Anode materials, batteries

The development of a negative electrode material with controlled pore volume and surface area through a continuous graphitization process addresses the limitations of conventional graphite, enhancing lithium ion diffusion and improving high-rate charging and discharging performance.

JP2024543292AActive Publication Date: 2024-11-21KAIFENG RUIFENG NEW MATERIAL CO LTD +1

Patent Information

Application Number
JP2024508469
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2022-11-16
Publication Date
2024-11-21
Estimated Expiration
2042-11-16

AI Technical Summary

Technical Problem

Conventional graphite negative electrode materials for lithium ion batteries face challenges in achieving optimal rate characteristics due to insufficient pore structure and lack of synergistic effects among multiple elements, leading to poor high-rate charging and discharging performance.

Method used

A negative electrode material with controlled pore volume, specific surface area, and oil absorption, produced through a continuous graphitization process, incorporating additives to form pores inside and on the surface of artificial graphite, ensuring sufficient electrochemical reaction space and improved lithium ion diffusion.

Benefits of technology

The material achieves enhanced high-rate charge/discharge performance by providing sufficient reaction interfaces and reducing concentration polarization, with reduced energy consumption and production costs, while maintaining environmental friendliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543292000001_ABST
    Figure 2024543292000001_ABST
Patent Text Reader

Abstract

The present application provides a negative electrode material and a battery. [Solution] The negative electrode material includes artificial graphite, and the artificial graphite has pores inside and / or on its surface. The negative electrode material has an oil absorption of 0 mL / 100 g and a pore volume of V cm 3 / kg, specific surface area is Sm 2 / g, 400≦O×V×S≦1500. The negative electrode material provided by the present application can improve the adsorption and infiltration ability of the negative electrode material for the electrolyte without affecting the processing performance, and can improve the high-rate charge / discharge performance of the negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the technical field of anode materials, specifically to anode materials, batteries. [Background technology]

[0002] Graphite has the advantages of high electrical conductivity, a large lithium ion diffusion coefficient, a small volume change before and after lithium absorption in its layered structure, a high lithium absorption capacity, and a low lithium absorption potential, making it the currently mainstream negative electrode material for commercial lithium ion batteries.

[0003] Conventional graphitization equipment for graphite anodes is mainly of two types: crucible furnace and box furnace. Both of them are batch-type operations, and the graphitization process requires power outages, making it impossible to realize continuous production. In addition, the heating and cooling processes of the equipment are limited, and the heating and cooling speed is slow, resulting in a long production cycle. Generally, the graphitization cycle is within 15 to 50 days. In the graphitization production process, volatile components and impurity elements in the raw materials are released under high temperature conditions, so pores are formed inside and / or on the surface of the graphite. Generally, artificial graphite has a certain number of pore structures, and the presence of pores is the cause of the Li + This increases the diffusion channels inside the graphite material, allowing Li + On the other hand, too many pores will increase the specific surface area of ​​the material, which will further deteriorate the initial efficiency and cycle performance of the product. In fact, simply improving the pore structure will not allow the rate performance to reach the optimum, and there is still a lot of room for improvement. Researchers have only studied the effect of a single factor on the performance of graphite materials, and have not studied in depth the synergistic effects between multiple factors to maximize the improvement of the rate performance of graphite.

[0004] Therefore, at the current mature stage of graphite material development, improving a single parameter cannot meet the market demand for low-cost, high-performance graphite materials. It is necessary to study the synergistic action mechanism of various factors and develop graphite anode materials that meet the market demand. Summary of the Invention [Problem to be solved by the invention]

[0005] In view of this, the present application provides a negative electrode material and a battery, which can improve active sites and diffusion channels for storing and releasing lithium ions in the negative electrode material, and can improve the high-rate charge-discharge performance of the negative electrode material. [Means for solving the problem]

[0006] In a first aspect, the present application provides a negative electrode material, the negative electrode material comprising artificial graphite, the artificial graphite having an internal and / or surface pore structure, the negative electrode material having an oil absorption of 0 mL / 100 g and a pore volume of V cm 3 / kg, specific surface area is Sm 2 / g, 400≦O×V×S≦1500, The pore volume was measured using an ASAP2460 device (Micromeritics, USA) and calculated within the pore diameter range of 17 Å to 3000 Å using the BJH Desorption cumulative volume of pores model.

[0007] In some embodiments, the negative electrode material has an oil absorption of O mL / 100 g, where 43≦O≦60.

[0008] In some embodiments, the negative electrode material has a pore volume of Vcm 3 / kg, V is 5≦V≦8.

[0009] In some embodiments, the negative electrode material has a specific surface area of ​​Sm 2 / g, 1.78≦S≦3.0.

[0010] In some embodiments, the negative electrode material has a particle size that satisfies 0.9≦(D90−D10) / D50≦1.8 and 10 μm≦D50≦30 μm.

[0011] In some embodiments, the negative electrode material further comprises amorphous carbon.

[0012] In some embodiments, the negative electrode material further includes amorphous carbon, and the mass percentage of the amorphous carbon in the negative electrode material is 0.1 wt % to 5 wt %.

[0013] In some embodiments, the negative electrode material is measured by Raman spectroscopy and has a Raman scattering intensity of 1300 cm -1 ~1400cm -1 Peak intensities in the range I D and 1580cm -1 ~1620cm -1 Peak intensities in the range I G Intensity ratio I D / I G 0.03≦I D / I G ≦0.10.

[0014] In some embodiments, the negative electrode material comprises primary synthetic graphite particles and / or secondary synthetic graphite particles.

[0015] In some embodiments, the pores comprise at least one of micropores and mesopores.

[0016] In a second aspect, the present application provides a battery comprising the artificial graphite negative electrode material according to the first aspect. Effect of the Invention

[0017] The technical solution of the present application has at least the following beneficial effects: Those skilled in the art will appreciate that the pore volume of artificial graphite within a certain range is Li +The applicant has found that the diffusion channel of the electrolyte can be increased, and a specific surface area within a certain range can ensure sufficient electrochemical reaction interface, promote the diffusion of lithium ions at the solid-liquid interface and in the solid phase, reduce concentration polarization, and is favorable for improving the capacity and rate characteristics of the negative electrode material. The applicant has conducted intensive research based on this and found that the release and absorption of lithium ions not only requires diffusion channels and reaction interfaces, but also requires electrolyte as a medium. If some pores are not infiltrated with the electrolyte due to the influence of surface morphology or other factors, they cannot exert their effect, and the corresponding surfaces naturally cannot cause electrochemical reactions, which corresponds to a lack of "effective electrochemical reaction space". Therefore, the rate characteristics are not necessarily effectively improved by only satisfying sufficient pore volume and specific surface area. The infiltration ability of the electrolyte is generally expressed by the amount of oil absorption. This application has conducted a large amount of experimental research by combining the three elements of pore volume, specific surface area and oil absorption, and has found that by controlling the O×V×S of the negative electrode material within the above range, the reaction space in the negative electrode material is sufficient to effectively release and absorb lithium ions, which is advantageous for improving the high-rate charge and discharge performance of the artificial graphite negative electrode material.

[0018] The negative electrode material provided by the present application is manufactured and processed by a continuous graphitization process, which continuously supplies and discharges materials, and the paths and times through which all materials pass are the same, and the times and temperatures through which they pass through the high temperature region are the same. In addition, the heating and cooling rates of the calcination and graphitization stages in the graphitization process are controlled, so that the volatile components, impurity elements and other substances in the material can be uniformly and quickly released, and at the same time, a certain amount of additives is introduced to precisely control the pore volume inside and / or on the surface of the graphite. Through the synergistic use of the above processes, the relationship between the specific surface area, oil absorption and pore volume can be precisely controlled to satisfy 400≦O×V×S≦1500.

[0019] The negative electrode material provided by the present application has low energy consumption per unit mass, obvious advantages in cost and production cycle, and is environmentally friendly. [Brief description of the drawings]

[0020] [Figure 1] 1 is a scanning electron microscope photograph of an artificial graphite negative electrode material provided in Example 12 of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] In order to better explain the present application and facilitate understanding of the technical solution of the present application, the present application will be described in more detail below. It should be noted that the following examples are merely simplified examples of the present application, and do not indicate or limit the scope of protection of the present application. The scope of protection of the present application is subject to the claims.

[0022] In the field of anode materials, the development of continuous graphitization equipment has continued for decades, and as early as 1987, a patent (US06619591) disclosed an apparatus capable of performing continuous graphitization treatment on carbon-containing materials. In recent years, applicants have also continued to develop continuous graphitization equipment, for example, a patent with registration publication number CN211425033U filed in 2019 discloses a vertical continuous kiln for producing anode materials for lithium batteries, which can continuously discharge materials from an outlet and continuously supply materials from a material pipe. Compared with conventional processes, the continuous graphitization process shortens the graphitization time from several days to several hours, and the reduction in energy consumption is quite significant, but the significant reduction in graphitization time results in changes in the microstructure of artificial graphite, especially changes in the pore structure and crystal shape inside the artificial graphite, compared with conventional artificial graphite. It has been proven in the industry that such changes make it difficult to meet the required performance of artificial graphite and difficult to improve, and therefore, even though continuous graphitization equipment has been in existence for 30 to 40 years, there is no precedent for successful mass production of continuously graphitized artificial graphite anode products.

[0023] In recent years, with the increasing energy scarcity, in order to further reduce the cost of artificial graphite, the applicant continues to develop the application of continuous graphitization equipment, develops an artificial graphite anode material with performance equivalent to or even better than the current normal graphitized anode material, and aims to reduce the energy consumption of the artificial graphite anode material and further reduce the cost. The applicant has developed various means to improve the rapid rise and fall of temperature that brings unfavorable changes to artificial graphite products through the development of a large-scale manufacturing process, and obtains a series of different types of artificial graphite anode materials through product selection. Although these artificial graphite anode materials have different microstructures from normal artificial graphite products, their electrical performance can be basically equivalent to that of normal artificial graphite products, and in some respects, the electrical performance and processing performance are better or more stable, and they have the conditions to replace normal artificial graphite products.

[0024] The manufacturing process and related products will be described in more detail below using a manufacturing process developed by the applicant as an example.

[0025] The method for preparing the negative electrode material includes the following steps. In S10, the raw coke is calcined at a temperature of 500 to 1200° C. for 3 to 6 hours, the temperature increase rate during the calcination process is 2 to 10° C. / min, and low temperature calcined coke is obtained after natural cooling. In S20, the low-temperature calcined coke is subjected to a shaping process to obtain coke powder having a median diameter of 10 μm to 20 μm. In S30, the mixture containing the coke powder, adhesive, additives and solvent is pressed at a pressure of 5 MPa to 100 MPa to obtain a precursor having a mass ratio of the coke powder to the additives of 100:(1 to 5). In S40, the precursor is placed in a continuous graphitization furnace and heated to 2800°C to 3200°C at a heating rate of 12°C / min to 20°C / min, and then further kept at 2800°C to 3200°C for 2h to 5h, and then cooled to 30°C at a heating rate of 15°C / min to 25°C / min to obtain the negative electrode material.

[0026] The method for preparing the negative electrode material provided by the present application is to crush the low-temperature calcined coke obtained by the raw coke calcination process into coke powder, and the heating rate in the low-temperature calcination stage is slow, which is favorable for the gradual release of volatile components, and control the initial formation process of the pore structure, and press the mixture of the coke powder, the adhesive, the additives and the solvent, and place the precursor directly in the continuous graphitization furnace, and the heating rate is very fast, and after the rapid heating, the precursor reaches the graphitization temperature in a short time, and the additives are rapidly volatilized and released, and further form pores in the interior and / or surface of the graphite particles, and the existence of pores contributes to the improvement of the specific surface area and oil absorption, and increases the reactive area of ​​the electrode of the negative electrode active material, which contributes to the improvement of the high-rate charge and discharge performance of the material. In addition, the process of loading and unloading the material in the continuous graphitization furnace is completed within a few hours, which has a high thermal energy utilization rate and can reduce production costs.

[0027] In some embodiments, the green coke feedstock comprises at least one of petroleum coke, needle coke, pitch coke, and isotropic coke.

[0028] In some embodiments, the heating rate during the calcination process may be specifically 2° C. / min, 3° C. / min, 5° C. / min, 6° C. / min, 8° C. / min, 9° C. / min, or 10° C. / min, etc. It can be seen that the heating rate during the calcination process within the above range is favorable for gradually releasing the volatile components in the raw materials, and preliminarily forming a pore structure, which, combined with the rapid heating during the subsequent graphitization process, results in a negative electrode material that satisfies 400≦O×V×S≦1500.

[0029] In some embodiments, the temperature of the calcination treatment may be specifically 500° C., 550° C., 600° C., 700° C., 750° C., 800° C., 850° C., 900° C., 1000° C., or 1200° C., but is not limited to the recited values, and other unrecited values ​​within the numerical ranges apply as well. As can be understood, having the calcination treatment temperature within the above ranges is advantageous for removing substances such as volatile components in the raw coke raw material.

[0030] In some embodiments, the heat retention time of the calcination treatment may be specifically 3h, 4h, 4.5h, 5h, 5.5h, or 6h, but is not limited to the listed values, and other values ​​not listed within the range apply as well. Preferably, the heat retention time of the calcination treatment is 3h to 4h.

[0031] In some embodiments, the shaping comprises at least one of grinding, spheronizing, or sieving.

[0032] The median diameter of the coke powder obtained by shaping is 10 μm to 20 μm, and more specifically, it may be 12 μm, 13 μm, 14 μm, 16 μm, 18 μm, 18.5 μm, 19 μm, or 20 μm, but is not limited to the numerical values ​​listed, and other numerical values ​​not listed within the numerical range are also applicable. By controlling the median diameter of the coke powder within the above range through multiple tests, it is advantageous to achieve both processing performance, capacity, and rate characteristics.

[0033] In some embodiments, the mass content of carbon in the coke powder is 80% or more, and may be specifically 80%, 81%, 82%, 85%, 90%, 95% or 96%, but is not limited to the recited values, and other unrecited values ​​within the numerical range apply as well.

[0034] In some embodiments, the solvent comprises at least one of water, ethanol, acetone, benzene, toluene, quinoline, tetrahydrofuran, and carbon tetrachloride.

[0035] In some embodiments, the adhesive comprises at least one of heavy oil, mineral oil, coal tar, pitch, petroleum resin, phenolic resin, epoxy resin, coumarone resin, potato starch, wheat starch, corn starch, sweet potato starch, arrowroot starch, and tapioca flour. The pitch may comprise at least one of petroleum-based liquid pitch and coal-based liquid pitch. Specifically, the petroleum-based liquid pitch may be petroleum pitch, modified pitch, mesophase pitch, and the like.

[0036] In some embodiments, the additive comprises at least one of boron oxide, boron carbide, boron nitride, silicon carbide, boron carbide, boron nitride, boric acid, boron chloride, and sodium borate, and the additive acts as a graphitization catalyst while being volatilized and released by rapid temperature increase and decrease during the graphitization process, which is advantageous in forming stable pores inside and / or on the surface of the artificial graphite.

[0037] In some embodiments, the mass ratio of the coke powder, the adhesive, the solvent, and the additive is 100:(3-20):(5-50):(1-5), specifically, it may be 100:3:5:1, 100:10:15:1, 100:15:20:5, 100:20:20:1, 100:20:15:3, 100:10:10:5, or 100:15:25:2, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable. By controlling the content of the additive within the above range, it is advantageous to catalyze the graphitization process, while a certain number of pores can be formed inside the graphite.

[0038] In some embodiments, the mixing method of the mixture includes at least one of mechanical stirring and ultrasonic dispersion.When mechanical stirring is adopted for mixing, a propeller type stirrer, a turbine type stirrer, a flat blade type stirrer, etc. can be adopted as long as each component in the mixture is sufficiently mixed uniformly.

[0039] In some embodiments, the stirring speed is 10 r / min to 1000 r / min, specifically, 10 r / min, 50 r / min, 70 r / min, 100 r / min, 120 r / min, 150 r / min, 200 r / min, 300 r / min, 350 r / min, 400 r / min, 500 r / min, or 1000 r / min, etc., but is not limited thereto. By controlling the stirring speed within the above range, it is advantageous to mix each component to form a uniform mixture.

[0040] The stirring may be performed at room temperature or in a preheated state. Preferably, the stirring temperature may be controlled to 25°C to 200°C. As can be understood, proper preheating is advantageous for mixing each component to form a uniform mixture.

[0041] In some embodiments, the pressing method includes at least one of extrusion, die pressing, roll pressing, and isostatic pressing.

[0042] In some embodiments, the pressing pressure may be specifically 5 MPa, 15 MPa, 25 MPa, 30 MPa, 35 MPa, 40 MPa, 45 MPa, 50 MPa, 55 MPa, 60 MPa, 70 MPa, 80 MPa, 90 MPa, or 100 MPa, etc., and the pressing process can improve the fluidity of the material during the graphitization process while increasing the furnace loading and production capacity of the material.

[0043] In some embodiments, the graphitization treatment temperature may be, for example, 2800°C, 2900°C, 3000°C, 3100°C, 3150°C, 3180°C, or 3200°C, but is not limited to the listed values, and other unlisted values ​​within the range apply as well.

[0044] In some embodiments, the graphitization incubation time may be, for example, 2h, 2.5h, 3h, 3.5h, 3.8h, 4h, 4.5h, or 5h, but is not limited to the listed values, and other unlisted values ​​within the range apply as well. Preferably, the graphitization incubation time is 2h to 3h.

[0045] In some embodiments, the heating rate of the graphitization treatment may be, but is not limited to, 12° C. / min, 13° C. / min, 14° C. / min, 16° C. / min, 18° C. / min, 18.5° C. / min, or 20° C. / min, etc. Rapid heating is advantageous for forming pores in and / or on the surface of the graphite material and for controlling the specific surface area.

[0046] In some embodiments, the cooling rate after graphitization is 15° C. / min to 25° C. / min, and may be specifically 15° C. / min, 16° C. / min, 17° C. / min, 18° C. / min, 20° C. / min, 21° C. / min, 22° C. / min, 23° C. / min, 24° C. / min, or 25° C. / min, but is not limited to the listed values, and other unlisted values ​​within the range of values ​​also apply. Rapid cooling is advantageous for controlling the specific surface area and oil absorption of the material, and can significantly shorten the graphitization processing cycle and reduce production costs.

[0047] In some embodiments, the graphitization process is followed by at least one of crushing, sieving, and degaussing. Preferably, the carbonization process is followed by crushing, degaussing, and sieving, in that order.

[0048] In some embodiments, the grinding means may be any one of a mechanical grinder, an airflow grinder, and a cryogenic grinder.

[0049] In some embodiments, the sieving method is any one of a fixed sieve, a drum screen, a resonating sieve, a roller sieve, a vibrating sieve, and a chain grizzly, and the mesh number of the sieving is 100 to 500 mesh. Specifically, the mesh number of the sieving may be 100 mesh, 200 mesh, 250 mesh, 325 mesh, 400 mesh, 500 mesh, etc., and controlling the particle size of the negative electrode material within the above range contributes to improving the processing characteristics of the negative electrode material.

[0050] In some embodiments, the demagnetizing device is one of a permanent magnet drum type magnetic separator, an electromagnetic iron remover, and a pulsating high gradient magnetic separator, and the demagnetizing is to finally control the content of magnetic materials in the negative electrode material, to avoid the discharging effect of magnetic materials on the lithium ion battery, and to ensure the safety of the battery during use.

[0051] A negative electrode material comprising artificial graphite, the artificial graphite having pores inside and / or on the surface, the negative electrode material having an oil absorption of 0 mL / 100 g and a pore volume of V cm 3 / kg, specific surface area is Sm 2 / g, 400≦O×V×S≦1500, and the pore volume was measured using an ASAP 2460 device manufactured by Micromeritics, Inc., USA, and calculated using the BJH Desorption cumulative volume of pores model within the pore diameter range of 17 Å to 3000 Å.

[0052] The negative electrode material provided by the present application is produced and processed through a continuous graphitization process, in which the material is first calcined at a low temperature by rapid heating, and then graphitized by rapid heating at a high temperature. At the same time, a certain amount of additives is added to the raw material to precisely control the pores inside and / or on the surface of the graphite, so that the pore volume, specific surface area and oil absorption of the material can be ideally adjusted and controlled to meet the design requirements.

[0053] Those skilled in the art will appreciate that the pore volume of artificial graphite within a certain range is Li +The applicant has found that the diffusion channel of the electrolyte can be increased, and a specific surface area within a certain range can ensure sufficient electrochemical reaction interface, promote the diffusion of lithium ions at the solid-liquid interface and in the solid phase, reduce concentration polarization, and is favorable for improving the capacity and rate characteristics of the negative electrode material. The applicant has conducted intensive research based on this and found that the release and absorption of lithium ions not only requires diffusion channels and reaction interfaces, but also requires electrolyte as a medium. If some pores are not infiltrated with the electrolyte due to the influence of surface morphology or other factors, they cannot exert their effect, and the corresponding surfaces naturally cannot cause electrochemical reactions, which corresponds to a lack of "effective electrochemical reaction space". Therefore, the rate characteristics are not necessarily effectively improved by only satisfying sufficient pore volume and specific surface area. The infiltration ability of the electrolyte is generally expressed by the amount of oil absorption. This application has conducted a large amount of experimental research by combining the three elements of pore volume, specific surface area and oil absorption, and has found that by controlling the O×V×S of the negative electrode material within the above range, the reaction space in the negative electrode material is sufficient to effectively release and absorb lithium ions, which is advantageous for improving the high-rate charge and discharge performance of the artificial graphite negative electrode material.

[0054] In some embodiments, the oil absorption of the negative electrode material is 43≦O≦60 when OmL / 100g, and specifically may be 43, 44, 45, 47, 49, 51, 52, 53, 54, 55, 57, 59, or 60, etc., but is not limited thereto. By controlling the oil absorption of the material within the above range, it is advantageous to improve the adsorption and infiltration performance of the material to the electrolyte, and the electrochemical performance of the negative electrode material is better.

[0055] In some embodiments, the pore volume of the negative electrode material is determined by the following formula: Vcm 3 / kg, 5≦V≦8, specifically, it may be 5.1, 5.2, 5.5, 5.8, 6.0, 6.2, 6.5, 6.8, 7.0, 7.2, 7.5, 8.0, etc., but is not limited thereto. When the pores generate an electrochemical reaction inside the electrode, the pores create more lithium ion diffusion channels and electrochemical reaction interfaces in the negative electrode material, promote the diffusion of lithium ions at the solid-liquid interface and in the solid phase, reduce concentration polarization, and are favorable for improving the rate characteristics of the negative electrode material.

[0056] In some embodiments, the specific surface area of ​​the negative electrode material is determined by Sm 2 / g, 1.78≦S≦3.0, specifically, 1.79, 1.85, 1.95, 2.00, 2.25, 2.43, 2.57, 2.61, 2.72, 2.85, 2.90, 3.0, etc., but not limited thereto. As can be understood, if the specific surface area is too large, it is easy to cause the formation of a solid electrolyte membrane, and the irreversible lithium salt is excessively consumed, which reduces the initial efficiency of the battery.

[0057] In some embodiments, the pores comprise at least one of micropores and mesopores.

[0058] In some embodiments, the particle size D of the negative electrode material 50 is 10 μm to 30 μm. Specifically, it may be 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 20 μm, 25 μm, 30 μm, or the like, and is not limited thereto.

[0059] In some embodiments, the particle size of the negative electrode material is 0.9≦(D 90 -D 10 ) / D 50 ≦1.8, specifically, it may be 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, etc., but is not limited thereto. By the particle size of the negative electrode material satisfying the above relationship, it is possible to ensure the concentration of the particle size distribution of the negative electrode material and the appropriate deposition density.

[0060] In addition, the cumulative particle size distribution based on volume measured by the laser diffraction method is D 10 represents the particle size when the percentage of the cumulative particle size distribution of the powder reaches 10%, and D 50 represents the particle size corresponding to the cumulative particle size distribution percentage reaching 50%, and D 90 represents the particle size corresponding to when the cumulative particle size distribution percentage reaches 90%.

[0061] In some embodiments, the negative electrode material further comprises amorphous carbon.

[0062] In some embodiments, the negative electrode material further comprises amorphous carbon, and the mass percentage of amorphous carbon in the negative electrode material is 0.1 wt% to 5 wt%, and the mass percentage of amorphous carbon in the negative electrode material may be specifically 0.1 wt%, 0.3 wt%, 0.5 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt%, or 5 wt%, and the presence of amorphous carbon provides more irregular and more open diffusion paths for lithium ions, which is advantageous for improving the rate characteristics of the material.

[0063] In some embodiments, the negative electrode material is measured by Raman spectroscopy and has a Raman scattering intensity of 1300 cm -1 ~1400cm -1 Peak intensities in the range I D and 1580cm -1 ~1620cm -1 Peak intensities in the range I G Intensity ratio I D / I G 0.03≦I D / I G ≦0.10, specifically, it may be 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, etc., but is not limited thereto. Intensity ratio I of negative electrode material D / I G By controlling the amount of carbon black within the above range, the degree of graphitization of the negative electrode material can be improved, resulting in better quality of graphite crystals.

[0064] In some embodiments, the negative electrode material includes primary synthetic graphite particles and / or secondary synthetic graphite particles.

[0065] In some embodiments, the pores comprise at least one of micropores and mesopores.

[0066] In some embodiments, the specific capacity of the negative electrode material is 320mAh / g to 370mAh / g, and specifically may be 320mAh / g, 340mAh / g, 342mAh / g, 345mAh / g, 353mAh / g, 355mAh / g, 357mAh / g, 360mAh / g, 365mAh / g, or 370mAh / g, etc., but is not limited thereto.

[0067] A battery comprising the above-described negative electrode material.

[0068] As will be apparent to those skilled in the art, the battery manufacturing method described above is merely an example, and other methods commonly used in the art may be adopted without departing from the scope of the present disclosure, and other types of batteries, such as sodium ion batteries, potassium ion batteries, etc., may be manufactured and measured. EXAMPLES

[0069] The embodiments of the present application will be further described below through a number of examples. However, the embodiments of the present application are not limited to the following specific examples. Appropriate modifications can be made within the scope of protection.

[0070] Example 1 The method for preparing the composite negative electrode material of this embodiment includes the following steps. (1) Daqing petroleum coke was calcined at 800℃ for 4h. The heating rate during the calcination process was 5℃ / min. After cooling, low-temperature calcined coke was obtained. (2) The low-temperature calcined coke is crushed and shaped in a shaping device to obtain crushed and shaped coke powder, and the median diameter is controlled to 15 μm. (3) Coke powder, coal tar, quinoline, and silicon carbide were uniformly mixed in a mass ratio of 100:5:15:2 to obtain a mixture. (4) The mixture was pressed at a pressure of 20 MPa to obtain a precursor. (5) The precursor was graphitized at 3000°C in a continuous graphitization furnace to obtain a graphitized product. The temperature rise curve shows that the temperature was raised to 3000°C at a rate of 16.5°C / min, the temperature was kept at 3000°C for 3 hours, and after the temperature hold, the temperature was lowered to 30°C at a rate of 16.0°C / min. (6) The graphitized product was subjected to processes such as dispersion, demagnetization, and sieving through a 250 mesh screen to obtain an artificial graphite negative electrode material.

[0071] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0072] Example 2 The method for preparing the composite negative electrode material of this embodiment includes the following steps. (1) The Takara steel pitch coke was calcined at 750℃ for 4 hours. The heating rate during the calcination process was 3℃ / min. After cooling, low-temperature calcined coke was obtained. (2) The low-temperature calcined coke is crushed and shaped in a shaping device to obtain crushed and shaped coke powder, and the median diameter is controlled to 15 μm. (3) Coke powder, starch, water, and sodium borate were uniformly mixed in a mass ratio of 100:6:20:2 to obtain mixture A. (4) The mixture was pressed at a pressure of 20 MPa to obtain a precursor. (5) The precursor was graphitized at 2950°C in a continuous graphitization furnace to obtain a graphitized product. The temperature rise curve was as follows: the temperature was raised to 2950°C at a rate of 15°C / min, the temperature was kept at 2950°C for 3 hours, and then the temperature was lowered to 30°C at a rate of 20°C / min. (6) The graphitized product was subjected to processes such as dispersion, demagnetization, and sieving through a 250 mesh screen to obtain an artificial graphite negative electrode material.

[0073] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0074] Example 3 The method for preparing the composite negative electrode material of this embodiment includes the following steps. (1) Daqing petroleum coke was calcined at 800℃ for 4h. The heating rate during the calcination process was 6℃ / min. After cooling, low-temperature calcined coke was obtained. (2) The low-temperature calcined coke is crushed and shaped in a shaping device to obtain crushed and shaped coke powder, and the median diameter is controlled to 15 μm. (3) Coke powder, coal tar, quinoline, and boron nitride were uniformly mixed in a mass ratio of 100:5:15:3 to obtain mixture A. (4) The mixture was pressed at a pressure of 20 MPa to obtain a precursor. (5) The precursor was graphitized at 2900°C in a continuous graphitization furnace to obtain a graphitized product. The temperature rise curve was as follows: the temperature was raised to 2900°C at a rate of 18°C / min, the temperature was kept at 2900°C for 3 hours, and after the temperature hold, the temperature was lowered to 30°C at a rate of 21.5°C / min. (6) The graphitized product was subjected to processes such as dispersion, demagnetization, and sieving through a 250 mesh screen to obtain an artificial graphite negative electrode material.

[0075] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0076] Example 4 The method for preparing the composite negative electrode material of this embodiment includes the following steps. (1) Daqing petroleum coke was calcined at 800℃ for 4h. The heating rate during the calcination process was 5℃ / min. After cooling, low-temperature calcined coke was obtained. (2) The low-temperature calcined coke is crushed and shaped in a shaping device to obtain crushed and shaped coke powder, and the median diameter is controlled to 15 μm. (3) Coke powder, starch, water, and boron carbide were uniformly mixed in a mass ratio of 100:6:20:2 to obtain mixture A. (4) The mixture was pressed at a pressure of 20 MPa to obtain a precursor. (5) The precursor was graphitized at 3000°C in a continuous graphitization furnace to obtain a graphitized product. The temperature rise curve was as follows: the temperature was raised to 3000°C at a rate of 20°C / min, the temperature was kept at 3000°C for 3 hours, and then the temperature was lowered to 30°C at a rate of 16.6°C / min. (6) The graphitized product was subjected to processes such as dispersion, demagnetization, and sieving through a 250 mesh screen to obtain an artificial graphite negative electrode material.

[0077] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0078] Example 5 The difference from Example 1 is that the calcination temperature in step (1) is 500°C.

[0079] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0080] Example 6 The difference from Example 1 is that the calcination temperature in step (1) is 1200°C.

[0081] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0082] Example 7 The difference from Example 1 is that the calcination time in step (1) is 3 hours.

[0083] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0084] Example 8 The difference from Example 1 is that the calcination time in step (1) is 6 hours.

[0085] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0086] Example 9 The difference from Example 1 is that in step (3), coke powder, coal tar, quinoline, and silicon carbide were uniformly mixed in a mass ratio of 100:3:15:2 to obtain a mixture.

[0087] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0088] Example 10 The difference from Example 1 is that in step (3), coke powder, coal tar, quinoline, and silicon carbide were uniformly mixed in a mass ratio of 100:20:15:2 to obtain a mixture.

[0089] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is secondary particle artificial graphite.

[0090] Example 11 The difference from Example 1 is that in step (3), coke powder, coal tar, quinoline, and silicon carbide were uniformly mixed in a mass ratio of 100:5:5:2 to obtain a mixture.

[0091] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0092] Example 12 The difference from Example 1 is that in step (3), coke powder, coal tar, quinoline, and silicon carbide were uniformly mixed in a mass ratio of 100:5:50:2 to obtain a mixture.

[0093] An electron microscope photograph of the above-mentioned negative electrode material is shown in FIG. 1. As can be seen from FIG. 1, the negative electrode material is composed of primary particles and secondary particles.

[0094] Example 13 The difference from Example 1 is that in step (3), coke powder, coal tar, quinoline, and silicon carbide were uniformly mixed in a mass ratio of 100:5:15:1 to obtain a mixture.

[0095] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0096] Example 14 The difference from Example 1 is that in step (3), coke powder, coal tar, quinoline, and silicon carbide were uniformly mixed in a mass ratio of 100:5:15:5 to obtain a mixture.

[0097] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0098] Example 15 The difference from Example 1 is that the pressing pressure in step (4) is 5 MPa.

[0099] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0100] Example 16 The difference from Example 1 is that the pressing pressure in step (4) is 100 MPa.

[0101] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0102] Example 17 The difference from Example 1 is that the graphitization temperature in step (5) is 2800°C.

[0103] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0104] Example 18 The difference from Example 1 is that the graphitization temperature in step (5) is 3200°C.

[0105] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0106] Example 19 The difference from Example 1 is that the heat retention time for the graphitization treatment in step (5) is 2 hours.

[0107] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0108] Example 20 The difference from Example 1 is that the heat retention time for the graphitization treatment in step (5) is 5 hours.

[0109] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0110] Comparative Example 1 The difference from Example 1 is that the precursor obtained in step (4) is placed in a graphite crucible, and then the graphite crucible is transferred to an Acheson furnace to obtain a negative electrode material through a high-temperature graphitization process. In the graphitization process, the maximum temperature is 2900°C, the maximum temperature is maintained for 3 hours, and the temperature increase rate is 0.6°C / min and the temperature decrease rate is 0.1°C / min.

[0111] Comparative Example 2 Daqing petroleum coke is crushed and shaped by a shaping device to obtain crushed and shaped coke powder. The obtained coke powder with a median diameter of 15 μm is directly put into a graphite crucible, and the graphite crucible is then transferred to an Acheson furnace to obtain a negative electrode material through high-temperature graphitization. In the graphitization process, the maximum temperature is 2900°C, the maximum temperature is kept for 8 hours, and the heating rate is 0.7°C / min and the cooling rate is 0.1°C / min.

[0112] Comparative Example 3 Daqing petroleum coke was calcined at 800℃ for 4 hours, the calcination rate was 1.5℃ / min, and then it was put into a continuous graphitization furnace. The temperature curve was 8℃ / min to 2900℃, kept at 2900℃ for 3 hours, and then cooled to 30℃ at 10℃ / min. The discharged material was crushed and shaped to a median diameter of 15μm to obtain anode material.

[0113] Measurement method (1) Method for measuring particle size of negative electrode material: The particle size distribution range of the composite anode material was measured by a Malvern laser granulometer.

[0114] (2) Measurement method for pore volume of negative electrode material: Measurements were performed using an ASAP 2460 device manufactured by Micromeritics, Inc., USA, and the pore volume V was calculated within the pore diameter range of 17 Å to 3000 Å using the BJH Desorption cumulative volume of pores model.

[0115] (3) Measurement method for the specific surface area of ​​the negative electrode material: The measurement was performed using a dynamic specific surface area analyzer JW-DX (manufactured by Beijing Jingwei Gaobo Science and Technology Co., Ltd.) and the unit is m 2 / g.

[0116] (4) Measurement method for the surface morphology of negative electrode material: The surface morphology of the negative electrode material particles was observed using a S4800 scanning electron microscope (Hitachi).

[0117] (5) Method for measuring oil absorption of negative electrode material: The oil absorption was measured using an ASAHI S-500 oil absorption measuring device (manufactured by ASAHISOUKEN, Japan). The oil absorption O is the amount of linseed oil dropped when the torque due to the change in viscosity characteristics reaches 70% of the maximum torque, and is expressed in mL / 100 g.

[0118] (6) Negative electrode material I D / I G Measurement method: Raman spectroscopy revealed that the composite anode material exhibited a peak at 1300 cm -1 ~1400cm -1 Peak intensities in the range I D And, 1580cm -1 ~1620cm -1 Peak intensities in the range I G Comparison with I D / I G was measured.

[0119] (7) Battery performance measurement method: The negative electrode materials prepared in Examples 1 to 22 and Comparative Examples 1 to 3, carboxymethyl cellulose, conductive carbon black, and styrene butadiene rubber were mixed uniformly in deionized water in a mass ratio of 95:1.5:1.5:2 for 8 hours under magnetic stirring. The mixed slurry was applied onto copper foil and vacuum dried at 60°C to obtain a working electrode. Metallic lithium was used as the counter electrode and reference electrode, the separator was Celgard2325, and the electrolyte was 1mol·L-1LiPF6-EC (ethylene carbonate) / DMC (dimethyl carbonate) / EMC (ethyl methyl carbonate) (volume ratio 1:1:1). The assembly of a CR2016 coin battery pack was completed in a glove box filled with high-purity argon gas.

[0120] The initial discharge capacity / initial discharge efficiency measurements were performed using a LAND battery measuring device, and the charge / discharge conditions were as follows: leave it for 2 hours, discharge at 0.1C to 0.005V, discharge at 0.09C, 0.08C...0.02C to 0.001V, leave it for 15 minutes, charge at 0.1C to 1.5V, and leave it for 15 minutes.

[0121] The rate characteristics of the button half-cell were measured in an environment of 25±2° C., and the charge / discharge specific capacity and coulombic efficiency at 0.2C, 1C, and 2C were obtained. The charge and discharge conditions for rate measurement of the button half cell were: (1) discharge at 0.1C to 0.01V, constant voltage for 5h, charge at 0.1C to 1.5V; (2) discharge at 0.2C to 0.01V, constant voltage to 0.01C, charge at 0.2C to 1.5V; (3) discharge at 0.2C to 0.01V, constant voltage to 0.01C, charge at 2C to 1.5V; (4) discharge at 0.2C to 0.01V, constant voltage to 0.01C, charge at 0.2C to 1.5V; (5) discharge at 1C to 0.01V, constant voltage to 0.01C, charge at 0.2C to 1.5V; (6) discharge at 2C to 0.01V.

[0122] Whole battery measurement: The negative electrode material obtained in each example was used as the negative electrode active material, and the mass percentage of the negative electrode active material, conductive agent, adhesive, and dispersant was 95.2:1.5:2:1.3. The material was dissolved in deionized water, mixed, and the solid content was controlled to 50 wt%, and the mixture was applied to a copper foil collector with a thickness of 8 μm and dried in a vacuum to produce a negative electrode piece. Lithium iron phosphate, polyvinylidene fluoride, and conductive carbon black were uniformly mixed with a solvent NMP (N-methylpyrrolidone) in a mass ratio of 95:2:3, and then applied to an aluminum foil with a thickness of 16 μm and dried in a vacuum to produce a positive electrode piece. The positive and negative electrode pieces that had been completely coated were subjected to sheet pressing, winding, drying, injection, sealing, chemical synthesis, capacity grading, and other processes to produce a 554065-type soft-pack lithium-ion battery.

[0123] The obtained soft-pack battery was subjected to charge / discharge measurements using a LAND battery test system (manufactured by Wuhan Jinnuo Electronics Co., Ltd.). The battery was charged / discharged at room temperature with a current of 1C / 1C, and the charge / discharge voltage was limited to 3.0V to 4.35V. The initial efficiency and the 500-cycle capacity retention rate were measured (the press density of the negative electrode piece was 1.60g / cm). 3 (It is.) The results of performance measurement of the negative electrode materials obtained in the above examples are shown in Table 1 below, and the results of performance measurement of the batteries manufactured using the negative electrode materials are shown in Table 2 below.

[0124] [Table 1]

[0125] [Table 2]

[0126] As can be seen from the measurement data of Examples 1 to 20, pores are formed inside and / or on the surface of the graphite prepared in the examples of the present application, and the high-rate charge / discharge performance of the material is obviously improved. This is because when the negative electrode material is prepared as an electrode and applied to a lithium-ion battery, the effective electrochemical reaction space inside the material is sufficient after the electrolyte is injected, which is favorable for improving the rate characteristics of the negative electrode material.

[0127] The negative electrode material produced in Comparative Example 1 had an oil absorption O that was too large, so that O×V×S was outside the above range, and both the rate and cycle performance of the material were poor.

[0128] The negative electrode material prepared in Comparative Example 2 has insufficient pores in the artificial graphite, a too small pore volume V, and an O×V×S ratio outside the above range, and thus the diffusion channels for lithium ions are insufficient, which is not favorable for improving the rate characteristics of the negative electrode material.

[0129] The negative electrode material produced in Comparative Example 3 had a temperature rise rate in the calcination treatment and graphitization treatment in the production process that was outside the optimized range of the production method of the present application, and therefore O×V×S was outside the above range, and the capacity and rate characteristics were inferior to those of Example 1 produced under equivalent process conditions.

[0130] Although the present application has been disclosed above by way of preferred embodiments, the scope of the claims is not limited thereto, and any person skilled in the art may make some possible changes or modifications without departing from the technical idea of ​​the present application, and therefore the scope of protection of the present application should conform to the scope defined in the claims of the present application.

Claims

1. A negative electrode material containing artificial graphite, The artificial graphite has pores inside and / or on the surface, The negative electrode material has an oil absorption of 0 mL / 100 g and a pore volume of V cm 3 / kg, specific surface area is Sm 2 / g, 400≦O×V×S≦1500, The pore volume is measured using an ASAP 2460 device manufactured by Micromeritics, Inc., USA, and calculated using the BJH Desorption cumulative volume of pores model within a pore diameter range of 17 Å to 3000 Å. A negative electrode material.

2. 2. The negative electrode material according to claim 1, wherein the oil absorption is 43≦O≦60 when the oil absorption is O mL / 100 g.

3. The pore volume is V cm 3 2. The negative electrode material according to claim 1, wherein V satisfies 5≦V≦8 when the total weight of the negative electrode material is 1.0 / kg.

4. The specific surface area is Sm 2 2. The negative electrode material according to claim 1, wherein S satisfies 1.78≦S≦3.0 when expressed as 1.78≦S≦3.0 / g.

5. 2. The negative electrode material according to claim 1, wherein the particle size satisfies 0.9≦(D90−D10) / D50≦1.8 and 10 μm≦D50≦30 μm.

6. The negative electrode material according to any one of claims 1 to 5, characterized in that it satisfies at least one of the following characteristics (1) to (2). (1) The negative electrode material further includes amorphous carbon; (2) The negative electrode material further contains amorphous carbon, and the mass ratio of the amorphous carbon in the negative electrode material is 0.1 wt % to 5 wt %.

7. The negative electrode material was measured by Raman spectroscopy at 1300 cm -1 ~1400cm -1 Peak intensities in the range of I D ) and 1580 cm -1 ~1620cm -1 Peak intensities in the range of I G ) and the intensity ratio (I D / I G ) is 0.03≦I D / I G 6. The negative electrode material according to claim 1, wherein the ratio of the stoichiometric ratio to the molecular weight of the negative electrode is ≦0.

10.

8. 6. The negative electrode material according to claim 1, comprising primary particles of artificial graphite and / or secondary particles of artificial graphite.

9. 6. The negative electrode material according to claim 1, wherein the pores include at least one of micropores and mesopores.

10. A battery comprising the negative electrode material according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • A method for preparing high-rate artificial graphite anode material

    CN109830669B

  • Graphite particle for nonaqueous secondary battery, negative electrode for nonaqueous secondary battery using the same, and nonaqueous secondary battery

    JP2014067680A

  • Carbon material, negative electrode for nonaqueous secondary battery, nonaqueous secondary battery and method for producing carbon material

    JP2015153664A

  • Graphite negative electrode material, negative electrode, lithium ion battery and method for manufacturing the same

    JP2022551407A

Cited By

  • Battery and its manufacturing method, power consumption device