Electrolyte for lithium secondary battery and lithium secondary battery including the same
The electrolyte for lithium secondary batteries, comprising a hydrocarbon-based polymer with a cationic functional group, flame-retardant liquid electrolyte, and crosslinking agent, addresses thermal instability and mechanical weaknesses by enhancing cation transport and conductivity, improving battery stability and performance.
Patent Information
- Application Number
- JP2024527647
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-03
- Filing Date
- 2023-04-12
- Publication Date
- 2024-11-21
AI Technical Summary
Lithium secondary batteries face issues with thermal instability due to exothermic reactions at the negative electrode, particularly when using lithium nickel cobalt manganese positive electrodes and graphite, leading to thermal runaway, and polymer electrolytes have weaker mechanical properties and lower ionic conductivity compared to inorganic solid electrolytes.
A lithium secondary battery electrolyte is formulated with a hydrocarbon-based polymer compound containing a cationic functional group, a flame-retardant liquid electrolyte, and a crosslinking agent, forming a cationic polymer backbone to minimize anion movement and enhance cation transport, thereby improving lithium ion transfer ability and mechanical properties.
The electrolyte enhances cation transport, reduces concentration polarization, and improves mechanical stability, resulting in higher ionic conductivity and thermal stability of lithium secondary batteries.
Smart Images

Figure 2024543427000001 
Figure 2024543427000002 
Figure 2024543427000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0045454 filed on April 13, 2022 and Korean Patent Application No. 10-2023-0043320 filed on April 3, 2023, and all contents disclosed in the documents of the relevant Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to an electrolyte for a lithium secondary battery and a lithium secondary battery including the same, and more particularly, to an electrolyte for a lithium secondary battery including the same, which can accelerate cations by forming a cationic polymer backbone to minimize the movement of anions, and can further improve the lithium ion transport ability and mechanical properties, including oxide ceramics. [Background technology]
[0003] Recently, with the rapid spread of electronic devices using batteries, such as mobile phones, laptops, and electric cars, the demand for secondary batteries, which are small, light, and have a relatively high capacity, is rapidly increasing. In particular, lithium secondary batteries, which are lightweight and have high energy density, are attracting attention as a driving power source for portable devices. As a result, research and development efforts to improve the performance of lithium secondary batteries are actively underway. In such lithium secondary batteries, electric energy is produced by oxidation and reduction reactions when lithium ions are inserted / extracted at the positive and negative electrodes, with an organic electrolyte or a polymer electrolyte filled between the positive and negative electrodes, which are made of active materials capable of intercalating and deintercalating lithium ions.
[0004] The positive electrode active materials for lithium secondary batteries include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2, LiMn2O4, etc.), lithium iron phosphate compound (LiFePO4), and lithium nickel cobalt manganese-based positive electrode active materials (or lithium NCM-based positive electrode active materials, or NCM-based lithium composite transition metal oxides, or high Ni positive electrode materials) that can realize high capacity by replacing part of nickel (Ni) with cobalt (Co) and manganese (Mn). However, the above-mentioned conventional lithium secondary batteries can go into thermal runaway due to the exothermic reaction starting from the decomposition reaction of the negative electrode solid electrolyte interface (SEI) and the reaction between the positive electrode, which becomes unstable as the content of nickel (Ni) increases, and the electrolyte containing a carbonate-based solvent, which acts as a major threat to the stability of the battery. In particular, lithium-ion batteries (LIBs), which use a lithium-nickel-cobalt-manganese positive electrode active material together with a graphite negative electrode, have the problem of being relatively more vulnerable to heat.
[0005] Therefore, the industry has attempted to change the components of the positive electrode active material and the components of the electrolyte, and in particular, has continued to make efforts to make up for the problems of conventional lithium secondary batteries by applying polymer compounds and inorganic compounds to the electrolyte. Furthermore, polymer electrolytes have excellent advantages in terms of flexibility, light weight, processability, and cost compared to inorganic solid electrolytes, and the number of cases in which they are applied to lithium secondary batteries is gradually increasing.
[0006] Although polymer electrolytes have various advantages, they are clearly inferior to other electrolytes, and efforts to remedy these problems are being made continuously. That is, polymer electrolytes have weaker mechanical properties and lower ionic conductivity than inorganic solid electrolytes. In addition, polymer electrolytes have a lower cation (Li-ion) transport coefficient (t+) than liquid electrolytes, so they are limited only by the large concentration polarization (resistance).
[0007] Therefore, while polymer electrolytes have various advantages, there is a pressing need to develop electrolytes for lithium secondary batteries that can accelerate cations by forming a cationic polymer backbone to minimize the movement of anions, and can further improve the lithium ion transport capacity and mechanical properties, including oxide ceramics. Summary of the Invention [Problem to be solved by the invention]
[0008] Therefore, an object of the present invention is to provide an electrolyte for a lithium secondary battery, which can accelerate cations by forming a cationic polymer backbone to minimize the movement of anions, and can further improve the lithium ion transport ability and mechanical properties, including oxide-based ceramics, and a lithium secondary battery including the same. [Means for solving the problem]
[0009] In order to achieve the above object, the present invention provides an electrolyte for a lithium secondary battery, comprising: a polymer electrolyte containing a hydrocarbon-based polymer compound containing a cationic functional group; a flame-retardant liquid electrolyte; and a crosslinking agent.
[0010] The present invention also provides a lithium secondary battery comprising: a positive electrode containing a lithium nickel cobalt manganese-based positive electrode active material; a negative electrode; and an electrolyte for lithium secondary batteries interposed between the positive electrode and the negative electrode. Effect of the Invention
[0011] The electrolyte for a lithium secondary battery and the lithium secondary battery including the same according to the present invention have the advantage that a cationic polymer backbone is formed to minimize the movement of anions, thereby accelerating cations and improving the transfer ability and mechanical properties of additional lithium ions, including oxide ceramics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below.
[0013] The electrolyte for a lithium secondary battery according to the present invention includes a polymer electrolyte containing a hydrocarbon-based polymer compound containing a cationic functional group, a flame-retardant liquid electrolyte, and a crosslinking agent.
[0014] Lithium secondary batteries produce electric energy through oxidation and reduction reactions when lithium ions are inserted / deintercalated between the positive and negative electrodes, with organic or polymer electrolytes filled between them. To improve thermal stability, lithium nickel cobalt manganese-based positive active materials, in which part of nickel (Ni) is replaced with cobalt (Co) and manganese (Mn), are used in the battery. However, conventional lithium secondary batteries can go into thermal runaway due to an exothermic reaction that starts with the decomposition reaction of the negative electrode solid electrolyte interface (SEI) and a reaction between the positive electrode, which becomes unstable as the nickel (Ni) content increases, and the electrolyte, which contains a carbonate-based solvent, which acts as a major threat to the stability of the battery. In particular, lithium ion batteries (LIBs) that use lithium nickel cobalt manganese-based positive active materials together with graphite negative electrodes have the problem of being relatively more vulnerable to heat.
[0015] Therefore, the industry has attempted to change the components of the positive electrode active material and the electrolyte, and has been making efforts to address the problems of conventional lithium secondary batteries by applying polymeric and inorganic compounds to the electrolyte. Polymeric electrolytes have advantages in terms of flexibility, light weight, processability, and cost compared to inorganic solid electrolytes, and their use in lithium secondary batteries is gradually increasing. Although polymeric electrolytes have various advantages, they are also clearly inferior to other electrolytes, and efforts to address these problems are also being made continuously. That is, it has been pointed out that polymeric electrolytes have weaker mechanical properties and lower ionic conductivity compared to inorganic solid electrolytes. In addition, polymeric electrolytes have a limitation in that they can only have a large concentration polarization (resistance) due to a lower cation (Li-ion) transport coefficient (t+) compared to liquid electrolytes.
[0016] Therefore, the present applicant has invented an electrolyte for lithium secondary batteries and a lithium secondary battery including the same, which uses a polymer electrolyte having various advantages, accelerates cations by forming a cationic polymer backbone to minimize the movement of anions, and further improves the lithium ion transfer ability and mechanical properties by including oxide ceramics.
[0017] The electrolyte for lithium secondary batteries according to the present invention will now be described in more detail. First, the polymer electrolyte included in the electrolyte for lithium secondary batteries according to the present invention includes a hydrocarbon-based polymer compound containing a cationic functional group. The hydrocarbon-based polymer compound containing the cationic functional group can accelerate the cations by minimizing the movement of anions through the cations (i.e., forming a polymer chain positively charged) formed on the polymer backbone. Thus, the transport coefficient of the cations is increased and the concentration polarization (resistance) can be reduced, as compared to the case where a conventional polymer electrolyte not containing a cationic functional group is used.
[0018] The hydrocarbon polymer compound containing a cationic functional group contains a structural unit of a hydrocarbon having 6 to 20 carbon atoms, preferably 8 to 14 carbon atoms, containing one or more cationic functional groups. The cationic functional group may contain one or more cations selected from nitrogen cations, oxygen cations, and sulfur cations, and preferably contains at least one nitrogen cation among these.
[0019] More specifically, the hydrocarbon-based polymer compound containing a cationic functional group is polydiallyldimethylammonium ((CH)) represented by the following chemical formula 1. 16 N + )n), polymethacryloxyethyltrimethylammonium ((C9H 18 NO2 + )n, 1≦n≦10,000), polyallylamine ([CHCH(CHNH)]n, 1≦n≦10,000), and polysodium 4-styrenesulfonate ((CHNaOS)n, 1≦n≦10,000).
[0020] [Chemical formula 1] [ka]
[0021] In the above Chemical Formula 1, n is a natural number of 1 to 10,000, preferably 1 to 100.
[0022] The anion whose movement is minimized by the cation located on the main chain of the hydrocarbon polymer compound is bound to the main chain of the polymer in which the cation is located, and thus the movement is reduced. The anion may be any anion that can be contained in the electrolyte, and specifically, may be an anion of a lithium salt contained in the electrolyte. In other words, the hydrocarbon polymer compound may further contain an anion as a counter ion to the cation contained in the cationic functional group. The anion of the lithium salt contained in the electrolyte may be, for example, TFSI of LiTFSI.- , LiSCN's SCN - , LiBr Br - and LiCl Cl - The anion may be an anion of a lithium salt generally known in the art, such as the above. In addition, the hydrocarbon-based polymer compound containing the cationic functional group may be in a state in which the anion described above is bonded as a counter ion to the cation from the beginning.
[0023] For example, when the hydrocarbon-based polymer compound containing the cationic functional group is polydiallyldimethylammonium represented by the above-mentioned Chemical Formula 1, the anion of the lithium salt (TFSI - ) can bind as a counterion to the cation (polydiallyldimethylammonium-bis(trifluoromethanesulfonyl)imide, DADMA-TFSI). The reduced movement of the anion accelerates the cation, which increases the transport coefficient of the cation and reduces the concentration polarization (resistance).
[0024] [Chemical formula 2] [ka]
[0025] In the above Chemical Formula 2, n is a natural number of 1 to 10,000, preferably 1 to 100.
[0026] Meanwhile, the polymer electrolyte contained in the electrolyte for a lithium secondary battery of the present invention may further contain a conventional polymer compound commonly used in the art, if necessary, in addition to the above-mentioned hydrocarbon-based polymer compound containing a cationic functional group.
[0027] The polymer electrolyte may be contained in an amount of 30 to 60 wt%, preferably 30 to 50 wt%, more preferably 35 to 40 wt%, based on the total weight of the electrolyte for the lithium secondary battery of the present invention. If the amount of the polymer electrolyte is less than 30 wt%, the effect of the cationic polymer may not be exhibited, and if it exceeds 60 wt%, the weight of the cationic polymer becomes excessive, which may hinder ion conduction.
[0028] Next, the flame-retardant liquid electrolyte contained in the electrolyte for the lithium secondary battery of the present invention will be described. The flame-retardant liquid electrolyte dissolves the hydrocarbon-based polymer compound containing a cationic functional group described above and dissociates and transfers the lithium salt, and must be included together with the hydrocarbon-based polymer compound containing a cationic functional group. The flame-retardant liquid electrolyte is confined in the hardened cationic polymer and does not flow or ooze out, but may be present in a liquid state in the finally manufactured electrolyte.
[0029] More specifically, the flame-retardant liquid electrolyte includes a solvent and a lithium salt. The solvent contained in the flame-retardant liquid electrolyte may be one or more selected from the group consisting of carbonate-based compounds, phosphate-based compounds, and ionic liquids. The carbonate-based compounds include dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate, methylpropyl carbonate, ethylmethyl carbonate, ethylpropyl carbonate, and methyl(2,2,2-trifluoroethyl)carbonate. The phosphate-based compounds include trimethyl phosphate, triethyl phosphate, and 2-(2,2,2-trifluoroethoxy)-1,3,2-dioxaphosphorane 2-oxide. The ionic liquid may include N-propyl-N-methylpyrrolidinium and 1-butyl-1-methylpyrrolidinium.
[0030] The solvent may further contain one or more of esters, ethers, or ketones, if necessary. Examples of these include aprotic organic solvents such as γ-butyrolactone, n-methyl acetate, n-ethyl acetate, n-propyl acetate, dibutyl ether, N-methyl-2-pyrrolidinone, 1,2-dimethoxyethane, tetrahydrofuran derivatives such as 2-methyltetrahydrofuran, dimethyl sulfoxide, formamide, dimethylformamide, dioxolane and its derivatives, acetonitrile, nitromethane, methyl formate, methyl acetate, trimethoxymethane, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, methyl propionate, and ethyl propionate.
[0031] The lithium salt contained in the flame-retardant liquid electrolyte is LiFSI, LiTFSI, LiCl, LiBr, LiI, LiClO4, LiBF4, LiPF6, LiB 10 Cl 10 , LiCF3SO3, LiCF3CO2, LiC4BO8, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (C2F5SO2)2NLi, (CF3SO2)3CLi, lithium chloroborane, lithium lower aliphatic carboxylate having 4 or less carbon atoms, lithium 4-phenylborate, and lithium imide. The lithium salt may be contained in the electrolyte for lithium secondary battery of the present invention to a concentration of 1.5M to 4.0M, preferably 1.5M to 2.0M. If the concentration of the lithium salt is less than 1.5M or exceeds 4.0M, the contribution to the thermal stability of the battery may be negligible, or there may be no further advantage in improving the thermal stability of the battery. In addition, if the concentration of the lithium salt is less than 1.5M, it is difficult to ensure ionic conductivity suitable for battery operation, and if the concentration exceeds 4.0M, the viscosity of the electrolyte increases, the mobility of lithium ions decreases, or the decomposition reaction of the lithium salt itself increases, which may result in a decrease in battery performance.
[0032] The flame-retardant liquid electrolyte may be contained in an amount of 30 to 50 wt %, preferably 30 to 40 wt %, and more preferably 35 to 40 wt %, based on the total weight of the electrolyte for the lithium secondary battery of the present invention. If the amount of the flame-retardant liquid electrolyte is less than 30 wt %, the ion conductivity may be too low to be used as an electrolyte, and if the amount of the flame-retardant liquid electrolyte is more than 50 wt %, there may be a problem that an excessive amount of components in a liquid state, rather than in a solid state, is present.
[0033] Next, the crosslinking agent contained in the electrolyte for lithium secondary batteries of the present invention will be described. The crosslinking agent is for preventing leakage and improving additional mechanical properties, and in particular plays a role in gelling or solidifying the electrolyte for lithium secondary batteries of the present invention. The crosslinking agent may be at least one selected from the group consisting of ethoxylated trimethylolpropane triacrylate (ETPTA), trimethylolpropane ethoxy triacrylate, dipentaerythritol penta / hexa-acrylate, and tris(2-hydroxyethyl)isocyanurate triacrylate, but is not limited thereto.
[0034] The crosslinking agent may be included in an amount of 2 to 30 wt %, preferably 10 to 30 wt %, and more preferably 20 to 30 wt %, based on the total weight of the electrolyte for a lithium secondary battery of the present invention. If the content of the crosslinking agent is less than 2 wt %, a problem may occur in which crosslinking is not normally performed, and if it exceeds 30 wt %, a problem may occur in which ion conduction is hindered due to the excessive weight of the crosslinking agent.
[0035] Meanwhile, the electrolyte for a lithium secondary battery according to the present invention may further include an active oxide ceramic for the purpose of improving the lithium ion transfer ability and mechanical properties. The active oxide ceramic may include Li 1+x Al x Ge 2-x (PO4)3(LAGP), Li7La3Zr2O 12 (LLZO) and Li 1+x Alx Ti 2-x (PO4)3(LATP). However, even if not exemplified here, as long as it is an active oxide ceramic having similar or equivalent properties to the above-mentioned LAGP, LLZO, and LATP, it can be applied as the active oxide ceramic of the present invention without any special restrictions.
[0036] The active oxide ceramic may be included in an amount of 15 to 100 parts by weight, preferably 40 to 65 parts by weight, based on 100 parts by weight of the total electrolyte for the lithium secondary battery including the polymer electrolyte, the flame-retardant liquid electrolyte, and the crosslinking agent.
[0037] Next, the lithium secondary battery according to the present invention will be described.
[0038] The lithium secondary battery includes a positive electrode including a lithium nickel cobalt manganese-based positive electrode active material, a negative electrode, and the lithium secondary battery electrolyte interposed between the positive electrode and the negative electrode. The positive electrode includes a lithium nickel cobalt manganese-based positive electrode active material (or a lithium NCM-based positive electrode active material, or a NCM-based lithium composite transition metal oxide, or a high Ni positive electrode material), and when the positive electrode is applied to a battery, a high capacity can be realized. The lithium nickel cobalt manganese-based positive electrode active material may have a surface coated with a metal oxide.
[0039] The lithium nickel cobalt manganese-based positive electrode active material may be commercially available or may be prepared according to a method well known in the art. For example, an ammonium cation-containing complex former and a basic compound are added to a transition metal solution containing a nickel-containing raw material, a cobalt-containing raw material, and a manganese-containing raw material, and a coprecipitation reaction is carried out to prepare a nickel-cobalt-manganese precursor, and then the nickel-cobalt-manganese precursor and a lithium raw material are mixed and over-fired at a temperature of 980° C. or higher to prepare a lithium nickel cobalt manganese-based positive electrode active material.
[0040] The nickel-containing source material may be, for example, nickel-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, but not limited to, Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, fatty acid nickel salt, nickel halide, or a combination thereof. The cobalt-containing source material may be, for example, cobalt-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, but not limited to, Co(OH)2, CoOOH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, CoSO4, Co(SO4)2·7H2O, or a combination thereof. The manganese-containing source material may be, for example, a manganese-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, oxyhydroxide, or a combination thereof, specifically, but not limited to, manganese oxides such as Mn2O3, MnO2, Mn3O4, etc.; manganese salts such as MnCO3, Mn(NO3)2, MnSO4, manganese acetate, manganese dicarboxylate, manganese citrate, and manganese fatty acid salt; manganese oxyhydroxide, manganese chloride, or a combination thereof.
[0041] The transition metal solution may be prepared by adding the nickel-containing raw material, the cobalt-containing raw material, and the manganese-containing raw material to a solvent, specifically, water or a mixed solvent of an organic solvent (e.g., alcohol, etc.) that can be uniformly mixed with water, or may be prepared by mixing an aqueous solution of the nickel-containing raw material, an aqueous solution of the cobalt-containing raw material, and a manganese-containing raw material. The ammonium cation-containing complexing agent may be, but is not limited to, NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, NH4CO3, or a combination thereof. Meanwhile, the ammonium cation-containing complexing agent may be used in the form of an aqueous solution, and the solvent may be water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that can be uniformly mixed with water.
[0042] The basic compound may be, for example, a hydroxide of an alkali metal or an alkaline earth metal such as NaOH, KOH, or Ca(OH)2, a hydrate thereof, or a combination thereof. The basic compound may also be used in the form of an aqueous solution, and the solvent used in this case may be water or a mixture of water and an organic solvent (specifically, an alcohol, etc.) that is uniformly miscible with water. The basic compound is added to adjust the pH of the reaction solution, and may be added in an amount that makes the pH of the metal solution 11 to 13.
[0043] Meanwhile, the coprecipitation reaction may be carried out at a temperature of 40 to 70°C under an inert atmosphere such as nitrogen or argon. Through the above-mentioned process, nickel-cobalt-manganese hydroxide particles are generated and precipitated in the reaction solution. The precipitated nickel-cobalt-manganese hydroxide particles are separated and dried according to a conventional method to obtain a nickel-cobalt-manganese precursor. The nickel-cobalt-manganese precursor may be a secondary particle formed by agglomeration of primary particles, and the average particle size (D50) of the secondary particles of the nickel-cobalt-manganese precursor may be 4 to 8 μm, preferably 4 to 7.5 μm, and more preferably 4 to 7 μm.
[0044] The lithium source material may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and is not particularly limited as long as it can be dissolved in water. Specifically, the lithium source may be Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, or Li3C6H5O7, and any one or a mixture of two or more of them may be used. The lithium source materials may be mixed so that the molar ratio (Li / M) of lithium (Li) to the total metal elements (M) of the nickel-cobalt-manganese precursor is 1 to 1.5, preferably 1 to 1.1.
[0045] The content of the lithium nickel cobalt manganese based positive electrode active material may be 50 to 95 parts by weight, preferably 60 to 90 parts by weight, based on 100 parts by weight of the positive electrode. If the content of the lithium nickel cobalt manganese based positive electrode active material is less than 50 parts by weight based on 100 parts by weight of the total positive electrode, the electrochemical properties of the battery due to the positive electrode active material may be deteriorated, and if it exceeds 95 parts by weight, additional components such as binders and conductive materials may be included in small amounts, making it difficult to efficiently manufacture the battery.
[0046] The positive electrode further includes a binder and a conductive material in addition to the positive electrode active material. The binder is a component that aids in binding between the positive electrode active material and the conductive material and between the positive electrode active material and the current collector. For example, one or more selected from the group consisting of polyvinylidene fluoride (PVdF), polyvinylidene fluoride-polyhexafluoropropylene copolymer (PVdF / HFP), polyvinyl acetate, polyvinyl alcohol, polyvinyl ether, polyethylene, polyethylene oxide, alkylated polyethylene oxide, polypropylene, polymethyl (meth)acrylate, polyethyl (meth)acrylate, polytetrafluoroethylene (PTFE), polyvinyl chloride, polyacrylonitrile, polyvinylpyridine, polyvinylpyrrolidone, styrene-butadiene rubber, acrylonitrile-butadiene rubber, ethylene-propylene-diene monomer (EPDM) rubber, sulfonated EPDM rubber, styrene-butylene rubber, fluororubber, carboxymethylcellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, and mixtures thereof may be used, but is not necessarily limited thereto.
[0047] The binder may be used in an amount of 1 to 50 parts by weight, preferably 3 to 15 parts by weight, per 100 parts by weight of the total positive electrode. If the binder content is less than 1 part by weight per 100 parts by weight of the total positive electrode, the adhesive strength between the positive electrode active material and the current collector may be insufficient. If the binder content is more than 50 parts by weight per 100 parts by weight of the total positive electrode, the adhesive strength is improved, but the content of the positive electrode active material is reduced accordingly, which may result in a low battery capacity.
[0048] The conductive material contained in the positive electrode is not particularly limited as long as it does not cause side reactions in the internal environment of the lithium secondary battery, does not cause chemical changes in the battery, and has excellent electrical conductivity. Representative examples include graphite or conductive carbon, and include, but are not limited to, graphite such as natural graphite and artificial graphite; carbon black, acetylene black, ketjen black, denka black, thermal black, channel black, furnace black, lamp black, and other carbon blacks; carbon-based substances having a graphene or graphite crystal structure; conductive fibers such as carbon fibers and metal fibers; carbon fluoride; metal powders such as aluminum powder and nickel powder; conductive whiskey such as zinc oxide and potassium titanate; conductive oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives. These may be used alone or in combination of two or more kinds.
[0049] The conductive material may be used in an amount of 0.5 to 50 parts by weight, preferably 1 to 30 parts by weight, based on 100 parts by weight of the total positive electrode. If the amount of the conductive material is less than 0.5 parts by weight based on 100 parts by weight of the total positive electrode, the effect of improving electrical conductivity may be difficult to expect, or the electrochemical properties of the battery may be deteriorated. If the amount of the conductive material is more than 50 parts by weight based on 100 parts by weight of the total positive electrode, the amount of the positive electrode active material may be relatively small, and the capacity and energy density may be reduced. The method of incorporating the conductive material into the positive electrode is not particularly limited, and a conventional method known in the art, such as coating the positive electrode active material, may be used. If necessary, a conductive second coating layer may be added to the positive electrode material to replace the addition of the conductive material.
[0050] In addition, a filler may be selectively added to the positive electrode of the present invention as a component for suppressing the expansion of the electrode. Such a filler is not particularly limited as long as it can suppress the expansion of the electrode without causing a chemical change in the battery, and for example, olefin polymers such as polyethylene and polypropylene; fibrous materials such as glass fiber and carbon fiber; etc. may be used.
[0051] The positive electrode active material, binder, conductive material, etc. are dispersed and mixed in a dispersion medium (solvent) to prepare a slurry, which is then applied onto a positive electrode current collector, and then dried and rolled to produce a positive electrode included in the lithium secondary battery of the present invention. The dispersion medium may be, but is not necessarily limited to, NMP (N-methyl-2-pyrrolidone), DMF (dimethyl formamide), DMSO (dimethyl sulfoxide), ethanol, isopropanol, water, or a mixture thereof.
[0052] The positive electrode current collector may be, but is not limited to, platinum (Pt), gold (Au), palladium (Pd), iridium (Ir), silver (Ag), ruthenium (Ru), nickel (Ni), stainless steel (STS), aluminum (Al), molybdenum (Mo), chromium (Cr), carbon (C), titanium (Ti), tungsten (W), ITO (In doped SnO2), FTO (F doped SnO2), and alloys thereof, and aluminum (Al) or stainless steel surface-treated with carbon (C), nickel (Ni), titanium (Ti) or silver (Ag). The positive electrode current collector may be in the form of a foil, film, sheet, punched, porous, foam, or the like.
[0053] The negative electrode can be manufactured according to a conventional method known in the art. For example, a negative electrode active material, a conductive material, a binder, and optionally a filler can be dispersed and mixed in a dispersion medium (solvent) to prepare a slurry, which can be applied to a negative electrode current collector, and then dried and rolled to manufacture a negative electrode. The negative electrode active material can be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Sb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β(0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites and Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, the carbon material may be both low crystalline carbon and high crystalline carbon. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, flake-like, spherical or fibrous natural graphite or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.
[0054] The binder and conductive material used in the negative electrode may be the same as those described above for the positive electrode. The negative electrode current collector may be, but is not limited to, platinum (Pt), gold (Au), palladium (Pd), iridium (Ir), silver (Ag), ruthenium (Ru), nickel (Ni), stainless steel (STS), copper (Cu), molybdenum (Mo), chromium (Cr), carbon (C), titanium (Ti), tungsten (W), ITO (In doped SnO2), FTO (F doped SnO2), and alloys thereof, and copper (Cu) or stainless steel surface-treated with carbon (C), nickel (Ni), titanium (Ti) or silver (Ag). The negative electrode current collector may be in the form of a foil, film, sheet, punched, porous, foam, or the like.
[0055] Meanwhile, in the lithium secondary battery, a solid electrolyte positioned as a layered membrane, i.e., the electrolyte for the lithium secondary battery according to the present invention, may be positioned between the positive electrode and the negative electrode. In this case, the solid electrolyte may also function as a separator (i.e., electrically insulate the negative electrode from the positive electrode while allowing lithium ions to pass through). In this case, the solid electrolyte may be attached in the form of a thin film to one side of the positive electrode or the negative electrode and included in the lithium secondary battery. Also, the solid electrolyte may be independently interposed between the positive electrode and the negative electrode. And, the lithium secondary battery according to the present invention may be a semi-solid battery using a liquid electrolyte and a solid electrolyte in combination, if necessary. In addition, in this case, a separate separator may be further included (i.e., at least one of a separator and a solid electrolyte may be interposed between the positive electrode and the negative electrode).
[0056] If a separate separation membrane is further included, olefin polymers such as polyethylene and polypropylene, glass fiber, etc. may be used in the form of a sheet, multi-layer membrane, microporous film, woven fabric, nonwoven fabric, etc., but are not necessarily limited thereto. However, it is preferable to use porous polyethylene or porous glass fiber nonwoven fabric (glass filter) as the separation membrane, and it is more preferable to use a porous glass filter (glass fiber nonwoven fabric) as the separation membrane. The separation membrane may be an insulating thin film having high ion permeability and mechanical strength, and the pore diameter of the separation membrane may be generally 0.01 to 10 μm, and the thickness may be generally 5 to 300 μm, but are not limited thereto.
[0057] Meanwhile, the lithium secondary battery of the present invention can be manufactured according to a conventional method in the art. For example, it can be manufactured by inserting a porous separator between a positive electrode and a negative electrode and pouring an electrolyte solution. The lithium secondary battery of the present invention can be applied to a battery cell used as a power source for a small device, and can be particularly suitably used as a unit battery of a battery module that is a power source for a medium- to large-sized device. In this respect, the present invention also provides a battery module including two or more lithium secondary batteries electrically connected (in series or parallel). Of course, the number of lithium secondary batteries included in the battery module can be variously adjusted in consideration of the use and capacity of the battery module.
[0058] Furthermore, the present invention provides a battery pack in which the battery modules are electrically connected according to a conventional technique in the art. The battery module and the battery pack can be used as a power source for one or more medium- to large-sized devices including, but not limited to, a power tool, an electric vehicle (EV), a hybrid electric vehicle (HEV), and an electric plug-in hybrid electric vehicle (PHEV), an electric truck, an electric commercial vehicle, or a power storage system.
[0059] Below, preferred embodiments are shown to aid in understanding the present invention. However, these are merely illustrative of the present invention, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical spirit of the present invention. Naturally, such changes and modifications also fall within the scope of the appended claims.
[0060] [Example 1] Manufacture of a lithium secondary battery Electrolyte production Polydiallyldimethylammonium-bis(trifluoromethanesulfonyl)imide (DADMA-TFSI, polymer electrolyte) was dissolved in a flame-retardant liquid electrolyte (SCE05, solvent: EC / EMC = 1:9 (v / v), lithium salt: 1M LiFSI and 1M LiPF6), and trimethylolpropane triacrylate (ETPTA, crosslinker) was added and mixed thereto, and then cured for about 40 seconds with a UV curing lamp to prepare a thin-film electrolyte for lithium secondary batteries. Meanwhile, the polymer electrolyte, the flame-retardant liquid electrolyte, and the crosslinker were used in a weight ratio of 1:1:0.8 (about 35.7 wt%:35.7 wt%:28.6 wt%).
[0061] Cathode manufacturing First, in a 40L batch-type reactor set at 50°C, NiSO4, CoSO4, and MnSO4 were mixed in water in amounts such that the molar ratio of nickel:cobalt:manganese was 80:10:10 to prepare a precursor formation solution with a concentration of 2.4M. After 13 L of deionized water was poured into a coprecipitation reactor (volume 40L), nitrogen gas was purged into the reactor at a rate of 25 L / min to remove dissolved oxygen in the water and create a non-oxidizing atmosphere inside the reactor. After that, 83 g of a 25% NaOH aqueous solution was poured in and stirred at a speed of 700 rpm at a temperature of 50°C to maintain a pH of 11.5. The precursor formation solution was then poured in at a rate of 1.9 L / hr, and a coprecipitation reaction was carried out for 48 hours while simultaneously pouring in an aqueous NaOH solution and an aqueous NH4OH solution, to obtain nickel-cobalt-manganese hydroxide (Ni 0.5 Co 0.3 Mn 0.2(OH)2) particles were formed. The hydroxide particles were separated, washed, and then dried in an oven at 120°C to prepare a nickel-cobalt-manganese precursor (D50 = 4.8 μm). The nickel-cobalt-manganese precursor and the lithium source LiOH were then put into a Henschel mixer (20 L) so that the Li / M (Ni, Co, Mn) molar ratio was 1.02, and mixed at 300 rpm at the center for 20 minutes. The mixed powder was placed in an alumina crucible of 330 mm x 330 mm size and fired at 1,010 to 1,030°C for 15 hours in an oxygen atmosphere to prepare a lithium nickel cobalt manganese-based positive electrode active material.
[0062] Next, the lithium nickel cobalt manganese-based positive electrode active material, carbon black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder were mixed in a weight ratio of 96.5:1.5:2 and dispersed in an NMP solvent to prepare a slurry, which was then coated on an aluminum foil (Al foil) having a thickness of 25 μm with a blade-type coating machine, a Labdryer / coater type LTE (Werner Mathis AG), to a uniform thickness, and dried in a vacuum oven at 120° C. for 13 hours to prepare a positive electrode for a lithium secondary battery.
[0063] Manufacture of lithium secondary batteries A negative electrode including graphite as an active material and the prepared positive electrode were positioned to face each other, and a thin film of the prepared electrolyte for a lithium secondary battery was interposed between them to prepare an electrode assembly. The electrode assembly was then placed inside a case to prepare a lithium secondary battery.
[0064] [Example 2] Manufacture of lithium secondary battery When a crosslinking agent (trimethylolpropane triacrylate, ETPTA) was added, Li7La3Zr2O 12A lithium secondary battery was manufactured in the same manner as in Example 1, except that (LLZO, active oxide ceramic) was added together. Meanwhile, the polymer electrolyte, the flame-retardant liquid electrolyte, the crosslinking agent, and the active oxide ceramic were used in a weight ratio of 1:1:0.8:0.5.
[0065] Comparative Example 1: Manufacture of a lithium secondary battery A lithium secondary battery was manufactured in the same manner as in Example 1, except that the polymer electrolyte was changed from polydiallyldimethylammonium-bis(trifluoromethanesulfonyl)imide (DADMA-TFSI) to polyethylene oxide (PEO, Mw=about 10,000).
[0066] Comparative Example 2: Manufacture of a lithium secondary battery A lithium secondary battery was manufactured in the same manner as in Example 1, except that a crosslinking agent (trimethylolpropane triacrylate, ETPTA) was not used.
[0067] Comparative Example 3: Manufacture of a lithium secondary battery A lithium secondary battery was manufactured in the same manner as in Example 1, except that the weight ratio of the polymer electrolyte, the flame-retardant liquid electrolyte, and the crosslinker was changed from 1:1:0.8 (about 35.7 wt%:35.7 wt%:28.6 wt%) to 1:2.2:1.78 (about 20 wt%:44.5 wt%:35.5 wt%).
[0068] Comparative Example 4: Manufacture of a lithium secondary battery A lithium secondary battery was manufactured in the same manner as in Example 1, except that the weight ratio of the polymer electrolyte, the flame-retardant liquid electrolyte, and the crosslinker was changed from 1:1:0.8 (about 35.7 wt%:35.7 wt%:28.6 wt%) to 1:2.55:0.7 (about 23.5 wt%:60 wt%:16.5 wt%).
[0069] [Experimental Example 1] Measurement of ionic conductivity The ionic conductivity of the electrolytes for lithium secondary batteries prepared in Examples 1 and 2 and Comparative Examples 1 to 4 was measured, and the results are shown in Table 1. The ionic conductivity was measured using an AC impedance measuring device, IVIUM STAT (Ivium Technologies, Netherlands).
[0070] [Table 1]
[0071] The ionic conductivity of the electrolytes for lithium secondary batteries prepared in Examples 1 and 2 and Comparative Examples 1 to 4 was measured, and as shown in Table 1, the electrolyte of Example 1 including a polymer electrolyte containing a hydrocarbon-based polymer compound containing a cationic functional group, a flame-retardant liquid electrolyte, and a crosslinking agent, and the electrolyte of Example 2 including an active oxide ceramic were higher in ionic conductivity than the electrolyte of Comparative Example 1 including a normal polymer electrolyte and the electrolyte of Comparative Example 2 in which only the crosslinking agent was removed from the electrolyte of Example 1. In addition, Comparative Example 3, in which the content of the polymer electrolyte is outside the scope of the present invention, and Comparative Example 4, in which the content of the flame-retardant liquid electrolyte is outside the scope of the present invention, also showed lower ionic conductivity than Examples 1 and 2. In addition, through the comparison and comparison of Examples 1 and 2, it was confirmed that the ionic conductivity was further increased when the electrolyte included an active oxide ceramic.
[0072] [Experimental Example 2] Measurement of cation transport coefficient A voltage of 10 mV was applied to the lithium secondary batteries prepared in Examples 1 and 2 and Comparative Examples 1 to 4 to induce polarization in the electrodes, and the current in the polarized state was measured, and the cation transport coefficient (t+) of the liquid electrolyte was measured based on the measured current value using the following Equation 1 according to the Bruce-Vincent method. Meanwhile, the measured current value is the current value per second when there is a current change of 1 μA (i.e., dl=1 μA & dt=1 sec).
[0073] [Formula 1]
number
[0074] In the above formula 1, I ss is the current flowing in the steady state, which is 25.5 μA (measured for up to 6 hours), I0 is the current flowing in the polarized state, which is 44.6 μA, ΔV is the potential difference applied across the cell, R0 is the interface resistance in the polarized state, which is 136.06, and R ss is the interface resistance at steady state, which is 314.74.
[0075] The cation transport coefficients of the lithium secondary batteries prepared in Examples 1 and 2 and Comparative Examples 1 to 4 were measured, and the results are shown in Table 2 below.
[0076] [Table 2]
[0077] As described above, the cation transport coefficients of the lithium secondary batteries manufactured in Examples 1 and 2 and Comparative Examples 1 to 4 were measured. As shown in Table 2, the electrolyte of Example 1 including the polymer electrolyte containing a hydrocarbon-based polymer compound containing a cationic functional group, the flame-retardant liquid electrolyte, and the crosslinking agent, and the electrolyte of Example 2 including the active oxide-based ceramic, showed higher cation transport coefficients than the electrolyte of Comparative Example 1 including a normal polymer electrolyte and the electrolyte of Comparative Example 2 in which only the crosslinking agent was removed from the electrolyte of Example 1. In addition, Comparative Example 3, in which the content of the polymer electrolyte is outside the scope of the present invention, and Comparative Example 4, in which the content of the flame-retardant liquid electrolyte is outside the scope of the present invention, also showed lower cation transport coefficients than Examples 1 and 2. Through this, it was confirmed that the present invention has an advantage of lowering concentration polarization (resistance) compared to normal electrolytes.
Claims
1. An electrolyte for a lithium secondary battery comprising: a polymer electrolyte containing a hydrocarbon-based polymer compound containing a cationic functional group; a flame-retardant liquid electrolyte; and a crosslinking agent.
2. 2. The electrolyte for lithium secondary batteries according to claim 1, wherein the hydrocarbon-based polymer compound contains a structural unit of a hydrocarbon having 6 to 20 carbon atoms and containing one or more cationic functional groups.
3. 2. The electrolyte for a lithium secondary battery according to claim 1, wherein the cationic functional group comprises at least one cation selected from the group consisting of a nitrogen cation, an oxygen cation, and a sulfur cation.
4. The hydrocarbon-based polymer compound containing a cationic functional group is polydiallyldimethylammonium (C 8 H 16 N + ) n, 1≦n≦10,000), polymethacryloxyethyltrimethylammonium ((C 9 H 18 NO 2 + ) n, 1≦n≦10,000), polyallylamine ([CH 2 CH (CH 2 N.H. 2 ) ]n, 1≦n≦10,000) and sodium poly(4-styrenesulfonate) ((C 8 H 7 NaO 3 2. The electrolyte for a lithium secondary battery according to claim 1, comprising at least one selected from the group consisting of: S) n, 1≦n≦10,000.
5. 2. The electrolyte for a lithium secondary battery according to claim 1, wherein the hydrocarbon-based polymer compound further contains an anion as a counter ion to the cation contained in the cationic functional group.
6. 6. The electrolyte for a lithium secondary battery according to claim 5, wherein the anion is an anion of a lithium salt contained in the electrolyte for a lithium secondary battery.
7. 2. The electrolyte for a lithium secondary battery according to claim 1, wherein the flame-retardant liquid electrolyte comprises at least one solvent selected from the group consisting of a carbonate-based compound, a phosphate-based compound, and an ionic liquid; and a lithium salt.
8. 2. The electrolyte for a lithium secondary battery according to claim 1, wherein the crosslinking agent is selected from the group consisting of ethoxylated trimethylolpropane triacrylate, trimethylolpropane ethoxy triacrylate, dipentaerythritol penta / hexa-acrylate, and tris(2-hydroxyethyl)isocyanurate triacrylate.
9. 2. The electrolyte for a lithium secondary battery according to claim 1, wherein the polymer electrolyte is present in an amount of 30 to 60 wt %, the flame-retardant liquid electrolyte is present in an amount of 30 to 50 wt %, and the crosslinker is present in an amount of 2 to 30 wt %.
10. The electrolyte for a lithium secondary battery according to claim 1 , further comprising an active oxide ceramic.
11. The active oxide ceramic is Li 1+x A x Ge 2-x (P.O. 4 ) 3 (LAGP), Li 7 La 3 Zr 2 O 12 (LLZO) and Li 1+x A x Ti 2-x (P.O. 4 ) 3 The electrolyte for a lithium secondary battery according to claim 10, wherein the electrolyte is selected from the group consisting of (LATP).
12. 11. The electrolyte for a lithium secondary battery according to claim 10, wherein the active oxide ceramic is included in an amount of 15 to 100 parts by weight based on 100 parts by weight of the total electrolyte for a lithium secondary battery including the polymer electrolyte, the flame-retardant liquid electrolyte, and the crosslinking agent.
13. A lithium secondary battery comprising: a positive electrode containing a lithium nickel cobalt manganese-based positive electrode active material; a negative electrode; and the electrolyte for lithium secondary batteries according to claim 1 interposed between the positive electrode and the negative electrode.
14. 14. The lithium secondary battery according to claim 13, wherein the electrolyte for the lithium secondary battery is attached in the form of a thin film to one surface of a positive electrode or a negative electrode, or is independently interposed between the positive electrode and the negative electrode.
15. The lithium secondary battery according to claim 13, further comprising a separate separator between the positive electrode and the negative electrode.
16. The lithium secondary battery according to claim 13, wherein the lithium secondary battery is a semi-solid battery including a liquid electrolyte and a solid electrolyte.
Citation Information
Patent Citations
Polyelectrolyte gel composition and method for producing the same
JP2001335706A
Nonaqueous absorber
JP2003251178A
Composition for polyelectrolytes, polyelectrolytes, electrical double layer capacitors and nonaqueous electrolyte secondary cells
WO2004027789A1
Bifunctional ionic liquids for electrolytes
WO2021225583A1