 42%, 44%, 46%, 47%, 48%, 49%, 50%, 52%, 54%, 56%, 58%, 60%, 62%, 64%, 66%, 68%, 70%, or a range of values ​​between any two thereof.

[0057] In some embodiments of the present invention, in order to apply the liquid crystal composition of the present invention to a high-transmittance liquid crystal display, the liquid crystal composition of the present invention further comprises at least one compound selected from the group consisting of compounds of general formula A-1 and general formula A-2. [ka] During the ceremony, R A1 and R A2 are each independently a straight-chain or branched-chain alkyl group containing 1 to 12 (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12) carbon atoms; [ka] or [ka] one or two or more non-adjacent -CH2- groups in the linear or branched alkyl group containing 1 to 12 carbon atoms may be each independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -CO-O- or -O-CO-; [ka] or [ka] one or more -H in each may be independently replaced by -F or -Cl; ring [ka] ,ring [ka] ring [ka] And ring [ka] are each independently [ka] or [ka] represents [ka] and [ka] one or more -CH2- in the ring may be replaced by -O-, and one or more single bonds in the ring may be replaced by a double bond; [ka] and [ka] one or more -H in the ring may be independently replaced by -F, -Cl or -CN, and one or more -CH= in the ring may be independently replaced by -N=; Z A11 , Z A21 and Z A22 each independently represents a single bond, -CH2CH2-, -CF2CF2-, -CO-O-, -O-CO-, -O-CO-O-, -CH=CH-, -CF=CF-, -CH2O- or -OCH2-, L A11 , L A12 , L A13 , L A21 and L A22 each independently represents -H, an alkyl group having 1 to 3 carbon atoms, or a halogen; X A1 and X A2 each independently represents a halogen, a linear or branched halogenated alkyl group or a halogenated alkoxy group containing 1 to 5 carbon atoms, or a linear or branched halogenated alkenyl group or a halogenated alkenyloxy group containing 2 to 5 carbon atoms; n A11 represents 0, 1, 2 or 3; n A11 = 2 or 3, the ring [ka] may be the same or different, Z A11 may be the same or different, n A12 represents 1 or 2, n A12 If =2, the ring [ka] may be the same or different, and n A2 represents 0, 1, 2 or 3; n A2 = 2 or 3, the ring [ka] may be the same or different, Z A21 may be the same or different.

[0058] In some embodiments of the present invention, the compound of formula A-1 is [ka] [ka] [ka] is selected from the group consisting of compounds During the ceremony, R A1 is a linear or branched alkyl group containing 1 to 8 carbon atoms; [ka] or [ka] one or two or more non-adjacent -CH2- groups in a linear or branched alkyl group containing 1 to 8 carbon atoms may each be independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -CO-O- or -O-CO-, and one or more -H groups in these groups may each be independently replaced by -F or -Cl; R v and R w each independently represents -CH2- or -O-; L A11 , L A12, L A11 ', L A12 ′, L A14 , L A15 and L A16 each independently represents -H or -F; L A13 and L A13 Each ' independently represents -H or -CH; X A1 represents -F, -CF3 or -OCF3, and v and w each independently represent 0 or 1.

[0059] In some embodiments of the present invention, the weight percentage of the compound of general formula A-1 in the liquid crystal composition is 0.1% to 50% (including all values ​​therebetween), for example, 0.1%, 1%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38%, 40%, 42%, 44%, 46%, 48%, 50%, or a range of values ​​between any two thereof.

[0060] Regarding the preferred content of the compound of general formula A-1, when the viscosity of the liquid crystal composition of the present invention is to be kept low and the response speed is to be kept high, it is preferable that the lower limit be slightly lower and the upper limit be slightly lower. Furthermore, when the clearing point of the liquid crystal composition of the present invention is to be kept high and the temperature stability is to be kept high, it is preferable that the lower limit be slightly lower and the upper limit be slightly lower. Furthermore, when it is desired to keep the driving voltage low and to increase the absolute value of the dielectric anisotropy, it is preferable that the lower limit be slightly higher and the upper limit be slightly higher.

[0061] In some embodiments of the present invention, the compound of formula A-2 is [ka] [ka] is selected from the group consisting of compounds During the ceremony, R A2 represents a linear or branched alkyl group containing 1 to 8 carbon atoms, in which one or two or more non-adjacent -CH2- groups in the linear or branched alkyl group containing 1 to 8 carbon atoms may each be independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -CO-O- or -O-CO-, and one or more -H present in these groups may each be independently replaced by -F or -Cl, L A21 , L A22 , L A23 , L A24 and L A25 each independently represents -H or -F, and X A2 represents -F, -CF3, -OCF3 or -CH2CH2CH=CF2.

[0062] In some embodiments of the present invention, the weight percentage of the compound of general formula A-2 in the liquid crystal composition is 0.1% to 50% (including all values ​​therebetween), for example, 0.1%, 1%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38%, 40%, 42%, 44%, 46%, 48%, 50%, or a range of values ​​between any two thereof.

[0063] Regarding the preferred content of the compound of general formula A-2, when the viscosity of the liquid crystal composition of the present invention is to be kept low and the response speed is to be kept high, it is preferable to make the lower limit slightly lower and the upper limit slightly lower. Furthermore, when the clearing point of the liquid crystal composition of the present invention is to be kept high and the temperature stability is to be kept high, it is preferable to make the lower limit slightly lower and the upper limit slightly lower. Furthermore, when it is desired to keep the driving voltage low and to increase the absolute value of the dielectric anisotropy, it is preferable to make the lower limit slightly higher and the upper limit slightly higher.

[0064] In some embodiments of the present invention, the weight percentage of the compound selected from the group consisting of compounds of general formula A-1 and general formula A-2 in the liquid crystal composition is 0.1% to 60% (including all values ​​therebetween), for example, 0.1%, 1%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38%, 40%, 42%, 44%, 46%, 48%, 50%, 52%, 54%, 56%, 58%, 60%, or a range of values ​​between any two thereof.

[0065] In some embodiments of the present invention, the liquid crystal composition further comprises at least one polymerizable compound of the general formula RM, [ka] During the ceremony, R1 is -H, halogen, -CN, -Sp2-P2, or a linear or branched alkyl group containing 1 to 12 (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12) carbon atoms; [ka] or [ka] represents a linear or branched alkyl group having 1 to 12 carbon atoms; [ka] or [ka] in which one or two or more non-adjacent -CH2- groups may each independently be replaced by -CH=CH-, -C≡C-, -O-, -CO-, -CO-O- or -O-CO-; and one or more -H groups may each independently be replaced by -F or -Cl; ring [ka] And ring [ka] are each independently [ka] or [ka] represents [ka] and [ka] one or more -CH2- in the ring may be replaced by -O-, and one or more single bonds in the ring may be replaced by a double bond; [ka] and [ka] one or more -H are each independently -F, -Cl, -CN, -Sp3-P3, a halogenated or non-halogenated linear alkyl group containing 1 to 12 (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12) carbon atoms, a halogenated or non-halogenated linear alkoxy group containing 1 to 11 carbon atoms, [ka] or [ka] and one or more -CH= in the ring may be replaced by -N=; ring [ka] teeth, [ka] or [ka] represents [ka] or [ka] one or more -H in each independently represents -F, -Cl, -CN, -Sp3-P3, a halogenated or non-halogenated linear alkyl group containing 1 to 12 (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12) carbon atoms, a halogenated or non-halogenated linear alkoxy group containing 1 to 11 (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, or 11) carbon atoms, [ka] or [ka] and one or more -CH= in the ring may be replaced by -N=; P1, P2, and P3 each independently represent a polymerizable group. Sp1, Sp2, and Sp3 each independently represent a spacer group or a single bond; Z1 and Z2 each independently represent -O-, -S-, -CO-, -CO-O-, -O-CO-, -O-CO-O-, -CHO-, -OCH-, -CHS-, -SCH-, -CFO-, -OCF-, -CFS-, -SCF-, -(CH) d -, -CF2CH2-, -CH2CF2-, -(CF2) d -, -CH=CH-, -CF=CF-, -CH=CF-, -CF=CH-, -C≡C-, -CH=CH-CO-O-, -O-CO-CH=CH-, -CH2CH2-CO-O-, -O-CO-CH2CH2-, -CHR 1-, -CR 1 R 2 - or a single bond, R 1 and R 2 each independently represents a linear or branched alkyl group containing 1 to 12 (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12) carbon atoms; d represents an integer of 1 to 4; X0 represents -O-, -S-, -CO-, -CF2-, -NH-, or -NF-; a represents 0, 1 or 2, b represents 0 or 1, and when a represents 2, the ring [ka] may be the same or different, and Z1 may be the same or different.

[0066] In some embodiments of the invention, the compound of general formula RM is [ka] [ka] [ka] [ka] [ka] is selected from the group consisting of compounds During the ceremony, X1~X 10 and X 12 each independently represents -F, -Cl, -Sp3-P3, a linear alkyl group or an alkoxy group having 1 to 5 carbon atoms; [ka] or [ka] Represents.

[0067] Polymerizable groups according to the invention are groups which are applied in polymerization reactions (for example free radical or ionic polymerization, addition polymerization or condensation polymerization) or in addition or condensation reactions in the polymer backbone. For chain polymerization, polymerizable groups containing -CH=CH- or -C≡C- are particularly preferred, and for ring-opening polymerization, for example, oxetanyl or epoxy groups are particularly preferred.

[0068] In some embodiments of the present invention, the polymerizable groups P1, P2, and P3 are each independently [ka] or -SH, and preferably, the polymerizable groups P1, P2 and P3 each independently represent [ka] or -SH, and more preferably, the polymerizable groups P1, P2 and P3 each independently represent [ka] or [ka] Represents.

[0069] As used herein, the term "spacer group" is known to those skilled in the art and described in the literature (e.g. Pure Appl. Chem. 2001, 73(5), 888 and C. Tschierske, G. Pelzl, S. Diele, Angew. Chem. 2004, 116, 6340-6368). As used herein, the term "spacer group" refers to a flexible group that connects a mesogenic group and a polymerizable group in a polymerizable compound. Typical spacer groups include, for example, -(CH2)p1-, -(CH2CH2O)q1-CH2CH2-, -(CH2CH2S)q1-CH2CH2-, -(CH2CH2NH)q1-CH2CH2-, -CR 0 R 00 -(CH2)p1 -or- (SiR 0 R 00 -O)p1-, p1 represents an integer of 1 to 12, q1 represents an integer of 1 to 3, R 0 and R 00 each independently represents -H, a linear or branched alkyl group containing 1 to 12 carbon atoms, or a cyclic alkyl group containing 3 to 12 carbon atoms. Particularly preferred spacer groups are -(CH2)p1-, -(CH2)p1-O-, -(CH2)p1-O-CO-, -(CH2)p1-CO-O-, -(CH2)p1-O-CO-O-, or -CR 0 R 00 -(CH2) p1 -It is.

[0070] In some embodiments of the present invention, the weight percentage of the polymerizable compound of general formula RM in the liquid crystal composition is 0.001% to 5% (including all values ​​therebetween), for example, 0.001%, 0.002%, 0.004%, 0.005%, 0.006%, 0.008%, 0.01%, 0.02%, 0.04%, 0.06%, 0.08%, 0. .1%, 0.2%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, 0.3%, 0.32%, 0.33%, 0.34%, 0.35%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.6%, 1.8%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% or a numerical range between any two thereof.

[0071] In some embodiments of the present invention, the liquid crystal composition further comprises at least one additive.

[0072] In addition to the above compounds, the liquid crystal composition of the present invention may contain a general nematic liquid crystal, a smectic liquid crystal, a cholesteric liquid crystal, a dopant, an antioxidant, an ultraviolet absorber, an infrared absorber, a polymerizable monomer, or a light stabilizer.

[0073] Dopants that may be preferably added to the liquid crystal composition according to the present invention are as follows: [ka] [ka] It is.

[0074] In some embodiments of the present invention, the weight percentage of the dopant in the liquid crystal composition is 0% to 5%, and preferably the weight percentage of the dopant in the liquid crystal composition is 0.01% to 1%.

[0075] The additives used in the liquid crystal composition of the present invention, such as an antioxidant, a light stabilizer, and an ultraviolet absorbing agent, are preferably the following substances. [ka] [ka] [ka] In the formula, n represents a positive integer of 1 to 12.

[0076] Preferably, the antioxidant is selected from the compounds listed below. [ka] In some embodiments of the present invention, the total weight percentage of the additives in the liquid crystal composition is 0% to 5%, and preferably the total weight percentage of the additives in the liquid crystal composition is 0.01% to 1%.

[0077] The liquid crystal composition containing the polymerizable compound of the present invention can be polymerized even in the absence of a polymerization initiator, but may further contain a polymerization initiator to promote polymerization. Examples of the polymerization initiator include benzoin ethers, benzophenones, acetophenones, benzil ketals, and acylphosphine oxides.

[0078] As for the polymerization method of the polymerizable compound, since rapid polymerization is desirable, a method of polymerization by irradiation with active energy rays such as ultraviolet rays or electron beams is preferable. When ultraviolet rays are used, a polarized light source may be used or a non-polarized light source may be used. When the liquid crystal composition is sandwiched between both substrates and polymerization is performed, at least the substrate on the irradiation side needs to have appropriate transparency to active energy rays. In addition, a mask may be used during light irradiation to polymerize only specific parts, and then the orientation state of the unpolymerized parts may be changed by changing conditions such as an electric field, a magnetic field, or temperature, and then polymerization may be performed by irradiating with active energy rays. In particular, when ultraviolet exposure is performed, preferably, a voltage is applied to the liquid crystal composition and ultraviolet exposure is performed at the same time.

[0079] The temperature at which active energy rays such as ultraviolet rays or electron beams are irradiated is preferably within a temperature range at which the liquid crystal composition of the present invention maintains its liquid crystal state. Polymerization is preferably carried out at a temperature close to room temperature (i.e., 15 to 35°C). Lamps that generate ultraviolet rays include metal halide lamps, high pressure mercury lamps, and ultra-high pressure mercury lamps. In addition, it is preferable to irradiate ultraviolet rays having a wavelength outside the absorption wavelength range of the liquid crystal composition, and it is preferable to use the ultraviolet rays while blocking them as necessary. The intensity of the irradiated ultraviolet rays is preferably 0.1 mW / cm. 2 ~50mW / cm 2 When irradiating ultraviolet rays, the intensity can be changed, and the irradiation time of ultraviolet rays can be appropriately selected according to the intensity of the irradiated ultraviolet rays, and is preferably 10 s to 600 s.

[0080] In another aspect, the present invention further provides a liquid crystal display device comprising the above liquid crystal composition.

[0081] In some embodiments of the present invention, the liquid crystal composition is particularly applicable to a VA, IPS or FFS type display device. Effect of the Invention

[0082] Compared with the prior art, the liquid crystal compound of the present invention has a high clearing point, a large optical anisotropy, and an equivalent or higher absolute value of dielectric anisotropy while maintaining an appropriate rotational viscosity. A liquid crystal composition containing the above liquid crystal compound of the present invention has a large optical anisotropy, a small rotational viscosity, a high VHR(UV) and a long low-temperature storage time while maintaining an appropriate clearing point, an appropriate absolute value of dielectric anisotropy and an appropriate VHR(initial), so that a liquid crystal display device containing the liquid crystal composition has a high contrast, a fast response speed, high reliability and high low-temperature storage stability. [Brief description of the drawings]

[0083] [Figure 1] This is the mass spectrum of compound F-2-4. [Diagram 2] 1 is a DSC cooling spectrum of compound F-2-4. [Diagram 3] 1 is a DSC heating spectrum of compound F-2-4. [Figure 4] This is the mass spectrum of compound F-1-4. [Diagram 5] 1 is a DSC cooling spectrum of compound F-1-4. [Figure 6] 1 is a DSC heating spectrum of compound F-1-4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0084] The present invention will be described below with reference to specific embodiments. Note that the following examples are illustrative of the present invention and are only intended to explain the present invention, and are not intended to limit the present invention. Other combinations and various improvements within the concept of the present invention can be made without departing from the spirit or scope of the present invention.

[0085] In the present invention, unless otherwise specified, all contents refer to percentages by weight.

[0086] For ease of explanation, in each of the following examples, the radical structures of each compound are represented by the codes shown in Table 2.

[0087] [Table 2]

[0088] Take the compound of the following structural formula as an example: [ka] When the structural formula is represented by the code shown in Table 2, it can be represented as nCCGF, where n in the code represents the number of C atoms in the alkyl group at the left end. For example, when n is "3", it represents that the alkyl group is -C3H7, C in the code represents a 1,4-cyclohexylene group, G represents a 2-fluoro-1,4-phenylene group, and F represents a fluorine substituent.

[0089] The abbreviations for the test items in the following examples are as follows. Cp Clearing point (nematic-isotropic phase transition temperature, °C) Δn Optical anisotropy (589nm, 20℃) Δε Dielectric constant anisotropy (1KHz, 20℃) VHR (initial) Initial voltage retention rate (%) VHR(UV) Voltage retention rate (%) after ultraviolet light (UV) irradiation t -30℃ Low temperature storage time (days, -30℃) γ1 rotational viscosity (mPa·s, 20℃) Cp is obtained by testing with a melting point apparatus. Δn is obtained by testing at 20° C. using an Abbe refractometer under a sodium lamp (589 nm) light source. For Δε, Δε = ε || -ε ⊥ and ε || is the dielectric constant parallel to the molecular axis, and ε ⊥ is the dielectric constant perpendicular to the molecular axis, and the test conditions are 20°C, 1KHz, and a VA type test box with a thickness of 6 μm is used. VHR (initial) is the initial voltage holding ratio, which is obtained by a test using a TOY06254 type liquid crystal physical property evaluation system, with a test temperature of 60°C, a test voltage of 5V, a test frequency of 6Hz, and a TN type test box with a thickness of 9μm. VHR (UV) was obtained by testing with a TOY06254 liquid crystal physical property evaluation system, with a wavelength of 365 nm and energy of 6000 mJ / cm 2 The liquid crystal is irradiated with UV light and then tested, the test temperature is 60° C., the test voltage is 5V, the test frequency is 6Hz, and a TN type test box with a thickness of 9 μm is used. t -30℃ is the time recorded when a nematic phase liquid crystal medium is placed in a glass bottle and stored at -30°C and crystal precipitation is observed. γ1 was obtained by a test using an LCM-2 type liquid crystal physical property evaluation system, and the test conditions were 20° C., 160 to 240 V, and a test box with a thickness of 20 μm.

[0090] The liquid crystal compounds of the general formula F of the present invention can be prepared by conventional organic synthesis methods, and methods for introducing the target end groups, ring structures and linking groups into starting materials are described in such literature as Organic Synthesis (John Wiley & Sons Inc.), Organic Reactions (John Wiley & Sons Inc.) and Comprehensive Organic Synthesis (Pergamon Press).

[0091] Linking group Z in liquid crystal compounds of formula F F1 ~Z F3 The synthesis method of MSG can be seen in the following scheme. 1 or MSG 2 is a monovalent organic group having at least one ring, and the multiple MSGs used in the following schemes 1 (or MSG 2 ) may be the same or different.

[0092] (1) Synthesis of a single bond [ka] The single bond compound IA is obtained by reacting arylboronic acid 1 with compound 2, which is synthesized by a known method, in the presence of a catalyst (e.g., tetrakis(triphenylphosphine)palladium (Pd(PPh3)4)) in an aqueous sodium carbonate solution. Alternatively, compound 3, which is synthesized by a known method, can be reacted with n-butyllithium (n-BuLi), further reacted with zinc chloride, and then reacted with compound 2 in the presence of a catalyst (dichlorobis(triphenylphosphine)palladium (PdCl2(PPh3)2)) to prepare the single bond compound IA.

[0093] (2) Synthesis of -CO-O- and -O-CO- [ka] Compound 3 is reacted with n-butyl lithium and further with carbon dioxide to obtain carboxylic acid 4. Compound 4 and compound 5, which is synthesized by a known method, are dehydrated in the presence of 1,3-dicyclohexylcarbodiimide (DCC) and 4-dimethylaminopyridine (DMAP) to synthesize compound IB having -CO-O-. Compounds having -O-CO- can also be synthesized by this method.

[0094] (3) Synthesis of -CF2O- and -OCF2- [ka] Compound IB was treated with a sulfurizing agent (e.g., Lawesson's reagent) to obtain compound 6, and then compound IC having -CF2O- was synthesized by fluorinating compound 6 with hydrogen fluoride-pyridine (HF-Py) and N-bromosuccinimide (NBS) as described in M. Kuroboshi et al., Chem. Lett., 1992, 827. Compound IC having -CF2O- can also be prepared by fluorinating compound 6 with (diethylamino)sulfur trifluoride (DAST) as described in WH Bunnelle et al., J. Org. Chem, 1990, 55, 768. Compound IC having -CF2O- can also be synthesized by these methods.

[0095] (4) Synthesis of -CH=CH- [ka] Compound 3 is reacted with n-butyllithium, and then with formamide (e.g., N,N-dimethylformamide (DMF)) to obtain compound 7. The phosphonium generated by reacting potassium tert-butoxide (t-BuOK) with phosphonium salt 8 synthesized by a known method is reacted with compound 7 to obtain compound ID. Depending on the reaction conditions, the cis form is generated by the above method. It should be understood that the cis form can be converted to a trans form by a known method, if necessary.

[0096] (5) Synthesis of -CH2CH2- [ka] Compound ID can be subjected to a hydrogenation reaction using a catalyst (eg, palladium on carbon (Pd / C)) to prepare compound IE.

[0097] (6) Synthesis of -CH2O- or -OCH2- [ka] Compound 7 is reduced with sodium borohydride (NaBH4) to obtain compound 9. Compound 9 is then halogenated with hydrobromic acid to obtain compound 10, or the hydroxyl group of compound 9 is protected with p-toluenesulfonic acid (TsOH) to obtain compound 11. Compound 10 or compound 11 is then reacted with compound 5 in the presence of potassium carbonate to obtain compound IF. Compounds having -OCH2- can also be synthesized by these methods.

[0098] (7) Synthesis of -CH=CF2 [ka] Compound IG can be prepared by removing the hydrofluoric acid at the end chain of compound 11 with a solution of lithium diisopropylamide (LDA) in tetrahydrofuran.

[0099] For ring structures such as a 1,4-cyclohexylene group, a 1,3-dioxane-2,5-diyl group, a 1,4-phenylene group, a 2-fluoro-1,4-phenylene group, a 2,3-difluoro-1,4-phenylene group, a 2,5-difluoro-1,4-phenylene group, a 2,6-difluoro-1,4-phenylene group, and a 2,3,5,6-tetrafluoro-1,4-phenylene group, the starting materials are already commercially available, or the synthesis methods thereof are known in the art.

[0100] A preferred method for synthesizing representative compounds is shown below. [Synthesis Example 1]

[0101] The synthetic route of compound F-2-4 is shown below. [ka]

[0102] Step 1: Preparation of compounds of formula B-3 In a 2L reaction flask, add 99g of the compound of general formula B-1 ((4-butoxy-2,3-difluorophenyl)boronic acid), 100g of the compound of general formula B-2 (2-bromo-6-fluorophenol) and 110g of sodium carbonate, and dissolve them thoroughly in 1.2L of a mixed solvent consisting of toluene, ethanol and water (the volume ratio of toluene, ethanol and water is 2:1:1). Under the protection of a nitrogen atmosphere, add 1.8g of Pd(PPh3)4 and reflux at 100°C for 6 hours. The reaction solution is cooled to room temperature, 300 mL of water is added to separate the liquid, the aqueous phase is extracted with 20 mL of toluene, the organic phase is combined, the organic phase is washed with saturated NaCl aqueous solution until pH=7, dried with anhydrous Na2SO4, concentrated, and recrystallized with a mixed solvent of petroleum ether and toluene (volume ratio of petroleum ether to toluene is 24:1) to obtain 109.5 g of a white solid compound of general formula B-3 (4'-butoxy-2',3',3-trifluoro-[1,1'-biphenyl]-2-ol) (yield: 85%).

[0103] Step 2: Preparation of compounds of formula B-4 In a 2L reaction flask, 110g of the compound of general formula B-3 and 72g of potassium carbonate are added, thoroughly dissolved in 700mL of N,N-dimethylformamide, and reacted at 120°C for 9 hours. The reaction mixture is cooled to room temperature, 3.5L of water is added, stirred, and suction filtered to obtain a crude product, which is slurried in ethanol, suction filtered, and dried over anhydrous Na2SO4 to obtain 88.5g of the compound of general formula B-4 (3-butoxy-4,6-difluorodibenzo[b,d]furan) as a gray solid (yield: 86.3%).

[0104] Step 3: Preparation of compounds of formula B-5 In a 2L reaction flask, add 38g of diisopropylamine, dissolve thoroughly in 500mL of tetrahydrofuran, and under the protective condition of nitrogen atmosphere, control the temperature at -20℃, add 150mL of n-butyllithium, control the temperature at -20℃ and react for 3 hours; add 90g of the compound of general formula B-4, control the temperature at -78℃ and react for 3 hours; add 70g of triisopropyl borate, control the temperature at 78℃ and react for 3 hours. The mixture is adjusted to pH=2-3 with dilute hydrochloric acid, separated, the aqueous phase is extracted with ethyl acetate, the organic phases are combined, the organic phase is washed with saturated aqueous NaCl solution until pH=7, dried over anhydrous Na2SO4, concentrated, slurried with dichloromethane, suction filtered, and the filter cake is dried to obtain 73 g of a white solid compound of general formula B-5 ((4,6-difluoro-7-butoxydibenzo[b,d]furan-3-yl)boronic acid) (yield: 70%).

[0105] Step 4: Preparation of compounds of formula B-6 In a 2L reaction flask, add 70g of the compound of general formula B-5, dissolve it sufficiently in 700mL of tetrahydrofuran, control the temperature at 10℃, add 68g of 30% hydrogen peroxide water, control the temperature at 10℃ and react for 9 hours, quench with 500mL of 5% sodium thiosulfate solution, separate, extract the aqueous phase with ethyl acetate, combine the organic phase, wash the organic phase with saturated NaCl aqueous solution until pH=7, dry with anhydrous Na2SO4, concentrate, slurry with 25mL of dichloromethane, suction filter, dry the filter cake to obtain 55.6g of the compound of general formula B-6 (4,6-difluoro-7-butoxydibenzo[b,d]furan-3-ol), which is a white solid (yield: 90%).

[0106] Step 5: Preparation of compounds of formula B-7 In a 2L reaction flask, add 70g of the compound of general formula B-6, dissolve it sufficiently in 700mL of tetrahydrofuran, control the temperature at 10℃ and add 68g of trifluoroethanol, control the temperature at 10℃ and react for 9 hours, extract the aqueous phase with ethyl acetate, combine the organic phase, wash the organic phase with saturated NaCl aqueous solution until pH=7, dry with anhydrous Na2SO4, concentrate, slurry with 25mL of dichloromethane, suction filter, dry the filter cake, obtain 53.8g of the compound of general formula B-7 (4,6-difluoro-3-butoxy-7-(2,2,2-trifluoroethoxy)dibenzo[b,d]furan) which is a white solid (yield: 60%).

[0107] Step 6: Preparation of compounds of formula F-2-4 In a 2L reaction flask, add 40g of the compound of general formula B-7, dissolve it sufficiently in 700mL of tetrahydrofuran, control the temperature at 10℃ and add 40g of 30% sodium hydroxide solution, react for 8 hours, quench the reaction with 500mL of 5% sodium thiosulfate, separate, extract the aqueous phase with ethyl acetate, combine the organic phase, wash the organic phase with saturated NaCl aqueous solution until pH=7, dry with anhydrous Na2SO4, concentrate, slurried with 25mL of dichloromethane, suction filtered, and dry the filter cake to obtain 28.4g of the compound of general formula F-2-4 (3-((2,2-difluorovinyl)oxy)-4,6-difluoro-7-butoxydibenzo[b,d]furan), which is a white solid (yield: 75%).

[0108] The mass spectrum of the compound of formula F-2-4 is shown in FIG.

[0109] The DSC cooling spectrum of the compound of the general formula F-2-4 is shown in FIG.

[0110] The DSC temperature rise spectrum of the compound of general formula F-2-4 is shown in FIG. [Synthesis Example 2]

[0111] The synthetic route of compound F-1-4 is shown below. [ka]

[0112] The compound of the formula B-3 was synthesized in the same manner as in Synthesis Example 1.

[0113] Step 1, Preparation of Compound of Formula B-8 In a 1L reaction flask, add 120g of the compound of general formula B-3, 120g of dimethylthiocarbamoyl chloride and 90g of triethylamine, dissolve thoroughly with 440mL of isododecane, and under the protective condition of nitrogen atmosphere, control the temperature at 165℃ to reflux and react for 18 hours, cool to 25℃, suction filter, recrystallize with ethanol, suction filter, and dry filter cake to obtain 78.9g of the compound of general formula B-8 (3-butoxy-4,6-difluorodibenzo[b,d]thiophene) which is a brown solid (yield: 66.667%).

[0114] Step 2: Preparation of compounds of formula B-9 In a 2L reaction flask, add 38g of diisopropylamine, dissolve thoroughly in 500mL of tetrahydrofuran, and under the protective condition of nitrogen atmosphere, add 150mL of n-butyllithium at -20℃, react for 3 hours at -20℃; add 80g of the compound of general formula B-8, react for 3 hours at -78℃; add 70g of triisopropyl borate, react for 3 hours at 78℃. The mixture is adjusted to pH=2-3 with dilute hydrochloric acid, separated, the aqueous phase is extracted with ethyl acetate, the organic phases are combined, the organic phase is washed with saturated aqueous NaCl solution until pH=7, dried over anhydrous Na2SO4, concentrated, slurried with dichloromethane, suction filtered, and the filter cake is dried to obtain 69 g of a white solid compound of general formula B-9 ((4,6-difluoro-7-butoxydibenzo[b,d]thiophen-3-yl)boronic acid) (yield: 75%).

[0115] Step 3: Preparation of compounds of formula B-10 In a 2L reaction flask, add 70g of the compound of general formula B-9, dissolve it sufficiently in 700mL of tetrahydrofuran, control the temperature at 10 ° C. and add 80g of 30% hydrogen peroxide water, control the temperature at 10 ° C. and react for 9 hours, quench with 500mL of 5% sodium thiosulfate solution, separate, extract the aqueous phase with ethyl acetate, combine the organic phase, wash the organic phase with saturated NaCl aqueous solution until pH = 7, dry with anhydrous Na2SO4, concentrate, slurry with 25mL of dichloromethane, suction filter, dry the filter cake to obtain 41.3g of the compound of general formula B-10 (4,6-difluoro-7-butoxydibenzo [b, d] thiophene-3-ol), which is a white solid (yield: 64.3%).

[0116] Step 4: Preparation of compounds of formula B-11 In a 2L reaction flask, add 70g of the compound of general formula B-10, dissolve it sufficiently in 700mL of tetrahydrofuran, control the temperature at 10℃ and add 68g of trifluoroethanol, control the temperature at 10℃ and react for 9 hours, extract the aqueous phase with ethyl acetate, combine the organic phase, wash the organic phase with saturated NaCl aqueous solution until pH=7, dry with anhydrous Na2SO4, concentrate, slurry with 25mL of dichloromethane, suction filter, dry the filter cake to obtain 56.7g of the compound of general formula B-11 (4,6-difluoro-3-butoxy-7-(2,2,2-trifluoroethoxy)dibenzo[b,d]furan) which is a white solid (yield: 64%).

[0117] Step 5: Preparation of compounds of formula F-1-4 In a 2L reaction flask, add 40g of the compound of general formula B-11, dissolve it sufficiently in 700mL of tetrahydrofuran, control the temperature at 10 ° C. and add 40g of 30% sodium hydroxide solution, control the temperature at 10 ° C. and react for 8 hours, quench the reaction with 500mL of 5% sodium thiosulfate, separate, extract the aqueous phase with ethyl acetate, combine the organic phase, wash the organic phase with saturated NaCl aqueous solution until pH = 7, dry with anhydrous Na2SO4, concentrate, slurry with 25mL of dichloromethane, suction filter, and dry the filter cake to obtain 30.4g of the compound of general formula F-1-4 (3-((2,2-difluorovinyl)oxy)-4,6-difluoro-7-butoxydibenzo[b,d]furan), which is a white solid (yield: 80%).

[0118] The mass spectrum of the compound of formula F-1-4 is shown in FIG.

[0119] The DSC cooling spectrum of the compound of the general formula F-1-4 is shown in FIG.

[0120] The DSC temperature rise spectrum of the compound of the general formula F-1-4 is shown in FIG.

[0121] The compound of formula F prepared in the above examples and the compound DB-1 ( [ka] ) and DB-2( [ka] ) and the base liquid crystal are mixed at 10% by weight:90% by weight to obtain a mixture. The performance parameter values ​​of the test compound are calculated by the extrapolation method, and the extrapolated values ​​of Cp, Δn, and Δε are ((measured value of the mixture)-0.9×(measured value of the base liquid crystal)) / 0.1, and the extrapolated value of γ1 is 10 10(lgA-0.9lgB) where A is the γ1 of the mixture and B is the γ1 of the parent liquid crystal. According to this method, the performance parameters such as the clearing point Cp, the optical anisotropy Δn, the dielectric anisotropy Δε, and the rotational viscosity γ1 are derived.

[0122] [Table 3]

[0123] The extrapolated liquid crystal performance parameters of the above compounds are shown in Table 4 below.

[0124] [Table 4]

[0125] Comparison of the test results of the performance parameters of compounds DB-1, DB-2 and the compound of general formula F of the present invention in Table 4 shows that the compound of general formula F of the present invention has a higher clearing point, a larger optical anisotropy, and the same or higher absolute value of dielectric anisotropy while maintaining an appropriate rotational viscosity.

[0126] The components used in the following examples can be synthesized by known methods or obtained commercially. These synthesis techniques are common and the resulting liquid crystal compounds have been measured to meet the standards of electronic compounds.

[0127] In the present invention, unless otherwise specified, all contents refer to percentages by weight.

[0128] The liquid crystal composition is prepared according to the blending ratio of each liquid crystal composition specified in the following examples. The liquid crystal composition is prepared by a general method in this field, for example, by mixing according to the ratio using a method such as heating, ultrasonic wave, suspension, etc. [Application comparison example 1]

[0129] According to each compound and their weight percentage shown in Table 5, a liquid crystal composition of Comparative Application Example 1 is prepared, and the liquid crystal composition is filled between both substrates of a liquid crystal display to carry out a performance test.

[0130] [Table 5] [Application Example 1]

[0131] According to each compound and their weight percentage shown in Table 6, the liquid crystal composition of Application Example 1 is prepared, and the liquid crystal composition is filled between both substrates of a liquid crystal display to carry out a performance test.

[0132] [Table 6]

[0133] A comparison between Application Comparison Example 1 and Application Example 1 shows that the liquid crystal composition of the present invention has a small rotational viscosity, a high VHR (UV) and a long low-temperature storage time while maintaining a suitable clearing point, suitable optical anisotropy, suitable dielectric anisotropy and suitable VHR (initial). [Application comparison example 2]

[0134] According to each compound and their weight percentage shown in Table 7, a liquid crystal composition of Comparative Application Example 2 is prepared, and the liquid crystal composition is filled between both substrates of a liquid crystal display to carry out a performance test.

[0135] [Table 7] [Application Example 2]

[0136] According to each compound and their weight percentage shown in Table 8, the liquid crystal composition of Application Example 2 is prepared, and the liquid crystal composition is filled between both substrates of a liquid crystal display to carry out a performance test.

[0137] [Table 8]

[0138] A comparison between Application Comparison Example 2 and Application Example 2 shows that the liquid crystal composition of the present invention has large optical anisotropy, small rotational viscosity, high VHR (UV) and long low-temperature storage time while maintaining an appropriate clearing point, appropriate absolute value of dielectric anisotropy and appropriate VHR (initial). [Application comparison example 3]

[0139] According to each compound and their weight percentage shown in Table 9, a liquid crystal composition of Comparative Application Example 3 is prepared, and the liquid crystal composition is filled between both substrates of a liquid crystal display to carry out a performance test.

[0140] [Table 9] [Application Example 3]

[0141] According to each compound and their weight percentage shown in Table 10, the liquid crystal composition of Application Example 3 is prepared, and the liquid crystal composition is filled between both substrates of a liquid crystal display to carry out a performance test.

[0142] [Table 10]

[0143] A comparison between Application Comparison Example 3 and Application Example 3 shows that the liquid crystal composition of the present invention has a small rotational viscosity, a high VHR (UV) and a long low-temperature storage time while maintaining a suitable clearing point, a suitable optical anisotropy, a suitable absolute value of dielectric anisotropy and a suitable VHR (initial). [Application Example 4]

[0144] A liquid crystal composition was prepared according to the compounds and their weight percentages shown in Table 11, and 0.3% by weight of [ka] The above was added to the liquid crystal composition shown in Table 11 to obtain Application Example 4, and the liquid crystal composition was filled between both substrates of a liquid crystal display to carry out a performance test.

[0145] [Table 11] [Application Example 5]

[0146] When 0.3% of the polymerizable compound RM-1-1 is added to the liquid crystal composition in Example 1, polymerization can be realized, and it has a fast angle formation speed and forms a small pretilt angle. [ka] [Application Example 6]

[0147] When 0.3% of the polymerizable compound RM-2-1 is added to the liquid crystal composition in Example 2, polymerization can be realized, and it has a fast angle formation speed and forms a small pretilt angle. [ka] [Application Example 7]

[0148] According to each compound and their weight percentage shown in Table 12, the liquid crystal composition of Application Example 7 is prepared, and the liquid crystal composition is filled between both substrates of a liquid crystal display to carry out a performance test.

[0149] [Table 12] [Application Example 8]

[0150] According to each compound and their weight percentage shown in Table 13, the liquid crystal composition of Application Example 8 is prepared, and the liquid crystal composition is filled between both substrates of a liquid crystal display to carry out a performance test.

[0151] [Table 13] [Application Example 9]

[0152] A liquid crystal composition was prepared according to the compounds and their weight percentages shown in Table 14, and 0.3% by weight [ka] The above was added to the liquid crystal composition shown in Table 14 to obtain Application Example 9, and the liquid crystal composition was filled between both substrates of a liquid crystal display to carry out a performance test.

[0153] [Table 14] [Application Example 10]

[0154] A liquid crystal composition was prepared according to the compounds and their weight percentages shown in Table 15, and 0.3% by weight [ka] The above was added to the liquid crystal composition shown in Table 15 to obtain Application Example 10, and the liquid crystal composition was filled between both substrates of a liquid crystal display to carry out a performance test.

[0155] [Table 15] [Application Example 11]

[0156] A liquid crystal composition was prepared according to the compounds and their weight percentages shown in Table 16, and 0.3% by weight of [ka] The above was added to the liquid crystal composition shown in Table 16 to obtain Application Example 11, and the liquid crystal composition was filled between both substrates of a liquid crystal display to carry out a performance test.

[0157] [Table 16] [Application Example 12]

[0158] A liquid crystal composition was prepared according to the compounds and their weight percentages shown in Table 17, and 0.3% by weight [ka] The above was added to the liquid crystal composition shown in Table 17 to obtain Application Example 12, and the liquid crystal composition was filled between both substrates of a liquid crystal display to carry out a performance test.

[0159] [Table 17] [Application Example 13]

[0160] A liquid crystal composition was prepared according to the compounds and their weight percentages shown in Table 18, and 0.3% by weight [ka] The above was added to the liquid crystal composition shown in Table 18 to obtain Application Example 13, and the liquid crystal composition was filled between both substrates of a liquid crystal display to carry out a performance test.

[0161] [Table 18]

[0162] From the above, the liquid crystal compound of general formula F of the present invention has a high clearing point, a large optical anisotropy and equal or greater absolute value of dielectric anisotropy while maintaining an appropriate rotational viscosity, and the liquid crystal composition of the present invention has large optical anisotropy, small rotational viscosity, high VHR(UV) and long low-temperature storage time while maintaining an appropriate clearing point, appropriate absolute value of dielectric anisotropy and appropriate VHR(initial), thereby allowing a liquid crystal display device including the liquid crystal composition to have high contrast, fast response speed, high reliability and high low-temperature storage stability.

[0163] The above embodiments are merely intended to explain the technical ideas and features of the present invention so that those skilled in the art can understand and practice the contents of the present invention, and are not intended to limit the protection scope of the present invention. Any equivalent modifications or modifications made based on the gist of the present invention should be included within the protection scope of the present invention. [Industrial Applicability]

[0164] The liquid crystal compound, the liquid crystal composition thereof, and the liquid crystal display device according to the present invention can be applied to the field of liquid crystals.

Claims

1. A liquid crystal compound represented by the general formula F. 【Chemistry 1】 (In the formula, R F1 is -H, a halogen, a linear or branched alkyl group containing 1 to 12 carbon atoms, 【Chemistry 2】 or 【Chemistry 3】 wherein the linear or branched alkyl group having 1 to 12 carbon atoms has one or more non-adjacent —CH 2 each - may be independently replaced by -C≡C-, -O-, -CO-, -CO-O- or -O-CO-; and one or more -H in the linear or branched alkyl group having 1 to 12 carbon atoms may be independently replaced by -F or -Cl; ring 【Chemistry 4】 And ring 【Chemistry 5】 are each independently 【Chemistry 6】 or 【Chemistry 7】 represents 【Chemistry 8】 and 【Chemistry 9】 At least one -CH 2 - may be replaced by -O-, and one or more single bonds in the ring may be replaced by a double bond; 【Chemistry 10】 and 【Chemistry 11】 one or more -H in the ring may be independently replaced by -CN, -F or -Cl, and one or more -CH= in the ring may be replaced by -N=; X F represents -O-, -S- or -CO-; L F1 and L F2 are each independently -H, -F, -Cl, or -CF 3 Or -OCF 3 represents Z F1 and Z F2 each independently represents a single bond, —CO—O—, —O—CO—, or —CH 2 O-, -OCH 2 -, -CH=CH-, -C≡C-, -CH 2 CH 2 -, -CF 2 CF 2 -, -(CH 2 ) 4 -, -CF 2 O- or -OCF 2 - represents n F1 and n F2 Each independently represents 0, 1 or 2; F1 If represents 2, the ring 【Chemistry 12】 may be the same or different, n F2 If represents 2, the ring 【Chemistry 13】 may be the same or different, Z F2 may be the same or different, and n F3 represents an integer from 0 to 4.)

2. The compound of the general formula F is 【Chemistry 14(1)】 【Chemistry 14(2)】 is selected from the group consisting of compounds During the ceremony, X F1 and X F2 are each independently -CH 2 The liquid crystal compound according to claim 1, characterized in that it represents - or -O-.

3. X F The liquid crystal compound according to claim 1, wherein represents -S-.

4. A liquid crystal composition comprising at least one liquid crystal compound of general formula F according to any one of claims 1 to 3.

5. The liquid crystal composition according to claim 4, further comprising at least one compound of general formula N. 【Chemistry 15】 (In the formula, R N1 and R N2 are each independently a linear or branched alkyl group containing 1 to 12 carbon atoms; 【Chemistry 16】 or 【Chemistry 17】 wherein the linear or branched alkyl group having 1 to 12 carbon atoms has one or more non-adjacent —CH 2 Each - may be independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -CO-O- or -O-CO-; ring 【Chemistry 18】 And ring 【Chemistry 19】 are each independently 【Chemistry 20】 or 【Chemistry 21】 represents 【Chemical 22】 At least one -CH 2 - may be replaced by -O-, and one or more single bonds in the ring may be replaced by a double bond; 【Chemistry 23】 one or more -H in the ring may be independently replaced by -F, -Cl or -CN, and one or more -CH= in the ring may be replaced by -N=; Z N1 and Z N2 each independently represents a single bond, —CO—O—, —O—CO—, or —CH 2 O-, -OCH 2 -, -CH=CH-, -C≡C-, -CH 2 CH 2 -, -CF 2 CF 2 -, -(CH 2 ) 4 -, -CF 2 O- or -OCF 2 - represents L N1 and L N2 each independently represents -H, an alkyl group having 1 to 3 carbon atoms, or a halogen; and n N1 represents 0, 1, 2 or 3; n N2 represents 0 or 1, and 0≦n N1 +n N2 ≦3, n N1 When = 2 or 3, the ring 【Chemistry 24】 may be the same or different, Z N1 may be the same or different.)

6. The compound of the general formula N is 【Chemistry 25(1)】 【Chemistry 25(2)】 【Chemistry 25(3)】 6. The liquid crystal composition according to claim 5, wherein the compound is selected from the group consisting of the compounds represented by the formula:

7. The liquid crystal composition according to claim 5, further comprising at least one compound represented by general formula M. 【Chemistry 26】 (In the formula, R M1 and R M2 are each independently a linear or branched alkyl group containing 1 to 12 carbon atoms; 【Chemistry 27】 or 【Chemistry 28】 wherein the linear or branched alkyl group having 1 to 12 carbon atoms has one or more non-adjacent —CH 2 Each - may be independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -CO-O- or -O-CO-; ring 【Chemical formula 29】 ,ring 【Chemistry 30】 And ring 【Chemistry 31】 are each independently 【Chemistry 32】 or 【Chemical 33】 represents 【Chemical 34】 At least one -CH 2 - may be replaced by -O-, and one or more single bonds in the ring may be replaced by a double bond; 【Chemistry 35】 at most one -H in may be replaced by halogen; Z M1 and Z M2 each independently represents a single bond, —CO—O—, —O—CO—, or —CH 2 O-, -OCH 2 -, -C≡C-, -CH=CH-, -CH 2 CH 2 - or - (CH 2 ) 4 - and n M represents 0, 1 or 2; n M If = 2, the ring 【Chemical 36】 may be the same or different, Z M2 may be the same or different.)

8. The compound of general formula M is 【Chemistry 37(1)】 【Chemistry 37(2)】 【Chemistry 37(3)】 8. The liquid crystal composition according to claim 7, wherein the compound is selected from the group consisting of the compounds represented by the formula:

9. 8. The liquid crystal composition according to claim 7, further comprising at least one polymerizable compound of general formula RM. 【Chemical 38】 (In the formula, R 1 is -H, halogen, -CN, -Sp 2 -P 2 or a linear or branched alkyl group containing 1 to 12 carbon atoms; 【Chemical Formula 39】 or 【Chemistry 40】 wherein said linear or branched alkyl group having 1 to 12 carbon atoms is 【Chemistry 41】 or 【Chemistry 42】 or two or more non-adjacent -CH 2 each - may be independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -CO-O- or -O-CO-; one or more -H may be independently replaced by -F or -Cl; ring 【Chemistry 43】 And ring 【Chemistry 44】 are each independently 【Chemistry 45】 or 【Chemistry 46】 represents 【Chemistry 47】 and 【Chemistry 48】 At least one -CH 2 - may be replaced by -O-, and one or more single bonds in the ring may be replaced by a double bond; 【Chemistry 49】 and 【Chemistry 50】 One or more -H in each group are independently -F, -Cl, -CN, -Sp 3 -P 3 , a halogenated or non-halogenated linear alkyl group containing 1 to 12 carbon atoms, a halogenated or non-halogenated linear alkoxy group containing 1 to 11 carbon atoms, 【Chemistry 51】 or 【Chemistry 52】 one or more -CH= in the ring may be replaced by -N=; ring 【Chemistry 53】 teeth, 【Chemical 54】 or 【Chemistry 55】 represents 【Chemistry 56】 or 【Chemistry 57】 One or more -H in each group are independently -F, -Cl, -CN, -Sp 3 -P 3 , a halogenated or non-halogenated linear alkyl group containing 1 to 12 carbon atoms, a halogenated or non-halogenated linear alkoxy group containing 1 to 11 carbon atoms, 【Chemistry 58】 or 【Chemical 59】 one or more -CH= in the ring may be replaced by -N=; P 1 , P 2 and P 3 each independently represents a polymerizable group, Sp 1 , Sp 2 and Sp 3 each independently represents a spacer group or a single bond, Z 1 and Z 2 each independently represents -O-, -S-, -CO-, -CO-O-, -O-CO-, -O-CO-O-, or -CH 2 O-, -OCH 2 --, --CH 2 S-, -SCH 2 -, -CF 2 O-, -OCF 2 -, -CF 2 S-, -SCF 2 -, -(CH 2 ) d -, -CF 2 CH 2 --, --CH 2 CF 2 -, - (CF 2 ) d -, -CH=CH-, -CF=CF-, -CH=CF-, -CF=CH-, -C≡C-, -CH=CH-CO-O-, -O-CO-CH=CH-, -CH 2 CH 2 -CO-O-, -O-CO-CH 2 CH 2 --, --CHR 1 -, -CR 1 R 2 - or a single bond; R 1 and R 2 each independently represents a linear or branched alkyl group containing 1 to 12 carbon atoms; d represents an integer of 1 to 4; X 0 is -O-, -S-, -CO-, -CF 2 represents -, -NH- or -NF-; a represents 0, 1 or 2; b represents 0 or 1; when a represents 2, the ring 【Chemistry 60】 may be the same or different, Z 1 may be the same or different.)

10. The liquid crystal composition according to claim 9, wherein the weight percentage of the compound of general formula F in the liquid crystal composition is 0.1% to 30%, the weight percentage of the compound of general formula N in the liquid crystal composition is 0.1% to 70%, the weight percentage of the compound of general formula M in the liquid crystal composition is 0.1% to 70%, and the weight percentage of the polymerizable compound of general formula RM in the liquid crystal composition is 0.001% to 5%.

11. The liquid crystal composition according to claim 4, further comprising at least one additive.

12. A liquid crystal display device comprising the liquid crystal composition according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Liquid crystal compound and composition thereof, and applications of composition

    CN107434973A

  • Liquid crystal medium

    JP2008189927A

  • Liquid crystal compound and liquid crystal medium

    JP2013112682A

  • Compound having fluorodibenzofuran ring, liquid crystal composition and liquid crystal display element

    JP2018150294A

  • Liquid-crystal medium

    JP2021109977A