Electrochemical and Electronic Devices

By using a tailored electrolyte composition with fluoroethylene carbonate and trinitrile compounds, along with specific metal elements in the positive electrode, the lithium-ion battery's high-temperature cycle and float charging characteristics are enhanced, addressing the temperature-related stability issues.

JP2024542588AActive Publication Date: 2024-11-15NINGDE AMPEREX TECHNOLOGY LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024531395
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-12-03
Publication Date
2024-11-15
Estimated Expiration
2041-12-03

AI Technical Summary

Technical Problem

Lithium-ion batteries face challenges with increased temperature rise during fast charging, leading to side reactions that affect their cycle characteristics and stability.

Method used

The electrochemical device incorporates a specific composition of fluoroethylene carbonate and a trinitrile compound in the electrolyte, with controlled mass ratios, along with a positive electrode containing metal elements like Ti, Mg, or Al, to enhance the structural stability and film formation, thereby improving high-temperature cycle and float charging characteristics.

Benefits of technology

The optimized electrolyte composition synergistically improves the lithium-ion battery's high-temperature cycle stability and float charging performance by adjusting the content of fluoroethylene carbonate, trinitrile compounds, and metal elements, resulting in better dynamic properties and extended battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542588000001
    Figure 2024542588000001
  • Figure 2024542588000002
    Figure 2024542588000002
  • Figure 2024542588000003
    Figure 2024542588000003
Patent Text Reader

Abstract

The present invention provides an electrochemical device and an electronic device, comprising a positive electrode, a negative electrode, a separator and an electrolyte, the electrolyte comprising fluoroethylene carbonate and a trinitrile compound, where, when the mass content of fluoroethylene carbonate is A%, relative to the mass of the electrolyte, A satisfies 4≦A≦10, and when the mass content of the trinitrile compound is B%, B satisfies 1≦B≦3, the positive electrode active material of the positive electrode comprises a metal element M, the metal element M comprising at least one of Ti, Mg and Al, and when the content of the metal element M in the positive electrode active material is C ppm, C and B satisfy 7≦C×B / 1000≦27. The present invention improves the float charge characteristics and cycle characteristics of the electrochemical device.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the electrochemical technology field, and in particular to electrochemical and electronic devices. [Background technology]

[0002] Lithium-ion batteries have the advantages of large specific energy, high operating voltage, low self-discharge rate, small volume, and light weight, and are widely used in various fields such as power storage, portable electronic devices, and electric vehicles. As the scope of use of lithium-ion batteries expands, higher requirements are placed on lithium-ion batteries. For example, lithium-ion batteries are required to have a faster charging speed and a longer service life.

[0003] However, as the charging speed of lithium ion batteries increases, the temperature also increases. At high temperatures, side reactions in lithium ion batteries increase, which affects the cycle characteristics of the lithium ion batteries. Summary of the Invention

[0004] The present invention provides an electrochemical device and an electronic device that can improve the cycle characteristics of the electrochemical device.

[0005] In a first aspect of the present invention, an electrochemical device is provided. The electrochemical device includes a positive electrode, a negative electrode, a separator, and an electrolyte, in which the electrolyte includes fluoroethylene carbonate and a trinitrile compound. When the mass content of fluoroethylene carbonate is A% relative to the mass of the electrolyte, A satisfies 4≦A≦10, and for example, A may be 4, 5, 6, 7, 8, 9, 10, or any range therebetween. When the mass content of the trinitrile compound is B%, B satisfies 1≦B≦3, and for example, B may be 1, 1.5, 2, 2.5, 3, or any range therebetween. The positive electrode includes a positive electrode active material, the positive electrode active material includes a metal element M, the metal element M includes at least one of Ti, Mg, and Al, and when the content of the metal element M in the positive electrode active material is C ppm, C and B satisfy 7≦C×B / 1000≦27, for example, C×B / 1000 may be 7, 10, 13, 15, 18, 20, 22, 25, 27, or any range therebetween. In the present invention, the positive electrode may be a positive electrode piece, and the negative electrode may be a negative electrode piece.

[0006] The inventors of the present invention have found that the high temperature cycle characteristics and float charge characteristics of a lithium ion battery can be improved by adjusting A, B and C×B / 1000 within the above ranges. Without being limited to any theory, it is believed that when the positive electrode active material contains a metal element M, the stability of the positive electrode structure can be improved. However, in order to improve the overall dynamic properties of a lithium ion battery, it is also necessary to improve the stability of the negative electrode structure. Based on this, the present invention improves the film formation stability of the negative electrode by adjusting the content of fluoroethylene carbonate in the electrolyte, and improves the high temperature cycle characteristics of a lithium ion battery by adjusting the content of trinitrile compound in the electrolyte, so that the lithium ion battery has good high temperature cycle characteristics and float charge characteristics.

[0007] In one embodiment of the present invention, A and B satisfy 6 ≤ A × B ≤ 22. For example, A × B may be 6, 8, 10, 12, 15, 17, 20, 22, or any range therebetween. By adjusting A × B within the above range, fluoroethylene carbonate and trinitrile compound act synergistically in the electrolyte, and the lithium ion battery has good high temperature cycle characteristics and float charging characteristics.

[0008] In one embodiment of the present invention, when the degree of the negative electrode defect is Id / Ig, Id / Ig satisfies 0.13 < Id / Ig ≤ 0.3. Id / Ig and A satisfy 6 ≤ A × (10 × Id / Ig) ≤ 24. For example, Id / Ig may be 0.13, 0.15, 0.2, 0.25, 0.3, or any range therebetween, and A × (10 × Id / Ig) may be 6, 8, 9, 10, 12, 15, 17, 29, 20, 22, 24, or any range therebetween. Without being limited to any theory, if A × (10 × Id / Ig) is too small (e.g., less than 6), the kinetic characteristics on the negative electrode side are not sufficient, side reactions increase, and the cycle stability of the lithium ion battery deteriorates. If A × (10 × Id / Ig) is too large (e.g., greater than 24), it affects the high temperature stability of the lithium ion battery. By adjusting A × (10 × Id / Ig) within the above range, a lithium ion battery having good high temperature cycle characteristics and float charging characteristics can be obtained.

[0009] In the present invention, in the degree of the negative electrode defect Id / Ig, Id is the intensity of the D peak in the Raman spectrum of the negative electrode active material, Ig is the intensity of the G peak in the Raman spectrum of the negative electrode active material, Id / Ig indicates the defect concentration of the negative electrode active material, and the larger the value of Id / Ig, the greater the degree of the defect.

[0010] In one embodiment of the present invention, the content C of metal element M in the positive electrode active material satisfies 5000ppm≦C≦9000ppm. For example, C may be 5000ppm, 5500ppm, 6000ppm, 6500ppm, 7000ppm, 7500ppm, 8000ppm, 8500ppm, 9000ppm, or any range therebetween. Without being limited by any theory, by adjusting C within the above range, a lithium ion battery with good high temperature cycle characteristics and energy density can be obtained.

[0011] In one embodiment of the present invention, C and Id / Ig satisfy 6≦C / (3000×Id / Ig)≦20. For example, C / (3000×Id / Ig) may be 6, 7, 10, 12, 15, 18, 20, or any range therebetween. Without being limited to any theory, by adjusting C / (3000×Id / Ig) within the above range, a lithium ion battery with good high temperature cycle characteristics and float charge characteristics can be obtained.

[0012] In one embodiment of the present invention, the electrolyte further comprises ethylene carbonate and propylene carbonate, and when the mass content of ethylene carbonate is D% and the mass content of propylene carbonate is E% relative to the mass of the electrolyte, D and E satisfy 20≦D+E≦50 and 1≦E / D≦3. For example, D+E may be 20, 25, 30, 35, 40, 45, 50 or any range therebetween, and E / D may be 1, 1.5, 2, 2.5, 3 or any range therebetween. Without being limited by any theory, by simultaneously adjusting D+E and E / D within the above ranges, the high temperature cycle characteristics and float charge characteristics of the lithium ion battery can be further improved.

[0013] In one embodiment of the present invention, the electrolyte further comprises a dinitrile compound, and when the mass content of the dinitrile compound is F% with respect to the mass of the electrolyte, F satisfies 1≦F≦3. For example, F may be 1, 1.5, 2, 2.5, 3, or any range therebetween. Without being limited to any theory, if the content of the dinitrile compound is too low (e.g., less than 1%), the protective effect on the positive electrode is not significant. If the content of the dinitrile compound is too high (e.g., greater than 3%), it will affect the viscosity of the electrolyte and increase the internal resistance of the lithium ion battery. By adjusting the content of the dinitrile compound within the above range, the high temperature cycle characteristic and float charge characteristic of the lithium ion battery can be further improved.

[0014] In one embodiment of the present invention, F and B satisfy 2≦F+B≦6. For example, F+B can be 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, or any range therebetween. Without being limited to any theory, by adjusting F+B within the above range, the high temperature cycle characteristics and float charge characteristics of the lithium ion battery can be further improved.

[0015] In one embodiment of the present invention, the electrolyte further comprises at least one of 1,3-propane sultone, ethylene sulfate, vinylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and γ-butyrolactone. The electrochemical device satisfies at least one of the following characteristics (a) to (g): a) a mass content of the 1,3-propane sultone is 0.5% to 5% with respect to the mass of the electrolytic solution; b) a mass content of the ethylene sulfate is 0.1% to 1% with respect to the mass of the electrolytic solution; c) a mass content of the vinylene carbonate is 0.1% to 1% with respect to the mass of the electrolytic solution; d) a mass content of the dimethyl carbonate is 0.1% to 30% with respect to the mass of the electrolytic solution; e) a mass content of the diethyl carbonate is 0.1% to 30% with respect to the mass of the electrolytic solution; f) a mass content of the ethyl methyl carbonate is 0.1% to 30% with respect to the mass of the electrolytic solution; and g) a mass content of the γ-butyrolactone is 0.01% to 5% with respect to the mass of the electrolytic solution. Without being limited to any theory, it is believed that by adjusting the additives of the electrolyte to fall within the range of the present invention, the high temperature cycle characteristics and float charge characteristics of the lithium ion battery can be further improved.

[0016] The present invention is not particularly limited to the trinitrile compound, and it is sufficient if the object of the present invention can be achieved. For example, the trinitrile compound includes at least one of 1,3,5-pentanetricarbonitrile, 1,2,3-propanetricarbonitrile, 1,3,6-hexanetricarbonitrile, 1,2,6-hexanetricarbonitrile, 1,2,3-tris(2-cyanoethoxy)propane, 1,2,4-tris(2-cyanoethoxy)butane, and 1,2,5-tris(cyanoethoxy)pentane.

[0017] The electrolyte solution according to the present invention contains a lithium salt, and the lithium salt is not particularly limited in the present invention, as long as it can achieve the object of the present invention. For example, the lithium salt contains at least one of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium bis(oxalato)borate, lithium difluoro(oxalato)borate, and lithium difluorophosphate.

[0018] The present invention is not particularly limited to the dinitrile compound, and it is sufficient if the object of the present invention can be achieved. For example, the dinitrile compound includes at least one of succinonitrile, glutaronitrile, adiponitrile, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 1,8-dicyanooctane, 1,9-dicyanononane, 1,10-dicyanodecane, 1,12-dicyanododecane, tetramethylsuccinonitrile, 2-methylglutaronitrile, 2,4-dimethylglutaronitrile, and 2,2,4,4-tetramethylglutaronitrile.

[0019] In a second aspect of the present invention, there is provided an electronic device, comprising the electrochemical device according to any of the above embodiments of the present invention.

[0020] The present invention provides an electrochemical device and an electronic device, in which an electrolyte in the electrochemical device comprises fluoroethylene carbonate and a trinitrile compound, in which, when the mass content of the fluoroethylene carbonate is A%, A satisfies 4≦A≦10, and when the mass content of the trinitrile compound is B%, B satisfies 1≦B≦3, and the mass content C% of a metal element M in a positive electrode active material and the mass content B% of the trinitrile compound are adjusted to satisfy 7≦C×B / 1000≦27, thereby improving the float charge characteristics and cycle characteristics of the electrochemical device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] In order to make the objectives, technical solutions and advantages of the present invention clearer, the present invention will be described in more detail below with reference to the embodiments. Obviously, the described embodiments are only some of the embodiments of the present invention, and are not all of the embodiments. Based on the embodiments in the present invention, all other technical solutions obtained by those skilled in the art belong to the scope of protection of the present invention.

[0022] In the embodiments of the present invention, the present invention will be described using a lithium ion battery as an example of an electrochemical device, but the electrochemical device of the present invention is not limited to a lithium ion battery.

[0023] The present invention is not particularly limited to the preparation method of the positive electrode active material containing the metal element M (hereinafter simply referred to as modified positive electrode active material), and a preparation method well known to those skilled in the art may be used. For example, the modified positive electrode active material can be obtained by adding an aluminum-containing compound (e.g., Al2O3, Al(OH)3, AlF3), a magnesium-containing compound (e.g., MgO) or a Ti-containing compound (e.g., TiO2) to the positive electrode active material LiCoO2. Note that the present invention can realize the change of the metal element M in the positive electrode active material layer by adjusting the content of the metal element M in the modified positive electrode active material, for example, by adjusting the amount of the compound containing the metal element M added. The present invention is not specifically limited to the preparation process, and it is sufficient to achieve the object of the present invention.

[0024] The positive electrode current collector in the present invention is not particularly limited and may be any positive electrode current collector in the relevant field, for example, aluminum foil, aluminum alloy foil, or composite current collector.

[0025] The negative electrode current collector in the present invention is not particularly limited and may be a material such as a metal foil material or a porous metal plate, for example, a foil material or a porous plate of a metal such as copper, nickel, titanium, or iron, or an alloy thereof, for example, a copper foil. The negative electrode active material layer includes a negative electrode active material, a conductive agent, a binder, and a thickener. The binder may be at least one of styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), water-based acrylic resin, and carboxymethyl cellulose (CMC), and the thickener may be carboxymethyl cellulose (CMC), etc.

[0026] The substrate of the separator of the present invention includes at least one selected from polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyimide (PI), and aramid, but is not limited thereto. For example, polyethylene includes at least one component selected from high density polyethylene, low density polyethylene, and ultra-high molecular weight polyethylene. In particular, polyethylene and polypropylene have excellent effects on preventing short circuits, and can improve the stability of electrochemical devices due to their shutdown effect. The substrate may be a single layer structure or a multi-layer composite structure in which multiple types are mixed, and has a thickness of 3 μm to 20 μm.

[0027] The electronic device of the present invention is not particularly limited and may be any electronic device used in the prior art. In some embodiments, the electronic device may include, but is not limited to, a notebook computer, a pen-input computer, a mobile computer, an electronic book player, a mobile phone, a mobile fax machine, a portable copy machine, a mobile printer, a head-mounted stereo headphone, a video recorder, a liquid crystal television, a mobile cleaner, a mobile CD player, a mini disk, a transceiver, an electronic organizer, a calculator, a memory card, a mobile recorder, a radio, a backup power source, a motor, an automobile, a motorcycle, an electric-assisted bicycle, a bicycle, a lighting device, a toy, a game machine, a clock, an electric tool, a flashlight, a camera, a large-scale household battery, a lithium-ion capacitor, and the like.

[0028] The manufacturing process of the electrochemical device is well known to those skilled in the art, and the present invention is not particularly limited. For example, a lithium ion battery is manufactured by stacking a positive electrode and a negative electrode with a separator therebetween, and then winding or folding the stack as necessary, placing the stack in a case, injecting an electrolyte into the case, and sealing the case. In addition, if necessary, an overcurrent protection element, a lead plate, or the like may be placed in the case to prevent pressure rise inside the lithium ion battery and overcharging and discharging.

[0029] Hereinafter, the embodiments of the present invention will be described in more detail with reference to examples and comparative examples. Various tests and evaluations are carried out according to the following methods. In addition, "parts" and "%" are based on mass unless otherwise specified.

[0030] Measurement methods and equipment Measurement of the content of metal element M in the positive electrode active material The active material of the positive electrode piece washed with DMC (dimethyl carbonate) was taken with a doctor blade and dissolved in a mixed solvent (for example, a mixed solvent of 10 ml of aqua regia (a 1:1 mixture of nitric acid and hydrochloric acid) and 2 ml of HF was used for 0.4 g of the positive electrode active material), and the volume was adjusted to 100 mL. The content of metal elements M such as Ti, Mg, and Al in the solution was measured using an ICP analyzer, and the unit was ppm.

[0031] Measuring the degree of defects in negative electrodes The dried negative electrode piece was placed on the sample stage of a Raman measuring device (JobinYvonLabRAM HR) so as to maintain the surface flat, and a Raman spectrum was obtained. The D peak intensity and G peak intensity were obtained from the Raman spectrum, and Id / Ig was calculated to determine the degree of defects in the negative electrode.

[0032] Measurement of cycle characteristics of lithium-ion batteries At 45°C, the lithium-ion battery was charged at a constant current of 0.7C (rate) up to 4.5V, then charged at a constant voltage until the current reached 0.05C, and then discharged at a constant current of 1C up to 3.0V, which constituted one charge-discharge cycle, and this was the first cycle, and the discharge capacity of the first cycle of the lithium-ion battery was recorded. The lithium-ion battery was subjected to charge-discharge cycles according to the above method, and the discharge capacity of each cycle was recorded. When the discharge capacity of the lithium-ion battery had decayed to 80% of the discharge capacity of the first cycle, the cycle was stopped, and the number of charge-discharge cycles was recorded.

[0033] Measurement of charging characteristics of lithium-ion battery float At 45°C, the lithium-ion battery was charged at a constant current of 0.7C up to 4.5V, and then charged at a constant voltage for 90 days. The thickness of the lithium-ion battery was measured and recorded with a micrometer, and the thickness of the lithium-ion battery was measured and recorded every three days during the period. The thickness expansion rate of the lithium-ion battery during float charging was calculated according to the following formula, and the time it took for the thickness expansion rate to reach 10% was used as an index to evaluate the superiority or inferiority of the float charging characteristics of the lithium-ion battery. The longer the time it takes for the thickness expansion rate to reach 10%, the better the float charging characteristics of the lithium-ion battery.

[0034] The thickness expansion rate of a lithium-ion battery = (thickness of a lithium-ion battery during float charging process - initial thickness of a lithium-ion battery) / initial thickness of a lithium-ion battery × 100%.

[0035] Example 1 <Preparation of modified positive electrode active material> Commercially available lithium cobalt oxide (LiCoO2) was mixed with an oxide containing a metal element M (a mixture of magnesium oxide (MgO), titanium dioxide (TiO2), and aluminum oxide (Al2O3)) and mixed in a high-speed mixer at 300 r / min for 20 min. The mixture was then placed in an air furnace, heated to 820°C at 5°C / min, held for 24 h, naturally cooled, removed, and sieved through a 300 mesh sieve to obtain a modified positive electrode active material (i.e., modified LiCoO2). In the modified positive electrode active material, the total content of the metal element M (Mg, Ti, Al) in the positive electrode active material was 7000 ppm, and the molar ratio of Mg, Ti, and Al was 1:1:1.

[0036] <Production of positive electrode sheet> The prepared modified LiCoO2, carbon nanotubes (CNT) as a conductive agent, and polyvinylidene fluoride as a binder were mixed in a mass ratio of 95:2:3, N-methylpyrrolidone (NMP) was added as a solvent, and the mixture was stirred with a vacuum stirrer until the system was homogeneous and a positive electrode slurry with a solid content of 75 wt% was obtained. The positive electrode slurry was uniformly applied to a positive electrode current collector aluminum foil with a thickness of 12 μm, dried under a condition of 85 ° C, and a positive electrode piece with a positive electrode active material layer thickness of 100 μm was obtained after cold pressing. Then, the above operation was repeated for the other surface of the corresponding positive electrode piece, and a positive electrode piece with a positive electrode active material layer applied on both sides was obtained. The positive electrode piece was cut into a size of 74 mm × 867 mm, and a tab was welded and left to stand by.

[0037] <Preparation of negative electrode piece> The negative electrode active materials, artificial graphite, styrene butadiene rubber (SBR) and carboxymethyl cellulose (CMC), were mixed in a mass ratio of 95:2:3, and deionized water was added as a solvent to prepare a slurry with a solid content of 70 wt%, which was then uniformly stirred. The slurry was uniformly applied to one surface of a copper foil with a thickness of 8 μm, dried at 110° C., and cold pressed to obtain a negative electrode piece with a negative electrode active material layer applied to one surface, the negative electrode active material layer having a thickness of 150 μm. The above operation was then repeated for the other surface of the negative electrode piece to obtain a negative electrode piece with a negative electrode active material layer applied to both surfaces. The negative electrode piece was cut to a size of 74 mm×867 mm, and the tab was welded and left to stand. The defect degree Id / Ig of the negative electrode piece was 0.17.

[0038] <Preparation of electrolyte> In a glove box with an argon gas atmosphere with a water content of less than 10 ppm, ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) were mixed uniformly in a weight ratio of 1:1:1 to form a base solvent. LiPF6, 1,3,6-hexanetricarbonitrile, a trinitrile compound, and fluoroethylene carbonate were added and stirred uniformly to form an electrolyte. The concentration of LiPF6 was 12.5 wt%, and the mass contents of 1,3,6-hexanetricarbonitrile, a trinitrile compound, and fluoroethylene carbonate are shown in Table 1.

[0039] <Preparation of separator> A polyethylene (PE) porous polymer film having a thickness of 15 μm was used as the separator.

[0040] <Lithium-ion battery manufacturing> The positive electrode, separator, and negative electrode are stacked in order, and the separator is placed between the positive and negative electrodes to serve as an insulator, and then wound to obtain an electrode assembly. The electrode assembly is placed in an aluminum plastic film packaging bag, and the moisture is removed at 80°C. The prepared electrolyte is injected, and the lithium ion battery is obtained through processes such as vacuum packaging, standing, formation, and shaping.

[0041] Example 2 to Example 12 The content of fluoroethylene carbonate in the electrolyte, the type and content of trinitrile compound, and the total content of metal element M were adjusted, and the corresponding preparation parameters and property changes were as shown in Table 1. Otherwise, the same as in Example 1.

[0042] Example 13 In <Preparation of modified positive electrode active material>, the oxide containing metal element M was a mixture of MgO and Al2O3, and the molar ratio of Mg element to Al element was 1:1. The correlated preparation parameters and characteristic changes were as shown in Table 1. The rest was the same as in Example 10.

[0043] Example 14 In <Preparation of modified positive electrode active material>, the oxide containing metal element M was Al2O3, and the correlated preparation parameters and characteristic changes were as shown in Table 1. The rest was the same as in Example 10.

[0044] Examples 15 to 17 As shown in Table 2, the content of fluoroethylene carbonate in the electrolyte and the degree of defects Id / Ig in the negative electrode pieces were adjusted, and the rest was the same as in Example 1.

[0045] Example 18 <Preparation of electrolyte solution> was different from that in Example 1, but the rest was the same as in Example 1. In a glove box with an argon gas atmosphere with a water content of less than 10 ppm, ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) were mixed uniformly in a weight ratio of 10:15:54.5 to form a base solvent. LiPF6, 1,3,6-hexanetricarbonitrile, a trinitrile compound, and fluoroethylene carbonate were added and stirred uniformly to form an electrolyte. Among them, the concentration of LiPF6 was 12.5 wt%, and the mass contents of 1,3,6-hexanetricarbonitrile, a trinitrile compound, and fluoroethylene carbonate, as well as the correlation preparation parameters and property changes are shown in Table 3.

[0046] Example 19 <Preparation of electrolyte solution> was different from that in Example 1, but the rest was the same as in Example 1. In a glove box with an argon gas atmosphere with a water content of less than 10 ppm, ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) were mixed uniformly in a weight ratio of 10:15:39.5 to form a base solvent. LiPF6, 1,3,6-hexanetricarbonitrile, a trinitrile compound, and fluoroethylene carbonate were added and stirred uniformly to form an electrolyte. Among them, the concentration of LiPF6 was 12.5 wt%, and the mass contents of 1,3,6-hexanetricarbonitrile, a trinitrile compound, and fluoroethylene carbonate, as well as the correlation preparation parameters and property changes are shown in Table 3.

[0047] Example 20 <Preparation of electrolyte solution> was different from that in Example 1, but the rest was the same as in Example 1. In a glove box with an argon gas atmosphere with a water content of less than 10 ppm, ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) were mixed uniformly in a weight ratio of 10:15:34.5 to form a base solvent. LiPF6, 1,3,6-hexanetricarbonitrile, a trinitrile compound, and fluoroethylene carbonate were added and stirred uniformly to form an electrolyte. Among them, the concentration of LiPF6 was 12.5 wt%, and the mass contents of 1,3,6-hexanetricarbonitrile, a trinitrile compound, and fluoroethylene carbonate, as well as the correlation preparation parameters and property changes are shown in Table 3.

[0048] Example 21 <Preparation of electrolyte solution> was different from that in Example 2, but the rest was the same as in Example 2. <Preparation of electrolyte> In a glove box with an argon gas atmosphere with a water content of less than 10 ppm, ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) were mixed uniformly in a weight ratio of 1:1:1 to form a base solvent. LiPF6, 1,3,6-hexanetricarbonitrile, a trinitrile compound, fluoroethylene carbonate, and succinonitrile, a dinitrile compound, were added and stirred uniformly to form an electrolyte. Among them, the concentration of LiPF6 was 12.5 wt%, and the mass contents of 1,3,6-hexanetricarbonitrile, a trinitrile compound, fluoroethylene carbonate, and succinonitrile, a dinitrile compound, the correlation preparation parameters, and property changes are shown in Table 4.

[0049] Examples 22 to 27 In <Preparation of Electrolyte Solution>, the type and content of the dinitrile compound were adjusted as shown in Table 4, and the rest was the same as in Example 21.

[0050] Example 28 <Preparation of electrolyte solution> was different from that in Example 2, but the rest was the same as in Example 2. <Preparation of electrolyte> In a glove box with an argon gas atmosphere with a water content of less than 10 ppm, ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) were mixed uniformly in a weight ratio of 1:1:1 to form a base solvent. LiPF6, 1,3,6-hexanetricarbonitrile, a trinitrile compound, fluoroethylene carbonate, and 1,3-propane sultone, an additive, were added and stirred uniformly to form an electrolyte. The concentration of LiPF6 was 12.5 wt%, and the mass contents of 1,3,6-hexanetricarbonitrile, a trinitrile compound, fluoroethylene carbonate, and 1,3-propane sultone, an additive, the correlation preparation parameters, and the changes in properties are shown in Table 5.

[0051] Example 29 to Example 30 In <Preparation of Electrolyte Solution>, the types and contents of additives were adjusted as shown in Table 5, and the rest was the same as in Example 28.

[0052] Comparative Examples 1 to 6 The type of trinitrile compound in the electrolyte, the content of fluoroethylene carbonate, the content of trinitrile compound, and the total content of metal element M were adjusted, and the correlation preparation parameters and property changes were as shown in Table 1, and the rest were the same as in Example 1.

[0053] Comparative Example 7 As shown in Table 2, the content of fluoroethylene carbonate in the electrolyte and the degree of defects Id / Ig in the negative electrode pieces were adjusted, and the rest was the same as in Example 1.

[0054] [Table 1]

[0055] [Table 2]

[0056] [Table 3]

[0057] [Table 4] In Table 4, " / " indicates not included or not measurable.

[0058] [Table 5] In Table 5, " / " indicates not included or not measurable.

[0059] As can be seen from Examples 1 to 7 and Comparative Examples 1 to 4 in Table 1, by adjusting A, B, and C×B / 1000 within the ranges of the present invention, the capacity retention rate and float charge characteristics of the lithium ion battery at 45° C. are clearly improved. This shows that the lithium ion battery of the present invention has good high-temperature cycle characteristics and float charge characteristics.

[0060] As can be further seen from Examples 1 to 14 in Table 1, by adjusting A×B while keeping A, B, and C×B / 1000 within the ranges of the present invention, the fluoroethylene carbonate and trinitrile compound in the electrolyte act synergistically, and a lithium ion battery having good high-temperature cycle characteristics and float charge characteristics can be obtained.

[0061] As can be seen from Example 8, Example 9, and Comparative Example 6 in Table 1, when the content of metal element M is too low (for example, Comparative Example 6), the capacity retention rate and float charge characteristics of the lithium ion battery at 45° C. are clearly reduced. As can be seen from Example 9 and Comparative Example 5 in Table 1, when the content of metal element M is too high (for example, Comparative Example 5), the improvement in the float charge characteristics of the lithium ion battery is not clear, but the capacity retention rate at 45° C. is conversely significantly reduced. As can be seen from this, by setting A, B, and C×B / 1000 within the ranges of the present invention and adjusting the content of metal element M within the ranges of the present invention, a lithium ion battery having good high-temperature cycle characteristics and float charge characteristics can be obtained.

[0062] As can be seen from Examples 9 and 10 in Table 1, by increasing the content of the trinitrile compound while keeping A, B, and C×B / 1000 within the ranges of the present invention, the float charge characteristics of the lithium ion battery can be further improved.

[0063] As can be seen from Examples 2, 11, and 12 in Table 1, as long as A, B, and C×B / 1000 are within the ranges of the present invention and the type of trinitrile compound is within the ranges of the present invention, a lithium ion battery having good high-temperature cycle characteristics and float charge characteristics can be obtained.

[0064] As can be seen from Examples 10, 13, and 14 in Table 1, as long as A, B, and C×B / 1000 are within the ranges of the present invention and the type of metal element M is within the range of the present invention, a lithium ion battery having good high-temperature cycle characteristics and float charge characteristics can be obtained.

[0065] As can be seen from Examples 15 to 17 and Comparative Example 7 in Table 2, by setting A, B, and C×B / 1000 within the ranges of the present invention and then adjusting A×(10×Id / Ig) within the ranges of the present invention, a lithium ion battery having good high-temperature cycle characteristics and float charge characteristics can be obtained.

[0066] As can be seen from Examples 1 to 17 in Table 3, by setting A, B, and C×B / 1000 within the ranges of the present invention and then adjusting C / (3000×Id / Ig) within the ranges of the present invention, a lithium ion battery having good high-temperature cycle characteristics and float charge characteristics can be obtained.

[0067] As can be seen from Example 8 and Examples 18 to 20 in Table 3, by adjusting the contents of ethylene carbonate and propylene carbonate in the electrolyte while keeping A, B, and C×B / 1000 within the ranges of the present invention, the high-temperature cycle characteristics and float charge characteristics of the lithium-ion battery can be further improved.

[0068] As can be seen from Example 2 and Example 21 to Example 26 in Table 4, when A, B, and C×B / 1000 are within the ranges of the present invention, the electrolyte further contains a dinitrile compound, and the total content of the dinitrile compound and the trinitrile compound is within the ranges of the present invention, the high temperature cycle characteristics and float charge characteristics of the lithium ion battery can be further improved.

[0069] As can be seen from Example 2 and Examples 28 to 30 in Table 5, when A, B, and C×B / 1000 are within the ranges of the present invention and the electrolyte contains at least one additive selected from the group consisting of 1,3-propane sultone, ethylene sulfate, vinylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and γ-butyrolactone, the high temperature cycle characteristics and float charge characteristics of the lithium ion battery can be further improved.

[0070] The above description is only a preferred embodiment of the present invention, and does not limit the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.

Claims

1. 1. An electrochemical device comprising: The battery includes a positive electrode, a negative electrode, a separator, and an electrolyte solution. The electrolyte includes fluoroethylene carbonate and a trinitrile compound, When the mass content of the fluoroethylene carbonate is A% with respect to the mass of the electrolytic solution, A satisfies 4≦A≦10; When the mass content of the trinitrile compound is B% with respect to the mass of the electrolytic solution, B satisfies 1≦B≦3; The positive electrode includes a positive electrode active material, The positive electrode active material contains a metal element M, The metal element M includes at least one of Ti, Mg, and Al, When the content of the metal element M in the positive electrode active material is C ppm, C and B satisfy 7≦C×B / 1000≦27. Electrochemical equipment.

2. 2. The electrochemical device according to claim 1, wherein A and B satisfy 6≦A×B≦22.

3. 2. The electrochemical device according to claim 1, wherein when the degree of defects in the negative electrode is Id / Ig, A and Id / Ig satisfy 0.13<Id / Ig≦0.3 and 6≦A×(10×Id / Ig)≦24.

4. The electrochemical device according to claim 3 , wherein a content C of the metal element M in the positive electrode active material satisfies 5000 ppm≦C≦9000 ppm.

5. 5. The electrochemical device according to claim 4, wherein C and Id / Ig satisfy 6≦C / (3000×Id / Ig)≦20.

6. The electrolyte further comprises ethylene carbonate and propylene carbonate; 2. The electrochemical device according to claim 1, wherein, when a mass content of the ethylene carbonate is D % and a mass content of the propylene carbonate is E % relative to the mass of the electrolytic solution, D and E satisfy 20≦D+E≦50 and 1≦E / D≦3.

7. The electrolyte further comprises a dinitrile compound; 2. The electrochemical device according to claim 1, wherein when a mass content of the dinitrile compound is F % with respect to a mass of the electrolyte solution, F satisfies 1≦F≦3.

8. The electrochemical device according to claim 7 , wherein F and B satisfy 2≦F+B≦6.

9. 10. The electrochemical device of claim 1, wherein the electrolyte further comprises at least one of 1,3-propane sultone, ethylene sulfate, vinylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and gamma-butyrolactone.

10. The electrochemical device satisfies at least one of the following characteristics (a) to (g): a) the mass content of the 1,3-propane sultone is 0.5% to 5% relative to the mass of the electrolyte; b) the mass content of the ethylene sulfate is 0.1% to 1% relative to the mass of the electrolyte; c) the mass content of the vinylene carbonate is 0.1% to 1% relative to the mass of the electrolyte; d) the mass content of the dimethyl carbonate is 0.1% to 30% relative to the mass of the electrolyte; e) the mass content of the diethyl carbonate is 0.1% to 30% relative to the mass of the electrolyte; f) the mass content of the ethyl methyl carbonate is 0.1% to 30% relative to the mass of the electrolyte; g) the mass content of the gamma-butyrolactone is 0.01% to 5% relative to the mass of the electrolyte; 10. The electrochemical device of claim 9.

11. The electrochemical device of claim 1, wherein the trinitrile compound comprises at least one of 1,3,5-pentanetricarbonitrile, 1,2,3-propanetricarbonitrile, 1,3,6-hexanetricarbonitrile, 1,2,6-hexanetricarbonitrile, 1,2,3-tris(2-cyanoethoxy)propane, 1,2,4-tris(2-cyanoethoxy)butane, and 1,2,5-tris(cyanoethoxy)pentane.

12. the electrolyte solution contains a lithium salt; 2. The electrochemical device of claim 1, wherein the lithium salt comprises at least one of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium bis(oxalato)borate, lithium difluoro(oxalato)borate, and lithium difluorophosphate.

13. The dinitrile compound includes at least one of succinonitrile, glutaronitrile, adiponitrile, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 1,8-dicyanoctane, 1,9-dicyanononane, 1,10-dicyanodecane, 1,12-dicyanododecane, tetramethylsuccinonitrile, 2-methylglutaronitrile, 2,4-dimethylglutaronitrile, and 2,2,4,4-tetramethylglutaronitrile. The electrochemical device of claim 7.

14. An electronic device comprising an electrochemical device according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • High-voltage lithium cobaltate / graphite battery and preparation method thereof

    CN110797530A

  • Positive electrode active material, and electrochemical device and electronic device using same

    CN113078309A

  • Lithium secondary battery

    JP2024537150A

  • Negative electrode active material, and electrochemical apparatus and electronic apparatus using said material