Secondary batteries and electrical appliances

By controlling non-Faradaic charge and adjusting parameters like capacitance, potential range, and contact angle, the solution enhances the cycle performance and life of secondary batteries by reducing lithium precipitation and polarization, thus improving their overall efficiency.

JP2024543316AActive Publication Date: 2024-11-21SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024523255
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-26
Filing Date
2022-12-22
Publication Date
2024-11-21
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

Existing secondary batteries face challenges in achieving improved cycle performance and cycle life due to issues such as lithium precipitation and sheet polarization, particularly in high energy density applications.

Method used

The solution involves controlling the non-Faradaic charge amount of the negative electrode sheet within a specific range (0.05≦Q≦2.5) by adjusting parameters like non-Faradaic capacitance (Cdl), potential range (ΔU), contact angle (θ), resistance (R), and particle size distribution of the negative electrode active material, along with the use of specific materials and coatings to enhance the balance of high magnification and charge/discharge characteristics.

Benefits of technology

This approach effectively reduces interface deterioration, improves consistency, and extends the cycle life and magnification performance of secondary batteries by minimizing lithium precipitation and sheet polarization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543316000003
    Figure 2024543316000003
  • Figure 2024543316000001
    Figure 2024543316000001
  • Figure 2024543316000002
    Figure 2024543316000002
Patent Text Reader

Abstract

The present application discloses a secondary battery and an electric device, the secondary battery comprising a positive electrode sheet, a separator, an electrolyte, and a negative electrode sheet, the negative electrode sheet comprising a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, where the non-faradaic charge of the negative electrode sheet is QC, which satisfies 0.05≦Q≦2.5, where Q=Cdl×ΔU, where Cdl nF is the non-faradaic capacity of the negative electrode sheet, and ΔUV is the potential range of the negative electrode active material layer. The negative electrode sheet of the present application is used in high energy density secondary battery products, which can better balance high charge / discharge characteristics and reduce interface degradation phenomena such as lithium precipitation caused by poor electrolyte infiltration, effectively reduce sheet polarization phenomena, improve battery consistency, prolong cycle life, and have excellent charge / discharge performance and dynamic performance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to a Chinese patent application filed with the China Patent Office on September 26, 2022, application number 202211175100.9, entitled "Secondary Battery and Electrochemical Device," the entire contents of which are incorporated herein by reference.

[0002] This application relates to the field of battery technology, and in particular to secondary batteries and electrochemical devices. [Background technology]

[0003] With the rapid development of the new energy industry, there is an urgent demand for secondary batteries with higher capacity, better durability, and stronger driving performance. The negative electrode material is an important part of the secondary battery, and improving the cycle life while ensuring the high capacity of the negative electrode material is also one of the effective means to solve the above problems. Therefore, the problem of how to improve the cycle performance and cycle life of secondary batteries is a problem that needs to be solved. Summary of the Invention [Problem to be solved by the invention]

[0004] The present application aims to provide a secondary battery and an electrochemical device, and to improve the cycle performance and cycle life of the battery. [Means for solving the problem]

[0005] In a first aspect, the present application provides a secondary battery, the secondary battery including a positive electrode sheet, a separator, an electrolyte, and a negative electrode sheet; the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, Here, the non-Faraday charge of the negative electrode sheet is QC, which satisfies 0.05≦Q≦2.5, and Q=Cdl×ΔU; Cdl nF is the non-faradaic capacity of the negative electrode sheet; ΔUV is the potential range of the negative electrode active material layer.

[0006] In some embodiments, the Cdl satisfies 0.5≦Cdl≦5, and the ΔU satisfies 0.1≦ΔU≦0.5.

[0007] In some embodiments, the negative electrode active material layer comprises one or more of synthetic graphite, natural graphite, soft carbon, hard carbon, amorphous carbon, carbon fibers, carbon nanotubes, or mesocarbon microspheres.

[0008] In some embodiments, the contact angle of the negative electrode active material layer with respect to the surface of the electrolyte is θ, and the θ satisfies 10°≦θ≦40°.

[0009] In some embodiments, the negative electrode active material layer has a resistance of R mΩ, where 5≦R≦20.

[0010] In some embodiments, the negative electrode active material layer has an OI value of 2-15.

[0011] In some embodiments, the negative electrode active material layer comprises a negative electrode active material, the negative electrode active material having a fine powder content of 0-80% by number and a coarse powder content of 0-60% by number.

[0012] The fine powder refers to negative electrode active material particles having a particle size of 2.2 μm or less, and the coarse powder refers to negative electrode active material particles having a particle size of 35 μm or more.

[0013] In some embodiments, the negative electrode active material has a fine powder content of 0-40% by quantity.

[0014] The negative electrode active material has a quantitative content of coarse powder of 0 to 30%.

[0015] In some embodiments, the electrolyte comprises a lithium salt additive, the lithium salt additive comprising one or more of lithium tetrafluoroborate, lithium bis(oxalato)borate, lithium difluorophosphate, lithium bis(trifluoromethanesulfonimide), and lithium bis(fluorosulfonyl)imide.

[0016] In some embodiments, the electrolyte contains a lithium salt additive in a content of X, where 0.1%≦X≦2%.

[0017] In some embodiments, the negative electrode active material layer includes a protective film layer, the protective film layer having a thickness of H nm, and 0.4≦10X·H+Q≦36.

[0018] In some embodiments, the thickness H of the overcoat layer satisfies 5≦H≦180.

[0019] In a second aspect, the electrochemical device according to the present application includes the secondary battery described above. Effect of the Invention

[0020] Compared with the prior art, the secondary battery of the present application limits the amount of non-Faraday charge of the negative electrode sheet and controls it to be within the range of 0.05C to 2.5C, and also limits the amount of non-Faraday charge of the negative electrode sheet to satisfy Q=Cdl×ΔU, so that in high energy density battery products, the negative electrode sheet can better balance high multiplication rate and charge / discharge characteristics, avoid interface deterioration phenomena such as lithium precipitation due to poor electrolyte infiltration, and effectively reduce sheet polarization phenomenon, resulting in better consistency of the manufactured secondary battery, longer cycle life, and excellent multiplication performance and dynamic performance. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a fitting curve showing a scan rate-current scatter diagram of the negative electrode sheet produced in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present application provides a secondary battery and an electrochemical device, and in order to make the objectives, technical solutions and effects of the present application clearer and more precise, the present application will be described in more detail below by way of examples with reference to the drawings. It should be understood that the specific examples described in the present specification are merely for the purpose of illustrating the present application, and are not intended to limit the present application.

[0023] With the development of new energy industry, the demand for secondary batteries is increasing. When secondary batteries, such as lithium ion batteries, are applied to electric vehicles, it is necessary to extend the driving distance and service life as much as possible. The secondary batteries used in electric vehicles will radiate heat during charging and discharging, which will lead to accelerated aging of the internal chemical system. Therefore, the secondary batteries will cause deterioration of battery performance during long-term cycles and storage, which is mainly manifested by the deterioration of capacity, increase in internal resistance and decrease in power performance of the secondary batteries.

[0024] In order to solve the above problems, the present application provides a negative electrode sheet having a specific non-Faraday charge, which allows the negative electrode sheet to better balance high multiplication rate and charge / discharge characteristics in a high energy density battery product, reduces the occurrence of interface deterioration phenomena such as lithium deposition due to poor electrolyte infiltration, effectively reduces sheet polarization phenomenon, and improves the consistency of the manufactured secondary battery, prolongs the cycle life, and provides excellent multiplication performance and dynamic performance.

[0025] In an embodiment of the present application, the present application provides a secondary battery, which includes the following positive electrode sheet, a separator, an electrolyte, and a negative electrode sheet.

[0026] I, negative electrode sheet

[0027] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer including a negative electrode active material.

[0028] 1. Non-Faraday charge

[0029] One of the features of the secondary battery in this application is that the non-faradaic charge of the negative electrode sheet is QC, which satisfies 0.05≦Q≦2.5, where Q=Cdl×ΔU, where Cdl nF is the non-faradaic capacity of the negative electrode sheet, and ΔUV is the potential range of the negative electrode active material layer.

[0030] Here, the non-Faraday charge of the negative electrode sheet is QC, and satisfies 0.05≦Q≦2.5. For example, the non-Faraday charge of the negative electrode sheet QC may be any one of 0.05C, 0.07C, 0.09C, 0.15C, 0.25C, 0.53C, 0.78C, 0.85C, 0.97C, 1.2C, 1.5C, 1.8C, 2.0C, 2.2C, and 2.5C, or a range consisting of any two of the numbers. Note that the specific numerical value of the non-Faraday charge Q is merely an example, and any value within the range of 0.05C to 2.5C is within the scope of protection of the present application.

[0031] As can be understood, the electrochemical reactions of secondary batteries are mainly surface reactions that occur on the electrode surface, and the reactions are as follows: (1) mass transfer reaction, ions are transferred to the electrode surface; (2) non-faradaic reaction, no charge transfer occurs through the electrode interface, and ions are physically adsorbed and desorbed on the active material surface to store and release charges; (3) faradaic reaction, the oxidation state of the active material changes, and charges are transferred inside the active material. The non-faradaic capacity value (Cdl) can represent the number of active sites of the negative electrode active material in the negative electrode sheet, and the non-faradaic capacity value can be evaluated by the curves of the linear scanning voltammogram (LSV) at different scanning speeds that are in the non-faradaic reaction range, that is, the current density changes according to the change in the scanning speed. Specifically, the non-faradaic capacity value (Cdl) can affect the number of electrochemical active sites, affect the contact between the material and the electrolyte, affect the ion-electron conduction speed, lower the charge transfer resistance, and thus affect the multiplication performance.

[0032] In the present application, the non-Faraday charge of the negative electrode sheet is limited within the above range, and the non-Faraday charge of the negative electrode sheet is limited to satisfy Q=Cdl×ΔU, so that the negative electrode sheet can better balance high multiplication and charge / discharge characteristics in a high energy density secondary battery product, reduce interface deterioration phenomena such as lithium precipitation due to poor electrolyte infiltration, effectively reduce sheet polarization phenomenon, improve the consistency of the manufactured secondary battery, prolong cycle life, and have excellent multiplication performance and dynamic performance. The non-Faraday charge of the negative electrode can be adjusted by the form of the negative electrode active material, the compressed density of the negative electrode sheet, the OI value of the negative electrode sheet, the configuration of the negative electrode, the slurry process of the negative electrode, etc. The control of the non-Faraday charge of the negative electrode is not limited to the above method, and it is sufficient to control the negative electrode sheet within the above range.

[0033] In the embodiment of the present application, the non-Faraday capacitance Cdl nF of the negative electrode sheet satisfies 0.5≦Cdl≦5. For example, the non-Faraday capacitance (Cdl nF) of the negative electrode sheet may be any of 0.5nF, 1nF, 1.5nF, 2nF, 2.5nF, 3nF, 3.5nF, 4nF, 4.5nF, and 5nF, or a range consisting of any two numbers thereamong. The specific value of the non-Faraday capacitance Cdl nF is merely an example, and any value within the range of 0.5nF to 5nF is within the scope of protection of the present application. In the present application, by controlling the non-Faraday capacitance Cdl nF of the negative electrode sheet within the range of 0.5nF to 5nF, it is advantageous for the contact between the material and the electrolyte, the ion-electron conduction speed is accelerated, the charge transfer resistance is reduced, and the magnification performance can be effectively improved.

[0034] In the embodiment of the present application, the non-Faraday capacitance Cdl nF of the negative electrode sheet satisfies 1.3≦Cdl≦4.7.

[0035] In the embodiment of the present application, the non-Faraday capacity Cdl nF of the negative electrode sheet satisfies 1.4≦Cdl≦4.3. When the non-Faraday capacity of the negative electrode sheet is in the above range, the number of active sites of the negative electrode active material in the negative electrode sheet is in a more appropriate range, which allows the secondary battery to have better overall performance.

[0036] In the embodiment of the present application, the potential range ΔUV of the negative electrode active material layer satisfies 0.1≦ΔU≦0.5. For example, the potential range ΔUV of the negative electrode active material layer may be any of 0.1V, 0.15V, 0.2V, 0.25V, 0.3V, 0.35V, 0.4V, 0.45V, and 0.5V, or a range consisting of any two numbers among them. Note that the specific value of the potential interval ΔUV is merely an example, and any value within the range of 0.1V to 0.5V is within the protection range of the present application. In the present application, the potential range ΔUV of the negative electrode active material layer is controlled to the range of 0.1V to 0.5V, which is favorable for the contact between the material and the electrolyte, accelerates the conduction speed of ions and electrons, reduces the charge transfer resistance, and effectively improves the efficiency performance.

[0037] 2, negative electrode active material layer

[0038] The negative electrode active material layer may be a single layer or a multi-layer, and each of the multiple negative electrode active material layers may contain the same or different negative electrode active materials. In the present embodiment, the chargeable capacity of the negative electrode active material is greater than the discharge capacity of the positive electrode active material to prevent lithium metal from being deposited on the negative electrode sheet during charging.

[0039] In the present embodiment, the negative active material layer includes, but is not limited to, artificial graphite, natural graphite, soft carbon, hard carbon, amorphous carbon, carbon fiber, carbon nanotubes, and mesocarbon microspheres. The negative active materials may be used alone or in any combination.

[0040] In the embodiment of the present application, the negative electrode active material layer includes, but is not limited to, petroleum coke and acicular coke, which have a relatively small microcrystalline structure, a relatively large damascene structure, and a relatively small streamlined structure. The negative electrode active materials may be used alone or in any combination. By adopting materials with the above structural characteristics, the negative electrode active material layer provides the negative electrode sheet with excellent isotropy and good magnification performance, and ensures relatively low resistance and material stability during cycling.

[0041] The microcrystalline structure, the damascene structure, and the streamlined structure of the negative electrode active material can be seen by observing the negative electrode active material using a scanning electron microscope (SEM).

[0042] In the embodiment of the present application, the surface of the negative electrode active material may have a coating layer, which may be a single layer or a double layer. For example, the surface of the negative electrode active material may be coated with soft carbon, which can accelerate the electron conduction, thereby increasing the conductivity of the material and protecting the graphite itself. By coating the surface of the negative electrode active material with an inorganic material, it is possible to promote the formation of a thin and dense solid electrolyte interface (SEI) film layer, provide a stable chemical and electrochemical reaction interface, and improve the long cycle performance of the material.

[0043] As can be seen, by adopting a two-layer coating, the present application can effectively suppress side reactions in secondary batteries while maintaining the integrity of graphite, and by adjusting the coating materials and coating processes of the inner and outer layers, the electronic and ionic conductivity of the material can be effectively controlled, thereby effectively controlling the rate of non-Faradic processes in the electrode and, therefore, the performance of the battery.

[0044] The coating layer of the negative electrode active material layer can be seen by observing it using a transmission electron microscope (TEM).

[0045] In the present embodiment, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte solution satisfies 10°≦θ≦40°. For example, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte solution may be any one of 10°, 15°, 20°, 25°, 30°, 35°, and 40°, or may be within a range consisting of any two of these numbers.

[0046] The contact angle of the negative active material layer to the surface of the electrolyte can reflect the surface properties of the negative active material layer. When the wetting contact angle between the negative electrode sheet and the electrolyte is small, the electrolyte is quickly adsorbed after being dropped onto the negative electrode sheet, which indicates that the compatibility between the negative electrode sheet and the electrolyte is better. Therefore, the electrolyte can be in intimate contact with the surface active points of the negative electrode sheet, and the diffusion and transmission efficiency of lithium ions in the electrolyte to the graphite surface can be improved, which is the advantage of excellent dynamic performance.

[0047] In the present application, the contact angle of the negative electrode active material layer with respect to the surface of the electrolyte is controlled within the above range. When the contact angle of the negative electrode active material layer with respect to the surface of the electrolyte is within the above range, the defects of pinholes and pits in the negative electrode sheet are reduced, and the greater the tendency of the electrolyte to spread on the negative electrode sheet, the greater the wettability and the better the compatibility with the electrolyte, so that lithium ions are more easily transferred in the negative electrode sheet, which is advantageous for reducing the internal resistance of the battery, and reduces defects such as lithium precipitation due to poor infiltration, an increase in by-products, and poor dynamic performance, thereby improving the multiplication performance and cycle life. On the other hand, the standing time after injection of the secondary battery is shortened, the infiltration speed of the electrolyte into the negative electrode sheet is improved, production efficiency and good product rate are improved, the state of the sheet interface of the manufactured battery is more uniform, the current density at the interface during the charge and discharge process is more uniform, and the dynamic performance and cycle life of the battery are improved.

[0048] In the embodiment of the present application, the contact angle of the negative electrode active material layer with respect to the surface of the electrolyte is θ, and the θ satisfies 12°≦θ≦35°. When the contact angle of the negative electrode active material layer with respect to the surface of the electrolyte is in the above range, the defects on the surface of the negative electrode sheet are further reduced, the battery has higher production efficiency and good yield rate, and the overall performance of the battery is further improved.

[0049] In the embodiment of the present application, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte can be measured using an optical contact angle meter in accordance with the nano-thin film contact angle measurement method of GB / T 30447-2013.

[0050] Here, the electrolyte contains lithium hexafluorophosphate, which is a lithium salt, cyclic carbonate and chain carbonate, which are organic solvents, and an electrolyte additive.

[0051] In the embodiment of the present application, the resistance of the negative electrode active material layer is R mΩ, and satisfies 5≦R≦20. For example, the resistance R mΩ of the negative electrode active material layer may be any one of 5 mΩ, 7.5 mΩ, 10 mΩ, 12.5 mΩ, 15 mΩ, 17.5 mΩ, and 20 mΩ, or may be within a range consisting of any two of these numbers.

[0052] As can be seen, factors affecting the resistance of the negative electrode sheet of the secondary battery include the interface state between the current collector and the active material layer, the distribution state of the conductive agent, and the contact state between the particles, and the like, and the resistance of the active material layer of the negative electrode sheet can reflect the state and performance of the material in the negative electrode sheet. The relatively low resistance of the active material layer can be obtained by adjusting parameters such as the interface state between the negative electrode current collector and the negative electrode active material layer, the distribution state of the conductive agent, and the contact state between the particles. The negative electrode sheet having a resistance value in the above range has a relatively high electron transfer efficiency, and the relatively low resistance between the current collector and the electrode active material layer can effectively reduce the DC internal resistance of the battery and improve the power performance of the battery, making the battery less likely to cause phenomena such as large polarization and lithium precipitation during long-term cycling, and effectively improving the cycle performance of the battery. Meanwhile, the resistance of the negative electrode active material layer is reduced, shortening the lithium ion transfer path.

[0053] In the embodiment of the present application, the resistance of the negative electrode active material layer is R mΩ, and satisfies 5≦R≦18. When R mΩ is in the above range, the battery has better power performance and cycle performance.

[0054] In the embodiment of the present application, the resistance of the negative electrode active material layer is R mΩ, and satisfies 5≦R≦12. When R mΩ is in the above range, the interface state between the negative electrode current collector and the negative electrode active material layer, the distribution state of the conductive agent, and the contact state between the particles are better, and the battery has better overall performance.

[0055] In the examples of the present application, the test method for the resistance R mΩ of the negative electrode active material layer is as follows.

[0056] The negative electrode sheet, on both sides of which the negative electrode active material layers are arranged, is placed on a substrate with an area of ​​1540.25 mm 2 The negative electrode sheet is cut into a circular sheet having a length of 10 mm, and the cut negative electrode sheet is placed at the center of the probe of a sheet resistance measuring instrument, and then the negative electrode sheet is tested using the sheet resistance measuring instrument to obtain the resistance of the negative electrode active material layer of the measured negative electrode sheet. The selected 10 negative electrode sheet samples are each measured using the sheet resistance measuring instrument, and the average resistance of the negative electrode active material layer of the obtained 10 measured negative electrode sheets is calculated to obtain the resistance of the negative electrode active material layer.

[0057] In the present embodiment, the OI value of the negative electrode active material layer is 2 to 15. For example, the OI value of the negative electrode active material layer may be any one of 2, 4, 6, 8, 10, 12, and 15, or a range consisting of any two of these numbers. Note that the specific numerical values ​​of the OI value are merely examples, and any value within the range of 2 to 15 falls within the scope of protection of the present application.

[0058] Here, the OI value of the negative electrode active material layer refers to the ratio of the intensities of the X-ray diffraction peaks of the negative electrode active material layer on the 004 crystal plane and the 110 crystal plane.

[0059] It can be seen that the OI value (C004 / C110) of the negative electrode sheet can affect the transport path of lithium ions. During the lithium absorption process, lithium ions enter the interlayer space of the graphite negative electrode material from the edge surface, undergo solid-state diffusion between the layers, and complete the lithium absorption process, with the relatively small graphite edge surface with isotropic microcrystalline structure being exposed on the sheet surface.

[0060] Therefore, when the compression density of the negative electrode sheet is consistent with the coating surface density, the OI value of the negative electrode sheet within the above range can affect the transition path, transition rate and electrochemical reaction kinetics of lithium ions, thus further realizing the high multiplier discharge performance of lithium ions and ensuring a relatively low impedance during the cycle process.In addition, when the OI value of the negative electrode sheet is within the above range, it can inhibit the expansion between the graphite layers, ensure a relatively high stability of the material structure during the cycle process, improve the cycle performance, and thus improve the multiplier charge capacity to achieve the purpose of optimizing the cycle.

[0061] In the embodiments of the present application, adjustment of the OI value of the negative electrode active material is more advantageous in controlling the sheet OI value. The OI value of the negative electrode active material can be changed by adjusting physicochemical properties such as the particle size and powder resistance of the negative electrode active material, and the OI value of the negative electrode sheet can be changed by adjusting factors such as the proportion of the conductive agent, the stirring process, the rolling process, etc.

[0062] In the present application, by controlling the OI value of the negative electrode active material layer within the above range, the transition path of lithium ions is shortened, the high-speed transition of lithium ions is realized, the electrochemical reaction kinetics is accelerated, and the high multiplier discharge performance of lithium ions is further realized, and the low impedance is ensured during the cycle process;Meanwhile, the expansion between graphite layers is suppressed, and the relatively high stability of the material structure during the cycle process is ensured, so that the cycle performance is improved, and the multiplier charge ability is improved, thereby achieving the purpose of optimizing the cycle.

[0063] In the embodiment of the present application, the magnitude of the OI value of the negative electrode active material layer is 2 to 10. When the OI value of the negative electrode active material layer is within the above range, the battery has better overall performance.

[0064] In the present embodiment, the negative active material layer includes a negative active material, which includes, but is not limited to, artificial graphite, natural graphite, soft carbon, amorphous carbon, carbon fiber, carbon nanotubes, and mesocarbon microspheres. The negative active materials may be used alone or in any combination.

[0065] In the present embodiment, the negative electrode active material layer includes, but is not limited to, petroleum coke and acicular coke having a relatively small microcrystalline structure, a relatively large damascene structure, and a relatively small streamlined structure. The negative electrode active materials may be used alone or in any combination.

[0066] The quantity content of the fine powder in the negative electrode active material is 0 to 80%. For example, the quantity content of the fine powder in the negative electrode active material may be any one of 0, 10%, 20%, 30%, 40%, 50%, 60%, 70%, and 80%, or a range consisting of any two of the numbers. Note that the specific numerical value of the quantity content of the fine powder is merely an example, and any value within the range of 0 to 80% is within the scope of protection of the present application.

[0067] The quantitative content of the coarse powder in the negative electrode active material is 0 to 80%. For example, the quantitative content of the coarse powder in the negative electrode active material may be any of 0, 10%, 20%, 30%, 40%, 50%, and 60%, or a range consisting of any two of these numbers. Note that the specific numerical value of the quantitative content of the coarse powder is merely an example, and any value within the range of 0 to 60% is within the scope of protection of the present application.

[0068] Here, the fine powder refers to negative electrode active material particles having a particle size of 2.2 μm or less, and the coarse powder refers to negative electrode active material particles having a particle size of 35 μm or more.

[0069] In the embodiments of the present application, the quantity content of the fine powder of the negative electrode active material is 0 to 40%, and for example, the quantity content of the fine powder of the negative electrode active material may be any one of 0, 10%, 15%, 20%, 25%, 30%, 35%, and 40%, or a range consisting of any two of these numbers.

[0070] The quantitative content of the coarse powder in the negative electrode active material is 0 to 30%. For example, the quantitative content of the coarse powder in the negative electrode active material may be any one of 0, 10%, 15%, 20%, 25%, and 30%, or a range consisting of any two of these numbers.

[0071] As can be seen, when the quantity content of the fine powder of the negative electrode active material is small, the negative electrode active material has a small number of negative electrode active material particles with a particle size of 2.2 μm or less, and when the quantity content of the coarse powder of the negative electrode active material is small, the negative electrode active material has a small number of negative electrode active material particles with a particle size of 35 μm or more. By limiting both, the gaps caused by the excessively large negative electrode active material particles are prevented from being filled with the excessively small negative electrode active material particles, thereby widening the gaps between the negative electrode active material particles, which is favorable for the Faradaic reaction in the battery, the non-Faraday capacity Cdl of the negative electrode sheet is increased, the number of electrochemically active points is increased, which is favorable for the contact between the material and the electrolyte, the conduction speed of ions and electrons is accelerated, the charge transfer resistance is reduced, and the multiplication performance of the secondary battery can be effectively improved.

[0072] As can be seen, in the present application, the quantitative content of the fine powder of the negative electrode active material is controlled to a range of 0 to 40%, and the quantitative content of the coarse powder of the negative electrode active material is controlled to a range of 0 to 30%, and by limiting both of them together, the width of the particle size distribution of the negative electrode active material can be effectively restricted, the particle size distribution of the negative electrode active material becomes more concentrated and the morphology becomes more regular, excellent isotropy of the negative electrode active material is ensured, electronic conductivity and ion transfer of the negative electrode active material are improved, and the speed of the non-Faraday process of the sheet can be effectively adjusted and controlled.

[0073] In the examples of the present application, a particle size distribution test of the negative electrode active material can be performed using a laser particle sizer for the quantitative content of fine powder in the negative electrode active material and the quantitative content of coarse powder in the negative electrode active material. By calculating the peak areas corresponding to the fine powder and the coarse powder, specific values ​​of the quantitative content of fine powder in the negative electrode active material and the quantitative content of coarse powder in the negative electrode active material can be obtained.

[0074] In the embodiment of the present application, the negative electrode active material layer 120 includes a protective film layer 130, and the thickness of the protective film layer 130 is H nm, and satisfies 5≦H≦180. For example, the thickness H nm of the protective film layer 130 may be any of 5 nm, 30 nm, 60 nm, 90 nm, 120 nm, 150 nm, and 160 nm, or a range consisting of any two numbers among them. Note that the specific numerical value of the thickness H nm is merely an example, and any value within the range of 5 nm to 180 nm is within the protection range of the present application. When the thickness of the protective film layer is within this range, the negative electrode active material can be protected better while the influence of, for example, an increase in internal resistance caused by the protective film layer can be reduced.

[0075] The thickness of the overcoat layer can be obtained by employing TEM testing.

[0076] 3, negative electrode current collector

[0077] In embodiments herein, the negative current collector includes, but is not limited to, a metal foil, a metal cylinder, a roll of metal tape, a metal sheet, a metal film, a metal sheet mesh, a stamping metal, a metal foam, and the like. In some embodiments, the negative current collector is a metal foil. In some embodiments, the negative current collector is a copper foil. As used herein, the term "copper foil" includes copper alloy foils.

[0078] 4. Testing and calculation of non-Faraday charge of negative electrode sheet

[0079] In an embodiment of the present application, the present application further provides a method for testing and calculating the non-Faraday charge amount of a negative electrode sheet, for testing and calculating the non-Faraday charge amount of any of the above-mentioned negative electrode sheets, specifically including the following steps:

[0080] S1, assemble the negative electrode sheet into a button battery, perform a cyclic voltammogram (CV) test on the button battery, and obtain the potential range UV of the button battery.

[0081] S2, select a potential range U of the button battery in step S1, perform a linear scanning voltammogram (LSV) test on the button battery, detect a scanning rate-voltage graph and a voltage-current graph, and obtain a potential range ΔUV of the negative electrode active material layer based on the voltage-current graph, where the scanning direction is from low potential to high potential.

[0082] S3, based on step S2, detect the scanning speed-current scatter diagram, and obtain the non-Faraday capacitance value Cdl of the negative electrode sheet based on the scanning speed-current scatter diagram.

[0083] In step S4, the non-Fradei charge Q is calculated based on the potential range ΔU and the non-Fradei capacitance value Cdl obtained in steps S2 and S3 by the formula Q=Cdl×ΔU.

[0084] In the embodiment of the present application, the step of assembling the negative electrode sheet into a button battery in step S1 specifically includes disassembling the secondary battery in a glove box or a drying room to obtain a negative electrode overhang area sheet, immersing it in a dimethyl carbonate (DMC) solution, cutting it, and then assembling it with a metallic lithium sheet into a button battery. A negative electrode sheet that has not been assembled into a battery may also be used.

[0085] Here, the overhang region refers to the portion of the negative electrode sheet that protrudes from the positive electrode sheet in the longitudinal and transverse directions.

[0086] The button battery in step S1 includes a positive electrode housing, a negative electrode sheet, a separator, an electrolyte, a lithium sheet, nickel foam, a gasket, and a negative electrode housing.

[0087] In the embodiment of the present application, the potential range UV of the button battery in step S1 satisfies 2.5≦U≦3. For example, the potential range UV of the button battery may be any one of 2.5V, 2.6V, 2.7V, 2.8V, 2.9V, and 3V, or a range consisting of any two of these numbers. Note that the specific numerical values ​​of the potential range UV are merely examples, and any value within the range of 2.5V to 3V falls within the protection scope of the present application.

[0088] In the embodiment of the present application, the scanning rate in the cyclic Voltammogram method in step S1 is V1, which satisfies 0.1 mV / s≦V1≦1 mV / s. For example, the scanning rate V1 may be any one of 0.1 mV / s, 0.2 mV / s, 0.3 mV / s, 0.4 mV / s, 0.5 mV / s, 0.6 mV / s, 0.7 mV / s, 0.8 mV / s, 0.9 mV / s, and 1 mV / s, or a range consisting of any two numbers among them. The specific numerical value of the scanning rate V1 is merely an example, and any value within the range of 0.1 mV / s to 1 mV / s is within the scope of protection of the present application.

[0089] As can be understood, the cyclic voltammogram (CV) method in the testing and calculation method of the non-Faraday charge of the negative electrode sheet provided in this application has the advantages of simple manufacture, simple operation, accurate and stable test data, safety and environmental friendliness, etc., and has practical application value.

[0090] In the embodiment of the present application, the potential range ΔUV of the negative electrode active material layer in step S2 satisfies 0.1≦ΔU≦0.5. For example, the potential range ΔUV of the negative electrode active material layer may be any one of 0.1V, 0.15V, 0.2V, 0.25V, 0.3V, 0.35V, 0.4V, 0.45V, and 0.5V, or a range consisting of any two numbers among them. Note that the specific value of this potential interval ΔUV is merely an example, and any value within the range of 0.1V to 0.5V falls within the protection scope of the present application.

[0091] In the embodiment of the present application, the scan rate V2 in the linear scanning voltammogram method in step S2 satisfies 0.05 mV / s ≦ V2 ≦ 5 mV / s. For example, the scan rate V2 may be any one of 0.05 mV / s, 0.5 mV / s, 1 mV / s, 1.5 mV / s, 2 mV / s, 2.5 mV / s, 3 mV / s, 3.5 mV / s, 4 mV / s, 4.5 mV / s, and 5 mV / s, or a range consisting of any two numbers among them. The specific numerical value of the scan rate V2 is merely an example, and any value within the range of 0.05 mV / s to 5 mV / s is within the protection scope of the present application.

[0092] In the embodiment of the present application, in step S3, the step of detecting the scanning speed-current scatter diagram based on step S2, and obtaining the non-Faraday capacitance value Cdl of the negative electrode sheet based on the scanning speed-current scatter diagram includes the following steps:

[0093] When performing a linear scan voltammogram test on the button battery, multiple scan rates are selected, and multiple median voltage values ​​are obtained based on the scan rate-voltage graph detected in step S2, where each scan rate corresponds to a corresponding median voltage value.

[0094] A plurality of current values ​​are obtained based on the obtained plurality of median voltage values ​​and a voltage-current graph, where each current value corresponds to a corresponding median voltage value.

[0095] According to the correspondence relationship between each scanning speed and the corresponding median voltage, and the correspondence relationship between each current value and the corresponding median voltage, a mapping relationship between the scanning speed and the current value was established, and thus a scanning speed-current scatter diagram was obtained.

[0096] Based on the scan rate-current scatter plot, a linear function is obtained by fitting, where the slope of the linear function is the non-faradaic capacitance value Cdl of the negative sheet.

[0097] 5. Manufacturing of negative electrode sheets

[0098] The negative electrode sheet in the secondary battery of the present application can be manufactured by any known method, for example, by adding a conductive agent, a binder, an additive, a solvent, etc. to a negative electrode active material to prepare a slurry, coating the slurry on a negative electrode current collector, drying it, and then rolling it to form an electrode.

[0099] II, electrolyte

[0100] The electrolytic solution used in the secondary battery of the present application contains an electrolyte and a solvent that dissolves the electrolyte.

[0101] 1. Additives

[0102] In the embodiment of the present application, the electrolyte includes, but is not limited to, lithium salt additives, including, but not limited to, lithium tetrafluoroborate (abbreviated as LiBF4), lithium bis(oxalato)borate (abbreviated as LiBOB), lithium difluorophosphate (abbreviated as LiPO2F2), lithium bis(trifluoromethanesulfonimide) (abbreviated as LiTFSI), and lithium bis(fluorosulfonyl)imide (abbreviated as LiFSI). The above lithium salt additives may be used alone or in any combination.

[0103] In the embodiment of the present application, the content of the lithium salt additive in the electrolyte is X based on the mass of the electrolyte, and satisfies 0.1%≦X≦2%. For example, the content X of the lithium salt additive in the electrolyte may be any of 0.1%, 0.4%, 0.7%, 1%, 1.3%, 1.6%, and 2%, or a range consisting of any two of these numbers. Note that the specific value of the content X is merely an example, and any value within the range of 0.1% to 2% is within the scope of protection of the present application.

[0104] In the embodiment of the present application, the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer, and the non-Faraday charge Q of the negative electrode sheet satisfy 0.4≦10X·H+Q≦36. When the above ranges are satisfied, the battery has better overall performance.

[0105] 2, electrolytes

[0106] In the present application, the electrolyte may be any known material that can be used as an electrolyte as long as it does not impair the effects of the present application, and is not particularly limited. In the case of a secondary battery, a lithium salt is usually used. In the embodiment of the present application, the electrolyte includes, but is not limited to, LiPF6.

[0107] On the other hand, in the present application, the content of the electrolyte is not particularly limited as long as it does not impair the effects of the present application. For example, the content of the electrolyte may be 0.8 mol / L to 2.2 mol / L.

[0108] 3. Solvent

[0109] In the present application, the solvent is not particularly limited and any known substance usable as a solvent may be used as long as it does not impair the effect of the present application.

[0110] In the present embodiment, the solvent includes, but is not limited to, ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC), dimethyl carbonate (DMC), butylene carbonate (BC), and methyl vinyl carbonate (MEC). The above solvents may be used alone or in any combination.

[0111] III. Positive electrode sheet

[0112] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector.

[0113] 1.Cathode active material layer

[0114] The positive electrode active material layer may be a single layer or a multilayer, and each of the multiple negative electrode active material layers may contain the same or different positive electrode active materials. The positive electrode active material is any material that can reversibly absorb and release metal ions, such as lithium ions.

[0115] positive electrode active material

[0116] The positive electrode active material layer may include, but is not limited to, positive electrode active materials including lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate (LFP), and ternary materials.

[0117] In the present embodiment, the ternary material includes, but is not limited to, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminate.

[0118] In an embodiment of the present application, the positive electrode active material includes lithium nickel cobalt manganese oxide, in which the mole of nickel, cobalt, and manganese in the lithium nickel cobalt manganese oxide is 1, and the content of nickel is 0.5 or more.

[0119] In an embodiment of the present application, the positive electrode active material includes lithium nickel cobalt manganese oxide, in which the molar ratio of nickel, cobalt, and manganese in the lithium nickel cobalt manganese oxide is 1, and the content of nickel is 0.85 or less.

[0120] In the present embodiment, the positive electrode active material includes at least one of NCM523, NCM622, or NCM811.

[0121] In the embodiment of the present application, the positive electrode active material further includes a doping element, and the doping element may include elements such as aluminum, magnesium, titanium, and zirconium, as long as the doping element can further stabilize the structure of the positive electrode active material.

[0122] In the embodiment of the present application, the positive electrode active material may further include a coating element, which may include elements such as aluminum, magnesium, titanium, and zirconium, as long as the coating element can further stabilize the structure of the positive electrode active material.

[0123] Positive electrode conductive material

[0124] In the present application, the type of the positive electrode conductive agent is not particularly limited, and any known substance that can be used as a conductive material can be used as long as it does not impair the effects of the present application.

[0125] In the present embodiment, the positive electrode conductive agent includes, but is not limited to, graphite such as natural graphite and artificial graphite, carbon black such as acetylene black, amorphous carbon such as needle coke, carbon nanotubes, graphene, etc. The above positive electrode conductive agents may be used alone or in any combination.

[0126] Positive electrode binder

[0127] The type of the positive electrode binder is not particularly limited as long as it does not impair the effects of the present invention. Specifically, in the case of a coating method, the positive electrode binder may be a material that is soluble or dispersible in the liquid medium used in the manufacture of the electrode.

[0128] In the present embodiment, the positive electrode binder may be a positive electrode conductive material such as polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, or nitrocellulose, either alone or in combination.

[0129] 2, Positive electrode current collector

[0130] In the present application, the type of the positive electrode current collector is not particularly limited, and any known material that can be used as a positive electrode current collector can be used as long as it does not impair the effects of the present application.

[0131] In the present embodiment, the positive electrode current collector includes, but is not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, tantalum, etc., and carbon materials such as carbon cloth, carbon paper, etc. In one embodiment, the positive electrode current collector is a metal material. In one embodiment, the positive electrode current collector is an aluminum foil.

[0132] 3. Manufacturing of positive electrode sheets

[0133] The positive electrode sheet in the secondary battery of the present application can be manufactured by any known method. For example, a conductive agent, a binder, a solvent, etc. are added to a positive electrode active material to prepare a slurry, and the slurry is coated on a positive electrode current collector, dried, and then rolled to form an electrode. A sheet-shaped electrode may be formed by rolling the negative electrode active material, or a particle electrode may be formed by compression molding.

[0134] IV, separator

[0135] In order to prevent short circuits, a separator is usually disposed between the positive electrode and the negative electrode, and in this case, the electrolyte of the present application is usually used by permeating the separator.

[0136] In the present application, the material, shape, thickness, porosity and average pore size of the separator are not particularly limited as long as they do not impair the effects of the present application.

[0137] The present application further provides an electrochemical device, which includes the secondary battery described above.

[0138] The electrochemical device may be a battery pack or a battery module.

[0139] The present application further provides an electricity-using device, which includes an electric vehicle, a storage battery, and the like.

[0140] Hereinafter, the manufacture of a lithium ion battery will be described in conjunction with specific examples using a lithium ion battery as an example. However, those skilled in the art should understand that the manufacturing methods described herein are merely examples, and other suitable manufacturing methods are within the scope of the present application.

[0141] Hereinafter, performance evaluation of the lithium ion battery of the present invention will be described using examples and comparative examples.

[0142] Example 1

[0143] 1. Lithium-ion battery manufacturing

[0144] 1. Manufacturing of positive electrode sheets

[0145] The positive electrode active material, the positive electrode conductive agent, and the positive electrode binder are mixed in a mass ratio of 96:2:2, and then a solvent is added to prepare a positive electrode slurry. The prepared positive electrode slurry is uniformly coated on both sides of an aluminum foil of a positive electrode current collector, which is then dried at 120°C, rolled and cut to obtain a positive electrode sheet.

[0146] Here, the positive electrode active material is NCM622, the positive electrode conductive agent is carbon black, the positive electrode binder is polyvinylidene fluoride (PVDF), and the solvent is N-methylpyrrolidone (NMP).

[0147] 2. Manufacturing of negative electrode sheets

[0148] The raw petroleum coke, which has a volatile content of 15% and an ash content of 0.3%, is crushed and premixed in a roll mill, and the particle size of the crushed raw petroleum coke is 10 μm.

[0149] The milled product is subjected to high-temperature graphitization treatment in a protective atmosphere, where the temperature is 2800-3200°C, the maximum temperature is maintained for 36 hours, and the protective atmosphere is argon gas.

[0150] In the continuous shaping system, the product is polished and shaped for 8 hours to make the surface of the material smooth and flat.

[0151] Graphite, the first coating material (soft carbon), and a solvent are mixed at a temperature of 250°C, the mixture is evacuated to remove the solvent, and then heat treated in a horizontal kettle at a temperature of 650°C for 12 hours to obtain a first mixture.

[0152] The first mixture is added to an aluminum chloride solution of a certain concentration, and ammonia water is added to keep the solution pH stable. After hydrolysis for 8 hours, the solution is filtered, repeatedly washed with deionized water and alcohol, dried, and then heat-treated in a horizontal furnace at 600°C for 5 hours to obtain a composite graphite-coated product coated with aluminum trioxide. Finally, the composite graphite-coated product is subjected to magnetic removal screening to obtain the final graphite finished product.

[0153] The above artificial graphite finished product, carbon black, sodium carboxymethylcellulose, styrene butadiene rubber, and a solvent are mixed in a specific ratio using a vacuum mixer to obtain a negative electrode slurry. The produced negative electrode slurry is uniformly coated on both sides of the copper foil of the negative electrode current collector, and then rolled and cut after baking and drying to obtain a negative electrode sheet. The baking temperature is 90 to 110°C.

[0154] Here, in the dry powder of the negative electrode slurry, the mass ratio of the artificial graphite, the carbon black, the sodium carboxymethyl cellulose, and the styrene-butadiene rubber was 96.5:1.5:1.5:0.5, calculated in terms of mass percentage.

[0155] Here, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte is 21°, the resistance R mΩ of the negative electrode active material layer is 9 mΩ, the OI value of the negative electrode active material layer is 4.4, the quantitative content of fine powder of the negative electrode active material is 20%, and the quantitative content of coarse powder of the negative electrode active material is 0.

[0156] 3. Electrolyte production

[0157] Ethylene carbonate (EC), methyl ethyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then 1 mol / L of LiPF6 is added and mixed uniformly to prepare an electrolyte.

[0158] 4. Separator manufacturing

[0159] PP film is used as a separator.

[0160] 5. Lithium-ion battery manufacturing

[0161] The negative electrode sheet and positive electrode sheet manufactured using the above steps are dried, and then wound together with a separator to manufacture an electric core. The positive electrode aluminum sheet and the negative electrode copper-nickel plated sheet are welded to the electric core. The welded electric core is then inserted into a perforated aluminum plastic film for packaging. After injection of electrolyte and constant volume chemical formation, a secondary battery is manufactured.

[0162] II. Test Method

[0163] 1. Testing and calculation method for non-Faraday charge

[0164] S1, assemble the negative electrode sheet into a button battery, perform a cyclic Voltammogram test on the button battery, and obtain the potential range UV of the button battery.

[0165] S2, select the potential range UV of the button battery in step S1, perform a linear scan Voltammogram test on the button battery, detect the scan rate-voltage graph and the voltage-current graph, and obtain the potential range ΔUV of the negative electrode active material layer based on the voltage-current graph, where the scan direction is from low potential to high potential.

[0166] S3, in conjunction with FIG. 1, based on step S2, detect the scan rate-current scatter diagram, and obtain the non-Faraday capacitance Cdl nF of the negative electrode sheet based on the scan rate-current scatter diagram.

[0167] S4: Based on the potential range ΔUV and the non-Fradei capacitance Cdl nF obtained from steps S2 and S3, the non-Fradei charge Q is calculated by the formula Q=Cdl×ΔU.

[0168] Here, the non-faradaic charge QC of the negative electrode sheet is 0.28C, the non-faradaic capacity Cdl nF of the negative electrode sheet is 1.4 nF, and the potential range ΔUV of the negative electrode active material layer is 0.2V.

[0169] 2. Test method for cycle performance of lithium-ion batteries

[0170] The lithium-ion battery is left at 25°C for 30 minutes, then discharged at a constant current of 1C, left at rest for 10 minutes, charged at a constant current and constant voltage of 1C, left at rest for 10 minutes, and then subjected to a full charge-full discharge cycle test. This is repeated until the capacity of the lithium-ion battery exceeds 80% of its initial capacity, and the number of cycles is recorded.

[0171] 3. Test method for high temperature cycling performance of lithium-ion batteries

[0172] The lithium-ion battery is left at 25°C for 30 minutes, then discharged at a constant current of 1C, left at rest for 10 minutes, charged at a constant current and constant voltage of 1C, left at rest for 10 minutes, and then a full charge-full discharge cycle test is performed. The initial charge-discharge capacity and the discharge capacity after 2000 cycles are recorded, and the capacity retention rate is calculated as follows: discharge capacity at 2000 cycles / initial discharge capacity x 100%.

[0173] Example 2

[0174] In Example 2, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as Example 1 except for the following differences.

[0175] The non-Faraday charge QC of the negative electrode sheet is 0.07C, the non-Faraday capacity Cdl nF of the negative electrode sheet is 0.7nF, the potential range ΔUV of the negative electrode active material layer is 0.1V, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte is 35°, the resistance R mΩ of the negative electrode active material layer is 18mΩ, the OI value of the negative electrode active material layer is 5, the quantitative content of fine powder of the negative electrode active material is 60%, and the quantitative content of coarse powder of the negative electrode active material is 50%.

[0176] Example 3

[0177] In Example 3, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as Example 1 except for the following differences.

[0178] The non-Faraday charge QC of the negative electrode sheet is 2C, the non-Faraday capacity Cdl nF of the negative electrode sheet is 4.0nF, the potential range ΔUV of the negative electrode active material layer is 0.5V, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte is 22°, the resistance R mΩ of the negative electrode active material layer is 8mΩ, the OI value of the negative electrode active material layer is 2.5, the quantitative content of fine powder of the negative electrode active material is 35%, and the quantitative content of coarse powder of the negative electrode active material is 30%.

[0179] Example 4

[0180] In Example 4, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as Example 1 except for the following differences.

[0181] The non-Faraday charge QC of the negative electrode sheet is 0.26 C, the non-Faraday capacity Cdl nF of the negative electrode sheet is 1.3 nF, the potential range ΔUV of the negative electrode active material layer is 0.2 V, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte is 20°, the resistance R mΩ of the negative electrode active material layer is 10 mΩ, the OI value of the negative electrode active material layer is 4.4, the quantitative content of fine powder of the negative electrode active material is 0%, and the quantitative content of coarse powder of the negative electrode active material is 20%.

[0182] At the same time, no lithium salt additive is added to the electrolyte of Example 4, the thickness H of the protective film layer is 60 nm, the content of the lithium salt additive in the electrolyte is X, and the thickness H of the protective film layer and the non-Faraday charge Q of the negative electrode sheet satisfy 10X·H+Q=0.26.

[0183] Example 5

[0184] In Example 5, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as Example 1 except for the following differences.

[0185] The negative electrode sheet had a non-Faraday charge QC of 2.5C, a non-Faraday capacity Cdl nF of 5.0nF, a potential range ΔUV of the negative electrode active material layer of 0.5V, a contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte of 10°, a resistance R mΩ of the negative electrode active material layer of 5mΩ, an OI value of the negative electrode active material layer of 2.1, a quantitative content of fine powder of the negative electrode active material of 10%, and a quantitative content of coarse powder of the negative electrode active material of 10%.

[0186] Example 6

[0187] In Example 6, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as Example 1 except for the following differences.

[0188] The non-Faraday charge QC of the negative electrode sheet is 0.54C, the non-Faraday capacity Cdl nF of the negative electrode sheet is 2.7nF, the potential range ΔUV of the negative electrode active material layer is 0.2V, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte is 25°, the resistance R mΩ of the negative electrode active material layer is 10mΩ, the OI value of the negative electrode active material layer is 4, the quantitative content of fine powder of the negative electrode active material is 0%, and the quantitative content of coarse powder of the negative electrode active material is 30%.

[0189] Example 7

[0190] In Example 7, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as Example 1 except for the following differences.

[0191] The non-Faraday charge QC of the negative electrode sheet is 0.78C, the non-Faraday capacity Cdl nF of the negative electrode sheet is 3.9nF, the potential range ΔUV of the negative electrode active material layer is 0.2V, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte is 23°, the resistance R mΩ of the negative electrode active material layer is 8mΩ, the OI value of the negative electrode active material layer is 2.5, the quantitative content of fine powder of the negative electrode active material is 35%, and the quantitative content of coarse powder of the negative electrode active material is 30%.

[0192] Example 8

[0193] In Example 8, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as those of Example 1 except for the following differences.

[0194] The non-Faraday charge QC of the negative electrode sheet is 0.96C, the non-Faraday capacity Cdl nF of the negative electrode sheet is 4.8nF, the potential range ΔUV of the negative electrode active material layer is 0.2V, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte is 12°, the resistance R mΩ of the negative electrode active material layer is 5mΩ, the OI value of the negative electrode active material layer is 2.2, the quantitative content of fine powder of the negative electrode active material is 15%, and the quantitative content of coarse powder of the negative electrode active material is 20%.

[0195] Example 9

[0196] In Example 9, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as those of Example 1 except for the following differences.

[0197] The non-Faraday charge QC of the negative electrode sheet is 1.11C, the non-Faraday capacity Cdl nF of the negative electrode sheet is 3.7nF, the potential range ΔUV of the negative electrode active material layer is 0.3V, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte is 22°, the resistance R mΩ of the negative electrode active material layer is 8mΩ, the OI value of the negative electrode active material layer is 2.4, the quantitative content of fine powder of the negative electrode active material is 35%, and the quantitative content of coarse powder of the negative electrode active material is 30%.

[0198] Example 10

[0199] In Example 10, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as Example 1 except for the following differences.

[0200] The non-Faraday charge QC of the negative electrode sheet was 1.41C, the non-Faraday capacity Cdl nF of the negative electrode sheet was 4.7nF, the potential range ΔUV of the negative electrode active material layer was 0.3V, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte was 12°, the resistance R mΩ of the negative electrode active material layer was 5mΩ, the OI value of the negative electrode active material layer was 2.2, the quantitative content of fine powder of the negative electrode active material was 0%, and the quantitative content of coarse powder of the negative electrode active material was 20%.

[0201] Example 11

[0202] In Example 11, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as Example 1 except for the following differences.

[0203] The negative electrode sheet had a non-Faraday charge QC of 1.72C, a non-Faraday capacity Cdl nF of 4.3nF, a potential range ΔUV of the negative electrode active material layer of 0.4V, a contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte of 20°, a resistance R mΩ of the negative electrode active material layer of 6mΩ, an OI value of the negative electrode active material layer of 2.2, a quantitative content of fine powder of the negative electrode active material of 35%, and a quantitative content of coarse powder of the negative electrode active material of 25%.

[0204] Example 12

[0205] In Example 12, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as Example 1 except for the following differences.

[0206] The non-Faraday charge QC of the negative electrode sheet is 0.12C, the non-Faraday capacity Cdl nF of the negative electrode sheet is 0.4nF, the potential range ΔUV of the negative electrode active material layer is 0.3V, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte is 37°, the resistance R mΩ of the negative electrode active material layer is 15mΩ, the OI value of the negative electrode active material layer is 5.5, the quantitative content of fine powder of the negative electrode active material is 25%, and the quantitative content of coarse powder of the negative electrode active material is 25%.

[0207] Example 13

[0208] In Example 13, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as Example 1 except for the following differences.

[0209] The non-Faraday charge QC of the negative electrode sheet is 0.225C, the non-Faraday capacity Cdl nF of the negative electrode sheet is 2.5nF, the potential range ΔUV of the negative electrode active material layer is 0.09V, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte is 20°, the resistance R mΩ of the negative electrode active material layer is 8mΩ, the OI value of the negative electrode active material layer is 6.5, the quantitative content of fine powder of the negative electrode active material is 10%, and the quantitative content of coarse powder of the negative electrode active material is 15%.

[0210] Example 14

[0211] In Example 14, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as Example 1 except for the following differences.

[0212] The negative electrode sheet had a non-Faraday charge QC of 0.45C, a non-Faraday capacity Cdl nF of 1.5nF, a potential range ΔUV of the negative electrode active material layer of 0.3V, a contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte of 25°, a resistance R mΩ of the negative electrode active material layer of 10mΩ, an OI value of the negative electrode active material layer of 7, a quantitative content of fine powder of the negative electrode active material of 25%, and a quantitative content of coarse powder of the negative electrode active material of 0%.

[0213] Example 15

[0214] In Example 15, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as Example 1 except for the following differences.

[0215] The non-Faraday charge QC of the negative electrode sheet is 0.12C, the non-Faraday capacity Cdl nF of the negative electrode sheet is 1.2nF, the potential range ΔUV of the negative electrode active material layer is 0.1V, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte is 22°, the resistance R mΩ of the negative electrode active material layer is 8mΩ, the OI value of the negative electrode active material layer is 9, the quantitative content of fine powder of the negative electrode active material is 0%, and the quantitative content of coarse powder of the negative electrode active material is 22%.

[0216] Example 16

[0217] In Example 16, a lithium ion battery is manufactured by the method of Example 4 and tested by the test method of Example 4, but the other parts are the same as those of Example 4 except for the following differences.

[0218] The type of lithium salt additive in the electrolyte is LiFSI, the content X of the lithium salt additive in the electrolyte is 1%, the thickness H of the protective film layer is 120 nm, and the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer, and the non-Faraday charge Q of the negative electrode sheet satisfy 10X H + Q = 12.26.

[0219] Example 17

[0220] In Example 17, a lithium ion battery is manufactured by the method of Example 4 and tested by the test method of Example 4, but the other parts are the same as those of Example 4 except for the following differences.

[0221] The type of lithium salt additive in the electrolyte is LiFSI, the content X of the lithium salt additive in the electrolyte is 0.5%, the thickness H of the protective film layer is 100 nm, and the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer, and the non-Faraday charge Q of the negative electrode sheet satisfy 10X H + Q = 5.26.

[0222] Example 18

[0223] In Example 18, a lithium ion battery is manufactured by the method of Example 4 and tested by the test method of Example 4, but the other parts are the same as those of Example 4 except for the following differences.

[0224] The type of lithium salt additive in the electrolyte is LiFSI, the content X of the lithium salt additive in the electrolyte is 1.5%, the thickness H of the protective film layer is 150 nm, and the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer, and the non-Faraday charge Q of the negative electrode sheet satisfy 10X H + Q = 22.76.

[0225] Example 19

[0226] In Example 19, a lithium ion battery is manufactured by the method of Example 4 and tested by the test method of Example 4, but the other parts are the same as those of Example 4 except for the following differences.

[0227] The type of lithium salt additive in the electrolyte is LiFSI, the content X of the lithium salt additive in the electrolyte is 2%, the thickness H of the protective film layer is 180 nm, and the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer, and the non-Faraday charge Q of the negative electrode sheet satisfy 10X H + Q = 36.26.

[0228] Example 20

[0229] In Example 20, a lithium ion battery is manufactured by the method of Example 4 and tested by the test method of Example 4, but the other parts are the same as those of Example 4 except for the following differences.

[0230] The type of lithium salt additive in the electrolyte is LiFSI, the content X of the lithium salt additive in the electrolyte is 2.5%, the thickness H of the protective film layer is 200 nm, and the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer, and the non-Faraday charge Q of the negative electrode sheet satisfy 10X H + Q = 50.26.

[0231] Example 21

[0232] In Example 21, a lithium ion battery is manufactured by the method of Example 4 and tested by the test method of Example 4, but the other parts are the same as those of Example 4 except for the following differences.

[0233] The type of lithium salt additive in the electrolyte is LiPO2F2, the content X of the lithium salt additive in the electrolyte is 1%, the thickness H of the protective film layer is 110 nm, and the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer, and the non-Faraday charge Q of the negative electrode sheet satisfy 10X·H+Q=11.26.

[0234] Example 22

[0235] In Example 22, a lithium ion battery is manufactured by the method of Example 4 and tested by the test method of Example 4, but the other parts are the same as those of Example 4 except for the following differences.

[0236] The type of lithium salt additive in the electrolyte is LiPO2F2, the content X of the lithium salt additive in the electrolyte is 0.8%, the thickness H of the protective film layer is 120 nm, and the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer, and the non-Faraday charge Q of the negative electrode sheet satisfy 10X·H+Q=5.26.

[0237] Example 23

[0238] In Example 23, a lithium ion battery is manufactured by the method of Example 4 and tested by the test method of Example 4, but the other parts are the same as those of Example 4 except for the following differences.

[0239] The type of lithium salt additive in the electrolyte is LiBF4, the content X of the lithium salt additive in the electrolyte is 0.5%, the thickness H of the protective film layer is 120 nm, and the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer, and the non-Faraday charge Q of the negative electrode sheet satisfy 10X·H+Q=5.26.

[0240] Example 24

[0241] In Example 24, a lithium ion battery is manufactured by the method of Example 4 and tested by the test method of Example 4, but the other parts are the same as those of Example 4 except for the following differences.

[0242] The type of lithium salt additive in the electrolyte is LiFSI+LiPO2F2, the content of LiFSI in the electrolyte is 0.5%, the content of LiPO2F2 in the electrolyte is 0.3%, the thickness H of the protective film layer is 120 nm, and the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer and the non-Faraday charge Q of the negative electrode sheet satisfy 10X·H+Q=9.86.

[0243] Example 25

[0244] In Example 25, a lithium ion battery is manufactured by the method of Example 4 and tested by the test method of Example 4, but the other parts are the same as those of Example 4 except for the following differences.

[0245] The type of lithium salt additive in the electrolyte is LiFSI+LiPO2F2, the content of LiFSI in the electrolyte is 0.5%, the content of LiPO2F2 in the electrolyte is 0.5%, the thickness H of the protective film layer is 150 nm, and the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer and the non-Faraday charge Q of the negative electrode sheet satisfy 10X·H+Q=15.26.

[0246] Example 26

[0247] In Example 26, a lithium ion battery is manufactured by the method of Example 4 and tested by the test method of Example 4, but the other parts are the same as those of Example 4 except for the following differences.

[0248] The type of lithium salt additive in the electrolyte is LiFSI+LiBF4, the content of LiFSI in the electrolyte is 0.3%, the content of LiBF4 in the electrolyte is 0.2%, the thickness H of the protective film layer is 130 nm, and the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer, and the non-Faraday charge Q of the negative electrode sheet satisfy 10X·H+Q=6.75.

[0249] Comparative Example 1

[0250] In Comparative Example 1, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as those of Example 1 except for the following differences.

[0251] The non-Faraday charge QC of the negative electrode sheet is 3C, the non-Faraday capacity Cdl nF of the negative electrode sheet is 6.0nF, the potential range ΔUV of the negative electrode active material layer is 0.5V, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte is 45°, the resistance R mΩ of the negative electrode active material layer is 5mΩ, the OI value of the negative electrode active material layer is 10, the quantitative content of fine powder of the negative electrode active material is 0%, and the quantitative content of coarse powder of the negative electrode active material is 65%.

[0252] Comparative Example 2

[0253] In Comparative Example 2, a lithium ion battery is manufactured by the method of Example 1 and tested by the test method of Example 1, but the other parts are the same as those of Example 1 except for the following differences.

[0254] The non-Faraday charge QC of the negative electrode sheet is 0.02C, the non-Faraday capacity Cdl nF of the negative electrode sheet is 0.2nF, the potential range ΔUV of the negative electrode active material layer is 0.1V, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte is 10°, the resistance R mΩ of the negative electrode active material layer is 25mΩ, the OI value of the negative electrode active material layer is 8, the quantitative content of fine powder of the negative electrode active material is 85%, and the quantitative content of coarse powder of the negative electrode active material is 65%.

[0255] 3. Test results

[0256] Table 1 shows the effects of the non-Faradaic charge QC of the negative electrode sheet, the non-Faradaic capacity Cdl nF of the negative electrode sheet, the potential range ΔUV of the negative electrode active material layer, the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte, the resistance R mΩ of the negative electrode active material layer, the OI value of the negative electrode active material layer, the quantitative content of fine powder in the negative electrode active material, and the quantitative content of coarse powder in the negative electrode active material, on the room temperature cycle performance and high temperature cycle performance of a lithium-ion battery.

[0257] [Table 1]

[0258] As a result, the cycle life of a lithium-ion battery can be significantly improved by controlling the non-Faraday charge QC of the negative electrode sheet within a range of 0.05C to 2.5C, the non-Faraday capacity Cdl nF of the negative electrode sheet within a range of 0.5nF to 5nF, the potential range ΔUV of the negative electrode active material layer within a range of 0.1V to 0.5V, the surface contact angle θ of the negative electrode active material layer with respect to the electrolyte within a range of 10 to 40°, the resistance R mΩ of the negative electrode active material layer within a range of 5mΩ to 20mΩ, the OI value of the negative electrode active material layer within a range of 2 to 15, the quantitative content of fine powder of the negative electrode active material within a range of 0 to 80%, and the quantitative content of coarse powder of the negative electrode active material within a range of 0 to 60%.

[0259] Furthermore, by controlling the Faraday capacity Cdl nF of the negative electrode sheet within a range of 1.4 nF to 4.3 nF, controlling the contact angle θ of the negative electrode active material layer with respect to the surface of the electrolyte within a range of 12 to 35°, controlling the resistance R mΩ of the negative electrode active material layer within a range of 5 mΩ to 12 mΩ, controlling the OI value of the negative electrode active material layer within a range of 2 to 10, controlling the quantitative content of fine powder in the negative electrode active material within a range of 0 to 40%, and controlling the quantitative content of coarse powder in the negative electrode active material within a range of 0 to 30%, the cycle life of the lithium-ion battery can be further improved.

[0260] Table 2 shows the effects of the type of lithium salt additive in the electrolyte, the content X of the lithium salt additive in the electrolyte, the thickness Hnm of the protective film layer, the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer, and the non-Faraday charge Q of the negative electrode sheet on the room temperature cycle performance and high temperature cycle performance of the lithium ion battery when the relationship satisfies 10X·H+Q.

[0261] [Table 2]

[0262] As a result, by controlling the type of lithium salt additive in the electrolyte to one or more of lithium tetrafluoroborate (abbreviated as LiBF4), lithium bis(oxalato)borate (abbreviated as LiBOB), lithium difluorophosphate (abbreviated as LiPO2F2), lithium bis(trifluoromethanesulfonimide) (abbreviated as LiTFSI), and lithium bis(fluorosulfonyl)imide (abbreviated as LiFSI), controlling the content X of the lithium salt additive in the electrolyte to within a range of 0.1% to 2%, controlling the thickness H nm of the protective film layer to within a range of 5 nm to 180 nm, and controlling the relationship 10X·H+Q between the content X of the lithium salt additive in the electrolyte, the thickness H of the protective film layer, and the non-Fladaic amount Q of the negative electrode sheet to within a range of 0.4 to 36, the cycle life of the lithium ion battery can be significantly improved.

[0263] The description provided in the above steps is only to help understand the method, structure and core idea of ​​the present application. It should be understood that those skilled in the art can make many improvements and modifications to the present application without departing from the principle of the present application, which also fall within the scope of protection of the claims of the present application.

Claims

1. A positive electrode sheet, a separator, an electrolyte, and a negative electrode sheet are included. the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, Here, the non-Faraday charge of the negative electrode sheet is QC, which satisfies 0.05≦Q≦2.5, and Q=Cdl×ΔU; Cdl nF is the non-faradaic capacity of the negative electrode sheet; ΔUV is the potential range of the negative electrode active material layer; Secondary battery.

2. The Cdl satisfies 0.5≦Cdl≦5, and the ΔU satisfies 0.1≦ΔU≦0.

5. The secondary battery according to claim 1 .

3. The negative electrode active material layer includes one or more of artificial graphite, natural graphite, soft carbon, hard carbon, amorphous carbon, carbon fiber, carbon nanotube, or mesocarbon microsphere; The secondary battery according to any one of claims 1 to 2.

4. a contact angle of the negative electrode active material layer with respect to a surface of an electrolyte solution is θ, and the θ satisfies 10°≦θ≦40°; The secondary battery according to any one of claims 1 to 3.

5. The resistance of the negative electrode active material layer is RmΩ, and satisfies 5≦R≦20. The secondary battery according to any one of claims 1 to 4.

6. The negative electrode active material layer has an OI value of 2 to 15. The secondary battery according to any one of claims 1 to 5.

7. the negative electrode active material layer includes a negative electrode active material, the negative electrode active material has a fine powder content of 0 to 80% by quantity and a coarse powder content of 0 to 60% by quantity; The fine powder refers to negative electrode active material particles having a particle size of 2.2 μm or less, and the coarse powder refers to negative electrode active material particles having a particle size of 35 μm or more. The secondary battery according to any one of claims 1 to 6.

8. The quantity content of the fine powder of the negative electrode active material is 0 to 40%; The quantity content of the coarse powder of the negative electrode active material is 0 to 30%; The secondary battery according to claim 7.

9. the electrolyte comprises a lithium salt additive, the lithium salt additive comprising one or more of lithium tetrafluoroborate, lithium bis(oxalato)borate, lithium difluorophosphate, lithium bis(trifluoromethanesulfonimide), and lithium bis(fluorosulfonyl)imide; The secondary battery according to any one of claims 1 to 8.

10. The content of the lithium salt additive in the electrolyte is X, and 0.1%≦X≦2% is satisfied; The secondary battery according to claim 9.

11. The negative electrode active material layer includes a protective film layer, and the protective film layer has a thickness of H nm. 0.4≦10X·H+Q≦36 is satisfied; The secondary battery according to any one of claims 1 to 10.

12. The thickness H nm of the protective film layer satisfies 5≦H≦180. The secondary battery according to claim 11.

13. A secondary battery comprising the secondary battery according to any one of claims 1 to 12. Electrochemical equipment.

Citation Information

Patent Citations

  • Nonaqueous electrolyte cell

    JP2002075458A

  • Lithium ion secondary battery

    JP2016110900A

  • Manufacturing method of negative electrode sheet

    JP2019057431A

  • Negative electrode material for lithium ion secondary battery, negative electrode for lithium ion secondary battery, and lithium ion secondary battery

    JP2020061245A

  • Anode material, anode containing said anode material, and electrochemical device

    JP2021536104A